Electrode sheet and preparation method therefor, and battery cell, battery and electric apparatus

By coating the thermoplastic polymer insulating layer on the current collector of the electrode sheet and flow curing after cutting, the burrs and exposed end face problems during the electrode sheet cutting process are solved, and the reliability and safety of the battery are improved.

WO2024239985A1PCT designated stage expired Publication Date: 2024-11-28CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/092628
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-22
Filing Date
2024-05-11
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

During the cutting process, the pole sheet in the battery cell is prone to burrs and exposed end faces, resulting in overlapping electrodes with opposite polarity, affecting the reliability and safety of the battery.

Method used

An electrode sheet is designed, the current collector includes a main body part and an electrode, and coats an active material layer and an insulating layer. A thermoplastic polymer is used in the insulating layer. The volume particle size distribution is 6 μm to 10 μm and the maximum particle size is 90 μm to 110 μm. By providing the second insulating layer through the cutting line, the thermoplastic polymer flows to the end face after cutting to cure, forming a uniformly dense insulating layer, reducing the risk of burrs and exposed end faces.

Benefits of technology

It improves the reliability of the pole sheet, reduces the risk of overlapping electrodes with opposite polarity, enhances the safety and performance of the battery, and extends the cycle life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024092628_28112024_PF_FP_ABST
    Figure CN2024092628_28112024_PF_FP_ABST
Patent Text Reader

Abstract

The embodiments of the present application belong to the technical field of batteries. Provided are an electrode sheet and a preparation method therefor, and a battery cell, a battery and an electric apparatus. The electrode sheet comprises a current collector, an active substance layer, a first insulating layer and a second insulating layer, wherein the current collector comprises a main portion and a tab, the tab extends from a first end of the main portion, and the first end is one end of the main portion in a first direction; the main portion comprises a coating area and a transition area, and the transition area is arranged between the coating area and the tab; the active substance layer is arranged on the surface of the coating area; the first insulating layer is arranged on the end face of the main portion at the first end; and at least part of the second insulating layer is arranged on the surface of the transition area, the second insulating layer comprises a thermoplastic polymer, the volume particle size distribution DV50 of the thermoplastic polymer ranges from 6μm to 10μm, and the maximum particle size Dmax of the thermoplastic polymer ranges from 90μm to 110μm. The technical solution of the present application facilitates an improvement in the reliability of a battery cell.
Need to check novelty before this filing date? Find Prior Art

Description

Pole piece and preparation method thereof, battery cell, battery, and electrical device

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to patent application 202310579352.6, filed on May 22, 2023, entitled “Pole piece and preparation method thereof, battery cell, battery, and electrical device,” and the entire contents of that application are incorporated herein by reference. Technical Field

[0003] The present application relates to the field of battery technology, and in particular to a pole piece and a preparation method thereof, a battery cell, a battery, and an electrical device. Background Art

[0004] With the increasing severity of environmental pollution, the new energy industry has attracted more and more attention. In the new energy industry, battery technology is an important factor in its development.

[0005] The development of battery technology requires consideration of multiple design factors, such as energy density, cycle life, and reliability. The design of the pole piece in a battery cell is crucial to its reliability. Therefore, how to provide a pole piece to improve the reliability of the battery cell is a technical problem that needs to be solved urgently.

[0006] Summary of the Invention

[0007] The present application is made in view of the above-mentioned problems, and its purpose is to provide a pole piece to improve the reliability of a battery cell.

[0008] In order to achieve the above-mentioned objectives, the present application provides a pole piece and a preparation method thereof, a battery cell, a battery, and an electrical device.

[0009] In a first aspect, a pole piece is provided, comprising a current collector, an active material layer, a first insulating layer, and a second insulating layer, wherein the current collector comprises a main body and a tab, the tab extending from a first end of the main body, the first end being an end of the main body along a first direction; the main body comprises a coating region and a transition region, the transition region being disposed between the coating region and the tab; the active material layer being disposed on a surface of the coating region; the first insulating layer being disposed on an end face of the main body at the first end; at least a portion of the second insulating layer being disposed on a surface of the transition region, the second insulating layer comprising a thermoplastic polymer, the volume particle size distribution of the thermoplastic polymer being D V 50 is 6 μm to 10 μm, and the maximum particle size D of the thermoplastic polymer is max 90μm~110μm.

[0010] An embodiment of the present application provides a pole piece comprising a current collector, an active material layer, a first insulating layer, and a second insulating layer. The current collector comprises a main body and a tab, the tab extending from a first end of the main body, the first end of the main body being defined as one end of the main body along a first direction. The main body comprises a coating region and a transition region, the transition region being disposed between the coating region and the tab, and the coating region being provided with an active material layer. The provision of the transition region allows the cutting tool to maintain a certain distance from the active material layer during the tab cutting process, thereby reducing the risk of the active material layer shedding. The first insulating layer is disposed on the end surface of the main body at the first end. This first insulating layer covers the end surface of the first end, reducing the risk of the current collector being exposed at the end surface, thereby reducing the risk of the exposed current collector at the end surface contacting an electrode of opposite polarity. Furthermore, the first insulating layer can cover burrs generated during the cutting process, reducing the risk of the burrs contacting an electrode of opposite polarity. At least a portion of the second insulating layer is disposed on the surface of the transition region, and the second insulating layer comprises a thermoplastic polymer. In this way, the cutting line is located in the transition zone. During the process of cutting the tab, the thermoplastic polymer in the second insulating layer on the surface of the transition zone changes from a solid state to a fluid state due to heat. The fluid thermoplastic polymer flows to the end face of the first end and solidifies at the end face after cooling. Volume particle size distribution of thermoplastic polymer D V 50 is 6 μm to 10 μm, and the maximum particle size D of the thermoplastic polymer is max The particle size of the thermoplastic polymer is 90 μm to 110 μm. By properly setting the particle size of the thermoplastic polymer, the thermoplastic polymer is not easily agglomerated. Moreover, the thermoplastic polymer has a suitable flow path after being heated, which is conducive to forming a uniform and dense first insulating layer at the end surface, thereby achieving a uniform and dense coating of the end surface. Therefore, the technical solution of the embodiment of the present application can improve the reliability of the battery cell.

[0011] In one possible implementation, the volume particle size distribution D of the thermoplastic polymer is V 50 is 7 μm to 8 μm, and the maximum particle size D of the thermoplastic polymer is max In this way, the thermoplastic polymer is not easy to agglomerate, and after being heated from a solid state to a fluid state, it has a more suitable flow path, which is conducive to forming a uniform and dense first insulating layer at the end face.

[0012] In a possible implementation, the thickness d2 of the second insulating layer is 22 μm to 48 μm; optionally, the thickness d2 of the second insulating layer is 22 μm to 30 μm.

[0013] In the above technical solution, when the thickness d2 of the second insulating layer is not less than 22 μm, during the cutting process of the current collector provided with the second insulating layer, the second insulating layer contains a large amount of thermoplastic polymer, so that more thermoplastic polymer can flow to the burrs and the exposed end surface of the current collector after being heated, which is conducive to uniformly and densely covering the exposed end surface and burrs. When the thickness d2 of the second insulating layer does not exceed 48 μm, it is conducive to reducing the energy consumed during the cutting process. Optionally, the thickness d2 of the second insulating layer is 22 μm to 30 μm, which can reduce the energy consumed in cutting while improving the coating effect on the exposed end surface and burrs.

[0014] In one possible implementation, the thickness d1 of the first insulating layer is 300 nm to 1800 nm. This allows the first insulating layer to cover burrs and exposed end surfaces while maintaining a relatively low thickness. Alternatively, the thickness d1 of the first insulating layer is 300 nm to 860 nm, which facilitates further reducing the thickness of the first insulating layer while effectively covering burrs and exposed end surfaces.

[0015] In one possible implementation, the thermoplastic polymer has a drop melting point of 80°C to 250°C. Thus, during the cutting process of the current collector provided with the second insulating layer, the heat generated by the cutting causes the thermoplastic polymer to change from a solid state to a fluid state. The fluid thermoplastic polymer can flow to the exposed end surfaces of the current collector after cutting and to the burrs generated by the cutting, thereby facilitating the preparation of the first insulating layer. Optionally, the thermoplastic polymer has a drop melting point of 80°C to 150°C, which helps reduce energy consumption during the cutting process.

[0016] In one possible implementation, the material of the thermoplastic polymer includes: at least one of a crystalline thermoplastic polymer and an amorphous thermoplastic polymer; optionally, the crystalline thermoplastic polymer includes: at least one of polyethylene, polypropylene, and polyamide; optionally, the amorphous thermoplastic polymer includes: at least one of microcrystalline wax, polystyrene, and polymethyl methacrylate.

[0017] In the above technical solution, the use of the above thermoplastic polymer is conducive to forming a uniform and dense coating on the end surface and burrs of the exposed current collector after cutting.

[0018] In a possible implementation, the second insulating layer further includes a binder, which is advantageous in increasing the bonding strength between the thermoplastic polymer and the current collector and reducing the risk of the second insulating layer falling off.

[0019] In a possible implementation, in the second insulating layer, the mass ratio of the thermoplastic polymer to the binder A:B is 60:40 to 80:20; optionally, in the second insulating layer, the mass ratio of the thermoplastic polymer to the binder A:B is 70:30 to 80:20.

[0020] In the above technical solution, by reasonably setting the mass ratio of the thermoplastic polymer and the binder in the second insulating layer, it is beneficial to reduce the risk of the second insulating layer falling off, and at the same time it is beneficial to form a uniform and dense first insulating layer on the end face and burrs of the exposed current collector.

[0021] In one possible implementation, the resistance R of the end surface provided with the first insulating layer satisfies the following conditions: R ≥ 100Ω; optionally, the resistance R of the end surface provided with the first insulating layer satisfies the following conditions: R ≥ 2000Ω. Meeting the above resistance condition at the end surface can reduce the risk of a battery cell short circuit caused by the end surface overlapping an electrode of opposite polarity.

[0022] In one possible implementation, the second insulating layer includes a first portion and a second portion, wherein the first portion is disposed on the surface of the transition region, and the second portion extends from the first portion along the first direction and is disposed on a portion of the surface of the tab. This reduces the risk of the tab overlapping an electrode of opposite polarity.

[0023] In one possible implementation, the first insulating layer is provided on the end surfaces of the tab at both ends of the region where the second portion is provided, along a second direction different from the first direction; optionally, the second direction is perpendicular to the first direction. In this way, the first insulating layer can cover the end surfaces of the tab exposed by cutting, thereby reducing the risk of overlapping the end surfaces with electrodes of opposite polarity.

[0024] In a possible implementation, the material of the first insulating layer is the same as the material of the thermoplastic polymer in the second insulating layer. This helps to simplify the preparation steps of the pole piece and speed up the production process.

[0025] In one possible implementation, the thermoplastic polymer in the first insulating layer is in film form, and the thermoplastic polymer in the second insulating layer includes both film-formed and granular thermoplastic polymers. Thus, the first insulating layer is formed by melting and solidifying the thermoplastic polymer in the second insulating layer. This simplifies the electrode sheet fabrication process, allowing the first insulating layer to be formed simultaneously with cutting.

[0026] In one possible implementation, the current collector comprises a metal foil or a composite current collector; optionally, the metal foil comprises aluminum foil or copper foil; optionally, the composite current collector comprises: a polymer material base layer and a metal layer located on at least one surface of the polymer material base layer; optionally, the current collector comprises aluminum foil. This facilitates selection of a suitable current collector according to actual needs. In the case where the current collector comprises aluminum foil, the electrode is a positive electrode electrode, which helps reduce the risk of overlap between the positive electrode electrode and the negative electrode electrode, and helps improve the reliability of the battery cell. In addition, it also helps reduce the risk of overlap between the positive electrode electrode and the negative electrode electrode.

[0027] In one possible implementation, the first insulating layer is further provided on the end surface of the main body at the second end, the second end being opposite the first end along the first direction. Thus, both the end surface of the main body at the first end and the end surface of the main body at the second end are provided with the first insulating layer, which further reduces the risk of short circuits in the battery cells.

[0028] In a second aspect, a method for preparing a pole piece is provided, comprising: providing a current collector; coating an active material on a first region of the current collector to form an active material layer; coating an insulating slurry on a second region of the current collector to form a second insulating layer, wherein the insulating slurry comprises a thermoplastic polymer and a binder, and the volume particle size distribution D of the thermoplastic polymer is V 50 is 6 μm to 10 μm, and the maximum particle size D of the thermoplastic polymer is max The thickness of the current collector is 90 μm to 110 μm; the current collector provided with the second insulating layer is cut along a cutting line, and at least part of the cutting line is provided in the second region.

[0029] In the above technical solution, by providing the second insulating layer, the first insulating layer can be formed at the same time as cutting, which is conducive to simplifying the preparation steps of the first insulating layer.

[0030] In one possible implementation, the volume particle size distribution D of the thermoplastic polymer is V 50 is 7 μm to 8 μm, and the maximum particle size D of the thermoplastic polymer is max It is 90μm~100μm.

[0031] In a possible implementation, the thickness d2 of the second insulating layer is 22 μm to 48 μm; optionally, the thickness d2 of the second insulating layer is 22 μm to 30 μm.

[0032] In a possible implementation, the thermoplastic polymer has a drop melting point of 80°C to 250°C; optionally, the thermoplastic polymer has a drop melting point of 80°C to 150°C.

[0033] In one possible implementation, the material of the thermoplastic polymer includes: at least one of a crystalline thermoplastic polymer and an amorphous thermoplastic polymer; optionally, the crystalline thermoplastic polymer includes: at least one of polyethylene, polypropylene, and polyamide; optionally, the amorphous thermoplastic polymer includes: at least one of microcrystalline wax, polystyrene, and polymethyl methacrylate.

[0034] In a possible implementation, in the insulating paste, the mass ratio of the thermoplastic polymer to the binder A:B is 60:40 to 80:20; optionally, in the second insulating layer, the mass ratio of the thermoplastic polymer to the binder A:B is 70:30 to 80:20.

[0035] In a possible implementation, cutting the current collector provided with the second insulating layer along a cutting line includes: controlling a laser processing tool to cut the current collector provided with the second insulating layer along the cutting line.

[0036] In the above technical solution, the current collector is cut by laser, which can generate more heat during the cutting process, which is conducive to the thermoplastic polymer in the second insulating layer becoming fluid and flowing to the end surface, thereby facilitating the formation of the first insulating layer.

[0037] In a third aspect, a battery cell is provided, comprising the electrode according to the first aspect and any possible implementation thereof, and / or the electrode prepared by the method according to the second aspect and any possible implementation thereof.

[0038] In a fourth aspect, a battery is provided, comprising the battery cell described in the third aspect.

[0039] In a fifth aspect, an electrical device is provided, comprising the battery described in the fourth aspect. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the following is a brief introduction to the drawings required for use in the embodiments of the present application. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on the drawings without creative work.

[0041] FIG1 is a schematic diagram of a pole piece before processing a pole lug according to an embodiment of the present application;

[0042] FIG2 is a schematic diagram of a pole piece according to an embodiment of the present application;

[0043] FIG3 is a cross-sectional view along the AA direction in FIG2 ;

[0044] FIG4 is a cross-sectional view along the BB direction in FIG2 ;

[0045] FIG5 is a schematic diagram of a method for preparing a pole piece according to an embodiment of the present application;

[0046] FIG6 is a schematic diagram of a current collector according to an embodiment of the present application;

[0047] FIG7 is a schematic diagram of a current collector coated with an active material layer according to an embodiment of the present application;

[0048] FIG8 is a schematic diagram of a current collector coated with a second insulating layer according to an embodiment of the present application;

[0049] FIG9 is a schematic diagram of a current collector showing a cutting line according to an embodiment of the present application;

[0050] FIG10 is a schematic diagram of a battery cell according to an embodiment of the present application;

[0051] FIG11 is a schematic diagram of a battery according to an embodiment of the present application;

[0052] FIG12 is a schematic diagram of an electrical device according to an embodiment of the present application;

[0053] FIG. 13 is a SEM image of an end surface provided with a first insulating layer according to an embodiment of the present application.

[0054] Figure numerals: 1: pole piece; 124: cutting line; 10: current collector; 11: active material layer; 121: first insulating layer; 122: second insulating layer; 101: main body; 102: pole ear; 1011: coating area; 1012: transition area; 1011a: end face; 1221: first part; 1222: second part. DETAILED DESCRIPTION

[0055] The embodiments of the electrode and its preparation method, battery cell, battery, and electrical device of the present application are specifically disclosed in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there may be cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0056] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0057] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0058] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0059] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0060] If not otherwise specified, the “include” and “comprising” mentioned in this application are open-ended. For example, the “include” and “comprising” may include or contain other components that are not listed.

[0061] Unless otherwise specified, the term "and / or" is inclusive in this application. For example, the phrase "A and / or B" means "A, B, or both A and B." More specifically, the condition "A and / or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0062] The development of battery technology must consider multiple design factors simultaneously, such as energy density, cycle life, discharge capacity, charge and discharge rate, reliability, etc. The design of the pole piece in the battery cell is crucial to the reliability of the battery cell. The pole piece usually includes a current collector and an active material layer and an insulating layer coated on different areas of the current collector. After the corresponding active material layer and insulating layer are coated on the current collector, the current collector coated with the active material layer and the insulating layer needs to be cut to cut out the pole lugs. During the cutting process, dust and burrs are easily generated, and the burrs may cause the pole piece to overlap with the electrode of opposite polarity, thereby causing a short circuit.

[0063] In some processing methods, the insulating layer coated on the current collector is set as a ceramic coating to reduce the burrs that appear during the cutting process. However, this processing method can only reduce the number of burrs. Burrs will still exist after cutting. Burrs may cause the pole piece to overlap with an electrode of opposite polarity, resulting in adverse effects. In addition, after cutting, the end face of the current collector is exposed. The exposed end face has the risk of overlapping with an electrode of opposite polarity, which may cause a short circuit in the battery cell and is not conducive to improving the reliability of the battery.

[0064] In order to further improve the reliability of the battery cell, an insulating layer is coated on a specific area of ​​the current collector, and the insulating layer includes a thermoplastic polymer. The cutting line is located in the area where the insulating layer is located. During the process of cutting the current collector to prepare the tab, the thermoplastic polymer in the insulating layer changes from a solid state to a fluid state due to heat, flows to the end face of the cut current collector, and solidifies at the end face after cooling to form a new insulating layer. The new insulating layer formed at the end face can cover the burrs generated by cutting and the exposed end face after cutting. However, the uniformity and density of the new insulating layer formed are poor, and the degree of improvement in the reliability of the battery cell is low.

[0065] In view of this, the present application provides a pole piece. In the pole piece, a specific area of ​​the current collector is coated with an insulating layer, and the volume particle size distribution D of the thermoplastic polymer in the insulating layer is V 50 is 6μm~10μm, the maximum particle size D of thermoplastic polymer maxThe particle size of the thermoplastic polymer is 90 μm to 110 μm. This allows the thermoplastic polymer to have a suitable particle size, which can reduce agglomeration during the insulation coating process. During the tab cutting process, the thermoplastic polymer, after changing from a solid state to a fluid state, has a suitable flow path, which is conducive to forming a uniform and dense insulating coating on the end surface, thereby improving the reliability of the battery cell.

[0066] [Pole piece]

[0067] Figure 1 is a schematic diagram of a pole piece before processing the pole lug according to an embodiment of the present application, Figure 2 is a schematic diagram of a pole piece according to an embodiment of the present application, Figure 3 is a cross-sectional view along the AA direction in Figure 2, and Figure 4 is a cross-sectional view along the BB direction in Figure 2.

[0068] As shown in Figures 1 and 2, Figure 1 is a schematic diagram of the electrode before the tab is processed, and Figure 2 is a schematic diagram of the electrode after the tab is processed. As shown in Figure 1, the black dotted line 124 is the cutting line for cutting the tab. After cutting along the cutting line 124, the electrode 1 shown in Figure 2 is obtained.

[0069] 1 to 4 , the electrode 1 includes a current collector 10 , an active material layer 11 , a first insulating layer 121 and a second insulating layer 122 .

[0070] The current collector 10 has two surfaces facing each other along its thickness direction, and the active material layer 11 can be provided on at least one of the two surfaces facing each other along the thickness direction of the current collector 10. For example, as shown in Figures 3 and 4, the active material layer 11 is provided on both surfaces facing each other along the thickness direction of the current collector 10.

[0071] The thickness direction of the current collector 10 may be the z direction as shown in FIG. 3 and FIG. 4 .

[0072] The current collector 10 includes a main body 101 and a tab 102 , wherein the tab 102 extends from a first end of the main body 101 . The first end of the main body 101 is one end of the main body 101 along a first direction.

[0073] The first direction is parallel to the plane where the current collector 10 is located, and the first direction is the direction in which the tab 102 protrudes relative to the main body 101. For example, the first direction is the y direction in FIG2 .

[0074] The main body 101 includes a coating area 1011 and a transition area 1012 . The transition area 1012 is disposed between the coating area 1011 and the tab 102 .

[0075] The active material layer 11 is provided on the surface of the coating area 1011. For example, as shown in Figures 3 and 4, the active material layer 11 is provided on both surfaces in the thickness direction of the current collector 10. In some embodiments, the active material layer 11 can be provided on one of the two surfaces in the thickness direction of the current collector 10.

[0076] The first insulating layer 121 is disposed on an end surface 1011 a of the main body 101 at the first end.

[0077] An end surface 1011a of the main body 101 at the first end is a surface parallel to the thickness direction of the current collector 10. For example, as shown in FIG3 , the end surface 1011a is a surface parallel to the x-direction and the z-direction.

[0078] The end surface 1011a at the first end of the main body 101 can be formed by the following process: Referring to FIG. 1 , during the cutting process of the current collector 10, the current collector 10 is cut along the cutting line 124. The end surface 1011a is the cut end surface of the transition region 1012. After cutting, the current collector 10 at the end surface 1011a is exposed, and burrs may be generated.

[0079] By providing a first insulating layer 121 at the end surface 1011a, the first insulating layer 121 can cover the burrs generated during the cutting process, thereby reducing the risk of the burrs overlapping with electrodes of opposite polarity. For example, after the electrode sheet 1 is assembled into an electrode assembly with a electrode sheet of opposite polarity (for example, the electrode sheet 1 is a positive electrode sheet and the electrode sheet of opposite polarity is a negative electrode sheet) by winding or laminating, and the electrode assembly is assembled with the end cover assembly and the shell into a battery cell, the burr may overlap with the electrode sheet of opposite polarity. By providing the first insulating layer 121, the first insulating layer 121 can cover the burrs, thereby reducing the risk of the burrs overlapping with electrodes of opposite polarity.

[0080] By providing the first insulating layer 121 on the end surface 1011a, the first insulating layer 121 can cover the exposed end surface 1011a of the trimmed current collector 10, thereby reducing the risk of the end surface 1011a overlapping with an electrode of opposite polarity. For example, if the electrode piece 1 is a positive electrode piece, the provision of the first insulating layer 121 can reduce the risk of internal short circuits in the battery cell caused by overlapping between the electrode piece 1 and the negative electrode piece.

[0081] At least a portion of the second insulating layer 122 is disposed on the surface of the transition region 1012. That is, the second insulating layer 122 is disposed on the surface of the transition region 1012. In addition to the transition region 1012, other regions of the current collector 10 may also be provided with the second insulating layer 122. Providing the second insulating layer 122 in the transition region 1012 helps reduce the risk of overlapping of the electrode 1 with an electrode 1 of opposite polarity.

[0082] The second insulating layer 122 includes a thermoplastic polymer, and the volume particle size distribution D of the thermoplastic polymer is V 50 is 6μm~10μm, the maximum particle size D of thermoplastic polymer max For example, the median particle size D of thermoplastic polymers is 90 μm to 110 μm. V 50 is 6μm, the maximum particle size is D max is 90μm; for another example, D V 50 is 8μm, D max is 100 μm; for another example, D V 50 is 10 μm, D max 110μm. As long as D V 50 and D max The above conditions may be met, and the embodiments of the present application include but are not limited to these.

[0083] Optionally, the volume particle size distribution D of the thermoplastic polymer V 50 and maximum particle size D max For example, due to the limitations of the preparation process of thermoplastic polymers, the volume particle size distribution D of thermoplastic polymers V When 50 is 6 μm, the maximum particle size D of the thermoplastic polymer max 90μm.

[0084] A thermoplastic polymer may be a polymer that softens when heated, solidifies when cooled, and can soften again. For example, when heated to a certain temperature, a thermoplastic polymer changes from solid particles to a flowable state, and when cooled, it can change into a layer or film.

[0085] When the thermoplastic polymer in the second insulating layer 122 is heated to certain conditions, it will change from a solid state to a fluid state. In this way, during the cutting process of the current collector 10 provided with the second insulating layer 122, the fluid thermoplastic polymer can flow to the burrs and the exposed end surface 1011a. After the temperature drops, the fluid thermoplastic polymer solidifies at the burrs and the exposed end surface 1011a, thereby covering the burrs and the exposed end surface 1011a, thereby reducing the risk of the burrs and the exposed end surface 1011a overlapping with electrodes of opposite polarity.

[0086] Volume particle size distribution D v 50 can refer to the particle size corresponding to when the cumulative volume distribution percentage of a sample reaches 50%.

[0087] If the thermoplastic polymer particle size is too small, the thermoplastic polymer is unevenly distributed and easily aggregates when the slurry is prepared and applied to the current collector 10. After the slurry is formed into the second insulating layer 122, the aggregated thermoplastic polymer has a long flow path during the die-cutting process, which is not conducive to forming a uniform and dense first insulating layer 121 at the end surface 1011a.

[0088] In the case where the particle size of the thermoplastic polymer is too large, the thermoplastic polymer with large particle size has a long flow path after changing from a solid state to a fluid state, which is not conducive to forming a uniform and dense first insulating layer 121 at the end surface 1011 a .

[0089] By properly setting the particle size of the thermoplastic polymer, it is beneficial to reduce the agglomeration of the thermoplastic polymer during the preparation process and to form a uniform and dense first insulating layer 121 at the end surface 1011 a.

[0090] An embodiment of the present application provides a pole piece 1, which includes a current collector 10, an active material layer 11, a first insulating layer 121, and a second insulating layer 122. The current collector 10 includes a main body 101 and a pole tab 102, wherein the pole tab 102 extends from a first end of the main body 101, and the first end of the main body 101 is an end of the main body 101 along a first direction. The main body 101 includes a coating area 1011 and a transition area 1012, wherein the transition area 1012 is arranged between the coating area 1011 and the pole tab 102, and the coating area 1011 is provided with an active material layer 11. In this way, by providing the transition area 1012, during the process of cutting the pole tab 102, the cutting tool can be kept at a certain distance from the active material layer 11, thereby reducing the shedding of the active material layer 11. The first insulating layer 121 is disposed on the end surface 1011a at the first end of the main body 101. In this way, the first insulating layer 121 can cover the end surface 1011a of the first end, reducing the risk of the current collector at the end surface 1011a being exposed, thereby reducing the risk of the exposed current collector 10 at the end surface 1011a overlapping with an electrode of opposite polarity. In addition, the first insulating layer 121 can also cover burrs generated during the cutting process, reducing the risk of the burrs overlapping with an electrode of opposite polarity. At least a portion of the second insulating layer 122 is disposed on the surface of the transition region 1012, and the second insulating layer 122 includes a thermoplastic polymer. In this way, the cutting line is located in the transition region 1012. During the process of cutting the tab 102, the thermoplastic polymer in the second insulating layer 122 on the surface of the transition region 1012 is heated to change from a solid state to a fluid state. The fluid thermoplastic polymer flows to the end surface 1011a of the first end and solidifies at the end surface 1011a after cooling. Volume particle size distribution D of thermoplastic polymers V 50 is 6 μm to 10 μm, and the maximum particle size D of the thermoplastic polymer is maxThe particle size of the thermoplastic polymer is 90 μm to 110 μm. By properly setting the particle size of the thermoplastic polymer, the thermoplastic polymer is not easily agglomerated. Moreover, after being heated, the thermoplastic polymer has a suitable flow path, which is conducive to forming a uniform and dense first insulating layer 121 at the end surface 1011a, thereby achieving a uniform and dense coating of the end surface. Therefore, the technical solution of the embodiment of the present application can improve the uniformity and density of the first insulating layer 121, thereby further improving the reliability of the battery cell.

[0091] In some embodiments, the volume particle size distribution D of the thermoplastic polymer is V 50 is 7 μm to 8 μm, and the maximum particle size D of the thermoplastic polymer is max In this way, the thermoplastic polymer is not easy to agglomerate, and after being heated from a solid state to a fluid state, it has a more suitable flow path, which is conducive to forming a uniform and dense first insulating layer 121 at the end surface.

[0092] In some embodiments, the thickness d2 of the second insulating layer 122 is 22 μm to 48 μm. For example, d2 is 22 μm, 25 μm, 30 μm, 40 μm, 45 μm, 48 μm, or any value within the above range.

[0093] The thickness d2 of the second insulating layer 122 refers to the thickness located on one side surface of the current collector 10. In the pole piece 1, along the thickness direction of the pole piece 1, the total thickness of the second insulating layer 122 is 44 μm to 96 μm.

[0094] The thickness d2 of the second insulating layer 122 is the average thickness of the second insulating layer 122 along the thickness direction of the current collector 10. For example, the thickness d2 is the average of the maximum dimension and the minimum dimension in the first direction.

[0095] When the thickness d2 of the second insulating layer 122 is not less than 22 μm, during the process of cutting the current collector 10 provided with the second insulating layer 122, there is more thermoplastic polymer in the second insulating layer 122, so that more thermoplastic polymer can flow to the burrs and the exposed end surface 1011a of the current collector 10 after being heated, which is conducive to uniformly and densely covering the exposed end surface 1011a and the burrs.

[0096] When the thickness d2 of the second insulating layer 122 does not exceed 48 μm, it is beneficial to reduce the energy consumed in the cutting process.

[0097] Optionally, the thickness d2 of the second insulating layer 122 is 20 μm to 30 μm, which can reduce the energy consumed in cutting while improving the covering effect on the exposed end surface 1011 a and burrs.

[0098] The thickness d2 of the second insulating layer 122 can be measured in the following manner: photograph the pole piece 1 along the thickness direction of the pole piece 1 using a scanning electron microscope (SEM), and measure the thickness d2 of the second insulating layer 122 from the obtained image.

[0099] Optionally, the second insulating layer 122 has a thickness of 20 μm to 50 μm, for example, 20 μm, 50 μm, or any value within the above range.

[0100] In some embodiments, the thickness d1 of the first insulating layer 121 is 300 nm to 1800 nm. For example, d1 can be 300 nm, 400 nm, 500 nm, 800 nm, 1000 nm, 1500 nm, 1800 nm, or any value within the above range.

[0101] The smaller the thickness d1 of the first insulating layer 121, the smaller the space occupied by the electrode 1, which is beneficial for improving the volumetric energy density of the battery cell. By setting the thickness d1 of the first insulating layer 121 to 300nm to 1800nm, the first insulating layer 121 can effectively cover burrs and exposed end surfaces 1011a while maintaining a relatively small thickness, thereby further improving the performance of the battery cell.

[0102] The thickness d1 of the first insulating layer 121 is an average thickness of the first insulating layer 121 along the first direction. For example, the thickness d1 is an average of the maximum dimension and the minimum dimension in the first direction.

[0103] The thickness d1 of the first insulating layer 121 can be measured in the following manner: photographing the end surface 1011 a of the pole piece 1 using a scanning electron microscope (SEM), and measuring the thickness d1 of the first insulating layer 121 based on the obtained image.

[0104] Optionally, the thickness d1 of the first insulating layer 121 is 300 nm to 860 nm, which is beneficial for further reducing the thickness of the first insulating layer 121 while better covering the burrs and the exposed end surface 1011 a.

[0105] Optionally, the thickness d1 of the first insulating layer 121 is 200 nm to 2000 nm. For example, d1 can be 200 nm, 2000 nm, or any value within the above range.

[0106] In some embodiments, the thermoplastic polymer has a drop melting point of 80° C. to 250° C. For example, the thermoplastic polymer has a drop melting point of 80° C., 100° C., 150° C., 200° C., 250° C., or any value within the above ranges.

[0107] The drop melting point of the thermoplastic polymer is not less than 80°C, thereby reducing the risk of the thermoplastic polymer melting or flowing due to heating of the pole piece 1 during other processing. The drop melting point of the thermoplastic polymer is not more than 250°C, thereby reducing the risk of the thermoplastic polymer not being able to transform into a fluid state during the cutting process, thereby reducing the risk of not being able to form the first insulating layer 121 on the end surface 1011a.

[0108] The drop melting point of a thermoplastic polymer is the temperature at which the thermoplastic polymer changes from a solid or semi-solid state to a liquid state.

[0109] During the process of cutting the current collector 10 provided with the second insulating layer 122, under the action of the heat generated by the cutting, the thermoplastic polymer changes from a solid state to a fluid state. The fluid thermoplastic polymer can flow to the end surface 1011a of the current collector 10 exposed after cutting and the burrs generated by the cutting, thereby facilitating the preparation of the first insulating layer 121.

[0110] Optionally, the thermoplastic polymer has a drop melting point of 80° C. to 150° C., which is beneficial for reducing energy consumption during the cutting process.

[0111] Optionally, the drop melting point of the thermoplastic polymer is 150° C. to 250° C., so that the risk of the thermoplastic polymer becoming a fluid state due to other factors during the process of not cutting the current collector 10 can be reduced.

[0112] In some embodiments, the material of the thermoplastic polymer includes: at least one of a crystalline thermoplastic polymer and an amorphous thermoplastic polymer; optionally, the crystalline thermoplastic polymer includes: at least one of polyethylene, polypropylene, and polyamide; optionally, the amorphous thermoplastic polymer includes: at least one of microcrystalline wax, polystyrene, and polymethyl methacrylate.

[0113] The drop melting point of a crystalline thermoplastic polymer may refer to the melting point of the crystalline thermoplastic polymer. The drop melting point of an amorphous thermoplastic polymer may refer to the glass transition temperature of the amorphous thermoplastic polymer.

[0114] In the above technical solution, the use of the aforementioned thermoplastic polymer facilitates forming a uniform and dense coating on the exposed end face 1011a and burrs of the cut current collector 10. Furthermore, the aforementioned thermoplastic polymer has high insulation and pressure resistance. When the electrode 1 is immersed in the electrolyte, the thermoplastic polymer does not undergo an electrochemical reaction with the electrolyte.

[0115] In some embodiments, the material of the second insulating layer 122 further includes an adhesive.

[0116] The provision of the adhesive in the second insulating layer 122 facilitates the adhesion of the thermoplastic polymer to the transition region 1012 , thereby reducing the risk of the second insulating layer 122 falling off from the transition region 1012 .

[0117] In some embodiments, in the second insulating layer 122 , the mass ratio of the thermoplastic polymer to the binder A:B is 60:40 to 80:20, for example, A:B is 60:40, 70:30, 75:25, 80:20, or any value within the above range.

[0118] In the above technical solution, by reasonably setting the mass ratio of the thermoplastic polymer and the binder in the second insulating layer 122, it is beneficial to reduce the risk of the second insulating layer 122 falling off, and at the same time it is beneficial to form a uniform and dense first insulating layer 121 on the end surface 1011a of the exposed current collector 10 and the burrs.

[0119] Optionally, in the second insulating layer 122 , the mass ratio of the thermoplastic polymer to the binder A:B is 70:30 to 80:20.

[0120] In some embodiments, the resistance R of the end surface 1011 a provided with the first insulating layer 121 satisfies: R≧100Ω. For example, R is 100Ω, 500Ω, or 1000Ω.

[0121] When the resistance of the end face 1011a is greater than 100Ω, even in some extreme cases, when the end face 1011a is overlapped with an electrode of opposite polarity, the battery cell will not have an internal short circuit due to the certain resistance of the end face 1011a, thereby reducing the risk of fire or even explosion caused by the internal short circuit.

[0122] Optionally, the resistance R of the end surface 1011a provided with the first insulating layer 121 satisfies: R≥2000Ω. For example, R is 200Ω, 5000Ω, or infinite. In this way, the risk of internal short circuit of the battery cell can be further reduced.

[0123] In some embodiments, the second insulating layer 122 includes a first portion 1221 and a second portion 1222. The first portion 1221 is disposed on the surface of the transition region 1012, and the second portion 1222 extends from the first portion 1221 along a first direction and is disposed on a portion of the surface of the tab 102. In this way, the risk of the tab 102 overlapping with an electrode of opposite polarity can be reduced.

[0124] Part of the area of ​​the tab 102 is provided with the second portion 1222 of the second insulating layer 122, while other areas are not provided with the second portion 1222. This facilitates welding of the tab 102 and subsequent use of the battery cell.

[0125] In some embodiments, along a second direction, the first insulating layer 121 is provided on end surfaces 1222 a at both ends of the region of the tab 102 where the second portion 1222 is provided. The second direction is different from the first direction.

[0126] In the case where the pole piece 1 includes a plurality of pole tabs 102, the second direction may be the arrangement direction of the plurality of pole tabs 102. For example, as shown in FIG2 , the second direction is the x direction.

[0127] When cutting the current collector 10 along the cutting line 124 to prepare the tab 102, the cutting tool passes through the area of ​​the second portion 1222. After cutting, the end surface 1222a of this area along the second direction is exposed. By providing the first insulating layer 121 on this end surface 1222a, the risk of the end surface 1222a overlapping with the electrode of opposite polarity can be reduced.

[0128] The first insulating layer 121 disposed on the end surfaces 1222 a at both ends of the second portion 1222 is formed during the process of cutting the current collector 10 .

[0129] Optionally, the second direction is perpendicular to the first direction, so as to facilitate cutting of the tab 102 .

[0130] In some embodiments, the material of the first insulating layer 121 is the same as the material of the thermoplastic polymer in the second insulating layer 122. This helps to simplify the preparation steps of the pole piece 1.

[0131] For example, the active material layer 11 and the second insulating layer 122 are first prepared on the current collector 10, and the first insulating layer 121 is simultaneously prepared during the cutting process. In this way, the tab 102 can be cut and the first insulating layer 121 can be prepared simultaneously in one step.

[0132] In some embodiments, the thermoplastic polymer in the first insulating layer 121 is in the form of a film, and the thermoplastic polymer in the second insulating layer 122 includes both a film-like thermoplastic polymer and a granular thermoplastic polymer. Thus, the first insulating layer 121 is formed by melting and solidifying the thermoplastic polymer in the second insulating layer 122. Once the thermoplastic polymer in the second insulating layer 122 becomes fluid, it flows to the end face 1011a and solidifies there to form the first insulating layer 121. This simplifies the preparation steps of the electrode 1, allowing the first insulating layer 121 to be formed simultaneously with the cutting and preparation of the electrode tab 102.

[0133] In the second insulating layer 122 , at least a portion of the granular thermoplastic polymer remains; in the first insulating layer 121 , the thermoplastic polymer is in a film-like state and has almost no granular shape.

[0134] The granular thermoplastic polymer may have various shapes, such as spheres, rods, and sheets. The granular thermoplastic polymer herein means that the thermoplastic polymer has not become a fluid state and is in a solid state.

[0135] Before cutting the second insulating layer 122, the thermoplastic polymer in the second insulating layer 122 is in a granular form. During the cutting process, some of the thermoplastic polymer in the second insulating layer 122 changes from a solid state to a fluid state (for example, the thermoplastic polymer near the cutting line 124 changes to a fluid state), while the remaining portion of the thermoplastic polymer remains in a solid granular form.

[0136] In some embodiments, the current collector 10 includes a metal foil or a composite current collector, so that the material of the current collector 10 can be easily configured according to actual needs.

[0137] Optionally, the metal foil includes aluminum foil or copper foil.

[0138] Optionally, the composite current collector includes: a polymer material base layer and a metal layer located on at least one surface of the polymer material base layer.

[0139] Optionally, the current collector comprises aluminum foil. In this case, the electrode sheet 1 is a positive electrode sheet, which helps reduce the risk of overlap between the positive electrode sheet and the negative electrode sheet, thereby improving the reliability of the battery cell. Furthermore, it helps reduce the risk of overlap between the positive electrode sheet and the negative electrode sheet due to lithium dendrites.

[0140] In some embodiments, the first insulating layer 121 is further disposed on an end surface of the main body 101 at a second end, where the second end is opposite to the first end along the first direction.

[0141] The main body 101 has two opposite ends along a first direction, wherein the two ends are a first end and a second end respectively. The tab 102 protrudes from the main body 101 at the first end, and the second end is opposite to the first end along the first direction.

[0142] The end faces of the main body 101 at the second end and the end faces at the first end are both provided with a first insulating layer 121. This is beneficial to reducing the risk of internal short circuit caused by the end faces at the first end and the second end overlapping with electrodes of opposite polarity, thereby further improving the reliability of the battery cell.

[0143] The above text describes the technical solution of the electrode in conjunction with Figures 1 to 4. The following text describes the method for preparing the electrode in conjunction with Figure 5. The parts corresponding to the electrode can be referred to above and will not be repeated here.

[0144] [Method for preparing electrode]

[0145] FIG5 is a schematic diagram of a method for preparing a pole piece according to an embodiment of the present application. The method 200 can be used to prepare the pole piece 1 in the above embodiment. The method 200 includes the following steps.

[0146] Step 210 , providing a current collector 10 .

[0147] FIG6 is a schematic diagram of a current collector according to an embodiment of the present application. For example, as shown in FIG6 , the current collector 10 is in the shape of a sheet or a rectangle. The shape and size of the current collector 10 can be set according to actual needs, and the embodiments of the present application include but are not limited to this.

[0148] In step 220 , an active material is coated on the first region of the current collector 10 to form an active material layer 11 .

[0149] Figure 7 is a schematic diagram of a current collector coated with an active material layer according to an embodiment of the present application. As shown in Figure 7 , an active material is coated in a first region of the current collector 10 to obtain a current collector 10 provided with an active material layer 11 .

[0150] The first region of the current collector 10 can be a region set according to actual needs. In the embodiment of the present application, the first region corresponds to the coating area 1011 of the main body 101 of the electrode 1.

[0151] In step 230 , an insulating paste is coated on the second region of the current collector 10 to form a second insulating layer 122 .

[0152] The insulation paste includes a thermoplastic polymer and a binder. The volume particle size distribution of the thermoplastic polymer is D V 50 is 6μm~10μm, the maximum particle size D of thermoplastic polymer max 90μm~110μm.

[0153] FIG8 is a schematic diagram of a current collector coated with a second insulating layer according to an embodiment of the present application. As shown in FIG8 , an insulating slurry is coated on the second region of the current collector 10 to obtain a current collector 10 provided with a second insulating layer 122 .

[0154] The size of the second region can be set according to actual needs. In the embodiment of the present application, the second region corresponds to the transition region 1012 of the main body 101 of the electrode 1 and the region of the electrode tab 102 where the second insulating layer 122 is provided.

[0155] In step 240 , the current collector 10 provided with the second insulating layer 122 is cut along the cutting lines 124 , wherein at least a portion of the cutting lines 124 is provided in the second region.

[0156] Figure 9 is a schematic diagram of a current collector showing a cutting line according to an embodiment of the present application. As shown in Figure 9 , the current collector 10 is cut along the cutting line 124 to obtain the electrode 1 shown in Figures 2 to 4 .

[0157] In the above technical solution, the first insulating layer 121 can be formed simultaneously with cutting by providing the second insulating layer 122, which helps to simplify the preparation steps of the first insulating layer 121. The pole piece 1 prepared by the above method is applied to a battery cell, which can make the battery cell have higher reliability.

[0158] In some embodiments, the volume particle size distribution D of the thermoplastic polymer is V 50 is 7 μm to 8 μm, and the maximum particle size D of the thermoplastic polymer is max It is 90μm~100μm.

[0159] In some embodiments, the thickness d2 of the second insulating layer 122 is 22 μm to 48 μm; optionally, d2 is 22 μm to 30 μm.

[0160] In some embodiments, the thermoplastic polymer has a drop melting point of 80°C to 250°C; alternatively, the thermoplastic polymer has a drop melting point of 80°C to 150°C.

[0161] In some embodiments, the material of the thermoplastic polymer includes: at least one of a crystalline thermoplastic polymer and an amorphous thermoplastic polymer; optionally, the crystalline thermoplastic polymer includes: at least one of polyethylene, polypropylene, and polyamide; optionally, the amorphous thermoplastic polymer includes: at least one of microcrystalline wax, polystyrene, and polymethyl methacrylate.

[0162] In some embodiments, in the insulating paste, the mass ratio of the thermoplastic polymer to the binder A:B is 60:40 to 80:20; optionally, in the second insulating layer 122 , the mass ratio of the thermoplastic polymer to the binder A:B is 70:30 to 80:20.

[0163] In some embodiments, step 240 includes controlling a laser processing tool to cut the current collector 10 provided with the second insulating layer 122 along a cutting line. As an example, the power of the laser processing tool is 200 W, the frequency is 200 kHz, and the feed speed is 30 m / min.

[0164] In the embodiments of the present application, laser parameters can be adjusted based on the melting point of the thermoplastic polymer, the thickness of the second insulating layer 122, and other factors. For example, if the melting point of the thermoplastic polymer is high or the second insulating layer 122 is thick, the power or frequency can be increased, or the feed rate can be reduced. For another example, cutting parameters suitable for all conditions (e.g., suitable for thermoplastic polymers with various melting points) can be selected to cut the current collector 10.

[0165] In the above technical solution, by using laser cutting, more heat can be generated during the cutting process, which is conducive to the thermoplastic polymer in the second insulating layer 122 becoming fluid and flowing to the end surface 1011a, thereby facilitating the formation of the first insulating layer 121.

[0166] [Positive electrode]

[0167] The electrode sheet 1 in the embodiment of the present application may be a positive electrode sheet, which includes a positive electrode current collector and a positive electrode film layer disposed on the positive electrode current collector.

[0168] The positive electrode current collector may be a metal foil or a composite current collector. For example, the positive electrode current collector may be an aluminum foil.

[0169] The composite current collector may include a polymer base layer and a metal layer formed on at least one surface of the polymer base layer. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, etc.) on a polymer substrate (such as a substrate made of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0170] The positive electrode film layer includes a positive electrode active material. The positive electrode active material can be a positive electrode active material for batteries known in the art. For example, the positive electrode active material is lithium iron phosphate, a ternary material, a lithium-rich manganese-based material, etc. As an example, the positive electrode active material is a ternary material, and further, a ternary material of a high nickel system. For example, LiNi 0.6 Co 0.2 Mn 0.2 O2, LiNi 0.8 Co 0.1 Mn 0.1 O2.

[0171] The positive electrode film layer may also optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), a vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, a vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, a tetrafluoroethylene-hexafluoropropylene copolymer, and a fluorine-containing acrylate resin.

[0172] The positive electrode film layer may further optionally include a conductive agent, which may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0173] [Negative electrode]

[0174] The electrode sheet 1 in the embodiment of the present application may be a negative electrode sheet, which includes a negative electrode current collector and a negative electrode film layer disposed on the negative electrode current collector.

[0175] The negative electrode current collector can be a metal foil or a composite current collector. The negative electrode current collector can be copper foil. The composite current collector can be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, silver alloy, etc.) on a polymer material substrate (such as polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0176] The negative electrode film layer includes a negative electrode active material. The negative electrode active material can be a negative electrode active material for batteries that is well known in the art. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, etc. The silicon-based material can be selected from at least one of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material can be selected from at least one of elemental tin, tin oxide compounds, and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries can also be used. These negative electrode active materials can be used alone or in combination of two or more.

[0177] The negative electrode film layer may further optionally include a conductive agent, which may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0178] [Electrolytes]

[0179] The electrolyte conducts ions between the positive and negative electrodes. The present invention does not specifically limit the type of electrolyte, and the electrolyte can be selected based on the needs. For example, the electrolyte can be liquid, gel, or solid.

[0180] In some embodiments, the electrolyte is an electrolyte solution comprising an electrolyte salt and a solvent.

[0181] The electrolyte salt may include at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bisfluorosulfonyl imide, lithium bistrifluoromethanesulfonyl imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium bisoxalatoborate, lithium difluorodioxalatophosphate, and lithium tetrafluorooxalatophosphate.

[0182] The solvent may include at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methylpropyl carbonate, ethylpropyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.

[0183] The electrolyte may also optionally include negative electrode film-forming additives, positive electrode film-forming additives, and may also include performance additives that can improve certain battery properties, such as improving battery overcharge performance, improving battery high or low temperature performance, etc.

[0184] [Isolation film]

[0185] The separator is used to separate the positive electrode sheet from the negative electrode sheet. The present invention has no particular restrictions on the type of separator, and any known porous separator with good chemical and mechanical stability can be used.

[0186] The material of the separator can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.

[0187] The positive electrode sheet, the negative electrode sheet and the separator can be made into an electrode assembly through a winding process or a lamination process.

[0188] [Battery Cell]

[0189] An embodiment of the present application provides a battery cell, comprising the pole piece 1 in the above embodiment.

[0190] The embodiment of the present application has no particular limitation on the shape of the battery cell, which can be cylindrical, square, or any other shape. The battery cell can be a lithium-ion battery, a lithium-sulfur battery, a sodium-ion battery, a magnesium-ion battery, or the like.

[0191] FIG10 is a schematic diagram of a battery cell according to an embodiment of the present application. For example, as shown in FIG10 , the battery cell 3 is a square battery cell. The battery cell 3 includes a housing 31 , an end cap assembly 32 , and an electrode assembly 33 disposed in the housing 31 .

[0192] The electrode assembly 33 can be made of a positive electrode sheet, a negative electrode sheet and a separator by a winding process or a lamination process. In some embodiments, the positive electrode sheet is the electrode sheet 1 in the embodiment of the present application.

[0193] The end cap assembly 32 includes an electrode terminal 322 . For example, as shown in FIG. 10 , the end cap assembly 32 includes two electrode terminals 322 , one of which is a positive electrode terminal and the other is a negative electrode terminal.

[0194] The battery cell 3 further includes a current collecting member 34, which is used to connect the electrode tab 331 of the electrode assembly 33 and the electrode terminal 322. For example, when the electrode sheet 1 in the embodiment of the present application is a positive electrode sheet, one current collecting member 34 is used to connect the positive electrode tab (which may also be the tab 102 of the electrode sheet 1) and the positive electrode terminal, and the other current collecting member 34 is used to connect the negative electrode tab and the negative electrode terminal.

[0195] In some embodiments, battery cells may be assembled into a battery module. The number of battery cells contained in a battery module may be one or more. The specific number may be selected by those skilled in the art based on the application and capacity of the battery module.

[0196] [Battery]

[0197] The present invention provides a battery comprising the battery cells of the above-mentioned embodiment. Figure 11 is a schematic diagram of a battery according to an embodiment of the present invention. As shown in Figure 11, the battery 5 may comprise a plurality of battery cells (not shown in the figure).

[0198] The battery cells 3 can be directly assembled into the battery 5 , or they can be assembled into battery modules first, and then multiple battery modules can be assembled into the battery 5 .

[0199] [Electrical devices]

[0200] An embodiment of the present application provides an electrical device, comprising the battery described in the above embodiment.

[0201] Figure 12 is a schematic diagram of an electric device according to an embodiment of the present application. As shown in Figure 12, the present application provides an electric device 6, which includes the battery according to the above embodiment.

[0202] Optionally, the electrical device may also be an energy storage device, a lighting device, a spacecraft, etc., and the embodiments of the present application include but are not limited to the above.

[0203] Below, the embodiment of the present application is described. The embodiment described below is exemplary and is only used to explain the present application, and is not to be construed as limiting the present application. Where specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. Reagents or instruments used that do not specify the manufacturer are conventional products that can be obtained commercially.

[0204] [Example]

[0205] Example 1

[0206] The pole piece in Example 1 has the structure shown in FIG2 .

[0207] In Example 1, the volume particle size distribution D of the thermoplastic polymer in the second insulating layer is V 50 is 6μm, the maximum particle size D max The thickness is 90 μm, the material of the thermoplastic polymer is microcrystalline wax, and the drop melting point of the microcrystalline wax is 80°C.

[0208] The thickness d2 of the second insulating layer is 30 μm, and the thickness d1 of the first insulating layer is 860 nm.

[0209] In the second insulating layer, the mass ratio of the thermoplastic polymer to the binder A:B is 80:20.

[0210] Examples 2-5

[0211] The difference between Example 2-5 and Example 1 is that in the second insulating layer, the volume particle size distribution D of the thermoplastic polymer is V 50 and maximum particle size D max The specific parameters can be found in Table 1.

[0212] Examples 6-9

[0213] The difference between Examples 6-9 and Example 1 is that the thickness of the second insulating layer is different.

[0214] Correspondingly, as the thickness of the second insulating layer changes, the thickness of the first insulating layer and the resistance of the end surface also change.

[0215] Examples 10-12

[0216] The difference between Examples 10-12 and Example 1 is that the materials of the thermoplastic polymer are different.

[0217] Accordingly, the drop melting points of thermoplastic polymers vary.

[0218] Among them, PTFE is polytetrafluoroethylene.

[0219] Examples 13-14

[0220] The difference between Examples 13-14 and Example 1 is that the mass ratio of the thermoplastic polymer to the binder in the second insulating layer is different.

[0221] Comparative Example 1

[0222] The difference between Comparative Example 1 and Example 1 is that the material of the second insulating layer does not include a thermoplastic polymer, and the material in the second insulating layer includes boehmite.

[0223] Comparative Examples 2-3

[0224] The difference between Comparative Example 2-3 and Example 12 is that the volume particle size distribution D of the thermoplastic polymer in the second insulating layer is V 50 and maximum particle size D max different.

[0225] Comparative Examples 4-6

[0226] The difference between Comparative Examples 4-6 and Example 1 is that the volume particle size distribution D of the thermoplastic polymer in the second insulating layer is V 50 and maximum particle size D max different.

[0227] Table 1 Parameters of Examples and Comparative Examples

[0228] Table 2 Experimental results of comparative examples and embodiments

[0229] [Preparation of battery cells]

[0230] (1) Preparing the slurry for the second insulating coating

[0231] A thermoplastic polymer and a binder are mixed in a specific ratio, and a solvent is added and stirred until uniformly mixed. The slurry has a viscosity of approximately 3000 mPa·s. The binder is polyvinylidene fluoride (PVDF), and the solvent is nitrogen-methyl pyrrolidone. The specific thermoplastic polymers and the ratio of thermoplastic polymer to binder are shown in Table 1.

[0232] (2) Coating and drying

[0233] When the positive electrode active slurry is coated on the aluminum foil to prepare the active material layer, the positive electrode active material in the positive electrode active slurry is LiNi 0.8 Co 0.1 Mn 0.1 O2 (NCM811); apply the above insulating coating slurry to a 3 mm width on aluminum foil. Oven dry at 100°C. The thickness of the second insulating layer after drying is shown in Table 1. The thickness of the second insulating layer here refers to the thickness of the second insulating layer on one side of the current collector.

[0234] (3) Laser die cutting

[0235] The above products were die-cut. The specific process parameters are shown in Table 1.

[0236] (4) Making battery cells

[0237] The positive electrode sheet is assembled together with other battery components: negative electrode sheet, separator, and electrolyte to form a lithium-ion battery cell.

[0238] [Confirmation of the first insulating layer]

[0239] The end face is observed using a scanning electron microscope (SEM) to check whether the first insulating layer is present at the end face. In addition, the thickness of the first insulating layer can also be observed through photos taken with the scanning electron microscope.

[0240] [Confirmation of the second insulating layer]

[0241] Use a scanning electron microscope to observe the surface of the electrode to check whether there is a second insulating layer on the surface. Cut the electrode open and photograph the cross section of the electrode using a scanning electron microscope. Observe the thickness of the second insulating layer based on the photograph.

[0242] [Overlapping full-charge anode test]

[0243] Use the laser die-cut end face to overlap the fully charged anode and observe whether it catches fire.

[0244] [After soaking in electrolyte, connect the fully charged anode for testing]

[0245] After the electrode pieces are cut, they are immersed in electrolyte at 70°C for 7 days. Then, the cut end faces are used to overlap the fully charged anodes to observe whether fire occurs.

[0246] [Slurry performance test]

[0247] During the process of preparing the coating slurry for the second insulating layer, observe whether the polymer particles in the slurry are agglomerated.

[0248] [Test of end surface resistance]

[0249] The resistance of the end face can be measured using an ohmmeter.

[0250] For example, one end of the ohmmeter is connected to the tab of the positive electrode sheet in the embodiment (specifically, the portion of the tab not coated with the second insulating layer), and the other end is connected to the tab of the negative electrode sheet, and the end faces of the negative electrode sheet and the positive electrode sheet are overlapped.

[0251] [Testing of particle size of thermoplastic polymers]

[0252] The volume particle size distribution of the thermoplastic polymer can be determined by a particle size analyzer-laser diffraction method. Specifically, the standard GB / T19077-2016 can be referred to, and a laser diffraction scattering particle size analyzer can be used for measurement according to the manufacturer's instructions. For example, before preparing the slurry for the second insulating layer, an appropriate amount of thermoplastic polymer is taken and the average volume particle size of the material is tested using a Malvern 2000 (MasterSizer 2000) laser particle size analyzer. Take an appropriate amount of the sample to be tested (the sample concentration is sufficient to ensure 8-12% shading), add 20 ml of deionized water, and simultaneously supercharge for 5 minutes (53KHz / 120W) to ensure that the sample is completely dispersed, and then measure the sample according to the GB / T19077-2016 / ISO 13320:2009 standard.

[0253] For another example, a scanning electron microscope can be used to test the electrode to obtain an image of the area of ​​the second insulating layer of the electrode. A specific size area is selected, and the volume particle size distribution Dv50 and the maximum particle size D of the thermoplastic polymer are calculated based on the number and size of the thermoplastic polymer in the image. max .

[0254] [Confirmation of the Drop Melting Point of Thermoplastic Polymers]

[0255] The drop melting point of thermoplastic polymers can be determined using GB / T8026-2014. For example, a cooled temperature sensor is vertically immersed in a sample, allowing the sample to adhere to the sensor. The sample is then placed in a test tube and heated at the required heating rate to begin melting. The temperature at which the first drop of sample falls from the sensor is the sample's drop melting point.

[0256] For another example, the drop melting point of a thermoplastic polymer can be determined based on the specific type of thermoplastic polymer. For example, for a crystalline thermoplastic polymer, the drop melting point refers to the melting point of the crystalline thermoplastic polymer; for an amorphous thermoplastic polymer, the drop melting point refers to the glass transition temperature of the amorphous thermoplastic polymer.

[0257] [Mass ratio of thermoplastic polymer to binder]

[0258] The mass ratio of the thermoplastic polymer to the binder can be obtained according to the mass of the thermoplastic polymer and the mass of the binder added during the preparation process.

[0259] Figure 13 is a SEM image of an end surface provided with a first insulating layer according to an embodiment of the present application. As shown in Figure 13 , a first insulating layer 121 is provided at the end surface of the pole piece.

[0260] As shown in Examples 1-14 and Comparative Example 1, a first insulating layer is provided at the end face of the pole piece. After the end face of the pole piece is overlapped with the fully charged anode, no fire will occur. Therefore, the technical solution of the embodiment of the present application can improve the reliability of the battery cell.

[0261] In combination with Examples 1-5 and Comparative Example 6, as well as Example 12 and Comparative Examples 2-3, by setting the volume particle size distribution D of the thermoplastic polymer in the second insulating layer to V 50 is 6μm~10μm and the maximum particle size D max The thickness of the nanostructured carbon fiber is 90 μm to 110 μm. During the process of preparing the slurry for the second insulating layer, the thermoplastic polymer in the slurry will not agglomerate, which facilitates the preparation of the second insulating layer.

[0262] In combination with Examples 1-5 and Comparative Examples 4-5, by setting the maximum particle size D of the thermoplastic polymer in the second insulating layer to max The diameter of the thermoplastic polymer is 90 μm to 110 μm. In the process of cutting the current collector to prepare the pole ear, the thermoplastic polymer changes from a solid state to a fluid state. The fluid thermoplastic polymer has a suitable flow path, which is convenient for flowing to the end face to coat the end face to form a uniform first insulating layer. In this way, when the pole piece overlaps the fully charged anode, no fire will occur; while in comparative examples 4-5, only some positions will not catch fire. In addition, after the pole piece is soaked in the electrolyte, when the pole piece overlaps the fully charged anode, no fire will occur; while in comparative examples 4-5, only some positions will not catch fire. Therefore, a reasonable setting of the particle size of the thermoplastic polymer is beneficial to improving the density of the first insulating layer, thereby improving the adhesion ability of the first insulating layer to the end face. Therefore, by reasonably setting the maximum particle size D of the thermoplastic polymer in the second insulating layer max , which is beneficial to improving the uniformity and density of the first insulating layer and further improving the reliability of the battery cell.

[0263] In combination with Examples 6-9, by reasonably setting the thickness of the second insulating layer, a first insulating layer with a suitable thickness can be obtained after cutting.

[0264] In conjunction with Examples 10-12, the thermoplastic polymer in the second insulating layer can be a variety of materials.

[0265] In combination with Examples 13-14, a reasonable arrangement of the thermoplastic polymer and the binder in the second insulating layer can be applied to a variety of different mass ratios.

[0266] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are merely examples, and any embodiments having substantially the same structure and effect as the technical concept within the scope of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the present application, any other embodiments that can be conceived by those skilled in the art and that combine some of the constituent elements in the embodiments are also included in the scope of the present application.

Claims

1. A pole piece, characterized in that: include: current collector, active material layer, first insulating layer and second insulating layer, The current collector includes a main body and a tab, wherein the tab extends from a first end of the main body, wherein the first end is an end of the main body along a first direction, and the main body includes a coating area and a transition area, wherein the transition area is disposed between the coating area and the tab; The active material layer is disposed on the surface of the coating area; The first insulating layer is disposed on an end surface of the main body at the first end; At least a portion of the second insulating layer is disposed on the surface of the transition zone, and the second insulating layer comprises a thermoplastic polymer, wherein the volume particle size distribution D of the thermoplastic polymer is V 50 is 6 μm to 10 μm, and the maximum particle size D of the thermoplastic polymer is max It is 90μm~110μm.

2. The pole piece according to claim 1, characterized in that: The volume particle size distribution D of the thermoplastic polymer V 50 is 7 μm to 8 μm, and the maximum particle size D of the thermoplastic polymer is max It is 90μm~100μm.

3. The pole piece according to claim 1 or 2, characterized in that: The thickness d2 of the second insulating layer is 22 μm to 48 μm.

4. The pole piece according to any one of claims 1 to 3, characterized in that: The thickness d1 of the first insulating layer is 300 nm to 1800 nm.

5. The pole piece according to any one of claims 1 to 4, characterized in that: The thermoplastic polymer has a drop melting point of 80°C to 250°C.

6. The pole piece according to any one of claims 1 to 5, characterized in that: The material of the thermoplastic polymer includes: at least one of a crystalline thermoplastic polymer and an amorphous thermoplastic polymer; the crystalline thermoplastic polymer includes: at least one of polyethylene, polypropylene, and polyamide; the amorphous thermoplastic polymer includes: at least one of microcrystalline wax, polystyrene, and polymethyl methacrylate.

7. The pole piece according to any one of claims 1 to 6, characterized in that: The second insulating layer further includes an adhesive.

8. The pole piece according to claim 7, characterized in that: In the second insulating layer, a mass ratio A:B of the thermoplastic polymer to the binder is 60:40 to 80:

20.

9. The pole piece according to any one of claims 1 to 8, characterized in that: The resistance R of the end surface provided with the first insulating layer satisfies: R≥100Ω.

10. The pole piece according to any one of claims 1 to 9, characterized in that: The second insulating layer includes a first portion and a second portion, wherein the first portion is disposed on the surface of the transition region, and the second portion extends from the first portion along the first direction and is disposed on a portion of the surface of the tab.

11. The pole piece according to claim 10, characterized in that: Along a second direction, the first insulating layer is disposed on end surfaces of both ends of a region of the electrode tab where the second portion is disposed, and the second direction is different from the first direction.

12. The pole piece according to any one of claims 1 to 11, characterized in that: The material of the first insulating layer is the same as the material of the thermoplastic polymer in the second insulating layer.

13. The pole piece according to any one of claims 1 to 12, characterized in that: The thermoplastic polymer in the first insulating layer is in the form of a film layer, and the thermoplastic polymer in the second insulating layer includes a film layer-shaped thermoplastic polymer and a particle-shaped thermoplastic polymer.

14. The pole piece according to any one of claims 1 to 13, characterized in that: The current collector includes aluminum foil.

15. The pole piece according to any one of claims 1 to 14, characterized in that: The first insulating layer is further disposed on an end surface of the main body at a second end, and the second end is opposite to the first end along the first direction.

16. A method for preparing a pole piece, characterized in that: include: providing a current collector; coating an active material on the first region of the current collector to form an active material layer; An insulating slurry is coated on the second region of the current collector to form a second insulating layer, wherein the insulating slurry includes a thermoplastic polymer and a binder, and the volume particle size distribution D of the thermoplastic polymer is V 50 is 6 μm to 10 μm, and the maximum particle size D of the thermoplastic polymer is max 90μm~110μm; The current collector provided with the second insulating layer is cut along a cutting line, and at least a portion of the cutting line is provided in the second region.

17. The method according to claim 16, characterized in that The volume particle size distribution D of the thermoplastic polymer V 50 is 7 μm to 8 μm, and the maximum particle size D of the thermoplastic polymer is max It is 90μm~100μm.

18. The method according to claim 16 or 17, characterized in that The thickness d2 of the second insulating layer is 22 μm to 48 μm.

19. The method according to any one of claims 16 to 18, characterized in that: The thermoplastic polymer has a drop melting point of 80°C to 250°C.

20. The method according to any one of claims 16 to 19, characterized in that The material of the thermoplastic polymer includes: at least one of a crystalline thermoplastic polymer and an amorphous thermoplastic polymer; the crystalline thermoplastic polymer includes: at least one of polyethylene, polypropylene, and polyamide; the amorphous thermoplastic polymer includes: at least one of microcrystalline wax, polystyrene, and polymethyl methacrylate.

21. The method according to any one of claims 16 to 20, characterized in that In the insulating paste, the mass ratio A:B of the thermoplastic polymer to the binder is 60:40 to 80:

20.

22. The method according to any one of claims 16 to 21, characterized in that The method of cutting the current collector provided with the second insulating layer along the cutting line comprises: The laser processing tool is controlled to cut the current collector provided with the second insulating layer along the cutting line.

23. A battery cell, characterized in that: It comprises a pole piece as described in any one of claims 1 to 15, and / or a pole piece prepared by the method as described in any one of claims 16 to 22.

24. A battery, characterized in that: Comprising the battery cell as claimed in claim 23.

25. An electrical device, characterized in that: Comprising a battery as claimed in claim 24.

Citation Information

Patent Citations

  • Pole piece and secondary battery with same

    CN114122327A

  • Pole piece for winding type multi-lug battery cell and winding type multi-lug battery cell

    CN212365995U

  • Powder compositions, method of preparing articles and coatings from the powder compositions, and articles prepared therefrom

    US20180244862A1

  • Polymer powder compositions containing tetrafluoroethylene polymers

    US4767821A