Low-temperature sulfur plasma passivated thin film solar cell absorption layer, preparation method therefor and use thereof

By ionizing sulfur plasma in the hydrogen sulfide atmosphere on the absorbing layer of the low-temperature thin-film solar cell, the surface of the absorption layer is passed through the problem of sulfur elements entering the grains, and the low temperature and low energy are achieved The passivation effect of consumption improves the efficiency and performance of solar cells.

WO2024239651A1PCT designated stage expired Publication Date: 2024-11-28SHENZHEN INST OF ADVANCED TECH CHINESE ACAD OF SCI
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/142448
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-24
Filing Date
2023-12-27
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

The traditional vulcanization method can easily cause sulfur elements to enter the grain during the vulcanization process of the absorbing layer of low-temperature thin-film solar cell, increasing defects and reducing film layer performance. Moreover, high-temperature vulcanization consumes high energy, which is not conducive to industrialization.

Method used

The sulfur plasma excitation device is used to ionize in the hydrogen sulfide atmosphere to generate sulfur plasma, passivate the surface of the absorbing layer, and reduce the plasma bombardment energy and contact distance through the magnetic field base and target design to ensure that passivation only occurs on the surface.

Benefits of technology

Low-temperature vulcanization without heating is achieved, and a passivation layer is formed only on the surface of nano-scale films, reducing processing time and cost, improving photoelectric conversion efficiency and reducing leakage current.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023142448_28112024_PF_FP_ABST
    Figure CN2023142448_28112024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed in the present invention are a low-temperature sulfur plasma passivated thin film solar cell absorption layer, a preparation method therefor and the use thereof. In the method, a newly designed sulfur plasma excitation device is used to perform sulfur plasma passivation treatment on the surface of a thin film solar cell absorption layer, so as to alter the state of aggregation of surface electron holes, which adjusts band alignment to suppress electron hole recombination at a grain boundary, thus reducing a leakage current and finally improving device efficiency. Provided in the present invention is a novel method which can effectively implement passivation without heating. With regard to a prepared CZTSe solar cell having subjected to passivation treatment, the open-circuit voltage is raised to 376.8 mV, the short-circuit current is reduced to 36.2 mA / cm2, the fill factor is increased to 69.5%, and the efficiency is increased to 8.98%.
Need to check novelty before this filing date? Find Prior Art

Description

A low-temperature sulfur plasma passivated thin-film solar cell absorber layer and its preparation method and application Technical Field

[0001] The present invention belongs to the technical field of solar cells, and in particular relates to a low-temperature sulfur plasma passivated thin-film solar cell absorption layer, a preparation method thereof, and an application thereof. Background Art

[0002] Thin-film solar cells, as a new type of photovoltaic energy storage device, utilize semiconductor technology to directly convert sunlight into electricity. Compared to traditional solar cells, thin-film solar cells, only a few microns thick, are translucent and flexible. They can effectively convert solar energy into electricity while reducing material usage, shortening deposition time, and enabling power generation even in low-light conditions. However, due to the low material quality, the efficiency of polycrystalline thin-film solar cells remains far below the theoretical SQ limit. The numerous defect sites in the absorber layer of these polycrystalline thin films serve as recombination sites for photogenerated electrons and holes, accelerating the recombination of photogenerated carriers.

[0003] Sulfurization of the surface of the absorption layer can reduce surface recombination and improve device efficiency by widening the band gap, and is considered to be an effective passivation method. However, the thin filmization of the absorption layer limits the realization of the passivation layer. Traditional sulfurization passivation usually requires high-temperature heat treatment. When the absorption layer material with a thickness of only a few microns is sulfurized and passivated, the sulfur element not only forms a passivation layer on the surface but also easily enters the interior of the grains, causing the absorption layer films such as CuInGaSe2 and Cu2ZnSnSe4 to form sulfur-containing quinary phase compounds, which increases the defects inside the grains and reduces the performance of the film layer. At the same time, high-temperature sulfurization requires higher temperatures and longer times, and requires higher energy consumption, which is very unfavorable for industrialization. Therefore, it is very necessary to find a sulfurization method that does not require heating and where passivation only occurs on the surface without affecting the interior of the grains.

[0004] Summary of the Invention

[0005] To overcome the shortcomings of the prior art, the present invention designs a sulfur plasma excitation device and provides a method for passivating the absorber layer of a thin-film solar cell using low-temperature sulfur plasma. The sulfur plasma excitation device generates sulfur plasma in a hydrogen sulfide atmosphere to passivate the absorber layer surface, including the following steps:

[0006] A method for preparing a low-temperature sulfur plasma passivated thin-film solar cell absorber layer comprises the following steps:

[0007] S1. Device construction:

[0008] A plasma excitation device is provided, including a magnetic field base, a target material, a grounded shell, etc.; a radio frequency power supply is used to provide high-voltage ionized plasma, and the energy of plasma bombarding the target surface is reduced by raising the distance between the target surface and the magnetic field, while reducing the distance between the target surface and the high voltage contact to increase the probability of plasma generation;

[0009] S2. Sample preparation:

[0010] Magnetron sputtering is sequentially performed on the substrate to prepare a bottom electrode and co-evaporation is performed to prepare an absorption layer of a thin-film solar cell;

[0011] S3, low temperature plasma surface sulfurization:

[0012] The sample prepared in step S2 is placed in a sulfur plasma excitation furnace of a plasma excitation device, a ceramic target is used as a working target, hydrogen sulfide is used as a working gas, and high voltage is applied to generate sulfur plasma to passivate the surface of the sample, so that a passivation layer is formed on the surface of the thin-film solar cell absorption layer of the sample to reduce dark current.

[0013] Preferably, in step S1 , the distance between the target surface and the magnetic field is raised so that the magnetic field intensity near the target surface is reduced to 10 Gauss to 20 Gauss.

[0014] Preferably, in step S1, the distance between the target surface and the high-voltage contact is reduced so that the distance between the positive electrode and the grounded shell is reduced to 1 mm to 5 mm.

[0015] Preferably, in step S2, the thin film solar cell absorption layer is selected from CdTe, CuInGaSe2, Cu2ZnSn(S,Se)4, Cu2Zn x Ⅱ 1-x Any one of SnS4(Ⅱ=Cd, Ba).

[0016] Preferably, in step S2, the thickness of the thin-film solar cell absorption layer is 1 μm to 2.5 μm.

[0017] Preferably, in step S3, the flow rate of hydrogen sulfide is 3 sccm to 10 sccm, the working gas pressure is 0.05 Pa to 1 Pa, the plasma excitation power is 40 W to 90 W, and the passivation treatment time is 1 min to 20 min.

[0018] Preferably, in step S3, the ceramic target is selected from any one of ZnO, SiO2, CdS, and Al2O3.

[0019] Preferably, the size of the ceramic target is The copper back target size is

[0020] The present invention also provides a low-temperature sulfur plasma passivation thin-film solar cell absorption layer prepared by the preparation method. A surface that inhibits electron-hole pair recombination is formed on the low-temperature sulfur plasma passivation thin-film solar cell absorption layer.

[0021] The present invention also provides the application of the low-temperature sulfur plasma passivated thin-film solar cell absorption layer prepared by the preparation method in a photovoltaic energy storage device, wherein a buffer layer, an intrinsic zinc oxide layer, a window layer and a second electrode layer are sequentially deposited on the low-temperature sulfur plasma passivated thin-film solar cell absorption layer to obtain a complete photovoltaic energy storage device.

[0022] Compared with the existing technology, the present invention has the following advantages:

[0023] This method does not require heating, and the sulfurization occurs only on the surface of the absorber layer of nanoscale thin-film solar cells, without affecting the interior of the grains, effectively reducing processing time and cost. The passivation layer formed by plasma surface sulfurization reduces the recombination of surface electron-hole pairs by widening the band gap, reducing leakage current and improving the photoelectric conversion efficiency of the device. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present invention and, together with the description, serve to explain the principles of the invention, in which:

[0025] FIG1 is a schematic diagram of a plasma excitation device provided by the present invention;

[0026] FIG2 is an SEM image of the copper-zinc-tin-selenium crystalline thin film absorption layer to be treated prepared in Examples 1 to 3 of the present invention;

[0027] 3 is an XPS graph of the surface of the copper-zinc-tin-selenium thin film absorber layer passivated by low-temperature sulfur plasma and after etching 3 nm prepared in Example 1 of the present invention;

[0028] 4 is a dark-state IV curve of the copper-zinc-tin-selenium thin film absorber layer before and after passivation by low-temperature sulfur plasma prepared in Example 3 of the present invention;

[0029] 5 is a comparison chart of the open circuit voltage, short circuit current, fill factor, and efficiency of the copper-zinc-tin-selenium thin film absorber layer before and after low-temperature sulfur plasma passivation prepared in Example 3 of the present invention;

[0030] FIG6 is a schematic flow chart of the present invention.

[0031] DETAILED DESCRIPTION

[0032] The following disclosure provides many different embodiments or examples for implementing different structures of the present invention. To simplify the disclosure of the present invention, the components and configurations of specific examples are described below. Of course, these are merely examples and are not intended to limit the present invention. In addition, the present invention may repeat reference numbers and / or reference letters in different examples. Such repetition is for the purpose of simplicity and clarity and does not in itself indicate the relationship between the various embodiments and / or configurations discussed.

[0033] Example 1

[0034] New device: By raising the distance between the target surface and the magnetic field, the magnetic field strength near the target surface is reduced to 10~20 gauss, thereby reducing the energy of plasma bombarding the target surface; at the same time, the distance between the target surface and the high-voltage contact is reduced, that is, the distance between the positive electrode and the grounded shell is reduced to 1~5mm, to increase the probability of plasma generation.

[0035] 10×10cm 2 Soda-lime glass of different sizes was used as the substrate. The glass substrate was cleaned conventionally with deionized water and a detergent. After the substrate was cleaned with high-purity nitrogen, molybdenum (Mo) was sputtered on its surface by a magnetron sputtering method in an argon atmosphere with a pressure of 0.5 Pa as a bottom electrode layer.

[0036] The metal thin film precursor was prepared by co-evaporation. The temperature control programs of copper, zinc, tin, selenium and substrate were raised to 1187 ℃, 368 ℃, 1181 ℃, 245 ℃ and 150 ℃ respectively, and co-evaporated and deposited on the molybdenum back electrode layer of the substrate. The precursor was maintained at this state for 30 minutes to form a copper-zinc-tin-selenium thin film precursor stacked on the molybdenum back electrode layer. It was then transferred to an annealing furnace, and H2Se with a flow rate of 50 sccm for 84 seconds and N2 with a flow rate of 2.0 slm for 86 seconds were introduced. The temperature was raised to 340 ℃ for 20 minutes and then maintained for 60 minutes. After that, the gas in the chamber was evacuated and H2Se with a flow rate of 50 sccm for 14 seconds and N2 with a flow rate of 2.0 slm for 84 seconds were introduced again. The temperature was raised to 490 ℃ for 30 minutes and maintained for 10 minutes. After cooling in the furnace, a high-quality CZTSe crystalline absorption layer thin film sample with a thickness of 1.2 μm was obtained.

[0037] The CZTSe sample to be processed was transferred to the sulfur plasma excitation furnace. CdS was selected as the target. The target and the magnetic field were raised to a magnetic field strength of 20 Gauss near the target. The distance between the positive electrode and the grounded shell was reduced to 2 mm. The background vacuum value in the plasma excitation furnace was ensured to be at least 8×10 -4Pa, then 40 sccm of argon gas was introduced into the plasma excitation furnace, and the working pressure in the sputtering chamber was adjusted to 0.5 Pa. The target surface was first pre-cleaned at 75 W for 5 minutes, with the gear lever turned off during the process to prevent contamination of the sample. After the pre-cleaning treatment was completed, the argon gas was stopped and 5 sccm of hydrogen sulfide gas was introduced. The working pressure was adjusted to 0.5 Pa, and the plasma excitation power was adjusted to 45 W. The sulfur plasma treatment of the sample surface was started for 2 minutes, and finally a surface-passivated CZTSe thin film sample was obtained. A buffer layer, an intrinsic zinc oxide layer, a window layer, and a second electrode layer were sequentially fabricated on the passivated CZTSe thin film absorption layer to obtain a complete device.

[0038] Figure 2 is an SEM image of the CZTSe crystalline thin film absorption layer to be treated prepared in Example 1 of the present invention; Figure 3 is an XPS image of the copper-zinc-tin-selenium thin film absorption layer passivated by low-temperature sulfur plasma prepared in Example 1 of the present invention before and after treatment and etching of 3nm. There is no S peak on the surface before passivation treatment, and an S 2p peak appears on the surface after low-temperature sulfur plasma treatment, indicating that the surface is successfully passivated by sulfur plasma, and the S 2p peak disappears after etching 3nm, indicating that the low-temperature sulfur plasma passivation method of the present invention only occurs on the surface within 3nm and does not occur inside the grains.

[0039] Example 2

[0040] 10×10cm 2 Soda-lime glass of different sizes was used as the substrate. The glass substrate was cleaned conventionally with deionized water and a detergent. After the substrate was cleaned with high-purity nitrogen, molybdenum (Mo) was sputtered on its surface by a magnetron sputtering method in an argon atmosphere with a pressure of 0.5 Pa as a bottom electrode layer.

[0041] The metal thin film precursor was prepared by co-evaporation. The temperature control programs of copper, zinc, tin, selenium and substrate were raised to 1187 ℃, 368 ℃, 1181 ℃, 245 ℃ and 150 ℃ respectively, and co-evaporated and deposited on the molybdenum back electrode layer of the substrate. The precursor was maintained at this state for 30 minutes to form a copper-zinc-tin-selenium thin film precursor stacked on the molybdenum back electrode layer. It was then transferred to an annealing furnace, and H2Se with a flow rate of 50 sccm for 84 seconds and N2 with a flow rate of 2.0 slm for 86 seconds were introduced. The temperature was raised to 340 ℃ for 20 minutes and then maintained for 60 minutes. After that, the gas in the chamber was evacuated and H2Se with a flow rate of 50 sccm for 14 seconds and N2 with a flow rate of 2.0 slm for 84 seconds were introduced again. The temperature was raised to 490 ℃ for 30 minutes and maintained for 10 minutes. After cooling in the furnace, a high-quality CZTSe crystalline absorption layer thin film sample with a thickness of 1.2 μm was obtained.

[0042] The CZTSe sample to be processed was transferred to a sulfur plasma excitation furnace. Al2O3 was selected as the target. The target and the magnetic field were raised to a magnetic field strength of 20 Gauss near the target. The distance between the positive electrode and the grounded shell was reduced to 1 mm. The background vacuum value in the plasma excitation furnace was ensured to be at least 8×10 -4 Pa, then 40 sccm of argon gas was introduced into the plasma excitation furnace, and the working pressure in the sputtering chamber was adjusted to 1 Pa. The target surface was first pre-cleaned at 75 W for 5 minutes, with the gear lever turned off during the process to prevent contamination of the sample. After the pre-cleaning treatment was completed, the argon gas was stopped and 5 sccm of hydrogen sulfide gas was introduced. The working pressure was adjusted to 1 Pa, and the plasma excitation power was adjusted to 45 W. The sulfur plasma treatment of the sample surface was started for 20 minutes, and finally a surface-passivated CZTSe thin film sample was obtained. A buffer layer, an intrinsic zinc oxide layer, a window layer, and a second electrode layer were sequentially fabricated on the passivated CZTSe thin film absorption layer to obtain a complete device.

[0043] FIG2 is a SEM image of the CZTSe crystalline thin film absorption layer to be treated prepared in Example 2 of the present invention.

[0044] Example 3

[0045] 10×10cm 2 Soda-lime glass of different sizes was used as a substrate. The glass substrate was cleaned conventionally using deionized water and a detergent. After being blown clean using high-purity nitrogen, molybdenum (Mo) was sputtered on its surface as a bottom electrode layer by a magnetron sputtering method in an argon atmosphere with a pressure of 0.5 Pa.

[0046] The metal thin film precursor was prepared by co-evaporation. The temperature control programs of copper, zinc, tin, selenium and substrate were raised to 1187 ℃, 368 ℃, 1181 ℃, 245 ℃ and 150 ℃ respectively, and then co-evaporated and deposited on the molybdenum back electrode layer of the substrate. It was maintained in this state for 30 minutes to form a copper-zinc-tin-selenium thin film precursor stacked on the molybdenum back electrode layer. It was then transferred to an annealing furnace, and H2Se with a flow rate of 50 sccm for 84 seconds and N2 with a flow rate of 2.0 slm for 86 seconds were introduced. The temperature was raised to 340 ℃ for 20 minutes and then maintained for 60 minutes. After that, the gas in the chamber was evacuated and H2Se with a flow rate of 50 sccm for 14 seconds and N2 with a flow rate of 2.0 slm for 84 seconds were introduced again. The temperature was raised to 490 ℃ for 30 minutes and maintained for 10 minutes. After cooling in the furnace, a high-quality CZTSe crystalline absorption layer thin film sample with a thickness of 1.2 μm was obtained.

[0047] The CZTSe sample to be processed was transferred to a sulfur plasma excitation furnace. ZnO was selected as the target. The target and the magnetic field were raised to a magnetic field strength of 20 Gauss near the target. The distance between the positive electrode and the grounded shell was reduced to 4 mm. The background vacuum value in the plasma excitation furnace was ensured to be at least 8×10 -4 Pa, then 40 sccm of argon gas was introduced into the plasma excitation furnace, and the working pressure in the sputtering chamber was adjusted to 0.2 Pa. First, the target surface was pre-cleaned at 85 W for 5 minutes, and the gear lever was turned off during the process to prevent contamination of the sample. After the pre-cleaning treatment was completed, the argon gas was stopped and 5 sccm of hydrogen sulfide gas was introduced. The working pressure was adjusted to 1 Pa, and the plasma excitation power was adjusted to 85 W. The sulfur plasma treatment of the sample surface was started for 3 minutes, and finally a surface passivated CZTSe thin film sample was obtained. The buffer layer, intrinsic zinc oxide layer, window layer and second electrode layer were sequentially fabricated on the passivated thin film absorption layer to obtain a complete device.

[0048] Figure 2 is an SEM image of the CZTSe crystalline thin film absorption layer to be treated prepared in Example 3 of the present invention; Figure 4 is a dark state IV curve of the copper zinc tin selenium thin film absorption layer before and after low-temperature sulfur plasma passivation prepared in Example 3 of the present invention. The dark current is effectively reduced after passivation treatment; Figure 5 is a comparison of the open circuit voltage, short circuit current, fill factor, and efficiency of the copper zinc tin selenium thin film absorption layer before and after low-temperature sulfur plasma passivation prepared in Example 3 of the present invention. After passivation treatment, the open circuit voltage is increased to 376.8mV and the short circuit current is reduced to 36.2mA / cm 2 , the fill factor is increased to 69.5% and the efficiency is increased to 8.98%.

[0049] Other embodiments of the present invention will readily occur to those skilled in the art upon consideration of the specification and practice of the invention herein. The present invention is intended to cover any variations, uses, or adaptations of the present invention that follow the general principles of the invention and include common knowledge or customary techniques in the art. The description and examples are to be considered as exemplary only, with the true scope and spirit of the invention being indicated by the claims.

[0050] It should be understood that the present invention is not limited to the exact construction described above and shown in the drawings, and that various modifications and changes may be made without departing from the scope thereof. The scope of the present invention is limited only by the appended claims.

Claims

1. A method for preparing a low-temperature sulfur plasma passivated thin-film solar cell absorber layer, characterized in that: The following steps are involved: S1. Device construction: A plasma excitation device is provided, including a magnetic field base, a target material, a grounded shell, etc.; a radio frequency power supply is used to provide high-voltage ionized plasma, and the energy of plasma bombarding the target surface is reduced by raising the distance between the target surface and the magnetic field, and the distance between the target surface and the high voltage contact is reduced to increase the probability of plasma generation; S2. Sample preparation: Magnetron sputtering is sequentially performed on the substrate to prepare a bottom electrode and co-evaporation is performed to prepare an absorption layer of a thin-film solar cell; S3, low temperature plasma surface sulfurization: The sample prepared in step S2 is placed in the sulfur plasma excitation furnace of the plasma excitation device, a ceramic target is used as a working target, hydrogen sulfide is used as a working gas, and high voltage is applied to generate sulfur plasma to passivate the surface of the sample, so that a passivation layer is formed on the surface of the thin-film solar cell absorption layer of the sample to reduce dark current.

2. The method for preparing the low-temperature sulfur plasma passivated thin-film solar cell absorber layer according to claim 1, characterized in that: In step S1, the distance between the target surface and the magnetic field is raised so that the magnetic field strength near the target surface is reduced to 10 Gauss to 20 Gauss.

3. The method for preparing the absorption layer of a low-temperature sulfur plasma passivated thin-film solar cell according to claim 1, characterized in that: In step S1, the distance between the target surface and the high voltage contact is reduced so that the distance between the positive electrode and the grounded shell is reduced to 1 mm to 5 mm.

4. The method for preparing the low-temperature sulfur plasma passivated thin-film solar cell absorber layer according to claim 1, characterized in that: In step S2, the thin film solar cell absorption layer is selected from CdTe, CuInGaSe2, Cu2ZnSn(S,Se)4, Cu2Zn x Ⅱ 1-x Any one of SnS4(Ⅱ=Cd, Ba).

5. The method for preparing the absorption layer of a low-temperature sulfur plasma passivated thin-film solar cell according to claim 1, characterized in that: In step S2, the thickness of the thin film solar cell absorption layer is 1 μm to 2.5 μm.

6. The method for preparing the absorption layer of a low-temperature sulfur plasma passivated thin-film solar cell according to claim 1, characterized in that: In step S3, the flow rate of hydrogen sulfide is 3 sccm to 10 sccm, the working gas pressure is 0.05 Pa to 1 Pa, the plasma excitation power is 40 W to 90 W, and the passivation treatment time is 1 min to 20 min.

7. The method for preparing the absorption layer of a low-temperature sulfur plasma passivated thin-film solar cell according to claim 1, characterized in that: In step S3, the ceramic target is selected from any one of ZnO, SiO2, CdS, and Al2O3.

8. The method for preparing the absorption layer of a low-temperature sulfur plasma passivated thin-film solar cell according to claim 1, characterized in that: The size of the ceramic target is The copper back target size is 9. The low-temperature sulfur plasma passivated thin-film solar cell absorption layer prepared by the preparation method according to any one of claims 1 to 8, characterized in that: The low-temperature sulfur plasma passivated thin-film solar cell absorption layer forms a surface that inhibits the recombination of electron-hole pairs.

10. Application of the low-temperature sulfur plasma passivated thin-film solar cell absorption layer prepared by the preparation method according to any one of claims 1 to 8 in photovoltaic energy storage devices, characterized in that: A buffer layer, an intrinsic zinc oxide layer, a window layer and a second electrode layer are sequentially deposited on the low-temperature sulfur plasma passivated thin-film solar cell absorption layer to obtain a complete photovoltaic energy storage device.

Citation Information

Patent Citations

  • Copper zinc tin sulfur thin film solar cell and preparation method thereof

    CN108336177A

  • Preparation method of copper-zinc-tin-sulfur-selenium thin film with sulfur component gradient

    CN112563117A

  • Copper-indium-gallium-selenium thin-film solar cell and preparation method thereof

    CN112736150A

  • Low-temperature sulfur plasma passivation thin-film solar cell absorption layer and preparation method and application thereof

    CN116544310A

  • Plasma annealing of thin film solar cells

    US20140045295A1