Green leaching of sewage sludge ash
Patent Information
- Application Number
- PCT/SG2024/050296
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-22
- Filing Date
- 2024-05-08
- Publication Date
- 2024-11-28
Smart Images

Figure SG2024050296_28112024_PF_FP_ABST
Abstract
Description
GREEN LEACHING OF SEWAGE SLUDGE ASHFIELD OF THE INVENTION
[0001] The present invention generally relates to a method of ash leaching. In particular, the present invention relates to a method of green leaching of Sewage Sludge Ash.BACKGROUND
[0002] Ash is obtained from incineration of a variety of solid waste sources such as municipal waste, sewage sludge, various industrial wastes and thus has varied composition depending on its sources and the batches of even the same source material. It is broadly classified into fly ash (20-30%) and bottom ash (70-80%), which is collected from different places from the incinerator and has varied size and composition. Thus, different ash has varied sizes (a few hundred microns to up to a few mm) and chemical composition (metal composition, hydrocarbons etc.). Ash because of its heterogeneous sources is also composed of toxic components such as heavy metals, dioxins etc. which are produced in the incineration process in stable forms. The toxic components limit the use of ash for various applications due to environmental concerns. This is due to the leakage of these toxins into solvents on exposure which is termed as leaching [2, 3] and affects water bodies and human health [4, 9]. National limits have been put in place as for waste such as ash to be used in various applications such as construction material, road bases, sound barriers, etc., and only those materials that pass these national limits will be considered for the above stated applications. These national limits do vary across places with regards to the leaching protocol to be tested and the toxin contents of the waste.
[0003] Sand has been widely used as aggregate for concrete given its size, chemical nature and abundant availability. 50 billion tonnes of sand and gravel are used every year and has doubled in the last decade and is the most consumed natural resource after water. This demand has also led to illegal mining of sand from riverbeds etc. which has affected the environment drastically in terms of nutrient scarcity, decline of marine species and flooding. Not all sand can be used for construction purposes. The desert sand is too fine, and the relatively coarser sand is preferred. Singapore has been the world’ s highest importer of sand for some time now and has a lot of reclaimed land using the imported sand. Singapore has increased its land mass by 20% in the last 40 years and is expected to increase more. There has been research on useof ash as substitutes to sand for building material where it has been used to replace concrete ingredients such as cement, sand etc. Success was been achieved with some types of ash such as coal ash, wood, rice husk ash, palm ash etc., which have been used at various replacement percentages here.
[0004] In order to make ash as substitutes for building materials, it has to be converted to non-toxic ash. Existing technologies use non-grccn, toxic, highly hazardous chemicals such as nitric acid and sulfuric acid to treat ash as to detoxify it to remove heavy metals. These technologies are not environment friendly due to post-treatment disposal concerns. Other technologies use high temperatures (> 1000 C) to lock the heavy metals inside the ash and thus are very energy intensive.
[0005] Thus, there is a need to overcome the above concerns and develop a novel method of removing the raw ash of its toxins so that it can be safely used in higher amounts as aggregates / fillers in concrete and other construction materials. The method needs to use green chemical which are more environmental friendly, and have low energy demand, compared to the existing technologies. This invention discloses a green, environment-friendly and low- energy method to remove the heavy metals in ash through chemical treatment, where a unique mix of green reagents was used to dissolve and chelate the heavy metals at temperatures less than 100 °C, within a short period of time such as 4 h. The reagent mix can be recycled, which improves the overall cost efficiency too.SUMMARY
[0006] In one aspect, the present disclosure refers to a method of synthesizing leached ash using a mixture of green chemical reagents comprising a main acid leachant and one or more chelating agent, the method comprising the following steps: a. incubating an ash with the mixture of green chemical reagents to dissolve and chelate heavy metal in the ash; and b. washing the ash using a solvent to remove the dissolved and chelated heavy metal.
[0007] Advantageously, the present disclosure converts the raw toxic incineration ash to safe non-toxic ash with heavy metal removed, which can be used as aggregates for construction applications in concrete, asphalt etc. The process involves green chemicals and low energydemand methods to remove the raw ash of its toxins so that it can be safely used in higher amounts as aggregates / fillers in concrete and other construction materials.BRIEF DESCRIPTION OF THE DRAWINGS
[0008] The invention will be better understood with reference to the detailed description when considered in conjunction with the non-limiting examples and the accompanying drawings, in which:
[0009] Figure 1 is a schematic diagram of processing ash using green chcmical / solvcnt.
[0010] Figure 2 is a set of bar graphs showing heavy metal removal using MSA. (a) IM MSA at different temperatures; (b) Various MSA concentrations at 100 °C; (c) 2M MSA at 100 °C at various time points- 2, 4, 12 and 24 h.
[0011] Figure 3 is a bar graph showing heavy metal removal of Sewage Sludge Ash using different green chemicals- nitrilotriacetic Acid (NTA), Ethylenediamine-N,N'-disuccinic acid (EDDS) , Citric Acid (CA), Malonic Acid (MA), and Methanesulfonic Acid (MSA).
[0012] Figure 4 is a set of bar graphs showing heavy metal removal of Sewage Sludge Ash using Methanesulfonic Acid (MSA) and Green Chelants- nitrilotriacetic Acid (NTA), Ethylenediamine-N,N' -disuccinic acid (EDDS) , Citric Acid (CA), and Malonic Acid (MA).
[0013] Figure 5 is a set of bar graphs showing heavy metal removal of Sewage Sludge Ash (a) Comparison of Raw Ash vs Ball Milled Ash; (b) Comparison of MSA vs Sulphuric Acid (SA).
[0014] Figure 6 is a bar graph showing recycling of acid for heavy metal removal.
[0015] Figure 7 is a set of Scanning electron microscope (SEM) images of (a) Raw Sewage Sludge Ash (SSA); (b) Treated and Washed Sewage Sludge Ash (G-SSA-W); (c) Treated and Unwashed Sewage Sludge Ash (G-SSA-UW). The SEM images shown in this figure were taken with 2000 x magnification. SSA- Raw Sewage Sludge Ash, G-SSA-W - Green Sewage Sludge Ash- Washed, G-SSA-UW- Green Sewage Sludge Ash- Unwashed.
[0016] Figure 8 is a line graph showing Particle Size Distribution of Raw & Treated Ash against ASTM standards for aggregate size.
[0017] Figure 9 is a line graph showing Sorption isotherms of Raw & Treated Sewage Sludge Ash.
[0018] Figure 10 is a graph showing Fourier-transform infrared (FTIR) spectroscopy images of Raw Sewage Sludge Ash (SSA); Treated & Washed Sewage Sludge Ash (G-SSA- W); and Treated & Unwashed Sewage Sludge Ash (G-SSA-UW).
[0019] Figure 11 is a graph showing X-ray diffraction (XRD) patterns of raw Sewage Sludge Ash (SSA); Treated & Washed Sewage Sludge Ash (G-SSA-W); and Treated & Unwashed Sewage Sludge Ash (G-SSA-UW).
[0020] Figure 12 is a graph showing thcrmogravimctric analysis (TGA) of raw and processed ash (washed and unwashed).DETAILED DESCRIPTION
[0021] The present disclosure describes a method to treat ash (sewage sludge ash in specific) obtained from incineration using green chemicals as to strip it of its toxins and thus make it a suitable aggregate both physically, chemically and toxicity wise, to be used in construction applications..
[0022] In one aspect, the present disclosure refers to a method of synthesizing leached ash using a mixture of green chemical reagents comprising a main acid leachant and one or more chelating agent, the method comprising the following steps: a. incubating an ash with the mixture of green chemical reagents to dissolve and chelate heavy metal in the ash; and b. washing the ash using a solvent to remove the dissolved and chelated heavy metal.
[0023] As used in, "leach", "leaching", "leached" or grammatical variants thereof means to dissolve out by the action of a percolating liquid. Specifically, when a chemical substance is leached from a material, it is removed by the action of a reagent passing through the material. For example, when a heavy metal is leached from an ash, it is removed by the action of a mixture of green chemical reagents comprising a main acid leachant and one or more chelating agent passing though the ash.
[0024] As used herein, "leachant" means a liquid used for leaching, for example, an acid such as Methane sulfonic acid (MSA) used for leaching.
[0025] As used herein, "chelating agent" means a chemical compound that can form stable complexes, called chelates, with metal ions by forming two or more coordinate covalent bonds with a metal ion. Common chelating agents in the field include nitrilotriacetic acid (NTA), citric acid (CA), malonic acid (MA), ethylenediamine-N,N'-disuccinic acid (EDDS), diethylenetriaminepentaacetic acid (DTPA), triethylenetetraminehexaacetic acid (TTHA), ethylenediaminetetraacetic acid (EDTA), tetrasodium glutamate diacetate (GLDA), Dimcrcapto Succinic Acid, penicillamine, Ethylcncbis(oxycthylcncnitrilo)tctraacctic acid(EGTA), 1,2-cyclohexylenedinitrilotetraacetic acid (CDTA), and so on. The chelating agents form stable chelates with a wide range of metal ions. Some chelating agents have a high degree of specificity for the target metal, while others chelate multiple types of metal.
[0026] In one example, the main acid leachant is methane sulfonic acid (MSA). MSA is a strong acid with a pKa of -1.19. It is also a green solvent which is non-oxidizing and biodegradable, and thus docs not cause harm to the environment.
[0027] In another example, the main acid leachant is nitrilotriacetic acid (NTA). In another example, the main acid leachant is ethylenediamine-N,N'-disuccinic acid (EDDS). In another example, the main acid leachant is citric acid (CA). In another example, the main acid leachant is malonic acid (MA).
[0028] In one example, the chelating agent is selected from the group consisting of nitrilotriacetic acid (NTA), ethylenediamine-N,N'-disuccinic acid (EDDS), citric acid (CA) and malonic acid (MA).
[0029] In one example, the concentration of the main acid leachant is 0.25-3 M and the concentration of the chelating agent is 0.1-1 M. In another example, the concentration of the main acid leachant is about 0.25 M. In another example, the concentration of the main acid leachant is about 0.5 M. In another example, the concentration of the main acid leachant is about 0.75 M. In another example, the concentration of the main acid leachant is about 1 M. In another example, the concentration of the main acid leachant is about 2 M. In another example, the concentration of the main acid leachant is about 3 M. In another example, the concentration of the chelating agent is about 0.1 M. In another example, the concentration of the chelating agent is about 0.2 M. In another example, the concentration of the chelating agent is about 0.3 M. In another example, the concentration of the chelating agent is about 0.4 M. In another example, the concentration of the chelating agent is about 0.5 M. In another example, the concentration of the chelating agent is about 0.6 M. In another example, the concentration of the chelating agent is about 0.7 M. In another example, the concentration of the chelating agent is about 0.8 M. In another example, the concentration of the chelating agent is about 0.9 M. In another example, the concentration of the chelating agent is about 1 M.
[0030] In one example, the incubation in step a is done at a temperature of 25 -100 °C. In another example, the incubation in step a is done at a temperature of about 25 °C. In another example, the incubation in step a is done at a temperature of about 50 °C. In another example, the incubation in step a is done at a temperature of about 75 °C. In another example, theincubation in step a is done at a temperature of about 100 °C. In another example, the incubation in step a is done at a temperature of 25- 125 °C.
[0031] In one example, the incubation duration in step a is 2-24 h. In another example, the incubation duration in step a is about 2 h. In another example, the incubation duration in step a is about 4 h. In another example, the incubation duration in step a is about 6 h. In another example, the incubation duration in step a is about 8 h. In another example, the incubation duration in step a is about 10 h. In another example, the incubation duration in step a is about 12 h. In another example, the incubation duration in step a is about 14 h. In another example, the incubation duration in step a is about 16 h. In another example, the incubation duration in step a is about 18 h. In another example, the incubation duration in step a is about 20 h. In another example, the incubation duration in step a is about 24 h. In another example, the incubation duration in step a is about 28 h. In another example, the incubation duration in step a is about 30 h.
[0032] In one particular example, the mixture of green chemical reagents comprises a main acid leachant which is methane sulfonic acid (MSA), and two chelating agents which are citric Acid (CA) and malonic Acid (MA). The concentration of MSA is 2 M or 3M, the concentration of CA is 0.1 M and the concentration of MA is 0.1 M. When this mixture of green chemical reagent is incubated with the ash, the ash:acid mass-volume ratio is 1:2-1:20. In one example, When this mixture of green chemical reagent is incubated with the ash, the ash:acid ratio is 1:10. In other words, 1 gram of ash was treated with 10 ml of acid. In another example, ash is incubated with this mixture of green chemical reagent at 100 °C for 4 h. Heavy metal removal increased with concentration of the mixture of green chemical reagents and temperature.
[0033] In one example, MSA alone is used to leach ash and remove heavy metals from the ash, and 2M concentration of MSA at 100 °C effected the highest heavy metal removal rate. The difference between 2M and 3M concentrations of MSA is insignificant. 4 hours incubation was found to be sufficient to remove heavy metal, which thus saves energy and cost.
[0034] In another example, nitrilotriacetic acid (NT A) alone is used to leach ash and remove heavy metals from the ash. In another example, ethylenediamine-N.N' -disuccinic acid (EDDS) alone is used to leach ash and remove heavy metals from the ash. In another example, citric acid (CA) alone is used to leach ash and remove heavy metals from the ash. In another example, malonic acid (MA) alone is used to leach ash and remove heavy metals from the ash. These acids arc incubated with ash at 25 -100 °C for 2-24 h.
[0035] In one example, the ash to be leached is a bottom ash or a flying ash. Ash is obtained from incineration of a variety of solid waste sources such as municipal waste, sewage sludge, and various industrial wastes. What is left over after solid waste incineration is ash. As used herein, a "bottom ash" refers to the coarser component of incineration ash. Rather than floating into the exhaust stacks, it settles to the bottom of the boiler. As used herein, a "flying ash" refers to a part of the incineration ash whose particles arc the smaller and lighter than the bottom ash, so that they “fly” up into the exhaust stacks. Fly ash is recyclable. The fine particles bind together and solidify, especially when mixed with water, making them an ideal ingredient in concrete and wallboard. Fly ash is captured from the flue gases using electrostatic precipitators (ESP) or in filter fabric collectors, commonly referred to as baghouses.
[0036] In one example, the bottom ash is Sewage Sludge Ash (SSA). Sewage Sludge Ash is the by-product produced during the combustion of dewatered sewage sludge in an incinerator. The raw Sewage Sludge Ash has a particle size distribution from a few hundred microns to up to a few mm (< 4.75mm) with the particles of irregular shape. In another example, the bottom ash is Incineration Bottom Ash (IBA). Incineration Bottom Ash refers to the incombustible materials that remain in the furnace after combustion of municipal solid waste (MSW).
[0037] The major threats to human health from heavy metals arc associated with exposure to arsenic, lead, cadmium, chromium, mercury, and so on. The effects of such heavy metals on human health have been extensively studied and reviewed by international organizations such as World Health Organization (WHO). Due to their toxicity, heavy metal contaminations have been regulated by national environmental standards in many countries. The present invention uses a mixture of green chemical reagents to leach the heavy metal (dissolve and chelate the heavy metal) in the ash. In one example, the heavy metal is selected from the group consisting of Aluminum (Al), Arsenic (As), Barium (Ba), Cadmium (Cd), Cobalt (Co), Chromium (Cr), Copper (Cu), Iron (Fe), Manganese (Mn), Nickel (Ni), Lead (Pb), Antimony (Sb), Vanadium (V) and Zinc (Zn). After leaching, 1-33% of the heavy metal of the ash is removed. In one example, after leaching using the mixture of green chemical reagents as disclosed herein, about 1% of the heavy metal of the ash is removed. In another example, after leaching using the mixture of green chemical reagents as disclosed herein, about 2% of the heavy metal of the ash is removed. In another example, after leaching using the mixture of green chemical reagents as disclosed herein, about 3% of the heavy metal of the ash is removed. In another example, afterleaching using the mixture of green chemical reagents as disclosed herein, about 5% of the heavy metal of the ash is removed. In another example, after leaching using the mixture of green chemical reagents as disclosed herein, about 7% of the heavy metal of the ash is removed. In another example, after leaching using the mixture of green chemical reagents as disclosed herein, about 8% of the heavy metal of the ash is removed. In another example, after leaching using the mixture of green chemical reagents as disclosed herein, about 10% of the heavy metal of the ash is removed. In another example, after leaching using the mixture of green chemical reagents as disclosed herein, about 12% of the heavy metal of the ash is removed. In another example, after leaching using the mixture of green chemical reagents as disclosed herein, about 15% of the heavy metal of the ash is removed. In another example, after leaching using the mixture of green chemical reagents as disclosed herein, about 18% of the heavy metal of the ash is removed. In another example, after leaching using the mixture of green chemical reagents as disclosed herein, about 20% of the heavy metal of the ash is removed. In another example, after leaching using the mixture of green chemical reagents as disclosed herein, about 22% of the heavy metal of the ash is removed. In another example, after leaching using the mixture of green chemical reagents as disclosed herein, about 25% of the heavy metal of the ash is removed. In another example, after leaching using the mixture of green chemical reagents as disclosed herein, about 28% of the heavy metal of the ash is removed. In another example, after leaching using the mixture of green chemical reagents as disclosed herein, about 30% of the heavy metal of the ash is removed. In another example, after leaching using the mixture of green chemical reagents as disclosed herein, about 33%> of the heavy metal of the ash is removed. In another example, after leaching using the mixture of green chemical reagents as disclosed herein, the heavy metal of the ash which is removed is in the range of about 1-33%, 1-30%, 1-28%, 1-25%, 1-22%, 1-20%, 1-18%, 1-15%, 1-12%, 1-10%, 1-8%, 1-5%, 2-33%, 2- 30%, 2-28%, 2-25%, 2-22%, 2-20%, 2-18%, 2-15%, 2-12%, 2-10%, 2-8%, 2-5%, 3-33%, 3- 30%, 3-28%, 3-25%, 3-22%, 3-20%, 3-18%, 3-15%, 3-12%, 3-10%, 3-8%, 3-5%, 5-33%, 5- 30%, 5-28%, 5-25%, 5-22%, 5-20%, 5-18%, 5-15%, 5-12%, 5-10%, 5-8%, 8-33%, 8-30%, 8- 28%, 8-25%, 8-22%, 8-20%, 8-18%, 8-15%, 8-12%, 8-10%, 10-33%, 10-30%, 10-28%, 10- 25%, 10-22%, 10-20%, 10-18%, 10-15%, 10-12%, 10-10%, 10-8%, 10-33%, 10-30%, 10-28%, 10-25%, 10-22%, 10-20%, 10-18%, 10-15%, 10-12%, 12-33%, 12-30%, 12-28%, 12-25%, 12-22%, 12-20%, 12-18%, 12-15%, 15-33%, 15-30%, 15-28%, 15-25%, 15-22%, 15-20%, 15-18%, 18-33%, 18-30%, 18-28%, 18-25%, 18-22%, 18-20%, 20-33%, 18-30%, 18-28%, 18-25%, 18-22%, 22-33%, 22-30%, 22-28%, 22-25%, 25-33%, 25-30%, 25-28%, 28- 33%, 28-30%, or 30-33%.
[0038] After incubating the ash with the mixture of green chemical reagents to dissolve and chelate heavy metal in the ash, the ash was then washed with a solvent. In one example, the solvent used for washing is water. In another example, the solvent used for washing is isopropanol. In another example, the solvent used for washing is a mixture of water and isopropanol.
[0039] After treatment using the method as disclosed herein, the treated ash has significantly reduced heavy metal concentrations, but with the elements of interest such as Calcium (Ca), Silicon (Si), Aluminium (Al) and Iron (Fe) that are necessary for construction related applications retained in the ash.
[0040] After washing, the ash may be dried in an oven at 80-110°C for 18-30 h. In one example, the ash is dried in an oven at 105 °C for 24 h.
[0041] The mixture of green chemical reagents from step a of the method as disclosed herein can also be recycled and reused to incubate a next batch of ash for leaching. The overall cost efficiency of the method is thus greatly improved. When recycling the mixture of green chemical reagents to incubate with the next batch of ash, the ash:acid mass-volume ratio is 1:10.
[0042] The thermal stability of the leached ash synthesized using the method as disclosed herein exhibits no weight loss up to 750 °C. The leached ash shows good thermal stability and is suitable to be used as aggregates as part of various applications. When used as a substitute for aggregate and cement to make mortars, up to 5% cement substitution and 30% aggregate substitution was made by the leached ash. The substituted material shows similar mechanical characteristics to that of the control (made purely using OPC & sand only), and at the same time, it does not have the issue of untreated ash, i.e. heavy metals leached from within causing harm to the environment.
[0043] As used in this application, the singular form “a,” “an,” and “the” include plural references unless the context clearly dictates otherwise. For example, the term “a metal” includes a plurality of metals, including mixtures and combinations thereof.
[0044] As used herein, the term “comprising” means “including.” Variations of the word "comprising", such as “comprise” and “comprises,” have correspondingly varied meanings.Thus, for example, a composition “comprising” X may consist exclusively of X or may include one or more additional unrecited components.
[0045] As used herein, the term “about” in the context of concentration of a substance, size of a substance, length of time, or other stated values means + / - 5% of the stated value, or + / - 4% of the stated value, or + / - 3% of the stated value, or + / - 2% of the stated value, or + / - 1% of the stated value, or + / - 0.5% of the stated value.
[0046] Throughout this disclosure, certain embodiments may be disclosed in a range format. It should be understood that the description in range format is merely for convenience and brevity and should not be construed as an inflexible limitation on the scope of the disclosed ranges. Accordingly, the description of a range should be considered to have specifically disclosed all the possible sub-ranges as well as individual numerical values within that range. For example, description of a range such as from 1 to 6 should be considered to have specifically disclosed sub-ranges such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6 etc., as well as individual numbers within that range, for example, 1 , 2, 3, 4, 5, and 6. This applies regardless of the breadth of the range.
[0047] The disclosure illustratively described herein may suitably be practiced in the absence of any element or elements, limitation or limitations, not specifically disclosed herein. Thus, for example, the terms "comprising", "including", "containing", etc. shall be read expansively and without limitation. Additionally, the terms and expressions employed herein have been used as terms of description and not of limitation, and there is no intention in the use of such terms and expressions of excluding any equivalents of the features shown and described or portions thereof, but it is recognized that various modifications are possible within the scope of the invention claimed. Thus, it should be understood that although the present invention has been specifically disclosed by preferred embodiments and optional features, modification and variation of the inventions embodied herein disclosed may be resorted to by those skilled in the art, and that such modifications and variations are considered to be within the scope of this invention.
[0048] The invention has been described broadly and generically herein. Each of the narrower species and subgeneric groupings falling within the generic disclosure also form part of the invention. This includes the generic description of the invention with a proviso or negative limitation removing any subject matter from the genus, regardless of whether or not the excised material is specifically recited herein.
[0049] Unless otherwise indicated, all technical and scientific terms used herein have the same meaning as commonly understood to one of ordinary skill in the art to which the invention belongs.
[0050] Other embodiments arc within the following claims and non-limiting examples.EXAMPLES
[0051] Non-limiting examples of the disclosure will be further described in greater detail by reference to specific Examples, which should not be construed as in any way limiting the scope of the disclosure.
[0052] In this invention, ash such as Sewage Sludge Ash (SSA) and Incineration Bottom Ash (IBA) is detoxified I modified using chemical methods and then explored for their applications such as being used as substitutes for cements / aggregates in concrete etc. Sewage Sludge Ash which is prominently produced in Singapore (600 tonnes per day) was tested initially for its geotechnical properties such as shear strength with sand, where both bottom ash and fly ash were found be similar [8]. The toxic content of ash was removed through chemical processing through use of various organic and inorganic acids [6] . Strong inorganic acids such as nitric acid and sulphuric acids have been commonly used for this purpose, but they lead to the issue of post-treatment disposal, causing concerns. Raw sewage sludge bottom ash was tested as a substitute for aggregate and cement to make mortars, where it was found that up to 5% cement substitution and 30% aggregate substitution was mechanically similar to that of the control (made purely using Ordinary Portland Cement (OPC) and sand only). Singapore has strict limits with regards to the heavy metal content of the leachates from ash to be used for commercial purposes. Use of green solvents is thus recommended, which does not cause harm to the environment. Methane sulfonic acid (MSA) is one such solvent [1, 10], which is a strong acid, with a pKa of -1.19
[0011] . It is non-oxidizing & biodegradable [1] and is thus environmentally friendly, which has been experimented previously for elemental leaching with success. In the past, MSA had been used for leaching Galena Concentrates, industrial byproducts such as iron, zinc rich residues (jarosite), silver granules, lamp phosphor residue, ores such as malachite, hemimorphite, and chalcopyrite [13-19]. It has not been used to leach Sewage Sludge Ash. The MSA used in this invention is process-optimized for heavy metal removal from Sewage Sludge Bottom Ash.
[0053] Example 1- Materials and Methods
[0054] Materials
[0055] Sewage Sludge Ash was received from Eco Special Waste Management. Methane sulfonic acid (MSA), Citric Acid, Malonic Acid, isopropanol as solvent were all purchased from sigma Aldrich. All chemicals were used without further purification and water used in all the experiments were obtained from Milli Q water system.
[0056] Synthesis of Leached Ash
[0057] Sewage Sludge Incineration Ash (1g) were leached using Methane Sulfonic Acid (IM) as the main reagent for heavy metal removal along with citric acid and malonic acid as chelating agents (ash / acid ratio of 1:10) at 100 °C for removal of heavy metals and were washed with solvent and dried in the oven (at 105 °C for 24 h). Solvents with different water: isopropanol ratios were used to wash the leached ash in order to ascertain the solvent effect on leaching. The optimized condition was to use pure water as solvent.
[0058] Characterization methods
[0059] Surface area of the raw and processed ash were measured using Quantachrome Autosorb iQ C-XR. All samples were degassed at 150 °C for 12 h before the N2 sorption analysis. Functional groups of the samples were analyzed by Fourier Transform InfraRed spectroscopy. Spectra were measured between 4000 and 400 cm-1on a Bruker Vertex 70 spectrometer with a Platinum attenuated total reflection (ATR) module. The X-ray diffraction (XRD) patterns were characterized on a Bruker D 8 Advance powder X-ray diffractometer. The morphology of the samples was examined by scanning electron microscope (FESEM) (JEOL, JSM-7610F) at an accelerating voltage of 20 kV, and high resolution transmission electron microscope (FETEM) (JEM-21 OOF) at an accelerating voltage of 200 kV. An elemental analyzer (EA, ThermoFisher Scientific FlashSmart CHNS Elemental Analyser) was used to investigate the composition of the samples. Thermal stability of the materials was carried out from 30 to 750 °C at a heating rate of 10 °C min-1under nitrogen atmosphere on a Perkin Elmer SII (Diamond series).
[0060] Leaching of Raw and Treated Ash
[0061] Raw and treated ashes were subjected to leaching using DT and seawater (at 27 Practical Salinity Unit (PSU)) at a liquid-to-solid (L / S) ratio of 2, based on EN 12457-1 to determine heavy metal contents. Leachates were filtered through a 0.45 pm membrane filter using vacuum pump and were acidified to pH <2 by adding concentrated HNO3 (I M, dilutedfrom 70 weight % HNOs purchased from Sigma Aldrich) and tested for various cations (Agilent ICP-OES 5100 and Agilent ICP-MS 7700x).
[0062] Example 2- Results
[0063] Referring to Fig. 1, the raw ash is processed using a green chemical mix consisting of a main acid leachant along with green chelating agents that help to solubilize the removed heavy metals that were acid-leached out. The treated ash has significantly reduced heavy metal concentrations, but with the elements of interest such as Calcium (Ca), Silicon (Si), Aluminium (Al) and Iron (Fe) etc. that are necessary for construction related applications retained in the ash. Thus the treated ash has relatively lesser toxicity concerns and can be used in greater amounts in construction materials.
[0064] Methane sulfonic acid (MSA) Treatment of Ash
[0065] Referring to Fig. 2, Methane sulfonic acid (MSA) was used for removing heavy metals from the Sewage Sludge Ash where it was seen that heavy metal removal increased with the concentration of MSA and temperature. 2M concentration of MSA at 100 °C effected the best removal. The difference between 2M and 3M concentrations was insignificant. The 2M MS A- 100 °C condition was tested for different time durations where 4 hours was found to be sufficient, which thus saved energy and cost.
[0066] Other Green Chelating Agents vs MSA Treatment of Ash
[0067] Referring to Fig. 3, other green reagents such as nitrilotriacetic acid (NTA), Ethylenediamine-N,N' -disuccinic acid (EDDS) , Citric acid (CA) and Malonic acid (MA) were all tested out at their best conditions against MSA to verify which green chemical was the most effective. It was seen that 2M MSA at 100 °C was the best condition for heavy metal removal amongst all tested green chemicals.
[0068] MSA + Green Chelating Agents Treatment of Ash
[0069] Referring to Fig. 4, an increase in heavy metal removal was observed when using CA and MA as individual and combined supplementary chelating agents, while EDDS as a supplementary chelating agent actually brought down the heavy metal removal efficiency (observed with both IM & 2M MSA), both individually and when used in combination with other chelating agents. 2M MSA+ 0.1M CA + 0.1M MA gave the best heavy metal removal effects of all the tested green mixes, where C A and MA played their combined role as chelating agents and enhanced metal removal effect of MSA, with the same pattern observed with IMMSA too. Thus, the green chemical reagents mixture of 2M MSA+ 0.1M CA + 0.1M MA was chosen as the best formulation for leaching ash. The leached ash was washed thoroughly, characterized and examined for elemental content and leaching, as discussed below.
[0070] Referring to Fig 5a, the best condition for heavy metal removal using MSA (2M MSA at 100 °C for 4 h) was tried with Ball- Milled Ash as it was expected that a finer particle size of Ball-Milled Ash would enhance metal removal. However, it was observed that the heavy metal removal of the Ball-Milled Ash was not very different from that of raw ash, with Ball- Milled SSA showing higher removal of V (10%), As (12.5%), Cd (4%), Co (2.5%) only. Otherwise, Ball-Milled SSA showed insignificant difference from raw SSA with regard to other types of heavy metal removal. In some cases, the best condition using MSA (2M MSA at 100 °C for 4 h) removed greater amounts of heavy metals such as Ba, Cu, Mn and Zn in raw ash as compared to Ball-Milled Ash. This thus showed that ball milling of the raw ash which is energy-intensive is not necessary for ash detoxification, in order to save the overall process cost. Referring to Fig. 5b, sulphuric acid (SA) which is a non-green but a strong acid which has been used for heavy metal removal due to its high strength as compared against Methane Sulfonic Acid at the best process conditions (100 °C for 4 h), and it was observed that SA exhibited similar' heavy metal removal effect as compared to MSA. This showed that green acids have comparable efficiency as non-green acids and thus their use shall be favored for environmental friendly reasons.
[0071] Referring to Fig. 6, in order to utilize a given amount of acid to the fullest, recycling of the acid (MSA) was experimented, using a fresh batch of raw ash (maintaining the ash / recycled acid mass-volume ratio of 1:10) using 2M MSA (100 °C, 4 h), where it was seen that the used / recycled acid was able to remove some amounts of the heavy metals from the new batch although at a significantly lower amount as compared to its first cycle. The lower amount heavy metal removal of the recycled MSA might be because it was already near the saturation concentration of heavy metal after using the MSA for the first cycle. This is promising for recycling of the spent acid to improve the cost-effectiveness of the whole process. Resuing the acid for the second cycle increased the amount of heavy metal removal per given volume of acid as compared to using it for just one cycle. Thus, recycling used a fixed volume of acid to its maximum potential as to bring down the cost.
[0072] Characterization of raw and leached ash
[0073] Referring to Fig. 7, raw Sewage Sludge Ash had a particle size distribution of from few hundred microns to up to a few mm (< 4.75mm) with the particles of irregular shape. The treated / leached ash had a significantly smaller size distribution but did retain a similar morphology to that of the raw ash. In addition, the washed ash had a cleaner surface as compared to the unwashed ash.
[0074] Particle Size
[0075] Referring to Fig. 8, ASTM C33 is the standard for particle size distribution for fine aggregates. The particle size distribution showed that while the raw ash particles were relatively bigger sized as compared to the ASTM C33 standard limits, they tended to fall out of the range mostly, while the treated ash fitted in more closely within the standard range for fine aggregates and was thus more likely to be adopted for future use in concrete etc.
[0076] Adsorption Isotherm and Porosity
[0077] Referring to Fig. 9, the BET isotherm showed that desorption curve followed the same pattern as the adsorption in the reverse manner, indicating no clogging of pores during the porosity estimation, thus establishing validity of the results.
[0078] Referring to Table 1, raw SSA had a low surface area, while G-SSA (green SSA, leached) showed a surface area which was almost 10 fold higher than that of the raw SSA. This could be due to the removal of heavy metals and dissolution of alkali based compounds [2] that induced pores in the ash. The overall porosity increase of the treated ash was also seen with a greater pore volume and pore diameter. The unwashed ash had a lower porosity as compared to the washed ones because of pore blockage.
[0079] Table 1. Surface Area of raw & treated ash (SSA- Raw' Sew'age Sludge Ash, G- SSA-W: Green Sewage Sludge Ash- washed, G-SSA-UW: Green Sewage Sludge Ash- unw'ashed)
[0080] FT1R of raw & treated ash
[0081] Referring to Fig. 10, the FTIR peaks of Raw SSA displayed peaks at 440 and 600 cm1corresponding to Si-O-Si bending and Si-O-Al stretching vibration given the rich Al (6.55 wt%) and Si (5.24 wt%) content of the ash. The ones near- 1040 cm'1was due to Si-O-Si and Al-O-Si asymmetric stretching and the multiple small peaks below 1000 cm'1were due to the metal-0 vibrations resulting from metal oxides and hydroxides which were mostly present in the ash. FTIR of the treated ash exhibited similar FTIR patterns as the raw ash except for the OH peaks around 3200 cm'1which could be due to moisture.
[0082] XRD of raw & treated ash
[0083] Referring to Fig. 11, raw Sewage Sludge Ash consisted of the phases such as Calcite (CaCOs), Quartz, Whitlockite (Calcium Phosphate), Alumina (AI2O3), Feldspar (aluminium based silicate) and Gypsum (Calcium Sulphate), as can be seen from the characteristic peaks which were observed previously with Sewage Sludge Ash [7]. The XRD of the treated unwashed ash showed peaks similar to that of the raw ash while that of the treated washed ash showed fewer and lower intensity peaks, due to removal and washing away of the metal content and its associated phases (gypsum, calcite).
[0084] Table 2. Peak Position and Phase for XRD patterns shown in Fig. 11
[0085] Thermogravimetric Analysis (TGA ) of raw and treated ash
[0086] Referring to Fig. 12, the thermal stability of the ash was shown where raw ash exhibited no weight loss up to 750 °C. Washed ash showed about 6% weight loss initially due to moisture loss and another 8% from 400 to 750 °C due to loss of organic content. Overall the ash showed good thermal stability in the tested regimen and was suitable to be used as aggregates as part of various applications.
[0087] Elemental contentTable 2 showed that that the treated ash had a much lower heavy metal content, especially for the highly toxic metals such as arsenic, lead, cobalt, vanadium and chromium etc. This loweredheavy metal content would lead to low amounts of leaching that is highly significant for environmental safety when used in applications such as construction materials
[0012] , where there was exposure to moisture. This is discussed in the next section.
[0088] Table 2. Elemental Content of Raw and Treated Ash.
[0089] Leaching
[0090] According to the Singapore Leaching Limits concerning heavy metals, out of the 19 elements tested (with the exception of Mercury), the raw ash failed with respect to 8 elements while the Treated and Washed Ash failed with respect to 4 elements. The importance of washing could be seen in the fact that the treated but unwashed ash leached out significantlyhigher amount of heavy metal than the Treated and Washed Ash and thus failed the SG leaching limits by 8 elements. This was because the residual acid in the green chemicals which removed heavy metals from the ash during the leaching process had not been washed away, unlike the thoroughly washed samples that had no residual green chemicals left.
[0091] Table 3. Heavy Metal Leachate Content of Raw & Treated Ash against SG limits- bolded and underlined means the leachate fails with respect to that clement with regard to the proposed SG limits.
[0092] Industrial Applicability
[0093] The invention converts the raw toxic incineration ash to safe non-toxic ash which can be used as aggregate for construction applications such as in concrete, asphalt etc. The treated ash synthesized through green treatment from raw incinerated ash can also be used for waste water treatment, adsorption of hazardous gas in the environment, or can be used as reinforcing agent for composite materials and pigments in inks.
[0094] It will be apparent that various other modifications and adaptations of the invention will be apparent to the person skilled in the art after reading the foregoing disclosure without departing from the spirit and scope of the invention and it is intended that all such modifications and adaptations come within the scope of the appended claims.References[1] Gemon, M.D. 1999. Environmental benefits of methanesulfonic acid. Comparative properties and advantages. Green chemistry, 1(3), 127-140.[2] Fedje, K. K., C. Ekberg, G. Skarnemark and B.-M. J. J. o. H. M. Steenari (2010). "Removal of hazardous metals from MSW fly ash — an evaluation of ash leaching methods." 173(1-3): 310-317.[3] Tang, J. and B.-M. J. W. m. Steenari (2016). "Leaching optimization of municipal solid waste incineration ash for resource recovery: A case study of Cu, Zn, Pb and Cd." 48: 315-322.[4] Stiemstrom, S., A. Enell, O. Wik, K. Hemstrdm and M. J. W. m. Breitholtz (2014). "Influence of leaching conditions for ecotoxicological classification of ash." 34(2): 421-429.[5] Yahya, A. A., N. Ali, N. L. M. Kamal, S. Shahidan, S. Beddu, M. F. Nuruddin and N. Shafiq (2017). Reducing Heavy Metal Element from Coal Bottom Ash by Using Citric Acid Leaching Treatment. MATEC Web of Conferences, EDP Sciences.[6] Prabhakar AK, Mohan BC, Tay TS, Lee SS-C, Teo SL-M, Wang C-H. Incinerated sewage sludge bottom ash-chemical processing, leaching patterns and toxicity testing. Journal of Hazardous Materials 2021; 402: 123350.[7] Cyr, M., M. Coutand, P. J. C. Clashes and C. Research (2007). "Technological and environmental behavior of Sewage Sludge Ash (SSA) in cement-based materials." 37(8): 1278-1289.L8J Lin, W. Y., W. C. Ng, B. S. E. Wong, S. L.-M. Teo, G. H. Baeg, Y. S. Ok and C.-H. J. J. o. h. m. Wang (2018). "Evaluation of sewage sludge incineration ash as a potential land reclamation material." 357: 63-72.[9] G Kalcikova, B Alic, T Skalar, M Bundschuh, and A Zgajnar Gotvajn (2017) "Wastewater treatment plant effluents as source of cosmetic polyethylene microbeads to freshwater". Chemosphere.188:25-31 .
[0010] V. Vijayalekshmi, Dipak Khastgir (2017) "Eco-friendly methanesulfonic acid and sodium salt of dodecylbenzene sulfonic acid doped cross-linked chitosan based green polymer electrolyte membranes for fuel cell applications" Journal of Membrane Science, Volume 523, 1 February 2017, Pages 45-59.
[0011] S. Patai, Z. Rappoport, The Chemistry of the Functional Groups (Ed.: S. Patai), Wiley, New York, 1991.
[0012] Ciaran J. Lynn, Ravindra K. Dhir, Gunnel S. Ghataora, 2018. Environmental impacts of sewage sludge ash in construction: Leaching assessment. Resources, Conservation and Recycling 136, 306-314.
[0013] Wu, Z., Drcisingcr, D.B., Urch, H., Fassbender, S., 2014. The kinetics of leaching galena concentrates with ferric methanesulfonate solution. Hydrometallurgy 142, 121- 130.
[0014] Palden, T., Onghena, B., Regadio, M., Binnemans, K., 2019. Methanesulfonic acid: a sustainable acidic solvent for recovering metals from the jarosite residue of the zinc industry. Green Chem 21, 5394-5404.
[0015] Zhang, Q., Wen, S., Feng, Q., Nie, W., Wu, D., 2019. Dissolution kinetics of hemimorphite in methane sulfonic acid. Physicochem Probl Mi 55,1-9.
[0016] Ahn, J., Wu, J., Lee, J., 2019. Investigation on chalcopyrite leaching with methanesulfonic acid (MSA) and hydrogen peroxide. Hydrometallurgy 187, 54-62.
[0017] Feng, Q., Wen, S.,Zhao, W., Lv, C., Bai, X., 2015. Leaching of copper from malachite with methane- sulfonic acid. Solvent Extr Res Dev 22, 159-168.
[0018] Rodrigucz Rodrigucz, N., Onghena, B., Binnemans, K., 2019. Recovery of lead and silver from zinc leaching residue using methanesulfonic acid. ACS Sustainable Chemistry Engineering Acs Sustain Chem Eng 7, 19807-19815.
[0019] Gijsemans, L., Forte, F., Onghena, B., Binnemans, K., 2018. Recovery of rare earths from the green lamp phosphor LaPO 4: Ce 3+, Tb 3+(LAP) by dissolution in concentrated methanesulphonic acid. Rsc Adv 8, 26349-26355.
Claims
Claims1. A method of synthesizing leached ash using a mixture of green chemical reagents comprising a main acid leachant and one or more chelating agent, the method comprising the following steps: a. incubating an ash with the mixture of green chemical reagents to dissolve and chelate heavy metal in the ash; and b. washing the ash using a solvent to remove the dissolved and chelated heavy metal.
2. The method of claim 1, wherein the main acid leachant is methane sulfonic acid (MSA).
3. The method of claim 1 or 2, wherein the chelating agent is selected from the group consisting of nitrilotriacetic acid (NTA), ethylenediamine-N,N'-disuccinic acid (EDDS), citric acid (CA) and malonic acid (MA).
4. The method of claim 1, wherein the concentration of the main acid leachant is 0.25-3 M, the concentration of the chelating agent is 0.1-1 M, the incubation in step a is at a temperature of 25 -100 °C, and the incubation duration is 2-24 h.
5. The method of claim 1, wherein the mixture of green chemical reagents comprises a main acid leachant which is methane sulfonic acid (MSA), and two chelating agents which are citric Acid (CA) and malonic Acid (MA).
6. The method of claim 5, wherein the concentration of MSA is 2 M or 3M, the concentration of CA is 0.1 M and the concentration of MA is 0.1 M.
7. The method of claim 6, wherein the astraeid mass-volume ratio is 1:10.
8. The method of claim 7, wherein the ash is incubated with the mixture of green chemical reagents at 100°C for 4 h.
9. The method of claim 1, wherein the ash is a bottom ash or a fly ash.
10. The method of claim 9, wherein the bottom ash is Sewage Sludge Ash (SSA).
11. The method of claim 10, wherein the SSA has a particle size of 100 pm - 4.75 mm.
12. The method of claim 1, wherein the heavy metal is selected from the group consisting of Aluminum (Al), Arsenic (As), Barium (Ba), Cadmium (Cd), Cobalt (Co), Chromium (Cr), Copper (Cu), Iron (Fe), Manganese (Mn), Nickel (Ni), Lead (Pb), Antimony (Sb), Vanadium (V) and Zinc (Zn).
13. The method of any one of claims 1-12, wherein the method further comprising: c. drying the washed ash in oven, at 80-110°C for 18-30 h.
14. The method of claim 13, wherein the washed ash is dried in oven at 105 °C for 24 h.
15. The method of any one of claims 1-14, wherein the method further comprising: d. recycling the mixture of green chemical reagents from step a and re-using it to incubate a next batch of ash for leaching.
16. The method of claim 15, wherein the recycled mixture of green chemical reagents is incubated with the next batch of ash at an ash:acid mass- volume ratio of 1: 10.
17. The method of any one of claims 1-16, wherein the leached ash retains elements selected from the group consisting of Calcium (Ca), Silicon (Si), Aluminium (Al) and Iron (Fe).
18. The method of any one of claims 1-17, wherein the leached ash exhibits no weight loss up to 750 °C.
19. The method of any one of claims 1-18, wherein the leached ash is for constituting up to5% cement substitution and up to 30% aggregate substitution to make mortars.
20. The method of claim 1, wherein the solvent is water.
Citation Information
Patent Citations
Extraction of metals from heavy metal-bearing wastes
WO1998024938A1
A method of treating an ash composition
WO2022191778A1
Cited By
Selective leaching method for copper in waste circuit board
CN120400548A