Method for collecting liquid from stack comprising wet wood veneers
The method of pressing wet wood veneers to remove and collect wood extractives addresses the quality issues in plywood production by reducing moisture and extracting wood extractives for versatile applications.
Patent Information
- Application Number
- PCT/FI2024/050252
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-22
- Filing Date
- 2024-05-22
- Publication Date
- 2024-11-28
AI Technical Summary
Wet wood veneers with high moisture and wood extractive content pose challenges in gluing properties and quality of final products like plywood, as elevated drying temperatures fail to collect all wood extractives effectively.
A method involving pressing a stack of wet wood veneers to remove liquid, including water and dissolved wood extractives, with surface pressures of 0.8-3.5 N/mm², followed by collection and potential conversion of the removed liquid for further use as a wood preservative or in other products.
Improves the quality of multi-layered wood veneer products by reducing moisture and extracting wood extractives, enabling their utilization in various applications, including as a wood preservative or in glues, cosmetics, and construction materials.
Smart Images

Figure FI2024050252_28112024_PF_FP_ABST
Abstract
Description
METHOD FOR COLLECTING LIQUID FROM STACK COMPRISING WET WOODVENEERSFIELD
[0001] The present invention relates to pressing of wet wood veneers, especially a method for collecting liquid from a stack comprising the wet wood veneers.BACKGROUND
[0002] A veneer is a thin, typically thinner than 4 mm, slice of wood. A veneer belt can be produced from logs by the action of peeling or cutting. The veneer belt can be then cut into veneer sheets and dried. The veneer sheets can be used to produce for example, a multi-layered wood veneer product.
[0003] Before drying, the veneer sheets can have a relatively high moisture and wood extractive content. Moisture and wood extractives can reduce gluing properties of the veneer sheets and thus the quality of the final product. On the other hand, when drying the wet wood veneers at an elevated temperature, all the wood extractives of the wet wood veneers cannot be collected.
[0004] An object of the present invention is this to mitigate at least some of the above- mentioned problems. An object of the present invention is thus to provide a method, which improves a quality of a final product, such as a plywood, and enables collecting the wood extractives.SUMMARY
[0005] According to a first aspect of the present disclosure, there is provided a method for collecting liquid from a stack comprising wet wood veneers, comprising: pressing the stack comprising the wet wood veneers in order to remove liquid from the wet wood veneers in the stack, and collecting the removed liquid, wherein the removed liquid comprises water and dissolved or dispersed wood extractives.
[0006] Significant benefits are gained with aid of the present method. The method enables improving a quality of a final product, such as a multi-layered wood veneer product, by removing moisture and wood extractives from the wet wood veneers. In addition, themethod enables collecting the removed liquid. Thus, the removed liquid comprising the wood extractives, such as stilbenes, can be utilized.
[0007] One or more embodiments may comprise one or more features from the following itemized list:- the wood extractives are selected from the group consisting of stilbenes, fatty acids, resin acids, steryl esters, triglycerides, terpenes, tannins, lignans, and any combinations thereof- a surface pressure is 0.8-3.5 N / mm2, preferably 1.2-2.6 N / mm2in the pressing- the moisture content of stack of wet wood veneers is higher before the pressing than after the pressing- as a result of said pressing the moisture content of at least the majority of the wet wood veneers decreases by at least 0.1 wt-%, such as 0.1-35 wt-%- the method further comprises heating of the veneers or the stack comprising the wet wood veneers before pressing- the pressing comprises cold pressing or pressing in an elevated temperature- the method further comprises converting the removed liquid- converting comprises concentrating the removed liquid or mixing solvent and / or other substances to the removed liquid- the method further comprising treating an object or a panel with the removed, optionally converted, liquid, or a fraction thereof- the object or the panel is surface treated, pressure treated, impregnated or coated by the removed, optionally converted, liquid- the removed, optionally converted, liquid or fraction thereof is suitable for use as a wood preservative composition or a component thereof- the removed, optionally converted, liquid or fraction thereof is suitable for use as a component of a glue, a cosmetic product, a food product, a construction material, a pulp product, a paper product, plastic, composite or a medicine- the wood preservative composition is a composition that increases hydrophobicity of wood or a fungicidal composition- the wet wood veneers comprise spruce, birch, Scotch pine, Douglas Fir, Southern Yellow Pine, Elliotis Pine, Taeda Pine, poplar, eucalyptus, larch, Radiata Pine, oak, beech, mahogany, maple, gurjan, kuring, ash, luan, meranti, apiton, kerning,okoume, bintangor, sapelle, walnut, basswood and / or teak veneers, or any combinations thereof
[0008] According to a second aspect of the present disclosure, there is provided an apparatus for collecting liquid from a stack comprising wet wood veneers, comprising: a hydraulic press for pressing the stack comprising the wet wood veneers in order to remove liquid from the wet wood veneers in the stack, and a container for collecting the removed liquid, wherein the removed liquid comprises water and dissolved or dispersed wood extractives.
[0009] Significant benefits are gained with aid of the present apparatus. The apparatus enables pressing the stack and collecting the removed liquid. Thus, the removed liquid can be collected for further use.
[0010] One or more embodiments may comprise one or more features from the following itemized list:- the wood extractives are selected from a group consisting of stilbenes, fatty acids, resin acids, steryl esters, triglycerides, terpenes, tannins and / or lignans, and any combinations thereof- the apparatus further comprises means for identifying the wet wood veneers- the apparatus further comprises or be connected to means for forming the stack of the wet wood veneers from the identified wet wood veneers- the apparatus further comprises or be connected to a heating unit for heating the wet wood veneers or the stack comprising the wet wood veneers- the apparatus further comprises or is connected to means for converting the removed liquid- the apparatus further comprises or is connected to means for treating an object or a panel with the removed liquidBRIEF DESCRIPTION OF THE DRAWINGS
[0011] FIGURE 1 illustrates a method in accordance with at least some embodiments;
[0012] FIGURE 2 illustrates a method in accordance with at least some embodiments; and
[0013] FIGURE 3 illustrates means for identifying the wet wood veneers in accordance with at least some embodiments.EMBODIMENTS
[0014] In the present context, the term “veneer” refers to a layer material intended for the manufacture of a layered sheet or corresponding product, preferably a thin sheet like material, which has been formed from a wooden or other fiber-based material. The veneer can be in the form of a sheet or a strip or a mat.
[0015] In the present context, the term “stack” refers to an organized pile of overlapping veneers.
[0016] In the present context, the term “wet wood veneer” refers to a veneer, which is not yet dried. The wet wood veneer can have a humidity above 10% by weight, for example above 20% by weight.
[0017] In the present context, the term “wood extractive” refers to compounds present in wood. The compounds can be extracted using solvents. The wood extractives include compounds such as alkaloids, waxes, fats, proteins, phenolics, gums, pectins, resins, terpenes, and essential oils.
[0018] In the present context, the term “multi-layered wood veneer product” refers to a veneer product comprising a plurality of veneers. The multi-layered wood veneer product can be for example, plywood or laminated veneer lumber (LVL).
[0019] In the present context, the term “pressing” means that the pressing can be conducted as a cyclic pressing or a static pressing. In the cyclic pressing, a pressure can be increased to a maximum value and decreased to a value between the maximum value and a minimum value after a predetermined time, which minimum value can be zero. This cycle can be repeated. In the static pressing, a pressure can be increased to a predetermined value for a predetermined time. After this, the pressure can be decreased to zero. The static pressing can be repeated.
[0020] A method 100 for collecting liquid from a stack comprising wet wood veneers comprises:- pressing 104 the stack comprising the wet wood veneers in order to remove liquid from wet wood veneers in the stack, and- collecting 105 the removed liquid, wherein the removed liquid comprises water and dissolved or dispersed wood extractives.
[0021] The method may enable improving a quality of a final product, such as a multilayered wood veneer product, by removing moisture and wood extractives from the wet wood veneers. In addition, the method enables collecting the removed liquid. Thus, the removed liquid comprising the wood extractives, such as stilbenes, can be utilized.
[0022] According to an embodiment, the wood extractives are selected from the group consisting of stilbenes, fatty acids, resin acids, steryl esters, triglycerides, terpenes, tannins and / or lignans, and any combinations thereof.
[0023] The wet wood veneers can be stacked at least partly on top of each other. The stack of wet wood veneers comprises 2-1000 wood veneers.
[0024] The stack of wet wood veneers can be pressed at least once. Pressing once is enough if enough liquid can be removed from the stack. Preferably, the stack of wet wood veneers is pressed 1-10 times, for example twice, such as three times. If necessary, pressing can be repeated as many times as is needed to remove enough liquid from the stack or a preferred moisture content of the stack is obtained.
[0025] According to an embodiment, a surface pressure is 0.8-3.5 N / mm2, preferably 1.2-2.6 N / mm2in the pressing. The minimum pressure is a pressure with which liquid can be pressed from the stack. The maximum pressure is a pressure with which the stack can be pressed without breaking the veneers.
[0026] The surface pressure can be at least 0.6 N / mm2, such as at least 0.8 N / mm2.
[0027] The surface pressure can be less than 4.0 N / mm2, such as less than 3.5 N / mm2.
[0028] According to an embodiment, the moisture content of stack of wet wood veneers is higher before the pressing than after the pressing. Thus, the pressing removes liquid from the stack, although it may also transfer liquid between the veneers of the stack and inside an individual veneer.
[0029] According to an embodiment, as a result of said pressing the moisture content of at least the majority of the wet wood veneers decreases by at least 0.1 wt-%, such as 0.1- 35 wt-%.
[0030] The method can further comprise identifying 101 wet wood veneers comprising wood extractives. The identifying can comprise determining a concentration profile of the wood extractives or a moisture content over the wet wood veneer surface. The identifying enables recognizing veneers and areas of veneers having higher wood extractive concentration. The moisture content can correlate with the concentration of the wood extractives. Thus, the moisture content can be used to determine the concentration of the wood extractives in some of the wood species, such as pine, or a part of the wood, such as heartwood, as explained in the following paragraphs. The concentration of the wood extractives can be determined by comparing the moisture content to a database. The database can be constructed in advance by measuring the concentration of the wood extractives with known moisture content, and plotting the concentration of the wood extractives as a function of the moisture content. Thus, when the moisture content is measured, the concentration of the wood extractives can be determined using the database. For example, different wood species and parts of a wood can have own databases. For example, sapwood of pine comprises fatty acids and rosin acids, but no or very small amounts of stilbenes. On the other hand, outer layers of heartwood before sapwood of pine comprises highest concentrations of stilbenes.
[0031] The wet wood veneer surface that is identified in each wet wood veneer forms at least 25%, such as at least 50%, such as at least 75% of the whole area of the respective surface of said wet wood veneer. For example, an entire lateral surface, such as a top surface of the wet wood veneer may be identified.
[0032] Preferably, the identified area is a uniform area of a surface of the wet wood veneer.
[0033] The concentration profile of the wood extractives or the moisture content over the wood veneer surface can be determined, for example, by means of ultra-violet fluorescence spectroscopy, near infrared (NIR) spectroscopy, x-ray spectroscopy or electrical conductivity, a laser, a camera, high-frequency electromagnetic resonance, or a non-contact vision-based wet veneer measuring method, or any combinations thereof. The moisture content can be used to determine the concentration profile of the wood extractives together with the said means.
[0034] In the fluorescence spectroscopy, the wood veneer surface can be illuminated with ultraviolet light. A wavelength of the ultraviolet light can be for example, 310-320 nm.The said wavelength can be used for identifying stilbenes in pine, for example. Then, a fluorescence image of the wood veneer surface can be captured. The fluorescence image can be captured by a color camera. After that, the fluorescence image can be processed to determine concentration of the wood extractives. An amount of fluorescence can be determined by intensity of color in the fluorescence image. A higher intensity of color can indicate higher amount of the wood extractives in the area or in the veneer than a lower intensity. In other words, the fluorescence intensity can indicate an amount of the wood extractives in the veneer. Veneers or areas of the veneers having a higher fluorescence can have a higher amount of the wood extractives than veneers or areas of the veneers having a lower fluorescence. The fluorescence spectroscopy can be conducted without sample preparation. So, it is fast and can be used in a production line.
[0035] Alternatively, or in addition, near infrared (NIR) spectroscopy can be used to detect the wood extractives and determine their concentration. A surface of a wet wood veneer can be illuminated with a wavelength of 780-2500 nm. The wavelengths that are illuminated on the veneer can be measured by examining the ratio between two frequencies: one reference and one at a resonant frequency. From these two measurements, calculations can be made to provide data based on the absorption and scattering of the wavelengths caused by the veneer. An amount of the wood extractives can be determined by the calculations. NIR penetrates deep into the veneer and thus provides reliable measurement. Further, there is no need for sample preparation. So, it is fast and can be used in a production line.
[0036] Alternatively, or in addition, x-ray spectroscopy with electrical conductivity measurement can be used to determine the moisture content over the wood veneer surface. The x-ray spectroscopy can be used for determining a density. The electrical conductivity measurement can be used for determining a moisture content. The electrical conductivity correlates with the moisture content, which correlates with the wood extractive concentration. The wood extractive concentration can be determined from the moisture content by a database as described above. By combining these measurements, and optionally by adding a color camera for a visual inspection for the veneer surface, the moisture content over the wood veneer surface can be detected. The x-ray spectroscopy and the electrical conductivity measurement provides a fast and non-destructive method for identifying the wet wood veneers comprising wood extractives.
[0037] Alternatively, or in addition, a laser can be used to determine the moisture content over the wood veneer surface. For example, a circular beam laser with a wavelength of 1064 nm can be employed. The moisture content variation within the volume creates different patterns of light scattering inside the wood. The moisture content can be determined by a database, which comprises moisture contents at a given laser scattering profiles. Because the moisture content correlates with the wood extractive concentration, the wood extractive concentration can be determined from the moisture content by the database as described above. The laser scattering profile provides a reliable and precise prediction of the moisture content.
[0038] Alternatively, or in addition, a high-frequency electromagnetic resonance can be used to determine the moisture content over the wood veneer surface. The high-frequency electromagnetic resonance allows measuring a moisture content of a veneer at measurement points, which moisture content correlates with wood extractive concentration. The wood extractive concentration can be determined from the moisture content by a database as described above. In the method, ground planes can be adapted on both sides of the veneer to be measured, between each ground plane and the veneer to be measured, at least one center conductor can be adapted approximately parallel to the veneer to be measured in order to form a quasi-TEM transmission line resonator. Electromagnetic RF energy can be fed into the quasi-TEM transmission line resonator so that the electromagnetic quasi-TEM waves propagate in the plane of the veneer to be measured. The high-frequency electromagnetic resonance provides a fast and non-destructive method for identifying the wet wood veneers comprising wood extractives.
[0039] Alternatively, or in addition, a non-contact vision-based wet veneer measuring method can be used to determine the moisture content over the wood veneer surface. In the method, a beam or beams of a specific light wave can be targeted at an underside of a veneer and a camera captures illumination levels of the veneer. The wavelength of the specific light wave can be for example, 380 to 700 nm. Algorithms can be adjusted to determine an exact moisture content within each veneer sheet by the captured illumination levels. The wood extractive concentration can be determined from the moisture content by a database as described above. The method provides a non-contact system and accurate wood extractive concentration results.
[0040] The method 100 can further comprise forming 102 a stack from the identified wet wood veneers after the identifying 101 wet wood veneers comprising wood extractives. The wet wood veneer can be stacked at least partially on top of each other. Thus, the wet wood veneers can be prepared for the pressing wherein the liquid can be removed from the stack of the wet wood veneers and collected for further use.
[0041] The stack of the wet wood veneers can comprise the wet wood veneers, which are identified comprising high concentration areas and / or low concentration areas of the wood extractives. The stack can be formed so that it comprises wet wood veneers having substantially similar wood extractive profile having high concentration areas and / or low concentration areas of the wood extractives. The stack can be also formed so that the wet wood veneers comprising high concentration areas alternate with the wet wood veneers comprising low concentration areas of the wood extractives. For example, every other wet wood veneer can be a wet wood veneer comprising high concentration areas and every other wet wood veneer can be a wet wood veneer comprising low concentration areas.
[0042] Alternatively, the stack of the wet wood veneers can comprise the wet wood veneers, which are identified comprising a first average concentration of the wood extractives and the wet wood veneers, which are identified comprising a second average concentration of the wood extractives, wherein the first average concentration is higher than the second average concentration. The wet wood veneers can be wet wood veneers without any large concentration variation over surfaces of the wet wood veneers.
[0043] In the following, the wet wood veneers, which are identified comprising the first average concentration of the wood extractives are also referred as “first average concentration veneers” and the wet wood veneers, which are identified comprising the second average concentration of the wood extractives are also referred as “second average concentration veneers”.
[0044] The stack can comprise the wet wood veneers having the first average concentration of the wood extractives alternating with the wet wood veneers having the second average concentration of the wood extractives. For example, every other wet wood veneer can be the first average concentration veneer and every other wet wood veneer can be the second average concentration veneer.
[0045] The wet wood veneers having a first average concentration of the wood extractives can be wet wood veneers of a first wood species and the wet wood veneers having a second average concentration of the wood extractives are wet wood veneers of a second wood species. It has been noticed that, wet wood veneers produced from particular wood species can be identified as the first average concentration veneers and some others as the second average concentration veneers. For example, pine wet wood veneers can be identified as the first average concentration veneers and spruce wet wood veneers can be identified as the second average concentration veneers. Then, the stack of the wet wood veneers can be formed from wet wood veneers of a first species having the first average concentration and wet wood veneers of a second species having the second average concentration, wherein the first average concentration is higher than the second average concentration. The stack of the wet wood veneer can be formed so that the wet wood veneers of the first species and the wet wood veneers of the second species alternate.
[0046] The wet wood veneers having a first average concentration of the wood extractives can be wet wood veneers comprising transition zone wood and / or heartwood and the wet wood veneers having a second average concentration of the wood extractives can be wet wood veneers comprising sapwood. It has been noticed that sapwood of pine comprises fatty acids and rosin acids, but no or very small amounts of stilbenes. On the other hand, transition zone wood and heartwood of pine comprises the wood extractives, such as stilbenes. Thus, transition zone wood and heartwood of pine can be identified as wet wood veneers comprising the wood extractives. Then, the stack of the wet wood veneers can be formed from wet wood veneers comprising sapwood, transition zone wood and / or heartwood.
[0047] According to the embodiment, the method 100 further comprises heating 103 of the veneers or the stack comprising the wet wood veneers before pressing 104. The wet wood veneers can be heated individually. Alternatively, the whole stack can be heated at the same time. The wet wood veneers can be heated by for example, hot air, a microwave heater or an infrared (IR) heater. The heating enables that more liquid can be removed from the wet wood veneers by the pressing.
[0048] An air temperature of 60-90 °C can be applied in the heating.
[0049] The IR heater or the microwave heater can operate at least at a temperature of60 °C.
[0050] According to an embodiment, the pressing 104 comprises cold pressing or pressing in an elevated temperature. The cold pressing can be conducted in a room temperature, when an air temperature is 20-30 °C. The pressing in an elevated temperature can be conducted at a temperature at least 35 °C, preferably 35-100 °C. When the pressing comprises the pressing in the elevated temperature, a separate preheating of the veneers before pressing may not be required, but heating can be done simultaneously with the pressing. Alternatively, the liquid can be removed even more efficiently from the stack by combining preheating and the pressing in the elevated temperature.
[0051] During the pressing 104, the temperature of the wet wood veneers may be at least 10 °C or in the range of 10-90 °C, preferably at least 20 °C.
[0052] Pressing in the elevated temperature can comprise pressing the stack comprising the wet wood veneers between warm plates. This enables of heating surfaces of outermost veneers of the stack. Then, heat conducts in the middle of the stack. This method can be used especially in a case of a thin stack, which stack can comprise for example, 2-10 veneers.
[0053] In a case of a thicker stack, such as a stack comprising 11-1000 veneers, a radio frequency pressing can be used. For example, a radio frequency of 10-200 kW can be used. The radio frequency pressing enables uniform heating of the veneers of the stack.
[0054] According to an embodiment, the method further comprises converting 106 the removed liquid. The converting enables modifying properties of the removed liquid so that the removed liquid or fraction thereof is suitable for further use.
[0055] The converting 106 may comprise concentrating the removed liquid, mixing solvent and / or other substances to the removed liquid, or separating substances from the removed liquid, or any combinations thereof. The said methods enable modifying properties of the removed liquid so that the removed liquid or fraction thereof is suitable for further use.
[0056] For example, a further wood preservative or an agent, which increases the hydrophobicity of wood can be added to the removed liquid. The further wood preservative can be for example, a biocide or a non-biocide. The agent, which increases the hydrophobicity of wood, can be for example, wax, such as paraffin wax or AKD, oil, such as wood oil, fat, alkane or a mixture thereof.
[0057] In the concentrating, water can be at least partly removed from the removed liquid. The concentration enables increasing of a content of the wood extractives in the removed liquid. By “removed” it is meant that at least 1 wt-% of water is removed, preferably at least 10 wt-% of water is removed. Thus, the removed liquid has higher content of compounds, which can be used as a wood preservative composition, a composition that increases hydrophobicity of wood or a fungicidal composition, for example. Further, the concentration reduces weight and volume of the liquid for transportation.
[0058] The concentrating the removed liquid can comprise removing water by a thermal concentration process or a membrane concentration process. This process enables a simple and cost-effective way to remove water from the removed liquid.
[0059] In some embodiments, at least 90 wt-% of water is removed. This enables of using wood extractives as a dry substance.
[0060] The thermal concentration process can be for example, evaporation. In the evaporation, the removed liquid can be heated to a temperature of 20-80 °C, preferably 30- 50 °C. This enables evaporation of water from the removed liquid, while the wood extractives are retained in a concentrated solution.
[0061] Optionally, the thermal concentration process can be conducted in a vacuum. The vacuum aids to remove water from the removed liquid by decreasing the atmospheric pressure over the liquid phase. By reducing the pressure exerted on the liquid phase, water molecules more easily enter the gas phase. Thus, the vacuum enables of using lower temperatures in the thermal concentration process, which in turn saves energy. The thermal concentration can be conducted at nearly atmospheric pressure or vacuum levels down to approximately 100 mbar.
[0062] The membrane concentration process can be for example, membrane distillation, osmotic distillation, direct osmosis or reverse osmosis. The membrane concentration process allows smaller molecules pass through membranes more easily than larger ones, thus enabling separation based on molecular size. Since water is one of the smallest molecules, concentration can be easily accomplished using membranes with appropriate molecular- weight cutoffs.
[0063] The separating substances from the removed liquid can comprise converting the removed liquid into two or more distinct products or product mixtures. The separatingsubstances from the removed liquid can be conducted by a separation process, such as filtration, distillation, drying, evaporation, or any combinations thereof. For example, individual wood extractives or their fractions can be separated from the removed liquid. This enables of using individual wood extractives, such as stilbenes, in applications wherein a high purity is needed or which only benefit for use of the individual wood extractive.
[0064] The method can further comprise utilizing 107 the removed, optionally converted, liquid. The utilizing 107 can comprise for example, treating an object or a panel with the removed, optionally converted, liquid, or a fraction thereof or producing a composition comprising the removed, optionally converted, liquid.
[0065] According to an embodiment, the method 100 further comprises treating an object or a panel with the removed, optionally converted, liquid, or a fraction thereof. The object can be a wood object, such as multi-layered wood veneer product. The panel can be a wood panel. This enables increasing of the hydrophobicity of the object or the panel and / or protecting the wood object or the wood panel against mould and blue staining.
[0066] According to an embodiment, the object or the panel is surface treated, pressure treated, impregnated or coated by the removed, optionally converted, liquid. These enables simple and cost-effective ways to protect the surface of the object or panel by the liquid.
[0067] The surface treating can comprise applying the removed, optionally converted, liquid on a surface of the object or the panel by a roller, a spray, a brush, casting or immersing the object or the panel into the removed, optionally concentrated, liquid.
[0068] The pressure treating can comprise placing the object or the panel in a cylinder, i.e. a vacuum pressure vessel. Once the object or the panel is loaded into the cylinder, the cylinder can be sealed. Air can be removed from the cylinder by for example, and a vacuum pump. After the, the cylinder is flooded with removed, optionally converted, liquid. Pressure is then applied to the liquid. This forces the liquid deep into the wood cells. Once the pressure treating has been completed, the cylinder can be drained and the vacuum pump can remove excess liquid from the object or the panel. The liquid can be returned back to a storage tank.
[0069] Preferably, the surface of the wood or the panel is completely covered by the removed, optionally converted, liquid. Alternatively, it is possible to form patterns or streakson the object or the panel by treating a portion of the surface the object or the panel by the liquid.
[0070] The treating the object or the panel can be conducted at room temperature (approximately at 20-30 °C).
[0071] Optionally, the treating of the object or the panel further comprises heating. The surface of the object or the panel can be preheated and / or heated during the treating. This facilitates absorption of the removed, optionally converted, liquid.
[0072] Optionally, the obj ect or the panel can be coated after the treating. For example, a coating film or a coating substance, such as a resin, a lacquer or a paint, can be placed on the treated surface. This improves in further the hydrophobicity of the object or the panel and / or protects the object or the panel.
[0073] Alternatively, the removed, optionally converted, liquid can be used for producing a composition comprising the removed, optionally converted, liquid. The removed liquid can be mixed to a product already during a manufacturing of the product. For example, the removed, optionally converted, liquid can be mixed with substances of a glue during manufacturing of the glue. The glue can be used for attaching veneers together for forming a multi-layered wood veneer product.
[0074] According to an embodiment, the removed, optionally converted, liquid or a fraction thereof is suitable to be used as a wood preservative composition or as a component thereof. The wood preservative composition can be for example a wood preservative, a paint, a resin or a lacquer.
[0075] According to an embodiment, the wood preservative composition is a composition that increases hydrophobicity of wood or a fungicidal composition.
[0076] Alternatively, the removed, optionally converted, liquid or a fraction thereof is suitable to be used as a component of a glue, a cosmetic product, a food product, a construction material, a pulp product, a paper product, plastic, composite or a medicine.
[0077] According to an embodiment, the wet wood veneers are spruce, birch, Scotch pine (Pinus sylvestris), Douglas Fir (Pseudostuga menziesii), Southern Yellow Pine (Pinus palustris), Elliotis Pine, Taeda Pine, poplar (populus species), eucalyptus, larch (larix species), Radiata Pine, oak, beech, mahogany, maple, gurjan, kuring, ash, luan, meranti,apiton, keruing, Okoume, bintangor, sapelle, walnut, basswood and / or teak veneers. Preferably, the wet wood veneers are pine, spruce or birch veneers, or any combinations of thereof. Thus, the stack of the wet wood veneers may comprise for example, pine and spruce veneers.
[0078] An apparatus for collecting liquid from a stack comprising wet wood veneers, comprises:- a hydraulic press for pressing the stack comprising the wet wood veneers in order to remove liquid from the wet wood veneers in the stack, and- a container for collecting the removed liquid, wherein the removed liquid comprises water and dissolved or dispersed wood extractives.
[0079] The apparatus enables pressing the stack and collecting the removed liquid. Thus, the removed liquid can be collected for further use.
[0080] The wood extractives can be selected from a group consisting of stilbenes, fatty acids, resin acids, steryl esters, triglycerides, terpenes, tannins and / or lignans, and any combinations thereof.
[0081] The container can be a drainage basin. The drainage basing can be placed under the hydraulic press. The removed liquid can be transferred from the drainage basin to a container for storage and further use.
[0082] The apparatus can further comprise means 300 for identifying the wet wood veneers. The means 300 can comprise a source 301, a detector 302 and a control unit 303, as illustrated in FIGURE 3. The source 301 can be for example, an ultraviolet (UV) source, a near infrared (NIR) source, an electron beam generator, a high-frequency electromagnetic resonator or a visible light source. The source directs UV-light, NIR-radiation, an electron beam, electromagnetic resonance or visible light to a surface of a wet wood veneer 304.
[0083] The detector 302 can be for example, a camera or a spectrometry, depending on a type of the source. In the case of UV-light, the detector 302 can be a camera, such a colour camera. The camera can capture an image of the illuminated wet wood veneer surface. In the case of NIR-radiation or the electron beam, the detector 302 can be a spectrometry.
[0084] The control unit 303 can be for example, a computer. The control unit 303 may be connected to the detector 302 or the detector 302 may comprise a transmitter configuredto transmit information to the control unit 303. The control unit 303 can be configured to determine a concentration profile or an average concentration of the wood extractives over the wet wood veneer surface.
[0085] The electrical conductivity measuring device can be for example, an electrical conductivity meter. With the aid of the electrical conductivity measuring device, electrical conductivity can be measured. The electrical conductivity correlates with the moisture content. The moisture content can be determined by comparing the electrical conductivity to a database. The database can be constructed in advance by measuring the electrical conductivity with known moisture content, and plotting the electrical conductivity as a function of the moisture content. Thus, when the electrical conductivity is measured, the moisture content can be determined using the database. For example, different wood species and parts of a wood can have own databases.
[0086] The electrical conductivity measuring device may comprise a probe, which is configured to be placed in contact with the measured wet wood veneer surface. The control unit 303 may be connected to the electrical conductivity measuring device or the electrical conductivity measuring device may comprise a transmitter configured to transmit information to the control unit 303.
[0087] The apparatus can further comprise or be connected to means for forming the stack of the wet wood veneers from the identified wet wood veneers. The means for forming the stack of the wet wood veneers can comprise for example, a veneer stacking machine. This enables automatic stacking of the wet wood veneers.
[0088] The apparatus can further comprise or be connected to a heating unit for heating the wet wood veneers or the stack comprising the wet wood veneers. The heating unit can be configured to heat the veneers individually or the whole stack of the veneers at the same time. The heating unit can comprise for example, an infrared (IR) heater, an electric heating platen, a warm water heater or a thermal oil heater. The warm water heater and the thermal oil heater may comprise metal plates, which comprise coils for warm water circulation. The hydraulic press can comprise or be connected to the heating unit. When the heating unit is connected to the hydraulic press, the wet wood veneers can be heated during the pressing. The heating unit enables that more liquid can be removed from the stack, which liquid can have a higher concentration of the wood extractives.
[0089] According to an embodiment, the apparatus may further comprise or be connected to means for converting the removed liquid. The means for converting the removed liquid can comprise for example, means for concentrating the removed liquid, such as a thermal concentration apparatus or a membrane concentration apparatus. The means for concentrating the removed liquid enable increasing of a content of the wood extractives in the removed liquid. Thus, the removed liquid has higher content of compounds, which can be used as a wood preservative composition, a composition that increases hydrophobicity of wood or a fungicidal composition, for example. Further, the means for concentrating the removed liquid reduces weight and volume of the liquid for transportation.
[0090] According to an embodiment, the apparatus further comprises or be connected to means for treating a wood object or a wood panel with the removed, optionally concentrated liquid. The means for treating a wood object or a wood panel can comprise a surface treating equipment or a pressure treating equipment. These enables simple and cost- effective ways to protect the wood surface by the removed, optionally concentrated, liquid.DETAILED DESCRIPTION OF THE DRAWINGS
[0091] FIGURE 1 illustrates a method 100 in accordance with at least some embodiments. The method 100 comprises pressing 104 the stack of wet wood veneers in order to remove liquid from the stack of wet wood veneers, and collecting 105 the removed liquid.
[0092] FIGURE 2 illustrates a method 200 in accordance with at least some embodiments. The method 200 comprises identifying 101 wet wood veneers comprising wood extractives, optionally heating 103 the wet wood veneers, forming 102 a stack from the identified wet wood veneers, optionally heating 103 the stack, pressing 104 the stack in order to remove liquid from the stack, collecting 105 the removed liquid, optionally converting 106 the removed liquid, and utilizing 107 the removed, optionally converted, liquid. The utilizing 107 can comprise treating an object or a panel with the removed, optionally converted, liquid, or producing a composition comprising the removed, optionally converted, liquid. The expression “producing a composition” means that the removed liquid can be mixed to a product already during a manufacturing of the product.
[0093] FIGURE 3 illustrates means 300 for identifying the wet wood veneers. The means comprise a source 301, a detector 302 and a control unit 303. The source 301 directs a beam to a wet wood veneer 304, which beam is reflected to the detector 302.
[0094] It is to be understood that the embodiments of the invention disclosed are not limited to the particular structures, process steps, or materials disclosed herein, but are extended to equivalents thereof as would be recognized by those ordinarily skilled in the relevant arts. It should also be understood that terminology employed herein is used for the purpose of describing particular embodiments only and is not intended to be limiting.
[0095] Furthermore, the described features, structures, or characteristics may be combined in any suitable manner in one or more embodiments. In the description, numerous specific details are provided, such as examples of lengths, widths, shapes, etc., to provide a thorough understanding of embodiments of the invention.
[0096] The verbs “to comprise” and “to include” are used in this document as open limitations that neither exclude nor require the existence of also un-recited features. The features recited in depending claims are mutually freely combinable unless otherwise explicitly stated. Furthermore, it is to be understood that the use of "a" or "an", i.e. a singular form, throughout this document does not exclude a plurality.
Claims
CLAIMS:
1. A method (100) for collecting liquid from a stack comprising wet wood veneers, comprising:- pressing (104) the stack comprising the wet wood veneers in order to remove liquid from the wet wood veneers in the stack, and- collecting (105) the removed liquid, wherein the removed liquid comprises water and dissolved or dispersed wood extractives.
2. The method (100) of claim 1, wherein the wood extractives are selected from the group consisting of stilbenes, fatty acids, resin acids, steryl esters, triglycerides, terpenes, tannins, lignans, and any combinations thereof.
3. The method (100) of any one of the preceding claims, wherein a surface pressure is 0.8— 3.5 N / mm2, preferably 1.2-2.6 N / mm2, in the pressing.
4. The method (100) of any one of the preceding claims, wherein the moisture content of stack of wet wood veneers is higher before the pressing (104) than after the pressing (104).
5. The method (100) of claim 4, wherein as a result of said pressing (104) the moisture content of at least the majority of the wet wood veneers decreases by at least 0.1 wt-%, such as 0.1-35 wt-%.
6. The method (100) of any one of the preceding claims, further comprising heating (103) of the veneers or the stack comprising the wet wood veneers before pressing.
7. The method (100) of any one of the preceding claims, wherein the pressing (104) comprises cold pressing or pressing in an elevated temperature.
8. The method (100) of any one of the preceding claims, further comprising converting (106) the removed liquid.
9. The method (100) of claim 8, wherein converting (106) comprises concentrating the removed liquid, mixing solvent and / or other substances to the removed liquid or separating substances from the removed liquid, or any combinations thereof.
10. The method (100) of any one of the preceding claims, further comprising treating an object or a panel with the removed, optionally converted, liquid, or a fraction thereof.
11. The method (100) of claim 10, wherein the object or the panel is surface treated, pressure treated, impregnated or coated by the removed, optionally converted, liquid.
12. The method (100) of any one of the preceding claims, wherein the removed, optionally converted, liquid or fraction thereof is suitable for use as a wood preservative composition or a component thereof, or a component of a glue, a cosmetic product, a food product, a construction material, a pulp product, a paper product, plastic, composite or a medicine.
13. The method (100) of claim 12, wherein the wood preservative composition is a composition that increases hydrophobicity of wood or a fungicidal composition.
14. The method of any one of the preceding claims, wherein the wet wood veneers comprise spruce, birch, Scotch pine, Douglas Fir, Southern Yellow Pine, Elliotis Pine, Taeda Pine, poplar, eucalyptus, larch, Radiata Pine, oak, beech, mahogany, maple, guq’an, kuring, ash, luan, meranti, apiton, kerning, okoume, bintangor, sapelle, walnut, basswood and / or teak veneers, or any combinations thereof.
15. An apparatus for collecting liquid from a stack comprising wet wood veneers, comprising:- a hydraulic press for pressing the stack comprising the wet wood veneers in order to remove liquid from the wet wood veneers in the stack, and- a container for collecting the removed liquid, wherein the removed liquid comprises water and dissolved or dispersed wood extractives.
16. The apparatus of claim 15, wherein the wood extractives are selected from a group consisting of stilbenes, fatty acids, resin acids, steryl esters, triglycerides, terpenes, tannins and / or lignans, and any combinations thereof.
17. The apparatus of any one of the preceding claims 15 to 16, the apparatus further comprises or is connected to means for converting the removed liquid.
18. The apparatus of any one of the preceding claims 15 to 16, the apparatus further comprises or is connected to means for treating an object or a panel with the removed liquid.
Citation Information
Patent Citations
Improved timber processing
CN101065222A
Dewatering Method for Correcting Water Content of Green Veneer for Plywood and Apparatus for Dewatering the Green Veneer
US20140000464A1
Biomass press with ultrasonic vibration
US20200324501A1