Negative electrode active material for secondary battery, and secondary battery

By optimizing the surface concentration of element A1 in silicon-containing particles within secondary batteries, the challenges of achieving both high rate and cycle characteristics are addressed, resulting in improved lithium ion diffusion and reduced particle cracking, enhancing battery performance and stability.

WO2024242105A1PCT designated stage expired Publication Date: 2024-11-28PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/018678
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-24
Filing Date
2024-05-21
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Secondary batteries using silicon-based materials face challenges in achieving both excellent rate characteristics and cycle characteristics due to issues with particle cracking and reactivity.

Method used

The development of silicon-containing particles with an ion-conducting phase and a silicon phase, where the concentration of element A1 (such as alkali metals or Group 2 elements) is higher on the surface than inside, improving reactivity and reducing particle cracking by forming a conductive layer and optimizing the composition and structure of the composite particles.

Benefits of technology

This approach enhances both the rapid charge/discharge capabilities and the cycle stability of secondary batteries by promoting lithium ion diffusion and reducing structural stress, thereby maintaining high capacity and performance over cycles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024018678_28112024_PF_FP_ABST
    Figure JP2024018678_28112024_PF_FP_ABST
Patent Text Reader

Abstract

This negative electrode active material for a secondary battery comprises silicon-containing particles containing an ion conductive phase, and a silicon phase dispersed in the ion conductive phase. The silicon-containing particles contain lithium and an element A1. The concentration of the element A1 is larger in the surface part than the inside of the silicon-containing particle, and the element A1 is at least one selected from the group consisting of an alkali metal element other than lithium and a group 2 element of the long-period periodic table.
Need to check novelty before this filing date? Find Prior Art

Description

Negative electrode active material for secondary battery and secondary battery

[0001] The present disclosure relates to a negative electrode active material for a secondary battery and a secondary battery.

[0002] The negative electrode of a secondary battery, such as a lithium-ion secondary battery, uses a negative electrode active material capable of absorbing and releasing lithium ions, and graphite is generally used as such a negative electrode active material. In recent years, silicon-containing materials, which have a higher capacity density than graphite, have been investigated as a negative electrode active material.

[0003] Patent Document 1 proposes "a negative electrode active material for a secondary battery, comprising silicate composite particles containing a silicate phase and silicon particles dispersed in the silicate phase, the silicate phase being an oxide phase containing Si, O, and an alkali metal, the alkali metal containing at least K and Li."

[0004] International Publication No. 2020 / 045256

[0005] Secondary batteries using silicon-containing materials are required to have both excellent rate characteristics and cycle characteristics.

[0006] In view of the above, one aspect of the present disclosure relates to a negative electrode active material for a secondary battery, comprising silicon-containing particles including an ion-conducting phase and a silicon phase dispersed within the ion-conducting phase, the silicon-containing particles including lithium and an element A1, the concentration of the element A1 being higher at the surface of the silicon-containing particles than at the interior thereof, and the element A1 being at least one element selected from the group consisting of alkali metal elements other than lithium and Group 2 elements of the long form periodic table.

[0007] Yet another aspect of the present disclosure relates to a secondary battery including a positive electrode, a negative electrode, and an electrolyte, wherein the negative electrode contains the above-described negative electrode active material for a secondary battery.

[0008] According to the present disclosure, it is possible to simultaneously achieve excellent rate characteristics and cycle characteristics for a secondary battery.

[0009] The novel features of the present invention are set forth in the appended claims, but the present invention, both in terms of structure and content, together with other objects and features of the present invention, will be better understood from the following detailed description taken in conjunction with the drawings.

[0010] 1 is a cross-sectional view schematically illustrating an example of a negative electrode active material (silicon-containing particles) according to an embodiment of the present disclosure; 2 is a schematic perspective view of a secondary battery according to an embodiment of the present disclosure, with a portion cut away;

[0011] The following describes embodiments of the present disclosure using examples, but the present disclosure is not limited to the examples described below. In the following description, specific numerical values ​​and materials may be exemplified, but other numerical values ​​and materials may be applied as long as the effects of the present disclosure are obtained. In this specification, the term "numerical value A to numerical value B" includes numerical value A and numerical value B and can be read as "numerical value A or more and numerical value B or less." In the following description, when lower and upper limits are exemplified for numerical values ​​of specific physical properties or conditions, any of the exemplified lower limits and any of the exemplified upper limits can be arbitrarily combined, as long as the lower limit is not equal to or greater than the upper limit. When multiple materials are exemplified, one of the materials may be selected and used alone, or two or more materials may be used in combination.

[0012] A negative electrode active material for a secondary battery according to one embodiment of the present disclosure includes silicon-containing particles. The silicon-containing particles include an ion-conducting phase and a silicon phase dispersed within the ion-conducting phase. The silicon-containing particles include lithium (Li) and element A1. The concentration of element A1 is higher at the surface of the silicon-containing particles than in the interior. Element A1 is at least one element selected from the group consisting of alkali metal elements other than lithium and Group 2 elements of the long form periodic table. Hereinafter, the silicon-containing particles are also referred to as "composite particles." Silicon is also referred to as "silicon" or "Si."

[0013] The composite particles may contain one or more types of element A1. When the composite particles contain multiple types of element A1, the total concentration of the multiple types is higher at the surface of the composite particles than at the interior. In this case, the concentrations of each of the multiple types may be higher at the surface of the composite particles than at the interior.

[0014] The ion-conducting phase may include, for example, at least one selected from the group consisting of a silicate phase and a silicon oxide phase. Hereinafter, at least one of the silicate phase and the silicon oxide phase is also referred to as a "silicon compound phase." The silicon compound phase may form an amorphous phase. Composite particles in which a silicon phase is dispersed within a silicate phase are also referred to as "silicate phase-containing composite particles." Silicate phase-containing composite particles in which the silicate phase is a lithium silicate phase are also referred to as "lithium silicate phase-containing composite particles." Composite particles in which a silicon phase is dispersed within a silicon oxide phase are also referred to as "silicon oxide phase-containing composite particles."

[0015] When the composite particles contain Li and the element A1 and the concentration of the element A1 is higher at the surface portion than at the interior portion of the composite particles, the reactivity of the composite particles is significantly improved, and the rate characteristics (rapid charge / discharge characteristics) are significantly improved by improving the overvoltage. By efficiently adding a small amount of the element A1 to the surface side of the composite particles, the reactivity of the composite particles can be significantly improved.

[0016] Although the detailed mechanism by which the reactivity of the composite particles is improved is unknown, it is speculated as follows: The presence of a large amount of element A1, which has a large ionization tendency, on the surface side of the composite particles promotes desolvation of Li ions on the surface of the composite particles. The presence of a large amount of element A1, which has a larger ionic radius than Li, on the surface side of the composite particles causes distortion in the amorphous structure of the ion-conducting phase on the surface of the composite particles, thereby improving the diffusion rate of Li ions inside the composite particles. It is speculated that these factors improve the reactivity of the composite particles (the reactivity of Li with the ion-conducting phase).

[0017] It can also be said that the composite particles of the present disclosure have a lower concentration of element A1 in the interior than in the surface. When the reactivity of a silicon-containing material is improved, particle cracking tends to occur during charging and discharging, and the active surface formed by the particle cracking comes into contact with the electrolyte, causing side reactions and resulting in a decrease in cycle performance. In contrast, in the composite particles of the present disclosure, the reactivity is improved by increasing the concentration of element A1 in the particle surface, but the concentration of element A1 is reduced inside the particles, which can suppress particle cracking and the resulting decrease in cycle performance. In other words, the present disclosure can achieve both excellent rate performance and cycle performance.

[0018] (Element A1 and Lithium) The element A1 and lithium are contained in the ion conductive phase. The element A1 and lithium are contained in the ion conductive phase including the case where the element A1 and lithium are present at the interface between the ion conductive phase and the silicon phase and the case where the element A1 and lithium are present on the surface of the composite particle. The element A1 may be contained as a compound containing the element A1 (such as an oxide) or in a solid solution state. The lithium may be contained as a compound containing lithium (such as lithium silicate) or in a solid solution state.

[0019] Alkali metal elements other than lithium include potassium (K), sodium (Na), etc. Group 2 elements of the long form periodic table include magnesium (Mg), calcium (Ca), etc. Element A1 is preferably at least one element selected from the group consisting of potassium, sodium, magnesium, and calcium.

[0020] The composite particle has a higher concentration of element A1 in the surface region than in the interior. When the concentration of element A1 at a depth of 100 nm from the surface of the composite particle is X% by mass and the concentration of element A1 in the entire composite particle is Y% by mass, the ratio of X / Y may be 2 or more, 3 or more, 5 or more, 10 or more, or 15 or more. The concentration X is, for example, 0.1 to 20% by mass. The concentration Y is, for example, 0.05 to 5% by mass.

[0021] The concentration X is the proportion (mass ratio) of element A1 to all elements present at a depth of 100 nm from the surface of the composite particle. The concentration X (mass %) of element A1 at a depth of 100 nm from the surface of the composite particle can be determined by X-ray photoelectron spectroscopy (XPS), energy dispersive X-ray spectroscopy using a scanning electron microscope (SEM-EDX), or the like.

[0022] The concentration Y is the proportion (mass ratio) of element A1 in the entire composite particle. The concentration Y (mass%) of element A1 in the entire composite particle can be determined by inductively coupled plasma optical emission spectroscopy (ICP), SEM-EDX analysis, etc. Details of the ICP analysis and SEM-EDX analysis of the composite particle will be described later.

[0023] Lithium may be distributed uniformly throughout the composite particle (depth direction), or the lithium concentration may be higher at the surface of the composite particle than at the interior. 2 CO 3 , Li 2 At least one selected from the group consisting of O and LiOH may be attached. These compounds can be used as raw materials containing Li in the process of producing the composite particles (the second step described below), and may remain on the surface of the particles as unreacted substances. The lithium contained in the composite particles may also include lithium remaining as unreacted substances.

[0024] (Element A2) The composite particles may contain element A2 (an element other than lithium, element A1, silicon, and oxygen). In this case, element A2 is contained within the ion-conducting phase. The element A2 being contained within the ion-conducting phase includes the case where element A2 is present at the interface between the ion-conducting phase and the silicon phase and the case where element A2 is present on the surface of the composite particles. The element A2 may be contained as a compound (such as an oxide) containing element A2, or may be contained in a solid solution state.

[0025] From the viewpoints of improving electrical conductivity and suppressing particle cracking (for example, improving Vickers hardness), element A2 is preferably at least one selected from the group consisting of aluminum (Al), boron (B), bismuth (Bi), antimony (Sb), germanium (Ge), zirconium (Zr), titanium (Ti), phosphorus (P), vanadium (V), tungsten (W), and lanthanum (La). In this case, rate characteristics and cycle characteristics are likely to be improved. The content of element A2 in the composite particle (the total content of Al and B) may be 0.01 mass% or more with respect to the entire composite particle. The composite particle may contain one type of element A2 or may contain multiple types of element A2. The concentration distribution of element A2 in the depth direction of the composite particle is not particularly limited.

[0026] (Composite Particles) The composite particles have a structure in which a silicon phase is dispersed within an ion-conducting phase (matrix). The ion-conducting phase relieves the stress associated with the expansion and contraction of the silicon phase during charge and discharge, suppressing cracking and fracture of the composite particles. This makes it possible to achieve both high capacity due to the inclusion of silicon and improved cycle characteristics. The ion-conducting phase may be composed of one phase or multiple phases.

[0027] The silicon oxide phase is composed of a compound of Si and O. The main component (for example, 95 to 100 mass%) of the silicon oxide phase may be silicon dioxide. The composite particles may be silicon oxide phase-containing composite particles. The silicon oxide phase-containing composite particles may be, for example, SiO x It is expressed by the formula (0.5≦x<1.6).

[0028] The silicate phase is composed of a compound containing a metal element, silicon (Si), and oxygen (O). Examples of the metal element include alkali metal elements such as lithium and Group 2 elements of the long periodic table. The silicate phase preferably contains at least lithium silicate. In this case, lithium ions can easily enter and exit the silicate phase. The lithium silicate phase has a smaller irreversible capacity than the silicon oxide phase. The composite particles may be silicate phase-containing composite particles. The ion-conducting phase may contain, for example, a silicate phase as a main component and a small amount of silicon oxide phase. Here, the "main component" refers to a component that accounts for 50% by mass or more of the total mass of the silicon compound phase, and may also account for 70% by mass or more. The silicate phase (lithium silicate phase) is composed of Li 2 Si 2 O 5 , Li 2 SiO 3 , and Li 4 SiO 4 The composition may include at least one selected from the group consisting of:

[0029] The atomic ratio of O to Si in the lithium silicate: O / Si is, for example, greater than 2 and less than 4. When the O / Si ratio is greater than 2 and less than 4 (z in the formula described below is 0<z<2), this is advantageous in terms of the stability of the silicate phase and lithium ion conductivity. Preferably, the O / Si ratio is greater than 2 and less than 3. The atomic ratio of Li to Si in the lithium silicate: Li / Si is, for example, greater than 0 and less than 4.

[0030] The composition of lithium silicate is represented by the formula: Li 2z SiO 2+z (0<z<2). From the viewpoints of stability, ease of preparation, lithium ion conductivity, etc., z preferably satisfies the relationship 0<z≦1, and more preferably z=1 / 2. For example, when z=1, lithium silicate is Li 2 SiO 3 When z = 1 / 2, Li 2 Si 2 O 5 It can be expressed as:

[0031] The average particle size of the fine silicon phase (before the first charge) dispersed within the ion-conducting phase may be 500 nm or less, 200 nm or more, or 50 nm or less. By appropriately miniaturizing the silicon phase in this manner, volume change during charge and discharge is reduced, improving structural stability. Furthermore, uniform expansion and contraction of the silicon phase is achieved, suppressing particle cracking and improving cycle performance. The average particle size of the silicon phase is measured by observing the cross section of the composite particle using a SEM or TEM. Specifically, it is determined by averaging the maximum diameters of 100 randomly selected silicon phases.

[0032] The silicon phase dispersed within the ion-conducting phase is a particulate phase of simple silicon (Si) and is composed of a single or multiple crystallites. From the viewpoint of reducing the volume change due to expansion and contraction of the silicon phase (silicon particles) during charging and discharging and facilitating improved cycle characteristics, the crystallite size of the silicon phase may be 50 nm or less, preferably 20 nm or less, and more preferably 10 nm or less. The lower limit of the crystallite size of the silicon phase is, for example, 5 nm or more. The crystallite size of the silicon phase is calculated using the Scherrer equation from the half-width of the diffraction peak assigned to the Si (111) plane in the X-ray diffraction (XRD) pattern.

[0033] From the viewpoint of increasing capacity and improving cycle characteristics, the content of the silicon phase in the composite particles may be 30% by mass or more (or 57% by mass or more) and 90% by mass or less, or may be 35% by mass or more and 75% by mass or less, relative to the entire composite particles.

[0034] The average particle size of the composite particles is, for example, 1 μm or more and 25 μm or less, or may be 4 μm or more and 15 μm or less. Within this range, good battery performance is likely to be obtained. The average particle size of the composite particles is the particle size (volume average particle size) at which the volume integrated value is 50% in the particle size distribution measured by a laser diffraction scattering method. For example, an "LA-750" manufactured by Horiba Ltd. can be used as the measuring device.

[0035] (Conductive Layer) From the viewpoint of improving conductivity, a conductive layer may be formed on the surface of the composite particle. The conductive layer contains, for example, a conductive carbon material. The thickness of the conductive layer is preferably thin enough not to substantially affect the average particle size of the composite particle. From the viewpoint of ensuring conductivity, the thickness of the conductive layer is preferably 1 nm or more.

[0036] The conductive layer is formed by mixing a raw material of a conductive carbon material with composite particles and calcining the mixture to carbonize the raw material of the conductive carbon material. Examples of the raw material of the conductive material include coal pitch, coal tar pitch, petroleum pitch, and phenolic resin. The mixture of the raw material of the conductive carbon material and the composite particles is calcined, for example, in an inert atmosphere (e.g., an argon or nitrogen atmosphere). The calcination temperature is preferably 450°C or higher and 1000°C or lower. Within this temperature range, a highly conductive layer is easily formed in a silicate phase with low crystallinity. The calcination temperature is preferably 550°C or higher and 900°C or lower, more preferably 650°C or higher and 850°C or lower. The calcination time is, for example, 1 hour or higher and 10 hours or lower. The formation of the conductive layer on the surface of the composite particles may be performed after the second step (addition of element A1, etc.) described below.

[0037] (Preparation of silicon-containing particles) The process for preparing silicon-containing particles includes, for example, a first step and a second step. In the first step, composite particles are prepared. If the composite particles (ion-conductive phase) prepared in the first step contain lithium, in the second step, a large amount of element A1 (or element A1 and lithium) is added to the surface side of the composite particles. If the composite particles (ion-conductive phase) prepared in the first step do not contain lithium, in the second step, a large amount of lithium and element A1 are added to the surface side of the composite particles.

[0038] (First Step) In the first step, composite particles are prepared, each of which includes an ion-conducting phase and a silicon phase dispersed within the ion-conducting phase. The ion-conducting phase includes at least one silicon compound phase selected from the group consisting of a silicate phase and a silicon oxide phase.

[0039] The composite particles (ion conductive phase) prepared in the first step may not contain element A1 or may contain element A1. The composite particles (ion conductive phase) prepared in the first step may contain element A2.

[0040] (Preparation of Silicon Oxide Phase-Containing Composite Particles) As the silicon oxide phase-containing composite particles, for example, SiO x Composite particles represented by the formula (0.5≦x<1.6) may be prepared. x The particles may be, for example, SiO 2 and Si particles are mixed, heated under vacuum conditions, vaporized, and then solidified. 2 By adding element A2 or a compound containing element A2 to Si particles, SiO x The particles (silicon oxide phase) may contain element A2. The above-described production method can obtain composite particles containing a silicon phase having a small crystallite size of, for example, 20 nm or less.

[0041] (Preparation of silicate phase-containing composite particles) As the silicate phase-containing composite particles, for example, Li 2z SiO 2+z Composite particles containing a lithium silicate phase represented by (0<z<2) may be prepared. The silicate phase-containing composite particles may be obtained, for example, by pulverizing a mixture of silicate (lithium silicate) and raw material silicon while stirring it in a ball mill or the like to form fine particles, then heat-treating the mixture in an inert atmosphere and pulverizing the sintered product obtained by the heat treatment. The silicate used as a raw material for the composite particles may contain element A2. Details of the method for producing the lithium silicate phase-containing composite particles will be described later.

[0042] (Second Step) When the composite particles (ion conductive phase) prepared in the first step contain lithium, in the second step, for example, a raw material containing element A1 is heated to obtain a melt containing element A1, and the composite particles are introduced into the melt for a predetermined period of time. In this way, the melt and the composite particles are brought into contact with each other for a predetermined period of time. This allows the element A to be distributed in large amounts on the surface side of the composite particles. When the composite particles (ion conductive phase) prepared in the first step do not contain lithium, in the second step, for example, a mixture of a raw material containing lithium and a raw material containing element A1 is heated to obtain a melt containing lithium and element A1, and the composite particles are introduced into the melt. This allows the lithium and element A1 to be distributed in large amounts on the surface side of the composite particles.

[0043] Examples of raw materials containing element A1 include carbonates, hydroxides, oxides, etc. When the composite particles prepared in the first step do not contain element A2, the melt may contain a raw material containing element A2.

[0044] The above-mentioned X / Y ratio (concentration gradient of element A1 in the depth direction of the composite particle) can be adjusted, for example, by the size (particle size) of the composite particle in the first step, the time for adding the composite particle to the melt in the second step, the temperature of the melt in the second step (heating temperature of the raw material containing element A1), etc.

[0045] The amount of element A1 added may be, for example, 0.1 to 10 parts by mass relative to 100 parts by mass of the composite particles. The amount of lithium added may be, for example, 0.1 to 10 parts by mass relative to 100 parts by mass of the composite particles. The amount of element A1 (or Li and element A1) added to the composite particles can be adjusted, for example, by the amount of composite particles added to the melt.

[0046] After the second step, the composite particles may be heat-treated. The heat treatment may cause crystal growth of the silicon phase of the composite particles to increase the crystallite size. The crystallite size of the silicon phase may be increased appropriately to improve the initial charge / discharge efficiency.

[0047] An example of a method for producing the lithium silicate phase-containing composite particles prepared in the first step will be described in detail below.

[0048] Step (i) (Step of Obtaining Lithium Silicate) A raw material mixture containing a Si-containing raw material and a Li raw material in a predetermined ratio is used as the raw material for lithium silicate. If necessary, another element M may be contained in the raw material mixture. Examples of element M include element A2. A mixture of predetermined amounts of the above raw materials is melted, and the molten liquid is passed through a metal roll to form flakes, thereby producing lithium silicate. The flaked silicate is then crystallized by heat treatment in an air atmosphere at a temperature above the glass transition point and below the melting point. The flaked silicate can also be used without crystallization. Alternatively, a predetermined amount of the mixture can be fired at a temperature below the melting point without being melted, thereby producing silicate by a solid-phase reaction.

[0049] The Si raw material can be silicon or silicon monoxide. The Li raw material can be, for example, lithium carbonate, lithium oxide, lithium hydroxide, lithium hydride, etc. The raw material containing element M can be, for example, oxide, hydroxide, carbonate compound, hydride, nitrate, sulfate, etc. of each element. The Si raw material that has not reacted with the Li raw material can remain in the lithium silicate. The remaining Si raw material is dispersed in the lithium silicate as fine silicon oxide crystals.

[0050] Step (ii) (Step of Obtaining Silicate Composite Particles) Next, lithium silicate is compounded with raw silicon to form composite particles. For example, the composite particles are produced through the following steps (a) to (c).

[0051] Step (a) First, raw silicon powder and lithium silicate powder are mixed in a mass ratio of, for example, 20:80 to 95:5. The raw silicon powder may be coarse silicon particles having an average particle size of several μm to several tens of μm.

[0052] Step (b): Next, using a grinding device such as a ball mill, the mixture of raw silicon and lithium silicate is ground and compounded while being finely divided. At this time, an organic solvent may be added to the mixture and wet-ground. A predetermined amount of organic solvent may be added to the grinding vessel all at once at the beginning of grinding, or a predetermined amount of organic solvent may be added to the grinding vessel intermittently in multiple batches during the grinding process. The organic solvent serves to prevent the material to be ground from adhering to the inner wall of the grinding vessel.

[0053] As the organic solvent, alcohols, ethers, fatty acids, alkanes, cycloalkanes, silicate esters, metal alkoxides, etc. can be used.

[0054] The raw silicon may be coarse silicon particles having an average particle size of several μm to several tens of μm. The silicon particles (silicon phase) finally obtained are preferably controlled so that the crystallite size, calculated from the half-width of the diffraction peak attributable to the Si(111) plane in the X-ray diffraction pattern using the Scherrer formula, is 5 nm or more and 50 nm or less.

[0055] The raw silicon and lithium silicate may be separately microparticulated and then mixed. Alternatively, silicon nanoparticles and amorphous lithium silicate nanoparticles may be prepared without using a pulverizer and then mixed. The nanoparticles may be prepared by known methods such as a gas phase method (e.g., a plasma method) or a liquid phase method (e.g., a liquid phase reduction method).

[0056] Step (c) Next, the pulverized material is fired under pressure using a hot press or the like to obtain a sintered body. The firing is carried out, for example, in an inert atmosphere (e.g., an argon, nitrogen, or other atmosphere). The firing temperature is preferably 450°C or higher and 1000°C or lower. Within this temperature range, fine silicon particles are easily dispersed within the silicate phase with low crystallinity. During sintering, the lithium silicate softens and flows to fill the gaps between the silicon particles. As a result, a dense block-shaped sintered body can be obtained, with the silicate phase forming a sea portion and silicon particles (silicon phase) forming islands. The firing temperature is preferably 550°C or higher and 900°C or lower, more preferably 650°C or higher and 850°C or lower. The firing time is, for example, 1 hour or higher and 10 hours or lower.

[0057] The resulting sintered body is pulverized to obtain composite particles. By appropriately selecting the pulverization conditions, composite particles of a predetermined average particle size can be obtained. Steps (i) and (ii) produce composite particles having a silicate phase as a matrix and a silicon phase dispersed in the matrix.

[0058] The composition of the composite particles can be determined, for example, by the following analytical method.

[0059] <EDX> From the cross-sectional image of the backscattered electron image of the negative electrode mixture layer taken by SEM, 10 composite particles with a maximum particle diameter of 5 μm or more are randomly selected, and elemental mapping analysis is performed on each particle using energy dispersive X-ray (EDX). The area ratio of the target element is calculated using image analysis software. The observation magnification is preferably 2000 to 20,000 times. The measured values ​​of the area ratio of a specific element contained in the 10 particles are averaged. The content of the target element is calculated from the obtained average value.

[0060] Desirable measurement conditions for cross-sectional SEM-EDX analysis are shown below. <SEM-EDX measurement conditions> Processing equipment: SM-09010 (Cross Section Polisher) manufactured by JEOL Processing conditions: Acceleration voltage 6 kV Current value: 140 μA Vacuum degree: 1×10 -3 ~2 x 10 -3Pa Measuring device: Electron microscope HITACHI SU-70 Acceleration voltage during analysis: 10 kV Field: Free mode Probe current mode: Medium Probe current range: High Anode Ap.: 3 OBJ Ap.: 2 Analysis area: 1 μm square Analysis software: EDAX Genesis CPS: 20500 Lsec: 50 Time constant: 3.2

[0061] <ICP> A sample of composite particles is completely dissolved in a heated acid solution (a mixed acid of hydrofluoric acid, nitric acid, and sulfuric acid), and the carbon remaining in the solution is filtered off. The filtrate is then analyzed by inductively coupled plasma emission spectroscopy (ICP) to measure the spectral intensity of each element. A calibration curve is then created using commercially available standard solutions of the elements, and the content of each element contained in the composite particles is calculated.

[0062] The contents of element A1 and element A2 contained in the composite particles can be quantitatively analyzed in accordance with JIS R3105 (1995) (method of analysis of borosilicate glass).

[0063] In silicate phase-containing composite particles, a silicate phase and a silicon phase exist, and these can be distinguished and quantified using Si-NMR. The Si content obtained by the above method is the sum of the amount of Si constituting the silicon phase and the amount of Si in the silicate phase. The amount of Si element contained in the composite particles is distributed between the silicate phase and the silicon phase using the results of quantitative analysis by Si-NMR. Note that the standard substance required for quantification can be a mixture containing a silicate phase and a silicon phase in a predetermined ratio with known Si contents.

[0064] Desirable Si-NMR measurement conditions are shown below. <Si-NMR measurement conditions> Measurement device: Varian solid-state nuclear magnetic resonance spectrometer (INOVA-400) Probe: Varian 7 mm CPMAS-2 MAS: 4.2 kHz MAS speed: 4 kHz Pulse: DD (45° pulse + signal acquisition time 1H decoupled) Repetition time: 1200 sec to 3000 sec Observation width: 100 kHz Observation center: near -100 ppm Signal acquisition time: 0.05 sec Number of accumulations: 560 Sample amount: 207.6 mg

[0065] FIG. 1 is a cross-sectional view schematically illustrating an example of a negative electrode active material (composite particle). The negative electrode active material 20 includes a composite particle 23 (mother particle). The composite particle 23 includes an ion-conducting phase 21 and a silicon phase (silicon particles) 22 dispersed within the ion-conducting phase 21. The composite particle 23 has a sea-island structure in which fine silicon phases 22 are dispersed within a matrix of the ion-conducting phase 21. The surface of the composite particle 23 is covered with a conductive layer 26. The composite particle 23 (ion-conducting phase 21) contains element A1 and lithium. The concentration of element A1 is higher on the surface side (closer to the conductive layer 26) of the composite particle 23 than on the interior side.

[0066] [Secondary Battery] A secondary battery according to an embodiment of the present disclosure includes a positive electrode, a negative electrode, and an electrolyte. The negative electrode contains the above-described negative electrode active material for a secondary battery. The negative electrode of the secondary battery and other components will be described below.

[0067] [Negative Electrode] The negative electrode includes, for example, a negative electrode mixture layer containing the above-described negative electrode active material for secondary batteries, and a negative electrode current collector supporting the negative electrode mixture layer. The negative electrode mixture layer can be formed by applying a negative electrode slurry, in which the negative electrode mixture is dispersed in a dispersion medium, to the surface of the negative electrode current collector and drying it. The dried coating may be rolled as necessary. The negative electrode mixture layer may be formed on one surface or both surfaces of the negative electrode current collector.

[0068] The negative electrode mixture contains the above-mentioned negative electrode active material for a secondary battery as an essential component, and may contain optional components such as a binder, a conductive agent, and a thickener. The silicon phase in the composite particles can absorb many lithium ions, thereby contributing to a high capacity of the negative electrode. The content of the composite particles in the negative electrode mixture layer may be 1 mass% or more and 50 mass% or less with respect to the entire negative electrode mixture layer.

[0069] The negative electrode active material may further contain another active material that electrochemically absorbs and releases lithium ions. A preferred example of such another active material is a carbon-based active material. Because the composite particles expand and contract in volume with charge and discharge, a large proportion of the composite particles in the negative electrode active material is likely to result in poor contact between the negative electrode active material and the negative electrode current collector with charge and discharge. On the other hand, the combined use of the composite particles and a carbon-based active material makes it possible to achieve excellent cycle characteristics while imparting high capacity to the negative electrode due to the silicon phase. The proportion of the composite particles in the total of the composite particles and the carbon-based active material is preferably 0.5 to 15 mass%, more preferably 1 to 5 mass%. This makes it easier to achieve both high capacity and improved cycle characteristics.

[0070] Examples of carbon-based active materials include graphite, easily graphitizable carbon (soft carbon), and hardly graphitizable carbon (hard carbon). Among these, graphite is preferred because of its excellent charge / discharge stability and low irreversible capacity. Graphite refers to a material having a graphite-type crystal structure, and includes, for example, natural graphite, artificial graphite, and graphitized mesophase carbon particles. One type of carbon-based active material may be used alone, or two or more types may be used in combination.

[0071] As the negative electrode current collector, a non-porous conductive substrate (such as a metal foil) or a porous conductive substrate (such as a mesh, net, or punched sheet) is used. Examples of the material for the negative electrode current collector include stainless steel, nickel, nickel alloys, copper, and copper alloys. The thickness of the negative electrode current collector is not particularly limited, but is preferably 1 to 50 μm, and more preferably 5 to 20 μm, from the viewpoint of balancing the strength and weight of the negative electrode.

[0072] Examples of binders include fluororesin, polyolefin resin, polyamide resin, polyimide resin, vinyl resin, styrene-butadiene copolymer rubber (SBR), polyacrylic acid and its derivatives. These may be used alone or in combination of two or more. Examples of conductive agents include carbon black, conductive fiber, carbon fluoride, and organic conductive materials. These may be used alone or in combination of two or more. Examples of thickeners include carboxymethyl cellulose (CMC) and polyvinyl alcohol. These may be used alone or in combination of two or more.

[0073] Examples of the dispersion medium include water, alcohol, ether, N-methyl-2-pyrrolidone (NMP), and a mixed solvent thereof.

[0074] [Positive Electrode] The positive electrode comprises, for example, a positive electrode current collector and a positive electrode mixture layer supported on the surface of the positive electrode current collector. The positive electrode mixture layer can be formed by applying a positive electrode slurry, in which the positive electrode mixture is dispersed in a dispersion medium, to the surface of the positive electrode current collector and drying it. The dried coating may be rolled as necessary. The positive electrode mixture layer may be formed on one surface or both surfaces of the positive electrode current collector.

[0075] The positive electrode mixture contains a positive electrode active material as an essential component, and may contain a binder, a conductive agent, and the like as optional components.

[0076] As the positive electrode active material, a lithium transition metal composite oxide can be used. Examples of the lithium transition metal composite oxide include Li a CoO2, Li a NiO2, Li a MnO2, Li a Co b Ni 1-b O2, Li a Co b M 1-b O c , Li a Ni 1-b M b O c , Li a Mn2O4, Li a Mn2-b M b Examples of suitable lithium-ion batteries include Li2O4, LiMePO4, and Li2MePO4F. Here, M is at least one element selected from the group consisting of Na, Mg, Sc, Y, Mn, Fe, Co, Ni, Cu, Zn, Al, Cr, Pb, Sb, and B. Me contains at least a transition element (e.g., at least one element selected from the group consisting of Mn, Fe, Co, and Ni). Here, 0≦a≦1.2, 0≦b≦0.9, and 2.0≦c≦2.3. The value a, which indicates the molar ratio of lithium, increases or decreases with charge and discharge.

[0077] The binder and conductive agent may be the same as those exemplified for the negative electrode. As the conductive agent, graphite such as natural graphite or artificial graphite may be used.

[0078] The shape and thickness of the positive electrode current collector can be selected from the shape and range corresponding to those of the negative electrode current collector. Examples of the material of the positive electrode current collector include stainless steel, aluminum, aluminum alloy, and titanium.

[0079] [Electrolyte] The electrolyte may be a liquid electrolyte (electrolytic solution), a gel electrolyte, or a solid electrolyte. The liquid electrolyte is, for example, an electrolytic solution containing a non-aqueous solvent and a salt dissolved in the non-aqueous solvent. The concentration of the salt in the electrolytic solution is, for example, 0.5 mol / L or more and 2 mol / L or less. The electrolytic solution may contain known additives.

[0080] The gel electrolyte contains a salt and a matrix polymer, or a salt, a non-aqueous solvent, and a matrix polymer. The matrix polymer is, for example, a polymer material that absorbs the non-aqueous solvent and gels. Examples of the polymer material include fluororesin, acrylic resin, polyether resin, and polyethylene oxide.

[0081] As the solid electrolyte, for example, a material known in all-solid-state lithium ion secondary batteries (for example, oxide-based solid electrolytes, sulfide-based solid electrolytes, halide-based solid electrolytes, etc.) can be used.

[0082] For example, a liquid non-aqueous electrolyte is prepared by dissolving a salt in a non-aqueous solvent. The salt is an electrolyte salt that ionizes in the electrolyte, and may include, for example, a lithium salt. The electrolyte may contain various additives. The electrolyte is usually used in its liquid state, but its fluidity may be limited by a gelling agent or the like.

[0083] Examples of non-aqueous solvents that can be used include cyclic carbonates, chain carbonates, cyclic carboxylic acid esters, and chain carboxylic acid esters. Examples of cyclic carbonates include propylene carbonate (PC), ethylene carbonate (EC), and vinylene carbonate (VC). Examples of chain carbonates include diethyl carbonate (DEC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC). Examples of cyclic carboxylic acid esters include γ-butyrolactone (GBL) and γ-valerolactone (GVL). Examples of chain carboxylic acid esters include methyl acetate, ethyl acetate, propyl acetate, methyl propionate (MP), and ethyl propionate (EP). One type of non-aqueous solvent may be used alone, or two or more types may be used in combination.

[0084] Other examples of the non-aqueous solvent include cyclic ethers, chain ethers, nitriles such as acetonitrile, and amides such as dimethylformamide.

[0085] Examples of lithium salts include lithium salts of chlorine-containing acids (LiClO4, LiAlCl4, LiB 10 Cl 10 Lithium salts such as fluorine-containing acids (LiPF, LiBF, LiSbF, LiAsF, LiCF, SO, LiCF, CO, etc.), lithium salts of fluorine-containing acid imides (LiN(CF, SO), LiN(CF) SO (CF, SO), LiN(CF, SO) (CF, SO), LiN(CF, SO), etc.), and lithium halides (LiCl, LiBr, LiI, etc.). One type of lithium salt may be used alone, or two or more types may be used in combination.

[0086] The concentration of the lithium salt in the electrolyte may be 1 mol / L or more and 2 mol / L or less, or may be 1 mol / L or more and 1.5 mol / L or less. By controlling the lithium salt concentration within the above range, an electrolyte having excellent ionic conductivity and appropriate viscosity can be obtained. However, the lithium salt concentration is not limited to the above.

[0087] [Separator] It is usually desirable to interpose a separator between the positive electrode and the negative electrode. The separator has high ion permeability and adequate mechanical strength and insulating properties. The separator can be made of a microporous thin film, a woven fabric, a nonwoven fabric, or the like. The separator can be made of polyolefins such as polypropylene and polyethylene.

[0088] An example of the structure of a secondary battery is a structure in which an electrode group formed by winding a positive electrode and a negative electrode with a separator interposed therebetween and a nonaqueous electrolyte are housed in an exterior body. Alternatively, instead of a wound electrode group, other types of electrode groups may be used, such as a stacked electrode group formed by stacking a positive electrode and a negative electrode with a separator interposed therebetween. The secondary battery may be in any shape, such as a cylindrical shape, a prismatic shape, a coin shape, a button shape, or a laminate shape.

[0089] Hereinafter, the structure of a prismatic non-aqueous electrolyte secondary battery as an example of a secondary battery according to the present disclosure will be described with reference to Fig. 2. Fig. 2 is a schematic perspective view of a secondary battery according to an embodiment of the present disclosure, with a portion cut away.

[0090] The battery includes a bottomed prismatic battery case 4, and an electrode group 1 and a nonaqueous electrolyte (not shown) housed within the battery case 4. The electrode group 1 includes a long strip-shaped negative electrode, a long strip-shaped positive electrode, and a separator interposed between them to prevent direct contact. The electrode group 1 is formed by winding the negative electrode, positive electrode, and separator around a flat plate-shaped winding core and then removing the winding core.

[0091] One end of a negative electrode lead 3 is attached to the negative electrode current collector by welding or the like. The other end of the negative electrode lead 3 is electrically connected to a negative electrode terminal 6 provided on the sealing plate 5 via a resin insulating plate (not shown). The negative electrode terminal 6 is insulated from the sealing plate 5 by a resin gasket 7. One end of a positive electrode lead 2 is attached to the positive electrode current collector by welding or the like. The other end of the positive electrode lead 2 is connected to the back surface of the sealing plate 5 via an insulating plate. That is, the positive electrode lead 2 is electrically connected to the battery case 4, which also serves as the positive electrode terminal. The insulating plate separates the electrode group 1 from the sealing plate 5 and also separates the negative electrode lead 3 from the battery case 4. The periphery of the sealing plate 5 fits into the open edge of the battery case 4, and the fitting portion is laser-welded. In this way, the opening of the battery case 4 is sealed with the sealing plate 5. A non-aqueous electrolyte injection hole provided in the sealing plate 5 is closed with a seal 8.

[0092] (Additional Notes) The above embodiments disclose the following technologies. (Technology 1) A negative electrode active material for a secondary battery, comprising silicon-containing particles including an ion-conducting phase and a silicon phase dispersed within the ion-conducting phase, the silicon-containing particles including lithium and an element A1, the concentration of the element A1 being higher in the surface portion of the silicon-containing particles than in the interior thereof, the element A1 being at least one element selected from the group consisting of alkali metal elements other than lithium and Group 2 elements of the long form periodic table. (Technology 2) The negative electrode active material for a secondary battery according to Technology 1, wherein the element A1 is at least one element selected from the group consisting of sodium, potassium, magnesium, and calcium. (Technology 3) The negative electrode active material for a secondary battery according to Technology 1 or 2, wherein the concentration of the element A1 at a depth of 100 nm from the surface of the silicon-containing particle is X% by mass, and the concentration of the element A1 in the entire silicon-containing particle is Y% by mass, the ratio of X / Y being 2 or greater. (Technology 4) The negative electrode active material for a secondary battery according to any one of Technologies 1 to 3, wherein the ion-conducting phase includes at least one selected from the group consisting of a silicate phase and a silicon oxide phase. (Technology 5) The silicate phase includes Li 2 Si 2 O5 , Li 2 SiO 3 , and Li 4 SiO 4 The negative electrode active material for a secondary battery according to Technology 4 includes at least one element selected from the group consisting of: (Technology 6) The negative electrode active material for a secondary battery according to any one of Technology 1 to 5, wherein the silicon-containing particles include element A2, and the element A2 is at least one element selected from the group consisting of aluminum, boron, bismuth, antimony, germanium, zirconium, titanium, phosphorus, vanadium, tungsten, and lanthanum. (Technology 7) The negative electrode active material for a secondary battery according to Technology 6, wherein the content of element A2 in the silicon-containing particles is 0.01 mass% or more, based on the total mass of the silicon-containing particles. (Technology 8) The negative electrode active material for a secondary battery according to any one of Technology 1 to 7, wherein the content of the silicon phase in the silicon-containing particles is 30 mass% or more and 90 mass% or less, based on the total mass of the silicon-containing particles. (Technology 9) The negative electrode active material for a secondary battery according to any one of Technology 1 to 8, wherein the crystallite size of the silicon phase is 20 nm or less. (Technology 10) The negative electrode active material for a secondary battery according to any one of Techniques 1 to 9, wherein the silicon-containing particles have an average particle size of 4 μm or more and 15 μm or less. (Technology 11) The negative electrode active material for a secondary battery according to any one of Techniques 1 to 9, wherein the silicon-containing particles have an average particle size of 4 μm or more and 15 μm or less. 2 CO 3 , Li 2 The negative electrode active material for a secondary battery according to any one of Techniques 1 to 10, to which at least one selected from the group consisting of O and LiOH is attached. (Technology 12) A secondary battery comprising: a positive electrode, a negative electrode, and an electrolyte, wherein the negative electrode comprises the negative electrode active material for a secondary battery according to any one of Techniques 1 to 11. (Technology 13) The secondary battery according to Technique 12, wherein the negative electrode comprises: a negative electrode mixture layer containing the negative electrode active material for a secondary battery, and a negative electrode current collector supporting the negative electrode mixture layer, and the content of the silicon-containing particles in the negative electrode mixture layer is 1 mass % or more and 50 mass % or less with respect to the entire negative electrode mixture layer.

[0093] Examples Examples of the present disclosure will be specifically described below, but the present disclosure is not limited to the following examples.

[0094] Example 1 (Preparation of silicon oxide phase-containing composite particles) SiO 2 and Si particles were mixed and heated under vacuum conditions to obtain a vapor, which was then solidified. x The sublimation source SiO 2 By adding aluminum metal and a boron compound to the mixture of SiO x The particles (silicon oxide phase) were doped with aluminum and boron.

[0095] The crystallite size of the silicon phase was 6 nm. The main component of the silicon oxide phase was SiO 2 The content of the silicon phase in the silicon oxide phase-containing composite particles was 51 mass %.

[0096] (Addition of Li and element A1 to silicon oxide phase-containing composite particles) In an inert atmosphere, Li 2 CO 3 , Na 2 CO 3 , and K 2 CO 3 The mixture was heated to 500°C to melt, and the silicon oxide phase-containing composite particles were added to the melt. In this way, a large amount of Li and element A1 (K and Na) was added to the surface side of the silicon oxide phase-containing composite particles.

[0097] The contents of Li, Na, K, Al, and B in the composite particles were the values ​​shown in Table 1. x The particle size and the amount of SiO in the melt x The particle introduction time was appropriately adjusted to set the X / Y ratio of the K concentration to 6. The concentration X was determined by the XPS method described above, and the concentration Y was determined by the ICP atomic emission spectroscopy method described above. In the XPS method, analysis was performed in the depth direction by Ar ion etching, and the concentration X was determined from the atomic ratio data obtained by the XPS method.

[0098] (Formation of Conductive Layer) Then, 100 parts by mass of the composite particles were mixed with 3 parts by mass of coal tar pitch, and the mixture was fired at 800°C in an inert atmosphere to coat the surfaces of the composite particles with conductive carbon. In this way, a conductive layer was formed on the surfaces of the composite particles. The coating amount of the conductive layer was 3% by mass based on the total weight of the composite particles and the conductive layer.

[0099] (Preparation of Negative Electrode) Graphite and composite particles having a conductive layer were mixed in a mass ratio of 90:10, and this was used as the negative electrode active material. 1 part by mass of carboxymethyl cellulose (CMC) and 1.5 parts by mass of styrene-butadiene rubber (SBR) were added to 97.5 parts by mass of the negative electrode active material, and a predetermined amount of water was further added to prepare a negative electrode slurry.

[0100] The negative electrode slurry was applied to both sides of a copper foil negative electrode current collector, the coating was dried, rolled, and then cut to a predetermined size to obtain a negative electrode having a negative electrode mixture layer formed on both sides of the negative electrode current collector. At this time, a negative electrode current collector exposed portion was provided in a part of the negative electrode.

[0101] (Preparation of Positive Electrode) 2.5 parts by mass of acetylene black and 2.5 parts by mass of polyvinylidene fluoride were added to 95 parts by mass of the positive electrode active material, and an appropriate amount of N-methyl-2-pyrrolidone (NMP) was further added to prepare a positive electrode slurry. 0.88 Co 0.09 Al 0.03 O 2 The lithium transition metal composite oxide represented by the following formula was used.

[0102] The positive electrode slurry was applied to both sides of an aluminum foil serving as a positive electrode current collector, the coating was dried, rolled, and then cut to a predetermined size to obtain a positive electrode having a positive electrode mixture layer formed on both sides of the positive electrode current collector. At this time, a positive electrode current collector exposed portion was provided in a part of the positive electrode.

[0103] (Preparation of non-aqueous electrolyte) Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) were mixed in a volume ratio of 20:5:75 to obtain a mixed solvent, and lithium hexafluorophosphate was dissolved in the mixed solvent at a concentration of 1 mol / L to prepare a non-aqueous electrolyte.

[0104] (Preparation of Test Cell) The negative electrode prepared above and lithium metal foil (counter electrode) were prepared. Leads were attached to the negative electrode (exposed portion of the negative electrode current collector) and the lithium metal foil. The negative electrode and lithium metal foil were spirally wound with a polyolefin separator between them and then pressed radially to prepare a flat electrode assembly. A polyolefin microporous film was used as the separator. The electrode assembly was housed in an exterior body made of an aluminum laminate sheet, and after injecting a nonaqueous electrolyte, the opening of the exterior body was sealed. At this time, portions of the leads attached to the negative electrode and counter electrode were exposed from the exterior body. In this way, test cell e1 was obtained. The test cell was prepared in an argon atmosphere.

[0105] The fabricated test cell e1 was used to carry out the following evaluations 1 and 2.

[0106] (Evaluation 1: Initial charge-discharge efficiency) In an environment of 25° C., charging was performed at 0.1 It until the voltage reached 0.005 V, and then charging was performed at a voltage of 0.005 V until the current reached 0.01 It. After charging, discharging was performed at a current of 0.1 It until the voltage reached 1 V in an environment of 25° C. The charge capacity C1 and discharge capacity D1 at this time were determined, and the charge-discharge efficiency was calculated as (D1 / C1)×100.

[0107] (Evaluation 2: Rate Characteristics) In an environment of 25°C, charging was performed at a current of 0.1 It until the voltage reached 0.005 V, and then charging was performed at a voltage of 0.005 V until the current reached 0.01 It. After charging, in an environment of 25°C, discharging was performed at a current of 2 It until the voltage reached 1 V. The discharge capacity D2 at this time was determined. Using the obtained discharge capacity D2 at 2 It discharge and the discharge capacity D1 at 0.1 It discharge determined from the above initial charge-discharge efficiency, (D2 / D1) x 100 was calculated to evaluate the rate characteristics.

[0108] (Preparation of Secondary Battery) The positive and negative electrodes prepared as described above were prepared. Leads were attached to the exposed current collectors of the positive and negative electrodes, respectively. The positive and negative electrodes were spirally wound with a polyolefin separator interposed therebetween and then pressed radially to prepare a flat electrode assembly. A polyolefin microporous film was used as the separator. The electrode assembly was housed in an exterior body made of an aluminum laminate sheet, and after injecting a nonaqueous electrolyte, the opening of the exterior body was sealed. At this time, portions of the leads attached to the positive and negative electrodes were exposed from the exterior body. In this way, a secondary battery E1 for evaluation was obtained.

[0109] The following evaluation 3 was carried out using the produced secondary battery E1.

[0110] (Evaluation 3: Cycle Retention Rate) A cycle test was carried out under the following charge / discharge conditions in an environment of 25° C. The rest period between charge and discharge was 10 minutes.

[0111] <Charging> The battery was charged at a current of 1 It (800 mA) until the voltage reached 4.2 V, and then charged at a voltage of 4.2 V until the current reached 1 / 20 It (40 mA).

[0112] <Discharge> Discharge was carried out at a current of 1 It (800 mA) until the voltage reached 2.75 V.

[0113] Charge and discharge were repeated up to 200 cycles under the above conditions, and the ratio of the discharge capacity at the 200th cycle to the discharge capacity at the 1st cycle was calculated as the cycle retention rate (%).

[0114] Example 2 A test cell e2 and a secondary battery E2 were produced and evaluated in the same manner as in Example 1, except that the silicon oxide phase-containing composite particles to which Li and element A1 (K and Na) had been added were further heat-treated at 800°C for 5 hours in an inert atmosphere. The crystallite size of the silicon phase was 6 nm. The X / Y ratio of the K concentration was set to 18 by appropriately adjusting the time for which the silicon oxide phase-containing composite particles were added to the melt.

[0115] Example 3 The same silicon oxide phase-containing composite particles as in Example 1 were prepared. 2 CO 3 and MgCO3 The mixture was heated to 500°C to melt, and the silicon oxide phase-containing composite particles were added to the melt. In this way, a large amount of Li and element A1 (Mg) was added to the surface side of the silicon oxide phase-containing composite particles.

[0116] The contents of Li, Mg, Al, and B in the composite particles were the values ​​shown in Table 1. x The particle size and the amount of SiO in the melt x The time for adding the particles was appropriately adjusted to set the X / Y ratio of the Mg concentration to 20.

[0117] Furthermore, the silicon oxide phase-containing composite particles to which Li and element A1 (Mg) had been added were subjected to heat treatment in an inert atmosphere at a predetermined temperature for a predetermined time. The crystallite size of the silicon phase was 13 nm.

[0118] A test cell e3 and a secondary battery E3 were produced and evaluated in the same manner as in Example 1, except that the composite particles produced above were used.

[0119] Examples 4 and 5 (Preparation of Lithium Silicate Phase-Containing Composite Particles) Lithium carbonate (Li 2 CO 3 ) and silicon dioxide (SiO 2 The mixture was obtained by mixing aluminum oxide (Al) with a raw material containing element A2. The atomic ratio of Li to Si: Si / Li was 1.05. 2 O 3 ) and boron oxide (B 2 O 3 The mixture was fired at 800°C for 10 hours in an inert gas atmosphere to obtain lithium silicate containing Al and B. The obtained lithium silicate was pulverized to an average particle size of 10 µm.

[0120] The crushed lithium silicate containing Al and B was mixed with raw silicon (3N, average particle size 10 μm) in a mass ratio of 40:60. The mixture was charged into a pot (SUS, volume: 500 mL) of a planetary ball mill (Fritsch, P-5). Next, 24 SUS balls (diameter 20 mm) were placed in the pot, the lid was closed, and the mixture was crushed at 200 rpm for 50 hours in an inert atmosphere.

[0121] The powder mixture was then removed from the inert atmosphere and fired at 600°C for 4 hours under pressure from a hot press to obtain a sintered body of the mixture. The sintered body was then crushed and passed through a 40 µm mesh to obtain composite particles (lithium silicate phase-containing composite particles). The composite particles were then sieved to obtain composite particles with an average particle size of 10 µm.

[0122] The crystallite size of the silicon phase was 50 nm. The main component of the silicate phase was Li. 2 Si 2 O 5 The content of the silicon phase in the lithium silicate phase-containing composite particles was about 60 mass %.

[0123] (Addition of element A1 to lithium silicate phase-containing composite particles) In an inert atmosphere, Na 2 CO 3 and K. 2 CO 3 The mixture was heated to 500° C. to melt, and the lithium silicate phase-containing composite particles were poured into the melt. In this way, a large amount of element A1 was added to the surface portion side of the lithium silicate phase-containing composite particles.

[0124] The contents of Li, Na, K, Al, and B in the composite particles were the values ​​shown in Table 1. The particle size of the composite particles and the time for adding the composite particles to the melt were appropriately adjusted to set the X / Y ratio of the K concentration to 3.

[0125] Test cells e4 to e5 and secondary batteries E4 to E5 were produced and evaluated in the same manner as in Example 1, except that the composite particles produced above were used.

[0126] Comparative Example 1: The silicon oxide phase of the composite particles did not contain Al and B. Lithium and element A1 were not added to the composite particles. A test cell r1 and a secondary battery R1 were produced and evaluated in the same manner as in Example 1, except for the above.

[0127] Comparative Example 2 A test cell r2 and a secondary battery R2 were produced and evaluated in the same manner as in Example 1, except that lithium and element A1 were not added to the composite particles.

[0128] Comparative Example 3 A test cell r3 and a secondary battery R3 were produced and evaluated in the same manner as in Example 1, except that element A1 was not added to the composite particles.

[0129] Comparative Examples 4 and 5: Lithium carbonate (Li 2 CO 3 ) and silicon dioxide (SiO 2 The mixture was obtained by mixing sodium carbonate (Na ), a raw material containing element A1, and a raw material containing element A2. The mixture was obtained so that the atomic ratio of Li to Si: Si / Li was 1.05. 2 CO 3 ) and potassium carbonate (K 2 CO 3 As a raw material containing element A2, aluminum oxide (Al 2 O 3 ) and boron oxide (B 2 O 3 The mixture was calcined at 800°C for 10 hours in an inert gas atmosphere to obtain a lithium silicate containing Na, K, Al, and B.

[0130] Composite particles containing a lithium silicate phase were prepared in the same manner as in Example 3, except that lithium silicate containing Na, K, Al, and B was used instead of lithium silicate containing Al and B. The contents of Li, Na, K, Al, and B in the composite particles were set to the values ​​shown in Table 1.

[0131] In this way, the element A1 (Na and K) was distributed almost uniformly in the depth direction of the composite particle. The X / Y ratio of the K concentration in the obtained composite particle was 1. The X / Y ratio of the Na concentration was also 1.

[0132] Test cells r4 to r5 and secondary batteries R4 to R5 were produced and evaluated in the same manner as in Example 1, except that the composite particles produced above were used.

[0133] The evaluation results are shown in Table 1. Table 1 also shows the X / Y ratio of the K concentration or Mg concentration. In E1 (e1) to E2 (e2), E4 (e4) to E5 (e5), and R4 (r4) to R5 (r5), K and Na were contained in the composite particles as element A1, but the X / Y ratio of the Na concentration was the same value as the X / Y ratio of the K concentration. The contents of Li, Na, K, Al, and B in the composite particles in Table 1 represent the mass ratio relative to the entire composite particles produced.

[0134]

[0135] In the examples, the reactivity of the composite particles was high, and the rate characteristics were improved (e1 to e5). In the examples, cracking of the composite particles was suppressed, and the deterioration of cycle characteristics due to particle cracking was suppressed (E1 to E5). In the comparative examples, the reactivity of the composite particles was low, and the rate characteristics were deteriorated (r1 to r5).

[0136] The secondary battery according to the present disclosure is useful as a main power source for mobile communication devices, portable electronic devices, and the like.

[0137] While the present invention has been described in terms of presently preferred embodiments, such disclosure is not to be interpreted as limiting. Various changes and modifications will no doubt become apparent to those skilled in the art to which the present invention pertains upon reading the above disclosure. It is therefore intended that the appended claims be interpreted to cover all changes and modifications that do not depart from the true spirit and scope of the invention.

[0138] 1: electrode group, 2: positive electrode lead, 3: negative electrode lead, 4: battery case, 5: sealing plate, 6: negative electrode terminal, 7: gasket, 8: sealing plug, 20: negative electrode active material, 21: ion-conducting phase, 22: silicon phase, 23: composite particle, 26: conductive layer

Claims

1. A negative electrode active material for a secondary battery comprising silicon-containing particles including an ion-conducting phase and a silicon phase dispersed within the ion-conducting phase, the silicon-containing particles including lithium and an element A1, the concentration of the element A1 being greater at the surface portion of the silicon-containing particles than at the interior portion thereof, and the element A1 being at least one element selected from the group consisting of alkali metal elements other than lithium and Group 2 elements of the long form periodic table.

2. The negative electrode active material for a secondary battery according to claim 1, wherein the element A1 is at least one selected from the group consisting of sodium, potassium, magnesium, and calcium.

3. The negative electrode active material for a secondary battery according to claim 1, wherein a concentration of the element A1 at a depth of 100 nm from the surface of the silicon-containing particle is X% by mass, and a concentration of the element A1 in the entire silicon-containing particle is Y% by mass, where X / Y is a ratio of 2 or more.

4. The negative electrode active material for a secondary battery according to claim 1, wherein the ion-conducting phase includes at least one phase selected from the group consisting of a silicate phase and a silicon oxide phase.

5. The silicate phase is Li 2 S 2 O 5 , Li 2 SiO 3 , and Li 4 SiO 4 The negative electrode active material for a secondary battery according to claim 4 , comprising at least one selected from the group consisting of:

6. The negative electrode active material for a secondary battery according to claim 1, wherein the silicon-containing particles contain element A2, and the element A2 is at least one selected from the group consisting of aluminum, boron, bismuth, antimony, germanium, zirconium, titanium, phosphorus, vanadium, tungsten, and lanthanum.

7. The negative electrode active material for a secondary battery according to claim 6, wherein the content of the element A2 in the silicon-containing particle is 0.01 mass % or more based on the entirety of the silicon-containing particle.

8. The negative electrode active material for a secondary battery according to claim 1, wherein the content of the silicon phase in the silicon-containing particle is 30 mass % or more and 90 mass % or less with respect to the entire silicon-containing particle.

9. The negative electrode active material for a secondary battery according to claim 1, wherein the crystallite size of the silicon phase is 20 nm or less.

10. The negative electrode active material for a secondary battery according to claim 1, wherein the silicon-containing particles have an average particle size of 4 μm or more and 15 μm or less.

11. Li is added to the surface of the silicon-containing particle. 2 CO 3 , Li 2 2. The negative electrode active material for a secondary battery according to claim 1, having at least one selected from the group consisting of O and LiOH attached thereto.

12. A secondary battery comprising a positive electrode, a negative electrode, and an electrolyte, wherein the negative electrode contains the negative electrode active material for secondary batteries according to claim 1.

13. The secondary battery described in claim 12, wherein the negative electrode comprises a negative electrode mixture layer containing the negative electrode active material for secondary batteries, and a negative electrode current collector supporting the negative electrode mixture layer, and the content of the silicon-containing particles in the negative electrode mixture layer is 1 mass % or more and 50 mass % or less with respect to the entire negative electrode mixture layer.

Citation Information

Patent Citations

  • Anode material, anode, battery, and their manufacturing method

    JP2009016245A

  • Negative electrode material for non-aqueous electrolyte secondary battery, and non-aqueous electrolyte secondary battery

    WO2022044454A1

  • Negative electrode active material for secondary batteries, negative electrode for secondary batteries, and secondary battery

    WO2022059340A1