Pulp-molded product and method for manufacturing same
By combining pulp with specific fiber and additive compositions and processing methods, the pulp molded products achieve high mechanical strength and rapid dehydration, addressing the issues of low strength and prolonged dehydration times in existing technologies.
Patent Information
- Application Number
- PCT/JP2024/014702
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-25
- Filing Date
- 2024-04-11
- Publication Date
- 2024-11-28
AI Technical Summary
Pulp molded products often have low mechanical strength and require extended dehydration times during manufacturing.
Incorporating pulp with a fiber diameter of 4 μm or more, fine cellulose fibers with diameters between 10 to 800 nm, amphoteric polyacrylamide as a paper strength enhancer, and cationically modified polyacrylamide as a drainage agent, along with a specific mass ratio and processing methods to form a pulp molded article with enhanced mechanical strength and rapid dehydration.
The resulting pulp molded products exhibit high mechanical strength and can be dehydrated quickly during manufacturing, achieving improved strength and productivity while maintaining excellent surface properties.
Smart Images

Figure JP2024014702_28112024_PF_FP_ABST
Abstract
Description
Pulp molded product and its manufacturing method
[0001] The present invention relates to a pulp molded product.
[0002] Paper containers are widely recognized as environmentally friendly containers, and demand for them is growing.
[0003] Pulp molding is a technology for producing molded articles from a slurry containing pulp and water. Pulp molding allows for greater freedom in the shape of paper products, such as paper containers. Pulp molding generally involves depositing pulp from the slurry on a mold to form a pulp layer, dehydrating the pulp layer, and then drying it in an oven. Molded articles obtained by this technology, i.e., pulp-molded articles, have excellent heat resistance, cold resistance, moisture absorption and desorption, and other physical properties characteristic of paper-based packaging materials. Pulp molding has come to be widely used as paper trays for food, fixed cushioning materials for fruit, and the like (Patent Document 1).
[0004] However, pulp-molded products produced by pulp molding can suffer from a problem of low strength. Patent Document 2 describes a technique for increasing the strength of pulp-molded products. In the technique described in Patent Document 2, a predetermined amount of cellulose nanofibers relative to the pulp is added to a pulp slurry. The cellulose nanofibers are preferably obtained by chemically modifying the raw cellulose material, such as by carboxylation, and typically have an average fiber diameter in the range of 3 to 500 nm and an average length-to-diameter ratio in the range of 50 to 1,000. This technique improves both tensile strength and burst strength by adding a predetermined amount of cellulose nanofibers.
[0005] Japanese Patent Publication No. 2008-285188 Japanese Patent Publication No. 2018-59254
[0006] An object of the present invention is to realize a pulp molded product that has high mechanical strength and can be dewatered in a short time during production.
[0007] According to one aspect of the present invention, there is provided a pulp molded product comprising pulp having a fiber diameter of 4 μm or more, fine fibers having a fiber diameter in the range of 10 to 800 nm, a paper strength agent, and a drainage agent.
[0008] According to another aspect of the present invention, there is provided the pulp molded product according to the above aspect, wherein the fine fibers are fine cellulose fibers.
[0009] According to yet another aspect of the present invention, there is provided a pulp molded product according to any one of the above aspects, wherein the paper strength agent is an amphoteric polyacrylamide.
[0010] According to yet another aspect of the present invention, there is provided a pulp molded product according to any one of the above aspects, wherein the drainage agent is a cation-modified polyacrylamide.
[0011] According to yet another aspect of the present invention, there is provided a pulp molded product according to any of the above aspects, wherein the fine fibers are fine cellulose fibers, the paper strength agent is amphoteric polyacrylamide, and the drainage agent is cation-modified polyacrylamide.
[0012] According to yet another aspect of the present invention, there is provided a pulp molded product according to any of the above aspects, wherein, when the mass of the pulp is 100 parts by mass, the amount of the fine fibers is in the range of 1.0 to 8.0 parts by mass, the amount of the paper strength agent is in the range of 0.1 to 5.0 parts by mass, and the amount of the drainage agent is in the range of 0.1 to 5.0 parts by mass.
[0013] According to yet another aspect of the present invention, there is provided a pulp molded product according to any of the above aspects, wherein the pulp has an average fiber diameter in the range of 15 to 40 μm, and the fine fibers have an average fiber diameter in the range of 50 to 500 nm.
[0014] According to yet another aspect of the present invention, there is provided a pulp molded product according to any of the above aspects, wherein the pulp has an average fiber length in the range of 0.5 to 2.0 mm, and the fine fibers have an average fiber length in the range of 10 to 1500 μm.
[0015] According to yet another aspect of the present invention, the density is 0.5 to 1.1 g / m 3The present invention provides a pulp molded article according to any of the above aspects, which is within the range of:
[0016] According to yet another aspect of the present invention, there is provided a pulp molded product according to any one of the above aspects, having a thickness in the range of 0.5 to 1.2 mm.
[0017] According to yet another aspect of the present invention, there is provided a pulp molded article according to any one of the above aspects, which is a container.
[0018] According to yet another aspect of the present invention, there is provided a method for producing a pulp molded product, the method including: preparing a slurry containing pulp having a fiber diameter of 4 μm or more, fine fibers having a fiber diameter in the range of 10 to 800 nm, a paper strength agent, a drainage agent, and water; depositing the pulp and the fine fibers on a three-dimensionally shaped mold to form a pulp layer; dehydrating the pulp layer to obtain an intermediate molded product; and sandwiching the undried intermediate molded product between a male mold and a female mold and heating it while applying pressure.
[0019] According to yet another aspect of the present invention, there is provided the method according to the above aspect, wherein the fine fibers are fine cellulose fibers.
[0020] According to yet another aspect of the present invention, there is provided a method according to any of the above aspects, wherein the paper strength agent is an amphoteric polyacrylamide.
[0021] According to yet another aspect of the present invention, there is provided a method according to any of the above aspects, wherein the drainage agent is a cationically modified polyacrylamide.
[0022] According to yet another aspect of the present invention, there is provided a method according to any of the above aspects, wherein the fine fibers are fine cellulose fibers, the paper strength agent is amphoteric polyacrylamide, and the drainage agent is cationically modified polyacrylamide.
[0023] According to yet another aspect of the present invention, there is provided a method according to any of the above aspects, wherein, when the mass of the pulp is 100 parts by mass, the amount of the fine fibers is in the range of 1.0 to 8.0 parts by mass, the amount of the paper strength agent is in the range of 0.1 to 5.0 parts by mass, and the amount of the drainage agent is in the range of 0.1 to 5.0 parts by mass.
[0024] According to yet another aspect of the present invention, there is provided a method according to any of the above aspects, wherein the pulp has an average fiber diameter in the range of 15 to 40 μm, and the fine fibers have an average fiber diameter in the range of 50 to 500 nm.
[0025] According to yet another aspect of the present invention, there is provided a method according to any of the above aspects, wherein the pulp has an average fiber length in the range of 0.5 to 2.0 mm, and the fine fibers have an average fiber length in the range of 10 to 1500 μm.
[0026] According to yet another aspect of the present invention, the density is 0.5 to 1.1 g / m 3
[0023] There is provided a method according to any of the above aspects, which results in a molded article within the range of
[0027] According to yet another aspect of the present invention, there is provided a method according to any of the above aspects for obtaining a moulded article having a thickness in the range of 0.5 to 1.2 mm.
[0028] According to yet another aspect of the present invention, there is provided a method according to any of the above aspects for obtaining a container.
[0029] According to the present invention, it is possible to realize a pulp molded product that has high mechanical strength and can be dewatered in a short time during production.
[0030] FIG. 1 is a perspective view showing a pulp molded product according to one embodiment of the present invention. FIG. 2 is a diagram schematically showing an example of a manufacturing apparatus that can be used to manufacture the pulp molded product of FIG. 1. FIG. 3 is a diagram showing a pulp layer formation step in pulp molding using the apparatus of FIG. 2. FIG. 4 is a cross-sectional view schematically showing an example of a pulp layer formed on a mold. FIG. 5 is a diagram showing a dewatering step in pulp molding using the apparatus of FIG. 2. FIG. 6 is a diagram showing a pulp layer conveying step in pulp molding using the apparatus of FIG. 2. FIG. 7 is a diagram showing a hot press formation step in pulp molding using the apparatus of FIG. 2. FIG. 8 is a cross-sectional view schematically showing an example of a pulp molded product obtained by the hot press step. FIG. 9 is a diagram showing a pulp molded product conveying step in pulp molding using the apparatus of FIG. 2. FIG. 10 is a diagram showing a state after the conveying step of FIG. 9 is completed.
[0031] Hereinafter, embodiments of the present invention will be described with reference to the drawings. The embodiments described below are more specific embodiments of any of the above aspects. The following items can be incorporated into each of the above aspects, either singly or in combination.
[0032] Furthermore, the embodiments shown below are merely examples of configurations for embodying the technical idea of the present invention, and the technical idea of the present invention is not limited by the materials, shapes, structures, etc. of the components described below. Various modifications can be made to the technical idea of the present invention within the technical scope defined by the claims.
[0033] In the drawings, elements having the same or similar functions are denoted by the same reference numerals, and redundant explanations will be omitted. Furthermore, the drawings are schematic, and the relationship between dimensions in one direction and dimensions in another direction, and the relationship between the dimensions of one member and the dimensions of another member, etc. may differ from the actual relationship.
[0034] <1> Pulp-molded product Fig. 1 is a perspective view showing a pulp-molded product according to one embodiment of the present invention. The pulp-molded product MP2 shown in Fig. 1 is a container. This pulp-molded product MP2 includes a bottom and a side wall, and is open at the top.
[0035] The bottom has a disk shape. The orthogonal projection of the bottom onto a plane perpendicular to the depth direction of the container may have a shape other than a circle, for example, a polygonal shape such as a square.
[0036] The side wall has a cylindrical shape extending upward from the edge of the bottom. The diameter of the side wall increases from the bottom toward the opening. The inner and outer surfaces of the side wall may be perpendicular to the upper surface of the bottom. However, the pulp molded product MP2, whose side wall increases in diameter from the bottom toward the opening, is advantageous in achieving high demoldability and is easy to stack.
[0037] The pulp-molded product MP2 may have various shapes such as a cup shape, a bowl shape, a tray shape, a box shape, etc. The pulp-molded product MP2 does not have to be a container as long as it is a three-dimensional product, i.e., a molded product having a three-dimensional shape, rather than a two-dimensional shape like a sheet.
[0038] The pulp molded product MP2 preferably has a thickness in the range of 0.5 to 1.2 mm. That is, the thickness of the wall portion of the pulp molded product MP2, specifically the thickness of the bottom and side wall portions, is preferably in the range of 0.5 to 1.2 mm. The thickness of the pulp molded product MP2 is more preferably in the range of 0.6 to 1.2 mm, and even more preferably in the range of 0.7 to 1.0 mm.
[0039] Thick pulp-molded products MP2 are bulky, especially when stacked. Furthermore, increasing the thickness makes it difficult to mold the pulp-molded products MP2 into complex shapes. On the other hand, thinning the walls of the pulp-molded products MP2 is advantageous in that it allows for quick dehydration and drying during production.
[0040] The pulp molded product MP2 has a density of 0.5 to 1.1 g / cm 3The density of the pulp molded product MP2 is preferably in the range of 0.7 to 1.1 g / cm 3 More preferably, it is in the range of 0.85 to 0.95 g / cm 3 It is more preferable that the temperature is in the range of
[0041] If the density is low, it is difficult to achieve good strength. Pulp molded products MP2 with excessively high density usually have low flexibility and are prone to cracking.
[0042] The pulp molded product MP2 has a basis weight of 500 to 1100 g / m 2 and preferably in the range of 616 to 1056 g / m 2 It is more preferable that the temperature is in the range of
[0043] Here, the above-mentioned thickness, density, and basis weight are values obtained by the following method. Specifically, square or rectangular test pieces are cut from a portion of the pulp molded product MP2 where the surface is not curved, and the dimensions, mass, and thickness are measured. For example, 10 test pieces, each having a strip shape of 15 mm wide and 145 mm long, are cut from the pulp molded product MP2. Then, the width, length, thickness, and mass of each test piece are measured. For example, a digital caliper is used to measure the width, length, and thickness. For example, an electronic balance is used to measure the mass. Then, the thickness, density, and basis weight of each test piece are calculated from the values obtained for each individual test piece. The above-mentioned thickness, density, and basis weight are then obtained by arithmetically averaging the values obtained for the 10 test pieces.
[0044] The pulp molded product MP2 contains pulp, fine fibers, a paper strength agent, and a drainage agent. The fine fibers are preferably fine cellulose fibers. The components contained in the pulp molded product MP2 are described below.
[0045] (Pulp) The fiber diameter of the pulp is 4 μm or more. The fiber diameter of the pulp is preferably 7 μm or more. The fiber diameter of the pulp is preferably 100 μm or less, and more preferably 80 μm or less. The average fiber diameter of the pulp is preferably in the range of 15 to 40 μm, and more preferably in the range of 17 to 25 μm. Pulp suitable for the pulp molded product MP2 has a fiber diameter within the above range.
[0046] Here, the fiber diameter of the pulp can be measured from an image obtained using a microscope such as an optical microscope, and the average fiber diameter of the pulp can be obtained by arithmetically averaging the fiber diameters measured from the image.
[0047] The pulp molded product MP2 may contain only one type of pulp, or may contain multiple types of pulp. For example, the pulp molded product MP2 may contain only a first pulp having an average fiber diameter in the range of 15 to 22 μm, or may contain the first pulp and a second pulp having an average fiber diameter in the range of 22 to 40 μm. The proportion of the first pulp in the pulp is preferably 50 mass% or more.
[0048] The average fiber length of the pulp is preferably in the range of 0.5 to 2.0 mm, more preferably in the range of 0.90 to 1.60 mm, and even more preferably in the range of 0.91 to 1.59 mm. Increasing the average fiber length allows for shorter drying times during production. However, excessively increasing the average fiber length may result in a decrease in the strength of the pulp molded product MP2.
[0049] Here, the average fiber length of pulp is a value obtained by the following method. That is, first, a 5 g test piece is obtained from the pulp molded product MP2. Next, this test piece is finely shredded and immersed in 500 mL of water overnight. Next, this is stirred with a stirrer to disintegrate the pulp from each other. In this way, a dispersion containing pulp is obtained. Next, 10 g of this dispersion is taken and diluted with water. This dilution is performed so that the total mass becomes 200 g. Using the sample obtained in this way, fiber length measurement is performed in accordance with JIS P8226-2:2011 "Pulp - Fiber length measurement method by optical automatic analysis - Part 2: Non-polarized light method." The average fiber length of pulp is determined as the length-weighted average fiber length L L Refers to...
[0050] (Fine Fibers) The fiber diameter of the fine fibers is in the range of 10 to 800 nm, and preferably in the range of 10 to 500 nm.
[0051] Fine fibers with a small fiber diameter can fill the gaps between adjacent pulp particles without interfering with hydrogen bonding between them. Therefore, in order to achieve excellent strength, it is preferable that the fine fibers have a small fiber diameter. However, the term "fine fibers" does not include cellulose nanofibers with an average fiber diameter of less than 10 nm.
[0052] On the other hand, some of the fine fibers may detach from the pulp layer along with water during the dehydration process in the production of the pulp molded product MP2. Fine fibers with a large fiber diameter are less likely to detach. Furthermore, fine fibers with a large fiber diameter do not excessively increase the residual moisture content of the pulp layer immediately before the drying process in the production of the pulp molded product MP2. Therefore, fine fibers with a large fiber diameter are advantageous in completing the drying process in a short time during the production of the pulp molded product MP2.
[0053] The average fiber diameter of the fine fibers is preferably in the range of 50 to 500 nm, and more preferably in the range of 100 to 300 nm. The fine fibers suitable for the pulp molded product MP2 have a fiber diameter within the above range.
[0054] Here, the fiber diameter of the fine fibers can be measured from an image obtained using a microscope such as a scanning electron microscope. The average fiber diameter of the fine fibers can be obtained by randomly selecting 20 fine fibers from the image and arithmetically averaging the fiber diameters measured for the selected fine fibers.
[0055] The average fiber length of the fine fibers is preferably in the range of 10 to 1500 μm.
[0056] Here, the average fiber length of the fine fibers refers to the value obtained according to the above-mentioned "Method for obtaining the average fiber length of pulp."
[0057] As described above, the fine fibers are preferably fine cellulose fibers. Examples of the fine cellulose fibers that can be used include those commercially available as "microfibrillated cellulose." Examples of the fine cellulose fibers that can be used include the Celish (registered trademark) series manufactured by Daicel Millize (e.g., KY100G, KY100S); the Valmet (registered trademark) series manufactured by Valmet; and the Exilva (registered trademark) series manufactured by Borregaard (e.g., Exilva F-01V, Exilva P-01V).
[0058] When the mass of pulp is taken as 100 parts by mass, the amount of fine fibers is preferably in the range of 1.0 to 8.0 parts by mass, more preferably in the range of 2.0 to 6.0 parts by mass, and even more preferably in the range of 3.5 to 4.5 parts by mass. If this ratio is reduced, the effect of adding fine cellulose fibers in improving the strength of the pulp molded product MP2 will be reduced. If this ratio is increased, the residual moisture content of the pulp layer immediately before the drying process during the production of the pulp molded product MP2 will increase. Therefore, it may take longer to dry the pulp molded product MP2 during production.
[0059] (Paper Strength Agent) The paper strength agent is preferably amphoteric polyacrylamide. Amphoteric polyacrylamide is a polyacrylamide containing cationic functional groups and anionic functional groups in the molecule to the same extent. Amphoteric polyacrylamide has a weight-average molecular weight of, for example, about 2 million to 6 million. As the molecular weight of the paper strength agent increases, the intermolecular interaction between pulp particles becomes stronger, and the effect of improving the paper strength of the pulp tends to increase.
[0060] The paper strength enhancer can be, for example, a commercially available "amphoteric polyacrylamide-based paper strength enhancer." Examples of the paper strength enhancer that can be used include the DS series (e.g., DS4424) manufactured by Seiko PMC Corporation; the Polystron (registered trademark) series (e.g., PS-1280) manufactured by Arakawa Chemical Industries, Ltd.; or the HARAMIDE (registered trademark) EX-200 series, EX-300 series, EX-400 series, and KS series manufactured by Harima Chemicals Co., Ltd.
[0061] When the mass of the pulp is taken as 100 parts by mass, the amount of the paper strength agent is preferably in the range of 0.1 to 5.0 parts by mass, more preferably in the range of 0.1 to 3.0 parts by mass, and even more preferably in the range of 1.0 to 2.5 parts by mass. Use of the paper strength agent can increase the strength of the pulp molded product MP2.
[0062] (Drainage Agent) The drainage agent is preferably cation-modified polyacrylamide. Cation-modified polyacrylamide is a polyacrylamide that contains both cationic and anionic functional groups in the molecule, but contains more cationic functional groups than anionic functional groups. Cation-modified polyacrylamide can be prepared, for example, by Hoffman modification. Because cation-modified polyacrylamide contains many cationic functional groups, it self-fixes to pulp. This causes pulp particles to bond together and increases the gaps between the pulp particles, improving drainage. Such drainage performance can be improved by the cation-modified polyacrylamide containing many cationic functional groups.
[0063] The filtering agent may be, for example, a commercially available "polyacrylamide filtering agent." Examples of the filtering agent that can be used include the RD series (e.g., RD-7144) manufactured by Seiko PMC Corporation, or the Polystron (registered trademark) series (e.g., PS-505) manufactured by Arakawa Chemical Industries, Ltd.
[0064] The amount of the filter agent is preferably in the range of 0.1 to 5.0 parts by mass, more preferably in the range of 0.1 to 1.0 parts by mass, and even more preferably in the range of 0.15 to 0.30 parts by mass, relative to 100 parts by mass of pulp. Use of the filter agent can shorten the slurry suction time during the production of the pulp molded product MP2, thereby increasing productivity.
[0065] The pulp molded product MP2 has an ISO ring crush compressive strength in the range of, for example, 9.5 to 20.0 kN / m. The ISO ring crush compressive strength of the pulp molded product MP2 is preferably in the range of 9.5 to 16.5 kN / m.
[0066] Here, the ISO ring crush compressive strength of the pulp molded product MP2 is a value obtained by the method specified in JIS P8126:2015 "Compression Strength Test Method - Ring Crush Method." The compressive strength is determined by sandwiching a thin, cylindrical (ring-shaped) test specimen between parallel upper and lower compression plates, applying a compressive load to the specimen, and obtaining the maximum load when buckling occurs. The maximum load obtained is then divided by the length of the test specimen. In this test method, the thin, rectangular test specimen measuring 15 mm wide and 145 mm long is prepared by cutting the pulp molded product MP2.
[0067] The pulp molded product MP2 with a high ISO ring crush compressive strength is less likely to buckle even when a large load is applied. However, if the ISO ring crush compressive strength of the pulp molded product MP2 is too high, it becomes more susceptible to breakage when an impact load is applied, such as when dropped.
[0068] The pulp suspension obtained by dispersing the pulp contained in the pulp molded product MP2 in water preferably has a Canadian Standard Freeness (CSF) in the range of 400 to 650 mL, more preferably in the range of 450 to 600 mL. The Canadian Standard Freeness of the pulp suspension is an index that indicates the degree of drainage of the pulp.
[0069] If the Canadian standard freeness is high, the strength of the pulp molded product MP2 tends to decrease. If the Canadian standard freeness is low, the strength of the pulp molded product MP2 increases, but the pulp molded product MP2 is prone to distortion during drying, which tends to cause unevenness on the surface of the pulp molded product MP2. Furthermore, if the Canadian standard freeness is low, the drying time during production tends to be long.
[0070] Here, the Canadian Standard Freeness is a value obtained by the following method. First, a test piece is obtained from the pulp molded product MP2, and a dispersion containing pulp is obtained by the same method as above. Next, this dispersion is diluted with water to a solids concentration of 0.3% by mass to obtain an aqueous suspension of pulp. Next, 1 L of this suspension is used to perform measurements as specified in JIS P8121-2:2012 "Pulp - Freeness Testing Method - Part 2: Canadian Standard Freeness Method." For this measurement, for example, a Canadian Freeness Tester manufactured by Kumagai Riki Kogyo Co., Ltd. is used. The measured value is corrected by referring to a correction table for the temperature of the suspension, which has been measured in advance. In this way, the Canadian Standard Freeness is obtained.
[0071] As described above, the pulp molded product MP2 contains, in addition to pulp, fine fibers, a paper strength agent, and a drainage agent. This configuration gives the pulp molded product MP2 high mechanical strength and enables dewatering during production to be completed in a short time. As demonstrated in the examples below, if at least one of the fine fibers, paper strength agent, and drainage agent is missing from the pulp molded product MP2, the two aforementioned effects cannot be achieved simultaneously.
[0072] <2> Manufacturing Apparatus for Pulp Molded Product Next, a manufacturing apparatus that can be used to manufacture the pulp molded product MP2 will be described. Fig. 2 is a diagram that schematically shows an example of a manufacturing apparatus that can be used to manufacture the pulp molded product of Fig. 1.
[0073] The manufacturing apparatus 1 shown in FIG. 2 includes a support 10 , a first station 20 , a second station 30 , and a third station 40 .
[0074] The support 10 includes a frame body and a rail installed on the upper part of the frame body.
[0075] The first station includes a container 210 , a lifting device 220 , a cover body 230 , a mold 240 , a moving device 250 , a lifting device 260 , and an upper mold 270 .
[0076] The container 210 is placed within the frame of the support 10. The container 210 is open at the top and contains a slurry S containing pulp, fine cellulose fibers, a crosslinking agent, and water.
[0077] The lifting device 220 is attached to the frame of the support body 10 above the container 210. The lifting device 220 includes, for example, a hydraulic cylinder. The lifting device 220 supports the cover body 230. The lifting device 220 can raise and lower the cover body 230 at the position of the opening of the container 210.
[0078] The cover body 230 is a hollow body having an opening at the top. A pump (not shown) is connected to the cover body 230.
[0079] The mold 240 is fixed to the opening of the cover body 230. Specifically, the mold 240 is fixed to the opening of the cover body 230 so that a space adjacent to one surface of the mold 240 is surrounded by the mold 240 and the cover body 230.
[0080] The mold 240 is a liquid-permeable mold. The mold 240 has a three-dimensional shape. That is, the mold 240 has one or more convex portions and / or one or more concave portions on the surface on which the pulp or the like is deposited. Specifically, the outer surface of the mold 240, i.e., the back surface of the surface adjacent to the space, has a shape corresponding to the pulp molded product. Here, the mold 240 is a male mold with a protruding upper surface.
[0081] The mold 240 includes, for example, a mold body having a large number of through holes and an outer surface having a shape corresponding to the pulp molded product, and a mesh body arranged on the outer surface of the mold body so as to fit along this outer surface.
[0082] The moving device 250 is movable between the first station 20 and the second station 30 along the rails of the support 10. The moving device 250 includes, for example, a motor as a power source. An elevator device 260 is attached to the moving device 250, and the elevator device 260 can be transported between the first station 20 and the second station 30.
[0083] As described above, the lifting device 260 is attached to the moving device 250. The lifting device 260 includes, for example, a hydraulic cylinder. The lifting device 260 supports the upper mold 270. The lifting device 260 can raise and lower the upper mold 270.
[0084] The upper mold 270 is a holder that sandwiches a pulp layer (described later) between itself and the mold 240 and holds the pulp layer by vacuum suction. The lower surface of the upper mold 270 has a shape that corresponds to the outer surface of the mold 240. In this example, the upper mold 270 is a female mold with a concave lower surface. The upper mold 270 has, for example, a number of through-holes that open at one end on the lower surface and are connected at the other end to a pump.
[0085] The second station 30 is provided near the first station 20. The second station 30 includes a table 310, a lower mold 320, a moving device 330, a pressing device 340, and an upper mold 350.
[0086] The base 310 is installed within the frame of the support 10. A lower mold 320 is installed on the base 310.
[0087] The lower mold 320 is a mold that is permeable to gas and / or liquid. The upper surface of the lower mold 320 has a shape that corresponds to the outer surface of the mold 240. Here, the lower mold 320 is a male mold with a protruding upper surface. The lower mold 320 has, for example, a large number of through holes, and has a smooth surface that corresponds to the outer surface of the mold 240.
[0088] The moving device 330 is movable along the rails of the support 10 between the second station 30 and a fourth station (not shown). The moving device 330 includes, for example, a motor as a power source. When the moving device 330 is located at the second station 30, its movement in the up-down, left-right, and front-rear directions can be restricted by a locking mechanism. In addition, a pressing device 340 is attached to the moving device 330, and it can be transported between the second station 30 and the fourth station.
[0089] As described above, the press device 340 is attached to the moving device 330. The press device 340 includes, for example, a hydraulic cylinder. The press device 340 supports the upper die 350. The press device 340 can raise and lower the upper die 350.
[0090] The upper mold 350 is a mold that is neither gas nor liquid permeable. The lower surface of the upper mold 350 has a shape corresponding to the outer surface of the mold 240. Here, the upper mold 350 is a female mold with a concave lower surface. The upper mold 350 has a smooth surface that has a shape corresponding to the outer surface of the mold 240.
[0091] The second station 30 further includes a heater and a pump (neither of which are shown). The heater heats both the lower mold 320 and the upper mold 350. The pump is connected to the space below the lower mold 320.
[0092] The third station 40 is provided near the second station 30. The third station 40 includes a platform 410, a moving device 420, a lifting device 430, and a holder 440.
[0093] The base 410 is installed within the frame of the support 10. On the base 410, a pulp molded product is placed.
[0094] The moving device 420 is movable between the second station 30 and the third station 40 along the rails of the support 10. The moving device 420 includes, for example, a motor as a power source. The moving device 420 is equipped with an elevator device 430, which can be transported between the second station 30 and the third station 40.
[0095] As described above, the lifting device 430 is attached to the moving device 420. The lifting device 430 includes, for example, a hydraulic cylinder. The lifting device 430 supports the holder 440. The lifting device 430 can raise and lower the holder 440.
[0096] The holder 440 is a holder that holds a pulp molded product (described later) by vacuum suction. The lower surface of the holder 440 has a shape that corresponds to the outer surface of the mold 240. In this example, the lower surface of the holder 440 has a concave shape. The holder 440 has, for example, a number of through holes that open at one end on the lower surface and are connected at the other end to a pump.
[0097] <3> Manufacturing Method of Pulp Molded Product In a manufacturing method according to one embodiment of the present invention, for example, a pulp molded product MP2 is manufactured using the above-described manufacturing apparatus 1. This will be described with reference to FIGS.
[0098] Fig. 3 is a diagram showing a pulp layer formation step in pulp molding using the apparatus of Fig. 2. Fig. 4 is a cross-sectional view schematically showing an example of a pulp layer formed on a mold. Fig. 5 is a diagram showing a dewatering step in pulp molding using the apparatus of Fig. 2. Fig. 6 is a diagram showing a pulp layer conveying step in pulp molding using the apparatus of Fig. 2. Fig. 7 is a diagram showing a heat press molding step in pulp molding using the apparatus of Fig. 2. Fig. 8 is a cross-sectional view schematically showing an example of a pulp molded product obtained by the heat press step. Fig. 9 is a diagram showing a pulp molded product conveying step in pulp molding using the apparatus of Fig. 2. Fig. 10 is a diagram showing a state after the conveying step of Fig. 9 is completed.
[0099] In this method, first, a slurry S is prepared. As described above, the slurry S contains pulp, fine fibers, a paper strength agent, a drainage agent, and water. The slurry S is a highly viscous suspension in which the pulp and fine fibers are dispersed in water, and the paper strength agent and drainage agent are dissolved or dispersed in water.
[0100] The pulp contained in the slurry S has substantially the same characteristics as those described above for the pulp contained in the molded pulp product MP2.
[0101] There are no particular limitations on the type of pulp used in the slurry S. Examples of pulp include wood pulp, non-wood pulp, and recycled paper, with wood pulp and non-wood pulp being preferred. From the perspective of environmental considerations such as forest conservation and utilization of unused resources, it is preferable to use non-wood pulp.
[0102] Pulp can be classified according to its preparation method. For example, examples of wood pulp include chemical pulps such as kraft pulp (KP), sulfite pulp (SP), and soda pulp (AP); semi-chemical pulps such as semi-chemical pulp (SCP) and chemi-groundwood pulp (CGP); groundwood pulp (GP), and thermomechanical pulp (TMP). Among these, chemical pulp is preferred. Pulp may be bleached or unbleached.
[0103] Wood pulp can be classified by raw material. Examples of wood pulp include softwood pulp and hardwood pulp. Examples of softwood pulp include pulp obtained from the fir and pine genera. Examples of hardwood pulp include pulp obtained from the acacia, eucalyptus, beech, and poplar (e.g., poplar).
[0104] Non-wood pulp is obtained from fibers extracted from the bark, stems, leaves, and leaf sheaths of plants. Specific examples include pulp obtained from cotton linters, cotton, linen, hemp, ramie, straw, esparto, Manila hemp, sisal, jute, flax, kenaf, bamboo, sugarcane, ganpi, mitsumata, mulberry, and mulberry. Among these, bamboo and sugarcane pulp are preferred.
[0105] These pulps can be used alone or in combination of two or more kinds in any ratio.
[0106] Pulp varies in fiber length and other properties depending on its raw material and manufacturing method. For example, pulp made from sugarcane generally has a shorter average fiber length than pulp made from bamboo. Furthermore, the average fiber length of pulp can be adjusted by any method, for example, mechanical processing such as beating or crushing. Therefore, pulp with certain characteristics can be obtained, for example, by selecting an appropriate one from multiple types of pulp or by appropriately combining two or more types of pulp. It is preferable to use non-wood pulp as the pulp, and it is preferable to use pulp made from sugarcane, pulp made from bamboo, or a combination thereof.
[0107] The pulp content of the slurry S is preferably in the range of 0.01 to 3.0% by mass, more preferably in the range of 0.01 to 0.5% by mass. If the pulp content is low, it is difficult to achieve high productivity. If the pulp content is high, the thickness of the pulp layer may vary greatly.
[0108] The fine fibers contained in the slurry S have substantially the same characteristics as those described above for the fine fibers contained in the pulp molded product MP2.
[0109] As described above for the fine fibers contained in the pulp molded product MP2, the amount of fine fibers contained in the slurry S is preferably in the range of 1.0 to 8.0 parts by mass per 100 parts by mass of pulp, more preferably in the range of 2.0 to 6.0 parts by mass, and even more preferably in the range of 3.5 to 4.5 parts by mass.
[0110] The strength agent contained in the slurry S has substantially the same characteristics as those of the strength agent contained in the pulp molded product MP2 described above.
[0111] As described above for the paper strength enhancer contained in the pulp molded product MP2, the amount of paper strength enhancer contained in the slurry S is preferably in the range of 0.1 to 5.0 parts by mass per 100 parts by mass of pulp, more preferably in the range of 0.1 to 3.0 parts by mass, and even more preferably in the range of 1.0 to 2.5 parts by mass.
[0112] The drainage agent contained in the slurry S has substantially the same characteristics as those described above for the drainage agent contained in the molded pulp product MP2.
[0113] As described above for the filterability agent contained in the pulp molded product MP2, the amount of filterability agent contained in the slurry S is preferably in the range of 0.1 to 5.0 parts by mass per 100 parts by mass of pulp, more preferably in the range of 0.1 to 1.0 part by mass, and even more preferably in the range of 0.15 to 0.30 parts by mass.
[0114] The slurry S may further contain other additives. Examples of the additives that can be used include organic low-molecular-weight materials, organic high-molecular-weight materials, inorganic materials, and combinations thereof. Examples of the additives include agents that impart water resistance or oil resistance (e.g., sizing agents), and the agent may be selected according to the performance requirements of the pulp-molded container.
[0115] The proportion of other additives in the total of pulp, fine fibers, paper strength agent, drainage agent, and other additives is preferably 3% by mass or less, and more preferably 1% by mass or less.
[0116] Next, the slurry S is supplied into the container 210. Next, as shown in FIG. 3, the cover body 230 is lowered by the lifting device 220 until the top surface of the mold 240 is positioned sufficiently below the liquid level of the slurry S. In this state, the pump is driven to reduce the pressure in the space surrounded by the cover body 230 and the mold 240. This causes the slurry S to flow across the mold 240, depositing a mixture of pulp and fine fibers on the mold 240. In this manner, a pulp layer MP1 is formed on the mold 240, as shown in FIG. 4.
[0117] Next, while the pump is still running, the cover body 230 is raised by the lifting device 220 as shown in FIG. 5, until the lower part of the mold 240 is positioned sufficiently above the liquid level of the slurry S. This dewaters the pulp layer MP1 under reduced pressure. Next, the lifting device 260 is driven to lower the upper mold 270 until its lower surface contacts the pulp layer MP1. Note that the pulp layer MP1 is not shown in FIG. 5. This dewatering process is performed without heating either the upper mold 270 or the mold 240.
[0118] The decompression time in the dehydration step is preferably in the range of 1 to 60 seconds, and more preferably in the range of 1 to 10 seconds.
[0119] The moisture content of the pulp layer MP1 immediately after dehydration is preferably in the range of 40 to 90% by mass, more preferably in the range of 50 to 70% by mass, and even more preferably in the range of 60 to 70% by mass. If the moisture content is low, the in-plane fiber movement within the pulp layer may be insufficient during the heat-pressing process. If the moisture content is high, the in-plane fiber movement within the pulp layer may be excessive during the heat-pressing process, or the shape retention of the pulp layer MP1 may be insufficient during the period from the end of the dehydration process to the start of the heat-pressing process.
[0120] After the decompression and pressurization of the space are stopped, the pump is driven to suction and hold the pulp layer MP1 to the upper mold 270. Note that the suction by the pump and the upper mold 270 does not cause further dehydration of the pulp layer MP1.
[0121] Next, with the pulp layer MP1 being suction-held by the upper mold 270, the lifting device 260 is driven to lift the upper mold 270 as shown in Figure 2. This causes the pulp layer MP1 to be peeled off from the mold 240.
[0122] Next, the moving devices 250 and 330 are driven to move the press device 340 and the upper mold 350 from the second station 30 to the fourth station 30, as shown in FIG. 6 , and the lifting device 260 and the upper mold 270 are moved from the first station 20 to the second station 30. The lifting device 260 is then driven to lower the upper mold 270 until the pulp layer MP1 contacts the lower mold 320. The suction by the pump and the upper mold 270 is then stopped, and the pulp layer MP1 is released from the upper mold 270. The lifting device 260 is then driven to lift the upper mold 270. In this manner, the pulp layer MP1 is transferred from the first station 20 to the second station 30, and the pulp layer MP1 is placed on the lower mold 320.
[0123] Next, the moving devices 250 and 330 are driven to move the lifting device 260 and upper mold 270 from the second station 30 to the first station 20, as shown in FIG. 2, and the press device 340 and upper mold 350 from the fourth station to the second station 30. Subsequently, the press device 340 is driven to lower the upper mold 350, as shown in FIG. 7. The pulp layer MP1 sandwiched between the upper mold 350 and the lower mold 320 is then pressed. At the same time, the heater is driven to heat the pulp layer MP1. Furthermore, the pump is driven to suction and remove water and / or water vapor from the space sandwiched between the upper mold 350 and the lower mold 320. This adjusts the surface shape of the pulp layer MP1 and densifies and dries the pulp layer MP1. In this manner, the pulp molded product MP2 shown in FIG. 8 is obtained.
[0124] The moisture content of the pulp layer MP1 immediately before the start of the heat pressing step is approximately equal to the moisture content of the pulp layer MP1 immediately after the completion of the dewatering step.
[0125] In this heat pressing process, the pressing pressure is set to a range of 0.1 to 3.0 MPa. It is more preferable to set this pressure to a range of 0.5 to 2.0 MPa. If the pressing pressure is too low, a high-density pulp molded product MP2 may not be obtained. The pulp layer MP1 contains pulp and fine fibers with short fiber lengths. Such pulp and fine fibers are likely to move within the pulp layer MP1, especially when the pressing pressure is excessively high. Therefore, if the pressing pressure is excessively high, the thickness of the pulp molded product MP2 is likely to vary.
[0126] In this heat pressing process, the heating temperature of the pulp layer MP1, i.e., the temperature of the upper mold 350 or the lower mold 320 heated by the heater, is set to a range of 130 to 250°C. This temperature is preferably set to a range of 150 to 190°C. Because the pulp layer MP1 contains pulp with short fiber length and fine fibers, it is difficult for water vapor to escape to the outside. Therefore, if the heating temperature is low, it takes a long time to dry the pulp layer MP1. If the heating temperature is high, the pulp layer MP1 shrinks more as it dries, which may result in greater distortion in the pulp molded product MP2.
[0127] The pressing time in the heat pressing step depends on the heating temperature, the shape of the molded product, etc., but is preferably in the range of 40 to 120 seconds, and more preferably in the range of 50 to 80 seconds.
[0128] When the above-mentioned hot pressing process is completed, the press device 340 is driven so that the upper die 350 moves up, and the pulp molded product MP2 is released from the upper die 350.
[0129] Next, the moving devices 330 and 420 are driven to move the press device 340 and upper mold 350 from the second station 30 to the fourth station, as shown in Figure 9, and the lifting device 430 and holder 440 are moved from the third station 40 to the second station 30. Next, the lifting device 430 is driven to lower the holder 440 until it contacts the pulp molded product MP2. Air is ejected from inside the lower mold to release the pulp molded product MP2 from the lower mold, and then the pump is driven to suction-hold the pulp molded product MP2 on the holder 440. Next, with the pulp molded product MP2 suction-held on the holder 440, the lifting device 430 is driven to raise the holder 440. Next, the moving devices 330 and 420 are driven to move the lifting device 430 and the holder 440 from the second station 30 to the third station 40, as shown in Figure 10, and move the press device 340 and the upper mold 350 from the fourth station to the second station 30. Next, suction by the pump and the holder 440 is stopped, and the pulp molded product MP2 is released from the holder 440. In this way, the pulp molded product MP2 is transferred from the second station 30 to the third station 40, and the pulp molded product MP2 is placed on the platform 410. In this manner, the pulp molded product MP2 is manufactured.
[0130] Thereafter, as necessary, the pulp molded product MP2 is subjected to post-treatment, such as printing with a pattern or solid color, coating, or a combination thereof. The coating layer formed by the post-treatment may be, for example, a layer containing a chemical that imparts water resistance or oil resistance, a layer filled with a material that imparts heat insulation, a layer foamed with a foaming agent, or a combination thereof. By performing the post-treatment, for example, the cosmetic properties of the pulp molded product MP2 can be further enhanced or new functions can be imparted to the pulp molded product MP2.
[0131] According to the above method, it is possible to produce a pulp molded product MP2 that has high mechanical strength and can be dehydrated in a short time during production.
[0132] Furthermore, the pulp molded product MP2 obtained by the above method has excellent surface properties, the reason for which will be explained below.
[0133] If drying is performed using an oven instead of the heat pressing process, the pulp layer will shrink, causing large unevenness on the surface. Furthermore, this method does not sufficiently densify the pulp layer, resulting in a pulp-molded product with high porosity. Therefore, in this case, it is not possible to produce a pulp-molded product with excellent surface quality.
[0134] Furthermore, if the dehydration step is followed by drying using an oven, and the dried product is humidified as necessary and subjected to a heat press treatment, the height difference of the unevenness occurring on the surface due to drying can be reduced by the subsequent humidification and heat press treatment. Furthermore, the porosity can be reduced by the humidification and heat press treatment. However, the height difference of the unevenness occurring on the surface due to drying using an oven is very large, and therefore cannot be sufficiently reduced by the subsequent humidification and heat press treatment. Furthermore, even if the humidification and heat press treatment are performed after drying, it is difficult to sufficiently reduce the porosity.
[0135] 2 to 10, the pulp layer MP1 is dried in the heat-pressing process. That is, in the above-mentioned method, the heat-pressing process is performed after the dehydration process without going through the drying process. Pulp and fine fibers having the above-mentioned fiber diameters are used as the fibers.
[0136] Because no drying process is performed before the heat-pressing process, the surface of the pulp layer MP1 does not have large unevenness with large height differences. During the heat-pressing process, the upper mold 350 and the lower mold 320 prevent deformation of the pulp layer MP1 due to drying. Furthermore, because the heat-pressing process is performed on a pulp layer MP1 with a high moisture content and an average pulp fiber length within the above-mentioned range, the fibers can move appropriately in the in-plane direction within the pulp layer MP1. The pulp layer MP1 can be densified without causing thickness variations.
[0137] 2 to 10, a pulp-molded product MP2 with excellent surface quality can be produced. Specifically, a pulp-molded product MP2 can be obtained whose surface has regions where one or more of the arithmetic mean roughness Ra, the maximum height roughness Rz, and the average length RSm of the roughness curve element are small. Such a pulp-molded product MP2 has excellent aesthetic appeal and can easily be coated with a printed layer or coating.
[0138] The arithmetic mean roughness Ra is preferably in the range of 2 to 10 μm, more preferably in the range of 2.5 to 4.5 μm. The maximum height roughness Rz is preferably in the range of 10 to 60 μm, more preferably in the range of 15 to 30 μm. The mean length RSm of the roughness curve elements is preferably in the range of 90 to 300 μm, more preferably in the range of 90 to 150 μm, and even more preferably in the range of 90 to 130 μm.
[0139] Here, "arithmetic mean roughness Ra," "maximum height roughness Rz," and "average length of roughness curve element RSm" are surface texture parameters defined in JIS B0601:2001. The surface texture parameters are measured using, for example, a Mitutoyo SJ-210 surface roughness measuring instrument (tip radius 2 μm, measuring force 0.75 mN) under the following conditions: Filter: Gasussian Cutoff λc: 0.25 mm Cutoff λs: 8 μm Measuring speed: 0.25 mm / s Number of sections: 5 A plate-shaped piece is taken from the pulp molded product MP2, and measurements are performed at any five locations to calculate the average value.
[0140] The entire surface of the pulp molded product MP2 may have the above-described surface texture, or only a portion of the surface may have the above-described surface texture. For example, only the area including the portion where post-processing such as printing is performed may have the above-described surface texture, while the other areas may not. Alternatively, one side of the pulp molded product MP2 may have the above-described surface texture, while the back side thereof may not have the above-described surface texture. Such a structure can be achieved, for example, by making the surface texture of the part of the surface of the upper mold 350 and the lower mold 320 that contacts the pulp layer MP1 different from that of the other areas.
[0141] 2 to 10, a pulp molded product MP2 having a small standard deviation of basis weight can be produced. The standard deviation of the basis weight of the pulp molded product MP2 is preferably 30 g / m 2 More preferably, it is 15 g / m or less. 2 The lower limit of this standard deviation is zero, and according to one example, 2 g / m 2 is.
[0142] Here, the standard deviation of the basis weight of the pulp molded product MP2 is a value obtained by the following method.
[0143] First, nine test pieces, each having a strip shape with a width of 15 mm and a length of 40 mm, were cut out from multiple regions located within a certain plane of the pulp molded product MP2. Next, the mass of these test pieces was measured. After that, the mass and area (600 mm) of each test piece were recorded. 2 The basis weight is calculated from the basis weight thus obtained. The standard deviation is calculated from the basis weight thus obtained.
[0144] Next, nine test pieces were cut out from multiple regions of the pulp molded product MP2 located in another plane in the same manner as above. The masses of these test pieces were also measured, and the basis weights and their standard deviations were calculated.
[0145] If the pulp molded product MP2 has additional surfaces, test pieces are cut out for each of the remaining surfaces, the masses are measured, and the basis weights and their standard deviations are calculated in the same manner as above. The maximum value of these standard deviations is then taken as the standard deviation of the basis weight of the pulp molded product MP2.
[0146] The inventors believe that the reason why the method described with reference to Figures 2 to 10 (hereinafter referred to as the first method) can produce a pulp molded product MP2 with a small standard deviation of basis weight is as follows.
[0147] The pulp molded product can also be produced, for example, by the method described below (hereinafter referred to as the second method).
[0148] In the second method, a female mold is first prepared as a mold. This mold includes a mold body with numerous through holes and a recessed upper surface corresponding to the shape of the pulp molded product, and a mesh body provided on and along the inner surface of the mold body.
[0149] Next, the mold is placed with its opening facing upward. A slurry containing pulp and water is then supplied into the cavity of the mold, filling it with the slurry. The supply of the slurry into the mold continues, depositing the pulp on the mesh. The supply of the slurry into the mold is carried out so that the slurry inside the mold is under pressure.
[0150] After a sufficient amount of pulp has accumulated on the mesh, the supply of slurry into the mold is stopped. Then, the water remaining in the mold is expelled from the mold, for example, by injecting compressed air into the mold.
[0151] Next, the pulp layer is pressed between the cutting mold and the upper mold, which is a male mold, to dehydrate the pulp layer. This dehydration process is performed without heating either the upper mold or the cutting mold. The moisture content of the pulp layer immediately after dehydration is set to be the same as the moisture content of the pulp layer MP1 immediately after dehydration in the first method.
[0152] Next, the pulp layer is held by suction on the upper mold, and in this state the upper mold is raised, thereby peeling the pulp layer from the mold.
[0153] Next, the upper mold, which is holding the pulp layer by suction, is moved to the position of the lower mold, which is the female mold. The upper mold is then lowered until the pulp layer comes into contact with the lower mold. After that, the suction is stopped and the pulp layer is released from the upper mold. In this way, the pulp layer is placed on the lower mold.
[0154] Next, the pulp layer is sandwiched between an upper mold and a lower mold for a hot press, and pressure is applied to the pulp layer between them. At the same time, a heater is driven to heat the pulp layer. Furthermore, a pump is driven to suction and remove water and / or water vapor from the space between the upper and lower molds. In the second method, a pulp molded product is obtained as described above.
[0155] In the second method, a circulating flow of slurry may occur within the mold during the period from when the supply of slurry into the mold begins until the mold is completely filled with the slurry. This circulating flow can prevent pulp settling. However, since the second method requires filling the mold with slurry, the mold cannot be designed to allow water to be quickly drained. Therefore, after the mold is completely filled with the slurry, even if the pressure of the slurry is increased, a circulating flow of slurry sufficient to prevent pulp settling does not occur, and pulp settling occurs in the slurry within the mold.
[0156] As a result, the amount of pulp deposited on the sidewall of the mold is greater at the bottom than at the top. If the slurry is supplied until a sufficient amount of pulp is deposited on the top of the sidewall of the mold, an excessive amount of pulp will be deposited at the bottom of the mold. Depositing excessive pulp results in a large variation in the amount of pulp deposited. For example, a large difference in the amount of pulp deposited near the through-holes provided in the mold body can occur compared to a position distant from the through-holes.
[0157] As described above, the second method results in large variations in the amount of pulp deposited. During the hot press process, fibers may move in the in-plane direction within the pulp layer, but the movement of each fiber is limited to a narrow range. This means that the variation in the amount of pulp deposited is not eliminated by the movement of fibers during the hot press process. Therefore, the second method cannot produce a pulp molded product with a small standard deviation in basis weight.
[0158] In contrast, in the first method, a mold 240 is placed on top of the cover body 230, and the composite is immersed in a slurry S. The depth of the slurry S is much greater than the height of the mold 240. Therefore, even if pulp settles in the slurry S, the pulp concentration does not differ significantly between the upper and lower positions of the mold 240. Therefore, according to the first method, the pulp can be deposited approximately uniformly on the mold 240, and a pulp molded product MP2 with a small standard deviation in basis weight can be produced.
[0159] The pulp molded product MP2 has an opening and does not expand in diameter in the direction away from the opening. Here, the pulp molded product MP2 has an opening and tapers in the direction away from the opening. This shape allows the volume of a stack formed by stacking multiple pulp molded products MP2 to be reduced.
[0160] In the first method, if the pulp layer MP1 is sandwiched between one of the upper and lower dies 350 and 320 and an elastic body and then pressurized instead of being pressed by the upper and lower dies 350 and 320, the elastic body will deform, and therefore sufficient pressure will not be applied to the pulp layer MP1, making it impossible to obtain a pulp molded product with excellent surface quality.
[0161] In the second method, if one of the upper and lower dies used in the hot press treatment is made of an elastic material, it is not possible to obtain a pulp molded product with excellent surface quality. In addition, in this case, the standard deviation of the basis weight becomes large, as described above.
[0162] The pulp molded product MP2 is, for example, a container. The pulp molded product MP2 may be an article other than a container. The pulp molded product MP2 may be a three-dimensional molded product, that is, a molded product having a three-dimensional shape, rather than a two-dimensional shape like a sheet.
[0163] 2 to 10 are provided to facilitate understanding of the method for manufacturing a pulp molded product according to one embodiment of the present invention. The above-described method can also be implemented using manufacturing apparatuses having other structures. For example, in the manufacturing apparatus 1, the upper mold 270 and the upper mold 350 are female molds, and the mold 240 and the lower mold 320 are male molds. The upper mold 270 and the upper mold 350 may be male molds, and the mold 240 and the lower mold 320 may be female molds. As such, various modifications are possible to the above-described manufacturing apparatus 1 and manufacturing method.
[0164] Specific examples of the present invention are described below, but the present invention is not limited to these specific examples.
[0165] <1> Production of pulp molded product (Example 1) A slurry containing pulp, fine cellulose fibers, a paper strength agent, a drainage agent, a sizing agent, and water was prepared using a pulper. The pulp content of the slurry was 0.3% by mass.
[0166] The pulp used was bamboo pulp (average fiber diameter 50 μm, average fiber length 1.590 mm) and sugarcane pulp (average fiber diameter 50 μm, average fiber length 0.918 mm). The amount of bamboo pulp per 100 parts by mass of the total amount of pulp was 70 parts by mass, and the amount of sugarcane pulp per 100 parts by mass of the total amount of pulp was 30 parts by mass. The average fiber diameter of the pulp was 50 μm, and the average fiber length of the pulp was 1.406 mm. The fiber diameter of the pulp was in the range of 4 to 100 μm.
[0167] The fine cellulose fibers used were Celish (registered trademark) KY100G (average fiber diameter 50 to 500 nm, average fiber length 10 to 1500 μm) manufactured by Daicel Miraizu Co., Ltd. The fiber diameter of the fine cellulose fibers was in the range of 10 to 800 nm. The amount of fine cellulose fibers (amount on a solid content basis) per 100 parts by mass of pulp was 4.0 parts by mass.
[0168] The paper strength agent used was Polystron (registered trademark) PS-1280 (amphoteric polyacrylamide) manufactured by Arakawa Chemical Industries, Ltd. The amount of the paper strength agent (amount on a solids basis) per 100 parts by mass of pulp was 2.0 parts by mass.
[0169] The filtering agent used was RD-7144 (cation-modified polyacrylamide) manufactured by Seiko PMC Co., Ltd. The amount of filtering agent (amount on a solids basis) per 100 parts by mass of pulp was 0.2 parts by mass.
[0170] The sizing agent used was Sizepine K-903-20 manufactured by Arakawa Chemical Industries, Ltd. The amount of sizing agent (amount on a solids basis) per 100 parts by mass of pulp was 0.3 parts by mass.
[0171] Using this slurry, a pulp molded product was produced by the method described with reference to Figures 2 to 10. Here, the dehydration process was carried out so that the moisture content of the pulp layer immediately after dehydration was 65% by mass. The heat pressing process was carried out at a heating temperature of 180°C, a pressing pressure of 1.2 MPa, and a pressing time of 120 seconds. In the dehydration and heat pressing processes, the clearance between the upper and lower dies was adjusted so as to obtain a pulp molded product with a wall thickness of 0.7 mm. In this manner, a container was produced as a pulp molded product.
[0172] Example 2 A pulp molded product was produced in the same manner as in Example 1, except that the amount of paper strength agent (amount on a solids basis) was changed from 2.0 parts by mass to 0.1 parts by mass per 100 parts by mass of pulp.
[0173] Example 3 A pulp molded product was produced in the same manner as in Example 1, except that the amount of paper strength agent (amount on a solids basis) was changed from 2.0 parts by mass to 5.0 parts by mass per 100 parts by mass of pulp.
[0174] Example 4 A pulp molded product was produced in the same manner as in Example 1, except that the amount of the filter agent (amount based on solids) was changed from 0.2 parts by mass to 0.1 parts by mass per 100 parts by mass of pulp.
[0175] Example 5 A pulp molded product was produced in the same manner as in Example 1, except that the amount of the filter agent (amount based on solids) was changed from 0.2 parts by mass to 5.0 parts by mass per 100 parts by mass of pulp.
[0176] Example 6 A pulp molded product was produced in the same manner as in Example 1, except that bamboo pulp was used instead of the mixture of 70 parts by mass of bamboo pulp and 30 parts by mass of sugarcane pulp.
[0177] (Example 7) A pulp molded product was produced in the same manner as in Example 1, except that a mixture of 80 parts by mass of bamboo pulp and 20 parts by mass of sugarcane pulp was used as the pulp instead of a mixture of 70 parts by mass of bamboo pulp and 30 parts by mass of sugarcane pulp.
[0178] (Example 8) A pulp molded product was produced in the same manner as in Example 1, except that a mixture of 50 parts by mass of bamboo pulp and 50 parts by mass of sugarcane pulp was used as the pulp instead of a mixture of 70 parts by mass of bamboo pulp and 30 parts by mass of sugarcane pulp.
[0179] Example 9 A pulp molded product was produced in the same manner as in Example 1, except that sugarcane pulp was used instead of the mixture of 70 parts by mass of bamboo pulp and 30 parts by mass of sugarcane pulp.
[0180] Example 10 A pulp molded product was produced in the same manner as in Example 1, except that the amount of pulp piled up was adjusted and the clearance between the upper and lower dies was changed from 0.7 mm to 0.6 mm.
[0181] Example 11 A pulp molded product was produced in the same manner as in Example 1, except that the amount of pulp piled up was adjusted and the clearance between the upper and lower dies was changed from 0.7 mm to 1.2 mm.
[0182] Comparative Example 1 A pulp molded product was produced in the same manner as in Example 1, except that the slurry in Example 1 was changed so that it did not contain fine cellulose fibers, paper strength agents, or drainage agents; that is, a "slurry consisting of pulp, a sizing agent, and water" was used.
[0183] Comparative Example 2 A pulp molded product was produced in the same manner as in Example 1, except that the slurry in Example 1 was changed so as not to contain fine cellulose fibers and a drainage agent, i.e., a "slurry consisting of pulp, a paper strength agent, a sizing agent, and water" was used.
[0184] Comparative Example 3 A pulp molded product was produced in the same manner as in Example 1, except that the slurry in Example 1 was changed so as not to contain fine cellulose fibers and a paper strength agent, i.e., a "slurry consisting of pulp, a drainage agent, a sizing agent, and water" was used.
[0185] Comparative Example 4 A pulp molded product was produced in the same manner as in Example 1, except that the slurry in Example 1 was changed so that it did not contain a paper strength agent or a drainage agent, i.e., a "slurry consisting of pulp, fine cellulose fibers, a sizing agent, and water" was used.
[0186] (Comparative Example 5) A pulp molded product was produced in the same manner as in Example 1, except that the slurry in Example 1 was changed so as not to contain fine cellulose fibers, i.e., a "slurry consisting of pulp, a paper strength agent, a drainage agent, a sizing agent, and water" was used as the pulp.
[0187] Comparative Example 6 A pulp molded product was produced in the same manner as in Example 1, except that the slurry in Example 1 was changed so that it did not contain a drainage agent, i.e., a "slurry consisting of pulp, fine cellulose fibers, a paper strength agent, a sizing agent, and water" was used as the pulp.
[0188] Comparative Example 7 A pulp molded product was produced in the same manner as in Example 1, except that the slurry in Example 1 was changed so as not to contain a paper strength agent, i.e., a "slurry consisting of pulp, fine cellulose fibers, a drainage agent, a sizing agent, and water" was used as the pulp.
[0189] Comparative Example 8 A pulp molded product was produced in the same manner as in Example 1, except that cellulose nanofibers were used instead of fine cellulose fibers as the slurry material, and no paper strength agent was used. TEMPO-oxidized cellulose nanofibers (product name: Cellenpia (registered trademark)) (average fiber diameter: 3 nm, average fiber length: 700 nm) manufactured by Nippon Paper Industries Co., Ltd. were used as the cellulose nanofibers. The amount of cellulose nanofibers (amount on a solids basis) was 4.0 parts by mass per 100 parts by mass of pulp. "TEMPO-oxidized cellulose nanofibers" are cellulose nanofibers obtained by treating wood fibers with a TEMPO (2,2,6,6-tetramethylpiperidine 1-oxyl) catalyst to convert the primary hydroxyl groups of cellulose to carboxyl groups, followed by mechanical defibration.
[0190] <2> Evaluation Methods The pulp molded products produced in Examples 1 to 11 and Comparative Examples 1 to 8 were subjected to various measurements by the methods described above.
[0191] The effect of shortening the slurry suction time was evaluated as follows. Papermaking was carried out using a mesh mold with a mesh diameter of 0.15 mm x 0.15 mm. The time required for papermaking (i.e., slurry suction time) was evaluated according to the following evaluation criteria. 1: The slurry suction time was 40% or more longer than the reference (10 seconds in the case of Comparative Example 1). That is, the slurry suction time was 14 seconds or more. 2: The slurry suction time was 20% or more longer than the reference (10 seconds in the case of Comparative Example 1). That is, the slurry suction time was 12 seconds or more but less than 14 seconds. 3: The slurry suction time was 10 seconds (in the case of Comparative Example 1). 4: The slurry suction time was reduced by 20% compared to the reference (10 seconds in the case of Comparative Example 1). That is, the slurry suction time was 8 seconds or more but less than 10 seconds. 5: The slurry suction time was reduced by 40% compared to the reference (10 seconds in the case of Comparative Example 1). That is, the slurry suction time was 6 seconds or more but less than 8 seconds.
[0192] <3> Results Tables 1 to 3 below show the results of various measurements and the evaluation results of the effect of shortening the slurry suction time.
[0193]
[0194]
[0195]
[0196] As is clear from the comparison of Examples 1 to 11 with Comparative Examples 1 to 8, when pulp was blended with fine cellulose fibers, a paper strength agent, and a drainage agent to produce a pulp molded product, it was possible to produce a pulp molded product that had high ISO ring crush strength and could complete dewatering during production in a short time. As shown in Comparative Examples 1 to 7, if at least one of the fine cellulose fibers, the paper strength agent, and the drainage agent was missing, it was not possible to achieve both of the above effects. Furthermore, as shown in Comparative Example 8, when cellulose nanofibers were blended instead of the fine cellulose fibers, the mechanical strength of the pulp molded product was increased, but the slurry suction time was prolonged.
[0197] 1... manufacturing apparatus, 10... support, 20... first station, 30... second station, 40... third station, 210... container, 220... lifting device, 230... cover body, 240... mold, 250... moving device, 260... lifting device, 270... upper mold, 310... table, 320... lower mold, 330... moving device, 340... press device, 350... upper mold, 410... table, 420... moving device, 430... lifting device, 440... holder, MP1... pulp layer, MP2... pulp molded product, S... slurry.
Claims
1. A pulp molded product comprising pulp having a fiber diameter of 4 μm or more, fine fibers having a fiber diameter in the range of 10 to 800 nm, a paper strength agent, and a drainage agent.
2. The pulp molded product according to claim 1, wherein the fine fibers are fine cellulose fibers.
3. A pulp molded product according to claim 1 or 2, wherein the paper strength agent is an amphoteric polyacrylamide.
4. A pulp molded product according to any one of claims 1 to 3, wherein the drainage agent is a cationically modified polyacrylamide.
5. A pulp molded product according to any one of claims 1 to 4, wherein the fine fibers are fine cellulose fibers, the paper strength agent is an amphoteric polyacrylamide, and the drainage agent is a cationically modified polyacrylamide.
6. A pulp molded product according to any one of claims 1 to 5, wherein, when the mass of the pulp is 100 parts by mass, the amount of the fine fibers is in the range of 1.0 to 8.0 parts by mass, the amount of the paper strength agent is in the range of 0.1 to 5.0 parts by mass, and the amount of the drainage agent is in the range of 0.1 to 5.0 parts by mass.
7. A pulp molded product according to any one of claims 1 to 6, wherein the pulp has an average fiber diameter in the range of 15 to 40 μm, and the fine fibers have an average fiber diameter in the range of 50 to 500 nm.
8. A pulp molded product according to any one of claims 1 to 7, wherein the pulp has an average fiber length in the range of 0.5 to 2.0 mm, and the fine fibers have an average fiber length in the range of 10 to 1500 µm.
9. Density: 0.5 to 1.1 g / m 3 The pulp molded product according to any one of claims 1 to 8, wherein the viscosity of the pulp molded product is within the range of 0.1 to 0.
5.
10. The pulp molded product according to any one of claims 1 to 9, having a thickness in the range of 0.5 to 1.2 mm.
11. The pulp molded product according to any one of claims 1 to 10, which is a container.
12. A method for manufacturing a pulp molded product, comprising: preparing a slurry containing pulp having a fiber diameter of 4 μm or more, fine fibers having a fiber diameter in the range of 10 to 800 nm, a paper strength agent, a drainage agent, and water; depositing the pulp and the fine fibers on a three-dimensional mold to form a pulp layer; dehydrating the pulp layer to obtain an intermediate molded product; and sandwiching the wet intermediate molded product between a male mold and a female mold and heating it while applying pressure.
13. The method for producing a pulp molded product according to claim 12, wherein the fine fibers are fine cellulose fibers.
14. A method for producing a pulp molded product according to claim 12 or 13, wherein the paper strength agent is an amphoteric polyacrylamide.
15. A method for producing a pulp molded product according to any one of claims 12 to 14, wherein the drainage agent is a cationically modified polyacrylamide.
16. A method for producing a pulp molded product described in any one of claims 12 to 15, wherein the fine fibers are fine cellulose fibers, the paper strength agent is an amphoteric polyacrylamide, and the drainage agent is a cationically modified polyacrylamide.
17. A method for producing a pulp molded product described in any one of claims 12 to 16, wherein, when the mass of the pulp is 100 parts by mass, the amount of the fine fibers is in the range of 1.0 to 8.0 parts by mass, the amount of the paper strength agent is in the range of 0.1 to 5.0 parts by mass, and the amount of the drainage agent is in the range of 0.1 to 5.0 parts by mass.
18. A method for producing a pulp molded product according to any one of claims 12 to 17, wherein the pulp has an average fiber diameter in the range of 15 to 40 μm, and the fine fibers have an average fiber diameter in the range of 50 to 500 nm.
19. A method for producing a pulp molded product according to any one of claims 12 to 18, wherein the pulp has an average fiber length in the range of 0.5 to 2.0 mm, and the fine fibers have an average fiber length in the range of 10 to 1500 μm.
20. Density is 0.5 to 1.1 g / m 3The method for producing a molded pulp product according to any one of claims 12 to 19, which produces a molded product having a viscosity within the range of 100:1 or 100:
2.
21. A method for producing a pulp molded product according to any one of claims 12 to 20, which produces a molded product having a thickness in the range of 0.5 to 1.2 mm.
22. A method for producing a pulp molded product according to any one of claims 12 to 21, for obtaining a container.
Citation Information
Patent Citations
Agent for imparting flexibility to paper and preventing occurrence of paper powder and method therefor
JP2018012904A
Pulp mold
JP2020165022A
Molded article and manufacturing method thereof
JP2020200545A
Formed member made of molded pulp
JP2021080619A
Softener for papermaking, paper, and method for producing paper
JP2022181700A