Lithium primary battery
The lithium primary battery design with a specific magnesium content in the lithium alloy and capacity ratio addresses the issues of positive electrode deterioration and Mn deposition, enhancing both output and storage characteristics by stabilizing the negative electrode and reducing internal resistance.
Patent Information
- Application Number
- PCT/JP2024/018691
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-25
- Filing Date
- 2024-05-21
- Publication Date
- 2024-11-28
AI Technical Summary
Lithium primary batteries experience a decrease in output characteristics and an increase in internal resistance due to positive electrode deterioration and manganese (Mn) deposition on the negative electrode during long-term use, affecting their performance and storage characteristics.
A lithium primary battery design featuring a positive electrode with manganese dioxide and a negative electrode made of a lithium alloy containing 0.02% to 11% magnesium, with a capacity ratio of the negative electrode to the positive electrode (N/P) between 0.85 and 1.00, which suppresses Mn precipitation and internal resistance, and maintains output characteristics.
The battery effectively suppresses the decrease in output characteristics and increase in internal resistance, ensuring improved storage and output performance by controlling the Mn precipitation and maintaining the integrity of the negative electrode.
Smart Images

Figure JP2024018691_28112024_PF_FP_ABST
Abstract
Description
Lithium primary battery
[0001] The present disclosure relates to lithium primary batteries.
[0002] Lithium primary batteries have a high energy density and low self-discharge, and are therefore used as power sources for many electronic devices. A lithium primary battery includes a positive electrode, a negative electrode, a separator disposed between the positive and negative electrodes, and a nonaqueous electrolyte. The positive electrode is typically made of manganese dioxide. The negative electrode is typically made of, for example, sheet-shaped (foil-shaped) lithium metal or a lithium alloy.
[0003] Patent Document 1 discloses a "non-aqueous electrolyte battery comprising an electrode plate assembly in which a strip-shaped negative electrode made of a light metal, a strip-shaped positive electrode having a positive electrode mixture supported on a current collector, and a separator separating the two electrodes are spirally wound, and a cylindrical case for accommodating the electrode plate assembly, wherein the positive electrode plate has a thin strip-shaped insulator attached to its surface in the longitudinal direction." Patent Document 1 also discloses that "the ratio of the theoretical capacity of the positive electrode active material to the theoretical capacity of the negative electrode is within the range of 1:0.9 to 1.1."
[0004] Patent Document 2 discloses a cylindrical non-aqueous electrolyte battery that houses, in a bottomed cylindrical outer can with an upper opening, a wound electrode body formed by winding a sheet-like positive electrode and a sheet-like negative electrode with a separator interposed therebetween, and a non-aqueous electrolyte, wherein the negative electrode uses a metal foil as a current collector, metallic lithium or a lithium alloy is disposed on one or both sides of the metal foil, the metallic lithium or lithium alloy is partially or not compressed onto the metal foil, and the ratio of the negative electrode capacity to the positive electrode capacity is negative electrode capacity / positive electrode capacity = 0.93 to 1.03.
[0005] Japanese Patent Laid-Open No. 9-134729 Japanese Patent Laid-Open No. 2005-149961
[0006] At the end of discharge, the output characteristics may decrease due to deterioration of the positive electrode. Furthermore, during long-term use of the battery, Mn may leach from the positive electrode and deposit on the negative electrode, causing an increase in internal resistance.
[0007] One aspect of the present disclosure relates to a lithium primary battery including a positive electrode, a negative electrode, a separator disposed between the positive electrode and the negative electrode, and a non-aqueous electrolyte, wherein the positive electrode contains manganese dioxide, the negative electrode contains a lithium alloy, and the lithium alloy contains 0.02 mass % or more and 11 mass % or less of magnesium, and a ratio N / P of a capacity N of the negative electrode to a capacity P of the positive electrode is 0.85 or more and 1.00 or less.
[0008] According to the present disclosure, it is possible to suppress the deterioration of output characteristics at the end of discharge and to suppress the increase in internal resistance during long-term use.
[0009] The novel features of the present invention are set forth in the appended claims, but the present invention, both in terms of structure and content, together with other objects and features of the present invention, will be better understood from the following detailed description taken in conjunction with the drawings.
[0010] FIG. 1 is a partially cross-sectional front view of a lithium primary battery according to an embodiment of the present disclosure.
[0011] The following describes embodiments of the present disclosure using examples, but the present disclosure is not limited to the examples described below. In the following description, specific numerical values and materials may be exemplified, but other numerical values and materials may be applied as long as the effects of the present disclosure are obtained. In this specification, the term "numerical value A to numerical value B" includes numerical value A and numerical value B and can be read as "numerical value A or more and numerical value B or less." In the following description, when lower and upper limits are exemplified for numerical values of specific physical properties or conditions, any of the exemplified lower limits and any of the exemplified upper limits can be arbitrarily combined, as long as the lower limit is not equal to or greater than the upper limit. When multiple materials are exemplified, one of the materials may be selected and used alone, or two or more materials may be used in combination.
[0012] A lithium primary battery according to an embodiment of the present disclosure includes an electrode group and a nonaqueous electrolyte. The electrode group includes a positive electrode, a negative electrode, and a separator disposed between the positive electrode and the negative electrode. The positive electrode includes manganese dioxide as a positive electrode active material. The negative electrode includes a lithium alloy as a negative electrode active material. The lithium alloy includes 0.02 mass% or more and 11 mass% or less of magnesium. The ratio N / P of the negative electrode capacity N to the positive electrode capacity P is 0.85 or more and 1.00 or less.
[0013] The electrode group may be a wound type, i.e., a strip-shaped positive electrode and a strip-shaped negative electrode may be spirally wound with a separator interposed therebetween. The electrode group may be a stacked type, i.e., a positive electrode and a negative electrode may be stacked with a separator interposed therebetween.
[0014] By having an N / P ratio of 1 or less, the depth of discharge of the positive electrode at the end of discharge (the ratio of the amount of discharged electricity to the positive electrode capacity P) is reduced, deterioration of the positive electrode at the end of discharge is suppressed, and a decrease in output characteristics (e.g., low-temperature pulse discharge characteristics) due to deterioration of the positive electrode is suppressed. Furthermore, by using a lithium alloy containing 0.02 mass% or more of Mg as the negative electrode active material, Mn eluted from the positive electrode during long-term use of the battery is suppressed from precipitating at the negative electrode, and an increase in internal resistance (deterioration of storage characteristics) due to Mn precipitation at the negative electrode is suppressed. When the N / P ratio is 1 or less, the amount of positive electrode relative to the negative electrode is large, so the amount of Mn eluted from the positive electrode during long-term use of the battery is large. However, even in this case, the use of the above-mentioned lithium alloy can sufficiently suppress Mn precipitation at the negative electrode and the resulting increase in internal resistance (deterioration of storage characteristics).
[0015] However, if the N / P ratio is below 0.85, the voids inside the battery become smaller, the amount of electrolyte contained in the electrode group decreases, and the output characteristics may deteriorate. Furthermore, since the amount of Mn eluted from the positive electrode becomes very large, even if 0.02% by mass or more of Mg is added, the storage characteristics may deteriorate. Furthermore, if the Mg content in the lithium alloy exceeds 11% by mass, the proportion of Mg in the negative electrode increases, the negative electrode resistance increases (the initial internal resistance increases), and the output characteristics may deteriorate. In this case, the proportion of Li in the negative electrode decreases, and the absolute amount of Li decreases, which may result in a decrease in discharge capacity.
[0016] If the N / P ratio exceeds 1.00, even if 0.02 mass % or more of Mg is added, the deterioration of the positive electrode at the end of discharge is significant, and output characteristics may be reduced.
[0017] (N / P ratio) From the viewpoint of improving storage characteristics, the N / P ratio is preferably 0.90 or more. From the viewpoint of improving output characteristics, the N / P ratio may be less than 1, and is preferably 0.95 or less. Furthermore, when the N / P ratio is less than 1 or 0.95 or less, the amount of Mn eluted from the positive electrode increases, and therefore, the effect of suppressing Mn precipitation in the negative electrode by using the lithium alloy of the present disclosure can be more significantly obtained.
[0018] The positive electrode capacity P is a capacity theoretically determined based on the amount of positive electrode active material in the positive electrode, and is determined by multiplying the mass of manganese dioxide contained in the positive electrode by the theoretical capacity (308 mAh) per gram of manganese dioxide.
[0019] The mass of manganese dioxide contained in the positive electrode is the mass of manganese dioxide filled into the positive electrode when the positive electrode is produced, and may be determined as follows. The positive electrode is removed from an undischarged (before use) battery, washed with a nonaqueous solvent (e.g., 1,2-dimethoxyethane), and dried to remove any nonaqueous electrolyte adhering to the positive electrode. A positive electrode mixture is sampled from the positive electrode, and its mass M1 is determined. Thereafter, the sampled positive electrode mixture is dissolved in an acid solution and filtered, and the residue is washed with water and dried, and its mass M2 is determined. The mass of (M1 - M2) is determined as the mass of manganese dioxide.
[0020] The negative electrode capacity N is a capacity theoretically determined based on the amount of negative electrode active material (lithium amount) in the negative electrode, and is determined by multiplying the mass of lithium contained in the negative electrode by the theoretical capacity per gram of lithium (3861 mAh).
[0021] The mass of lithium contained in the negative electrode can be determined as follows. The negative electrode (lithium alloy) is removed from an undischarged (unused) battery, washed with a nonaqueous solvent (e.g., 1,2-dimethoxyethane), and dried to remove any nonaqueous electrolyte adhering to the negative electrode. The mass of the negative electrode is measured, and then the negative electrode is dissolved in an acid solution and the lithium content (mass%) in the negative electrode is measured by inductively coupled plasma (ICP) atomic emission spectrometry. The mass of lithium contained in the negative electrode is determined based on the measured mass of the negative electrode and the lithium content in the negative electrode. The object to be measured may be the negative electrode (lithium alloy) used during battery production. When the negative electrode includes a negative electrode current collector supporting lithium alloy foil, the lithium alloy foil is separated from the negative electrode current collector, and the amount of lithium contained in the lithium alloy foil is determined.
[0022] (Lithium Alloy) The negative electrode contains a lithium alloy, and the lithium alloy contains 0.02 to 11 mass % of Mg. From the viewpoint of reducing internal resistance and ensuring capacity, the Li content in the lithium alloy may be 89 mass % or more, or may be 95 mass % or more.
[0023] The lithium alloy preferably contains at least 0.02 mass % or more of Mg and further contains Al from the viewpoint of improving output voltage. Hereinafter, a lithium alloy containing Mg but substantially no Al will also be referred to as a "Li-Mg alloy." A lithium alloy containing Mg and Al will also be referred to as a "Li-Mg-Al alloy." Note that "substantially no Al" means that the amount of Al is below the detection limit in composition analysis of the lithium alloy (e.g., ICP atomic emission spectroscopy, atomic absorption spectroscopy, etc.).
[0024] When the lithium alloy contains Al, a low-resistance coating is formed. When the lithium alloy contains Mg together with Al, uneven consumption of Li due to segregation of Al is suppressed. In this case, the effects of Mg and Al are stably obtained throughout the negative electrode, and Li is uniformly consumed on the surface of the negative electrode, resulting in a larger proportion of Li that can contribute to the discharge reaction at the end of discharge. In a lithium alloy with an Mg content of 0.02% by mass or more, the effect of adding Al is more pronounced than in the case of a lithium alloy or lithium metal with an Mg content of less than 0.02% by mass, and a low-resistance coating is easily formed stably, the output voltage at the end of discharge is further increased, and the increase in internal resistance during long-term use is further suppressed.
[0025] From the viewpoint of improving storage characteristics, the Mg content in the lithium alloy is preferably 0.1% by mass or more, more preferably 0.2% by mass or more, and even more preferably 0.3% by mass or more. From the viewpoint of improving output characteristics, the Mg content in the lithium alloy is preferably 8% by mass or less, more preferably 5% by mass or less, and even more preferably 3% by mass or less. The Mg content in the lithium alloy may be, for example, 0.02% by mass or more and 3% by mass or less, or 0.3% by mass or more and 3% by mass or less. The Mg content in the above lithium alloy is the Mg content in a Li-Mg alloy or a Li-Mg-Al alloy.
[0026] The Al content in the lithium alloy (Li-Mg-Al alloy) is preferably 0.01% by mass or more and 0.5% by mass or less, more preferably 0.01% by mass or more and 0.35% by mass or less. When the Al content is 0.01% by mass or more, the above-mentioned effects of adding Al are easily obtained. When the Al content is 0.5% by mass or less, it is easy to reduce the negative electrode resistance (internal resistance) and ensure the flexibility of the negative electrode. The total content of Mg and Al in the Li-Mg-Al alloy may be 0.03% by mass or more and 11.5% by mass or less (or 11% by mass or less), 0.2% by mass or more and 5% by mass or less, or 0.4% by mass or more and 4% by mass or less. In the case of a Li-Mg-Al alloy, the mass ratio of Mg to Al: Mg / Al may be, for example, in the range of 0.02 / 0.5 (or 0.3 / 0.5) to 3 / 0.01.
[0027] The lithium alloy may contain metal elements other than Li, Mg, and Al. Examples of the other metal elements include Sn, Ni, Pb, In, K, Na, Ca, and Zn. From the viewpoint of ensuring discharge capacity and stabilizing internal resistance, the total content of metal elements other than lithium contained in the lithium alloy is preferably 11 mass% or less.
[0028] The composition of the lithium alloy can be determined by inductively coupled plasma (ICP) emission spectroscopy or atomic absorption spectroscopy (AAS).
[0029] The structure and shape of the lithium primary battery are not particularly limited. The lithium primary battery may include, for example, a wound electrode group configured by spirally winding a strip-shaped positive electrode and a strip-shaped negative electrode with a separator interposed therebetween. The wound electrode group may be cylindrical or flat. The shape of the lithium primary battery may be cylindrical or prismatic. The cylindrical battery may have a spiral structure or an inside-out structure. The lithium primary battery may also be, for example, a coin-type battery including a stacked electrode group configured by stacking a disc-shaped positive electrode and a disc-shaped negative electrode with a separator interposed therebetween.
[0030] The lithium primary battery of the present disclosure will be described in more detail below.
[0031] (Negative Electrode) The negative electrode may include, for example, a foil (sheet) of a lithium alloy. The lithium alloy is formed into any shape and thickness depending on the shape, dimensions, performance specifications, etc. of the lithium primary battery.
[0032] The negative electrode used in the wound electrode group may include a negative electrode current collector (e.g., copper foil) supporting a lithium alloy, or may be a foil (sheet) lithium alloy without a negative electrode current collector. When the lithium alloy contains Mg, the relatively high strength of Mg remains at the end of discharge, allowing the negative electrode to be constructed using only a foil (sheet) lithium alloy without a negative electrode current collector. By using a lithium alloy containing 0.02 mass% or more of Mg, breakage or partial loss of the negative electrode at the end of discharge when the negative electrode does not include a negative electrode current collector is suppressed. The shape of the negative electrode (lithium alloy) is maintained even at the end of discharge, and the conductivity of the entire negative electrode is ensured even without a negative electrode current collector.
[0033] In the case of coin-type batteries, a hoop-shaped lithium alloy may be punched into a disk shape and used as the negative electrode. In the case of cylindrical batteries, a sheet-shaped lithium alloy may be used as the negative electrode. The sheet may be obtained, for example, by extrusion molding. More specifically, in cylindrical batteries, a lithium alloy foil or the like having a shape with a longitudinal direction and a lateral direction is used.
[0034] (Positive Electrode) The positive electrode contains manganese dioxide as a positive electrode active material. As the manganese dioxide, calcined electrolytic manganese dioxide is preferably used. A positive electrode containing manganese dioxide exhibits a relatively high voltage and is advantageous in terms of improving discharge characteristics (pulse discharge characteristics). It may also contain chemical manganese dioxide. The manganese dioxide may be in a mixed crystal state containing multiple types of crystal states.
[0035] The positive electrode includes, for example, a strip-shaped positive electrode current collector and a positive electrode mixture layer held on the positive electrode current collector. The positive electrode mixture layer is formed, for example, by applying a wet positive electrode mixture to the surface of the sheet-shaped positive electrode current collector or by filling the positive electrode current collector with the wet positive electrode mixture, pressing the positive electrode mixture in the thickness direction, and drying the sheet-shaped positive electrode current collector.
[0036] The positive electrode mixture may contain a positive electrode active material, a binder, a conductive agent, etc. Examples of the binder include fluororesin such as polytetrafluoroethylene, rubber particles, and acrylic resin. Examples of the conductive agent include a conductive carbon material. Examples of the conductive carbon material include natural graphite, artificial graphite, carbon black, and carbon fiber.
[0037] Examples of materials for the positive electrode current collector include stainless steel, aluminum, and titanium. The positive electrode current collector is preferably a perforated current collector. Examples of perforated current collectors include expanded metal, net, and punched metal.
[0038] In the case of a coin-type battery, the positive electrode may be constructed by attaching a ring-shaped positive electrode current collector having an L-shaped cross section to a positive electrode mixture pellet, or by using only the positive electrode mixture pellet. The positive electrode mixture pellet can be obtained, for example, by compression-molding a wet positive electrode mixture prepared by adding an appropriate amount of water to a positive electrode active material, etc., and then drying the resulting mixture.
[0039] In the case of a cylindrical battery with a spiral structure, a positive electrode including a sheet-shaped positive electrode current collector and a positive electrode mixture layer supported on the positive electrode current collector can be used. The sheet-shaped positive electrode current collector is preferably a perforated current collector. Examples of perforated current collectors include expanded metal, netting, and punched metal. The positive electrode mixture layer can be obtained, for example, by applying the above-mentioned wet positive electrode mixture to the surface of the sheet-shaped positive electrode current collector or by filling the positive electrode current collector with the wet positive electrode mixture, pressing it in the thickness direction, and drying it. In the case of a cylindrical battery with an inside-out structure, a hollow cylindrical positive electrode mixture pellet can be used as the positive electrode.
[0040] (Non-aqueous electrolyte) The non-aqueous electrolyte contains, for example, a non-aqueous solvent and a lithium salt. The concentration of lithium ions contained in the non-aqueous electrolyte (total concentration of the lithium salt) is, for example, 0.2 mol / L or more and 2.0 mol / L or less, and may be 0.3 mol / L or more and 1.5 mol / L or less.
[0041] Examples of non-aqueous solvents include organic solvents that are commonly used in non-aqueous electrolytes for lithium primary batteries. Examples of non-aqueous solvents include ethers, esters, and carbonate esters. Examples of non-aqueous solvents that can be used include dimethyl ether, γ-butyl lactone, propylene carbonate (PC), ethylene carbonate (EC), dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, 1,2-dimethoxyethane (DME), 1,2-diethoxyethane, methyl acetate, ethyl acetate, and propyl acetate. The non-aqueous electrolyte may contain one non-aqueous solvent or two or more non-aqueous solvents.
[0042] From the viewpoint of improving the discharge characteristics of a lithium primary battery, the nonaqueous solvent preferably contains a cyclic carbonate having a high boiling point and a chain ether having low viscosity even at low temperatures. The cyclic carbonate preferably contains at least one selected from the group consisting of PC and EC, with PC being particularly preferred. The chain ether preferably contains DME.
[0043] Examples of the lithium salt include lithium salts used as solutes in lithium primary batteries. Examples of such lithium salts include LiCF 3 SO 3 , LiClO 4 , LiBF 4 , LiPF 6 , LiRaSO 3 (Ra is a fluorinated alkyl group having 1 to 4 carbon atoms), LiFSO 3 , LiN(SO 2 Rb)(SO 2 Rc) (Rb and Rc each independently represent a fluorinated alkyl group having 1 to 4 carbon atoms), LiN(FSO 2 ) 2 , LiN(SO 2 CF 3 ) 2 , LiN(SO 2 F) (POF 2 ), LiPO 2 F 2 , LiB(C 2 O 4 ) 2 , LiBF 2 (C2 O 4 Among them, from the viewpoint of stability with respect to lithium alloys containing Mg (or Mg and Al), LiCF 3 SO 3 , LiBF 4 , and LiN(FSO 2 ) 2 The non-aqueous electrolyte may contain one or more of these lithium salts.
[0044] The nonaqueous electrolyte may further contain other components such as the additives described above. Examples of other components besides the additives include propane sultone, propene sultone, ethylene sulfite, 3,2-dioxathiolane-2,2-dioxide, vinylene carbonate, vinylethylene carbonate, fluoroethylene carbonate, adiponitrile, succinonitrile, and succinic anhydride. The other components may be lithium salts or may be capable of generating lithium ions.
[0045] (Separator) A lithium primary battery usually includes a separator interposed between the positive electrode and the negative electrode. As the separator, a porous sheet formed of an insulating material that is resistant to the internal environment of a lithium primary battery may be used. Specific examples include a synthetic resin nonwoven fabric, a synthetic resin microporous membrane, or a laminate thereof.
[0046] Examples of synthetic resins used for nonwoven fabrics include polypropylene, polyphenylene sulfide, and polybutylene terephthalate. Examples of synthetic resins used for microporous membranes include polyolefin resins such as polyethylene, polypropylene, and ethylene-propylene copolymers. The microporous membrane may contain inorganic particles as needed.
[0047] The thickness of the separator is, for example, 5 μm or more and 100 μm or less.
[0048] A partially cross-sectional front view of a lithium primary battery according to one embodiment of the present invention is shown in Fig. 1. Fig. 1 shows an example of a lithium primary battery, and the lithium primary battery according to the present disclosure is not limited to this.
[0049] The cylindrical lithium primary battery 10 includes a cylindrical case 100 (battery can) with a bottom, a wound electrode group 200 housed in the case 100, and a sealing plate 300 that closes the opening of the case 100. Examples of materials for the case include stainless steel, nickel-plated steel, iron, titanium, and aluminum. The sealing plate 300 is fixed to the case 100 near the opening by welding. An opening is formed in the center of the sealing plate 300, and an external terminal 330 is disposed in this opening. An insulating gasket 310 is disposed between the external terminal 330 and the sealing plate 300. The electrode group 200 is housed inside the case 100 together with a nonaqueous electrolyte (not shown). To prevent internal short circuits, an upper insulating plate 230A and a lower insulating plate 230B are disposed on the upper and lower parts of the electrode group 200, respectively.
[0050] The electrode group 200 is formed by spirally winding a strip-shaped positive electrode 201 and a strip-shaped negative electrode 202 with a separator 203 interposed therebetween. A negative electrode lead 210 is connected to the negative electrode 202. The negative electrode lead 210 is connected to an external terminal 330 (negative electrode terminal) by welding or the like. A positive electrode lead 220 is connected to the positive electrode 201. The positive electrode lead 220 is connected to the inner bottom surface of the case 100 by welding or the like.
[0051] The negative electrode 202 includes at least a foil-shaped (or sheet-shaped) lithium alloy. The lithium alloy contains 0.02 to 11 mass % of Mg. The ratio N / P of the capacity N of the negative electrode 202 to the capacity P of the positive electrode 201 is 0.85 to 1.00. The positive electrode 201 is disposed at the outermost periphery of the electrode assembly 200.
[0052] Although the external terminal in Fig. 1 is used as a negative electrode terminal, it may also be used as a positive electrode terminal. That is, the positive electrode lead may be connected to the external terminal, and the negative electrode lead may be connected to the inner bottom surface of the battery case. Also, in Fig. 1, the positive electrode and negative electrode are spirally wound so that the positive electrode is disposed at the outermost periphery of the electrode group, but the positive electrode and negative electrode may also be spirally wound so that the negative electrode is disposed at the outermost periphery of the electrode group.
[0053] <<Appendix>> The above embodiments disclose the following technologies. (Technology 1) A lithium primary battery comprising a positive electrode, a negative electrode, a separator disposed between the positive electrode and the negative electrode, and a non-aqueous electrolyte, wherein the positive electrode contains manganese dioxide, and the negative electrode contains a lithium alloy, the lithium alloy containing 0.02% by mass or more and 11% by mass or less of magnesium, and the ratio of the capacity of the negative electrode to the capacity of the positive electrode is 0.85 or more and 1.00 or less. (Technology 2) The lithium primary battery according to Technology 1, wherein the lithium alloy contains aluminum, the content of the magnesium in the lithium alloy is 0.02% by mass or more and 3% by mass or less, and the content of the aluminum in the lithium alloy is 0.01% by mass or more and 0.5% by mass or less. (Technology 3) The lithium primary battery according to Technology 1 or 2, wherein the strip-shaped positive electrode and the strip-shaped negative electrode are spirally wound with the separator interposed therebetween. (Technology 4) The lithium primary battery according to Technology 3, wherein the negative electrode is the lithium alloy in a foil form, and does not include a negative electrode current collector.
[0054] [Examples] Hereinafter, the present disclosure will be specifically described based on examples and comparative examples, but the present disclosure is not limited to the following examples.
[0055] Batteries A1 to A28 and Batteries B1 to B50 (Preparation of Negative Electrodes) Lithium metal foil or lithium alloy foil was cut to obtain strip-shaped negative electrodes (147 mm long, 40 mm wide). The thickness of the negative electrode of Battery A1 was 0.3 mm. The thickness of the negative electrode of each battery other than Battery A1 was adjusted appropriately so that the amount of lithium in the negative electrode was the same as that of Battery A1. The elements other than Li contained in the lithium alloy foil were Mg and / or Al. Li-Mg alloy foil, Li-Al alloy foil, or Li-Mg-Al alloy foil was used as the lithium alloy foil. Note that Li-Al alloy refers to a lithium alloy containing Al but substantially free of Mg. "Substantially free of Mg" means that the amount of Mg is below the detection limit in compositional analysis of the lithium alloy (e.g., ICP atomic emission spectroscopy). The Mg content in the Li-Mg alloy foil was as shown in Tables 1 and 2. The Al content in the Li-Al alloy foil was set to the value shown in Table 3. The Mg content and Al content in the Li-Mg-Al alloy were set to the values shown in Table 4. In batteries A1 to A16 in Table 2, the Li content in the Li-Mg alloy was 89 mass % or more. In batteries A17 to A28 in Table 4, the Li content in the Li-Mg-Al alloy was 89 mass % or more.
[0056] One end of a nickel negative electrode lead was connected to a predetermined position on the negative electrode by pressure welding.
[0057] (Preparation of Positive Electrode) 100 parts by mass of the positive electrode active material were mixed with 5 parts by mass of Ketjen Black as a conductive agent, 5 parts by mass of polytetrafluoroethylene as a binder, and an appropriate amount of pure water to prepare a wet positive electrode mixture. Electrolytic manganese dioxide (MnO) that had been baked at 400°C for 5 hours was used as the positive electrode active material. 2 ) was used.
[0058] Next, the positive electrode mixture was filled into a positive electrode current collector made of stainless steel expanded metal (height 0.2 mm) to prepare a positive electrode precursor. The positive electrode precursor was then dried, rolled by a roll press, and cut to obtain a strip-shaped positive electrode (length 185 mm, width 42 mm). The active material density of the positive electrode was 2.7 g / cm. 3 Subsequently, a part of the filled positive electrode mixture was peeled off, and one end of a stainless steel positive electrode lead was resistance-welded to the exposed part of the positive electrode current collector.
[0059] The negative electrode capacity N was kept constant, and the positive electrode capacity P was appropriately adjusted to obtain the N / P ratios shown in Tables 1 to 4. The positive electrode capacity P was adjusted by changing the thickness of the positive electrode (the amount of positive electrode mixture filled into the positive electrode current collector). The opposing area of the negative electrode and positive electrode was kept constant. The N / P ratio was calculated using the negative electrode capacity N and positive electrode capacity P determined by the method described above.
[0060] (Preparation of Electrode Assembly) An electrode assembly was prepared by winding a positive electrode and a negative electrode with a separator interposed therebetween. The positive electrode was disposed on the outermost periphery of the electrode assembly. A 25 μm thick microporous polypropylene film was used as the separator.
[0061] (Preparation of non-aqueous electrolyte) LiCF was dissolved in a mixed solvent of propylene carbonate (PC), ethylene carbonate (EC), and 1,2-dimethoxyethane (DME) (volume ratio 25:25:50). 3 SO 3 was dissolved in the solution at a concentration of 0.6 mol / L to prepare a non-aqueous electrolyte solution.
[0062] (Assembly of Lithium Primary Battery) The electrode group was housed in a stainless steel, bottomed, cylindrical case (outer diameter 17.5 mm, height 50.5 mm) that also served as a positive electrode terminal. An upper insulating plate and a lower insulating plate were placed on the upper and lower end surfaces of the electrode group, respectively. The other end of the positive electrode lead was connected to the inner surface of the bottom of the case by resistance welding. A sealing plate equipped with an external terminal (negative electrode terminal) was prepared. A gasket was interposed between the sealing plate and the external terminal. The other end of the negative electrode lead was connected to the external terminal by resistance welding. A nonaqueous electrolyte was injected into the battery case, and then the open end of the case and the periphery of the sealing plate were laser welded, and the opening of the case was sealed with the sealing plate. In this way, a lithium primary battery (Battery A1) with the structure shown in Figure 1 was fabricated. The battery immediately after assembly was aged for 7 days in an atmosphere at 45°C. Note that A1 to A28 in the table are batteries of the example. B1 to B50 are comparative example batteries.
[0063] The following evaluations were carried out on each of the obtained batteries.
[0064] [Evaluation] (Pulse Discharge Characteristics (Output Characteristics)) The aged batteries were subjected to constant current discharge at 20 mA in an environment of 23±2°C until the depth of discharge (DOD) reached 80% (until the discharged quantity of electricity reached 80% of the negative electrode capacity). The batteries with a DOD of 80% were left in an environment of -40°C for 4 hours or more, and then pulse discharged at 150 mA for 5 seconds in an environment of -40°C, and the minimum voltage at this time was determined. If the minimum voltage was 2 V or higher, the pulse discharge characteristics (output characteristics) were determined to be good.
[0065] (Storage characteristics) After pulse discharge, a load of 100 kΩ was connected to the battery in an environment of 60° C., and the internal resistance was measured every 5 days to determine the storage period until the internal resistance reached 0.5 Ω. If the storage period was 100 days or more, it was determined that the storage characteristics were good.
[0066] The evaluation results are shown in Tables 1 to 4. Table 3 also shows the results of B1 to B6 in Table 1. Table 4 also shows the results of A5 to A8 and B21 to B22 in Table 2.
[0067]
[0068]
[0069]
[0070]
[0071] When the Mg content in the lithium alloy was 0.02 to 11 mass% and the N / P ratio was 0.85 to 1, excellent output characteristics and storage characteristics were simultaneously obtained (A1 to A28). In particular, when the Mg content was 0.02 to 3 mass%, the Al content was 0.01 to 0.5 mass%, and the N / P ratio was 0.85 to 1, the output characteristics and storage characteristics were further improved (A17 to A28). Note that, although the Li-Mg-Al alloy of this example (Table 4) shows a case where the Mg content was 0.3 mass%, similar effects to those of this example can be obtained if the Mg content is in the range of 0.02 to 11 mass% (preferably 0.02 to 3 mass%).
[0072] As shown in Table 3, when the N / P ratio was 0.85 to 1 and no Mg was added, the addition of Al produced little or no improvement in power output and storage characteristics (B2 to B5 → B28 to B31, B34 to B37, B40 to B43). On the other hand, as shown in Table 4, when the N / P ratio was 0.85 to 1 and the Mg content was 0.02 mass% or more, the addition of Al produced significant improvements in power output and storage characteristics (A5 to A8 → A17 to A20, A21 to A24, A25 to A28). This indicates that the improvement in power output and storage characteristics due to the addition of Al is particularly pronounced when the lithium alloy contains Mg.
[0073] When the N / P ratio was less than 0.85, the thickness of the positive electrode increased, the remaining space inside the battery decreased, the amount of electrolyte contained in the electrode group decreased, and the output characteristics deteriorated. When the N / P ratio was more than 1, the depth of discharge of the positive electrode at the end of discharge increased, the internal resistance increased due to deterioration of the positive electrode, and the output characteristics deteriorated. When the N / P ratio was less than 0.85, even when 0.02 mass% or more of Mg was added, the amount of Mn eluted from the positive electrode increased, and the storage characteristics deteriorated.
[0074] When Li metal foil, Li-Mg alloy foil with a Mg content of less than 0.02% by mass, or Li-Al alloy foil was used, Mn precipitation at the negative electrode was not suppressed, resulting in a deterioration in storage characteristics. When the negative electrode was Li metal foil, Li-Mg alloy foil with a Mg content of less than 0.02% by mass, or Li-Al alloy foil and did not include a negative electrode current collector, a small N / P ratio made foil breakage more likely at the end of discharge, resulting in a deterioration in output characteristics. When the Mg content exceeded 11% by mass, the negative electrode resistance (initial internal resistance) increased, resulting in a deterioration in output characteristics and storage characteristics.
[0075] The lithium primary battery of the present disclosure is suitable for use, for example, as a main power source or memory backup power source for various meters (for example, smart meters for electricity, water, gas, etc.).
[0076] While the present invention has been described in terms of presently preferred embodiments, such disclosure is not to be interpreted as limiting. Various changes and modifications will no doubt become apparent to those skilled in the art to which the present invention pertains upon reading the above disclosure. It is therefore intended that the appended claims be interpreted to cover all changes and modifications that do not depart from the true spirit and scope of the invention.
[0077] 10: Lithium primary battery, 100: Case, 200: Electrode group, 201: Positive electrode, 202: Negative electrode, 203: Separator, 210: Negative electrode lead, 220: Positive electrode lead, 230A: Upper insulating plate, 230B: Lower insulating plate, 300: Sealing plate, 310: Gasket, 330: External terminal
Claims
1. A lithium primary battery comprising: a positive electrode, a negative electrode, a separator disposed between the positive electrode and the negative electrode, and a non-aqueous electrolyte; the positive electrode contains manganese dioxide; the negative electrode contains a lithium alloy; the lithium alloy contains 0.02 mass % or more and 11 mass % or less of magnesium; and a ratio of a capacity N of the negative electrode to a capacity P of the positive electrode: N / P is 0.85 or more and 1.00 or less.
2. The lithium primary battery according to claim 1, wherein the lithium alloy contains aluminum, the magnesium content in the lithium alloy is 0.02% by mass or more and 3% by mass or less, and the aluminum content in the lithium alloy is 0.01% by mass or more and 0.5% by mass or less.
3. The lithium primary battery according to claim 1, wherein the strip-shaped positive electrode and the strip-shaped negative electrode are spirally wound with the separator interposed therebetween.
4. The lithium primary battery according to claim 3, wherein the negative electrode is a foil of the lithium alloy without including a negative electrode current collector.
Citation Information
Patent Citations
Nonaqueous electrolyte battery
JP1997134729A
Improved lithium cathode
JP1983209862A
Nonaqueous electrolyte battery
JP1995022069A
Non-aqueous electrolyte battery
JP2005149961A
Electrode material in the form of a lithium-based alloy and a method for producing same - Patent Application 20070122997
JP2020530937A