Cladding material for laser welding, bonding structure using cladding material for laser welding, and battery manufacturing method
The use of a cladding material with a specific thickness range for laser welding of aluminum and iron-based alloys addresses the challenge of downsizing battery assembly bonding structures by reducing energy losses and space requirements, achieving efficient and strong bonding between dissimilar metals.
Patent Information
- Application Number
- PCT/JP2024/016566
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-25
- Filing Date
- 2024-04-26
- Publication Date
- 2024-11-28
AI Technical Summary
Conventional methods for joining dissimilar metals in battery assemblies, such as those used in electric vehicles, face challenges in downsizing and reducing space requirements due to energy losses in resistance welding and the need for thick aluminum layers in laser welding, which complicates the bonding process and increases the size of the bonding structure.
A cladding material for laser welding comprising an aluminum layer of 20 μm to 140 μm thickness bonded with an iron-based alloy layer, where the aluminum layer is melted first to reduce heat transfer and prevent excessive thickness, allowing for efficient laser welding of dissimilar metals with reduced energy loss and space requirements.
This configuration enables efficient laser welding of dissimilar metals with improved bonding strength and reduced protrusion height, allowing for the downsizing of the bonding structure and minimizing space, while maintaining suitable bonding performance and preventing damage from protrusions.
Smart Images

Figure JP2024016566_28112024_PF_FP_ABST
Abstract
Description
Clad material for laser welding, joint structure using clad material for laser welding, and method for manufacturing battery
[0001] The present invention relates to a clad material for laser welding, a joint structure using the clad material for laser welding, and a method for manufacturing a battery.
[0002] Conventionally, a battery pack configured with multiple cells having a structure in which bus bars are joined to terminals has been known for use in vehicles and other applications that require high impact resistance. A battery pack having such a structure is disclosed, for example, in Japanese Patent Application Laid-Open No. 2008-66001.
[0003] The above-mentioned Japanese Patent Application Laid-Open No. 2008-66001 discloses a battery pack that is suitable for vehicle use and is made up of multiple batteries. In this application, multiple batteries are arranged side by side, and adjacent batteries are connected by bus bars (lead plates). The bus bars are also welded to the battery terminals.
[0004] Although not disclosed in the above-mentioned JP 2008-66001 A, there are cases in which the battery terminal is made of an iron-based alloy and the bus bar is made of pure aluminum or an aluminum alloy. A battery terminal made of an iron-based alloy and a bus bar made of pure aluminum or an aluminum alloy are welded together, which is dissimilar metals, and therefore a brittle intermetallic compound is formed at the joint between the battery terminal and the bus bar, resulting in a decrease in joint strength.
[0005] Therefore, it has been proposed to place a clad insert between the bus bar and the battery terminal, as disclosed in, for example, Japanese Patent Laid-Open Publication No. 7-155964.
[0006] Japanese Patent Laid-Open Publication No. 7-155964 discloses a clad insert material suitable for resistance welding, which is configured by overlapping and joining steel and aluminum. In Japanese Patent Laid-Open Publication No. 7-155964, a steel layer of the clad insert material, which is an iron-based alloy, is resistance welded to a surface-treated steel sheet, and an aluminum layer of the clad insert material is resistance welded to an aluminum sheet. Specifically, resistance welding is performed by sandwiching the surface-treated steel sheet, the clad insert material, and the aluminum sheet, which are overlapped in this order, between a pair of resistance welding electrodes.
[0007] JP 2008-66001 JP 7-155964
[0008] Resistance welding is a welding method that melts and welds a welded portion by utilizing Joule heat generated at the welded portion due to contact resistance between the metals being welded or Joule heat generated by the resistance of the metals being welded themselves. Resistance welding involves significant energy loss when welding a narrow portion because the generated heat is easily lost by conduction to the metals being welded and the electrodes. Therefore, the clad insert material disclosed in JP-A-7-155964 is believed to have an aluminum layer thickness of more than 0.2 mm (claim 1 of JP-A-7-155964), which is easily melted with a smaller amount of heat. Therefore, clad insert materials used in welding methods that melt and join joints, such as resistance welding, are believed to need to ensure (enough thick) an aluminum layer with a low melting point.
[0009] Furthermore, when the clad insert material disclosed in JP-A-7-155964 is used for resistance welding, a pair of electrodes must be arranged to sandwich the clad insert material. However, depending on the structure of the battery pack, the space may be small and it may be difficult to arrange electrodes for each battery. In such cases, laser welding, which does not require electrodes as in resistance welding and is advantageous for space saving, has been proposed. Note that when using a clad insert material for laser welding, which melts and joins the welded portion by laser irradiation, it is also considered necessary to ensure a sufficient thickness (enough thickness) of the aluminum layer, which has a low melting point.
[0010] In recent years, the rapid spread of electric vehicles, driven by environmental issues such as global warming, has led to a strong demand for improved performance and downsizing (miniaturization) of on-board battery packs. Therefore, there is an urgent need to improve the performance of battery packs and to downsize the numerous joint structures that make up the battery packs. However, the clad insert material disclosed in the above-mentioned Japanese Patent Laid-Open Publication No. 7-155964 has a problem in that it is difficult to downsize the material because the thickness of the aluminum layer must be sufficiently large.
[0011] The present invention has been made to solve the problem of downsizing the joining structure that constitutes the above-mentioned assembled battery, and one object of the present invention is to provide a clad material for laser welding, a joining structure using a clad material for laser welding, and a method for manufacturing a battery, which are suitable for laser welding, which allows downsizing of a joining structure that involves joining dissimilar metals, and which can reduce the space required to arrange the joining structure.
[0012] In order to achieve the above object, the inventors of the present application focused on the configuration of the aluminum layer (Al layer) of the clad insert material disclosed in the above Patent Document 2, and conducted extensive research to develop a clad material (clad insert material) suitable for laser welding, and found the following configuration: That is, a clad material for laser welding according to a first aspect of the present invention is a clad material for laser welding to be laser welded to another member made of an iron-based alloy, and is composed of an Al layer made of pure aluminum or an aluminum alloy and an Fe layer made of an iron-based alloy and roll-bonded to the Al layer, the Al layer having a thickness of 20 μm or more and 140 μm or less, and the Fe layer is laser welded to the other member by laser irradiation from the Al layer side.
[0013]
[0013] The laser welding clad material according to a first aspect of the present invention, as described above, is composed of an Al layer made of pure aluminum or an aluminum alloy and an Fe layer made of an iron-based alloy roll-bonded to the Al layer, the Al layer having a thickness of 20 μm or more and 140 μm or less, and is laser welded to another member by laser irradiation from the Al layer side. Since the Al layer has a thickness of 20 μm or more, the Al layer, which has a melting point sufficiently lower than that of the Fe layer, is rapidly melted by laser irradiation from the Al layer side, thereby rapidly transferring heat from the molten Al layer to the Fe layer, and rapidly melting the laser welding clad material in the thickness direction. As a result, a laser welding clad material can be provided that can be joined to another member made of an iron-based alloy by general laser welding, which does not involve significant energy loss as in resistance welding.
[0014] Furthermore, since the thickness of the Al layer is 140 μm or less, an Al amount (thickness of the Al layer) suitable for laser welding is ensured, while an excessive Al amount (thickness of the Al layer) is not present, and therefore the thickness of the clad material for laser welding can be prevented from becoming excessively large. As a result, the entire clad material for laser welding can be made thinner, and therefore, it is possible to downsize a joining structure in which dissimilar metals are joined using the clad material for laser welding.
[0015] Furthermore, by setting the thickness of the Al layer to 20 μm or more and 140 μm or less, the protrusion height of the protrusion formed on the laser-irradiated side of the Al layer due to volumetric changes when the Al layer melted by laser irradiation solidifies can be reduced. As a result, the protrusion height of the protrusion formed on the exposed surface of the Al layer due to laser welding is small, and the entire laser welding clad material can be thinned, thereby enabling downsizing of a joint structure in which dissimilar metals are joined using a laser welding clad material. Note that the inventors of the present application have found through experiments (Examples) described below that the above effects can be achieved by setting the thickness of the Al layer to 20 μm or more and 140 μm or less. Furthermore, by enabling downsizing of the joint structure, the space required for arranging the joint structure can be reduced. As a result, the joint structure involving the joining of dissimilar metals can be downsized and the space required for arranging the joint structure can be reduced.
[0016] In the clad material for laser welding according to the first aspect, the thickness of the Al layer is preferably 40 μm or more and 140 μm or less. With this configuration, the proportion of the volume change that occurs when the Al layer melted by laser irradiation solidifies is contained within the Al layer, and it has been found through experiments described below that the protrusion height of the protrusion formed on the exposed surface of the Al layer on the laser irradiation side can be made smaller.
[0017] A joining structure using a clad material for laser welding according to a second aspect of the present invention includes a clad material for laser welding including an Al layer made of pure aluminum or an aluminum alloy, and an Fe layer made of an iron-based alloy and roll-joined to the Al layer, where the Al layer has a thickness of 20 μm or more and 140 μm or less, and another member made of an iron-based alloy and laser-welded to the Fe layer, and the Fe layer is laser-welded to the other member by laser irradiation from the Al layer side.
[0018]
[0013] A joining structure using a clad material for laser welding according to a second aspect of the present invention includes an Al layer made of pure aluminum or an aluminum alloy and an Fe layer made of an iron-based alloy roll-bonded to the Al layer, the Al layer having a thickness of 20 μm to 140 μm, and the Al layer is laser welded to another member by laser irradiation from the Al layer side. Because the Al layer has a thickness of 20 μm or more, the Al layer, which has a melting point significantly lower than that of the Fe layer, is rapidly melted by laser irradiation from the Al layer side, thereby rapidly transferring heat from the molten Al layer to the Fe layer and rapidly melting the clad material for laser welding in the thickness direction. As a result, general laser welding can be applied as described above, and a joining structure can be provided in which dissimilar metals are joined by laser welding using a clad material for laser welding.
[0019] Furthermore, since the thickness of the Al layer is 140 μm or less, an amount of Al suitable for laser welding (thickness of the Al layer) is ensured, while an excessive amount of Al (thickness of the Al layer) is not present, and therefore, the thickness of the clad material for laser welding can be prevented from becoming excessively large. As a result, as described above, it is possible to downsize the joining structure in which dissimilar metals are joined using the clad material for laser welding.
[0020] Furthermore, by setting the thickness of the Al layer to 20 μm or more and 140 μm or less, the protrusion height of the protrusion formed on the laser-irradiated side of the Al layer due to the volume change when the Al layer melted by laser irradiation solidifies can be reduced. As a result, as described above, it is possible to downsize a joint structure in which dissimilar metals are joined using a laser welding clad material. Note that the inventors of the present application have found through experiments (examples) described below that the above effects can be achieved by setting the thickness of the Al layer to 20 μm or more and 140 μm or less. Furthermore, by being able to downsize the joint structure, the space required for arranging the joint structure can be reduced. As a result, it is possible to downsize a joint structure involving the joining of dissimilar metals, and it is also possible to reduce the space required for arranging the joint structure.
[0021] In the joining structure using the clad material for laser welding according to the second aspect, preferably, the length of the molten portion formed on the joining surface between the Fe layer and the other member by laser welding in the direction of extension of the joining surface is 40 μm or more. With this configuration, the joining strength between the clad material for laser welding and the other member can be appropriately increased. Note that the inventors of the present application have found through experiments (examples) described below that the above-mentioned effect can be obtained by setting the length of the molten portion in the direction of extension of the joining surface to 40 μm or more.
[0022] In the joining structure using the laser welding clad material according to the second aspect, preferably, the protrusion formed on the exposed surface of the Al layer opposite the surface where the Fe layer is roll-joined by laser irradiation from the Al layer side has a protrusion height of 20 μm or less. With this configuration, the protrusion height is sufficiently small, which can prevent the protrusion from contacting members other than the laser welding clad material. As a result, the risk of the protrusion being damaged by contact with members other than the laser welding clad material and causing fragments of the damaged protrusion to become unstable in the joining structure and the operation of the battery pack can be reduced.
[0023] In this case, preferably, the thickness of the Al layer is 40 μm or more and 140 μm or less, and the protrusion height formed on the exposed surface of the Al layer opposite the surface where the Fe layer is roll-bonded by irradiating a laser from the Al layer side to the Fe layer side is 15 μm or less. With this configuration, the protrusion height of 15 μm or less can be further prevented from contacting components other than the laser welding clad material. As a result, the risk of instability in the joint structure and the operation of the battery pack due to the protrusion contacting components other than the laser welding clad material can be further reduced. The inventors of the present application have found through experiments described below that the protrusion height of the protrusion can be reduced to 15 μm or less by setting the thickness of the Al layer to 40 μm or more and 140 μm or less.
[0024] A battery manufacturing method according to a third aspect of the present invention includes the steps of: preparing a clad material for laser welding by roll-bonding an Al plate made of pure aluminum or an aluminum alloy with an Fe plate made of an iron-based alloy, the clad material being composed of an Al layer and an Fe layer, the Al layer having a thickness of 20 μm or more and 140 μm or less; bonding a battery terminal member made of an iron-based alloy to the Fe layer; bonding one end of an Al-based wire for bonding to the Al layer by wire bonding; and bonding the other end of the Al-based wire to a bus bar made of pure aluminum or an aluminum alloy.
[0025] A battery manufacturing method according to a third aspect of the present invention includes the step of preparing a clad material for laser welding by roll-bonding an Al plate made of pure aluminum or an aluminum alloy with an Fe plate made of an iron-based alloy, the clad material being composed of an Al layer and an Fe layer, the Al layer having a thickness of 20 μm to 140 μm. Because the Al layer has a thickness of 20 μm or more, the Al layer, which has a melting point significantly lower than that of the Fe layer, is rapidly melted by laser irradiation from the Al layer side, thereby rapidly transferring heat from the molten Al layer to the Fe layer and rapidly melting the clad material for laser welding in the thickness direction. As a result, a battery can be manufactured using general laser welding, as described above.
[0026] Furthermore, by having an Al layer thickness of 140 μm or less, an Al amount (thickness of the Al layer) suitable for laser welding is ensured, while the absence of an excessive Al amount (thickness of the Al layer) prevents the thickness of the clad material for laser welding from becoming excessively large. As a result, as described above, this is advantageous for downsizing a joining structure in which dissimilar metals are joined using a clad material for laser welding, making it possible to manufacture a battery that can be downsized appropriately. Furthermore, by being able to downsize the joining structure, the space required to arrange the joining structure can be reduced, making it possible to manufacture a battery that can be downsized.
[0027] Furthermore, by setting the thickness of the Al layer to 20 μm or more and 140 μm or less, the protrusion height of the protrusion formed on the laser-irradiated side of the Al layer due to the volume change when the Al layer melted by laser irradiation solidifies can be reduced. As a result, as described above, this is advantageous for downsizing a joint structure in which dissimilar metals are joined using a laser welding clad material, making it possible to manufacture a battery that can be appropriately downsized. Note that the inventors of the present application have found through experiments (examples) described below that the above effects can be achieved by setting the thickness of the Al layer to 20 μm or more and 140 μm or less. As a result, it is possible to downsize a joint structure involving the joining of dissimilar metals, and it is also possible to reduce the space required to place the joint structure.
[0028] According to the present invention, it is possible to provide a clad material for laser welding, a joint structure using a clad material for laser welding, and a method for manufacturing a battery, which are suitable for laser welding that enables downsizing of a joint structure involving joining of metals together and reduces the space required to arrange the joint structure.
[0029] 1 is a diagram showing an assembled battery according to the present embodiment; FIG. 2 is a diagram showing an example of a clad material for laser welding according to the present embodiment; FIG. 3 is a diagram showing a state in which the clad material for laser welding according to the present embodiment and a lid material are joined; FIG. 4 is a diagram showing a laser irradiation position on the clad material for laser welding when the clad material for laser welding according to the present embodiment is laser welded to a battery terminal; FIG. 5 is a cross-sectional view of a part of a joining structure using a clad material for laser welding, showing a state in which the clad material for laser welding has been laser welded to a lid material; FIG. 6 is a diagram showing an example of a cell according to the present embodiment; FIG. 7 is a diagram showing a manufacturing method of the clad material for laser welding according to the present embodiment; FIG. 8 is a diagram for explaining a method of joining the clad material for laser welding according to the present embodiment to a battery terminal; FIG. 9 is a diagram for explaining a wire bonding method according to the present embodiment; FIG. 10 is a graph showing the relationship between the thickness of the Al layer of the clad material for laser welding and the joining strength, fusion width, penetration depth, and protrusion height; and FIG. 11 is a diagram showing an assembled battery according to a modified example.
[0030] Hereinafter, an embodiment of the present invention will be described with reference to the drawings.
[0031] As shown in FIG. 1 , a clad material for laser welding 1 according to an embodiment of the present invention is used in a battery pack 100. The battery pack 100 is configured by electrically connecting a plurality of lithium ion secondary batteries 10 via bus bars 20. Note that while the battery pack 100 is shown in a simplified form in FIG. 1 , the number of lithium ion secondary batteries 10 constituting the battery pack 100 for vehicle use or the like is greater than that shown in FIG. 1 . The vehicle battery pack 100 is a large battery system mounted in an electric vehicle (EV) or a hybrid electric vehicle (HEV). Note that the battery pack 100 is an example of a "battery" as defined in the claims.
[0032] As shown in Fig. 2, the laser welding clad material 1 is composed of an Al layer 1a and an Fe layer 1b. In Fig. 2, the laser welding clad material 1 has a circular shape, but the shape of the laser welding clad material 1 is not limited to this.
[0033] The Al layer 1a is made of pure aluminum or an aluminum alloy. Pure aluminum has an aluminum content of 99% or more and 100% or less, such as JIS A1000 series aluminum alloys including A1050. Aluminum alloys are alloys in which other elements such as Mn or Mg are added to Al, such as JIS A3000 series aluminum alloys including A3003 and JIS A5000 series aluminum alloys including A5052.
[0034] The Fe layer 1b is made of an iron-based alloy. The iron-based alloy is an alloy in which Fe is the largest content among the constituent metal elements. Among iron-based alloys, those containing approximately 10% by mass or more of Cr are considered to be stainless steel. From the viewpoint of durability, the iron-based alloy constituting the Fe layer 1b is preferably an iron-based stainless steel containing 10% by mass or more of Cr. Furthermore, the iron-based alloy constituting the Fe layer 1b is preferably a ferritic stainless steel, which is a stainless steel that does not contain Ni, in order to reduce the difference in hardness with the Al layer 1a. The ferritic stainless steel is a stainless steel that contains 16% by mass or more and 18% by mass or less of Cr and whose main metal structure is a ferrite phase with a body-centered cubic lattice structure even at room temperature, such as SUS430.
[0035] As shown in Figures 2 and 5, the total thickness t1 of the laser welding clad material 1 is 200 µm or more and 400 µm or less. The thickness t2 of the Al layer 1a is 20 µm or more and 140 µm or less. The thickness t2 of the Al layer 1a is set to 20 µm or more so that the Al layer 1a, which has a melting point sufficiently lower than that of the Fe layer 1b, can be rapidly melted by laser irradiation from the Al layer 1a side, rapidly transferring heat from the Al layer 1a to the Fe layer 1b, and rapidly penetrating toward the Z2 side in the thickness direction (Z direction) of the laser welding clad material 1. The thickness t2 of the Al layer 1a is set to 140 µm or less so that the total thickness t1 of the laser welding clad material 1 does not become excessively large by ensuring an Al content suitable for laser welding without an excessive Al content. Furthermore, the thickness t2 of the Al layer 1a is set to 20 μm or more and 140 μm or less in order to reduce the protrusion height x3 of the protrusion 1d formed on the laser irradiation side of the Al layer 1a due to the volume change when the Al layer melted by laser irradiation solidifies.
[0036] The thickness t2 of the Al layer 1a is set to 20 μm or more to prevent peeling of a portion of the Al layer 1a by setting the protrusion height x3 of the protrusion 1d formed on the exposed surface 1c (Z1-side surface) of the Al layer 1a, which is the surface of the Al layer 1a opposite to the surface bonded to the Fe layer 1b, to 20 μm or less. The thickness t2 of the Al layer 1a is set to 40 μm or more and 140 μm or less to further prevent peeling of a portion of the Al layer 1a by setting the protrusion height x3 of the protrusion 1d formed on the exposed surface 1c (Z1-side surface) of the Al layer 1a to 15 μm or less.
[0037] As shown in FIG. 3 , a terminal (negative or positive electrode terminal) made of an iron-based alloy of a lithium-ion secondary battery 10 is joined to the Fe layer 1b of the laser welding clad material 1. FIG. 3 shows a configuration example in which a lid member 12 made of an iron-based alloy, which serves as a positive electrode terminal, is joined to the Fe layer 1b. The joining method is laser welding. By irradiating the Al layer 1a with a laser from the Z1 side, the Al layer 1a and the Fe layer 1b melt in the Z direction and a portion of the lid member 12 melts, joining the laser welding clad material 1 and the lid member 12. The type of laser can be selected depending on various conditions such as the joining structure, and is not limited. The lid member 12 is an example of the "other member" and "electronic terminal member" described in the claims.
[0038] For example, when the laser welding clad material 1 has a circular shape, the laser irradiation to the Al layer 1a can be performed in a circular shape within the region where the laser welding clad material 1 and the lid material 12 overlap, as shown by the dashed line in Fig. 4 which shows the laser irradiation position on the laser welding clad material 1. For example, when the diameter of the laser welding clad material 1 and the lid material 12 is about 23 mm, the laser irradiation can be performed in a circular shape with a diameter of about 20 mm or less (for example, 15 mm).
[0039] For example, when laser irradiation is performed from the Z1 side of the Al layer 1a to laser-weld the laser welding clad material 1 to the lid member 12, the laser irradiation melts the laser welding clad material 1 and fuses it into the lid member 12, as indicated by the two-dot chain line in Figure 5, which shows a portion of the joint structure. At this time, the length (melt width) x1 of the molten portion formed on the joining surface 1e by laser welding between the Fe layer 1b of the laser welding clad material 1 and the lid member 12 in the extending direction (X direction) of the joining surface 1e is preferably 40 μm or more. Note that while Figure 5 shows an X-Z cross section, the joining surface 1e of the molten portion is parallel to the X-Y plane. Also, although the extending direction of the joining surface 1e of the molten portion is the X direction in Figure 5, the extending direction of the joining surface 1e may be the Y direction.
[0040] 5 may be 50 μm or more and 130 μm or less. This configuration allows the lid material 12 to be thinned while being bonded to the laser welding clad material 1 with an appropriate bonding strength. As a result, it is possible to downsize the bonding structure between dissimilar metals using the laser welding clad material 1. The penetration depth refers to the amount (length) of the lid material 12 melted in the Z direction by laser irradiation, based on the bonding surface 1e of the molten portion.
[0041] As shown in Fig. 5, a protrusion 1d is formed on the exposed surface 1c of the Al layer 1a, protruding toward the opposite side (Z1 side) from the lid member 12 (Fe layer 1b) due to a volume change when the Al layer 1a melted by laser irradiation solidifies. The protrusion height x3 of the protrusion 1d is preferably 20 µm or less to prevent breakage of the protrusion 1d. Furthermore, the protrusion height x3 of the protrusion 1d is more preferably 15 µm or less to further prevent breakage of the protrusion 1d.
[0042] A bus bar 20 is bonded to the exposed surface 1c of the Al layer 1a. For bonding to the bus bar 20, for example, wire bonding is used. Specifically, as shown in Fig. 9, one end of an Al-based bonding wire 2 is bonded to the Al layer 1a by wire bonding, and the other end of the Al-based bonding wire 2 is bonded to a recess 20a of the bus bar 20 by wire bonding. The Al-based wire 2 is made of pure aluminum or an aluminum alloy.
[0043] 6 , lithium ion secondary battery 10 includes cylindrical housing 11, lid 12 that seals the opening of housing 11, and power storage element 13 disposed within housing 11. Housing 11 is made of Ni-plated steel sheet and also serves as the negative electrode terminal of lithium ion secondary battery 10.
[0044] The housing 11 contains a storage element 13 and an electrolyte (not shown). The lid member 12 is made of an iron-based alloy and also serves as the positive electrode terminal of the lithium-ion secondary battery 10. The storage element 13 is formed by winding a positive electrode 14, a negative electrode 15, and an insulating separator 16 disposed between the positive electrode 14 and the negative electrode 15. The positive electrode 14 includes a positive electrode current collector (not shown) made of aluminum foil and a positive electrode active material layer (not shown) disposed on the surface of the positive electrode current collector. The positive electrode active material layer includes a positive electrode active material such as lithium manganate and a binder formed of a resin material.
[0045] The lithium-ion secondary battery 10 further includes a positive electrode lead material 17 for connecting the positive electrode 14 and the positive electrode terminal (lid material 12), and a negative electrode lead material 18 for connecting the negative electrode 15 and the negative electrode terminal (casing 11). The positive electrode lead material 17 is made of aluminum foil and is joined to the positive electrode current collector of the positive electrode 14 and the lid material 12 by resistance welding or the like. The negative electrode lead material 18 is made of copper foil and is joined to the negative electrode current collector of the negative electrode 15 and the casing 11 by resistance welding or the like.
[0046] As shown in FIG. 1 , the busbar 20 is made of pure aluminum or an aluminum alloy. The busbar 20 electrically connects the terminals (negative electrode terminal, positive electrode terminal) of the lithium-ion secondary battery 10. In this embodiment, the busbar 20 has a plate-like shape and electrically connects the positive electrode terminals of multiple cells (lithium-ion secondary batteries 10). In this embodiment, the laser welding clad material 1 is disposed between the busbar 20 and the positive electrode terminal of the lithium-ion secondary battery 10. As shown in FIG. 1 , a recess 20 a is provided in a portion of the busbar 20 where the Al-based wire 2 is connected. Note that while FIG. 1 illustrates an example in which the recess 20 a is provided on one side (X1 side) in the short direction, the recess 20 a may be provided on both the one side (X1 side) and the other side (X2 side) in the short direction. A single busbar 20 can simultaneously connect multiple terminals. Although not shown in FIG. 1 , negative electrode terminals are also connected to each other by another busbar. The negative electrode terminal and another bus bar are joined by laser welding, spot welding, or the like. The battery pack 100 shown in FIG. 1 is intended to illustrate an example of the configuration of the portion connecting the positive electrode terminals to each other with the bus bar 20, and other connection portions and the like are omitted. The battery pack may also be configured to connect the positive electrode terminal and the negative electrode terminal with a bus bar. The battery pack may also be configured to combine a configuration in which the positive electrode terminals are connected to each other with a bus bar and the negative electrode terminals are connected to each other with a bus bar, with a configuration in which the positive electrode terminal and the negative electrode terminal are connected to each other with a bus bar.
[0047] (Battery Manufacturing Method) As shown in FIG. 7 , an Al plate 50a and an Fe plate 50b are roll-bonded to prepare a laser welding clad material 1, which is composed of an Al layer 1a and an Fe layer 1b, with the Al layer 1a having a thickness of 20 μm or more and 140 μm or less. The Al plate 50a is a plate made of the same pure aluminum or aluminum alloy as the Al layer 1a. The Fe plate 50b is a plate made of the same iron-based alloy as the Fe layer 1b. In the roll-bonding, the rolling ratio (degree of processing) is set so that the thicknesses of the Al plate 50a and the Fe plate 50b before rolling are the same as the thicknesses of the Al layer 1a and the Fe layer 1b after rolling. Although not shown in FIG. 7 , diffusion annealing may be performed after the Al plate 50a and the Fe plate 50b are roll-bonded. Furthermore, softening annealing may be performed before the Al plate material 50a and the Fe plate material 50b are roll-bonded together. Furthermore, after the Al plate material 50a and the Fe plate material 50b are roll-bonded together, further rolling may be performed to obtain the desired thickness of the Al layer 1a and the desired thickness of the Fe layer 1b. Furthermore, softening annealing may be performed before further rolling. The produced laser welding clad material 1 is then processed, for example, into a circular shape. The method of processing into a circular shape may be performed by punching the laser welding clad material 1. The diameter of the circularly formed laser welding clad material 1 is set to be suitable for the diameter of the terminal to be joined.
[0048] When constructing the battery pack 100 shown in FIG. 1 , the Fe layer 1b of the laser-welded clad material 1 is joined to a battery terminal member as shown in FIG. 8 . In FIG. 8 , the battery terminal member is the lid member 12 (positive terminal). Depending on the configuration of the battery pack, the negative terminal (the outer bottom surface of the housing 11) can also be joined to the Fe layer 1b of the laser-welded clad material 1. The method for joining the Fe layer 1b of the laser-welded clad material 1 to the battery terminal member is laser welding. In laser welding, the laser irradiation unit 40 is positioned on the Al layer 1a side (Z1 side) and laser irradiation is performed. For example, as shown by the dashed line in FIG. 4 , the laser irradiation is performed so as to form a circular trajectory along the outer periphery of the circular laser-welded clad material 1. This forms a joint structure involving joining dissimilar metals composed of the laser-welded clad material 1 and the lid member 12.
[0049] 9, after the laser welding clad material 1 is joined to the battery terminal member, the bus bar 20 is joined to the Al layer 1a. The method of joining the bus bar 20 to the Al layer 1a involves joining one end of an Al-based wire 2 for joining to the Al layer 1a by wire bonding, and also joining the other end of the Al-based wire 2 to the recess 20a of the bus bar 20 by wire bonding.
[0050] Wire bonding can be performed in two ways: one in which one end and the other end of the Al-based wire 2 are melted to form a ball-shaped bond, and the other in which no ball-shaped bond is formed. Methods for bonding one end and the other end of the Al-based wire 2 to the Al layer 1 a and the bus bar 20, respectively, include a method using heat, a method using pressure, a method using ultrasonic waves, or a method using an appropriate combination of heat, pressure, ultrasonic waves, etc. When ultrasonic waves are used, for example, one end of the wire is pressed against the Al layer 1 a of the laser welding clad material 1 with a tool 50, and ultrasonic vibrations are applied to generate heat inside, melting and bonding the one end of the wire and the vicinity of the surface of the Al layer 1 a.
[0051] <Effects of this embodiment> In this embodiment, the following effects can be obtained.
[0052] In this embodiment, the laser welding clad material 1 is composed of an Al layer 1a made of pure aluminum or an aluminum alloy and an Fe layer 1b made of an iron-based alloy and roll-bonded to the Al layer 1a. The Al layer 1a has a thickness of 20 μm or more and 140 μm or less, and is laser welded to another member by laser irradiation from the Al layer 1a side. Because the Al layer 1a has a thickness of 20 μm or more, the Al layer 1a, which has a melting point sufficiently lower than that of the Fe layer 1b, is quickly melted by laser irradiation from the Al layer 1a side. Therefore, heat is quickly transferred from the molten Al layer 1a to the Fe layer 1b, and the laser welding clad material 1 can be quickly melted in the thickness direction (Z direction) of the laser welding clad material 1. As a result, it is possible to provide a laser welding clad material 1 that can be joined to another member (lid member 12) made of an iron-based alloy by general laser welding, which does not involve significant energy loss like resistance welding. Furthermore, since the thickness of the Al layer 1a is 140 μm or less, an Al content suitable for laser welding is ensured, while the absence of an excessive Al content prevents the laser welding clad material 1 from becoming excessively thick. As a result, the entire laser welding clad material 1 can be thinned, thereby enabling downsizing of a joining structure in which dissimilar metals are joined using the laser welding clad material 1. Furthermore, since the thickness of the Al layer 1a is 20 μm or more and 140 μm or less, the protrusion height of the protrusion 1d formed on the laser irradiation side (Z1 side) of the Al layer 1a due to a volume change when the Al layer 1a melted by laser irradiation solidifies can be reduced. As a result, the protrusion height of the protrusion 1d formed on the exposed surface 1c of the Al layer 1a due to laser welding is small, and the entire laser welding clad material 1 can be thinned, which is advantageous for downsizing of a joining structure in which dissimilar metals are joined using the laser welding clad material 1. The inventors of the present invention have found through experiments (Examples) described below that the above-mentioned effects can be obtained by setting the thickness of the Al layer 1a to 20 μm or more and 140 μm or less. In addition, the junction structure can be downsized, thereby reducing the space required for arranging the junction structure.As a result, it is possible to downsize a joining structure involving joining of dissimilar metals, and also to reduce the space required to arrange the joining structure.
[0053] In this embodiment, the thickness of the Al layer 1a is 40 μm or more and 140 μm or less. This increases the proportion of the volume change that occurs when the Al layer 1a melted by laser irradiation solidifies within the Al layer 1a, and it has been found through experiments described below that this makes it possible to further reduce the protrusion height of the protrusion 1d formed on the exposed surface 1c of the Al layer 1a on the laser irradiation side (Z1 side).
[0054] Furthermore, the joining structure using the laser welding clad material 1 according to this embodiment is composed of an Al layer 1a made of pure aluminum or an aluminum alloy and an Fe layer 1b made of an iron-based alloy and roll-bonded to the Al layer 1a, as described above. The thickness t2 of the Al layer 1a is 20 μm or more and 140 μm or less, and the Al layer 1a is laser-welded to the lid member 12 by laser irradiation from the Al layer 1a side. Since the thickness of the Al layer 1a is 20 μm or more, the Al layer 1a, which has a melting point sufficiently lower than that of the Fe layer 1b, is quickly melted by laser irradiation from the Al layer 1a side (Z1 side). Therefore, heat transfer from the molten Al layer 1a to the Fe layer 1b is quickly performed, and the laser welding clad material 1 can quickly penetrate in the thickness direction (Z direction). As a result, since general laser welding can be applied as described above, a welding structure in which dissimilar metals are joined by laser welding using the laser welding clad material 1 can be provided. Furthermore, by having the thickness of the Al layer 1a be 140 μm or less, an Al content suitable for laser welding is ensured, while the absence of an excessive Al content prevents the thickness of the laser welding clad material 1 from becoming excessively large. As a result, as described above, the laser welding clad material 1 can be used to downsize a joining structure involving laser welding of dissimilar metals. Furthermore, by having the thickness of the Al layer 1a be 20 μm or more and 140 μm or less, the protrusion height of the protrusion 1d formed on the laser irradiation side (Z1 side) of the Al layer 1a due to a volume change when the Al layer 1a melted by laser irradiation solidifies can be reduced. As a result, as described above, the laser welding clad material 1 can be used to downsize a joining structure involving laser welding of dissimilar metals. The inventors of the present application have found through experiments (examples) described below that the above-mentioned effects can be achieved by setting the thickness of the Al layer 1a to be 20 μm or more and 140 μm or less. Furthermore, the ability to downsize the joining structure allows for a reduction in the space required to place the joining structure. As a result, it is possible to downsize the joining structure involving the joining of dissimilar metals, and also to reduce the space required to place the joining structure.
[0055] In this embodiment, the length of the molten portion formed on the joining surface 1e by laser welding between the Fe layer 1b and another member in the extending direction of the joining surface is 40 μm or more. This allows the joining strength between the laser welding clad material 1 and the other member (lid material 12) to be appropriately increased. Note that the inventors of the present application have found through experiments (examples) described below that the above-mentioned effects can be obtained by setting the length of the molten portion in the extending direction (X direction) of the joining surface 1e to 40 μm or more.
[0056] Furthermore, in this embodiment, as described above, the protrusion height of the protrusion 1d formed on the exposed surface 1c of the Al layer 1a opposite to the surface to which the Fe layer 1b is roll-bonded by laser irradiation from the Al layer 1a side is 20 μm or less. This sufficiently small protrusion height of the protrusion 1d can prevent the protrusion 1d from contacting members other than the laser welding clad material 1. As a result, a joining structure can be provided that can reduce the risk of the protrusion 1d being damaged by contact with members other than the laser welding clad material 1 and causing fragments of the damaged protrusion 1d to become unstable in the operation of the joining structure and the battery pack.
[0057] In this embodiment, the thickness of the Al layer 1a is preferably 40 μm or more and 140 μm or less, and the protrusion height x3 of the protrusion 1d formed on the exposed surface 1c of the Al layer 1a opposite to the surface to which the Fe layer 1b is roll-bonded by irradiating the Al layer 1a side (Z1 side) with a laser is 15 μm or less. This further prevents the protrusion 1d from contacting components other than the laser-welded clad material 1. As a result, the risk of instability in the joint structure and the operation of the battery pack due to the protrusion 1d contacting components other than the laser-welded clad material 1 can be further reduced. Note that the inventors of the present application have found through experiments described below that the protrusion height x3 of the protrusion 1d can be reduced to 15 μm or less by setting the thickness of the Al layer 1a to 40 μm or more and 140 μm or less.
[0058] The battery manufacturing method of this embodiment also includes a step of preparing a laser-welded clad material 1, which is composed of an Al layer 1a and an Fe layer 1b, by roll-bonding an Al plate 50a made of pure aluminum or an aluminum alloy and an Fe plate 50b made of an iron-based alloy, where the Al layer 1a has a thickness of 20 μm or more and 140 μm or less. Because the Al layer 1a has a thickness of 20 μm or more, the Al layer 1a, which has a melting point sufficiently lower than that of the Fe layer 1b, is rapidly melted by laser irradiation from the Al layer 1a side (Z1 side). This allows rapid heat transfer from the molten Al layer 1a to the Fe layer 1b, and rapid penetration of the laser-welded clad material 1 in the thickness direction (Z direction). As a result, a battery can be manufactured using general laser welding, as described above. Furthermore, by having the thickness of the Al layer 1a be 140 μm or less, an Al content suitable for laser welding is ensured, while the absence of an excessive Al content prevents the thickness of the laser welding clad material 1 from becoming excessively large. As a result, as described above, this is advantageous for downsizing a joint structure in which dissimilar metals are joined by laser welding using the laser welding clad material 1, making it possible to manufacture a battery that can be appropriately downsized. Furthermore, by having the thickness of the Al layer 1a be 20 μm or more and 140 μm or less, it is possible to reduce the protrusion height of the protrusion 1d formed on the laser irradiated side of the Al layer 1a due to a volume change when the Al layer 1a melted by laser irradiation solidifies. As a result, as described above, this is advantageous for downsizing a joint structure in which dissimilar metals are joined by laser welding using the laser welding clad material 1, making it possible to manufacture a battery that can be appropriately downsized. The inventors of the present invention have found through experiments (Examples) described below that the above-mentioned effects can be obtained by setting the thickness of the Al layer 1 a to 20 μm or more and 140 μm or less. As a result, it is possible to downsize the joining structure involving joining dissimilar metals, and also to reduce the space required to arrange the joining structure.
[0059] [Example] An experiment (example) will be described in which the joining strength, fusion width x1, penetration depth x2, and protrusion height x3 of the protrusion 1d of the laser weld formed by laser welding as shown in FIG. 5 were measured and evaluated for a joining structure in which a test specimen, a clad material for laser welding 1, and another member made of an iron-based alloy were joined by laser welding.
[0060] First, six types of laser welding clad materials 1 (Examples 1 to 5 and Comparative Example 2) were prepared as test specimens having an Al layer 1a. Each test specimen had an overall thickness t1 of 300 μm and was composed of an Al layer 1a made of A1050 and an Fe layer 1b made of SUS430. The thicknesses t2 of the Al layer 1a varied. Furthermore, a 300 μm thick SUS430 single plate made of ferritic stainless steel (Comparative Example 1) was prepared as a test specimen without an Al layer. Furthermore, a 300 μm thick SUS430 single plate was prepared as a separate member made of an iron-based alloy. The thicknesses t2 of the Al layer 1a of the six types of laser welding clad materials 1 used as test specimens were 10 μm (Comparative Example 2), 20 μm (Example 1), 40 μm (Example 2), 60 μm (Example 3), 90 μm (Example 4), and 140 μm (Example 5).
[0061] Next, the Al layer 1a of the test specimens of Examples 1 to 5 and Comparative Example 2 was partially joined to another member by laser welding to prepare a joint structure including a dissimilar metal joint between Al050 and SUS430. Furthermore, the test specimen of Comparative Example 1 was partially joined to another member by laser welding to prepare a joint structure including a homogeneous metal joint between SUS430 and SUS430. In each joint structure, the laser was irradiated at a laser output of 300 W and a laser irradiation speed of 500 mm / s, drawing a circle with a diameter of 15 mm on the Z1-side surface of the Al layer 1a.
[0062] A test to evaluate the joining strength of the laser welded portion was conducted for the joint structures of Examples 1 to 5 and Comparative Examples 1 and 2. Specifically, a tensile test was conducted for the joint structures of Examples 1 to 5 and Comparative Examples 1 and 2, in which the test specimen and the other member were pulled in opposite directions so that a load in the shear direction was applied to the laser welded portion. In addition, the laser-welded interface (joint surface 1e) was observed with an electron microscope.
[0063] Table 1 shows the measured values (joint strength, fusion width x1, penetration depth x2, and protrusion height of protrusion 1d) of the joint structures of Examples 1 to 5 and Comparative Example 1 and Comparative Example 2 relative to the thickness t2 of the Al layer 1a. Table 2 also shows the ratios (hereinafter referred to as "comparison values") of the measured values of the joint structures of Examples 1 to 5 and Comparative Example 2 relative to the measured values of the joint structure of Comparative Example 1 (Al layer thickness: 0 μm). Furthermore, FIG. 10 shows a graph using the values listed in Table 1, plotting the thickness t2 of the Al layer 1a on the horizontal axis and the joint strength, fusion width x1, penetration depth x2, and protrusion height x3 of the laser welded portion of each joint structure on the vertical axis. The dotted line in FIG. 10 is a polynomial approximation (cubic) curve of the thickness t2 of the Al layer 1a and each measured value.
[0064]
[0065]
[0066] In the joining structure using the SUS430 single plate of Comparative Example 1 (the thickness of the Al layer was 0 μm), as shown in Table 1, the joining strength was 1999 N, the fusion width x1 was 54 μm, the penetration depth x2 was 123 μm, and the protrusion height x3 of the protrusion 1d was 30 μm.
[0067] In the welded structure using the laser welding clad material 1 of Comparative Example 2 in which the thickness t2 of the Al layer 1a was 10 μm, the joint strength was 1859 N, the fusion width x1 was 54 μm, the penetration depth x2 was 133 μm, and the protrusion height x3 of the protrusion 1d was 30 μm, as shown in Table 1. Furthermore, as shown in Table 2, the comparison values with Comparative Example 1 were the joint strength of 0.93, the fusion width x1 was 1.00, the penetration depth x2 was 1.08, and the protrusion height x3 of the protrusion 1d was 1.00.
[0068] In the welded structure using the laser welding clad material 1 of Example 1 in which the thickness t2 of the Al layer 1a was 20 μm, the joint strength was 2066 N, the fusion width x1 was 54 μm, the penetration depth x2 was 123 μm, and the protrusion height x3 of the protrusion 1d was 20 μm, as shown in Table 1. Furthermore, as shown in Table 2, the comparison values with Comparative Example 1 were the joint strength of 1.03, the fusion width x1 of 1.00, the penetration depth x2 of 1.00, and the protrusion height x3 of the protrusion 1d of 0.67.
[0069] In the welded structure using the laser welding clad material 1 of Example 2 in which the thickness t2 of the Al layer 1a was 40 μm, the joint strength was 1865 N, the fusion width x1 was 49 μm, the penetration depth x2 was 99 μm, and the protrusion height x3 of the protrusion 1d was 15 μm, as shown in Table 1. Furthermore, as shown in Table 2, the comparison values with Comparative Example 1 were the joint strength of 0.93, the fusion width x1 of 0.91, the penetration depth x2 of 0.80, and the protrusion height x3 of the protrusion 1d of 0.50.
[0070] In the welded structure using the laser welding clad material 1 of Example 3 in which the thickness t2 of the Al layer 1a was 60 μm, the joint strength was 2054 N, the fusion width x1 was 50 μm, the penetration depth x2 was 73 μm, and the protrusion height x3 of the protrusion 1d was 5 μm, as shown in Table 1. Furthermore, as shown in Table 2, the comparison values with Comparative Example 1 were the joint strength of 1.03, the fusion width x1 of 0.93, the penetration depth x2 of 0.59, and the protrusion height x3 of the protrusion 1d of 0.17.
[0071] In the welded structure using the laser welding clad material 1 of Example 4 in which the thickness t2 of the Al layer 1a was 90 μm, the joint strength was 1961 N, the fusion width x1 was 55 μm, the penetration depth x2 was 61 μm, and the protrusion height x3 of the protrusion 1d was 10 μm, as shown in Table 1. Furthermore, as shown in Table 2, the comparison values with Comparative Example 1 were the joint strength of 0.98, the fusion width x1 was 1.02, the penetration depth x2 was 0.50, and the protrusion height x3 of the protrusion 1d was 0.33.
[0072] In the welded structure using the laser welding clad material 1 of Example 5 in which the thickness t2 of the Al layer 1a was 140 μm, the joint strength was 1921 N, the fusion width x1 was 54 μm, the penetration depth x2 was 78 μm, and the protrusion height x3 of the protrusion 1d was 10 μm, as shown in Table 1. Furthermore, as shown in Table 2, the comparison values with Comparative Example 1 were the joint strength of 0.96, the fusion width x1 was 1.00, the penetration depth x2 was 0.63, and the protrusion height x3 of the protrusion 1d was 0.33.
[0073] As described above, the joint strength of the laser-welded joints of the joint structure was slightly higher when the thickness t2 of the Al layer 1a was 20 μm (Example 1) and 60 μm (Example 3) compared to Comparative Example 1, which did not have an Al layer, and slightly lower when the thickness t2 of the Al layer 1a was 10 μm (Comparative Example 2), 40 μm (Example 2), 90 μm (Example 4), and 140 μm (Example 5). This indicates that the joint strength of the laser-welded joints of the joint structure varies regardless of the thickness t2 of the Al layer 1a. This phenomenon of joint strength variability regardless of the thickness t2 of the Al layer 1a can also be confirmed by the joint strength plot and its approximation curve shown in Figure 10. Furthermore, the degree of joint strength variation is estimated to be approximately 10%, as shown in Table 2, from 0.93 (minimum) to 1.03 (maximum) for the case with the Al layer 1a, with a fluctuation range of 0.10 (-3% to +7%). From the above, it was found that the joint strength of the laser welded part of the joint structure having the Al layer 1a is substantially equivalent to that of the laser welded part of the joint structure not having the Al layer, although there is a possibility of variation of about 10%, and is at a sufficiently practical level. Therefore, it was found that the laser welding clad material 1 having the Al layer 1a is suitable for laser welding with other members made of iron-based alloys from the viewpoint of the joint strength of the laser welded part of the joint structure using it.
[0074] Furthermore, as described above, the fusion width x1 of the laser welded portion of the joint structure was equivalent to that of Comparative Example 1 without an Al layer when the thickness t2 of the Al layer 1a was 10 μm (Comparative Example 2), 20 μm (Example 1), and 140 μm (Example 5). However, it was slightly larger when the thickness t2 of the Al layer 1a was 90 μm (Example 4) and slightly smaller when the thickness t2 of the Al layer 1a was 40 μm (Example 2) and 60 μm (Example 3). This indicates that the fusion width x1 of the laser welded portion of the joint structure varies regardless of the thickness t2 of the Al layer 1a. This phenomenon of fusion width x1 varying regardless of the thickness t2 of the Al layer 1a can also be confirmed by the plot of fusion width x1 and its approximation curve shown in Figure 10. Furthermore, the degree of variation in fusion width x1 is considered to be approximately 10%, as shown in Table 2, where the comparison value for the case with the Al layer 1a ranges from 0.91 (minimum) to 1.02 (maximum), with a fluctuation range of 0.11 (-9% to +2%). From the above, it was found that the fusion width x1 of the laser weld in the joint structure having the Al layer 1a may vary by about 10%, but is at a level that is substantially equivalent to that of the laser weld in the joint structure without the Al layer and is sufficiently practical. Therefore, it was found that the laser welding clad material 1 having the Al layer 1a is suitable for laser welding with other members made of iron-based alloys from the viewpoint of the fusion width x1 of the laser weld in the joint structure using it.
[0075] Furthermore, as described above, the penetration depth x2 of the laser welded portion of the joint structure was equivalent to that of Comparative Example 1, which did not have an Al layer, when the thickness t2 of the Al layer 1a was 20 μm (Example 1), but was larger when it was 10 μm (Comparative Example 2) and smaller when it was 40 μm (Example 2) to 140 μm (Example 5). Furthermore, when comparing the values with Comparative Example 1 shown in Table 2, a tendency can be seen in which the penetration depth x2 decreases as the thickness t2 of the Al layer 1a increases from 10 μm to 90 μm. This indicates that the penetration depth x2 of the laser welded portion of the joint structure is affected by the thickness t2 of the Al layer 1a. The fact that the penetration depth x2 is affected by the thickness t2 of the Al layer 1a can also be confirmed by the plot of penetration depth x2 and its approximate curve shown in FIG. 10. From the above, it was found that the penetration depth x2 of the laser weld in a joint structure having an Al layer 1a is affected by the thickness t2 of the Al layer 1a, and is, for example, equal to or less than that of a joint structure not having an Al layer (Comparative Example 1) in joint structures in which the thickness t2 of the Al layer 1a is 20 μm or more and 140 μm or less (Examples 1 to 5), and is smaller in joint structures in which the thickness t2 of the Al layer 1a is 40 μm or more and 140 μm or less (Examples 2 to 5). Therefore, it was found that a laser welding clad material 1 in which the thickness t2 of the Al layer 1a is 20 μm or more and 140 μm or less (preferably 40 μm or more and 140 μm or less) is suitable for laser welding with other members made of an iron-based alloy, from the viewpoint of the penetration depth x2 of the laser weld in a joint structure using it.
[0076] Here, in a joining structure in which the penetration depth x2 of the laser weld is large, the molten liquid of the laser welding clad material 1 may reach and solidify near the surface opposite the welded surface of the laser-welded other component (positive terminal) to the laser-welded clad material 1. In such a case, problems such as a decrease in mechanical strength and increased susceptibility to cracking may occur, making it necessary to increase the thickness of the other component. However, in the joining structures (Examples 1 to 5) in which the thickness t2 of the Al layer 1a is 20 μm or more and 140 μm or less, the penetration depth x2 is equal to or less than that of the joining structure (Comparative Example 1) without an Al layer, eliminating the need to increase the thickness of the other component to be laser-welded. In particular, in the joining structures (Examples 2 to 5) in which the thickness t2 of the Al layer 1a is 40 μm or more and 140 μm or less, the penetration depth x2 is sufficiently smaller than that of the joining structure (Comparative Example 1) without an Al layer, allowing the thickness of the other component to be laser-welded to be further reduced. 10, the penetration depth x2 tends to increase as the thickness t2 of the Al layer 1a increases from 90 μm to 140 μm, and therefore it is considered undesirable for the thickness t2 of the Al layer 1a to exceed 140 μm. From this perspective, the laser welding clad material 1 in which the thickness t2 of the Al layer 1a is 140 μm or less is not excessively thick and can be placed in a smaller space, allowing for downsizing of the joining structure using this.
[0077] Furthermore, as described above, the protrusion height x3 of the protrusion 1d of the joint structure was 30 μm when the thickness t2 of the Al layer 1a was 10 μm (Comparative Example 2) compared to Comparative Example 1, which did not have an Al layer. However, it was smaller, being 20 μm or less, when the thickness t2 of the Al layer 1a was 20 μm (Example 1) to 140 μm (Example 5). Furthermore, when comparing the values with Comparative Example 1 shown in Table 2, it can be seen that the protrusion height x3 tends to decrease as the thickness t2 of the Al layer 1a increases from 10 μm to 140 μm. This indicates that the protrusion height x3 of the protrusion 1d of the joint structure is affected by the thickness t2 of the Al layer 1a. The fact that the protrusion height x3 is affected by the thickness t2 of the Al layer 1a can also be confirmed by the plot of the protrusion height x3 and its approximate curve shown in FIG. 10. From the above, it was found that the protrusion height x3 of the protrusion 1d of the joint structure having the Al layer 1a is affected by the thickness t2 of the Al layer 1a, and that, for example, in the joint structures (Examples 1 to 5) in which the thickness t2 of the Al layer 1a is 20 μm or more and 140 μm or less, it can be made smaller, at 20 μm or less, than in the joint structure (Comparative Example 1) that does not have an Al layer, and that in the joint structures (Examples 2 to 5) in which the thickness t2 of the Al layer 1a is 40 μm or more and 140 μm or less, it can be made even smaller, at 15 μm or less. Therefore, it was found that the laser welding clad material 1 in which the thickness t2 of the Al layer 1a is 20 μm or more and 140 μm or less (preferably 40 μm or more and 140 μm or less) is suitable for laser welding with other members made of an iron-based alloy, from the viewpoint of the protrusion height x3 of the protrusion 1d of the laser weld in the joint structure using it.
[0078] Here, when the protrusion height x3 of the protrusion 1 d of the joining structure using the laser welding clad material 1 is small, the thickness is not excessively large, making it possible to reduce the space required for placement, and the protrusion 1 d is less likely to come into contact with members other than the laser welding clad material and be damaged, thereby reducing the risk of the joining structure and the battery pack becoming unstable due to damage to the protrusion 1 d. From this perspective, a laser welding clad material 1 in which the thickness t2 of the Al layer 1 a that results in the protrusion height x3 of the protrusion 1 d of the joining structure being 20 μm or less and the thickness t2 of the Al layer 1 a that results in the protrusion height x3 of the protrusion 1 d being 20 μm or less, preferably 40 μm or more and the thickness t2 of the Al layer 1 a that results in the protrusion height x3 of the protrusion 1 d being 15 μm or less, is suitable for laser welding with other members made of an iron-based alloy and is also advantageous for downsizing joining structures using this.
[0079] From the above, based on the evaluation results of the joining strength of the laser weld, the fusion width x1, the penetration depth x2, and the protrusion height x3 of the protrusion 1d of the joining structure in which the clad material for laser welding 1 and another member are joined by laser welding, the inventors of the present application have found that the clad material for laser welding 1 in which the thickness t2 of the Al layer 1a is 20 μm or more and 140 μm or less can be placed in a small space, is suitable for laser welding involving joining of dissimilar metals with another member made of an iron-based alloy, and that it is possible to downsize the joining structure using the clad material for laser welding.
[0080] [Modifications] The embodiments and examples disclosed herein should be considered to be illustrative in all respects and not restrictive. The scope of the present invention is indicated by the claims, not by the description of the embodiments and examples above, and further includes all modifications (modifications) within the meaning and scope equivalent to the claims.
[0081] For example, in the present embodiment, a configuration example in which the clad material for laser welding 1 is used in the assembled battery 100 has been shown, but the present invention is not limited to this. In the present invention, for example, the clad material for laser welding 1 may be used in other applications than the assembled battery 100, such as in electrical and electronic circuit boards for automotive applications.
[0082] In addition, in the present embodiment, a configuration example has been shown in which the clad material 1 for laser welding is joined to the bus bar 20 by wire bonding, but the present invention is not limited to this. In the present invention, the clad material 1 for laser welding may be used in a configuration in which it is joined to the bus bar 20 by laser welding, for example.
[0083] In the present embodiment, the clad material 1 for laser welding has a configuration in which the thickness t2 of the Al layer 1a is smaller than the thickness t3 of the Fe layer 1b as shown in Fig. 2, but the present invention is not limited to this. In the clad material 1 for laser welding, the thickness t2 of the Al layer 1a may be equal to or larger than the thickness t3 of the Fe layer 1b, for example.
[0084] In addition, in the present embodiment, a configuration example in which the clad material for laser welding 1 is used in the cylindrical lithium ion secondary battery 10 shown in Fig. 6 has been shown, but the present invention is not limited to this. In the present invention, the clad material for laser welding 1 may be used in a prismatic lithium ion secondary battery 10 as shown in Fig. 11.
[0085] In addition, in the present embodiment, an example of a configuration in which the Fe layer 1b of the laser-welded clad material 1 is laser-welded to the lid member 12 (battery terminal member) made of an iron-based alloy, which is the positive electrode terminal, has been shown, but the present invention is not limited to this. In the present invention, the Fe layer 1b of the laser-welded clad material 1 may be laser-welded to a housing that also serves as the negative electrode terminal, for example.
[0086] In addition, in the present embodiment, a configuration example has been shown in which the Fe layer 1b of the laser welding clad material 1 is directly laser welded to the lid member 12 (battery terminal member), but the present invention is not limited to this. In the present invention, another component may be provided between the Fe layer 1b of the laser welding clad material 1 and the lid member 12. In this case, the other component provided between the Fe layer 1b of the laser welding clad material 1 and the lid member 12 becomes the battery terminal member.
[0087] REFERENCE SIGNS LIST 1 Laser welding clad material 1a Al layer 1b Fe layer 1c Exposed surface 1d Protruding portion 1e Joint surface 12 Lid material (other member, battery terminal member) 20 Bus bar 50a Al plate material 50b Fe plate material 100 Assembled battery (battery)
Claims
1. A clad material for laser welding (1) to be laser welded to another member made of an iron-based alloy, comprising: an Al layer (1a) made of pure aluminum or an aluminum alloy; and an Fe layer (1b) made of an iron-based alloy and roll-bonded to the Al layer, the thickness of the Al layer being 20 μm or more and 140 μm or less; and the Fe layer being laser welded to the other member by laser irradiation from the Al layer side.
2. The clad material for laser welding according to claim 1, wherein the thickness of the Al layer is 40 μm or more and 140 μm or less.
3. A joining structure using a clad material for laser welding, comprising: an Al layer (1a) made of pure aluminum or an aluminum alloy; an Fe layer (1b) made of an iron-based alloy and roll-joined to the Al layer, the Al layer having a thickness of 20 μm to 140 μm; and another member made of an iron-based alloy and laser-welded to the Fe layer, wherein the Fe layer is laser-welded to the other member by laser irradiation from the Al layer side.
4. A joint structure using the clad material for laser welding described in claim 3, wherein the length of the molten portion formed on the joint surface by laser welding between the Fe layer and the other component in the direction of extension of the joint surface is 40 μm or more and 140 μm or less.
5. A joining structure using the clad material for laser welding described in claim 3, wherein the height of a protrusion formed on the exposed surface of the Al layer opposite the surface to which the Fe layer is roll-joined by laser irradiation from the Al layer side is 20 μm or less.
6. A joining structure using a clad material for laser welding as described in claim 5, wherein the thickness of the Al layer is 40 μm or more and 140 μm or less, and a protrusion height formed on an exposed surface of the Al layer opposite to a surface where the Fe layer is roll-joined by irradiating a laser from the Al layer side to the Fe layer side is 15 μm or less.
7. A method for manufacturing a battery (100), comprising the steps of: preparing a clad material (1) for laser welding by roll-bonding an Al plate material (50a) made of pure aluminum or an aluminum alloy and an Fe plate material (50b) made of an iron-based alloy, the clad material (1) being composed of an Al layer (1a) and an Fe layer (1b), the Al layer having a thickness of 20 μm or more and 140 μm or less; bonding a battery terminal member (12) made of an iron-based alloy to the Fe layer by irradiating a laser from the Al layer side toward the Fe layer side; and bonding a bus bar (20) made of pure aluminum or an aluminum alloy to the Al layer.
Citation Information
Patent Citations
Clad insert material suitable for resistance welding of surface treated steel sheet and a1 sheet
JP1995155964A
Battery pack
JP2008066001A
Method for joining steel material with aluminum material
JP1992081288A
Joined clad plate and its manufacture