Separator, electrochemical apparatus, and electronic device
By setting a dense and high pore coating on the lithium-ion battery separator, the problem of deterioration in the battery cycle performance caused by cathode dissolution is solved, the high-temperature and low-temperature performance of the battery cell is improved, and the overall stability and heat resistance of the battery are improved. .
Patent Information
- Application Number
- PCT/CN2024/091477
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-23
- Filing Date
- 2024-05-07
- Publication Date
- 2024-11-28
AI Technical Summary
After the dynamic performance of the existing lithium-ion battery separators improve the cell, the stability of the cathode material decreases, resulting in an increase in cathode dissolution, which in turn affects the battery circulation performance, especially the performance deteriorates under high and low temperature conditions.
Two coatings with different porosity are provided on both sides of the membrane, a dense first coating and a high porosity second coating. By regulating their porosity and pore size, they cooperate to block the cathode dissolution and improve the electrolyte by regulating their porosity and pore size, and jointly working together to block the cathode dissolution and improve the electrolyte. The transmission channel reduces the lithium ion impedance.
It significantly improves the cycling performance of the battery cell, especially the high-temperature cycling performance and low-temperature discharge performance, extends the service life of the battery, and improves the heat resistance of the diaphragm.
Smart Images

Figure CN2024091477_28112024_PF_FP_ABST
Abstract
Description
Separators, electrochemical devices, and electronic devices Technical Field
[0001] The present application relates to the field of battery technology, and in particular to a diaphragm, an electrochemical device, and an electronic device. Background Art
[0002] The diaphragm is a key component of the battery. At present, the diaphragms used in conventional lithium-ion batteries are mostly polypropylene (PP) porous membranes, polyethylene (PE) porous membranes or polypropylene (PP) / polyethylene (PE) / polypropylene (PP) composite porous membranes. However, with the improvement of the kinetic performance of the battery cell, the demand for anode EL (electrolyte) increases. Moreover, with the increase of the voltage of the cathode material, the stability of the cathode material decreases, which increases the cathode dissolution and leads to poor battery cycle performance.
[0003] Summary of the Invention
[0004] In view of this, the present application provides a diaphragm, an electrochemical device and an electronic device, wherein two coatings with different porosities are respectively provided on both sides of the diaphragm, and the porosities of the two coatings are regulated within an appropriate range and cooperate with each other to improve the cycle performance of the battery.
[0005] In a first aspect, the present application provides a separator comprising a separator substrate, a first coating layer, and a second coating layer. The separator substrate comprises a first surface and a second surface disposed opposite each other, the first surface facing the cathode and the second surface facing the anode. The first coating layer is disposed on the first surface, and the second coating layer is disposed on the second surface. The first coating layer is a solid filler coating layer, the porosity of the first coating layer being denoted as D1 and satisfying the following: 10% ≤ D1 < 30%. The second coating layer is a solid filler coating layer, the porosity of the second coating layer being denoted as D2 and satisfying the following: 30% ≤ D2 ≤ 60%. A solid filler coating layer refers to a coating layer containing added solid particles. The present application provides a dense first coating layer and a highly porous second coating layer on both outer surfaces of the separator substrate. The dense first coating layer helps prevent cathode dissolution from entering the internal pores of the separator substrate and even entering the anode. In the present application, cathode dissolution primarily refers to cathode electrode dissolution, namely, metal elements such as Co, Mn, Ni, and Al that may be dissolved from the active material, as well as low-molecular-weight polyacrylic acid (PAA) and uncross-linked acrylate molecules that may be dissolved from auxiliary materials such as binders. Controlling the porosity of the first coating within an appropriate range can, on the one hand, improve the transport of cathode extracts between the anode and cathode, thereby inhibiting the cathode extracts from participating in the electrochemical reaction. On the other hand, the lower porosity of the first coating within an appropriate range, in conjunction with the higher porosity of the second coating, helps improve the cycling performance of the battery cell, especially significantly improving the high-temperature cycling performance of the battery cell. In some embodiments, the following conditions are met: 15% ≤ D1 ≤ 25%. In some embodiments, the following conditions are met: 40% ≤ D2 ≤ 50%.
[0006] In some embodiments, the average volume pore size D of the first coating 50 The pore size D of the first coating is 1nm to 90nm. 50 Setting it in a suitable range is more conducive to improving the cycle performance of the battery cell. In some embodiments, the pore size D of the first coating is 50 5nm to 60nm.
[0007] In some embodiments, the thickness of the first coating layer is 20 nm to 500 nm. By controlling the thickness of the first coating layer within the above range, on the one hand, it is beneficial to coordinate the pore size D of the first coating layer. 50 The porosity D1 creates pores with a screening function on the cathode side of the separator, better preventing cathode extractables from entering the pores / anode inside the separator, thereby further improving the high-temperature cycling performance of the battery cell. On the other hand, it can also prevent cathode particles from piercing the separator. In some embodiments, the thickness of the first coating is 200nm to 500nm.
[0008] In some embodiments, the pore size D' of the second coating layer 50 The pore size D' of the second coating is 100nm to 500nm.50 In some embodiments, the pore size D' of the second coating is 50 150nm to 300nm.
[0009] In some embodiments, 20≤D′ is satisfied. 50 / D 50 ≤60. This is more conducive to improving the heat resistance of the diaphragm.
[0010] In some embodiments, the thickness of the second coating layer is 0.5 μm to 2 μm. By controlling the thickness of the second coating layer within the above range, the pore size D′ of the second coating layer can be coordinated. 50 The porosity D2 creates an EL-friendly channel on the anode side of the separator, which helps improve the EL transmission channel in the coating, further increasing the efficiency of electrolyte transport at the anode, improving the kinetic performance of the battery cell, and further improving the purple spot interfacial lithium precipitation caused by electrolyte loss at the anode. In some embodiments, the thickness of the second coating is 0.5 μm to 1 μm.
[0011] In some embodiments, the sum of the lithium ion impedances of the first and second coatings is between 0.001Ω and 0.015Ω. At low temperatures, the overall kinetic performance of the EL system is low (lithium ion transfer efficiency decreases). By reducing the diaphragm impedance to an appropriate range, the lithium ion transfer impedance is reduced, the transfer efficiency is improved, and thus the low-temperature discharge performance of the battery cell is improved. In some embodiments, the sum of the lithium ion impedances of the first and second coatings is between 0.001Ω and 0.01Ω.
[0012] In some embodiments, the following condition is satisfied: 2.3 ≤ D2 / D1 ≤ 3.2. The porosity ratio of the first coating layer to the second coating layer is further regulated within the above range and coordinated with an appropriate pore size ratio, so that the ceramic coating layer has high mechanical properties at high temperatures, thereby suppressing thermal shrinkage of the separator substrate and improving the heat resistance of the separator.
[0013] In a second aspect, the present application provides an electrochemical device, comprising a cathode electrode piece, an anode electrode piece, and a separator disposed between the cathode electrode piece and the anode electrode piece, wherein the separator comprises any one of the separators described above.
[0014] In a third aspect, the present application provides an electronic device comprising the above-mentioned electrochemical device. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without paying any creative work.
[0016] FIG1 is a schematic diagram of the structure of the diaphragm prepared in an embodiment of the present application.
[0017] In the figure: 1, diaphragm substrate; 2, first coating; 3, second coating. DETAILED DESCRIPTION
[0018] In order to make the purpose, technical solutions and advantages of this application more clearly understood, the present application is further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain this application and are not intended to limit this application.
[0019] electrochemical devices
[0020] The present application provides an electrochemical device, which includes a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the separator is arranged between the positive electrode sheet and the negative electrode sheet.
[0021] diaphragm
[0022] The diaphragm includes a diaphragm substrate, a first coating and a second coating. The diaphragm substrate includes two opposite surfaces in its thickness direction, namely a first surface and a second surface, the first surface facing the cathode and the second surface facing the anode. The first coating is provided on the first surface, and the second coating is provided on the second surface. The first coating is a dense solid filler coating. The porosity of the first coating is denoted as D1 and satisfies: 10% ≤ D1 < 30%. Exemplarily, the porosity D1 of the first coating is 10%, 13%, 15%, 17%, 20%, 25%, 27%, 29% or a range consisting of any two of the above values. Furthermore, in some embodiments, the following is satisfied: 15% ≤ D1 ≤ 25%.
[0023] The second coating layer is a highly porous solid filler coating layer. The porosity of the second coating layer is denoted as D2 and satisfies the following conditions: 30% ≤ D2 ≤ 60%. For example, the porosity D2 of the second coating layer is 30%, 35%, 40%, 45%, 50%, 55%, 60%, or a range consisting of any two of the foregoing values. Furthermore, in some embodiments, the following conditions are satisfied: 40% ≤ D2 ≤ 50%.
[0024] In some embodiments, the pore size D of the first coating layer is 501 nm to 90 nm. For example, the pore size D of the first coating layer is 50 is 1 nm, 5 nm, 10 nm, 15 nm, 20 nm, 25 nm, 30 nm, 35 nm, 40 nm, 45 nm, 50 nm, 55 nm, 60 nm, 65 nm, 70 nm, 75 nm, 80 nm, 85 nm, 90 nm, or a range consisting of any two of the above values. Further, in some embodiments, the pore size D of the first coating layer is 50 5nm to 60nm.
[0025] In some embodiments, the thickness of the first coating layer is 20 nm to 500 nm. For example, the thickness of the first coating layer is 20 nm, 40 nm, 50 nm, 60 nm, 80 nm, 100 nm, 150 nm, 200 nm, 220 nm, 240 nm, 260 nm, 280 nm, 300 nm, 340 nm, 350 nm, 380 nm, 400 nm, 450 nm, 500 nm, or a range consisting of any two of the above values. Further, in some embodiments, the thickness of the first coating layer is 200 nm to 500 nm.
[0026] In some embodiments, the pore size D' of the second coating layer 50 For example, the pore size D' of the second coating layer is 100 nm to 500 nm. 50 is 100 nm, 120 nm, 140 nm, 150 nm, 160 nm, 180 nm, 200 nm, 220 nm, 240 nm, 260 nm, 280 nm, 300 nm, 350 nm, 400 nm, 450 nm, 500 nm, or a range consisting of any two of the above values. Further, in some embodiments, the pore size D′ of the second coating layer is 50 150nm to 300nm.
[0027] In some embodiments, the second coating layer has a thickness of 0.5 μm to 2 μm. For example, the second coating layer has a thickness of 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, 1 μm, 1.5 μm, 2 μm, or a range consisting of any two of the foregoing values. Furthermore, in some embodiments, the second coating layer has a thickness of 0.5 μm to 1 μm.
[0028] In some embodiments, the sum of the lithium ion impedances of the first coating layer and the second coating layer is 0.001Ω to 0.015Ω. For example, the sum of the lithium ion impedances of the first coating layer and the second coating layer is 0.001Ω, 0.003Ω, 0.005Ω, 0.008Ω, 0.01Ω, 0.013Ω, 0.015Ω, or a range consisting of any two of the foregoing values. Furthermore, in some embodiments, the sum of the lithium ion impedances of the first coating layer and the second coating layer is 0.001Ω to 0.01Ω.
[0029] In some embodiments, 20≤D′ is satisfied. 50 / D 50 ≤60. For example, D′ 50 / D 50 20, 25, 30, 35, 40, 45, 50, 55, 60 or a range consisting of any two of the above values.
[0030] In some embodiments, the porosity of the first coating layer is denoted as D1, and the porosity of the second coating layer is denoted as D2, satisfying the following relationship: 2.3≤D2 / D1≤3.2. For example, D2 / D1 is 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, 3.2, or a range consisting of any two of the foregoing values.
[0031] In some embodiments, the first coating and the second coating include a solid filler, a binder, and a wetting agent. In the first coating, the mass ratio of the solid filler, the binder, and the wetting agent is (96.5-99.3)%: (0.5-3)%: (0.2-0.5)%; in the second coating, the mass ratio of the solid filler, the binder, and the wetting agent is (94.5-99.3)%: (0.5-5)%: (0.2-0.5)%.
[0032] In some embodiments, in the first coating layer, the average volume particle size d of the solid filler is 50 The range of is 10nm to 200nm. 50 is 10 nm, 15 nm, 20 nm, 40 nm, 60 nm, 80 nm, 100 nm, 150 nm, 180 nm, 200 nm, or a range consisting of any two of the above values. Further, in some embodiments, in the first coating, the particle size d of the solid filler is 50 The range is 20nm to 100nm.
[0033] In some embodiments, in the second coating layer, the solid filler particle size d' 50 The range of d' is 200 nm to 1000 nm.50 is 200 nm, 250 nm, 300 nm, 400 nm, 450 nm, 500 nm, 600 nm, 700 nm, 800 nm, 900 nm, 1000 nm, or a range consisting of any two of the above values. Further, in some embodiments, in the second coating layer, the particle size d' of the solid filler is 50 The range is 250nm to 500nm.
[0034] In some embodiments, the solid filler is selected from at least one of boehmite, alumina, zirconium oxide, titanium dioxide, magnesium oxide, mullite, silicon carbide, silicon nitride, boron nitride, aluminum nitride, poly(p-phenylene terephthalamide) (PPTA), and polyimide. The binder is selected from at least one of polyvinyl alcohol (PVA), hydroxymethyl cellulose, styrene-butadiene rubber (SBR), and polyacrylate. The wetting agent is selected from at least one of polyoxyethylene alkylphenol ethers, polyoxyethylene fatty alcohol ethers, polyoxyethylene-polyoxypropylene block copolymers, and polyether-modified trimethylsiloxane.
[0035] In some embodiments, the thickness of the separator substrate is 2 μm to 7 μm. For example, the thickness of the separator substrate is 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, or a range consisting of any two of the above values.
[0036] In some embodiments, the separator substrate may be a non-woven fabric, a film, or a composite film having a porous structure, and the material of the separator substrate may include at least one of polyethylene, polypropylene, polyethylene terephthalate, or polyimide.
[0037] Exemplary preparation method of the separator:
[0038] (1) Preparation of the first coating
[0039] Exemplarily: step a. mixing deionized water, a solid filler, an adhesive and a wetting agent, wherein the solid filler, the adhesive and the wetting agent are mixed in a mass ratio of (96.5-99.3)%: (0.5-3)%: (0.2-0.5)% (excluding the dispersion medium deionized water), and fully dispersed in a stirrer to obtain a slurry A to be coated; step b. uniformly coating the slurry A to be coated in step a on the first surface of the diaphragm substrate, and completing the preparation of the first coating after drying.
[0040] (2) Preparation of the second coating
[0041] Exemplarily: Step c. Mix deionized water, solid filler, adhesive and wetting agent, wherein the solid filler, adhesive and wetting agent are mixed in a mass ratio of (94.5-99.3)%: (0.5-5)%: (0.2-0.5)% (excluding the dispersion medium deionized water), and fully disperse them in a stirrer to obtain a slurry B to be coated; Step d. Evenly apply the slurry B to be coated in step c on the second surface of the diaphragm substrate, and complete the preparation of the second coating after drying to obtain the diaphragm.
[0042] other
[0043] The positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer disposed on at least one surface of the positive electrode current collector. The positive electrode active material in the positive electrode active material layer can be selected from one or more of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium iron phosphate, and compounds obtained by adding other transition metals or non-transition metals to the above compounds. For example, the positive electrode current collector can be made of a metal foil or porous metal plate, such as a foil or porous plate made of a metal such as aluminum, copper, nickel, titanium, or iron, or an alloy thereof, such as Al (aluminum) foil.
[0044] The positive electrode sheet can be prepared according to conventional methods in the art.
[0045] The negative electrode sheet includes a negative electrode current collector and a negative electrode active layer disposed on the surface of the negative electrode current collector. The negative electrode active layer includes a negative electrode active material. The present application does not particularly limit the thickness of the negative electrode active layer, as long as it can achieve the objectives of the present application. For example, the thickness of the negative electrode active layer is 30μm to 120μm. In some embodiments, the negative electrode active material may include at least one of a carbon material or a silicon-based material. In some embodiments, the carbon material includes, but is not limited to, at least one of natural graphite, artificial graphite, mesophase microcarbon beads, hard carbon, or soft carbon. In some embodiments, the silicon-based material includes, but is not limited to, at least one of silicon, a silicon-oxygen composite material, or a silicon-carbon composite material. The present application does not particularly limit the thickness of the negative electrode current collector, as long as it can achieve the objectives of the present application. For example, it may include copper foil, copper alloy foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, or a composite current collector (e.g., a composite current collector with a metal layer disposed on the surface of a polymer layer). The present application does not particularly limit the thickness of the negative electrode current collector, as long as it can achieve the objectives of the present application. For example, the thickness of the negative electrode current collector is 5μm to 12μm. The negative electrode active layer may also include a binder and a thickener. This application does not specifically limit the types of binder and thickener, as long as they can achieve the objectives of this application. For example, the binder may include, but is not limited to, at least one of polyvinyl alcohol, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, styrene-butadiene rubber, or acrylated styrene-butadiene rubber; the thickener may include, but is not limited to, at least one of sodium carboxymethyl cellulose or lithium carboxymethyl cellulose. The negative electrode active layer may also include a conductive agent. This application does not specifically limit the type of conductive agent, as long as it can achieve the objectives of this application. For example, the conductive agent may include, but is not limited to, at least one of conductive carbon black, carbon nanotubes (CNTs), carbon fibers, Ketjen black, graphene, a metallic material, or a conductive polymer. This application does not specifically limit the mass ratio of the negative electrode active material, conductive agent, binder, and thickener in the negative electrode active layer. Those skilled in the art may select the ratio based on actual needs, as long as it can achieve the objectives of this application. Optionally, the negative electrode plate may also include a conductive layer, which is located between the negative electrode current collector and the negative electrode active layer. The present application does not particularly limit the composition of the conductive layer, and it may be any conductive layer commonly used in the art. For example, the conductive layer may include a conductive agent and a binder. The present application does not particularly limit the conductive agent and binder in the conductive layer, and for example, it may be at least one of the conductive agent and binder used in the negative electrode active layer described above.
[0046] The electrolyte includes an organic solvent and a lithium salt; the organic solvent includes a carbonate solvent, a carboxylate solvent, or a combination thereof; wherein the carbonate solvent includes at least one of diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methylpropyl carbonate (MPC), ethylpropyl carbonate (EPC), ethylmethyl carbonate (MEC), ethylene carbonate (EC), propylene carbonate (PC), or butylene carbonate (BC); and the carboxylate solvent includes at least one of ethyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, butyl butyrate, ethyl difluoroacetate, difluoroethyl acetate, ethyl trifluoroacetate, trifluoroethyl acetate, or methyl trifluoropropionate. The lithium salt includes at least one of lithium hexafluorophosphate (LiPF6), lithium bis(oxalatoborate) (LiB(C2O4)2, LiBOB), lithium difluorooxalatoborate (LiBF2(C2O4), LiDFOB), lithium tetrafluoroborate (LiBF4), lithium bis(fluorosulfonyl)imide (LiFSI) or lithium bis(trifluoromethanesulfonyl)imide (LiTFSI).
[0047] The electrolyte may further include an electrolyte additive, which may include but is not limited to at least one of fluoroethylene carbonate (FEC), vinyl ethylene carbonate (VC) or 1,3-propane sultone (PS).
[0048] The electrochemical device of the present application may include any device that generates an electrochemical reaction, and specific embodiments thereof include all types of primary batteries or secondary batteries. In particular, the electrochemical device is a lithium secondary battery, including a lithium metal secondary battery, a lithium ion secondary battery, a lithium polymer secondary battery, or a lithium ion polymer secondary battery.
[0049] electronic devices
[0050] The electronic devices described in this application include any of the above-mentioned electrochemical devices. The electronic devices described in this application include, but are not limited to, mobile phones, laptops, tablet computers, game consoles, drones, electric cars, electric bicycles, power tools, and Bluetooth headsets.
[0051] Hereinafter, embodiments of the present application will be described in more detail with reference to examples and comparative examples.
[0052] Example 1
[0053] (1) Preparation of lithium-ion batteries
[0054] Preparation of diaphragm
[0055] Step a. Deionized water, boehmite (ceramic filler), PVA (binder) and polyoxyethylene alkylphenol ether (wetting agent) are mixed in a mass ratio of 99%: 0.5%: 0.5% (excluding the dispersion medium, deionized water), and the mixture is fully dispersed in a stirrer to obtain a slurry to be coated A;
[0056] Step b. The slurry A to be coated in step a is evenly coated on the first surface of the diaphragm substrate (material: polyethylene, thickness 7 μm), and the first coating layer is prepared after drying.
[0057] Step c. Deionized water, magnesium oxide (ceramic filler), SBR (binder) and polyoxyethylene fatty alcohol ether (wetting agent) are mixed in a mass ratio of 98%: 1.5%: 0.5% (excluding the dispersion medium deionized water) and fully dispersed in a stirrer to obtain a slurry to be coated B;
[0058] Step d. The slurry B to be coated in step c is evenly coated on the second surface of the diaphragm substrate, and the second coating layer is prepared after drying to obtain the diaphragm. Specific parameters are shown in Table 1.
[0059] In Examples 2 to 7, the difference from Example 1 is that the pore size D of the first coating layer is adjusted. 50 and porosity D1; in Examples 8 to 10, the difference from Example 1 is that the porosity D2 of the second coating layer is adjusted; in Examples 11 to 17, the difference from Example 1 is that the thickness of the first coating layer is adjusted; in Example 18, the difference from Example 3 is that the ceramic particles on both sides are replaced with PPTA particles. In Example 19, the difference from Example 3 is that the ceramic particles on both sides are replaced with polyimide particles. In Examples 20 to 25 and Examples 30 to 31, the difference from Example 8 is that the pore size D′ of the second coating layer is adjusted. 50 and porosity D2; in Examples 26 to 29 and Example 32, the difference from Example 25 is that the thickness of the second coating is adjusted; in Examples 34 to 37, the difference from Example 31 is that D' is adjusted 50 / D 50 and the ratio of D2 / D1.
[0060] In Comparative Examples 1 and 2, the difference from Example 1 is that the pore size D of the first coating layer is adjusted. 50 and porosity D1; in Comparative Examples 3 to 4, the difference from Example 8 is that the porosity D2 of the second coating layer is adjusted.
[0061] Preparation of positive electrode
[0062] The positive electrode active material - lithium cobalt oxide active material LiCoO2, conductive carbon black Super-P, and binder PVDF are mixed in an N-methylpyrrolidone NMP solvent system in a weight ratio of 97.6:1.3:1.1 by a vacuum mixer and fully stirred to obtain a positive electrode slurry; the positive electrode slurry is coated on both surfaces of a 9μm Al foil substrate with a coating weight of 280 mg, and then dried, cold pressed, slit, and cut to obtain a positive electrode sheet. The thickness of the positive electrode sheet after cold pressing is 95μm.
[0063] Preparation of negative electrode sheet
[0064] The negative electrode active material artificial graphite, the conductive agent acetylene black, the binder styrene-butadiene rubber (SBR), and the thickener sodium methyl cellulose (CMC) are mixed evenly in a deionized water solvent in a mass ratio of 95:2:2:1, coated on one side of the Cu foil and dried, and the above steps are repeated on the other side of the Cu foil to obtain a negative electrode sheet coated with a negative electrode active layer on both sides. After cold pressing and cutting, the negative electrode sheet is obtained.
[0065] Preparation of electrolyte
[0066] Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) are mixed in a mass ratio of 1:1:1 to obtain an organic solvent. LiPF6 is dissolved in the organic solvent, and vinylene carbonate is added and mixed to obtain an electrolyte. The mass percentage of LiPF6 is 12.5% and the mass percentage of vinylene carbonate is 3% based on the total mass of the electrolyte.
[0067] Preparation of lithium-ion batteries
[0068] The positive electrode sheet, separator and negative electrode sheet are stacked in sequence, and the separator separates the positive electrode sheet and the negative electrode sheet. The bare battery cell is formed by winding, and the bare battery cell is placed in the aluminum-plastic film shell to be sealed. After high-temperature baking, electrolyte injection, vacuum packaging, standing, formation, shaping and capacity testing, a lithium-ion battery is obtained.
[0069] (2) Testing of lithium-ion batteries
[0070] (1) Lithium ion impedance test
[0071] Electrochemical impedance spectroscopy (EIS) is used to test the ionic impedance of the ceramic coating. The specific test method is to first test the substrate impedance and then test the ceramic coating (coated on both sides) diaphragm impedance. The difference between the two is the ceramic coating impedance.
[0072] (2) Normal temperature cycle performance test
[0073] At 25°C, charge the lithium-ion battery at a constant current of 0.7C to 4.5V, then charge it at a constant voltage to a current of 0.5C. At this point, the lithium-ion battery is fully charged. Record the charge capacity at this point, which is the first-cycle charge capacity. After the lithium-ion battery is allowed to rest for 5 minutes, discharge it at a constant current of 0.5C to 3V and let it rest for 5 minutes. This is a cyclic charge and discharge process. Record the discharge capacity at this point, which is the first-cycle discharge capacity. Cycle 1000 times under this condition and calculate the capacity retention rate at the 1000th cycle. Among them, the capacity retention rate of 1000 cls at 25°C = (discharge capacity of the cycle / first-cycle discharge capacity) * 100%.
[0074] (3) High temperature cycle performance test
[0075] At 45°C, charge the lithium-ion battery at a constant current of 0.7C to 4.5V, then charge it at a constant voltage to a current of 0.5C. At this point, the lithium-ion battery is fully charged. Record the charge capacity at this point, which is the first-cycle charge capacity. After the lithium-ion battery is allowed to rest for 5 minutes, discharge it at a constant current of 0.5C to 3V and let it rest for 5 minutes. This is a cyclic charge and discharge process. Record the discharge capacity at this point, which is the first-cycle discharge capacity. Cycle 1000 times under this condition and calculate the capacity retention rate at the 1000th cycle. Among them, the capacity retention rate at 45°C 1000cls = (discharge capacity of the cycle / first-cycle discharge capacity) * 100%.
[0076] (4) Low temperature discharge performance test
[0077] The lithium-ion battery was charged to full capacity at a constant current of 1C, then placed in a low-temperature test chamber, cooled to -20°C, and discharged to 3V. The discharge capacity, Q, of the lithium-ion battery was recorded. The discharge capacity of each embodiment and the comparative example was recorded separately. The discharge capacity of each embodiment was denoted as Q2, and the discharge capacity of comparative example 1 was denoted as Q1. The low-temperature discharge performance improvement rate = [(Q2 - Q1) / Q1] × 100%.
[0078] (5) Diaphragm thermal shrinkage test
[0079] Use a specific mold to punch out the diaphragm to be tested into a length and width of 72.5cm and 54.2cm respectively. Place the punched diaphragm flatly between two A4 papers and bake it in a 150℃ oven for 1h. Take out the baked diaphragm and measure the length and width to be X1 and X2 respectively. The thermal shrinkage calculation formula is as follows: MD thermal shrinkage = (72.5-X1) / 72.5*100%; TD thermal shrinkage = (54.2-X2) / 54.2*100%.
[0080] Table 1
[0081] It can be seen from the parameter characteristics and test data in Table 1 that the present application sets a dense first coating and a high-porosity second coating on the outer surfaces of both sides of the diaphragm substrate respectively. Through the coordinated cooperation of the first coating and the second coating, the cycle performance of the battery cell can be improved, especially the high-temperature cycle performance.
[0082] Specifically, from the comparison of Examples 1 to 7 and Examples 18 to 19, it can be seen that by regulating the porosity D1 of the first coating to vary within an appropriate range, it is beneficial to cooperate with the second coating to improve the cycle performance of the battery cell. For example, the room temperature capacity retention rate of the lithium ion battery prepared in Example 3 is 85.9%, and the high temperature capacity retention rate is as high as 95.5%. At the same time, combined with Examples 8 to 10, it can be seen that further regulating the porosity D2 of the second coating can further improve the cycle performance of the battery cell. For example, the room temperature capacity retention rate of the lithium ion battery prepared in Example 9 can reach 90.5% and its high temperature capacity retention rate is as high as 97.5%.
[0083] A comparison of Examples 11 to 17 with Example 3 shows that further regulating the thickness of the first coating can better improve the cycle performance of the battery cell. For example, the room temperature capacity retention rate of the lithium-ion battery prepared in Example 12 can reach 89.8%, and its high temperature capacity retention rate can reach 97.8%.
[0084] From the comparison of Comparative Examples 1 to 4 and Example 3, it can be seen that the porosity of the first coating in Comparative Examples 1 and 2 is not in the appropriate range, and the porosity of the second coating in Comparative Examples 3 and 4 is not in the appropriate range. At this time, the room temperature and high temperature cycle performance of the battery cell are poor.
[0085] Table 2
[0086] From the parameter characteristics and test data in Table 2, it can be seen that by controlling the pore size D′ of the second coating 50 The sum of the porosity D2, porosity D2, and lithium-ion impedance within an appropriate range is beneficial for improving the low-temperature discharge performance of the battery cell. For example, the lithium-ion battery prepared in Example 25 achieved a low-temperature discharge improvement rate of up to 9.0%. A comparison of Examples 25-29 and Example 32 with Example 25 shows that further increasing the thickness of the second coating leads to deterioration in low-temperature discharge performance.
[0087] Table 3
[0088] It can be seen from the parameter characteristics and test data in Table 3 that the heat resistance of the diaphragm can be improved by synergistically controlling the porosity ratio and pore size ratio of the first coating and the second coating within an appropriate range.
[0089] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent replacements and improvements made within the spirit and principles of the present application should be included in the scope of protection of the present application.
Claims
1. A diaphragm, characterized in that: The isolation film includes a membrane substrate, a first coating layer and a second coating layer; The separator substrate comprises a first surface and a second surface arranged opposite to each other, wherein the first surface is used to face the cathode, and the second surface is used to face the anode; The first coating is disposed on the first surface, and the second coating is disposed on the second surface; The first coating is a solid filler coating, and the porosity of the first coating is denoted as D1, which satisfies: 10%≤D1<30%; The second coating layer is a solid filler coating layer, and the porosity of the second coating layer is denoted as D2, which satisfies: 30%≤D2≤60%.
2. The diaphragm according to claim 1, characterized in that The isolation film satisfies at least one of the following conditions: Condition I: The pore size D of the first coating 50 1nm to 90nm; Condition II: the thickness of the first coating layer is 20 nm to 500 nm; Condition III: 15%≤D1≤25%.
3. The diaphragm according to claim 2, characterized in that The isolation film satisfies at least one of the following conditions: Condition i: The pore size D of the first coating 50 5nm to 60nm; Condition ii: The thickness of the first coating layer is 200 nm to 500 nm.
4. The diaphragm according to claim 2, characterized in that The isolation film satisfies at least one of the following conditions: Condition A: The pore size D' of the second coating 50 100nm to 500nm; Condition B: the thickness of the second coating layer is 0.5 μm to 2 μm; Condition C: 40% ≤ D2 ≤ 50%.
5. The diaphragm according to claim 4, characterized in that The isolation film satisfies at least one of the following conditions: Condition a: The pore size D' of the second coating 50 150nm to 300nm; Condition b: The thickness of the second coating layer is 0.5 μm to 1 μm.
6. The diaphragm according to any one of claims 1 to 5, characterized in that: The sum of lithium ion resistances of the first coating layer and the second coating layer is 0.001Ω to 0.015Ω.
7. The diaphragm according to claim 6, characterized in that The sum of lithium ion resistances of the first coating layer and the second coating layer is 0.001Ω to 0.01Ω.
8. The diaphragm according to claim 4, characterized in that The isolation film satisfies: (1) 20≤D′ 50 / D 50 ≤60; (2)2.3≤D2 / D1≤3.
2.
9. An electrochemical device, characterized in that: The electrochemical device comprises a cathode electrode sheet, an anode electrode sheet and a separator arranged between the cathode electrode sheet and the anode electrode sheet; The diaphragm is the diaphragm according to any one of claims 1 to 8.
10. An electronic device, characterized in that: The electronic device comprises the electrochemical device according to claim 9.
Citation Information
Patent Citations
Electrode assembly and lithium secondary battery having same
CN104600240A
Viscous battery separator and lithium ion battery employing same
CN107316968A
Ceramic composite diaphragm and preparation method thereof, and battery
CN112635916A
Separator, electrochemical device, and electronic apparatus
CN116315459A
A Section Reducing Member and a Fixing Frame for Concrete Structure and a Construction Method thereof
KR1020230046923A