Anode catalyst, water electrolysis cell, and water electrolysis cell stack

The anode catalyst with a perovskite structure and specific ion composition addresses the issue of catalyst dissolution in water electrolysis, enhancing stability and current density maintenance, thereby improving the longevity and performance of water electrolysis cells.

WO2024241608A1PCT designated stage expired Publication Date: 2024-11-28TOKYO GAS CO LTD

Patent Information

Application Number
PCT/JP2023/041879
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-24
Filing Date
2023-11-21
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Anode catalysts used in water electrolysis, containing elements like ruthenium and iridium, are prone to dissolution in strong oxidizing atmospheres, leading to a shortened lifespan due to exposure during the electrolysis process, which affects the efficiency and durability of water electrolysis cells.

Method used

Development of an anode catalyst with a perovskite structure containing alkaline earth metal ions, tetravalent metal ions, and iridium ions, along with transition metal element ions such as manganese, nickel, copper, iron, or cobalt, with a molar concentration of iridium ions at 30 mol% or more, to enhance stability and catalytic activity.

Benefits of technology

The proposed anode catalyst design significantly extends the lifespan of water electrolysis cells by stabilizing the perovskite structure and maintaining high current density, as evidenced by higher current density maintenance rates compared to comparative examples.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2023041879_28112024_PF_FP_ABST
    Figure JP2023041879_28112024_PF_FP_ABST
Patent Text Reader

Abstract

This anode catalyst comprises A-site ions including alkaline earth metal ions, and B-site ions including tetravalent metal ions and iridium ions. The molar concentration of the iridium ions is 30 mol% or more. The anode catalyst also comprises an oxide having a perovskite structure and including transition metal element ions.
Need to check novelty before this filing date? Find Prior Art

Description

Anode catalyst, water electrolysis cell and water electrolysis cell stack

[0001] The present disclosure relates to an anode catalyst, a water electrolysis cell, and a water electrolysis cell stack.

[0002] Water electrolysis (hereinafter sometimes referred to as "water electrolysis") is a method for producing hydrogen and oxygen from water by electrolysis. For example, among technologies that utilize hydrogen as an energy source, water electrolysis is a promising technology for sustainable hydrogen production.

[0003] A water electrolysis cell used for water electrolysis includes an anode separator, an anode gas diffusion layer, an anode catalyst, an electrolyte membrane, a cathode catalyst, a cathode gas diffusion layer, a cathode separator, etc. Regarding the anode catalyst and cathode catalyst, catalysts suitable for water electrolysis are being studied.

[0004] For example, International Publication No. 2018 / 159644 discloses PdRu solid solution nanoparticles containing palladium (Pd) and ruthenium (Ru), and discloses that these nanoparticles can be used as a catalyst for water electrolysis.

[0005] Anode catalysts containing elements with anode activity, such as ruthenium and iridium, have high catalytic activity. However, because the anode catalyst is exposed to a strongly oxidizing atmosphere during water electrolysis, elements such as ruthenium and iridium are easily dissolved, and the life of anode catalysts containing such elements is likely to be shortened.

[0006] For example, in a water electrolysis catalyst containing ruthenium as disclosed in Patent Document 1, ruthenium is easily dissolved, and there is a risk that the catalyst will have a short life.

[0007] An object of the present disclosure is to provide a long-life anode catalyst, and a water electrolysis cell and a water electrolysis cell stack including the same.

[0008] The present disclosure includes the following aspects. <1> An anode catalyst including alkaline earth metal ions as A-site ions and tetravalent metal ions and iridium ions as B-site ions, wherein the molar concentration of the iridium ions is 30 mol% or more, and including an oxide having a perovskite structure, the oxide further including a transition metal element ion. <2> The anode catalyst according to <1>, wherein the alkaline earth metal ions include strontium ions. <3> The anode catalyst according to <1> or <2>, wherein the tetravalent metal ions include titanium ions. <4> The anode catalyst according to any one of <1> to <3>, wherein the transition metal element ions include at least one type of ion selected from manganese ions, nickel ions, copper ions, iron ions, and cobalt ions. <5> The anode catalyst according to any one of <1> to <4>, wherein the ratio of the number of moles of the transition metal element ions to the sum of the number of moles of the transition metal element ions and the tetravalent metal ions is 5% or more and 91% or less. <6> The anode catalyst according to any one of <1> to <4>, wherein the ratio of the number of moles of the transition metal element ions to the sum of the number of moles of the transition metal element ions and the tetravalent metal ions is 14% or more and 82% or less. <7> The anode catalyst according to any one of <1> to <4>, wherein the ratio of the number of moles of the transition metal element ions to the sum of the number of moles of the transition metal element ions and the tetravalent metal ions is 21% or more and 75% or less. <8> A water electrolysis cell comprising an anode gas diffusion layer, the anode catalyst according to any one of <1> to <7>, an electrolyte membrane, a cathode catalyst, a cathode gas diffusion layer, and a separator. <9> A water electrolysis cell stack comprising a plurality of water electrolysis cells according to <8> stacked one on top of the other.

[0009] According to the present disclosure, there are provided a long-life anode catalyst, and a water electrolysis cell and a water electrolysis cell stack including the same.

[0010] Fig. 1 is a schematic cross-sectional view of a water electrolysis cell. Fig. 2 is a graph showing the relationship between the proportion of transition metal element ions and the current density maintenance rate in each example and each comparative example.

[0011] Hereinafter, embodiments of the present disclosure will be described. The present disclosure is not limited to the following embodiments, and can be implemented by making appropriate modifications within the scope of the object of the present disclosure. The dimensional ratios in the drawings do not necessarily represent the actual dimensional ratios.

[0012] In the present disclosure, a numerical range expressed using "to" means a range that includes the numerical values ​​before and after "to" as the lower and upper limits.

[0013] In the numerical ranges described in stages in the present disclosure, the upper limit value described in one numerical range may be replaced with the upper limit value of another numerical range described in stages, and the lower limit value described in one numerical range may be replaced with the lower limit value of another numerical range described in stages. In the numerical ranges described in stages in the present disclosure, the upper or lower limit value described in one numerical range may be replaced with a value shown in the examples.

[0014] In the present disclosure, a combination of two or more preferred aspects is a more preferred aspect.

[0015] <Anode Catalyst> The anode catalyst of the present disclosure includes alkaline earth metal ions as A-site ions and tetravalent metal ions (hereinafter also referred to as specific metal ions) and iridium ions as B-site ions, with the molar concentration of the iridium ions being 30 mol% or more. The anode catalyst includes an oxide having a perovskite structure, and the oxide further contains transition metal element ions. The anode catalyst of the present disclosure tends to have a long life due to the inclusion of the oxide having the perovskite structure. This is presumably because the molar concentration of iridium ions is 30 mol% or more and the oxide contains transition metal element ions, which effectively stabilizes the perovskite structure of the oxide. However, the present disclosure is not limited to this presumption. In the present disclosure, the molar concentration of iridium ions refers to the molar concentration of iridium ions relative to the total molar concentration of iridium ions, tetravalent metal ions, and transition metal element ions.

[0016] Oxides having a perovskite structure containing alkaline earth metal ions as A-site ions, specific metal ions and iridium ions as B-site ions, and further containing transition metal element ions can be produced by conventionally known methods. For example, oxides having a perovskite structure can be produced by conventionally known solid-phase methods, liquid-phase methods, etc. Solid-phase methods include methods based on direct reaction of solid raw materials, and liquid-phase methods include the Pezzini method, complex polymerization, and hydrothermal synthesis.

[0017] The anode catalyst of the present disclosure includes an oxide having a perovskite structure. The oxide having a perovskite structure is generally ABO 3 It is represented by the chemical formula: Some oxides with a perovskite structure have oxygen variability. The amount of oxygen may be deficient or excessive, relative to 3. Furthermore, the A-site ions and B-site ions may be partially substituted with different elements. Whether or not an anode catalyst has a perovskite structure can be analyzed by X-ray diffraction (XRD).

[0018] The A-site ions of the perovskite structure include alkaline earth metal ions. Examples of alkaline earth metal ions include calcium ions, strontium ions, barium ions, and radium ions. In the present disclosure, the alkaline earth metal ions serving as the A-site ions preferably include at least one selected from the group consisting of strontium ions, calcium ions, and barium ions, and more preferably include strontium ions. The A-site ions may be one type of alkaline earth metal ion or two or more types of alkaline earth metal ions. For example, the A-site ions may be strontium ions alone, or may be a combination of strontium ions and one or more other alkaline earth metal ions.

[0019] The B-site ions in the perovskite structure include specific metal ions and iridium ions.

[0020] The specific metal ion is not particularly limited as long as it is a tetravalent metal ion, and examples thereof include at least one selected from zirconium ions and titanium ions, and it is preferable to include titanium ions.

[0021] The oxide having a perovskite structure further contains transition metal element ions. For example, the transition metal element ions may be contained in A-site ions, B-site ions, or may be located on the oxide surface. When the transition metal element ions are contained in B-site ions and are tetravalent metal ions, the tetravalent transition metal element ions are classified as specific metal ions rather than transition metal element ions.

[0022] Examples of transition metal element ions include ions of elements present in Groups 3 to 12 of the periodic table (excluding specific metal ions and iridium ions). Examples include ions of scandium (Sc), yttrium (Y), vanadium (V), niobium (Nb), tantalum (Ta), chromium (Cr), molybdenum (Mo), tungsten (W), manganese (Mn), iron (Fe), ruthenium (Ru), cobalt (Co), nickel (Ni), copper (Cu), and zinc (Zn). The transition metal element ion is preferably at least one ion selected from manganese ions, nickel ions, copper ions, iron ions, and cobalt ions. The transition metal element ions contained in the oxide may be one type of transition metal element ion or two or more types of transition metal element ions.

[0023] The transition metal element ions preferably include at least one type of ion selected from manganese ions, nickel ions, copper ions, iron ions, and cobalt ions.

[0024] The B-site ions may or may not contain ions other than the specific metal ions and iridium ions. When the B-site ions contain other ions, examples of the other ions include the transition metal element ions described above, gallium (Ga), indium (In), tin (Sn), antimony (Sb), and the like.

[0025] In the anode catalyst of the present disclosure, the A-site ions preferably include alkaline earth metal ions, and the B-site ions preferably include titanium ions and iridium ions.

[0026] The molar concentration of iridium ions relative to the total molar concentration of iridium ions, tetravalent metal ions, and transition metal element ions is preferably 30 mol% or more, more preferably 35 mol% or more, and may be 70 mol% or less, or 50 mol% or less.

[0027] From the viewpoint of extending the life of the anode catalyst, the ratio of the number of moles of the transition metal element ion to the sum of the number of moles of the transition metal element ion and the specific metal ion (preferably titanium ion) is preferably 5% or more and 91% or less, more preferably 14% or more and 82% or less, and even more preferably 21% or more and 75% or less.

[0028] The molar concentration of iridium and the ratio of the molar numbers to the total molar concentration of iridium ions, tetravalent metal ions, and transition metal element ions can be determined by analyzing the anode catalyst using inductively coupled plasma (ICP). Furthermore, the metal concentrations can be quantitatively evaluated by imaging the catalyst powder and performing elemental analysis using a scanning electron microscope (SEM) and energy dispersive X-ray spectroscopy (EDS).

[0029] The anode catalyst of the present disclosure contains alkaline earth metal ions as A-site ions and tetravalent metal ions and iridium ions as B-site ions, with the molar concentration of iridium ions being 30 mol% or more, has a perovskite structure, and may further contain components other than the oxide containing transition metal element ions, such as catalytically active components other than the oxide having a perovskite structure, unreacted components of raw materials used to generate the oxide having a perovskite structure, and side reaction components.

[0030] The content of the oxide having a perovskite structure in the anode catalyst of the present disclosure is not particularly limited, and is preferably 50% by mass to 100% by mass, more preferably 70% by mass to 100% by mass, and even more preferably 90% by mass to 100% by mass, relative to the total amount of the anode catalyst.

[0031] <Water Electrolysis Cell> A water electrolysis cell according to the present disclosure includes an anode gas diffusion layer, the anode catalyst according to the present disclosure, an electrolyte membrane, a cathode catalyst, a cathode gas diffusion layer, and a separator.

[0032] The anode gas diffusion layer, electrolyte membrane, cathode catalyst, cathode gas diffusion layer, and separator may be members used in conventionally known water electrolysis cells.

[0033] The water electrolysis cell may further include other components. The other components may be selected from known components of water electrolysis cells. Examples of the other components include a gasket and a sealant.

[0034] For example, the anode gas diffusion layer and the cathode gas diffusion layer can each independently be made of a material that allows fluid to flow through the layer, such as a porous body, a powder sintered body, a fiber sintered body, a metal mesh, or felt.

[0035] The anode gas diffusion layer may be coated with a corrosion-resistant conductive material to prevent the resistance from increasing due to oxidation, such as platinum, gold, silver, titanium nitride, titanium carbide, or titanium carbonitride.

[0036] The electrolyte membrane may be selected from known electrolyte membranes (which may be ion exchange membranes) used in water electrolysis. + ) is preferably selectively permeable. Examples of the electrolyte membrane include a polymer electrolyte membrane (PEM). Examples of the polymer electrolyte membrane include a perfluorocarbon membrane having a sulfonic acid group. Examples of the perfluorocarbon membrane having a sulfonic acid group include a Nafion membrane.

[0037] The electrolyte membrane is a polymer having proton conductivity due to the presence of ionic groups, and may be, for example, either a fluorine-based polymer electrolyte or a hydrocarbon-based polymer electrolyte.

[0038] Here, the fluorine-based polymer electrolyte refers to one in which most or all of the hydrogen atoms in the alkyl and / or alkylene groups in the polymer have been substituted with fluorine atoms. Representative examples of fluorine-based polymer electrolytes having ionic groups include commercially available products such as "Nafion" (registered trademark) (manufactured by Chemours Inc.), "Aquivion" (registered trademark) (manufactured by Solvay), "Flemion" (registered trademark) (manufactured by AGC Inc.), and "Aciplex" (registered trademark) (manufactured by Asahi Kasei Corporation).

[0039] The hydrocarbon-based polymer electrolyte is preferably an aromatic hydrocarbon-based polymer having an aromatic ring in the main chain. Here, the aromatic ring may include not only a hydrocarbon-based aromatic ring consisting only of carbon atoms and hydrogen atoms, such as a benzene ring or a naphthalene skeleton, but also a heterocycle such as a pyridine ring, an imidazole ring, or a thiol ring. In addition, the polymer may also include aliphatic units in addition to the aromatic ring units.

[0040] Specific examples of aromatic hydrocarbon polymers include polymers having a structure selected from polysulfone, polyethersulfone, polyphenylene oxide, polyarylene ether, polyphenylene sulfide, polyphenylene sulfide sulfone, polyparaphenylene, polyarylene, polyarylene ketone, polyether ketone, polyarylene phosphine oxide, polyether phosphine oxide, polybenzoxazole, polybenzothiazole, polybenzimidazole, polyamide, polyimide, polyetherimide, and polyimide sulfone in the main chain together with an aromatic ring. Note that the terms "polysulfone," "polyethersulfone," and "polyether ketone" are generic terms for structures having a sulfone bond, an ether bond, a ketone bond, or the like in the molecular chain, and include polyether ketone ketone, polyether ether ketone, polyether ether ketone ketone, polyether ketone ether ketone ketone, and polyether ketone sulfone. The aromatic hydrocarbon polymer may have a plurality of these structures. Among these, polymers having a polyether ketone skeleton, that is, polyether ketone polymers, are particularly preferred as aromatic hydrocarbon polymers.

[0041] The electrolyte membrane may be combined with a reinforcing material, which can reduce the risk of gas leakage and short circuits within the electrodes due to membrane damage when the electrolyte membrane and electrodes are joined by hot pressing, for example.

[0042] Specific examples of reinforcing materials include homogeneous porous films made of fluorine-based polymers such as PTFE (polytetrafluoroethylene), PFA (tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer), PVDF (polyvinylidene fluoride), and FEP (tetrafluoroethylene-hexafluoropropylene copolymer), or thermoplastic resins such as PE (polyethylene) and PP (polypropylene), and engineering plastics such as PI (polyimide), PSF (polysulfone), PES (polyethersulfone), PEEK (polyetheretherketone), PPSS (polyphenylene sulfide sulfone), PPO (polyphenylene oxide), PEK (polyetherketone), PBI (polybenzimidazole), PPS (polyphenylene sulfide), PPP (polyparaphenylene), PPQ (polyphenylquinoxaline), polybenzoxazole (PBO), polybenzothiazole (PBT), and polyparaphenylene terephthalamide (PPTA).

[0043] The cathode catalyst may be selected from known catalysts used in water electrolysis. Examples of catalyst components include platinum, gold, silver, palladium, iridium, rhodium, ruthenium, tin, iron, cobalt, nickel, molybdenum, tungsten, vanadium, alloys thereof, and oxides thereof. The catalyst may be in the form of particles. The anode catalyst may also include a catalyst supported on a carrier. Examples of the carrier include titanium oxide and tin oxide. The cathode catalyst may also include a catalyst supported on a carrier. Examples of the carrier include carbon black.

[0044] The water electrolysis cell may include an anode catalyst layer containing an anode catalyst (preferably anode catalyst particles) and an ionomer, or may include a cathode catalyst layer containing a cathode catalyst (preferably cathode catalyst particles) and an ionomer, which increases the contact area between the catalyst and the ionomer in the catalyst layer and tends to promote the reaction.

[0045] The primary particle diameter of the anode catalyst is preferably 1 nm to 10 μm, more preferably 2 nm to 1 μm, and even more preferably 5 nm to 100 nm. When the primary particle diameter of the anode catalyst is 1 nm or more, the mixing ratio of the ionomer required to increase the contact area does not become too large, and many electron conduction paths can be secured inside the anode catalyst layer, which tends to make the resistance less likely to increase. When the primary particle diameter of the anode catalyst is 10 μm or less, the decrease in the contact area with the ionomer is suppressed, which tends to make the resistance less likely to increase.

[0046] The separator may be an anode separator disposed on the anode gas diffusion layer side, or a cathode separator disposed on the cathode gas diffusion layer side. Examples of separator materials include titanium, stainless steel, and carbon. From the viewpoint of suppressing oxidation due to oxygen generated on the anode side, the anode separator preferably contains titanium.

[0047] The anode separator may be coated with a corrosion-resistant conductive material to prevent high resistance due to oxidation, such as platinum, gold, silver, titanium nitride, titanium carbide, or titanium carbonitride.

[0048] The arrangement of each component in the water electrolysis cell may be determined with reference to known water electrolysis cells. In the water electrolysis cell, the electrolyte membrane is preferably located between the anode catalyst and the cathode catalyst. In the water electrolysis cell, the electrolyte membrane, the anode catalyst, and the cathode catalyst are preferably located between the anode gas diffusion layer and the cathode gas diffusion layer. In the water electrolysis cell, the electrolyte membrane, the anode catalyst, the cathode catalyst, and the anode gas diffusion layer and the cathode gas diffusion layer are preferably located between two separators.

[0049] The anode catalyst layer or cathode catalyst layer may be mixed with an ionomer and a solvent to form a slurry, which may then be applied to an electrolyte membrane to form a catalyst-layered electrolyte membrane. Alternatively, the catalyst layer may be applied to a film such as a Teflon (registered trademark) sheet and then transferred to the electrolyte membrane. The catalyst layer may also be applied to a gas diffusion layer to form a gas diffusion electrode. Apparatuses for applying the catalyst layer slurry include spray coaters, comma coaters, die coaters, reverse roll coaters, gravure coaters, bar coaters, dip coaters, slit coaters, and lip coaters.

[0050] An example of a water electrolysis cell is shown in Fig. 1 . Fig. 1 is a schematic cross-sectional view of a water electrolysis cell. As shown in Fig. 1 , a water electrolysis cell 100 includes, in order from the top of Fig. 1 , an anode separator 60, an anode gas diffusion layer 20, an anode catalyst 12, an electrolyte membrane 11, a cathode catalyst 13, a cathode gas diffusion layer 30, and a cathode separator 70. Furthermore, a gasket 40 is disposed between the anode separator 60 and the electrolyte membrane 11, and a gasket 50 is disposed between the cathode separator 70 and the electrolyte membrane 11.

[0051] <Water Electrolysis Apparatus> The water electrolysis apparatus according to the present disclosure may be a water electrolysis cell stack formed by stacking a plurality of the water electrolysis cells according to the present disclosure, or may be an apparatus including the water electrolysis cell stack or the water electrolysis cell according to the present disclosure and other components.

[0052] The other components may be selected from known components of a water electrolysis device, such as auxiliary devices such as a power conditioner, a water pump, an ion exchange resin, a heat exchanger, and a dehumidifier.

[0053] The present disclosure will be described in detail below using examples. However, the present disclosure is not limited to the following examples. The matters shown in the following examples may be appropriately changed without departing from the spirit of the present disclosure.

[0054] Example 1 Iridium ions and manganese ions were ionized by the Pezzini method to form strontium titanate (SrTiO 3A catalyst powder containing an oxide having a perovskite structure incorporated into strontium carbonate (SrCO) was obtained. 3 ), titanium tetrabutoxide (C 16 H 36 O 4 Ti), potassium hexachloroiridate (K 2 IrCl 6 Manganese nitrate hexahydrate was weighed so that the manganese ion concentration was 4M (mol / L) and dissolved in water to prepare an aqueous solution. The concentration of the aqueous manganese nitrate solution was analyzed by ICP. 3 0.2794g, K 2 IrCl 6 0.0800 g, 17.7 μL of manganese nitrate aqueous solution, citric acid monohydrate (C 6 H 8 O 7 ・H 2 0.2800 g of nitric acid (1.38) and 0.3 mL of nitric acid (1.38) were weighed, added to 10 mL of pure water, mixed, and dissolved by stirring at room temperature for 10 minutes or more. This mixed solution was designated as Solution A. 16 H 36 O 4 0.081 g of Ti was weighed out and dissolved in 4 mL of ethylene glycol (C 2 H 6 O 2) were mixed and stirred for at least 10 minutes. This mixed solution was designated Solution B. Solution A was added to Solution B, and the mixture was stirred and mixed at 70°C for at least 3 hours using a hot stirrer. The mixed solution was then transferred to a zirconia crucible and heat-treated at 180°C for 12 hours, 200°C for 6 hours, 300°C for 6 hours, 500°C for 3 hours, and 600°C for 6 hours. The heat-treated powder was collected and placed in a beaker with 50 mL of 1M hydrochloric acid solution and stirred for at least 3 hours to remove unreacted components. The resulting mixed solution was washed with water using a suction filter and dried in an oven at 60°C to obtain a catalyst powder. X-ray diffraction measurement of the synthesized catalyst powder revealed a diffraction pattern derived from a perovskite structure. The composition of the resulting powder was analyzed using FE-SEM / EDS. The powder composition was applied to a carbon tape, and the atomic concentrations of iridium, titanium, and manganese were evaluated by mapping analysis in three fields of view magnified 10,000 times, and the average atomic concentration of each element was defined as the concentration of the element. As a result, the molar concentration of iridium ions relative to the total molar concentration of iridium ions, titanium ions, and manganese ions was 35 mol%, and the ratio of the number of moles of the transition metal element ions (manganese ions in Example 1) to the sum of the number of moles of the transition metal element ions and titanium ions (hereinafter also referred to as the "manganese ion ratio", corresponding to the transition metal element ion ratio in Table 1) was 7.8%.

[0055] Example 2: Synthesized SrTiO 3 The manganese ion content of the manganese ion solution was adjusted to 11.8% by adding 35.5 μL of manganese nitrate solution and C 16 H 36 O 4 A catalyst powder containing an oxide having a perovskite structure was obtained in the same manner as in Example 1, except that the amount of Ti was changed to 0.0564 g.

[0056] Example 3: Synthesized SrTiO 3 For the manganese ions incorporated in the solution, 47.3 μL of manganese nitrate solution and C were added so that the manganese ion ratio was 19.1%. 16 H 36 O 4A catalyst powder containing an oxide having a perovskite structure was obtained in the same manner as in Example 1, except that the amount of Ti was changed to 0.0401 g.

[0057] Example 4: Synthesized SrTiO 3 For the manganese ions incorporated in the solution, 59.1 μL of manganese nitrate solution and C were added so that the manganese ion ratio was 26.7%. 16 H 36 O 4 A catalyst powder containing an oxide having a perovskite structure was obtained in the same manner as in Example 1, except that the amount of Ti was changed to 0.0242 g.

[0058] Example 5: Synthesized SrTiO 3 For the manganese ions incorporated in the solution, 71.0 μL of manganese nitrate solution and C were added so that the manganese ion ratio was 37.4%. 16 H 36 O 4 A catalyst powder containing an oxide having a perovskite structure was obtained in the same manner as in Example 1, except that the amount of Ti was changed to 0.0080 g.

[0059] Example 6 Iridium ions and nickel ions were incorporated into SrTiO by the Pezzini method in the same manner as in Example 1, except that nickel ions were incorporated instead of manganese ions as the transition metal element ions. 3 The catalyst powder was obtained containing an oxide having a perovskite structure incorporated into the starting material. 3 , C 16 H 36 O 4 Ti, K 2 IrCl 6 and nickel nitrate hexahydrate. Nickel nitrate hexahydrate was weighed so that the nickel ion concentration was 4 M, and dissolved in water to prepare an aqueous solution. The concentration of the aqueous nickel nitrate solution was analyzed by ICP. 3 0.2794g, K 2 IrCl 6 0.0800 g of nickel nitrate solution, 17.7 μL of C 6 H 8 O 7 ・H 20.2800 g of HCl and 0.3 mL of nitric acid (1.38) were weighed, added to 10 mL of pure water, mixed, and dissolved by stirring at room temperature for 10 minutes or more. This mixed solution was designated as Solution A. 16 H 36 O 4 Weigh out 0.0805 g of Ti and add it to 4 mL of C 2 H 6 O 2 The two were mixed and stirred for 10 minutes or more. This mixed solution was designated Solution B. The subsequent operations were the same as in Example 1, and a catalyst powder was recovered. The molar concentration of iridium ions relative to the total molar concentration of iridium ions, titanium ions, and nickel ions, determined in the same manner as in Example 1, was 35 mol %, and the ratio of the number of moles of the transition metal element ions (nickel ions in Example 6) to the sum of the number of moles of the transition metal element ions and titanium ions (hereinafter also referred to as the "nickel ion ratio") was 13.5%.

[0060] Example 7: Synthesized SrTiO 3 A catalyst powder containing an oxide having a perovskite structure was obtained in the same manner as in Example 1, except that the amount of the nickel nitrate aqueous solution was changed to 35.5 μL so that the proportion of nickel ions incorporated in the catalyst was 17.9%.

[0061] Example 8: Synthesized SrTiO 3 For the nickel ions incorporated in the solution, 35.5 μL of nickel nitrate solution and C were added so that the nickel ion ratio was 19.6%. 16 H 36 O 4 A catalyst powder containing an oxide having a perovskite structure was obtained in the same manner as in Example 1, except that the amount of Ti was changed to 0.0564 g.

[0062] Example 9: Synthesized SrTiO 3 For the nickel ions incorporated in the solution, 59.1 μL of nickel nitrate solution and C were added so that the nickel ion ratio was 60.3%. 16 H 36 O 4 A catalyst powder containing an oxide having a perovskite structure was obtained in the same manner as in Example 1, except that the amount of Ti was changed to 0.0242 g.

[0063] Example 10: Synthesized SrTiO 3 For the nickel ions incorporated in the solution, 71.0 μL of nickel nitrate solution and C were added so that the nickel ion ratio was 80.1%. 16 H 36 O 4 A catalyst powder containing an oxide having a perovskite structure was obtained in the same manner as in Example 1, except that the amount of Ti was changed to 0.0080 g.

[0064] Example 11 Iridium ions and copper ions were incorporated into SrTiO by the Pezzini method in the same manner as in Example 1, except that copper ions were incorporated instead of manganese ions as the transition metal element ions. 3 The catalyst powder was obtained containing an oxide having a perovskite structure incorporated into the starting material. 3 , C 16 H 36 O 4 Ti, K 2 IrCl 6 and copper nitrate trihydrate. Copper nitrate trihydrate was weighed so that the copper ion concentration was 4 M, and dissolved in water to prepare an aqueous solution. The concentration of the copper nitrate aqueous solution was analyzed by ICP. 3 0.2794g, K 2 IrCl 6 0.0800 g of copper nitrate solution, 17.7 μL of C 6 H 8 O 7 ・H 2 0.2800 g of HCl and 0.3 mL of nitric acid (1.38) were weighed, added to 10 mL of pure water, mixed, and dissolved by stirring at room temperature for 10 minutes or more. This mixed solution was designated as Solution A. 16 H 36 O 4 Weigh out 0.0805 g of Ti and add it to 4 mL of C 2 H 6 O 2The two were mixed and stirred for 10 minutes or more. This mixed solution was designated Solution B. The subsequent operations were the same as in Example 1, and a catalyst powder was recovered. The molar concentration of iridium ions relative to the total molar concentration of iridium ions, titanium ions, and copper ions, determined in the same manner as in Example 1, was 35 mol %, and the ratio of the number of moles of the transition metal element ions (copper ions in Example 11) to the sum of the number of moles of the transition metal element ions and titanium ions (hereinafter also referred to as the "copper ion ratio") was 19.4%.

[0065] Example 12: Synthesized SrTiO 3 The copper ion content of the copper ions incorporated in the solution was adjusted to 22.2% by adding 35.5 μL of copper nitrate solution and C 16 H 36 O 4 A catalyst powder containing an oxide having a perovskite structure was obtained in the same manner as in Example 1, except that the amount of Ti was changed to 0.0564 g.

[0066] Example 13: Synthesized SrTiO 3 For the copper ions incorporated in the solution, 59.1 μL of copper nitrate solution and C were added so that the copper ion ratio was 37.4%. 16 H 36 O 4 A catalyst powder containing an oxide having a perovskite structure was obtained in the same manner as in Example 1, except that the amount of Ti was changed to 0.0242 g.

[0067] Example 14: Synthesized SrTiO 3 For the copper ions incorporated in the solution, 71.0 μL of copper nitrate solution and C were added so that the copper ion ratio was 46.2%. 16 H 36 O 4 A catalyst powder containing an oxide having a perovskite structure was obtained in the same manner as in Example 1, except that the amount of Ti was changed to 0.0080 g.

[0068] Example 15 Iridium ions and iron ions were incorporated into SrTiO by the Pezzini method in the same manner as in Example 1, except that iron ions were incorporated instead of manganese ions as the transition metal element ions. 3The catalyst powder was obtained containing an oxide having a perovskite structure incorporated into the starting material. 3 , C 16 H 36 O 4 Ti, K 2 IrCl 6 and iron nitrate nonahydrate. The iron nitrate nonahydrate was weighed so that the iron ion concentration was 4 M, and dissolved in water to prepare an aqueous solution. The concentration of the aqueous iron nitrate solution was analyzed by ICP. 3 0.2794g, K 2 IrCl 6 0.0800 g of iron nitrate solution, 17.7 μL of C 6 H 8 O 7 ・H 2 0.2800 g of HCl and 0.3 mL of nitric acid (1.38) were weighed, added to 10 mL of pure water, mixed, and dissolved by stirring at room temperature for 10 minutes or more. This mixed solution was designated as Solution A. 16 H 36 O 4 Weigh out 0.0805 g of Ti and add it to 4 mL of C 2 H 6 O 2 The two were mixed and stirred for 10 minutes or more. This mixed solution was designated Solution B. The subsequent operations were the same as in Example 1, and a catalyst powder was recovered. The molar concentration of iridium ions relative to the total molar concentration of iridium ions, titanium ions, and iron ions, determined in the same manner as in Example 1, was 35 mol %, and the ratio of the number of moles of the transition metal element ions (iron ions in Example 15) to the sum of the number of moles of the titanium ions (hereinafter also referred to as the "iron ion ratio") was 10.1%.

[0069] Example 16: Synthesized SrTiO 3 The iron ion content of the iron ion incorporated in the solution was 19.5% by weight, and 35.5 μL of iron nitrate solution and C 16 H 36 O 4 A catalyst powder containing an oxide having a perovskite structure was obtained in the same manner as in Example 1, except that the amount of Ti was changed to 0.0564 g.

[0070] Example 17: Synthesized SrTiO3 For the iron ions incorporated in the solution, 59.1 μL of iron nitrate solution and C were added so that the iron ion ratio was 34.9%. 16 H 36 O 4 A catalyst powder containing an oxide having a perovskite structure was obtained in the same manner as in Example 1, except that the amount of Ti was changed to 0.0242 g.

[0071] Example 18: Synthesized SrTiO 3 For the iron ions incorporated in the solution, 71.0 μL of iron nitrate solution and C were added so that the iron ion ratio was 50.5%. 16 H 36 O 4 A catalyst powder containing an oxide having a perovskite structure was obtained in the same manner as in Example 1, except that the amount of Ti was changed to 0.0080 g.

[0072] Example 19 Iridium ions and cobalt ions were incorporated into SrTiO by the Pezzini method in the same manner as in Example 1, except that cobalt ions were incorporated instead of manganese ions as the transition metal element ions. 3 The catalyst powder was obtained containing an oxide having a perovskite structure incorporated into the starting material. 3 , C 16 H 36 O 4 Ti, K 2 IrCl 6 Cobalt nitrate hexahydrate was weighed so that the cobalt ion concentration was 4M, and dissolved in water to prepare an aqueous solution. The concentration of the aqueous cobalt nitrate solution was analyzed by ICP. 3 0.2794g, K 2 IrCl 6 0.0800 g, cobalt nitrate 17.7 μL, C 6 H 8 O 7 ・H 2 0.2800 g of HCl and 0.3 mL of nitric acid (1.38) were weighed, added to 10 mL of pure water, mixed, and dissolved by stirring at room temperature for 10 minutes or more. This mixed solution was designated as Solution A. 16 H 36 O 4Weigh out 0.0805 g of Ti and add it to 4 mL of C 2 H 6 O 2 The two were mixed and stirred for 10 minutes or more. This mixed solution was designated as Solution B. The subsequent operations were the same as in Example 1, and a catalyst powder was recovered. The molar concentration of iridium ions relative to the total molar concentration of iridium ions, titanium ions, and cobalt ions, determined in the same manner as in Example 1, was 35 mol%, and the ratio of the number of moles of the transition metal element ions (cobalt ions in Example 19) to the sum of the number of moles of the transition metal element ions and titanium ions (hereinafter also referred to as the "cobalt ion ratio") was 12.4%.

[0073] Example 20: Synthesized SrTiO 3 For the cobalt ions incorporated in the sol, 35.5 μL of cobalt nitrate solution and C were added so that the cobalt ion ratio was 20.8%. 16 H 36 O 4 A catalyst powder containing an oxide having a perovskite structure was obtained in the same manner as in Example 1, except that the amount of Ti was changed to 0.0564 g.

[0074] Example 21: Synthesized SrTiO 3 For the cobalt ions incorporated in the solution, 59.1 μL of cobalt nitrate solution and C were added so that the cobalt ion ratio was 62.3%. 16 H 36 O 4 A catalyst powder containing an oxide having a perovskite structure was obtained in the same manner as in Example 1, except that the amount of Ti was changed to 0.0242 g.

[0075] Example 22: Synthesized SrTiO 3 For the cobalt ions incorporated in the sol, 71.0 μL of cobalt nitrate solution and C were added so that the cobalt ion ratio was 80.6%. 16 H 36 O 4 A catalyst powder containing an oxide having a perovskite structure was obtained in the same manner as in Example 1, except that the amount of Ti was changed to 0.0080 g.

[0076] Example 23: Synthesized SrTiO 3The molar concentration of iridium ions incorporated in SrCO was 67 mol % and the manganese ion ratio was 32.6%. 3 0.2920 g of manganese nitrate solution and 9.3 μL of C 16 H 36 O 4 A catalyst powder containing an oxide having a perovskite structure was obtained in the same manner as in Example 1, except that the amount of Ti was changed to 0.0152 g.

[0077] Comparative Example 1 Iridium ions were added to SrTiO by the Pezzini method in the same manner as in Example 1, except that no transition metal element ions were incorporated. 3 The catalyst powder was obtained containing an oxide having a perovskite structure incorporated into the starting material. 3 , C 16 H 36 O 4 Ti and K 2 IrCl 6 SrCO 3 0.2794g, K 2 IrCl 6 0.0800 g of C 6 H 8 O 7 ・H 2 0.2800 g of HCl and 0.3 mL of nitric acid (1.38) were weighed, added to 10 mL of pure water, mixed, and dissolved by stirring at room temperature for 10 minutes or more. This mixed solution was designated as Solution A. 16 H 36 O 4 Weigh out 0.1048 g of Ti and add it to 4 mL of C 2 H 6 O 2 The two were mixed and stirred for 10 minutes or more. This mixed solution was designated Solution B. The subsequent operations were carried out in the same manner as in Example 1, and the catalyst powder was recovered. The molar concentration of iridium ions relative to the total molar concentration of iridium ions and titanium ions, determined in the same manner as in Example 1, was 35 mol %.

[0078] Comparative Example 2 Iridium ions were added to strontium manganate (SrMnO) by the Pezzini method in the same manner as in Example 1, except that titanium ions were not incorporated into the B-site ions. 3The catalyst powder was obtained containing an oxide having a perovskite structure in which SrCO was incorporated into the B-site ions. 3 , K. 2 IrCl 6 and manganese nitrate hexahydrate. Manganese nitrate hexahydrate was weighed so that the manganese ion concentration was 4 M, and dissolved in water to prepare an aqueous solution. The concentration of the manganese nitrate aqueous solution was analyzed by ICP. 3 0.2794g, K 2 IrCl 6 0.0800 g of manganese nitrate solution, 76.9 μL of C 6 H 8 O 7 ・H 2 0.2800 g of HCl and 0.3 mL of nitric acid (1.38) were weighed, added to 10 mL of pure water, mixed, and dissolved by stirring at room temperature for 10 minutes or more. This mixed solution was designated Solution A. Using only Solution A, a catalyst powder was recovered in the same manner as in Example 1. The molar concentration of iridium ions relative to the total molar concentration of iridium ions and manganese ions, determined in the same manner as in Example 1, was 35 mol%, and the manganese ion ratio was 100%.

[0079] Comparative Example 3 In the same manner as in Example 6, except that titanium ions were not incorporated into the B-site ions, iridium ions were substituted for strontium nickelate (SrNiO) by the Pezzini method. 3 The catalyst powder was obtained containing an oxide having a perovskite structure in which SrCO was incorporated into the B-site ions. 3 , K. 2 IrCl 6 and nickel nitrate hexahydrate. Nickel nitrate hexahydrate was weighed so that the nickel ion concentration was 4 M, and dissolved in water to prepare an aqueous solution. The concentration of the aqueous nickel nitrate solution was analyzed by ICP. 3 0.2794g, K 2 IrCl 6 0.0800 g, 76.9 μL of nickel nitrate solution, C 6 H 8 O 7 ・H 20.2800 g of HCl and 0.3 mL of nitric acid (1.38) were weighed, added to 10 mL of pure water, mixed, and dissolved by stirring at room temperature for 10 minutes or more. This mixed solution was designated Solution A. Using only Solution A, a catalyst powder was recovered in the same manner as in Example 1. The molar concentration of iridium ions relative to the total molar concentration of iridium ions and nickel ions, determined in the same manner as in Example 1, was 35 mol%, and the proportion of nickel ions was 100%.

[0080] Comparative Example 4 Iridium ions were converted into strontium cuprate (SrCuO) by the Pezzini method in the same manner as in Example 11, except that titanium ions were not incorporated into the B-site ions. 3 The catalyst powder was obtained containing an oxide having a perovskite structure in which SrCO was incorporated into the B-site ions. 3 , K. 2 IrCl 6 and copper nitrate trihydrate. Copper nitrate trihydrate was weighed so that the copper ion concentration was 4 M, and dissolved in water to prepare an aqueous solution. The concentration of the copper nitrate aqueous solution was analyzed by ICP. 3 0.2794g, K 2 IrCl 6 0.0800 g of copper nitrate solution, 76.9 μL of C 6 H 8 O 7 ・H 2 0.2800 g of HCl and 0.3 mL of nitric acid (1.38) were weighed, added to 10 mL of pure water, mixed, and dissolved by stirring at room temperature for 10 minutes or more. This mixed solution was designated Solution A. Using only Solution A, a catalyst powder was recovered in the same manner as in Example 1. The molar concentration of iridium ions relative to the total molar concentration of iridium ions and copper ions, determined in the same manner as in Example 1, was 35 mol%, and the proportion of copper ions was 100%.

[0081] Comparative Example 5 Iridium ions were added to strontium cobaltate (SrCoO) by the Pezzini method in the same manner as in Example 19, except that titanium ions were not incorporated into the B-site ions. 3 The catalyst powder was obtained containing an oxide having a perovskite structure in which SrCO was incorporated into the B-site ions.3 , K. 2 IrCl 6 Cobalt nitrate hexahydrate was weighed so that the cobalt ion concentration was 4M, and dissolved in water to prepare an aqueous solution. The concentration of the aqueous cobalt nitrate solution was analyzed by ICP. 3 0.2794g, K 2 IrCl 6 0.0800 g of cobalt nitrate solution, 76.9 μL of C 6 H 8 O 7 ・H 2 0.2800 g of HCl and 0.3 mL of nitric acid (1.38) were weighed, added to 10 mL of pure water, mixed, and dissolved by stirring at room temperature for 10 minutes or more. This mixed solution was designated Solution A. Using only Solution A, a catalyst powder was recovered in the same manner as in Example 1. The molar concentration of iridium ions relative to the total molar concentration of iridium ions and cobalt ions, determined in the same manner as in Example 1, was 35 mol%, and the proportion of cobalt ions was 100%.

[0082] Comparative Example 6: Synthesized SrTiO 3 The molar concentration of iridium ions incorporated into the B site ions was 20 mol % and the manganese ion ratio was 23.3%. 3 0.2930 g of manganese nitrate solution and 103.3 μL of C 16 H 36 O 4 A catalyst powder containing an oxide having a perovskite structure was obtained in the same manner as in Example 1, except that the amount of Ti was changed to 0.0844 g.

[0083] [Current Density Measurement] The relationship between current density and voltage of the synthesized catalyst was evaluated at room temperature using the rotating disk electrode method. 10 mg of catalyst powder, 0.1 mL of a 5% by mass Nafion dispersion, 0.4 mL of 2-propanol, and 1.5 mL of pure water were weighed and transferred to a glass container and mixed for at least 30 minutes using a homogenizer. 10 μL of the resulting mixed solution was applied to a 5 mm diameter glassy carbon electrode. After drying, the electrode was set using a rotating disk electrode device to form a working electrode. A platinum wire was used as the counter electrode, and an aqueous Ag / AgCl reference electrode was used as the reference electrode. These electrodes and the working electrode were placed in a beaker containing 0.5 M sulfuric acid aqueous solution. After maintaining the catalyst in an open circuit for 10 minutes or more, 60 cycles of cyclic voltammetry measurements were performed at room temperature in the range of 0.05 V to 1.4 V relative to the reversible hydrogen electrode (RHE), at a sweep rate of 100 mV / sec, and at a rotation speed of 1,600 rpm, to perform electrochemical cleaning of the catalyst surface. Subsequently, 30 cycles of cyclic voltammetry measurements were performed in the range of 1.2 V to 1.6 V relative to the RHE, at a sweep rate of 5 mV / sec, and at a rotation speed of 1,600 rpm, to measure the current at 1.6 V in the first cycle and the 30th cycle. The current value was divided by the area of ​​the glassy carbon electrode to determine the current density (unit: mA / cm). 2 The current density retention rate (unit: %) was calculated based on the measurement results of the current density in the first cycle and the current density in the 30th cycle. The results are shown in Table 1.

[0084]

[0085] As shown in Table 1, Examples 1 to 23 had a higher current density retention rate than Comparative Examples 1 to 6. For example, Examples 1 to 23, in which the molar concentration of iridium ions was 30 mol % or more and transition metal element ions and titanium ions were incorporated, had a higher current density retention rate than Comparative Examples 1 to 5, which did not contain transition metal element ions or titanium ions. Furthermore, Examples 1 to 23 had a higher current density retention rate than Comparative Example 6, in which the molar concentration of iridium ions was less than 30 mol % and transition metal element ions and titanium ions were incorporated.

[0086] 2 is a graph showing the relationship between the transition metal element ion ratio and the current density retention rate in each example and each comparative example. As shown in FIG. 2, adjusting the transition metal element ion ratio tended to result in a high current density retention rate. For example, it can be seen from the graph that at threshold 1, where the transition metal element ion ratio was 5% or more and 91% or less, the current density retention rate was 60% or more; at threshold 2, where the transition metal element ion ratio was 14% or more and 82% or less, the current density retention rate was 75% or more; and at threshold 3, where the transition metal element ion ratio was 21% or more and 75% or less, the current density retention rate was 85% or more. In other words, it was found that a high current density retention rate was obtained by incorporating transition metal element ions at a molar concentration of iridium ions of 30 mol% or more, and an even higher current density retention rate could be obtained by adjusting the transition metal element ion ratio.

[0087] The disclosure of Japanese Patent Application No. 2023-085750, filed on May 24, 2023, is incorporated herein by reference in its entirety. All documents, patent applications, and technical standards described herein are incorporated by reference into this specification to the same extent as if each individual document, patent application, and technical standard was specifically and individually indicated to be incorporated by reference.

[0088] 11: Electrolyte membrane 12: Anode catalyst 13: Cathode catalyst 20: Anode gas diffusion layer 30: Cathode gas diffusion layer 40: Gasket 50: Gasket 60: Anode separator 70: Cathode separator 100: Water electrolysis cell

Claims

1. An anode catalyst comprising an oxide having a perovskite structure, the oxide further comprising a transition metal element ion, the tetravalent metal ion comprising a titanium ion, and the transition metal element ion comprising at least one type of ion selected from manganese ions, nickel ions, copper ions, iron ions, and cobalt ions, the molar concentration of which is 30 mol% or more.

2. The anode catalyst of claim 1, wherein said alkaline earth metal ions include strontium ions.

3. The anode catalyst according to claim 1, wherein the ratio of the number of moles of the transition metal element ions to the sum of the number of moles of the transition metal element ions and the tetravalent metal ions is 5% or more and 91% or less.

4. The anode catalyst according to claim 1, wherein the ratio of the number of moles of the transition metal element ions to the sum of the number of moles of the transition metal element ions and the tetravalent metal ions is 14% or more and 82% or less.

5. The anode catalyst according to claim 1, wherein the ratio of the number of moles of the transition metal element ions to the sum of the number of moles of the transition metal element ions and the tetravalent metal ions is 21% or more and 75% or less.

6. A water electrolysis cell comprising an anode gas diffusion layer, the anode catalyst according to any one of claims 1 to 5, an electrolyte membrane, a cathode catalyst, a cathode gas diffusion layer, and a separator.

7. A water electrolysis cell stack comprising a plurality of water electrolysis cells according to claim 6 stacked together.

Citation Information

Patent Citations

  • Synthesis for catelysis of bifunctional perovskite compound

    US20100140569A1

  • Electrocatalysts for efficient water electrolysis

    WO2016156599A1

Cited By

  • Separator and cell module

    WO2026172699A1