Selective oxidation catalysts
The selective oxidation catalyst, featuring nanoparticles of copper and surface-dispersed platinum or cobalt, addresses the inefficiencies of existing catalysts by achieving high ammonia conversion and selectivity to N2 across a wide temperature range, effectively reducing emissions and meeting stringent regulations.
Patent Information
- Application Number
- PCT/GB2024/051324
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-24
- Filing Date
- 2024-05-22
- Publication Date
- 2024-11-28
AI Technical Summary
Current selective catalytic oxidation catalysts, such as those using Pt, achieve high ammonia conversion at high temperatures but suffer from low N2 selectivity above 300°C, failing to effectively reduce ammonia emissions over a wide temperature range while avoiding over-oxidation to NOX species.
A selective oxidation catalyst comprising nanoparticles of a first metal, such as copper, and particles of a second metal like platinum or cobalt, arranged on the surface of the nanoparticles, which enhances catalytic activity and selectivity for ammonia conversion to N2 and H2O across a broad temperature range.
The catalyst provides high conversion and selectivity of ammonia to N2 with minimal NOX production, effectively reducing ammonia emissions from vehicle exhausts and industrial waste streams, meeting stringent emission regulations like Euro-7, and maintaining stability over prolonged use.
Smart Images

Figure GB2024051324_28112024_PF_FP_ABST
Abstract
Description
[0001] Selective Oxidation Catalysts
[0002] Field
[0003] The present invention relates to a selective oxidation catalyst, a method of preparing such a selective oxidation catalyst and a method of catalytic oxidation of ammonia. In particular the present invention relates to an oxidation catalyst comprising nanoparticles of a first metal and particles of a second metal, for improving the selectivity and / or yield of an oxidation process, for example the catalytic oxidation of ammonia.
[0004] Background
[0005] Global emissions of ammonia (NH3) from vehicle exhaust and industrial waste gas streams are projected to be over 220,000 tonnes per year, posing a severe environmental pollution problem. The use of ammonia as a fuel for various modes of transportation is also increasing, which frequently results in undesired ammonia passing through systems unreacted, known as ammonia slip. Regarding vehicle exhaust emissions, ammonia may be used (for example derived from urea) in a diesel engine exhaust system for a selective catalytic reduction step (SCR) to reduce NOXcontent of the exhaust gases to water and N2. Some ammonia inevitably passes through the SCR unreacted (ammonia slip) and is therefore subsequently treated with oxygen in a selective catalytic oxidation step (SOC) to convert the remaining ammonia to water and N2. The effectiveness of this SOC step determines how much ammonia is ultimately emitted by the diesel engine exhaust.
[0006] Although ammonia only stays in the atmosphere for a relatively short time after emission, it can rapidly react with other gases to produce particulate matter which can persist for longer periods. Exposure to high concentrations of such particulate matter has been linked to severe health problems. Also, deposition of ammonia in the environment can cause significant damage to sensitive wildlife habitats and to agricultural land and crops. Current EU regulations restrict ammonia gas emissions to less than 10 ppm. These restrictions are expected to become more stringent in future.
[0007] The selective catalytic oxidation (SCO) of NHs to N2 discussed above may provide a practical method of reducing or eliminating ammonia emissions from various exhaust and waste gas streams, if the efficiency of the oxidation reaction is sufficiently high. A major challenge in the SCO of ammonia is the achievement of a high conversion of NH3 over a wide temperature range of operation of an exhaust system in normal use, such as 150-500°C, whilst avoiding over-oxidation to NOXspecies (such as N2O and NO). The current commercially used Pt catalysts can achieve almost complete NH3 conversion at high reaction temperatures but suffer from low N2 selectivity when the temperature is above 300°C.
[0008] Therefore a need remains for improved oxidation catalysts for use in selective catalytic oxidation processes, for example in the oxidation of NH3 to N2 and H2O. Summary of the Invention
[0009] It is one aim of the present invention, amongst others, to provide a selective oxidation catalyst that addresses at least one disadvantage of the prior art, whether identified here or elsewhere, or to provide an alternative to existing oxidation catalysts used in SCO. For instance, it may be an aim of the present invention to provide a selective oxidation catalyst which provides a conversion of NH3 to N2 and H2O with a high efficiency and selectivity.
[0010] According to aspects of the present invention, there is provided a selective oxidation catalyst and methods as set forth in the appended claims. Other features of the invention will be apparent from the dependent claims, and from the description which follows.
[0011] According to a first aspect of the present invention, there is provided a selective oxidation catalyst comprising: a support; nanoparticles comprising a first metal; and particles of a second metal selected from platinum, palladium, ruthenium, rhodium, cobalt, silver and gold; wherein the nanoparticles are arranged on the support and the particles of the second metal are arranged on outer surfaces of the nanoparticles.
[0012] The first metal and the second metal are suitably different metals.
[0013] The particles of the second metal are suitably single atoms of the second metal, are sub-nanometre particles of the second metal, or are a mixture of single atoms and sub-nanometre particles of the second metal. The particles of the second metal are therefore significantly smaller than the nanoparticles comprising the first metal.
[0014] The inventors have found that the catalyst of this first aspect, which combines the catalytic activity of the nanoparticles comprising the first metal and the catalytic activity of the particles of the second metal, can provide a high conversion of NH3 and a highly selective formation of N2 over NOXspecies, over a range of useful temperatures of operation. The catalyst may therefore provide an improvement on current catalysts used in the selective catalytic oxidation of NH3 and may be used to reduce NH3 emissions, particularly from vehicle exhaust (i.e. in diesel or NH3 powered vehicles) and from industrial waste gas streams. The selective oxidation catalyst may be effective in reducing or substantially eliminating ammonia slip from exhaust and waste gas streams. In particular, the selective oxidation catalyst may be used in a diesel exhaust engine system in conjunction with a selective catalytic reduction module to reduce NH3 emissions to meet the prospective Euro-7 regulations.
[0015] The catalyst of this first aspect comprises the support, the nanoparticles arranged on the support and the particles of the second metal arranged on the nanoparticles. The nanoparticles are suitably bonded to and / or immobilised on the support. Suitably the nanoparticles are impregnated into the support. The particles of the second metal are suitably bonded to and / or immobilised on the nanoparticles. Suitably the catalyst consists essentially or consists of the support, nanoparticles and the particles of the second metal.
[0016] The support
[0017] The support is formed from a support material. The support material may be any suitable material used for supporting active catalyst materials, suitably in a fixed bed reactor and / or in a vehicle exhaust catalytic convertor. Suitably the support material is catalytically inactive towards the substrates intended to be reacted by the selective oxidation catalyst.
[0018] The support material may be selected from AI2O3, TiC>2 or CeC>2. The support suitably comprises aluminium oxide, preferably Y-AI2O3. Suitably the support material is aluminium oxide, preferably Y-AI2O3. Suitably the support consists essentially or consists of aluminium oxide, preferably Y-AI2O3. The aluminium oxide suitably has a particle size between 10 and 50 nm and a surface area of approximately 20 m2 / g.
[0019] The support material is suitably present in an amount of from 88 to 99 wt%, based on the weight of the selective oxidation catalyst, suitably from 91 to 98 wt% or from 92 to 96 wt%.
[0020] The nanoparticles
[0021] The nanoparticles may be formed in situ on the support. The nanoparticles may be impregnated into the support, suitably wherein the support material is porous. Suitably the nanoparticles are spaced apart (or dispersed) on the support and are suitably exposed on the surface of the support, in order to be accessible to the catalyst substrate during a selective catalytic oxidation reaction.
[0022] The nanoparticles are suitably formed from the first metal or an oxide of the first metal. The nanoparticles may be formed from on and in the support using a wet impregnation method. The nanoparticles comprising the first metal are suitably nanoparticles of the first metal.
[0023] Suitably the nanoparticles are catalytically active towards the substrates intended to be reacted by the selective oxidation catalyst. For example, the nanoparticles are suitably catalytically active towards the oxidation of ammonia. Therefore the first metal is suitably catalytically active towards the substrate for the selective oxidation catalyst, i.e. ammonia. The first metal is suitably copper. Therefore the nanoparticles suitably comprise copper. The nanoparticles suitably consist essentially of or consist of the first metal or an oxide of the first metal, preferably copper.
[0024] Preferably, the nanoparticles are copper oxide nanoparticles. Therefore the nanoparticles may be considered to consist essentially or consist of copper oxide. The copper oxide nanoparticles may be formed onto the support by the reduction of a copper species, such as copper(ll) nitrate, in the presence of the support material.
[0025] The nanoparticles are suitably present in an amount of at least 1 wt%, based on the weight of the whole selective oxidation catalyst. Therefore the selective oxidation catalyst suitably comprises at least 1 wt% of the nanoparticles. Suitably the nanoparticles are present in an amount of at least 2 wt% or at least 3 wt%, based on the weight of the whole selective oxidation catalyst.
[0026] Suitably the nanoparticles are present in an amount of up to 20 wt%, based on the weight of the selective oxidation catalyst, suitably up to 10 wt% or up to 8 wt%.
[0027] The nanoparticles are suitably present in an amount of from 1 to 10 wt%, based on the weight of the selective oxidation catalyst, suitably from 2 to 8 wt% or from 3 to 8 wt%.
[0028] The nanoparticles suitably have an average particle size of from 1 to 50 nm, suitably from 2 to 20 nm or from 2 to 10 nm.
[0029] The particles of the second metal
[0030] As discussed above, the particles of the second metal are suitably single atoms of the second metal, are sub-nanometre particles of the second metal, or are a mixture of single atoms and sub-nanometre particles of the second metal.
[0031] The particles of the second metal may be formed in situ on the nanoparticles. The particles of the second metal may be impregnated into the nanoparticles. Suitably the particles of the second metal are spaced apart (or dispersed) on the nanoparticles and are suitably exposed on the surface of the nanoparticles, in order to be accessible to the catalyst substrate during a selective catalytic oxidation reaction.
[0032] The particles of the second metal are suitably provided by galvanic replacement of atoms of the first metal in the nanoparticles with the second metal. Such a galvanic replacement method suitably allows accurate control of the amount of the second metal to be incorporated in the catalyst and deposits the highly active (single atom or sub-nanometre) particles of the second metal only at the surface of the nanoparticles, so that substantially all of the particles of the second metal is available for catalysis. Suitably the particles of the second metal are catalytically active towards the substrates intended to be reacted by the selective oxidation catalyst. For example, the particles of the second metal are suitably catalytically active towards the oxidation of ammonia. Therefore the second metal is suitably catalytically active towards the substrate for the selective oxidation catalyst, i.e. ammonia.
[0033] The second metal is suitably selected from platinum, palladium, ruthenium, rhodium, cobalt, silver and gold. The second metal may be selected from platinum and cobalt.
[0034] In one preferred embodiment, the second metal is platinum.
[0035] In one preferred embodiment, the second metal is cobalt.
[0036] The particles of the second metal are suitably present in an amount of at least 0.01 wt%, based on the weight of the whole selective oxidation catalyst, suitably at least 0.05 wt% or at least 0.1 wt%.
[0037] Suitably the particles of the second metal are present in an amount of up to 2.0 wt%, based on the weight of the whole selective oxidation catalyst, suitably up to 1 .0 wt% or up to 0.8 wt%.
[0038] The particles of the second metal are suitably present in an amount of from 0.01 to 2.0 wt%, based on the weight of the whole selective oxidation catalyst, suitably from 0.01 to 1.0 wt%, from 0.1 to 0.8 wt%, or from 0.4 to 0.8 wt%.
[0039] In some embodiments, the second metal is platinum and the nanoparticles are copper oxide nanoparticles. The inventors have found that this combination of nanoparticles of copper oxide and particles of platinum dispersed on the nanoparticles may provide a particularly active and selective catalyst for the selective catalytic oxidation of ammonia. Without being bound by theory, the inventors believe that the atomic and oligomeric platinum sites on the surface of copper oxide nanoparticles balances the rate of NO formation and N-N coupling, therefore providing a catalyst that is more efficient at low-temperature and more selective at high temperatures, which is ideal for reducing the ammonia and NOXemissions of diesel engines, particularly during a cold start.
[0040] In some embodiments, the second metal is cobalt and the nanoparticles are copper oxide nanoparticles. The inventors have found that this combination of nanoparticles of copper oxide and particles of cobalt dispersed on the nanoparticles may also provide a particularly active and selective catalyst for the selective catalytic oxidation of ammonia.
[0041] According to a further aspect of the invention, there is provided a selective catalytic oxidation module for oxidising ammonia in a gas stream to N2, the selective catalytic oxidation module comprising a selective oxidation catalyst according to the first aspect. The selective catalytic oxidation module may be a vehicle catalytic convertor or part of a vehicle catalytic convertor. Suitable configurations of selective catalytic oxidation modules and methods of manufacturing the same would be known to the skilled person. Method of preparing the catalyst
[0042] According to a second aspect of the present invention, there is provided a method of preparing a selective oxidation catalyst according to the first aspect, the method comprising the steps of: a) admixing a support material with a material comprising the first metal; b) converting the mixture obtained in step a) to a catalyst precursor comprising the support and nanoparticles comprising the first metal; c) treating the catalyst precursor with a source of the second metal to carry out a galvanic replacement of atoms of the first metal of the nanoparticles with particles of the second metal and provide the selective oxidation catalyst.
[0043] The selective oxidation catalyst, support material, first metal and second metal may have any of the suitable features and advantages described above in relation to the first aspect.
[0044] The steps of the method are suitably carried out in the order of step a) followed by step b) followed by step c).
[0045] Suitably the support material is aluminium oxide. Suitably the material comprising the first metal is copper(ll) nitrate.
[0046] Step a) suitably involves suspending the support material in a solvent and adding the material comprising the first metal to the suspension. The solvent may be an alcohol, for example ethanol. The material comprising the first metal may be added slowly to the suspension, for example dropwise. Suitably the suspension is stirred for at least 6 hours, suitably at room temperature. Suitably the solvent is then evaporated from the mixture of the support material and the material comprising the first metal.
[0047] Suitably step b) involves heating the mixture obtained in step a), suitably to a temperature of between 200 and 400°C, for example from 250 to 350°C or approximately 300°C.
[0048] Suitably step b) involves a reduction reaction of the material comprising the first metal which forms the nanoparticles. Step b) may involve treating the mixture obtained in step a) with a reducing agent, suitably hydrogen gas. Step b) may involve treating the mixture obtained in step a) with a mixture of hydrogen and argon, for example a 15% mixture of hydrogen in argon. Suitably step b) involves heating the mixture obtained in step a) to the temperatures described above in the presence of a reducing agent, such as hydrogen gas. Step b) may be carried out in a tube furnace.
[0049] Step b) produces a catalyst precursor comprising the support and nanoparticles comprising the first metal arranged on / impregnated in the support material. Suitably the catalyst precursor produced in step b) comprises an aluminium oxide support having copper oxide nanoparticles arranged on / impregnated in the support.
[0050] Suitably, the support material is aluminium oxide, the material comprising the first metal is copper(ll) nitrate and the catalyst precursor produced in step b) is an aluminium oxide comprising copper oxide nanoparticles.
[0051] Step c) involves treating the catalyst precursor with a source of the second metal to carry out a galvanic replacement of atoms of the first metal of the nanoparticles with particles of the second metal and provide the selective oxidation catalyst. Suitably step c) provides the particles of the second metal spaced apart (or dispersed) on the nanoparticles and suitably exposed on the surface of the nanoparticles.
[0052] Step c) suitably involves dispersing the catalyst precursor obtained in step b) in a solvent and adding the source of the second metal to the suspension. The solvent may be an alcohol, for example ethanol. The source of the second metal may be added slowly to the suspension, for example dropwise. Suitably the suspension is stirred for at least 30 minutes or 1 hour, suitably at a temperature of between 30 and 50°C, for example approximately 40°C to form the selective oxidation catalyst. The solid selective oxidation catalyst may be separated from the solvent by centrifuge.
[0053] Suitably, the second metal is platinum. In such embodiments, the source of the second metal used in step c) is a source of platinum, for example a platinum complex such as H2PtCle.
[0054] The selective oxidation catalyst may be obtained after step c) as a powder. The selective oxidation catalyst may be subsequently immobilised on a further support structure in a fixed bed catalytic reactor or a vehicle catalytic convertor, using know techniques, in order to be used for the selective catalytic oxidation of ammonia in gas streams.
[0055] In some embodiments of the present invention, the second metal is cobalt. In such embodiments the selective oxidation catalyst may be prepared by:
[0056] A) admixing a support material with a material comprising the first metal and a source of the cobalt, for example Co(NC>3)3, suitably in a solvent such as water; and
[0057] B) treating the mixture obtained in step A) with a reducing agent, for example NaBH4, to provide the selective oxidation catalyst.
[0058] According to a third aspect of the present invention, there is provided a method of catalytic oxidation of NH3, the method comprising the steps of:
[0059] 1) providing a selective oxidation catalyst according to the first aspect; 2) contacting the selective oxidation catalyst with an incoming gas stream comprising NHs and C>2 to selectively oxidise the NH3 to N2 and produce an exhaust gas stream; and
[0060] 3) removing the exhaust gas stream from the selective oxidation catalyst.
[0061] The selective oxidation catalyst may have any of the suitable features and advantages described above in relation to the first aspect.
[0062] The steps of the method are suitably carried out in the order of step 1) followed by step 2) followed by step 3).
[0063] As shown by the examples discussed below, the inventors have found that the selective oxidation catalyst of the first aspect can provide a highly efficient and selective method of catalytic oxidation of NH3 in an incoming gas stream, in a method of this third aspect.
[0064] The selective oxidation catalyst provided in step 1) is suitably arranged on a further support structure in a fixed bed catalytic reactor or a vehicle catalytic convertor, using know techniques. In some embodiments, the selective oxidation catalyst is provided in a vehicle exhaust catalytic convertor system and arranged downstream in the system from a selective catalytic reduction module in said catalytic convertor and is arranged to receive an incoming gas stream from the selective catalytic reduction module which may contain ammonia. Suitable arrangements of such systems are known in the art.
[0065] Step 2) of the method involves contacting the selective oxidation catalyst with an incoming gas stream comprising NH3 and O2 to selectively oxidise the NH3 to N2. The incoming gas stream suitably comprises at least 20 ppm NH3, at least 50 ppm NH3 or at least 100 ppm NH3. The incoming gas stream may comprise up to 10,000 ppm or up to 5,000 ppm NH3. The incoming gas stream suitably comprises at least 5,000 ppm O2, at least 2% O2 or at least 10% O2. Step 2) suitably involves providing O2 to the incoming gas stream from a source of O2 gas, for example atmospheric air which may be drawn into the system operating the method of this third aspect.
[0066] Suitably the selectivity of the oxidation of NH3 to N2 in step 2) is at least 85%, at least 90% or at least 95%.
[0067] Suitably the incoming gas stream has a temperature of at least 150°C or at least 200°C. Suitably the incoming gas stream has a temperature of from 150 to 500°C, suitably from 200 to 500°C or from 200 to 400°C. Such temperatures over which the method of this third aspect can operate with high conversion and selectivity mean that the method can be effective with incoming gas streams of varying temperature, for example as produced in a diesel-powered vehicle wherein the exhaust gases produced by the vehicle are initially relatively cool after start-up and become hotter as the vehicle engine warms up during continued operation. The method operating effectively over this range of temperature is beneficial for the overall reduction in NH3 (and NOX) production of the vehicle.
[0068] Suitably the selective oxidation catalyst selectively oxidises the NH3 in the incoming gas stream to N2 in the presence of O2 to N2, with minimal production of NOXspecies and minimal passage of unreacted NH3 through the catalyst.
[0069] Suitably the exhaust gas stream comprises less than 10 ppm NH3, suitably less than 5 ppm NH3, suitably less than 2 ppm NH3.
[0070] Suitably the exhaust gas stream comprises less than 10 ppm NO, suitably less than 5 ppm NO, suitably less than 2 ppm NO.
[0071] Examples
[0072] Synthesis of Example 1
[0073] The following procedure was used to prepare the PtiCu / ALOs selective oxidation catalyst of Example 1 which comprises particles of platinum dispersed on the copper oxide nanoparticles, the nanoparticles being impregnated in the AI2O3 support. The Pti denotes particles of platinum (single atoms and / or sub-nanometre particles of platinum).
[0074] Synthesis of Cu / A Oy. The Y-AI2O3 (0.5 g, Johnson Matthey) was dispersed in ethanol (20 mL) under vigorous stirring at room temperature. To the resulting suspension, a solution containing CU(NO3)23H2O (95 mg, 0.4 mmol) in ethanol (5 mL) was slowly added, and stirring was continued for 12 h at room temperature. The reaction mixture was further heated at 40°C under stirring until all the solvent had evaporated. The remaining solid was heated to 300°C for 1 h under 15% F Ar in a tube furnace to afford the CU / AI2O3 catalyst precursor having nanoparticles of copper oxide dispersed on the AI2O3 support.
[0075] Synthesis of PtiCu / A Oy. The Pti-Cu / AhOs selective oxidation catalyst was prepared via galvanic replacement between the copper nanoparticles and H2PtCle. CU / AI2O3 was dispersed in ethanol (25 mL), avoiding contact with air, and the resulting suspension was heated at 60°C for 10 min. A solution of H2 tCle (2 mg) dissolved in ethanol (2 mL) was added slowly to the reaction mixture. After stirring for 2 h at 40°C, the solution was cooled to room temperature, and then the sample was collected by centrifugation and washed with ethanol (5 x 30 mL). After drying at 40°C for 24 h, the selective oxidation catalyst Pti-Cu / ALOs containing particles of platinum dispersed on the copper oxide nanoparticles was obtained as a grey powder. The platinum content of the Pti-Cu / ALOs catalyst was between 0.4 and 0.8 wt%, based on the weight of the selective oxidation catalyst. The copper oxide content of the Pti-Cu / ALOs catalyst was approximately 5 wt%, based on the weight of the selective oxidation catalyst. Synthesis of Examples 2-5
[0076] The above procedure was used to prepare the further example catalysts 2-5 of formula M1CU / AI2O3 catalysts of the present invention, wherein M = Au (Example 2), Ag (Example 3), Rh (Example 4) and Ru (Example 5), via galvanic replacement using AuCh, AgNOs, RhCh, RuCh, respectively, to replace the H2PtCle. Mi in formula M1CU / AI2O3 denotes particles of the second metal M (single atoms and / or sub-nanometre particles of M).
[0077] Synthesis of Example 6
[0078] The following procedure was used to prepare the C01CU / AI2O3 catalyst (Example 6). Y-AI2O3 (0.5 g, Johnson Matthey), Cu(NC>3)23H2O (100 mg), Co(NC>3)36H20 (2.5 mg) were dispersed in H2O (10 mL) under vigorous stirring in an ice bath. To the resulting suspension, a solution containing NaBH4 (36 mg) in H2O (5 mL) was slowly added, and stirring was continued for 2 h without contacting air. Then the sample was collected by centrifugation and washed with H2O (5 x 30 mL). After drying at 40°C for 24 h, the C01CU / AI2O3 catalyst was obtained. C01 denotes particles of cobalt (single atoms and / or sub-nanometre particles of cobalt).
[0079] Catalytic performance measurement
[0080] The performance of the catalyst of Example 1 and the comparative known catalysts listed below in ammonia selective catalytic oxidation was evaluated in a fixed-bed flow reactor using the following procedure.
[0081] Comparative catalysts:
[0082] Ptr / o-Cu / ALOs
[0083] Pto i%-Cu / AI203
[0084] Pt / ALOs
[0085] CU / AI2O3
[0086] The reaction gas flow contained: 5000 ppm NH3, 5 vol% O2, and the balance He. The gas flowed at a rate of 100 mL / min. 50 mg of catalyst was placed in a reaction tube, and the quantification of products was performed with the Quadrupole Mass Spectrometer (MS) Quantitative Gas Analyser (Hiden Analytical, UK). The reaction was investigated at temperatures ranging from 200°C to 450°C. The reaction was kept stable for at least 30 minutes after attaining a steady-state at each reaction temperature to detect the MS signals of (NH3 and O2) and products (N2, N2O and NO). Results
[0087] Figure 1 shows the catalytic performance of the Example 1 catalyst and the comparative catalysts in the selective catalytic oxidation of ammonia. Figure 1 (a) shows NH3 conversion at 5000 ppm NH3 as a function of temperature for the different catalysts. These results show that the Example 1 catalyst is significantly more effective in terms of NH3 conversion at lower temperatures than the comparative catalysts. Figure 1 (b) shows N2 selectivity of the catalysts at different temperatures. These results show that the Example 1 catalyst has high selectivity for N2 formation across the range of temperatures tested - 150 to 450°C. The concentration of 5000 ppm NH3 used is five times higher than the standard NH3 slip conditions commonly encountered in real-world situations.
[0088] Figure 2 shows the yield of N2, N2O and NO of the Example 1 Pti-Cu / AhOs catalyst at different temperatures. Figures 3(a) and 3(b) show the yield of N2, N2O and NO for the example and comparative catalysts at 250°C and 400°C, respectively. The Example 1 catalyst showed the best combination of yield of N2 and selectivity for N2 over NOXspecies, at these temperatures.
[0089] Figures 4A-4E show NH3 conversion and N2 selectivity as a function of temperature for alternative example M1CU / AI2O3 catalysts (Examples 2-6) of the present invention, wherein M = Au, Ag, Rh, Ru and Co, respectively. These results show that each example provides a beneficial combination of NH3 conversion and selectivity. The C0CU / AI2O3 catalyst of Example 6 shows a particularly advantageous high conversion of NH3 at relatively low temperatures 150-200°C, whilst providing high selectivity for N2 production.
[0090] In addition to activity and selectivity, the stability of such catalysts over prolonged periods is also important for effective performance in use. The long-term stability of the Example 1 Pti-Cu / AhOs catalyst was tested in a fixed bed reactor under continuous flow conditions. Figure 5 shows the results of this stability test of 1wt% Pti-Cu / AhOs at a temperature of 200°C for 100 h. The reaction conditions used were as follows: 50 mg catalyst, 5000 ppm NH3, 5% O2 balanced in He, gas flow: 100 mL / min, WHSV=600 mlNH3-h’1-g’1. The NH3 concentration used is five times higher than the standard NH3 slip conditions in a diesel engine exhaust. These results show that the activity and selectivity did not change over time, demonstrating that the Example 1 Pti-Cu / AhOs catalyst is stable without any deactivation over continued use.
[0091] XPS analysis
[0092] X-ray photoelectron spectroscopy (XPS) data were recorded using a Thermo-scientific XPS K-alpha surface analysis machine using an Al source. Samples of the Example 1 catalyst, the Example 6 catalyst and the comparative CU / AI2O3 catalyst were immobilized on silicon chips for measurement. C1s electron at 284.8 eV was used as a standard reference to calibrate the photoelectron energy shift. The XPS spectra obtained are shown in Figures 6A-6C, respecitvely. The XPS spectra show that these catalysts have similar Cu chemical oxidation state, and the main surface species is Cu+. XRD analysis
[0093] X-ray diffraction (XRD) measurements of the Example 1 , 2, 4 and 6 catalysts and the comparative CU / AI2O3 catalyst were performed on StadiP diffractometer from STOE with a Mo source (Ka = 0.7093165 A). The operating voltage and current are 40kV and 30mA, respectively. With a resolution of 0.015° each step, the signals of 20 in the range of 2°-40° were collected. The XRD spectra are shown in Figure 7. These spectra show only diffraction peaks from AI2O3 and are therefore similar, due to the nanoparticles providing a small proportion of the catalysts.
[0094] STEM analysis
[0095] Scanning transmission electron microscope (STEM) images were recorded for the Example 1 catalyst using the JEOL ARM 200F and 300F transmission electron microscopes in bright field (BF) (Figure 8a) and high-angle annular dark field (HAADF) (Figure 8b) modes at 200keV in Diamond Light Source. The samples were loaded onto Au grids by sprinkling a small amount of dry sample powder.
[0096] In the HAADF images, nanoparticles are brighter with higher Z contrasts, while in BF images they are darker. Nanoparticles with a similar average particle size (2 nm) are uniformly dispersed over the support in the catalyst of Example 1 .
[0097] In conclusion, the Example 1 (Pti-Cu / AhOs) catalyst out-performed known catalysts in ammonia selective catalytic oxidation. The Example 1 catalyst achieved a higher than 95% selectivity of N2 between 150°C and 400°C. This high selectivity was achieved across a wide temperature of operation. Example 1 therefore surpasses the performance of the commercially available Pt / ALOs catalysts and the other comparative catalysts. The addition of Pt particles appears to significantly promote the activity of Pti-Cu / AhOs. Compared with 1wt% Pt / ALOs, the T50 (the temperature which achieves 50% NH3 conversion) reduces from 265°C to 215°C. Similarly beneficial results were obtained with the Example 2-6 catalysts having alternative metals providing the particles of the second metal on the nanoparticles of the first metal. In particular, Example 6 wherein M = Co demonstrated advantageous high conversion of NH3 at relatively low temperatures 150-200°C, whilst providing high selectivity for N2 production. The selective oxidation catalysts of the present invention may therefore beneficially provide a more effective selective catalytic reduction of ammonia in vehicle exhaust or industrial waste gas streams, compared to currently used catalysts. The catalysts and methods of the present invention may therefore provide a reduction in ammonia and NOXemissions from said vehicle exhaust or industrial waste gas streams, and consequently reduce pollution and the environmental damage which it causes. Although a few preferred embodiments have been shown and described, it will be appreciated by those skilled in the art that various changes and modifications might be made without departing from the scope of the invention, as defined in the appended claims.
[0098] Throughout this specification, the term “comprising” or “comprises” means including the component(s) specified but not to the exclusion of the presence of other components. The term “consisting essentially of’ or “consists essentially of’ means including the components specified but excluding other components except for materials present as impurities, unavoidable materials present as a result of processes used to provide the components, and components added for a purpose other than achieving the technical effect of the invention. Typically, when referring to compositions, a composition consisting essentially of a set of components will comprise less than 5% by weight, typically less than 3% by weight, more typically less than 1 % by weight of non-specified components.
[0099] The term “consisting of’ or “consists of’ means including the components specified but excluding addition of other components.
[0100] Whenever appropriate, depending upon the context, the use of the term “comprises” or “comprising” may also be taken to encompass or include the meaning “consists essentially of’ or “consisting essentially of’, and may also be taken to include the meaning “consists of’ or “consisting of’.
[0101] For the avoidance of doubt, wherein amounts of components in a composition are described in wt%, this means the weight percentage of the specified component in relation to the whole composition referred to.
[0102] The optional features set out herein may be used either individually or in combination with each other where appropriate and particularly in the combinations as set out in the accompanying claims. The optional features for each aspect or exemplary embodiment of the invention as set out herein are also to be read as applicable to any other aspect or exemplary embodiments of the invention, where appropriate. In other words, the skilled person reading this specification should consider the optional features for each exemplary embodiment of the invention as interchangeable and combinable between different exemplary embodiments.
[0103] Attention is directed to all papers and documents which are filed concurrently with or previous to this specification in connection with this application and which are open to public inspection with this specification, and the contents of all such papers and documents are incorporated herein by reference.
[0104] All of the features disclosed in this specification (including any accompanying claims, and drawings), and / or all of the steps of any method or process so disclosed, may be combined in any combination, except combinations where at least some of such features and / or steps are mutually exclusive. Each feature disclosed in this specification (including any accompanying claims, and drawings) may be replaced by alternative features serving the same, equivalent or similar purpose, unless expressly stated otherwise. Thus, unless expressly stated otherwise, each feature disclosed is one example only of a generic series of equivalent or similar features. The invention is not restricted to the details of the foregoing embodiment(s). The invention extends to any novel one, or any novel combination, of the features disclosed in this specification (including any accompanying claims, and drawings), or to any novel one, or any novel combination, of the steps of any method or process so disclosed.
Claims
Claims1 . A selective oxidation catalyst comprising: a support; nanoparticles comprising a first metal; and particles of a second metal selected from platinum, palladium, ruthenium, rhodium, cobalt, silver and gold; wherein the nanoparticles are arranged on the support and the particles of the second metal are arranged on outer surfaces of the nanoparticles.
2. The selective oxidation catalyst according to claim 1 , wherein the first metal is copper, preferably wherein the nanoparticles are copper oxide nanoparticles.
3. The selective oxidation catalyst according to claim 1 or claim 2, wherein the second metal is platinum.
4. The selective oxidation catalyst according to claim 1 or claim 2, wherein the second metal is cobalt.
5. The selective oxidation catalyst according to any one of the preceding claims, wherein the support comprises aluminium oxide, preferably Y-AI2O3.
6. The selective oxidation catalyst according to any one of the preceding claims, wherein the particles of the second metal are present in an amount of from 0.01 to 0.8 wt%, based on the weight of the selective oxidation catalyst.
7. The selective oxidation catalyst according to any one of the preceding claims, wherein the nanoparticles comprising the first metal are present in an amount of from 1 to 10 wt%, based on the weight of the selective oxidation catalyst.
8. The selective oxidation catalyst according to any one of the preceding claims, wherein the particles of the second metal are provided by galvanic replacement of atoms of the first metal in the nanoparticles with the particles of the second metal.
9. A method of preparing a selective oxidation catalyst according to any one of claims 1 to 8, the method comprising the steps of: a) admixing a support material with a material comprising the first metal;b) converting the mixture obtained in step a) to a catalyst precursor comprising the support and nanoparticles comprising the first metal; c) treating the catalyst precursor with a source of the second metal to carry out a galvanic replacement of atoms of the first metal of the nanoparticles with the second metal and provide the selective oxidation catalyst.
10. The method of claim 9, wherein the support material is aluminium oxide, the material comprising the first metal is copper(ll) nitrate and the catalyst precursor produced in step b) is an aluminium oxide comprising copper oxide nanoparticles.
11. The method according to claim 9 or claim 10, wherein step b) involves heating the mixture obtained in step a) to a temperature of between 200 and 400°C.
12. The method according to any one of claims 9 to 11 , wherein the second metal is platinum, preferably wherein the source of the second metal used in step c) is H2PtCle.
13. A method of catalytic oxidation of NH3, the method comprising the steps of:1) providing a selective oxidation catalyst according to any one of claims 1 to 8;2) contacting the selective oxidation catalyst with an incoming gas stream comprising NHs and C>2 to selectively oxidise the NH3 to N2 and produce an exhaust gas stream; and3) removing the exhaust gas stream from the selective oxidation catalyst.
14. The method according to claim 13, wherein the incoming gas stream comprises at least 100 ppm NH3.
15. The method according to claim 13 or claim 14, wherein the exhaust gas stream comprises less than 10 ppm NH3.
16. The method according to any one of claims 13 to 15, wherein the incoming gas stream has a temperature of at least 200°C.
17. The method according to any one of claims 13 to 16, wherein the selectivity of the oxidation of NH3 to N2 in step 2) is at least 90%.
Citation Information
Patent Citations
Ammonia Decomposition Catalyst and Process for Decomposition of Ammonia Using the Catalyst
US20090060809A1
Oxidation catalyst for a diesel engine exhaust
US20180085707A1