Low-temperature adsorption catalyst and preparation method therefor

By using active metal and barium oxide support in the low-temperature adsorption catalyst, combined with the first and second zeolite molecular sieve support, the problem of poor adsorption performance of existing catalysts at low temperatures is solved, efficient adsorption and catalytic conversion are achieved, and the vehicle is satisfied Environmental protection needs for exhaust gas treatment.

WO2024240104A1PCT designated stage expired Publication Date: 2024-11-28CATARC AUTOMOTIVE TEST CENT TIANJIN CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/094148
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-22
Filing Date
2024-05-20
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

The existing low-temperature adsorption catalysts have poor performance in adsorbing nitrogen oxides and hydrocarbons at low temperatures, and cannot effectively treat pollutants in vehicle exhaust.

Method used

Using a low-temperature adsorption catalyst supported by active metals and barium oxides, the first zeolite molecular sieve and the second zeolite molecular sieve as support, through reconstruction reaction and hydrothermal treatment, it is prepared to efficiently adsorb nitrogen oxides and carbons at 200°C. The catalyst of hydride is catalyzed in the range of 200°C to 400°C.

Benefits of technology

A catalyst that effectively adsorbs nitrogen oxides and hydrocarbons at low temperatures can be heat-discharged within the range of 200℃-400℃, significantly improving the exhaust gas treatment efficiency and meeting the environmental protection requirements of vehicle exhaust gas treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024094148_28112024_PF_FP_ABST
    Figure CN2024094148_28112024_PF_FP_ABST
Patent Text Reader

Abstract

The present application relates to the technical field of catalysts. Specifically provided are a low-temperature adsorption catalyst and a preparation method therefor. The low-temperature adsorption catalyst comprises a load and a carrier, wherein the carrier comprises a first zeolite molecular sieve and a second zeolite molecular sieve, the first zeolite molecular sieve being an eight-membered ring molecular sieve, and the second zeolite molecular sieve being a ten-membered ring molecular sieve or a twelve-membered ring molecular sieve.
Need to check novelty before this filing date? Find Prior Art

Description

Low-temperature adsorption catalyst and preparation method thereof

[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on May 22, 2023, with application number 202310571954.7, the entire contents of which are incorporated by reference into this application. Technical Field

[0002] The present application relates to the field of catalyst technology, for example, to a low-temperature adsorption catalyst and a preparation method thereof. Background Art

[0003] With the increasing requirements for environmental protection, more and more attention has been paid to the treatment of vehicle exhaust. Due to the low exhaust temperature during the cold start phase, the after-treatment device cannot play an efficient catalytic conversion role. In related technologies, catalysts have been developed that can adsorb and fix exhaust at low temperatures and desorb and catalytically convert it at high temperatures. However, the performance of existing catalysts in simultaneously adsorbing nitrogen oxides and hydrocarbons at low temperatures is poor. Therefore, there is an urgent need for a catalyst that can simultaneously and efficiently adsorb nitrogen oxides and hydrocarbons at low temperatures.

[0004] Summary of the Invention

[0005] In view of this, the purpose of this application is to provide a low-temperature adsorption catalyst and a preparation method thereof.

[0006] Based on the above purpose, the present application provides a low-temperature adsorption catalyst, including: a load and a carrier, the carrier including a first zeolite molecular sieve and a second zeolite molecular sieve, the first zeolite molecular sieve is an eight-membered ring molecular sieve, and the second zeolite molecular sieve is a ten-membered ring molecular sieve or a twelve-membered ring molecular sieve.

[0007] Optionally, the load includes active components and / or auxiliary agents, the active component is an active metal or an oxide of the active metal, the active metal is one or more of Pd, Pt, Au, Ag, Co, Sm, Ce, Mn, Cr, Fe, Cu, Ni, Ir, Re, Ru, Zr, Ti, Sr, K and Na; the auxiliary agent is barium oxide; the first zeolite molecular sieve is one or more of AFX type molecular sieve, AFT type molecular sieve, AEI type molecular sieve, CHA type molecular sieve, ERI type molecular sieve, LTA type molecular sieve, KFI type molecular sieve, RHO type molecular sieve and RTH type molecular sieve; the second zeolite molecular sieve is one or more of BEA type molecular sieve, FAU type molecular sieve, MFI type molecular sieve, MOR type molecular sieve, OFF type molecular sieve and GME type molecular sieve.

[0008] Optionally, the mass ratio of the auxiliary agent to the active component is 0-50, the mass ratio of the active component to the carrier is 1%-10%, the silicon-aluminum ratio in the carrier is 0.1-200, and the mass ratio of the first zeolite molecular sieve to the second zeolite molecular sieve is 0.5-3.

[0009] The present application provides a preparation method for the above-mentioned low-temperature adsorption catalyst, wherein the load includes an active component and / or an auxiliary agent, and the method includes: uniformly dispersing the carrier in a first solvent, shearing to obtain a suspension, adding a silicon source and an aluminum source to the suspension to carry out a reconstruction reaction, filtering, washing, drying and calcining after the reconstruction reaction to obtain a reconstructed carrier; dissolving a soluble precursor of the active component in a second solvent to obtain a first solution; adding the reconstructed carrier to a third solvent, stirring evenly, adding a surface charge regulator, and then adding the first solution for hydrothermal treatment to achieve quantitative ion exchange, filtering, washing, drying and calcining after the hydrothermal treatment to obtain an initial catalyst; dissolving the precursor of the auxiliary agent in a fourth solvent, loading the auxiliary agent in the fourth solvent on the initial catalyst by a catalyst loading method, and drying and calcining the initial catalyst to obtain a low-temperature adsorption catalyst.

[0010] Optionally, the method of obtaining a suspension by shearing includes: obtaining a carrier particle size D by shearing. 50 The method comprises adding the silicon source and the aluminum source to the suspension to carry out a reconstruction reaction, wherein the silicon source and the aluminum source are added to the suspension, and the reconstruction reaction is carried out under closed conditions, the reconstruction reaction temperature is 120°C-200°C, and the reconstruction reaction time is 6.5h-72h.

[0011] Optionally, the reconstructed carrier is added to a third solvent and stirred evenly, including: adding the reconstructed carrier to the third solvent, stirring evenly under conditions of 40°C-100°C, and adjusting the pH value to 1-10; the first solution is then added for hydrothermal treatment to achieve quantitative ion exchange, including: adding the first solution for heating and stirring to form a second solution, the heating and stirring temperature is 50°C-100°C, and the heating and stirring time is 6h-12h; when the supernatant of the second solution is colorless, the second solution is hydrothermally treated, the hydrothermal treatment temperature is 120°C-180°C, and the hydrothermal treatment time is 2h-48h.

[0012] Optionally, the first solvent is an aqueous solvent containing a soluble organic base and a soluble organic alcohol; the soluble organic base is one or more of ethylenediamine, triethylamine, diethylamine, pyridine, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, tetrahydropyrrole, N,N,N-trimethyl-1-adamantylammonium hydroxide, choline cation and benzyltrimethylammonium; the soluble organic alcohol is one or more of methanol, ethanol, propanol, ethylene glycol and glycerol; the silicon source is one or more of montmorillonite, coal gangue, diatomaceous earth, silica sol, solid silica gel, silicon oxide, aluminum silicate, potassium silicate, sodium silicate, sodium aluminosilicate, ZSM-5 molecular sieve, clinoptilol molecular sieve, Y-type molecular sieve, Beta molecular sieve and all-silicon molecular sieve; the aluminum source is one or more of pseudo-boehmite, aluminum sol, aluminum oxide, aluminum hydroxide, sodium aluminum hydride, aluminum sulfate, potassium aluminum sulfate, aluminum nitrate, aluminum chloride, sodium aluminate, aluminum silicate and aluminum acetate.

[0013] Optionally, the mass ratio of the first solvent to the carrier is 1-300; the molar ratio of the soluble organic base to the silicon source is 0.1-20; the volume ratio of the soluble organic alcohol to the water in the first solvent is 0.1%-30%, and the molar ratio of the silicon source, the aluminum source and the water in the first solvent is 1:5-35:50-1000.

[0014] Optionally, the second solvent and the third solvent are water, the coordinating anions of the soluble precursor of the active component are one or more of hydrochloride ion, nitrate ion, nitrite ion, carbonate ion, acetate ion, bicarbonate ion, sulfate ion, sulfite ion, bisulfate ion, fluoride ion, iodate ion, chlorate ion, cyanate ion and thiocyanate ion; and the surface charge regulator is one or more of ammonia water, nitric acid, acetic acid, formic acid, dimethyl oxalate, methylal, ethylhydrazine, ethylhydroxylamine, diethylhydroxylamine, L-alanine-4-nitroaniline, isobutanolamine, acrylic acid and sodium polyacrylate.

[0015] Optionally, the precursor of the auxiliary agent is one or more of barium nitrate, barium acetate, barium chloride, barium sulfate, barium carbonate, barium ethanol, barium phosphate, barium tert-butoxide, barium aluminum oxide, barium hydrogen phosphate, barium acetylacetonate, isopropoxide barium, barium dihydrogen phosphate, barium di(2-hexyl acetate), barium molybdate, barium hydroxide, barium titanate, barium perchlorate and barium oxide; the fourth solvent is water; and the catalyst loading method is an equal volume impregnation method or a liquid phase deposition method.

[0016] As can be seen from the above, the low-temperature adsorption catalyst and its preparation method provided by the present application are loaded to adsorb and store nitrogen oxides and hydrocarbons from exhaust gas; the first zeolite molecular sieve is an eight-membered ring molecular sieve with a size of 0.4nm-0.5nm and a small pore size. It itself adsorbs a small amount of nitrogen oxides, thereby enhancing the catalyst's adsorption effect on nitrogen oxides; the second zeolite molecular sieve is a ten-membered ring molecular sieve or a twelve-membered ring molecular sieve with a size of 0.5nm-0.9nm and a large pore size. It can itself adsorb a large amount of hydrocarbons, thereby enhancing the catalyst's adsorption effect on hydrocarbons; the two zeolite molecular sieves serve as loaded carriers and can cooperate with each other to greatly improve the exhaust gas adsorption effect; the low-temperature adsorption catalyst and its preparation method can simultaneously and efficiently adsorb nitrogen oxides and hydrocarbons at 200°C. The adsorption amount of nitrogen oxides at 200°C is 330μmol / g, and the adsorption amount of hydrocarbons at 200°C is 524μmol / g, and they are thermally decomposed and released in the range of 200°C-400°C for catalytic conversion. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the technical solutions in this application or related technologies, the following briefly introduces the drawings required for use in the embodiments or related technical descriptions. Obviously, the drawings described below are merely embodiments of this application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.

[0018] FIG1 is a schematic diagram showing a comparison of the aging performance of catalyst Pd-SSZ-13;

[0019] FIG2 is a schematic diagram showing a comparison of the adsorption performance of catalysts Pd-SSZ-13 and BaO-Pd / SSZ-13;

[0020] FIG3 is a schematic diagram of the nitrogen oxide adsorption performance of the catalyst BaO-Pd / (SSZ-13+Beta) in the embodiment of the present application;

[0021] FIG4 is a schematic diagram of the electron microscope structure of the catalyst BaO-Pd / SSZ-13 prepared by the equal volume impregnation method;

[0022] Figure 5 is a schematic diagram of the electron microscope structure of the catalyst Ag / Beta;

[0023] Figure 6 is a schematic diagram of the electron microscope structure of the catalyst BaO-Pd / SSZ-13 prepared by liquid phase deposition. DETAILED DESCRIPTION

[0024] In order to make the objectives, technical solutions and advantages of the present disclosure more clear, the present disclosure is further described in detail below with reference to specific embodiments.

[0025] It should be noted that, unless otherwise defined, the technical terms used in the following examples have the same meanings as commonly understood by those skilled in the art to which this application relates. The experimental reagents used in the following examples, unless otherwise specified, are all conventional biochemical reagents; the experimental methods described, unless otherwise specified, are all conventional methods.

[0026] With increasing environmental protection requirements, vehicle exhaust treatment is receiving increasing attention. Due to the low exhaust temperature during the cold start phase, after-treatment devices cannot perform efficient catalytic conversion, especially below 150°C. Related technologies have developed catalysts that can adsorb and fix exhaust at low temperatures and desorb and catalytically convert it at high temperatures. For example, passive NOx adsorption (PNA) technology is used. Its principle is to adsorb and store nitrogen oxides at low temperatures. After the cold start, as the exhaust temperature rises, the adsorbed nitrogen oxides can be quickly released and efficiently converted to nitrogen through the downstream SCR catalyst. Alternatively, hydrocarbon trap technology (HCT) can be used. Its principle is to adsorb hydrocarbons at low temperatures and catalyze their oxidation to hydrogen and carbon dioxide at high temperatures. Similar to PNA technology, HCT technology can solve the problem of cold start pollutant emissions.

[0027] However, existing low-temperature adsorption catalysts have poor performance in simultaneously adsorbing nitrogen oxides and hydrocarbons. For example, the catalyst Pb-Ce / SSZ-13 has a good adsorption effect on nitrogen oxides, but extremely poor adsorption of hydrocarbons. Therefore, there is an urgent need for a catalyst that can simultaneously and efficiently adsorb nitrogen oxides and hydrocarbons at low temperatures.

[0028] In the process of realizing this application, it was found that the molecular sieve carrier has a rich microporous structure. Taking into account the differences in molecular size and chemical properties of hydrocarbons and nitrogen oxides, the molecular sieve carriers suitable for the two are also different. Hydrocarbon molecules are larger, so the molecular sieve carriers required have larger micropore channels; in addition, the molecular sieve has a high specific surface area and strong solid acidity. The carrier itself can efficiently adsorb long-chain, short-chain and aromatic hydrocarbons such as decane, propane and toluene at low temperatures, and also has a sufficiently high desorption temperature; however, the molecular sieve carrier itself has a weak ability to adsorb nitrogen oxides. It can be considered to carry active components to exert the chemical adsorption effect of nitrogen oxides, while synergistically improving the adsorption capacity of unsaturated hydrocarbon compounds.

[0029] The technical solution of the present application is described in detail below through specific embodiments.

[0030] In some embodiments of the present application, a low-temperature adsorption catalyst is provided, including: a load and a carrier, wherein the carrier includes a first zeolite molecular sieve and a second zeolite molecular sieve, the first zeolite molecular sieve is an eight-membered ring molecular sieve, and the second zeolite molecular sieve is a ten-membered ring molecular sieve or a twelve-membered ring molecular sieve.

[0031] The load includes active components and / or auxiliary agents, the auxiliary agent is barium oxide; the active component is an active metal or an oxide of the active metal, the active metal is one or more of Pd, Pt, Au, Ag, Co, Sm, Ce, Mn, Cr, Fe, Cu, Ni, Ir, Re, Ru, Zr, Ti, Sr, K and Na, for example, the active metal is Pd, Pd and Pt, or Ag and Ce; the first zeolite molecular sieve is AFX molecular sieve, AFT molecular sieve, AEI molecular sieve, CHA molecular sieve, ERI molecular sieve, LTA molecular sieve, KFI molecular sieve, RHO One or more of type molecular sieves and RTH type molecular sieves, for example, the first zeolite molecular sieve uses CHA type molecular sieve, selects LTA type molecular sieve, or selects CHA type molecular sieve and LTA type molecular sieve, etc.; the second zeolite molecular sieve is one or more of BEA type molecular sieve, FAU type molecular sieve, MFI type molecular sieve, MOR type molecular sieve, OFF type molecular sieve and GME type molecular sieve, for example, the second zeolite molecular sieve uses BEA type molecular sieve, selects OFF type molecular sieve, or selects BEA type molecular sieve and OFF type molecular sieve, etc.; the second zeolite molecular sieve can be a twelve-membered ring molecular sieve, which has a stronger adsorption capacity for hydrocarbons.

[0032] The mass ratio of the auxiliary agent to the active component is 0-50, for example, a mass ratio of 1, 5, 10, 20, 30, 40 or 50; the mass ratio of the active component to the carrier is 1%-10%, for example, a mass ratio of 1%, 5% or 10%, etc.; the silicon-aluminum ratio in the carrier is 0.1-200, and can be optionally 10-50, for example, a silicon-aluminum ratio of 10, 20, 30, 40 or 50, etc., taking into account both catalytic adsorption performance and stability; the mass ratio of the first zeolite molecular sieve to the second zeolite molecular sieve is 0.5-3, for example, a mass ratio of 0.5, 1, 1.5, 2, 2.5 or 3, etc.

[0033] The active component has a strong adsorption capacity for unsaturated hydrocarbons in the exhaust gas, thereby improving the catalyst's adsorption performance for hydrocarbons. At the same time, the active component can form an effective chemical bond with the nitrogen oxides in the exhaust gas, thereby enhancing the catalyst's adsorption effect on hydrocarbons. The additive can stabilize the active component and cooperate with the active component to adsorb and store nitrogen oxides and hydrocarbons from the exhaust gas. The first zeolite molecular sieve is an octahedral ring molecular sieve with a size of 0.4nm-0.5nm and a small pore size. It can adsorb a small amount of nitrogen oxides by itself, thereby enhancing the catalyst's adsorption effect on nitrogen oxides. If the first zeolite molecular sieve If a smaller molecular sieve, such as a six-membered ring molecular sieve, is used, nitrogen oxides will not easily enter the pores, resulting in poor adsorption effect; the second zeolite molecular sieve is a ten-membered ring molecular sieve or a twelve-membered ring molecular sieve, with a size of 0.5nm-0.9nm, a large pore size, and can adsorb a large amount of hydrocarbons by itself, thereby enhancing the catalyst's adsorption effect on hydrocarbons. If the second zeolite molecular sieve uses a larger molecular sieve, such as a sixteen-membered ring molecular sieve, the cost is high, the skeleton is easily collapsed by water absorption, and the stability is poor; the two zeolite molecular sieves, as carriers of active components and additives, can work together to greatly improve the exhaust gas adsorption effect.

[0034] This low-temperature adsorption catalyst can efficiently adsorb nitrogen oxides and hydrocarbons simultaneously at 200°C. The adsorption capacity of low-temperature nitrogen oxides at 200°C is 330μmol / g, and the adsorption capacity of low-temperature hydrocarbons at 200°C is 524μmol / g. These gases are thermally decomposed and released in the range of 200°C-400°C for catalytic conversion. Hydrocarbons are catalytically converted into water and carbon dioxide, and some nitrogen oxides are catalytically converted into nitrogen dioxide. The remaining gases are catalytically converted into harmless nitrogen, water and carbon dioxide through downstream units such as the diesel oxidation catalyst (DOC), selective catalytic reduction (SCR) or selective catalytic reduction filter (SCR coating on DPF, SCRF).

[0035] The low-temperature adsorption catalyst can be used upstream of DOC and SCR, or can be used to replace DOC, or can be used in combination with DOC, or can be used in combination with SCR catalyst.

[0036] The chemical formula of the low temperature adsorption catalyst is zBaO·{yMO p·[Al2O3·xSiO2]·n(H2O)}, wherein M is an active metal, p is 0-3, for example, p is 1, 2 or 3, etc., x is 0.1-200, for example, x is 1, 10, 50, 100, 150 or 200, etc., y is 0.01-10, for example, y is 1, 5 or 10, etc., z is 0-50, for example, z is 1, 10, 20, 30, 40 or 50, etc., n is a positive number, for example, n is 1, 5 or 10, etc., [Al2O3·xSiO2] represents a carrier, i.e., a zeolite molecular sieve, composed of aluminum oxide, silicon oxide and their composites, MOp is an active component, and BaO is an auxiliary agent.

[0037] The carrier is used to support active components and additives. The additives adsorb hydrocarbons and nitrogen oxides from the exhaust gas to the carrier surface. The active components in the carrier are selectively chemically adsorbed and stored. The active components in the second zeolite molecular sieve are more likely to migrate, and the micropore confinement effect of the molecular sieve is weaker than that of the first zeolite molecular sieve.

[0038] In some embodiments, the active component and the auxiliary agent are located on the outer surface, shell, inner wall, pore, lattice, ion exchange site, skeleton or molecular sieve cage of the carrier; the active component is combined with the carrier in one or more states of nano-oxide cluster state, isolated active site cation state, coordination state and atomic state; the auxiliary agent is combined with the carrier in one or more states of nano-barium oxide, barium ion, hydroxyl barium, barium atom and barium alloy.

[0039] After the active component is combined with the carrier, the adsorption capacity of unsaturated hydrocarbons in the exhaust gas is improved. In addition, the active component can form an effective chemical bond with the nitrogen oxides in the exhaust gas. Its structural formula is one or more of the following:

[0040] The desorption temperature range for hydrocarbons is 100°C-250°C, and the desorption temperature range for nitrogen oxides is 250°C-450°C. As the temperature rises, the active components catalytically convert some hydrocarbons into water and carbon dioxide before the hydrocarbons are completely desorbed. Simultaneously, some nitrogen oxides are catalytically oxidized to nitrogen dioxide before the nitrogen oxides are completely desorbed. It is generally believed that nitrogen dioxide has a higher oxidizing power than oxygen and can oxidize soot at 250°C, which is beneficial for DPF (Diesel Particulate Filter) regeneration. Furthermore, increased nitrogen dioxide induces a rapid SCR reaction, which benefits the downstream selective catalytic reduction of nitrogen oxides.

[0041] SCR reactions include:

[0042] Standard SCR reaction 4NH3(ads)+4NO+O2→4N2+6H2O,

[0043] Fast SCR reaction 4NH3(ads)+2NO+2NO2→4N2+6H2O,

[0044] Slow SCR reaction 4NH3(ads)+3NO2→7 / 2N2+6H2O.

[0045] The additive is combined with the carrier in one or more states of nano-barium oxide, barium ions, hydroxyl barium, barium atoms and barium alloys. The barium oxide itself is a good adsorption material and desiccant, which can adsorb water at low temperature, reduce the competitive adsorption of water vapor, and ensure the active component's adsorption of hydrocarbons and nitrogen oxides. In addition, it can also adsorb nitrogen oxides, hydrocarbons, and sulfur oxides. The barium oxide and the active component act synergistically to adsorb and store nitrogen oxides in the exhaust gas. The active component can convert part of the nitrogen monoxide into nitrogen dioxide, which forms nitrate or nitrite with the barium oxide and is stored, and decomposes and releases when the temperature rises. The barium oxide can also stabilize the active component and improve the durability of the catalyst.

[0046] In some embodiments, a method for preparing a low-temperature adsorption catalyst is provided, comprising the following steps:

[0047] S1. The carrier is uniformly dispersed in a first solvent, and a suspension is obtained by shearing. A silicon source and an aluminum source are added to the suspension to carry out a reconstruction reaction. After the reconstruction reaction is completed, the suspension is filtered, washed, dried and calcined to obtain a reconstructed carrier.

[0048] This step is the process of reducing and reconstructing the carrier grains, which can effectively improve the adsorption performance of the catalyst.

[0049] The first solvent is an aqueous solvent containing a soluble organic base and a soluble organic alcohol; the soluble organic base is ethylenediamine, triethylamine, diethylamine, pyridine, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, tetrahydropyrrole, N,N,N-trimethyl-1-adamantylammonium hydroxide, choline cation (C5H 14 ON +) and one or more of benzyltrimethylammonium, for example, the soluble organic base is ethylenediamine, diethylamine, or ethylenediamine and diethylamine; the soluble organic alcohol specifically refers to a water-soluble organic alcohol containing at least one hydroxyl group and a molecular weight not exceeding 1000; the soluble organic alcohol is one or more of methanol, ethanol, propanol, ethylene glycol and glycerol, for example, the soluble organic alcohol is methanol, ethanol, or methanol and ethanol; the silicon source is montmorillonite, coal gangue, diatomaceous earth, silica sol, solid silica gel, silicon oxide, aluminum silicate , potassium silicate, sodium silicate, sodium aluminosilicate, ZSM-5 molecular sieve, oblique hair molecular sieve, Y-type molecular sieve, Beta molecular sieve and all-silicon molecular sieve, for example, the silicon source is silica sol, silicon oxide, or silica sol and silicon oxide, etc.; the aluminum source is one or more of pseudo-boehmite, aluminum sol, aluminum oxide, aluminum hydroxide, sodium aluminum hydride, aluminum sulfate, potassium aluminum sulfate, aluminum nitrate, aluminum chloride, sodium aluminate, aluminum silicate and aluminum acetate, for example, the aluminum source is aluminum sol, aluminum oxide, or aluminum sol and aluminum oxide, etc.

[0050] The mass ratio of the first solvent to the carrier is 1-300, for example, a mass ratio of 1, 10, 50, 100, 150, 200, 250 or 300; the molar ratio of the soluble organic base to the silicon source is 0.1-20, for example, a molar ratio of 1, 5, 10, 15 or 20; the volume ratio of the soluble organic alcohol to the water in the first solvent is 0.1%-30%, for example, a volume ratio of 1%, 5%, 10%, 15%, 20%, 25% or 30%; the molar ratio of the silicon source, the aluminum source and the water in the first solvent is 0.1%-30%. The molar ratio is 1:5-35:50-1000, for example, 1:5:50, 1:10:100, 1:15:200, 1:20:300, 1:25:500, 1:30:750 or 1:35:1000, etc., which is used to control the silicon-aluminum ratio of the carrier. The silicon-aluminum ratio is a key indicator affecting the performance of the molecular sieve. The higher the silicon-aluminum ratio, the more stable the molecular sieve structure, but the surface acidity decreases, which is not conducive to adsorption and catalytic reactions; on the contrary, the lower the silicon-aluminum ratio, the stronger the surface acidity, but the worse the structural stability.

[0051] In step S1, a suspension is obtained by shearing, including: obtaining a carrier particle size D by shearing 50 For a suspension of 100nm-500nm, for example, the carrier particle size D 50 It is 100nm, 200nm, 300nm, 400nm or 500nm, etc.

[0052] In step S1, a silicon source and an aluminum source are added to the suspension for a reconstruction reaction, including: adding the silicon source and the aluminum source to the suspension, and carrying out a reconstruction reaction under closed conditions. The reconstruction reaction temperature is 120°C-200°C, for example, the reconstruction reaction temperature is 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, 190°C or 200°C, and the reconstruction reaction time is 6.5h-72h, for example, the reconstruction reaction time is 6.5h, 12h, 18h, 24h, 36h, 48h, 60h or 72h, etc. The purpose is to allow the crushed grains to undergo a rapid reconstruction reaction with the silicon source and the aluminum source under the guidance of the organic base to form a carrier of fine grains. Optionally, the reconstruction reaction temperature is 150°C-180°C, for example, the reconstruction reaction temperature is 150°C, 160°C, 170°C or 180°C, etc.

[0053] S2. Dissolve the soluble precursor of the active component in a second solvent to obtain a first solution; add the reconstructed support into a third solvent and stir evenly, add a surface charge regulator, and then add the first solution for hydrothermal treatment to achieve quantitative ion exchange. After the hydrothermal treatment, filter, wash, dry and calcine to obtain the initial catalyst.

[0054] This step is the process of adsorption and effective binding of active components. By adding a surface charge regulator, the carrier becomes electronegative, which facilitates electrostatic adsorption with active components, allowing the active components to be enriched on the carrier, providing an important basis for quantitative ion exchange. Hydrothermal treatment causes the carrier to dissociate from the surface charge regulator, and then combines with nearby active components, thereby achieving quantitative loading of active components, making the loading amount controllable and improving accuracy. Quantitative ion exchange also promotes the dispersion of active metals. The more active metal elements are exposed, the greater the probability of chemical adsorption, and the more hydrocarbons and nitrogen oxides are adsorbed at low temperatures.

[0055] The second solvent and the third solvent are water, and the coordinating anions of the soluble precursor of the active component are one or more of hydrochloride ion, nitrate ion, nitrite ion, carbonate ion, acetate ion, bicarbonate ion, sulfate ion, sulfite ion, bisulfate ion, fluoride ion, iodate ion, chlorate ion, cyanate ion and thiocyanate ion, for example, the coordinating anions are hydrochloride ion, nitrate ion, or hydrochloride ion and nitrate ion; the surface charge regulator is one or more of ammonia water, nitric acid, acetic acid, formic acid, dimethyl oxalate, methylal, ethylhydrazine, ethylhydroxylamine, diethylhydroxylamine, L-alanine-4-nitroaniline, isobutanolamine, acrylic acid and sodium polyacrylate, for example, the surface charge regulator is formic acid, acetic acid, or formic acid and acetic acid.

[0056] In step S2, the reconstructed carrier is added to the third solvent and stirred evenly, including: adding the reconstructed carrier to the third solvent, stirring evenly under conditions of 40°C-100°C, for example, the stirring temperature is 40°C, 50°C, 60°C, 70°C, 80°C, 90°C or 100°C, and adjusting the pH value to 1-10, for example, the pH value is 1, 2, 3, 4, 5, 6, 7, 8, 9 or 10, to avoid excessive alkalinity, which causes precipitation of the active components and affects the binding effect.

[0057] In step S2, the first solution is then added for hydrothermal treatment to achieve quantitative ion exchange, including: adding the first solution and heating and stirring to form a second solution, the heating and stirring temperature is 50°C-100°C, for example, the heating and stirring temperature is 50°C, 60°C, 70°C, 80°C, 90°C or 100°C, and the heating and stirring time is 6h-12h, for example, the heating and stirring time is 6h, 7h, 8h, 9h, 10h, 11h or 12h, etc., the process is mainly adsorption, and is also accompanied by ion exchange; when the supernatant of the second solution is colorless, The representative carrier is completely enriched with the active component, and the second solution is hydrothermally treated to provide a driving force for the active component to enter the interior of the carrier and promote the migration of the active component. The hydrothermal treatment temperature is 120°C-180°C, for example, the hydrothermal treatment temperature is 120°C, 130°C, 140°C, 150°C, 160°C, 170°C or 180°C, and the hydrothermal treatment time is 2h-48h, for example, the hydrothermal treatment time is 2h, 6h, 12h, 24h, 36h or 48h, etc.

[0058] The main function of the surface charge modifier is to generate species after binding with the carrier. The species structure is shown below:

[0059] The species make the carrier electronegative, which is easy to undergo electrostatic adsorption with active metal cations or cationic groups. The active metal precursors are all enriched on the carrier surface and in the micropores, providing a basis for quantitative ion exchange reactions.

[0060] In the traditional sense, ion exchange reactions involve the direct exchange of active component ions in a solution with ions on a carrier. However, since ion exchange is a microscopic and uncontrollable process, it is difficult to achieve quantitative loading of active components. In the quantitative ion exchange reaction of this embodiment, the active component is completely enriched on the carrier surface according to a preset metering method, and then the active component is bound to the ion exchange site of the carrier under a hydrothermal environment. The species formed by the surface charge regulator and the carrier gradually dissociate with heating and stirring, entering the liquid phase environment, and the adsorbed active metal cations or cationic groups migrate to the ion exchange site of the carrier to form an effective ZM-OH bonding structure.

[0061] S3. Dissolving the precursor of the auxiliary agent in a fourth solvent, loading the auxiliary agent in the fourth solvent on the initial catalyst by a catalyst loading method, and drying and calcining the initial catalyst to obtain a low-temperature adsorption catalyst.

[0062] This step is the process of dispersion and precipitation of the additive.

[0063] The precursor of the auxiliary agent is one or more of barium nitrate, barium acetate, barium chloride, barium sulfate, barium carbonate, barium ethanol, barium phosphate, barium tert-butoxide, barium aluminum oxide, barium hydrogen phosphate, barium acetylacetonate, isopropoxy barium, barium dihydrogen phosphate, barium di(2-hexyl acetate), barium molybdate, barium hydroxide, barium titanate, barium perchlorate and barium oxide. For example, the precursor is barium acetate, barium nitrate, or barium acetate and barium nitrate; the fourth solvent is water; and the catalyst loading method is an equal volume impregnation method or a liquid phase deposition method.

[0064] In some embodiments, the nitrogen oxide adsorption performance test method includes: taking 1g of the sample to be tested and performing pretreatment, the pretreatment includes constant temperature treatment at 550°C for 30 minutes in nitrogen containing 10% oxygen, and then reducing the temperature to 100°C. After pretreatment, an adsorption test is performed, the adsorption temperature is 100°C, and the adsorption atmosphere conditions include nitrogen as the balance gas, 10% oxygen, 5% water, 500ppm nitrogen monoxide, and 500ppm carbon monoxide are introduced; the adsorption time is 10 minutes; and then desorption is performed, the desorption temperature range is 100°C-500°C, and the desorption heating rate is 5°C / min.

[0065] In some embodiments, the hydrocarbon adsorption performance testing method includes: taking 1 g of the sample to be tested and performing pretreatment, the pretreatment including constant temperature purging at 400°C in an argon environment for 1 hour, and performing an adsorption test after pretreatment. The adsorption temperature is room temperature, and the adsorption atmosphere conditions include nitrogen as the balance gas, 10% oxygen, and 2000 ppm propylene; the gas flow rate is 1000 mL / min; and then desorption is performed, the desorption temperature range is 25°C-500°C, and the desorption heating rate is 5°C / min.

[0066] Comparative Example 1

[0067] Take 325g of the carrier SSZ-13 molecular sieve and disperse it in 1000mL of deionized water, stir evenly, add 42.2g of N,N,N-trimethyl-1-adamantyl ammonium hydroxide and 10mL of ethanol; perform high-speed shearing, monitor the slurry liquid crystal particle size D50≤500nm and then stop shearing to obtain a suspension; add 5g of sodium aluminate and 45g of silica sol with a solid content of 30% to the suspension, stir thoroughly, then transfer to a sealed container, and perform constant temperature hydrothermal treatment at 170°C for 24h to carry out a reconstruction reaction; after the reconstruction reaction is completed, cool to room temperature, obtain a filter cake by high-speed centrifugal filtration, wash the filter cake, dry it at 120°C, and calcined at 550°C to obtain a reconstructed carrier SSZ-13 molecular sieve.

[0068] 6.5 g of palladium nitrate was dissolved in deionized water to prepare a palladium nitrate aqueous solution; the reconstructed carrier SSZ-13 molecular sieve was stirred and dispersed in 2000 mL of water, and dilute nitric acid was added to control the pH of the solution to ≤ 6. 1 mL of acrylic acid was added to adjust the surface charge of the reconstructed carrier; the palladium nitrate aqueous solution was slowly added, and the reaction was heated and stirred at 95°C for 6 hours. When the supernatant was monitored to be colorless and transparent, the solution was transferred to a hydrothermal synthesis reactor and hydrothermally treated at a constant temperature of 120°C for 12 hours; after the hydrothermal treatment was completed, the solution was cooled to room temperature, the solution was separated into solid and liquid, and the filter cake was washed, dried, and calcined to obtain the initial catalyst, i.e., the powder Pd / SSZ-13 loaded with active components.

[0069] The above-mentioned nitrogen oxide adsorption performance test method was used for testing. The low-temperature nitrogen oxide adsorption capacity of the catalyst Pd / SSZ-13 was 85 μmol / g. At the same time, the nitrogen oxide adsorption performance was basically unaffected by impurity gases such as water vapor, carbon monoxide, methane, propane, and propylene, and nitrogen oxides were released by thermal decomposition in the range of 200°C-400°C.

[0070] The catalyst Pd / SSZ-13 was made into 40-60 mesh samples and divided into two parts. The first part of the catalyst was directly tested for nitrogen oxide adsorption performance to test the catalyst performance before aging; the second part of the catalyst was treated with 10% water vapor at a constant temperature of 800°C for 24 hours, and then tested for nitrogen oxide adsorption performance to test the catalyst performance after aging. The test results are shown in Figure 1. The nitrogen oxide storage characteristics of the catalyst Pd / SSZ-13 before and after aging are similar, with low-temperature nitrogen oxide adsorption storage capacities of 85μmol / g and 82μmol / g, respectively. The adsorption time for both is about 10 minutes, which can cover the vehicle cold start time. At the same time, the nitrogen oxide release temperature range of both is within the range of 250°C-450°C.

[0071] Comparative Example 2

[0072] 38g of barium acetate was added to deionized water to prepare a barium acetate solution. The active ingredient-loaded Pd / SSZ-13 powder from Comparative Example 1 was added to the barium acetate solution using an equal volume impregnation method. Deionized water was then slowly added dropwise until the powder reached adsorption saturation. The powder was then microwave-dried and calcined at 550°C to produce the low-temperature adsorption catalyst BaO-Pd / SSZ-13. The catalyst morphology is shown in Figure 4.

[0073] SSZ-13 molecular sieve belongs to CHA type molecular sieve, which is an octagonal small pore molecular sieve with weak low-temperature hydrocarbon adsorption capacity. It was tested using the aforementioned nitrogen oxide and hydrocarbon adsorption performance test method. The low-temperature nitrogen oxide adsorption capacity of the catalyst BaO-Pd / SSZ-13 was 476 μmol / g, and the low-temperature hydrocarbon adsorption capacity was 53 μmol / g. It thermally decomposed and released nitrogen oxides in the range of 200℃-400℃. At the same time, the released nitrogen oxides did not contain nitrous oxide.

[0074] Comparing the low-temperature nitrogen oxide adsorption performance of catalysts Pd / SSZ-13 and BaO-Pd / SSZ-13, as shown in Figure 2, the nitrogen oxide adsorption capacity of catalyst BaO-Pd / SSZ-13 far exceeds that of the former, reaching 476 μmol / g.

[0075] Comparative Example 3

[0076] The carrier SSZ-13 molecular sieve in Comparative Example 2 was replaced with a carrier ZSM-5 molecular sieve to prepare a low-temperature adsorption catalyst BaO-Pd / ZSM-5. The ZSM-5 molecular sieve belongs to the MFI type molecular sieve, which is a ten-membered ring mesoporous molecular sieve with a relatively strong low-temperature hydrocarbon adsorption capacity. The aforementioned hydrocarbon and nitrogen oxide adsorption performance test method was used for testing. The low-temperature nitrogen oxide adsorption capacity of the catalyst BaO-Pd / ZSM-5 reached 102 μmol / g, and the hydrocarbon adsorption capacity was 178 μmol / g.

[0077] Comparative Example 4

[0078] The palladium element in Comparative Example 1 was replaced with copper to prepare an initial catalyst, i.e., a powder Cu / SSZ-13 loaded with active components, with the copper content controlled at 2wt%-5wt%. The catalyst was subjected to a vehicle simulated flue gas test. Nitrogen was used as the balance gas in the simulated flue gas, and 10% oxygen, 10% water, 500ppm nitric oxide, and 500ppm ammonia were introduced. The total flow rate was 1000mL / min, the reaction space velocity was 30000 / h, and the temperature range for the test nitrogen oxide conversion rate exceeding 90% was 175°C-550°C.

[0079] Comparative Example 5

[0080] The BaO-Pd / SSZ-13 catalyst in Comparative Example 2 was placed upstream of the vehicle exhaust treatment, and the Cu / SSZ-13 catalyst in Comparative Example 4 was placed downstream of the vehicle exhaust treatment. The reductant filling port required for the SCR (Selective Catalytic Reduction) reaction was placed between the two. The vehicle simulated flue gas test method of Comparative Example 4 was used, and the temperature range for testing the nitrogen oxide conversion rate exceeding 90% was 100°C-550°C.

[0081] Comparative Example 6

[0082] The reductant filling port required for the SCR reaction in Comparative Example 5 was placed upstream of the BaO-Pd / SSZ-13 catalyst. Using the vehicle simulated flue gas test method of Comparative Example 4, the nitrogen oxide conversion rate was less than 90% at 150°C, indicating that the BaO-Pd / SSZ-13 catalyst was able to catalyze the oxidation-reducing agent ammonia, resulting in a decrease in the efficiency of the downstream SCR catalytic conversion of nitrogen oxides.

[0083] Comparative Example 7

[0084] The palladium element in Comparative Example 1 was replaced with platinum to prepare an initial catalyst, namely, a powder Pt / SSZ-13 loaded with active components. The catalyst was tested using the aforementioned nitrogen oxide and hydrocarbon adsorption performance test method. The low-temperature nitrogen oxide adsorption capacity of the catalyst Pt / SSZ-13 was 61 μmol / g, and the low-temperature hydrocarbon adsorption capacity was 53 μmol / g. This performance was basically unaffected by impurity gases such as water vapor, carbon monoxide, methane, propane, and propylene.

[0085] Comparative Example 8

[0086] Based on the catalyst Pt / SSZ-13 in Comparative Example 7, a low-temperature adsorption catalyst BaO-Pt / SSZ-13 was prepared by liquid phase deposition. The morphology of the catalyst is shown in FIG6 . The catalyst was tested using the aforementioned nitrogen oxide adsorption performance test method. The low-temperature nitrogen oxide adsorption capacity of the catalyst BaO-Pt / SSZ-13 was 368 μmol / g, and the hydrocarbon adsorption capacity was 89 μmol / g.

[0087] Comparative Example 9

[0088] The carrier SSZ-13 molecular sieve in Comparative Example 2 was replaced with a carrier LTA molecular sieve to prepare a low-temperature adsorption catalyst BaO-Pd / LTA. The LTA molecular sieve is an octagonal small-pore molecular sieve with relatively weak low-temperature hydrocarbon adsorption capacity and strong nitrogen oxide adsorption performance. The above-mentioned nitrogen oxide and hydrocarbon adsorption performance test method was used for testing. The low-temperature nitrogen oxide adsorption capacity of the catalyst BaO-Pd / LTA was 337 μmol / g, and the low-temperature hydrocarbon adsorption capacity was 53 μmol / g.

[0089] Comparative Example 10

[0090] Take 500g of carrier Beta molecular sieve and disperse it in 1500mL of deionized water, stir evenly, add 50g of tetraethylammonium hydroxide and 14mL of methanol; perform high-speed shearing and monitor the size of the liquid crystal particles D in the slurry. 50 After the particle size is ≤500nm, shearing is stopped to obtain a suspension; 4.6g of sodium aluminate and 60g of silica sol with a solid content of 30% are added to the suspension, and the mixture is fully stirred. The suspension is then transferred to a sealed container and subjected to a constant temperature hydrothermal treatment at 180°C for 12h to perform a reconstruction reaction; after the reconstruction reaction is completed, the mixture is cooled to room temperature, and a filter cake is obtained by high-speed centrifugation. The filter cake is washed, dried at 120°C, and calcined at 550°C to obtain a reconstructed carrier Beta molecular sieve.

[0091] 8.4 g of silver nitrate was dissolved in deionized water to prepare a silver nitrate aqueous solution; the reconstructed carrier Beta molecular sieve was stirred and dispersed in 2000 mL of water, and ammonia water was added to control the pH of the solution to ≤10. 1 mL of isobutanolamine was added to adjust the surface charge of the reconstructed carrier; the palladium nitrate aqueous solution was slowly added, and the reaction was heated and stirred at 95°C for 6 hours. When the supernatant was monitored to be colorless and transparent, the solution was transferred to a hydrothermal synthesis reactor and hydrothermally treated at a constant temperature of 120°C for 12 hours; after the hydrothermal treatment, the solution was cooled to room temperature, and the solution was separated into solid and liquid. The filter cake was washed, dried, and calcined to obtain the initial catalyst, i.e., powdered Ag / Beta loaded with active components. The morphology of the catalyst is shown in Figure 5.

[0092] Beta molecular sieve is a BEA type molecular sieve, which is a twelve-membered ring large-pore molecular sieve with a strong low-temperature hydrocarbon adsorption capacity. It was tested using the aforementioned nitrogen oxide and hydrocarbon adsorption performance test method. The low-temperature nitrogen oxide adsorption capacity of the catalyst Ag / Beta was 17μmol / g, and the low-temperature hydrocarbon adsorption capacity was 42μmol / g.

[0093] Comparative Example 11

[0094] 40g of barium chloride was added to deionized water to prepare a barium chloride solution. Using an equal volume impregnation method, the active ingredient-loaded Ag / Beta powder from Comparative Example 10 was added to the barium chloride solution. Deionized water was slowly added dropwise until the powder was saturated with adsorption. The powder was then microwave-dried and calcined at 550°C to produce the low-temperature adsorption catalyst BaO-Ag / Beta.

[0095] The above-mentioned nitrogen oxide and hydrocarbon adsorption performance test method was used for testing. The low-temperature nitrogen oxide adsorption capacity of the catalyst BaO-Ag / Beta was 31μmol / g, and the low-temperature hydrocarbon adsorption capacity was 296μmol / g. It can adsorb and store hydrocarbons below 200℃ and release them by thermal decomposition in the range of 200℃-400℃.

[0096] Comparative Example 12

[0097] Based on the catalyst Pd / SSZ-13 in Comparative Example 1, a low-temperature adsorption catalyst BaO-Pd / SSZ-13 with a barium content of 5% was prepared by liquid phase deposition. The catalyst was tested using the aforementioned nitrogen oxide and hydrocarbon adsorption performance test method. The low-temperature nitrogen oxide adsorption capacity of the catalyst reached 235 μmol / g, and the hydrocarbon adsorption capacity was 46 μmol / g.

[0098] Comparative Example 13

[0099] Based on the catalyst Pd / SSZ-13 in Comparative Example 1, low-temperature adsorption catalysts BaO-Pd / SSZ-13 with barium contents of 2%, 3%, 4%, 6%, 7% and 8% were prepared by liquid phase deposition method, and tested by the above-mentioned nitrogen oxide and hydrocarbon adsorption performance test method. The low-temperature nitrogen oxide adsorption amounts of this type of catalyst were 93 μmol / g, 137 μmol / g, 283 μmol / g, 461 μmol / g, 455 μmol / g and 453 μmol / g, respectively, and the hydrocarbon adsorption amounts were 58 μmol / g, 54 μmol / g, 50 μmol / g, 47 μmol / g, 44 μmol / g and 43 μmol / g, respectively.

[0100] Comparative Example 14

[0101] The palladium element in Comparative Example 12 was replaced with palladium and platinum elements, with a molar ratio of Pt to Pd of 1, to prepare a low-temperature adsorption catalyst BaO-Pt-Pd / SSZ-13. The catalyst was tested using the aforementioned nitrogen oxide and hydrocarbon adsorption performance test method. The low-temperature nitrogen oxide adsorption capacity of the catalyst BaO-Pt-Pd / SSZ-13 was 438 μmol / g, and the hydrocarbon adsorption capacity was 52 μmol / g.

[0102] Comparative Example 15

[0103] The silver element in Comparative Example 11 was replaced with silver and cerium elements, with a molar ratio of Ce to Ag of 3, to prepare a low-temperature adsorption catalyst BaO-Ag-Ce / Beta. The catalyst was tested using the aforementioned nitrogen oxide and hydrocarbon adsorption performance test method. The low-temperature nitrogen oxide adsorption capacity of the catalyst BaO-Ag-Ce / Beta was 118 μmol / g, and the hydrocarbon adsorption capacity was 312 μmol / g.

[0104] Comparative Example 16

[0105] The carrier SSZ-13 molecular sieve in Comparative Example 2 was directly combined with the active component without undergoing a reconstruction reaction to prepare a low-temperature adsorption catalyst BaO-Pd / SSZ-13. The catalyst was tested using the aforementioned nitrogen oxide and hydrocarbon adsorption performance test method. The low-temperature nitrogen oxide adsorption capacity of the catalyst BaO-Pd / SSZ-13 was 165 μmol / g, and the hydrocarbon adsorption capacity was 44 μmol / g.

[0106] Comparative Example 17

[0107] The Beta molecular sieve carrier in Comparative Example 11 was directly combined with the active component without undergoing a reconstruction reaction to prepare a low-temperature adsorption catalyst BaO-Ag / Beta. The catalyst was tested using the aforementioned nitrogen oxide and hydrocarbon adsorption performance test method. The low-temperature nitrogen oxide adsorption capacity of the catalyst was 24 μmol / g, and the hydrocarbon adsorption capacity was 136.16 μmol / g.

[0108] Example 1

[0109] The 325 g SSZ-13 molecular sieve carrier in Comparative Example 2 was replaced with 300 g SSZ-13 molecular sieve carrier and 100 g Beta molecular sieve carrier, and the low-temperature adsorption catalyst BaO-Pd / (SSZ-13+Beta) was prepared by the equal volume impregnation method. The catalyst has the ability to simultaneously and efficiently adsorb nitrogen oxides and hydrocarbons at low temperature. The above-mentioned nitrogen oxide and hydrocarbon adsorption performance test method was used for testing. As shown in Figure 3, the low-temperature nitrogen oxide adsorption capacity of the catalyst BaO-Pd / (SSZ-13+Beta) is 330 μmol / g, and the low-temperature hydrocarbon adsorption capacity is 524 μmol / g. Compared with Comparative Examples 2 and 11, the hydrocarbon adsorption capacity is greatly improved. Nitrogen oxides and hydrocarbons can be adsorbed and stored simultaneously below 200°C, released by thermal decomposition in the range of 200°C-400°C, and hydrocarbons are catalytically converted into water and carbon dioxide.

[0110] Example 2

[0111] 38 g of barium acetate was added to deionized water to prepare a barium acetate solution. The active component-loaded Pd / SSZ-13 powder from Comparative Example 1 and 100 g of Beta molecular sieve were simultaneously added to the barium acetate solution using an equal volume impregnation method. Deionized water was slowly added dropwise until the powder was saturated with adsorption. The powder was microwave-dried and calcined at 550°C to produce a low-temperature adsorption catalyst, BaO-Pd / (SSZ-13+Beta). Testing using the aforementioned nitrogen oxide and hydrocarbon adsorption performance test methods revealed that the catalyst exhibited low-temperature nitrogen oxide adsorption of 328 μmol / g and low-temperature hydrocarbon adsorption of 536 μmol / g.

[0112] Example 3

[0113] According to the method of Example 1, low-temperature adsorption catalysts BaO-Pd / (SSZ-13+Beta) having a mass ratio of SSZ-13 molecular sieve to Beta molecular sieve of 0.5, 1, 1.5, 2, 2.5 and 3 were prepared respectively. The above-mentioned nitrogen oxide and hydrocarbon adsorption performance test methods were used for testing. The low-temperature nitrogen oxide adsorption amounts of this type of catalyst were 281 μmol / g, 289 μmol / g, 295 μmol / g, 304 μmol / g, 328 μmol / g and 330 μmol / g, respectively; the hydrocarbon adsorption amounts were 536 μmol / g, 504 μmol / g, 484 μmol / g, 451 μmol / g, 424 μmol / g and 361 μmol / g, respectively. As the content of Beta molecular sieve decreased, the low-temperature hydrocarbon adsorption effect decreased significantly.

[0114] Example 4

[0115] The method of Example 1 was used to prepare a low-temperature adsorption catalyst BaO-NiO / (SSZ-13+Beta). The catalyst was tested using the aforementioned nitrogen oxide and hydrocarbon adsorption performance test methods. The low-temperature nitrogen oxide adsorption capacity of the catalyst was 313 μmol / g, and the low-temperature hydrocarbon adsorption capacity was 496 μmol / g.

[0116] Example 5

[0117] The method of Example 1 was used to prepare a low-temperature adsorption catalyst BaO-Pt-Pd / (SSZ-13+Beta). The catalyst was tested using the aforementioned nitrogen oxide and hydrocarbon adsorption performance test methods. The low-temperature nitrogen oxide adsorption capacity of the catalyst was 347 μmol / g, and the low-temperature hydrocarbon adsorption capacity was 541 μmol / g.

[0118] Example 6

[0119] The low-temperature adsorption catalyst BaO-Fe2O3 / (LTA+ZSM-5) was prepared by the method of Example 1 and tested using the aforementioned nitrogen oxide and hydrocarbon adsorption performance test method. The low-temperature nitrogen oxide adsorption capacity of the catalyst was 310 μmol / g, and the low-temperature hydrocarbon adsorption capacity was 520 μmol / g.

[0120] Example 7

[0121] The initial catalyst Pd / (SSZ-13+Beta) was prepared by the method of Comparative Example 1 and tested using the aforementioned nitrogen oxide and hydrocarbon adsorption performance test method. The low-temperature nitrogen oxide adsorption capacity of the catalyst was 100 μmol / g, and the low-temperature hydrocarbon adsorption capacity was 144 μmol / g.

[0122] Example 8

[0123] The method of Example 1 was used to prepare low-temperature adsorption catalysts BaO-Pd / (SSZ-13+Beta) with carrier silicon-aluminum ratios of 10, 20, and 30, respectively. The catalysts were tested using the aforementioned nitrogen oxide and hydrocarbon adsorption performance test methods. The low-temperature nitrogen oxide adsorption capacities of these catalysts were 488 μmol / g, 423 μmol / g, and 302 μmol / g, respectively; and the hydrocarbon adsorption capacities were 672 μmol / g, 532 μmol / g, and 429 μmol / g, respectively. As the silicon-aluminum ratio increased, the adsorption capacity gradually decreased.

[0124] Example 9

[0125] The method of Example 1 was used to prepare low-temperature adsorption catalysts BaO-Pd / (SSZ-13+Beta) with mass ratios of barium oxide to Pd of 10, 20, 35, and 50, respectively. The catalysts were tested using the aforementioned nitrogen oxide and hydrocarbon adsorption performance test methods. The nitrogen oxide adsorption amounts of these catalysts were 327 μmol / g, 352 μmol / g, 391 μmol / g, and 423 μmol / g, respectively; and the hydrocarbon adsorption amounts were 518 μmol / g, 486 μmol / g, 482 μmol / g, and 474 μmol / g, respectively. As the mass ratio of barium oxide to Pd increased, the adsorption amount of nitrogen oxides increased significantly.

[0126] Example 10

[0127] Low-temperature adsorption catalysts BaO-Pd / (SSZ-13+Beta) having a Pd to carrier mass ratio of 1%, 5%, and 10% were prepared using the method of Example 1. The catalysts were tested using the aforementioned nitrogen oxide and hydrocarbon adsorption performance test methods. The nitrogen oxide adsorption amounts of these catalysts were 342 μmol / g, 484 μmol / g, and 524 μmol / g, respectively; and the hydrocarbon adsorption amounts were 538 μmol / g, 566 μmol / g, and 543 μmol / g, respectively. The nitrogen oxide adsorption amount increased significantly with increasing Pd content.

[0128] Those skilled in the art should understand that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of the present disclosure (including the claims) is limited to these examples. Within the scope of the present disclosure, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of the different aspects of the embodiments of the present disclosure as described above, which are not provided in detail for the sake of simplicity.

[0129] The embodiments of the present disclosure are intended to cover all such substitutions, modifications, and variations that fall within the broad scope of the appended claims. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the embodiments of the present disclosure should be included in the scope of protection of the present disclosure.

Claims

1. A method for preparing a low-temperature adsorption catalyst, in, The low-temperature adsorption catalyst comprises a load and a carrier, the carrier comprises a first zeolite molecular sieve and a second zeolite molecular sieve, the first zeolite molecular sieve is an eight-membered ring molecular sieve, the second zeolite molecular sieve is a ten-membered ring molecular sieve or a twelve-membered ring molecular sieve, the load comprises an active component and / or an auxiliary agent, the active component is an active metal or an oxide of the active metal, the active metal is one or more of Pd, Pt, Au, Ag, Co, Sm, Ce, Mn, Cr, Fe, Cu, Ni, Ir, Re, Ru, Zr and Ti; the auxiliary agent is barium oxide; the first zeolite molecular sieve is one or more of AFX molecular sieve, AFT molecular sieve, AEI molecular sieve, CHA molecular sieve, ERI molecular sieve, LTA molecular sieve, KFI molecular sieve, RHO molecular sieve and RTH molecular sieve; the second zeolite molecular sieve is one or more of BEA molecular sieve, FAU molecular sieve, MFI molecular sieve, MOR molecular sieve, OFF molecular sieve and GME molecular sieve, the method comprises: The carrier is uniformly dispersed in a first solvent, and a suspension is obtained by shearing, a silicon source and an aluminum source are added to the suspension to perform a reconstruction reaction, and after the reconstruction reaction is completed, the reconstructed carrier is obtained by filtering, washing, drying and calcining; The soluble precursor of the active component is dissolved in a second solvent to obtain a first solution; the reconstructed carrier is added to a third solvent and stirred evenly, and a surface charge regulator is added, and then the first solution is added for hydrothermal treatment to achieve quantitative ion exchange, and after the hydrothermal treatment, the initial catalyst is obtained by filtering, washing, drying and calcining; The precursor of the auxiliary agent is dissolved in a fourth solvent, the auxiliary agent in the fourth solvent is loaded on the initial catalyst by a catalyst loading method, and the auxiliary agent loaded initial catalyst is dried and calcined to obtain a low-temperature adsorption catalyst.

2. The method for preparing the low-temperature adsorption catalyst according to claim 1, in, The mass ratio of the auxiliary agent to the active component is 0-50, the mass ratio of the active component to the carrier is 1%-10%, the silicon-aluminum ratio in the carrier is 0.1-200, and the mass ratio of the first zeolite molecular sieve to the second zeolite molecular sieve is 0.5-3.

3. The method for preparing the low-temperature adsorption catalyst according to claim 1, in, The method of obtaining a suspension by shearing includes: obtaining a carrier particle size D by shearing 50 It is a suspension of 100nm-500nm; The step of adding the silicon source and the aluminum source to the suspension to carry out a reconstruction reaction comprises: adding the silicon source and the aluminum source to the suspension, carrying out a reconstruction reaction under closed conditions, the reconstruction reaction temperature being 120° C.-200° C., and the reconstruction reaction time being 6.5 h-72 h.

4. The method for preparing the low-temperature adsorption catalyst according to claim 1, in, Adding the reconstructed carrier to the third solvent and stirring evenly comprises: adding the reconstructed carrier to the third solvent, stirring evenly at 40° C.-100° C., and adjusting the pH value to 1-10; The method of subsequently adding the first solution to perform hydrothermal treatment to achieve quantitative ion exchange includes: adding the first solution to heat and stir to form a second solution, the heating and stirring temperature is 50°C-100°C, and the heating and stirring time is 6h-12h; when the supernatant of the second solution is colorless, performing hydrothermal treatment on the second solution, the hydrothermal treatment temperature is 120°C-180°C, and the hydrothermal treatment time is 2h-48h.

5. The method for preparing the low-temperature adsorption catalyst according to claim 1, in, The first solvent is an aqueous solvent containing a soluble organic base and a soluble organic alcohol; the soluble organic base is one or more of ethylenediamine, triethylamine, diethylamine, pyridine, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, tetrahydropyrrole, N,N,N-trimethyl-1-adamantylammonium hydroxide, choline cation and benzyltrimethylammonium; the soluble organic alcohol is one or more of methanol, ethanol, propanol, ethylene glycol and glycerol; the silicon source is one or more of montmorillonite, coal gangue, diatomaceous earth, silica sol, solid silica gel, silicon oxide, aluminum silicate, potassium silicate, sodium silicate, sodium aluminosilicate, ZSM-5 molecular sieve, clinoptilol molecular sieve, Y-type molecular sieve, Beta molecular sieve and all-silicon molecular sieve; the aluminum source is one or more of pseudo-boehmite, aluminum sol, aluminum oxide, aluminum hydroxide, sodium aluminum hydride, aluminum sulfate, potassium aluminum sulfate, aluminum nitrate, aluminum chloride, sodium aluminate, aluminum silicate and aluminum acetate.

6. The method for preparing the low-temperature adsorption catalyst according to claim 5, in, The mass ratio of the first solvent to the carrier is 1-300; the molar ratio of the soluble organic base to the silicon source is 0.1-20; the volume ratio of the soluble organic alcohol to the water in the first solvent is 0.1%-30%, and the molar ratio of the silicon source, the aluminum source and the water in the first solvent is 1:5-35:50-1000.

7. The method for preparing the low-temperature adsorption catalyst according to claim 1, in, The second solvent and the third solvent are water, the coordinating anions of the soluble precursor of the active component are one or more of hydrochloride ion, nitrate ion, nitrite ion, carbonate ion, acetate ion, bicarbonate ion, sulfate ion, sulfite ion, bisulfate ion, fluoride ion, iodate ion, chlorate ion, cyanate ion and thiocyanate ion; the surface charge regulator is one or more of ammonia water, nitric acid, acetic acid, formic acid, dimethyl oxalate, methylal, ethylhydrazine, ethylhydroxylamine, diethylhydroxylamine, L-alanine-4-nitroaniline, isobutanolamine, acrylic acid and sodium polyacrylate.

8. The method for preparing the low-temperature adsorption catalyst according to claim 1, in, The precursor of the auxiliary agent is one or more of barium nitrate, barium acetate, barium chloride, barium sulfate, barium carbonate, barium ethanol, barium phosphate, barium tert-butoxide, barium aluminum oxide, barium hydrogen phosphate, barium acetylacetonate, isopropoxy barium, barium dihydrogen phosphate, barium di(2-hexyl acetate), barium molybdate, barium hydroxide, barium titanate, barium perchlorate and barium oxide; the fourth solvent is water; and the catalyst loading method is an equal volume impregnation method or a liquid phase deposition method.

Citation Information

Patent Citations

  • Double-molecular-sieve petroleum solvent oil refined adsorbent as well as preparation method and application thereof

    CN103769046A

  • Method for preparing high-silicon CHA type SSZ-13 molecular sieve

    CN107758691A

  • Low-temperature adsorption catalyst and preparation method thereof