Device, control device and method for laser-induced arc evaporation

The method enhances arc evaporation by controlling excitation and power pulses to address the limitations of material and layer architecture suitability, achieving improved layer properties and productivity while reducing energy input and heating in the laser-induced arc evaporation process.

WO2024240292A1PCT designated stage expired Publication Date: 2024-11-28VON ARDENNE ASSET GMBH & CO KG
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
PCT/DE2024/100422
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-19
Filing Date
2024-05-13
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

The limitations of arc evaporation in achieving full potential due to restricted material and layer architecture suitability, leading to incomplete exploitation of its capabilities, especially when conflicting requirements such as temperature sensitivity, layer properties, and productivity are involved.

Method used

A device and method for laser-induced arc evaporation that enhances the selection of the operating point by controlling excitation and power pulses to reduce excessive heating and energy input, allowing for a broader range of material selection and improved layer properties through precise control of plasma discharge parameters.

Benefits of technology

This approach enables reduced energy input into substrates during coating, minimizing excessive heating and maintaining layer quality and productivity, thereby expanding the applicability of arc evaporation processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure DE2024100422_28112024_PF_FP_ABST
    Figure DE2024100422_28112024_PF_FP_ABST
Patent Text Reader

Abstract

According to various embodiments, a method can comprise: actuating a laser source (110) and an electric power source (118) in accordance with an operating sequence; wherein the operating sequence comprises a plurality of phases, in every phase of which: by means of the laser source, an excitation pulse directed to a target (112) is generated to excite an arc discharge at the target, by means of the electric power source (118) a first electric power pulse (120) is generated to electrically supply the arc discharge, and / or by means of the electric power source (118) a second electric power pulse (122) is generated to accelerate a material flow (116) away from the target, said material flow being separated from the target by means of the arc discharge; wherein the plurality of phases have: one or more than one first phase, of which in every first phase, for each excitation pulse, the first electric power pulse (120) and / or the second electric power pulse (122) are / is generated; and a second phase in which, for each second electric power pulse (122), two excitation pulses (114) and / or two first electric power pulses (120) are generated.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Description

[0002] Device, control device and method for laser-induced arc evaporation

[0003] Various embodiments relate to a device, such as a vacuum arrangement, a control device and a method for laser-induced arc evaporation.

[0004] In general, a substrate (e.g. a workpiece) can be coated so that the chemical and / or physical properties of the substrate can be changed. The coating of the substrate can take place in a vacuum, in which one or more layers are deposited on the substrate by means of physical vapor deposition. An economically and technically attractive process for physical vapor deposition is so-called arc evaporation, in which a material is evaporated by means of an arc discharge. However, to date only a few materials and layer architectures are suitable for arc evaporation, which is why the potential of arc evaporation cannot usually be fully exploited. This applies analogously to other types of evaporation using a plasma, for which reference is made here to arc evaporation as an example.

[0005] The object arising from this background is achieved by various embodiments provided herein and aspects explained therein.

[0006] According to various embodiments, it has been recognized that arc evaporation provides additional flexibility in selecting the operating point to influence the properties of the resulting layer, particularly when additional conflicting requirements exist. These include, for example, requirements due to a temperature-sensitive substrate, requirements regarding the properties of the layer, and / or productivity requirements.

[0007] Various embodiments relate to a device, such as a vacuum arrangement, a control device and a method (for example for laser-induced arc evaporation), which increase the scope for selecting the operating point (AP) of the arc evaporation.

[0008] This makes it easier, for example, to mitigate the effects of arc evaporation, such as a high evaporation rate and / or a high degree of excitation and / or ionization of the resulting material vapor. This makes it easier, for example, to reduce the energy input into the substrate (e.g., a bipolar plate) during coating (e.g., with carbon), thus inhibiting excessive heating of the substrate and minimizing the associated losses in coating properties and / or productivity.

[0009] Various examples are described below that relate to what is described herein and illustrated in the figures. For ease of understanding, a laser-excited arc discharge (also referred to as a laser-induced arc discharge) is referred to as an exemplary pulse-excited plasma discharge, in which an arc discharge is excited by a laser pulse. The description here can be understood as applying analogously to any other type of pulse-excited plasma discharge that does not necessarily have to be an arc discharge and / or does not necessarily have to be excited by a laser pulse (see the following examples 53 and 54), for example, pulsed sputtering or the like.

[0010] Example 1 is a method (e.g. for carrying out laser-induced arc evaporation), comprising: controlling an excitation source (e.g. laser source) according to an operating sequence (e.g. implemented by means of code segments, e.g. stored); controlling an electrical power source according to the operating sequence; wherein the operating sequence preferably has several phases, of which in each phase preferably: by means of the excitation source (e.g. laser source) an excitation pulse (e.g. laser pulse) directed at a target is generated to excite a plasma discharge (e.g. arc discharge) on the target; by means of the power source a first electrical power pulse is generated to electrically supply the plasma discharge (e.g. arc discharge) by means of the target; and / or by means of the power source a second electrical power pulse is generated to accelerate (e.g. the ionized portion) of a plasma discharge (e.g.Arc discharge) from the target away from the target and / or towards a substrate holder (e.g. by means of which a bipolar plate is held).

[0011] An operating sequence is understood herein to be a specification according to which one or more actuators configured to influence the generation of the plasma discharge (e.g., arc discharge) are controlled. The operating sequence can specify one or more target parameters according to which the first and / or second power pulse and / or the excitation pulse (e.g., laser pulse) are generated. Examples of such parameters include: frequency, total power, pulse shape, pulse duration, (temporal) delay (e.g., a temporal offset) of a pulse, etc.

[0012] Example 2 is configured according to Example 1, wherein the first electrical power pulse is delivered by means of the target and / or an anode associated with the target; and / or wherein the second electrical power pulse is delivered by means of a substrate holder toward which the material flow is directed and / or an anode associated with the substrate holder. For example, a reference potential, such as electrical ground (also referred to as ground potential), can be applied to the anode.

[0013] Example 3 is set up according to example 1 or 2, wherein the plurality of phases comprise one or more than one first phase (also referred to as a first-type phase), of which in each first phase per excitation pulse (e.g.

[0014] Laser pulse), the first electrical power pulse and / or the second electrical power pulse are generated, and have a second phase (also referred to as a second-type phase) in which at least two (ie two or more than two) excitation pulses (e.g. laser pulses) and / or at least two (ie two or more than two) first electrical power pulses are generated per second electrical power pulse. Example 4 is set up according to Example 3, wherein the plurality of phases have at least two or three first phases per second phase.

[0015] Example 5 is configured according to any one of Examples 1 to 4, wherein the first electrical power pulse is generated according to a desired pulse length that is in a range of about 30 pis to about 600 pis, preferably in a range of about 150 pis to about 350 pis.

[0016] Example 6 is configured according to any one of Examples 1 to 5, wherein the first electrical power pulse is generated according to a desired pulse length that is in a range of about 250 pis to about 350 pis.

[0017] Example 7 is configured according to any one of examples 1 to 6, wherein the first electrical power pulse is generated according to a desired current pulse (e.g., amplitude, duration, slope, etc.); and / or wherein the second electrical power pulse is generated according to a desired voltage pulse (e.g., amplitude, duration, slope, etc.).

[0018] Example 8 is configured according to any one of examples 1 to 7, wherein each phase of the operating sequence is configured such that the first electrical power pulse is generated according to a desired pulse frequency, wherein a ratio of the desired pulse frequency to an actual length of the target is in a range of approximately 400 Hz / m (e.g., 750 Hz / m) to approximately 2500 Hz / m (e.g., 2000 Hz / m), preferably in a range of approximately 1200 Hz / m to approximately 2000 Hz / m, further preferably in a range of approximately 1200 Hz / m to approximately 1600 Hz / m.

[0019] Example 9 is configured according to any one of the examples, wherein the second electrical power pulse has a desired peak value in a range of approximately 300 V to approximately 1500 V (eg, 1000 V), preferably in a range of approximately 500 V to approximately 1000 V, further preferably in a range of approximately 700 V to approximately 900 V.

[0020] Example 10 is configured according to any one of examples 1 to 9, wherein the first electrical power pulse is generated according to a desired pulse shape (as a desired time dependence of the power), which is, for example, a sinusoidal pulse shape, a rectangular pulse shape or a triangular pulse shape (see also Fig.3) and / or has an asymmetrical pulse shape.

[0021] For example, the peak value of an asymmetric triangular pulse shape can be reached after approximately 65% ​​of the pulse duration. Alternatively or additionally, the falling edge of an asymmetric pulse shape can be as short as possible.

[0022] The contribution of the falling edge to the integrated current of an asymmetric pulse (also referred to as the current pulse integral) can, for example, be smaller than the contribution of the rising edge to the current pulse integral (e.g., approximately 50% of the latter). The contribution of the falling edge to the integrated power of an asymmetric pulse (also referred to as the power pulse integral) can, for example, be smaller than the contribution of the rising edge to the power pulse integral (e.g., approximately 25% of the latter). A triangular pulse shape is understood to be a time-dependence of the pulse in which the rising edge and / or the falling edge of the pulse have a constant gradient (e.g., the same gradient). Furthermore, the peak value can, but does not necessarily have to, be reached after half the pulse duration of the pulse.

[0023] A sine pulse shape refers to a time-dependent pulse, which can essentially be described by a sine function. For example, the rising edge and / or the falling edge can have a decreasing gradient toward the peak value, which, for example, tends toward zero toward the peak value.

[0024] Example 11 is configured according to Example 10, wherein the electrical power source comprises an output filter configured to influence a time dependency of the electrical power pulse in response to being controlled according to the desired pulse shape.

[0025] Example 12 is configured according to any one of Examples 1 to 11, wherein the first electrical power pulse is generated according to a desired time dependency having a gradient in a range of about 5'MA / s (megaamperes per second) to about 150'MA / s, e.g., 5'MA / s to about 70'MA / s, e.g., 10'MA / s to about 24'MA / s.

[0026] Example 13 is configured according to any one of Examples 1 to 12, wherein the target comprises or consists of carbon.

[0027] Example 14 is configured according to any one of Examples 1 to 13, wherein in at least one (e.g., each) phase of the plurality of phases, a first electrical power pulse and a second electrical power pulse are generated, which only partially overlap each other (in time).

[0028] Example 15 is configured according to Example 14, wherein, in the at least one (e.g., each) phase of the plurality of phases, the second electrical power pulse is generated with a time offset (also referred to as a target time offset and / or target time delay) with respect to the first electrical power pulse; and / or wherein, in the at least one (e.g., each) phase of the plurality of phases, the first electrical power pulse is generated according to a first target time interval (also referred to as a first target time delay) (e.g., a first target time delay = 0) from a start of the at least one phase, and wherein the second electrical power pulse is generated according to a second target time interval (also referred to as a second target time delay) (e.g., a second target time delay > 0, for example, up to 500 ps, ​​e.g.,up to 100 ps) from the beginning of the at least one phase, wherein the second target time interval is greater than the first target time interval. Alternatively or additionally, the target time interval can correspond to twice the duration of the first power pulse.

[0029] Illustratively, the second electrical power pulse in the at least one phase can begin before or after the first electrical power pulse. Example 16 is configured according to example 14 or 15, wherein the second electrical power pulse (e.g., according to a target time offset) is generated in the at least one phase after the first electrical power pulse.

[0030] Example 17 is configured according to any one of Examples 14 to 16, wherein the first electrical power pulse is generated according to a first target pulse duration and the second electrical power pulse is generated according to a second target pulse duration such that the second electrical power pulse ends (in time) before the first electrical power pulse.

[0031] Example 18 is configured according to any one of Examples 14 to 17, wherein the first electrical power pulse and the second electrical power pulse are generated such that the second electrical power pulse begins temporally after the first electrical power pulse and / or ends before the first electrical power pulse.

[0032] Example 19 is a computer program configured, when executed by a processor, to cause the processor to perform the method of any one of Examples 1 to 18.

[0033] Example 20 is a computer-readable medium storing instructions configured, when executed by a processor, to cause the processor to perform the method of any of Examples 1 to 18.

[0034] Example 21 is a control device comprising one or more than one processor configured to perform the method of any of Examples 1 to 18.

[0035] Example 22 is an apparatus (e.g., a vacuum assembly) comprising: the control apparatus according to Example 21; the power source; the excitation source (e.g., laser source); and a target holder for holding the target, wherein the target holder is electrically coupled to the power source; wherein the target holder optionally provides an axis of rotation and is configured to impart a rotational movement to the target about the axis of rotation.

[0036] Example 23 is configured according to Example 22, further comprising: a vacuum chamber coupled to the excitation source (e.g., laser source) and the power source, and in which the target holder is arranged.

[0037] Example 24 is configured according to example 22 or 23, further comprising: the substrate holder coupled to the power source and optionally arranged in the vacuum chamber.

[0038] Example 25 is configured according to Example 24, wherein a distance between the rotation axis (or a target held in the target holder) and the substrate holder is in a range of about 200 mm (eg, 410 mm) to about 750 mm or less.

[0039] Example 26 is configured according to any one of Examples 22 to 25, further comprising: a transport device for transporting a substrate along a transport path past the target holder. Example 27 is configured according to any one of Examples 22 to 26, further comprising: a particle filter arranged between the target holder and the substrate holder and configured to filter the material flow released from the target by means of the plasma discharge (e.g., arc discharge).

[0040] Example 28 is configured according to any one of Examples 22 to 27, further comprising: an anode coupled to the power source.

[0041] Example 29 is configured according to any one of examples 22 to 28, wherein the target holder is configured to drive the rotational movement (e.g., wherein the target holder has a drive, e.g., electric motor, configured to supply a torque to the target).

[0042] Example 30 is configured according to example 29, wherein a (eg target) frequency of the rotary movement is in a range of approximately 10 revolutions per minute to approximately 40 revolutions per minute, preferably in a range of approximately 20 revolutions per minute to approximately 30 revolutions per minute.

[0043] Example 31 is a method comprising: arranging (e.g., transporting) a (e.g., metallic) bipolar plate in a vacuum; and performing pulse-induced (e.g., laser-induced) arc evaporation (e.g., as a plasma discharge) in the vacuum by controlling an excitation source (e.g., laser source) and an electrical power source according to the method according to any one of Examples 1 to 18 (e.g., by means of a device according to any one of Examples 22 to 30), for example, configured according to Example 13, wherein the material stream dissolved out by means of the plasma discharge (e.g., arc discharge) comprises the carbon emitted toward the bipolar plate.

[0044] Bipolar plates (also called electrode plates) are used, for example, in fuel cells. In a fuel cell, several membrane electrode assemblies can be stacked. A bipolar plate can be arranged between each two adjacent membrane electrode assemblies. This can serve to separate the gases between the two adjacent membrane electrode assemblies. A bipolar plate can, for example, have one or more (e.g. meander-shaped) channels (e.g. in the form of trenches) (e.g. in the form of a flow profile) by means of which the reaction gases oxygen and hydrogen can be supplied to a respective membrane electrode unit. The multiple channels can serve to evenly distribute the reaction gases. Furthermore, the water produced during the reaction can be removed via channels in the bipolar plate (e.g. as water vapor).These channels can, for example, be milled or pressed into the bipolar plate on both sides.

[0045] A metallic bipolar plate can be electrically conductive and can therefore serve as an electrically conductive connection between the anode of one adjacent membrane electrode assembly and the cathode of the other adjacent membrane electrode assembly. To achieve high electrical conductivity (e.g., above 10 5To achieve a high thermal conductivity (e.g., s / m) of the (e.g., metallic) bipolar plates, these can be coated with a carbon layer, as described herein. Such a bipolar plate can be used, for example, for a proton exchange membrane fuel cell (a PEM fuel cell). For example, the metallic bipolar plate can comprise or consist of steel (e.g., type 316L and / or type 304L) and / or titanium. Alternatively or additionally, the metallic bipolar plate (e.g., comprising steel) can be coated with titanium. A native oxide layer can, for example, be removed prior to coating.

[0046] Optionally, the proton exchange membrane of the bipolar plate can be coated with a catalyst, such as platinum or palladium. Optionally, the bipolar plate can have a mounting structure (e.g., having one or more through holes) in its edge region, by means of which the bipolar plate can be mounted.

[0047] Example 32 is configured according to Example 31, wherein a carbon layer is formed on the bipolar plate by means of the material flow.

[0048] Example 33 is configured according to example 31 or 32, wherein the vacuum is provided by means of a vacuum chamber having, for example, two substrate transfer openings through which the bipolar plate is transported and between which a coating region is arranged into which the material stream is emitted.

[0049] Example 34 is configured according to Example 33, wherein the driving and the transporting are configured relative to each other such that a (eg dynamic) rate (ie amount of material / time) at which the carbon layer is formed on the bipolar plate (also referred to as deposition rate of the carbon layer) is greater than or equal to 50 nm'm / min.

[0050] Example 35 is configured according to Example 34, further comprising: performing an additional pulse-induced (e.g., laser-induced) plasma evaporation (e.g., arc evaporation) in the vacuum by additionally controlling an additional excitation source (e.g., laser source) and an additional electrical power source according to any one of Examples 1 to 34, for example, configured according to the method of claim 13, such that an additional carbon layer is formed between the carbon layer and the bipolar plate; wherein the additional controlling and the transporting are configured relative to one another such that an additional rate (amount of material / time) at which the additional carbon layer is formed (also referred to as a deposition rate of the additional carbon layer) is less than 50 nm / min and / or less than the deposition rate of the carbon layer.

[0051] Example 36 is configured according to any one of Examples 31 to 35, wherein the bipolar plate is coated with a titanium layer when performing a pulse-induced (e.g., laser-induced) plasma evaporation (e.g., arc evaporation), wherein the titanium layer is optionally formed in the vacuum, for example by means of physical vapor deposition (e.g., a sputtering process), before the pulse-induced (e.g., laser-induced) plasma evaporation (e.g., arc evaporation).

[0052] Example 37 is configured according to Example 36, performing a coating process to form the titanium layer on the bipolar plate before performing the plasma evaporation (e.g., before forming the carbon layer), e.g., arc evaporation. Example 38 is configured according to Example 36 or 37, wherein the titanium layer is formed by magnetron sputtering, by plasma evaporation (e.g., arc evaporation), or by high-pulse magnetron sputtering.

[0053] Example 39 is configured according to any one of Examples 36 to 38, wherein the titanium layer has a layer thickness in a range of about 20 nm to about 400 nm, preferably in a range of about 50 nm to about 150 nm.

[0054] Example 40 is configured according to any one of Examples 36 to 39, further comprising: plasma etching a surface of the bipolar plate on which the titanium layer is formed prior to forming the titanium layer.

[0055] Example 41 is configured according to any one of Examples 31 to 40, wherein the bipolar plate has a surface roughness with a mean arithmetic height less than or equal to 0.3 pim, preferably less than or equal to 0.2 pim, and / or a maximum height less than or equal to 4.0 pim, preferably less than or equal to 2.5 pim.

[0056] Example 42 is a bipolar plate having a carbon layer and / or additional carbon layer formed by the method of any one of Examples 31 to 41.

[0057] Example 43 is configured according to any one of Examples 1 to 42, wherein the carbon layer and / or additional carbon layer (e.g., formed by means of the material flow) has a layer thickness in a range from approximately 10 nm to approximately 150 nm, preferably in a range from approximately 20 nm (e.g., 30 nm) to approximately 90 nm.

[0058] Example 44 is configured according to any one of Examples 1 to 43, wherein the carbon layer and / or additional carbon layer (e.g. formed by means of the material flow) has a surface contact resistance less than or equal to 10 mCTcm 2 , preferably less than or equal to 1 mCTcm 2 , further preferably less than or equal to 0.5 mQ'cm 2 (e.g. 0.3 mCTcm 2 ), and / or greater than 0.1 mC cm 2 has.

[0059] Example 45 is configured according to any one of Examples 1 to 44, wherein a carbon content of the carbon layer (eg formed by means of the material flow) and / or additional carbon layer is greater than approximately 90%, preferably greater than approximately 95%, further preferably greater than approximately 99%.

[0060] Example 46 is configured according to any one of Examples 1 to 45, wherein at least 60%, preferably at least 80%, further preferably at least 95%, of the carbon of the carbon layer (e.g. formed by means of the material flow) and / or additional carbon layer sp 2 -hy bridized.

[0061] Example 47 is configured according to any one of Examples 1 to 46, wherein the carbon layer and / or additional carbon layer (e.g. formed by means of the material flow) has a specific resistance of less than or equal to 1 Ωm, preferably less than or equal to 0.1 Ωm.

[0062] Example 48 is configured according to any one of Examples 1 to 47, wherein the carbon layer and / or additional carbon layer (e.g. formed by means of the material flow) has a contact angle to water greater than or equal to 60°, preferably greater than or equal to 85°, further preferably greater than or equal to 100°.

[0063] Example 49 is configured according to any one of Examples 1 to 48, wherein the carbon layer (eg formed by means of the material flow) and / or additional carbon layer has a refractive index in a range of about 2.0 to about 3.5, preferably in a range of about 2.5 to about 3.0, at a wavelength of about 0.5 pim.

[0064] Example 50 is configured according to any one of Examples 1 to 49, wherein the carbon layer (eg formed by means of the material flow) and / or additional carbon layer has a refractive index in a range of about 2.0 to about 5.0, preferably in a range of about 2.5 to about 3.5, at a wavelength of about 1 pim.

[0065] Example 51 is configured according to any one of Examples 1 to 50, wherein the carbon layer and / or additional carbon layer (e.g. formed by means of the material flow) has an average reflectance of less than or equal to 0.5 pim, preferably less than or equal to 0.3 pim, at a wavelength of approximately 0.5 pim.

[0066] Example 52 is configured according to any one of Examples 1 to 51, wherein the carbon layer and / or additional carbon layer (e.g., formed by means of the material flow) has a nanohardness in a range of approximately 10 GPa to approximately 80 GPa, preferably in a range of approximately 20 GPa to approximately 70 GPa, further preferably in a range of approximately 30 GPa to approximately 50 GPa.

[0067] Example 53 is any one of Examples 1 to 52, wherein the excitation source comprises a laser source configured to generate a laser pulse (e.g., directed at the target) as the excitation pulse; and / or wherein the plasma discharge comprises an arc discharge / or wherein the plasma evaporation comprises an arc evaporation.

[0068] Example 54 is any one of Examples 1 to 52, wherein the excitation source comprises an electrical power source configured to generate an electrical power pulse (e.g., directed at the target) as the excitation pulse; and / or wherein the plasma discharge comprises a glow discharge; and / or wherein the plasma evaporation comprises sputtering (i.e., atomization by means of a plasma), e.g., pulse magnetron sputtering, e.g., high-energy pulse magnetron sputtering (HiPIMS). In the context of a glow discharge, for example, a discharge pulse may be provided which comprises the excitation pulse and the first electrical power pulse, which, for example, merge into one another. The excitation pulse may, for example, excite a voltage breakdown which merges into the plasma discharge, which is supplied by means of the first electrical power pulse.

[0069] Example 55 a method (e.g. according to any one of examples 1 to 54), comprising: controlling an excitation source according to the operating sequence; controlling an electrical power source according to the operating sequence; wherein the operating sequence has a plurality of phases, of which in each phase: by means of the excitation source (110) an excitation pulse (114) directed at a target (112) is generated to excite a plasma discharge on the target (112); by means of the electrical power source (118) a first electrical power pulse (120) is generated to electrically supply the plasma discharge by means of the target (112); and / or by means of the electrical power source (118) a second electrical power pulse (122) is generated to accelerate a material stream (116) released from the target (112) by means of the plasma discharge away from the target (112) and / or towards a substrate holder (104);Updating the operating sequence based on a result of the plasma discharge, so that the plurality of phases: comprise one or more than one first phase, of which in each first phase the first electrical power pulse (120) and / or the second electrical power pulse (122) are generated per excitation pulse (114), and comprise a second phase in which: two excitation pulses (114) and / or two first electrical power pulses (120) are generated per second electrical power pulse (122), and / or a first electrical power pulse and a second electrical power pulse are generated which only partially overlap one another;

[0070] Example 56 is one of Examples 1 to 55, further comprising: determining (e.g., forming and / or updating) the operating sequence based on a result of the plasma discharge, e.g., based on a result of a coating process that occurs by means of the plasma discharge; wherein determining the operating sequence preferably comprises determining (e.g., forming and / or updating) the one or more first phases, and / or determining (e.g., forming and / or updating) the one or more second phases. Determining the operating sequence may, for example, comprise determining a ratio (e.g., of the number) of first phases to (e.g., of the number) of second phases. Determining the operating sequence may, for example, comprise, per second phase, a ratio (e.g., of the number, duty cycle, and / or power) of the excitation pulse (e.g., of the number, duty cycle, and / or power) of power pulses (e.g.,first power pulse and / or second power pulse). Determining the operating sequence may, for example, comprise determining an overlap (e.g., expressed as an overlap time and / or overlap integral) of the first electrical power pulse and the second electrical power pulse. Determining the operating sequence may, for example, comprise determining a state (e.g., power, temporal distribution, e.g., duration and / or start time, amplitude, etc.) of one or more than one power pulse (e.g., first power pulse and / or second power pulse).

[0071] Example 57 is any one of Examples 1 to 56, wherein the operating sequence is determined based on a result of a coating process (e.g., as a result of the plasma discharge) performed by means of the plasma discharge; and / or wherein the operating sequence is determined based on a state of a substrate (e.g., as a result of the plasma discharge) exposed to the plasma discharge. For example, a temperature (e.g., a change in the temperature) and / or a condition (e.g., a change in the condition) of the substrate can be considered as a condition.

[0072] Example 58 is one of Examples 1 to 57 arranged according to one of the appended claims (e.g.

[0073] 1 to 16); and / or is one of the appended claims (e.g. 1 to 16), which is further configured according to any one of examples 1 to 57.

[0074] They show, according to various embodiments: Figure 1 shows a vacuum chamber arrangement for coating by means of laser-induced arc evaporation according to various embodiments in a schematic plan view or side view;

[0075] Figures 2A to 2C each show different characteristics regarding a relationship between temperature and rate during coating by laser-induced arc evaporation and resulting properties.

[0076] Figure 3 different pulse shapes of power pulses according to different embodiments

[0077] Figure 4 shows a vacuum chamber arrangement for coating by means of laser-induced arc evaporation in a continuous system according to various embodiments in a schematic top view or schematic side view;

[0078] Figures 5A and 5B each show an exemplary continuous system with several coating devices for laser-induced arc evaporation according to various embodiments in a schematic plan view;

[0079] Figure 6 shows an operating sequence in a schematic diagram according to various embodiments;

[0080] Figures 7 and 8 each show an operating sequence with schematic timing diagrams according to various embodiments;

[0081] Figure 9A shows an exemplary power pulse according to various embodiments; and Figure 9B shows a diagram according to various embodiments.

[0082] In the following detailed description, reference is made to the accompanying drawings, which form a part hereof, and in which is shown by way of illustration specific embodiments in which the invention may be practiced. In this regard, directional terminology such as "top," "bottom," "front," "back," "fore," "rear," etc., is used with reference to the orientation of the described figure(s). Since components of embodiments can be positioned in a number of different orientations, the directional terminology is for purposes of illustration and is in no way limiting. It is to be understood that other embodiments may be utilized and structural or logical changes may be made without departing from the scope of the present invention.It is understood that the features of the various exemplary embodiments described herein may be combined with one another unless specifically stated otherwise. The following detailed description is therefore not to be construed in a limiting sense, and the scope of the present invention is defined by the appended claims.

[0083] Throughout this description, the terms "connected," "attached," and "coupled" are used to describe both a direct and an indirect connection (e.g., resistive and / or electrically conductive, e.g., an electrically conductive connection), a direct or indirect connection, and a direct or indirect coupling. In the figures, identical or similar elements are provided with identical reference numerals where appropriate.

[0084] According to various embodiments, the term "coupled" or "coupling" can be understood in the sense of a (e.g., mechanical, hydrostatic, thermal, and / or electrical), e.g., direct or indirect, connection and / or interaction. For example, several elements can be coupled to one another along an interaction chain, along which the interaction can be exchanged, e.g., a fluid (then also referred to as fluidically coupled). For example, two coupled elements can exchange an interaction with one another, e.g., a mechanical, hydrostatic, thermal, and / or electrical interaction. A coupling of several vacuum components (e.g., valves, pumps, chambers, etc.) to one another can include fluidically coupling them. According to various embodiments, "coupled" can be understood in the sense of a mechanical (e.g., physical) coupling, e.g.,by means of direct physical contact. A clutch can be configured to transmit a mechanical interaction (e.g., force, torque, etc.).

[0085] In the context of vacuum components (e.g., a pump, a chamber, a line, a valve, etc.), the term "coupled" or "coupling" can be understood in the sense of a connection to a common vacuum system. The components of the vacuum system can be configured to exchange a gas with each other via the coupling, whereby the coupling can be gas-separated from an external part of the vacuum system.

[0086] The actual state of an entity (e.g., a device, a system, or a process) can be understood as the actual or sensorily detectable state of the entity. The desired state of the entity can be understood as the desired state, i.e., a specification. Control can be understood as an intentional influencing of the current state (also referred to as the actual state) of the entity. The current state can be changed according to the specification (also referred to as the desired state), e.g., by changing one or more operating parameters (then also referred to as manipulated variables) of the entity, e.g., by means of an actuator. Regulation can be understood as controlling, whereby a change in state is additionally counteracted by disturbances. For this purpose, the actual state is compared with the desired state, and the entity is influenced in such a way, e.g.,by means of an actuator, so that the deviation of the actual state from the desired state is minimized. In contrast to purely forward-directed sequential control, the control thus implements a continuous influence of the output variable on the input variable, which is effected by the so-called control loop (also referred to as feedback). In other words, this can be understood as meaning that, alternatively or in addition to open-loop control (or actuation), closed-loop control can be used, or, alternatively or in addition to open-loop control, closed-loop control can be used.

[0087] The state of a controllable device (e.g. a structuring device) or a controllable process (e.g. structuring) can be specified as a point (also referred to as the working point or operating point) in a space (also referred to as the state space) spanned by the variable parameters of the device or process (also referred to as operating parameters). The state of the device or process is thus a function of the respective value of one or more operating parameters, which thus represents the state of the device or process. The actual state can be determined based on a measurement (e.g. using a measuring element) of one or more operating parameters (then also referred to as the controlled variable).

[0088] The term "control device" can be understood as any type of logic-implementing entity, which may, for example, comprise circuitry and / or a processor capable of executing software stored in a storage medium, firmware, or a combination thereof, and issuing instructions based thereon. The control device can, for example, be configured using code segments (e.g., software) to control the operation of a system (e.g., its operating point), e.g., a machine or a system, e.g., at least its kinematic chain.

[0089] Control can be understood as the intentional influencing of a system. The current state of the system (also referred to as the actual state) can be changed according to a specification (also referred to as the target state). The parameters explained here (also referred to as target parameters) of the target state can, for example, be implemented using code segments or be stored on a storage medium in some other way. Regulation can be understood as control, whereby a change in the state of the system is additionally counteracted by disturbances. Illustratively, the control system can have a forward-facing control path and thus clearly implement a sequential control that converts an input variable (e.g. the specification) into an output variable. However, the control path can also be part of a control loop, so that a closed-loop control is implemented.For control purposes, corresponding actuators of the system can be activated, which influence the actual state of the system. Examples of actuators include: a drive device (e.g., for providing torque), a valve (e.g., for controlling pressure), a switch (e.g., for closing a discharge path). The drive device can, for example, comprise a linear drive (e.g., a reciprocating piston) or an electric motor.

[0090] The term "actuator" (e.g., having an actuator) can be understood as a converter configured to influence a state, a process (e.g., a coating process), or a device in response to actuation of the actuator. The actuator can convert a control signal supplied thereto (by means of which the actuation takes place) into mechanical movements or changes in physical quantities such as pressure or temperature. An electromechanical (also referred to as electromotive) actuator can, for example, be configured to convert electrical power into mechanical power (e.g., through movement) in response to actuation. An electrothermal actuator can, for example, be configured to convert electrical power into thermal power in response to actuation.An electrothermal actuator can, for example, be configured to convert electrical power into thermal power in response to the control. An electrical actuator can, for example, be configured to convert electrical energy into electrical energy (e.g., of a specific voltage, current, and / or power) in response to the control.

[0091] An actuator can be configured to influence the actual state (also referred to as the operating point) of the process (e.g., its manipulated variable), which is supplied by the actuator. This influence can be direct or indirect. For example, the manipulated variable and the controlled variable can differ from each other. The controlled variable (e.g., pressure) can then be a function of one or more manipulated variables (e.g., voltage).

[0092] For example, the actuator can change an electrical voltage as a manipulated variable by means of which an arc discharge is supplied, so that as a result a coating rate or a layer thickness is changed as a controlled variable. For example, the actuator can change an inflow rate of a gas as a manipulated variable, so that as a result a pressure is changed as a controlled variable. For example, the actuator can change a property of a power pulse (e.g. frequency, total power, pulse shape, pulse duration, etc.) so that as a result a coating rate or a property of the carbon layer (e.g. layer thickness, electrical conductivity and / or carbon modification) is changed as a controlled variable. For example, the actuator can change a frequency at which an excitation pulse (e.g. laser pulse) is generated, so that as a result a coating rate or a property of the carbon layer is changed.

[0093] Examples of components of an actuator include: a power source (if present), a valve (e.g., a pump arrangement and / or gas supply device), a motor (e.g., a valve or a pump), a circuit (e.g., for controlling the excitation source (e.g., laser source)), or the like. The power source can, for example, be configured to generate one or more voltages (and / or a time dependence thereof), one or more currents (and / or a time dependence thereof), and / or power (and / or a time dependence thereof) according to the control and supply them to the coating process. The pump arrangement can, for example, be configured to pump out one or more gases according to the control and thus remove them from the coating process. The gas supply device can, for example, be configured to supply one or more gases to the coating process according to the control (also referred to as gas supply).The supplied gas can have a gas flow rate (i.e., gas flow per unit time). The gas flow can, for example, be a standard volume flow supplied to the coating process.

[0094] With regard to the control of an actuator, reference is made, among other things, to the more easily understood manipulated variable or its control value, which is influenced by the actuator. What has been described here can apply analogously to the controlled variable or its control value, which are fed to the actuator for control, and vice versa. The actuator acts as a converter, converting a control signal into the manipulated variable or its control value, so that the control value is a function of the control value. Modern actuators, for example, are provided as a complex assembly comprising an actuator and its own control device (also referred to as an actuator control device). The actuator control device can be configured to receive the control value as input using the control signal and to control the actuator according to the control value.The generation and transmission of the control variable then takes place within the actuator, so that the manipulated variable is fed to the actuator. Less complex actuators can only process the control variable as a control signal, so the control variable is fed to them for control.

[0095] More generally, an actuator can be controlled using a control signal, where the control signal can represent the manipulated variable or its control value and / or the controlled variable or its control value. Alternatively or additionally, the control signal can contain instructions that specify how the manipulated variable or its control value is to be changed (e.g., its relative change).

[0096] A "pulse" related to a physical quantity (e.g. power, then also referred to as a power pulse) can be understood as a temporal change of the quantity such that the value of the quantity increases (e.g. starting from an initial value, e.g. zero), exceeds a maximum (also referred to as a peak value), and then decreases again (e.g. to the initial value). The properties of the pulse are a function of the time dependence of the temporal change of the quantity. In a pulse, a value of the quantity can change over time from an initial value (e.g. base value) to a peak value (also referred to as the rising edge of the pulse) and then change over time from the peak value back to the initial value (also referred to as the falling edge of the pulse). Examples of the properties of the pulse include: a frequency of the pulse (specified as frequency), a starting time of the pulse (e.g.defined by a time delay with respect to a reference time), a length of the pulse (also referred to as pulse length or pulse duration), the peak value (e.g., an amplitude), the pulse shape, and / or the rise of the rising edge and / or the falling edge. The temporal duration (also referred to as pulse duration) of the pulse is specified herein in some aspects as an easily understandable width of the time-dependent value curve (e.g., half-width or twice the half-width) of the pulse, but can be specified differently by analogy. The half-width corresponds to the temporal width of the signal at half the peak value. In some aspects, the pulse duration is specified as a target time duration according to which the pulse is generated by means of a control device (e.g., by controlling an actuator).The pulse shape clearly describes the geometry of the curve, which describes the size as a function of time, and can be specified as a geometric shape, for example as a rectangle (then also called a rectangular function), sine, triangle, etc. If the pulse can be described, for example, as a rectangular function, the half-width of the rectangular function can be the width of the rectangular function.

[0097] If a pulse is generated here, it can be generated according to a target pulse, which clearly indicates the target state of the pulse to be generated. The target pulse can be specified, for example, as the target time dependency of the pulse to be generated or at least as properties thereof (e.g., target start time and / or target time delay, target pulse duration, target frequency, target peak value, target pulse shape, and / or target rise of the rising edge and / or the falling edge).

[0098] An "electrical power pulse" (short: power pulse) can be understood as a pulse according to a time-dependent electrical power and can be generated according to a target power pulse. An electrical power pulse can be implemented, for example, by means of a current pulse if the target power pulse defines a time dependence of the electrical current (e.g., a current peak value, a current rise, etc.), according to which the power pulse is, for example, controlled and / or regulated (e.g., by using this as a reference variable). Alternatively or additionally, an electrical power pulse can be implemented by means of a voltage pulse if the target power pulse defines a time dependence of the electrical voltage (e.g., a voltage peak value, a voltage rise, etc.), according to which the power pulse is, for example, controlled and / or regulated (e.g., by using this as a reference variable).

[0099] Exemplary electrical power pulses (e.g. as current pulses or as voltage pulses) are shown in FIG.3. Here, the current or voltage can be increased over time, t, from the initial value to the peak value V ma x or I m ax rise along the rising edge 302 and then fall back to the initial value along the falling edge 304. A target power pulse can, for example, have a target pulse shape. This can, for example, be a triangular shape (in 300a) or a sinusoidal shape (in 300b).

[0100] Arc evaporation, i.e. evaporation by means of an arc discharge, belongs to the class of thermal evaporation processes, which have in common that a material to be evaporated (here simply also referred to as coating material) is heated in such a way that it changes into its gaseous state (e.g. by absorbing latent heat). In this process, a melt of the material can (but does not necessarily have to) be present as an intermediate step. For example, this can evaporate from the melt or sublimate directly. Arc discharge is a form of gas discharge in which the plasma formed is drawn together into a tube (or descriptively thin thread, the so-called arc). Within the plasma tube thus formed, high gas temperatures (e.g. in a range from approximately 5000 Kelvin to approximately 50,000 Kelvin), current intensities (e.g.in a range of approximately 2000 amperes or more) as well as gas pressures, by means of which the coating material is converted into the gaseous phase (also referred to as evaporation). The arc discharge and thus the plasma formation can be of short duration, so that it occurs in pulses. Arc evaporation must be distinguished from the process of cathode atomization (so-called sputtering), in which the plasma is generated by means of a (e.g. continuous or pulsed) glow discharge. In cathode atomization, instead of thermal evaporation, the material is primarily mechanically atomized by large-area ion bombardment from the plasma, whereby the plasma is provided by means of the continuous glow discharge (e.g. at a voltage of less than 1000 volts). In cathode atomization, the pressure is also increased.

[0101] An excitation source (e.g. laser source) is a device that is designed to generate an excitation pulse, for example a radiation pulse, a power pulse (e.g. conveyed as a current pulse or a voltage pulse) or the like. The excitation source is generally designed to excite (e.g. trigger) a plasma discharge (e.g. plasma formation and / or electrical charge transfer by means of the plasma) using the excitation pulse. For example, an electrical voltage pulse can be used as an excitation pulse to trigger the plasma discharge. A laser source is a device that is designed to generate a laser beam. A laser beam is understood to be a directed (e.g. collinear and / or collimated) propagation of electromagnetic waves, which is, for example, stimulated and / or coherent.The laser source can, for example, comprise an electromagnetic resonator, through which the stimulated emission of the laser beam occurs. In contrast to a continuous-wave laser, a pulsed laser source generates pulsed laser radiation (also referred to as a laser pulse). The laser pulse can be generated by pulsed excitation or, for example, by means of a Q-switch in the laser itself. Examples of laser sources include gas lasers (e.g., carbon dioxide lasers) and solid-state lasers (e.g., semiconductor lasers).

[0102] In uncontrolled arc evaporation (also known as arc evaporation), the location where the arc discharge occurs is left to chance. Depending on the material, however, a local "burn-in" of the cathode can occur, so that the arc discharge is increasingly influenced by its own effects. However, this feedback follows interactions that are difficult to control, making it difficult to reproduce results.

[0103] Particularly in the case of arc evaporation (also referred to as ARC evaporation) of carbon, a modification of arc evaporation conventionally uses a laser to control the ignition of the arc discharge, which locally stimulates the formation of a plasma (also referred to as laser-induced or laser-assisted arc discharge). The laser generates a very short pulsed plasma within the plasma chamber between the anode and the cathode (to ignite an initial plasma). This initial plasma, lasting a few tens of ns (nanoseconds) to 100 ns, is then amplified in pulse length and power by an arc discharge using an electrical power source (e.g., pulsed power source and / or pulsed current source). The plasma thus formed lowers the impedance between the cathode and anode, so that a voltage U arc(also called arc voltage) leads to a discharge current through the plasma. In other words, a pulsed arc discharge can be excited using the laser.

[0104] To begin with, various aspects according to various embodiments are explained below.

[0105] The temporal course of the electrical current pulse (also called pulse current course) of such an arc discharge (also called cathode discharge) at this ignition point can be adjusted by means of a pulse current source, for example with regard to the pulse shape (e.g. triangle, square, half-sine, etc.), the amplitude I K and / or and the pulse length t P of the current pulse.

[0106] The laser is guided over the cathode using a mirror system, allowing the location of the arc discharge to be precisely adjusted. The laser influences the location of the ignition on the cathode, thus ensuring uniform, contact-free ablation of the target material.

[0107] For example, the frequency of the change of location and / or the pulse frequency of the current pulse can be adjusted using the clock frequency f of the laser.

[0108] These parameters can be divided into the so-called source power P Q transfer, for example according to the following relation:

[0109] The source power serves as a measure of the electrical power converted by the arc discharge to which the substrate is exposed. The source power P thus determined Q is, to a first approximation, proportional to the coating rate R in nm / min (nanometers per minute).

[0110] According to various embodiments, it has been recognized that the arc generated by the laser-induced arc discharge can enable a comparatively high deposition rate R(PQ) (i.e., the amount of material vaporized per unit time). In a continuous-flow system, the deposition rate (rate at which the transported substrate is coated) and / or the layer thickness are often specified normalized to the transport speed v of the substrate, which is then referred to, for example, as the dynamic deposition rate ddr (e.g., in nnrrn / min).

[0111] In a continuous flow system, the rate at which the transported substrate is coated (also referred to as coating rate) is often specified as the dynamic coating rate (e.g. in nnrrn / min), which is a function of the product of a layer thickness generated by coating and a transport speed at which the substrate is transported, which provides more comparable values ​​for the coating rate for different scenarios. The dynamic coating rate clearly indicates, for a rate R PQ), the resulting coated length I of the substrate per time t (e.g. in minutes), where I can be expressed, for example, according to the following relationship: I = v ■ t (e.g. in minutes). The ddr is therefore a function of the transport speed v at which the substrate is transported past the coating source.

[0112] In a (e.g. inline) continuous system, a substrate (such as the bipolar plate) can be transported by means of a transport device along a transport path past the cathode of the coating source, so that the material evaporated by means of the arc discharge (also referred to as material flow) hits the substrate and thus the material layer, such as the carbon layer (e.g. according to one or more than one specification, such as a target layer thickness) is formed.

[0113] Examples of parameters for which specifications exist include: the layer thickness (also referred to as target layer thickness), the properties of the coating (also referred to as target layer properties) and / or the throughput (also referred to as productivity), which can be expressed, for example, as the length of the substrate that is coated per time and / or is related to the entire system (then also referred to as system throughput).

[0114] Because the layer thickness is a function of the deposition rate and the transport speed, and thus also a function of the source power.

[0115] The coating of the substrate (also referred to as the deposition of a layer on the substrate) according to one or more than one specification (e.g., a target layer thickness and / or a target transport speed) can be carried out using the source power as a control variable. For example, to a first approximation, the source power is proportional to the target transport speed, provided the target layer thickness is invariant, which allows the system throughput to be scaled. However, the energy introduced into the substrate (e.g., normalized to the surface of the substrate) (also referred to as energy input) is a function of the target layer thickness and thus of the dynamic rate ddr.

[0116] According to various embodiments, it is addressed that the energy input of the coating plasma heats the substrate, which can cause its temperature to rise comparatively sharply. The properties of some substrates (e.g., their materials and / or coatings) can deteriorate above (at least) a critical material temperature. An analysis of the calorimetric properties of the substrate (e.g., the substrate material), which is explained below as an example, provides insight into this relationship, particularly for assessing the feasibility of the coating process using laser-induced arc evaporation on an industrial scale.

[0117] For example, the heat capacity C of a substrate, such as a stainless steel foil (e.g., for the production of a bipolar plate), decreases with increasing substrate thickness and can be in the range of 1 to 10 mJ / K (millijoules per Kelvin), e.g., normalized to a square centimeter of the substrate (then also referred to as the surface heat capacity) exposed to the plasma (e.g., in millijoules per square centimeter and per Kelvin). The surface heat capacity of a metallic foil of thickness t D from a material (such as stainless steel or titanium) of density p and specific heat capacity c results in C = cpt D . The energy input E (e.g. in J / cm 2) of a coating source leads to a temperature increase of the substrate by AT = E / C. At the same time, the substrate can release part of the heat (e.g. via radiation or thermal conduction), which inhibits the temperature increase of the substrate, but makes such a small contribution in a vacuum that this can be neglected in the dynamics of the coating and at least on the short time scale of the energy input in a first approximation.

[0118] In an industrial plant, processes that extract thermal energy from the substrate can be difficult to implement (e.g., compared to a laboratory plant). Furthermore, an industrial plant often has higher demands on its robustness to disturbances (e.g., compared to a laboratory plant).

[0119] In this context, it was recognized that one example of this is carbon layers that can be formed on a substrate (e.g., a bipolar plate). Such carbon layers can be subject to stringent requirements, for example, with regard to their properties (also referred to as layer properties), such as surface contact resistance, corrosion resistance, adhesion, etc., to ensure high quality.

[0120] These properties (e.g. quality) can also be influenced by a voltage applied to the substrate (also known as substrate bias voltage (U B), which accelerates the plasma ions further in addition to the initial energy. High-energy ions can, for example, influence the layer morphology, but also increase the energy input into the substrate. Depending on the plasma transmission in the coating chamber, a portion p of the arc current integral generated on the cathode is fed to the substrate as ion current with a time-of-flight-dependent delay. This ion current, which is a function of the substrate bias voltage (U B ) resulting additional power input P B (also called bias power) can be expressed in a first approximation by the following relation:

[0121] If there is a minimum energy for the high-energy ions to promote the formation of a desired layer morphology, this can result in a lower limit for the substrate bias voltage, for example in the range of 800V or higher.

[0122] The energy input into a substrate, which is transported past the plasma with an (e.g. invariant) actual transport speed, can thus be calculated as a function of two power sources (?< and P B ), which depend on the operating point of the plasma source and the substrate. This relationship is illustrated exemplarily in diagram 900b (see Fig. 9B), in which the energy density 911 introduced into the substrate is plotted schematically (au) against the bias power 913 and the source power 915.

[0123] From a maximum temperature T max As a specification, which the substrate should not exceed when coating the substrate, for example, the maximum energy input E max as a specification that is applied to the substrate during coating, for example according to the following relation: E max = T max — T o) C. Optionally, upstream processes to which the substrate is exposed and which determine the starting temperature T o of the substrate must also be taken into account. In an exemplary implementation, the maximum temperature (as the critical material temperature) may be approximately 600°C, above which carbon layers (e.g., formed by laser-induced arc evaporation) tend to grow in a morphology that deviates significantly from the desired one (e.g., a substantially amorphous carbon modification or a substantially crystalline carbon modification without crystallographic texture), and thus no longer meet the property requirements.

[0124] According to various embodiments, it has been recognized that, in addition to the parameters explained above, additional control variables (see exemplary embodiments) exist by means of which the energy input (and the resulting power input) into the substrate can be influenced (e.g., reduced) and which simultaneously enable high-quality carbon coatings produced with them. This is based, among other things, on the realization that only a portion of the high-energy ions is sufficient to promote the formation of the desired coating properties.

[0125] In an exemplary implementation, the source of the substrate bias voltage (also referred to as bias pulse current source) is provided (e.g., controlled) in such a way that only a portion of the ionized plasma is re-accelerated by means of the substrate bias voltage, which reduces the energy input into the substrate. For this purpose, pulse overlap and / or pulse omission are implemented according to various embodiments. For example, the period for which the substrate bias voltage is applied to the substrate can be provided in such a way that only a portion PO (in %) of the substrate power pulse is effective. For example, it has been recognized that the value of PO can be reduced to 25% without significantly affecting the layer properties.

[0126] In an exemplary implementation, the operating point (AP, of which AP1, AP2, AP3, AP4 are shown) can be determined as follows (see Fig. 9). According to one or more specifications, a target rate R = R1 can be determined for the coating rate R, for example, based on a specification for the layer thickness and / or the system throughput. In the example for material A, R = R1 results in an energy input at the operating point AP1 that exceeds the maximum energy input as threshold value 917 (black line). Based on this, the target rate could be set to R = R2 (see Variant 1). <R1 verringern und ein möglicher Arbeitspunkt AP2 auf Kosten der Schichtdicke verringern. Im Falle des Beispiels des Bildens einer Kohlenstoffschicht kann eine kritische Material-Temperatur als Schwellenwert 917 die dynamische Beschichtungsrate (z.B. pro Kathode) beschränken, beispielsweise auf weniger als 50 nnTm / min.At a fixed transport speed, the scope for selecting the operating point (also referred to as the selection range) is increased by the manipulated variable of the bias power 913. Illustratively, the bias power was traditionally specified invariantly based on the existing boundary conditions. In contrast, according to various embodiments, the bias power 913 is available as a manipulated variable, which can be varied alternatively or in addition to the manipulated variables of the source power and the transport speed.

[0127] Alternatively or additionally, various embodiments allow the energy input to be reduced to the operating point AP3 by means of pulse overlap and / or pulse omission (see variant 2) without necessarily having to change the target rate. For example, in the case of a thermally even more sensitive material B, both the target rate and the target rate can be reduced to R=R2. <R1 verringert (was eine eine geringer Schichtdicke nach sich zieht) werden als auch die Pulsüberdeckung und / oder Pulsauslassung verändert werden, um eine Beschichtung des Substrats im Arbeitspunkt AP4 gemäß den Anforderungen an die Qualität der Beschichtung zu begünstigen. Stellt R2 beispielsweise den Wert dar, bei dem die minimale Schichtdicke auf dem Substrat generiert wird, so wird für das Material B überhaupt erst ein AP (siehe AP4) erschlossen, der herkömmlich nicht zugänglich ist.

[0128] Fig. 1 illustrates a vacuum chamber arrangement 100 for coating by means of laser-induced arc evaporation according to various embodiments in a schematic top view (or a schematic side view). Pulsed signals are indicated by means of a circumflex " A " marked.

[0129] The vacuum arrangement 100 can have a vacuum chamber 102. A vacuum chamber 102 can be provided, for example, by means of a chamber housing in which one or more vacuum chambers can be provided. The chamber housing can be coupled, for example, to a pump arrangement, e.g., a vacuum pump arrangement, to provide a negative pressure or a vacuum (vacuum chamber housing) and can be configured so that it can withstand the effects of air pressure in the pumped-out state. The pump arrangement (comprising at least one vacuum pump, e.g., a high-vacuum pump, e.g., a turbomolecular pump) can make it possible to pump out a portion of the gas from the interior of the vacuum chamber 102. The or each vacuum chamber 102 can optionally have a chamber lid that seals the interior of the vacuum chamber 102 in a vacuum-tight manner. The plasma of the arc discharge can accordingly have a negative pressure (e.g., a vacuum).

[0130] The chamber housing, e.g. a vacuum chamber 102 provided therein, may be configured such that a negative pressure (ie a pressure less than atmospheric pressure) can be provided therein, e.g. a vacuum (ie a pressure of less than 0.3 bar), e.g. a pressure in a range of approximately 10 mbar to approximately 1 mbar (in other words rough vacuum) or less, e.g. a pressure in a range of approximately 1 mbar to approximately 10 3 mbar (in other words fine vacuum) or less, e.g. a pressure in a range of approximately 10 3 mbar to approximately 10 7 mbar (in other words high vacuum) or less, e.g. a pressure less than high vacuum, e.g. less than about 10 7 mbar. Atmospheric pressure (e.g., 1 bar) can be the pressure acting on the chamber housing from the outside.

[0131] The vacuum arrangement 100 may include a coating device 108. The coating device 108 may be configured for coating using a laser-induced arc discharge.

[0132] The gas pressure used to operate the coating device 108 (also referred to as operating pressure) and / or the gas or gas mixture supplied to the coating device 108 (also referred to as operating gas) can be highly application-dependent. For example, the operating pressure can be in a range from approximately 10 mbar (millibar) to approximately 5-10 4mbar. For example, the operating gas may comprise one or more of the following gases: oxygen (e.g., molecular oxygen, i.e., O2), nitrogen (e.g., molecular nitrogen, i.e., N2), hydrogen (e.g., molecular hydrogen, i.e., H2), one or more hydrocarbon compounds, or a gas mixture thereof. The operating gas may comprise the working gas (e.g., an inert gas) and / or a reactive gas. The reactive gas may, for example, comprise hydrogen. The coating apparatus 108 may comprise a target holder (not shown) for holding a target 112. The target holder may provide an axis of rotation and may be configured to impart rotational movement to the target 112 (when held in the target holder) about the axis of rotation.

[0133] The coating device 108 may include a laser source 110. The laser source 110 may be configured to generate a laser pulse 114 (ie, pulsed laser beam) in the direction of the target holder (eg, in the direction of the target 112 held in the target holder).

[0134] During operation of the vacuum assembly 100, the target 112 can be held in the target holder. The laser source 110 can be configured to generate the laser pulse 114 directed at the target 112. This laser pulse 114 can excite (e.g., induce) an arc discharge at the target 112. The target 112 can be operated as a cathode. Therefore, the target holder can also be referred to as a cathode end block.

[0135] A cathode end block (hereinafter also simply referred to as end block) can be a device which is configured to hold and supply a cathode, e.g. with a torque for rotating the cathode, with electrical energy and optionally with a cooling fluid. To provide the torque, the end block can have a drive device (e.g. a motor) or at least be coupled to such a device. The end block can be fastened inside a vacuum chamber, e.g. at a through-opening in the chamber wall (also referred to as a supply opening). The electrical energy and / or the cooling fluid (and optionally the torque) can be supplied to the end block through the supply opening. Optionally, one or more additional media can be supplied to the end block which serve to supply the cathode, e.g. data for controlling and / or reading out a sensor.

[0136] The target 112 may generally comprise or consist of a coating material which is to be converted into a gaseous state.

[0137] The target 112 can generally be tubular (a so-called tubular cathode). The target 112 can, for example, have a tubular support (a so-called support tube) on which a (e.g., brittle and / or fragile) coating material can be attached. For example, the target 112 can have a support tube by means of which the coating material is carried. Illustratively, the coating material can surround the target base tube in a jacket-like manner. Alternatively, the target 112 can have a tubular coating material (a so-called target tube) (e.g., a tube made of coating material) or be formed therefrom. The diameter of the tubular target can, for example, be in a range from approximately 10 cm (centimeters) to approximately 50 cm, e.g., approximately 20 cm or more.

[0138] The vacuum arrangement 100 can have an electrical power source 118 (can also be referred to as an electrical power supply). The electrical power source 118 can be configured to provide an operating voltage (e.g., a direct current voltage), e.g., pulsed. For this purpose, the electrical power source 118 can, for example, comprise or be formed from a pulsed current source. The operating voltage can be applied between an anode and the target holder. The operating voltage to be applied can clearly be configured such that an electrical current can discharge between the anode and the cathode, but not yet spontaneously ignite (uncontrolled start of the discharge). For this purpose, the operating voltage can be lower than the ignition voltage (i.e., the voltage at which an arc discharge is ignited) and higher than a burning voltage (i.e., the voltage at which an arc discharge occurs).For example, an anode potential at the anode may be in a range from about 10 to about 20 V. A cathode potential at the cathode may, for example, be negative (e.g., with respect to electrical ground) and / or its magnitude may be in a range from about 240 V to about 350 V.

[0139] The electrical power source 118 can be configured to generate a first electrical power pulse 120. The first electrical power pulse 120 can be applied to the target 112. The first electrical power pulse 120 can be configured to electrically supply the arc discharge (induced by the laser pulse 114) (e.g., via the target 112). For this purpose, the target holder can be electrically coupled to the electrical power source 118.

[0140] The vacuum arrangement 100 can have a control device 124. The control device 124 can be configured to control the laser source 110. For example, the control device 124 can control the laser source 110 to generate the laser pulse 114 and thus initiate a laser-induced arc discharge. The control device 124 can be configured to control the electrical power source 118. For example, the control device 124 can control the electrical power source 118 to generate the first electrical power pulse 120. In this case, the control device 124 can control the electrical power source 118 to generate the first electrical power pulse 120 according to a (first) desired power pulse (e.g., a desired current pulse). The first electrical power pulse 120 can be imparted by means of a current pulse generated (or controlled) by the electrical power source 118.

[0141] The electrical power source 118 may include an output filter configured to be controlled in response to a desired power pulse to influence a time dependency of the electrical power pulse.

[0142] The (first) target power pulse (e.g., target current pulse) may define a time dependence of the electrical power (e.g., the electrical current). According to various aspects, the (first) target power pulse may define a target current pulse according to a target time dependence with a gradient in a range of approximately 10-10 6 A / s until approximately 24' 10 6 A / s (see for example the rising and falling edges 302, 304 shown in FIG.3).

[0143] Consecutive pulses can be generated with a temporal offset from one another, e.g., according to a target frequency. This frequency can also be referred to as the pulse frequency. The target pulse frequency of the (first) target power pulse can, for example, be specified as in Example 9.

[0144] If reference is made herein to a target parameter (e.g., a target power pulse, a target time delay, and / or a target frequency, etc.), this can be implemented using code segments, which can be stored, for example, in a data memory associated with the control device 124. The code segments can be stored in the data memory in a suitable manner, for example, as a list (e.g., table), a series of values, an algorithm, etc. A data memory (more generally also referred to as a storage medium) can, for example, be a non-transitory data memory. The data memory can, for example, comprise or be formed from a hard disk and / or at least one semiconductor memory (such as read-only memory, random access memory, and / or flash memory). The read-only memory can, for example, be an erasable programmable read-only memory (can also be referred to as EPROM).The random access memory can be a non-volatile random access memory (also called NVRAM - "non-volatile random access memory").

[0145] Control performed by the control device 124 may be performed according to an operating sequence. This operating sequence may be stored in the data memory in a suitable manner, for example, as an algorithm or in another way using code segments.

[0146] The target holder can be configured to excite a rotational movement of the target 112 around a rotational axis. For example, the target holder can have a drive (e.g., an electric motor) configured to supply torque to the target. The control device 124 can be configured to control the drive of the target holder in order to thereby control the rotational movement (e.g., a rotational frequency). The rotational frequency can be, for example, as specified in Example 25.

[0147] By means of the arc, the (e.g., solid) target material can be at least partially converted (e.g., at the discharge point on the target 112) into the gaseous state (also referred to simply as the gaseous state or vapor). This conversion can also be referred to simply as evaporation, but can generally also involve sublimation (i.e., a direct transition from the solid state of the target material to the gaseous state). The material dissolved from the target 112 (e.g., evaporated from the target 112) by means of the arc discharge can form a material stream 116 away from the target 112.

[0148] During operation of the vacuum assembly 100, one (or more than one) substrate 106 can be coated using the material flow 116. For this purpose, the vacuum assembly 100 can have a substrate holder 104 configured to hold the one or more substrates. The substrate holder 104 can be arranged in the vacuum chamber 102. In various embodiments, a distance between the rotation axis and the substrate holder can range from approximately 410 mm to approximately 750 mm.

[0149] The or each substrate may generally comprise a workpiece, e.g., a semi-finished product (e.g., a rod, sleeve, or plate) or a component of a more complex device. Examples of a substrate include: a piston ring, a bearing component, a tool, a chain, a drive chain, an obtuse-angled geometry, a knife, or a sliding friction-sensitive component. The or each substrate may, for example, be cylindrical, plate-shaped, or have another shape. The or each substrate may comprise or be formed from at least one of the following: a ceramic, a glass, a semiconductor (e.g., amorphous, polycrystalline, or single-crystal semiconductor such as silicon), a metal, and / or a polymer (e.g., plastic). The ceramic may, for example, comprise an oxide, a nitride, and / or a carbide of a metal.

[0150] In the context of this description, a metal (also referred to as a metallic material) can comprise (or be formed from) at least one metallic element (i.e. one or more metallic elements), e.g. at least one element from the following group of elements: copper (Cu), iron (Fe), titanium (Ti), nickel (Ni), silver (Ag), chromium (Cr), platinum (Pt), gold (Au), magnesium (Mg), aluminum (Al), zirconium (Zr), tantalum (Ta), molybdenum (Mo), tungsten (W), vanadium (V), barium (Ba), hafnium (Hf), samarium (Sm), silver (Ag), and / or lithium (Li). For example, a metal can comprise or be formed from a metallic compound (e.g. an intermetallic compound or an alloy) or a compound of at least one metallic element (e.g. from the group of elements) and at least one non-metallic element (e.g. carbon), such as steel.

[0151] In one illustrative example, the substrate 104 can be a (e.g., metallic) bipolar plate, and the target 112 can comprise or consist of carbon, so that a carbon layer can be formed on the bipolar plate by means of the material flow 116 generated by the laser-induced arc discharge. The carbon layer can, for example, comprise or be formed from tetrahedral amorphous carbon, in which hydrogen is optionally incorporated. However, the carbon can also be present in another carbon modification.

[0152] The carbon of the carbon layer can, for example, be present in one of the following carbon modifications: graphite; amorphous carbon; tetrahedral carbon; diamond-like carbon; fullerenes; diamond; carbon nanotubes; amorphous-tetrahedral carbon; and / or nanocrystalline carbon, e.g., nanocrystalline graphite. Optionally, hydrogen can be incorporated into the carbon (i.e., a hydrogen-added carbon configuration).

[0153] According to various aspects, the electrical power source 118 can be configured to generate a second electrical power pulse 122. The second electrical power pulse 122 can be configured to accelerate the (e.g., ionized portion of) the material stream 116 away from the target 112 or toward the substrate holder 104. For this purpose, the substrate holder 104 can be electrically coupled to the electrical power source 118. The second electrical power pulse 122 can increase the kinetic energy with which the material of the material stream 116 strikes the substrate 106. This can, for example, form a more compact layer. In some applications, this second electrical power pulse 122 can even promote the achievement of desired properties (e.g., a minimum surface contact resistance or a minimum corrosion resistance in the case of a carbon-coated bipolar plate).The control device 124 can control the electrical power source 118 to generate the second electrical power pulse 122 according to a second desired power pulse (e.g., a desired voltage pulse). The second electrical power pulse 122 can be imparted by means of a voltage pulse generated (or controlled) by the electrical power source 118. A maximum pulse current of the arc discharge can be limited (e.g., by means of the operating sequence), for example, to a maximum pulse current in a range of approximately 1000 A to approximately 5000 A, preferably in a range of approximately 1600 A to approximately 3000 A, further preferably in a range of approximately 2000 A to approximately 2500 A.

[0154] According to various aspects, the laser pulse 114, the first electrical power pulse 120 and optionally also the second electrical power pulse 122 can be coordinated with one another, i.e. synchronized (e.g. by means of the operating sequence), e.g. such that they overlap with one another in time. For this purpose, the control device 124 can, for example, have a clock generator, by means of which the laser pulse 114, the first electrical power pulse 120 and optionally also the second electrical power pulse 122 are coordinated with one another. Each clock pulse of the clock generator can define a reference time, e.g. exactly one reference time per phase and / or at which the phase begins. Illustratively, the reference time can be a start of the phase.Optionally, there can be a time offset (e.g. in the pis range) between the laser pulse 114 and the first electrical power pulse 120 and / or between the laser pulse 114 and the first electrical power pulse 120 and / or between the first electrical power pulse 120 and the second electrical power pulse 122, etc., which can take into account, for example, the duration between the generation of the laser pulse 114 and its impact on the target 112 and / or the duration between the generation of the material stream 116 and its impact on the substrate 106. For example, the second electrical power pulse 122 (if it is generated in a cycle and / or a phase) can be generated with a (second) target time interval (also referred to as a target time delay) from the reference time (e.g. the start of the respective phase).Illustratively, the second electrical power pulse 122 can begin after the first electrical power pulse 120 (if the latter is generated without a target time delay or with a smaller target time delay than the second electrical power pulse 122).

[0155] According to various aspects, the substrate 106 can be coated by iteratively (according to a desired frequency) generating a respective arc discharge with an associated material flow 116. Iteration is understood herein as the repeated excitation of the arc discharge by means of one or more pulses, for example, by means of the laser pulse 114 and the first electrical power pulse 120. The laser pulse 114, the first electrical power pulse 120, and optionally the second electrical power pulse 122 can be generated per iteration.

[0156] For example, the operating sequence may have one or more than one phase of the first type, in which the laser pulse 114, the first electrical power pulse 120, and the second electrical power pulse 122 are generated per iteration. For example, the operating sequence may have one or more than one phase of the second type (which, for example, has twice the duration of the first phase), in which two (or more than two) iterations occur, of which the laser pulse 114 and the first electrical power pulse 120 are generated in each iteration, but the second electrical power pulse 122 is generated in only one of the two (or more than two) iterations. For example, the operating sequence may have at least one phase in which the laser pulse 114, the first electrical power pulse 120, and the second electrical power pulse 122 are generated, wherein the first electrical power pulse 120 and the second electrical power pulse 122 only partially overlap (in time).Although a single electrical power source 118 is described herein, it is understood that the vacuum assembly 100 may also include multiple electrical power sources, each power source capable of generating a power pulse described herein, for example, a first power source capable of generating the first power pulse and a second power source capable of generating the second power pulse.

[0157] Optionally, the vacuum arrangement 100 can include a particle filter arranged between the target holder and the substrate holder 104 and configured to filter the material stream 116 released from the target 112 by the arc discharge. Filtering a material stream can be understood as separating the material stream into a first part and a second part, wherein the first part is fed to the substrate 106 and the second part is not. For example, the second part of the material stream can be captured before it reaches the substrate 106.

[0158] FIG.2A to FIG.2C each show different characteristics of coating by laser-induced arc evaporation, namely with regard to a relationship between temperature and rate and its influence on the surface contact resistance, ICR, of the correspondingly produced layer, which is shown schematically.

[0159] The term "surface contact resistance" can refer to the contribution of the surface to the total resistance of a system, which can be attributed to the contact areas of electrical wires and connections as opposed to the intrinsic resistance.

[0160] It is understood that surface contact resistance is an exemplary material property and is used here for illustrative purposes. Accordingly, it is understood that the principles described herein may apply analogously to other properties.

[0161] As illustrated by the rate-temperature curve 204 in diagram 200a of FIG. 2A, a higher (e.g., dynamic) deposition rate, R, leads to a higher material temperature of the layer due to the energy input into the formed layer. Diagrams 200b and 200c show that the surface contact resistance, ICR, can increase with increasing temperature and rate, respectively.

[0162] For example, if a layer is to be produced that has a surface contact resistance less than or equal to a target contact resistance, ICR*, this limits the temperature that the material may reach during coating to a critical temperature, T c Since the temperature depends on the coating rate, the coating rate is also controlled to a critical coating rate, R c , limited. The critical temperature, T c , may be accompanied by a critical change in the properties of the layer (e.g. due to detachment of the layer).

[0163] The second electrical power pulse 122 described herein (e.g., as a voltage pulse, then also referred to as a bias voltage pulse) can promote the surface contact resistance to reach or fall below the target contact resistance, ICR*, (and / or other desired properties, such as a desired corrosion resistance). For example, in the case of a carbon coating, the use of the second electrical power pulse 122 can lead to a columnar structure of the carbon or at least promote its formation, which can improve properties such as the target contact resistance, ICR*, and / or the corrosion resistance. For example, with increasing peak value of the second electrical power pulse 122, a sp 2-hybridized carbon bond fraction can be increased. For example, the columnar structure can be created starting at a peak value of approximately 700 V. The columnar diameter can be less than or equal to 50 nm, preferably less than or equal to 25 nm.

[0164] The diagrams 200a, 200b, 200c shown in FIG.2A refer to a respective curve in the case that the second electrical power pulse 122 is generated per generation of the arc discharge (ie in each iteration).

[0165] It has been recognized that if this second electrical power pulse 122 is omitted in some iterations of generating the arc discharge, the temperature, T, of the layer can be reduced without significantly affecting the contact resistance, so that, for example, the target contact resistance, ICR*, can still be undercut. In this case, phases can occur in which multiple arc discharges are excited per second electrical power pulse 122.

[0166] Diagram 202a in FIG.2B shows a schematic rate-temperature curve 206 for the case where the second electrical power pulse 122 is omitted in some iterations. Diagrams 202a, 202b, 202c show that, at the same critical temperature, T c , the critical rate of R ciin the case of the rate-temperature curve 204 to RC2 in the case of the rate-temperature curve 206. Consequently, this enables the use of higher (e.g., dynamic) coating rates. According to various aspects, simply omitting the second electrical power pulse 122 from every tenth iteration enables a dynamic coating rate of significantly greater than or equal to 50 nnTm / min. By omitting the second electrical power pulse 122 from every fifth iteration, for example, a dynamic coating rate greater than or equal to 300 nnTm / min can be achieved in the case of coating the bipolar plate with carbon.

[0167] The control device 124 can be configured to implement the omission of a second electrical power pulse 122, e.g., to control it, e.g., by means of the operating sequence. For this purpose, the control device 124 can, for example, have a counter that counts the first and / or second power pulse and / or the generation of the laser pulse. However, omitting too many second electrical power pulses 122 can result in certain target properties no longer being achieved. Therefore, the omission of the second electrical power pulse 122 can be limited to at most every nth iteration, where n can be any natural number greater than or equal to two (e.g., three or more, e.g., four or more, e.g., five or more). This can depend on the target properties of the layer to be produced, the material, etc.For example, in the case of coating the bipolar plate with carbon, the omission of the second electrical power pulse 122 can be limited to a maximum of every fifth iteration so that the target contact resistance, ICR*, is still achieved. For example, the operating sequence can have one second-type phase per multiple (e.g., two, three, or four) first-type phases. A coating process can have multiple phases, each of which can have one or more iterations of generating the arc discharge. If the second electrical power pulse 122 is not omitted in the one or more iterations of a first phase, then in this first phase, exactly one first electrical power pulse 120 and exactly one second electrical power pulse 122 are generated per laser pulse.If the second electrical power pulse 122 is omitted in one of two iterations of a second phase, two laser pulses 114 and two first electrical power pulses 120 are generated per second electrical power pulse 122 in these two iterations of the second phase.

[0168] An exemplary operating sequence 600 in this regard is shown in FIG.6.

[0169] Furthermore, it was recognized that the temperature, T, of the layer can be additionally or alternatively reduced if the second electrical power pulse 122 and the first electrical power pulse 120 (if they are generated in one phase and / or one clock cycle) only partially overlap in time. This temporal overlap can also be referred to as pulse overlap. If a first pulse and a second pulse begin at the same time (e.g., the reference time of a clock cycle) and the first pulse and the second pulse end at the same time (e.g., because they have the same target pulse duration), then there is a complete temporal overlap. In this case, the pulse overlap is equal to 1 (i.e., 100%). If a pulse begins after another pulse (e.g., due to a target time delay with respect to the reference time of a clock cycle) and / or a pulse ends before another pulse (e.g.,(due to different target pulse durations), these pulses only partially overlap. In this case, the pulse overlap is less than 1 (i.e., less than 100%).

[0170] Illustratively, the temperature, T, of the layer can be additionally or alternatively reduced by reducing the pulse coverage.

[0171] FIG.7 shows an exemplary operating sequence 700 with a schematic timing diagram of the first electrical power pulse 120 and the second electrical power pulse 122, wherein the generation of the power pulse is shown over time t.

[0172] The operating sequence 700 may include multiple phases 701. In each phase 701, a first electrical power pulse 120 and a second electrical power pulse 122 may be generated.

[0173] Each electrical power pulse can be generated in such a way (e.g., according to a desired time delay and a desired pulse duration) that it has a start time, to, and an end time, ti, whose distance is specified as the pulse duration.

[0174] According to various aspects, the first electrical power pulse 120 (e.g., according to a first target time delay and a first target pulse duration) and the second electrical power pulse 122 (e.g., according to a second target time delay and a second target pulse duration) can be generated in a phase 701 such that they only partially overlap. As explained herein, they only partially overlap, for example, if they begin at a different start time, t0, (i.e., t0, 120 + t0, 122) and / or end at a different end time, t1, (i.e., t1, 120 + t-1, 122). In this case, the pulse overlap is less than 1. A duration of the pulse overlap can be a duration between an overlap start time, t0, p u isoverlap, and an overlap end time, ti,p u iscoverage, where:

[0175] As explained herein, the reference time of a phase can be the beginning of the phase. The target time delay described herein can be a target time interval from the reference time of a phase (e.g., the beginning of the phase).

[0176] In the operating sequence 700 shown by way of example in FIG. 7, the first electrical power pulse 120 is generated in each phase 701 at the reference time of the clock (i.e., according to a first target time delay = 0), and the second electrical power pulse 122 is generated in each phase 701 according to a (second) target time delay after the reference time of the clock (i.e., according to a second target time delay > 0). Furthermore, in this exemplary operating sequence 700, the first electrical power pulse 120 is generated according to a first target pulse duration, and the second electrical power pulse 122 is generated according to a second target pulse duration that is shorter than the first target pulse duration (and shorter than the difference between the first target pulse duration and the second target time delay, so that the second electrical power pulse 122 ends before the first electrical power pulse 120).Thus, the second target time delay can be greater than the first target time delay and the second target pulse duration (= t-1,122 - t o, 122) can be less than the first target pulse duration (= t-1,120 - t o, 120).

[0177] According to various aspects, the omission of individual second electrical power pulses 122 and the reduction of the pulse overlap between the first electrical power pulse 120 and the second electrical power pulse 122 can be combined to significantly increase the critical coating rate. In this case, the increase in the schematic rate-temperature curve 206 (see FIG. 2B) would be significantly reduced, so that the critical temperature, T c , with a significantly higher critical rate R C 2 is reached.

[0178] FIG.8 shows an exemplary operating sequence 800 with a schematic timing diagram of the first electrical power pulse 120 and the second electrical power pulse 122, wherein in phases 701 the first electrical power pulse 120 and the second electrical power pulse 122 are generated and wherein in a phase 801 the first electrical power pulse 120 is generated, but the second electrical power pulse 122 is not generated (i.e. is omitted).

[0179] If an electrical power pulse is measured, the start time, t0, and the end time, t1, of the electrical power pulse can be determined, for example, using a threshold value. FIG. 9 shows the time profile of the voltage and current of an exemplary power pulse 900a with a peak value Vmax of the voltage and peak value Imax of the current. The threshold value (Vth or Ith) can be a predefined proportion (e.g., 10% or less, e.g., 5% or less) of the peak value V ma x or l m ax. In this case, the pulse width is the time interval between the two times to and ti at which the time course reaches the threshold value.

[0180] The desired pulse length of the (e.g., first) power pulse can generally be in a range from approximately 30 pis to approximately 600 pis. In this regard, it has been recognized that if this desired pulse length, l(p), (and thus essentially the pulse length of the first electrical power pulse 120) is in a range from approximately 250 pis to approximately 350 pis, the surface contact resistance, ICR, of the formed layer (e.g., in the case of carbon layers) is reduced. This is schematically illustrated in diagram 208a in FIG.2C. The use of a desired pulse length of the first electrical power pulse 120 from the range from approximately 250 pis to approximately 350 pis can, in the case of carbon arc evaporation, result in the formation of both singly charged and doubly charged carbon ions. In this regard, it was recognized that this promotes layer formation and can therefore lead to the reduction of the surface contact resistance, ICR.It is understood that the pulse length depends on the rise of the rising edge and the falling edge of the pulse, so that a target rise can also represent the target pulse length.

[0181] In diagram 208b, curve 210 refers to a layer produced using a target pulse length of the first electrical power pulse 120 in the range of approximately 250 ps to approximately 350 ps. It can be clearly seen that the reduction in the surface contact resistance, ICR, results in the target contact resistance, ICR*, only being reached at a higher critical temperature, T C 2 , is reached (or exceeded). Consequently, the (e.g., dynamic) coating rate can be increased in this case as well, with a low risk of damage to the carbon layer.

[0182] According to various aspects, the omission of individual second electrical power pulses 122 and / or the reduction of the pulse coverage may be combined with the selection of the desired pulse length of the first electrical power pulse 120 from the range of approximately 250 pis to approximately 350 pis to further increase the critical coating rate.

[0183] In general, the coating rate can be increased by increasing the pulse frequency and / or the pulse length of the first electrical power pulse 120. If the pulse length of the first electrical power pulse 120 is selected from the above range, the coating rate can be increased by increasing the pulse frequency of the first electrical power pulse 120.

[0184] According to various aspects, omitting individual second electrical power pulses 122 and / or selecting the desired pulse length of the first electrical power pulse 120 from the range of approximately 250 pis to approximately 350 pis may facilitate fabricating a carbon layer on a substrate having one or more of the properties specified in Examples 38 to 47.

[0185] As described herein, laser-induced arc evaporation can be used to coat a substrate in a continuous system. FIG. 4 shows an exemplary vacuum chamber arrangement 400 for coating by means of laser-induced arc evaporation in a continuous system according to various embodiments in a schematic top view or schematic side view. Here, the vacuum chamber arrangement 400 can have a transport device 402. The transport device 402 can be configured to transport the substrate 106 along a transport path (e.g., in the transport direction 101) past the coating device 108. Optionally, the vacuum chamber arrangement 400 can have a cooling element 404 (e.g., a cooling plate) for cooling the substrate 106. Cooling the substrate 106 by means of the cooling element can, for example, determine the critical coating rate, R c , additionally increase.

[0186] In this case, the transport device 402 and the vacuum arrangement 100 can be controlled such that the coating rate with which the layer on the substrate 106 (eg a carbon layer on a bipolar plate) is formed is greater than or equal to 50 nnim / min.

[0187] FIG.5A and FIG.5B show an exemplary continuous system 500 with several coating devices 108 according to various embodiments in a schematic plan view.

[0188] As shown in FIG. 5A, in the continuous system 500, at least one substrate 106 can be conveyed past a plurality of coating devices 108(k, m) by means of the transport device 402. Coating devices 108(k, m) can be arranged on both sides of the transport path (e.g., on the left with k=1 and on the right with k=2 with respect to the transport direction 101). For example, M coating devices 108 can be arranged on each side of the transport path, where M can be any integer greater than or equal to one. A coating device 108(k, m) can therefore be specified by the integers k and m (where 1 < m < M).

[0189] For example, the at least one substrate 106 can be arranged in a carrier, which can be transported along the transport path by means of the transport device 402. The second electrical power pulse 122 described herein can be applied to this carrier in some embodiments.

[0190] According to various aspects, one coating device 108(k*, m*) of the plurality of coating devices may have a first (e.g., dynamic) coating rate, and another coating device 108(k*, m \ m*) of the plurality of coating devices may have a second coating rate different from the first coating rate. For example, a first coating device 108(1, 1) may form a first carbon layer over the substrate 106 at a coating rate of less than 50 nm / min, and a second

[0191] Coating device 108(1, 2) can then form a second carbon layer on the first carbon layer at a coating rate greater than or equal to 50 nm / min. For example, the first carbon layer can serve as a nucleation layer for the second carbon layer in this case. Optionally, in connection with the last coating device 108(k, 3), a higher peak power (e.g., peak voltage) of the second electrical power pulse 122 (compared to the other coating devices 108(k, m \ 3)) can be used. This can serve to break material peaks of the formed layer in order to smooth the layer.

[0192] In general, the continuous-flow system 500 can have two substrate transfer openings through which the (at least one) substrate 106 can be guided into and out of the continuous-flow system 500. A plurality of processing areas can be arranged between these two substrate transfer openings. For example, one or more of the processing areas can each have one or more coating devices 108. Consequently, the coating devices 108(k, m) shown in FIG. 5A can, for example, form three processing areas (wherein the substrate 106 can be coated on both sides in each processing area).

[0193] FIG. 5B shows an exemplary embodiment of the continuous processing system 500 with multiple processing areas between a first substrate transfer opening 502 for feeding at least one substrate 106 (e.g., a bipolar plate) into the continuous processing system 500 and a second substrate transfer opening 502 for guiding the at least one substrate 106 out of the continuous processing system 500. A vacuum may be present in the continuous processing system 500.

[0194] The continuous processing system 500 may include at least one plasma source 506(k) for plasma etching a surface of the substrate 106 (e.g., the bipolar plate). For example, the continuous processing system 500 may include a first plasma source 506(k) and a second plasma source 506(k) for plasma etching both sides of the substrate 106. The plasma etching may be performed, for example, using argon ion bombardment (e.g., by magnetron sputter etching, by inverse etching, or by processing with an argon ion source).

[0195] Optionally, the substrate 106 (e.g., the bipolar plate) can be heated (e.g., heated) after plasma etching and then cooled.

[0196] Optionally, the continuous system 500 can have one or more coating sources 508(k, o) in addition to the coating devices 108(k, m). These can also optionally be arranged on both sides of the transport direction 101.

[0197] A coating source 508(k,o) may, for example, be a coating source for magnetron sputtering, arc evaporation, or high-pulse magnetron sputtering.

[0198] In an exemplary method, a bipolar plate as a substrate can be coated on both sides in the continuous system 500. The bipolar plate can, for example, have a surface roughness with an average arithmetic height of less than or equal to 0.3 pim, preferably less than or equal to 0.2 pim, and / or a maximum height of less than or equal to 4.0 pim, preferably less than or equal to 2.5 pim. In the exemplary method, the surface of the bipolar plate can be cleaned on both sides using the first plasma source 506(1) and the second plasma source 506(1).

[0199] Then, one or more than one metal layer can be formed on the (cleaned surface of the) bipolar plate using the plurality of coating sources 508(k, o). A metal layer can be, for example, a titanium layer. For example, a first metal layer can be formed on the bipolar plate using a first pair of coating sources 508(k, 1), a second metal layer can be formed on the first metal layer using a second pair of coating sources 508(k, 2), and a third metal layer can be formed on the second metal layer using a third pair of coating sources 508(k, 3). In one example, the first metal layer, the second metal layer, and the third metal layer can each be a titanium layer or form a common titanium layer. The common titanium layer can have a layer thickness in a range from approximately 20 nm to approximately 400 nm, preferably in a range from approximately 50 nm to approximately 150 nm.It is understood that the three metal layers are exemplary, and that fewer metal layers (e.g., one or two) or even more than three metal layers may be formed (and the continuous-flow system 500 may have corresponding coating sources). The (common) titanium layer, for example, can increase the corrosion resistance of the bipolar plate.

[0200] The layer described herein (e.g., as a carbon layer) can then be formed on the (common) titanium layer by means of the coating devices 108(k,m). Also with regard to the coating devices 108(k,m), it is understood that the illustrated number of coating devices is exemplary and the continuous-flow system 500 can also have more or fewer coating devices 108(k,m). For example, in some embodiments, one-sided processing of the substrate can be performed (so that k = 1). As explained herein, (by omitting individual second electrical power pulses 122 and / or by selecting the desired pulse length of the first electrical power pulse 120 from the range of approximately 250 pis to approximately 350 pis), for example, a carbon layer can be formed that has one or more of the properties specified in Examples 38 to 47.

[0201] Optionally, the continuous processing system 500 can have one or more cooling zones (e.g., between two consecutive processing zones) to reduce the temperature of the substrate (and thus of the already formed layer). A cooling zone can, for example, have cooling plates or another suitable type of cooling.

[0202] While the layer (e.g., the carbon layer) is produced in the continuous line 500 according to the principles described herein, it is understood that the layer may also be produced correspondingly in other lines, such as drum coater lines.

[0203] FIG.6 shows an exemplary operating sequence 600 in a schematic diagram in which the power P is shown as an exemplary time-dependent size of the pulses over time t.

[0204] The operating sequence 600 has a plurality of phases 601, 603, in each of which: at least one laser pulse 114, at least one first electrical power pulse 120, and a maximum of one second electrical power pulse 122 are generated. The plurality of phases 601, 603 have a series (also referred to as a phase series) of a plurality (e.g., two, three, or four) immediately successive phases 601 of the first type. In each phase 601 of the first type, exactly one laser pulse 114, exactly one first electrical power pulse 120, and exactly one second electrical power pulse 122 are generated. The plurality of phases 601, 603 have one or more than one phase 603 of the second type, which is arranged between two immediately successive phase series, and in which exactly two laser pulses 114, exactly two first electrical power pulses 120, and exactly one second electrical power pulse 122 are generated. It can be understood that the pulse numbers are exemplary.

Claims

Patent claims 1. A method comprising: • controlling an excitation source (110) according to an operating sequence; • controlling an electrical power source (118) according to the operating sequence; • the operating sequence comprising several phases, in each phase of which: • by means of the excitation source (110) an excitation pulse (114) directed at a target (112) is generated to excite a plasma discharge on the target (112); • a first electrical power pulse (120) is generated by means of the electrical power source (118) for electrically supplying the plasma discharge by means of the target (112); and / or • a second electrical power pulse (122) is generated by means of the electrical power source (118) for accelerating a material stream (116) released from the target (112) by means of the plasma discharge away from the target (112) and / or towards a substrate holder (104); wherein the plurality of phases: • have one or more than one first phase, of which the first electrical power pulse (120) and / or the second electrical power pulse (122) are generated in each first phase per excitation pulse (114), and • have a second phase in which: o two excitation pulses (114) and / or two first electrical power pulses (120) are generated per second electrical power pulse (122), and / or o a first electrical power pulse and a second electrical power pulse are generated which only partially overlap one another.

2. The method according to claim 1, wherein the first electrical power pulse (120) is delivered by means of the target (112) and / or an anode associated with the target (112); and / or wherein the second electrical power pulse (122) is delivered by means of a substrate holder, toward which the material flow (116) is directed, and / or an anode associated with the substrate holder.

3. The method according to claim 1 or 2, wherein the plurality of phases comprise at least two or three first phases per second phase.

4. The method according to any one of claims 1 to 3, wherein the first electrical power pulse (120) is generated according to a desired pulse length that is in a range of approximately 250 pis to approximately 350 pis.

5. The method according to one of claims 1 to 4, wherein the first electrical power pulse (120) is generated according to a desired current pulse; and / or wherein the second electrical power pulse (122) is generated according to a desired voltage pulse.

6. The method according to any one of claims 1 to 5, wherein the target (112) comprises or consists of carbon.

7. A process according to any one of claims 1 to 6, wherein in each of the first and / or second phases: • wherein the first electrical power pulse is generated according to a first target time interval from a start of the phase and wherein the second electrical power pulse is generated according to a second target time interval from the start of the phase, wherein the second target time interval is greater than the first target time interval; and / or • wherein the first electrical power pulse is generated according to a first target pulse duration and wherein the second electrical power pulse is generated according to a second target pulse duration, wherein the second target pulse duration is shorter than the first target pulse duration.

8. A computer program arranged, when executed by a processor, to cause the processor to perform the method according to any one of claims 1 to 7.

9. A computer-readable medium storing instructions arranged, when executed by a processor, to cause the processor to perform the method according to any one of claims 1 to 7.

10. Control device (124) comprising one or more than one processor configured to perform the method according to one of claims 1 to 7.

11. Device comprising: • the control device (124) according to claim 10; • the power source (118); • the excitation source (110); and • a target holder for holding the target (112), the target holder being electrically coupled to the power source (118); • wherein the target holder optionally provides a rotation axis and is configured to cause the target (112) to rotate around the rotation axis.

12. A method comprising: • Placing a bipolar plate in a vacuum; and • Performing laser-induced arc evaporation in the vacuum by controlling an excitation source (110) and an electrical power source (118) according to the method of any one of claims 1 to 7, wherein the material stream (116) dissolved out by means of the plasma discharge comprises the carbon and is emitted towards the bipolar plate.

13. Method according to claim 12, wherein the vacuum is provided by means of a vacuum chamber, which preferably has two substrate transfer openings through which the bipolar plate is transported and between which a coating region is arranged, into which the material stream (116) is emitted; wherein preferably furthermore the driving and the transporting are arranged relative to one another such that a rate at which the carbon layer is formed on the bipolar plate is greater than or equal to 50 nnrrn / min.

14. A method comprising: • controlling an excitation source (110) according to the operating sequence; • controlling an electrical power source (118) according to the operating sequence; • the operating sequence comprising several phases, in each phase of which: • by means of the excitation source (110) an excitation pulse (114) directed at a target (112) is generated to excite a plasma discharge on the target (112); • a first electrical power pulse (120) is generated by means of the electrical power source (118) for electrically supplying the plasma discharge by means of the target (112); and / or • a second electrical power pulse (122) is generated by means of the electrical power source (118) for accelerating a material flow (116) released from the target (112) by means of the plasma discharge away from the target (112) and / or towards a substrate holder (104); • Updating the operating sequence based on a result of the plasma discharge so that the multiple phases: • have one or more than one first phase, of which the first electrical power pulse (120) and / or the second electrical power pulse (122) are generated in each first phase per excitation pulse (114), and • have a second phase in which: o two excitation pulses (114) and / or two first electrical power pulses (120) are generated per second electrical power pulse (122), and / or o a first electrical power pulse and a second electrical power pulse are generated which only partially overlap one another.

Citation Information

Patent Citations

  • Method for depositing thick tetrahedral amorphous carbon film under cooperative control of pulsed cathode arc / workpiece bias pulse

    CN114875367A

  • Surface treated carbon coatings for flow field plates

    US20100323276A1