Method for manufacturing organic semiconductor device, method for manufacturing light-emitting device, and method for manufacturing photosensor

The method of forming a convex structure layer and using specific materials like aluminum oxide and indium gallium zinc oxide addresses the adhesion issues between protective and organic semiconductor layers, enhancing the yield and quality of high-definition organic semiconductor devices by reducing peeling and defects.

WO2024241140A1PCT designated stage expired Publication Date: 2024-11-28SEMICON ENERGY LAB CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/IB2024/054615
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-19
Filing Date
2024-05-13
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

The challenge in manufacturing high-definition organic semiconductor devices is the occurrence of defects due to poor adhesion between protective layers and organic semiconductor layers, leading to peeling issues during processing, which affects the yield and quality of the devices.

Method used

A method involving the formation of a structure layer with a convex shape on the organic semiconductor layer, followed by a protective layer and a mask layer, using materials like aluminum oxide and indium gallium zinc oxide, to enhance adhesion and reduce peeling, thereby suppressing defects and improving yield.

Benefits of technology

This approach effectively reduces peeling and defects, allowing for the production of high-definition organic semiconductor devices with improved yield and quality by increasing the contact area between the protective layer and the substrate, ensuring better adhesion and processing stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure IB2024054615_28112024_PF_FP_ABST
    Figure IB2024054615_28112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides a method for manufacturing an organic semiconductor device, the method being applicable to high-definition organic semiconductor devices and making it possible to suppress the occurrence of defects. Provided is a method for manufacturing an organic semiconductor device, the method including the steps of: forming a first layer on a first electrode; forming, on the first layer, a second layer of a material that forms a structure with a protruding shape; forming a third layer on the first layer and the structure; processing the third layer into a predetermined shape; and processing the first layer using the processed third layer as a mask, wherein the first layer is an organic semiconductor layer and the third layer is formed from a material different than the material constituting each of the organic semiconductor and the second layer.
Need to check novelty before this filing date? Find Prior Art

Description

Method for manufacturing organic semiconductor device, method for manufacturing light-emitting device, and method for manufacturing photosensor

[0001] One embodiment of the present invention relates to an organic compound, an organic EL device, a display module, a lighting module, a display device, a light-emitting device, an electronic device, a lighting device, and an electronic device. Note that one embodiment of the present invention is not limited to the above technical field. The technical field of one embodiment of the invention disclosed in this specification etc. relates to an object, a method, or a manufacturing method. Alternatively, one embodiment of the present invention relates to a process, a machine, manufacture, or a composition of matter. Therefore, more specific examples of the technical field of one embodiment of the present invention disclosed in this specification include semiconductor devices, display devices, liquid crystal display devices, light-emitting devices, lighting devices, power storage devices, memory devices, imaging devices, driving methods thereof, and manufacturing methods thereof.

[0002] Organic EL devices that utilize electroluminescence (EL) using organic compounds are becoming increasingly practical. These organic EL devices basically consist of a pair of electrodes sandwiching an organic compound layer (EL layer) containing a light-emitting material between them. By applying a voltage to this device, carriers are injected, and the recombination energy of the carriers is utilized to emit light from the light-emitting material.

[0003] Since such organic EL devices are self-luminous, when used as display pixels, they have advantages such as higher visibility and no need for backlighting compared to liquid crystals, making them particularly suitable for flat panel displays. Another major advantage of displays using such organic EL devices is that they can be fabricated to be thin and lightweight. Another feature is their extremely fast response speed.

[0004] Furthermore, these organic EL devices can have a continuous light-emitting layer formed two-dimensionally, enabling them to emit light in a planar form. This is a feature that is difficult to obtain with point light sources such as incandescent lamps and LEDs, or linear light sources such as fluorescent lamps, making them highly useful as planar light sources for lighting and other applications.

[0005] Thus, light-emitting devices using organic EL devices are suitable for a variety of electronic devices, but research and development is ongoing to seek organic EL devices with even better characteristics.

[0006] In order to obtain a light-emitting device with higher resolution using an organic EL device, research has been conducted into patterning of organic layers by photolithography using photoresist, etc., instead of vapor deposition using a metal mask. By using photolithography, a high-resolution light-emitting device with an EL layer spacing of several micrometers can be obtained (see, for example, Patent Document 1).

[0007] Special table 2018-521459 publication

[0008] When the organic semiconductor layer is shaped by photolithography, a layer for protecting the organic semiconductor layer (hereinafter also referred to as a protective layer) may be formed on the organic layer.

[0009] The protective layer must satisfy many requirements, including minimal damage to the organic layer during formation and shaping, and a low selectivity to etching during shaping of the organic layer. However, even protective layers that satisfy these requirements can peel off or disappear during processes other than the protective layer peeling process (processing of the protective layer or the organic layer). One possible cause of this is poor adhesion between the protective layer and the organic layer. If the protective layer peels off or disappears during a process that requires protection of the organic layer, processing cannot be performed as expected, preventing the formation of the desired organic semiconductor layer, resulting in defects.

[0010] Therefore, an object of one embodiment of the present invention is to provide a manufacturing method for an organic semiconductor device that can suppress the occurrence of defects.An object of one embodiment of the present invention is to provide a manufacturing method for an organic semiconductor device that can be applied to a high-resolution organic semiconductor device and can suppress the occurrence of defects.Another object of one embodiment of the present invention is to provide a manufacturing method for an organic semiconductor device that can produce an organic semiconductor device with good characteristics.Another object of one embodiment of the present invention is to provide a manufacturing method for an organic semiconductor device with a high yield.

[0011] That is, one aspect of the present invention is a method for manufacturing an organic semiconductor device, comprising the steps of: forming a first layer on a first electrode; forming a second layer on the first layer from a material that forms a structure having a convex shape; forming a third layer on the first layer and the second layer; processing the third layer into a predetermined shape; and processing the first layer using the processed third layer as a mask, wherein the first layer is an organic semiconductor layer and the third layer is composed of a material different from the materials that constitute the first layer and the second layer.

[0012] Alternatively, another aspect of the present invention is a method for manufacturing an organic semiconductor device, the method comprising the steps of: forming a first layer on a first electrode; forming a second layer on the first layer, the second layer being made of a material that forms a structure having a convex shape; forming a third layer on the first layer and the second layer; forming a fourth layer on the third layer; processing the third layer and the fourth layer into predetermined shapes; and processing the first layer using one or both of the processed third layer and the fourth layer as a mask; the first layer is an organic semiconductor layer, and the third layer and the fourth layer are made of a material different from that of the first layer and the second layer, and the third layer and the fourth layer are made of different materials.

[0013] Another embodiment of the present invention is a method for manufacturing an organic semiconductor device having the above structure, wherein the first layer is processed by dry etching or wet etching.

[0014] Another embodiment of the present invention is a method for manufacturing an organic semiconductor device having the above structure, wherein the fourth layer contains an inorganic compound.

[0015] Another embodiment of the present invention is a method for manufacturing an organic semiconductor device having the above structure, wherein the fourth layer is made of one or more selected from aluminum, indium, tungsten, molybdenum, gallium, zinc, silicon, and oxides or nitrides thereof.

[0016] Another embodiment of the present invention is the method for manufacturing an organic semiconductor device having the above structure, wherein the glass transition temperature of the material contained in the second layer is 120° C. or lower.

[0017] Alternatively, another aspect of the present invention is a method for manufacturing an organic semiconductor device having the above-described structure, wherein, in differential scanning calorimetry of the material contained in the second layer, a crystallization temperature is observed during one or both of a temperature increase process and a temperature decrease process.

[0018] Another embodiment of the present invention is a method for manufacturing an organic semiconductor device having the above structure, wherein the structure has a width of 10 nm to 200 nm and a height of 5 nm to 100 nm.

[0019] Another embodiment of the present invention is a method for manufacturing an organic semiconductor device having the above structure, wherein the structure has a width of 100 nm to 150 nm and a height of 20 nm to 60 nm.

[0020] Alternatively, in the above-described configuration, another aspect of the present invention is a method for manufacturing a semiconductor device, wherein the density of the structures is 0.1 / μm 2 0.5 pieces / μm or more 2 The following is a method for fabricating an organic semiconductor device.

[0021] Another embodiment of the present invention is a method for manufacturing an organic semiconductor device having the above structure, wherein a material forming the second layer contains an organometallic complex.

[0022] Another embodiment of the present invention is a method for manufacturing an organic semiconductor device having the above structure, wherein the material forming the second layer has an electron transporting property.

[0023] Another embodiment of the present invention is a method for manufacturing an organic semiconductor device having the above structure, wherein a material constituting the second layer has a π-electron-deficient heterocycle in its molecular structure.

[0024] Another embodiment of the present invention is a method for manufacturing an organic semiconductor device having the above structure, wherein the material constituting the second layer has an electron-withdrawing substituent in its molecular structure.

[0025] Another embodiment of the present invention is a method for manufacturing an organic semiconductor device having the above structure, wherein the third layer contains an inorganic compound.

[0026] Another embodiment of the present invention is a method for manufacturing an organic semiconductor device having the above structure, wherein the third layer is made of one or more selected from aluminum, indium, tungsten, molybdenum, gallium, zinc, silicon, and oxides or nitrides thereof.

[0027] Another embodiment of the present invention is a method for manufacturing an organic semiconductor device having the above structure, wherein the third layer is a layer containing aluminum oxide.

[0028] Another embodiment of the present invention is a method for manufacturing an organic semiconductor device having the above structure, wherein the third layer is formed by an atomic layer deposition (ALD) method.

[0029] Another embodiment of the present invention is a method for manufacturing a light-emitting device having any of the above structures, in which the first layer includes a light-emitting layer.

[0030] Another embodiment of the present invention is a method for manufacturing a light-emitting device having the above structure, wherein the first layer has a stacked structure including, from the first electrode side, a hole injection layer, a hole transport layer, a light-emitting layer, and an electron transport layer.

[0031] Another embodiment of the present invention is a method for manufacturing a photosensor having the above structure, in which the first layer includes a photoelectric conversion layer.

[0032] Another embodiment of the present invention is a method for manufacturing an organic transistor having any of the above structures, in which the first layer includes an active layer.

[0033] Another embodiment of the present invention is a method for manufacturing an organic semiconductor device having the above structure, wherein the second layer is formed by a vacuum deposition method.

[0034] In this specification, the term "light-emitting device" includes an image display device using an organic EL device. The term "light-emitting device" may also include a module in which a connector, such as an anisotropic conductive film or a TCP (Tape Carrier Package), is attached to an organic EL device, a module in which a printed wiring board is provided at the end of a TCP, or a module in which an IC (integrated circuit) is directly mounted on an organic EL device using a COG (Chip On Glass) method. Furthermore, lighting fixtures and the like may have a light-emitting device.

[0035] One embodiment of the present invention can provide a manufacturing method for an organic semiconductor device that can suppress the occurrence of defects. Alternatively, one embodiment of the present invention can provide a manufacturing method for an organic semiconductor device that can be applied to a high-resolution organic semiconductor device and can suppress the occurrence of defects. Alternatively, one embodiment of the present invention can provide a manufacturing method for an organic semiconductor device that can manufacture an organic semiconductor device with good characteristics. Alternatively, one embodiment of the present invention can provide a manufacturing method for an organic semiconductor device with a high yield.

[0036] Note that the description of this effect does not preclude the existence of other effects. Note that one embodiment of the present invention does not necessarily have all of these effects. Note that effects other than these will become apparent from the description in the specification, drawings, claims, etc., and it is possible to extract other effects from the description in the specification, drawings, claims, etc.

[0037] FIGS. 1A and 1B are schematic diagrams of an organic semiconductor layer, a structural layer, and a protective layer. FIGS. 2A and 2B are schematic diagrams of an organic semiconductor layer, a structural layer, and a protective layer. FIGS. 3A to 3E are diagrams illustrating a method for processing an organic semiconductor layer. FIGS. 4A to 4D are diagrams illustrating a method for processing an organic semiconductor layer. FIGS. 5A to 5C are schematic diagrams of an organic semiconductor device. FIGS. 6A and 6B are schematic diagrams of an organic semiconductor device. FIGS. 7A to 7E are diagrams illustrating a method for manufacturing an organic semiconductor device. FIGS. 8A to 8D are diagrams illustrating a method for manufacturing an organic semiconductor device. FIGS. 9A to 9D are diagrams illustrating a method for manufacturing an organic semiconductor device. FIGS. 10A to 10C are diagrams illustrating a method for manufacturing an organic semiconductor device. FIGS. 11A to 11C are diagrams illustrating a method for manufacturing an organic semiconductor device. FIGS. 12A to 12C are diagrams illustrating a method for manufacturing an organic semiconductor device. FIG. 13 is a schematic diagram of a light-emitting device. FIGS. 14A and 14B are perspective views illustrating an example of a display module configuration. 15A and 15B are cross-sectional views showing an example of the configuration of a display device. FIG. 16 is a perspective view showing an example of the configuration of a display device. FIG. 17 is a cross-sectional view showing an example of the configuration of a display device. FIG. 18 is a cross-sectional view showing an example of the configuration of a display device. FIG. 19 is a cross-sectional view showing an example of the configuration of a display device. FIGS. 20A to 20D are views showing an example of an electronic device. FIGS. 21A to 21F are views showing an example of an electronic device. FIGS. 22A to 22G are views showing an example of an electronic device. FIGS. 23A and 23B are length-measuring SEM photographs of samples having structure layers of Structure 1 and Structure 5. FIGS. 24A and 24B are cross-sectional TEM photographs of samples having structure layers of Structure 1 and Structure 5. FIG. 25 is an optical microscope photograph and a cross-sectional TEM photograph of samples having structure layers of Structures 2 to 4.

[0038] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings. However, the present invention is not limited to the following description, and it will be readily understood by those skilled in the art that various changes in form and details can be made without departing from the spirit and scope of the present invention. Therefore, the present invention should not be interpreted as being limited to the description of the embodiments shown below.

[0039] In this specification, etc., a device fabricated using a metal mask or an FMM (fine metal mask, high-resolution metal mask) may be referred to as a device with an MM (metal mask) structure. In addition, in this specification, etc., a device fabricated without using a metal mask or an FMM may be referred to as a device with an MML (metal-maskless lithography) structure.

[0040] Furthermore, in this specification and the like, a film that has not undergone shape processing after deposition is generally referred to as a "film," and a film that has undergone shape processing is generally referred to as a "layer." However, these terms are used solely for the purpose of making it easier to understand the progress of the process, and there is no significant difference between them, so "film" can be read as a "layer" and "layer" as a "film." In particular, when describing a film that has not undergone a processing step, both terms are considered to have the same meaning.

[0041] (Embodiment 1) Vacuum deposition using a metal mask (mask deposition) is widely used as one method for fabricating an organic semiconductor film into a predetermined shape. However, with the recent trend toward higher density and higher definition, mask deposition is approaching its limit in achieving higher definition due to various reasons, including problems with alignment accuracy and the spacing between the mask and the substrate. On the other hand, by processing the shape of an organic semiconductor film using a photolithography method, it is possible to form a denser pattern. In addition, since photolithography can easily be used to fabricate large-area films, research into processing organic semiconductor films using photolithography is also being conducted.

[0042] However, in order to process the shape of an organic semiconductor film using photolithography, it is necessary to overcome many problems, such as the influence of exposure of the organic semiconductor film to the atmosphere, the influence of light irradiation when exposing the photosensitive resin, and the influence of the developer used when developing the exposed photosensitive resin.

[0043] These effects are considered problematic because they can cause situations such as the organic semiconductor film itself disappearing or the surface of the organic semiconductor film being damaged, resulting in a significant deterioration in the characteristics of devices subsequently fabricated.

[0044] 2A , a protective layer 1152 may be provided on the organic semiconductor film 1151 during processing by photolithography. It is preferable to further form a layer 1153 (hereinafter, sometimes referred to as a mask layer 1153) on the protective layer. By providing the protective layer 1152 or the mask layer 1153 and then performing a photolithography process, it is possible to reduce the influence of light irradiation and the influence of a developing solution when processing a photosensitive resin.

[0045] The protective layer 1152 needs to have a small selectivity with respect to etching when shaping the organic semiconductor film 1151. Therefore, the protective layer 1152 is preferably a layer having different properties from the organic semiconductor film 1151. A representative example of a material having different properties from the organic semiconductor film 1151, which is an organic compound, is an inorganic compound. Furthermore, it is preferable that the protective layer 1152 inflicts minimal damage on the organic semiconductor film 1151 when it is formed and shaped.

[0046] However, when a protective layer 1152 made of a material with different properties is provided on the organic semiconductor film 1151, the adhesion is often poor in principle, and separation (also called peeling) may occur between the organic semiconductor film and the protective layer as shown in Fig. 2B In particular, a film formed under gentle conditions (for example, a film formed by atomic layer deposition (ALD)) is dense, but may have poor adhesion to the underlying film (organic semiconductor film), and is therefore prone to peeling.

[0047] If peeling of the protective layer 1152 occurs, normal pattern formation of the organic semiconductor film cannot be performed, which directly leads to the occurrence of defects. Therefore, by suppressing peeling of the protective layer 1152, it is possible to suppress a decrease in yield.

[0048] Here, before providing the protective layer 1152 on the organic semiconductor film 1151, a layer (structure layer 1154) made of a material for forming the structure 1155 having a convex shape as shown in FIGS. 1A and 1B is provided, and the protective layer 1152 is provided thereon. This makes it possible to suppress peeling of the protective layer 1152 and to prevent defects. In one embodiment of the present invention, the structure 1155 refers to an island-like object made of a material different from that of the organic semiconductor film 1151 and provided on the organic semiconductor film 1151 or the surface 1156 of the structure layer 1154. Having a convex shape means that the structure 1155 has a height relative to the surface on which the structure 1155 is to be formed, and the height of the structure 1155 does not necessarily have a single peak. In other words, the structure 1155 may have multiple peaks, or may have valleys or holes and have an uneven shape. The surface on which the structure 1155 is to be formed refers to the surface of the organic semiconductor film 1151 or the surface 1156 of the structure layer 1154 excluding the portion on which the structure 1155 is to be formed. Even when the structures 1155 are provided in an island shape and not in a layer shape, the entire structure will be referred to as the structure layer 1154 for convenience.

[0049] The structure layer 1154 is a layer made of a material that, when formed by vapor deposition, forms a convex structure 1155 having a width of 10 nm or more and 200 nm or less, preferably 80 nm or more and 150 nm or less, and more preferably 100 nm or more and 150 nm or less, and a height of 5 nm or more and 100 nm or less, preferably 20 nm or more and 80 nm or less, and more preferably 20 nm or more and 60 nm or less.

[0050] In this specification, the width of the structure 1155 is defined as the distance between two points on the outline of the structure 1155 at the widest position when the structure 1155 is viewed from a direction perpendicular to the surface of the electrode. Alternatively, assuming a line that is approximately parallel to the electrode in a cross-sectional view of the structure 1155, the width is defined as the distance between the outlines of the structure on the line at the widest position.

[0051] The density of the structures 1155 is 0.01 pieces / μm 2 It is preferable that the number of particles is 0.1 / μm or more. 2It is more preferable that the number of particles is 50 / μm or more. 2 Preferably, the number is 5 or less per μm. 2 In the case of a high-definition semiconductor device with a resolution of 200 ppi or more, the number of particles is preferably 0.05 particles / μm or less. 2 1 piece / μm or more 2 Preferably, it is 0.1 particles / μm or less. 2 0.5 pieces / μm or more 2 More preferably, it is:

[0052] The structure layer 1154 is preferably formed using an organic compound or an organometallic complex having a glass transition point of 120° C. or lower. By using an organic compound or an organometallic complex having a glass transition point of 120° C. or lower, partial crystallization occurs during film formation, making it possible to form a convex structure.

[0053] The structure layer 1154 is preferably formed of an organic compound or an organometallic complex whose crystallization temperature is observed in one or both of a temperature increase process and a temperature decrease process in differential scanning calorimetry. By using an organic compound or an organometallic complex whose crystallization temperature is observed in one or both of a temperature increase process and a temperature decrease process in differential scanning calorimetry, partial crystallization occurs during film formation, making it possible to form a convex structure.

[0054] Furthermore, it is preferable that the material constituting the structure layer 1154 be a material having a π-electron-deficient heterocycle in its molecular structure or a material having an electron-transporting property, including a material having an electron-withdrawing group, because this allows for an organic semiconductor device with excellent characteristics to be obtained. Typically, the structure layer 1154 is removed from the organic semiconductor layer before a subsequent process is performed, but there are cases in which the structure layer 1154 is not completely removed and remains on the organic semiconductor layer 1151a. By including a material having a π-electron-deficient heterocycle in its molecular structure, including a material having an electron-withdrawing group, or having electron-transporting property, it is possible to suppress a deterioration in the characteristics of the organic semiconductor device even when the structure layer 1154 is not completely removed and remains on the organic semiconductor layer 1151a.

[0055] When the structure layer 1154 is a material having a π-electron-deficient heterocycle in its molecular structure, specific examples of the π-electron-deficient heterocycle include pyridine, pyrazine, pyrimidine, pyridazine, quinoline, quinolinol, isoquinoline, isoquinolinol, quinoxaline, quinazoline, azatriphenylene, dibenzoquinoxaline, dibenzoquinazoline, triazatriphenylene, tetraazatriphenylene, pentaazatriphenylene, hexaazatriphenylene, etc. Further examples include a fused ring in which two or more of the π-electron-deficient heterocycles are fused, and a fused ring in which two or more of the π-electron-deficient heterocycles are fused with a benzene ring.

[0056] When the material constituting the structure layer 1154 includes a material having an electron-withdrawing group, the electron-withdrawing group specifically refers to a halogen, a substituted or unsubstituted halogenated alkyl group having 1 to 6 carbon atoms, a substituted or unsubstituted alkoxy group having 1 to 6 carbon atoms, a substituted or unsubstituted halogenated alkoxy group having 1 to 6 carbon atoms, a cyano group, a nitro group, a carbonyl group, a carboxylic acid group, etc.

[0057] Specific examples of materials constituting the structure layer 1154 include (8-quinolinolato)lithium (abbreviation: Liq) and tris(8-quinolinolato)aluminum (abbreviation: Alq 3 ), bis(2-methyl-8-quinolinolato)(4-phenylphenolato)aluminum(III) (abbreviation: BAlq), (8-quinolinolato)sodium (abbreviation: Naq), (8-quinolinolato)potassium (abbreviation: Kq), bis(8-quinolinolato)zinc (abbreviation: Znq2), bis(8-quinolinolato)copper(II) (abbreviation: Cuq 2 ), tris(8-quinolinolato)cobalt(III) (abbreviation: Coq 3 ), tris(8-quinolinolato)gallium(III) (abbreviation: Gaq 3 ), tetrakis(8-quinolinolato)zirconium(VI) (abbreviation: Zrq 4 In addition to organometallic complexes such as those represented by the general formulas (G1) to (G4) below, organic compounds represented by the general formulas (G1) to (G4) below can also be suitably used.

[0058]

[0059] However, in the organic compound represented by the general formula (G1), X 1 ~X 6 each independently represents a carbon atom or a nitrogen atom. 1 ~R 12 each independently represents hydrogen, halogen, a substituted or unsubstituted halogenated alkyl group having 1 to 6 carbon atoms, a substituted or unsubstituted alkoxy group having 1 to 6 carbon atoms, a substituted or unsubstituted halogenated alkoxy group having 1 to 6 carbon atoms, a cyano group, a nitro group, a carbonyl group, or a carboxylic acid group, and adjacent substituents may be bonded to each other to form a ring. 1 ~X 6 is nitrogen, the nitrogen does not have hydrogen or a substituent, and therefore the corresponding R 1 , R 4 , R 5 , R 8 , R 9 , and R 12 is ignored. 1 ~R 12 is a carboxylic acid group, adjacent carboxylic acid groups may be dehydrated and condensed to form an acid anhydride ring.

[0060]

[0061] However, in the organic compound represented by the general formula (G2), X 1 ~X 12 each independently represents a carbon atom or a nitrogen atom. 1 ~R 18 each independently represents hydrogen, halogen, a substituted or unsubstituted halogenated alkyl group having 1 to 6 carbon atoms, a substituted or unsubstituted alkoxy group having 1 to 6 carbon atoms, a substituted or unsubstituted halogenated alkoxy group having 1 to 6 carbon atoms, a cyano group, a nitro group, a carbonyl group, or a carboxylic acid group, and adjacent substituents may be bonded to each other to form a ring. 1 ~X 12 is nitrogen, the nitrogen does not have hydrogen or a substituent, and therefore the corresponding R 1 , R 2 , R 5 ~R 8, R 11 ~R 14 , R 17 and R 18 is ignored. 1 ~R 18 is a carboxylic acid group, adjacent carboxylic acid groups may be dehydrated and condensed to form an acid anhydride ring.

[0062]

[0063] However, in the organic compound represented by the general formula (G3), X 1 ~X 10 each independently represents a carbon atom or a nitrogen atom. 1 ~R 13 and R 18 ~R 20 each independently represents hydrogen, halogen, a substituted or unsubstituted halogenated alkyl group having 1 to 6 carbon atoms, a substituted or unsubstituted alkoxy group having 1 to 6 carbon atoms, a substituted or unsubstituted halogenated alkoxy group having 1 to 6 carbon atoms, a cyano group, a nitro group, a carbonyl group, or a carboxylic acid group, and adjacent substituents may be bonded to each other to form a ring. 1 ~X 10 When is nitrogen, it does not have hydrogen or a substituent, and therefore the corresponding R 1 , R 2 , R 5 ~R 8 , R 11 ~R 13 , and R 18 is ignored. 1 ~R 13 and R 18 ~R 20 is a carboxylic acid group, adjacent carboxylic acid groups may be dehydrated and condensed to form an acid anhydride ring.

[0064]

[0065] However, in the organic compound represented by the general formula (G4), X 1 ~X 8 each independently represents a carbon atom or a nitrogen atom. 1 ~R7 , R 12 , R 13 and R 18 ~R 22 each independently represents hydrogen, halogen, a substituted or unsubstituted halogenated alkyl group having 1 to 6 carbon atoms, a substituted or unsubstituted alkoxy group having 1 to 6 carbon atoms, a substituted or unsubstituted halogenated alkoxy group having 1 to 6 carbon atoms, a cyano group, a nitro group, a carbonyl group, or a carboxylic acid group, and adjacent substituents may be bonded to each other to form a ring. 1 ~X 8 When is nitrogen, it does not have hydrogen or a substituent, and therefore the corresponding R 1 , R 2 , R 5 ~R 7 , R 12 , R 13 , and R 18 is ignored. 1 ~R 7 , R 12 , R 13 and R 18 ~R 22 is a carboxylic acid group, adjacent carboxylic acid groups may be dehydrated and condensed to form an acid anhydride ring.

[0066] Among the organic compounds represented by the general formulas (G1) to (G4), it is preferable to use an organic compound having a dipole moment of less than 20 Debye, since the organic compound is likely to aggregate, thereby facilitating the formation of a structure, and it is particularly preferable to use an organic compound having a dipole moment of less than 11 Debye. Among the organic compounds represented by the general formulas (G1) to (G4), it is preferable to use a compound whose crystallization temperature is observed in DSC (Differential Scanning Calorimetry), since this facilitates the formation of a structure. When a glass transition point is observed, it is preferable for the temperature to be less than 120° C., since this facilitates the formation of a structure. Furthermore, in TG-DTA (Thermogram-Differential Thermal Analysis), it is preferable that the thermal behavior of melting is not observed at a temperature lower than the temperature at which the mass change occurs, and that the mass change occurs by sublimation, because this facilitates the formation of the structure. TG-DTA is performed at a pressure of 1×10 −4 It is preferable to carry out the process within the range of Pa, but more preferably, it is carried out under reduced pressure (10 Pa or less) as in the case of forming a thin film.

[0067] Examples of organic compounds represented by the above general formulas include organic compounds represented by the following structural formulas (1) to (40).

[0068]

[0069]

[0070] The organic compound represented by any of the general formulas (G1) to (G4) is deposited on the active layer by vacuum deposition to a thickness of 1 nm to 30 nm, forming the structure 1155. Note that the materials used to form the structure 1155 do not form flat films. Therefore, the deposition amount of the structure is determined using any material that forms a flat film as a reference material. For example, 4,4'-bis[N-(1-naphthyl)-N-phenylamino]biphenyl (abbreviation: NPB) can be used as the reference material, and deposition can be performed using the calibration curve of NPB. By using the calibration curve of the same substance each time, it is possible to control the deposition amount even if the exact deposition amount is unknown. In this study, NPB was used as the reference material, and the organic compound represented by any of the general formulas (G1) to (G4) was deposited in an amount corresponding to a thickness of 1 nm to 30 nm, forming the structure. That is, the deposition of a film amount equivalent to a film thickness of 1 nm to 30 nm can be said to be, more precisely, deposition of a film amount equivalent to a film thickness of 1 nm to 30 nm for NPB.

[0071] By providing the structure layer 1154 as described above, the presence of the convex portions of the structure 1155 increases the contact area with the deposition surface of the protective layer 1152. This makes it possible to suppress peeling of the protective layer 1152.

[0072] As described above, the protective layer 1152 preferably has a small selectivity with respect to etching when shaping the organic semiconductor layer. That is, the protective layer 1152 is preferably a layer having different characteristics from the organic semiconductor layer. Representative examples of materials having different characteristics from the organic semiconductor, which is an organic compound, include inorganic compounds. Specific examples include metal materials such as aluminum, indium, tungsten, titanium, molybdenum, tantalum, gallium, and zinc, as well as non-metallic inorganic materials such as silicon, and alloys and compounds containing these materials. Specific examples of these compounds and alloys include aluminum oxide, silicon nitride, silicon oxide, tantalum nitride, alloys containing molybdenum and niobium, alloys containing molybdenum and tungsten, indium gallium zinc oxide (In-Ga-Zn oxide, also referred to as IGZO), indium oxide, indium zinc oxide (In-Zn oxide), indium tin oxide (In-Sn oxide), indium titanium oxide (In-Ti oxide), indium tin zinc oxide (In-Sn-Zn oxide), indium titanium zinc oxide (In-Ti-Zn oxide), and indium gallium tin zinc oxide (In-Ga-Sn-Zn oxide). Alternatively, indium tin oxide containing silicon can also be used. Aluminum oxide, IGZO, molybdenum oxide, and the like are particularly preferred for the protective layer.

[0073] Among these, it is more preferable that the protective layer be made of a material that can be applied with a film formation method that causes little damage to the organic semiconductor layer during film formation, such as an ALD method or a chemical vapor deposition (CVD) method. It is also more preferable that the protective layer be made of a material that can be applied with a film formation method that causes little damage to the organic semiconductor layer during processing and removal. The protective layer may also be formed by a film formation method such as a sputtering method.

[0074] An aluminum oxide film formed by the ALD method is particularly suitable as a protective layer because it causes little damage to the organic semiconductor layer during film formation, is dense and has high barrier properties, and causes little damage to the organic semiconductor layer during shaping and removal. However, on the other hand, aluminum oxide films formed by the ALD method tend to have low adhesion to the organic semiconductor layer, partly due to the mild film formation conditions. For this reason, the embodiment in which an aluminum oxide protective layer formed by the ALD method is used is an embodiment in which the effect of providing a structural layer is particularly significant. Similarly, a silicon nitride film formed by the CVD method is also suitable as a protective layer.

[0075] The mask layer formed on the protective layer can be made of a material different from that of the protective layer, selected from the materials listed above as materials that can be used for the protective layer. The mask layer is preferably made of a material for which a processing method exists that can obtain a selectivity with respect to the protective layer. Since the mask layer is formed on the protective layer, it has little effect on the organic semiconductor layer during film formation, allowing for a wide range of film formation methods. Among the above-mentioned materials, tungsten, molybdenum, IGZO, etc. are particularly preferred for the mask layer. These can be formed by sputtering.

[0076] The method for manufacturing an organic semiconductor device by photolithography using the structure layer, the protective layer, and the mask layer as described above can be a manufacturing method with a low frequency of defects and a high yield, and as a result, the organic semiconductor device manufactured using this manufacturing method can be an inexpensive organic semiconductor device.

[0077] The protective layer and the mask layer may each be formed as a single layer or as a multi-layer.

[0078] The structure of this embodiment mode can be used in appropriate combination with other structures.

[0079] Embodiment 2 In this embodiment, a method for processing an organic semiconductor layer according to one embodiment of the present invention will be described with reference to FIGS.

[0080] First, an organic semiconductor film 1151 is formed on an underlayer film 1150 (FIG. 3A). The underlayer film may be an insulating film or a conductive film depending on the device to be fabricated. The organic semiconductor film 1151 may be formed by a dry method such as vapor deposition, or by a wet method such as spin coating.

[0081] Next, a structure layer 1154 is formed on the organic semiconductor film 1151 using the material described in Embodiment Mode 1 (FIG. 3A). The structure layer 1154 is formed by a vacuum evaporation method, and a structure 1155 is formed by evaporation.

[0082] Next, a protective layer 1152 is formed on the structure layer 1154 (FIG. 3A). The protective layer 1152 can be formed using the material described in Embodiment 1. The protective layer 1152 is preferably a dense film with high barrier properties, and is preferably formed of aluminum oxide by an ALD method. Note that aluminum oxide formed by an ALD method is preferable because it causes less damage to the base, but on the other hand, it has poor adhesion to the organic semiconductor film 1151, so providing the structure layer 1154 is very effective. IGZO is also preferable for the protective layer 1152.

[0083] A mask layer 1153 is preferably formed on the protective layer 1152 ( FIG. 3B ). The presence of the structure layer 1154 and the protective layer 1152 makes it possible to suppress damage to the organic semiconductor film 1151 when forming the mask layer 1153. Therefore, it is easy to select a film formation method that causes relatively large damage to the surface on which the mask layer 1153 is formed, such as a sputtering method. Examples of materials that can be used to form the mask layer 1153 include silicon, silicon nitride, silicon oxide, tungsten, titanium, molybdenum, tantalum, tantalum nitride, alloys containing molybdenum and niobium, alloy metal oxides containing molybdenum and tungsten, and metal oxides such as indium gallium zinc oxide (In—Ga—Zn oxide, also referred to as IGZO). Furthermore, indium oxide, indium zinc oxide (In—Zn oxide), indium tin oxide (In—Sn oxide), indium titanium oxide (In—Ti oxide), indium tin zinc oxide (In—Sn—Zn oxide), indium titanium zinc oxide (In—Ti—Zn oxide), indium gallium tin zinc oxide (In—Ga—Sn—Zn oxide), etc. can also be used. Alternatively, indium tin oxide containing silicon can also be used.

[0084] Thereafter, a photosensitive resin is applied onto the mask layer 1153 to form a resin film 1175 (FIG. 3C). The photosensitive resin may be a positive resist or a negative resist.

[0085] Next, the resin is exposed to light in accordance with its photosensitivity and developed to form a photomask layer 1175a (FIG. 3D). The mask layer 1153 is etched using the photomask layer 1175a to form a mask layer 1153a (FIG. 3E). The mask layer 1153 may be etched by wet etching or dry etching. It is preferable to select conditions for the etching that result in a higher selectivity for the mask layer 1153 than for the protective layer 1152.

[0086] After the mask layer 1153a is formed, the photomask layer 1175a is removed (FIG. 4A). The presence of the mask layer 1153 and the protective layer 1152 prevents the organic semiconductor film 1151 from being adversely affected, such as being lost or damaged, during the processes of forming and removing the photomask layer 1175a, and therefore an organic semiconductor device with excellent characteristics can be fabricated.

[0087] Note that, at this time, depending on the chemical solution used to remove the photomask layer 1175a, the protective layer 1152 can be simultaneously etched. However, on the other hand, when the structure layer 1154 is not formed in this step, peeling is likely to occur between the protective layer 1152 and the organic semiconductor film 1151. In one embodiment of the present invention, by forming the structure layer 1154, peeling can be suppressed even when the photomask layer 1175a and the protective layer 1152 are simultaneously etched, and defects can be prevented.

[0088] Thereafter, etching is performed using the mask layer 1153a as a mask to form the organic semiconductor layer 1151a, the structural layer 1154a, and the protective layer 1152a (FIG. 4B). These etchings may be performed by wet etching or dry etching, but dry etching is preferred.

[0089] After processing of the organic semiconductor layer 1151a is completed, the mask layer 1153a is removed (FIG. 4C). The mask layer 1153a can be removed by etching, which may be wet etching or dry etching, but dry etching is preferred. The etching is preferably performed under conditions in which the mask layer 1153a has a higher selective ratio than the protective layer 1152a.

[0090] Finally, the protective layer 1152a and the structure layer 1154a are removed (FIG. 4D). The mask layer 1153a and the structure layer 1154a may be removed by etching, which may be wet etching or dry etching, but wet etching is preferred. The etching is preferably performed under conditions that provide a high selectivity between the protective layer 1152a and the structure layer 1154a and between the protective layer 1152a and the structure layer 1154a and the organic semiconductor layer 1151a.

[0091] The organic semiconductor layer 1151a processed by such a process can be easily processed into a desired shape by suppressing peeling of the protective layer 1152. As a result, organic semiconductor devices and organic semiconductor devices using the organic semiconductor layer 1151a processed by such a process can be manufactured with a high yield and at low cost.

[0092] The organic semiconductor layer 1151a can be used in an organic TFT having an organic semiconductor layer 1151a, a gate insulating layer 161, a gate electrode 162, and source and drain electrodes 163 and 164 provided on an insulating layer 160 as shown in Figure 5A; a photoelectric conversion device such as a solar cell or a photosensor having a first electrode 165 and a second electrode 169 and a photoelectric conversion layer 167 provided on an insulating layer 160 as shown in Figure 5B; and an organic EL device having a first electrode 165, a second electrode 169 and an emitting layer 168 provided on an insulating layer 160 as shown in Figure 5C.

[0093] The structure of this embodiment mode can be used in appropriate combination with other structures.

[0094] Embodiment 3 In this embodiment, a method for manufacturing an organic semiconductor device according to one embodiment of the present invention will be described, taking as an example a method for manufacturing a display device (a display device using an organic EL device).

[0095] As shown in FIGS. 6A and 6B, a plurality of light-emitting devices 130 are formed on an insulating layer 175 to form the display device 100.

[0096] The display device has a pixel portion 177 in which a plurality of pixels 178 are arranged in a matrix. The pixel 178 has a sub-pixel 110R, a sub-pixel 110G, and a sub-pixel 110B.

[0097] In this specification and the like, when describing matters common to, for example, the subpixels 110R, 110G, and 110B, they may be referred to as the subpixels 110. When describing matters common to other components distinguished by alphabets, they may also be described using symbols without the alphabets.

[0098] The subpixel 110R emits red light, the subpixel 110G emits green light, and the subpixel 110B emits blue light. This allows an image to be displayed in the pixel portion 177. In this embodiment, three subpixels of red (R), green (G), and blue (B) are described as an example. However, combinations of subpixels of other colors may also be used. The number of subpixels is not limited to three, and may be four or more. Examples of four subpixels include four subpixels of R, G, B, and white (W); four subpixels of R, G, B, and Y; and four subpixels of R, G, B, and infrared (IR). A sensor may also be provided within the pixel 178. In an organic photodiode sensor using an organic compound, a portion of the carrier transport layer can be formed using the same material as the light-emitting device.

[0099] In this specification, the row direction may be referred to as the X direction, and the column direction may be referred to as the Y direction. The X direction and the Y direction intersect, for example, perpendicularly.

[0100] 6A shows an example in which subpixels of different colors are arranged side by side in the X direction, and subpixels of the same color are arranged side by side in the Y direction. Note that subpixels of different colors may also be arranged side by side in the Y direction, and subpixels of the same color may also be arranged side by side in the X direction.

[0101] A connection portion 140 and a region 141 may be provided outside the pixel portion 177. The region 141 is provided between the pixel portion 177 and the connection portion 140. The organic compound layer 103 is provided in the region 141. In addition, the connection portion 140 is provided with a conductive layer 111C.

[0102] 6A shows an example in which the region 141 and the connection portion 140 are located on the right side of the pixel portion 177, but the positions of the region 141 and the connection portion 140 are not particularly limited. The region 141 and the connection portion 140 may be singular or plural.

[0103] Fig. 6B is an example of a cross-sectional view taken along dashed line A1-A2 in Fig. 6A. As shown in Fig. 6B, the display device has an insulating layer 171, a conductive layer 172 on the insulating layer 171, an insulating layer 173 on the insulating layer 171 and on the conductive layer 172, an insulating layer 174 on the insulating layer 173, and an insulating layer 175 on the insulating layer 174. The insulating layer 171 is provided on a substrate (not shown). The insulating layers 175, 174, and 173 have openings that reach the conductive layer 172, and plugs 176 are provided to fill the openings.

[0104] In the pixel section 177, the light-emitting device 130 is provided on the insulating layer 175 and the plug 176. A protective layer 131 is provided to cover the light-emitting device 130. The substrate 120 is bonded to the protective layer 131 by a resin layer 122. Preferably, an inorganic insulating layer 125 and an insulating layer 127 on the inorganic insulating layer 125 are provided between adjacent light-emitting devices 130.

[0105] 6B shows a plurality of cross sections of the inorganic insulating layer 125 and the insulating layer 127, it is preferable that the inorganic insulating layer 125 and the insulating layer 127 are connected to one another when the display device is viewed from above. In other words, it is preferable that the insulating layer 127 is an insulating layer having an opening over the first electrode.

[0106] 6B shows light-emitting device 130R, light-emitting device 130G, and light-emitting device 130B. Light-emitting device 130R, light-emitting device 130G, and light-emitting device 130B are light-emitting devices that emit light of different colors. For example, light-emitting device 130R can emit red light, light-emitting device 130G can emit green light, and light-emitting device 130B can emit blue light. Light-emitting device 130R, light-emitting device 130G, or light-emitting device 130B may also emit other visible light or infrared light.

[0107] The display device of one embodiment of the present invention can be, for example, a top-emission type in which light is emitted in a direction opposite to a substrate on which a light-emitting device is formed. Note that the display device of one embodiment of the present invention may also be a bottom-emission type.

[0108] The light-emitting device 130R has the structure described in Embodiment 2. It includes a first electrode 101R (pixel electrode) composed of a conductive layer 151R and a conductive layer 152R, a first EL layer 104R on the first electrode 101R, an organic compound layer (a second EL layer 105 on the first EL layer 104R), and a second electrode 102 (common electrode) on the second EL layer 105. The second EL layer 105 is preferably located closer to the second electrode 102 (common electrode) than the light-emitting layer, and is preferably a hole-blocking layer, an electron-transporting layer, an electron-injecting layer, or a laminate of these. This structure can reduce damage to the light-emitting layer or active layer during photolithography, and is expected to provide excellent film quality and electrical characteristics. Furthermore, the common layer in contact with the second electrode 102 (common electrode) may include several layers, such as an electron-injecting layer.

[0109] The light-emitting device 130G has the structure described in Embodiment 2. It includes a first electrode 101G (pixel electrode) including a conductive layer 151G and a conductive layer 152G, a first EL layer 104G on the first electrode 101G, a second EL layer 105 on the first EL layer 104G, and a second electrode 102 (common electrode) on the second EL layer 105. The second EL layer 105 is preferably a hole-blocking layer, an electron-transporting layer, an electron-injecting layer, or a stack of these layers.

[0110] The light-emitting device 130B has the structure described in Embodiment 2. It includes a first electrode 101B (pixel electrode) including a conductive layer 151B and a conductive layer 152B, a first EL layer 104B on the first electrode 101B, a second EL layer 105 on the first EL layer 104B, and a second electrode 102 (common electrode) on the second EL layer 105. The second EL layer 105 is preferably a hole-blocking layer, an electron-transporting layer, an electron-injecting layer, or a stack of these layers.

[0111] One of a pixel electrode (first electrode) and a common electrode (second electrode) of a light-emitting device functions as an anode, and the other functions as a cathode. In this embodiment, unless otherwise specified, the pixel electrode functions as an anode and the common electrode functions as a cathode.

[0112] The first EL layer 104R, the first EL layer 104G, and the first EL layer 104B are independent and island-like, respectively, or for each emitted color. It is preferable that the first EL layer 104R, the first EL layer 104G, and the first EL layer 104B do not overlap with each other. By providing the first EL layer 104 in an island-like form for each light-emitting device 130, leakage current between adjacent light-emitting devices 130 can be suppressed even in a high-resolution display device. This prevents crosstalk and realizes a display device with extremely high contrast. In particular, a display device with high current efficiency at low luminance can be realized.

[0113] The island-shaped first EL layer 104 is formed by depositing an EL film and processing the EL film by photolithography.

[0114] The first EL layer 104 is preferably provided on the upper surface of the first electrode 101 (pixel electrode) of the light-emitting device 130. This makes it easy to suppress the occurrence of leakage current and provide a light-emitting device with good color purity. Furthermore, covering the side surface of the pixel electrode of the light-emitting device 130 with the first EL layer 104 prevents the pixel electrode from contacting the second electrode 102, thereby preventing short circuits in the light-emitting device 130.

[0115] In the display device of one embodiment of the present invention, the first electrode 101 (pixel electrode) of the light-emitting device preferably has a stacked-layer structure. For example, in the example shown in FIG. 6B , the first electrode 101 of the light-emitting device 130 has a stacked-layer structure of a conductive layer 151 provided on the insulating layer 171 side and a conductive layer 152 provided on the organic compound layer side.

[0116] For example, a metal material can be used as the conductive layer 151. Specifically, metals such as aluminum (Al), titanium (Ti), chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), gallium (Ga), zinc (Zn), indium (In), tin (Sn), molybdenum (Mo), tantalum (Ta), tungsten (W), palladium (Pd), gold (Au), platinum (Pt), silver (Ag), yttrium (Y), and neodymium (Nd), as well as alloys containing appropriate combinations of these metals, can also be used.

[0117] An oxide containing one or more selected from indium, tin, zinc, gallium, titanium, aluminum, and silicon can be used for the conductive layer 152. For example, it is preferable to use a conductive oxide containing one or more of indium oxide, indium tin oxide, indium zinc oxide, zinc oxide, zinc oxide containing gallium, titanium oxide, indium zinc oxide containing gallium, indium zinc oxide containing aluminum, indium tin oxide containing silicon, and indium zinc oxide containing silicon. In particular, indium tin oxide containing silicon has a large work function, for example, a work function of 4.0 eV or more, and therefore can be suitably used for the conductive layer 152.

[0118] The conductive layer 151 may have a stacked structure of multiple layers containing different materials, and the conductive layer 152 may have a stacked structure of multiple layers containing different materials. In this case, the conductive layer 151 may include a layer containing a material that can be used for the conductive layer 152, such as a conductive oxide, or the conductive layer 152 may include a layer containing a material that can be used for the conductive layer 151, such as a metal material. For example, when the conductive layer 151 has a stacked structure of two or more layers, a layer in contact with the conductive layer 152 can be a layer containing a material that can be used for the conductive layer 152.

[0119] Note that the end portion of the conductive layer 151 may have a tapered shape. Specifically, the end portion of the conductive layer 151 preferably has a tapered shape with a taper angle of less than 90°. In this case, the conductive layer 152 provided along the side surface of the conductive layer 151 also has a tapered shape. By tapering the side surface of the conductive layer 152, coverage of the first EL layer 104 provided along the side surface of the conductive layer 152 can be improved. Note that the end portion of the conductive layer 151 may not have a tapered shape and may be approximately perpendicular to the substrate surface. In this case, the distance between adjacent EL layers can be narrowed, and therefore a light-emitting device with a high aperture ratio can be provided.

[0120] The light-emitting device of one embodiment of the present invention can be a highly reliable light-emitting device because the light-emitting device 130 has the structure described in Embodiment 2. Furthermore, the light-emitting device of one embodiment of the present invention includes the steps described in Embodiment 1 in its manufacturing process, and therefore, the occurrence of defects is suppressed, the light-emitting device can be manufactured with a high yield, and the light-emitting device can be manufactured at a relatively low cost.

[0121] Next, an example of a method for manufacturing a display device having the structure shown in FIG. 6A will be described with reference to FIGS.

[0122] [Example of Manufacturing Method] Thin films (insulating films, semiconductor films, conductive films, etc.) constituting the display device can be formed using a sputtering method, a chemical vapor deposition (CVD) method, a vacuum evaporation method, a pulsed laser deposition (PLD) method, an ALD method, or the like.

[0123] Furthermore, thin films (insulating films, semiconductor films, conductive films, etc.) constituting the display device can be formed by wet film formation methods such as spin coating, dipping, spray coating, inkjet, dispensing, screen printing, offset printing, doctor knife method, slit coating, roll coating, curtain coating, or knife coating.

[0124] Furthermore, when processing the thin films that constitute the display device, they can be processed using, for example, photolithography.

[0125] In photolithography, the light used for exposure may be, for example, i-line (wavelength 365 nm), g-line (wavelength 436 nm), h-line (wavelength 405 nm), or a mixture of these. Other light sources that can be used include ultraviolet light, KrF laser light, and ArF laser light. Exposure may also be performed by immersion exposure technology. Extreme ultraviolet (EUV) light or X-rays may also be used as the light used for exposure. An electron beam may also be used instead of the light used for exposure.

[0126] The thin film can be etched by dry etching, wet etching, sandblasting, or the like.

[0127] 7A , an insulating layer 171 is formed on a substrate (not shown). Subsequently, conductive layers 172 and 179 are formed on the insulating layer 171, and an insulating layer 173 is formed on the insulating layer 171 so as to cover the conductive layers 172 and 179. Subsequently, an insulating layer 174 is formed on the insulating layer 173, and an insulating layer 175 is formed on the insulating layer 174.

[0128] The substrate may be a substrate having heat resistance sufficient to withstand at least a subsequent heat treatment, such as a glass substrate, a quartz substrate, a sapphire substrate, a ceramic substrate, an organic resin substrate, a single crystal semiconductor substrate made of silicon, silicon carbide, or the like, a polycrystalline semiconductor substrate, a compound semiconductor substrate made of silicon germanium, or the like, or an SOI substrate.

[0129] 7A, openings are formed in the insulating layers 175, 174, and 173, reaching the conductive layer 172. Then, plugs 176 are formed to fill the openings.

[0130] 7A , a conductive film 151f, which will later become the conductive layers 151R, 151G, 151B, and 151C, is formed on the plugs 176 and the insulating layer 175. The conductive film 151f can be made of, for example, a metal material.

[0131] 7A, a resist mask 191 is formed over the conductive film 151f. The resist mask 191 can be formed by applying a photosensitive material (photoresist) and then performing exposure and development.

[0132] 7B, the conductive film 151f is removed from the region that does not overlap with the resist mask 191. In this way, the conductive layer 151 is formed.

[0133] 7C, the resist mask 191 is removed by, for example, ashing using oxygen plasma.

[0134] Next, as shown in FIG. 7D , an insulating film 156f, which will later become insulating layers 156R, 156G, 156B, and 156C, is formed on the conductive layer 151R, the conductive layer 151G, the conductive layer 151B, the conductive layer 151C, and the insulating layer 175.

[0135] The insulating film 156f can be an inorganic insulating film such as an insulating oxide film, an insulating nitride film, an insulating oxynitride film, or an insulating nitride oxide film, for example, a silicon oxynitride film.

[0136] Subsequently, as shown in FIG. 7E, the insulating film 156f is processed to form insulating layers 156R, 156G, 156B, and 156C.

[0137] Subsequently, as shown in FIG. 8A, a conductive film 152f is formed on the conductive layer 151R, the conductive layer 151G, the conductive layer 151B, the conductive layer 151C, the insulating layer 156R, the insulating layer 156G, the insulating layer 156B, the insulating layer 156C, and the insulating layer 175.

[0138] The conductive film 152f can be formed using, for example, a conductive oxide. The conductive film 152f may also be a stacked film.

[0139] Subsequently, as shown in FIG. 8B, the conductive film 152f is processed to form conductive layers 152R, 152G, 152B, and 152C.

[0140] 8C, the organic compound film 103Rf is formed on the conductive layer 152R, the conductive layer 152G, the conductive layer 152B, and the insulating layer 175. Note that, as shown in FIG. 8C, the organic compound film 103Rf is not formed on the conductive layer 152C.

[0141] Subsequently, as shown in FIG. 8C, a structural layer 153Rf, a protective film 158Rf, and a mask film 159Rf are formed.

[0142] By providing the protective film 158Rf on the organic compound film 103Rf, damage to the organic compound film 103Rf during the manufacturing process of the display device can be reduced, and the reliability of the light-emitting device can be improved. Furthermore, by forming the structural layer 153Rf, it is possible to prevent the protective film 158Rf from peeling off from the organic compound film 103Rf or the organic compound layer 103R during the manufacturing process.

[0143] The protective film 158Rf is made of a film that is highly resistant to the processing conditions of the organic compound film 103Rf, specifically, a film that has a large etching selectivity with respect to the organic compound film 103Rf.The mask film 159Rf is made of a film that has a large etching selectivity with respect to the protective film 158Rf.

[0144] Furthermore, the structural layer 153Rf, the protective film 158Rf, and the mask film 159Rf are formed at a temperature lower than the heat resistance temperature of the organic compound film 103Rf. The substrate temperature when forming the protective film 158Rf and the mask film 159Rf is typically 100° C. or higher and 200° C. or lower, preferably 100° C. or higher and 150° C. or lower, and more preferably 100° C. or higher and 120° C. or lower. Since the structural layer 153Rf is an organic compound or an organometallic complex as described in the first embodiment, it can be formed under the same conditions as those for an organic compound film.

[0145] It is preferable to use films that can be removed by wet etching or dry etching for the structural layer 153Rf, the protective film 158Rf, and the mask film 159Rf.

[0146] The protective film 158Rf formed in a position close to the organic compound film 103Rf is preferably formed using a formation method that causes less damage to the organic compound film 103Rf than the mask film 159Rf. For example, the ALD method (Atomic Layer Deposition method) or the vacuum evaporation method is more preferable than the sputtering method.

[0147] The protective film 158Rf and the mask film 159Rf may each be made of one or more of a metal film, an alloy film, a metal oxide film, a semiconductor film, an organic insulating film, an inorganic insulating film, or the like.

[0148] The protective film 158Rf and the mask film 159Rf can each be made of a metal material such as gold, silver, platinum, magnesium, nickel, tungsten, chromium, molybdenum, iron, cobalt, copper, palladium, titanium, aluminum, yttrium, zirconium, or tantalum, or an alloy material containing such a metal material. It is particularly preferable to use a low-melting-point material such as aluminum or silver. Using a metal material capable of blocking ultraviolet rays for one or both of the protective film 158Rf and the mask film 159Rf is preferable because it can prevent the organic compound film 103Rf from being irradiated with ultraviolet rays during pattern exposure, thereby suppressing deterioration of the organic compound film 103Rf.

[0149] Furthermore, the protective film 158Rf and the mask film 159Rf may each be made of a metal oxide such as In—Ga—Zn oxide, indium oxide, In—Zn oxide, In—Sn oxide, indium titanium oxide (In—Ti oxide), indium tin zinc oxide (In—Sn—Zn oxide), indium titanium zinc oxide (In—Ti—Zn oxide), indium gallium tin zinc oxide (In—Ga—Sn—Zn oxide), or indium tin oxide containing silicon.

[0150] In addition, in the above metal oxide, an element M (wherein M is one or more elements selected from aluminum, silicon, boron, yttrium, copper, vanadium, beryllium, titanium, iron, nickel, germanium, zirconium, molybdenum, lanthanum, cerium, neodymium, hafnium, tantalum, tungsten, and magnesium) may be used instead of gallium.

[0151] The protective film 158Rf and the mask film 159Rf are preferably made of a semiconductor material such as silicon or germanium, which has a high affinity with the semiconductor manufacturing process. Alternatively, compounds containing the semiconductor materials may be used.

[0152] Furthermore, various inorganic insulating films can be used for the protective film 158Rf and the mask film 159Rf. In particular, oxide insulating films are preferable because they have higher adhesion to the organic compound film 103Rf than nitride insulating films. Nitride insulating films are preferable because they are dense and have high barrier properties. Silicon nitride films are particularly preferable as nitride insulating films.

[0153] 8C, a resist mask 190R is formed by applying a photosensitive material (photoresist) and then exposing and developing it.

[0154] The resist mask 190R is provided in a position overlapping with the conductive layer 152R. The resist mask 190R is preferably provided also in a position overlapping with the conductive layer 152C. This can prevent the conductive layer 152C from being damaged during the manufacturing process of the display device.

[0155] 8D , a resist mask 190R is used to remove part of the mask film 159Rf to form a mask layer 159R. The mask layer 159R remains on the conductive layer 152R and the conductive layer 152C. The resist mask 190R is then removed. The mask layer 159R is then used as a mask (also referred to as a hard mask) to remove part of the protective film 158Rf to form a protective layer 158R.

[0156] By using the wet etching method, damage to the organic compound film 103Rf during processing of the protective film 158Rf and the mask film 159Rf can be reduced compared to when using the dry etching method. When using the wet etching method, it is preferable to use an acid aqueous solution such as a developing solution, an alkaline aqueous solution such as a tetramethylammonium hydroxide (TMAH) aqueous solution, or a chemical solution using dilute hydrofluoric acid, oxalic acid, phosphoric acid, acetic acid, nitric acid, or a mixture of these.

[0157] Furthermore, when dry etching is used to process the protective film 158Rf, deterioration of the organic compound film 103Rf can be suppressed by not using a gas containing oxygen as the etching gas.

[0158] The resist mask 190R can be removed in the same manner as the resist mask 191.

[0159] 8D , the structural layer 153Rf and the organic compound film 103Rf are processed to form the structural layer 153R and the organic compound layer 103R. For example, the structural layer 153Rf and the organic compound film 103Rf are partially removed using the mask layer 159R and the protective layer 158R as hard masks to form the structural layer 153R and the organic compound layer 103R.

[0160] 8D, a laminated structure of the organic compound layer 103R, the structural layer 153R, the protective layer 158R, and the mask layer 159R remains on the conductive layer 152R. Also, the conductive layers 152G and 152B are exposed.

[0161] The organic compound film 103Rf is preferably processed by anisotropic etching, particularly anisotropic dry etching, or wet etching may be used.

[0162] When dry etching is used, deterioration of the organic compound film 103Rf can be suppressed by not using a gas containing oxygen as the etching gas.

[0163] Alternatively, a gas containing oxygen may be used as the etching gas. By using an etching gas containing oxygen, the etching rate can be increased. Therefore, etching can be performed under low power conditions while maintaining a sufficiently high etching rate. This makes it possible to suppress damage to the organic compound film 103Rf. Furthermore, problems such as adhesion of reaction products generated during etching can be suppressed.

[0164] When dry etching is used, for example, H 2 , C.F. 4 , C 4 F 8 , SF 6 , CHF 3 , Cl 2 , H 2 O, BCl 3 It is preferable to use a gas containing one or more of Group 18 elements such as He and Ar as the etching gas. Alternatively, it is preferable to use a gas containing one or more of these elements and oxygen as the etching gas. Alternatively, oxygen gas may be used as the etching gas.

[0165] Subsequently, as shown in FIG. 9A, an organic compound film 103Gf, which will later become the organic compound layer 103G, is formed.

[0166] The organic compound film 103Gf can be formed by the same method as that used to form the organic compound film 103Rf.

[0167] 9A , a structural layer 153Gf, a protective film 158Gf, and a mask film 159Gf are formed in this order. Then, a resist mask 190G is formed. The materials and formation methods of the structural layer 153Gf, the protective film 158Gf, and the mask film 159Gf are the same as those applicable to the structural layer 153Rf, the protective film 158Rf, and the mask film 159Rf. The materials and formation method of the resist mask 190G are the same as those applicable to the resist mask 190R.

[0168] The resist mask 190G is preferably provided in a position overlapping with the conductive layer 152G.

[0169] Next, as shown in FIG. 9B , a resist mask 190G is used to remove a portion of the mask film 159Gf to form a mask layer 159G. The mask layer 159G remains on the conductive layer 152G. The resist mask 190G is then removed. Next, using the mask layer 159G as a mask, a portion of the protective film 158Gf is removed to form a protective layer 158G. Next, the structure layer 153Gf and the organic compound film 103Gf are processed to form a structure layer 153G and an organic compound layer 103G. As a result, as shown in FIG. 9B , a stacked structure of the organic compound layer 103G, the structure layer 153G, the protective layer 158G, and the mask layer 159G remains on the conductive layer 152G. Furthermore, the mask layer 159R and the conductive layer 152B are exposed.

[0170] Subsequently, as shown in FIG. 9C, an organic compound film 103Bf is formed.

[0171] The organic compound film 103Bf can be formed by the same method as that used to form the organic compound film 103Rf.

[0172] 9C , a structural layer 153Bf, a protective film 158Bf, and a mask film 159Bf are formed in this order. Then, a resist mask 190B is formed. The materials and formation methods of the structural layer 153Bf, the protective film 158Bf, and the mask film 159Bf are the same as those applicable to the structural layer 153Rf, the protective film 158Rf, and the mask film 159Rf. The materials and formation method of the resist mask 190B are the same as those applicable to the resist mask 190R.

[0173] The resist mask 190B is provided in a position overlapping with the conductive layer 152B.

[0174] 9D , a resist mask 190B is used to remove a portion of the mask film 159Bf to form a mask layer 159B. The mask layer 159B preferably remains on the conductive layer 152B. The resist mask 190B is then removed. The mask layer 159B is then used as a mask to remove a portion of the protective film 158Bf to form a protective layer 158B. The structure layer 153Bf and the organic compound film 103Bf are then processed to form the organic compound layer 103B. For example, the mask layer 159B and the protective layer 158B are used as hard masks to remove a portion of the structure layer 153Bf and the organic compound film 103Bf to form the structure layer 153B and the organic compound layer 103B.

[0175] 9D, a laminated structure of the organic compound layer 103B, the structural layer 153B, the protective layer 158B, and the mask layer 159B remains on the conductive layer 152B. Also, the mask layers 159R and 159G are exposed.

[0176] It is preferable that the side surfaces of the organic compound layers 103R, 103G, and 103B are perpendicular or substantially perpendicular to the surface on which they are formed. For example, it is preferable that the angle formed between the surface on which they are formed and these side surfaces be 60 degrees or more and 90 degrees or less.

[0177] As described above, the distance between adjacent pairs of the organic compound layers 103R, 103G, and 103B formed using photolithography can be narrowed to 8 μm or less, 5 μm or less, 3 μm or less, 2 μm or less, or 1 μm or less. Here, the distance can be defined, for example, as the distance between the opposing ends of adjacent pairs of the organic compound layers 103R, 103G, and 103B. By narrowing the distance between the island-shaped organic compound layers in this manner, a display device with high definition and a large aperture ratio can be provided. Furthermore, the distance between the first electrodes of adjacent light-emitting devices can also be narrowed, for example, to 10 μm or less, 8 μm or less, 5 μm or less, 3 μm or less, or 2 μm or less. Note that the distance between the first electrodes of adjacent light-emitting devices is preferably 2 μm or more and 5 μm or less.

[0178] Subsequently, as shown in FIG. 10A, it is preferable to remove the mask layers 159R, 159G, and 159B.

[0179] The mask layer removal process can be performed using the same method as the mask film processing process. In particular, by using a wet etching method, damage to the organic compound layer 103 during the mask layer removal can be reduced compared to when a dry etching method is used.

[0180] The mask layer may also be removed by dissolving it in a polar solvent such as water or alcohol, such as ethyl alcohol, methyl alcohol, isopropyl alcohol (IPA), or glycerin.

[0181] After removing the mask layer, a drying treatment may be performed to remove water adsorbed on the surface. For example, a heat treatment can be performed in an inert gas atmosphere or a reduced pressure atmosphere. The heat treatment can be performed at a substrate temperature of 50°C or higher and 200°C or lower, preferably 60°C or higher and 150°C or lower, and more preferably 70°C or higher and 120°C or lower. A reduced pressure atmosphere is preferred because it allows drying at a lower temperature.

[0182] Subsequently, as shown in FIG. 10B, an inorganic insulating film 125f is formed.

[0183] Subsequently, as shown in FIG. 10C, an insulating film 127f, which will later become the insulating layer 127, is formed on the inorganic insulating film 125f.

[0184] The substrate temperature when forming the inorganic insulating film 125f and the insulating film 127f is preferably 60°C or higher, 80°C or higher, 100°C or higher, or 120°C or higher, and 200°C or lower, 180°C or lower, 160°C or lower, 150°C or lower, or 140°C or lower, respectively.

[0185] As the inorganic insulating film 125f, it is preferable to form an insulating film having a thickness of 3 nm or more, 5 nm or more, or 10 nm or more, and 200 nm or less, 150 nm or less, 100 nm or less, or 50 nm or less within the above substrate temperature range.

[0186] The inorganic insulating film 125f is preferably formed by, for example, the ALD method. The ALD method is preferable because it can reduce film formation damage and form a film with high coverage. The inorganic insulating film 125f is preferably formed as an aluminum oxide film by, for example, the ALD method.

[0187] The insulating film 127f is preferably formed by the wet film formation method described above. The insulating film 127f is preferably formed by, for example, spin coating using a photosensitive material, more specifically, using a photosensitive resin composition containing an acrylic resin.

[0188] Subsequently, exposure is performed to expose a portion of the insulating film 127f to visible light or ultraviolet light. The insulating layer 127f is formed in a region sandwiched between any two of the conductive layers 152R, 152G, and 152B, and around the conductive layer 152C.

[0189] The width of the insulating layer 127 to be formed later can be controlled by the exposed region of the insulating film 127f. In this embodiment mode, the insulating layer 127 is processed to have a portion overlapping with the top surface of the conductive layer 151.

[0190] The light used for exposure preferably contains i-line (wavelength 365 nm), and may contain at least one of g-line (wavelength 436 nm) and h-line (wavelength 405 nm).

[0191] Subsequently, as shown in FIG. 11A, development is performed to remove the exposed area of ​​the insulating film 127f, thereby forming an insulating layer 127a.

[0192] 11B, an etching process is performed using the insulating layer 127a as a mask to remove a portion of the inorganic insulating film 125f and reduce the thickness of portions of the protective layer 158R, the protective layer 158G, and the protective layer 158B. As a result, the inorganic insulating layer 125 is formed below the insulating layer 127a. Furthermore, the surfaces of the thin portions of the protective layer 158R, the protective layer 158G, and the protective layer 158B are exposed. Note that, hereinafter, the etching process using the insulating layer 127a as a mask may be referred to as the first etching process.

[0193] The first etching treatment can be performed by dry etching or wet etching. Note that it is preferable to form the inorganic insulating film 125f using the same material as the protective layers 158R, 158G, and 158B because the first etching treatment can be performed all at once.

[0194] When dry etching is performed, it is preferable to use a chlorine-based gas. 2 , BCl 3 , SiCl 4 , and CCl 4 The above-mentioned chlorine-based gas may be appropriately added with oxygen gas, hydrogen gas, helium gas, argon gas, or the like, either alone or in combination of two or more gases. By using dry etching, thin regions of the protective layer 158R, the protective layer 158G, and the protective layer 158B can be formed with good in-plane uniformity.

[0195] The dry etching apparatus may be a dry etching apparatus having a high-density plasma source, such as an inductively coupled plasma (ICP) etching apparatus, or a capacitively coupled plasma (CCP) etching apparatus having parallel plate electrodes.

[0196] Furthermore, it is preferable to perform the first etching process by wet etching. Using the wet etching method can reduce damage to the organic compound layer 103R, the organic compound layer 103G, and the organic compound layer 103B compared to using the dry etching method. For example, the wet etching can be performed using an alkaline solution. For example, TMAH, which is an alkaline solution, can be used for wet etching of an aluminum oxide film. Alternatively, an acid solution containing fluoride can also be used. In this case, the wet etching can be performed by the paddle method. Note that if the inorganic insulating film 125f is formed using the same material as the protective layer 158R, the protective layer 158G, and the protective layer 158B, the above-mentioned etching process can be performed simultaneously, which is preferable.

[0197] In the first etching process, the protective layer 158R, the protective layer 158G, and the protective layer 158B are not completely removed, and the etching process is stopped when the film thicknesses of the protective layers 158R, 158G, and 158B are reduced. In this manner, by leaving the protective layers 158R, 158G, and 158B on the organic compound layers 103R, 103G, and 103B, respectively, it is possible to prevent the organic compound layers 103R, 103G, and 103B from being damaged in subsequent processes.

[0198] Note that after the first etching treatment, peeling is likely to occur between the organic compound layer 103 and the protective layer 158. However, in the method for manufacturing an organic semiconductor device of one embodiment of the present invention, the occurrence of peeling can be suppressed by providing the structure layer 153 between the protective layer 158 and the organic compound layer 103. As a result, organic semiconductor devices (display devices, respectively) can be manufactured with high yield, and inexpensive organic semiconductor devices can be easily provided.

[0199] Subsequently, the entire substrate is exposed to visible light or ultraviolet light, and the insulating layer 127a is preferably irradiated with the energy density of the exposure. 2 Larger than 800 mJ / cm 2 It is preferable that the dose is 0 mJ / cm or less. 2 Greater than 500 mJ / cm 2 It is more preferable to perform the following. By performing such exposure after development, the transparency of the insulating layer 127a can be improved in some cases. Furthermore, the substrate temperature required for heat treatment to transform the insulating layer 127a into a tapered shape in a later step can be reduced in some cases.

[0200] Here, the presence of a barrier insulating layer against oxygen (e.g., an aluminum oxide film, etc.) as the protective layer 158R, the protective layer 158G, and the protective layer 158B can reduce the diffusion of oxygen into the organic compound layer 103R, the organic compound layer 103G, and the organic compound layer 103B.

[0201] Next, heat treatment (also referred to as post-baking) is performed. By performing the heat treatment, the insulating layer 127a can be transformed into an insulating layer 127 having tapered side surfaces ( FIG. 11C ). The heat treatment is performed at a temperature lower than the upper temperature limit of the organic compound layer. The heat treatment can be performed at a substrate temperature of 50° C. to 200° C., preferably 60° C. to 150° C., more preferably 70° C. to 130° C. The heating atmosphere may be an air atmosphere or an inert gas atmosphere. The heating atmosphere may be an atmospheric pressure atmosphere or a reduced-pressure atmosphere. This can improve the adhesion between the insulating layer 127 and the inorganic insulating layer 125 and also improve the corrosion resistance of the insulating layer 127.

[0202] By leaving the protective layers 158R, 158G, and 158B in a thinner state without completely removing them in the first etching treatment, the organic compound layers 103R, 103G, and 103B can be prevented from being damaged and deteriorated in the heat treatment, thereby improving the reliability of the light-emitting device.

[0203] 11A , an etching process is performed using the insulating layer 127 as a mask to remove portions of the structure layer 153R, the protective layer 158R, the structure layer 153G, the protective layer 158G, the structure layer 153B, and the protective layer 158B. As a result, openings are formed in each of the structure layer 153R, the protective layer 158R, the structure layer 153G, the protective layer 158G, the structure layer 153B, and the protective layer 158B, exposing the top surfaces of the organic compound layer 103R, the organic compound layer 103G, the organic compound layer 103B, and the conductive layer 152C. Note that, hereinafter, this etching process may be referred to as a second etching process.

[0204] The end of inorganic insulating layer 125 is covered with insulating layer 127. Also, Fig. 12A shows an example in which part of the end of protective layer 158G (specifically, the tapered portion formed by the first etching process) is covered with insulating layer 127, and the tapered portion formed by the second etching process is exposed.

[0205] The second etching process is performed by wet etching. By using wet etching, damage to the organic compound layer 103R, the organic compound layer 103G, and the organic compound layer 103B can be reduced compared to when dry etching is used. Wet etching can be performed using, for example, an alkaline solution or an acidic solution. An aqueous solution is preferably used so that the organic compound layer 103 does not dissolve.

[0206] 12B , a common electrode 155 is formed on the organic compound layer 103R, the organic compound layer 103G, the organic compound layer 103B, the conductive layer 152C, and the insulating layer 127. The common electrode 155 can be formed by a method such as sputtering or vacuum evaporation. At this time, as shown in FIG. 6B , the organic compound layer 103 may be formed as a stacked structure of the first EL layer 104 and the second EL layer 105, and the common electrode 155 may be formed thereon.

[0207] 12C, a protective layer 131 is formed on the common electrode 155. The protective layer 131 can be formed by a method such as a vacuum deposition method, a sputtering method, a CVD method, or an ALD method.

[0208] Subsequently, the substrate 120 is attached over the protective layer 131 using the resin layer 122, whereby a display device can be manufactured. As described above, in the method for manufacturing a display device of one embodiment of the present invention, the insulating layer 156 is provided so as to have a region overlapping with a side surface of the conductive layer 151, and the conductive layer 152 is formed so as to cover the conductive layer 151 and the insulating layer 156. This can increase the yield of the display device and suppress the occurrence of defects.

[0209] As described above, in the manufacturing method of a display device according to one embodiment of the present invention, the island-shaped organic compound layers 103R, 103G, and 103B are formed by forming films over the entire surface and then processing them, rather than by using a fine metal mask. This allows the island-shaped layers to be formed with uniform thicknesses. This allows a high-resolution display device or a display device with a high aperture ratio to be realized. Furthermore, even when the resolution or aperture ratio is high and the distance between subpixels is extremely short, the organic compound layers 103R, 103G, and 103B can be prevented from contacting each other in adjacent subpixels. Therefore, leakage current between subpixels can be suppressed. This prevents crosstalk and realizes a display device with extremely high contrast. Furthermore, even in a display device including tandem light-emitting devices manufactured by photolithography, a display device with excellent characteristics can be provided.

[0210] The structure of this embodiment mode can be used in appropriate combination with other structures.

[0211] In this embodiment, the configuration of an organic EL device, which is an organic semiconductor device having an EL layer as an organic semiconductor layer, will be described with reference to Fig. 13. The organic EL device is an organic semiconductor device including a configuration including an EL layer having a light-emitting layer between a first electrode 101 and a second electrode 102.

[0212] One of the first electrode 101 and the second electrode 102 functions as an anode, and the other functions as a cathode. Fig. 13 illustrates an example in which the first electrode 101 is the anode.

[0213] The anode is preferably formed using a metal, alloy, conductive compound, or mixture thereof having a large work function (specifically, 4.0 eV or more). Specific examples include indium oxide-tin oxide (ITO), indium oxide-tin oxide containing silicon or silicon oxide (ITSO), indium oxide-zinc oxide, and indium oxide containing tungsten oxide and zinc oxide (IWZO). These conductive metal oxide films are usually formed by sputtering, but may also be formed by applying a sol-gel method. As an example of a fabrication method, indium oxide-zinc oxide can be formed by sputtering using a target in which 1 to 20 wt % of zinc oxide is added to indium oxide. Indium oxide containing tungsten oxide and zinc oxide (IWZO) can also be formed by sputtering using a target containing 0.5 to 5 wt % tungsten oxide and 0.1 to 1 wt % zinc oxide relative to indium oxide. Other materials that can be used for the anode include, for example, gold (Au), platinum (Pt), nickel (Ni), tungsten (W), chromium (Cr), molybdenum (Mo), iron (Fe), cobalt (Co), copper (Cu), palladium (Pd), titanium (Ti), aluminum (Al), or nitrides of metal materials (e.g., titanium nitride). A layer formed by stacking these materials can also be used as the anode. For example, a film formed by stacking Al, Ti, and ITSO on Ti in this order is preferred because it has good reflectivity, is highly efficient, and enables high resolution of several thousand ppi. Graphene can also be used as the anode material. In addition, by using a composite material capable of forming the hole injection layer 111 described later as a layer in contact with the anode (typically, a hole injection layer), it becomes possible to select an electrode material regardless of the work function.

[0214] The hole injection layer 111 is provided in contact with the anode and has a function of facilitating injection of holes into the organic compound layer 103. The hole injection layer 111 is made of phthalocyanine (abbreviation: H 2The organic EL element can be formed from a phthalocyanine compound or complex compound such as copper phthalocyanine (abbreviated as CuPc), 4,4'-bis[N-(4-diphenylaminophenyl)-N-phenylamino]biphenyl (abbreviated as DPAB) or 4,4'-bis(N-{4-[N'-(3-methylphenyl)-N'-phenylamino]phenyl}-N-phenylamino)biphenyl (abbreviated as DNTPD), or a polymer such as poly(3,4-ethylenedioxythiophene) / (polystyrenesulfonic acid) (abbreviated as PEDOT / PSS).

[0215] The hole injection layer 111 may be formed using a substance having electron acceptor properties. Examples of the substance having electron acceptor properties include organic compounds having an electron-withdrawing group (such as a halogen group or a cyano group), such as 7,7,8,8-tetracyano-2,3,5,6-tetrafluoroquinodimethane (abbreviation: F4-TCNQ), chloranil, 2,3,6,7,10,11-hexacyano-1,4,5,8,9,12-hexaazatriphenylene (abbreviation: HAT-CN), 1,3,4,5,7,8-hexafluorotetracyano-naphthoquinodimethane (abbreviation: F6-TCCNNQ), and 2-(7-dicyanomethylene-1,3,4,5,6,8,9,10-octafluoro-7H-pyren-2-ylidene)malononitrile. In particular, compounds in which an electron-withdrawing group is bonded to a fused aromatic ring having a plurality of heteroatoms, such as HAT-CN, are thermally stable and preferred. Also, [3]radialene derivatives having an electron-withdrawing group (especially a halogen group such as a fluoro group, a cyano group, etc.) are preferred because they have very high electron-accepting properties, and specific examples thereof include α,α',α''-1,2,3-cyclopropane triylidene tris[4-cyano-2,3,5,6-tetrafluorobenzeneacetonitrile], α,α',α''-1,2,3-cyclopropane triylidene tris[2,6-dichloro-3,5-difluoro-4-(trifluoromethyl)benzeneacetonitrile], and α,α',α''-1,2,3-cyclopropane triylidene tris[2,3,4,5,6-pentafluorobenzeneacetonitrile]. In addition to the organic compounds described above, transition metal oxides such as molybdenum oxide, vanadium oxide, ruthenium oxide, tungsten oxide, and manganese oxide can also be used as electron acceptor materials.

[0216] The hole-injection layer 111 is preferably formed using a composite material containing the above-mentioned material having an electron acceptor property and an organic compound having a hole-transport property.

[0217] As the organic compound having a hole transport property used in the composite material, various organic compounds can be used, such as aromatic amine compounds, heteroaromatic compounds, aromatic hydrocarbons, and polymer compounds (oligomers, dendrimers, polymers, etc.). 6 cm 2 / Vs or more. The organic compound having hole transport properties used in the composite material is preferably a compound having a fused aromatic hydrocarbon ring or a π-electron-rich heteroaromatic ring. As the fused aromatic hydrocarbon ring, an anthracene ring, a naphthalene ring, or the like is preferred. As the π-electron-rich heteroaromatic ring, a fused aromatic ring containing at least one of a pyrrole skeleton, a furan skeleton, and a thiophene skeleton in the ring is preferred, and specifically, a carbazole ring, a dibenzothiophene ring, or a ring in which an aromatic ring or a heteroaromatic ring is further fused to the above ring is preferred.

[0218] Such organic compounds having hole-transporting properties preferably have a carbazole skeleton, a dibenzofuran skeleton, a dibenzothiophene skeleton, or an anthracene skeleton. In particular, aromatic amines having a substituent containing a dibenzofuran ring or a dibenzothiophene ring, aromatic monoamines having a naphthalene ring, or aromatic monoamines in which a 9-fluorenyl group is bonded to the nitrogen of the amine via an arylene group may be used. It is preferable that these organic compounds having hole-transporting properties are substances having an N,N-bis(4-biphenyl)amino group, since this allows the fabrication of light-emitting devices with a long lifetime.

[0219] Specific examples of the organic compound having hole transport properties as described above include N-(4-biphenyl)-6,N-diphenylbenzo[b]naphtho[1,2-d]furan-8-amine (abbreviation: BnfABP), N,N-bis(4-biphenyl)-6-phenylbenzo[b]naphtho[1,2-d]furan-8-amine (abbreviation: BBABnf), 4,4'-bis(6-phenylbenzo[b]naphtho[1,2-d]furan-8-yl)-4"-phenyltriphenylamine (abbreviation: BnfBB1BP), N,N-bis(4-biphenyl)benzylamine (abbreviation: BnfBB1BP), and N,N-bis(4-biphenyl)benzylamine (abbreviation: BnfBB1BP). N,N-bis(4-biphenyl)benzo[b]naphtho[1,2-d]furan-6-amine (abbreviation: BBABnf(6)), N,N-bis(4-biphenyl)benzo[b]naphtho[1,2-d]furan-8-amine (abbreviation: BBABnf(8)), N,N-bis(4-biphenyl)benzo[b]naphtho[2,3-d]furan-4-amine (abbreviation: BBABnf(II)(4)), N,N-bis[4-(dibenzofuran-4-yl)phenyl]-4-amino-p-terphenyl (abbreviation: DBfBB1TP), N-[4-(dibenzothiophen-4-yl)phenyl]-4-amino-p-terphenyl] ]-N-phenyl-4-biphenylamine (abbreviation: ThBA1BP), 4-(2-naphthyl)-4',4''-diphenyltriphenylamine (abbreviation: BBAβNB), 4-[4-(2-naphthyl)phenyl]-4',4''-diphenyltriphenylamine (abbreviation: BBAβNBi), 4,4'-diphenyl-4''-(6;1'-binaphthyl-2-yl)triphenylamine (abbreviation: BBAαNβNB), 4,4'-diphenyl-4''-(7;1'-binaphthyl-2-yl)triphenylamine (abbreviation: BBAαNβ NB-03), 4,4'-diphenyl-4"-(7-phenyl)naphthyl-2-yltriphenylamine (abbreviation: BBAPβNB-03), 4,4'-diphenyl-4"-(6;2'-binaphthyl-2-yl)triphenylamine (abbreviation: BBA(βN2)B), 4,4'-diphenyl-4"-(7;2'-binaphthyl-2-yl)triphenylamine (abbreviation: BBA(βN2)B-03), 4,4'-diphenyl-4"-(4;2'-binaphthyl-1-yl)triphenylamine (abbreviation: BBAβNαNB), 4,4'-Diphenyl-4"-(5;2'-binaphthyl-1-yl)triphenylamine (abbreviation: BBAβNαNB-02), 4-(4-biphenylyl)-4'-(2-naphthyl)-4"-phenyltriphenylamine (abbreviation: TPBiAβNB), 4-(3-biphenylyl)-4'-[4-(2-naphthyl)phenyl]-4"-phenyltriphenylamine (abbreviation: mTPBiAβNBi), 4-(4-biphenylyl)-4'-[4-(2-naphthyl)phenyl] [4'-(3-phenyl-9H-carbazol-9-yl)biphenyl-4-yl]triphenylamine (abbreviation: TPBiAβNBi), 4-phenyl-4'-(1-naphthyl)triphenylamine (abbreviation: αNBA1BP), 4,4'-bis(1-naphthyl)triphenylamine (abbreviation: αNBB1BP), 4,4'-diphenyl-4"-[4'-(carbazol-9-yl)biphenyl-4-yl]triphenylamine (abbreviation: YGTBi1BP), 4'-[4-(3-phenyl-9H-carbazol-9-yl)f N-[4-(9-phenyl-9H-carbazol-3-yl)phenyl]-N-[4-(1-naphthyl)phenyl]-9,9'-spirobi[9H-fluorene]-2-amine (abbreviation: PCBNBSF), N,N- Bis(biphenyl-4-yl)-9,9'-spirobi[9H-fluorene]-2-amine (abbreviation: BBASF), N,N-bis(biphenyl-4-yl)-9,9'-spirobi[9H-fluorene]-4-amine (abbreviation: BBASF(4)), N-(biphenyl-2-yl)-N-(9,9-dimethyl-9H-fluoren-2-yl)-9,9'-spirobi[9H-fluorene]-4-amine (abbreviation: oFBiSF), N-(biphenyl-4-yl)-N-(9,9-dimethyl-9H-fluoren-2-yl)dibenzofuran-4-amine (abbreviation: FrBiF), N-[4-(1-naphthyl)phenyl]-N-[3-(6-phenyldibenzofuran-4-yl)phenyl]-1-naphthylamine (abbreviation: mPDBfBNBN), 4-phenyl-4'-(9-phenylfluoren-9-yl)triphenylamine (abbreviation: BPAFLP), 4-phenyl-3'-(9-phenylfluoren-9-yl)triphenylamine (abbreviation: mBPAFLP), 4-phenyl-4' -[4-(9-phenylfluoren-9-yl)phenyl]triphenylamine (abbreviation: BPAFLBi), 4-phenyl-4'-(9-phenyl-9H-carbazol-3-yl)triphenylamine (abbreviation: PCBA1BP), 4,4'-diphenyl-4"-(9-phenyl-9H-carbazol-3-yl)triphenylamine (abbreviation: PCBBi1BP), 4-(1-naphthyl)-4'-(9-phenyl-9H-carbazol-3-yl)triphenylamine (abbreviation: PCBANB), 4,4'- Di(1-naphthyl)-4"-(9-phenyl-9H-carbazol-3-yl)triphenylamine (abbreviation: PCBNBB), N-phenyl-N-[4-(9-phenyl-9H-carbazol-3-yl)phenyl]-9,9'-spirobi[9H-fluorene]-2-amine (abbreviation: PCBASF), N-(biphenyl-4-yl)-N-[4-(9-phenyl-9H-carbazol-3-yl)phenyl]-9,9-dimethyl-9H-fluorene-2-amine (abbreviation: PCBBiF), N,N-bis( 9,9-dimethyl-9H-fluoren-2-yl)-9,9'-spirobi-9H-fluoren-4-amine, N,N-bis(9,9-dimethyl-9H-fluoren-2-yl)-9,9'-spirobi-9H-fluoren-3-amine, N,N-bis(9,9-dimethyl-9H-fluoren-2-yl)-9,9'-spirobi-9H-fluoren-2-amine, N,N-bis(9,9-dimethyl-9H-fluoren-2-yl)-9,9'-spirobi-9H-fluoren-1-amine, etc. can be mentioned.

[0220] In addition, other aromatic amine compounds such as N,N'-di(p-tolyl)-N,N'-diphenyl-p-phenylenediamine (abbreviation: DTDPPA), 4,4'-bis[N-(4-diphenylaminophenyl)-N-phenylamino]biphenyl (abbreviation: DPAB), 4,4'-bis(N-{4-[N'-(3-methylphenyl)-N'-phenylamino]phenyl}-N-phenylamino)biphenyl (abbreviation: DNTPD), and 1,3,5-tris[N-(4-diphenylaminophenyl)-N-phenylamino]benzene (abbreviation: DPA3B) can also be used as the material having hole transport properties.

[0221] By forming the hole injection layer 111, the hole injection property becomes good, and a light emitting device with a low driving voltage can be obtained.

[0222] Among substances having electron acceptor properties, organic compounds having electron acceptor properties are easy to use because they can be easily vapor-deposited and formed into a film.

[0223] The hole transport layer 112 is formed by containing an organic compound having a hole transport property. −6 cm 2 It is preferable that the material has a hole mobility of 1.0 V or more.

[0224] Examples of the material having hole transport properties include 4,4'-bis[N-(1-naphthyl)-N-phenylamino]biphenyl (abbreviation: NPB), N,N'-diphenyl-N,N'-bis(3-methylphenyl)-4,4'-diaminobiphenyl (abbreviation: TPD), N,N'-bis(9,9'-spirobi[9H-fluoren]-2-yl)-N,N'-diphenyl-4,4'-diaminobiphenyl (abbreviation: BSPB), 4-phenyl-4'-(9-phenylfluoren-9-yl)triphenylamine (abbreviation: BPAFLP), 4-phenyl-3'- (9-Phenylfluoren-9-yl)triphenylamine (abbreviation: mBPAFLP), 4-phenyl-4'-(9-phenyl-9H-carbazol-3-yl)triphenylamine (abbreviation: PCBA1BP), 4,4'-diphenyl-4"-(9-phenyl-9H-carbazol-3-yl)triphenylamine (abbreviation: PCBBi1BP), 4-(1-naphthyl)-4'-(9-phenyl-9H-carbazol-3-yl)triphenylamine (abbreviation: PCBANB), 4,4'-di(1-naphthyl)-4"-(9-phenyl-9H-carbazol-3-yl)triphenylamine (abbreviation: PCBANB), compounds having an aromatic amine skeleton such as 9,9-dimethyl-N-phenyl-N-[4-(9-phenyl-9H-carbazol-3-yl)phenyl]fluoren-2-amine (abbreviation: PCBAF), and N-phenyl-N-[4-(9-phenyl-9H-carbazol-3-yl)phenyl]-9,9'-spirobi[9H-fluorene]-2-amine (abbreviation: PCBASF); 1,3-bis(N-carbazolyl)benzene (abbreviation: mCP); 4,4'-di(N-carbazol-3-yl)triphenylamine (abbreviation: PCBNBB); 9,9'-bis(biphenyl-4-yl)-3,3'-bi-9H-carbazole (abbreviation: BisBPCz), 9,9'-bis(biphenyl-3-yl)-3,3'-bi-9H-carbazole (abbreviation: BismBPCz), 9-(biphenyl-3-yl)-9'-(biphenyl-4-yl)-9H,9'H-3,3'-bicarbazole (abbreviation: mBPCCBP), 9-(2-naphthyl)-9'-phenyl-9H,9'H-3,3'-bicarbazole (abbreviation: βNCCP), 9-(3-biphenyl)-9'-(2-naphthyl)-3,3'-bi-9H-carbazole (abbreviation: βNCCmBP), 9-(4-biphenyl)-9'-(2-naphthyl)-3,3'-bi-9H-carbazole (abbreviation: βNCCBP), 9,9'-di-2-naphthyl-3,3'-9H,9'H-bicarbazole (abbreviation: BisβNCz), 9-( 2-naphthyl)-9'-[1,1':4',1"-terphenyl]-3-yl-3,3'-9H,9'H-bicarbazole, 9-(2-naphthyl)-9'-[1,1':3',1"-terphenyl]-3-yl-3,3'-9H,9'H-bicarbazole, 9-(2-naphthyl)-9'-[1,1':3',1"-terphenyl]-5'-yl-3,3'-9H,9'H-bicarbazole, 9-(2-naphthyl)-9'-[1,1':4',1"-terphenyl]-4-yl-3,3'-9H,9'H- Bicarbazole, 9-(2-naphthyl)-9'-[1,1':3',1"-terphenyl]-4-yl-3,3'-9H,9'H-bicarbazole, 9-(2-naphthyl)-9'-(triphenylen-2-yl)-3,3'-9H,9'H-bicarbazole, 9-phenyl-9'-(triphenylen-2-yl)-3,3'-9H,9'H-bicarbazole (abbreviation: PCCzTp), 9,9'-bis(triphenylen-2-yl)-3,3'-9H,9'H-bicarbazole, 9-(4-biphenyl)- compounds having a carbazole skeleton such as 9'-(triphenylen-2-yl)-3,3'-9H,9'H-bicarbazole, 9-(triphenylen-2-yl)-9'-[1,1':3',1"-terphenyl]-4-yl-3,3'-9H,9'H-bicarbazole, and 9-[4-(9-phenyl-9H-carbazol-3-yl)phenyl]phenanthrene (abbreviation: PCPPn); 4,4',4"-(benzene-1,3,5-triyl)tri(dibenzothiophene) (abbreviation: DBT3P-II);Examples of suitable compounds include compounds having a thiophene skeleton, such as 8-diphenyl-4-[4-(9-phenyl-9H-fluoren-9-yl)phenyl]dibenzothiophene (abbreviation: DBTFLP-III) and 4-[4-(9-phenyl-9H-fluoren-9-yl)phenyl]-6-phenyldibenzothiophene (abbreviation: DBTFLP-IV), and compounds having a furan skeleton, such as 4,4′,4″-(benzene-1,3,5-triyl)tri(dibenzofuran) (abbreviation: DBF3P-II) and 4-{3-[3-(9-phenyl-9H-fluoren-9-yl)phenyl]phenyl}dibenzofuran (abbreviation: mmDBFFLBi-II). Among the compounds listed above, compounds having an aromatic amine skeleton and compounds having a carbazole skeleton are preferred because they have good reliability, high hole transport properties, and contribute to reducing driving voltage. Note that the substances listed as the materials having hole transport properties used in the composite material of the hole injection layer 111 can also be suitably used as materials for forming the hole transport layer 112.

[0225] The light-emitting layer 113 is a layer containing a light-emitting substance, and preferably contains a light-emitting substance and a host material. The light-emitting layer may also contain other materials. Alternatively, the light-emitting layer may be a stack of two layers with different compositions.

[0226] The luminescent material may be a fluorescent material, a phosphorescent material, a material exhibiting thermally activated delayed fluorescence (TADF), or any other luminescent material.

[0227] Examples of materials that can be used as fluorescent materials in the light-emitting layer include the following: In addition, fluorescent materials other than these can also be used.

[0228] 5,6-bis[4-(10-phenyl-9-anthryl)phenyl]-2,2'-bipyridine (abbreviation: PAP2BPy), 5,6-bis[4'-(10-phenyl-9-anthryl)biphenyl-4-yl]-2,2'-bipyridine (abbreviation: PAPP2BPy), N,N'-diphenyl-N,N'-bis[4-(9-phenyl-9H-fluoren-9-yl)phenyl]pyrene-1,6-diamine (abbreviation: 1,6FLPAPrn), N,N'-bis(3-methylphenyl)-N,N'-bis[3-(9-phenyl-9H-fluoren-9-yl)phenyl]pyrene-1,6-diamine )phenyl]pyrene-1,6-diamine (abbreviation: 1,6mMemFLPAPrn), N,N'-bis[4-(9H-carbazol-9-yl)phenyl]-N,N'-diphenylstilbene-4,4'-diamine (abbreviation: YGA2S), 4-(9H-carbazol-9-yl)-4'-(10-phenyl-9-anthryl)triphenylamine (abbreviation: YGAPA), 4-(9H-carbazol-9-yl)-4'-(9,10-diphenyl-2-anthryl)triphenylamine (abbreviation: 2YGAPPA), N,9-diphenyl-N-[4-( 10-phenyl-9-anthryl)phenyl]-9H-carbazol-3-amine (abbreviation: PCAPA), perylene, 2,5,8,11-tetra-tert-butylperylene (abbreviation: TBP), 4-(10-phenyl-9-anthryl)-4'-(9-phenyl-9H-carbazol-3-yl)triphenylamine (abbreviation: PCBAPA), N,N''-(2-tert-butylanthracene-9,10-diyldi-4,1-phenylene)bis(N,N',N'-triphenyl-1,4-phenylenediamine) (abbreviation: DPABPA), N,9 -diphenyl-N-[4-(9,10-diphenyl-2-anthryl)phenyl]-9H-carbazol-3-amine (abbreviation: 2PAPPA), N-[4-(9,10-diphenyl-2-anthryl)phenyl]-N,N',N'-triphenyl-1,4-phenylenediamine (abbreviation: 2DPAPPA), N,N,N',N',N'',N'',N'''',N'''-octaphenyldibenzo[g,p]chrysene-2,7,10,15-tetraamine (abbreviation: DBC1), Coumarin 30, N-(9,10-diphenyl-2-anthryl)-N,9-Diphenyl-9H-carbazole-3-amine (abbreviation: 2PCAPA), N-[9,10-bis(biphenyl-2-yl)-2-anthryl]-N,9-diphenyl-9H-carbazole-3-amine (abbreviation: 2PCABPhA), N-(9,10-diphenyl-2-anthryl)-N,N',N'-triphenyl-1,4-phenylenediamine (abbreviation: 2DPAPA), N-[9,10-bis(biphenyl-2-yl)-2-anthryl]-N,N',N'-triphenyl-1,4-phenylenediamine (abbreviation: 2DPABPhA) , 9,10-bis(biphenyl-2-yl)-N-[4-(9H-carbazol-9-yl)phenyl]-N-phenylanthracen-2-amine (abbreviation: 2YGABPhA), N,N,9-triphenylanthracen-9-amine (abbreviation: DPhAPhA), Coumarin 545T, N,N'-diphenylquinacridone (abbreviation: DPQd), rubrene, 5,12-bis(biphenyl-4-yl)-6,11-diphenyltetracene (abbreviation: BPT), 2-(2-{2-[4-(dimethylamino)phenyl]ethenyl}-6-methyl-4H-pyra N,N,N',N'-tetrakis(4-methylphenyl)acenaphtho[1,2-a]fluoranthene-3,10-diamine (abbreviation: p-mPhTD), 2-{2-methyl-6-[2-(2,3,6,7-tetrahydro-1H,5H-benzo[ij]quinolizin-9-yl)ethenyl]-4H-pyran-4-ylidene}propanedinitrile (abbreviation: DCM1), 2-{2-methyl-6-[2-(2,3,6,7-tetrahydro-1H,5H-benzo[ij]quinolizin-9-yl)ethenyl]-4H-pyran-4-ylidene}propanedinitrile (abbreviation: DCM2), N,N,N',N'-tetrakis(4-methylphenyl)tetracene-5,11-diamine (abbreviation: p-mPhTD), 7,14-diphenyl-N,N,N',N'-tetrakis(4-methylphenyl)acenaphtho[1,2-a]fluoranthene-3,10-diamine (abbreviation: p-mPhTD), Name: p-mPhAFD), 2-{2-isopropyl-6-[2-(1,1,7,7-tetramethyl-2,3,6,7-tetrahydro-1H,5H-benzo[ij]quinolizin-9-yl)ethenyl]-4H-pyran-4-ylidene}propanedinitrile (abbreviation: DCJTI), 2-{2-tert-butyl-6-[2-(1,1,7,7-tetramethyl-2,3,6,7-tetrahydro-1H,5H-benzo[ij]quinolizin-9-yl)ethenyl]-4H-pyran-4-ylidene}propanedinitrile (abbreviation: DCJTB), 2-(2,6-bis{2-[4-(dimethylamino)phenyl]ethenyl}-4H-pyran-4-ylidene)propanedinitrile (abbreviation: BisDCM), 2-{2,6-bis[2-(8-methoxy-1,1,7,7-tetramethyl-2,3,6,7-tetrahydro-1H,5H-benzo[ij]quinolizin-9-yl)ethenyl]-4H-pyran-4-ylidene}propanedinitrile (abbreviation: BisDCJ™), N,N'-diphenyl-N,N'-(1,6-pyren-diyl)bis[(6-phenylbenzo[b ]naphtho[1,2-d]furan)-8-amine] (abbreviation: 1,6BnfAPrn-03), 3,10-bis[N-(9-phenyl-9H-carbazol-2-yl)-N-phenylamino]naphtho[2,3-b;6,7-b']bisbenzofuran (abbreviation: 3,10PCA2Nbf(IV)-02), and 3,10-bis[N-(dibenzofuran-3-yl)-N-phenylamino]naphtho[2,3-b;6,7-b']bisbenzofuran (abbreviation: 3,10FrA2Nbf(IV)-02). In particular, condensed aromatic diamine compounds typified by pyrene diamine compounds such as 1,6FLPAPrn, 1,6mMemFLPAPrn, and 1,6BnfAPrn-03 are preferred because they have high hole-trapping properties and excellent luminous efficiency or reliability. ,

[0229] Also, 5,9-diphenyl-5,9-diaza-13b-boranaphtho[3,2,1-de]anthracene (abbreviation: DABNA1), 9-(diphenyl-3-yl)-N,N,5,11-tetraphenyl-5,9-dihydro-5,9-diaza-13b-boranaphtho[3,2,1-de]anthracene-3-amine (abbreviation: DABNA2), 2,12-di(tert-butyl)-5,9-di(4-tert-butylphenyl)-N,N-diphenyl-5H,9H-[1,4]benzazaborino[2,3,4-kl]phenazaborine -7-amine (abbreviation: DPhA-tBu4DABNA), 2,12-di(tert-butyl)-N,N,5,9-tetra(4-tert-butylphenyl)-5H,9H-[1,4]benzazaborino[2,3,4-kl]phenazaborin-7-amine (abbreviation: tBuDPhA-tBu4DABNA), 2,12-di(tert-butyl)-5,9-di(4-tert-butylphenyl)-7-methyl-5H,9H-[1,4]benzazaborino[2,3,4-kl]phenazaborin (abbreviation: Me-tBu4DABNA), N 7 , N 7 , N 13 , N 13 Condensed heteroaromatic compounds containing nitrogen and boron, such as 5,9,11,15-octaphenyl-5H,9H,11H,15H-[1,4]benzazaborino[2,3,4-kl][1,4]benzazaborino[4',3',2':4,5][1,4]benzazaborino[3,2-b]phenazaborine-7,13-diamine (abbreviation: v-DABNA), and 2-(4-tert-butylphenyl)benz[5,6]indolo[3,2,1-jk]benzo[b]carbazole (abbreviation: tBuPBibc), in particular compounds having a diazaboranaphthoanthracene skeleton, can be suitably used because they have a narrow emission spectrum and can emit blue light with good color purity.

[0230] In addition to these, 9,10,11-tris[3,6-bis(1,1-dimethylethyl)-9H-carbazol-9-yl]-2,5,15,18-tetrakis(1,1-dimethylethyl)indolo[3,2,1-de]indolo[3',2',1':8,1][1,4]benzazaborino[2,3,4-kl]phenazaborine (abbreviation: BBCz-G), 9,11-bis[3,6-bis(1,1-dimethylethyl)-9H-carbazol-9-yl]-2,5,15,18-tetrakis(1,1-dimethylethyl)indolo[3,2,1-de]indolo[3',2',1':8,1][1,4]benzazaborino[2,3,4-kl]phenazaborine (abbreviation: BBCz-Y) and the like can be preferably used.

[0231] When a phosphorescent material is used as the light-emitting material in the light-emitting layer, examples of materials that can be used include the following.

[0232] Tris{2-[5-(2-methylphenyl)-4-(2,6-dimethylphenyl)-4H-1,2,4-triazol-3-yl-κN]phenyl-κC}iridium(III) (abbreviation: [Ir(mpptz-dmp) 3 ]), tris(5-methyl-3,4-diphenyl-4H-1,2,4-triazolato)iridium(III) (abbreviation: [Ir(Mptz) 3 organometallic iridium complexes having a 4H-triazole skeleton, such as tris[3-methyl-1-(2-methylphenyl)-5-phenyl-1H-1,2,4-triazolato]iridium(III) (abbreviation: [Ir(Mptz1-mp) 3 ]), tris(1-methyl-5-phenyl-3-propyl-1H-1,2,4-triazolato)iridium(III) (abbreviation: [Ir(Prptz1-Me) 3 organometallic iridium complexes having a 1H-triazole skeleton, such as fac-tris[1-(2,6-diisopropylphenyl)-2-phenyl-1H-imidazole]iridium(III) (abbreviation: [Ir(iPrpim) 3]), tris[3-(2,6-dimethylphenyl)-7-methylimidazo[1,2-f]phenanthridinato]iridium(III) (abbreviation: [Ir(dmpimpt-Me) 3 organometallic iridium complexes having an imidazole skeleton, such as tris(2-[1-{2,6-bis(1-methylethyl)phenyl}-1H-imidazol-2-yl-κN]-4-cyanophenyl-κC) (abbreviation: CNImIr), tris[(6-tert-butyl-3-phenyl-2H-imidazo[4,5-b]pyrazin-1-yl-κC)phenyl-κC]iridium(III) (abbreviation: [Ir(cb) 3 organometallic complexes having a benzimidazolidene skeleton, such as bis[2-(4',6'-difluorophenyl)pyridinato-N,C 2′ ]iridium(III) tetrakis(1-pyrazolyl)borate (abbreviation: FIr6), bis[2-(4',6'-difluorophenyl)pyridinato-N,C 2′ ]iridium(III) picolinate (abbreviation: FIrpic), bis{2-[3',5'-bis(trifluoromethyl)phenyl]pyridinato-N,C 2′} Iridium(III) picolinate (abbreviation: [Ir(CF 3 ppy) 2 (pic)]), bis[2-(4',6'-difluorophenyl)pyridinato-N,C 2′ ] Organometallic iridium complexes having a phenylpyridine derivative having an electron-withdrawing group as a ligand, such as iridium(III) acetylacetonate (abbreviation: FIracac), are examples of such compounds that exhibit blue phosphorescence and have an emission peak in the wavelength range of 450 nm to 520 nm.

[0233] Also, tris(4-methyl-6-phenylpyrimidinato)iridium(III) (abbreviation: [Ir(mppm) 3 ]), tris(4-t-butyl-6-phenylpyrimidinato)iridium(III) (abbreviation: [Ir(tBuppm) 3 ]), (acetylacetonato)bis(6-methyl-4-phenylpyrimidinato)iridium(III) (abbreviation: [Ir(mppm)2 (acac)]), (acetylacetonato)bis(6-tert-butyl-4-phenylpyrimidinato)iridium(III) (abbreviation: [Ir(tBuppm) 2 (acac)]), (acetylacetonato)bis[6-(2-norbornyl)-4-phenylpyrimidinato]iridium(III) (abbreviation: [Ir(nbppm) 2 (acac)]), (acetylacetonato)bis[5-methyl-6-(2-methylphenyl)-4-phenylpyrimidinato]iridium(III) (abbreviation: [Ir(mpmppm) 2 (acac)]), (acetylacetonato)bis(4,6-diphenylpyrimidinato)iridium(III) (abbreviation: [Ir(dppm) 2 organometallic iridium complexes having a pyrimidine skeleton, such as (acetylacetonato)bis(3,5-dimethyl-2-phenylpyrazinato)iridium(III) (abbreviation: [Ir(mppr-Me) 2 (acac)]), (acetylacetonato)bis(5-isopropyl-3-methyl-2-phenylpyrazinato)iridium(III) (abbreviation: [Ir(mppr-iPr) 2 organometallic iridium complexes having a pyrazine skeleton, such as tris(2-phenylpyridinato-N,C(acac)]); 2′ ) Iridium(III) (abbreviation: [Ir(ppy) 3 ]), bis(2-phenylpyridinato-N,C 2′ ) Iridium(III) acetylacetonate (abbreviation: [Ir(ppy) 2 (acac)]), bis(benzo[h]quinolinato)iridium(III) acetylacetonate (abbreviation: [Ir(bzq) 2 (acac)]), tris(benzo[h]quinolinato)iridium(III) (abbreviation: [Ir(bzq) 3 ]), tris(2-phenylquinolinato-N,C 2′ ) Iridium(III) (abbreviation: [Ir(pq) 3 ]), bis(2-phenylquinolinato-N,C 2′ ) iridium(III) acetylacetonate (abbreviation: [Ir(pq)2 (acac)]), [2-d 3 -methyl-8-(2-pyridinyl-κN)benzofuro[2,3-b]pyridine-κC]bis[2-(5-d 3 [Ir(5mppy-d-methyl-2-pyridinyl-κN)phenyl-κC]iridium(III) (abbreviation: [Ir(5mppy-d-methyl-2-pyridinyl-κN)phenyl-κC]iridium(III) 3 ) 2 (mbfpypy-d 3 ) )]), [2-d 3 [2-(2-pyridinyl-κN)phenyl-κC]iridium(III) (abbreviation: [Ir(ppy) 2 (mbfpypy-d 3 )]), [2-(4-d 3 -methyl-5-phenyl-2-pyridinyl-κN)phenyl-κC]bis[2-(5-d 3 [Ir(5mppy-d-methyl-2-pyridinyl-κN)phenyl-κC]iridium(III) (abbreviation: [Ir(5mppy-d-methyl-2-pyridinyl-κN)phenyl-κC]iridium(III) 3 ) 2 (mdppy-d 3 ) )]), [2-methyl-(2-pyridinyl-κN)benzofuro[2,3-b]pyridine-κC]bis[2-(2-pyridinyl-κN)phenyl-κC]iridium(III) (abbreviation: [Ir(ppy) 2 (mbfpypy)]), [2-(4-methyl-5-phenyl-2-pyridinyl-κN)phenyl-κC]bis[2-(2-pyridinyl-κN)phenyl-κC]iridium (abbreviation: [Ir(ppy) 2 In addition to organometallic iridium complexes having a pyridine skeleton, such as tris(acetylacetonato)(monophenanthroline)terbium(III) (abbreviation: [Tb(acac)]), 3 These compounds mainly exhibit green phosphorescence, with an emission peak in the wavelength range of 500 nm to 600 nm. Organometallic iridium complexes having a pyrimidine skeleton are particularly preferred because they are remarkably excellent in reliability and luminous efficiency.

[0234] Also, (diisobutyrylmethanato)bis[4,6-bis(3-methylphenyl)pyrimidinato]iridium(III) (abbreviation: [Ir(5mdppm) 2 (dibm)]), bis[4,6-bis(3-methylphenyl)pyrimidinato](dipivaloylmethanato)iridium(III) (abbreviation: [Ir(5mdppm) 2 (dpm)]), bis[4,6-di(naphthalen-1-yl)pyrimidinato](dipivaloylmethanato)iridium(III) (abbreviation: [Ir(dpm) 2 organometallic iridium complexes having a pyrimidine skeleton, such as (acetylacetonato)bis(2,3,5-triphenylpyrazinato)iridium(III) (abbreviation: [Ir(tppr) 2 (acac)]), bis(2,3,5-triphenylpyrazinato)(dipivaloylmethanato)iridium(III) (abbreviation: [Ir(tppr) 2 (dpm)]), (acetylacetonato)bis[2,3-bis(4-fluorophenyl)quinoxalinato]iridium(III) (abbreviation: [Ir(Fdpq) 2 organometallic iridium complexes having a pyrazine skeleton, such as tris(1-phenylisoquinolinato-N,C(acac)]); 2′ ) Iridium(III) (abbreviation: [Ir(piq) 3 ]), bis(1-phenylisoquinolinato-N,C 2′ ) iridium(III) acetylacetonate (abbreviation: [Ir(piq) 2(acac)]), (3,7-diethyl-4,6-nonanedionato-κO4,κO6)bis[2,4-dimethyl-6-[7-(1-methylethyl)-1-isoquinolinyl-κN]phenyl-κC]iridium(III), (3,7-diethyl-4,6-nonanedionato-κO4,κO6)bis[2,4-dimethyl-6-[5-(1-methylethyl)-2-quinolinyl-κN]phenyl-κC]iridium(III). In addition to organometallic iridium complexes having a pyridine skeleton such as [ru-κC]iridium(III), platinum complexes such as 2,3,7,8,12,13,17,18-octaethyl-21H,23H-porphyrinplatinum(II) (abbreviation: PtOEP), tris(1,3-diphenyl-1,3-propanedionato)(monophenanthroline)europium(III) (abbreviation: [Eu(DBM) 3 (Phen)]), tris[1-(2-thenoyl)-3,3,3-trifluoroacetonato](monophenanthroline)europium(III) (abbreviation: [Eu(TTA) 3 Examples of rare earth metal complexes include iridium complexes such as iridium complexes containing pyrazine skeletons and iridium complexes containing iridium ions. These compounds exhibit red phosphorescence and have an emission peak in the wavelength range of 600 nm to 700 nm. Organometallic iridium complexes containing pyrazine skeletons exhibit red emission with good chromaticity.

[0235] In addition to the phosphorescent compounds described above, known phosphorescent compounds may be selected and used.

[0236] Examples of TADF materials that can be used include fullerene and its derivatives, acridine and its derivatives, and eosin derivatives. Other examples include metal-containing porphyrins containing magnesium (Mg), zinc (Zn), cadmium (Cd), tin (Sn), platinum (Pt), indium (In), or palladium (Pd). Examples of metal-containing porphyrins include protoporphyrin-tin fluoride complexes (SnF) represented by the following structural formula: 2 (Proto IX)), mesoporphyrin-tin fluoride complex (SnF 2 (Meso IX)), hematoporphyrin-tin fluoride complex (SnF 2(Hemato IX)), coproporphyrin tetramethyl ester-tin fluoride complex (SnF 2 (Copro III-4Me)), octaethylporphyrin-tin fluoride complex (SnF 2 (OEP)), etioporphyrin-tin fluoride complex (SnF 2 (Etio I)), octaethylporphyrin-platinum chloride complex (PtCl 2 OEP) and the like.

[0237]

[0238] Further, 2-(biphenyl-4-yl)-4,6-bis(12-phenylindolo[2,3-a]carbazol-11-yl)-1,3,5-triazine (abbreviation: PIC-TRZ), 9-(4,6-diphenyl-1,3,5-triazin-2-yl)-9'-phenyl-9H,9'H-3,3'-bicarbazole (abbreviation: PCCzTzn), 2-{4-[3-(N-phenyl-9H-carbazol-3-yl)-9H-carbazol-9-yl]phenyl}-4,6-diphenyl-1,3,5-triazine (abbreviation: PCCzPTzn), 2-[4-(10H-phenoxazin-10-yl)phenyl]-4,6-diphenyl-1,3,5-triazine (abbreviation: PCCzPTzn), and Heterocyclic compounds having one or both of a π-electron rich heteroaromatic ring and a π-electron deficient heteroaromatic ring, such as 3-[4-(5-phenyl-5,10-dihydrophenazin-10-yl)phenyl]-4,5-diphenyl-1,2,4-triazole (abbreviation: PPZ-3TPT), 3-(9,9-dimethyl-9H-acridin-10-yl)-9H-xanthen-9-one (abbreviation: ACRXTN), bis[4-(9,9-dimethyl-9,10-dihydroacridine)phenyl]sulfone (abbreviation: DMAC-DPS), and 10-phenyl-10H,10′H-spiro[acridine-9,9′-anthracene]-10′-one (abbreviation: ACRSA), can also be used. The heterocyclic compound has a π-electron-rich heteroaromatic ring and a π-electron-deficient heteroaromatic ring, and therefore has high electron transport and hole transport properties, and is therefore preferred. Among the skeletons having a π-electron-deficient heteroaromatic ring, pyridine skeleton, diazine skeleton (pyrimidine skeleton, pyrazine skeleton, pyridazine skeleton), and triazine skeleton are preferred because they are stable and reliable. In particular, benzofuropyrimidine skeleton, benzothienopyrimidine skeleton, benzofuropyrazine skeleton, and benzothienopyrazine skeleton are preferred because they have high electron acceptor properties and are reliable. Furthermore, among the skeletons having a π-electron-rich heteroaromatic ring, acridine skeleton, phenoxazine skeleton, phenothiazine skeleton, furan skeleton, thiophene skeleton, and pyrrole skeleton are preferred because they are stable and reliable.The furan skeleton is preferably a dibenzofuran skeleton, and the thiophene skeleton is preferably a dibenzothiophene skeleton. Furthermore, the pyrrole skeleton is particularly preferably an indole skeleton, a carbazole skeleton, an indolocarbazole skeleton, a bicarbazole skeleton, or a 3-(9-phenyl-9H-carbazole-3-yl)-9H-carbazole skeleton. Furthermore, in a substance in which a π-electron-rich heteroaromatic ring and a π-electron-deficient heteroaromatic ring are directly bonded, the electron-donating property of the π-electron-rich heteroaromatic ring and the electron-accepting property of the π-electron-deficient heteroaromatic ring are both enhanced, resulting in S. 1 Level and T 1 This is particularly preferred because the energy difference between the levels is small, allowing thermally activated delayed fluorescence to be obtained efficiently. Instead of the π-electron-deficient heteroaromatic ring, an aromatic ring bonded to an electron-withdrawing group such as a cyano group may be used. Furthermore, an aromatic amine skeleton, a phenazine skeleton, or the like can be used as the π-electron-rich skeleton. Furthermore, as the π-electron-deficient skeleton, a xanthene skeleton, a thioxanthene dioxide skeleton, an oxadiazole skeleton, a triazole skeleton, an imidazole skeleton, an anthraquinone skeleton, a boron-containing skeleton such as phenylborane or boranthrene, an aromatic ring having a nitrile group or a cyano group such as benzonitrile or cyanobenzene, a heteroaromatic ring, a carbonyl skeleton such as benzophenone, a phosphine oxide skeleton, a sulfone skeleton, or the like can be used. In this way, a π-electron-deficient skeleton and a π-electron-rich skeleton can be used in place of at least one of the π-electron-deficient heteroaromatic ring and the π-electron-rich heteroaromatic ring.

[0239]

[0240] The TADF material is S 1 Level and T 1 This material has a small difference in energy level between triplet and singlet excitations, and has the ability to convert energy from triplet excitation to singlet excitation through reverse intersystem crossing. Therefore, triplet excitation energy can be upconverted to singlet excitation energy (reverse intersystem crossing) with a small amount of thermal energy, allowing for efficient generation of a singlet excited state. In addition, triplet excitation energy can be converted into luminescence.

[0241] In addition, an excited complex (also called an exciplex) that forms an excited state with two kinds of substances is S 1 Level and T 1 The difference between the triplet excitation energy and the singlet excitation energy is extremely small, and the TADF material functions as a TADF material that can convert triplet excitation energy into singlet excitation energy.

[0242] In addition, T 1 The phosphorescence spectrum observed at low temperatures (for example, 77 K to 10 K) can be used as an index of the level. For the TADF material, a tangent line is drawn at the base of the fluorescence spectrum on the short wavelength side, and the energy of the wavelength of the extrapolated line is expressed as S 1 The energy level is set as the level, and a tangent line is drawn at the base of the phosphorescence spectrum on the short wavelength side. The energy of the wavelength of the extrapolated line is T 1 When the level is reached, the S 1 Level and T 1 The difference in level is preferably 0.3 eV or less, and more preferably 0.2 eV or less.

[0243] In addition, when a TADF material is used as a light-emitting material, the S 1 The level is S of the TADF material. 1 It is preferable that the T level of the host material is higher than that of the 1 The level is the T 1 It is preferable that the level is higher.

[0244] As the host material of the light-emitting layer, various carrier transport materials such as a material having an electron transport property and / or a material having a hole transport property, and the above-mentioned TADF material can be used.

[0245] The material having hole transport properties is preferably an organic compound having an amine skeleton or a π-electron-rich heteroaromatic ring skeleton. The π-electron-rich heteroaromatic ring is preferably a fused aromatic ring containing at least one of an acridine skeleton, a phenoxazine skeleton, a phenothiazine skeleton, a furan skeleton, a thiophene skeleton, and a pyrrole skeleton, and specifically preferably a carbazole ring, a dibenzothiophene ring, or a ring in which an aromatic ring or a heteroaromatic ring is further fused to the carbazole ring, a dibenzothiophene ring, or the ring in which the π-electron-rich heteroaromatic ring is further fused to the carbazole ring, a dibenzothiophene ring, or the ring in which ... a dibenzothiophene ring, or the ring in which the carbazole ring, a dibenzothiophene ring, a dibenzothiophene ring, or the ring in which the carbazole ring, a dibenzothiophene ring, a dibenzothiophene ring, a dibenzothiophene ring, a dibenzothiophene ring, a dibenzothiophene ring, a dibenzothiophene ring, a dibenzothiophene ring, a dibenzothiophene ring, a dibenzothiophene

[0246] Such organic compounds having hole-transporting properties preferably have a carbazole skeleton, a dibenzofuran skeleton, a dibenzothiophene skeleton, or an anthracene skeleton. In particular, aromatic amines having a substituent containing a dibenzofuran ring or a dibenzothiophene ring, aromatic monoamines having a naphthalene ring, or aromatic monoamines in which a 9-fluorenyl group is bonded to the nitrogen of the amine via an arylene group may be used. It is preferable that these organic compounds having hole-transporting properties are substances having an N,N-bis(4-biphenyl)amino group, since this allows the fabrication of light-emitting devices with a long lifetime.

[0247] Examples of such organic compounds include 4,4'-bis[N-(1-naphthyl)-N-phenylamino]biphenyl (abbreviation: NPB), N,N'-diphenyl-N,N'-bis(3-methylphenyl)-4,4'-diaminobiphenyl (abbreviation: TPD), N,N'-bis(9,9'-spirobi[9H-fluoren]-2-yl)-N,N'-diphenyl-4,4'-diaminobiphenyl (abbreviation: BSPB), 4-phenyl-4'-(9-phenylfluoren-9-yl)triphenylamine (abbreviation: BPAFLP), 4-phenyl-3'-(9-phenylfluoren-9-yl)triphenylamine (abbreviation: mBPAFLP), 4-phenyl-4'-(9-phenyl-9H-carbazol-3-yl)triphenylamine (abbreviation: PCBA1BP), 4,4'-diphenyl-4"-(9-phenyl-9H-carbazol-3-yl)triphenylamine (abbreviation: PCBBi1BP), 4-(1-naphthyl)-4'-(9-phenyl-9H-carbazol-3-yl)triphenylamine (abbreviation: PC aromatic amines such as 4,4'-di(1-naphthyl)-4"-(9-phenyl-9H-carbazol-3-yl)triphenylamine (abbreviation: PCBNBB), 9,9-dimethyl-N-phenyl-N-[4-(9-phenyl-9H-carbazol-3-yl)phenyl]fluoren-2-amine (abbreviation: PCBAF), and N-phenyl-N-[4-(9-phenyl-9H-carbazol-3-yl)phenyl]-9,9'-spirobi[9H-fluorene]-2-amine (abbreviation: PCBASF). compounds having a carbazole skeleton such as 1,3-bis(N-carbazolyl)benzene (abbreviation: mCP), 4,4'-di(N-carbazolyl)biphenyl (abbreviation: CBP), 3,6-bis(3,5-diphenylphenyl)-9-phenylcarbazole (abbreviation: CzTP), and 9,9'-diphenyl-9H,9'H-3,3'-bicarbazole (abbreviation: PCCP); compounds having a carbazole skeleton such as 4,4',4''-(benzene-1,3,5-triyl)tri(dibenzothiophene) (abbreviation: DBT3P-II);Examples of suitable compounds include compounds having a thiophene skeleton, such as 8-diphenyl-4-[4-(9-phenyl-9H-fluoren-9-yl)phenyl]dibenzothiophene (abbreviation: DBTFLP-III) and 4-[4-(9-phenyl-9H-fluoren-9-yl)phenyl]-6-phenyldibenzothiophene (abbreviation: DBTFLP-IV), and compounds having a furan skeleton, such as 4,4′,4″-(benzene-1,3,5-triyl)tri(dibenzofuran) (abbreviation: DBF3P-II) and 4-{3-[3-(9-phenyl-9H-fluoren-9-yl)phenyl]phenyl}dibenzofuran (abbreviation: mmDBFFLBi-II). Among the compounds listed above, compounds having an aromatic amine skeleton or a carbazole skeleton are preferred because they have good reliability, high hole transport properties, and contribute to reducing driving voltage. In addition, the organic compounds listed as examples of materials having hole transport properties in the hole transport layer can also be used.

[0248] An example of a material having electron transport properties is bis(10-hydroxybenzo[h]quinolinato)beryllium(II) (abbreviation: BeBq 2 Preferred are metal complexes such as bis(2-methyl-8-quinolinolato)(4-phenylphenolato)aluminum(III) (abbreviation: BAlq), bis(8-quinolinolato)zinc(II) (abbreviation: Znq), bis[2-(2-benzoxazolyl)phenolato]zinc(II) (abbreviation: ZnPBO), and bis[2-(2-benzothiazolyl)phenolato]zinc(II) (abbreviation: ZnBTZ), as well as organic compounds having a π-electron-deficient heteroaromatic ring. Examples of organic compounds having a π-electron-deficient heteroaromatic ring skeleton include organic compounds having a heteroaromatic ring with a polyazole skeleton, organic compounds having a heteroaromatic ring with a pyridine skeleton, organic compounds having a heteroaromatic ring with a diazine skeleton, and organic compounds having a heteroaromatic ring with a triazine skeleton.

[0249] Among these, organic compounds containing a heteroaromatic ring having a diazine skeleton (pyrimidine skeleton, pyrazine skeleton, pyridazine skeleton), organic compounds containing a heteroaromatic ring having a pyridine skeleton, and organic compounds containing a heteroaromatic ring having a triazine skeleton are preferred because of their high reliability. In particular, organic compounds containing a heteroaromatic ring having a diazine (pyrimidine or pyrazine) skeleton and organic compounds containing a heteroaromatic ring having a triazine skeleton have high electron transport properties and contribute to reducing driving voltage. In addition, benzofuropyrimidine skeletons, benzothienopyrimidine skeletons, benzofuropyrazine skeletons, and benzothienopyrazine skeletons are preferred because of their high electron acceptor properties and high reliability.

[0250] Examples of organic compounds having a π-electron-deficient heteroaromatic ring skeleton include 2-(4-biphenylyl)-5-(4-tert-butylphenyl)-1,3,4-oxadiazole (abbreviation: PBD), 3-(4-biphenylyl)-4-phenyl-5-(4-tert-butylphenyl)-1,2,4-triazole (abbreviation: TAZ), 1,3-bis[5-(p-tert-butylphenyl)-1,3,4-oxadiazol-2-yl]benzene (abbreviation: OXD-7), 9-[4-(5-phenyl-1,3,4-oxadiazole- organic compounds having an azole skeleton, such as 2,2',2''-(1,3,5-benzenetriyl)tris(1-phenyl-1H-benzimidazole) (abbreviation: TPBI), 2-[3-(dibenzothiophen-4-yl)phenyl]-1-phenyl-1H-benzimidazole (abbreviation: mDBTBIm-II), and 4,4'-bis(5-methylbenzoxazol-2-yl)stilbene (abbreviation: BzOs); )phenyl]pyridine (abbreviation: 35DCzPPy), 1,3,5-tri[3-(3-pyridyl)phenyl]benzene (abbreviation: TmPyPB), bathophenanthroline (abbreviation: Bphen), bathocuproine (abbreviation: BCP), 2,9-di(naphthalen-2-yl)-4,7-diphenyl-1,10-phenanthroline (abbreviation: NBphen), 2,2'-(1,3-phenylene)bis(9-phenyl-1,10-phenanthroline) (abbreviation: mPPhen2P), 2-[3-(2-triphenylenyl)phenyl]-1,10 organic compounds containing a heteroaromatic ring having a pyridine skeleton, such as 2-[3-(dibenzothiophen-4-yl)phenyl]dibenzo[f,h]quinoxaline (abbreviation: 2mDBTPDBq-II), 2-[3-(3'-dibenzothiophen-4-yl)biphenyl]dibenzo[f,h]quinoxaline (abbreviation: 2mDBTBPDBq-II), 2-[3'-(9H-carbazol-9-yl)biphenyl-3-yl]dibenzo[f,h]quinoxaline (abbreviation: 2mCzBPDBq), 2-[4'-(9-phenyl-9H-carbazol-3-yl)-3,1'-biphenyl-1-yl]dibenzo[f,h]quinoxaline (abbreviation: 2mpPCBPDBq), 2-[4-(3,6-diphenyl-9H- carbazol-9-yl)phenyl]dibenzo[f,h]quinoxaline (abbreviation: 2CzPDBq-III), 7-[3-(dibenzothiophen-4-yl)phenyl]dibenzo[f,h]quinoxaline (abbreviation: 7mDBTPDBq-II), and 6-[3-(dibenzothiophen-4-yl)phenyl]dibenzo[f,h]quinoxaline (abbreviation: 6mDBTPDBq-II), 9-[3'-(dibenzothiophen-4-yl)biphenyl-3-yl]naphtho[1',2':4,5]furo[2,3-b]pyrazine (abbreviation: 9mDBtBPNfpr), 9-[ (3'-dibenzothiophen-4-yl)biphenyl-4-yl]naphtho[1',2':4,5]furo[2,3-b]pyrazine (abbreviation: 9pmDBtBPNfpr), 4,6-bis[3-(phenanthrene-9-yl)phenyl]pyrimidine (abbreviation: 4,6mPnP2Pm), 4,6-bis[3-(4-dibenzothienyl)phenyl]pyrimidine (abbreviation: 4,6mDBTP2Pm-II), 4,6-bis[3-(9H-carbazol-9-yl)phenyl]pyrimidine (abbreviation: 4,6mCzP2Pm), 9,9'-[pyrimidine-4,6-diylbis(biphenyl)] phenyl-3,3'-diyl)]bis(9H-carbazole) (abbreviation: 4,6mCzBP2Pm), 8-(biphenyl-4-yl)-4-[3-(dibenzothiophen-4-yl)phenyl]-[1]benzofuro[3,2-d]pyrimidine (abbreviation: 8BP-4mDBtPBfpm), 3,8-bis[3-(dibenzothiophen-4-yl)phenyl]benzofuro[2,3-b]pyrazine (abbreviation: 3,8mDBtP2Bfpr), 4,8-bis[3-(dibenzothiophen-4-yl)phenyl]-[1]benzofuro[3,2-d]pyrimidine (abbreviation: 4,8mDBtP2Bfpm), 8-[3'-(dibenzothiophen-4-yl)biphenyl-3-yl]naphtho[1',2':4,5]furo[3,2-d]pyrimidine (abbreviation: 8mDBtBPNfpm), 8-[(2,2'-binaphthalen)-6-yl]-4-[3-(dibenzothiophen-4-yl)phenyl]-[1]benzofuro[3,2-d]pyrimidine (abbreviation: 8(βN2)-4mDBtPBfpm), 2,2'-(pyridine-2,6-diyl)bis(4-phenylbenzo[h]quinazoline) (abbreviation: 2,6(P-Bqn)2Py), 2,2'-(pyridine-2,6-diyl)bis{4-[4-(2-naphthyl)phenyl]-6-phenylpyrimidine} (abbreviation: 2,6(NP-PPm)2Py), 6-(biphenyl-3-yl)-4-[3,5-bis(9H-carbazol-9-yl)phenyl]-2-phenylpyrimidine (abbreviation: 6mBP-4Cz2PPm), 2,6-bis(4-naphthalen-1-ylphenyl)-4-[4-(3-pyridyl)phenyl]pyrimidine (abbreviation: 2,4NP-6PyPPm), 4-[3,5-bis(9H-carbazol-9-yl)phenyl ]-2-phenyl-6-(biphenyl-4-yl)pyrimidine (abbreviation: 6BP-4Cz2PPm), 7-[4-(9-phenyl-9H-carbazol-2-yl)quinazolin-2-yl]-7H-dibenzo[c,g]carbazole (abbreviation: PC-cgDBCzQz), organic compounds having a diazine skeleton such as 2-(biphenyl-4-yl)-4-phenyl-6-(9,9'-spirobi[9H-fluoren]-2-yl)-1,3,5-triazine (abbreviation: BP-SFTzn), 2-{3-[3-(benzo[b]naphtho[1,2-d]furan- 8-yl)phenyl]phenyl}-4,6-diphenyl-1,3,5-triazine (abbreviation: mBnfBPTzn), 2-{3-[3-(benzo[b]naphtho[1,2-d]furan-6-yl)phenyl]phenyl}-4,6-diphenyl-1,3,5-triazine (abbreviation: mBnfBPTzn-02), 2-{4-[3-(N-phenyl-9H-carbazol-3-yl)-9H-carbazol-9-yl]phenyl}-4,6-diphenyl-1,3,5-triazine (abbreviation: PCCzPTzn), 9-[3-(4,6-diphenyl-1,3,5-triazin-2-yl)phenyl]-9'-phenyl-2,3'-bi-9H-carbazole (abbreviation: mPCCzPTzn-02), 2-[3'-(9,9-dimethyl-9H-fluoren-2-yl)biphenyl-3-yl]-4,6-diphenyl-1,3,5-triazine (abbreviation: mFBPTzn), 5-[3-(4,6-diphenyl-1,3,5-triazin-2-yl)phenyl]-7,7-dimethyl-5H,7H-indeno[2,1-b]carbazole carbazole (abbreviation: mINc(II)PTzn), 2-{3-[3-(dibenzothiophen-4-yl)phenyl]phenyl}-4,6-diphenyl-1,3,5-triazine (abbreviation: mDBtBPTzn), 2,4,6-tris[3'-(pyridin-3-yl)biphenyl-3-yl]-1,3,5-triazine (abbreviation: TmPPPyTz), 2-[3-(2,6-dimethyl-3-pyridinyl)-5-(9-phenanthrenyl)phenyl]-4,6- Diphenyl-1,3,5-triazine (abbreviation: mPn-mDMePyPTzn), 11-[4-(biphenyl-4-yl)-6-phenyl-1,3,5-triazin-2-yl]-11,12-dihydro-12-phenylindolo[2,3-a]carbazole (abbreviation: BP-Icz(II)Tzn), 2-[3'-(triphenylen-2-yl)biphenyl-3-yl]-4,6-diphenyl-1,3,5-triazine (abbreviation: mTpBPTzn), 3 Examples of suitable organic compounds include organic compounds containing a heteroaromatic ring with a triazine skeleton, such as 2-(biphenyl-3-yl)-4-phenyl-6-{8-[(1,1':4',1''-terphenyl)-4-yl]-1-dibenzofuranyl}-1,3,5-triazine (mBP-TPDBfTzn). Organic compounds containing a heteroaromatic ring with a diazine skeleton, organic compounds containing a heteroaromatic ring with a pyridine skeleton, and organic compounds containing a heteroaromatic ring with a triazine skeleton are preferred due to their high reliability. In particular, organic compounds containing a heteroaromatic ring with a diazine (pyrimidine or pyrazine) skeleton and organic compounds containing a heteroaromatic ring with a triazine skeleton have high electron transport properties and contribute to reduced driving voltage.

[0251] The TADF materials that can be used as the host material can be the same as those listed above. When a TADF material is used as a host material, triplet excitation energy generated in the TADF material is converted into singlet excitation energy by reverse intersystem crossing, and the energy is further transferred to a light-emitting substance, thereby improving the luminous efficiency of the light-emitting device. In this case, the TADF material functions as an energy donor, and the light-emitting substance functions as an energy acceptor.

[0252] This is very effective when the luminescent material is a fluorescent luminescent material. 1 The level is the S of the fluorescent material. 1 It is preferable that the T of the TADF material is higher than the T level. 1 The level is the S of the fluorescent material. 1 Therefore, the T 1 The level is the T 1 It is preferable that the level is higher.

[0253] It is also preferable to use a TADF material that emits light that overlaps with the wavelength of the lowest-energy absorption band of the fluorescent material, since this allows for smooth transfer of excitation energy from the TADF material to the fluorescent material, resulting in efficient light emission.

[0254] Furthermore, in order to efficiently generate singlet excitation energy from triplet excitation energy through reverse intersystem crossing, it is preferable that carrier recombination occurs in the TADF material. It is also preferable that the triplet excitation energy generated in the TADF material does not transfer to the triplet excitation energy of the fluorescent material. To this end, it is preferable that the fluorescent material has a protecting group around the luminophore (the skeleton responsible for light emission) possessed by the fluorescent material. The protecting group is preferably a substituent without a π bond, and is preferably a saturated hydrocarbon. Specific examples include alkyl groups having 3 to 10 carbon atoms, substituted or unsubstituted cycloalkyl groups having 3 to 10 carbon atoms, and trialkylsilyl groups having 3 to 10 carbon atoms. It is even more preferable that the protecting group has multiple protecting groups. Substituents without a π bond have poor carrier transport function, so the distance between the TADF material and the luminophore of the fluorescent material can be increased without significantly affecting carrier transport or carrier recombination. Here, the luminophore refers to the atomic group (skeleton) responsible for light emission in the fluorescent material. The luminophore preferably has a skeleton having a π bond, preferably contains an aromatic ring, and preferably has a fused aromatic ring or a fused heteroaromatic ring. Examples of such luminophores include a phenanthrene skeleton, a stilbene skeleton, an acridone skeleton, a phenoxazine skeleton, a phenothiazine skeleton, a naphthalene skeleton, an anthracene skeleton, a fluorene skeleton, a chrysene skeleton, a triphenylene skeleton, a tetracene skeleton, a pyrene skeleton, a perylene skeleton, a coumarin skeleton, a quinacridone skeleton, and a naphthobisbenzofuran skeleton. In particular, fluorescent materials having a naphthalene skeleton, an anthracene skeleton, a fluorene skeleton, a chrysene skeleton, a triphenylene skeleton, a tetracene skeleton, a pyrene skeleton, a perylene skeleton, a coumarin skeleton, a quinacridone skeleton, or a naphthobisbenzofuran skeleton are preferred because of their high fluorescence quantum yield.

[0255] When a fluorescent light-emitting substance is used as the light-emitting substance, a material having an anthracene skeleton is suitable as the host material. Using a substance having an anthracene skeleton as a host material for a fluorescent light-emitting substance makes it possible to realize an emitting layer with both excellent luminous efficiency and durability. As a substance having an anthracene skeleton used as a host material, a diphenylanthracene skeleton, particularly a 9,10-diphenylanthracene skeleton, is preferred because it is chemically stable. Furthermore, a host material having a carbazole skeleton is preferred because it enhances hole injection and transport properties. However, a host material containing a benzocarbazole skeleton in which a benzene ring is further condensed to the carbazole skeleton is more preferred because its HOMO level is about 0.1 eV shallower than that of a host material having a carbazole skeleton, making it easier for holes to enter. In particular, a host material containing a dibenzocarbazole skeleton is preferred because its HOMO level is about 0.1 eV shallower than that of a host material having a carbazole skeleton, making it easier for holes to enter, and it also has excellent hole transport properties and high heat resistance. Therefore, a more preferable host material is a substance having both a 9,10-diphenylanthracene skeleton and a carbazole skeleton (or a benzocarbazole skeleton or a dibenzocarbazole skeleton). Note that, in view of the hole injection / transport property, a benzofluorene skeleton or a dibenzofluorene skeleton may be used instead of the carbazole skeleton.Examples of such substances include 9-phenyl-3-[4-(10-phenyl-9-anthryl)phenyl]-9H-carbazole (abbreviation: PCzPA), 3-[4-(1-naphthyl)phenyl]-9-phenyl-9H-carbazole (abbreviation: PCPN), 9-[4-(10-phenyl-9-anthracenyl)phenyl]-9H-carbazole (abbreviation: CzPA), 7-[4-(10-phenyl-9-anthryl)phenyl]-7H-dibenzo[c,g]carbazole (abbreviation: cgDBCzPA), 6-[3-(9,10-diphenyl-2-anthryl)phenyl]benzo[b]naphtho[1,2-d]furan (abbreviation: 2mBnfPPA), 9-phenyl-10-[4-(9-phenyl-9H-fluoren-9-yl)biphenyl-4′- 9-(1-naphthyl)-10-[4-(2-naphthyl)phenyl]anthracene (abbreviation: αN-βNPAnth), 9-(1-naphthyl)-10-(2-naphthyl)anthracene (abbreviation: α,βADN), 2-(10-phenylanthracen-9-yl)dibenzofuran, 2-(10-phenyl-9-anthracenyl)benzo Examples include zo[b]naphtho[2,3-d]furan (abbreviation: Bnf(II)PhA), 9-(2-naphthyl)-10-[3-(2-naphthyl)phenyl]anthracene (abbreviation: βN-mβNPAnth), 1-{4-[10-(biphenyl-4-yl)-9-anthracenyl]phenyl}-2-ethyl-1H-benzimidazole (abbreviation: EtBImPBPhA), etc. In particular, CzPA, cgDBCzPA, 2mBnfPPA, and PCzPA are preferred choices because they exhibit very good properties.

[0256] The host material may be a mixture of a plurality of substances. When a mixture of host materials is used, it is preferable to mix a material having electron transport properties with a material having hole transport properties. By mixing a material having electron transport properties with a material having hole transport properties, the transport properties of the light-emitting layer 113 can be easily adjusted, and the recombination region can also be easily controlled. The weight ratio of the content of the material having hole transport properties to the material having electron transport properties may be 1:19 to 19:1 (material having hole transport properties:material having electron transport properties).

[0257] A phosphorescent material can be used as part of the mixed material. The phosphorescent material can be used as an energy donor that provides excitation energy to a fluorescent material when the fluorescent material is used as a light-emitting material.

[0258] Furthermore, these mixed materials may form an exciplex. It is preferable to select a combination that forms an exciplex that emits light that overlaps with the wavelength of the lowest-energy absorption band of the light-emitting material, because this allows for smooth energy transfer and efficient light emission. Furthermore, using this structure is also preferable because it reduces the driving voltage.

[0259] At least one of the materials forming the exciplex may be a phosphorescent material, which allows efficient conversion of triplet excitation energy into singlet excitation energy through reverse intersystem crossing.

[0260] As a combination of materials that efficiently form an exciplex, it is preferable that the HOMO level of the material having hole transport properties is equal to or higher than the HOMO level of the material having electron transport properties. Also, it is preferable that the LUMO level of the material having hole transport properties is equal to or higher than the LUMO level of the material having electron transport properties. Note that the LUMO level and HOMO level of the material can be derived from the electrochemical properties (reduction potential and oxidation potential) of the material measured by cyclic voltammetry (CV).

[0261] The formation of exciplexes can be confirmed, for example, by comparing the emission spectra of a material having hole transport properties, a material having electron transport properties, and a mixed film obtained by mixing these materials, and observing the phenomenon in which the emission spectrum of the mixed film is shifted to longer wavelengths than the emission spectra of each material (or has a new peak on the longer wavelength side). Alternatively, the formation of exciplexes can be confirmed by comparing the transient photoluminescence (PL) of a material having hole transport properties, the transient PL of a material having electron transport properties, and a mixed film obtained by mixing these materials, and observing differences in transient response, such as the transient PL lifetime of the mixed film having a longer-lifetime component or a larger proportion of delayed components than the transient PL lifetimes of the individual materials. The above-mentioned transient PL may also be interpreted as transient electroluminescence (EL). In other words, the formation of exciplexes can also be confirmed by comparing the transient EL of a material having hole transport properties, the transient EL of a material having electron transport properties, and a mixed film obtained by mixing these materials, and observing the differences in transient response.

[0262] The electron transport layer 114 is a layer containing a substance having an electron transport property. The material having an electron transport property is a material having an electron mobility of 1×10 or less at a square root of an electric field strength [V / cm] of 600. −7 cm 2 / Vs or more, preferably 1×10 −6 cm 2 A substance having an electron mobility of 1 / Vs or more is preferred. Note that, other substances can be used as long as they have a higher electron transporting property than holes. Note that, as the organic compound, an organic compound having a π-electron-deficient heteroaromatic ring is preferred. As the organic compound having a π-electron-deficient heteroaromatic ring, for example, one or more of an organic compound including a heteroaromatic ring having a polyazole skeleton, an organic compound including a heteroaromatic ring having a pyridine skeleton, an organic compound including a heteroaromatic ring having a diazine skeleton, and an organic compound including a heteroaromatic ring having a triazine skeleton are preferred.

[0263] As the organic compound having electron transport properties that can be used in the electron transport layer 114, the same organic compounds that can be used as the organic compound having electron transport properties in the light-emitting layer 113 can be used. Among them, organic compounds containing a heteroaromatic ring having a diazine skeleton, organic compounds containing a heteroaromatic ring having a pyridine skeleton, and organic compounds containing a heteroaromatic ring having a triazine skeleton are preferred because of their high reliability. In particular, organic compounds containing a heteroaromatic ring having a diazine (pyrimidine or pyrazine) skeleton and organic compounds containing a heteroaromatic ring having a triazine skeleton have high electron transport properties and contribute to reduced driving voltage. Among them, organic compounds having a phenanthroline skeleton, such as mTpPPhen, PnNPhen, and mPPhen2P, are preferred, and organic compounds having a phenanthroline dimer structure, such as mPPhen2P, are more preferred because of their excellent stability.

[0264] The electron transport layer 114 is preferably a bipolar layer, i.e., a layer with relatively high hole transport properties. Therefore, the HOMO level of the organic compound contained in the electron transport layer 114 is preferably −5.90 eV or more and −5.00 eV or less, preferably −5.80 eV or more and −5.00 eV or less, and more preferably −5.70 eV or more and −5.15 eV or less. Furthermore, since good electron transport properties are also required, the LUMO level of the organic compound contained in the first electron transport layer is preferably −3.15 eV or more and −2.50 eV or less, and more preferably −3.00 eV or more and −2.70 eV or less.

[0265] The electron transport layer 114 may be a layer composed of a plurality of organic compounds. When the first electron transport layer contains a plurality of organic compounds, it is preferable that the HOMO level of the organic compound having the highest HOMO level falls within the above-described range. When the first electron transport layer contains a plurality of organic compounds, it is preferable that the LUMO level of the organic compound having the lowest LUMO level falls within the above-described range. When the first electron transport layer contains a plurality of organic compounds, it is preferable that at least one of the organic compounds has an electron-transporting property and at least one of the organic compounds has a hole-transporting property.

[0266] It is preferable that the electron-transporting organic compound and the hole-transporting organic compound are the same organic compound, that is, it is more preferable that the first electron-transporting layer contains an organic compound having both electron-transporting and hole-transporting properties, because this makes it easier to obtain a light-emitting device with good characteristics.

[0267] An organic compound having electron transport properties or an organic compound having both electron transport properties and hole transport properties has an electron mobility of 1×10 at a square root of an electric field strength [V / cm] of 600. −7 cm 2 / Vs or more, preferably 1×10 −6 cm 2 In addition, a hole-transporting organic compound or an organic compound having both an electron-transporting property and a hole-transporting property preferably has a hole mobility of 1×10 / Vs or more at a square root of an electric field strength [V / cm] of 600. −7 cm 2 / Vs or more, preferably 1×10 −6 cm 2 A substance having a hole mobility of 1 / Vs or more is preferred.

[0268] The first electron transport layer preferably contains an organic compound having an acid dissociation constant pKa of 4 or less and having electron transport properties.

[0269] The first electron transport layer preferably contains an organic compound having an electron-transporting skeleton and an organic compound having a hole-transporting skeleton. Note that the organic compound having the electron-transporting skeleton and the organic compound having the hole-transporting skeleton are preferably the same organic compound. That is, it is more preferable that the first electron transport layer contains an organic compound having both an electron-transporting skeleton and a hole-transporting skeleton, because this makes it easier to obtain a light-emitting device with good characteristics.

[0270] Note that the electron transport layer 114 may have a stacked structure. When the electron transport layer 114 has a stacked structure, it is preferable that all of the stacked layers have the structure described in Embodiment 1. When the electron transport layer 114 has a stacked structure, a layer in contact with the light-emitting layer 113 may function as a hole-blocking layer. When the electron transport layer in contact with the light-emitting layer is made to function as a hole-blocking layer, it is preferable to use a material whose HOMO level is 0.5 eV or more deeper than the HOMO level of a material contained in the light-emitting layer.

[0271] Between the electron transport layer 114 and the second electrode 102, an electron injection layer 115 containing lithium oxide (Li 2 O), lithium fluoride (LiF), cesium fluoride (CsF), calcium fluoride (CaF 2 Alternatively, a layer containing an alkali metal or alkaline earth metal, such as (8-quinolinolato)lithium (abbreviation: Liq), or a compound thereof may be provided. The electron-injection layer 115 may be a layer made of a substance having an electron-transporting property containing an alkali metal or alkaline earth metal, or a compound thereof, or may be an electride. Examples of the electride include a mixed oxide of calcium and aluminum to which electrons are added at a high concentration. The organic compounds listed as strong basic organic compounds in Embodiment 1 may also be used.

[0272] The electron-injecting layer 115 may be formed by using any of the above substances alone, or by using a layer made of a substance having an electron-transporting property containing any of the above substances.

[0273] Note that a layer containing a substance having an electron transport property (preferably an organic compound having a bipyridine skeleton) containing a fluoride of the alkali metal or alkaline earth metal at a concentration (50 wt % or more) that results in a microcrystalline state can also be used as the electron-injection layer 115. Since this layer has a low refractive index, it is possible to provide a light-emitting device with better external quantum efficiency.

[0274] The second electrode 102 is an electrode including a cathode. The second electrode 102 may have a laminated structure, in which case the layer in contact with the organic compound layer 103 functions as the cathode. Materials that form the cathode include metals, alloys, electrically conductive compounds, and mixtures thereof, each having a small work function (specifically, 3.8 eV or less). Specific examples of such cathode materials include alkali metals such as lithium (Li) or cesium (Cs), elements belonging to Group 1 or Group 2 of the periodic table such as magnesium (Mg), calcium (Ca), and strontium (Sr), and alloys (MgAg, AlLi) and compounds (lithium fluoride (LiF), cesium fluoride (CsF), calcium fluoride (CaF), etc.) containing these elements. 2 However, by providing the electron injection layer 115 or a thin film of the above-mentioned material having a small work function between the second electrode 102 and the electron transport layer, various conductive materials such as Al, Ag, ITO, indium oxide-tin oxide containing silicon or silicon oxide can be used as the cathode regardless of the magnitude of the work function.

[0275] In addition, when the second electrode 102 is formed using a material that is transparent to visible light, a light-emitting device can be formed that emits light from the second electrode 102 side, and when the first electrode 101 is formed using a material that is transparent to visible light, a light-emitting device can be formed that emits light from the first electrode 101 side.

[0276] These conductive materials can be formed into films by dry methods such as vacuum deposition or sputtering, inkjet methods, spin coating methods, etc. Alternatively, they may be formed by wet methods using a sol-gel method, or by wet methods using a paste of a metal material.

[0277] In addition, various methods, whether dry or wet, can be used to form the organic compound layer 103. For example, vacuum deposition, gravure printing, offset printing, screen printing, inkjet printing, spin coating, or the like may be used.

[0278] Furthermore, the above-mentioned electrodes or layers may be formed using different film formation methods.

[0279] The configuration of the layer provided between the anode and cathode is not limited to the above, but a configuration in which the light-emitting region where holes and electrons recombine is provided at a location away from the anode and cathode is preferred so as to suppress quenching caused by the proximity of the light-emitting region to the electrodes and the metal used in the carrier injection layer.

[0280] Furthermore, the hole transport layer and electron transport layer in contact with the light-emitting layer 113, and particularly the carrier transport layer close to the recombination region in the light-emitting layer 113, are preferably made of a substance having a band gap larger than the band gap of the light-emitting material constituting the light-emitting layer or the light-emitting material contained in the light-emitting layer, in order to suppress energy transfer from excitons generated in the light-emitting layer.

[0281] Note that the structure of this embodiment mode can be used in appropriate combination with structures of other embodiments.

[0282] Embodiment 5 In this embodiment, a display device according to one embodiment of the present invention will be described.

[0283] The display device of the present embodiment can be a high-definition display device, and can therefore be used, for example, as a display unit for a wristwatch-type or bracelet-type information terminal (wearable device), as well as a display unit for a wearable device that can be worn on the head, such as a head-mounted display (HMD) for VR, or a glasses-type device for AR.

[0284] The display device of the present embodiment can be a high-resolution display device or a large-sized display device. Therefore, the display device of the present embodiment can be used in electronic devices having relatively large screens, such as television devices, desktop or notebook personal computers, computer monitors, digital signage, and large game machines such as pachinko machines, as well as in the display units of digital cameras, digital video cameras, digital photo frames, mobile phones, portable game machines, personal digital assistants, and sound reproducing devices.

[0285] 14A shows a perspective view of display module 280. Display module 280 has display device 100A and FPC 290. Note that the display device included in display module 280 is not limited to display device 100A, and may be either display device 100B or display device 100E, which will be described later.

[0286] The display module 280 has a substrate 291 and a substrate 292. The display module 280 has a display portion 281. The display portion 281 is a region that displays an image in the display module 280, and is a region where light from each pixel provided in a pixel portion 284 (described later) can be viewed.

[0287] 14B is a perspective view schematically illustrating the configuration on the substrate 291 side. A circuit portion 282, a pixel circuit portion 283 on the circuit portion 282, and a pixel portion 284 on the pixel circuit portion 283 are stacked on the substrate 291. A terminal portion 285 for connecting to the FPC 290 is provided in a portion of the substrate 291 that does not overlap with the pixel portion 284. The terminal portion 285 and the circuit portion 282 are electrically connected by a wiring portion 286 composed of a plurality of wirings.

[0288] The pixel section 284 has a plurality of periodically arranged pixels 284a. An enlarged view of one pixel 284a is shown on the right side of Fig. 14B. The various configurations described in the previous embodiments can be applied to the pixel 284a. Fig. 14B shows an example in which the pixel 284a has the same configuration as the pixel 178 shown in Fig. 7.

[0289] The pixel circuit section 283 has a plurality of pixel circuits 283a arranged periodically.

[0290] One pixel circuit 283a is a circuit that controls the driving of a plurality of elements included in one pixel 284a.

[0291] The circuit portion 282 includes a circuit for driving each pixel circuit 283 a of the pixel circuit portion 283. For example, the circuit portion 282 preferably includes one or both of a gate line driver circuit and a source line driver circuit. In addition, the circuit portion 282 may include at least one of an arithmetic circuit, a memory circuit, a power supply circuit, and the like.

[0292] The FPC 290 functions as wiring for supplying a video signal, a power supply potential, or the like from the outside to the circuit portion 282. An IC may be mounted on the FPC 290.

[0293] The display module 280 can be configured such that one or both of the pixel circuit unit 283 and the circuit unit 282 are stacked below the pixel unit 284, thereby making it possible to extremely increase the aperture ratio (effective display area ratio) of the display unit 281.

[0294] Because such a display module 280 has extremely high resolution, it can be suitably used in VR devices such as HMDs or eyeglass-type AR devices. For example, even in a configuration in which the display unit of the display module 280 is viewed through lenses, the display module 280 has an extremely high-resolution display unit 281, so that even if the display unit is enlarged with the lens, the pixels are not visible, allowing for a highly immersive display. Furthermore, the display module 280 is not limited to this, and can be suitably used in electronic devices having relatively small display units.

[0295] Display Device 100A The display device 100A shown in FIG. 15A includes a substrate 301, a light-emitting device 130R, a light-emitting device 130G, a light-emitting device 130B, a capacitor 240, and a transistor 310.

[0296] The substrate 301 corresponds to the substrate 291 in FIGS. 14A and 14B . The transistor 310 is a transistor having a channel formation region in the substrate 301. The substrate 301 can be, for example, a semiconductor substrate such as a single crystal silicon substrate. The transistor 310 includes a part of the substrate 301, a conductive layer 311, a low-resistance region 312, an insulating layer 313, and an insulating layer 314. The conductive layer 311 functions as a gate electrode. The insulating layer 313 is located between the substrate 301 and the conductive layer 311 and functions as a gate insulating layer. The low-resistance region 312 is a region in which the substrate 301 is doped with impurities and functions as a source or drain. The insulating layer 314 is provided to cover a side surface of the conductive layer 311.

[0297] An element isolation layer 315 is provided between two adjacent transistors 310 so as to be embedded in the substrate 301 .

[0298] In addition, an insulating layer 261 is provided to cover the transistor 310 , and a capacitor 240 is provided over the insulating layer 261 .

[0299] The capacitor 240 has a conductive layer 241, a conductive layer 245, and an insulating layer 243 located therebetween. The conductive layer 241 functions as one electrode of the capacitor 240, the conductive layer 245 functions as the other electrode of the capacitor 240, and the insulating layer 243 functions as a dielectric of the capacitor 240.

[0300] The conductive layer 241 is provided over the insulating layer 261 and is buried in the insulating layer 254. The conductive layer 241 is electrically connected to one of the source and the drain of the transistor 310 by a plug 271 buried in the insulating layer 261. The insulating layer 243 is provided to cover the conductive layer 241. The conductive layer 245 is provided in a region overlapping with the conductive layer 241 with the insulating layer 243 interposed therebetween.

[0301] An insulating layer 255 is provided to cover the capacitor 240, an insulating layer 174 is provided on the insulating layer 255, and an insulating layer 175 is provided on the insulating layer 174. Light-emitting device 130R, light-emitting device 130G, and light-emitting device 130B are provided on the insulating layer 175. An insulator is provided in the region between adjacent light-emitting devices.

[0302] An insulating layer 156R is provided to have a region overlapping with a side surface of the conductive layer 151R, an insulating layer 156G is provided to have a region overlapping with a side surface of the conductive layer 151G, and an insulating layer 156B is provided to have a region overlapping with a side surface of the conductive layer 151B. Furthermore, a conductive layer 152R is provided to cover the conductive layer 151R and the insulating layer 156R, a conductive layer 152G is provided to cover the conductive layer 151G and the insulating layer 156G, and a conductive layer 152B is provided to cover the conductive layer 151B and the insulating layer 156B. A protective layer 158R is located on the organic compound layer 103R, a protective layer 158G is located on the organic compound layer 103G, and a protective layer 158B is located on the organic compound layer 103B.

[0303] The conductive layer 151R, the conductive layer 151G, and the conductive layer 151B are electrically connected to one of the source and the drain of the transistor 310 by an insulating layer 243, an insulating layer 255, an insulating layer 174, a plug 256 embedded in the insulating layer 175, a conductive layer 241 embedded in the insulating layer 254, and a plug 271 embedded in the insulating layer 261. Various conductive materials can be used for the plugs.

[0304] Furthermore, a protective layer 131 is provided on the light-emitting devices 130R, 130G, and 130B. A substrate 120 is bonded to the protective layer 131 with a resin layer 122. For details of the components from the light-emitting device 130 to the substrate 120, refer to embodiment 3. The substrate 120 corresponds to the substrate 292 in FIG. 14A .

[0305] Fig. 15B is a modified example of the display device 100A shown in Fig. 15A. The display device shown in Fig. 15B has a colored layer 132R, a colored layer 132G, and a colored layer 132B, and the light-emitting device 130 has an area where it overlaps with one of the colored layers 132R, 132G, and 132B. In the display device shown in Fig. 15B, the light-emitting device 130 can emit, for example, white light. Furthermore, for example, the colored layer 132R can transmit red light, the colored layer 132G can transmit green light, and the colored layer 132B can transmit blue light.

[0306] [Display Device 100B] FIG. 16 shows a perspective view of the display device 100B, and FIG. 17 shows a cross-sectional view of the display device 100B.

[0307] The display device 100B has a configuration in which a substrate 352 and a substrate 351 are bonded together. In Fig. 16, the substrate 352 is indicated by a dashed line.

[0308] The display device 100B includes a pixel portion 177, a connection portion 140, a circuit 356, wiring 355, and the like. Fig. 16 shows an example in which an IC 354 and an FPC 353 are mounted on the display device 100B. Therefore, the configuration shown in Fig. 16 can also be called a display module including the display device 100B, an IC (integrated circuit), and an FPC. Here, a display device in which a connector such as an FPC is attached to a substrate or a display device in which an IC is mounted on the substrate is called a display module.

[0309] The connection portion 140 is provided outside the pixel portion 177. There may be one or more connection portions 140. The connection portion 140 electrically connects the common electrode of the light-emitting device and the conductive layer, and can supply a potential to the common electrode.

[0310] The circuit 356 can be, for example, a scanning line driver circuit.

[0311] The wiring 355 has a function of supplying signals and power to the pixel portion 177 and the circuit 356. The signals and power are input to the wiring 355 from the outside via the FPC 353 or from the IC 354.

[0312] 16 shows an example in which an IC 354 is provided on a substrate 351 by a chip-on-glass (COG) method, a chip-on-film (COF) method, or the like. The IC 354 can be, for example, an IC having a scanning line driver circuit or a signal line driver circuit. The display device 100B and the display module may not include an IC. Alternatively, the IC may be mounted on an FPC by a COF method, for example.

[0313] Figure 17 shows an example of a cross section of the display device 100B, where a portion of the region including the FPC 353, a portion of the circuit 356, a portion of the pixel portion 177, a portion of the connection portion 140, and a portion of the region including the end portion are cut.

[0314] [Display Device 100C] The display device 100C shown in Figure 17 has, between a substrate 351 and a substrate 352, a transistor 201, a transistor 205, a light-emitting device 130R that emits red light, a light-emitting device 130G that emits green light, and a light-emitting device 130B that emits blue light.

[0315] For details of the light emitting device 130R, the light emitting device 130G, and the light emitting device 130B, refer to the first to third embodiments.

[0316] Light-emitting device 130R has conductive layer 224R, conductive layer 151R on conductive layer 224R, and conductive layer 152R on conductive layer 151R. Light-emitting device 130G has conductive layer 224G, conductive layer 151G on conductive layer 224G, and conductive layer 152G on conductive layer 151G. Light-emitting device 130B has conductive layer 224B, conductive layer 151B on conductive layer 224B, and conductive layer 152B on conductive layer 151B.

[0317] The conductive layer 224R is connected to the conductive layer 222b of the transistor 205 through an opening provided in the insulating layer 214. An end of the conductive layer 151R is located outside an end of the conductive layer 224R. An insulating layer 156R is provided to have a region in contact with the side surface of the conductive layer 151R, and a conductive layer 152R is provided to cover the conductive layer 151R and the insulating layer 156R.

[0318] Conductive layer 224G, conductive layer 151G, conductive layer 152G, and insulating layer 156G in light-emitting device 130G, and conductive layer 224B, conductive layer 151B, conductive layer 152B, and insulating layer 156B in light-emitting device 130B are similar to conductive layer 224R, conductive layer 151R, conductive layer 152R, and insulating layer 156R in light-emitting device 130R, and therefore detailed description thereof will be omitted.

[0319] Recesses are formed in the conductive layers 224R, 224G, and 224B so as to cover the openings provided in the insulating layer 214. A layer 128 is buried in the recesses.

[0320] The layer 128 has a function of planarizing the recesses of the conductive layer 224R, the conductive layer 224G, and the conductive layer 224B. The conductive layer 151R, the conductive layer 151G, and the conductive layer 151B, which are electrically connected to the conductive layer 224R, the conductive layer 224G, and the conductive layer 224B, are provided on the conductive layer 224R, the conductive layer 224G, and the conductive layer 224B and the layer 128. Therefore, the regions overlapping with the recesses of the conductive layer 224R, the conductive layer 224G, and the conductive layer 224B can also be used as light-emitting regions, thereby increasing the aperture ratio of the pixel.

[0321] The layer 128 may be an insulating layer or a conductive layer. Various inorganic insulating materials, organic insulating materials, and conductive materials can be used as appropriate for the layer 128. In particular, the layer 128 is preferably formed using an insulating material, and more preferably using an organic insulating material. For example, the organic insulating material that can be used for the insulating layer 127 described above can be used for the layer 128.

[0322] A protective layer 131 is provided on the light-emitting device 130R, the light-emitting device 130G, and the light-emitting device 130B. The protective layer 131 and the substrate 352 are bonded via an adhesive layer 142. A light-shielding layer 157 is provided on the substrate 352. A solid sealing structure, a hollow sealing structure, or the like can be applied to seal the light-emitting device 130. In FIG. 17 , the space between the substrate 352 and the substrate 351 is filled with the adhesive layer 142, and a solid sealing structure is applied. Alternatively, the space may be filled with an inert gas (nitrogen, argon, etc.), and a hollow sealing structure may be applied. In this case, the adhesive layer 142 may be provided so as not to overlap with the light-emitting device. Alternatively, the space may be filled with a resin different from the frame-shaped adhesive layer 142.

[0323] 17 shows an example in which the connection portion 140 has a conductive layer 224C obtained by processing the same conductive film as the conductive layers 224R, 224G, and 224B, a conductive layer 151C obtained by processing the same conductive film as the conductive layers 151R, 151G, and 151B, and a conductive layer 152C obtained by processing the same conductive film as the conductive layers 152R, 152G, and 152B. Also, FIG. 17 shows an example in which an insulating layer 156C is provided so as to have a region overlapping with a side surface of the conductive layer 151C.

[0324] The display device 100B is a top-emission type. Light emitted by the light-emitting device is emitted toward the substrate 352. The substrate 352 is preferably made of a material that is highly transparent to visible light. If the light-emitting device emits infrared or near-infrared light, it is preferably made of a material that is highly transparent to such light. The pixel electrode contains a material that reflects visible light, and the counter electrode (common electrode 155) contains a material that transmits visible light.

[0325] An insulating layer 211, an insulating layer 213, an insulating layer 215, and an insulating layer 214 are provided over the substrate 351 in this order. A part of the insulating layer 211 functions as a gate insulating layer for each transistor. A part of the insulating layer 213 functions as a gate insulating layer for each transistor. The insulating layer 215 is provided to cover the transistor. The insulating layer 214 is provided to cover the transistor and functions as a planarization layer. Note that the number of gate insulating layers and the number of insulating layers covering the transistors are not limited, and each may be a single layer or two or more layers.

[0326] The insulating layers 211, 213, and 215 are each preferably formed using an inorganic insulating film.

[0327] The insulating layer 214 that functions as a planarizing layer is preferably an organic insulating layer.

[0328] The transistor 201 and the transistor 205 each include a conductive layer 221 functioning as a gate, an insulating layer 211 functioning as a gate insulating layer, a conductive layer 222a and a conductive layer 222b functioning as a source and a drain, a semiconductor layer 231, an insulating layer 213 functioning as a gate insulating layer, and a conductive layer 223 functioning as a gate.

[0329] A connection portion 204 is provided in a region of the substrate 351 where the substrate 352 does not overlap. In the connection portion 204, a source electrode or a drain electrode of the transistor 201 is electrically connected to the FPC 353 through a conductive layer 166 and a connection layer 242. The conductive layer 166 has an example of a stacked structure including a conductive film obtained by processing the same conductive film as the conductive layers 224R, 224G, and 224B, a conductive film obtained by processing the same conductive film as the conductive layers 151R, 151G, and 151B, and a conductive film obtained by processing the same conductive film as the conductive layers 152R, 152G, and 152B. The conductive layer 166 is exposed on the top surface of the connection portion 204. This allows the connection portion 204 and the FPC 353 to be electrically connected via the connection layer 242.

[0330] It is preferable to provide a light-shielding layer 157 on the surface of the substrate 352 facing the substrate 351. The light-shielding layer 157 can be provided between adjacent light-emitting devices, on the connection section 140, on the circuit 356, etc. In addition, various optical members can be arranged on the outside of the substrate 352.

[0331] The materials that can be used for the substrate 120 can be used for the substrate 351 and the substrate 352 .

[0332] The adhesive layer 142 can be made of a material that can be used for the resin layer 122 .

[0333] The connection layer 242 may be an anisotropic conductive film (ACF), an anisotropic conductive paste (ACP), or the like.

[0334] [Display Device 100D] A display device 100D shown in FIG. 18 differs from the display device 100C shown in FIG. 17 mainly in that it is a bottom-emission display device.

[0335] Light emitted from the light-emitting device is emitted toward the substrate 351. A material that is highly transparent to visible light is preferably used for the substrate 351. On the other hand, the light-transmitting property of the material used for the substrate 352 does not matter.

[0336] It is preferable to form a light-shielding layer between the substrate 351 and the transistor 201 and between the substrate 351 and the transistor 205. Figure 18 shows an example in which a light-shielding layer 157 is provided over the substrate 351, an insulating layer 253 is provided over the light-shielding layer, and the transistors 201, 205, and the like are provided over the insulating layer 253.

[0337] Light emitting device 130R includes conductive layer 112R, conductive layer 126R on conductive layer 112R, and conductive layer 129R on conductive layer 126R.

[0338] Light emitting device 130B includes conductive layer 112B, conductive layer 126B on conductive layer 112B, and conductive layer 129B on conductive layer 126B.

[0339] The conductive layers 112R, 112B, 126R, 126B, 129R, and 129B are made of a material that is highly transparent to visible light. The common electrode 155 is preferably made of a material that reflects visible light.

[0340] Although the light emitting device 130G is not shown in FIG. 18, the light emitting device 130G is also provided.

[0341] Although FIG. 18 and other figures show an example in which the top surface of the layer 128 has a flat portion, the shape of the layer 128 is not particularly limited.

[0342] [Display Device 100E] The display device 100E shown in FIG. 19 is a modification of the display device 100C shown in FIG. 17, and differs from the display device 100C mainly in that it has colored layers 132R, 132G, and 132B.

[0343] In the display device 100E, the light-emitting device 130 has an area that overlaps one of the colored layers 132R, 132G, and 132B. The colored layers 132R, 132G, and 132B can be provided on the surface of the substrate 352 facing the substrate 351. An end of the colored layer 132R, an end of the colored layer 132G, and an end of the colored layer 132B can overlap the light-shielding layer 157.

[0344] In the display device 100E, the light-emitting device 130 can emit, for example, white light. Furthermore, for example, the colored layer 132R can transmit red light, the colored layer 132G can transmit green light, and the colored layer 132B can transmit blue light. The display device 100E may be configured such that the colored layers 132R, 132G, and 132B are provided between the protective layer 131 and the adhesive layer 142.

[0345] 17 and 19 show an example in which the top surface of the layer 128 has a flat portion, but the shape of the layer 128 is not particularly limited.

[0346] This embodiment mode can be combined with other embodiment modes or examples as appropriate. In addition, in this specification, when a plurality of configuration examples are shown in one embodiment mode, the configuration examples can be combined as appropriate.

[0347] Embodiment 6 In this embodiment, an electronic device according to one embodiment of the present invention will be described.

[0348] The electronic devices of this embodiment include the display device of one embodiment of the present invention in their display portions. The display device of one embodiment of the present invention has high display performance and can easily achieve high definition and high resolution. Therefore, the display device of one embodiment of the present invention can be used in the display portions of various electronic devices.

[0349] Examples of electronic devices include electronic devices with relatively large screens such as television sets, desktop or notebook personal computers, computer monitors, digital signage, large game machines such as pachinko machines, as well as digital cameras, digital video cameras, digital photo frames, mobile phones, portable game machines, personal digital assistants, and sound playback devices.

[0350] In particular, the display device of one embodiment of the present invention can have high resolution and can therefore be suitably used in electronic devices having a relatively small display area. Examples of such electronic devices include wristwatch-type and bracelet-type information terminals (wearable devices), and head-mounted wearable devices such as VR devices (e.g., head-mounted displays), AR glasses-type devices, and MR devices.

[0351] The electronic device of this embodiment may have a sensor (including a function to measure force, displacement, position, velocity, acceleration, angular velocity, rotation speed, distance, light, liquid, magnetism, temperature, chemical substance, sound, time, hardness, electric field, current, voltage, power, radiation, flow rate, humidity, gradient, vibration, odor, or infrared rays).

[0352] An example of a wearable device that can be worn on the head will be described with reference to FIGS. 20A to 20D.

[0353] The electronic device 700A shown in FIG. 20A and the electronic device 700B shown in FIG. 20B each have a pair of display panels 751, a pair of housings 721, a communication unit (not shown), a pair of mounting units 723, a control unit (not shown), an imaging unit (not shown), a pair of optical members 753, a frame 757, and a pair of nose pads 758.

[0354] The display device of one embodiment of the present invention can be applied to the display panel 751. Therefore, the electronic device can be highly reliable.

[0355] Each of the electronic device 700A and the electronic device 700B can project an image displayed on the display panel 751 onto a display area 756 of the optical member 753. Because the optical member 753 is translucent, the user can see the image displayed in the display area superimposed on a transmitted image visible through the optical member 753.

[0356] The electronic device 700A and the electronic device 700B may be provided with a camera capable of capturing an image in front of them as an imaging unit. Furthermore, the electronic device 700A and the electronic device 700B may each be provided with an acceleration sensor such as a gyro sensor, thereby detecting the orientation of the user's head and displaying an image corresponding to that orientation in the display area 756.

[0357] The communication unit has a wireless communication device, and can supply, for example, a video signal via the wireless communication device. Note that instead of or in addition to the wireless communication device, a connector to which a cable through which a video signal and a power supply potential can be connected may be provided.

[0358] Furthermore, the electronic device 700A and the electronic device 700B are provided with batteries, which can be charged wirelessly and / or wired.

[0359] The housing 721 may be provided with a touch sensor module.

[0360] Various touch sensors can be used as the touch sensor module. For example, various types of touch sensors can be used, such as a capacitance type, a resistive film type, an infrared type, an electromagnetic induction type, a surface acoustic wave type, or an optical type. In particular, it is preferable to use a capacitance type or an optical type sensor in the touch sensor module.

[0361] The electronic device 800A shown in Figure 20C and the electronic device 800B shown in Figure 20D each have a pair of display units 820, a housing 821, a communication unit 822, a pair of mounting units 823, a control unit 824, a pair of imaging units 825, and a pair of lenses 832.

[0362] The display device of one embodiment of the present invention can be applied to the display portion 820. Therefore, the electronic device can have high reliability.

[0363] The display unit 820 is provided inside the housing 821 at a position that can be viewed through the lens 832. In addition, by displaying different images on the pair of display units 820, it is possible to perform three-dimensional display using parallax.

[0364] It is preferable that electronic device 800A and electronic device 800B each have a mechanism that allows the left and right positions of lens 832 and display unit 820 to be adjusted so that they are optimally positioned according to the position of the user's eyes.

[0365] The mounting portion 823 allows the user to mount the electronic device 800A or the electronic device 800B on the head.

[0366] The imaging unit 825 has a function of acquiring external information. Data acquired by the imaging unit 825 can be output to the display unit 820. An image sensor can be used for the imaging unit 825. Furthermore, multiple cameras may be provided to support multiple angles of view, such as telephoto and wide-angle.

[0367] The electronic device 800A may have a vibration mechanism that functions as a bone conduction earphone.

[0368] The electronic device 800A and the electronic device 800B may each have an input terminal to which a cable can be connected for supplying a video signal from a video output device or the like and power for charging a battery provided in the electronic device.

[0369] The electronic device of one embodiment of the present invention may have a function of wirelessly communicating with the earphone 750 .

[0370] 20B includes earphone unit 727. A portion of the wiring connecting earphone unit 727 and the control unit may be disposed inside housing 721 or attachment unit 723.

[0371] 20D includes an earphone unit 827. For example, the earphone unit 827 and the control unit 824 may be configured to be connected to each other by wire.

[0372] As described above, as electronic devices according to one embodiment of the present invention, both glasses-type devices (such as the electronic devices 700A and 700B) and goggle-type devices (such as the electronic devices 800A and 800B) are suitable.

[0373] The electronic device 6500 shown in FIG. 21A is a portable information terminal that can be used as a smartphone.

[0374] The electronic device 6500 includes a housing 6501, a display portion 6502, a power button 6503, a button 6504, a speaker 6505, a microphone 6506, a camera 6507, a light source 6508, and the like. The display portion 6502 has a touch panel function.

[0375] The display device of one embodiment of the present invention can be applied to the display portion 6502. Therefore, the electronic device can have high reliability.

[0376] FIG. 21B is a schematic cross-sectional view including the end of the housing 6501 on the microphone 6506 side.

[0377] A light-transmitting protective member 6510 is provided on the display surface side of the housing 6501, and a display panel 6511, an optical member 6512, a touch sensor panel 6513, a printed circuit board 6517, a battery 6518, etc. are arranged in the space surrounded by the housing 6501 and the protective member 6510.

[0378] A display panel 6511, an optical member 6512, and a touch sensor panel 6513 are fixed to the protective member 6510 by adhesive layers (not shown).

[0379] In a region outside the display portion 6502, a part of the display panel 6511 is folded back, and an FPC 6515 is connected to the folded back part. An IC 6516 is mounted on the FPC 6515. The FPC 6515 is connected to a terminal provided on a printed circuit board 6517.

[0380] The display device of one embodiment of the present invention can be applied to the display panel 6511. Therefore, an extremely lightweight electronic device can be realized. Furthermore, since the display panel 6511 is extremely thin, a large-capacity battery 6518 can be mounted thereon while keeping the thickness of the electronic device small. Furthermore, by folding back a part of the display panel 6511 and arranging a connection portion with the FPC 6515 on the back side of the pixel portion, an electronic device with a narrow frame can be realized.

[0381] 21C shows an example of a television set. A television set 7100 has a display portion 7000 built into a housing 7171. Here, the housing 7171 is supported by a stand 7173.

[0382] The display device of one embodiment of the present invention can be applied to the display portion 7000. Therefore, the electronic device can have high reliability.

[0383] The television device 7100 shown in FIG. 21C can be operated using operation switches provided on the housing 7171 and a separate remote control 7151.

[0384] 21D shows an example of a laptop personal computer 7200. The laptop personal computer 7200 includes a housing 7211, a keyboard 7212, a pointing device 7213, and an external connection port 7214. The housing 7211 includes a display portion 7000.

[0385] The display device of one embodiment of the present invention can be applied to the display portion 7000. Therefore, the electronic device can have high reliability.

[0386] 21E and 21F show an example of digital signage.

[0387] 21E includes a housing 7301, a display portion 7000, and a speaker 7303. The digital signage 7300 may further include an LED lamp, operation keys (including a power switch or an operation switch), a connection terminal, various sensors, a microphone, and the like.

[0388] 21F shows a digital signage 7400 attached to a cylindrical pillar 7401. The digital signage 7400 has a display unit 7000 provided along the curved surface of the pillar 7401.

[0389] 21E and 21F, the display device of one embodiment of the present invention can be applied to the display portion 7000. Therefore, the electronic device can have high reliability.

[0390] The larger the display unit 7000, the more information can be provided at one time. Also, the larger the display unit 7000, the more easily it will attract people's attention, which can increase the advertising effectiveness of, for example, advertisements.

[0391] Furthermore, as shown in Figures 21E and 21F, it is preferable that the digital signage 7300 or the digital signage 7400 be able to wirelessly connect with an information terminal 7311 or an information terminal 7411 such as a smartphone carried by a user.

[0392] The electronic device shown in Figures 22A to 22G has a housing 9000, a display unit 9001, a speaker 9003, operation keys 9005 (including a power switch or an operation switch), a connection terminal 9006, a sensor 9007 (including a function to measure force, displacement, position, speed, acceleration, angular velocity, rotation speed, distance, light, liquid, magnetism, temperature, chemical substance, sound, time, hardness, electric field, current, voltage, power, radiation, flow rate, humidity, gradient, vibration, odor or infrared rays), a microphone 9008, etc.

[0393] 22A to 22G have various functions, such as a function to display various information (still images, videos, text images, etc.) on a display unit, a touch panel function, a function to display a calendar, date, time, etc., a function to control processing using various software (programs), a wireless communication function, a function to read and process programs or data recorded on a recording medium, etc.

[0394] Details of the electronic device shown in Figures 22A to 22G will be described below.

[0395] FIG. 22A is a perspective view showing a mobile information terminal 9171. The mobile information terminal 9171 can be used as, for example, a smartphone. Note that the mobile information terminal 9171 may be provided with a speaker 9003, a connection terminal 9006, a sensor 9007, or the like. The mobile information terminal 9171 can display text and image information on multiple surfaces. FIG. 22A shows an example in which three icons 9050 are displayed. Information 9051, indicated by a dashed rectangle, can also be displayed on another surface of the display unit 9001. Examples of the information 9051 include notifications of incoming emails, SNS messages, phone calls, etc., the title of the email or SNS message, the sender's name, the date and time, the remaining battery level, and radio wave intensity. Alternatively, the icon 9050 or the like may be displayed in the position where the information 9051 is displayed.

[0396] 22B is a perspective view showing a mobile information terminal 9172. The mobile information terminal 9172 has a function of displaying information on three or more surfaces of the display portion 9001. Here, an example is shown in which information 9052, information 9053, and information 9054 are displayed on different surfaces. For example, a user can check information 9053 displayed in a position that can be observed from above the mobile information terminal 9172 while the mobile information terminal 9172 is stored in a breast pocket of clothes.

[0397] 22C is a perspective view showing a tablet terminal 9173. The tablet terminal 9173 is capable of executing various applications such as mobile phone calls, e-mail, text browsing and creation, music playback, internet communication, and computer games, for example. The tablet terminal 9173 has a display unit 9001, a camera 9002, a microphone 9008, and a speaker 9003 on the front side of a housing 9000, operation keys 9005 as operation buttons on the left side of the housing 9000, and a connection terminal 9006 on the bottom.

[0398] FIG. 22D is a perspective view showing a wristwatch-type mobile information terminal 9200. The mobile information terminal 9200 can be used as, for example, a smart watch (registered trademark). The display surface of the display unit 9001 is curved, and display can be performed along the curved display surface. The mobile information terminal 9200 can also perform hands-free calling by communicating with, for example, a headset capable of wireless communication. The mobile information terminal 9200 can also perform data transmission and charging with another information terminal through a connection terminal 9006. Note that charging may be performed by wireless power supply.

[0399] 22E to 22G are perspective views showing a foldable mobile information terminal 9201. Also, FIG. 22E is a perspective view of the mobile information terminal 9201 in an unfolded state, FIG. 22G is a perspective view of the mobile information terminal 9201 in a folded state, and FIG. 22F is a perspective view of a state in the process of changing from one of FIGS. 22E and 22G to the other. The mobile information terminal 9201 has excellent portability in a folded state, and excellent display visibility due to a seamless, wide display area in an unfolded state. A display portion 9001 of the mobile information terminal 9201 is supported by three housings 9000 connected by hinges 9055. For example, the display portion 9001 can be bent with a curvature radius of 0.1 mm or more and 150 mm or less.

[0400] This embodiment mode can be combined with other embodiment modes or examples as appropriate. In addition, in this specification, when a plurality of configuration examples are shown in one embodiment mode, the configuration examples can be combined as appropriate.

[0401] At least a part of the configuration examples exemplified in this embodiment and the corresponding drawings can be combined as appropriate with other configuration examples or drawings.

[0402] This embodiment mode can be implemented by appropriately combining at least a part thereof with other embodiment modes described in this specification.

[0403] In this example, the results of examining the occurrence of peeling depending on the presence or absence and type of the structure layer, as well as the shape and density of the structure, are shown.

[0404] First, to investigate the occurrence of peeling depending on the presence or absence and type of structural layer, samples of light-emitting devices with different resolutions were fabricated using five different structures (Structure 1 to Structure 5) with different structural layer configurations, and the presence or absence of peeling was observed.

[0405] (Sample Fabrication Method) First, 50 nm of titanium (Ti), 70 nm of aluminum (Al), and 6 nm of titanium (Ti) were sequentially laminated by sputtering on a silicon substrate with wiring. This was then heat-treated in an air atmosphere at 300°C for 1 hour. After the heat treatment and cleaning, a 10 nm film of indium tin oxide containing silicon oxide (ITSO) was formed by sputtering. This laminated film was patterned by photolithography to form a first electrode.

[0406] The first electrode is patterned so that light emitting devices equivalent to 50 ppi, 100 ppi, 200 ppi, 300 ppi, 400 ppi, and 500 ppi can be fabricated in addition to a 2 mm square electrode.

[0407] Next, as a pretreatment for forming a light-emitting device on the substrate, the substrate was heat-treated at 120° C. for 120 seconds, and then 1,1,1,3,3,3-hexamethyldisilazane (abbreviation: HMDS) was vaporized and sprayed for 120 seconds onto the substrate heated to 60° C. This makes it possible to make the laminated film formed on the first electrode less likely to peel off from the first electrode during the manufacturing process.

[0408] After that, about 1 × 10 −4 The substrate was introduced into a vacuum deposition apparatus whose inside had been reduced in pressure to 100 Pa, and was subjected to vacuum baking at 170° C. for 60 minutes in a heating chamber of the vacuum deposition apparatus, after which the substrate was allowed to cool for approximately 60 minutes.

[0409] Next, the substrate was fixed to a holder installed in a vacuum deposition apparatus so that the surface on which the first electrode was formed faced downward, and an EL layer including an emissive layer (hole injection layer, hole transport layer, emissive layer, electron transport layer) was deposited on the first electrode. After this, a structural layer was formed by deposition. The materials and deposition amounts of the structural layer were as follows. These were deposited using the calibration curve of NPB.

[0410]

[0411] In addition, Alq 3 represents tris(8-quinolinolato)aluminum(III), PPDN represents pyrazino[2,3-f][1,10]phenanthroline-1,3-dicarbonitride, and HATNA represents diquinoxalino[2,3-a:2',3'-c]phenazine. The structure layer of Structure 2 is formed by co-evaporating PPDN and HATNA in a weight ratio of 1:1. Alq 3 The structural formulae of PPDN and HATNA are shown below.

[0412]

[0413] Next, the sample with the structural layer formed thereon was removed from the vacuum deposition apparatus and exposed to the atmosphere. After that, an aluminum oxide film was formed by ALD to a thickness of 30 nm to form a protective layer. The aluminum oxide film was formed by ALD using trimethylaluminum (abbreviated as TMA) as a precursor and water vapor as an oxidizing agent.

[0414] A mask layer was formed on the protective layer by sputtering molybdenum (Mo) to a thickness of 40 nm.

[0415] A photoresist was applied onto the mask layer, and processing was carried out by exposure and development.

[0416] Next, using the photoresist as a mask, 4 , O 2 The mask layer was processed using an etching gas containing He. Using the processed mask layer as a mask, the sample was immersed in a basic etching solution (2.38% TMAH) at room temperature for 90 seconds to remove the photoresist and a portion of the protective layer (corresponding to a film thickness of 15 nm).

[0417] Thereafter, an optical microscope inspection (reflection mode, 50x objective) was performed to check for the occurrence of peeling. The results are shown below. In the table below, ○ indicates a good result with no peeling, and × indicates that peeling was observed.

[0418]

[0419] Thus, it was found that when processing by photolithography, the presence or absence of a layer (structural layer) between the protective layer and the EL layer and the material thereof influence whether peeling occurs or not.

[0420] Here, FIGS. 23A and 23B show length-measuring scanning electron microscope (SEM) photographs of samples having structure layer structures of Structure 1 and Structure 5. FIG. 23A is a photograph of a sample having a structure layer configuration of Structure 5, and FIG. 23B is a photograph of a sample having a structure layer configuration of Structure 1. Also, FIGS. 23A and 23B are photographs of an area equivalent to approximately one pixel. In both the samples of FIGS. 23A and 23B, one pixel has a size of 7.92 μm × 7.92 μm.

[0421] As can be seen from Figure 23B, in samples with structures such as Structure 1 where peeling does not occur, clumped foreign matter was observed in the area indicated by the arrow. This is not visible in the sample of Structure 5 in Figure 23A where peeling occurs. Figures 24A and 24B show cross-sectional photographs taken with a transmission electron microscope (TEM) of samples having the structure layer structures of Structure 1 and Structure 5. As can be seen, no convex structure is formed in Structure 5, while a convex structure 1155 is formed in Structure 1. Note that the convex structure 1155 in Structure 1 is unclear because it is out of focus.

[0422] FIG. 25 shows an optical microscope photograph (left) and a cross-sectional photograph (right) taken by a TEM of a sample having a structure layer with another structure. As shown in FIG. 25, it was found that similar convex structures were formed in the protective layers of Structures 2 to 4.

[0423] The size and density of the convex structures contained in these samples were investigated, and the results are shown below (however, structure 5 is omitted because it has no structure).

[0424]

[0425] In this way, in an organic semiconductor device that is processed by photolithography, by providing a structure layer that forms the convex structures 1155 under the protective layer, it is possible to suppress peeling of the protective layer, as shown in Table 3. The size of the convex structures is preferably a width of 10 nm to 200 nm, more preferably 80 nm to 150 nm, and even more preferably 100 nm to 150 nm. The height of the convex structures is preferably 5 nm to 100 nm, more preferably 20 nm to 80 nm, and even more preferably 20 nm to 60 nm.

[0426] The density of the convex structures is 0.01 pieces / μm 2 More than 50 pieces / μm 2 Preferably, the number is 0.1 or less per μm. 2 More than 5 pieces / μm 2 In the case of a high-definition semiconductor device with a resolution of 200 ppi or more, the number of particles is preferably 0.05 particles / μm or less. 2 1 piece / μm or more 2 Preferably, it is 0.1 particles / μm or less. 2 0.50 pieces / μm or more 2 It is more preferable that:

[0427] As described above, by providing a layer forming convex structures such as those of Structures 1 to 4 between the protective layer and the organic semiconductor layer, peeling during photolithography can be suppressed, high-definition organic semiconductor devices can be produced with good yield, and inexpensive organic semiconductor devices and organic semiconductor devices can be provided.

[0428] 100: display device, 100A: display device, 100B: display device, 100C: display device, 100D: display device, 100E: display device, 101B: first electrode, 101G: first electrode, 101R: first electrode, 101: first electrode, 102: second electrode, 103B: organic compound layer, 103Bf: organic compound film, 103G: organic compound layer, 103Gf: organic compound film, 103R: organic compound layer, 103Rf: organic compound film, 103: organic compound layer, 104B: first EL layer, 104G: first EL layer, 104R: first EL layer, 104: first EL layer, 105: Second EL layer, 110B: subpixel, 110G: subpixel, 110R: subpixel, 110: subpixel, 111: hole injection layer, 111C: conductive layer, 112B: conductive layer, 112R: conductive layer, 112: hole transport layer, 113: light emitting layer, 114: electron transport layer, 115: electron injection layer, 120: substrate, 122: resin layer, 125f: inorganic insulating film, 125: inorganic insulating layer, 126B: conductive layer, 126R: conductive layer, 127a: insulating layer, 127f: insulating film, 127: insulating layer, 128: layer, 129B: conductive layer, 129R: conductive layer, 130B: light emitting device, 130G: light emitting device, 130R : light-emitting device, 130: light-emitting device, 131: protective layer, 132B: colored layer, 132G: colored layer, 132R: colored layer, 140: connecting portion, 141: region, 142: adhesive layer, 151B: conductive layer, 151C: conductive layer, 151f: conductive film, 151G: conductive layer, 151R: conductive layer, 151: conductive layer, 152B: conductive layer, 152C: conductive layer, 152f: conductive film, 152G: conductive layer, 152R: conductive layer, 152: conductive layer, 153B: structural layer, 153Bf: structural layer, 153G: structural layer, 153Gf: structural layer, 153R: structural layer, 153Rf: structural layer, 153 : structural layer, 154: structural layer, 155: common electrode, 156B: insulating layer, 156C: insulating layer, 156f: insulating film, 156G: insulating layer, 156R: insulating layer, 156: insulating layer, 157: light-shielding layer, 158B: protective layer, 158Bf: protective film, 158G: protective layer, 158Gf: protective film, 158R: protective layer, 158Rf: protective film, 158: protective layer, 159B: mask layer, 159Bf: mask film, 159G: mask layer, 159Gf: mask film, 159R: mask layer, 159Rf: mask film, 160: insulating layer, 161: gate insulating layer, 162: gate electrode, 163: electrode,164: electrode, 165: first electrode, 166: conductive layer, 167: photoelectric conversion layer, 168: light-emitting layer, 169: second electrode, 171: insulating layer, 172: conductive layer, 173: insulating layer, 174: insulating layer, 175: insulating layer, 176: plug, 177: pixel portion, 178: pixel, 179: conductive layer, 190B: resist mask, 190G: resist mask, 190R: resist mask, 191: resist mask, 201: transistor, 204: connection portion, 205: transistor, 211: insulating layer, 213: insulating layer, 214: insulating layer, 215: insulating layer, 221: conductive layer, 222a : conductive layer, 222b: conductive layer, 223: conductive layer, 224B: conductive layer, 224C: conductive layer, 224G: conductive layer, 224R: conductive layer, 231: semiconductor layer, 240: capacitor, 241: conductive layer, 242: connection layer, 243: insulating layer, 245: conductive layer, 253: insulating layer, 254: insulating layer, 255: insulating layer, 256: plug, 261: insulating layer, 271: plug, 280: display module, 281: display section, 282: circuit section, 283a: pixel circuit, 283: pixel circuit section, 284a: pixel, 284: pixel section, 285: terminal section, 286: wiring section, 290: FPC, 291: substrate, 2 92: substrate, 301: substrate, 310: transistor, 311: conductive layer, 312: low resistance region, 313: insulating layer, 314: insulating layer, 315: element isolation layer, 351: substrate, 352: substrate, 353: FPC, 354: IC, 355: wiring, 356: circuit, 700A: electronic device, 700B: electronic device, 721: housing, 723: wearing part, 727: earphone part, 750: earphone, 751: display panel, 753: optical member, 756: display area, 757: frame, 758: nose pad, 800A: electronic device, 800B: electronic device, 820: display part, 821: housing, 82 2: communication unit, 823: wearing unit, 824: control unit, 825: imaging unit, 827: earphone unit, 832: lens, 1150: base film, 1151a: organic semiconductor layer, 1151: organic semiconductor film, 1152a: protective layer, 1152: protective layer, 1153a: mask layer, 1153: mask layer, 1154a: structure layer, 1154: structure layer, 1155: structure, 1156: surface, 1175a: photomask layer, 1175: resin film, 6500: electronic device, 6501: housing, 6502: display unit, 6503: power button, 6504: button, 6505: speaker, 6506: microphone,6507: camera, 6508: light source, 6510: protective member, 6511: display panel, 6512: optical member, 6513: touch sensor panel, 6515: FPC, 6516: IC, 6517: printed circuit board, 6518: battery, 7000: display unit, 7100: television device, 7151: remote control device, 7171: housing, 7173: stand, 7200: notebook personal computer, 7211: housing, 7212: keyboard, 7213: pointing device, 7214: external connection port, 7300: digital signage, 7301: Housing, 7303: speaker, 7311: information terminal, 7400: digital signage, 7401: pillar, 7411: information terminal, 9000: housing, 9001: display unit, 9002: camera, 9003: speaker, 9005: operation keys, 9006: connection terminal, 9007: sensor, 9008: microphone, 9050: icon, 9051: information, 9052: information, 9053: information, 9054: information, 9055: hinge, 9171: mobile information terminal, 9172: mobile information terminal, 9173: tablet terminal, 9200: mobile information terminal, 9201: mobile information terminal,

Claims

forming a first layer on the first electrode; forming a second layer made of a material that forms a structure having a convex shape on the first layer; forming a third layer on the first layer and the second layer; processing the third layer into a predetermined shape; and processing the first layer using the processed third layer as a mask, the first layer is an organic semiconductor layer; The method for producing an organic semiconductor device, wherein the third layer is composed of a material different from the materials constituting the first layer and the second layer. forming a first layer on the first electrode; forming a second layer made of a material that forms a structure having a convex shape on the first layer; forming a third layer on the first layer and the second layer; forming a fourth layer on the third layer; processing the third layer and the fourth layer into a predetermined shape; and processing the first layer using one or both of the processed third layer and the processed fourth layer as a mask; the first layer is an organic semiconductor layer; the third layer and the fourth layer are made of a material different from a material constituting the first layer and the second layer; The method of making an organic semiconductor device, wherein the third layer and the fourth layer are composed of different materials. In claim 2, The method for producing an organic semiconductor device, wherein the fourth layer is a layer containing an inorganic compound. In claim 3, The method for producing an organic semiconductor device, wherein the fourth layer is one or more selected from aluminum, indium, tungsten, molybdenum, gallium, zinc, and silicon, and oxides or nitrides thereof. In any one of claims 1 to 4, The method for producing an organic semiconductor device, wherein the material contained in the second layer has a glass transition temperature of 120° C. or lower. In any one of claims 1 to 4, The method for producing an organic semiconductor device, wherein the structure has a width of 10 nm or more and 200 nm or less and a height of 5 nm or more and 100 nm or less. In any one of claims 1 to 4, The method for producing an organic semiconductor device, wherein the structure has a width of 100 nm or more and 150 nm or less and a height of 20 nm or more and 60 nm or less. In any one of claims 1 to 4, The density of the structures is 0.1 / μm 2 0.5 pieces / μm or more 2 A method for fabricating an organic semiconductor device, comprising: In any one of claims 1 to 4, A method for producing an organic semiconductor device, wherein the material constituting the second layer includes an organometallic complex. In any one of claims 1 to 4, The method for producing an organic semiconductor device, wherein the third layer is a layer containing an inorganic compound. In any one of claims 1 to 4, The method for producing an organic semiconductor device, wherein the third layer is one or more selected from aluminum, indium, tungsten, molybdenum, gallium, zinc, and silicon, and oxides or nitrides thereof. In any one of claims 1 to 4, The method for producing an organic semiconductor device, wherein the third layer is a layer comprising aluminum oxide. In any one of claims 1 to 4, The method of making a light emitting device, wherein the first layer comprises a light emitting layer. In any one of claims 1 to 4, The method for manufacturing a photosensor, wherein the first layer includes a photoelectric conversion layer.

Citation Information

Patent Citations

  • Method for high-resolution patterning of an organic layer

    JP2018521459A

  • Method of manufacturing display device

    JP2023008872A

  • Organic semiconductor device, organic el device, light-emitting apparatus, electronic equipment, and lighting apparatus

    JP2023091772A