Substrate processing apparatus and substrate processing method
The substrate processing apparatus and method address the issue of uneven etching interfaces by forming a stable liquid film and sequentially applying etching liquids, ensuring a uniform etching interface on semiconductor wafers.
Patent Information
- Application Number
- PCT/JP2024/017586
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-25
- Filing Date
- 2024-05-13
- Publication Date
- 2024-11-28
AI Technical Summary
Existing substrate processing methods often result in uneven and jagged etching interfaces due to high etching rates, which are difficult to correct, especially when removing natural oxide films from semiconductor wafers using chemical solutions like hydrofluoric acid.
A substrate processing apparatus and method that involves a substrate rotation unit and a processing liquid supply unit, controlled by a control unit to form a stable liquid film on the substrate's peripheral edge before applying an etching treatment liquid, using a combination of DIW and chemical solutions in specific etching modes to ensure a uniform etching interface.
The method effectively suppresses non-uniformity in the etching interface, achieving a more regular and stable shape by controlling the etching process through sequential supply of processing liquids, thereby improving the uniformity of the etched surface.
Smart Images

Figure JP2024017586_28112024_PF_FP_ABST
Abstract
Description
Substrate processing apparatus and substrate processing method
[0001] The present disclosure relates to a substrate processing apparatus and a substrate processing method.
[0002] 2. Description of the Related Art There is known an apparatus for removing a native oxide film formed on the peripheral edge of a substrate such as a semiconductor wafer by using a chemical solution such as hydrofluoric acid (see Patent Document 1).
[0003] Patent No. 6971699
[0004] When removing the oxide film from the peripheral edge of a substrate, the etching interface can become uneven and jagged. Once a jagged etching interface has formed on the peripheral edge of the substrate, it is not easy to eliminate it through subsequent processing.
[0005] The present disclosure provides advantageous techniques for obtaining a uniform etching interface during etching of a substrate.
[0006] One aspect of the present disclosure relates to a substrate processing apparatus including a substrate rotation unit that holds and rotates a substrate, a processing liquid supply unit that supplies a processing liquid to a peripheral portion of the substrate, and a control unit that controls the substrate rotation unit and the processing liquid supply unit, wherein the control unit controls the substrate rotation unit and the processing liquid supply unit in an adjusted etching mode in which, while rotating the substrate, a liquid film forming processing liquid is supplied from the processing liquid supply unit to the peripheral portion to form a liquid film in an etching region of the peripheral portion, and then, while the liquid film is formed, an etching processing liquid is supplied to the etching region to etch the surface film of the etching region.
[0007] The present disclosure is advantageous in obtaining a uniform etching interface by etching a substrate.
[0008] FIG. 1 is a schematic diagram of an example of a substrate processing system. FIG. 2 is a partial cross-sectional view showing an example of a processing unit. FIG. 3 is a schematic diagram showing an example of a drive system for moving a first processing liquid nozzle, a second processing liquid nozzle, and a third processing liquid nozzle. FIG. 4 is a block diagram showing an example of the functional configuration of a control unit. FIG. 5 is a cross-sectional view for explaining an example of an etching process on a peripheral portion of a substrate. FIG. 6 is an enlarged plan view of the peripheral portion of a substrate, showing an example of a state immediately after a processing liquid nozzle discharging a processing liquid moves from a retracted position to a processing position. FIG. 7 is an enlarged plan view of the peripheral portion of a substrate, showing an example of a liquid film of a processing liquid in a state in which at least a portion of a substrate main body is exposed by etching removal of a surface film. FIG. 8 is an enlarged plan view of the peripheral portion of a substrate, showing another example of a liquid film of a processing liquid in a state in which at least a portion of a substrate main body is exposed by etching removal of a surface film. FIG. 9 is a graph showing an example of a processing sequence in a first standard etching mode. FIG. 10 is a graph showing an example of a processing sequence in a first adjustment etching mode. FIG. 11A is a diagram illustrating the concept of a processing sequence in the first adjustment etching mode. FIG. 11B is a diagram illustrating the concept of a processing sequence in the first adjustment etching mode. FIG. 11C is a diagram illustrating the concept of a processing sequence in the first adjustment etching mode. FIG. 12 is a graph illustrating an example of a processing sequence in the second adjustment etching mode. FIG. 13 is a graph illustrating an example of a processing sequence in the second standard etching mode. FIG. 14 is a graph illustrating an example of a processing sequence in the third adjustment etching mode. FIG. 15A is a diagram illustrating the concept of a processing sequence in the third adjustment etching mode. FIG. 15B is a diagram illustrating the concept of a processing sequence in the third adjustment etching mode. FIG. 15C is a diagram illustrating the concept of a processing sequence in the third adjustment etching mode. FIG. 16 is a graph illustrating an example of a processing sequence in the fourth adjustment etching mode. FIG. 17 is a graph illustrating an example of a processing sequence in the fifth adjustment etching mode. FIG. 18 is a plan view schematically illustrating an example of a substrate having an etching processing liquid (e.g., a chemical liquid) supplied to its peripheral portion from a processing liquid nozzle.Fig. 19A is an enlarged plan view of the region designated by the symbol "XIXA" in Fig. 18, particularly illustrating an example in which the peripheral portion of the substrate to which the etching treatment liquid is applied has hydrophilic surface characteristics. Fig. 19B is an enlarged plan view of the region designated by the symbol "XIXA" in Fig. 18, particularly illustrating an example in which the peripheral portion of the substrate to which the etching treatment liquid is applied has hydrophobic surface characteristics. Fig. 20 is a flowchart illustrating an example of an etching mode determination method.
[0009] Exemplary embodiments of the present disclosure will be described with reference to the drawings. The shapes and sizes of elements shown in the drawings do not necessarily correspond to the shapes and sizes of the actual objects, and the positional relationships and dimensional ratios between elements do not necessarily correspond to the positional relationships and dimensional ratios between the actual objects. Furthermore, the positional relationships and dimensional ratios between elements do not necessarily correspond between the drawings.
[0010] FIG. 1 is a schematic diagram illustrating an example of a substrate processing system 80 .
[0011] 1 includes a loading / unloading station 91 and a processing station 92. The loading / unloading station 91 includes a mounting section 81 equipped with a plurality of carriers C, and a transport section 82 provided with a first transport mechanism 83 and an exchange section 84. Each carrier C accommodates a plurality of substrates W in a horizontal position. The substrates W are typically semiconductor wafers, but are not limited to such. The processing station 92 is provided with a plurality of processing units 10 installed on both sides of a transport path 86, and a second transport mechanism 85 that reciprocates along the transport path 86.
[0012] The substrate W is taken out of the carrier C by the first transport mechanism 83 and placed on the transfer part 84, and is taken out of the transfer part 84 by the second transport mechanism 85. The substrate W is then carried into the corresponding processing unit 10 by the second transport mechanism 85, and is subjected to a predetermined process in the corresponding processing unit 10. Thereafter, the substrate W is taken out of the corresponding processing unit 10 by the second transport mechanism 85 and placed on the transfer part 84, and is then returned to the carrier C on the receiver 81 by the first transport mechanism 83. The substrate W may be returned to the carrier C after being processed in a plurality of processing units 10.
[0013] In the above-described substrate processing system 80, two or more of the processing units 10 may have the same configuration as each other or different configurations, and may perform the same process as each other or different processes as each other. Each processing unit 10 can perform various processes on the substrate W by applying various processing fluids (e.g., processing liquids such as chemical liquids, rinse liquids, and cleaning liquids) to the substrate W.
[0014] The substrate processing system 80 includes a control unit 93. The control unit 93 is configured, for example, by a computer, and includes an arithmetic processing unit and a memory unit. The memory unit of the control unit 93 stores programs and data for various processes performed in the substrate processing system 80. The arithmetic processing unit of the control unit 93 controls various mechanisms of the substrate processing system 80 to perform various processes by appropriately reading and executing the programs stored in the memory unit.
[0015] The programs and data stored in the storage unit of the control unit 93 may be recorded on a computer-readable storage medium and installed into the storage unit from the storage medium. Examples of computer-readable storage media include a hard disk (HD), a flexible disk (FD), a compact disk (CD), a magnetic optical disk (MO), and a memory card.
[0016] 1 , the mounting part 81 equipped with a plurality of carriers C functions as a substrate holding unit that holds a plurality of substrates W. Each processing unit 10 functions as a substrate processing apparatus that processes each substrate W. The transport part 82, the first transport mechanism 83, the delivery part 84, the second transport mechanism 85, and the transport path 86 function as a substrate transport unit that transports each substrate W between the substrate holding unit and the substrate processing apparatus. The control part 93 functions as a process control part that controls the substrate processing apparatus.
[0017] FIG. 2 is a partial cross-sectional view showing an outline of an example of the processing unit 10. As shown in FIG.
[0018] The processing unit 10 shown in Figure 2 is an apparatus for etching away a surface film (e.g., a native oxide film) formed on the peripheral portion of a substrate W, and is equipped with a substrate rotation unit 11 that holds and rotates the substrate W, and a processing liquid supply unit 12 that can supply a processing liquid to the substrate W (e.g., the peripheral portion Wp).
[0019] The substrate rotation unit 11 has a holding unit 31 that holds the substrate W horizontally, a rotation shaft 32 that is attached to the holding unit 31 and extends downward (vertically) from the holding unit 31, and a rotation drive unit 33 that rotates the holding unit 31 via the rotation shaft 32.
[0020] The substrate W is held by the holder 31 while being placed on the upper surface of the holder 31, and can rotate together with the holder 31. The method of holding the substrate W by the holder 31 is not limited, and the holder 31 can hold the substrate W by vacuum suction, for example.
[0021] The rotating shaft 32 is rotatably supported by a chamber 39 via a bearing 38. The rotation drive unit 33 has a pulley 34 attached to the lower end of the rotating shaft 32, a motor 35, a pulley 36 attached to the rotating shaft of the motor 35, and a drive belt 37 wound around the pulley 34 and the pulley 36. The rotation drive force of the motor 35 is transmitted to the rotating shaft 32 via the pulley 36, the drive belt 37, and the pulley 34, causing the rotating shaft 32 to rotate, and ultimately causing the holder 31 and the substrate W to rotate integrally with the rotating shaft 32.
[0022] The holder 31 is disposed in a chamber 39, and the substrate W held by the holder 31 is located within the chamber 39. The ceiling of the chamber 39 has an upper opening 40, through which gas (e.g., an inert gas such as nitrogen) from an FFU (fan filter unit) (not shown) is supplied into the chamber 39, forming a downflow within the chamber 39. The bottom of the chamber 39 has a lower opening 41, through which gas within the chamber 39 is exhausted to the outside. The side of the chamber 39 has a side opening 42, and a shutter 43 for opening and closing the side opening 42 is attached to the side of the chamber 39. The substrate W is loaded into the chamber 39 from the outside and unloaded from the chamber 39 to the outside via the side opening 42.
[0023] The processing liquid supply unit 12 may have any configuration as long as it can supply the liquid film forming processing liquid and the etching processing liquid to the peripheral portion Wp of the substrate W, as described below. The processing liquid supply unit 12 shown in FIG. 2 includes a first processing liquid supply unit 50, a second processing liquid supply unit 60, and a third processing liquid supply unit 70.
[0024] The first processing liquid supply unit 50 includes a first processing liquid nozzle 51 disposed in the chamber 39, a first processing liquid supply source 53 connected to the first processing liquid nozzle 51 via a first processing liquid supply pipe 52, and a first processing liquid valve 54 provided on the first processing liquid supply pipe 52. The first processing liquid nozzle 51 discharges the first processing liquid supplied from the first processing liquid supply source 53 via the first processing liquid supply pipe 52. The flow rate of the first processing liquid flowing through the first processing liquid supply pipe 52 is adjusted by the first processing liquid valve 54. That is, the first processing liquid valve 54 adjusts whether or not to supply the first processing liquid to the first processing liquid nozzle 51 and the amount of the first processing liquid supplied under the control of the control unit 93 (see FIG. 1 ).
[0025] Similarly, in the second processing liquid supply unit 60, a second processing liquid nozzle 61 disposed in the chamber 39 discharges the second processing liquid supplied from a second processing liquid supply source 63 via a second processing liquid supply pipe 62. A second processing liquid valve 64, under the control of the control unit 93, adjusts whether or not to supply the second processing liquid to the second processing liquid nozzle 61 and the amount of supply. In the third processing liquid supply unit 70, a third processing liquid nozzle 71 disposed in the chamber 39 discharges the third processing liquid supplied from a third processing liquid supply source 73 via a third processing liquid supply pipe 72. A third processing liquid valve 74, under the control of the control unit 93, adjusts whether or not to supply the third processing liquid to the third processing liquid nozzle 71 and the amount of supply.
[0026] Thus, the specific compositions of the first, second, and third processing liquids discharged from the first, second, and third processing liquid nozzles 51, 61, and 71 are not limited. As an example, the first processing liquid discharged from the first processing liquid nozzle 51 may be deionized water (DIW). The second processing liquid discharged from the second processing liquid nozzle 61 may be hydrofluoric acid (e.g., diluted hydrofluoric acid (DHF)). The third processing liquid discharged from the third processing liquid nozzle 71 may be SC1 (a mixture of ammonia and hydrogen peroxide).
[0027] FIG. 3 is a diagram showing a schematic configuration of an example of a drive system for moving the first processing liquid nozzle 51, the second processing liquid nozzle 61, and the third processing liquid nozzle 71.
[0028] The first processing liquid nozzle 51, the second processing liquid nozzle 61, and the third processing liquid nozzle 71 of this embodiment may have any configuration suitable for discharging the first to third processing liquids toward the peripheral edge Wp of the substrate W. In the example shown in FIG. 3 , the first processing liquid nozzle 51, the second processing liquid nozzle 61, and the third processing liquid nozzle 71 are arranged so that the first to third processing liquids are applied at a predetermined angle to the peripheral edge Wp (particularly the upper surface of the substrate W). The angles at which the first processing liquid nozzle 51, the second processing liquid nozzle 61, and the third processing liquid nozzle 71 discharge the first to third processing liquids are not limited. For example, the corresponding processing liquid may be discharged from each processing liquid nozzle 51, 61, and 71 obliquely toward the downstream side in the rotation direction of the substrate W with respect to the vertical direction. Furthermore, in a plan view, the corresponding processing liquid may be discharged from each processing liquid nozzle 51, 61, and 71 obliquely toward the downstream side in the rotation direction of the substrate W with respect to the radial direction of the substrate W (i.e., radially outward).
[0029] The first processing liquid nozzle 51, the second processing liquid nozzle 61, and the third processing liquid nozzle 71 can be positioned at processing positions P1, P2, P3 for discharging the processing liquid toward the peripheral edge Wp of the substrate W, and at retracted positions Q1, Q2, Q3 which are different from the processing positions in the radial direction of the substrate W. The processing positions P1, P2, P3 are set at positions where the processing liquid discharged from each processing liquid nozzle 51, 61, 71 is applied to a desired region (an etching region described below) on the peripheral edge Wp of the substrate W. On the other hand, the retracted positions Q1, Q2, Q3 are set at positions where even if the processing liquid is discharged from each processing liquid nozzle 51, 61, 71, the processing liquid does not reach the substrate W.
[0030] 3 , the first processing liquid nozzle 51 is moved between a processing position P1 and a retracted position Q1 by a first nozzle driving unit 55 driven under the control of the control unit 93. Similarly, the second processing liquid nozzle 61 and the third processing liquid nozzle 71 are moved between processing positions P2, P3 and retracted positions Q2, Q3 by a second nozzle driving unit 65 and a third nozzle driving unit 75 driven under the control of the control unit 93.
[0031] The processing unit 10 shown in Figure 2 further includes a heating mechanism 44 that heats the substrate W held by the holding part 31, and an imaging device 49 that images the upper surface (processing surface) of the substrate W held by the holding part 31.
[0032] The heating mechanism 44 in this example has a heating fluid supply unit 45 that discharges an inert gas (heating fluid) such as nitrogen gas heated by a heater 47, and the substrate W held by the holder 31 is heated using the inert gas discharged from the heating fluid supply unit 45. In the heating fluid supply unit 45 shown in FIG. 2, under the control of the control unit 93 (see FIG. 1), the inert gas sent from a heating fluid supply source 48 is discharged from the heating fluid jetting unit 46 toward the back surface of the substrate W. The inert gas is heated by the heater 47 while traveling from the heating fluid supply source 48 through the transport line to the heating fluid jetting unit 46. Note that the heating mechanism 44 is not limited to a configuration that heats the substrate W with a heating fluid, and the substrate W may be heated using a heater that uses another heating device, such as a lamp or laser, arranged above or below the substrate W.
[0033] The imaging device 49 performs imaging under the control of the control unit 93 (see FIG. 1 ), acquires image data (imaging data) of the upper surface (processing surface) of the substrate W, and sends the image data to the control unit 93. The installation position of the imaging device 49 is not limited to the example shown in FIG. 2 , and the imaging device 49 can be installed in any position and attitude that allows it to acquire image data of a desired location on the upper surface (particularly the peripheral edge Wp) of the substrate W.
[0034] FIG. 4 is a block diagram showing an example of the functional configuration of the control unit 93.
[0035] The control unit 93 controls each part of the processing unit 10. The components of the processing unit 10 controlled by the control unit 93 are not limited, and the control target and the control content are determined depending on the processing content.
[0036] 4, the control unit 93 of this embodiment controls the substrate rotation unit 11, the processing liquid supply unit 12, the heating mechanism 44, and the imaging device 49 in order to remove a native oxide film formed on the peripheral edge Wp of the substrate W. Specific control contents by the control unit 93 will be described later.
[0037] [Etching Method (Substrate Processing Method)] As described above, when the surface film of the peripheral edge portion Wp of the substrate W is removed by etching, the etching interface may become uneven and jagged.
[0038] As a result of extensive research and trial and error into such non-uniform etching interfaces, the present inventors have come to the knowledge that the higher the etching rate, the more non-uniform the etching interface tends to become.
[0039] FIG. 5 is a cross-sectional view for explaining an outline of an example of etching processing on the peripheral edge portion Wp of the substrate W. In FIG.
[0040] In general, a surface film Ws covering the surface of a substrate body Wb such as silicon (Si) is etched away by a processing liquid L discharged from a processing liquid nozzle N (corresponding to the processing liquid nozzles 51, 61, and 71 shown in FIGS. 2 and 3 ). In the example shown in FIG. 5 , the processing liquid L is discharged from the processing liquid nozzle N particularly toward the peripheral edge Wp of the substrate W, and the surface film Ws is etched away from the peripheral edge Wp.
[0041] Fig. 6 is an enlarged plan view of the peripheral edge Wp of the substrate W, showing an example of a state immediately after the processing liquid nozzle N discharging the processing liquid L has moved from the retracted position Q (corresponding to the retracted positions Q1 to Q3 shown in Fig. 3) to the processing position P (corresponding to the processing positions P1 to P3 shown in Fig. 3). Fig. 7 is an enlarged plan view of the peripheral edge Wp of the substrate W, showing an example of a liquid film of the processing liquid L in a state in which at least a portion of the substrate main body Wb has been exposed by etching away the surface film Ws. Fig. 8 is an enlarged plan view of the peripheral edge Wp of the substrate W, showing another example of a liquid film of the processing liquid L in a state in which at least a portion of the substrate main body Wb has been exposed by etching away the surface film Ws.
[0042] The processing liquid L (particularly the etching processing liquid) discharged from the processing liquid nozzle N located at the processing position P lands on the peripheral edge Wp of the rotating substrate W and spreads to form a liquid film over the etching region R of the peripheral edge Wp. This liquid film of the processing liquid L gradually etches away the surface film Ws in the etching region R, gradually exposing the substrate main body Wb.
[0043] Therefore, for example, when a hydrophobic substrate main body portion Wb is covered with a hydrophilic surface film Ws, the etching region R changes from an entirely hydrophilic state, through a mixed hydrophilic and hydrophobic state, and finally reaches an entirely hydrophobic state as etching progresses. On the other hand, when a hydrophilic substrate main body portion Wb is covered with a hydrophobic surface film Ws, the etching region R changes from an entirely hydrophobic state, through a mixed hydrophobic and hydrophilic state, and finally reaches an entirely hydrophilic state as etching progresses.
[0044] In this way, when the substrate main body Wb and the surface film Ws have different "affinities for water (hydrophilic / hydrophobic)", there is a state in which both hydrophobic and hydrophilic regions are present in the peripheral portion Wp of the substrate W during the etching removal process of the surface film Ws.
[0045] On the other hand, immediately after the processing liquid nozzle N moves from the retracted position Q to the processing position P, the state of the liquid film of the processing liquid L on the etching region R is unstable, and the contour of the liquid film (particularly the interface (gas-liquid interface) B on the substrate center side) may have an irregular jagged shape, as shown in Fig. 6. Thereafter, with the passage of time, the shape of the liquid film of the processing liquid L discharged from the processing liquid nozzle N on the etching region R gradually stabilizes, and ideally the contour of the liquid film (particularly the interface B on the substrate center side) will have a regular shape (see Fig. 7).
[0046] However, in reality, the shape of the liquid film of the processing liquid L on the etching region R may not stabilize over time, and the contour of the liquid film (particularly the interface B on the center side of the substrate) may continue to maintain an irregular jagged shape (see FIG. 8). In this case, the shape of the etching interface may eventually become uneven and jagged.
[0047] As a result of further trial and error, the present inventors have come to the knowledge that the etching interface is likely to become uneven and jagged when both hydrophilic and hydrophobic surfaces are exposed in the etching region R while the liquid film shape of the processing liquid L on the etching region R is not sufficiently stabilized. In other words, it has been found that when both hydrophilic and hydrophobic surfaces are exposed in the etching region R while the outline of the liquid film of the processing liquid L on the etching region R (particularly the interface B on the substrate center side) is irregular, the outline of the liquid film tends to continue to maintain an irregular shape.
[0048] More specifically, if the substrate main body Wb is exposed by etching away the surface film Ws before the outline of the liquid film (interface B) of the processing liquid L on the etching region R reaches a state in which it has the desired regular shape, the shape of the etching interface tends to become uneven and jagged. This is thought to be because the liquid film remains in an unstable state, and both areas where the liquid is likely to exist (hydrophilic surfaces) and areas where it is unlikely to exist (hydrophobic surfaces) are generated in the etching region R, preventing the stabilization of the liquid film shape, and the unstable state of the liquid film shape is maintained during the etching process.
[0049] Based on these findings, the present inventors have newly discovered that performing an etching process in the following manner is advantageous in effectively avoiding an uneven shape of the etching interface and realizing an etching interface having a desired regular shape.
[0050] That is, in a state in which a liquid film forming processing liquid is supplied to the peripheral edge portion Wp of the substrate W to form a stable liquid film in the etching region R, the etching processing liquid is supplied to the etching region R to remove the surface film Ws, thereby effectively suppressing non-uniformity in the shape of the etching interface. More specifically, by forming a liquid film of the processing liquid L with a regular shape in the etching region R before the substrate main body portion Wb is exposed in the etching region R, the etching interface in the etching region R after the etching process can have a more uniform shape.
[0051] The liquid film forming treatment liquid referred to here is a treatment liquid having an etching rate for etching the surface film Ws lower than that of the etching treatment liquid, for example, an etching treatment liquid having a lower concentration of etching components for etching the surface film Ws than that of the etching treatment liquid.
[0052] Therefore, as an example, the liquid film forming treatment liquid may be a treatment liquid that does not etch the surface film Ws, and the etching rate of the surface film Ws by the liquid film forming treatment liquid may be substantially "zero (0)." As another example, the liquid film forming treatment liquid L1 may be a treatment liquid that etches the surface film Ws, or may be a mixture of a treatment liquid that etches the surface film Ws and a treatment liquid that does not etch the surface film Ws. The etching treatment liquid may be a treatment liquid that has a temperature on the substrate W that is more suitable for etching the surface film Ws (a temperature that achieves a high etching rate) than the liquid film forming treatment liquid, and may be, for example, a treatment liquid that has a higher temperature on the substrate W than the liquid film forming treatment liquid.
[0053] A more specific etching method will be described below.
[0054] In each etching mode described below, as an example, DIW supplied to the peripheral portion Wp of the substrate W by a first processing liquid supply unit 50 (see FIGS. 2 and 3) is used as a first processing liquid that does not etch the surface film Ws (e.g., an oxide film), and a chemical liquid Lc (e.g., hydrofluoric acid) supplied to the peripheral portion Wp of the substrate W by a second processing liquid supply unit 60 (see FIGS. 2 and 3) is used as a second processing liquid that etches the surface film Ws.
[0055] [First Standard Etching Mode] FIG. 9 is a graph showing an example of a processing sequence in the first standard etching mode.
[0056] The horizontal axis in Fig. 9 represents elapsed time (sec), with the left end position of the horizontal axis representing the origin ("0"). The vertical axis in Fig. 9 represents the nozzle position, with the processing position P described above being on the positive side (upper side in Fig. 9) of the origin ("0") of the vertical axis, and the retracted position Q described above being on the negative side (lower side in Fig. 9).
[0057] 9 shows a case where "DIW," which is an example of a liquid that does not substantially contribute to the etching process of the surface film Ws of the substrate W, and a "chemical liquid," which is a liquid that substantially contributes to the etching process of the surface film Ws of the substrate W, can be applied to the peripheral portion Wp of the substrate W. As an example, a case will be described in which the "DIW" shown in Fig. 9 is ejected from the "first processing liquid nozzle 51" shown in Figs. 2 and 3, and the "chemical liquid" shown in Fig. 9 is ejected from the "second processing liquid nozzle 61" shown in Figs. 2 and 3.
[0058] However, the graph relating to "DIW" and "chemical solution" shown in FIG. 9 is merely an example of a standard sequence for etching processing, and the first standard etching mode may be performed based on another sequence. Also, instead of "DIW" in FIG. 9, another processing solution whose contribution to the etching processing of the surface film Ws is lower than that of the "chemical solution" may be used. For example, if the surface film Ws is a material (e.g., aluminum oxide (AlO x ) and germanium oxide (GeO x )), a processing liquid that does not etch the material may be used instead of the DIW in Fig. 9, and the DIW may be used instead of the chemical liquid in Fig. 9. As such a processing liquid that does not etch the surface film Ws, for example, isopropyl alcohol (IPA) or acetone may be used in some cases.
[0059] Furthermore, the processing liquid nozzle N from which the "DIW" and the "chemical liquid" are ejected is not limited, and the "chemical liquid" may be ejected, for example, from the "third processing liquid nozzle 71 (third processing liquid supply unit 70)" shown in Figures 2 and 3.
[0060] 9 , in a standby process in which the processing liquids (DIW and chemical liquid) are not applied to the substrate W, the nozzles that discharge the chemical liquid and DIW (in this example, the first processing liquid nozzle 51 and the second processing liquid nozzle 61) are positioned at the retracted position Q. On the other hand, in the first standard etching mode, in an etching process in which an etching region R (particularly the surface film Ws) of the peripheral portion Wp of the substrate W is etched, the second processing liquid nozzle 61 is moved from the retracted position Q to the processing position P. Then, the chemical liquid discharged from the second processing liquid nozzle 61 positioned at the processing position P is applied to the etching region R to etch the surface film Ws of the etching region R. Note that in the etching process shown in FIG. 9 , the first processing liquid nozzle 51 is continuously positioned at the retracted position Q, and DIW is not supplied to the substrate W from the first processing liquid nozzle 51.
[0061] In the first standard etching mode of FIG. 9, depending on the processing conditions, the etching process may proceed without sufficient stabilization of the liquid film shape of the processing liquid L on the etching region R, as described above, resulting in an uneven and jagged shape of the etching interface (see FIG. 8).
[0062] [First Adjustment Etching Mode] Next, a first adjustment etching mode that is effective in promoting uniformity in the shape of the etching interface will be described.
[0063] 10 is a graph showing an example of a processing sequence in the first adjustment etching mode, in which the horizontal and vertical axes represent elapsed time (sec.) and nozzle position, respectively, similar to the horizontal and vertical axes of FIG.
[0064] 11A to 11C are diagrams illustrating the concept of the processing sequence in the first adjustment etching mode.
[0065] In the first adjustment etching mode, the supply of the etching processing liquid L2 is started to the etching region R of the peripheral portion Wp of the substrate W when a liquid film of the liquid film forming processing liquid L1 is stably formed in the desired shape, thereby etching the surface film Ws of the etching region R.
[0066] That is, the control unit 93 (see Figure 1) controls the substrate rotation unit 11 and the processing liquid supply unit 12 (see Figure 2) to sequentially perform the liquid film formation process and the etching process while rotating the substrate W supported by the holding unit 31.
[0067] In the liquid film formation process, DIW (see reference symbol "Ld" in FIGS. 11A to 11C; hereinafter also referred to as "DIWLd") is supplied from the first processing liquid nozzle 51 of the processing liquid supply unit 12 to the peripheral portion Wp of the substrate W. As a result, in the liquid film formation process, a liquid film of DIWLd (i.e., liquid film forming processing liquid L1) is formed in the etching region R of the peripheral portion Wp (see FIG. 11A).
[0068] 10 , after a standby process in which the first processing liquid nozzle 51 and the second processing liquid nozzle 61 are positioned at the retracted position Q, the first processing liquid nozzle 51 that discharges DIWLd moves to the processing position P, whereby the DIWLd that serves as the liquid film forming processing liquid L1 is supplied to the peripheral edge portion Wp. In this manner, the liquid film forming process is performed by supplying DIWLd from the first processing liquid supply unit 50 to the etching region R while stopping the supply of the chemical liquid Lc from the second processing liquid supply unit 60 to the etching region R.
[0069] In the subsequent etching process, the chemical liquid Lc is supplied to the peripheral portion Wp of the substrate W from the second processing liquid nozzle 61 of the processing liquid supply unit 12 (see Figure 11B), and a liquid film of the chemical liquid Lc (i.e., the etching processing liquid L2) is formed in the etching region R of the peripheral portion Wp (see Figure 11C).
[0070] Specifically, with the first processing liquid nozzle 51 that discharges the DIWLd positioned at the processing position P, the second processing liquid nozzle 61 is moved from the retracted position Q to the processing position P. Thereafter, with the second processing liquid nozzle 61 that discharges the chemical liquid Lc positioned at the processing position P, the first processing liquid nozzle 51 is moved from the processing position P to the retracted position Q.
[0071] Therefore, while the first processing liquid supply unit 50 continues to supply the DIWLd to the etching region R, the second processing liquid supply unit 60 starts to supply the chemical liquid Lc to the etching region R. In this manner, the supply of the chemical liquid Lc (etching processing liquid L2) is started to the etching region R of the peripheral portion Wp of the substrate W in a state where a liquid film of DIWLd (liquid film forming processing liquid L1) is formed.
[0072] Thereafter, the supply of DIWLd from the first processing liquid supply unit 50 to the etching region R is stopped, while the supply of the chemical liquid Lc from the second processing liquid supply unit 60 to the etching region R is continued. As a result, the supply of DIWLd (liquid film forming processing liquid L1) is stopped while the chemical liquid Lc (etching processing liquid L2) is being supplied to the etching region R of the peripheral portion Wp of the substrate W.
[0073] After the surface film Ws in the etching region R of the substrate W is removed, the second processing liquid nozzle 61 is moved from the processing position P to the retracted position Q, the supply of the chemical liquid Lc to the peripheral portion Wp is stopped, and the etching process is terminated.
[0074] By starting and carrying out the etching process according to the above-described series of sequences, it is possible to suppress the disturbance of the shape of the liquid film in the etching region R while changing the constituent components of the liquid film from DIWLd (liquid film forming treatment liquid L1) to chemical liquid Lc (etching treatment liquid L2).
[0075] The surface film Ws in the etching region R is then etched by the liquid film of the chemical liquid Lc formed in this manner. In particular, in this adjustment etching mode, the processing liquid supplied to the etching region R is changed from DIWLd (liquid film forming processing liquid L1) to the chemical liquid Lc (etching processing liquid L2) while the surface film Ws is maintained in the etching region R and the substrate main body portion Wb is not exposed. Therefore, the processing liquid supplied to the etching region R can be changed from DIWLd to the chemical liquid Lc while the affinity (hydrophilicity / hydrophobicity) of the etching region R to water is uniform overall. As a result, the chemical liquid Lc can be supplied to the etching region R without excessively disturbing the state of the liquid film formed in the liquid film formation process.
[0076] As described above, according to this adjustment etching mode, the etching process can be started and carried out in a state where the liquid film of the liquid film forming processing liquid L1 (particularly the interface B on the substrate center side) stably maintains a regular shape in the etching region R. This effectively prevents the shape of the etching interface from becoming uneven and jagged, and makes it possible to realize an etching interface having a contour with a regular shape closer to the ideal state.
[0077] [Second Adjustment Etching Mode] Next, a second adjustment etching mode that is effective in promoting uniformity in the shape of the etching interface will be described.
[0078] 12 is a graph showing an example of a processing sequence in the second adjustment etching mode, in which the horizontal and vertical axes represent elapsed time (sec.) and nozzle position, respectively, similar to the horizontal and vertical axes of FIG.
[0079] In the second adjustment etching mode, DIWLd and the chemical liquid Lc are supplied to the peripheral edge Wp of the substrate W, thereby forming a liquid film of the liquid film forming treatment liquid L1 in the etching region R of the peripheral edge Wp. That is, in this adjustment etching mode, the liquid film forming treatment liquid L1 contains DIWLd and the chemical liquid Lc. On the other hand, by continuing to supply the chemical liquid Lc to the peripheral edge Wp while stopping the supply of DIWLd, the etching treatment liquid L2 is applied to the etching region R.
[0080] In the second adjustment etching mode, the control unit 93 (see Figure 1) controls the substrate rotation unit 11 and the processing liquid supply unit 12 (see Figure 2) to rotate the substrate W supported by the holding unit 31 while performing the liquid film formation process and etching process as follows.
[0081] That is, the liquid film forming process is performed by supplying DIWLd to the peripheral edge Wp of the substrate W from the first processing liquid nozzle 51 of the processing liquid supply unit 12, and supplying the chemical liquid Lc to the peripheral edge Wp from the second processing liquid nozzle 61.
[0082] 12 , the supply of DIWLd to the peripheral edge Wp is started first, followed by the supply of the chemical liquid Lc to the peripheral edge Wp. That is, the supply of the chemical liquid Lc to the etching region R from the second processing liquid supply unit 60 is stopped, while the DIWLd is supplied to the etching region R from the first processing liquid supply unit 50. Thereafter, while the supply of DIWLd to the etching region R from the first processing liquid supply unit 50 continues, the chemical liquid Lc is supplied to the etching region R from the second processing liquid supply unit 60, and a liquid film of the liquid film forming processing liquid L1 is formed in the etching region R.
[0083] In this manner, in the liquid film forming process, the concentration of the chemical liquid Lc is diluted by the DIWLd, so that the chemical liquid Lc supplied to the peripheral portion Wp can effectively prevent the etching of the surface film Ws in the etching region R from progressing and exposing the substrate main body portion Wb.
[0084] The timings at which the supply of DIWLd and the supply of the chemical liquid Lc in the liquid film formation process are not limited to the example shown in Fig. 12. That is, in the liquid film formation process, as long as the shape of the liquid film of the liquid film forming treatment liquid L1 can be stably formed in the etching region R before the substrate main body portion Wb is exposed, the DIWLd and the chemical liquid Lc can be supplied to the substrate W at any timing. Therefore, the timing at which the supply of the chemical liquid Lc to the peripheral portion Wp starts may be immediately after the timing at which the supply of DIWLd to the peripheral portion Wp starts, or may be simultaneous with the timing at which the supply of DIWLd to the peripheral portion Wp starts.
[0085] Thereafter, in a state in which the liquid film of the liquid film forming processing liquid L1 has been formed in a stable shape on the etching region R as described above, the liquid film formation processing is terminated, while the etching processing is continued. That is, the supply of the DIWLd from the first processing liquid supply unit 50 to the etching region R is stopped, while the supply of the chemical liquid Lc from the second processing liquid supply unit 60 to the etching region R is continued. More specifically, the first processing liquid nozzle 51 that discharges the DIWLd is moved from the processing position P to the retracted position Q, while the second processing liquid nozzle 61 that discharges the chemical liquid Lc remains positioned at the processing position P.
[0086] After the surface film Ws in the etching region R of the substrate W is removed, the second processing liquid nozzle 61 is moved from the processing position P to the retracted position Q, the supply of the chemical liquid Lc to the peripheral portion Wp is stopped, and the etching process is terminated.
[0087] By carrying out the above-described series of processing sequences, the constituent components of the liquid film can be changed from the liquid film forming processing liquid L1 (a mixture of DIWLd and chemical liquid Lc) to the etching processing liquid L2 (chemical liquid Lc) while suppressing the disturbance of the shape of the liquid film in the etching region R.
[0088] In this manner, the adjustment etching mode controls the concentration of the etching component that etches the surface film Ws of the substrate W, thereby preventing the substrate main body portion Wb from being exposed before a liquid film with a stable shape is formed in the etching region R. As a result, even in the adjustment etching mode, the etching process can be performed in a state in which the shape of the liquid film of the liquid film forming processing liquid L1 (particularly the outline of the interface B toward the center of the substrate) in the etching region R is stably maintained as a regular shape. In particular, in the adjustment etching mode, the etching process for etching away the surface film Ws is performed not only after the liquid film formation process but also during the liquid film formation process. Therefore, according to the adjustment etching mode, the overall time from the start of the liquid film formation process to the end of the etching process can be shortened compared to the first adjustment etching mode described above.
[0089] [Second Standard Etching Mode] FIG. 13 is a graph showing an example of a processing sequence in the second standard etching mode.
[0090] The horizontal axis of Fig. 13 represents elapsed time (sec.). The vertical axis on the left side of Fig. 13 represents the chemical liquid flow rate [ml / min.], which is the discharge flow rate of the chemical liquid Lc from the processing liquid nozzle N (second processing liquid nozzle 61 in this example). The vertical axis on the right side of Fig. 13 represents the flow rate (heating fluid flow rate [L / min. (minute)]) of the "inert gas discharged from the heating fluid discharge part 46 (see Fig. 2) of the heating fluid supply part 45," which is the heating fluid used to heat the substrate W supported by the substrate rotation part 11.
[0091] In the second standard etching mode shown in FIG. 13, etching processing is started in a state where the temperature of the substrate W (particularly the peripheral edge portion Wp) is adjusted to a temperature suitable for etching the surface film Ws of the substrate W.
[0092] That is, prior to the etching process in which the chemical liquid Lc is supplied to the substrate W, a preheating process is performed in which an inert gas (heating fluid) is supplied to the substrate W to raise the temperature of the substrate W (particularly the peripheral portion Wp).
[0093] 13 , a first preheating process is performed in which a relatively small flow rate of inert gas is sprayed onto the substrate W from the heating fluid supply unit 45, followed by a second preheating process in which a relatively large flow rate of inert gas is sprayed onto the substrate W from the heating fluid supply unit 45. The second preheating process increases the temperature of the substrate W to a greater extent per unit time than the first preheating process. Note that the first preheating process may gradually increase the temperature of the substrate W over time, but the temperature of the substrate W does not necessarily have to increase gradually. For example, the temperature of the substrate W may be approximately constant during at least a portion of the first preheating process (e.g., the entire period).
[0094] After the substrate W has been sufficiently heated by the preheating process (particularly the second preheating process), the chemical liquid Lc is supplied to the substrate W to perform the etching process of the surface film Ws. By starting the etching process in this state in which the etching rate of the surface film Ws by the chemical liquid Lc has been increased by the preheating process, an efficient etching process can be achieved. In the example shown in Fig. 13, the second processing liquid nozzle 61 is positioned at the retracted position Q during the "first preheating process" and the "second preheating process", and is positioned at the processing position P2 during the "etching process".
[0095] In the example shown in FIG. 13, even after the start of the etching process, the inert gas is sprayed onto the substrate W at the same flow rate as in the second preheating process, and a heating process for heating the substrate W is carried out simultaneously with the etching process.
[0096] According to the above-described present standard etching mode, the time required for exposing the substrate main body portion Wb is also relatively short, since the etching process of the surface film Ws of the substrate W progresses efficiently immediately after the start of the supply of the chemical liquid Lc to the substrate W. Therefore, even in the present standard etching mode, as in the above-described first standard etching mode (see FIG. 9 ), the substrate main body portion Wb may be exposed in a state in which the shape of the liquid film of the chemical liquid Lc on the etching region R is not sufficiently stable, and the shape of the etching interface may become uneven and jagged.
[0097] The third adjustment etching mode described below is effective in suppressing the non-uniformity of the shape of the etching interface caused by the second standard etching mode.
[0098] [Third Adjustment Etching Mode] Next, a third adjustment etching mode that is effective in promoting uniformity in the shape of the etching interface will be described.
[0099] Fig. 14 is a graph showing an example of a processing sequence in the third adjustment etching mode. The horizontal axis, left vertical axis, and right vertical axis of Fig. 14 respectively represent elapsed time (sec.), chemical flow rate [ml / min.], and heating fluid flow rate [L / min.], similar to the horizontal axis, left vertical axis, and right vertical axis of Fig. 13 described above.
[0100] 15A to 15C are diagrams illustrating the concept of the processing sequence in the third adjustment etching mode.
[0101] In the third adjustment etching mode, the temperature of the substrate W (particularly the etching region R of the peripheral edge Wp) is adjusted to control the progress of the etching process, thereby preventing the etching interface from becoming non-uniform.
[0102] That is, the control unit 93 (see Figure 1) controls the substrate rotation unit 11, the processing liquid supply unit 12, and the heating fluid supply unit 45 (heating mechanism 44; see Figure 2), and performs each process as follows while rotating the substrate W supported by the holder 31.
[0103] During the preheating process, while no chemical liquid Lc is supplied to the substrate W from the second processing liquid nozzle 61, a relatively small flow rate of inert gas (heating fluid) is sprayed onto the back surface of the substrate W from the heating fluid ejection portion 46 of the heating fluid supply unit 45 (see Figure 15A).
[0104] Then, while inert gas is being sprayed onto the rear surface of the substrate W from the heating fluid ejection section 46, a chemical liquid Lc is supplied from the second processing liquid nozzle 61 to the peripheral portion Wp of the substrate W, and etching processing and heating processing are performed simultaneously.
[0105] In particular, the substrate W is heated by the heating fluid supply unit 45 with a first heat quantity from the time the substrate W is held by the substrate rotation unit 11 until a liquid film of the chemical liquid Lc (a liquid film having a particularly stable shape) is formed in the etching region R (see FIG. 15B ). After the liquid film of the chemical liquid Lc (a liquid film having a particularly stable shape) is formed in the etching region R, the substrate W is heated by the heating fluid supply unit 45 with a second heat quantity greater than the first heat quantity while the chemical liquid Lc is being supplied to the etching region R (see FIG. 15C ). More specifically, the control unit 93 controls the heating fluid supply unit 45 so that the flow rate of the inert gas discharged from the heating fluid supply unit 45 is greater while the substrate W is heated with the second heat quantity than while the substrate W is heated with the first heat quantity (see FIGS. 15B and 15C ).
[0106] Therefore, from the start of supply of the chemical liquid Lc to the substrate W until the shape of the liquid film of the chemical liquid Lc formed in the etching region R (particularly the outline of the interface B on the substrate center side) stabilizes, etching of the surface film Ws proceeds at a relatively low etching rate. After the shape of the liquid film of the chemical liquid Lc formed in the etching region R stabilizes, etching of the surface film Ws proceeds at a relatively high etching rate.
[0107] As a result, etching of the surface film Ws is performed so as not to expose the substrate main body portion Wb until the shape of the liquid film of the chemical liquid Lc formed in the etching region R is stabilized, thereby effectively preventing the liquid film stabilization from being hindered due to partial exposure of the substrate main body portion Wb. After the shape of the liquid film of the chemical liquid Lc formed in the etching region R is stabilized, etching of the surface film Ws can be performed efficiently.
[0108] In the adjustment etching mode thus performed, the chemical liquid Lc supplied to the substrate W until the shape of the liquid film of the chemical liquid Lc formed in the etching region R becomes stable acts as the liquid film forming treatment liquid described above. On the other hand, the chemical liquid Lc supplied to the substrate W after the shape of the liquid film of the chemical liquid Lc formed in the etching region R becomes stable acts as the etching treatment liquid described above.
[0109] The preheating process and / or the heating process using an inert gas (heating fluid) may be combined with other adjusted etching modes (see the first and second adjusted etching modes described above) that adjust the timing of starting and stopping the supply of the chemical liquids Lc and DIWLd to the substrate W. Examples of adjusted etching modes related to such combinations are described below.
[0110] [Fourth Adjustment Etching Mode] Next, a fourth adjustment etching mode that is effective in promoting uniformity in the shape of the etching interface will be described.
[0111] 16 is a graph showing an example of a processing sequence in the fourth adjustment etching mode, in which the horizontal axis represents elapsed time (sec.), the left vertical axis represents the flow rates of the chemical solutions Lc and DIWLd (ml / min.), and the right vertical axis represents the heating fluid flow rate (L / min.).
[0112] This adjustment etching mode is based on a combination of the first adjustment etching mode (see Figure 10), in which the etching process is started after the liquid film formation process, and the adjustment etching mode (see Figure 14), in which the substrate W is heated by an inert gas (heating fluid).
[0113] That is, in this adjustment etching mode shown in Figure 16, similar to the first adjustment etching mode described above, after a liquid film formation process using DIWLd from the first processing liquid nozzle 51, an etching process using chemical liquid Lc from the second processing liquid nozzle 61 is performed.
[0114] On the other hand, prior to the liquid film formation process, an inert gas (heating fluid) is sprayed from the heating fluid jetting unit 46 of the heating fluid supply unit 45 onto the rear surface of the substrate W to raise the temperature of the substrate W. In the example shown in Fig. 16, a substantially constant flow rate of inert gas is ejected from the heating fluid jetting unit 46 throughout almost the entire process and sprayed onto the substrate W. The process in which the temperature of the substrate W is raised by an inert gas is classified as a preheating process before the start of the etching process (e.g., during the liquid film formation process), and is classified as a heating process after the start of the etching process.
[0115] In this adjustment etching mode, before the start of the etching process, the chemical liquid Lc that contributes to etching the surface film Ws is not supplied to the substrate W, so there is basically no need to suppress heating of the substrate W to increase the etching rate. Therefore, in this adjustment etching mode, unlike the above-mentioned third adjustment etching mode (see FIG. 14 ), the substrate W can be heated by the inert gas even before the etching process to the same extent as during the etching process, and a more efficient etching process can be achieved.
[0116] [Fifth Adjustment Etching Mode] Next, a fifth adjustment etching mode that is effective in promoting uniformity in the shape of the etching interface will be described.
[0117] 17 is a graph showing an example of a processing sequence in the fifth adjustment etching mode, in which the horizontal axis, left vertical axis, and right vertical axis represent elapsed time (sec.), flow rates of the chemical solutions Lc and DIWLd (ml / min.), and heating fluid flow rate (L / min.), respectively, as in the above-mentioned FIG.
[0118] This adjustment etching mode is based on a combination of a second adjustment etching mode (see Figure 12) in which the etching process is started during the liquid film formation process and an adjustment etching mode (see Figure 14) in which the substrate W is heated by an inert gas (heating fluid).
[0119] 17 , similarly to the second adjustment etching mode described above, both the DIWLd from the first processing liquid nozzle 51 and the chemical liquid Lc from the second processing liquid nozzle 61 are supplied to the peripheral edge Wp of the substrate W to perform the liquid film formation process. That is, both the DIWLd and the chemical liquid Lc are used as the liquid film forming processing liquid L1, and a liquid film of the DIWLd and the chemical liquid Lc (liquid film forming processing liquid L1) is stably formed in the etching region R. Note that in the example shown in FIG. 17 , unlike the example shown in FIG. 12 described above, the supply of the DIWLd and the chemical liquid Lc to the peripheral edge Wp is started simultaneously during the liquid film formation process.
[0120] Thereafter, in this adjustment etching mode, as in the above-described second adjustment etching mode, the supply of DIWLd to the etching region R is stopped and the liquid film formation process is terminated in a state in which the liquid film of the liquid film forming processing liquid L1 is stably formed in the etching region R. On the other hand, the supply of the chemical liquid Lc to the etching region R continues, and the etching process continues even after the liquid film formation process is terminated.
[0121] On the other hand, prior to the liquid film formation process and the etching process, an inert gas (heating fluid) is sprayed from the heating fluid jetting part 46 of the heating fluid supply part 45 onto the rear surface of the substrate W to raise the temperature of the substrate W. However, in this adjustment etching mode, since the surface film Ws is etched even during the liquid film formation process, the flow rate of the inert gas is suppressed until the liquid film shape of the liquid film forming processing liquid L1 on the etching region R is stabilized, as in the above-mentioned third adjustment etching mode (see FIG. 14 ).
[0122] That is, until the shape of the liquid film of the liquid film forming processing liquid L1 formed in the etching region R of the substrate W becomes stable (i.e., until the liquid film formation process is completed), a relatively small flow rate of inert gas is supplied to the substrate W from the heating fluid jetting part 46, thereby suppressing an increase in the etching rate. After the shape of the liquid film of the liquid film forming processing liquid L1 formed in the etching region R becomes stable (i.e., after the liquid film formation process is completed), a relatively large flow rate of inert gas is supplied to the substrate W from the heating fluid jetting part 46, thereby promoting an increase in the etching rate.
[0123] As a result, etching of the surface film Ws is performed so as not to expose the substrate main body portion Wb until the shape of the liquid film of the liquid film forming treatment liquid L1 formed in the etching region R is stabilized, and the inhibition of liquid film stabilization due to partial exposure of the substrate main body portion Wb is effectively suppressed. After the shape of the liquid film of the chemical liquid Lc formed in the etching region R is stabilized, etching of the surface film Ws can be performed efficiently.
[0124] [Method of Determining Etching Mode] Even in cases where the etching interface becomes non-uniform in the standard etching modes (first and second standard etching modes) as described above, the adjustment etching modes (first to fifth adjustment etching modes) described above can effectively suppress non-uniformity in the shape of the etching interface.
[0125] However, in reality, whether or not a uniform etching interface can be achieved is determined by the interaction of various etching conditions, and therefore cannot necessarily be easily determined in advance. For example, for substrates W having the same characteristics in terms of specifications, even if a uniform etching interface can be achieved using a standard etching mode for substrates from one lot, the etching interface may become non-uniform for substrates from another lot using the standard etching mode.
[0126] Therefore, the etching mode of the substrate W to be processed may be adaptively determined by the following etching mode determination method. For example, an appropriate etching mode can be determined by performing the following etching mode determination method using a substrate W that represents the plurality of substrates W to be processed, and other substrates W can be processed in accordance with the appropriate etching mode determined in this manner.
[0127] Fig. 18 is a plan view showing an example of a substrate W having an etching treatment liquid L2 (e.g., chemical liquid Lc) supplied to its peripheral edge Wp from a treatment liquid nozzle N. Fig. 19A is an enlarged plan view showing the region indicated by reference symbol "XIXA" in Fig. 18, particularly showing an example in which the peripheral edge Wp of the substrate W to which the etching treatment liquid L2 is applied has hydrophilic surface properties. Fig. 19B is an enlarged plan view showing the region indicated by reference symbol "XIXA" in Fig. 18, particularly showing an example in which the peripheral edge Wp of the substrate W to which the etching treatment liquid L2 is applied has hydrophobic surface properties.
[0128] Note that the notch (cutout) of the substrate W shown in Figures 18 to 19B is indicated by the symbol "n." As is clear from the position of the notch n in Figures 18 to 19B, Figure 18 does not correspond in time to Figures 19A and 19B.
[0129] 18 to 19B , the etching treatment liquid L2 discharged from the treatment liquid nozzle N and applied to the peripheral portion Wp of the substrate W behaves differently depending on the surface characteristics (particularly hydrophilicity / hydrophobicity) of the peripheral portion Wp. That is, when the peripheral portion Wp has hydrophilic surface characteristics (see FIG. 19A ), the etching treatment liquid L2 tends to wet and spread over the peripheral portion Wp and is hardly repelled by the peripheral portion Wp. On the other hand, when the peripheral portion Wp has hydrophobic surface characteristics (see FIG. 19B ), at least a portion of the etching treatment liquid L2 tends to be repelled by the peripheral portion Wp and to splash outward from the peripheral portion Wp as a mist of release liquid Lr.
[0130] In this way, the etching processing liquid L2 applied to the peripheral portion Wp of the substrate W behaves differently depending on the surface characteristics (particularly hydrophilicity / hydrophobicity) of the peripheral portion Wp, and therefore it is possible to select an appropriate etching mode based on this behavior.
[0131] FIG. 20 is a flowchart showing an example of an etching mode determination method.
[0132] The etching mode determination method of FIG. 20 described below is executed by the control unit 93 (see FIG. 1) appropriately controlling the various devices that constitute the substrate processing system 80 (processing unit 10).
[0133] That is, under the control of the control unit 93, the substrate W is rotated by the substrate rotation unit 11 while the etching processing liquid L2 (e.g., chemical liquid Lc) is supplied from the processing liquid supply unit 12 to the etching region R of the peripheral portion Wp of the substrate W.
[0134] The control unit 93 acquires image data (S1 in FIG. 20) obtained by capturing an image of the peripheral portion Wp and its vicinity using the imaging device 49 (see FIG. 2) while the etching treatment liquid L2 is being supplied to the etching region R (particularly within a certain observation time range). The image data acquired in this manner includes images (still images and / or video images) that show the state and behavior of the etching treatment liquid L2 in the peripheral portion Wp and its vicinity.
[0135] The above-mentioned "observation time range" includes the "liquid film formation time," which is the time from when the supply of the etching treatment liquid L2 from the treatment liquid supply unit 12 to the etching region R begins to occur until a liquid film of the etching treatment liquid L2 is formed in the etching region R with a stable shape.
[0136] The control unit 93 then analyzes the imaging data (S2) and, based on the imaging data, detects whether or not there has been a change in the surface state of the peripheral portion Wp of the substrate W (particularly the etching region R) during the observation time range. Generally, whether or not there has been a change in the surface state of the peripheral portion Wp is reflected in whether or not there has been a change in the state of the liquid film on the peripheral portion Wp. Therefore, based on the imaging data, the control unit 93 determines whether or not there has been a change in the state of the liquid film of the etching treatment liquid L2 on the peripheral portion Wp during the observation time range (S3). For example, if the removed liquid Lr (see FIG. 19B ) changes from being observed to not being observed, or if the removed liquid Lr changes from not being observed to being observed, it may be determined that there has been a change in the state of the liquid film (and thus the surface state of the peripheral portion Wp).
[0137] The control unit 93 determines whether or not to execute the adjustment etching mode based on the detection result of whether or not there has been a change in the surface condition of the substrate W. That is, when it is determined that there has been no change in the liquid film state of the etching processing liquid L2 on the peripheral edge Wp (and consequently the surface condition of the peripheral edge Wp) (N in S3), the control unit 93 selects the standard etching mode and determines not to execute the adjustment etching mode (S6).
[0138] On the other hand, if it is determined that there has been a change in the liquid film state of the etching treatment liquid L2 on the peripheral edge Wp (and thus in the surface state of the peripheral edge Wp) (Y in S3), the control unit 93 determines whether the change in the liquid film state occurred before the formation of a uniform liquid film with a stable shape (S4). If the change in the liquid film state occurred after the liquid film had a stable shape but not before (N in S4), the control unit 93 selects the standard etching mode and decides not to execute the adjusted etching mode (S6). On the other hand, if the change in the liquid film state occurred before the liquid film had a stable shape (Y in S4), the control unit 93 selects the adjusted etching mode instead of the standard etching mode and decides to execute the adjusted etching mode (S5).
[0139] Whether the liquid film of the etching treatment liquid L2 on the peripheral edge Wp is a uniform liquid film with a stable shape can be determined, for example, by the control unit 93 analyzing image data and acquiring the state of the liquid film of the etching treatment liquid L2 on the peripheral edge Wp. The specific method for determining whether the liquid film is a uniform liquid film is not limited. For example, if the shape of the outline of the liquid film on the peripheral edge Wp (e.g., the outline of the interface B on the substrate center side) does not change for a predetermined time, or if the rate of change of the shape remains below a threshold for a predetermined time or longer, the liquid film may be determined to be a uniform liquid film with a stable shape.
[0140] In this way, when the control unit 93 detects a change in the surface condition of the peripheral edge Wp of the substrate W, it can acquire the liquid film formation timing, which is the timing at which a stable liquid film of the etching treatment liquid L2 is formed in the etching region R, by analyzing the image data. The control unit 93 then determines whether to execute the adjusted etching mode based on the timing at which the change in the surface condition of the peripheral edge Wp of the substrate W occurs and this liquid film formation timing. That is, if the change in the surface condition of the peripheral edge Wp occurs before the liquid film formation timing, the adjusted etching mode is executed instead of the standard etching mode. On the other hand, if the change in the surface condition of the peripheral edge Wp occurs after the liquid film formation timing, the standard etching mode is executed instead of the adjusted etching mode.
[0141] 20, when the adjustment etching mode is selected and executed, the control unit 93 may select an optimal adjustment etching mode from among multiple adjustment etching modes (see the first to fifth adjustment etching modes described above). The optimal adjustment etching mode may be selected based on various processing conditions, such as the liquid film formation time. The "liquid film formation time" is the time from the start of supply of the etching treatment liquid L2 from the treatment liquid supply unit 12 to the etching region R until a stable liquid film of the treatment liquid L2 is formed in the etching region R, as described above, and can be obtained by the control unit 93 analyzing image data.
[0142] For example, when the liquid film formation time is relatively short (for example, when "liquid film formation time ≦ 1 second"), an adjustment etching mode (for example, the above-mentioned first or fourth adjustment etching mode) in which the etching process is performed after the liquid film formation process may be selected. On the other hand, when the liquid film formation time is relatively long (for example, when "liquid film formation time > 1 second"), an adjustment etching mode (for example, the above-mentioned second, third or fifth adjustment etching mode) in which the etching process is started during the liquid film formation process may be selected.
[0143] It should be noted that the embodiments and modifications disclosed in this specification are merely illustrative in all respects and should not be construed as limiting. The above-described embodiments and modifications may be omitted, substituted, and modified in various ways without departing from the scope and spirit of the appended claims. For example, the above-described embodiments and modifications may be combined in whole or in part, and embodiments other than those described above may be combined with the above-described embodiments or modifications. Furthermore, the effects of the present disclosure described in this specification are merely illustrative, and other effects may be obtained.
[0144] The technical category embodying the above technical idea is not limited. For example, the above technical idea may be embodied by a computer program that causes a computer to execute one or more procedures (steps) included in a method of manufacturing or using the above device. The above technical idea may also be embodied by a computer-readable non-transitory recording medium on which such a computer program is recorded.
Claims
1. A substrate processing apparatus comprising: a substrate rotation unit which holds and rotates a substrate; a processing liquid supply unit which supplies a processing liquid to a peripheral portion of the substrate; and a control unit which controls the substrate rotation unit and the processing liquid supply unit, wherein the control unit controls the substrate rotation unit and the processing liquid supply unit in an adjusted etching mode in which, while rotating the substrate, a liquid film forming processing liquid is supplied from the processing liquid supply unit to the peripheral portion to form a liquid film in an etching region of the peripheral portion, and then, while the liquid film is formed, an etching processing liquid is supplied to the etching region to etch a surface film in the etching region.
2. The substrate processing apparatus according to claim 1, wherein the liquid film forming processing liquid is an etching processing liquid having an etching component for etching the surface film at a concentration lower than that of the etching processing liquid.
3. The substrate processing apparatus according to claim 2, wherein the liquid film forming processing liquid is a mixture of a processing liquid that etches the surface film and a processing liquid that does not etch the surface film.
4. The substrate processing apparatus according to claim 1, wherein the liquid film forming processing liquid is a processing liquid that does not etch the surface film.
5. The substrate processing apparatus according to claim 1, wherein the processing liquid supply unit has: a first processing liquid supply unit which supplies a first processing liquid that does not etch the surface film to the peripheral portion; and a second processing liquid supply unit which supplies a second processing liquid that etches the surface film to the peripheral portion; and the control unit controls the substrate rotation unit and the processing liquid supply unit so as to, while rotating the substrate, supply the first processing liquid from the first processing liquid supply unit to the etching region while stopping the supply of the second processing liquid from the second processing liquid supply unit to the etching region, thereafter supply the second processing liquid from the second processing liquid supply unit to the etching region while continuing the supply of the first processing liquid from the first processing liquid supply unit to the etching region, and thereafter continue the supply of the second processing liquid from the second processing liquid supply unit to the etching region while stopping the supply of the first processing liquid from the first processing liquid supply unit to the etching region.
6. The substrate processing apparatus of claim 5, wherein the control unit, while rotating the substrate, supplies the first processing liquid from the first processing liquid supply unit to the etching region while stopping the supply of the second processing liquid from the second processing liquid supply unit to the etching region, then supplies the second processing liquid from the second processing liquid supply unit to the etching region while continuing the supply of the first processing liquid from the first processing liquid supply unit to the etching region to form the liquid film, and then stops the supply of the first processing liquid from the first processing liquid supply unit to the etching region while continuing the supply of the second processing liquid from the second processing liquid supply unit to the etching region.
7. A substrate processing apparatus as described in claim 1, further comprising a heating mechanism controlled by the control unit for heating the substrate, wherein the control unit controls the heating mechanism so that the substrate is heated by the heating mechanism with a first amount of heat from the time the substrate is held by the substrate rotation unit until the liquid film is formed in the etching region, and thereafter, while the etching processing liquid is being supplied to the etching region, the substrate is heated by the heating mechanism with a second amount of heat greater than the first amount of heat.
8. A substrate processing apparatus as described in claim 7, wherein the heating mechanism has a heating fluid supply unit that discharges a heating fluid heated by a heater, and the substrate is heated using the heating fluid discharged from the heating fluid supply unit, and the control unit controls the heating fluid supply unit so that the flow rate of the heating fluid discharged from the heating fluid supply unit is greater while the substrate is heated with the second amount of heat than while the substrate is heated with the first amount of heat.
9. A substrate processing apparatus as described in claim 1, further comprising an imaging device for imaging the substrate held by the substrate rotation unit, wherein the control unit: supplies the etching treatment liquid from the treatment liquid supply unit to the etching region while rotating the substrate; acquires imaging data obtained by imaging the peripheral portion by the imaging device while the etching treatment liquid is being supplied to the etching region; detects whether or not there has been a change in the surface condition of the substrate based on the imaging data; and determines whether or not to execute the adjusted etching mode based on the detection result of whether or not there has been a change in the surface condition of the substrate.
10. The substrate processing apparatus of claim 9, wherein the control unit, when detecting a change in the surface condition of the substrate, obtains a liquid film formation timing, which is the timing at which the liquid film is formed in the etching region, by analyzing the imaging data, and decides whether or not to execute the adjusted etching mode based on the timing at which the change in the surface condition of the substrate occurs and the liquid film formation timing.
11. A substrate processing method for processing the substrate in an adjusted etching mode, the method including the steps of: supplying a liquid film forming treatment liquid to the peripheral portion while rotating the substrate, thereby forming a liquid film in an etching region of the peripheral portion; and supplying an etching treatment liquid to the etching region while the liquid film is formed, thereby etching a surface film of the etching region.
12. The substrate processing method according to claim 11, wherein the liquid film forming processing liquid is an etching processing liquid containing an etching component at a lower concentration than the etching processing liquid.
13. The substrate processing method according to claim 12, wherein the liquid film forming processing liquid is a mixture of a processing liquid that etches the surface film and a processing liquid that does not etch the surface film.
14. The substrate processing method according to claim 11, wherein the liquid film forming processing liquid is a processing liquid that does not etch the surface film.
15. The substrate processing method according to claim 11, comprising the steps of: while rotating the substrate, supplying a first processing liquid to the etching region while stopping the supply of a second processing liquid to the etching region; thereafter, while continuing the supply of the first processing liquid to the etching region, supplying the second processing liquid to the etching region; and thereafter, while stopping the supply of the first processing liquid to the etching region, continuing the supply of the second processing liquid to the etching region.
16. The substrate processing method according to claim 15, comprising the steps of: supplying the first processing liquid to the etching region while stopping the supply of the second processing liquid to the etching region while rotating the substrate; thereafter, supplying the second processing liquid to the etching region while continuing the supply of the first processing liquid to the etching region to form the liquid film; and thereafter, continuing the supply of the second processing liquid to the etching region while stopping the supply of the first processing liquid to the etching region.
17. The substrate processing method according to claim 11, comprising: a step of heating the substrate with a first amount of heat until the liquid film is formed in the etching region; and a step of heating the substrate with a second amount of heat greater than the first amount of heat while supplying the etching processing liquid to the etching region.
18. A substrate processing method as described in claim 17, wherein the substrate is heated using a heating fluid discharged from a heating fluid supply unit, and the flow rate of the heating fluid discharged from the heating fluid supply unit is greater while the substrate is heated with the second amount of heat than while the substrate is heated with the first amount of heat.
19. A substrate processing method as described in claim 11, comprising the steps of: supplying the etching treatment liquid to the etching region while rotating the substrate; acquiring image data of the peripheral portion by an imaging device while the etching treatment liquid is being supplied to the etching region; detecting whether or not there has been a change in the surface condition of the substrate based on the image data; and determining whether or not to execute the adjustment etching mode based on the detection result of whether or not there has been a change in the surface condition of the substrate.
20. A substrate processing method as described in claim 19, wherein, when a change in the surface condition of the substrate is detected, a liquid film formation timing, which is the timing at which the liquid film is formed in the etching area, is obtained by analyzing the imaging data, and whether or not to execute the adjusted etching mode is determined based on the timing at which the change in the surface condition of the substrate occurs and the liquid film formation timing.
Citation Information
Patent Citations
Substrate processing method and substrate processing equipment
JP2004319990A
Device and method for processing substrate
JP2008047629A
Substrate processing method and substrate processing apparatus
JP2008177584A
Substrate processing device and processing method of substrate processing device
JP2017183492A
Substrate treatment system and substrate treatment method
WO2021210431A1