Perovskite thin film layer and preparation method therefor, and perovskite-crystalline silicon tandem cell and preparation method therefor
Through the design of a perovskite film layer with a two-layer structure, the first perovskite layer reacts with lead iodide to reduce residues, and the second perovskite layer is formed through low-pressure drying and annealing, the problem of lead iodide residues in traditional methods is solved. , improves the efficiency and stability of perovskite crystal silicon stacked batteries.
Patent Information
- Application Number
- PCT/CN2024/090405
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-23
- Filing Date
- 2024-04-28
- Publication Date
- 2024-11-28
AI Technical Summary
In the traditional perovskite film layer preparation method, the two-step method of combining thermal evaporation and solution method can easily lead to the residue of lead iodide, affecting the stability of the interface between the perovskite film layer and the hole transport layer and the battery efficiency.
A perovskite film layer adopts a two-layer structure, the first perovskite layer with a thickness of 5nm to 10nm and the second perovskite layer with a thickness of 480nm to 530nm, through A-position cations and iodine The lead-iodide reaction is prepared to reduce the residue of lead iodide, and dry it under low pressure to form the first perovskite layer and anneale to form the second perovskite layer.
The suede-retaining effect and stability of the perovskite film layer are achieved, the lead iodide residue is reduced, and the energy conversion efficiency and electrical performance of the perovskite crystalline silicon stacked battery are improved.
Smart Images

Figure CN2024090405_28112024_PF_FP_ABST
Abstract
Description
Perovskite thin film layer and preparation method, perovskite crystalline silicon stacked cell and preparation method
[0001] This application claims priority to the Chinese patent application filed with the Patent Office of China on May 23, 2023, with application number CN202310590372.3 and public name “Perovskite thin film layer and preparation method, perovskite crystalline silicon stacked cell and preparation method”, the entire contents of which are incorporated by reference into this application. Technical Field
[0002] The present disclosure relates to the field of solar cells, and in particular to a perovskite thin film layer and a preparation method thereof, and a perovskite crystalline silicon stacked cell and a preparation method thereof. Background Art
[0003] The perovskite thin film is the photoactive layer in the top cell, playing a key role in absorbing sunlight to generate photocurrent. High-efficiency perovskite / crystalline silicon tandem cells require a perovskite film thickness of approximately 500nm. This thickness is difficult to achieve with a velvet-like finish using traditional solution-based methods.
[0004] Currently, perovskite thin films that maintain a textured surface are typically prepared using a two-step process combining thermal evaporation and solution deposition. However, this two-step process is prone to residual lead iodide at the bottom of the perovskite layer. Lead iodide is an n-type semiconductor, and for pin-structured perovskite top cells, it hinders hole extraction at the interface between the perovskite thin film and the hole transport layer, thereby affecting device efficiency.
[0005] Summary of the Invention
[0006] According to various embodiments of the present disclosure, a perovskite thin film layer is provided, comprising a first perovskite layer and a second perovskite layer stacked on the first perovskite layer, wherein the first perovskite layer has a thickness of 5 nm to 10 nm, and the second perovskite layer is formed by reacting an A-site cation solution with lead iodide.
[0007] In some embodiments of the present disclosure, the composition of the first perovskite layer includes Cs x FA y MA 1- x-y PbI z Br 3-z , where x=0~1, y=0~1, z=0~3.
[0008] In some embodiments of the present disclosure, x is 0 to 0.1, and y is 0.6 to 0.8.
[0009] In some embodiments of the present disclosure, the optical band gap of the first perovskite layer is lower than the optical band gap of the second perovskite layer, and the optical band gap of the first perovskite layer is 1.60 eV to 1.65 eV.
[0010] In some embodiments of the present disclosure, the A-site cation is one or a combination of iodomethane, bromomethylamine and chloromethylamine.
[0011] In some embodiments of the present disclosure, the A-site cation includes iodoformamidine, bromomethylamine and chloromethylamine, and the mass ratio of iodoformamidine, bromomethylamine and chloromethylamine is (30-40): (5-10): (2-6).
[0012] In some embodiments of the present disclosure, the thickness of the second perovskite layer is 480 nm to 530 nm.
[0013] According to various embodiments of the present disclosure, a method for preparing a perovskite thin film layer is also provided, comprising the following steps:
[0014] Preparation of the first perovskite layer: forming a first perovskite layer with a thickness of 5 nm to 10 nm on the hole transport layer of the perovskite crystalline silicon tandem cell by evaporation or solution film formation;
[0015] Preparing a second perovskite layer: preparing a lead iodide skeleton layer on the side of the first perovskite layer away from the hole transport layer, coating an A-site cation solution on the side of the lead iodide skeleton layer away from the hole transport layer, and annealing to form a second perovskite layer.
[0016] In some embodiments of the present disclosure, the composition of the first perovskite layer includes Cs x FA y MA 1- x-y PbI z Br 3-z , where x=0~1, y=0~1, z=0~3.
[0017] In some embodiments of the present disclosure, x is 0 to 0.1, and y is 0.6 to 0.8.
[0018] In some embodiments of the present disclosure, the optical band gap of the first perovskite layer is lower than the optical band gap of the second perovskite layer, and the optical band gap of the first perovskite layer is 1.60 eV to 1.65 eV.
[0019] In some embodiments of the present disclosure, the A-site cation is one or a combination of iodomethane, bromomethylamine and chloromethylamine.
[0020] In some embodiments of the present disclosure, the A-site cation includes iodoformamidine, bromomethylamine and chloromethylamine, and the mass ratio of iodoformamidine, bromomethylamine and chloromethylamine is (30-40): (5-10): (2-6).
[0021] In some embodiments of the present disclosure, the thickness of the second perovskite layer is 480 nm to 530 nm.
[0022] In some embodiments of the present disclosure, in the step of preparing the first perovskite layer, the solution film forming method is: taking a perovskite precursor solution and coating it on the hole transport layer, and then drying it to obtain the first perovskite layer.
[0023] In some embodiments of the present disclosure, in the step of preparing the first perovskite layer, the drying is performed at an air pressure below 100 Pa and maintained for 40s to 60s.
[0024] In some embodiments of the present disclosure, at least one of 2-methoxyethanol and acetonitrile is used as a solvent in the perovskite precursor solution.
[0025] In some embodiments of the present disclosure, the 2-methoxyethanol and the acetonitrile are used together as a solvent, and the mass ratio of the 2-methoxyethanol to the acetonitrile is (6-8):(2-4).
[0026] In some embodiments of the present disclosure, the solution is formed into a film by slit coating, spraying, inkjet printing or doctor blade coating.
[0027] In some embodiments of the present disclosure, the thickness of the lead iodide skeleton layer is 300 nm to 350 nm.
[0028] According to various embodiments of the present disclosure, a perovskite crystalline silicon stacked cell is provided, comprising a crystalline silicon bottom cell with a suede structure, a carrier recombination layer, a hole transport layer, a perovskite thin film layer, and an electron transport layer stacked in sequence;
[0029] The perovskite thin film layer is the above-mentioned perovskite thin film layer or the perovskite thin film layer prepared by the above-mentioned method for preparing a perovskite thin film layer;
[0030] The perovskite crystalline silicon stacked cell further includes a positive electrode and a negative electrode. The negative electrode forms an ohmic contact with the transparent conductive oxide layer, and the positive electrode forms an ohmic contact with the back surface of the crystalline silicon bottom cell.
[0031] In some embodiments of the present disclosure, the perovskite crystalline silicon stacked cell further includes a buffer layer, the buffer layer is tin dioxide, and the thickness of the buffer layer is 20 nm to 30 nm.
[0032] In some embodiments of the present disclosure, the thickness of the crystalline silicon bottom cell is 5 nm to 10 nm.
[0033] In some embodiments of the present disclosure, the carrier recombination layer includes nickel oxide, PTAA or Spiro-TBB, and the thickness of the carrier recombination layer is 15 nm to 25 nm.
[0034] In some embodiments of the present disclosure, the electron transport layer is C60 or PCBM, and the thickness of the electron transport layer is 20 nm to 25 nm.
[0035] In some embodiments of the present disclosure, the positive electrode and the negative electrode are both made of silver, the thickness of the positive electrode is 250 nm to 350 nm, and the thickness of the negative electrode is 150 nm to 350 nm.
[0036] According to various embodiments of the present disclosure, a method for preparing a perovskite crystalline silicon tandem cell is also provided, comprising the following steps:
[0037] Provide crystalline silicon bottom cells;
[0038] Preparing a carrier recombination layer on the N-side of the crystalline silicon bottom cell;
[0039] preparing a hole transport layer on the carrier recombination layer;
[0040] Preparing the above-mentioned perovskite thin film layer or the perovskite thin film layer prepared by the above-mentioned method for preparing the perovskite thin film layer on the hole transport layer;
[0041] preparing an electron transport layer on the perovskite thin film layer;
[0042] preparing a transparent conductive oxide layer on the electron transport layer;
[0043] Post-processing is performed to obtain perovskite crystalline silicon tandem cells.
[0044] In some embodiments of the present disclosure, the hole transport layer is prepared by magnetron sputtering.
[0045] In some embodiments of the present disclosure, the electron transport layer is prepared by evaporation.
[0046] In some embodiments of the present disclosure, the transparent conductive oxide layer is prepared by magnetron sputtering.
[0047] In some embodiments of the present disclosure, the positive electrode and the negative electrode are both prepared by thermal evaporation.
[0048] The details of one or more embodiments of the present disclosure are set forth in the accompanying drawings and the description below. Other features, objects, and advantages of the present disclosure will become apparent from the description, drawings, and claims. BRIEF DESCRIPTION OF THE DRAWINGS
[0049] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0050] FIG1 is a schematic diagram of the steps for preparing the perovskite thin film layer of Example 1 (upper figure) and Comparative Example 1 (lower figure) of the present application, wherein a represents slit coating, b represents thermal evaporation, and c represents slit coating.
[0051] FIG2 is a cross-sectional view of the perovskite crystalline silicon tandem cell of the present application.
[0052] FIG3 is a SEM image of Application Example 1.
[0053] FIG4 is a SEM image of the comparative example 1.
[0054] FIG5 is an IV curve diagram of Application Example 1 and Comparative Example 1 of the present application.
[0055] Icons: 1. Crystalline silicon bottom cell; 2. Carrier recombination layer; 3. Hole transport layer; 4. Perovskite thin film layer; 41. First perovskite layer; 42. Lead iodide skeleton layer; 43. Second perovskite layer; 5. Electron transport layer; 6. Buffer layer; 7. Transparent conductive oxide layer; 8. Positive electrode; 9. Negative electrode. DETAILED DESCRIPTION
[0056] The following will clearly and completely describe the technical solutions in the embodiments of the present invention in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. All other embodiments obtained by ordinary technicians in this field based on the embodiments of the present invention without making any creative efforts shall fall within the scope of protection of the present invention.
[0057] Perovskite crystalline silicon tandem cells are devices that convert solar energy directly into electrical energy. The perovskite thin film layer serves as the photoactive layer in the top cell, absorbing light and generating photogenerated electrons and holes. Traditional crystalline silicon cells have a pyramidal surface. To maximize compatibility with the existing production process for crystalline silicon bottom cells, the various process layers of the perovskite top cell must also maintain a conformal finish. This means that each layer of the top cell should be deposited parallel to the pyramidal surface of the bottom cell, and after deposition, each layer should have the same pyramidal shape as the bottom cell. This velvet-conserving process has two main functions. First, the velvet pyramid size of the current mainstream crystalline silicon bottom cell is approximately 2μm to 5μm. If the velvet of each film layer of the top cell is not conformal, in order to completely cover the velvet pyramid of the crystalline silicon bottom cell, the thickness of each film layer should exceed the height of the velvet pyramid. That is, each film layer must be prepared to a thickness of micrometers. The thickness of each film layer of conventional perovskite solar cells is nanometers, which will significantly increase the material consumption of each film layer. Second, if the velvet is not conformal, the thickness of each film layer of the top cell will be uneven compared to the crystalline silicon bottom cell. For example, the film layer near the top of the pyramid is thinner, and the film layer near the base of the pyramid is thicker. The uneven film thickness is not conducive to the balance of charge transfer, which in turn reduces the efficiency of the device. Changing the production process of the crystalline silicon bottom cell to prepare a crystalline silicon bottom cell with a smaller velvet or polished crystalline silicon bottom cell is one way to reduce the impact of the velvet conformal of the crystalline silicon bottom cell. However, this will increase the difficulty and cost of bottom cell production, which is not conducive to large-scale production.
[0058] High-efficiency perovskite silicon tandem cells require a perovskite film thickness of approximately 500nm. Traditional solution-based methods for producing perovskite films of this thickness cannot achieve a conformal texture. The commonly used two-step process for preparing textured perovskite films is a combination of thermal evaporation and solution deposition. First, a conformal lead iodide layer is deposited via thermal evaporation as a backbone. Then, a solution-based method is used to prepare a layer of A-site cation solution that reacts with the lead iodide backbone to form the conformal textured perovskite film.
[0059] The bottom of the perovskite thin film layer prepared by the two-step method combining thermal evaporation and solution method often has residual lead iodide that has not reacted with the A-site cation solution. Lead iodide is an N-type semiconductor with poor hole transport performance. The residual lead iodide at the interface between the perovskite thin film layer and the hole transport layer will hinder the extraction of holes, thereby reducing the energy conversion efficiency of the battery.
[0060] The present application provides a perovskite thin film layer and a preparation method thereof, a perovskite crystalline silicon stacked battery and a preparation method thereof. The perovskite thin film layer has a good suede surface shape retention effect and can overcome the defect that lead iodide residue is easily generated in the perovskite thin film layer prepared by the reaction of lead iodide and A-site cations.
[0061] In the first aspect, the present application provides a perovskite thin film layer for a perovskite crystalline silicon tandem cell. Referring to Figure 1, the perovskite thin film layer 4 includes a first perovskite layer 41 disposed on the hole transport layer 3 of the perovskite crystalline silicon tandem cell and a second perovskite layer 43 stacked on the first perovskite layer 41. The first perovskite layer 41 has a thickness of 5nm to 10nm, and the second perovskite layer 43 has a thickness of 480nm to 530nm. The second perovskite layer 43 is made by reacting an A-site cation solution with lead iodide.
[0062] The perovskite thin film layer 4 has a first perovskite layer 41 with a thickness of 5nm to 10nm as the film layer on the surface of the hole transport layer 3, and a second perovskite layer 43 with a thickness of 480nm to 530nm is stacked on the first perovskite layer 41 of this thickness. The resulting perovskite thin film layer 4 has a uniform overall thickness and a good textured surface conformal effect, making it suitable for use on crystalline silicon bottom cells 1 with textured surface conformal requirements. The perovskite thin film layer 4 of the present application is not prone to lead iodide residue, which is beneficial to improving the stability of the interface between the perovskite thin film layer 4 and the electron transport layer 5. This is because the present application sets the first perovskite layer 41 and controls the thickness of the first perovskite layer 41 to 5nm to 10nm, which can fully induce the reaction of lead iodide and A-site cations to form perovskite crystals, and the first perovskite layer 41 itself can also react with the contacted lead iodide, thereby reducing the lead iodide residue caused by the difficulty of fully reacting lead iodide and A-site cations, reducing the generation of defects at the interface between the perovskite film layer 4 and the electron transport layer 5, and improving the stability of the perovskite film layer 4. At the same time, the first perovskite layer 41 of this thickness can also play a role in isolating lead iodide and the hole transport layer 3, and can block the negative impact of the residual lead iodide from the reaction on the hole extraction at the interface between the hole transport layer 3 and the perovskite film layer 4, thereby reducing the generation of defects at the interface between the hole transport layer 3 and the perovskite film layer 4, and further improving the stability at the interface between the perovskite film layer 4 and the electron transport layer 5.
[0063] For example, the thickness of the first perovskite layer 41 can be 5nm, 6nm, 7nm, 8nm, 9nm, 10nm, and the thickness of the second perovskite layer 43 can be 480nm, 485nm, 490nm, 495nm, 500nm, 505nm, 510nm, 515nm, 520nm, 525nm, 530nm. When the thickness of the first perovskite layer 41 is greater than 10nm, the overall velvet shape retention effect of the perovskite thin film layer 4 is poor, and the film thickness is prone to unevenness, which is not conducive to the balance of charge transfer, thereby reducing the electrical properties of the overall perovskite. When the thickness of the first perovskite layer 41 is less than 5nm, the first perovskite layer 41 has a poor effect of isolating lead iodide and inducing the reaction crystallization of lead iodide and A-site cations. Lead iodide residue is likely to appear, which is not conducive to hole extraction at the interface between the electron transport layer 5 and the perovskite thin film layer 4.
[0064] In some embodiments, the composition of the first perovskite layer 41 is Cs x FA y MA 1-x-y PbI z Br 3-z , where x=0~1, y=0~1, z=0~3.
[0065] In the first perovskite layer 41, FA represents a formamidinium ion, and MA represents a methylamine ion. The first perovskite layer 41 of this composition has a stable lattice, effectively inducing the growth and crystallization of the subsequently prepared lead iodide skeleton layer 42 and promoting the reaction between the A-site cations and lead iodide, thereby reducing residual lead iodide. Furthermore, the first perovskite layer 41 and the second perovskite layer 43 of this composition are easily combined in the subsequent annealing step, thereby eliminating the influence of the contact interface between the first perovskite layer 41 and the second perovskite layer 43, forming an overall perovskite film layer 4 with excellent crystallization properties, and reducing defects in the perovskite film layer 4.
[0066] Preferably, the optimal range of x is 0 to 0.1, and the optimal value is 0.05. The optimal range of y is 0.6 to 0.8, and the optimal value is 0.77. In the first perovskite layer 41 of the above ratio, FA is used as the main cation, the y value is high, and the contents of Cs and MA are low. The adjustment of Br ions is beneficial to adjusting the band gap, and Cs ions offset the lattice distortion caused by Br, thereby improving the phase stability of the perovskite. In addition, the FA ion radius is large, and the perovskite lattice distortion is large, resulting in poor stability of the perovskite film layer 4. The addition of MA can balance the lattice distortion of FA and improve the stability of the perovskite. At the same time, an appropriate amount of Cs ions is added to make the main component of the second perovskite layer close to that of the first perovskite layer. After the annealing treatment of the second perovskite layer 43, the first perovskite layer 41 is more easily combined with the second perovskite layer 43, reducing the influence of the contact interface between the first perovskite layer 41 and the second perovskite layer 43.
[0067] In some embodiments, the optical band gap of the first perovskite layer 41 is 1.60 eV to 1.65 eV.
[0068] The optimal band gap of the second perovskite layer 43 is 1.66 eV. The band gap of the first perovskite layer 41 is slightly smaller than that of the second perovskite layer 43. Because the first perovskite layer 41 is located at the bottom of the second perovskite layer 43, most of the short-wave sunlight is absorbed by the second perovskite layer 43. Therefore, the first perovskite layer 41 is provided with a narrower optical band gap to absorb the remaining small amount of long-wave sunlight, thereby improving the light absorption effect of the perovskite thin film layer 4. In addition, the first perovskite layer 41 with such an optical band gap can induce the growth and crystallization of lead iodide, promote the reaction between the A-site cation and lead iodide, and help reduce the residual lead iodide.
[0069] In some embodiments, the A-site cation is one or more of iodoformamidine, bromomethylamine, and chloromethylamine. More preferably, the mass ratio of iodoformamidine, bromomethylamine, and chloromethylamine is (30-40): (5-10): (2-6). Lead iodide mixed with the A-site cations in the aforementioned ratio reacts rapidly and crystallizes to form a second perovskite layer 43 with a good suede-like shape retention and a thickness of 480 nm to 530 nm.
[0070] In a second aspect, the present application further provides a method for preparing a perovskite thin film layer for a perovskite crystalline silicon tandem cell according to the first aspect, comprising the following steps:
[0071] Preparation of the first perovskite layer 41: forming a first perovskite layer 41 with a thickness of 5 nm to 10 nm on the hole transport layer 3 of the perovskite crystalline silicon stacked cell by evaporation or solution film formation;
[0072] Preparation of the second perovskite layer 43: A lead iodide skeleton layer 42 is prepared on the side of the first perovskite layer 41 away from the hole transport layer 3, and an A-site cation solution is coated on the side of the lead iodide skeleton layer 42 away from the hole transport layer 3. After annealing, a second perovskite layer 43 with a thickness of 480 nm to 530 nm is obtained.
[0073] The second perovskite layer 43 is prepared on the basis of the above-mentioned first perovskite layer 41. Lead iodide is easy to react completely, and lead iodide can react completely within a larger operating range. The process window is large and the requirements for the control accuracy of process parameters are low, which is conducive to reducing production difficulty and improving yield. The Voc and FF of the device are significantly improved, and the energy conversion efficiency of the device is finally significantly improved.
[0074] In some embodiments, the solution film forming method is as follows: in the step of preparing the first perovskite layer 41 , drying is performed at an air pressure below 100 Pa for 40 seconds to 60 seconds.
[0075] The step of preparing the first perovskite layer 41 can adopt a solution film forming method. After the perovskite precursor solution is coated on the hole transport layer 3, it is dried under the condition of air pressure less than or equal to 100 Pa to quickly evaporate the solvent of the perovskite precursor solution. Generally, the drying can be completed in 40s to 60s, and a first perovskite layer 41 with a thickness of 5nm to 10nm is formed. On this basis, when preparing the second perovskite layer, the lead iodide skeleton layer 42 is reacted with the A-site cation solution and then annealed to obtain a second perovskite layer of a specific thickness, thereby forming a perovskite thin film layer. Among them, the above-mentioned drying of the perovskite precursor solution can be carried out at room temperature, without special requirements, and can fluctuate within the room temperature range, for example, it can be carried out under conventional temperature conditions such as 15°C, 20°C, 25°C or 30°C.
[0076] Unlike the practice of performing annealing once when preparing a perovskite layer, the embodiment of the present application adopts a solution film formation method of drying the perovskite precursor solution under room temperature and low pressure conditions when preparing the first perovskite layer, and annealing is performed again when preparing the second perovskite layer. Since annealing operation is not required when preparing the first perovskite layer, the problem of excessive grain size in the thinner first perovskite layer due to annealing can be avoided. This approach can further improve the overall performance of the perovskite film layer of the embodiment of the present application.
[0077] Specifically, when preparing the first perovskite layer 41 with a relatively thin thickness, by controlling the above-mentioned drying conditions, the solvent in the perovskite precursor solution can be quickly volatilized and removed, prompting the perovskite precursor to gradually crystallize to form the first perovskite layer 41 with a smaller grain size and a larger grain specific surface area, thereby ensuring that the prepared first perovskite layer 41 has the characteristics of a smaller grain size and a larger grain specific surface area while having a relatively thin thickness, providing structural advantages for exerting the isolation effect of the first perovskite layer and the subsequent reaction with the residual lead iodide in the second perovskite layer. On this basis, in the process of preparing the second perovskite layer, after the A-site cation solution is coated on the lead iodide skeleton layer, the annealing treatment can not only promote the reaction of lead iodide with the A-site cation, but also further promote the first perovskite layer 41 with a small grain size and a large grain specific surface area to fully contact and react with the remaining lead iodide in the second perovskite layer 42, thereby reducing the residual lead iodide and at the same time forming a well-crystalline perovskite film layer 4 overall structure, effectively reducing the defects of the perovskite film layer 4, and promoting the overall performance improvement of the perovskite film layer 4.
[0078] In some embodiments, the solution film formation method includes slit coating, spray coating, inkjet printing, and doctor blade coating. The first perovskite layer 41 is relatively thin. This solution film formation method has high raw material utilization, high precision, and low energy consumption. The resulting perovskite thin layer has good uniformity and is suitable for the preparation of large-area perovskite film layers.
[0079] In some embodiments, 2-methoxyethanol and / or acetonitrile are used as solvents in the perovskite precursor solution.
[0080] Compared with the general perovskite precursor solution using DMF or DMSO as a solvent, 2-methoxyethanol and / or acetonitrile are used as solvents in this application. This is because 2-methoxyethanol and acetonitrile have a lower boiling point and are more volatile. When the gas pressure drops below 100 Pa, they can evaporate quickly without annealing. The grain size of the first perovskite layer 41 obtained after the solvent evaporates is smaller.
[0081] In some embodiments, the ratio of 2-methoxyethanol to acetonitrile is (6-8):(2-4). 2-methoxyethanol has a high viscosity, which is not conducive to the coating operation of the perovskite precursor solution. Mixing acetonitrile and 2-methoxyethanol in the above ratio can obtain a more suitable viscosity, which facilitates the coating operation.
[0082] In some embodiments, the thickness of the lead iodide skeleton layer 42 is 300 nm to 350 nm. The thickness of the lead iodide skeleton layer 42 is 300 nm, 305 nm, 310 nm, 315 nm, 320 nm, 325 nm, 330 nm, 335 nm, 340 nm, 345 nm, and 350 nm. At this thickness, the overall suede surface of the perovskite thin film layer 4 is better in shape retention, better in compatibility with the suede surface of the crystalline silicon bottom cell 1, higher in photoelectric conversion efficiency, and the lead iodide can react well with the A-site cations to form perovskite crystals, so that lead iodide residue is less likely to appear.
[0083] On the third aspect, the present application also provides a perovskite crystalline silicon tandem cell. Referring to Figure 2, the perovskite crystalline silicon tandem cell includes a crystalline silicon bottom cell 1 with a velvet structure, a carrier recombination layer 2, a hole transport layer 3, the above-mentioned perovskite thin film layer 4, an electron transport layer 5 and a transparent conductive oxide layer 7 stacked in sequence. The perovskite crystalline silicon tandem cell also includes a positive electrode 8 and a negative electrode 9. The negative electrode 9 forms an ohmic contact with the transparent conductive oxide layer 7, and the positive electrode 8 forms an ohmic contact with the back of the crystalline silicon bottom cell 1.
[0084] The residual content of lead iodide at the interface between the above-mentioned perovskite thin film layer 4 and the hole transport layer 3 is relatively small, and the overall crystallization effect of the perovskite thin film layer 4 is better, with fewer defects, and it can contact and cooperate with the hole transport layer 3 and the electron transport layer 5. The hole transport and electron transport 5 effects are better, which is beneficial to improving the energy conversion efficiency of the perovskite crystalline silicon stacked battery.
[0085] In some embodiments, the perovskite crystalline silicon tandem cell further includes a buffer layer 6, which is tin dioxide and has a thickness of 20 nm to 30 nm. Using tin dioxide as the buffer layer 6 can effectively mitigate damage to the perovskite thin film layer 4 and the electron transport layer 5 that may be caused during processing, thereby improving the structural stability of the perovskite crystalline silicon tandem cell.
[0086] In some embodiments, the thickness of the crystalline silicon bottom cell 1 is 5nm to 10nm; and / or, the carrier recombination layer 2 includes nickel oxide, PTAA or Spiro-TBB, and the thickness of the carrier recombination layer 2 is 15nm to 25nm; and / or, the electron transport layer 5 is C60 or PCBM, and the thickness of the electron transport layer 5 is 20nm to 25nm; and / or, the positive electrode 8 and the negative electrode 9 are both silver, the thickness of the positive electrode 8 is 250nm to 350nm, and the thickness of the negative electrode 9 is 150nm to 350nm.
[0087] A method for preparing a perovskite / crystalline silicon tandem cell comprises the following steps:
[0088] Providing a crystalline silicon bottom cell 1;
[0089] Prepare a carrier recombination layer 2 on the N side of the crystalline silicon bottom cell 1;
[0090] A hole transport layer 3 is prepared on the carrier recombination layer 2;
[0091] Preparing any one of the above-mentioned perovskite thin film layers 4 on the hole transport layer 3;
[0092] An electron transport layer 5 is formed on the perovskite thin film layer 4;
[0093] forming a transparent conductive oxide layer 7 on the electron transport layer 5;
[0094] Post-processing is performed to obtain perovskite crystalline silicon tandem cells.
[0095] In some embodiments, the hole transport layer 3 is prepared by magnetron sputtering, the electron transport layer 5 is prepared by evaporation, the transparent conductive oxide layer 7 is prepared by magnetron sputtering, and the positive electrode 8 and the negative electrode are both prepared by thermal evaporation.
[0096] The technical solution of the present invention will be further described below in conjunction with embodiments and drawings.
[0097] Example 1
[0098] The first embodiment of the present application provides a perovskite film layer. Referring to FIG2 , the perovskite film layer includes a first perovskite layer stacked on a hole transport layer and a second perovskite layer stacked on the first perovskite layer. The first perovskite layer is composed of Cs 0.05 (FA 0.77 MA 0.23 ) 0.95 (PbI 0.77 Br 0.23 )3, the optical band gap is 1.62eV, the second perovskite layer is made by the reaction of A-site cations and lead iodide, the A-site cations are composed of iodomethane, bromomethylamine and chloromethylamine in a mass ratio of 35:7:4, and the optical band gap is 1.66eV.
[0099] Specifically, the preparation method of the perovskite thin film layer is as follows:
[0100] Using the hole transport layer as the substrate, 2-methoxyethanol and acetonitrile were mixed in a mass ratio of 7:3 as a mixed solvent to prepare a perovskite precursor solution. The perovskite precursor solution was coated on the surface of the hole transport layer by a slit coating method. The air pressure was reduced to 100 Pa and maintained for 50 seconds to obtain a first perovskite layer with a thickness of 7 nm.
[0101] A 325nm thick lead iodide skeleton layer was prepared by thermal evaporation on the side of the first perovskite layer away from the hole transport layer, and then a layer of A-site cations was prepared by slit coating on the side of the lead iodide skeleton layer away from the hole transport layer. After annealing, a 470nm thick perovskite film layer was obtained.
[0102] Example 2
[0103] Example 2 of the present application provides a perovskite thin film layer. Compared with Example 1, the thickness of the first perovskite layer of the perovskite thin film layer is 5 nm, and the rest is consistent with Example 1.
[0104] Example 3
[0105] Example 3 of the present application provides a perovskite thin film layer. Compared with Example 1, the thickness of the first perovskite layer of the perovskite thin film layer is 10 nm, and the rest is consistent with Example 1.
[0106] Example 4
[0107] Example 4 of the present application provides a perovskite thin film layer. Compared with Example 1, in the preparation process of the first perovskite layer, after the perovskite precursor solution is coated on the surface of the hole transport layer, it is annealed at 170° C. for 45 minutes to obtain a first perovskite layer with a thickness of 7 nm.
[0108] Example 5
[0109] The fifth embodiment of the present application provides a perovskite thin film layer. Compared with the first embodiment, the gas pressure of the perovskite thin film layer is normal pressure.
[0110] Example 6
[0111] Example 6 of the present application provides a perovskite thin film layer. Compared with Example 1, the air pressure of the perovskite thin film layer is reduced to 200 Pa.
[0112] Comparative Example 1
[0113] Comparative Example 1 of the present application provides a perovskite thin film layer, which is composed of only a second perovskite layer, and the rest is consistent with Example 1.
[0114] Comparative Example 2
[0115] Comparative Example 2 of the present application provides a perovskite thin film layer. In the perovskite thin film layer, the thickness of the first perovskite layer is 3 nm, and the rest is consistent with Example 1.
[0116] Comparative Example 3
[0117] Comparative Example 3 of the present application provides a perovskite thin film layer. In the perovskite thin film layer, the thickness of the first perovskite layer is 12 nm, and the rest is consistent with Example 1.
[0118] Application Example 1
[0119] This application example 1 provides a perovskite crystalline silicon tandem cell, comprising:
[0120] Silicon heterojunction bottom cell;
[0121] The carrier recombination layer stacked on the silicon heterojunction bottom cell is made of indium tin oxide with a thickness of 7.5nm;
[0122] A hole transport layer is stacked on the side of the carrier recombination layer away from the silicon heterojunction bottom cell. The hole transport layer is nickel oxide with a thickness of 20nm.
[0123] The perovskite thin film layer of Example 1 is stacked on the side of the hole transport layer facing away from the silicon heterojunction bottom cell;
[0124] The electron transport layer stacked on the side of the perovskite thin film layer of Example 1 facing away from the silicon heterojunction bottom cell is C60 with a thickness of 22.5 nm;
[0125] A buffer layer stacked on the side of the electron transport layer away from the silicon heterojunction bottom cell, the buffer layer is tin dioxide and has a thickness of 25nm;
[0126] A transparent conductive oxide layer stacked on the side of the buffer layer away from the silicon heterojunction bottom cell, the transparent conductive oxide layer is indium zinc oxide and has a thickness of 110nm;
[0127] The electrodes include a silver positive electrode and a silver negative electrode, the silver negative electrode forms an ohmic contact with the transparent conductive oxide layer, and the silver positive electrode forms an ohmic contact with the back side of the crystalline silicon bottom cell.
[0128] A method for preparing a perovskite crystalline silicon tandem battery comprises the following steps:
[0129] Provided is a silicon heterojunction bottom cell;
[0130] Prepare a carrier recombination layer on the N-side of a silicon heterojunction bottom cell;
[0131] A hole transport layer is prepared on the carrier recombination layer by magnetron sputtering;
[0132] Preparing the perovskite thin film layer of Example 1 on the hole transport layer;
[0133] Vapor-depositing an electron transport layer on the perovskite thin film layer of Example 1;
[0134] A buffer layer is formed on the electron transport layer using atomic layer deposition;
[0135] forming a transparent conductive oxide layer on the buffer layer using magnetron sputtering;
[0136] Silver with a thickness of 300 nm was thermally evaporated on the transparent conductive oxide layer as the negative electrode, and silver with a thickness of 200 nm was thermally evaporated on the back carrier recombination layer of the silicon heterojunction bottom cell as the positive electrode.
[0137] Application Example 2
[0138] This application example 2 provides a perovskite crystalline silicon stacked cell. Compared with application example 1, the perovskite thin film layer of embodiment 1 is replaced by the perovskite thin film layer of embodiment 2, and the rest is consistent with application example 1.
[0139] Application Example 3
[0140] This application example three provides a perovskite crystalline silicon stacked cell. Compared with application example one, the perovskite thin film layer of embodiment three is used to replace the perovskite thin film layer of embodiment one, and the rest is consistent with application example one.
[0141] Application Example 4
[0142] This application example 4 provides a perovskite crystalline silicon stacked cell. Compared with application example 1, the perovskite thin film layer of embodiment 4 is used to replace the perovskite thin film layer of embodiment 1, and the rest is consistent with application example 1.
[0143] Application Example 5
[0144] This application example five provides a perovskite crystalline silicon stacked cell. Compared with application example one, the perovskite thin film layer of embodiment five is used to replace the perovskite thin film layer of embodiment one, and the rest is consistent with application example one.
[0145] Application Example 6
[0146] This application example six provides a perovskite crystalline silicon stacked cell. Compared with application example one, the perovskite thin film layer of embodiment six is used to replace the perovskite thin film layer of embodiment one, and the rest is consistent with application example one.
[0147] Application Comparative Example 1
[0148] Comparative Example 1 of this application provides a perovskite crystalline silicon stacked cell. Compared with Application Example 1, the perovskite thin film layer of Comparative Example 1 is used to replace the perovskite thin film layer of Example 1, and the rest is consistent with Application Example 1.
[0149] Application Comparative Example 2
[0150] Comparative Example 2 of this application provides a perovskite crystalline silicon stacked cell. Compared with Application Example 1, the perovskite thin film layer of Comparative Example 2 is used to replace the perovskite thin film layer of Example 1, and the rest is consistent with Application Example 1.
[0151] Application Comparative Example 3
[0152] Comparative Example 3 of this application provides a perovskite crystalline silicon stacked cell. Compared with Application Example 1, the perovskite thin film layer of Comparative Example 3 is used to replace the perovskite thin film layer of Example 1, and the rest is consistent with Application Example 1.
[0153] experiment
[0154] The following tests were performed on the perovskite tandem cells prepared in the above application examples and comparative examples:
[0155] Experiment 1
[0156] The perovskite morphologies of Example 1 and Comparative Example 1 were characterized using a scanning electron microscope. The test results are shown in Figures 3 and 4.
[0157] Application example 1 is to first deposit a first perovskite layer of a specific thickness on the electron transport layer, and then prepare a second perovskite layer by reacting lead iodide with A-site cations. From Figure 3, it can be observed that the interface between the perovskite film layer and the electron transport layer is flat and smooth, and the residual lead iodide is significantly reduced, which proves that the perovskite film layer prepared in this application overcomes the defect that lead iodide is easily left in the perovskite film layer due to the direct reaction of lead iodide and A-site cations, which is beneficial to improving the hole extraction efficiency at the interface between the perovskite film layer and the hole transport layer, promoting the improvement of the performance of the perovskite crystalline silicon stacked battery, and showing significant progress.
[0158] Comparative Example 1 was used without preparing the first perovskite layer. From the SEM image in FIG4 , it can be clearly observed that there is obvious lead iodide residue at the interface between the perovskite thin film layer and the electron transport layer, which affects the hole extraction at the interface between the perovskite thin film layer and the hole transport layer.
[0159] Experiment 2
[0160] The halm test sorting equipment is used to perform performance tests on open circuit voltage, short circuit current density, fill factor, and energy conversion efficiency. The halm machine is a device that simulates sunlight and is equipped with electronic loads, data acquisition and computing equipment to test the electrical properties of photovoltaic devices (including solar cells and perovskite cells), such as Eta, Voc, A, FF, Irev2, Jsc, PCE, etc. These parameters are used to reflect the performance of the above perovskite silicon tandem cells. PCE represents energy conversion efficiency in %, Voc represents open circuit voltage in V, and Jsc represents short circuit current density in mA / cm2 FF stands for fill factor, in %. The experimental test results are detailed in Table 1. With Voc as the horizontal axis and Jsc as the vertical axis, IV curves of Application Example 1 and Application Comparative Example 1 are plotted, as shown in Figure 5.
[0161] Table 1
[0162] It can be seen from the test results in Table 1 and Figure 5 that the Voc, Jsc, FF and PCE of the above application example 1 are better than those of the application comparison example 1, among which FF is increased by 7.05%, PCE is increased by 10.08%, Jsc is increased by 1.05%, and Voc is increased by 1.76%, which proves that the interface contact performance of application example 1 is better, non-radiative recombination is reduced, Voc is improved, and the charge extraction at the interface is better, and FF is improved. It can be seen that the perovskite thin film layer prepared by combining the first perovskite layer and the second perovskite layer can significantly improve the various electrical properties of the perovskite crystalline silicon stacked battery, and the photovoltaic characteristics are better than those of the application comparison example 1, thereby greatly improving the PCE of the solar cell.
[0163] Moreover, the difference between Application Example 1 and Application Comparison Example 2 and Application Comparison Example 3 is that the thickness of the first perovskite layer is changed. Compared with Application Comparison Example 2, the FF of Application Example 1 is increased by 6.24%, the PCE is increased by 9.46%, the Jsc is increased by 1.29%, and the Voc is increased by 1.64%. Compared with Application Comparison Example 3, the FF of Application Example 1 is increased by 6.78%, the PCE is increased by 9.84%, the Jsc is increased by 1.19%, and the Voc is increased by 1.58%, which is a significant improvement. It proves that only a first perovskite layer of a specific thickness can achieve better velvet retention and reduce lead iodide residue, thereby significantly improving the PCE of the perovskite crystalline silicon stacked battery. If the thickness of the first perovskite layer is too high, it is easy to cause uneven thickness of the perovskite film layer due to poor velvet retention, resulting in poor contact effect. If the thickness of the first perovskite layer is too thin, the effect of reducing lead iodide residue is poor. Lead iodide residue can easily cause defects in the perovskite film layer, affecting the various performances of the perovskite crystalline silicon stacked battery.
[0164] Compared with Application Example 1, the FF of Application Example 4 decreased by 4.57%, the PCE decreased by 7.15%, the Jsc increased by 1.18%, and the Voc increased by 1.44%. This proves that during the preparation of the first perovskite layer, direct drying at 100 Pa without annealing treatment resulted in less lead iodide content in the obtained perovskite thin film layer, lower defect density, and higher energy conversion efficiency of the perovskite crystalline silicon stacked battery.
[0165] Compared with Application Example 1, the FF of Application Example 5 decreased by 4.31%, the PCE decreased by 6.28%, the Jsc increased by 0.66%, and the Voc increased by 1.32%. Compared with Application Example 1, the FF of Application Example 6 decreased by 3.27%, the PCE decreased by 5.01%, the Jsc increased by 0.56%, and the Voc increased by 1.15%. This proves that under specific air pressure conditions, the drying treatment has a better crystallization effect of the first perovskite layer, which can better block the contact between the residual lead iodide from the reaction and the hole transport layer, and the first perovskite layer and the residual lead iodide from the reaction can better contact and react with each other, thereby further reducing the residual lead iodide content, reducing the defect density of the perovskite thin film layer, and improving the energy conversion efficiency of the perovskite crystalline silicon stacked battery.
[0166] The technical features of the above embodiments can be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0167] The above embodiments merely illustrate several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the patent. It should be noted that a person skilled in the art would be able to make various modifications and improvements without departing from the spirit of the present invention, all of which fall within the scope of protection of the present invention. Therefore, the scope of protection of the patent for this invention shall be determined by the appended claims.
Claims
1. A perovskite thin film layer, comprising a first perovskite layer and a second perovskite layer stacked on the first perovskite layer, wherein the first perovskite layer has a thickness of 5 nm to 10 nm, and the second perovskite layer is made by reacting an A-site cation solution with lead iodide.
2. The perovskite thin film layer according to claim 1, wherein the composition of the first perovskite layer comprises Cs x FA y MA 1-x-y PbI z Br 3-z , where x=0~1, y=0~1, z=0~3. 3 . The perovskite thin film layer according to claim 2 , wherein x is 0 to 0.1, and y is 0.6 to 0.
8. 4 . The perovskite thin film layer according to claim 1 , wherein the optical band gap of the first perovskite layer is lower than the optical band gap of the second perovskite layer, and the optical band gap of the first perovskite layer is 1.60 eV to 1.65 eV. 5 . The perovskite thin film layer according to claim 1 , wherein the A-site cation is one or a combination of iodoformamidine, bromomethylamine and chloromethylamine.
6. The perovskite thin film layer according to any one of claims 1 to 5, wherein the A-site cations include iodoformamidine, bromomethylamine and chloromethylamine, and the mass ratio of iodoformamidine, bromomethylamine and chloromethylamine is (30-40): (5-10): (2-6). 7 . The perovskite thin film layer according to claim 1 , wherein the thickness of the second perovskite layer is 480 nm to 530 nm.
8. A method for preparing a perovskite thin film layer, comprising the following steps: Preparing a first perovskite layer: forming a first perovskite layer with a thickness of 5 nm to 10 nm on the hole transport layer of the perovskite crystalline silicon stacked cell by evaporation or solution film formation; Prepare a second perovskite layer: prepare a lead iodide skeleton layer on the side of the first perovskite layer away from the hole transport layer, apply an A-site cation solution on the side of the lead iodide skeleton layer away from the hole transport layer, and anneal to form a second perovskite layer.
9. The preparation method according to claim 8, wherein the first perovskite layer comprises Cs x FA y MA 1-x-y PbI z Br 3-z , where x=0~1, y=0~1, z=0~3. 10 . The preparation method according to claim 9 , wherein x is 0 to 0.1, and y is 0.6 to 0.
8. 11 . The preparation method according to claim 8 , wherein the optical band gap of the first perovskite layer is lower than the optical band gap of the second perovskite layer, and the optical band gap of the first perovskite layer is 1.60 eV to 1.65 eV.
12. The preparation method according to any one of claims 8 to 11, wherein the A-position cation is one or a combination of iodoformamidine, bromomethylamine and chloromethylamine.
13. The preparation method according to any one of claims 8 to 12, wherein the A-site cation comprises iodoformamidine, bromomethylamine and chloromethylamine, and the mass ratio of iodoformamidine, bromomethylamine and chloromethylamine is (30-40): (5-10): (2-6). 14 . The preparation method according to claim 8 , wherein the thickness of the second perovskite layer is 480 nm to 530 nm.
15. The preparation method according to any one of claims 8 to 14, wherein in the step of preparing the first perovskite layer, the solution film forming method is: coating a perovskite precursor solution on the hole transport layer, and drying to obtain the first perovskite layer. 16 . The preparation method according to claim 15 , in the step of preparing the first perovskite layer, the drying is performed at an air pressure below 100 Pa and maintained for 40 seconds to 60 seconds. 17 . The preparation method according to claim 15 , wherein the perovskite precursor solution uses at least one of 2-methoxyethanol and acetonitrile as a solvent.
18. The preparation method according to claim 17, wherein the 2-methoxyethanol and the acetonitrile are used as solvents, and the mass ratio of the 2-methoxyethanol to the acetonitrile is (6-8):(2-4).
19. The preparation method according to any one of claims 8 to 18, wherein the solution is formed into a film in a manner comprising slit coating, spraying, inkjet printing or doctor blade coating.
20. The preparation method according to any one of claims 8 to 18, wherein the thickness of the lead iodide skeleton layer is 300 nm to 350 nm.
21. A perovskite crystalline silicon stacked cell, comprising a crystalline silicon bottom cell with a velvet structure, a carrier recombination layer, a hole transport layer, a perovskite thin film layer, and an electron transport layer stacked in sequence; The perovskite thin film layer is the perovskite thin film layer according to any one of claims 1 to 7 or the perovskite thin film layer prepared by the preparation method of the perovskite thin film layer according to any one of claims 8 to 20; The perovskite crystalline silicon stacked cell further includes a positive electrode and a negative electrode, wherein the negative electrode forms an ohmic contact with the transparent conductive oxide layer, and the positive electrode forms an ohmic contact with the back side of the crystalline silicon bottom cell.
22. The perovskite crystalline silicon tandem cell according to claim 21, further comprising a buffer layer, wherein the buffer layer is tin dioxide, and the thickness of the buffer layer is 20 nm to 30 nm.
23. The perovskite crystalline silicon stacked cell according to any one of claims 21 to 22, wherein the thickness of the crystalline silicon bottom cell is 5 nm to 10 nm. 24 . The perovskite crystalline silicon stacked cell according to claim 21 , wherein the carrier recombination layer comprises nickel oxide, PTAA or Spiro-TBB, and the thickness of the carrier recombination layer is 15 nm to 25 nm. 25 . The perovskite crystalline silicon stacked cell according to claim 21 , wherein the electron transport layer is C60 or PCBM, and the thickness of the electron transport layer is 20 nm to 25 nm.
26. The perovskite crystalline silicon stacked cell according to any one of claims 21 to 25, wherein the positive electrode and the negative electrode are both silver, the thickness of the positive electrode is 250nm to 350nm, and the thickness of the negative electrode is 150nm to 350nm.
27. A method for preparing a perovskite crystalline silicon tandem battery, comprising the following steps: Provide crystalline silicon bottom cells; Preparing a carrier recombination layer on the N-side of the crystalline silicon bottom cell; preparing a hole transport layer on the carrier recombination layer; The perovskite thin film layer prepared by the method for preparing the perovskite thin film layer according to any one of claims 1 to 7 or any one of claims 8 to 20 is prepared on the hole transport layer; preparing an electron transport layer on the perovskite thin film layer; preparing a transparent conductive oxide layer on the electron transport layer; Post-processing is performed to obtain perovskite crystalline silicon tandem cells.
28. The preparation method according to claim 27, wherein the hole transport layer is prepared by magnetron sputtering.
29. The preparation method according to any one of claims 27 to 28, wherein the electron transport layer is prepared by evaporation. 30 . The preparation method according to claim 27 , wherein the transparent conductive oxide layer is prepared by magnetron sputtering.
31. The preparation method according to any one of claims 27 to 30, wherein the positive electrode and the negative electrode are both prepared by thermal evaporation.
Citation Information
Patent Citations
Perovskite-silicon-based laminated solar cell and manufacturing method thereof
CN116133448A
Perovskite thin film layer and preparation method thereof, perovskite crystalline silicon laminated cell and preparation method thereof
CN116709886A
Cited By
Perovskite thin film gas passivation method and tandem solar cell
WO2026144175A1
Method for forming textured surface of cell, and tandem cell and preparation method therefor
WO2026153262A1