Electrode sheet and manufacturing method therefor, battery cell, battery, and electric device
By setting a first insulating layer on the exposed end face and burrs after the electrode is cut, and forming a second insulating layer using a thermoplastic polymer in the transition zone, the overlapping problem caused by burrs and exposed end faces during the electrode cutting process is solved, thereby improving the reliability and safety of the battery cell.
Patent Information
- Application Number
- PCT/CN2024/092630
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-22
- Filing Date
- 2024-05-11
- Publication Date
- 2024-11-28
AI Technical Summary
In existing battery cells, burrs and exposed end faces are easily generated during the cutting process of the electrode sheets, which leads to the overlap of electrodes with opposite polarity, affecting the reliability and safety of the battery.
A first insulating layer with a thickness of 200nm to 2000nm is provided on the exposed end face and burr area after the electrode is cut, and a second insulating layer containing thermoplastic polymer is provided in the transition area. The thermoplastic polymer flows to the end face and burr area during the cutting process to form a coating, reducing the risk of overlap.
It effectively reduces the risk of overlap between the electrode and the electrode with opposite polarity, improves the reliability and safety of the battery cell, and does not affect the volumetric energy density of the battery while ensuring that the insulation layer thickness is small.
Smart Images

Figure CN2024092630_28112024_PF_FP_ABST
Abstract
Description
Pole piece and preparation method thereof, battery cell, battery, and electrical device
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to patent application 202310579255.7, filed on May 22, 2023, entitled “Pole piece and preparation method thereof, battery cell, battery, and electrical device,” and the entire contents of that application are incorporated herein by reference. Technical Field
[0003] The present application relates to the field of battery technology, and in particular to a pole piece and a preparation method thereof, a battery cell, a battery, and an electrical device. Background Art
[0004] With the increasing severity of environmental pollution, the new energy industry has attracted more and more attention. In the new energy industry, battery technology is an important factor in its development.
[0005] The development of battery technology requires consideration of multiple design factors, such as energy density, cycle life, and reliability. The design of the pole piece in a battery cell is crucial to its reliability. Therefore, how to provide a pole piece to improve the reliability of the battery cell is a technical problem that needs to be solved urgently.
[0006] Summary of the Invention
[0007] The present application is made in view of the above-mentioned problems, and its purpose is to provide a pole piece to improve the reliability of a battery cell.
[0008] In order to achieve the above-mentioned objectives, the present application provides a pole piece and a preparation method thereof, a battery cell, a battery, and an electrical device.
[0009] In a first aspect, a pole piece is provided, comprising a current collector, an active material layer and a first insulating layer, the current collector comprising a main body and a pole tab, the pole tab extending from a first end of the main body, the first end being an end of the main body along the first direction, the main body comprising a coating area; the active material layer is arranged on the surface of the coating area; the first insulating layer is arranged on the end face of the main body at the first end, and the thickness d1 of the first insulating layer is 200nm to 2000nm.
[0010] An embodiment of the present application provides a pole piece, which includes a current collector, an active material layer, and a first insulating layer. The current collector includes a main body and a tab, the tab extending from a first end of the main body, and the first end of the main body is an end of the main body along a first direction. The main body includes a coating area, and the active material layer is disposed on the surface of the coating area. The first insulating layer is disposed on the end face of the main body at the first end. In this way, the first insulating layer can cover the end face of the first end, reducing the risk of the current collector at the end face being exposed, thereby reducing the risk of the exposed current collector at the end face overlapping with an electrode of opposite polarity; in addition, the first insulating layer can also cover burrs generated by the cutting process, reducing the risk of the burrs overlapping with an electrode of opposite polarity. The thickness d1 of the first insulating layer is 200nm to 2000nm. In this way, the first insulating layer can better cover burrs and exposed end faces while having a relatively small thickness. Therefore, the technical solution of the embodiment of the present application can improve the reliability of the battery cell.
[0011] In a possible implementation, the thickness d1 of the first insulating layer is 200 nm to 500 nm, which is beneficial for better covering burrs and exposed end faces while further reducing the thickness of the first insulating layer.
[0012] In one possible implementation, the main body also includes a transition zone, which is arranged between the coating zone and the pole lug; the pole piece also includes a second insulating layer, at least a portion of the second insulating layer is arranged on the surface of the transition zone, and the material of the second insulating layer includes a thermoplastic polymer.
[0013] In the above technical solution, the transition zone is arranged between the coating zone and the pole ear. In the process of cutting the pole ear, the cutting tool (such as a laser) can be at a certain distance from the active material layer, which can reduce the shedding of the active material layer. A second insulating layer is provided on the surface of the transition zone, which is conducive to reducing the risk of the pole piece overlapping with the pole piece of opposite polarity. The material of the second insulating layer includes a thermoplastic polymer. When the thermoplastic polymer is heated to certain conditions, it will change from a solid state to a fluid state. In this way, in the process of cutting the current collector provided with the second insulating layer, the fluid thermoplastic polymer can flow to the burrs and the exposed end faces. After the temperature drops, the fluid thermoplastic polymer solidifies at the burrs and the exposed end faces to cover the burrs and the exposed end faces, thereby reducing the risk of the burrs and the exposed end faces overlapping with the electrodes of opposite polarity.
[0014] In a possible implementation, the thickness d2 of the second insulating layer is 20 μm to 50 μm; optionally, the thickness d2 of the second insulating layer is 20 μm to 30 μm.
[0015] In the above technical solution, when the thickness d2 of the second insulating layer is no less than 20 μm, during the cutting process of the current collector provided with the second insulating layer, the second insulating layer contains a large amount of thermoplastic polymer, so that more thermoplastic polymer can flow to the burrs and the exposed end surface of the current collector after being heated, which is conducive to uniformly and densely covering the exposed end surface and burrs. When the thickness d2 of the second insulating layer does not exceed 50 μm, it is conducive to reducing the energy consumed during the cutting process and the burrs generated during the cutting process. Optionally, the thickness d2 of the second insulating layer is 20 μm to 30 μm, which can reduce the energy consumed during the cutting process and reduce the burrs generated during the cutting process while improving the covering effect on the exposed end surface and burrs.
[0016] In one possible implementation, the thermoplastic polymer has a drop melting point of 80°C to 200°C. Thus, during the process of cutting the current collector provided with the second insulating layer, the heat generated by the cutting causes the thermoplastic polymer to change from a solid state to a fluid state. The fluid thermoplastic polymer can flow to the exposed end faces of the current collector after cutting and to the burrs generated by the cutting, thereby facilitating the preparation of the first insulating layer. Alternatively, the thermoplastic polymer has a drop melting point of 150°C to 200°C. This can reduce the risk of the thermoplastic polymer becoming fluid due to other factors while the current collector is not being cut.
[0017] In one possible implementation, the material of the thermoplastic polymer includes: at least one of a crystalline thermoplastic polymer and an amorphous thermoplastic polymer; optionally, the crystalline thermoplastic polymer includes: at least one of polyethylene, polypropylene, and polyamide; optionally, the amorphous thermoplastic polymer includes: at least one of microcrystalline wax, polystyrene, and polymethyl methacrylate.
[0018] In the above technical solution, the use of the above thermoplastic polymer is conducive to forming a uniform and dense coating on the end surface and burrs of the exposed current collector after cutting.
[0019] In a possible implementation, the second insulating layer further includes an adhesive, which facilitates the thermoplastic polymer to adhere to the transition zone, thereby reducing the risk of the second insulating layer falling off from the transition zone.
[0020] In a possible implementation, in the second insulating layer, the mass ratio of the thermoplastic polymer to the binder A:B is 60:40 to 80:20; optionally, in the second insulating layer, the mass ratio of the thermoplastic polymer to the binder A:B is 70:30 to 80:20.
[0021] In the above technical solution, by reasonably setting the mass ratio of the thermoplastic polymer and the binder in the second insulating layer, it is beneficial to reduce the risk of the second insulating layer falling off, and at the same time it is beneficial to form a uniform and dense first insulating layer on the end face and burrs of the exposed current collector.
[0022] In one possible implementation, the second insulating layer includes a first portion and a second portion, wherein the first portion is disposed on the surface of the transition region, and the second portion extends from the first portion along the first direction and is disposed on a portion of the surface of the tab. This reduces the risk of the tab overlapping an electrode of opposite polarity.
[0023] In one possible implementation, the first insulating layer is provided on the end surfaces of the tab at both ends of the region where the second portion is provided, along a second direction different from the first direction; optionally, the second direction is perpendicular to the first direction. In this way, the first insulating layer can cover the end surfaces of the tab exposed by cutting, thereby reducing the risk of overlapping the end surfaces with electrodes of opposite polarity.
[0024] In a possible implementation, the material of the first insulating layer is the same as the material of the thermoplastic polymer in the second insulating layer. This helps to simplify the preparation steps of the pole piece and speed up the production process.
[0025] In one possible implementation, the thermoplastic polymer in the first insulating layer is in film form, and the thermoplastic polymer in the second insulating layer includes both film-formed and granular thermoplastic polymers. Thus, the first insulating layer is formed by melting and solidifying the thermoplastic polymer in the second insulating layer. This simplifies the electrode sheet fabrication process, allowing the first insulating layer to be formed simultaneously with cutting.
[0026] In one possible implementation, the current collector comprises a metal foil or a composite current collector; optionally, the metal foil comprises aluminum foil or copper foil; optionally, the composite current collector comprises: a polymer material base layer and a metal layer located on at least one surface of the polymer material base layer; optionally, the current collector comprises aluminum foil. This facilitates selection of a suitable current collector according to actual needs. In the case where the current collector comprises aluminum foil, the electrode is a positive electrode electrode, which helps reduce the risk of overlap between the positive electrode electrode and the negative electrode electrode, and helps improve the reliability of the battery cell. In addition, it also helps reduce the risk of overlap between the positive electrode electrode and the negative electrode electrode.
[0027] In one possible implementation, the first insulating layer is further provided on the end surface of the main body at the second end, the second end being opposite the first end along the first direction. Thus, both the end surface of the main body at the first end and the end surface of the main body at the second end are provided with the first insulating layer, which further reduces the risk of short circuits in the battery cells.
[0028] In a second aspect, a method for preparing a pole piece is provided, comprising: providing a current collector; coating an active material on a first region of the current collector to form an active material layer in the first region; coating an insulating slurry on a second region of the current collector to form a second insulating layer in the second region, wherein the insulating slurry comprises a thermoplastic polymer and a binder, and the thickness d2 of the second insulating layer is 20 μm to 50 μm; and cutting the current collector provided with the second insulating layer along a cutting line, wherein at least part of the cutting line is provided in the second region.
[0029] In the above technical solution, by providing the second insulating layer, the first insulating layer can be formed at the same time as cutting, which is conducive to simplifying the preparation steps of the first insulating layer.
[0030] In a possible implementation, the thickness d2 of the second insulating layer is 20 μm to 30 μm.
[0031] In a possible implementation, the thermoplastic polymer has a drop melting point of 80°C to 200°C.
[0032] In one possible implementation, the material of the thermoplastic polymer includes: at least one of a crystalline thermoplastic polymer and an amorphous thermoplastic polymer; optionally, the crystalline thermoplastic polymer includes: at least one of polyethylene, polypropylene, and polyamide; optionally, the amorphous thermoplastic polymer includes: at least one of microcrystalline wax, polystyrene, and polymethyl methacrylate.
[0033] In a possible implementation, in the insulating paste, the mass ratio of the thermoplastic polymer to the binder A:B is 60:40 to 80:20; optionally, in the insulating paste, the mass ratio of the thermoplastic polymer to the binder A:B is 70:30 to 80:20.
[0034] In one possible implementation, cutting the current collector provided with the second insulating layer along the cutting line includes: controlling a laser processing tool to cut the current collector provided with the second insulating layer along the cutting line, wherein the power of the laser processing tool is 20 to 200 W, the frequency is 100 to 800 kHz, and the feed speed is 5 m / min to 30 m / min; optionally, the power of the laser processing tool is 20 to 100 W, the frequency is 100 to 300 kHz, and the feed speed is 5 m / min to 15 m / min.
[0035] In the above technical solution, reasonable control of the use parameters of the laser processing tool is conducive to obtaining a more uniform and dense first insulating layer, reducing burrs generated during the cutting process, and reducing the risk of the second insulating layer falling off.
[0036] In a third aspect, a battery cell is provided, comprising the electrode according to the first aspect and any possible implementation thereof, and / or the electrode prepared by the method according to the second aspect and any possible implementation thereof.
[0037] In a fourth aspect, a battery is provided, comprising the battery cell described in the third aspect.
[0038] In a fifth aspect, an electrical device is provided, comprising the battery described in the fourth aspect.
[0039] In a sixth aspect, a pole piece is provided, comprising: a current collector and a first insulating layer, wherein the first insulating layer is disposed on at least a portion of an end surface of the current collector, and a thickness d1 of the first insulating layer is between 200 nm and 2000 nm. Providing the first insulating layer on at least a portion of the end surface of the current collector reduces the risk of short circuits caused by the end surface and burrs overlapping with electrodes of opposite polarity. By setting d1 to between 200 nm and 2000 nm, the first insulating layer can better cover at least a portion of the end surface while maintaining a relatively small thickness. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the following is a brief introduction to the drawings required for use in the embodiments of the present application. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on the drawings without creative work.
[0041] FIG1 is a schematic diagram of a pole piece before processing a pole lug according to an embodiment of the present application;
[0042] FIG2 is a schematic diagram of a pole piece according to an embodiment of the present application;
[0043] FIG3 is a cross-sectional view along the AA direction in FIG2 ;
[0044] FIG4 is a cross-sectional view along the BB direction in FIG2 ;
[0045] FIG5 is a schematic diagram of a method for preparing a pole piece according to an embodiment of the present application;
[0046] FIG6 is a schematic diagram of a current collector according to an embodiment of the present application;
[0047] FIG7 is a schematic diagram of a current collector coated with an active material layer according to an embodiment of the present application;
[0048] FIG8 is a schematic diagram of a current collector coated with a second insulating layer according to an embodiment of the present application;
[0049] FIG9 is a schematic diagram of a current collector showing a cutting line according to an embodiment of the present application;
[0050] FIG10 is a schematic diagram of a battery cell according to an embodiment of the present application;
[0051] FIG11 is a schematic diagram of a battery according to an embodiment of the present application;
[0052] FIG12 is a schematic diagram of an electrical device according to an embodiment of the present application;
[0053] FIG13 is a SEM image of an end surface provided with a first insulating layer according to an embodiment of the present application;
[0054] FIG14 is a schematic diagram of a pole piece according to another embodiment of the present application;
[0055] FIG15 is a cross-sectional view taken along the AA direction of FIG14;
[0056] FIG16 is a cross-sectional view taken along the CC direction of FIG14 .
[0057] Reference numerals: 1: pole piece; 124: cutting line; 10: current collector; 11: active material layer; 121: first insulating layer; 122: second insulating layer; 101: main body; 102: tab; 1011: coating area; 1012: transition area; 1221: first part; 1222: second part. DETAILED DESCRIPTION
[0058] The embodiments of the electrode and its preparation method, battery cell, battery, and electrical device of the present application are specifically disclosed in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there may be cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0059] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0060] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0061] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0062] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0063] If not otherwise specified, the “include” and “comprising” mentioned in this application represent open-endedness. For example, the “include” and “comprising” may mean including or comprising other components not listed.
[0064] Unless otherwise specified, the term "or" is inclusive in this application. For example, the phrase "A and / or B" means "A, B, or both A and B." More specifically, the condition "A and / or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0065] The development of battery technology must consider multiple design factors simultaneously, such as energy density, cycle life, discharge capacity, charge and discharge rate, reliability, etc. The design of the pole piece in the battery cell is crucial to the reliability of the battery cell. The pole piece usually includes a current collector and an active material layer and an insulating layer coated on different areas of the current collector. After the corresponding active material layer and insulating layer are coated on the current collector, the current collector coated with the active material layer and the insulating layer needs to be cut to cut out the pole lugs. During the cutting process, dust and burrs are easily generated, and the burrs may cause the pole piece to overlap with the electrode of opposite polarity, thereby causing a short circuit.
[0066] In some processing methods, the insulating layer coated on the current collector is set as a ceramic coating to reduce the burrs that appear during the cutting process. However, this processing method can only reduce the number of burrs. Burrs will still exist after cutting. Burrs may cause the pole piece to overlap with an electrode of opposite polarity, resulting in adverse effects. In addition, after cutting, the end face of the current collector is exposed. The exposed end face has the risk of overlapping with an electrode of opposite polarity, which may cause a short circuit in the battery cell and is not conducive to improving the reliability of the battery.
[0067] In view of this, the present application provides a pole piece, which includes a current collector and an active material layer arranged on the current collector. The exposed end surface of the current collector after cutting is provided with a first insulating layer, and the thickness of the first insulating layer is 200nm to 2000nm. In this way, through the provision of the first insulating layer, the first insulating layer can cover the exposed end surface of the current collector after cutting and the burrs after cutting, reduce the overlap of the pole piece with the electrode of opposite polarity, reduce the risk of internal short circuit, and thus improve the reliability of the battery cell. The thickness of the first insulating layer is 200nm to 2000nm. In this way, the first insulating layer can better cover the burrs and exposed end surface while having a smaller thickness, thereby further improving the performance of the battery cell.
[0068] [Pole piece]
[0069] Figure 1 is a schematic diagram of a pole piece before processing the pole lug according to an embodiment of the present application, Figure 2 is a schematic diagram of a pole piece according to an embodiment of the present application, Figure 3 is a cross-sectional view along the AA direction in Figure 2, and Figure 4 is a cross-sectional view along the BB direction in Figure 2.
[0070] As shown in Figures 1 and 2, Figure 1 is a schematic diagram of the electrode before the tab is processed, and Figure 2 is a schematic diagram of the electrode after the tab is processed. As shown in Figure 1, the black dotted line 124 is the cutting line for cutting the tab. After cutting along the cutting line 124, the electrode 1 shown in Figure 2 is obtained.
[0071] 1 to 4 , the electrode 1 includes a current collector 10 and an active material layer 11 .
[0072] The current collector 10 has two surfaces facing each other along its thickness direction, and the active material layer 11 can be provided on at least one of the two surfaces facing each other along the thickness direction of the current collector 10. For example, as shown in Figures 3 and 4, the active material layer 11 is provided on both surfaces facing each other along the thickness direction of the current collector 10.
[0073] The thickness direction of the current collector 10 may be the z direction as shown in FIG. 3 and FIG. 4 .
[0074] The current collector 10 includes a main body 101 and a tab 102 , wherein the tab 102 extends from a first end of the main body 101 . The first end of the main body 101 is one end of the main body 101 along a first direction.
[0075] The first direction is parallel to the plane where the current collector 10 is located, and the first direction is the direction in which the tab 102 protrudes relative to the main body 101. For example, the first direction is the y direction in FIG2 .
[0076] The main body 101 includes a coating region 1011, and the active material layer 11 is disposed on a surface of the coating region 1011. For example, as shown in Figures 3 and 4, the active material layer 11 is disposed on both surfaces of the current collector 10 in the thickness direction. In some embodiments, the active material layer 11 can be disposed on one of the two surfaces of the current collector 10 in the thickness direction.
[0077] The first insulating layer 121 is disposed on the end surface 1011a at the first end of the main body 101. The thickness d1 of the first insulating layer 121 is 200 nm to 2000 nm. For example, d1 can be 200 nm, 300 nm, 400 nm, 500 nm, 800 nm, 1000 nm, 1500 nm, 2000 nm, or any value within the above range.
[0078] An end surface 1011a of the main body 101 at the first end is a surface parallel to the thickness direction of the current collector 10. For example, as shown in FIG3 , the end surface 1011a is a surface parallel to the x-direction and the z-direction.
[0079] The end surface 1011a at the first end of the main body 101 can be formed by the following process: Referring to FIG. 1 , during the cutting process of the current collector 10, the current collector is cut along the cutting line 124. The end surface 1011a is the cut end surface of the transition region 1012. After cutting, the current collector at the end surface 1011a is exposed, and burrs may be generated.
[0080] By providing a first insulating layer 121 at the end surface 1011a, the first insulating layer 121 can cover the burrs generated during the cutting process, thereby reducing the risk of the burrs overlapping with electrodes of opposite polarity. For example, after the electrode sheet 1 is assembled into an electrode assembly with a electrode sheet of opposite polarity (for example, the electrode sheet 1 is a positive electrode sheet and the electrode sheet of opposite polarity is a negative electrode sheet) by winding or laminating, and the electrode assembly is assembled with the end cover assembly and the shell into a battery cell, the burr may overlap with the electrode sheet of opposite polarity, thereby possibly causing abnormal self-discharge of the battery cell. By providing the first insulating layer 121, the first insulating layer 121 can cover the burrs, thereby reducing the risk of self-discharge abnormalities caused by the burrs overlapping with electrodes of opposite polarity.
[0081] By providing the first insulating layer 121 on the end surface 1011a, the first insulating layer 121 can cover the exposed end surface 1011a of the trimmed current collector 10, thereby reducing the risk of the end surface 1011a overlapping with an electrode of opposite polarity. For example, if the electrode piece 1 is a positive electrode piece, the provision of the first insulating layer 121 can reduce the risk of internal short circuits in the battery cell caused by overlapping between the electrode piece 1 and the negative electrode piece.
[0082] The smaller the thickness d1 of the first insulating layer 121, the smaller the space occupied by the pole piece 1, which is beneficial for improving the volumetric energy density of the battery cell. By setting the thickness d1 of the first insulating layer 121 to 200nm to 2000nm, the first insulating layer 121 can effectively cover burrs and exposed end surfaces 1011a while maintaining a relatively small thickness, thereby further improving the performance of the battery cell.
[0083] The thickness d1 of the first insulating layer 121 is the average thickness of the first insulating layer 121 along the thickness direction of the current collector 10. For example, the thickness d1 is the average of the maximum and minimum dimensions of the first insulating layer 121 along the thickness direction.
[0084] The thickness d1 of the first insulating layer 121 can be measured in the following manner: photographing the end surface 1011 a of the pole piece 1 using a scanning electron microscope (SEM), and measuring the thickness d1 of the first insulating layer 121 based on the obtained image.
[0085] An embodiment of the present application provides a pole piece 1, comprising a current collector 10, an active material layer 11, and a first insulating layer 121. The current collector 10 comprises a main body 101 and a tab 102, wherein the tab 102 extends from a first end of the main body 101, the first end of the main body 101 being an end of the main body 101 along a first direction. The main body 101 comprises a coating region 1011, and the active material layer 11 is disposed on a surface of the coating region 1011. The first insulating layer 121 is disposed on an end surface 1011a of the main body 101 at the first end. Thus, the first insulating layer 121 can cover the end surface 1011a of the first end, reducing the risk of the current collector 10 being exposed at the end surface 1011a, thereby reducing the risk of the exposed current collector 10 at the end surface 1011a contacting an electrode of opposite polarity. Furthermore, the first insulating layer 121 can also cover burrs generated during the cutting process, reducing the risk of the burrs contacting an electrode of opposite polarity. The thickness d1 of the first insulating layer 121 is 200 nm to 2000 nm. Thus, the first insulating layer 121 can better cover the burrs and the exposed end surface 1011 a while having a relatively small thickness. Therefore, the technical solution of the embodiment of the present application can improve the reliability of the battery cell.
[0086] In some embodiments, the thickness d1 of the first insulating layer 121 is 200 nm to 500 nm, which is beneficial for further reducing the thickness of the first insulating layer 121 while better covering the burrs and the exposed end surface 1011 a.
[0087] In some embodiments, the main body 101 also includes a transition zone 1012, which is arranged between the coating zone 1011 and the pole ear 102; the pole piece 1 also includes a second insulating layer 122, at least part of which is arranged on the surface of the transition zone 1012, and the material of the second insulating layer 122 includes a thermoplastic polymer.
[0088] The transition region 1012 is disposed between the coating region 1011 and the tab 102 . Thus, during the process of cutting the tab 102 , the cutting tool (eg, laser) can be kept at a certain distance from the active material layer 11 , thereby reducing the shedding of the active material layer 11 .
[0089] At least a portion of the second insulating layer 122 is disposed on the surface of the transition region 1012 , meaning that the second insulating layer 122 may be disposed not only on the surface of the transition region 1012 but also in other regions not coated with the active material layer 11 . For example, the second insulating layer 122 may also be disposed in a portion of the tab 102 .
[0090] A thermoplastic polymer may be a polymer that softens when heated, solidifies when cooled, and can soften again. For example, when heated to a certain temperature, a thermoplastic polymer changes from solid particles to a flowable state, and when cooled, it can change into a layer or film.
[0091] A second insulating layer 122 is provided on the surface of the transition region 1012 , which helps to reduce the risk of the pole piece 1 overlapping with a pole piece 1 of opposite polarity.
[0092] When the thermoplastic polymer in the second insulating layer 122 is heated to certain conditions, it will change from a solid state to a fluid state. In this way, during the cutting process of the current collector 10 provided with the second insulating layer 122, the fluid thermoplastic polymer can flow to the burrs and the exposed end surface 1011a. After the temperature drops, the fluid thermoplastic polymer solidifies at the burrs and the exposed end surface 1011a, thereby covering the burrs and the exposed end surface 1011a, thereby reducing the risk of the burrs and the exposed end surface 1011a overlapping with electrodes of opposite polarity.
[0093] In some embodiments, the thickness d2 of the second insulating layer 122 is 20 μm to 50 μm. For example, d2 is 20 μm, 25 μm, 30 μm, 40 μm, 45 μm, 50 μm, or any value within the above range.
[0094] When the thickness d2 of the second insulating layer 122 is not less than 20 μm, during the process of cutting the current collector 10 provided with the second insulating layer 122, there is more thermoplastic polymer in the second insulating layer 122, so that more thermoplastic polymer can flow to the burrs and the exposed end surface 1011a of the current collector 10 after being heated, which is conducive to uniformly and densely covering the exposed end surface 1011a and the burrs.
[0095] When the thickness d2 of the second insulating layer 122 does not exceed 50 μm, it is beneficial to reduce the energy consumed in the cutting process and to reduce the burrs generated in the cutting process.
[0096] Optionally, the thickness d2 of the second insulating layer 122 is 20 μm to 30 μm, which can reduce the energy consumed in cutting and the burrs generated by cutting, while improving the covering effect on the exposed end surface 1011 a and the burrs.
[0097] In some embodiments, the thermoplastic polymer has a drop melting point of 80° C. to 200° C. For example, the thermoplastic polymer has a drop melting point of 80° C., 100° C., 150° C., 200° C., or any value within the above ranges.
[0098] The drop melting point of the thermoplastic polymer is not less than 80°C, thereby reducing the risk of the thermoplastic polymer melting or flowing due to heating of the pole piece 1 during other processing. The drop melting point of the thermoplastic polymer is not more than 200°C, thereby reducing the risk of the thermoplastic polymer not being able to transform into a fluid state during the cutting process, thereby reducing the risk of not being able to form the first insulating layer 121 on the end surface 1011a.
[0099] The drop melting point of a thermoplastic polymer is the temperature at which the thermoplastic polymer changes from a solid or semi-solid state to a liquid state.
[0100] During the process of cutting the current collector 10 provided with the second insulating layer 122, under the action of the heat generated by the cutting, the thermoplastic polymer changes from a solid state to a fluid state. The fluid thermoplastic polymer can flow to the end surface 1011a of the current collector 10 exposed after cutting and the burrs generated by the cutting, thereby facilitating the preparation of the first insulating layer 121.
[0101] Optionally, the drop melting point of the thermoplastic polymer is 150° C. to 200° C., so that the risk of the thermoplastic polymer becoming a fluid state due to other factors during the process of not cutting the current collector 10 can be reduced.
[0102] In some embodiments, the material of the thermoplastic polymer includes: at least one of a crystalline thermoplastic polymer and an amorphous thermoplastic polymer; optionally, the crystalline thermoplastic polymer includes: at least one of polyethylene, polypropylene, and polyamide; optionally, the amorphous thermoplastic polymer includes: at least one of microcrystalline wax, polystyrene, and polymethyl methacrylate.
[0103] The drop melting point of a crystalline thermoplastic polymer may refer to the melting point of the crystalline thermoplastic polymer. The drop melting point of an amorphous thermoplastic polymer may refer to the glass transition temperature of the amorphous thermoplastic polymer.
[0104] In the above technical solution, the use of the aforementioned thermoplastic polymer facilitates forming a uniform and dense coating on the exposed end face 1011a and burrs of the cut current collector 10. Furthermore, the aforementioned thermoplastic polymer has high insulation and pressure resistance. When the electrode 1 is immersed in the electrolyte, the thermoplastic polymer does not undergo an electrochemical reaction with the electrolyte.
[0105] In some embodiments, the second insulating layer 122 further includes a binder. The provision of the binder in the second insulating layer 122 facilitates coating the corresponding slurry on the current collector 10 to form the second insulating layer 122, facilitates bonding of the thermoplastic polymer to the current collector 10 or the transition region 1012, and reduces the risk of the second insulating layer 122 falling off the current collector 10 or the transition region 1012.
[0106] In some embodiments, in the second insulating layer 122 , the mass ratio of the thermoplastic polymer to the binder A:B is 60:40 to 80:20, for example, A:B is 60:40, 70:30, 75:25, 80:20, or any value within the above range.
[0107] In the above technical solution, by reasonably setting the mass ratio of the thermoplastic polymer and the binder in the second insulating layer 122, it is beneficial to reduce the risk of the second insulating layer 122 falling off, and at the same time it is beneficial to form a uniform and dense first insulating layer 121 on the end surface 1011a of the exposed current collector 10 and the burrs.
[0108] Optionally, in the second insulating layer 122 , the mass ratio of the thermoplastic polymer to the binder A:B is 70:30 to 80:20.
[0109] In some embodiments, the second insulating layer 122 includes a first portion 1221 and a second portion 1222. The first portion 1221 is disposed on the surface of the transition region 1012, and the second portion 1222 extends from the first portion 1221 along a first direction and is disposed on a portion of the surface of the tab 102. In this way, the risk of the tab 102 overlapping with an electrode of opposite polarity can be reduced.
[0110] In some embodiments, along a second direction, the first insulating layer 121 is provided on end surfaces 1222 a at both ends of the region of the tab 102 where the second portion 1222 is provided. The second direction is different from the first direction.
[0111] In the case where the pole piece 1 includes a plurality of pole tabs 102, the second direction may be the arrangement direction of the plurality of pole tabs 102. For example, as shown in FIG2 , the second direction is the x direction.
[0112] When cutting the current collector 10 along the cutting line 124 to prepare the tab 102, the cutting tool passes through the area of the second portion 1222. After cutting, the end surface 1222a of this area along the second direction is exposed. By providing the first insulating layer 121 on this end surface 1222a, the risk of the end surface 1222a overlapping with the electrode of opposite polarity can be reduced.
[0113] Optionally, the first insulating layer 121 provided on the end surfaces 1222 a at both ends of the region of the second portion 1222 is formed during the process of cutting the current collector 10 .
[0114] Optionally, the second direction is perpendicular to the first direction, so as to facilitate cutting of the tab 102 .
[0115] In some embodiments, the material of the first insulating layer 121 is the same as the material of the thermoplastic polymer in the second insulating layer 122. This helps to simplify the preparation steps of the pole piece 1 and speed up the production process.
[0116] For example, the current collector 10 coated with the active material layer 11 can be cut first, and then a hot melt tool (such as a hot melt gun) can be used to form the first insulating layer 121 at the end surface 1011a and the second insulating layer 122 can be formed in the transition region 1012 and a portion of the tab 102. In this way, the first insulating layer 121 and the second insulating layer 122 can be simultaneously formed in one step.
[0117] For another example, the active material layer 11 and the second insulating layer 122 are first prepared on the current collector 10, and the first insulating layer 121 is simultaneously prepared during the cutting process. In this way, the tab 102 can be cut and the first insulating layer 121 can be prepared simultaneously in one step.
[0118] In some embodiments, the thermoplastic polymer in the first insulating layer 121 is in the form of a film, and the thermoplastic polymer in the second insulating layer 122 includes both a film-like thermoplastic polymer and a granular thermoplastic polymer. Thus, the first insulating layer 121 is formed by melting and solidifying the thermoplastic polymer in the second insulating layer 122. Once the thermoplastic polymer in the second insulating layer 122 becomes fluid, it flows to the end face 1011a and solidifies there to form the first insulating layer 121. This simplifies the preparation steps of the electrode 1, allowing the first insulating layer 121 to be formed simultaneously with the cutting and preparation of the electrode tab 102.
[0119] In the second insulating layer 122 , at least a portion of the granular thermoplastic polymer remains; in the first insulating layer 121 , the thermoplastic polymer is in a film-like state and has almost no granular shape.
[0120] The granular thermoplastic polymer may have various shapes, such as spheres, rods, and sheets. The granular thermoplastic polymer herein means that the thermoplastic polymer has not become a fluid state and is in a solid state.
[0121] Before cutting the second insulating layer 122, the thermoplastic polymer in the second insulating layer 122 is in a granular form. During the cutting process, some of the thermoplastic polymer in the second insulating layer 122 changes from a solid state to a fluid state (for example, the thermoplastic polymer near the cutting line 124 changes to a fluid state), while the remaining portion of the thermoplastic polymer remains in a solid granular form.
[0122] In some embodiments, the current collector 10 includes a metal foil or a composite current collector, so that the material of the current collector 10 can be easily configured according to actual needs.
[0123] Optionally, the metal foil includes aluminum foil or copper foil.
[0124] Optionally, the composite current collector includes: a polymer material base layer and a metal layer located on at least one surface of the polymer material base layer.
[0125] Optionally, the current collector comprises aluminum foil. In this case, the electrode sheet 1 is a positive electrode sheet, which helps reduce the risk of overlap between the positive electrode sheet and the negative electrode sheet, thereby improving the reliability of the battery cell. Furthermore, it helps reduce the risk of overlap between the positive electrode sheet and the negative electrode sheet due to lithium dendrites.
[0126] In some embodiments, the first insulating layer 121 is further disposed on an end surface of the main body 101 at a second end, where the second end is opposite to the first end along the first direction.
[0127] The main body 101 has two opposite ends along a first direction, wherein the two ends are a first end and a second end respectively. The tab 102 protrudes from the main body 101 at the first end, and the second end is opposite to the first end along the first direction.
[0128] The end faces of the main body 101 at the second end and the end faces at the first end are both provided with a first insulating layer 121. This is beneficial to reducing the risk of internal short circuit caused by the end faces at the first end and the second end overlapping with electrodes of opposite polarity, thereby further improving the reliability of the battery cell.
[0129] The above text describes the technical solution of the electrode in conjunction with Figures 1 to 4. The following text describes the method for preparing the electrode in conjunction with Figure 5. The parts corresponding to the electrode can be referred to above and will not be repeated here.
[0130] [Method for preparing electrode]
[0131] FIG5 is a schematic diagram of a method for preparing a pole piece according to an embodiment of the present application. The method 200 can be used to prepare the pole piece 1 in the above embodiment. The method 200 includes the following steps.
[0132] Step 210 , providing a current collector 10 .
[0133] FIG6 is a schematic diagram of a current collector according to an embodiment of the present application. For example, as shown in FIG6 , the current collector 10 is in the shape of a sheet or a rectangle. The shape and size of the current collector 10 can be set according to actual needs, and the embodiments of the present application include but are not limited to this.
[0134] In step 220 , an active material is coated on the first region of the current collector 10 to form an active material layer 11 in the first region.
[0135] Figure 7 is a schematic diagram of a current collector coated with an active material layer according to an embodiment of the present application. As shown in Figure 7 , an active material is coated in a first region of the current collector 10 to obtain a current collector 10 provided with an active material layer 11 .
[0136] The first region of the current collector 10 can be a region set according to actual needs. In the embodiment of the present application, the first region corresponds to the coating area 1011 of the main body 101 of the electrode 1.
[0137] In step 230 , an insulating paste is coated on the second region of the current collector 10 to form a second insulating layer 122 in the second region. The insulating paste includes a thermoplastic polymer and a binder. The thickness d2 of the second insulating layer 122 is 20 μm to 50 μm.
[0138] FIG8 is a schematic diagram of a current collector coated with a second insulating layer according to an embodiment of the present application. As shown in FIG8 , an insulating slurry is coated on the second region of the current collector 10 to obtain a current collector 10 provided with a second insulating layer 122 .
[0139] The size of the second region can be set according to actual needs. In the embodiment of the present application, the second region corresponds to the transition region 1012 of the main body 101 of the electrode 1 and the region of the electrode tab 102 where the second insulating layer 122 is provided.
[0140] Step 240 , cutting the current collector 10 provided with the second insulating layer 122 along cutting lines, wherein at least a portion of the cutting lines 124 are provided in the second region.
[0141] Figure 9 is a schematic diagram of a current collector showing a cutting line according to an embodiment of the present application. As shown in Figure 9 , the current collector 10 is cut along the cutting line 124 to obtain the electrode 1 shown in Figures 2 to 4 .
[0142] In the above technical solution, by providing the second insulating layer 122 , the first insulating layer 121 can be formed simultaneously with cutting, which is beneficial for simplifying the preparation steps of the first insulating layer 121 .
[0143] In some embodiments, the thickness d2 of the second insulating layer 122 is 20 μm to 30 μm.
[0144] In some embodiments, the thermoplastic polymer has a drop melting point of 80°C to 200°C.
[0145] In some embodiments, the material of the thermoplastic polymer includes: at least one of a crystalline thermoplastic polymer and an amorphous thermoplastic polymer; optionally, the crystalline thermoplastic polymer includes: at least one of polyethylene, polypropylene, and polyamide; optionally, the amorphous thermoplastic polymer includes: at least one of microcrystalline wax, polystyrene, and polymethyl methacrylate.
[0146] In some embodiments, in the insulating paste, the mass ratio of the thermoplastic polymer to the binder A:B is 60:40 to 80:20; optionally, in the insulating paste, the mass ratio of the thermoplastic polymer to the binder A:B is 70:30 to 80:20.
[0147] In some embodiments, step 240 includes: controlling a laser processing tool to cut the current collector 10 provided with a second insulating layer 122 along a cutting line, wherein the power of the laser processing tool is 20 to 200 W, the frequency is 100 to 800 kHz, and the feed speed is 5 m / min to 30 m / min; optionally, the power of the laser processing tool is 20 to 100 W, the frequency is 100 to 300 kHz, and the feed speed is 5 m / min to 15 m / min.
[0148] The power of the laser processing tool can be 20W, 50W, 100W, 200W or any value within the above range, the frequency can be 100kHz, 200kHz, 300kHz, 500kHz, 800kHz or any value within the above range, and the feed speed can be 5m / min, 15m / min, 20m / min, 30m / min or any value within the above range.
[0149] In the above technical solution, reasonable control of the use parameters of the laser processing tool is conducive to obtaining a more uniform and dense first insulating layer 121, reducing burrs generated during the cutting process, and reducing the risk of the second insulating layer 122 falling off.
[0150] In some embodiments, the electrode sheet 1 can also be prepared by the following method: providing a current collector 10; coating a first region of the current collector 10 with an active material to form an active material layer 11 in the first region; coating a second region of the current collector 10 with an insulating slurry to form a second insulating layer 122 in the second region; cutting the current collector 10 provided with the second insulating layer 122 along a cutting line, with at least a portion of the cutting line being provided in the second region; controlling a hot melt tool to coat the end surface produced by the cutting with a molten thermoplastic polymer to form the first insulating layer 121. The material of the second insulating layer 122 is not specifically limited and can be alumina, boehmite, or the like.
[0151] In some embodiments, the electrode sheet 1 can also be prepared by the following method: providing a current collector 10; coating an active material on a first region of the current collector 10 to form an active material layer 11 in the first region; cutting the current collector 10 provided with the active material layer 11 along a cutting line, with at least part of the cutting line being provided in a second region; and controlling a hot melt tool to coat a molten thermoplastic polymer on the end surface produced by the cutting and the second region of the current collector 10 to form a first insulating layer 121 and a second insulating layer 122.
[0152] [Positive electrode]
[0153] The electrode sheet 1 in the embodiment of the present application may be a positive electrode sheet, which includes a positive electrode current collector and a positive electrode film layer disposed on the positive electrode current collector.
[0154] The positive electrode current collector may be a metal foil or a composite current collector. For example, the positive electrode current collector may be an aluminum foil.
[0155] The composite current collector may include a polymer base layer and a metal layer formed on at least one surface of the polymer base layer. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, etc.) on a polymer substrate (such as a substrate made of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0156] The positive electrode film layer includes a positive electrode active material. The positive electrode active material can be a positive electrode active material for batteries known in the art. For example, the positive electrode active material is lithium iron phosphate, a ternary material, a lithium-rich manganese-based material, etc. As an example, the positive electrode active material is a ternary material, and further, a ternary material of a high nickel system. For example, LiNi 0.6 Co 0.2 Mn 0.2 O2, LiNi 0.8 Co 0.1 Mn 0.1 O2.
[0157] The positive electrode film layer may also optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), a vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, a vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, a tetrafluoroethylene-hexafluoropropylene copolymer, and a fluorine-containing acrylate resin.
[0158] The positive electrode film layer may further optionally include a conductive agent, which may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0159] [Negative electrode]
[0160] The electrode sheet 1 in the embodiment of the present application may be a negative electrode sheet, which includes a negative electrode current collector and a negative electrode film layer disposed on the negative electrode current collector.
[0161] The negative electrode current collector can be a metal foil or a composite current collector. The negative electrode current collector can be copper foil. The composite current collector can be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, silver alloy, etc.) on a polymer material substrate (such as polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0162] The negative electrode film layer includes a negative electrode active material. The negative electrode active material can be a negative electrode active material for batteries that is well known in the art. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, etc. The silicon-based material can be selected from at least one of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material can be selected from at least one of elemental tin, tin oxide compounds, and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries can also be used. These negative electrode active materials can be used alone or in combination of two or more.
[0163] The negative electrode film layer may further optionally include a conductive agent, which may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0164] [Electrolytes]
[0165] The electrolyte conducts ions between the positive and negative electrodes. The present invention does not specifically limit the type of electrolyte, and the electrolyte can be selected based on the needs. For example, the electrolyte can be liquid, gel, or solid.
[0166] In some embodiments, the electrolyte is an electrolyte solution comprising an electrolyte salt and a solvent.
[0167] The electrolyte salt may include at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bisfluorosulfonyl imide, lithium bistrifluoromethanesulfonyl imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium bisoxalatoborate, lithium difluorodioxalatophosphate, and lithium tetrafluorooxalatophosphate.
[0168] The solvent may include at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methylpropyl carbonate, ethylpropyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, sulfolane, dimethyl sulfone, methyl ethyl sulfone, and diethyl sulfone.
[0169] The electrolyte may also optionally include negative electrode film-forming additives, positive electrode film-forming additives, and may also include performance additives that can improve certain battery properties, such as improving battery overcharge performance, improving battery high or low temperature performance, etc.
[0170] [Isolation film]
[0171] The separator is used to separate the positive electrode sheet from the negative electrode sheet. The present invention has no particular restrictions on the type of separator, and any known porous separator with good chemical and mechanical stability can be used.
[0172] The material of the separator can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.
[0173] The positive electrode sheet, the negative electrode sheet and the separator can be made into an electrode assembly through a winding process or a lamination process.
[0174] [Battery Cell]
[0175] An embodiment of the present application provides a battery cell, comprising the pole piece 1 in the above embodiment, and / or a pole piece prepared by the method in the above embodiment.
[0176] The embodiment of the present application has no particular limitation on the shape of the battery cell, which can be cylindrical, square, or any other shape. The battery cell can be a lithium-ion battery, a lithium-sulfur battery, a sodium-ion battery, a magnesium-ion battery, or the like.
[0177] FIG10 is a schematic diagram of a battery cell according to an embodiment of the present application. For example, as shown in FIG10 , the battery cell 3 is a square battery cell. The battery cell 3 includes a housing 31 , an end cap assembly 32 , and an electrode assembly 33 disposed in the housing 31 .
[0178] The electrode assembly 33 can be made of a positive electrode sheet, a negative electrode sheet and a separator by a winding process or a lamination process. In some embodiments, the positive electrode sheet is the electrode sheet 1 in the embodiment of the present application.
[0179] The end cap assembly 32 includes an electrode terminal 322 . For example, as shown in FIG. 10 , the end cap assembly 32 includes two electrode terminals 322 , one of which is a positive electrode terminal and the other is a negative electrode terminal.
[0180] The battery cell 3 further includes a current collecting member 34, which is used to connect the electrode tab 331 of the electrode assembly 33 and the electrode terminal 322. For example, when the electrode sheet 1 in the embodiment of the present application is a positive electrode sheet, one current collecting member 34 is used to connect the positive electrode tab (which may also be the tab 102 of the electrode sheet 1) and the positive electrode terminal, and the other current collecting member 34 is used to connect the negative electrode tab and the negative electrode terminal.
[0181] In some embodiments, battery cells may be assembled into a battery module. The number of battery cells contained in a battery module may be one or more. The specific number may be selected by those skilled in the art based on the application and capacity of the battery module.
[0182] [Battery]
[0183] The present invention provides a battery comprising the battery cells of the above-mentioned embodiment. Figure 11 is a schematic diagram of a battery according to an embodiment of the present invention. As shown in Figure 11, the battery 5 may comprise a plurality of battery cells (not shown in the figure).
[0184] The battery cells 3 can be directly assembled into the battery 5 , or they can be assembled into battery modules first, and then multiple battery modules can be assembled into the battery 5 .
[0185] [Electrical devices]
[0186] An embodiment of the present application provides an electrical device, comprising the battery described in the above embodiment.
[0187] Figure 12 is a schematic diagram of an electric device according to an embodiment of the present application. As shown in Figure 12, the present application provides an electric device 6, which includes the battery according to the above embodiment.
[0188] Optionally, the electrical device may also be an energy storage device, a lighting device, a spacecraft, etc., and the embodiments of the present application include but are not limited to the above.
[0189] Figure 14 is a schematic diagram of a pole piece according to another embodiment of the present application, Figure 15 is a cross-sectional view along the AA direction in Figure 14, and Figure 16 is a cross-sectional view along the CC direction in Figure 14. As shown in Figures 14 to 16, the present embodiment provides a pole piece 1, comprising a current collector 10 and a first insulating layer 121. The first insulating layer 121 is disposed on at least a portion of the end surface of the current collector 10, and the thickness d1 of the first insulating layer 121 is 200 nm to 2000 nm.
[0190] The pole piece 1 includes a current collector 10 and a first insulating layer 121 , and may further include an active material layer 11 .
[0191] As an example, the current collector 10 includes a main body 101 and a tab 102. The tab 102 is a bare foil (for example, aluminum foil) that protrudes from the main body 101. The active material layer 11 is provided on both sides of the main body 101 along its own thickness direction. The first insulating layer 121 is provided on the end surface 1012a of one end of the main body 101 along a first direction. The first direction is the direction in which the tab 102 protrudes from the main body 101. By providing the first insulating layer 121 on the end surface 1012a of one end of the main body 101 along the first direction, the first insulating layer 121 can cover the burrs on the end surface 1012a, thereby reducing the risk of internal short circuits in the battery cell caused by burrs piercing the diaphragm, and reducing the risk of short circuits caused by the end surface 1012a overlapping with electrodes of opposite polarity.
[0192] In the example shown in FIG14 , the tab 102 does not need to be cut. As an example, the first insulating layer 121 can be formed by applying a hot melt coating to the end surface 1012a of the current collector 10. As another example, a film layer comprising a thermoplastic polymer can be applied to the surface of the current collector 10 and then heated to form the first insulating layer 121.
[0193] As another example, the first insulating layer 121 is provided on both the end surface 1013 along the second direction and the end surface 1012a along the first direction of the current collector 10, where the second direction is perpendicular to the first direction. For example, the first direction is the y-direction in the figure, and the second direction is the x-direction in the figure. This further reduces the risk of burrs on the current collector 10 puncturing the separator and causing internal short circuits in the battery cell, and reduces the risk of short circuits caused by overlapping of each end surface with an electrode of opposite polarity.
[0194] The description of the first insulating layer 121 can be found in the above description and will not be repeated here.
[0195] Below, the embodiment of the present application is described. The embodiment described below is exemplary and is only used to explain the present application, and is not to be construed as limiting the present application. Where specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. Reagents or instruments used that do not specify the manufacturer are conventional products that can be obtained commercially.
[0196] [Example]
[0197] Example 1
[0198] In Example 1, the structure of pole piece 1 is shown in Figure 2 . The thickness d1 of first insulating layer 121 is 200 nm, and the thickness d2 of second insulating layer 122 is 20 μm. The thermoplastic polymer in second insulating layer 122 is microcrystalline wax, which has a drop melting point of 80°C. The mass ratio of the thermoplastic polymer to the binder, A:B, is 80:20.
[0199] Examples 2-6
[0200] The difference between Example 2-6 and Example 1 is that the thickness of the second insulating layer 122 is different; accordingly, the thickness of the first insulating layer 121 is different. Specific parameters can be found in Table 1.
[0201] Examples 7-8
[0202] The difference between Example 7-8 and Example 1 is that the mass ratio of thermoplastic polymer to binder is different.
[0203] In Examples 7 and 8, the mass ratios of the thermoplastic polymer to the binder are 70:30 and 60:40, respectively.
[0204] Examples 9-10
[0205] The difference between Examples 9 and 10 and Example 8 is that the materials of the thermoplastic polymer in the second insulating layer 122 are different. In the second insulating layer 122, the materials of the thermoplastic polymer are polypropylene and polyamide respectively.
[0206] In Examples 1-10, the electrode 1 is prepared using the preparation method 200. The thickness d1 of the first insulating layer 121 is related to the thickness d2 of the second insulating layer 122. The thickness d2 of the second insulating layer 122 can be seen in Table 1.
[0207] Examples 11-13
[0208] In Examples 11-12, the first insulating layer 121 and the second insulating layer 122 were prepared using a hot melt tool. Specifically, after the current collector 10 provided with the active material layer 11 was cut along the cutting line, a hot melt tool filled with a thermoplastic polymer was used to coat the end surface 1011a and the second region (corresponding to the transition region and the portion of the tab, see the above description for details) with a thermoplastic polymer to prepare the first insulating layer 121 and the second insulating layer 122 having corresponding thicknesses.
[0209] In Example 13, the first insulating layer 121 was prepared using a hot melt tool. Specifically, after the current collector 10, provided with the active material layer 11 and the second insulating layer 122, was cut along the cutting line, a hot melt tool containing a thermoplastic polymer was used to coat the end surface 1011a with the thermoplastic polymer to prepare the first insulating layer 121 having a corresponding thickness. The second insulating layer 122 comprised boehmite and was formed by coating a slurry comprising boehmite on the second region of the current collector 10.
[0210] Comparative Example 1
[0211] In Comparative Example 1, the material of the second insulating layer includes boehmite, and the first insulating layer is not provided on the end surface 1011 a .
[0212] Comparative Example 2
[0213] In Comparative Example 2, the thickness of the second insulating layer is 19 μm, and the thickness of the first insulating layer is 190 nm.
[0214] Comparative Example 3
[0215] In Comparative Example 3, the thickness of the second insulating layer is 51 μm, and the thickness of the first insulating layer is 2100 nm.
[0216] In Comparative Examples 1-3, pole pieces were prepared using the same method as in Example 1, wherein the specific materials and cutting parameters may be different, as shown in Table 1.
[0217] In Table 1, d1 is the thickness of the first insulating layer 121, d2 is the thickness of the second insulating layer 122, and A:B is the mass ratio of the thermoplastic polymer to the binder in the second insulating layer. "Same process" indicates whether the first and second insulating layers were produced using the same process. In Table 1, "yes" indicates that the first and second insulating layers were produced using the same process, and "no" indicates that the first and second insulating layers were produced using different processes.
[0218] Table 1 Parameters of Examples and Comparative Examples
[0219] Table 2 Experimental results of comparative examples and embodiments
[0220] [Preparation of battery cells]
[0221] (1) Prepare coating slurry
[0222] A thermoplastic polymer and a binder are mixed in a specific ratio, and a solvent is added and stirred until uniformly mixed. The slurry has a viscosity of approximately 3000 mPa·s. The binder is polyvinylidene fluoride (PVDF), and the solvent is nitrogen-methyl pyrrolidone. The specific thermoplastic polymers and the ratio of thermoplastic polymer to binder are shown in Table 1.
[0223] (2) Coating and drying
[0224] When the positive electrode active slurry is coated on the aluminum foil to prepare the active material layer, the positive electrode active material in the positive electrode active slurry is LiNi 0.8 Co 0.1 Mn 0.1 O2 (NCM811); apply the above insulating coating slurry to an aluminum foil with a coating width of 3 mm. Oven dry at 100°C. The thickness of the second insulating layer after drying is shown in Table 1. The thickness of the second insulating layer here refers to the thickness of the second insulating layer on one side of the current collector.
[0225] (3) Laser die cutting
[0226] The above products were die-cut. The specific process parameters are shown in Table 1.
[0227] (4) Making battery cells
[0228] The positive electrode plate and other components required for the battery: negative electrode plate, separator, and electrolyte are assembled together to form a lithium battery cell.
[0229] It should be noted that the above-mentioned method for preparing the battery cell is applicable to Examples 1-10 of the present application. The preparation of Examples 11-13 can be referred to as described above and will not be repeated here.
[0230] [Confirmation of the first insulating layer]
[0231] A scanning electron microscope (SEM) is used to observe the end face to check whether there is a first insulating layer at the end face; in addition, the thickness of the first insulating layer can also be observed through photos taken by the scanning electron microscope.
[0232] [Confirmation of the second insulating layer]
[0233] Use a scanning electron microscope to observe the surface of the electrode to check whether there is a second insulating layer on the surface. Cut the electrode open and photograph the cross section of the electrode using a scanning electron microscope. Observe the thickness of the second insulating layer based on the photograph.
[0234] [Number of burrs]
[0235] A charge coupled device (CCD) is used to observe whether the number of burrs on the end face after laser die cutting is qualified.
[0236] When the number of burrs within a size range of 30 μm to 40 μm is ≤10 and the maximum size of the burrs is ≤40 μm, the number of burrs is considered acceptable.
[0237] [Overlapping full-charge anode test]
[0238] Use the laser die-cut end face to overlap the fully charged anode and observe whether it catches fire.
[0239] [Self-discharge test]
[0240] The battery is adjusted to 80% SOC and stored for 48 hours. The voltage before storage is V1, and the voltage after storage is V2. k = (V1-V2) / 48.
[0241] Among them, k is used to characterize the self-discharge performance of the battery. When k≤0.2mV / h, it means that the self-discharge test has passed.
[0242] [Confirmation of the Drop Melting Point of Thermoplastic Polymers]
[0243] The drop melting point of thermoplastic polymers can be determined using GB / T8026-2014. For example, a cooled temperature sensor is vertically immersed in a sample, allowing the sample to adhere to the sensor. The sample is then placed in a test tube and heated at the required heating rate to begin melting. The temperature at which the first drop of sample falls from the sensor is the sample's drop melting point.
[0244] For another example, the drop melting point of a thermoplastic polymer can be determined based on the specific type of thermoplastic polymer. For example, for a crystalline thermoplastic polymer, the drop melting point refers to the melting point of the crystalline thermoplastic polymer; for an amorphous thermoplastic polymer, the drop melting point refers to the glass transition temperature of the amorphous thermoplastic polymer.
[0245] [Mass ratio of thermoplastic polymer to binder]
[0246] The mass ratio of the thermoplastic polymer to the binder can be obtained according to the mass of the thermoplastic polymer and the mass of the binder added during the preparation process.
[0247] Figure 13 is a SEM image of an end surface provided with a first insulating layer according to an embodiment of the present application. As shown in Figure 13 , a first insulating layer 121 is provided at the end surface of the pole piece.
[0248] As shown in Examples 1-13 and Comparative Example 1, a first insulating layer is provided at the end face of the pole piece. After the end face of the pole piece is overlapped with the fully charged anode, no fire will occur. Therefore, the technical solution of the embodiment of the present application can improve the reliability of the battery cell.
[0249] As shown in Examples 1-6 and Comparative Example 2, when fully charged anodes were overlapped, the battery cells in Examples 1-6 did not catch fire, while fire did occur in Comparative Example 2. By properly adjusting the thickness of the second insulating layer, a first insulating layer with a suitable thickness and a relatively uniform first insulating layer can be obtained, thereby improving the reliability of the battery cells.
[0250] As shown in Examples 1-6 and Comparative Example 3, although a thicker second insulating layer is conducive to obtaining a more uniform and appropriately thick first insulating layer, the thicker second insulating layer causes more burrs to be generated during the cutting process, and self-discharge anomalies may occur.
[0251] In combination with Examples 7-8, a reasonable arrangement of the thermoplastic polymer and the binder in the second insulating layer can be applied to a variety of different mass ratios.
[0252] In conjunction with Examples 9 and 10, the thermoplastic polymer in the second insulating layer can be a variety of materials.
[0253] In conjunction with Examples 1-6 and 11-12, by using a hot melt tool to prepare the first and second insulating layers, although the thickness of the second insulating layer exceeds 50 μm, since the aluminum foil is cut during cutting, the number of burrs caused by the large thickness of the second insulating layer will not be large; the thickness of the second insulating layer is less than 20 μm, and since the first insulating layer is not formed by melting and solidifying the thermoplastic polymer in the second insulating layer, the phenomenon of fire occurring at some locations when overlapping a fully charged anode will not occur. In conjunction with Examples 11-13, the electrode pieces of the embodiments of the present application can be prepared by various methods.
[0254] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are merely examples, and any embodiments having substantially the same structure and effect as the technical concept within the scope of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the present application, any other embodiments that can be conceived by those skilled in the art and that combine some of the constituent elements in the embodiments are also included in the scope of the present application.
Claims
1. A pole piece, It is characterized in that include: current collector, active material layer and first insulating layer, The current collector includes a main body and a tab, wherein the tab extends from a first end of the main body, the first end is an end of the main body along a first direction, and the main body includes a coating area; The active material layer is disposed on the surface of the coating area; The first insulating layer is disposed on an end surface of the main body at the first end, and a thickness d1 of the first insulating layer is 200 nm to 2000 nm.
2. The pole piece according to claim 1, It is characterized in that The thickness d1 of the first insulating layer is 200 nm to 500 nm.
3. The pole piece according to claim 1 or 2, It is characterized in that The main body also includes a transition zone, which is arranged between the coating zone and the tab; The pole piece further includes a second insulating layer, at least a portion of which is disposed on a surface of the transition region, and a material of the second insulating layer includes a thermoplastic polymer.
4. The pole piece according to claim 3, It is characterized in that The thickness d2 of the second insulating layer is 20 μm to 50 μm.
5. The pole piece according to claim 3 or 4, It is characterized in that The thermoplastic polymer has a drop melting point of 80°C to 200°C.
6. The pole piece according to any one of claims 3 to 5, It is characterized in that The thermoplastic polymer includes: at least one of a crystalline thermoplastic polymer and an amorphous thermoplastic polymer; the crystalline thermoplastic polymer includes: at least one of polyethylene, polypropylene, and polyamide; the amorphous thermoplastic polymer includes: at least one of microcrystalline wax, polystyrene, and polymethyl methacrylate.
7. The pole piece according to any one of claims 3 to 6, It is characterized in that The second insulating layer further includes an adhesive.
8. The pole piece according to claim 7, It is characterized in that In the second insulating layer, a mass ratio A:B of the thermoplastic polymer to the binder is 60:40 to 80:
20.
9. The pole piece according to any one of claims 3 to 8, It is characterized in that The second insulating layer includes a first portion and a second portion, wherein the first portion is disposed on the surface of the transition region, and the second portion extends from the first portion along the first direction and is disposed on a portion of the surface of the tab.
10. The pole piece according to claim 9, It is characterized in that Along a second direction, the first insulating layer is disposed on end surfaces of both ends of a region of the electrode tab where the second portion is disposed, and the second direction is different from the first direction.
11. A pole piece according to any one of claims 3 to 10, It is characterized in that The material of the first insulating layer is the same as the material of the thermoplastic polymer in the second insulating layer.
12. The pole piece according to any one of claims 3 to 11, It is characterized in that The thermoplastic polymer in the first insulating layer is in the form of a film layer, and the thermoplastic polymer in the second insulating layer includes a film layer-shaped thermoplastic polymer and a particle-shaped thermoplastic polymer.
13. The pole piece according to any one of claims 1 to 12, It is characterized in that The current collector includes aluminum foil.
14. The pole piece according to any one of claims 1 to 13, It is characterized in that The first insulating layer is further disposed on an end surface of the main body at a second end, and the second end is opposite to the first end along the first direction.
15. A method for preparing a pole piece, It is characterized in that include: providing a current collector; coating an active material on a first region of the current collector to form an active material layer on the first region; Applying an insulating paste on the second region of the current collector to form a second insulating layer in the second region, wherein the insulating paste includes a thermoplastic polymer and a binder, and a thickness d2 of the second insulating layer is 20 μm to 50 μm; The current collector provided with the second insulating layer is cut along a cutting line, and at least a portion of the cutting line is provided in the second region.
16. The method according to claim 15, It is characterized in that The thickness d2 of the second insulating layer is 20 μm to 30 μm.
17. The method according to claim 15 or 16, It is characterized in that The thermoplastic polymer has a drop melting point of 80°C to 200°C.
18. The method according to any one of claims 15 to 17, It is characterized in that The material of the thermoplastic polymer includes: at least one of a crystalline thermoplastic polymer and an amorphous thermoplastic polymer; the crystalline thermoplastic polymer includes: at least one of polyethylene, polypropylene, and polyamide; the amorphous thermoplastic polymer includes: at least one of microcrystalline wax, polystyrene, and polymethyl methacrylate.
19. The method according to any one of claims 15 to 18, It is characterized in that In the insulating paste, the mass ratio A:B of the thermoplastic polymer to the binder is 60:40 to 80:
20.
20. The method according to any one of claims 15 to 19, It is characterized in that The method of cutting the current collector provided with the second insulating layer along the cutting line comprises: Controlling a laser processing tool to cut the current collector provided with the second insulating layer along the cutting line, wherein the The power of the laser processing tool is 20 to 200 W, the frequency is 100 to 800 kHz, and the feed speed is 5 to 30 m / min.
21. A battery cell, It is characterized in that It comprises a pole piece as described in any one of claims 1-14, and / or a pole piece prepared by the method as described in any one of claims 15-20.
22. A battery, It is characterized in that Comprising the battery cell as claimed in claim 21.
23. An electrical device, It is characterized in that Comprising a battery as claimed in claim 22.
24. A pole piece, It is characterized in that include: a current collector and a first insulating layer, The first insulating layer is disposed on at least a portion of the end surface of the current collector, and a thickness d1 of the first insulating layer is 200 nm to 2000 nm.
Citation Information
Patent Citations
Lithium ion battery
CN102683739A
Electrode sheet and lithium ion battery
CN105655540A
Laminate and secondary battery
CN110224170A
Pole piece and secondary battery with same
CN114122327A
Electrode assembly, battery cell, battery and electric device
CN214254666U