Dielectric and functional element

A dielectric material with a controlled molar ratio of hafnium, cerium, and oxygen stabilizes cerium valence, enhancing chemical stability and ferroelectricity in capacitors and other functional elements.

WO2024241758A1PCT designated stage expired Publication Date: 2024-11-28PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/015007
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-19
Filing Date
2024-04-15
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Conventional dielectric materials, such as HfO2, exhibit fluctuations in cerium valence at the interface with electrodes, leading to unstable dielectric properties in capacitors, which affects the performance of functional devices.

Method used

A dielectric material with a specific molar ratio of hafnium, cerium, and oxygen (0.031 ≤ x ≤ 0.052 and 0 < y ≤ 1.50) is developed, where x represents the cerium content and y the oxygen content, to stabilize the valence of cerium and improve chemical stability, incorporating a fluorite-type crystal structure and a polycrystalline film with a rectangular phase for ferroelectricity.

Benefits of technology

The proposed dielectric material enhances chemical stability and ferroelectric properties, reducing fluctuations in cerium valence and improving the characteristics of capacitors and other functional elements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024015007_28112024_PF_FP_ABST
    Figure JP2024015007_28112024_PF_FP_ABST
Patent Text Reader

Abstract

This dielectric includes an oxide containing hafnium and cerium. The molar ratio of the cerium content to the sum of the hafnium content and cerium content is 0.031-0.052. The molar ratio of the oxygen content to the sum of the hafnium content and cerium content is greater than 0 and less than or equal to 1.50.
Need to check novelty before this filing date? Find Prior Art

Description

Dielectric and functional elements

[0001] The present disclosure relates to a dielectric and a functional device.

[0002] It has been known that adding other metal elements to HfO2 with a fluorite structure changes the crystal phase and changes the dielectric properties from paraelectric to ferroelectric. For example, Non-Patent Document 1 describes that HfO2 doped with elements such as Si, Al, Zr, and Y exhibits ferroelectricity.

[0003] Non-Patent Document 2 states that (Hf 1-x Ce x It has been reported that films of solid solutions represented by xO2 exhibit ferroelectric properties. In these films, x ranges from 0.15 to 0.20.

[0004] M. H. Park et al. , Adv. Mater. 2015, 27, 1811-1831K. Hirai et al. , Jpn. J. Appl. Phys. 2022, 61, SN1019

[0005] An object of the present disclosure is to provide a novel dielectric suitable for use in functional elements such as capacitors.

[0006] The present disclosure provides a dielectric comprising an oxide containing hafnium and cerium, wherein a molar ratio of a cerium content to a sum of a hafnium content and a cerium content is 0.031 or more and 0.052 or less, and a molar ratio of an oxygen content to the sum is greater than 0 and 1.50 or less.

[0007] According to the present disclosure, a novel dielectric material suitable for use in functional elements such as capacitors can be provided.

[0008] Fig. 1 is a cross-sectional view showing an example of a functional element of the present disclosure. Fig. 2 is a cross-sectional view showing another example of a functional element of the present disclosure. Fig. 3 is a graph showing the relationship between polarization and electric field strength in dielectric films according to Examples 1 to 3. Fig. 4 is a graph showing the relationship between polarization and electric field strength in dielectric films according to Comparative Examples 1 to 4. Fig. 5 is a graph showing X-ray diffraction patterns of the dielectrics according to Examples 1 to 3.

[0009] (Findings on which the present disclosure is based) 1-x Ce x In CeO2, the concentration of Ce added is 0.15 to 0.20. Ce in CeO2 is 4+ and Ce 3+ The valence easily changes between 0 and 1. When a capacitor is manufactured using a dielectric containing HfO2 to which Ce is added, the valence of Ce is likely to change, for example, at the interface between the dielectric and the electrode, depending on the oxygen concentration in the electrode. When the valence of Ce changes, the electronic state around the Ce cation changes, which may cause fluctuations in the characteristics of the dielectric. When the characteristics of the dielectric change, the characteristics of the capacitor constructed using that dielectric also change. For these reasons, it is desirable to suppress fluctuations in the valence of Ce cations in the dielectric in order to suppress fluctuations in the characteristics of functional elements such as capacitors and to obtain a chemically stable dielectric.

[0010] In view of these circumstances, the present inventors have conducted extensive research to improve the chemical stability of a functional device using a dielectric containing an oxide containing hafnium and cerium. As a result, the present inventors have newly discovered that the chemical stability of a dielectric can be improved by adjusting the contents of hafnium, cerium, and oxygen to a predetermined relationship. Based on this new finding, the present inventors have devised the dielectric of the present disclosure.

[0011] Embodiments Hereinafter, embodiments of the present disclosure will be described with reference to the drawings, but the present disclosure is not limited to the following embodiments.

[0012] FIG. 1 is a cross-sectional view showing an example of a functional device 1a according to the present disclosure. As shown in FIG. 1, the functional device 1a includes a dielectric 10. The dielectric 10 includes an oxide containing hafnium and cerium. The molar ratio of the cerium content to the sum of the hafnium content and the cerium content is 0.031 or more and 0.052 or less, and the molar ratio of the oxygen content to the sum is greater than 0 and less than 1.50. This configuration can improve the chemical stability of the dielectric 10. The dielectric 10 may also include Zr, which is contained in a precursor material for Hf.

[0013] In the dielectric 10 according to this embodiment, the element concentration of Ce contained in the dielectric 10 is reduced. Specifically, the molar ratio of the cerium content to the sum of the hafnium content and the cerium content satisfies 0.031 or more and 0.052 or less. Therefore, in the dielectric 10, the region where the valence of Ce is likely to fluctuate can be made smaller. In other words, a chemically stable dielectric 10 can be obtained.

[0014] Additionally, in the dielectric 10 according to this embodiment, the molar ratio of the oxygen content to the sum of the hafnium content and the cerium content is greater than 0 and not greater than 1.50. That is, the concentration of oxygen contained in the dielectric 10 is kept low. This makes it possible to reduce the elemental concentration of Ce in the dielectric 10. As a result, it is possible to reduce the region in the dielectric 10 where the valence of Ce is likely to fluctuate. That is, a chemically stable dielectric 10 can be obtained.

[0015] The molar ratio of the cerium content to the sum of the hafnium content and the cerium content in the dielectric 10 may be 0.031 or more and 0.050 or less, or may be 0.031 or more and 0.048 or less. The molar ratio may be 0.035 or more and 0.052 or less, 0.040 or more and 0.052 or less, 0.045 or more and 0.052 or less, or may be 0.048 or more and 0.052 or less.

[0016] The molar ratio of the oxygen content to the sum of the hafnium content and the cerium content in the dielectric 10 may be 1.44 or more and 1.50 or less. In this case, the region in which the valence of Ce is likely to fluctuate can be made smaller. As a result, a chemically more stable dielectric 10 can be obtained. The molar ratio may be 1.44 or more and 1.47 or less.

[0017] The dielectric 10 has the composition formula Hf 1-x Ce x O yIn this composition formula, 0.031≦x≦0.052 and 0<y≦1.50 are satisfied. With this configuration, the chemical stability of the dielectric 10 can be improved.

[0018] Dielectric 10 may satisfy 0.031≦x≦0.050, or may satisfy 0.031≦x≦0.048. Dielectric 10 may satisfy 0.035≦x≦0.052, or may satisfy 0.040≦x≦0.052, or may satisfy 0.045≦x≦0.052, or may satisfy 0.048≦x≦0.052.

[0019] The dielectric 10 may satisfy 1.44≦y≦1.50. In this case, the region in which the valence of Ce is likely to fluctuate can be made smaller. As a result, a chemically more stable dielectric 10 can be obtained. The dielectric 10 may satisfy 1.44≦y≦1.47.

[0020] The dielectric 10 may include a crystalline phase having a fluorite-type crystalline structure. In addition, the dielectric 10 may be a polycrystalline film. With such a configuration, the dielectric 10 is likely to exhibit ferroelectricity. The crystalline phase having the fluorite-type crystalline structure is, for example, an orthorhombic phase, a monoclinic phase, a tetragonal phase, or a cubic phase.

[0021] The dielectric 10 may contain an orthorhombic phase as a crystalline phase. The orthorhombic phase may have polarization in the out-of-plane direction. Therefore, when the dielectric 10 contains an orthorhombic phase as a crystalline phase, the dielectric 10 is likely to exhibit ferroelectricity.

[0022] The dielectric 10 may have a monoclinic phase, a tetragonal phase, a cubic phase, and an orthorhombic phase, which makes the dielectric 10 more likely to exhibit ferroelectricity.

[0023] The X-ray diffraction (XRD) pattern of dielectric 10 may satisfy 0.87≦a / (a+b)≦0.98, where a is the peak area of ​​a diffraction peak attributable to reflection from the (111) plane of the orthorhombic phase in the X-ray diffraction pattern of dielectric 10, and b is the peak area of ​​a diffraction peak attributable to reflection from the (001) plane of the orthorhombic phase in the X-ray diffraction pattern of dielectric 10. With this configuration, dielectric 10 is likely to exhibit ferroelectricity.

[0024] Peak area a indicates the area of ​​a diffraction peak observed in the XRD spectrum near 2θ = 30.2°. This peak is a diffraction peak attributed to reflection from the (111) plane of the orthorhombic phase. Peak area b indicates the area of ​​a diffraction peak observed in the XRD spectrum near 2θ = 35.4°. This peak is a diffraction peak attributed to reflection from the (001) plane of the orthorhombic phase.

[0025] In the present disclosure, the phrases "around 2θ=30.2°" and "around 2θ=35.4°" mean "2θ=30.2±0.5°" and "2θ=35.4±0.5°", respectively.

[0026] When the (111) plane and the (001) plane are present in the orthorhombic phase, the dielectric 10 is likely to have polarization in the out-of-plane direction. As a result, the dielectric 10 is likely to exhibit ferroelectricity. On the other hand, when the (001) plane is present in the orthorhombic phase, the (010) plane is likely to coexist. When the (010) plane is present, the dielectric 10 is likely to have polarization in the in-plane direction and is unlikely to have polarization in the out-of-plane direction. When the dielectric 10 includes the (001) plane of the orthorhombic phase, the dielectric also includes the (010) plane, which tends to cause variations in the dielectric properties. In this embodiment, the dielectric 10 satisfies 0.87≦a / (a+b)≦0.98. With this configuration, the peak area of ​​the diffraction peak attributable to reflection from the (001) plane is smaller than the peak area of ​​the diffraction peak attributable to reflection from the (111) plane. That is, in the orthorhombic phase, the abundance ratio of the (001) plane is reduced compared to the abundance ratio of the (111) plane. Accordingly, the abundance ratio of the (010) plane can also be reduced in the orthorhombic phase. That is, by satisfying 0.87≦a / (a+b)≦0.98, it is possible to obtain a dielectric 10 in which the (010) plane is unlikely to exist, and therefore the dielectric 10 is likely to exhibit ferroelectricity. The dielectric 10 may satisfy 0.90≦a / (a+b)≦0.98.

[0027] The peak area a and the peak area b can be determined as follows. An XRD measurement is performed on the dielectric 10 to obtain an XRD pattern. For this XRD pattern, Peak Parameters processing is performed on desired peaks using Malvern Panalytical's analysis software Data Viewer. This makes it possible to calculate the peak area a and the peak area b. The desired peaks are the peaks near 2θ = 30.2° and the peaks near 2θ = 35.4°. The Peak Parameters processing is a function that can automatically calculate the net peak area. Note that in calculating the peak area a and the peak area b, manual peak fitting and baseline adjustment were not performed.

[0028] Dielectric 10 may include a solid solution of hafnium oxide and cerium oxide.

[0029] There is no particular limitation on the method for manufacturing the dielectric 10. The method for manufacturing the dielectric 10 includes, for example, manufacturing a film for the dielectric and crystallizing the film for the dielectric.

[0030] For manufacturing the dielectric film, a film formation method such as RF magnetron sputtering, pulsed laser deposition (PLD), atomic layer deposition (ALD), chemical vapor deposition (CVD), mist CVD, sol-gel method, hydrothermal method, anodic oxidation, etc. For crystallization of the dielectric film, a method such as rapid thermal processing (RTA) can be used. This allows a crystalline dielectric 10 to be obtained.

[0031] By appropriately adjusting the conditions for producing the dielectric 10, it is possible to obtain a dielectric 10 in which the molar ratio of the oxygen content to the sum of the hafnium content and the cerium content is greater than 0 and not greater than 1.50. For example, by appropriately adjusting the environment during film formation and the environment during rapid thermal processing, or by appropriately selecting the material of the electrodes in contact with the dielectric 10, it is possible to obtain a dielectric 10 in which the molar ratio is greater than 0 and not greater than 1.50, and a functional device 1a using this dielectric 10.

[0032] As shown in Fig. 1, the functional element 1a includes a first electrode 21, a dielectric 10, and a second electrode 22. The dielectric 10 is located between the first electrode 21 and the second electrode 22. The dielectric 10 is disposed in contact with the first electrode 21. The second electrode 22 may cover at least a portion of the dielectric 10. The first electrode 21 may be disposed on a support. Since the functional element 1a includes the dielectric 10, the chemical stability of the functional element 1a is likely to be improved.

[0033] 2 is a cross-sectional view showing another example of a functional element according to the present disclosure. The functional element 1b shown in FIG. 2 has the same configuration as the functional element 1a, except for portions that will be particularly described. The same reference numerals are used to designate components of the functional element 1b that are the same as or correspond to components of the functional element 1a, and detailed descriptions thereof will be omitted. The description of the functional element 1a also applies to the functional element 1b, unless technically inconsistent.

[0034] 2, in the functional device 1b, at least a portion of the first electrode 21 is porous. This configuration facilitates an increase in the surface area of ​​the first electrode 21. Such a porous structure can be formed by etching a metal foil, sintering a powder, or the like.

[0035] 2, for example, a film of dielectric 10 is formed on the surface of the porous portion of first electrode 21. In this case, the method for forming dielectric 10 can be an atomic layer deposition method (ALD method) or a chemical vapor deposition method such as a CVD method or a mist CVD method.

[0036] The first electrode 21 may contain at least one selected from the group consisting of a metal, a conductive nitride, and a conductive oxide. Examples of metals are Pt, Au, Al, Ta, and Zr. Examples of conductive nitrides are TiN and TaN. Examples of conductive oxides are indium tin oxide (ITO), antimony tin oxide (ATO), and ZnO. The first electrode 21 preferably contains a metal. That is, the first electrode 21 preferably contains at least one selected from the group consisting of Pt, Au, Al, Ta, and Zr. The first electrode 21 may contain Al or may be Al.

[0037] The second electrode 22 may contain at least one selected from the group consisting of a metal, a conductive nitride, and a conductive oxide. Examples of the metal, the conductive nitride, and the conductive oxide are as described above.

[0038] The first electrode 21 and the second electrode 22 can be manufactured by a method such as RF magnetron sputtering, pulsed laser deposition (PLD), atomic layer deposition (ALD), chemical vapor deposition (CVD), mist CVD, sol-gel method, hydrothermal method, or vacuum deposition.

[0039] In the functional elements 1a and 1b, an electrolyte 23 may be disposed between the first electrode 21 and the second electrode 22, more specifically, between the dielectric 10 and the second electrode 22. The electrolyte 23 may be in contact with the second electrode 22. The electrolyte 23 may be in contact with the dielectric 10. In the functional element 1b, the electrolyte 23 is disposed so as to fill voids around the porous portion of the first electrode 21, for example.

[0040] The electrolyte 23 includes, for example, at least one selected from the group consisting of an electrolytic solution, a conductive polymer, and manganese oxide. Examples of the conductive polymer include polypyrrole, polythiophene, polyaniline, and derivatives thereof. The electrolyte 23 may be a manganese compound such as manganese oxide. The electrolyte 23 may also include a solid electrolyte.

[0041] The functional elements 1a and 1b are not limited to specific elements. For example, the functional elements 1a and 1b are at least one selected from the group consisting of a capacitor, an electro-optical element, a memory element, a transistor, a ferroelectric data storage, a piezoelectric element, and a pyroelectric element. For example, the ferroelectricity of the dielectric 10 can be utilized in these functional elements. The functional elements 1a and 1b are preferably at least one selected from the group consisting of a capacitor and a memory element.

[0042] The functional elements 1a and 1b are disposed in at least one selected from the group consisting of an actuator, an inkjet head, a gyro sensor, a vibration power generating element, a surface acoustic wave resonator, a film bulk resonator, a piezoelectric mirror, and a piezoelectric sensor. In this case, the piezoelectric effect due to the ferroelectricity of the dielectric 10 can be utilized in the actuator, etc.

[0043] (Additional Note) From the above description, the following techniques are disclosed.

[0044] (Technology 1) A dielectric comprising an oxide containing hafnium and cerium, wherein a molar ratio of a cerium content to a sum of a hafnium content and a cerium content is 0.031 or more and 0.052 or less, and a molar ratio of an oxygen content to the sum is greater than 0 and 1.50 or less.

[0045] According to the first technique, a novel dielectric 10 suitable for use in functional elements such as capacitors can be provided.

[0046] (Technology 2) The dielectric according to Technology 1, wherein the molar ratio of the oxygen content to the sum is 1.44 or more and 1.50 or less.

[0047] According to the technique 2, a chemically more stable dielectric 10 can be obtained.

[0048] (Technology 3) The dielectric is a compound represented by the composition formula Hf 1-x Ce x O y 3. The dielectric according to claim 1, wherein the dielectric has a composition represented by the following formula:

[0049] (Technology 4) The dielectric according to Technology 3, which satisfies 1.44≦y≦1.50.

[0050] (Technology 5) The dielectric according to any one of Technologies 1 to 4, wherein the dielectric contains a crystalline phase having a fluorite-type crystal structure, and the dielectric is a polycrystalline film.

[0051] According to the fifth technique, the dielectric 10 tends to exhibit ferroelectricity.

[0052] (Technology 6) The dielectric according to any one of Technologies 1 to 5, wherein the dielectric contains an orthorhombic phase, and an X-ray diffraction pattern of the dielectric satisfies 0.87≦a / (a+b)≦0.98, where a is a peak area of ​​a diffraction peak in the X-ray diffraction pattern that is attributed to reflection from a (111) plane of the orthorhombic phase, and b is a peak area of ​​a diffraction peak in the X-ray diffraction pattern that is attributed to reflection from a (001) plane of the orthorhombic phase.

[0053] According to the sixth technique, the dielectric 10 tends to exhibit ferroelectricity.

[0054] (Technology 7) A functional element comprising: a first electrode; a second electrode; and the dielectric according to any one of Technologies 1 to 6, located between the first electrode and the second electrode.

[0055] According to the seventh technique, the functional element 1a includes the dielectric 10, which makes it easier to improve the chemical stability of the functional element 1a.

[0056] (Technology 8) The functional element according to Technology 7, wherein at least a part of the first electrode is porous.

[0057] According to Technique 8, the surface area of ​​the first electrode 21 is likely to increase.

[0058] (Technology 9) The functional element according to Technology 7 or 8, wherein the first electrode includes at least one selected from the group consisting of a metal, a conductive nitride, and a conductive oxide.

[0059] (Technology 10) The functional element according to any one of Techniques 7 to 9, wherein the first electrode includes at least one selected from the group consisting of Pt, Au, Al, Ta, and Zr.

[0060] (Technology 11) The functional element according to any one of Techniques 7 to 10, wherein the first electrode contains Al.

[0061] According to Techniques 9 to 11, since the dielectric 10 is provided, the chemical stability of the functional element 1a is likely to be improved.

[0062] (Technology 12) The functional element according to any one of Techniques 7 to 11, further comprising an electrolyte located between the second electrode and the dielectric, wherein the electrolyte includes at least one selected from the group consisting of an electrolytic solution, a conductive polymer, and manganese oxide.

[0063] According to Technique 12, the chemical stability of the functional element 1b including the electrolyte is likely to be improved.

[0064] (Technology 13) The functional element according to any one of Techniques 7 to 12, wherein the functional element is at least one selected from the group consisting of a capacitor, an electro-optical element, a memory element, a transistor, a ferroelectric data storage, a piezoelectric element, and a pyroelectric element.

[0065] According to the technique 13, a functional element can be provided that makes use of the ferroelectricity of the dielectric 10.

[0066] (Technology 14) The functional element according to any one of Techniques 7 to 13, wherein the dielectric is in contact with the first electrode, and the second electrode covers at least a part of the dielectric.

[0067] The present disclosure will be described in more detail below based on examples, but the present disclosure is not limited to the following examples.

[0068] (Sample Preparation) A Si (111) wafer was used as the substrate. A ZrO2 buffer layer was formed on this substrate. The buffer layer had a thickness of 60 nm. A Pt (111) film was epitaxially grown on this buffer layer to form a thin film as a lower electrode. The thickness of this thin film was 150 nm. In this way, a substrate with a lower electrode formed on the substrate was obtained.

[0069] Next, a dielectric film was formed on the lower electrode of the substrate by RF magnetron sputtering using HfO2 and CeO2 targets. The sputtering time was adjusted so that the dielectric thickness would be 10 to 30 nm. During sputtering, the substrate environment was maintained at a pressure of 2 Pa, with argon gas occupying 100% of the volume. The substrate was not heated.

[0070] The dielectric film was then crystallized by rapid thermal annealing (RTA) to obtain a dielectric film. The rapid thermal annealing environment was maintained at 1 atmosphere pressure, with nitrogen gas and oxygen gas mixed in the desired ratio. The rapid thermal annealing was performed by heating the film to 750°C at a rate of 5°C / sec, holding the film at this temperature for 30 seconds, and then allowing it to cool naturally. A 150 nm-thick Au film was then formed on the dielectric film by vacuum deposition to obtain an Au electrode as the upper electrode. The diameter of the Au electrode was 200 μm. In this manner, samples according to Examples 1 to 3 and Comparative Examples 1 to 4 were fabricated.

[0071] (Composition Evaluation) The composition of the dielectric of each sample was evaluated using an X-ray photoelectron spectroscopy (XPS) analyzer JPS-9010TR manufactured by JEOL Ltd. First, after forming the upper electrode, X-ray photoelectron spectroscopy (XPS) was performed on the dielectric film of each sample to obtain narrow spectra of the Hf4f orbital, Ce3d orbital, and O1s orbital of the dielectric film of each sample. Based on the obtained spectra, the element concentration of each element contained in the dielectric film of each sample was determined using the analysis software SpecSurf attached to the above-mentioned analyzer. Then, using the obtained element concentrations, the composition formula of the dielectric was changed to Hf 1-x Cex O y Assuming this, the values ​​of x and y of the dielectric film for each sample were determined. Specifically, the value of x was determined by calculating the ratio of the elemental concentration of Ce to the elemental concentration of Hf and Ce. The value of y was determined by calculating the ratio of the elemental concentration of O to the elemental concentration of Hf and Ce. The results are shown in Table 1.

[0072] (Evaluation of Dielectric Properties) After forming the upper electrode, a polarization-electric field measurement was performed on the dielectric film of each sample using a ferroelectric tester Premier II manufactured by Radiant Technology, and a P-E curve of the dielectric film of each sample was obtained. Based on this P-E curve, the dielectric properties of the dielectric films of the Examples and Comparative Examples were evaluated. When the dielectric film exhibited ferroelectricity, it was evaluated as "A," and when it exhibited paraelectricity, it was evaluated as "B." The results are shown in Table 1.

[0073] (Evaluation of Crystalline Phase) The crystalline phase contained in the dielectric films according to Examples 1 to 3 was evaluated using an X-ray diffractometer, X'Pert PRO MPD, manufactured by Malvern Panalytical. Before forming the upper electrode, X-ray diffraction measurements were performed on the dielectric films according to Examples 1 to 3 to obtain XRD patterns by 2θ / θ scanning. In this measurement, Cu-Kα radiation was used as the X-ray source. The peak areas a and b were then calculated for the XRD patterns using the Data Viewer analysis software provided with the device, according to the method described above. Then, a / (a + b) was calculated. Here, the peak area a is the area of ​​the diffraction peak attributable to reflection from the (111) plane in the XRD spectrum of the dielectric. The peak area b is the area of ​​the diffraction peak attributable to reflection from the (001) plane in the XRD spectrum of the dielectric. Specifically, the value of a was determined by calculating the area of ​​the peak observed near 2θ = 30.2°. The value of b was determined by calculating the area of ​​the peak observed around 2θ=35.4°. The results are shown in Table 1.

[0074] As shown in Table 1, the dielectrics according to Examples 1 to 3 exhibited ferroelectricity. 1-x Ce x O y In the above, 0.031≦x≦0.052 and 0<y≦1.50 were satisfied. In the dielectrics according to Examples 1 to 3, the concentration of Ce added was reduced, and therefore it can be seen that the chemical stability was improved.

[0075] 3 is a graph showing the relationship between polarization and electric field strength in the dielectric films according to Examples 1 to 3. In Fig. 3, the vertical axis represents polarization and the horizontal axis represents electric field strength. As shown in Fig. 3, in the dielectric films according to Examples 1 to 3, when the electric field strength was 0 MV / cm, the polarization was 0 μC / cm. 2 Instead, remanent polarization was observed. That is, the dielectrics according to Examples 1 to 3 exhibited ferroelectricity.

[0076] 4 is a graph showing the relationship between polarization and electric field strength in the dielectric films according to Comparative Examples 1 to 4. In FIG. 4, the vertical axis represents polarization, and the horizontal axis represents electric field strength. As shown in FIG. 4, in the dielectric films according to Comparative Examples 1 to 4, the polarization is 0 μC / cm when the electric field strength is 0 MV / cm. 2 This polarization was due to leakage current. The dielectric films according to Comparative Examples 1 to 4 did not exhibit ferroelectricity. The dielectric films according to Comparative Examples 1 to 4 had paraelectricity.

[0077] 5 is a graph showing the X-ray diffraction patterns of the dielectrics according to Examples 1 to 3. As shown in FIG. 5, peaks were observed near 2θ=30.2° and near 2θ=35.4° in the dielectric films according to Examples 1 to 3. In addition, as shown in Table 1, the relationship 0.87≦a / (a+b)≦0.98 was satisfied in Examples 1 to 3. This result indicates that the dielectrics used in Examples 1 to 3 are excellent in terms of exhibiting ferroelectricity.

[0078]

[0079] The dielectric of the present disclosure is advantageous in terms of improving chemical stability.

[0080] 1a, 1b Functional element 10 Dielectric 21 First electrode 22 Second electrode 23 Electrolyte

Claims

1. A dielectric comprising an oxide containing hafnium and cerium, wherein the molar ratio of the cerium content to the sum of the hafnium content and the cerium content is 0.031 or more and 0.052 or less, and the molar ratio of the oxygen content to the sum is greater than 0 and less than 1.

50.

2. The dielectric material according to claim 1, wherein the molar ratio of the content of oxygen to the sum is equal to or greater than 1.44 and equal to or less than 1.

50.

3. The dielectric has the composition formula Hf 1-x C.E. x O y The dielectric material according to claim 1 , having a composition represented by the following formula:

4. The dielectric material according to claim 3, wherein 1.44≦y≦1.50 is satisfied.

5. The dielectric according to claim 1, wherein the dielectric contains a crystalline phase having a fluorite type crystal structure, and the dielectric is a polycrystalline film.

6. The dielectric according to claim 1, wherein the dielectric contains an orthorhombic phase, and an X-ray diffraction pattern of the dielectric satisfies 0.87≦a / (a+b)≦0.98, where a is a peak area of ​​a diffraction peak in the X-ray diffraction pattern attributable to reflection from a (111) plane of the orthorhombic phase, and b is a peak area of ​​a diffraction peak in the X-ray diffraction pattern attributable to reflection from a (001) plane of the orthorhombic phase.

7. A functional element comprising: a first electrode; a second electrode; and a dielectric material according to any one of claims 1 to 6 located between the first electrode and the second electrode.

8. The functional element according to claim 7, wherein at least a portion of the first electrode is porous.

9. The functional element according to claim 7, wherein the first electrode includes at least one selected from the group consisting of a metal, a conductive nitride, and a conductive oxide.

10. The functional element according to claim 7, wherein the first electrode contains at least one selected from the group consisting of Pt, Au, Al, Ta, and Zr.

11. The functional element according to claim 7, wherein the first electrode contains Al.

12. The functional element according to claim 7, further comprising an electrolyte located between the second electrode and the dielectric, the electrolyte including at least one selected from the group consisting of an electrolytic solution, a conductive polymer, and manganese oxide.

13. The functional element according to claim 7, wherein the functional element is at least one selected from the group consisting of a capacitor, an electro-optical element, a memory element, a transistor, a ferroelectric data storage, a piezoelectric element, and a pyroelectric element.

14. The functional element according to claim 7, wherein the dielectric is in contact with the first electrode, and the second electrode covers at least a portion of the dielectric.

Citation Information

Patent Citations

  • Semiconductor device and method for manufacturing the same

    WO2006025350A1