Cured product for lithium ion secondary batteries, negative electrode for lithium ion secondary batteries, and lithium ion secondary battery

The use of a water-soluble polymer crosslinked with hexacoordination metal-containing agents in lithium ion secondary batteries addresses the issue of silicon-based negative electrode expansion, enhancing cycle characteristics and stability by creating a robust binder that adheres well to the active material, thus improving battery performance.

WO2024241999A1PCT designated stage expired Publication Date: 2024-11-28TDK CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/018036
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-24
Filing Date
2024-05-15
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Lithium ion secondary batteries face challenges in maintaining cycle characteristics due to volumetric expansion of silicon-based negative electrode active materials, leading to cracks and decomposition of the Solid Electrolyte Interphase, which deteriorates battery performance.

Method used

A cured product for lithium ion secondary batteries is developed, featuring a water-soluble polymer crosslinked with a metal-containing crosslinking agent capable of forming a hexacoordination structure, such as titanium or zirconium, with an ion exchange rate of 50% or more and less than 90%, and containing 0.1 to 10 parts by mass of the crosslinking agent per 100 parts by mass of polymer, which improves binding properties and stability.

Benefits of technology

The solution enhances the cycle characteristics of lithium ion secondary batteries by providing a strong and elastic binder that effectively adheres to the negative electrode active material, reducing volumetric expansion-induced damage and maintaining battery performance over cycles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024018036_28112024_PF_FP_ABST
    Figure JP2024018036_28112024_PF_FP_ABST
Patent Text Reader

Abstract

This cured product for lithium ion secondary batteries comprises a water-soluble polymer that is crosslinked with a crosslinking agent. The water-soluble polymer has a carboxy group and a COOX group that is obtained by ion exchanging a part of a carboxy group. The crosslinking agent is a compound which contains a metal that can have a six-coordinate structure.
Need to check novelty before this filing date? Find Prior Art

Description

Cured material for lithium ion secondary battery, negative electrode for lithium ion secondary battery, and lithium ion secondary battery

[0001] The present invention relates to a cured material for a lithium ion secondary battery, a negative electrode for a lithium ion secondary battery, and a lithium ion secondary battery. This application claims priority based on Japanese Patent Application No. 2023-085647, filed on May 24, 2023, the contents of which are incorporated herein by reference.

[0002] Lithium-ion secondary batteries are also widely used as a power source for mobile devices such as mobile phones and laptop computers, as well as hybrid cars.

[0003] The capacity of a lithium-ion secondary battery depends primarily on the active material of the electrode. Graphite is generally used as the negative electrode active material, but there is a demand for a negative electrode active material with higher capacity. For example, silicon (Si) is said to have a theoretical capacity much greater than that of graphite (372 mAh / g).

[0004] A negative electrode active material containing Si undergoes significant volume expansion during charging. The volume expansion of the negative electrode active material causes a deterioration in the cycle characteristics of the battery. When the negative electrode active material expands in volume, cracks may occur in the negative electrode active material, peeling may occur at the interface between the negative electrode active material layer and the current collector, or cracks may occur in the SEI (Solid Electrolyte Interphase) coating, causing decomposition of the electrolyte. These may deteriorate the cycle characteristics of the battery.

[0005] For example, Patent Document 1 discloses a binder in which a water-soluble polymer containing a carboxyl group is crosslinked with a water-soluble crosslinking agent. This binder follows the volume change of the negative electrode active material that accompanies charge and discharge, and the cycle characteristics of a battery using this binder are excellent.

[0006] Patent No. 6961939

[0007] Further improvement in cycle characteristics is required.

[0008] The present disclosure has been made in view of the above problems, and aims to provide a cured material for a lithium ion secondary battery that can improve the cycle characteristics of the lithium ion secondary battery.

[0009] In order to solve the above problems, the following means are provided.

[0010] (1) A cured material for a lithium ion secondary battery according to a first aspect has a water-soluble polymer crosslinked with a crosslinking agent, the water-soluble polymer having a carboxy group and a COOX group formed by ion-exchange of a portion of the carboxy group, and the crosslinking agent is a compound containing a metal capable of forming a hexacoordinated structure.

[0011] (2) In the cured material for a lithium ion secondary battery according to the above aspect, the metal capable of forming a hexacoordination structure may be any one selected from the group consisting of titanium, zirconium, chromium, manganese, cobalt, and nickel.

[0012] (3) In the cured material for a lithium ion secondary battery according to the above aspect, the metal capable of forming a hexacoordination structure may be titanium or zirconium.

[0013] (4) In the cured material for a lithium ion secondary battery according to the above aspect, the water-soluble polymer may have an ion exchange rate of 50% or more and less than 90%, where the ion exchange rate is the ratio of the COOX groups to the total of the carboxy groups and the COOX groups.

[0014] (5) The cured material for a lithium ion secondary battery according to the above aspect may contain 0.1 parts by mass or more and 10 parts by mass or less of the crosslinking agent per 100 parts by mass of the water-soluble polymer.

[0015] (6) The cured material for a lithium ion secondary battery according to the above embodiment is a cured material obtained by dissolving 1 mol / L of LiPF in a non-aqueous solvent containing ethylene carbonate and diethyl carbonate. 6 The liquid absorption rate after immersion for one week in an electrolyte solution containing the compound may be not less than −5% and less than 15%.

[0016] (7) A negative electrode for a lithium ion secondary battery according to a second aspect includes a negative electrode active material and the cured material for a secondary battery according to the above aspect.

[0017] (8) A lithium ion secondary battery according to a third aspect includes a negative electrode for a lithium ion secondary battery, a positive electrode, and a separator disposed between the negative electrode for a secondary battery according to the above aspect and the positive electrode.

[0018] The cured material for lithium ions according to the above embodiment improves the cycle characteristics of a lithium ion secondary battery.

[0019] 1 is a schematic diagram of a lithium ion secondary battery according to a first embodiment; FIG. 2 is a schematic diagram of a binder according to a first embodiment; FIG. 3 is a schematic diagram of the binder according to the first embodiment before crosslinking;

[0020] Hereinafter, the embodiments will be described in detail with reference to the drawings as appropriate. The drawings used in the following description may show characteristic portions enlarged for convenience in order to make the features easier to understand, and the dimensional ratios of each component may differ from the actual ones. The materials, dimensions, etc. exemplified in the following description are merely examples, and the present invention is not limited thereto. Appropriate changes can be made within the scope of the present invention.

[0021] "Lithium-ion secondary battery" FIG. 1 is a schematic diagram of a lithium-ion secondary battery according to a first embodiment. The lithium-ion secondary battery 100 shown in FIG. 1 includes a power generating element 40, an exterior body 50, and a non-aqueous electrolyte (not shown). The exterior body 50 covers the periphery of the power generating element 40. The power generating element 40 is connected to the outside via a pair of terminals 60, 62 connected to the power generating element 40. The non-aqueous electrolyte is accommodated in the exterior body 50. Although FIG. 1 illustrates a case where one power generating element 40 is contained within the exterior body 50, multiple power generating elements 40 may be stacked. The lithium-ion secondary battery 100 may be any of a cylindrical type, a prismatic type, a laminate type, a button type, etc.

[0022] (Power Generation Element) The power generation element 40 includes a separator 10 , a positive electrode 20 , and a negative electrode 30 .

[0023] <Positive Electrode> The positive electrode 20 includes, for example, a positive electrode current collector 22 and a positive electrode active material layer 24. The positive electrode active material layer 24 is in contact with at least one surface of the positive electrode current collector 22.

[0024] [Positive Electrode Current Collector] The positive electrode current collector 22 is, for example, a conductive plate material. The positive electrode current collector 22 is, for example, a thin metal plate made of aluminum, copper, nickel, titanium, stainless steel, or the like. Aluminum, which is lightweight, is preferably used for the positive electrode current collector 22. The average thickness of the positive electrode current collector 22 is, for example, 10 μm or more and 30 μm or less.

[0025] [Positive Electrode Active Material Layer] The positive electrode active material layer 24 contains, for example, a positive electrode active material. The positive electrode active material layer 24 may contain a conductive additive and a binder as necessary.

[0026] The positive electrode active material includes an electrode active material that can reversibly absorb and release lithium ions, desorb and insert (intercalate) lithium ions, or dope and dedope lithium ions with counter anions.

[0027] The positive electrode active material is, for example, a composite metal oxide. The composite metal oxide is, for example, lithium cobalt oxide (LiCoO 2 ), lithium nickel oxide (LiNiO 2 ), lithium manganese oxide (LiMnO 2 ), lithium manganese spinel (LiMn 2 O 4 ), and the general formula: LiNi x Co y Mn z M a O 2 (wherein x+y+z+a=1, 0≦x<1, 0≦y<1, 0≦z<1, 0≦a<1, M is one or more elements selected from Al, Mg, Nb, Ti, Cu, Zn, and Cr), lithium vanadium compounds (LiV 2 O 5 ), olivine-type LiMPO 4 (wherein M represents one or more elements selected from Co, Ni, Mn, Fe, Mg, Nb, Ti, Al, and Zr, or VO), lithium titanate (Li 4 Ti 5 O 12 ), LiNi x Co y Al z O 2(0.9<x+y+z<1.1). The positive electrode active material may be an organic material. For example, the positive electrode active material may be polyacetylene, polyaniline, polypyrrole, polythiophene, or polyacene.

[0028] The positive electrode active material may be a lithium-free material, such as FeF 3 Examples of the non-lithium-containing material include conjugated polymers containing organic conductive materials, Chevrel phase compounds, transition metal chalcogenides, vanadium oxides, and niobium oxides. The non-lithium-containing material may be any one of these materials alone or in combination. When the positive electrode active material is a non-lithium-containing material, for example, discharge is first performed. Lithium is inserted into the positive electrode active material by discharging. Alternatively, a non-lithium-containing positive electrode active material may be pre-doped with lithium chemically or electrochemically.

[0029] The conductive additive enhances the electronic conductivity between the positive electrode active materials. Examples of the conductive additive include carbon powder, carbon nanotubes, carbon materials, metal powder, a mixture of carbon materials and metal powder, and conductive oxides. Examples of the carbon powder include carbon black, acetylene black, and ketjen black. Examples of the metal powder include powders of copper, nickel, stainless steel, and iron.

[0030] There are no particular limitations on the content of the conductive additive in the positive electrode active material layer 24. For example, the content of the conductive additive relative to the total mass of the positive electrode active material, the conductive additive, and the binder is 0.5 mass% or more and 20 mass% or less, and preferably 1 mass% or more and 5 mass% or less.

[0031] The binder in the positive electrode active material layer 24 binds the positive electrode active material together. Known binders can be used. The binder may also be the same as that used in the negative electrode active material layer 34 described below. The binder is preferably insoluble in the electrolyte, oxidation-resistant, and adhesive. Examples of binders include fluororesin. Examples of binders include polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyamide (PA), polyimide (PI), polyamideimide (PAI), polybenzimidazole (PBI), polyethersulfone (PES), polyacrylic acid and its copolymers, metal ion-crosslinked polyacrylic acid and its copolymers, maleic anhydride-grafted polypropylene (PP) or polyethylene (PE), and mixtures thereof. PVDF is particularly preferred as the binder used in the positive electrode active material layer.

[0032] The binder content in the positive electrode active material layer 24 is not particularly limited. For example, the binder content relative to the total mass of the positive electrode active material, conductive additive, and binder is 1% by mass or more and 15% by mass or less, and preferably 1.5% by mass or more and 5% by mass or less. If the binder content is low, the adhesive strength of the positive electrode 20 will be weakened. If the binder content is high, the binder will be electrochemically inactive and will not contribute to the discharge capacity, resulting in a low energy density of the lithium-ion secondary battery 100.

[0033] <Negative Electrode> The negative electrode 30 includes, for example, a negative electrode current collector 32 and a negative electrode active material layer 34. The negative electrode active material layer 34 is formed on at least one surface of the negative electrode current collector 32. The negative electrode 30 is an example of a negative electrode for a lithium ion secondary battery.

[0034] [Negative Electrode Current Collector] The negative electrode current collector 32 is, for example, a conductive plate material. The negative electrode current collector 32 may be the same as the positive electrode current collector 22.

[0035] [Negative Electrode Active Material Layer] The negative electrode active material layer 34 contains a negative electrode active material and a binder. The negative electrode active material layer 34 may contain a conductive additive as needed. The binder is an example of a cured material for a lithium ion secondary battery.

[0036] The negative electrode active material includes silicon or a silicon compound. The silicon compound is, for example, a silicon alloy or silicon oxide. For example, the silicon or silicon compound may be crystalline, amorphous, or amorphous with crystalline dispersed therein. Amorphous silicon or silicon compound can be produced by a melt-spun method, a gas atomization method, or the like. The negative electrode active material may be a known material other than silicon or a silicon compound.

[0037] Silicon alloys are X n The formula is Si. X is a cation. X is, for example, Ba, Mg, Al, Zn, Sn, Ca, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Ge, Y, Zr, Nb, Mo, W, Au, Ti, Na, K, etc. n satisfies 0≦n≦0.5. Silicon oxide is SiO x where x satisfies, for example, 0.8≦x≦2. Silicon oxide is represented by SiO 2 It may consist of only SiO, or may consist of SiO and SiO 2 The silicon oxide may be a mixture of the above. The silicon oxide may have some oxygen deficiencies.

[0038] The negative electrode active material may be a composite of silicon or a silicon compound. The composite is a silicon or silicon compound particle in which at least a portion of the surface is coated with a conductive material. Examples of the conductive material include carbon materials, Al, Ti, Fe, Ni, Cu, Zn, Ag, and Sn. For example, a silicon-carbon composite material (Si—C) is an example of the composite. The amount of the conductive material coated on the silicon or silicon compound particles is, for example, 0.01% by mass or more and 30% by mass or less, and preferably 0.1% by mass or more and 20% by mass or less, relative to the total mass of the composite. The composite can be produced, for example, by mechanical alloying, chemical vapor deposition, a wet process, or a method in which a polymer is coated and then the polymer is thermally decomposed and carbonized.

[0039] The specific surface area of ​​the negative electrode active material determined by the BET method is, for example, 0.5 m 2 / g or more 100m 2 / g or less, preferably 1.0m 2 / g or more 20m 2 / g or less. If the specific surface area is small, it becomes difficult for Li ions to be inserted and released between the negative electrode active material. If the specific surface area is large, a large amount of binder is required to form an electrode, resulting in a small capacity per unit volume.

[0040] The binder adheres to the surface of the negative electrode active material and binds the negative electrode active materials together and the negative electrode active material and the negative electrode current collector. Fig. 2 is a schematic diagram of a binder 1 according to the first embodiment. The binder 1 includes a water-soluble polymer 2 and a crosslinking agent 3. The binder 1 is formed by crosslinking the water-soluble polymer 2 with the crosslinking agent 3. When the binder 1 hardens, it adheres to the surface of the negative electrode active material.

[0041] The water-soluble polymer 2 is, for example, a polymer having a carboxy group, some of which has been partially ion-exchanged. The water-soluble polymer 2 has, for example, a carboxy group 2A and a COOX group 2B in which a portion of the carboxy group has been substituted. The COOX group 2B is formed by ion-exchanging a hydrogen atom of the carboxy group with a cation. The cation that is ion-exchanged with a portion of the carboxy group is, for example, Li, Na, or K. X in the COOX group is, for example, Li, Na, or K.

[0042] For example, 50% or more and less than 90% of the carboxy groups in the water-soluble polymer 2 are ion-exchanged. That is, the ion-exchange rate of the water-soluble polymer 2 is preferably 50% or more and less than 90%, and more preferably 60% or more and 80% or less. The ion-exchange rate is the ratio of COOX groups 2B to the total of carboxy groups 2A and COOX groups 2B in which a portion of the carboxy groups have been ion-exchanged.

[0043] Ion-exchanging some of the carboxyl groups in the water-soluble polymer 2 with COOX groups 2B can suppress intramolecular crosslinking of the water-soluble polymer 2. When the water-soluble polymer 2 undergoes intramolecular crosslinking, the water-soluble polymer 2 gels, reducing the functionality of the binder 1. Furthermore, when the water-soluble polymer 2 has COOX groups 2B, the COOX groups 2B function as a catalyst for the crosslinking reaction and promote crosslinking between molecular chains of the water-soluble polymer 2.

[0044] The carboxyl groups 2A are responsible for bonding to the negative electrode active material and cross-linking with the cross-linking agent 3. Therefore, the presence of carboxyl groups 2A that have not been ion-exchanged in the binder 1 increases the binding strength between the binder 1 and the negative electrode active material, and the binder 1 forms a network structure. The proportion of ion-exchanged carboxyl groups in the water-soluble polymer 2 can be determined by the amount of alkali consumption required for hydrolysis of the copolymerization units or by composition analysis using nuclear magnetic resonance (NMR).

[0045] Examples of the water-soluble polymer 2 include polyacrylic acid, carboxymethyl cellulose, a copolymer of acrylic acid and vinyl alcohol, a copolymer of sodium acrylate and vinyl alcohol, sodium carboxymethyl cellulose, polynorbornene dicarboxylic acid, and polymethacrylic acid. One type of water-soluble polymer 2 may be used alone, or multiple types may be used in combination.

[0046] The weight-average molecular weight of the water-soluble polymer 2 is, for example, 25,000 or more and 640,000 or less. If the molecular weight of the water-soluble polymer 2 is small, there are fewer crosslinking points for crosslinking between the water-soluble polymers 2, and the elasticity of the binder 1 after crosslinking decreases. If the molecular weight of the water-soluble polymer 2 is large, the binder 1 gels, making uniform dispersion difficult. The weight-average molecular weight of the water-soluble polymer 2 can be determined by analyzing the water-soluble polymer before crosslinking, if the water-soluble polymer 2 before crosslinking is available. If the water-soluble polymer 2 before crosslinking is not available, it can be roughly estimated from the weight-average molecular weight of the binder 1 and the abundance ratio of the water-soluble polymer 2 to the crosslinking agent 3 in the binder 1.

[0047] Here, whether a polymer is "water-soluble" can be determined by the following procedure. First, a mixture is prepared by adding 1 part by weight of polymer (equivalent to the solid content) to 100 parts by weight of ion-exchanged water and stirring. This mixture is adjusted to a temperature of 20 to 95°C and a pH of 3 to 12 (pH is adjusted using an aqueous NaOH solution and / or an aqueous HCl solution). Next, this mixture is passed through a 250-mesh screen. If the weight of the solid content of the residue that does not pass through the screen and remains on the screen does not exceed 50% by weight of the solid content of the polymer added, the polymer can be said to be water-soluble. Note that even if the mixture of the polymer and water is in an emulsion state that separates into two phases when left to stand, the polymer is still water-soluble if it satisfies the above definition.

[0048] The crosslinking agent 3 crosslinks the water-soluble polymers 2. The crosslinking agent 3 is a compound containing a metal capable of forming a hexacoordinate structure. The metal capable of forming a hexacoordinate structure is any one selected from the group consisting of titanium, zirconium, chromium, manganese, cobalt, and nickel. The metal capable of forming a hexacoordinate structure is preferably titanium or zirconium.

[0049] 2 shows an example in which the cross-linking agent 3 is a compound containing titanium. The cross-linking agent 3 has a metal-oxygen bond at the bond site with the water-soluble polymer 2. The metal-oxygen bond is strong, and the cross-linking agent 3 strongly cross-links the water-soluble polymers 2 together.

[0050] Fig. 3 is a schematic diagram of the binder according to the first embodiment before crosslinking. Fig. 3 illustrates an example of a compound in which the crosslink precursor 4 contains titanium. Although shown in a simplified form in Fig. 3, for example, the following chemical formula (1) is the chemical structural formula of the crosslink precursor 4 when the metal capable of forming a hexacoordinate structure is titanium.

[0051]

[0052] For example, a carboxy group of the water-soluble polymer 2 reacts with a hydroxyl group of the crosslinking precursor 4, whereby the water-soluble polymers 2 are crosslinked with each other by the crosslinking agent 3. In the above chemical formula (1), the two hydroxyl groups of the crosslinking precursor 4 form metal-oxygen bonds with the water-soluble polymer 2.

[0053] A portion of the carboxy groups of the water-soluble polymer 2 does not react with the crosslinked precursor 4 and remains unreacted. The remaining carboxy groups interact with the negative electrode active material, improving the binding strength between the negative electrode active material and the binder 1. Here, an example in which carboxy groups react with each other to bond is shown, but the bond between the water-soluble polymer 2 and the crosslinked precursor 4 is not limited to this example. For example, an alkoxy group of the crosslinked precursor 4 may be released and react with a hydroxyl group of the water-soluble polymer 2. Furthermore, for example, an isocyanate group, a carboxy group, etc. of the crosslinked precursor 4 may undergo a bonding reaction with a carboxy group of the water-soluble polymer 2.

[0054] The crosslinked precursor 4 is a compound containing a metal capable of forming a hexacoordinate structure within its structure. The metal capable of forming a hexacoordinate structure is any one selected from the group consisting of titanium, zirconium, chromium, manganese, cobalt, and nickel. The metal capable of forming a hexacoordinate structure is preferably titanium or zirconium.

[0055] The crosslinked precursor 4 is, for example, an organometallic compound containing a metal capable of forming a hexacoordinate structure. For example, the case where the metal capable of forming a hexacoordinate structure is titanium or zirconium will be exemplified. While specific examples of titanium or zirconium will be exemplified here, similar compounds can also be used as the crosslinked precursor 4 when the metal capable of forming a hexacoordinate structure is chromium, manganese, cobalt, or nickel.

[0056] The titanium compound containing titanium is an organic titanium compound, for example, a titanium chelate. Examples of the titanium compound include titanium lactate, titanium triethanolamine, titanium lactate ammonium salt, titanium diethanolamine, and titanium aminoethylaminoethylate. The zirconium compound containing zirconium is an organic zirconium compound, for example, a zirconium chelate. Examples of the zirconium compound include zirconium lactate, zirconium triethanolamine, zirconium lactate ammonium salt, zirconium diethanolamine, and zirconium aminoethylaminoethylate. For example, organic titanium compounds and organic zirconium compounds manufactured by Matsumoto Fine Chemical Co., Ltd. can be used as the crosslinked precursor 4.

[0057] The crosslinking precursor 4 reacts with the carboxyl group of the water-soluble polymer 2 to become the crosslinking agent 3 that connects the water-soluble polymers 2 together. The crosslinking agent 3 containing a metal compound is compact, and when the water-soluble polymer 2 is crosslinked using this, the crystallinity of the water-soluble polymer 2 is easily maintained.

[0058] The amount of the crosslinking agent 3 is, for example, 0.1 parts by mass or more and less than 10 parts by mass, preferably 0.1 parts by mass or more and 9.8 parts by mass or less, and more preferably 0.5 parts by mass or more and 3.1 parts by mass or less, relative to 100 parts by mass of the water-soluble polymer 2. The mass ratio of the crosslinking agent 3 to the water-soluble polymer 2 is equal to the amount of the crosslinking precursor 4 added to the water-soluble polymer 2 before crosslinking.

[0059] A low ratio of crosslinking agent 3 in binder 1 means that there are few crosslinking points within binder 1 that crosslink water-soluble polymers 2 together. If there are few crosslinking points within binder 1, the elasticity of binder 1 decreases. Furthermore, a high ratio of crosslinking agent 3 means that there are many crosslinking points within binder 1, and it is thought that the water-soluble polymers 2 are intramolecularly crosslinked. If the water-soluble polymers 2 are intramolecularly crosslinked, the viscosity of binder 1 increases or the binder 1 gels, thereby reducing the functionality of binder 1. Furthermore, if the ratio of crosslinking agent 3 is high, the proportion of carboxyl groups that can be freely present within binder 1 decreases, and the binding strength between the binder 1 and the negative electrode active material and negative electrode current collector 32 decreases.

[0060] When a binder precursor solution before the crosslinking reaction in which the water-soluble polymer 2 and the crosslinking precursor 4 are mixed is available, the mass ratio of the crosslinking agent 3 to the water-soluble polymer 2 in the binder 1 can be determined from the mass ratio of the water-soluble polymer 2 to the crosslinking precursor 4 in the binder precursor solution.

[0061] The mass ratio of the crosslinking agent 3 to the water-soluble polymer 2 can be determined from a lithium ion secondary battery containing the binder 1 after the crosslinking reaction, for example, by the following procedure. First, the binder 1 is separated from the lithium ion secondary battery. The negative electrode 30 from which the electrolytic solution has been removed is immersed in water, and the resulting solution is dried to extract the binder 1 as a solid. The binder 1 extracted as a solid is analyzed, for example, by Fourier transform infrared spectroscopy (FT-IR). The water-soluble polymer 2, which is the main component of the binder 1, is identified through the analysis. Next, the mass ratio of the crosslinking agent 3 to the water-soluble polymer 2 is determined from the binder 1. These mass ratios can be determined, for example, by comparing the results of thermogravimetric differential thermal analysis (TG-DTA) of the extracted binder 1 with the results of TG-DTA using the polymer material (water-soluble polymer 2), which is the main component, identified by the above FT-IR analysis, as a standard sample. Since the water-soluble polymer 2 and the cross-linking agent 3 have different decomposition temperatures, the TG-DTA measurement makes it possible to quantitatively analyze the binder 1.

[0062] When the amount of crosslinker is so small that TG-DTA measurement is difficult, qualitative and quantitative analysis of the crosslinker may be performed using gas chromatography mass spectrometry (GC / MS), high-performance liquid chromatography / photodiode array detection (LC / PDA), liquid chromatography mass spectrometry (LC / MS), etc. Depending on the properties of the crosslinker, each chromatography may be combined with an appropriate detection method (e.g., MS, flame ionization detection, barrier discharge detection, fluorescence detection, differential refractive index detection, GC / quadrupole time-of-flight mass spectrometry (Q-TOFMS), liquid chromatography quadrupole time-of-flight mass spectrometry (LC / Q-TOFMS), etc.).

[0063] The liquid absorption rate of the binder 1 is, for example, −5% or more and less than 15%. The liquid absorption rate is determined by dissolving 1 mol / L of LiPF 6 in a non-aqueous solvent containing ethylene carbonate and diethyl carbonate. 6 The liquid absorption rate is the rate after immersion for one week in an electrolyte solution containing the binder 1. The liquid absorption rate can be calculated from the weight of the binder 1 before and after immersion in the electrolyte solution using the following formula: Liquid absorption rate (%) = 100 - (weight of the binder after immersion in the electrolyte solution and drying / weight of the binder before immersion in the electrolyte solution x 100)

[0064] First, the weight of the binder 1 before immersion in the electrolyte solution is measured. Next, LiPF 6 is added as an electrolyte to a mixed solvent of ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of EC:DEC=3:7. 6 An electrolyte solution is prepared by dissolving the above to a concentration of 1 mol / L. Binder 1 is immersed in this electrolyte solution at 25°C for one week. After immersing binder 1 in the electrolyte solution at 25°C for one week, binder 1 reaches a saturated liquid absorption state. The saturated liquid absorption state refers to a state in which the weight of the cured product hardly changes even if it is immersed in the electrolyte solution for a longer period of time. Then, binder 1 after immersion is wiped dry. The weight of binder 1 after drying is measured.

[0065] The liquid absorption rate shows a negative value when the binder 1 dissolves in the electrolyte solution, and a positive value when the binder 1 absorbs the electrolyte solution. When the liquid absorption rate of the binder 1 is within the above range, the binder 1 is unlikely to dissolve or swell in the electrolyte solution and is stable.

[0066] The content of binder 1 in the negative electrode active material layer 34 is not particularly limited. For example, the content of binder 1 relative to the total mass of the negative electrode active material, conductive additive, and binder 1 is 0.5 mass% or more and 20 mass% or less, and preferably 5 mass% or more and 15 mass% or less. If the content of binder 1 is low, the adhesive strength of the negative electrode 30 will be weakened. If the content of binder 1 is high, the binder 1 will be electrochemically inactive and will not contribute to the discharge capacity, resulting in a low energy density of the lithium-ion secondary battery 100.

[0067] The conductive additive in the negative electrode active material layer 34 enhances the electronic conductivity between the negative electrode active materials. The conductive additive may be the same as that in the positive electrode active material layer 24.

[0068] There are no particular limitations on the content of the conductive additive in the negative electrode active material layer 34. For example, the content of the conductive additive relative to the total mass of the negative electrode active material, the conductive additive, and the binder is 5% by mass or more and 20% by mass or less, and preferably 1% by mass or more and 12% by mass or less.

[0069] <Separator> The separator 10 is sandwiched between the positive electrode 20 and the negative electrode 30. The separator 10 separates the positive electrode 20 from the negative electrode 30 and prevents short-circuiting between the positive electrode 20 and the negative electrode 30. The separator 10 extends in-plane along the positive electrode 20 and the negative electrode 30. Lithium ions can pass through the separator 10.

[0070] The separator 10 has, for example, an electrically insulating porous structure. The separator 10 is, for example, a monolayer or laminate of a polyolefin film. The separator 10 may be a stretched membrane of a mixture of polyethylene, polypropylene, or the like. The separator 10 may be a fibrous nonwoven fabric made of at least one constituent material selected from the group consisting of cellulose, polyester, polyacrylonitrile, polyamide, polyethylene, and polypropylene. The separator 10 may be, for example, a solid electrolyte. The solid electrolyte may be, for example, a polymer solid electrolyte, an oxide-based solid electrolyte, or a sulfide-based solid electrolyte. The separator 10 may also be an inorganic-coated separator. The inorganic-coated separator is formed by coating the surface of the above-mentioned film with a mixture of a resin such as PVDF or CMC and an inorganic material such as alumina or silica. The inorganic-coated separator has excellent heat resistance and suppresses the deposition of transition metals eluted from the positive electrode onto the negative electrode surface.

[0071] <Electrolyte> The electrolyte is sealed in the exterior body 50 and impregnates the power generating element 40. The non-aqueous electrolyte includes, for example, a non-aqueous solvent and an electrolytic salt. The electrolytic salt is dissolved in the non-aqueous solvent.

[0072] The electrolyte may be a known electrolyte, and may contain, for example, a non-aqueous solvent and an electrolyte salt.

[0073] The electrolyte salt is, for example, a lithium salt. 6 , LiClO 4 , LiBF 4 , LiCF 3 SO 3 , LiCF 3 CF 2 SO 3 , LiC(CF 3 SO 2 ) 3 , LiN(CF 3 SO2 ) 2 , LiN(CF 3 CF 2 SO 2 ) 2 , LiN(CF 3 SO 2 ) (C 4 F 9 SO 2 ), LiN(CF 3 CF 2 CO) 2 , LiBOB, LiN(FSO 2 ) 2 The lithium salt may be used alone or in combination of two or more. From the viewpoint of the degree of ionization, the electrolyte is preferably LiPF 6 The concentration of the electrolytic salt is, for example, 0.8 mol / L or more and 5.0 mol / L or less.

[0074] The non-aqueous solvent is, for example, an aprotic organic solvent. The organic solvent is, for example, a cyclic carbonate, a chain carbonate, an ether, a mixture thereof, or an ionic liquid.

[0075] The cyclic carbonate solvates the electrolyte. Examples of the cyclic carbonate include ethylene carbonate, propylene carbonate, butylene carbonate, and fluoroethylene carbonate. The cyclic carbonate preferably contains at least fluoroethylene carbonate. Fluoroethylene carbonate (FEC) has a high oxidation-reduction potential and is easily reduced and decomposed. Reductive decomposition of a portion of the fluoroethylene carbonate (FEC) makes the electrolyte and remaining solvent in the electrolyte solution less likely to decompose. Furthermore, fluoroethylene carbonate (FEC) forms a thin, stable coating (SEI coating) on ​​the entire surface of the negative electrode active material during the initial use of the lithium ion secondary battery. The SEI coating prevents direct contact between the negative electrode active material and the electrolyte solution, preventing decomposition of the electrolyte solution.

[0076] The chain carbonate reduces the viscosity of the cyclic carbonate. Examples of the chain carbonate include diethyl carbonate, dimethyl carbonate, and ethyl methyl carbonate. The non-aqueous solvent may also contain methyl acetate, ethyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, 1,2-dimethoxyethane, and 1,2-diethoxyethane.

[0077] The electrolyte may also contain a solid electrolyte interface (SEI) forming material, a surfactant, etc. Examples of additives include vinylene carbonate, vinylethylene carbonate, phenylethylene carbonate, succinic anhydride, lithium bisoxalate, lithium tetrafluoroborate, dinitrile compounds, propane sultone, butane sultone, propene sultone, 3-sulfolene, fluorinated allyl ether, and fluorinated acrylate.

[0078] <Exterior Body> The exterior body 50 seals the power generating element 40 and the non-aqueous electrolyte solution inside. The exterior body 50 prevents the non-aqueous electrolyte solution from leaking to the outside and prevents moisture and the like from entering the lithium-ion secondary battery 100 from the outside.

[0079] 1, the exterior body 50 has a metal foil 52 and a resin layer 54 laminated on each side of the metal foil 52. The exterior body 50 is a metal laminate film in which the metal foil 52 is coated on both sides with a polymer film (resin layer 54).

[0080] The metal foil 52 can be, for example, aluminum foil. The resin layer 54 can be a polymer film such as polypropylene. The materials constituting the inner and outer resin layers 54 can be different. For example, the outer material can be a polymer with a high melting point, such as polyethylene terephthalate (PET) or polyamide (PA), and the inner polymer film can be made of polyethylene (PE), polypropylene (PP), or the like.

[0081] <Terminals> The terminals 60 and 62 are connected to the negative electrode 30 and the positive electrode 20, respectively. The terminal 62 connected to the positive electrode 20 is a positive electrode terminal, and the terminal 60 connected to the negative electrode 30 is a negative electrode terminal. The terminals 60 and 62 are responsible for electrical connection between the outside and the power generating element 40. The terminals 60 and 62 are made of a conductive material such as aluminum, nickel, or copper. The connection method may be welding or screw fastening. It is preferable to protect the terminals 60 and 62 with insulating tape to prevent short circuits.

[0082] "Method for manufacturing lithium-ion secondary battery" The lithium-ion secondary battery 100 is fabricated by preparing and assembling the negative electrode 30, the positive electrode 20, the separator 10, the electrolyte, and the exterior body 50. An example of a method for manufacturing the lithium-ion secondary battery 100 will be described below.

[0083] First, the negative electrode 30 is produced. The negative electrode 30 is produced, for example, by sequentially carrying out a precursor solution production step, a slurry production step, an electrode application step, a curing step, and a rolling step.

[0084] First, a precursor solution preparation step is performed. First, a water-soluble polymer solution and a crosslinking precursor are prepared. As the crosslinking precursor, an organometallic compound containing a metal capable of forming a hexacoordinated structure is prepared. As the crosslinking precursor, for example, an organotitanium compound or an organozirconium compound manufactured by Matsumoto Fine Chemical Co., Ltd. can be used.

[0085] The water-soluble polymer solution is one in which some of the carboxyl groups have been ion-exchanged. 2 CO 3 , LiOH, Li 2 CO 3 , K. 2 CO 3 By adding an aqueous solution of NaOH or NaOH to a polymer solution and stirring it, some of the carboxyl groups of the water-soluble polymer can be ion-exchanged. 2 CO 3 , LiOH, Li 2 CO 3 , K. 2 CO 3 The cations contained in the aqueous solution of the above neutralize the carboxyl groups, and the protons of the carboxyl groups undergo ion exchange with the cations.

[0086] Next, the water-soluble polymer solution and the crosslinking precursor are mixed to prepare a binder precursor solution. The mixing ratio of the water-soluble polymer solution and the crosslinking precursor is adjusted depending on the desired binder composition.

[0087] Although it varies depending on the type of water-soluble polymer, when dissolving the water-soluble polymer in water, stirring is carried out for at least one hour at room temperature to 100°C or less. The rotation speed during stirring is set to 550 rpm or more and 1500 rpm or less to allow complete dissolution. Thereafter, the crosslinking precursor is added to the water-soluble polymer solution and stirred at room temperature for at least five minutes. The rotation speed during stirring is, for example, 180 rpm or more and 600 rpm or less. By thoroughly dispersing the crosslinking precursor in the water-soluble polymer solution, the crosslinking reaction can be carried out evenly.

[0088] Next, a slurry preparation step is carried out, in which a negative electrode active material (silicon or a silicon compound) and a conductive additive are added to a binder precursor solution.

[0089] The solvent is, for example, water. The composition ratio of the negative electrode active material, the conductive additive, and the binder precursor solution is, for example, 70 wt % to 99 wt %: 0 wt % to 10 wt %: 1 wt % to 20 wt % by mass. These mass ratios are adjusted so that the total is 100 wt %.

[0090] The negative electrode active material may be a composite obtained by mixing active material particles and a conductive material while applying shearing force. When the active material particles are mixed under shearing force to a degree that does not alter their properties, the surfaces of the active material particles are coated with the conductive material. The particle size of the negative electrode active material can be adjusted by adjusting the degree of mixing. The negative electrode active material may also be sieved after preparation to make the particle size uniform.

[0091] Next, an electrode coating step is performed. The electrode coating step is a step of coating a slurry on the surface of the negative electrode current collector 32. The method for coating the slurry is not particularly limited. For example, a slit die coating method or a doctor blade method can be used as the method for coating the slurry.

[0092] Next, a curing step is carried out. In the curing step, the slurry is annealed. By annealing the slurry, the water-soluble polymer and the crosslinking precursor are crosslinked. In the curing step, the solvent is removed. The curing step is carried out, for example, in a nitrogen atmosphere. The curing temperature is, for example, 120°C or higher and 150°C or lower. The temperature rise rate up to the curing temperature is, for example, 2°C / min or higher and 5°C / min or lower. The temperature drop rate after curing is, for example, 2°C / min or higher and 5°C / min or lower. By curing the binder under the above conditions, it is possible to suppress uneven crosslinking sites and also to sufficiently proceed with the crosslinking reaction.

[0093] The rolling step is performed as necessary. The rolling step is a step of applying pressure to the negative electrode active material layer 34 to adjust the density of the negative electrode active material layer 34. The rolling step is performed using, for example, a roll press device.

[0094] The positive electrode 20 can be produced by the same procedure as that for the negative electrode 30. The separator 10 and the outer casing 50 can be commercially available products.

[0095] Next, the prepared positive electrode 20 and negative electrode 30 are stacked so that the separator 10 is positioned between them to prepare the power generating element 40. When the power generating element 40 is a wound body, the positive electrode 20, the negative electrode 30, and one end side of the separator 10 are wound around the axis.

[0096] Finally, the power generation element 40 is sealed in the exterior body 50. A non-aqueous electrolyte solution is poured into the exterior body 50. After the non-aqueous electrolyte solution is poured, the pressure is reduced, heating, etc. is performed, so that the non-aqueous electrolyte solution is impregnated into the power generation element 40. The exterior body 50 is sealed by applying heat, etc., to obtain the lithium-ion secondary battery 100. Note that instead of pouring the electrolyte solution into the exterior body 50, the power generation element 40 may be impregnated with the electrolyte solution.

[0097] The lithium-ion secondary battery 100 according to the first embodiment has excellent cycle characteristics. This is thought to be because the binder 1 contained in the negative electrode active material layer 34 has a large network structure in which a water-soluble polymer 2 is crosslinked with a crosslinking agent 3, resulting in high strength and high elasticity. The binder 1 is also strongly crosslinked by metal-oxygen bonds connecting the water-soluble polymer and the crosslinking agent, resulting in high strength. Unreacted carboxy groups in the binder interact with the negative electrode active material, forming a strong bond. In other words, the lithium-ion secondary battery 100 according to the first embodiment has excellent cycle characteristics because it has a binder 1 that is highly elastic and can strongly bond to the negative electrode active material.

[0098] The above describes the embodiments of the present invention in detail with reference to the drawings. However, each configuration and combination thereof in each embodiment is an example, and additions, omissions, substitutions, and other modifications of the configurations are possible within the scope that does not deviate from the spirit of the present invention.

[0099] Example 1 First, polyacrylic acid having a weight-average molecular weight of 25,000 was prepared as a base polymer. Then, 60% of the carboxy groups contained in the polyacrylic acid were subjected to ion exchange, thereby substituting H of the carboxy groups with Li. While stirring the polyacrylic acid aqueous solution at 500 rpm, an LiOH aqueous solution was gradually added dropwise to perform the ion exchange.

[0100] Next, titanium lactate ammonium salt (manufactured by Matsumoto Fine Chemical Co., Ltd.: Orgatix TC-335) was prepared as a crosslinking precursor.

[0101] Next, 100 parts by mass of the water-soluble polymer and water were added, and the mixture was stirred at room temperature for 2 hours or more, with the rotation speed set to 550 rpm or more and 1500 rpm or less, until the mixture was completely dissolved. After that, 0.5 parts by mass of the crosslinking precursor was added to the aqueous water-soluble polymer solution.

[0102] The crosslinking reaction of the binder was carried out in a nitrogen atmosphere by increasing the temperature at a rate of 5°C / min, keeping it at 150°C for 3 hours, and then decreasing the temperature at a rate of 5°C / h. Before sintering, the binder precursor solution containing the crosslinking precursor and the water-soluble polymer aqueous solution was stirred at a rotation speed of 300 rpm for 30 minutes or more.

[0103] The liquid absorption rate of the binder prepared was measured. The liquid absorption rate of the binder of Example 1 was 2%.

[0104] The negative electrode active material and the conductive additive were added to a binder-containing solution prepared under the same conditions as the sample for which the liquid absorption rate was measured. The negative electrode active material was SiO.sub.2, which was subjected to a disproportionation reaction by heat treatment at 1000°C under reduced pressure. x The conductive additive was Super-P (registered trademark). 25 g of the negative electrode active material, 1.4 g of the conductive additive, and 13.5 g of an aqueous binder solution (solid content concentration 10%) were mixed to prepare a coating liquid (slurry). The total solid content concentration in the coating liquid was 35 wt %. Next, the slurry was applied to a copper foil serving as a negative electrode current collector using a doctor blade.

[0105] Next, the negative electrode current collector coated with the slurry was annealed in a nitrogen atmosphere. The annealing was performed under the conditions of increasing the temperature at 5°C / min, keeping it at 150°C for 2 hours, and decreasing the temperature at 5°C / min. The annealing caused crosslinking between the water-soluble polymer and the crosslinking agent, hardening the slurry. The negative electrode current collector after hardening was then rolled to form the negative electrode active material layer 34. A die was used to punch out an electrode size of 22 x 32 mm, producing a negative electrode.

[0106] The positive electrode active material is Li x CoO 2 The conductive additive was Ketjen black. The binder was polyvinylidene fluoride (PVDF). The solvent was N-methyl-2-pyrrolidone. 96 parts by mass of the positive electrode active material, 2 parts by mass of the conductive additive, 2 parts by mass of the binder, and 70 parts by mass of the solvent were mixed to prepare a positive electrode slurry. The positive electrode slurry was then applied to one side of a 15 μm thick aluminum foil, which was then vacuum dried at 100°C for 2 hours and rolled to form a positive electrode active material layer 24. The positive electrode was then punched out using a mold to prepare an electrode size of 22 × 32 mm.

[0107] Next, an electrolyte solution was prepared. The solvent was a mixture of ethylene carbonate (EC) and diethyl carbonate (DEC) in a mass ratio of 3:7. The electrolyte salt was LiPF 6 LiPF was used. 6The concentration was set to 1 mol / L.

[0108] (Preparation of Lithium-Ion Secondary Battery for Evaluation) The prepared negative and positive electrodes were stacked with a separator (porous polyethylene sheet) interposed between them so that the positive and negative active material layers faced each other, to obtain a laminate. A nickel negative electrode lead was attached to the negative electrode of the laminate. An aluminum positive electrode lead was attached to the positive electrode of the laminate. The positive and negative electrode leads were welded using an ultrasonic welder. This laminate was inserted into an exterior body made of aluminum laminate film and heat-sealed except for one peripheral location to form a closed opening. Finally, the above-mentioned electrolyte solution was injected into the exterior body, and the remaining location was heat-sealed while reducing the pressure using a vacuum sealer, to prepare a lithium-ion secondary battery.

[0109] (Measurement of Capacity Retention Rate After 100 Cycles) The cycle characteristics of the lithium ion secondary battery were measured using a secondary battery charge / discharge tester (manufactured by Hokuto Denko Corporation).

[0110] The battery was charged at a constant current charge rate of 0.5 C (a current value at which charging is completed in 1 hour when constant current charging is performed at 25°C) until the battery voltage reached 4.2 V, and then discharged at a constant current discharge rate of 1.0 C until the battery voltage reached 2.5 V. The discharge capacity after the end of charging and discharging was detected, and the battery capacity Q before the cycle test was 1 asked for.

[0111] The battery capacity Q 1 The battery for which Q was determined was again charged using a secondary battery charge / discharge tester at a constant current charge rate of 0.5 C until the battery voltage reached 4.2 V, and then discharged at a constant current discharge rate of 1.0 C until the battery voltage reached 2.5 V. The above charge / discharge cycle was counted as one cycle, and 100 charge / discharge cycles were performed. After that, the discharge capacity after 100 charge / discharge cycles was measured, and the battery capacity Q after 100 cycles was determined. 2 asked for.

[0112] The capacity Q calculated above 1 , Q 2 The capacity retention rate E after 100 cycles was calculated from the above. The capacity retention rate E was calculated as follows: E = Q 2 / Q1 × 100 The capacity retention rate of Example 1 was 71%.

[0113] Examples 2 to 4 Examples 2 to 4 differ from Example 1 in that the molecular weight of the base polymer of the water-soluble polymer was changed. Other conditions in Examples 2 to 4 were basically the same as in Example 1, and the liquid absorption rate and capacity retention rate were determined. Note that the temperature conditions during production, etc. were adjusted based on the difference in the water-soluble polymer.

[0114] Examples 5 to 7 Examples 5 to 7 differ from Example 4 in that the ion exchange rate of the carboxyl group of polyacrylic acid, which is the base polymer of the water-soluble polymer, was changed. The other conditions in Examples 5 to 7 were basically the same as in Example 4, and the liquid absorption rate and capacity retention rate were determined. Note that the temperature conditions during production, etc. were adjusted based on the difference in the water-soluble polymer.

[0115] Examples 8 to 13 Examples 8 to 13 differ from Example 4 in that the amount of crosslinked precursor added to the aqueous water-soluble polymer solution was changed. The amount of crosslinked precursor added to the aqueous water-soluble polymer solution corresponds to the mass ratio of the water-soluble polymer to the crosslinking agent in the binder. Other conditions in Examples 8 to 13 were basically the same as in Example 4, and the liquid absorption rate and capacity retention rate were determined.

[0116] Examples 14 to 18 Examples 14 to 18 differ from Example 4 in that the type of crosslinked precursor was changed. In Example 14, the crosslinked precursor was titanium lactate ammonium salt (manufactured by Matsumoto Fine Chemical Co., Ltd.: Orgatix TC-300). In Example 15, the crosslinked precursor was titanium lactate (manufactured by Matsumoto Fine Chemical Co., Ltd.: Orgatix TC-315). In Example 16, the crosslinked precursor was titanium triethanolamine (manufactured by Matsumoto Fine Chemical Co., Ltd.: Orgatix TC-400). In Example 17, the crosslinked precursor was titanium ethanolamine (manufactured by Matsumoto Fine Chemical Co., Ltd.: Orgatix TC-500). In Example 18, the crosslinked precursor was zirconium lactate ammonium salt (manufactured by Matsumoto Fine Chemical Co., Ltd.: Orgatix ZC-300). The other conditions in Examples 14 to 18 were basically the same as those in Example 4, and the liquid absorption rate and capacity retention rate were determined. Note that the temperature conditions during production were adjusted depending on the difference in the crosslinking agent.

[0117] Examples 19 and 20: Examples 19 and 20 differ from Example 4 in that the cations used for ion exchange were changed. 2 CO 3 The H of the carboxy group was substituted with Na. 2 CO 3 The H of the carboxy group was substituted with K using the above compound. The other conditions in Examples 19 and 20 were basically the same as in Example 4, and the liquid absorption rate and capacity retention rate were determined. Note that the temperature conditions during production and the like were adjusted depending on the water-soluble polymer.

[0118] Example 21 differs from Example 20 in that the ion exchange rate of the carboxy group of polyacrylic acid, which is the base polymer of the water-soluble polymer, was changed. The other conditions in Example 21 were basically the same as those in Example 20, and the liquid absorption rate and capacity retention rate were determined.

[0119] Examples 22 to 37 Examples 22 to 37 differ from Example 4 in that the type of crosslinked precursor was changed. In Example 22, the crosslinked precursor was chromium lactate ammonium salt. In Example 23, the crosslinked precursor was chromium lactate. In Example 24, the crosslinked precursor was chromium triethanolamine. In Example 25, the crosslinked precursor was chromium diethanolamine. In Example 26, the crosslinked precursor was manganese lactate ammonium salt. In Example 27, the crosslinked precursor was manganese lactate. In Example 28, the crosslinked precursor was manganese triethanolamine. In Example 29, the crosslinked precursor was manganese diethanolamine. In Example 30, the crosslinked precursor was cobalt lactate ammonium salt. In Example 31, the crosslinked precursor was cobalt lactate. In Example 32, the crosslinked precursor was cobalt triethanolamine. In Example 33, the crosslinked precursor was cobalt diethanolamine. In Example 34, the crosslinked precursor was nickel lactate ammonium salt. In Example 35, the crosslinked precursor was nickel lactate. In Example 36, the crosslinked precursor was nickel triethanolamine. In Example 37, the crosslinked precursor was nickel diethanolamine. Other conditions in Examples 22 to 37 were basically the same as in Example 4, and the liquid absorption rate and capacity retention rate were determined. Note that the temperature conditions during production, etc. were adjusted based on the difference in crosslinking agent.

[0120] Comparative Example 1 differs from Example 4 in that the ion exchange rate of the carboxy groups of polyacrylic acid, which is the base polymer of the water-soluble polymer, was changed, and all of the carboxy groups were ion-exchanged. Other conditions in Comparative Example 1 were basically the same as in Example 4, and the liquid absorption rate and capacity retention rate were determined.

[0121] Comparative Example 2 Comparative Example 2 differs from Example 4 in that the carboxyl groups of polyacrylic acid, which is the base polymer of the water-soluble polymer, were not ion-exchanged. Other conditions in Comparative Example 2 were basically the same as in Example 4, and the liquid absorption rate and capacity retention rate were determined.

[0122] Comparative Example 3 Comparative Example 3 differs from Example 4 in that no crosslinking precursor was added. Other conditions in Comparative Example 3 were basically the same as in Example 4, and the liquid absorption rate and capacity retention rate were determined.

[0123] The conditions and measurement results for Examples 1 to 37 and Comparative Examples 1 to 3 are summarized in Tables 1 and 2. The crosslinking agents shown in Examples 1 to 21 in Table 1 are all trade names (Orgatics) manufactured by Matsumoto Fine Chemical Co., Ltd. The amounts of crosslinking precursor added in Tables 1 and 2 correspond to parts by mass of crosslinking agent per 100 parts by mass of water-soluble polymer.

[0124]

[0125]

[0126] All of Examples 1 to 37 had excellent cycle characteristics compared to Comparative Examples 1 to 3. In contrast, Comparative Example 1 did not exhibit sufficient cycle characteristics. This is thought to be because the water-soluble polymer in the binder of Comparative Example 1 did not have a carboxyl group, so the reaction between the water-soluble polymer and the crosslinker did not proceed sufficiently. If the water-soluble polymer does not react with the crosslinker, the binder cannot form a network structure, and high strength and high elasticity are not achieved. Furthermore, in Comparative Example 2, the binder gelled, and the lithium-ion secondary battery did not operate normally. The binder of Comparative Example 2 is thought to have gelled due to the complete lack of ion exchange of the carboxyl groups in the water-soluble polymer, resulting in intramolecular crosslinking. Furthermore, Comparative Example 3 did not exhibit sufficient cycle characteristics. This is thought to be because the binder of Comparative Example 3 did not have a crosslinker, so a high-strength, high-elasticity network structure could not be formed.

[0127] REFERENCE SIGNS LIST 1 binder 2 water-soluble polymer 2A carboxy group 2B COOX group 3 cross-linking agent 4 cross-linking precursor 10 separator 20 positive electrode 22 positive electrode current collector 24 positive electrode active material layer 30 negative electrode 32 negative electrode current collector 34 negative electrode active material layer 40 power generating element 50 exterior body 52 metal foil 54 resin layer 60, 62 terminal 100 lithium ion secondary battery

Claims

1. A cured material for a lithium ion secondary battery, comprising a water-soluble polymer crosslinked with a crosslinking agent, the water-soluble polymer having a carboxy group and a COOX group formed by ion exchange of a portion of the carboxy group, and the crosslinking agent being a compound containing a metal capable of forming a hexacoordination structure.

2. The cured material for a lithium ion secondary battery according to claim 1, wherein the metal capable of forming a hexacoordination structure is any one selected from the group consisting of titanium, zirconium, chromium, manganese, cobalt, and nickel.

3. The cured material for a lithium ion secondary battery according to claim 1, wherein the metal capable of forming a hexacoordination structure is titanium or zirconium.

4. The cured material for a lithium ion secondary battery according to claim 1, wherein the ion exchange rate of the water-soluble polymer is 50% or more and less than 90%, and the ion exchange rate is a ratio of the COOX group to the sum of the carboxy group and the COOX group.

5. The cured material for a lithium ion secondary battery according to claim 1, comprising 0.1 parts by mass or more and 10 parts by mass or less of the crosslinking agent per 100 parts by mass of the water-soluble polymer.

6. 1 mol / L LiPF in a non-aqueous solvent containing ethylene carbonate and diethyl carbonate 6 2. The cured material for a lithium ion secondary battery according to claim 1, wherein the liquid absorption rate after immersion for one week in an electrolyte solution containing the above is -5% or more and less than 15%.

7. A negative electrode for a lithium ion secondary battery, comprising a negative electrode active material and the cured material for a lithium ion secondary battery according to claim 1.

8. A lithium ion secondary battery comprising the negative electrode for a lithium ion secondary battery according to claim 7, a positive electrode, and a separator disposed between the negative electrode for a lithium ion secondary battery and the positive electrode.

Citation Information

Patent Citations

  • Composition for power storage device, slurry for power storage device, separator for power storage device, power storage device electrode and power storage device

    JP2016219358A

  • Lithium ion secondary battery electrode

    JP2019091539A

  • Negative electrode agent for non-aqueous electrolyte secondary battery, negative electrode for non-aqueous electrolyte secondary battery, and non-aqueous electrolyte secondary battery

    JP6961939B2

  • Electrode mixture for non-aqueous electrolyte secondary battery

    WO2019054350A1