Positive electrode material, and positive electrode slurry, positive electrode, and lithium secondary battery comprising same
By combining small particle cathode active materials with perlithium manganese-based oxide and lithium transition metal oxides, the challenges of rate characteristics and electrode density in lithium secondary batteries are addressed, resulting in improved energy density and manufacturing efficiency.
Patent Information
- Application Number
- PCT/KR2024/005282
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-04-18
- Filing Date
- 2024-04-19
- Publication Date
- 2024-11-28
AI Technical Summary
Lithium secondary batteries using perlithium manganese-based oxide as a cathode material face limitations in rate characteristics and electrode density due to high BET specific surface area, leading to increased slurry viscosity and particle breakage during rolling.
Incorporating a small particle cathode active material in the form of single or quasi-single particles with perlithium manganese-based oxide, adjusting the D50 value to enhance surface area and stability, and using a lithium transition metal oxide to create a two-phase crystal structure, reducing cobalt content and improving manufacturing costs.
This approach increases electrode density, reduces particle breakage, and maintains high capacity while lowering resistance and viscosity, enabling easier rolling and higher energy density with reduced manufacturing costs.
Smart Images

Figure KR2024005282_28112024_PF_FP_ABST
Abstract
Description
Cathode material, cathode slurry containing same, cathode and lithium secondary battery
[0001] Cross-citation with related application(s)
[0002] This application claims the benefit of priority to Korean Patent Application No. 10-2023-0065296, filed May 19, 2023, and Korean Patent Application No. 10-2024-0052072, filed April 18, 2024, the entire contents of which are incorporated herein by reference.
[0003] The present disclosure relates to a cathode material comprising a lithium manganese oxide having a D50 value higher than a certain value as an opposing electrode, a lithium transition metal oxide in the form of a single particle or a pseudo-single particle as a small particle, and a cathode slurry, a cathode, and a lithium secondary battery having improved physical properties by including the cathode material.
[0004] Recently, as the application areas of lithium secondary batteries have rapidly expanded to include not only power supply for electronic devices such as electric, electronic, communication, and computer devices, but also power storage for large-area devices such as automobiles and power storage devices, the demand for high-capacity, high-output, and high-stability secondary batteries is increasing.
[0005] The above lithium secondary battery is generally composed of a positive electrode containing a positive electrode active material, a negative electrode containing a negative electrode active material, an electrolyte that serves as a medium for transferring lithium ions, and a separator. At this time, carbon-based active materials, silicon-based active materials, etc. can be used as the negative electrode active material. In addition, lithium transition metal oxides such as lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), and lithium nickel-cobalt-manganese composite oxide having a layered structure can be used as the positive electrode active material.
[0006] Recently, lithium manganese-rich oxides (LiMnO) have been attracting attention as next-generation cathode active materials. LiMnO is relatively inexpensive and contains a high amount of abundant manganese (Mn), which offers the advantage of high capacity. However, these LiMnOs suffer from compositional limitations, such as low rate characteristics. Therefore, efforts have been made to improve this by manufacturing small primary particles to increase the BET surface area of the secondary particles. However, applying these large-surface-area cathode active materials can lead to another problem: a lower rolling density of the cathode.
[0007] To solve this problem, a method of strengthening surface stability by coating metal oxides on the surface of the positive electrode lithium manganese oxide has been mainly introduced, but this has been pointed out as a limitation due to problems such as further deterioration of the rate characteristics.
[0008] The present disclosure provides a cathode material for a lithium secondary battery with enhanced electrode density and particle durability by mixing a single-particle type small-particle cathode active material together with a lithium manganese oxide as a cathode material.
[0009] In addition, the present disclosure provides a cathode slurry for a lithium secondary battery having an increased solid content while maintaining an appropriate viscosity by including the cathode material as described above.
[0010] In addition, the present disclosure provides a cathode and a lithium secondary battery having improved lifespan and resistance characteristics by applying the cathode material as described above.
[0011] According to one embodiment, the present disclosure provides a first positive electrode active material comprising a lithium manganese oxide represented by the following chemical formula 1; and
[0012] A second cathode active material comprising a lithium transition metal oxide, having at least one single particle or a composite of 30 or fewer nodules, and having a pseudo-single particle form,
[0013] The D50 of the first positive electrode active material is 8㎛ or more, and a positive electrode material for a lithium secondary battery having a larger value than the D50 of the second positive electrode active material is provided.
[0014] [Chemical Formula 1]
[0015] Li 1+a [Mn 1-(b+c) Ni b M c ]O 2+d
[0016] In the above chemical formula 1,
[0017] M contains at least one selected from the group consisting of Co, Fe, Cr, V, Cu, Zn, Ti, Al, Mg, B, W, Ga, In, Ru, Nb, Sn, Sr and Zr,
[0018] 0.10≤a≤0.45, 0≤b≤0.5, 0≤c≤0.5, 0 <b+c≤0.5, 0≤d≤1이다.
[0019] In addition, the present disclosure provides a cathode slurry for a lithium secondary battery including the cathode material, a binder, a conductive material, and a solvent.
[0020] In addition, the present disclosure provides a positive electrode including a positive electrode current collector; and a positive electrode active material layer provided on the positive electrode current collector and including a positive electrode material,
[0021] The above cathode material comprises a first cathode active material including a lithium manganese oxide represented by the above chemical formula 1, and a second cathode active material having at least one single particle or a pseudo-single particle form which is a composite of 30 or fewer nodules, and including a lithium transition metal oxide.
[0022] The D50 of the first positive electrode active material is 8㎛ or more, and a positive electrode for a lithium secondary battery having a larger value than the D50 of the second positive electrode active material is provided.
[0023] In addition, the present disclosure provides a lithium secondary battery including the positive electrode.
[0024] The cathode material for a lithium secondary battery according to the present disclosure includes a lithium manganese oxide, and therefore has a high capacity and can be competitive in terms of raw material supply and price compared to existing cathode active materials containing a relatively high content of nickel or cobalt.
[0025] In addition, by mixing with a small-particle cathode active material in the form of a real single particle, it is possible to solve the limitations of existing lithium manganese oxides, such as the problem of reduced rolling density or manufacturing processability of the cathode due to high BET specific surface area.
[0026] Furthermore, the cathode material according to the present disclosure can produce a slurry with a higher solids content at the same viscosity compared to conventional lithium manganese oxide cathode materials containing only secondary particles. As a result, the cathode material is advantageous in reducing the coating thickness during the cathode manufacturing process, and the subsequent rolling process is easily controlled. Therefore, a cathode with a higher density and less particle breakage during the rolling process can be provided.
[0027] Figure 1 is a drawing showing the results of analyzing the PSD (volume cumulative particle size distribution) of the powder including the cathode material before and after rolling, respectively, for the cathode material manufactured in Example 4.
[0028] Figure 2 is a drawing showing the results of analyzing the PSD of the powder including the cathode material before and after rolling for the cathode material manufactured in Comparative Example 2.
[0029] Figure 3 is a drawing showing the change in porosity of a positive electrode active material layer according to the number of rolling cycles when manufacturing a positive electrode including a positive electrode material manufactured in Example 4 and Comparative Example 2.
[0030] Figure 4 is a drawing showing the results of measuring the rheological properties of a cathode slurry containing a cathode material manufactured in Example 4 and Comparative Example 2.
[0031] Figure 5 is a drawing of the positive electrode active material A used in the examples and comparative examples observed using a scanning electron microscope.
[0032] Figure 6 is a drawing of the positive electrode active material C used in the examples and comparative examples observed using a scanning electron microscope.
[0033] Figure 7 is a drawing of the positive electrode active material D used in the examples and comparative examples observed using a scanning electron microscope.
[0034] Figure 8 is a drawing of a particle cross-section of positive electrode active material A used in examples and comparative examples observed using a scanning electron microscope.
[0035] Hereinafter, specific implementation examples of the invention will be described in more detail.
[0036] Hereinafter, “single particle” refers to a particle composed of one single nodule, and “quasi-single particle” refers to a particle that is a composite particle formed of 30 or fewer nodules. However, unless otherwise specified below, “single particle” should be viewed as an inclusive term that also includes “quasi-single particle.”
[0037] In addition, “primary particle” means a particle unit that has no apparent grain boundary when observed under a magnification of 5,000 to 20,000 times using a scanning electron microscope, and “secondary particle” means a particle formed by the aggregation of multiple primary particles.
[0038] And, “nodule” means a particle unit body that constitutes a single particle and a pseudo-single particle, and the nodule may be a single crystal lacking a crystalline grain boundary, or a polycrystal in which no grain boundary exists in appearance when observed at a field of view of 5,000 to 20,000 times using a scanning electron microscope (SEM).
[0039] Additionally, “average particle size of primary particles” refers to the arithmetic mean calculated by measuring the particle sizes of at least 20 primary particles observed in scanning electron microscope images. Here, the particle size refers to the longest axis diameter of the primary particles.
[0040] In addition, “D50” refers to the particle size corresponding to 50% of the volume cumulative particle size distribution of the target powder, and can be measured using a laser diffraction method. For example, after dispersing the positive active material powder in a dispersion medium, it can be measured by introducing it into a commercially available laser diffraction particle size measuring device (e.g., Microtrac S-3500), irradiating it with ultrasonic waves of about 28 kHz at an output of 60 W, obtaining a volume cumulative particle size distribution graph, and finding the particle size at the point where the volume cumulative amount is 50% from the obtained graph.
[0041] In addition, the “BET specific surface area” is measured by the BET (Brunauer-Emmett-Teller) method, and can be specifically calculated from a nitrogen adsorption isotherm obtained under a 77K liquid nitrogen atmosphere using BELSORP-MAX (MicrotracBEL corp.).
[0042] Additionally, in each of the chemical formulas 1, 1a, 2 and 3 described below, the subscripts included in each chemical formula indicate the molar ratio of each element.
[0043]
[0044] cathode material
[0045] According to one embodiment of the invention, a cathode material comprises: a first cathode active material comprising a lithium manganese oxide represented by the following chemical formula 1; and a second cathode active material having at least one single particle shape consisting of one nodule or a quasi-single particle shape consisting of a composite of 30 or fewer nodules, and comprising a lithium transition metal oxide, wherein the D50 of the first cathode active material is 8 μm or more and has a larger value than the D50 of the second cathode active material.
[0046] [Chemical Formula 1]
[0047] Li 1+a [Mn 1-(b+c) Ni b M c ]O 2+d
[0048] In the above chemical formula 1,
[0049] M contains at least one selected from the group consisting of Co, Fe, Cr, V, Cu, Zn, Ti, Al, Mg, B, W, Ga, In, Ru, Nb, Sn, Sr and Zr,
[0050] 0.10≤a≤0.45, 0≤b≤0.5, 0≤c≤0.5, 0 <b+c≤0.5, 0≤d≤1이다.
[0051]
[0052] In the above cathode material, the lithium manganese peroxide contains manganese in an amount of 50 mol% or more, or 55 mol% or more, of the total metal excluding lithium, and may contain lithium in an excess molar ratio defined as 1+a. Due to the excess content of lithium and manganese, the lithium manganese peroxide may have a two-phase crystal structure in which a rock salt phase and a layered phase are mixed, and in particular, the rock salt phase may be contained in an amount exceeding a certain ratio. Due to the additional activation of the rock salt phase, the lithium manganese peroxide may have a higher capacity and energy density than existing layered structure cathode active materials, such as currently commercialized lithium nickel cobalt manganese (NCM) active materials. In addition, there is an advantage in that the amount of cobalt contained in the cathode material can be significantly reduced or the content of cobalt can be substantially excluded, thereby reducing the manufacturing cost.
[0053] However, perlithium manganese oxides containing high manganese contents have high resistance and low rate characteristics due to the relatively slow oxygen redox reaction and Mn ion oxidation / reduction reactions. Therefore, improvements in these aspects are required for the commercialization of lithium secondary batteries using perlithium manganese oxides as cathode materials.
[0054] Previously, to improve this, methods were applied to reduce the (average) particle size of the primary particles and increase the BET surface area of the secondary particles. However, this method resulted in additional problems, such as increased slurry viscosity, decreased electrode processability, particle breakage during the rolling process, and decreased anode density after rolling.
[0055] Accordingly, the inventors of the present invention mixed lithium manganese oxide with a single-particle active material and controlled the D50 of the lithium manganese oxide and the single-particle active material within a certain range. As a result, it was confirmed that the overall specific surface area of the cathode material could be increased to suppress increases in resistance, while lowering the slurry viscosity and increasing the solids content. This allows for a lower slurry coating thickness, facilitating drying, and since the target thickness can be achieved with less pressure during the rolling process, the stress applied to the cathode material can also be reduced.
[0056] Meanwhile, lithium manganese oxide has a large BET surface area compared to NCM active materials, and has limitations such as low electrode density and increased particle breakage during rolling due to the presence of pores inside due to the secondary particle form. For example, Fig. 8 is an SEM image observing the particle cross-section of the positive electrode active material A used in the examples below, through which it can be confirmed that large pores are formed inside the lithium manganese oxide particles. However, when applying the positive electrode material of one embodiment, since the rolling process is easy to control as described above, not only can particle breakage be suppressed during rolling, but also it is possible to provide a positive electrode having a higher density after rolling.
[0057] Meanwhile, in one embodiment of the cathode material of one embodiment, the cathode material may exhibit an overall bimodal particle size distribution due to different particle size distributions of the first cathode active material, which is an opposing material, and the second cathode active material, which is a small particle. In this case, since the small particles fill the gaps between the opposing materials during electrode rolling, there is an advantage in that the electrode density increases and high energy density can be realized.
[0058] Meanwhile, in the chemical formula 1, a is an excess molar ratio of Li contained in the lithium manganese oxide, and a in the chemical formula 1 can satisfy 0.10≤a≤0.45, or 0.15≤a≤0.4, or 0.20≤a≤0.38. When a satisfies the above range, high capacity can be achieved. Conversely, when the value of a is too small, it becomes difficult to achieve high capacity due to activation of the rock salt phase, etc., and when the value of a is too large, the crystal structure of the lithium manganese oxide itself may become unstable, or side reactions, etc. may significantly increase.
[0059] In addition, the above b is a molar ratio of Ni in the lithium manganese oxide, and b in the above chemical formula 1 can satisfy 0≤b<0.5, or 0.1≤b≤0.45, or 0.3≤b≤0.4.
[0060] The above c is a molar ratio of an additional element M in the lithium manganese oxide, and c in the above chemical formula 1 may be 0≤c<0.5, or 0≤c≤0.2, or 0≤c≤0.1, or 0≤c≤0.05. At this time, the additional element M may be an additional element forming a crystal structure of the lithium manganese oxide, or may be a doping element or coating element on the lithium manganese oxide. When the M is an additional element forming a crystal structure of the lithium manganese oxide, the M may not include cobalt. As a result, the two-phase crystal structure of the lithium manganese oxide is stabilized, so that high capacity characteristics, etc. can be exhibited, while the manufacturing cost can be reduced.
[0061] However, even if cobalt is not included among the elements forming the crystal structure of the lithium manganese oxide, cobalt may be added as a doping element or coating element on the lithium manganese oxide, and even in such a case, it may be included in the category of the lithium manganese oxide that does not substantially contain cobalt. In this case, the cobalt content may satisfy a ratio of c≤0.1, or 0≤c≤0.05.
[0062] Meanwhile, if the content of the additional element of the above M is too high, it may not only have a negative effect on the capacity of the active material, but also may cause gas generation and deterioration of the positive electrode active material during the oxygen redox reaction to be aggravated, which may result in a deterioration of the life characteristics.
[0063] The above 1-(b+c) is the molar ratio of Mn in the lithium manganese oxide, and b and c in the above chemical formula 1 are 0. <b+c≤0.5, 혹은 0<b+c<0.5, 혹은 0.1≤b+c≤0.45, 혹은 0.3≤b+c≤0.4을 만족할 수 있다. 특히, Mn이 리튬을 제외한 다른 금속 대비 보다 많은 몰 비로 포함되고, 예를 들어, 0.55≤1-(b+c) 등의 범위를 충족함에 따라, 상기 과리튬 망간계 산화물 내에 충분한 암염상이 포함될 수 있다. 이로서, 상기 과리튬 망간계 산화물의 우수한 용량 발현이 가능하고, 결정 구조적 안정성이 담보될 수 있다.
[0064] The above 2+d is the molar ratio of oxygen in the lithium manganese oxide, and d in the above chemical formula 1 can satisfy 0≤d≤0.5, 0≤d≤0.45, or 0≤d≤0.4.
[0065] Meanwhile, in the lithium manganese oxide represented by the above chemical formula 1, the molar ratio of Li to the molar ratio of all metal elements excluding Li (Li / Me) may be, for example, 1.10 to 1.45, or 1.15 to 1.4, or 1.20 to 1.38. When the Li / Me ratio satisfies the above range, the rate characteristics and capacity characteristics are excellent. If the Li / Me ratio is too high, the electrical conductivity may decrease and the rock salt phase (Li2MnO3) may increase, which may accelerate the degradation rate, and if it is too low, the effect of improving the energy density is minimal.
[0066] Meanwhile, the lithium manganese oxide containing an excess of lithium has a crystal structure in which a layered phase (LiM'O2) and a rock salt phase (Li2MnO3) are mixed, and the two-phase crystal structure of this lithium manganese oxide can be represented by the following chemical formula 1a. In this way, the lithium manganese oxide can be clearly distinguished from the existing layered structure positive electrode active material by the two-phase crystal structure in which the rock salt phase is mixed in a certain ratio or more, and can exhibit higher capacity and energy density even with a lower content of nickel, cobalt, etc.
[0067] [Chemical Formula 1a]
[0068] A·Li2MnO3·(1-A)·Li[Ni 1-n-m Mn n M m ]O2
[0069] In the above chemical formula 1a,
[0070] M contains at least one selected from the group consisting of Co, Fe, Cr, V, Cu, Zn, Ti, Al, Mg, B, W, Ga, In, Ru, Nb, Sn, Sr and Zr,
[0071] 0.10≤A≤0.45, 0.4≤n<1, 0≤m≤0.2.
[0072] The above A represents the ratio of the rock salt phase (Li2MnO3 phase) in the lithium manganese oxide, and the above n and m represent the molar ratio of Mn and the additional element M in the LiM'O2 layer, respectively, and can also be converted from the content ratio of each metal element in the above-described chemical formula 1.
[0073] Meanwhile, if necessary, a coating layer may be further included on the surface of the lithium manganese oxide. In this case, the coating layer can suppress contact between the lithium manganese oxide and the electrolyte, thereby reducing electrolyte side reactions and improving the life characteristics of the battery.
[0074] The above coating layer comprises a coating element M 1 may include the coating element M 1 For example, the M may include at least one selected from the group consisting of Al, B, Co, W, Mg, V, Ti, Zn, Ga, In, Ru, Nb, Sn, Sr and Zr. In a specific example, the M 1 The coating element M may be Al, Co, Nb, W or a combination thereof, and in more specific examples, Al, Co and a combination thereof. 1 It may contain two or more kinds, for example, it may contain Al and Co.
[0075] The above coating element is in the form of oxide within the coating layer, i.e., M 1 It can exist as Oz(1≤z≤4).
[0076] The above coating layer can be formed through methods such as dry coating, wet coating, chemical vapor deposition (CVD), physical vapor deposition (PVD), and atomic layer deposition (ALD). Among these, the atomic layer deposition method is preferred because it can form a large coating layer area.
[0077] The formation area of the above coating layer may be 10% to 100%, or 30% to 100%, or 50% to 100% based on the total surface area of the lithium manganese oxide particles. When the formation area of the coating layer satisfies the above range, the effect of improving the life characteristics is excellent.
[0078] Meanwhile, the lithium transition metal oxide included in the second positive electrode active material may be represented by the following chemical formula 2 or chemical formula 3.
[0079] [Chemical Formula 2]
[0080] Li 1+p (Ni q Co r Mn s M 2 t )O2
[0081] In the above chemical formula 2,
[0082] M 2 contains at least one selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B and Mo,
[0083] -0.2≤p≤0.2, 0.50≤q<1, 0 <r≤0.40, 0<s≤0.40, 0≤t≤0.10, q+r+s+t=1이고,
[0084] [Chemical Formula 3]
[0085] Li 1+w [Mn 1-(x+y) Ni x M 3 y ]O 2+z
[0086] In the above chemical formula 3,
[0087] M 3 It contains at least one selected from the group consisting of Co, Fe, Cr, V, Cu, Zn, Ti, Al, Mg, B, W, Ga, In, Ru, Nb, Sn, Sr and Zr,
[0088] 0 <w, 0≤x≤0.5, 0≤y≤0.5, 0<x+y≤0.5, 0≤z≤1이다.
[0089]
[0090] In one example, the lithium transition metal oxide included in the second positive electrode active material is represented by the chemical formula 2, and q, r, s, and t are 0.60≤q<1, 0, respectively. <r≤0.30, 0<s≤0.30, 0≤t≤0.10을 만족할 수 있다. 즉, 상기 제2 양극 활물질에 포함된 리튬 전이금속 산화물은 전이금속 중 니켈의 함량이 60몰% 이상인 리튬 니켈코발트망간계 산화물일 수 있다.
[0091] The above 1+p represents the molar ratio of lithium in the lithium nickel cobalt manganese oxide, and may be -0.2≤p≤0.2, or -0.1≤p≤0.2, or 0≤p≤0.2. When the molar ratio of lithium satisfies the above range, the crystal structure of the lithium nickel cobalt manganese oxide can be stably formed.
[0092] The above q represents the molar ratio of nickel among the total metals excluding lithium in the lithium nickel cobalt manganese oxide, and may be 0.50≤q<1, or 0.60≤q<1, or 0.70≤q<1, or 0.80≤q<1, or 0.85≤q<1. When the molar ratio of nickel satisfies the above range, a high energy density is exhibited, enabling high capacity implementation.
[0093] The above r represents the molar ratio of cobalt among all metals excluding lithium in lithium nickel cobalt manganese oxide, and is 0. <r≤0.40, 혹은 0<r≤0.30, 혹은 0<r≤0.20, 혹은 0<r≤0.15, 혹은 0<r≤0.10일 수 있다. 코발트의 몰 비가 상기 범위를 만족할 때, 양호한 저항 특성 및 출력 특성을 구현할 수 있다.
[0094] The above s represents the molar ratio of manganese among all metals excluding lithium in lithium nickel cobalt manganese oxide, and is 0. <s≤0.40, 혹은 0<s≤0.30, 혹은 0<s≤0.20, 혹은 0<s≤0.15, 혹은 0<s≤0.10 일 수 있다. 망간의 몰 비가 상기 범위를 만족할 때, 양극 활물질의 구조 안정성이 우수하게 나타난다.
[0095] In a specific example of the above cathode material, the lithium nickel cobalt manganese oxide represented by the above chemical formula 2 may include one or more additional elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B and Mo, in which case structural degradation may be suppressed and improved high-temperature durability may be exhibited. In a specific example, the lithium nickel cobalt manganese oxide represented by the above chemical formula 2 may include Al as the additional element. In addition, t, which represents the molar ratio of the additional element among the total metal excluding lithium in the lithium nickel cobalt manganese oxide, may be 0≤t≤0.10, or 0≤t≤0.08, or 0≤t≤0.06, or 0≤t≤0.05.
[0096] Meanwhile, when the lithium transition metal oxide included in the second positive electrode active material is a compound represented by the chemical formula 3, the description of the lithium manganese oxide of the first positive electrode active material can be applied substantially in the same manner.
[0097] For example, in the above chemical formula 3, w is 0 <w, 혹은 0.10≤w≤0.45, 혹은 0.15≤w≤0.40, 혹은 0.2≤w≤0.38을 만족할 수 있으며, 상기 x는 0≤x<0.5, 혹은 0.1≤x≤0.45, 혹은 0.3≤x≤0.4을 만족할 수 있고, 상기 y는 0≤y<0.5, 혹은 0≤y≤0.2, 혹은 0≤y≤0.1, 혹은 0≤y≤0.05를 만족할 수 있다. 또한, 상기 1-(x+y)는 상기 화학식 3으로 표시되는 화합물 내 Mn의 몰 비로, 0<x+y≤0.5, 혹은 0<x+y<0.5, 혹은 0.1≤x+y≤0.45, 혹은 0.3≤x+y≤0.4을 만족할 수 있으며, 상기 z는 0≤z≤1, 혹은 0≤z≤0.5, 혹은 0≤z≤0.45 혹은 0≤z≤0.4를 만족할 수 있다.
[0098] In a specific embodiment, the positive electrode material may include the first positive electrode active material and the second positive electrode active material in a weight ratio of 50:50 to 90:10, or 50:50 to 80:20, or 60:40 to 70:30, or 60:40 to 65:35. When the weight ratio of the first positive electrode active material and the second positive electrode active material is within the above range, the packing density can be increased as the space between the opposing particles is appropriately filled, and the rolling stress can be alleviated during the rolling process.
[0099] Meanwhile, the first positive electrode active material may be composed of secondary particles in which a plurality of primary particles are aggregated, and based on these secondary particles, the D50 of the first positive electrode active material may be 8 µm or more, or 8 µm to 15 µm, or 8 µm to 12 µm. If the D50 of the first positive electrode active material is less than 8 µm, the difference in particle size with the second positive electrode active material may be small, making it difficult to sufficiently implement the effect of improving the filling rate due to the bimodal configuration.
[0100] In addition, the BET specific surface area of the first positive electrode active material is 1.3 m2 / g or more, or 1.5m 2 / g or more, and thus high capacity and efficiency can be realized. However, considering the electrode processability, large surface area, low sphericity, surface side reactions, and increased non-uniformity, etc., 4.0 m 2 / g or less, or 3.0 m 2 / g can be less.
[0101] In addition, the D50 of the second positive electrode active material may be 2 µm to 5 µm, or 2.5 µm to 4.5 µm, and the BET specific surface area of the second positive electrode active material may be 0.5 m 2 / g to 1.2m 2 / g. Due to the D50 of the second positive electrode active material, the voids between the particles of the first positive electrode active material are effectively filled, thereby reducing particle breakage during rolling and providing a positive electrode with a higher density after rolling.
[0102] Meanwhile, the cathode material of the above-described embodiment may have a particle breakage rate of the first cathode active material according to the following formula 1 of 20% or less, or 0% to 18%, or 3% to 15%.
[0103] [Formula 1]
[0104] Particle breakage rate (%) of the first cathode active material = particle distribution rate (%) at the maximum peak obtained from the PSD (volume cumulative particle size distribution) of the cathode material before rolling - particle distribution rate (%) at the maximum peak obtained from the PSD of the cathode material after rolling
[0105] In the above equation 1,
[0106] The PSD of the cathode material before rolling means the PSD of the powder obtained by drying and crushing the cathode slurry containing the cathode material.
[0107] The PSD of the cathode material after rolling means the PSD of the cathode material powder recovered from the cathode, which includes the cathode material but has a porosity of 30% or less.
[0108]
[0109] anode slurry
[0110] Next, a cathode slurry including the cathode material of the above-described embodiment is described.
[0111] The above cathode slurry comprises the cathode material, binder, conductive material and solvent of the above-described embodiment.
[0112] In a specific embodiment, the positive electrode slurry may have a solid content of 65 wt% or more and a viscosity of 14,500 cP or less based on the total weight of the positive electrode slurry. That is, by including the positive electrode material, a solid content of a certain level or more can be secured without excessively increasing the viscosity, thereby securing both the capacity and processability of the positive electrode. In this case, the solid content is measured by drying the positive electrode slurry in an oven to remove all solvent and measuring the remaining weight, and the viscosity is measured at 25°C with a Brookfield DV2T LV TJ0 model equipment at 12 rpm and spindle 64 (LV-03).
[0113] Specifically, the solid content in the positive electrode slurry may be 66 wt% or more, or 67 wt% or more, or 68 wt% or more. A higher solid content in the slurry is preferable in terms of suppressing binder migration and increasing electrode productivity. In the case of a dry electrode, the solid content may be 100 wt%, but when a solvent is used, it may be 85 wt% or less to prevent the viscosity from becoming excessively high. Meanwhile, the viscosity of the positive electrode slurry may be 14,000 cP or less, or 13,000 cP or less, or 12,000 cP or less in consideration of the ease of slurry transport and coating processability. However, in consideration of slurry sedimentation and phase stability, it may be 5,000 cP or more, more specifically, 8,000 cP or more.
[0114] Meanwhile, the positive electrode active material may be included in an amount of 90 wt% to 99 wt%, specifically 95 wt% to 99 wt%, and more specifically 97 wt% to 98 wt%, based on the total weight of the solid content in the positive electrode slurry. If the content of the positive electrode active material in the solid content is 90 wt% or less, the energy density may be lowered, resulting in a decrease in capacity.
[0115] Meanwhile, the binder may include at least one selected from the group consisting of polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethylcellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated-EPDM, styrene butadiene rubber (SBR), fluororubber, and various copolymers thereof, and specifically may include polyvinylidene fluoride (PVDF).
[0116] The above binder may be included in an amount of 0.5 wt% to 2.5 wt%, or 1 wt% to 2 wt%, or 1.5 wt% to 2 wt%, based on the total weight of the solid content in the positive electrode slurry. When the content of the binder is within the above range, sufficient adhesion to the current collector and bonding between particles can be secured, thereby improving the durability of the positive electrode while maintaining a low initial resistance.
[0117] The conductive material may be at least one selected from the group consisting of graphite such as natural graphite or artificial graphite; carbon black such as acetylene black, Ketjen black, channel black, furnace black, lamp black, and summer black; carbon-based materials such as carbon fibers and carbon nanotubes; metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive polymers such as polyphenylene derivatives, and more specifically, it may be carbon nanotubes or carbon black.
[0118] The conductive agent may be included in an amount of 0.1 wt% to 2.5 wt%, or 0.3 wt% to 2 wt%, or 0.5 wt% to 1 wt%, based on the total weight of the solid content in the positive electrode slurry. When the content of the conductive agent is within the above range, the dead volume within the active material layer can be reduced while maintaining conductivity between the active materials.
[0119] In addition, the above cathode slurry may optionally further include a dispersant, and the dispersant may be hydrogenated nitrile butadiene rubber (HNBR).
[0120] Meanwhile, the solvent of the positive electrode slurry may be a solvent generally used in the relevant technical field, and examples thereof include N-methylpyrrolidone (NMP), dimethyl sulfoxide (DMSO), isopropyl alcohol, dimethyl formamide (DMF), acetone, water, or a mixture of two or more thereof. The solvent may be used in an amount adjusted to have the viscosity of the positive electrode slurry described above.
[0121]
[0122] anode
[0123] Next, a description is given of an anode including a cathode material of an embodiment.
[0124] According to another embodiment of the invention, a positive electrode comprises: a positive electrode current collector; and a positive electrode active material layer provided on the positive electrode current collector and including a positive electrode material.
[0125] The above cathode material comprises a first cathode active material including a lithium manganese oxide represented by the above chemical formula 1 and at least one pseudo-single particle form consisting of one nodule or a composite of 30 or fewer nodules, and a second cathode active material including a lithium transition metal oxide.
[0126] The D50 of the above first positive electrode active material is 8㎛ or more, and may have a larger value than the D50 of the above second positive electrode active material.
[0127] In addition, it includes a positive electrode active material layer formed by coating the above-described positive electrode slurry on at least one surface of a positive electrode current collector.
[0128] Since the cathode material and cathode slurry have been described above, a detailed description will be omitted, and only the remaining components will be described in detail below.
[0129] The positive electrode current collector may include a highly conductive metal, and is not particularly limited as long as it is easily adhered to by the positive electrode active material layer and is non-reactive within the voltage range of the battery. The positive electrode current collector may be, for example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. In addition, the positive electrode current collector may typically have a thickness of 3 to 500 μm, and fine unevenness may be formed on the surface of the current collector to increase the adhesion of the positive electrode active material. For example, the positive electrode current collector may be used in various forms such as a film, a sheet, a foil, a net, a porous body, a foam, a non-woven fabric, etc.
[0130] The above-mentioned positive electrode can be manufactured according to a conventional positive electrode manufacturing method, except that the above-mentioned positive electrode material is used. Specifically, the positive electrode can be manufactured by applying the positive electrode slurry onto a positive electrode current collector, followed by drying and rolling, or by casting the positive electrode slurry onto a separate support, then peeling the film from the support, and laminating the resulting film onto a positive electrode current collector.
[0131] Meanwhile, the above anode is 7ton / 1.327cm at room temperature 2 When pressurized, the rolling density may be 2.9 g / cc or more, or 2.91 g / cc or more, or 2.97 g / cc or more and 3.50 g / cc or less. As described above, despite the high BET specific surface area and porosity of the lithium manganese oxide, the energy density can be improved by implementing such a high rolling density.
[0132] In addition, the above anode has a loading amount of 420 mg / 25 cm 2 540mg / 25cm 2 , or 440mg / 25cm 2 520mg / 25cm 2 , or 460mg / 25cm 2 500mg / 25cm2 It can be done. When the loading amount is within the above range, there is an advantage in that high energy density can be achieved while appropriately securing electrode fairness and output.
[0133]
[0134] lithium secondary battery
[0135] Next, a lithium secondary battery according to another embodiment of the invention will be described.
[0136] The lithium secondary battery specifically includes a positive electrode, a negative electrode positioned opposite the positive electrode, and a separator and electrolyte interposed between the positive electrode and the negative electrode. Since the positive electrode is the same as described above, a detailed description thereof will be omitted, and only the remaining components will be described in detail below.
[0137] In addition, the lithium secondary battery may optionally further include a battery container that houses the electrode assembly of the positive electrode, the negative electrode, and the separator, and a sealing member that seals the battery container.
[0138] In the above lithium secondary battery, the negative electrode includes a negative electrode current collector and a negative electrode active material layer positioned on the negative electrode current collector.
[0139] The negative electrode current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery. For example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., aluminum-cadmium alloy, etc. can be used. In addition, the negative electrode current collector can typically have a thickness of 3 ㎛ to 500 ㎛, and like the positive electrode current collector, fine unevenness can be formed on the surface of the current collector to strengthen the bonding strength of the negative electrode active material. For example, it can be used in various forms such as a film, a sheet, a foil, a net, a porous body, a foam, a non-woven fabric, etc.
[0140] The cathode active material layer optionally includes a binder and a conductive material together with the cathode active material.
[0141] As the negative electrode active material, a compound capable of reversible intercalation and deintercalation of lithium may be used. Specific examples include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloy, Sn alloy, or Al alloy; SiO β (0 <β< 2), SnO2, vanadium oxide, lithium vanadium oxide, and other metal oxides capable of doping and dedoping lithium; or composites containing the above metallic compounds and carbonaceous materials, such as Si-C composites or Sn-C composites, and any one or a mixture of two or more of these may be used. In addition, a metallic lithium thin film may be used as the negative electrode active material. The negative electrode active material may be included in an amount of 80 wt% to 99 wt% based on the total weight of the negative electrode active material layer.
[0142] The above binder is a component that assists in bonding between the conductive material, the active material, and the current collector, and is typically added in an amount of 0.1 wt% to 10 wt% based on the total weight of the negative electrode active material layer. Examples of such binders include polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene-butadiene rubber, nitrile-butadiene rubber, fluororubber, and various copolymers thereof.
[0143] The conductive agent is a component for further improving the conductivity of the negative electrode active material, and may be added in an amount of 10 wt% or less, or 5 wt% or less, or 0.1 wt% to 4 wt% based on the total weight of the negative electrode active material layer. The conductive agent is not particularly limited as long as it has conductivity without causing a chemical change in the battery, and examples thereof include graphite such as natural graphite or artificial graphite; carbon black such as acetylene black, Ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fiber or metal fiber; fluorinated carbon; metal powder such as aluminum or nickel powder; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.
[0144] The above negative electrode active material layer can be manufactured by applying and drying a negative electrode composite prepared by dissolving or dispersing a negative electrode active material, and optionally a binder and a conductive material in a solvent, on a negative electrode current collector, or by casting the negative electrode composite on a separate support and then laminating the obtained film by peeling it off from the support on a negative electrode current collector.
[0145] Meanwhile, in the lithium secondary battery, the separator separates the negative electrode and the positive electrode and provides a passage for lithium ions to move. Any separator commonly used in lithium secondary batteries can be used without special restrictions, and in particular, one having low resistance to ion movement of the electrolyte and excellent electrolyte moisture absorption capacity is preferable. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof, may be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of high-melting-point glass fiber, polyethylene terephthalate fiber, etc. may be used. In addition, a coated separator containing a ceramic component or a polymer material to secure heat resistance or mechanical strength may be used, and may optionally be used in a single-layer or multi-layer structure.
[0146] In addition, the electrolyte used in the lithium secondary battery may include, but is not limited to, organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, or molten inorganic electrolytes, which have been previously known to be usable in the manufacture of secondary batteries.
[0147] Specifically, the electrolyte may include an organic solvent and a lithium salt.
[0148] The organic solvent may be used without any particular limitation as long as it can serve as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the organic solvent may include ester solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, and ε-caprolactone; ether solvents such as dibutyl ether or tetrahydrofuran; ketone solvents such as cyclohexanone; aromatic hydrocarbon solvents such as benzene and fluorobenzene; Carbonate solvents such as dimethylcarbonate (DMC), diethylcarbonate (DEC), methylethylcarbonate (MEC), ethylmethylcarbonate (EMC), ethylene carbonate (EC), and propylene carbonate (PC); alcohol solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as R-CN (where R represents a linear, branched, or cyclic hydrocarbon group having 2 to 20 carbon atoms and may include a double-bonded aromatic ring or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes can be used. Among these, a carbonate solvent is suitable, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate, etc.) having high ionic conductivity and high dielectric constant that can improve the charge / discharge performance of the battery and a low-viscosity linear carbonate compound (e.g., ethyl methyl carbonate, dimethyl carbonate, or diethyl carbonate, etc.) is more preferable.
[0149] The above lithium salt can be used without any special limitation as long as it is a compound that can provide lithium ions used in a lithium secondary battery. Specifically, the anion of the above lithium salt is F - , Cl - , Br - , I - , NO3 - , N(CN)2 - , BF4 - , CF3CF2SO3 - , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - and (CF3CF2SO2)2N - It may include at least one selected from the group consisting of. Specifically, the lithium salts include LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAl04, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2) 2. LiCl, LiI, or LiB(C2O4)2 can be used. It is recommended that the concentration of the lithium salt be within the range of 0.1 to 4.0 M. When the concentration of the lithium salt is within the above range, the electrolyte can exhibit excellent electrolyte performance because it has appropriate conductivity and viscosity, and lithium ions can move effectively.
[0150] In addition to the electrolyte components, the electrolyte may further include one or more additives, such as haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethanolamine, cyclic ethers, ethylene diamine, n-glyme, hexaphosphate triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride, for the purpose of improving the life characteristics of the battery, suppressing battery capacity decrease, and improving the discharge capacity of the battery. At this time, the additives may be included in an amount of 0.1 to 5 wt% based on the total weight of the electrolyte.
[0151] As described above, a lithium secondary battery including a cathode material of an embodiment of the present invention stably exhibits excellent discharge capacity, output characteristics, and lifespan characteristics, and is therefore useful in portable devices such as mobile phones, laptop computers, and digital cameras, and electric vehicles such as hybrid electric vehicles (HEVs).
[0152] Accordingly, according to an additional embodiment, a battery module including the lithium secondary battery as a unit cell and a battery pack including the same are provided.
[0153] The above battery module or battery pack can be used as a power source for one or more medium- to large-sized devices, such as power tools; electric vehicles including electric vehicles (EVs), hybrid electric vehicles, and plug-in hybrid electric vehicles (PHEVs); or power storage systems.
[0154] There are no particular restrictions on the external shape of the lithium secondary battery included in such a module or pack, but it may be cylindrical, square, pouch-shaped, or coin-shaped using a can. Such a lithium secondary battery can be used not only as a battery cell used as a power source for a small device, but also as a unit battery in a medium- to large-sized battery module including a plurality of battery cells.
[0155] Examples of the above medium and large devices include, but are not limited to, electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, and power storage systems.
[0156]
[0157] Hereinafter, specific embodiments of the invention will be described in more detail.
[0158]
[0159] <Example - Manufacturing of positive electrode material>
[0160] The positive electrode active materials A to G used in the following examples and comparative examples were commercially obtained and used with the composition and characteristics shown in Table 1 below.
[0161]
[0162] Composition D50 (㎛) Particle shape SEM photo BET specific surface area (m 2 / g) Anode active material ALi 1.36 [Mn 0.65 Ni 0.35 ]O2102 secondary particle size 53.8 BLi, a cathode active material 1.36 [Mn 0.65 Ni 0.35 ]O28.52nd particle-2.4Cathode active material CLi 1.36 [Mn 0.65 Ni 0.35 ]O26.22nd particle size 62.1 Cathode active material DLi 1.36 [Mn 0.65 Ni 0.35 ]O232 secondary particle size 73.7 Cathode active material ELi 1.03 [Ni 0.60 Co 0.10Mn 0.30 ]O23.7 single particle-0.9 positive electrode active material FLi 1.03 [Ni 0.86 Co 0.08 Mn 0.06 ]O24.3 single particle-0.7 cathode active material GLi 1.03 [Ni 0.86 Co 0.08 Mn 0.06 ]O23.7 single particle-0.8
[0163] Example 1.
[0164] The positive electrode active material A and the positive electrode active material E were mixed in a weight ratio of 70:30 to manufacture a positive electrode material.
[0165]
[0166] Example 2.
[0167] The positive electrode active material B and the positive electrode active material F were mixed in a weight ratio of 65:35 to manufacture a positive electrode material.
[0168]
[0169] Example 3.
[0170] A cathode material was manufactured by mixing the above cathode active material A and cathode active material G in a weight ratio of 60:40.
[0171]
[0172] Example 4.
[0173] The positive electrode active material A and the positive electrode active material G were mixed in a weight ratio of 65:35 to manufacture a positive electrode material.
[0174]
[0175] Example 5.
[0176] The positive electrode active material A and the positive electrode active material G were mixed in a weight ratio of 70:30 to manufacture a positive electrode material.
[0177]
[0178] Example 6.
[0179] The positive electrode active material A and the positive electrode active material G were mixed in a weight ratio of 50:50 to manufacture a positive electrode material.
[0180]
[0181] Example 7.
[0182] The positive electrode active material A and the positive electrode active material G were mixed in a weight ratio of 80:20 to manufacture a positive electrode material.
[0183]
[0184] Comparative Example 1.
[0185] As a cathode material, only the cathode active material C was used alone.
[0186]
[0187] Comparative Example 2.
[0188] The positive electrode active material A and the positive electrode active material D were mixed in a weight ratio of 65:35 to manufacture a positive electrode material.
[0189]
[0190] Comparative Example 3.
[0191] The positive electrode active material C and the positive electrode active material G were mixed in a weight ratio of 65:35 to manufacture a positive electrode material.
[0192]
[0193] <Experimental Example>
[0194] Experimental Example 1.
[0195] (1) Preparation of positive electrode slurry
[0196] For each of the cathode materials manufactured in the above examples and comparative examples, cathode slurry was manufactured using the following method.
[0197] First, a cathode material powder, a carbon nanotube as a conductive material, a polyvinylidene fluoride as a binder, and a dispersant including HNBR were added to N-methylpyrrolidone as a solvent at a weight ratio of 97.46:0.62:1.7:0.22, and mixed using a homodisper at a speed of 2,500 rpm for 75 minutes to prepare a cathode slurry.
[0198]
[0199] (2) Measurement of solid content and viscosity of positive slurry
[0200] The solids content was confirmed by measuring the remaining weight after drying each positive electrode slurry prepared in the above (1) in an oven to remove all solvent. In addition, each positive electrode slurry was filled to more than 2 / 3 of the volume in a 250 mL bottle, and the viscosity was measured at 25°C using a Brookfield DV2T LV TJ0 model equipment with a spindle of 64 (LV-03) at 12 rpm. The measurement results are shown in Table 2 below.
[0201]
[0202] (3) Measurement of rheological properties of positive electrode slurry
[0203] For the positive electrode slurries manufactured in (1) above, each containing the positive electrode materials of Example 4 and Comparative Example 2, the shear viscosity corresponding to the shear rate was measured.
[0204] Specifically, a Rheometer (DHR2) from TA Instrument was used, and 10 mL of each positive electrode slurry was placed in a concentric cylinder within the device, and the shear viscosity was measured while gradually increasing the shear rate at 25°C. The same process was repeated twice, and the results of the measurements are shown in Fig. 4.
[0205]
[0206] Experimental example 2.
[0207] (1) Manufacturing of powder containing cathode material
[0208] Each positive electrode slurry manufactured in Experimental Example 1 was vacuum-dried at a temperature of 130°C for 3 hours, then finely ground using a mortar and pestle, and then classified using a 250 mesh sieve to obtain a powder containing a positive electrode material from the positive electrode slurry.
[0209]
[0210] (2) Measurement of rolling density of powder containing cathode material
[0211] 2g of each powder manufactured in the above (1) was placed in a cylindrical metal mold in a powder resistance measuring device (HPRM-1000, Hantech Co.), and 7ton / 1.327cm 2 The pressure was applied with the surface pressure of . The height of the pressurized mold was measured with Vernier calipers, and the rolling density was calculated using this, and the results are shown in Table 2 below.
[0212]
[0213] (3) PSD measurement of powder containing cathode material
[0214] For each powder manufactured in (1) above, a volumetric cumulative particle size distribution (PSD) was obtained for the powder containing the cathode material of Example 4 using Microtrac's S-3500. The obtained particle size distribution graph is shown as pre-rolling data in Figure 1 below.
[0215] For the powder containing the cathode material of Comparative Example 2, the PSD was obtained in the same manner and was shown as data before rolling in Figure 2 below.
[0216]
[0217] Experimental Example 3.
[0218] (1) Positive slurry coating
[0219] Each positive electrode slurry prepared in (1) of the above experimental example 1 was loaded at a loading amount of 480 mg / 25 cm 2 The positive electrode active material layer was formed by applying the film to an aluminum film, which is a 15㎛ thick positive electrode current collector, and drying at 130℃. The thickness of the positive electrode active material layer was measured in this state and is shown in Table 2 below.
[0220]
[0221] (2) Rolling
[0222] For the slurry containing the positive electrode materials of Example 4 and Comparative Example 2, a positive electrode active material layer was coated on the positive electrode current collector as in (1) above. Thereafter, rolling was performed repeatedly using a roll press until the porosity of the positive electrode active material layer became less than 30%. A graph observing the change in porosity of the positive electrode active material layer according to the number of rolling cycles is shown in Fig. 3. At this time, the porosity was calculated using the true density of the raw material after measuring the thickness of the electrode.
[0223]
[0224] (3) PSD measurement of the anode
[0225] In the above (2), the cathode of Example 4 (porosity 28.3%), in which the porosity was controlled to 30% or less, was heat-treated in a furnace at 700°C for 10 hours to collect the cathode material, which was then finely ground using a mortar and pestle, and then classified using a 250 mesh sieve to obtain cathode material powder. For the obtained powder, a volumetric cumulative particle size distribution (PSD) was obtained using Microtrac's S-3500. The obtained particle size distribution graph is shown as data after rolling in Fig. 1.
[0226] For the positive electrode of Comparative Example 2 (porosity 29.4%), the PSD was obtained using the same method and was shown as data after rolling in Fig. 2 above.
[0227]
[0228] Experimental Example 1 Experimental Example 2 Experimental Example 3 Solid content (wt%) Viscosity (cP) Rolling density (g / cc) Thickness of coated positive electrode active material layer (nm) Example 16812,310 2.99 110 Example 26811,840 2.98 111 Example 36810,650 2.97 113 Example 46812,589 2.99 109 Example 56814,100 3.00 110 Example 66613,700 2.92 115 Example 76813,800 2.96 113 Comparative Example 16312,500 2.80 131 Comparative Example 26614,693 2.83 118 Comparative Example 36411,9002.85125
[0229] First, referring to Table 1 above, it was confirmed that the slurry containing the positive electrode material of the example had a solids content of 65 wt% or more and a viscosity of no more than 14,500 cP. From this, it was confirmed that it was advantageous to reduce the thickness of the positive electrode active material layer, and that the rolling process was easily controlled, and as a result, the rolling density was all expressed at 2.9 g / cc or more.
[0230] On the other hand, it was confirmed that Comparative Example 1, which only includes a lithium manganese oxide corresponding to the first positive electrode active material, Comparative Example 2, which uses a positive electrode active material in the form of secondary particles as the second positive electrode active material, and Comparative Example 3, which does not exhibit bimodal characteristics because the D50 of the lithium manganese oxide is 6.7 μm, exhibited lower solid content, higher viscosity, or lower rolling density under the same rolling conditions compared to Examples 1 to 7.
[0231] In addition, referring to FIGS. 1 and 2 comparing Comparative Example 2, which used a secondary particle-type positive electrode active material as the second positive electrode active material, with Example 4, it was confirmed that the particle breakage phenomenon of the electrode before / after rolling occurred at a very small rate in Example 4 compared to Comparative Example 2. Specifically, in Example 4, the particle breakage rate of the first positive electrode active material according to the above formula 1 was 14%, but in Comparative Example 2, the particle breakage rate of the first positive electrode active material according to the above formula 1 was confirmed to be 28%.
[0232] Meanwhile, referring to FIG. 3, in the case of Example 4, the porosity dropped below 30% after only two rollings, but in the case of Comparative Example 2, it was confirmed that the porosity dropped below 30% only after four rollings.
[0233] Additionally, referring to FIG. 4, it was confirmed that the slurry obtained from Example 4 had a lower viscosity than that of Comparative Example 2.
[0234] Meanwhile, looking at Examples 3 to 7 in which positive electrode active material A was used as the first positive electrode active material and positive electrode active material G was used as the second positive electrode active material, but only the ratio between them was changed, Examples 3 to 5 in which the weight ratio was set to 60:40 to 70:30 had a solid content of 68 wt% with a viscosity of 14,500 cP or less, and at the same time, a rolling density of 2.97 g / cc or more was secured. In particular, Examples 3 and 4 in which the weight ratio was set to 60:40 to 65:35 had a solid content of 68 wt% with a rolling density of 2.97 g / cc or more without exceeding 13,000 cP, and were confirmed to exhibit low viscosity that ensures excellent processability along with a higher solid content and rolling density.
Claims
1. A first positive electrode active material comprising a lithium manganese oxide represented by the following chemical formula 1; and A second cathode active material comprising a lithium transition metal oxide, having at least one single particle or a composite of 30 or fewer nodules, and having a pseudo-single particle form, A cathode material for a lithium secondary battery, wherein the D50 of the first cathode active material is 8㎛ or more and has a larger value than the D50 of the second cathode active material: [Chemical Formula 1] Li 1+a [Mr 1-(b+c) Ni b M c ]O 2+d In the above chemical formula 1, M contains at least one selected from the group consisting of Co, Fe, Cr, V, Cu, Zn, Ti, Al, Mg, B, W, Ga, In, Ru, Nb, Sn, Sr and Zr, 0.10≤a≤0.45, 0≤b≤0.5, 0≤c≤0.5, 0 <b+c≤0.5, 0≤d≤1이다.
2. In claim 1, A cathode material for a lithium secondary battery exhibiting an overall bimodal particle size distribution due to different particle size distributions of the first cathode active material and the second cathode active material.
3. In claim 1, the first positive electrode active material is a positive electrode material for a lithium secondary battery that substantially does not contain cobalt.
4. In claim 1, The lithium transition metal oxide contained in the second positive electrode active material is a positive electrode material for a lithium secondary battery represented by the following chemical formula 2 or chemical formula 3: [Chemical Formula 2] Li 1+p (Ni q Co r Mr s M 2 t )O2 In the above chemical formula 2, M 2 It contains at least one selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B and Mo, -0.2≤p≤0.2, 0.50≤q<1, 0 <r≤0.40, 0<s≤0.40, 0≤t≤0.10, q+r+s+t=1이고, [Chemical Formula 3] Li 1+w [Mr 1-(x+y) Ni x M 3 y ]O 2+z In the above chemical formula 3, M 3 It contains at least one selected from the group consisting of Co, Fe, Cr, V, Cu, Zn, Ti, Al, Mg, B, W, Ga, In, Ru, Nb, Sn, Sr and Zr, 0 <w, 0≤x≤0.5, 0≤y≤0.5, 0<x+y≤0.5, 0≤z≤1이다.
5. In claim 4, The lithium transition metal oxide included in the second positive electrode active material is represented by the chemical formula 2, and q, r, s and t are 0.60≤q<1, 0, respectively. <r≤0.30, 0<s≤0.30, 0≤t≤0.10을 만족하는 리튬 이차전지용 양극재.
6. In claim 1, A cathode material for a lithium secondary battery, wherein b and c in the above chemical formula 1 satisfy 0.1≤b+c≤0.
45.
7. In claim 1, A cathode material for a lithium secondary battery comprising the first cathode active material and the second cathode active material in a weight ratio of 90:10 to 60:
40.
8. In claim 1, A cathode material for a lithium secondary battery, wherein the D50 of the first cathode active material is 8㎛ to 15㎛.
9. In claim 1, A cathode material for a lithium secondary battery, wherein the D50 of the second cathode active material is 2㎛ to 5㎛.
10. In claim 1, The BET specific surface area of the first positive electrode active material is 1.3 m 2 / g to 4.0m 2 / g of cathode material for lithium secondary batteries.
11. In claim 1, The above first positive electrode active material is a positive electrode material for a lithium secondary battery having a crystal structure in which a layered phase and a rock salt phase are mixed.
12. In claim 1, The above first positive electrode active material is a positive electrode material for a lithium secondary battery having a two-phase crystal structure represented by the following chemical formula 1a: [Chemical Formula 1a] A·Li2MnO3·(1-A)·Li[Ni 1-n-m Mr n M m ]O2 In the above chemical formula 1a, M contains at least one selected from the group consisting of Co, Fe, Cr, V, Cu, Zn, Ti, Al, Mg, B, W, Ga, In, Ru, Nb, Sn, Sr and Zr, 0.10≤A≤0.45, 0.4≤n<1, 0≤m≤0.
2.
13. In claim 1, A cathode material for a lithium secondary battery having a particle breakage rate of 20% or less of the first cathode active material according to the following formula 1: [Formula 1] Particle breakage rate (%) of the first cathode active material = particle distribution rate (%) at the maximum peak obtained from the PSD (volume cumulative particle size distribution) of the cathode material before rolling - particle distribution rate (%) at the maximum peak obtained from the PSD of the cathode material after rolling In the above equation 1, The PSD of the cathode material before rolling means the PSD of the powder obtained by drying and crushing the cathode slurry containing the cathode material. The PSD of the cathode material after rolling means the PSD of the cathode material powder recovered from the cathode, which includes the cathode material but has a porosity of 30% or less.
14. A cathode slurry for a lithium secondary battery comprising a cathode material, a binder, a conductive material, and a solvent according to any one of claims 1 to 13.
15. In claim 14, A positive electrode slurry for a lithium secondary battery having a solid content of 65 wt% or more and a viscosity of 14,500 cP or less relative to the total weight of the positive electrode slurry.
16. A positive electrode including a positive electrode current collector; and a positive electrode active material layer including a positive electrode material provided on the positive electrode current collector, The above cathode material comprises a first cathode active material including a lithium manganese oxide represented by the following chemical formula 1, and at least one pseudo-single particle form consisting of one nodule or a composite of 30 or fewer nodules, and a second cathode active material including a lithium transition metal oxide. A positive electrode for a lithium secondary battery, wherein the D50 of the first positive electrode active material is 8㎛ or more and has a larger value than the D50 of the second positive electrode active material: [Chemical Formula 1] Li 1+a [Mr 1-(b+c) Ni b M c ]O 2+d In the above chemical formula 1, M contains at least one selected from the group consisting of Co, Fe, Cr, V, Cu, Zn, Ti, Al, Mg, B, W, Ga, In, Ru, Nb, Sn, Sr and Zr, 0.10≤a≤0.45, 0≤b≤0.5, 0≤c≤0.5, 0 <b+c≤0.5, 0≤d≤1이다.
17. In claim 16, 7 tons / 1.327 cm at room temperature 2 A positive electrode for a lithium secondary battery having a rolling density of 2.9 g / cc or more when pressurized.
18. In claim 16, Loading amount is 420mg / 25cm 2 540mg / 25cm 2 Anode for lithium secondary batteries.
19. A lithium secondary battery comprising the positive electrode and negative electrode of claim 16.
Citation Information
Patent Citations
Single crystal material precursor and composite oxide powder as well as preparation method and application thereof
CN112174227A
Test apparatus of elevator
KR102005732B1
Positive active material for rechargeable lithium battery, method of preparing the same, and positive electrode for rechargeable lithium battery and rechargeable lithium battery including the same
KR1020150004645A
Method for manufacturing over-lithiated layered lithium metal composite oxide
KR1020160032246A
Image Sensor
KR102898632B1
Cited By
Positive electrode for lithium secondary battery and lithium secondary battery comprising same
WO2026205843A1