Method for manufacturing electrode, electrode manufactured thereby, and lithium secondary battery comprising same electrode

The use of a lithium metal layer with a lithium buffer layer on both sides for pre-lithiation in lithium secondary batteries addresses the challenges of volume changes and ignition risks, enhancing battery lifespan and capacity while maintaining energy density.

WO2024242400A1PCT designated stage expired Publication Date: 2024-11-28LG ENERGY SOLUTION LTD

Patent Information

Application Number
PCT/KR2024/006628
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-23
Filing Date
2024-05-16
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Lithium secondary batteries with silicon-based active material particles face rapid volume changes during cycling, leading to reduced lifespan due to excessive heat generation and ignition risks during the pre-lithiation process, which involves direct contact of lithium metal with silicon-based materials.

Method used

A method involving a lithium metal layer with a lithium buffer layer formed on both sides is used to minimize side reactions, allowing pre-lithiation in a stable atmosphere and preventing inactive layer formation, thereby reducing heat generation and ignition risks, and the lithium buffer layer decomposes to provide additional lithium without affecting electrode thickness.

Benefits of technology

This approach enhances the lifespan of lithium secondary batteries by controlling the available area of the negative electrode, maximizing pre-lithiation effects, and reducing the risk of excessive heat and ignition, while maintaining energy density and improving capacity utilization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024006628_28112024_PF_FP_ABST
    Figure KR2024006628_28112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a method for manufacturing an electrode, the method comprising: a P1 step of disposing a transfer laminate including a lithium metal layer having lithium buffer layers formed on both surfaces thereof on a preliminary electrode active material layer to form an electrode structure such that the lithium buffer layer and the preliminary electrode active material layer are in contact with each other; a P2 step of rolling the electrode structure; and a P3 step of aging the rolled electrode structure in a nitrogen atmosphere, wherein the nitrogen atmosphere is an atmosphere containing 80 vol % or more of nitrogen.
Need to check novelty before this filing date? Find Prior Art

Description

Method for manufacturing an electrode, an electrode manufactured thereby, and a lithium secondary battery including the electrode

[0001] Cross-citation with related applications

[0002] This application claims the benefit of priority to Korean Patent Application No. 10-2023-0066491, filed May 23, 2023, the entire contents of which are incorporated herein by reference.

[0003]

[0004] Technology field

[0005] The present invention relates to a method for manufacturing an electrode, an electrode manufactured thereby, and a lithium secondary battery including the electrode.

[0006]

[0007] Due to the rapid increase in fossil fuel use, the demand for alternative or clean energy is increasing, and as part of this, the most actively researched field is power generation and storage using electrochemical reactions.

[0008] Secondary batteries are a prime example of electrochemical devices that utilize this electrochemical energy, and their applications are expanding. With the recent technological development and increasing demand for portable devices such as laptops, mobile phones, and cameras, the demand for secondary batteries as an energy source has rapidly increased. Among these secondary batteries, lithium secondary batteries, which boast high energy density and high capacity, have been extensively studied and are now commercialized and widely used.

[0009] In general, a secondary battery is composed of a positive electrode, a negative electrode, an electrolyte, and a separator. The negative electrode includes a negative electrode active material that inserts and deintercalates lithium ions from the positive electrode, and silicon-based active material particles with a large discharge capacity can be used as the negative electrode active material. The silicon-based active material particles are Si or SiO. X(0 <X<2) 등에 해당될 수 있다. 실리콘계 활물질 입자는 이론 용량이 크고 가격이 저렴한 장점이 있다. 다만, 실리콘계 활물질 입자는 전지 구동 시, 부피 변화가 지나치게 크므로, 전지의 사이클이 진행될수록 전지의 수명이 급격히 줄어드는 단점이 있다.

[0010] Therefore, in order to minimize the volume change of silicon-based active material particles, a method exists to use only a portion of the total capacity of the silicon-based active material particles. For this purpose, the so-called prelithiation process is used, which inserts lithium ions into the negative electrode containing silicon-based active material particles in advance. Specifically, when lithium ions are inserted into the negative electrode by a method such as transferring lithium metal to the negative electrode, the lithium ions react with the irreversible sites of the negative electrode, reducing the total capacity of the negative electrode to the level of the reversible capacity. Therefore, since the amount of lithium ions inserted during battery operation can be suitably reduced to the level required for battery operation, the volume change of the silicon-based active material particles can be minimized.

[0011] However, during the process of lithiation by placing lithium metal on the surface of the negative electrode, excessive heat is generated due to the alloying reaction between lithium and silicon, and the possibility of ignition due to the reaction between lithium and moisture also increases. Furthermore, during the process of notching and punching the negative electrode, the possibility of ignition can be further increased due to the increase in the reaction area between lithium and silicon-based active materials, and there is also the possibility of ignition due to silicon-based active material particles that have undergone lithiation, which presents a serious safety issue.

[0012] Therefore, a new technology is required that can improve the life of a battery by pre-inserting lithium ions into the negative electrode before battery operation, while suppressing excessive heat generation and the possibility of ignition.

[0013]

[0014] The problem to be solved by the present invention is to provide a method for manufacturing an electrode in which, when transferring lithium metal to an electrode and performing prelithiation, a lithium metal layer having a lithium buffer layer formed on both sides thereof is used, thereby preventing the formation of an inactive layer on the surface of the lithium metal layer due to a side reaction of highly reactive lithium while performing the prelithiation reaction in a stable atmosphere, and in which the lithium buffer layer is decomposed upon activation after prelithiation and does not affect the electrode thickness, thereby preventing a decrease in energy density, and in which the decomposition is utilized as an additional lithium source to maximize the prelithiation effect.

[0015] Another problem to be solved by the present invention is to provide a secondary battery, which includes an electrode manufactured by the above-mentioned manufacturing method, and has improved life characteristics according to control of the available area of ​​the negative electrode, and can implement the unique characteristics of the negative electrode active material without any disadvantages.

[0016]

[0017] In order to solve the above problem, in one aspect of the present invention, a method for manufacturing an electrode is provided, comprising: a P1 step of forming an electrode structure by disposing a transfer laminate including a lithium metal layer having a lithium buffer layer formed on both sides thereof on a preliminary electrode active material layer so that the lithium buffer layer and the preliminary electrode active material layer are in contact; a P2 step of rolling the electrode structure; and a P3 step of aging the rolled electrode structure in a nitrogen atmosphere; wherein the nitrogen atmosphere is an atmosphere containing 80% by volume or more of nitrogen.

[0018] In order to solve the above problem, in another aspect of the present invention, an electrode is provided, comprising: a current collector; an electrode active material layer disposed on the current collector; and a lithium buffer layer disposed on the electrode active material layer; wherein the lithium buffer layer includes lithium carbonate and at least one of lithium oxide and lithium hydroxide, and does not contain lithium nitride.

[0019] In order to solve the above problem, in another aspect of the present invention, a lithium secondary battery is provided, which includes a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode as described above, wherein the positive electrode or the negative electrode is the above-described electrode.

[0020]

[0021] The method for manufacturing an electrode according to the present invention uses a lithium metal layer having a lithium buffer layer formed on both sides thereof, thereby preventing the formation of an inactive layer on the surface of the lithium metal layer due to a side reaction of highly reactive lithium, thereby solving the problem of increased resistance. In addition, upon activation after prelithiation, the lithium buffer layer is decomposed and does not affect the electrode thickness, thereby preventing a decrease in energy density. In addition, the lithium buffer layer can be utilized as an additional lithium source through decomposition, thereby maximizing the prelithiation effect. In addition, the risk in the process caused by direct contact of the lithium metal with the negative electrode can be reduced.

[0022] In addition, the lithium secondary battery according to the present invention can increase the available area of ​​the negative electrode by including an electrode manufactured by the above-described manufacturing method, thereby increasing the capacity. In particular, when using a silicon-based negative electrode active material, only a portion of the available area can be used without lithium loss from the positive electrode due to prelithiated lithium, thereby minimizing volume change, thereby having the advantage of improving life characteristics.

[0023]

[0024] FIG. 1 is a schematic diagram showing step P1 in a method for manufacturing an electrode according to one embodiment of the present invention.

[0025] FIG. 2 is a schematic diagram showing step P1 using a conductive laminate including a polymer layer in a method for manufacturing an electrode according to one embodiment of the present invention.

[0026] Figure 3 is a schematic diagram showing step P2 in a method for manufacturing an electrode according to one embodiment of the present invention.

[0027] Fig. 4 is a schematic diagram showing the P2` step in a method for manufacturing an electrode according to one embodiment of the present invention.

[0028] FIG. 5 is a photograph of the electrode surface of Example 1-1 taken after performing lithiation according to one embodiment of the present invention.

[0029] Figure 6 is a photograph of the electrode surface of Comparative Example 1-1 taken after performing lithiation.

[0030] Figure 7 is a photograph of the electrode surface of Comparative Example 1-4 taken after performing lithiation.

[0031]

[0032] Hereinafter, the present invention will be described in more detail to help understand the present invention.

[0033] Terms or words used in this specification and claims should not be interpreted as limited to their usual or dictionary meanings, but should be interpreted as meanings and concepts that conform to the technical idea of ​​the present invention, based on the principle that the inventor can appropriately define the concept of the term to explain his or her own invention in the best way.

[0034] The terminology used herein is for the purpose of describing exemplary embodiments only and is not intended to limit the present invention. Singular expressions include plural expressions unless the context clearly dictates otherwise.

[0035] In this specification, it should be understood that the terms “include,” “comprising,” or “having” are intended to specify the presence of a feature, number, step, component, or combination thereof, but do not preclude the possibility of the presence or addition of one or more other features, numbers, steps, components, or combinations thereof.

[0036] In this specification D 50In the particle size distribution curve of silver particles, it can be defined as the particle size corresponding to 50% of the volume accumulation amount. The above D 50 For example, it can be measured using the laser diffraction method. The laser diffraction method can generally measure particle diameters from the submicron range to several mm, and can obtain results with high reproducibility and high resolution.

[0037]

[0038] Method for manufacturing electrodes

[0039] The present invention provides a method for manufacturing an electrode, comprising: a P1 step of forming an electrode structure by placing a transfer laminate including a lithium metal layer having a lithium buffer layer formed on both sides thereof on a preliminary electrode active material layer so that the lithium buffer layer and the preliminary electrode active material layer are in contact; a P2 step of rolling the electrode structure; and a P3 step of aging the rolled electrode structure in a nitrogen atmosphere.

[0040]

[0041] According to one embodiment of the present invention, in the method for manufacturing the electrode, the step P1 is a step of forming an electrode structure by placing a transfer laminate including a lithium metal layer having a lithium buffer layer formed on both sides on a preliminary electrode active material layer formed on a current collector so that the lithium buffer layer and the preliminary electrode active material layer are in contact with each other.

[0042] Referring to FIG. 1, the transfer laminate (300) includes a lithium metal layer (320), and a lithium buffer layer (321) is formed on both sides of the lithium metal layer. In addition, the transfer laminate (300) may preferably further include a base film (310), and in this case, it may include a base film (310) and a lithium metal layer (320) positioned on the base film (310), and may have a structure in which a lithium buffer layer (321) is formed on both sides of the lithium metal layer. The base film (310) may be made of any material that can withstand high temperature conditions generated in the process of depositing the lithium metal layer (320) on the base film (310) without limitation. Specifically, the substrate film may include at least one selected from the group consisting of polyethylene terephthalate (PET), polyimide (PI), poly(methylmethacrylate) (PMMA), polypropylene, polyethylene, and polycarbonate.

[0043] According to one embodiment of the present invention, the lithium metal layer serves to supply lithium ions to the preliminary electrode active material layer. Specifically, the preliminary electrode active material layer may be positioned between the electrode current collector and the lithium buffer layer on the lithium metal layer.

[0044] The above lithium metal layer includes solid lithium metal, and specifically, the lithium metal layer may be made of solid lithium metal. The lithium metal layer may be inserted into the electrode active material layer through solid-state diffusion of lithium metal through a series of processes such as transfer, rolling, and aging, and thus, after activation, the lithium metal layer may not exist and may exist in an extremely thin state.

[0045] Meanwhile, the lithium metal layer may be formed of solid lithium metal, and lithium metal is a highly reactive metal that can react with oxygen (O2), nitrogen (N2), or water vapor (H2O) even in an air atmosphere, and the reaction may cause loss of the lithium metal or form an inactive layer such as lithium nitride or lithium oxide on the surface. The presence of such an inactive layer may act as resistance and cause a problem of lowering the output characteristics of the secondary battery, and since a layer that does not have a special function exists on the electrode, the effect may not be significant at the cell level, but a decrease in energy density may become a problem at the module or pack level.

[0046] In order to solve this problem, according to one embodiment of the present invention, the lithium metal layer has a lithium buffer layer formed on both sides, so that even when the base film is removed from the electrode structure, the lithium metal layer is not exposed to the outside and the lithium buffer layer exists as the uppermost layer. The lithium buffer layer may include lithium carbonate (Li2CO3), and the main component may be lithium carbonate, and may further include at least one of lithium oxide (LiO, Li2O) and lithium hydroxide (LiOH) as a by-product, but is characterized in that it does not include at least lithium nitride (Li3N). Specifically, the lithium buffer layer may include lithium carbonate in an amount of 80 wt% or more, preferably 85 wt% or more, more preferably 90 wt% or more, or 95 wt% or more. If the lithium carbonate content is less than the above content, the amount of other lithium compounds relatively increases, and in this case, it may be difficult to expect the aforementioned effect.

[0047] According to one embodiment of the present invention, the lithium buffer layer formed between the lithium metal layer and the base film can significantly reduce the possibility of causing a side reaction by preventing the lithium metal layer from being exposed to the air before or after prelithiation or during the transfer process, thereby preventing an inactive layer mainly composed of lithium nitride and / or lithium oxide from being formed on the surface of the lithium metal layer.

[0048]

[0049] In addition, lithium carbonate, which is the main component of the lithium buffer layer, can be decomposed in the activation process after prelithiation, and the lithium generated during decomposition can be used as an additional lithium source, which has the advantage of contributing to improving the capacity and lifespan of the battery. Furthermore, since there is no transfer laminate used for prelithiation remaining on the electrode after the activation process, it may not affect the electrode thickness at all, and this can be expected to improve the energy density in modules or packs.

[0050] Meanwhile, the lithium buffer layer may include lithium oxide and / or lithium hydroxide, which may be compounds that are inevitably generated when forming the lithium buffer layer on the lithium metal layer.

[0051] In addition, in the case of the lithium nitride, it is characterized by not being included in the lithium buffer layer. Lithium nitride has a higher stability than other lithium compounds and has a characteristic of not being easily decomposed even after tens or hundreds of cycles, and it may be a compound that fixes lithium at a large proportion, which may result in a large loss of lithium, and may then act as a resistor and lower the output characteristics. Accordingly, the lithium buffer layer according to one embodiment of the present invention may not include lithium nitride, and this can be appropriately controlled through surface treatment of the lithium metal layer when manufacturing a transfer laminate.

[0052]

[0053] According to one embodiment of the present invention, the transfer laminate may be manufactured by a method including a step (S1) of surface-treating both sides of a lithium metal layer to form a lithium buffer layer. In addition, when the transfer laminate includes a substrate film, the method may further include a step (S2) of arranging the substrate film on one of the lithium buffer layers.

[0054] The method for surface-treating both sides of the lithium metal layer may be a method in which, when depositing lithium to form a film, a mixed gas atmosphere of CO2 and Ar is created at the beginning of deposition to induce a reaction with lithium, and then the mixed gas atmosphere is created again after the deposition of lithium to a desired thickness is completed. Alternatively, a lithium metal film may be placed in a vacuum chamber to create the mixed gas atmosphere, thereby forming a lithium buffer layer mainly composed of lithium carbonate on both sides simultaneously. The mixed gas may be a mixture of CO2 and Ar in a volume ratio of about 3:97 to 40:60, preferably a volume ratio of 5:95 to 30:70 may be applied, and more preferably 5:95 to 20:80.

[0055]

[0056] According to one embodiment of the present invention, the thickness of the lithium buffer layer may be 50 nm or less, and this can be controlled to an appropriate level by adjusting the conditions of the method. When the thickness of the lithium buffer layer is 50 nm or less, it can act as a lithium source that can be decomposed through activation, and can effectively prevent side reactions in the lithium metal layer.

[0057] According to one embodiment of the present invention, in the transfer laminate, the thickness of the lithium metal layer may be 1 µm to 10 µm, specifically 3 µm to 9 µm, and more specifically 4 µm to 6.5 µm. When the above range is satisfied, the degree of breakage of the positive electrode active material particles on the positive electrode surface can be reduced, and an explosive reaction at the negative electrode can be prevented in advance, so that the initial capacity decrease of the battery can be suppressed.

[0058] According to one embodiment of the present invention, the loading amount of the lithium metal layer (unit: mAh / cm) 2 ) is the loading amount of the preliminary electrode active material layer (unit: mAh / cm 2 ) can be 4% to 40%, specifically 12% to 35%, and more specifically 20% to 30%. When the above range is satisfied, the generation of by-products is small, and lithium can be easily inserted into the electrode active material, so that the target lithium insertion capacity can be easily achieved.

[0059]

[0060] According to one embodiment of the present invention, in the P1 step, referring to FIG. 1, the preliminary electrode active material layer (120') is positioned on the electrode current collector (110), and the transfer laminate (300) is positioned on the preliminary electrode active material layer (120'), so that the electrode structure (400) can be formed such that the lithium buffer layer (321) and the preliminary electrode active material layer are in contact with each other.

[0061]

[0062] Meanwhile, referring to FIG. 2, the transfer laminate (300) according to one embodiment of the present invention may further include a polymer layer (330). The polymer layer (330) may be positioned on the lithium buffer layer (321). The polymer layer may play a role in enabling the lithium metal layer to be effectively peeled off from the transfer laminate during the manufacture of the electrode, thereby allowing the lithium metal layer to be easily transferred to the electrode active material layer. That is, the polymer layer may be separated from the transfer laminate together with the lithium metal layer and positioned on the electrode active material layer. The polymer layer may be present in contact with the electrode active material layer, or, in contrast, when the lithium metal layer is not entirely transferred to the electrode active material layer, a lithium metal layer may be present between the polymer layer and the electrode active material layer.

[0063] The polymer layer may be at least one selected from the group consisting of polyethylene terephthalate (PET), polyimide (PI), poly(methylmethacrylate) (PMMA), polypropylene, polyethylene, and polycarbonate. Accordingly, in a secondary battery including the electrode, the polymer layer may be dissolved in an electrolyte included in the secondary battery, thereby preventing the resistance of the battery from increasing. In particular, the polymer layer may include PMMA, in which case the above-described effect may be further improved.

[0064] The thickness of the polymer layer may be 0.1 ㎛ to 10 ㎛, specifically 0.5 ㎛ to 5 ㎛, and more specifically 1 ㎛ to 2.5 ㎛. When the above range is satisfied, the lithium metal layer can be easily transferred to the electrode active material layer, and the reverse transfer phenomenon in which the electrode active material layer is transferred to the transfer laminate can be prevented.

[0065]

[0066] According to one embodiment of the present invention, the step P2 in the method for manufacturing the electrode is a step of rolling the electrode structure.

[0067] Referring to FIG. 3, in step P2, the manufactured electrode structure (400) can be rolled. The rolling can be performed using a roll press method. Specifically, pressure can be applied vertically to the electrode structure (400) passing through the space by two rolls (R) spaced apart from each other in the vertical direction with a predetermined space, and the pressure can be a linear pressure. Through the rolling process, the lithium metal layer included in the transfer laminate can be fixed as one layer within the positive electrode structure, and at least a portion of the lithium can begin to be inserted into the preliminary electrode active material layer.

[0068] The pressure applied to the electrode structure during the above rolling may be 10 kgf / cm to 90 kgf / cm, specifically 15 kgf / cm to 80 kgf / cm, and more specifically 20 kgf / cm to 40 kgf / cm.

[0069] When the above rolling pressure is applied within the above range, the lithium metal layer can be effectively transferred. Accordingly, the effect of simultaneously satisfying both lifespan improvement and capacity characteristics can be achieved.

[0070]

[0071] According to one embodiment of the present invention, the method for manufacturing the electrode may further include a step of removing the substrate film from the electrode structure after the rolling in the P2 step, when the transfer laminate (300) includes a substrate film (310).

[0072] Referring to FIG. 4, in the P2` step, the electrode (100) can be manufactured by removing the base film (310) from the electrode structure after the rolling performed in the P2 step. When the polymer layer (330) is positioned on the lithium buffer layer (321), the polymer layer (330) is positioned between the base film (310) and the lithium buffer layer (321), thereby allowing the base film (310) to be removed more easily.

[0073]

[0074] According to one embodiment of the present invention, the method for manufacturing the electrode includes a P3 step of aging the rolled electrode structure in a nitrogen atmosphere.

[0075] The above aging may be a step of resting (leaving) for 1 minute to 600 minutes, specifically 1 minute to 30 minutes, in a nitrogen atmosphere, and at this time, the nitrogen atmosphere may have a nitrogen concentration of 80% by volume or more, or 85% by volume or more, and preferably 90% by volume or more, and the aging may be performed at 15°C to 40°C, preferably 17°C or more, or 20°C or more, and preferably 35°C or less, more preferably 30°C or less, or 28°C or less. The above aging conditions are such that by applying a nitrogen atmosphere, the explosive prelithiation reaction is effectively controlled, and thus the risk of fire is significantly reduced, and the stability that the reaction can proceed stably can be expected. Furthermore, since the lithium buffer layer prevents the formation of lithium nitride on the surface of the lithium metal even when a nitrogen atmosphere is applied, there is an advantage in that problems such as an increase in resistance caused by the formation of lithium nitride can be prevented.

[0076]

[0077] electrode

[0078] An electrode according to the present invention comprises: a current collector; an electrode active material layer disposed on the current collector; and a lithium buffer layer disposed on the electrode active material layer; wherein the lithium buffer layer comprises lithium carbonate and at least one of lithium oxide and lithium hydroxide, and is characterized in that it does not contain lithium nitride.

[0079] Specifically, the electrode may be derived from an electrode structure including a transfer laminate including a lithium metal layer having a lithium buffer layer formed on both sides thereof; and a current collector and a preliminary electrode including a preliminary electrode active material layer disposed on the current collector; and the lithium buffer layer of the transfer laminate and the preliminary electrode active material layer of the preliminary electrode are disposed so as to be in contact.

[0080]

[0081] According to one embodiment of the present invention, the electrode may be a positive electrode, and the positive electrode includes a positive electrode active material layer. The positive electrode active material layer may constitute the positive electrode by itself, but the positive electrode active material layer may be positioned on a positive electrode current collector, and the positive electrode active material layer may be positioned on one or both sides of the positive electrode current collector.

[0082] According to one embodiment of the present invention, the positive electrode current collector is not particularly limited as long as it is conductive and does not cause a chemical change in the battery, and for example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. may be used. In addition, the positive electrode current collector may typically have a thickness of 3 to 500 μm, and fine unevenness may be formed on the surface of the current collector to increase the adhesive strength of the positive electrode active material. For example, the positive electrode current collector may be used in various forms such as a film, a sheet, a foil, a net, a porous body, a foam, a non-woven fabric, etc.

[0083]

[0084] According to one embodiment of the present invention, the positive electrode active material layer includes a positive electrode active material, and the positive electrode active material is a material capable of causing an electrochemical reaction, and may be a lithium transition metal oxide. For example, the positive electrode active material may be a layered compound such as lithium cobalt oxide, lithium nickel oxide, etc. substituted with one or more transition metals; lithium manganese oxide substituted with one or more transition metals; Li[Ni 1-y M 1 y ]O2(where, M 1 Lithium nickel-based oxide expressed as Li is at least one selected from Co, Mn, Al, Cu, Fe, Mg, B, Cr, Zn, and Ga, and 0.01≤y≤0.7; 1+z [Ni b Mn c Co 1-(b+c+d) M 2 d ]O (2-e) A e (Here, M 2 Lithium nickel cobalt manganese composite oxide expressed as (wherein -0.5≤z≤0.5, 0.1≤b≤0.8, 0.1≤c≤0.8, 0≤d≤0.2, 0≤e≤0.2, b+c+d<1) wherein A is at least one selected from the group consisting of Al, Mg, Cr, Ti, Si, and Y, and A is at least one selected from the group consisting of F, P, and Cl; Li 1+x [M 3 1-q M 4 q ]PO 4-r X r (Here, M 3 is at least one selected from the group consisting of Fe, Mn, Co, and Ni, and M 4is at least one selected from the group consisting of Al, Mg, and Ti, X is at least one selected from the group consisting of F, S, and N, and may include at least one selected from the group consisting of olivine-based lithium metal phosphates expressed by (-0.5≤x≤0.5, 0≤q≤0.5, 0≤r≤0.1).

[0085] Specifically, the positive electrode active material may be composed of a lithium nickel-based oxide, a lithium nickel cobalt manganese composite oxide, an olivine-based lithium metal phosphate, or a combination thereof, and these may be combined to form a positive electrode active material layer as one layer or as separate layers.

[0086] According to one embodiment of the present invention, more specifically, the positive electrode active material may include a compound of the following chemical formula 1, and more specifically, may be a compound of the following chemical formula 1.

[0087] [Chemical Formula 1]

[0088] Li 1+x [Ni a Co b Mn c M 1 (1-a-b-c) ]O (2-d) A d

[0089] In the above chemical formula 1,

[0090] M 1 may be at least one selected from the group consisting of Al, Mg, Cr, Ti, Si, and Y, and may be specifically Al.

[0091] A is at least one selected from the group consisting of F, P, and Cl, and may be specifically F.

[0092] The above x can satisfy -0.5≤x≤0.5, specifically -0.3≤x≤0.3.

[0093] The above a can satisfy 0.6≤a<1, specifically 0.7≤a≤0.9.

[0094] The above b can satisfy 0.03≤b≤0.1, specifically 0.05≤b≤0.1.

[0095] The above c can satisfy 0.03≤c≤0.1, specifically 0.05≤c≤0.1.

[0096] The above d can satisfy 0≤d≤0.1, specifically 0≤d≤0.05.

[0097] Above a, b, c are 0 <a+b+c≤1, 구체적으로 a+b+c=1를 만족한다.

[0098] The compound of the above chemical formula 1 may be in particle form.

[0099] The compound of the above chemical formula 1 may be in the form of a secondary particle in which a plurality of primary particles are bonded to each other. Specifically, the compound of the above chemical formula 1 may be in the form of a secondary particle in which 10 or more primary particles are bonded to each other. Accordingly, there is an effect in which lithium can be uniformly inserted and de-inserted into the positive electrode active material.

[0100] D of the compound of the above chemical formula 1 50 The size may be 5 ㎛ to 15 ㎛, specifically 7 ㎛ to 12 ㎛, and more specifically 9 ㎛ to 10 ㎛. The above D 50 D of secondary particles 50 It can be. When the above range is satisfied, the positive electrode slurry can be easily dispersed, enabling uniform coating of the positive electrode active material layer.

[0101] The positive electrode active material may be included in the positive electrode active material layer at 90 wt% to 99 wt%, specifically at 92 wt% to 98 wt%, and more specifically at 95 wt% to 98 wt%.

[0102] According to one embodiment of the present invention, the positive electrode active material layer may further include a positive electrode binder. The positive electrode binder serves to improve adhesion between positive electrode active material particles and adhesion between the positive electrode active material and the positive electrode current collector. Specific examples thereof include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene butadiene rubber (SBR), fluoroelastomer, or various copolymers thereof, and one of these may be used alone or a mixture of two or more thereof.

[0103] The positive electrode binder may be included in the positive electrode active material layer at 0.5 wt% to 5.0 wt%, specifically at 1.0 wt% to 2.5 wt%, and more specifically at 1.0 wt% to 2.0 wt%.

[0104] According to one embodiment of the present invention, the positive electrode active material layer may further include a positive electrode conductive material. The positive electrode conductive material is used to provide conductivity to the electrode, and in the battery to be formed, any material that does not cause a chemical change and has electronic conductivity may be used without particular limitation. Specific examples thereof include graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, summer black, and carbon fiber; metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and the like. One of these may be used alone or a mixture of two or more may be used.

[0105] The positive electrode conductive material may be included in the positive electrode active material layer at 0.5 wt% to 30.0 wt%, specifically at 0.5 wt% to 10.0 wt%, and more specifically at 1.0 wt% to 4.0 wt%.

[0106] According to one embodiment of the present invention, in the positive electrode, the porosity of the positive electrode active material layer may be 10% to 40%, specifically 15% to 35%, and more specifically 25% to 30%. In this case, no additional thickness change may occur during rolling.

[0107]

[0108] According to one embodiment of the present invention, the electrode may be a negative electrode, the negative electrode may include a negative electrode active material layer, the negative electrode active material layer may include a negative electrode active material, and the negative electrode active material may be a silicon-based negative electrode active material, a carbon-based negative electrode active material, or a combination thereof.

[0109] According to one embodiment of the present invention, the negative electrode active material may include a silicon-based negative electrode active material. The silicon-based negative electrode active material may include Si and SiO. x (0 <X<2) 중 적어도 어느 하나를 포함할 수 있다.

[0110] The above Si is a silicon particle. It may be a silicon particle (particle made of silicon) called so-called pure silicon. The silicon particle can effectively improve the capacity of the negative electrode. The SiO x (0 <X<2)는 Si 및 SiO2가 포함된 형태일 수 있으며, 상기 Si는 상(phase)을 이루고 있을 수도 있다. 즉, 상기 X는 상기 SiO x (0 <X<2) 내에 포함된 Si에 대한 O의 개수비에 해당한다. 상기 실리콘계 복합 입자가 상기 SiO x(0 <X<2)를 포함하는 경우, 이차 전지의 방전 용량이 개선될 수 있다.

[0111] According to one embodiment of the present invention, the silicon-based negative electrode active material has a problem of very poor lifespan characteristics due to extreme volume change during battery operation, but when combined with a positive electrode according to the method for manufacturing an electrode according to the present invention, when activated from a pre-lithiated positive electrode, excess lithium ions other than lithium in the positive electrode active material, which determine the capacity, move to the silicon-based negative electrode active material and react with the silicon-based negative electrode active material in advance, thereby forming an irreversible phase and reducing the available area, thereby minimizing the extreme volume change during battery operation, so that the lifespan can be significantly improved, and the high-capacity characteristic, which is a characteristic inherent to the silicon-based negative electrode active material, can be sufficiently expressed. Furthermore, even when the method for manufacturing according to one embodiment of the present invention is applied to the silicon-based negative electrode active material itself, while obtaining the same effect as described above, it is possible to control the pre-lithiation reaction through the lithium buffer layer, thereby reducing the risk caused by the existing alloying reaction of lithium and silicon.

[0112]

[0113] According to one embodiment of the present invention, the negative electrode active material may further include a carbon-based negative electrode active material. The carbon-based negative electrode active material may include at least one selected from the group consisting of artificial graphite, natural graphite, and graphitized mesocarbon microbeads.

[0114] According to one embodiment of the present invention, the negative electrode active material layer may further include a negative electrode binder. The above negative electrode binder may include at least one selected from the group consisting of polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride, polyacrylonitrile, polymethylmethacrylate, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, polyacrylic acid, ethylene-propylene-diene monomer (EPDM), sulfonated EPDM, styrene butadiene rubber (SBR), fluoroelastomer, polyacrylic acid, and a material in which hydrogens of these are substituted with Li, Na, Ca, etc., and may also include various copolymers thereof.

[0115] According to one embodiment of the present invention, the negative electrode active material layer may further include a negative electrode conductive material. The negative electrode conductive material is not particularly limited as long as it is conductive and does not cause a chemical change in the battery, and examples thereof include graphite such as natural graphite or artificial graphite; carbon black such as acetylene black, Ketjen black, channel black, paneth black, lamp black, thermal black, etc.; conductive fibers such as carbon fiber or metal fiber; conductive tubes such as carbon nanotubes; metal powders such as fluorocarbon, aluminum, and nickel powder; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.

[0116]

[0117] According to one embodiment of the present invention, the electrode is formed by depositing a lithium metal layer on the electrode through a transfer method, and lithium from the lithium metal layer is inserted into the electrode active material layer through solid-phase diffusion through rolling. This lithium can serve to reduce the available area of ​​the negative electrode.

[0118] Therefore, the available area of ​​the anode capacity can be reduced without loss of lithium in the cathode active material by prelithiated lithium, thereby suppressing excessive volume change of silicon-based active materials and improving battery life characteristics. Furthermore, this enables the capacity of the cathode active material to be available across the entire range, thereby increasing battery efficiency and maximizing energy density.

[0119] According to one embodiment of the present invention, the positive electrode is characterized in that, rather than conventionally performing prelithiation by bringing a lithium metal layer into contact with the negative electrode, a lithium metal layer is transferred and rolled onto the positive electrode, and then lithium ions inserted into the positive electrode are moved to the negative electrode during the activation process of the battery.

[0120] An electrode according to one embodiment of the present invention may be a positive electrode or a negative electrode, preferably a negative electrode, and more preferably a negative electrode in which a silicon-based active material is applied as a negative electrode active material, and specifically, the silicon-based active material may be silicon (Pure Si).

[0121]

[0122] lithium secondary battery

[0123] A lithium secondary battery according to the present invention includes a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode, and the positive electrode or the negative electrode is manufactured by the method described above.

[0124] Since the description of the positive and negative electrodes has been described above, their description is omitted.

[0125]

[0126] According to one embodiment of the present invention, the secondary battery includes a separator. The separator separates the negative electrode and the positive electrode and provides a passage for lithium ions to move. Any separator commonly used in secondary batteries can be used without particular limitation, and in particular, one having low resistance to ion movement of the electrolyte and excellent electrolyte moisture retention capacity is preferable. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof, may be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of high-melting-point glass fiber, polyethylene terephthalate fiber, etc. may be used. In addition, a coated separator containing a ceramic component or a polymer material to secure heat resistance or mechanical strength may be used, and may optionally be used in a single-layer or multi-layer structure.

[0127]

[0128] According to one embodiment of the present invention, the secondary battery may further include an electrolyte. Examples of the electrolyte include, but are not limited to, organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the manufacture of lithium secondary batteries.

[0129] Specifically, the electrolyte may include a non-aqueous organic solvent and a metal salt. As the above non-aqueous organic solvent, for example, an aprotic organic solvent such as N-methyl-2-pyrrolidinone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, gamma-butyrolactone, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyl tetrahydrofuran, dimethylsulfoxide, 1,3-dioxolan, formamide, dimethylformamide, dioxolan, acetonitrile, nitromethane, methyl formate, methyl acetate, triester phosphate, trimethoxy methane, dioxolan derivatives, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl pyrropionate, ethyl propionate, etc. can be used.

[0130] In particular, among the above carbonate-based organic solvents, ethylene carbonate and propylene carbonate, which are cyclic carbonates, are high-viscosity organic solvents with high dielectric constants and thus can be preferably used because they easily dissociate lithium salts. In addition, when low-viscosity, low-dielectric constant linear carbonates such as dimethyl carbonate and diethyl carbonate are mixed and used in an appropriate ratio with these cyclic carbonates, an electrolyte with high electrical conductivity can be produced, so that they can be used even more preferably.

[0131] The metal salt may be a lithium salt, and the lithium salt is a substance that is easily dissolved in the non-aqueous electrolyte, for example, the anion of the lithium salt is F - , Cl - , I - , NO3 - , N(CN)2 - , BF4 - , ClO4 - , PF6 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P- , CF3SO3 - , CF3CF2SO3 - , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - and (CF3CF2SO2)2N - One or more selected from the group consisting of may be used.

[0132] In addition to the electrolyte components, the electrolyte may further include one or more additives, such as, for example, a haloalkylene carbonate compound such as difluoroethylene carbonate, pyridine, triethylphosphite, triethanolamine, a cyclic ether, ethylene diamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride, for the purpose of improving the life characteristics of the battery, suppressing battery capacity decrease, and improving the discharge capacity of the battery.

[0133]

[0134] As described above, a secondary battery including a positive electrode according to the present invention stably exhibits excellent capacity and capacity retention, and is therefore useful in portable devices such as mobile phones, laptop computers, and digital cameras, and electric vehicles such as hybrid electric vehicles (HEVs).

[0135] Accordingly, according to another embodiment of the present invention, a battery module including the secondary battery as a unit cell and a battery pack including the same are provided.

[0136] The above battery module or battery pack can be used as a power source for one or more medium- to large-sized devices, such as a power tool; an electric vehicle (EV), a hybrid electric vehicle, and a plug-in hybrid electric vehicle (PHEV); or a power storage system.

[0137]

[0138] Example

[0139] Hereinafter, preferred embodiments are presented to help understand the present invention, but the above embodiments are only illustrative of the present disclosure, and it is obvious to those skilled in the art that various changes and modifications are possible within the scope and technical idea of ​​the present disclosure, and it is natural that such changes and modifications fall within the scope of the appended patent claims.

[0140]

[0141] Electrode manufacturing

[0142] Example 1-1: Preparation of cathode

[0143] The lithium metal was placed in a vacuum chamber so that both sides were exposed, and a mixed gas atmosphere of 95 vol% Ar and 25 vol% CO was created at room temperature (approximately 25°C) to form a lithium buffer layer with a thickness of 50 nm on the surface. The lithium buffer layer was analyzed using X-ray photoelectron spectroscopy (XPS) (Nexsa ESCA System, Thermo Fisher Scientific (ESCA-02)), and it was confirmed that lithium carbonate was the main component through the presence of 35 vol% Li, 25 vol% C, and 40 vol% O.

[0144] PET film (base film), a polymer layer (1 μm thick) made of PMMA and placed on the PET film, a lithium metal layer (6.2 μm thick, 1.28 mAh / cm) made of solid lithium metal and having lithium buffer layers formed on both sides and placed on the polymer layer 2 A transfer laminate containing a loading amount was prepared.

[0145] Meanwhile, the average particle diameter D of the negative active material 50 These 5 μm silicon particles were used. An anode including a preliminary anode active material layer containing the above-mentioned anode active material, a cathode binder, carboxymethyl cellulose (CMC), and a cathode conductive material, carbon nanotubes, in a weight ratio of 80:10:10 was prepared. The loading amount of the preliminary anode active material layer was 10 mAh / cm 2 and the thickness was 75 ㎛.

[0146] The above transfer laminate was placed on a preliminary negative electrode active material layer so that the lithium buffer layer and the preliminary negative electrode active material layer were in contact, and then rolled using a roll press method, and then aged for 120 minutes at room temperature in an atmosphere containing 90% by volume of nitrogen so that lithium was inserted into the negative electrode active material layer.

[0147]

[0148] Example 1-2: Preparation of cathode

[0149] When preparing the transfer layer, the lithium metal layer thickness is about 4 ㎛ thick (0.82 mAh / cm 2 A prelithiated negative electrode was manufactured in the same manner except that the loading amount was changed.

[0150]

[0151] Example 1-3: Preparation of cathode

[0152] A prelithiated negative electrode was manufactured using the same method, except that the thickness of the lithium buffer layer formed on both sides of the lithium metal layer was set to approximately 30 nm by controlling the time the lithium metal layer was exposed to the mixed gas atmosphere.

[0153]

[0154] Comparative Example 1-1: Manufacturing of a cathode

[0155] A negative electrode was manufactured in the same manner as in Example 1-1, except that a lithium metal layer without a lithium buffer layer was applied.

[0156]

[0157] Comparative Example 1-2: Manufacturing of the cathode

[0158] A negative electrode was manufactured in the same manner as in Example 1-1, except that a lithium metal layer without a lithium buffer layer was applied and that an air atmosphere (nitrogen of about 78 volume%) was applied instead of a nitrogen atmosphere during aging.

[0159]

[0160] Example 1-4: Preparation of the anode

[0161] A transfer laminate was prepared in the same manner as in Example 1-1 above.

[0162] Meanwhile, Li[Ni 0.86 Co 0.05 Mn 0.08 Al 0.01 ]O2 was used. The positive electrode active material was Li[Ni 0.86 Co 0.05 Mn 0.08 Al 0.01 ]O21 Multiple primary particles (10 or more) are combined to form secondary particles, and the average particle diameter of the secondary particles is D 50The thickness of the positive electrode active material was 9 μm. A positive electrode active material layer including the positive electrode active material, the positive electrode binder PVdF, and the positive electrode conductive material carbon nanotubes in a weight ratio of 98:1:1 was prepared, and the positive electrode current collector aluminum foil (thickness: 12 μm) was used. The loading amount of the positive electrode active material layer was 4.5 mAh / cm 2 , and the thickness was 140㎛.

[0163] The above transfer laminate was placed on a preliminary negative electrode active material layer so that the lithium buffer layer and the preliminary negative electrode active material layer were in contact, and then rolled using a roll press method, and then aged for 120 minutes at room temperature in an atmosphere containing 90% by volume of nitrogen so that lithium was inserted into the positive electrode active material layer.

[0164]

[0165] Example 1-5: Preparation of the anode

[0166] When preparing the transfer layer, the lithium metal layer thickness is about 4 ㎛ thick (0.82 mAh / cm 2 A prelithiated negative electrode was manufactured in the same manner except that the loading amount was changed.

[0167]

[0168] Example 1-6: Preparation of the anode

[0169] A prelithiated negative electrode was manufactured using the same method, except that the thickness of the lithium buffer layer formed on both sides of the lithium metal layer was set to approximately 30 nm by controlling the time the lithium metal layer was exposed to the mixed gas atmosphere.

[0170]

[0171] Comparative Example 1-3: Manufacturing of the anode

[0172] A positive electrode was manufactured in the same manner as in Example 1-2, except that a lithium metal layer without a lithium buffer layer was applied.

[0173]

[0174] Comparative Example 1-4: Manufacturing of the anode

[0175] A positive electrode was manufactured in the same manner as in Example 1-2, except that a lithium metal layer without a lithium buffer layer was applied and that an air atmosphere (nitrogen of about 78 volume%) was applied instead of a nitrogen atmosphere during aging.

[0176]

[0177] Experimental Example 1: Evaluation of the Lithium Ionization Reaction

[0178] For the lithiation reactions of Examples 1-1 to 1-6 and Comparative Examples 1-1 to 1-4, the peak temperature of the reaction and the time for forming lithium nitride were measured and are shown in Table 1 below.

[0179] 1) Peak temperature (℃): The peak temperature is the highest reaction temperature recorded during the lithiation reaction.

[0180] 2) Lithium nitride formation time (min): The lithium nitride formation time is the time when the electrode surface began to show a green light during the lithiation reaction without removing the polymer layer (release layer) from the electrode structure. When lithium nitride is formed on the electrode surface, a green light appears due to the polymer layer on the surface. For electrodes whose surface color did not change to green during the lithiation reaction, the change in electrode condition was observed for up to 7 days.

[0181] Electrode peak temperature (℃) Lithium nitride formation time Example 1-1 Cathode 28 > 120 min Example 1-2 Cathode 27 > 120 min Example 1-3 Cathode 29 > 120 min Comparative Example 1-1 Cathode 45 < 10 min (Front) Comparative Example 1-2 Cathode > 60 < 10 min (Front) Example 1-4 Anode 28 > 120 min Example 1-5 Anode 28 > 120 min Example 1-6 Anode 29 > 120 min Comparative Example 1-3 Anode 40 < 10 min (Front) Comparative Example 1-4 Anode 52 < 10 min (Partial)

[0182] Referring to Table 1 above, in the examples, lithium nitride was not formed during the reaction, and as a result of continuous storage and observation thereafter, it was confirmed that even after about 7 days, green light was not observed, as in Fig. 5, but rather a purple light was observed due to the surface polymer layer, and it can be seen that the lithiation reaction also proceeded very stably within the room temperature range. However, in the case of Comparative Examples 1-1 and 1-3, it was confirmed that the peak temperature of the pre-lithiation reaction was relatively high because the lithium metal layer was not surface-treated, and it was observed that lithium nitride was formed in just 10 minutes after the start of the reaction, and it was confirmed through FIG. 6 that greenish lithium nitride was formed on the entire electrode surface of Comparative Example 1-1. In addition, Comparative Examples 1-2 and 1-4 are cases in which pre-lithiation was carried out under general atmospheric conditions without surface treatment, and in Comparative Example 1-2, which is the negative electrode, the reaction was stopped when the reaction temperature exceeded 60℃ due to the risk of explosion during the pre-lithiation reaction, and in Comparative Example 1-4, the pre-lithiation reaction progressed at a somewhat dangerous level, and the formation of lithium nitride was observed on a part of the electrode surface in just 10 minutes after the start of the reaction, and as can be confirmed in FIG. 7, it can be seen that greenish lithium nitride was formed on a part of the surface.

[0183]

[0184] Manufacturing of lithium secondary batteries

[0185] Examples 2-1 to 2-2 and Comparative Examples 2-1 to 2-2: Manufacturing of lithium secondary batteries

[0186] Li[Ni as a cathode active material 0.86 Co 0.05 Mn 0.08 Al 0.01 ]O2 was used. The positive electrode active material was Li[Ni 0.86 Co 0.05 Mn 0.08 Al 0.01]O21 Multiple primary particles (10 or more) are combined to form secondary particles, and the average particle diameter of the secondary particles is D 50 The thickness of the positive electrode active material layer was 9 μm. The positive electrode active material layer, which included the positive electrode active material, the positive electrode binder PVdF, and the positive electrode conductive material carbon nanotubes in a weight ratio of 98:1:1, was prepared with an aluminum foil (thickness: 12 μm) as a positive electrode current collector. The loading amount of the positive electrode active material layer was 4.5 mAh / cm 2 , and the thickness was 140㎛.

[0187] The negative electrodes of Examples 1-1 and 1-2 and Comparative Examples 1-1 and 1-2, the positive electrode, and the porous polyethylene separator were assembled for each Example and Comparative Example using a winding method, and an electrolyte (ethylene carbonate (EC) / ethyl methyl carbonate (EMC) = 3 / 7 (volume ratio) and lithium hexafluorophosphate (LiPF6 1 mol)) was injected into the assembled battery to manufacture a preliminary lithium ion secondary battery.

[0188] The above-mentioned spare lithium ion secondary battery was charged to 4.2 V at a C-rate of 0.1 C and then discharged to 2.5 V to perform an activation process.

[0189]

[0190] Examples 2-4 to 2-5 and Comparative Examples 2-3 to 2-4: Manufacturing of lithium secondary batteries

[0191] Average particle diameter D as negative active material 50 These 5 μm silicon particles were used. An anode including a preliminary anode active material layer containing the above-mentioned anode active material, the anode binder CMC, and the anode conductive material carbon nanotubes in a weight ratio of 80:10:10 was prepared. The loading amount of the preliminary anode active material layer was 10 mAh / cm 2 and the thickness was 75 ㎛.

[0192] The positive electrode, the negative electrode, and the porous polyethylene separator of Examples 1-4 and 1-5 and Comparative Examples 1-3 and 1-4 were each assembled by winding method for each Example and Comparative Example, and an electrolyte (ethylene carbonate (EC) / ethyl methyl carbonate (EMC) = 3 / 7 (volume ratio)) and lithium hexafluorophosphate (LiPF6 1 mol) were injected into the assembled battery to manufacture a preliminary lithium ion secondary battery.

[0193] The above-mentioned spare lithium ion secondary battery was charged to 4.2 V at a C-rate of 0.1 C and then discharged to 2.5 V to perform an activation process.

[0194]

[0195] Experimental Example 2: Evaluation of Resistance and Lifetime Characteristics

[0196] Charging and discharging were performed on each of the lithium secondary batteries of Examples 2-1, 2-2, 2-4 and 2-5 and Comparative Examples 2-1 to 2-4, and the resistance characteristics and life characteristics were evaluated using the following method, and the results are shown in Table 2 below.

[0197] 1) Resistance characteristics: For the lithium secondary battery, the resistance was measured by applying a 2.5C pulse current for a specific time at 50% SOC during discharge per cycle while performing charge / discharge cycles under the conditions below.

[0198] Resistance increase rate: [(resistance value after 200 cycles) / (resistance value after 1 cycle)] x 100

[0199] 2) Life characteristics: The 1st and 2nd cycles were charged and discharged at 0.1C, and from the 3rd cycle onwards, the cycle was performed at 1C charge and 0.5C discharge, and the number of cycles at which the SOC was maintained at 80% or higher was measured.

[0200] Charging conditions: CC (constant current) / CV (constant voltage) (5mV / 0.005C current cut-off) 4.2V

[0201] Discharge conditions: CC (constant current) condition 2.5 V

[0202]

[0203] Resistance (mΩ) SOC 80% maintenance cycle number 1 time 50 times 100 times 150 times 200 times Resistance increase rate (%) Cathode Example 2-10.88 0.88 0.95 1.05 1.23 139% 200 Example 2-20.88 0.89 0.85 1.01 1.28 145% 200 Comparative Example 2-11.47 1.87 2.10 2.15 2.33 158% 30 Comparative Example 2-21.25 1.24 1.41 1.87 2.09 167% 50 Anode Example 2-40.87 0.87 0.88 0.90 1.01 116% 350 Example 2-50.930.920.931.001.11119%250Comparative example 2-30.981.101.171.251.48151%250Comparative example 2-40.981.011.081.191.52155%150

[0204] Referring to Table 2 above, in the case of lithium secondary batteries of Examples 2-1 and 2-2 equipped with negative electrodes to which the pre-lithiation method according to the present invention was applied, it can be confirmed that the initial resistance and the resistance increase rate are lower than those of the lithium secondary batteries of Comparative Examples 2-1 and 2-2 equipped with negative electrodes to which the pre-lithiation method according to the present invention was applied, and thus the resistance characteristics are excellent. This is because lithium nitride is formed on the surface and acts as a resistor, and it can be seen that it continues to act as a resistor without being decomposed even during the cycle. It can be confirmed that these results are the same for the positive electrode as well through a comparison of Examples 2-4 and 2-5 and Comparative Examples 2-3 and 2-4. In particular, in the case of the positive electrode, there was no extreme difference in the initial resistance value as in the negative electrode, but it can be confirmed that the resistance increased significantly in the case of the Comparative Example.

[0205] Meanwhile, in terms of life characteristics, when comparing Examples 2-1 and 2-2 with Comparative Examples 2-1 and 2-2, it can be seen that the effect of the method of the present invention is maximized when applied to the cathode, and when comparing Examples 2-4 and 2-5, which are positive electrodes, with Comparative Examples 2-3 and 2-4, it can be confirmed that there is a clear improvement, although the difference is not as large as in the case of the cathode.

[0206]

[0207] [Explanation of symbols]

[0208] 110: Electrode current collector

[0209] 120, 120`: Preliminary electrode active material layer

[0210] 300: Warrior Laminate

[0211] 310: Base film

[0212] 320: Lithium metal layer

[0213] 321: Lithium buffer layer

[0214] 330: Polymer layer

[0215] 400: Electrode structure

[0216] R: Roll

Claims

1. Step P1 of forming an electrode structure by placing a transfer laminate including a lithium metal layer having a lithium buffer layer formed on both sides on a preliminary electrode active material layer so that the lithium buffer layer and the preliminary electrode active material layer are in contact; Step P2 of rolling the above electrode structure; and P3 step of aging the above rolled electrode structure in a nitrogen atmosphere; A method for manufacturing an electrode, wherein the above nitrogen atmosphere is an atmosphere containing 80% by volume or more of nitrogen.

2. In claim 1, A method for manufacturing an electrode, wherein the aging of the above P4 step is performed at 15°C to 40°C.

3. In claim 1, A method for manufacturing an electrode, wherein the lithium buffer layer comprises lithium carbonate.

4. In claim 3, A method for manufacturing an electrode, wherein the lithium buffer layer further comprises at least one of lithium oxide and lithium hydroxide.

5. In claim 3, A method for manufacturing an electrode, characterized in that the lithium buffer layer does not contain lithium nitride.

6. In claim 1 A method for manufacturing an electrode, wherein the thickness of the lithium metal layer is 1 ㎛ to 10 ㎛.

7. In claim 1 A method for manufacturing an electrode, wherein the thickness of the lithium buffer layer is 50 nm or less.

8. In claim 1 A method for manufacturing an electrode, wherein the above-mentioned transfer laminate is manufactured by a method including a step (S1) of surface-treating both sides of a lithium metal layer to form a lithium buffer layer.

9. In claim 1, A method for manufacturing an electrode, wherein the above electrode is a cathode, and the electrode active material is a cathode active material, and includes a silicon-based cathode active material.

10. A current collector; an electrode active material layer disposed on the current collector; and a lithium buffer layer disposed on the electrode active material layer; An electrode wherein the lithium buffer layer comprises lithium carbonate, at least one of lithium oxide and lithium hydroxide, and does not contain lithium nitride.

11. In claim 10, The above electrodes are A transfer laminate comprising a lithium metal layer having a lithium buffer layer formed on both sides; and A pre-electrode including a current collector and a pre-electrode active material layer disposed on the current collector; An electrode derived from an electrode structure in which the lithium buffer layer of the above-mentioned transfer laminate and the preliminary electrode active material layer of the above-mentioned preliminary electrode are arranged in contact.

12. In claim 10, An electrode wherein the above electrode is a cathode, and the electrode active material is a cathode active material, and includes a silicon-based cathode active material.

13. A lithium secondary battery comprising a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode, wherein the positive electrode or the negative electrode is the electrode of claim 10.

Citation Information

Patent Citations

  • Laminated lithium-ion battery

    JP2013084420A

  • Operating method of server load balancing apparatus, local domain name server and content delivery service system

    KR1020210007231A

  • Laser generator including burst pulse amplifier

    KR1020230161815A

  • Crown of dental implant

    KR102043772B1

  • Artificial intelligence-based counterfeit screening inspection and digital certificate issuance method, device and program

    KR102472427B1

Cited By

  • Lithium supplementing method, pre-lithiated negative pole piece, secondary battery and electronic device

    CN119920844A