Electrode for secondary batteries, and secondary battery
The secondary battery electrode design with strategically placed insulating and exposed portions on the secondary battery electrodes addresses the issue of internal short circuits and electrolyte permeation, enhancing rapid charge/discharge characteristics and capacity retention.
Patent Information
- Application Number
- PCT/JP2024/018355
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-23
- Filing Date
- 2024-05-17
- Publication Date
- 2024-11-28
AI Technical Summary
Secondary battery electrodes face challenges in maintaining rapid charge/discharge characteristics due to internal short circuits caused by insulating parts at the longitudinal ends, which hinder electrolyte permeation and lead to capacity deterioration.
A wound-type secondary battery electrode design with a strip-shaped core and composite material layer, featuring a first exposed portion on the longitudinal side without the composite material layer, covered by a first insulating part, and a second exposed portion on the lateral side, allowing electrolyte permeation through a gap between the lateral exposed portion and the separator, while preventing internal short circuits.
This design effectively suppresses the deterioration of rapid charge/discharge characteristics by ensuring electrolyte access while preventing internal short circuits, thereby enhancing battery capacity retention and reducing short circuit occurrences.
Smart Images

Figure JP2024018355_28112024_PF_FP_ABST
Abstract
Description
Secondary battery electrode and secondary battery
[0001] The present disclosure relates to an electrode for a secondary battery and a secondary battery.
[0002] Secondary batteries such as lithium-ion secondary batteries are used as power sources for a wide range of devices, including electric vehicles, and there is a demand for ever higher capacity. A secondary battery has a configuration in which, for example, a wound electrode assembly in which a positive electrode and a negative electrode are wound with a separator interposed therebetween is sealed in an outer can or the like together with an electrolyte solution and the like.
[0003] For example, Patent Document 1 discloses that in a nonaqueous electrolyte secondary battery including a wound electrode body in which a positive electrode having a positive electrode composite layer provided on a strip-shaped positive electrode core and a negative electrode having a negative electrode composite layer provided on a negative electrode core are wound with a separator interposed therebetween, an exposed portion formed at an end in the longitudinal direction of the positive electrode core where the positive electrode composite layer is not provided is covered with an insulating portion.
[0004] Furthermore, for example, Patent Document 2 discloses an electrode that constitutes a wound electrode body having a strip-shaped core body and a composite layer provided on the core body, in which an exposed portion that exposes the core body surface is formed at one widthwise end of the core body, at a position away from one longitudinal end of the core body that is arranged on the outside of the winding of the electrode body, and the composite layer has a thin-walled portion in at least a part of a first region that is aligned with the exposed portion in the longitudinal direction of the core body, and whose layer thickness is thinner than a second region that is a region other than the first region.
[0005] JP 2008-204920 A International Publication No. 2017 / 077698
[0006] In positive and negative electrodes, covering the exposed portions formed at the longitudinal ends of the core with an insulating portion can prevent internal short circuits caused by the separation of the composite layer or by the pressing force acting when the electrode is wound. However, providing an insulating portion at the longitudinal end of the core causes the insulating portion to adhere to the separator facing the insulating portion, making it difficult for the electrolyte to penetrate into the composite layer from the longitudinal end of the electrode, thereby degrading rapid charge / discharge characteristics.
[0007] Therefore, an object of the present disclosure is to provide a secondary battery electrode and a secondary battery that can suppress the deterioration of rapid charge / discharge characteristics.
[0008] The present disclosure relates to an electrode for a secondary battery that constitutes a wound electrode body having a strip-shaped core body and a composite layer arranged on the core body, characterized in that a first longitudinal side exposed portion on which the composite layer is not arranged is provided at one longitudinal end of the core body, and the first longitudinal side exposed portion is covered by a first insulating portion, and a short side exposed portion on which the composite layer is not arranged is provided at one short end of the core body, at a position away from both longitudinal ends of the core body.
[0009] The present disclosure also provides a secondary battery having a wound electrode body in which a positive electrode and a negative electrode are wound with a separator interposed therebetween, and at least one of the positive electrode and the negative electrode is an electrode for the secondary battery.
[0010] According to the present disclosure, it is possible to provide a secondary battery electrode and a secondary battery capable of suppressing deterioration in rapid charge / discharge characteristics.
[0011] Fig. 2 is a schematic cross-sectional view of a secondary battery that is an example of an embodiment. Fig. 3 is a schematic plan view showing an example of the configuration of an electrode for a secondary battery. Fig. 4 is a schematic cross-sectional view of an electrode for a secondary battery taken along line AA in Fig. 2. Fig. 5 is a schematic plan view showing another example of the configuration of an electrode for a secondary battery.
[0012] An example of an embodiment of a secondary battery according to the present disclosure will be described in detail below.
[0013] Fig. 1 is a cross-sectional view of a secondary battery according to an embodiment. The secondary battery 10 shown in Fig. 1 includes a wound electrode assembly 14 formed by winding a positive electrode 11 and a negative electrode 12 with a separator 13 interposed therebetween, an electrolyte, insulating plates 18 and 19 disposed above and below the electrode assembly 14, and a battery case 15 for accommodating the above components. The battery case 15 is composed of a cylindrical case body 16 with a bottom and a sealing body 17 that closes the opening of the case body 16. Examples of the battery case 15 include a cylindrical or rectangular metal case, a resin case formed by laminating a resin sheet (a so-called laminate type), and the like.
[0014] The electrolyte solution is, for example, an electrolyte solution having lithium ion conductivity. The electrolyte solution is, for example, a non-aqueous electrolyte solution containing a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. Examples of the non-aqueous solvent include esters, ethers, nitriles, amides, and mixed solvents of two or more of these. Examples of the non-aqueous solvent include ethylene carbonate (EC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), diethyl carbonate (DEC), and mixed solvents of these. The non-aqueous solvent may contain a halogen-substituted compound (e.g., fluoroethylene carbonate) in which at least a portion of the hydrogen atoms of these solvents are substituted with halogen atoms such as fluorine. The electrolyte salt may be, for example, LiPF 6 The non-aqueous electrolyte is just an example, and an aqueous electrolyte may be used if applicable.
[0015] The case body 16 is, for example, a cylindrical metal container with a bottom. A gasket 28 is provided between the case body 16 and the sealing body 17 to ensure airtightness inside the battery. The case body 16 has, for example, a protruding portion 22, which is a portion of the side surface that protrudes inward and supports the sealing body 17. The protruding portion 22 is preferably formed in an annular shape along the circumferential direction of the case body 16, and supports the sealing body 17 on its upper surface.
[0016] The sealing body 17 has a structure in which a filter 23, a lower valve body 24, an insulating member 25, an upper valve body 26, and a cap 27 are stacked in this order from the electrode body 14 side. Each component constituting the sealing body 17 has, for example, a disk or ring shape, and all components except for the insulating member 25 are electrically connected to each other. The lower valve body 24 and the upper valve body 26 are connected to each other at their respective centers, and the insulating member 25 is interposed between their respective peripheral edges. If the internal pressure of the secondary battery 10 increases due to heat generation caused by an internal short circuit or the like, for example, the lower valve body 24 may deform and rupture, pushing the upper valve body 26 toward the cap 27, thereby interrupting the current path between the lower valve body 24 and the upper valve body 26. If the internal pressure further increases, the upper valve body 26 may rupture, and gas may be discharged from the opening of the cap 27.
[0017] In the secondary battery 10 shown in Fig. 1, a positive electrode lead 20 attached to the positive electrode 11 passes through a through-hole in the insulating plate 18 and extends toward the sealing body 17, and a negative electrode lead 21 attached to the negative electrode 12 passes outside the insulating plate 19 and extends toward the bottom side of the case body 16. The positive electrode lead 20 is connected by welding or the like to the underside of a filter 23, which is the bottom plate of the sealing body 17, and a cap 27, which is the top plate of the sealing body 17 and is electrically connected to the filter 23, serves as the positive electrode terminal. The negative electrode lead 21 is connected by welding or the like to the inner bottom surface of the case body 16, and the case body 16 serves as the negative electrode terminal.
[0018] The separator 13 may be, for example, a porous sheet having ion permeability and insulating properties. Specific examples of porous sheets include a microporous thin film, a woven fabric, and a nonwoven fabric. Suitable materials for the separator include olefin-based resins such as polyethylene and polypropylene, and cellulose. The separator 13 may be a laminate having a cellulose fiber layer and a thermoplastic resin fiber layer such as an olefin-based resin. Alternatively, the separator 13 may be a multilayer separator including a polyethylene layer and a polypropylene layer, and the surface of the separator 13 may be coated with a material such as an aramid-based resin or ceramic.
[0019] The following describes electrodes for secondary batteries that are applied to at least one of the positive electrode 11 and the negative electrode 12. The following electrodes for secondary batteries are preferably applied to the positive electrode.
[0020] Fig. 2 is a schematic plan view showing an example of the configuration of a secondary battery electrode, and Fig. 3 is a schematic cross-sectional view of the secondary battery electrode taken along line A-A in Fig. 2. The secondary battery electrode 30 shown in Figs. 2 and 3 is in a state before being wound. In Fig. 2, in order to clarify the configuration of the secondary battery electrode 30, a first insulating portion 38 and a second insulating portion 42, which will be described later, are shown in a see-through view and indicated by dashed lines.
[0021] 2 (the direction of arrow X) is the winding direction of the electrode body 14, and the short side of the secondary battery electrode 30 (the direction of arrow Y, the width direction of the secondary battery electrode 30) is the winding axis direction of the electrode body 14. Note that one end side of the secondary battery electrode 30 in the longitudinal direction may be the winding start side of the electrode, and the other end side of the secondary battery electrode 30 in the longitudinal direction may be the winding end side of the electrode, or one end side of the secondary battery electrode 30 in the longitudinal direction may be the winding end side of the electrode, and the other end side of the secondary battery electrode 30 in the longitudinal direction may be the winding start side of the electrode.
[0022] 3, the secondary battery electrode 30 includes a strip-shaped core body 32 and a composite layer 34 disposed on the strip-shaped core body 32. The composite layer 34 may be provided on both sides of the core body 32, as shown in FIG.
[0023] When the secondary battery electrode 30 is applied to the negative electrode 12, the negative electrode core corresponding to the core 32 can be, for example, a foil of a metal such as copper or a copper alloy that is stable in the potential range of the negative electrode 12, or a film with such a metal disposed on the surface layer. When the secondary battery electrode 30 is applied to the positive electrode 11, the positive electrode core corresponding to the core 32 can be, for example, a foil of a metal such as aluminum that is stable in the potential range of the positive electrode 11, or a film with such a metal disposed on the surface layer.
[0024] The mixture layer 34 includes, for example, an active material, a binder, a conductive material, etc. The mixture layer 34 is formed by applying a mixture slurry including the active material, the binder, the conductive material, etc. onto the core 32 and compressing the applied slurry.
[0025] When the secondary battery electrode 30 is applied to the negative electrode 12, the negative electrode composite layer corresponding to the composite layer 34 contains, for example, a negative electrode active material. Examples of the negative electrode active material include materials that can reversibly absorb and release lithium ions, such as carbon materials such as natural graphite and artificial graphite, metals such as Si and Sn, alloys, or oxides. When the secondary battery electrode 30 is applied to the positive electrode 11, the positive electrode composite layer corresponding to the composite layer 34 contains, for example, a positive electrode active material. Examples of the positive electrode active material include lithium transition metal oxides containing transition metal elements such as Co, Mn, and Ni. Examples of the lithium transition metal oxides include, for example, Li x CoO 2 , Li x NiO 2 , Li x MnO 2 , Li x Co y Ni 1-y O 2 , Li x Co y M 1-y O z , Li x Ni 1-y M y O z , Li x Mn 2 O 4 , Li x Mn 2-y M y O 4 , LiMPO 4 , Li 2 MPO 4 F (M: at least one of Na, Mg, Sc, Y, Mn, Fe, Co, Ni, Cu, Zn, Al, Cr, Pb, Sb, and B, 0<x≦1.2, 0<y≦0.9, 2.0≦z≦2.3). These may be used alone or in combination.
[0026] Examples of binders contained in the composite layer 34 include fluorine-based resins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVDF), polyacrylonitrile (PAN), polyimide-based resins, acrylic-based resins, polyolefin-based resins, styrene-butadiene rubber (SBR), carboxymethyl cellulose (CMC) or a salt thereof, polyacrylic acid (PAA) or a salt thereof, polyvinyl alcohol (PVA), and polyethylene oxide (PEO).
[0027] Examples of the conductive material contained in the composite layer 34 include carbon materials such as carbon black (CB), acetylene black (AB), ketjen black, carbon nanotubes (CNT), graphene, and graphite.
[0028] As shown in Figures 2 and 3, a first longitudinal exposed portion 36 where no composite layer 34 is disposed is provided at one longitudinal end of the core body 32. The first longitudinal exposed portion 36 may be provided on one side of the core body 32, or as shown in Figure 3, it may be provided on both sides of the core body 32. A first insulating portion 38 covering the first longitudinal exposed portion 36 is disposed at one longitudinal end of the core body 32. This makes it possible to prevent internal short circuits caused by the composite layer 34 falling off or by pressure acting when the electrodes are wound. Note that it is desirable for the first insulating portion 38 to cover not only the first longitudinal exposed portion 36 but also one longitudinal end of the composite layer 34.
[0029] 2 and 3, a second longitudinal exposed portion 40 where the composite layer 34 is not disposed is preferably also provided at the other longitudinal end of the core 32. The second longitudinal exposed portion 40 may be provided on one side of the core 32, or as shown in FIG. 3, it may be provided on both sides of the core 32. A second insulating portion 42 covering the second longitudinal exposed portion is preferably provided at the other longitudinal end of the core 32. This further reduces the occurrence of internal short circuits due to the detachment of the composite layer 34 or the pressing force acting when winding the electrodes. It is desirable that the second insulating portion 42 cover not only the second longitudinal exposed portion 40 but also the other longitudinal end of the composite layer 34.
[0030] 2 , a short-side exposed portion 44 where the composite layer 34 is not disposed is provided at one end in the short direction (width direction) of the core 32, at a position away from both ends in the longitudinal direction of the core 32. A plurality of short-side exposed portions 44 may be provided at a predetermined interval in the longitudinal direction of the core 32, or only one short-side exposed portion 44 may be provided. In this embodiment, it is sufficient that the short-side exposed portion 44 is provided at one end in the short direction of the core 32, but the short-side exposed portions 44 may also be provided at both ends in the short direction of the core 32. Furthermore, the short-side exposed portion 44 may be provided on one side of the core 32 or on both sides of the core 32.
[0031] As described above, the occurrence of internal short circuits can be suppressed by covering the exposed portions at the longitudinal ends of the core 32 with insulating portions. However, this also makes it difficult for the electrolyte to penetrate from the longitudinal ends of the electrode into the composite layer 34, which raises concerns about a deterioration in rapid charge / discharge characteristics. However, in this embodiment, by providing the lateral side exposed portions 44 at the lateral ends of the core 32, a gap is formed between the lateral side exposed portions 44 and the separator 13, ensuring a path for the electrolyte to penetrate from the lateral ends of the electrode into the composite layer 34. This suppresses a deterioration in rapid charge / discharge characteristics.
[0032] The ratio (W2 / W1) of the widthwise length (W2) of the short-side exposed portion 44 along the short-side direction of the core 32 to the short-side length (W1) of the core 32 is, for example, preferably 0.6 to 0.99, and more preferably 0.5 to 0.9, in order to increase the capacity of the battery. The length (W3) of the short-side exposed portion 44 in the direction perpendicular to the widthwise direction is not particularly limited, but is preferably, for example, 1 / 3 to 2 times the widthwise length (W2) of the short-side exposed portion 44.
[0033] The first longitudinal side exposed portion 36, the second longitudinal side exposed portion 40, and the short side exposed portion 44 may be formed by applying a composite layer 34 onto the core body 32 and then removing a portion of the composite layer 34 to expose a portion of the core body 32, or by intermittently applying a composite slurry onto the core body 32 to expose a portion of the core body 32.
[0034] The first insulating portion 38 and the second insulating portion 42 may be made of a non-conductive material, such as a sheet, tape, or coating of a polyolefin resin such as polyethylene, polypropylene, or polybutylene, a polyester resin such as polyvinyl chloride or polyethylene terephthalate, or a resin such as polyimide, polyamide, or polyphenylene sulfide.
[0035] FIG. 4 is a schematic cross-sectional view of the secondary battery electrode taken along line B-B in FIG. 2 . As shown in FIGS. 2 and 4 , the composite layer 34 has a first region 46 aligned with the short-side exposed portion 44 in the longitudinal direction of the core 32, and a second region 48 other than the first region 46. As shown in FIG. 2 , the first region 46 is aligned with the short-side exposed portion 44 in the longitudinal direction of the core 32 and overlaps with the short-side exposed portion 44 in the longitudinal direction of the core 32. The region that overlaps even partially with the short-side exposed portion 44 in the longitudinal direction of the core 32 is the first region 46. The second region 48 is not aligned with the short-side exposed portion 44 in the longitudinal direction of the core 32 and does not overlap with the short-side exposed portion 44 in the longitudinal direction. The first region 46 and the second region 48 may be formed on both sides of the core 32 or on one side of the core 32.
[0036] 4, the composite layer thickness (V1) of first region 46 is preferably thinner than the composite layer thickness (V2) of second region 48. By making the composite layer thickness (V1) of first region 46 thinner than the composite layer thickness (V2) of second region 48, the electrolyte can more easily permeate from the short-side ends of secondary battery electrode 30 into composite layer 34, further suppressing the deterioration of rapid charge / discharge characteristics.
[0037] The ratio (V1 / V2) of the composite layer thickness (V1) in the first region 46 to the composite layer thickness (V2) in the second region 48 is preferably 0.99 or less, and more preferably 0.7 to 0.99, in order to further suppress deterioration of rapid charge / discharge characteristics. The composite layer thickness can be measured using a contact thickness gauge. The composite layer thickness is the average of the thickness measurements at 20 arbitrary locations in the region to be measured.
[0038] One example of a method for forming the first region 46 and the second region 48 is to apply a smaller amount of composite slurry to the core 32 in the first region 46 than in the second region 48. As a result, if the compression conditions for each region after the composite slurry application are the same, the densities of the regions can be made approximately the same, and the composite layer thickness in the first region 46 can be made thinner than the composite layer thickness in the second region 48. Another example of a method for forming the first region 46 and the second region 48 is to roll the coating film after the composite slurry application more strongly in the first region 46 than in the second region 48. As a result, if the coating amounts of the first region 46 and the second region 48 are the same, the density of the first region 46 can be made higher than the density of the second region 48, and the composite layer thickness in the first region 46 can be made thinner than the composite layer thickness in the second region 48.
[0039] Fig. 5 is a schematic plan view showing another example of the configuration of a secondary battery electrode. In the secondary battery electrode 30a in Fig. 5, components similar to those in the secondary battery electrode 30 shown in Fig. 2 are designated by the same reference numerals, and their description will be omitted. In Fig. 5, in order to clarify the configuration of the secondary battery electrode 30a, the first insulating portion 38, the second insulating portion 42, and a third insulating portion 50 (described later) are shown in a see-through view with dashed lines.
[0040] As shown in FIG. 5 , a third insulating portion 50 is provided at one lateral end of the core 32, covering the lateral side exposed portion 44 where the composite layer 34 is not disposed. The third insulating portion 50 may not only cover the lateral side exposed portion 44 but also the composite layer 34 surrounding the lateral side exposed portion 44. Providing the third insulating portion 50 can further suppress the occurrence of internal short circuits. Furthermore, when the third insulating portion 50 is provided, a gap is formed between the lateral end of the secondary battery electrode 30 where the third insulating portion 50 is not disposed and the separator 13, ensuring a path for the electrolyte to permeate from the lateral end of the secondary battery electrode 30 to the composite layer 34. This suppresses degradation of rapid charge / discharge characteristics. The third insulating portion 50 may be made of the same material as the first insulating portion 38 and the second insulating portion 42.
[0041] The present disclosure will be further described below with reference to examples, but the present disclosure is not limited to these examples.
[0042] Example 1 [Preparation of Positive Electrode] 100 parts by mass of LiCoO 2 1 part by mass of acetylene black (AB) and 0.9 parts by mass of polyvinylidene fluoride (PVDF) were mixed, and an appropriate amount of N-methyl-2-pyrrolidone (NMP) was added to prepare a positive electrode composite slurry. Next, the positive electrode composite slurry was coated on both sides of a 15 μm thick aluminum foil, and after drying the coating, the coating was rolled using a roller. When coating the positive electrode composite slurry on the aluminum foil, intermittent coating was performed to form a first exposed portion on the longitudinal side at the start of winding and three exposed portions on the lateral side. The ratio (W2 / W1) of the width direction length (W2) of the exposed portion on the lateral side to the length (W1) of the lateral side of the aluminum foil was set to 0.9. In addition, the ratio (V1 / V2) of the thickness (V1) of the positive electrode composite layer in the first region to the thickness (V2) of the positive electrode composite layer in the second region was set to 1. In all examples, the thickness of the positive electrode composite layer in each region was adjusted by changing the coating amount of the positive electrode composite slurry in each region.
[0043] A polyethylene terephthalate tape serving as a first insulating portion was attached to the obtained positive electrode so as to cover the first exposed portion on the longitudinal direction side, as shown in FIG.
[0044] [Preparation of Negative Electrode] 100 parts by mass of graphite powder, 1 part by mass of carboxymethyl cellulose sodium (CMC-Na), and 1 part by mass of a dispersion of styrene butadiene rubber (SBR) were mixed, and an appropriate amount of water was added to prepare a negative electrode composite slurry. Next, the negative electrode composite slurry was applied to both sides of a copper foil with a thickness of 8 μm, and the coating was dried. Then, a negative electrode was prepared by rolling the coating using a roller.
[0045] [Preparation of Non-Aqueous Electrolyte] 5 parts by mass of vinylene carbonate (VC) was added to 100 parts by mass of a mixed solvent in which ethylene carbonate (EC) and dimethyl carbonate (DMC) were mixed in a volume ratio of 3:7, and lithium hexafluorophosphate (LiPF 6 ) was dissolved in a concentration of 1.5 mol / L to prepare a non-aqueous electrolyte solution.
[0046] [Preparation of Secondary Battery] A positive electrode lead was attached to the positive electrode, and a negative electrode lead was attached to the negative electrode. The positive and negative electrodes were then wound with a separator interposed therebetween to prepare a wound electrode body. Insulating plates were placed above and below the electrode body, and the electrode body was housed in a case body. The negative electrode lead was welded to the bottom of the case body, and the positive electrode lead was welded to a sealing member. After injecting a nonaqueous electrolyte into the case body, the opening of the case body was sealed with a sealing member via a gasket to prepare a secondary battery.
[0047] Example 2 A secondary battery was produced in the same manner as in Example 1, except that in producing the positive electrode, a second longitudinal exposed portion at the winding end side and three lateral exposed portions were formed as exposed portions, and a polyethylene terephthalate tape, which served as a second insulating portion, was attached so as to cover the second longitudinal exposed portions.
[0048] Example 3 A secondary battery was produced in the same manner as in Example 1, except that in producing the positive electrode, a first exposed portion on the longitudinal side at the winding start side, a second exposed portion on the longitudinal side at the winding end side, and three exposed portions on the lateral side were formed as exposed portions, a polyethylene terephthalate tape serving as a first insulating portion was attached to cover the first exposed portion on the longitudinal side, and a polyethylene terephthalate tape serving as a second insulating portion was attached to cover the second exposed portion on the longitudinal side.
[0049] Example 4 A secondary battery was fabricated in the same manner as in Example 3, except that in fabricating the positive electrode, the ratio (V1 / V2) of the thickness (V1) of the positive electrode composite layer in the first region to the thickness (V2) of the positive electrode composite layer in the second region was set to 1.05.
[0050] Example 5 A secondary battery was fabricated in the same manner as in Example 3, except that in fabricating the positive electrode, the ratio (V1 / V2) of the thickness (V1) of the positive electrode composite layer in the first region to the thickness (V2) of the positive electrode composite layer in the second region was set to 0.995.
[0051] Example 6 A secondary battery was fabricated in the same manner as in Example 3, except that in fabricating the positive electrode, the ratio (V1 / V2) of the thickness (V1) of the positive electrode composite layer in the first region to the thickness (V2) of the positive electrode composite layer in the second region was set to 0.95.
[0052] Example 7 A secondary battery was fabricated in the same manner as in Example 3, except that in fabricating the positive electrode, the ratio (V1 / V2) of the thickness (V1) of the positive electrode composite layer in the first region to the thickness (V2) of the positive electrode composite layer in the second region was set to 0.9.
[0053] Example 8 A secondary battery was fabricated in the same manner as in Example 3, except that in fabricating the positive electrode, the ratio (V1 / V2) of the thickness (V1) of the positive electrode composite layer in the first region to the thickness (V2) of the positive electrode composite layer in the second region was set to 0.7.
[0054] Example 9 A secondary battery was fabricated in the same manner as in Example 3, except that in fabricating the positive electrode, the ratio (V1 / V2) of the thickness (V1) of the positive electrode composite layer in the first region to the thickness (V2) of the positive electrode composite layer in the second region was set to 0.6.
[0055] Example 10 A secondary battery was fabricated in the same manner as in Example 3, except that in fabricating the positive electrode, the ratio (V1 / V2) of the thickness (V1) of the positive electrode composite layer in the first region to the thickness (V2) of the positive electrode composite layer in the second region was set to 0.5.
[0056] Example 11 A secondary battery was produced in the same manner as in Example 6, except that in producing the positive electrode, the ratio (W2 / W1) of the length in the width direction (W2) of the short-side exposed portion to the length in the short-side direction (W1) of the aluminum foil was set to 0.99.
[0057] Example 12 A secondary battery was produced in the same manner as in Example 6, except that in producing the positive electrode, the ratio (W2 / W1) of the width direction length (W2) of the short-side exposed portion to the short-side length (W1) of the aluminum foil was set to 0.8.
[0058] Example 13 A secondary battery was produced in the same manner as in Example 6, except that in producing the positive electrode, the ratio (W2 / W1) of the width direction length (W2) of the short-side exposed portion to the short-side length (W1) of the aluminum foil was set to 0.6.
[0059] Example 14 A secondary battery was produced in the same manner as in Example 6, except that in producing the positive electrode, the ratio (W2 / W1) of the length in the width direction (W2) of the short-side exposed portion to the length in the short-side direction (W1) of the aluminum foil was set to 0.5.
[0060] Comparative Example 1 A secondary battery was produced in the same manner as in Example 1, except that in producing the positive electrode, a first exposed portion on the longitudinal side at the winding start side and a second exposed portion on the longitudinal side at the winding end side were formed as exposed portions, a polyethylene terephthalate tape serving as a first insulating portion was attached to cover the first exposed portion on the longitudinal side, and a polyethylene terephthalate tape serving as a second insulating portion was attached to cover the second exposed portion on the longitudinal side.
[0061] [Rapid Charge / Discharge Test] The secondary batteries of each Example and Comparative Example were charged at a constant current of 1.5 C in an environment of 25° C. until the battery voltage reached 4.2 V, and then discharged at a constant current of 1.5 C until the battery voltage reached 2.7 V. This charge / discharge cycle was repeated 300 times, and the capacity retention rate was calculated using the following formula. The results are shown in Table 1. A higher capacity retention rate indicates that the deterioration of the rapid charge / discharge characteristics was more suppressed. Capacity retention rate (%) = (discharge capacity at 300th cycle / discharge capacity at 1st cycle) × 100
[0062] [Short-Circuit Test] The secondary batteries of each Example and Comparative Example were charged at a constant current of 0.5 C in an environment of 60° C. until the battery voltage reached 4.2 V, and then stored in that state for one month in an environment of 60° C. An internal short-circuit accelerated test was performed. The number of batteries that experienced an internal short circuit out of 50 tested batteries was counted. The results are summarized in Table 1.
[0063]
[0064] In Examples 1 to 14, the number of short circuits that occurred was equivalent to that of Comparative Example 1, and the capacity retention rate in the rapid charge-discharge test was higher than that of Comparative Example 1. From these results, it can be said that in an electrode in which the longitudinal exposed portion of the core is covered with an insulating portion, by providing a lateral exposed portion on which no composite layer is disposed at one lateral end of the core, at a position away from both longitudinal ends of the core, it is possible to suppress the deterioration of rapid charge-discharge characteristics.
[0065] [Notes] (1) A secondary battery electrode constituting a wound electrode body including a strip-shaped core and a composite layer disposed on the core, wherein a first longitudinal exposed portion where the composite layer is not disposed is provided at one longitudinal end of the core, and the first longitudinal exposed portion is covered with a first insulating portion, and a second longitudinal exposed portion where the composite layer is not disposed is provided at one lateral end of the core, at a position away from both longitudinal ends of the core. (2) The secondary battery electrode according to (1) above, wherein a second longitudinal exposed portion where the composite layer is not disposed is provided at the other longitudinal end of the core, and the second longitudinal exposed portion is covered with a second insulating portion. (3) The electrode for a secondary battery according to (1) or (2) above, wherein the composite layer has a first region aligned with the short-side exposed portion in the longitudinal direction of the core and a second region other than the first region, and wherein the composite layer thickness (V1) of the first region is thinner than the composite layer thickness (V2) of the second region. (4) The electrode for a secondary battery according to (4) above, wherein the ratio (V1 / V2) of the composite layer thickness (V1) of the first region to the composite layer thickness (V2) of the second region is 0.99 or less. (5) The electrode for a secondary battery according to any one of (1) to (4) above, wherein the ratio (W2 / W1) of the width direction length (W2) of the short-side exposed portion along the short direction of the core to the length (W1) of the core in the short direction is 0.6 or more and 0.99 or less. (6) The electrode for a secondary battery according to (4) above, wherein a ratio (V1 / V2) of the thickness of the composite layer in the first region (V1) to the thickness of the composite layer in the second region (V2) is 0.7 or more and 0.99 or less. (7) A secondary battery having a wound electrode body in which a positive electrode and a negative electrode are wound with a separator interposed therebetween, wherein at least one of the positive electrode and the negative electrode is the electrode for a secondary battery according to any one of (1) to (6) above.
[0066] 10 Secondary battery, 11 Positive electrode, 12 Negative electrode, 13 Separator, 14 Electrode body, 15 Battery case, 16 Case body, 17 Sealing body, 18 Insulating plate, 18, 19 Insulating plate, 20 Positive electrode lead, 21 Negative electrode lead, 22 Protruding portion, 23 Filter, 24 Lower valve body, 25 Insulating member, 26 Upper valve body, 27 Cap, 28 Gasket, 30, 30a Secondary battery electrode, 32 Core body, 34 Composite layer, 36 First longitudinal exposed portion, 38 First insulating portion, 40 Second longitudinal exposed portion, 42 Second insulating portion, 44 Short-side exposed portion, 46 First region, 48 Second region, 50 Third insulating portion.
Claims
1. An electrode for a secondary battery constituting a wound-type electrode body having a band-shaped core body and a composite layer arranged on the core body, wherein one longitudinal end of the core body has a first longitudinal side exposed portion on which the composite layer is not arranged, and the first longitudinal side exposed portion is covered by a first insulating portion, and one lateral end of the core body has a lateral side exposed portion on which the composite layer is not arranged, located away from both longitudinal ends of the core body.
2. An electrode for a secondary battery as described in claim 1, wherein the other longitudinal end of the core body has a second longitudinal side exposed portion on which the composite layer is not arranged, and the second longitudinal side exposed portion is covered by a second insulating portion.
3. An electrode for a secondary battery as described in claim 1 or 2, wherein the composite layer has a first region aligned with the short-side exposed portion in the longitudinal direction of the core body, and a second region which is a region other than the first region, and the composite layer thickness (V1) of the first region is thinner than the composite layer thickness (V2) of the second region.
4. An electrode for a secondary battery as described in claim 3, wherein the ratio (V1 / V2) of the composite layer thickness (V1) in the first region to the composite layer thickness (V2) in the second region is 0.99 or less.
5. An electrode for a secondary battery as described in claim 1 or 2, wherein the ratio (W2 / W1) of the widthwise length (W2) of the short-side exposed portion along the short direction of the core body to the short-side length (W1) of the core body is 0.6 or more and 0.99 or less.
6. An electrode for a secondary battery as described in claim 4, wherein the ratio (V1 / V2) of the composite layer thickness (V1) in the first region to the composite layer thickness (V2) in the second region is 0.7 or more and 0.99 or less.
7. A secondary battery having a wound electrode body in which a positive electrode and a negative electrode are wound with a separator interposed therebetween, wherein at least one of the positive electrode and the negative electrode is an electrode for a secondary battery according to claim 1 or 2.
Citation Information
Patent Citations
Nonaqueous electrolyte secondary battery, and manufacturing method of nonaqueous electrolyte secondary battery
JP2008204920A
Electrode plate for power storage device and power storage device
WO2017077698A1
Nonaqueous secondary battery
JP2005285691A
Electrode for non-aqueous electrolyte secondary battery, and non-aqueous electrolyte secondary battery
WO2018079291A1
Battery
WO2020209176A1