Vanadium oxide and battery using same

The novel vanadium oxide composition, specifically Li(3+x+α-y)Fe_yV_(1-x)M_xO_(4+(α/2)+y), addresses limitations in charge/discharge efficiency and capacity by enhancing electronic conductivity and lithium handling, resulting in improved battery performance for solid-state batteries.

WO2024241688A1PCT designated stage expired Publication Date: 2024-11-28PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011303
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-22
Filing Date
2024-03-22
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Current battery technologies using vanadium oxide as negative electrode active materials face limitations in achieving optimal charge and discharge characteristics and capacity due to constraints in electronic conductivity and lithium insertion/extraction efficiency.

Method used

The development of novel vanadium oxides with the composition formula Li(3+x+α-y)Fe_yV_(1-x)M_xO_(4+(α/2)+y), where 0<α<1.0, 0

Benefits of technology

The proposed vanadium oxide composition significantly improves battery capacity and charge/discharge efficiency by optimizing lithium insertion and extraction, making it suitable for high-performance solid-state batteries with enhanced energy density and output.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024011303_28112024_PF_FP_ABST
    Figure JP2024011303_28112024_PF_FP_ABST
Patent Text Reader

Abstract

This vanadium oxide is represented by compositional formula (1): Li(3+x+α-y)FeyV(1-x)MxO(4+(α / 2)+y). In the compositional formula (1), 0≤α<1.0, 0≤x<1.0, and 0<y<0.7 are satisfied, and M is at least one element selected from the group consisting of tetravalent metal elements and tetravalent metalloid elements. This battery 1000 comprises a positive electrode 201, a negative electrode 203, and an electrolyte layer 202 that is disposed between the positive electrode 201 and the negative electrode 203. The negative electrode 203 comprises the vanadium oxide according to the present disclosure.
Need to check novelty before this filing date? Find Prior Art

Description

Vanadium oxide and battery using the same

[0001] The present disclosure relates to vanadium oxides and batteries using the same.

[0002] Li3VO4 has attracted attention as a next-generation negative electrode active material due to its low reaction potential and high capacity. Patent Document 1 discloses a nonaqueous secondary battery using Li3VO4 as a negative electrode active material.

[0003] Patent Document 2 discloses (Li[3-ax+(5-b)y]A x ) (V 1-y B y The present invention discloses a co-fired all-solid-state battery using a negative electrode active material represented by the formula (I)O4. Here, A is at least one element selected from the group consisting of Mg, Al, Ga, and Zn, and B is at least one element selected from the group consisting of Zn, Al, Ga, Si, Ge, P, and Ti. x and y satisfy the conditions 0≦x≦1.0 and 0≦y≦0.6, respectively. a is the average valence of A, and b is the average valence of B.

[0004] JP 2008-77847 A International Publication No. 2019 / 044902

[0005] The present disclosure provides novel vanadium oxides that can be used as battery materials.

[0006] The present disclosure provides a composition comprising the compound of formula (1): Li (3+x+α-y) Fe y V (1-x) M x O (4+(α / 2)+y) wherein in the composition formula (1), 0≦α<1.0, 0≦x<1.0, and 0<y<0.7 are satisfied, and M is at least one element selected from the group consisting of tetravalent metal elements and tetravalent metalloid elements.

[0007] The present disclosure provides novel vanadium oxides that can be used as battery materials.

[0008] Fig. 1 shows a cross-sectional view of a battery 1000 according to the second embodiment. Fig. 2 shows a cross-sectional view of a battery 1001 according to a modified example. Fig. 3 shows a cross-sectional view of an electrode material 1100 according to the second embodiment. Fig. 4 is a graph showing the initial discharge characteristics of the battery according to Sample 1.

[0009] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings. The present disclosure is not limited to the following embodiments.

[0010] First Embodiment A vanadium oxide according to a first embodiment is represented by the following composition formula (1): In composition formula (1), 0≦α<1.0, 0≦x<1.0, and 0<y<0.7 are satisfied, and M is at least one element selected from the group consisting of tetravalent metal elements and tetravalent metalloid elements.

[0011] Li (3+x+α-y) Fe y V (1-x) M x O (4+(α / 2)+y) ...(1)

[0012] The vanadium oxide according to the first embodiment can be used as a battery material. The vanadium oxide according to the first embodiment can be used, for example, as a negative electrode active material. The vanadium oxide according to the first embodiment can be used, for example, to obtain a battery having excellent charge / discharge characteristics. The vanadium oxide according to the first embodiment is suitable, for example, for improving battery capacity. An example of the battery is a solid-state battery. The solid-state battery may be a primary battery or a secondary battery.

[0013] In composition formula (1), when 0<y<0.7 is satisfied, the capacity of a battery using the vanadium oxide according to the first embodiment is improved, for example. This is because the doping of Fe improves the electronic conductivity of the vanadium oxide, facilitating the insertion and desorption of Li into and from the vanadium oxide.

[0014] The amount of Fe and O represented by y in composition formula (1) may be incorporated into the vanadium oxide particles, or may exist outside the particles as a second phase different from the first phase constituting the particles.

[0015] In the composition formula (1), 0.183≦y≦0.61 may be satisfied. With this configuration, the vanadium oxide according to the first embodiment can improve the battery capacity.

[0016] The upper and lower limits of the range of y in composition formula (1) may be defined by any combination selected from the following values: greater than 0.0 (0<y), 0.092, 0.183, 0.244, 0.366, 0.610, and less than 0.7 (y<0.7).

[0017] In composition formula (1), the capacity of a battery using the vanadium oxide according to the first embodiment is also improved by satisfying 0≦α<1.0, because this facilitates the insertion and desorption of Li into and from the vanadium oxide according to the first embodiment.

[0018] In composition formula (1), 0 < α < 1.0 may be satisfied. That is, the vanadium oxide according to the first embodiment may contain Li and O in amounts exceeding those derived from the stoichiometric composition. With this configuration, the vanadium oxide according to the first embodiment can improve battery capacity. This is because the excess Li and O improve the electronic conductivity of the vanadium oxide, facilitating the insertion and desorption of Li into the vanadium oxide according to the first embodiment. A stoichiometric composition means a composition in which the molar ratios of the elements constituting the vanadium oxide are an integer multiple. For example, Li3VO4 has a stoichiometric composition.

[0019] The amount of Li and O represented by α in composition formula (1) may be incorporated within the vanadium oxide particles, or may exist outside the particles as a second phase different from the first phase constituting the particles. Note that the vanadium oxides disclosed in Patent Documents 1 and 2 do not contain Li and O equivalent to the amount represented by α.

[0020] In the composition formula (1), 0≦α<0.85 or 0<α<0.85 may be satisfied. According to this configuration, the vanadium oxide according to the first embodiment can improve the battery capacity.

[0021] In the composition formula (1), 0.2≦α≦0.6 may be satisfied. With this configuration, the vanadium oxide according to the first embodiment can improve the battery capacity.

[0022] The upper and lower limits of the range of α in composition formula (1) may be defined by any combination selected from the following values: 0 or more (0≦α), greater than 0 (0<α), 0.171, 0.219, 0.258, 0.277, 0.287, 0.301, 0.316, 0.589, 0.85, and less than 1.0 (α<1.0).

[0023] In composition formula (1), 0<x<1.0 may be satisfied. With this configuration, the vanadium oxide according to the first embodiment can improve battery capacity. This is thought to be because the electronic conductivity of the vanadium oxide is improved by replacing some of the vanadium ions with ions of the metal M.

[0024] In composition formula (1), 0<x≦0.1 may be satisfied. With this configuration, the vanadium oxide according to the first embodiment can improve battery capacity. x may be in the range of 0.04 to 0.06, or may be 0.05.

[0025] In the composition formula (1), when x satisfies the above range, insertion and desorption of Li into and from the vanadium oxide according to the first embodiment is further facilitated, and therefore, as described above, the vanadium oxide according to the first embodiment can improve the battery capacity.

[0026] As described above, M is at least one element selected from tetravalent metal elements and tetravalent metalloid elements. Examples of tetravalent metal elements and tetravalent metalloid elements include Ti, Zr, Si, Ge, and Sn. When the pentavalent V element is substituted with a tetravalent metal element and / or a tetravalent metalloid element, holes and / or Li ions become charge carriers. This makes it easier to insert and extract Li into the vanadium oxide.

[0027] In the composition formula (1), M may contain Ti. According to this structure, the vanadium oxide according to the first embodiment can improve the battery capacity. M may be Ti.

[0028] The vanadium oxide according to the first embodiment may have a β-phase crystalline phase, a γ-phase crystalline phase, or both of these crystalline phases. The vanadium oxide according to the first embodiment may have only a β-phase crystalline phase.

[0029] The shape of the vanadium oxide according to the first embodiment is not limited. Examples of the shape include needle-like, spherical, and oval-spherical shapes. The vanadium oxide according to the first embodiment may be in the form of particles. The vanadium oxide according to the first embodiment may be formed into the shape of a pellet or a plate.

[0030] When the vanadium oxide according to the first embodiment is particulate (e.g., spherical), the vanadium oxide particles may have a median diameter of 0.1 μm or more and 100 μm or less, or may have a median diameter of 0.5 μm or more and 10 μm or less. This allows the vanadium oxide according to the first embodiment and other materials, such as a solid electrolyte, to be dispersed well.

[0031] The median particle size refers to the particle size (d50) corresponding to 50% cumulative volume in the volume-based particle size distribution. The volume-based particle size distribution can be measured using a laser diffraction measurement device or an image analysis device.

[0032] <Method for Producing Vanadium Oxide> The vanadium oxide according to the first embodiment can be produced by the following method.

[0033] Raw material powders are prepared to have a desired composition, and examples of raw material powders include oxides, hydroxides, carbonates, nitrates, and organic salts.

[0034] As an example, the composition formula (1): Li (3+x+α-y) Fe y V (1-x) M x O (4+(α / 2)+y)In the vanadium oxide represented by the formula (1), it is assumed that M is Ti, and that x, α, and Fe are 0.1 when the raw materials are mixed. In this case, LiCO, VO, TiO, and FeO are mixed in a molar ratio of LiCO:VO:TiO:FeO=(2.95 / 2):(0.95 / 2):0.05:0.1.

[0035] When α≠0, a Li source material, for example, Li2CO3, may be further added and mixed with the raw material powder, taking into consideration the value of α in the target composition. The amount of the excess Li source to be mixed in excess can be determined appropriately depending on, for example, the value of α in the target composition and the material used as the Li source. For example, to produce a vanadium oxide that satisfies 0<x<1.0 and 0<α<1.0, the Li source may be used in excess in the range of, for example, 0.5% by mass to 40% by mass, or 1% by mass to 30% by mass, relative to the amount of the Li source whose molar ratio is determined assuming that α is 0.

[0036] Lithium hydroxide or its hydrate may be used instead of Li2CO3.

[0037] The mixture of raw material powders is fired to obtain a reaction product. The firing atmosphere may be air or an inert gas atmosphere. The inert atmosphere is, for example, an argon atmosphere or a nitrogen atmosphere.

[0038] Alternatively, a mixture of raw material powders may be reacted with each other mechanochemically (by mechanochemical milling) in a mixing device such as a planetary ball mill to obtain a reactant.

[0039] By these methods, the vanadium oxide according to the first embodiment can be obtained.

[0040] Here, the molar ratio of the raw materials when mixed does not necessarily match the molar ratio of the reactants, because the raw materials may not be incorporated into the reactants due to evaporation during the reaction.

[0041] The composition of vanadium oxide is determined by quantitative analysis. Li is quantified by atomic absorption spectrometry. V, Fe, and M are quantified by inductively coupled plasma (ICP) atomic emission spectrometry. The value of x in composition formula (1) can be determined from the amount of element M in the vanadium oxide. The value of y in composition formula (1) can be determined from the amount of Fe in the vanadium oxide. The value of α in composition formula (1) can be determined from the amount of Li, the amount of Fe, and the amount of element M in the vanadium oxide.

[0042] Second Embodiment A second embodiment will be described below, and the matters described in the first embodiment will be omitted as appropriate.

[0043] The battery according to the second embodiment includes a positive electrode, an electrolyte layer, and a negative electrode. The electrolyte layer is disposed between the positive electrode and the negative electrode. The negative electrode includes the vanadium oxide according to the first embodiment.

[0044] The battery according to the second embodiment has excellent charge / discharge characteristics.

[0045] FIG. 1 shows a cross-sectional view of a battery 1000 according to a second embodiment.

[0046] The battery 1000 includes a positive electrode 201, an electrolyte layer 202, and a negative electrode 203. The electrolyte layer 202 is disposed between the positive electrode 201 and the negative electrode 203.

[0047] The positive electrode 201 contains positive electrode active material particles 204 and solid electrolyte particles 100 .

[0048] The electrolyte layer 202 contains an electrolyte material, such as a solid electrolyte material.

[0049] The negative electrode 203 contains negative electrode active material particles 205 and solid electrolyte particles 100 .

[0050] The negative electrode active material particles 205 are particles containing the vanadium oxide according to the first embodiment. The negative electrode active material particles 205 may be particles containing the vanadium oxide according to the first embodiment as a main component. Particles containing the vanadium oxide according to the first embodiment as a main component refer to particles in which the vanadium oxide according to the first embodiment is the component contained in the largest amount by mass ratio. The negative electrode active material particles 205 may be particles made of the vanadium oxide according to the first embodiment. The shape of the negative electrode active material particles 205 is, for example, spherical.

[0051] The negative electrode active material particles 205 may have a median diameter of 0.1 μm or more and 100 μm or less. When the negative electrode active material particles 205 have a median diameter of 0.1 μm or more, the negative electrode active material particles 205 and the solid electrolyte particles 100 can be well dispersed in the negative electrode 203. This improves the charge / discharge characteristics of the battery. When the negative electrode active material particles 205 have a median diameter of 100 μm or less, the lithium diffusion rate within the negative electrode active material particles 205 improves. This allows the battery 1000 to operate at high output.

[0052] The negative electrode active material particles 205 may have a larger median diameter than the solid electrolyte particles 100. This allows the negative electrode active material particles 205 and the solid electrolyte particles 100 to be dispersed well.

[0053] In order to improve the energy density and output of the battery 1000, in the negative electrode 203, the ratio of the volume of the negative electrode active material particles 205 to the sum of the volume of the negative electrode active material particles 205 and the volume of the solid electrolyte particles 100 may be 0.30 or more and 0.95 or less.

[0054] To improve the energy density and output of the battery 1000, the negative electrode 203 may have a thickness of 10 μm or more and 500 μm or less.

[0055] The solid electrolyte particles 100 contained in the negative electrode 203 may be a sulfide solid electrolyte, a halide solid electrolyte, an oxide solid electrolyte, or a polymer solid electrolyte.

[0056] In the present disclosure, a "sulfide solid electrolyte" refers to a solid electrolyte containing sulfur. An "oxide solid electrolyte" refers to a solid electrolyte containing oxygen. The oxide solid electrolyte may contain anions other than oxygen (excluding sulfur anions and halogen anions). A "halide solid electrolyte" refers to a solid electrolyte that contains a halogen element but does not contain sulfur. The halide solid electrolyte may contain not only a halogen element but also oxygen.

[0057] Examples of sulfide solid electrolytes include Li2S-P2S5, Li2S-SiS2, Li2S-B2S3, Li2S-GeS2, and Li 3.25 Ge 0.25 P 0.75 S4, Li 10 GeP2S 12 And so on.

[0058] Examples of halide solid electrolytes include Li a Me b Y c X6, where the formula: a + mb + 3c = 6, and c > 0 is satisfied. Me is at least one element selected from the group consisting of metal elements other than Li and Y and metalloid elements. X is at least one element selected from the group consisting of F, Cl, Br, and I. The value of m represents the valence of Me.

[0059] "Metalloid elements" are B, Si, Ge, As, Sb, and Te. "Metal elements" are all elements in groups 1 to 12 of the periodic table (except H) and all elements in groups 13 to 16 of the periodic table (except B, Si, Ge, As, Sb, Te, C, N, P, O, S, and Se).

[0060] In order to increase the ionic conductivity of the halide solid electrolyte, Me may be at least one selected from the group consisting of Mg, Ca, Sr, Ba, Zn, Sc, Al, Ga, Bi, Zr, Hf, Ti, Sn, Ta, and Nb.

[0061] Another example of a halide solid electrolyte is Li α’ Me' β Oγ X δ where α', β, γ, and δ are all greater than 0, Me' is at least one element selected from the group consisting of metal elements and metalloid elements other than Li, X is at least one element selected from the group consisting of Cl, Br, and I, and the following mathematical formulas are satisfied: 0.9≦α'≦1.2, β=1.0, 1.0≦γ≦1.3, and 3.6≦δ≦4.0.

[0062] Examples of oxide solid electrolytes include: (i) NASICON-type solid electrolytes such as LiTi2(PO4)3 and elemental substitution products thereof; (ii) perovskite-type solid electrolytes such as (LaLi)TiO3; (iii) Li 14 ZnGeO 16 LISICON-type solid electrolytes such as LiSiO, LiGeO, and elemental substitution products thereof; (iv) LiLaZrO 12 (v) Li3PO4 or an N-substituted LiPO4, etc.

[0063] An example of a polymer solid electrolyte is a compound of a polymer compound and a lithium salt. The polymer compound may have an ethylene oxide structure. A polymer compound having an ethylene oxide structure can contain a large amount of lithium salt, and therefore has higher ionic conductivity. The polymer solid electrolyte may be, for example, a composite compound of polyethylene oxide and a lithium salt. An example of such a polymer solid electrolyte is lithium bis(trifluoromethanesulfonyl)imide.

[0064] Examples of lithium salts include LiPF, LiBF, LiSbF, LiAsF, LiSOCF, LiN(SOCF), LiN(SOCF), LiN(SOCF)(SOCF), LiC(SOCF), etc. One lithium salt selected from these may be used alone. Alternatively, a mixture of two or more lithium salts selected from these may be used.

[0065] The positive electrode 201 contains a material capable of absorbing and releasing metal ions such as lithium ions, and also contains, for example, a positive electrode active material (for example, positive electrode active material particles 204).

[0066] Examples of the positive electrode active material include lithium-containing transition metal oxides, transition metal fluorides, polyanion materials, fluorinated polyanion materials, transition metal sulfides, transition metal oxysulfides, transition metal oxynitrides, etc. Examples of lithium-containing transition metal oxides include Li(Ni,Co,Al)O, Li(Ni,Co,Mn)O, LiCoO, etc.

[0067] In the present disclosure, "(A, B, C)" means "at least one selected from the group consisting of A, B, and C."

[0068] From the viewpoint of cost and safety of the battery 1000, lithium phosphate or lithium-containing transition metal phosphate may be used as the positive electrode active material.

[0069] The positive electrode active material particles 204 may have a median diameter of 0.1 μm or more and 100 μm or less. When the positive electrode active material particles 204 have a median diameter of 0.1 μm or more, the positive electrode active material particles 204 and the solid electrolyte particles 100 can be well dispersed in the positive electrode 201. This improves the charge / discharge characteristics of the battery. When the positive electrode active material particles 204 have a median diameter of 100 μm or less, the lithium diffusion rate within the positive electrode active material particles 204 improves. This allows the battery 1000 to operate at high power.

[0070] The positive electrode active material particles 204 may have a larger median diameter than the solid electrolyte particles 100. This allows the positive electrode active material particles 204 and the solid electrolyte particles 100 to be dispersed well.

[0071] In order to improve the energy density and output of the battery 1000, in the positive electrode 201, the ratio of the volume of the positive electrode active material particles 204 to the sum of the volume of the positive electrode active material particles 204 and the volume of the solid electrolyte particles 100 may be 0.30 or more and 0.95 or less.

[0072] A coating layer may be formed on the surface of the positive electrode active material particles 204 to prevent the positive electrode active material particles 204 from reacting with the solid electrolyte particles 100. This can suppress an increase in the reaction overvoltage of the battery. Examples of coating materials contained in the coating layer include solid electrolytes such as sulfide solid electrolytes, oxide solid electrolytes, polymer solid electrolytes, and halide solid electrolytes.

[0073] The coating material may be a halide solid electrolyte or an oxide solid electrolyte. The halide solid electrolyte may contain F. This improves the stability of the coating material at high potentials. As a result, the battery 1000 has high charge / discharge efficiency. The oxide solid electrolyte may be lithium niobate or a polyanion material, which has excellent stability even at high potentials. As a result, the battery 1000 has high charge / discharge efficiency.

[0074] To improve the energy density and output of the battery 1000, the positive electrode 201 may have a thickness of 10 μm or more and 500 μm or less.

[0075] The solid electrolyte particles 100 contained in the positive electrode 201 may be a solid electrolyte such as a sulfide solid electrolyte, a halide solid electrolyte, an oxide solid electrolyte, a polymer solid electrolyte, or an organic polymer solid electrolyte.

[0076] The electrolyte layer 202 contains an electrolyte material. The electrolyte material is, for example, a solid electrolyte material. The electrolyte layer 202 may be a solid electrolyte layer. The solid electrolyte material contained in the electrolyte layer 202 may be a sulfide solid electrolyte, a halide solid electrolyte, or a polymer solid electrolyte.

[0077] The electrolyte layer 202 may have a thickness of 1 μm or more and 100 μm or less. When the electrolyte layer 202 has a thickness of 1 μm or more, the positive electrode 201 and the negative electrode 203 are less likely to short-circuit. When the electrolyte layer 202 has a thickness of 100 μm or less, the battery 1000 can operate at high power.

[0078] At least one selected from the group consisting of the positive electrode 201, the electrolyte layer 202, and the negative electrode 203 may contain a non-aqueous electrolyte, a gel electrolyte, or an ionic liquid for the purpose of facilitating the exchange of lithium ions and improving the output characteristics of the battery.

[0079] The nonaqueous electrolyte contains a nonaqueous solvent and a lithium salt dissolved in the nonaqueous solvent. Examples of the nonaqueous solvent include cyclic carbonate ester solvents, chain carbonate ester solvents, cyclic ether solvents, chain ether solvents, cyclic ester solvents, chain ester solvents, and fluorine solvents. Examples of the cyclic carbonate ester solvents include ethylene carbonate, propylene carbonate, and butylene carbonate. Examples of the chain carbonate ester solvents include dimethyl carbonate, ethyl methyl carbonate, and diethyl carbonate. Examples of the cyclic ether solvents include tetrahydrofuran, 1,4-dioxane, and 1,3-dioxolane. Examples of the chain ether solvents include 1,2-dimethoxyethane and 1,2-diethoxyethane. An example of the cyclic ester solvent is γ-butyrolactone. An example of the chain ester solvent is methyl acetate. Examples of fluorine-containing solvents include fluoroethylene carbonate, methyl fluoropropionate, fluorobenzene, fluoroethyl methyl carbonate, and fluorodimethylene carbonate. One nonaqueous solvent selected from these may be used alone. Alternatively, a mixture of two or more nonaqueous solvents selected from these may be used.

[0080] Examples of lithium salts include LiPF, LiBF, LiSbF, LiAsF, LiSOCF, LiN(SOCF), LiN(SOCF), LiN(SOCF)(SOCF), and LiC(SOCF). One lithium salt selected from these may be used alone. Alternatively, a mixture of two or more lithium salts selected from these may be used. The concentration of the lithium salt is, for example, in the range of 0.5 mol / L to 2 mol / L.

[0081] The gel electrolyte may be a polymer material impregnated with a non-aqueous electrolyte solution, such as polyethylene oxide, polyacrylonitrile, polyvinylidene fluoride, polymethyl methacrylate, or a polymer having an ethylene oxide bond.

[0082] Examples of cations contained in the ionic liquid include: (i) aliphatic chain quaternary salts such as tetraalkylammonium and tetraalkylphosphonium; (ii) aliphatic cyclic ammoniums such as pyrrolidiniums, morpholiniums, imidazoliniums, tetrahydropyrimidiniums, piperaziniums, and piperidiniums; and (iii) nitrogen-containing heterocyclic aromatic cations such as pyridiniums and imidazoliums.

[0083] An example of an anion contained in an ionic liquid is PF6 - , BF4 - , SbF6 - , AsF6 - , SO3CF3 - , N(SO2CF3)2 - , N(SO2C2F5)2 - , N(SO2CF3)(SO2C4F9) - , C(SO2CF3)3 - And so on.

[0084] The ionic liquid may contain a lithium salt.

[0085] At least one selected from the group consisting of the positive electrode 201, the electrolyte layer 202, and the negative electrode 203 may contain a binder for the purpose of improving adhesion between particles.

[0086] Examples of binders include polyvinylidene fluoride, polytetrafluoroethylene, polyethylene, polypropylene, aramid resin, polyamide, polyimide, polyamideimide, polyacrylonitrile, polyacrylic acid, polymethyl ester of acrylic acid, polyethyl ester of acrylic acid, polyhexyl ester of acrylic acid, polymethacrylic acid, polymethyl ester of methacrylic acid, polyethyl ester of methacrylic acid, polyhexyl ester of methacrylic acid, polyvinyl acetate, polyvinylpyrrolidone, polyether, polyethersulfone, hexafluoropolypropylene, styrene-butadiene rubber, and carboxymethyl cellulose. Copolymers may also be used as binders. Examples of such binders include copolymers of two or more materials selected from the group consisting of tetrafluoroethylene, hexafluoroethylene, hexafluoropropylene, perfluoroalkyl vinyl ether, vinylidene fluoride, chlorotrifluoroethylene, ethylene, propylene, pentafluoropropylene, fluoromethyl vinyl ether, acrylic acid, and hexadiene. Mixtures of two or more materials selected from the above materials may also be used.

[0087] At least one selected from the positive electrode 201 and the negative electrode 203 may contain a conductive additive for the purpose of increasing electronic conductivity.

[0088] Examples of the conductive additive include: (i) graphites such as natural graphite and artificial graphite, (ii) carbon blacks such as acetylene black and ketjen black, (iii) conductive fibers such as carbon fiber and metal fiber, (iv) carbon fluoride, (v) metal powders such as aluminum, (vi) conductive whiskers such as zinc oxide and potassium titanate, (vii) conductive metal oxides such as titanium oxide, and (viii) conductive polymer compounds such as polyaniline, polypyrrole, and polythiophene. To reduce costs, the conductive additives (i) or (ii) above may be used.

[0089] The negative electrode 203 may contain not only the negative electrode active material particles 205 but also a conductive additive 207. Examples of materials for the conductive additive 207 are as described above.

[0090] The conductive additive 207 may cover at least a part of the surface of the negative electrode active material particles 205. This increases the contact area between the conductive additive 207 and the negative electrode active material particles 205. As a result, the battery resistance decreases, and the output can be increased.

[0091] In the negative electrode 203, the ratio of the volume of the conductive additive 207 to the total volume of the negative electrode active material particles 205 and the conductive additive 207 may be 0.01 or more and 0.4 or less.

[0092] FIG. 2 shows a cross-sectional view of a battery 1001 according to a modified example. As shown in FIG. 2 , another electrolyte layer (i.e., a second electrolyte layer) may be further provided between the electrolyte layer 202 and the negative electrode 203. When the electrolyte layer 202 is composed of a first electrolyte layer 212 and a second electrolyte layer 222, the second electrolyte layer 222 may be composed of a different solid electrolyte material that is electrochemically more stable than the first electrolyte layer 212. Specifically, the reduction potential of the solid electrolyte material constituting the second electrolyte layer 222 may be lower than the reduction potential of the solid electrolyte material constituting the first electrolyte layer 212. This allows the solid electrolyte material contained in the first electrolyte layer 212 to be used without being reduced. As a result, the charge / discharge efficiency of the battery 1001 can be improved.

[0093] FIG. 3 shows a cross-sectional view of an electrode material 1100 according to a second embodiment. The electrode material 1100 shown in FIG. 3 may be contained in the negative electrode 203. In order to prevent the solid electrolyte particles 100 from reacting with the negative electrode active material (i.e., the electrode active material particles 206), a coating layer 216 may be formed on the surface of the electrode active material particles 206. This allows the battery to have high charge / discharge efficiency. Therefore, the vanadium oxide according to the first embodiment contained in the negative electrode 203 may be coated with a coating material.

[0094] Examples of the coating material contained in the coating layer 216 include a sulfide solid electrolyte, an oxide solid electrolyte, a polymer solid electrolyte, and a halide solid electrolyte.

[0095] An example of a sulfide solid electrolyte is Li2S-P2S5. An example of an oxide solid electrolyte is trilithium phosphate. An example of a polymer solid electrolyte is a composite compound of polyethylene oxide and a lithium salt. An example of such a polymer solid electrolyte is lithium bis(trifluoromethanesulfonyl)imide.

[0096] Examples of the shape of the battery according to the second embodiment include coin type, cylindrical type, square type, sheet type, button type, flat type, and laminate type.

[0097] The battery according to the second embodiment may be manufactured, for example, by preparing a material for forming a positive electrode, a material for forming an electrolyte layer, and a material for forming a negative electrode, and by a known method, fabricating a laminate in which the positive electrode, the electrolyte layer, and the negative electrode are arranged in this order.

[0098] (Other Embodiments) (Additional Notes) The above description of the embodiments discloses the following techniques.

[0099] (Technology 1) Composition formula (1): Li (3+x+α-y) Fe y V (1-x) M x O (4+(α / 2)+y) wherein, in the composition formula (1), 0≦α<1.0, 0≦x<1.0, and 0<y<0.7 are satisfied, and M is at least one element selected from the group consisting of tetravalent metal elements and tetravalent metalloid elements.

[0100] The vanadium oxide according to Technology 1 is a novel substance that can be used as a battery material. The vanadium oxide according to Technology 1 can be used, for example, as a negative electrode active material. The vanadium oxide according to Technology 1 is suitable for improving, for example, the charge / discharge characteristics of a battery, and is suitable for improving, for example, the battery capacity.

[0101] (Technology 2) The vanadium oxide according to Technology 1, wherein in the composition formula (1), M contains Ti.

[0102] (Technology 3) The vanadium oxide according to Technology 1 or 2, wherein in the composition formula (1), 0≦α<0.85 is satisfied.

[0103] (Technology 4) The vanadium oxide according to Technology 1 or 2, wherein in the composition formula (1), 0<α<1.0 is satisfied.

[0104] (Technology 5) The vanadium oxide according to Technology 1 or 2, wherein in the composition formula (1), 0.2≦α≦0.6 is satisfied.

[0105] (Technology 6) The vanadium oxide according to any one of Technologies 1 to 5, wherein in the composition formula (1), 0<x<1.0 is satisfied.

[0106] (Technology 7) The vanadium oxide according to any one of Technologies 1 to 5, wherein in the composition formula (1), 0<x≦0.1 is satisfied.

[0107] (Technology 8) The vanadium oxide according to any one of Technologies 1 to 7, wherein in the composition formula (1), 0.183≦y≦0.61 is satisfied.

[0108] The vanadium oxides of techniques 2 to 8 are more suitable for improving the battery capacity.

[0109] (Technology 9) A battery comprising: a positive electrode; a negative electrode; and an electrolyte layer disposed between the positive electrode and the negative electrode, wherein the negative electrode contains the vanadium oxide according to any one of Technologies 1 to 8.

[0110] The battery according to Technique 9 has excellent charge / discharge characteristics.

[0111] (Technology 10) The battery according to Technology 9, wherein the negative electrode further contains a conductive additive. The battery according to Technology 10 can increase the electronic conductivity of the negative electrode. Therefore, the battery according to Technology 9 has better charge / discharge characteristics.

[0112] The present disclosure will be described in more detail below. Each sample of vanadium oxide was prepared according to the formula (1): Li (3+x+α-y) Fe y V (1-x) M x O (4+(α / 2)+y) It can be expressed as:

[0113] Sample 1 Preparation of Vanadium Oxide Raw material powders were prepared: Li2CO3 (manufactured by Kojundo Chemical Laboratory Co., Ltd., purity 99.9%), VO (manufactured by Kojundo Chemical Laboratory Co., Ltd., purity 99.9%), TiO2 (manufactured by Kojundo Chemical Laboratory Co., Ltd., purity 99.9%), and FeO (manufactured by Kojundo Chemical Laboratory Co., Ltd., purity 99.9%), in a molar ratio of Li2CO3:VO5:TiO2:FeO = 1.525:0.475:0.05:0.092. Furthermore, the Li2CO3 was prepared in an amount 10 wt% in excess of the above composition. These raw material powders were mixed in a mortar to obtain a mixed powder. The obtained mixed powder was calcined in air at 600°C for 3 hours. The calcined powder was then fired in air at 920°C for 15 hours. In both the pre-firing and the firing, the temperature increase rate was 10° C. per minute, and the temperature decrease rate was 5° C. per minute. In this way, vanadium oxide according to Sample 1 was obtained.

[0114] In the vanadium oxide of Sample 1, x in the composition formula (1) was 0.05, y was 0.092, and α was 0.301.

[0115] x and y were determined by analyzing the Ti and Fe amounts using an ICP optical emission spectrometer (PS3520VDDII manufactured by Hitachi High-Tech Science Corporation). α was determined by analyzing the Li amount using an atomic absorption spectrophotometer (Z-2300 manufactured by Hitachi High-Tech Norges Corporation), and then using the results of the analysis, the Ti amount (i.e., the value of x), and the Fe amount (i.e., the value of y).

[0116] [Battery Fabrication] Vanadium oxide according to Sample 1 and solid electrolyte Li3PS4 were prepared in an argon atmosphere with a dew point of -60°C or less, at a volume ratio of vanadium oxide:Li3PS4 = 60:40. Furthermore, 5 parts by mass of acetylene black was prepared for every 100 parts by mass of vanadium oxide. These materials were mixed in an agate mortar. In this way, a negative electrode mixture was obtained.

[0117] A solid electrolyte Li3PS4 (80 mg) and a negative electrode mixture (6.5 mg) were stacked in an insulating cylinder with an inner diameter of 9.5 mm to obtain a laminate. A pressure of 360 MPa was applied to this laminate to form a solid electrolyte layer and a negative electrode. The solid electrolyte layer had a thickness of 500 μm.

[0118] Next, Li (thickness: 300 μm) was laminated on the solid electrolyte layer, and a pressure of 80 MPa was applied to this laminate to form a positive electrode.

[0119] Next, current collectors made of stainless steel were attached to the positive and negative electrodes, and current collecting leads were attached to the current collectors.

[0120] Finally, the inside of the insulating tube was isolated from the outside atmosphere using an insulating ferrule, and the inside of the tube was sealed.

[0121] As a result, a battery using Sample 1 was obtained. The battery using Sample 1 is a single-electrode test cell with the negative electrode as the working electrode and the positive electrode as the counter electrode, and is used to test the performance of the negative electrode. Specifically, the negative electrode to be tested is used as the working electrode, and an appropriate active material in an amount sufficient to cover the reaction at the working electrode is used as the counter electrode. Since this test cell is intended to test the performance of the negative electrode, metallic Li was used as the counter electrode. The negative electrode whose performance has been tested using such a test cell can be used as a secondary battery, for example, by combining it with a positive electrode containing a positive electrode active material such as that described in the above embodiment, such as a transition metal oxide containing Li.

[0122] [Charge / Discharge Test] Fig. 4 is a graph showing the initial discharge characteristics of the battery of Sample 1. The horizontal axis represents the discharge capacity, and the vertical axis represents the voltage. The results shown in Fig. 4 were measured by the following method.

[0123] A charge-discharge test was conducted using a battery of Sample 1 as follows. As described above, the battery fabricated using Sample 1 was a single-electrode test cell, corresponding to a half cell of the negative electrode. Therefore, for Sample 1, the direction in which Li ions are inserted into the negative electrode and the potential of the half cell decreases is referred to as charging, and the direction in which the potential increases is referred to as discharging. In other words, charging for Sample 1 is essentially discharging (i.e., in the case of a full cell), and discharging for Sample 1 is essentially charging.

[0124] The battery according to Sample 1 was placed in a thermostatic chamber maintained at 25°C.

[0125] The battery of Sample 1 was discharged at a current value corresponding to a 1 C rate (1 hour rate) relative to the theoretical capacity of the battery until the voltage reached 0.3 V. Next, the battery of Sample 1 was charged at a current value corresponding to a 0.05 C rate until the voltage reached 2.5 V.

[0126] As a result of the charge-discharge test, the battery of Sample 1 had an initial discharge capacity of 157 mAh / g.

[0127] Samples 2 to 10 Preparation of Vanadium Oxide For Sample 2, LiCO, VO, TiO, and FeO were prepared in a molar ratio of LiCO:VO:TiO:FeO = 1.434:0.475:0.05:0.183, where x was 0.05, y was 0.183, and α was 0.287.

[0128] In Sample 3, LiCO, VO, TiO, and FeO were prepared in a molar ratio of LiCO:VO:TiO:FeO = 1.403:0.475:0.05:0.244, where x was 0.05, y was 0.244, and α was 0.277.

[0129] In Sample 4, LiCO, VO, TiO, and FeO were prepared in a molar ratio of LiCO:VO:TiO:FeO = 1.342:0.475:0.05:0.366, where x was 0.05, y was 0.366, and α was 0.258.

[0130] In Sample 5, LiCO, VO, TiO, and FeO were prepared in a molar ratio of LiCO:VO:TiO:FeO = 1.220:0.475:0.05:0.610, where x was 0.05, y was 0.610, and α was 0.219.

[0131] In Sample 6, Li2CO3, VO, TiO2, and FeO were prepared in a molar ratio of Li2CO3:VO:TiO2:FeO = 1.434:0.475:0.05:0.183. No excess Li2CO3 was added to Sample 6. x was 0.05, y was 0.183, and α was 0.

[0132] For Sample 7, Li2CO3, VO, TiO2, and FeO were prepared in a molar ratio of Li2CO3:VO:TiO2:FeO = 1.434:0.475:0.05:0.183. For Sample 7, Li2CO3 was prepared in 20 wt% excess. x was 0.05, y was 0.183, and α was 0.589.

[0133] In Sample 8, Li2CO3, VO, TiO2, and FeO were prepared in a molar ratio of Li2CO3:VO:TiO2:FeO = 1.434:0.475:0.05:0.183. In Sample 8, Li2CO3 was prepared in 30 wt% excess. x was 0.05, y was 0.183, and α was 0.891.

[0134] In Sample 9, Li2CO3, VO, and TiO2 were prepared in a molar ratio of Li2CO3:VO:TiO2 = 1.525:0.475:0.05, x was 0.05, y was 0, and α was 0.316.

[0135] In Sample 10, LiCO, VO, TiO, and FeO were prepared in a molar ratio of LiCO:VO:TiO:FeO = 1.068:0.475:0.05:0.915, where x was 0.05, y was 0.920, and α was 0.171.

[0136] Other than the above, vanadium oxides according to Samples 2 to 10 were obtained in the same manner as Sample 1.

[0137] [Charge-Discharge Test] Batteries using the vanadium oxides of Samples 2 to 10 as negative electrodes were fabricated in the same manner as Sample 1, and the initial discharge capacity was measured in the same manner as Sample 1. The measurement results are shown in Table 1.

[0138]

[0139] <<Discussion>> As can be seen from Table 1, the battery using the vanadium oxide represented by composition formula (1) as the active material had a high discharge capacity.

[0140] As can be seen from a comparison of Samples 1 to 8 with Sample 9, when y was greater than 0 and equal to or less than 0.61, a high discharge capacity was confirmed.

[0141] From the results of Sample 6 and Sample 10, if y is too large, the discharge capacity is lost. Since y for Sample 6 is 0.610 and y for Sample 10 is 0.920, it can be considered that the upper limit of y is around 0.7.

[0142] As can be seen from a comparison of Samples 1 to 7 with Sample 8, when α was smaller than 0.891, a high discharge capacity was confirmed.

[0143] As can be seen from a comparison between Sample 6 and Sample 7, when α was greater than 0, a higher discharge capacity was confirmed.

[0144] As described above, the vanadium oxide according to the present disclosure is suitable for providing a battery with excellent charge-discharge characteristics.

[0145] The vanadium oxide of the present disclosure is used as a battery material, for example, as a material for all-solid-state lithium-ion secondary batteries.

Claims

1. Composition formula (1): Li (3+x+α-y) Fe y V (1-x) M x O (4+(α / 2)+y) wherein in said composition formula (1), 0≦α<1.0, 0≦x<1.0, and 0<y<0.7 are satisfied, and M is at least one element selected from the group consisting of tetravalent metal elements and tetravalent metalloid elements.

2. The vanadium oxide according to claim 1, wherein in the composition formula (1), M contains Ti.

3. The vanadium oxide according to claim 1, wherein in the composition formula (1), 0≦α<0.85 is satisfied.

4. The vanadium oxide according to claim 1, wherein in the composition formula (1), 0<α<1.0 is satisfied.

5. The vanadium oxide according to claim 1, wherein in the composition formula (1), 0.2≦α≦0.6 is satisfied.

6. The vanadium oxide according to claim 1, wherein in the composition formula (1), 0<x<1.0 is satisfied.

7. The vanadium oxide according to claim 1, wherein in the composition formula (1), 0<x≦0.1 is satisfied.

8. The vanadium oxide according to claim 1, wherein in the composition formula (1), 0.183≦y≦0.61 is satisfied.

9. A battery comprising: a positive electrode; a negative electrode; and an electrolyte layer disposed between said positive electrode and said negative electrode, said negative electrode comprising the vanadium oxide of claim 1.

10. The battery according to claim 9, wherein the negative electrode further comprises a conductive additive.

Citation Information

Patent Citations

  • Composite oxide containing lithium and iron and method for manufacturing the same

    JP2010126399A

  • Oxide-based solid electrolyte and all-solid lithium ion battery

    JP2023110591A