Hydrogen production from seawater
The saltwater electrolysis apparatus with a metallic layered double hydroxide anode coating absorbs chloride ions to enhance oxygen evolution reaction activity and stability, overcoming corrosion issues and achieving efficient, scalable hydrogen production from seawater with reduced energy costs.
Patent Information
- Application Number
- PCT/AU2024/050578
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-06-01
- Filing Date
- 2024-05-31
- Publication Date
- 2024-12-05
AI Technical Summary
Current seawater electrolysis technologies face challenges due to the corrosive nature of chloride ions, which hinder the oxygen evolution reaction and lead to corrosion issues, limiting the scalability and efficiency of hydrogen production from seawater.
A saltwater electrolysis apparatus with a metallic layered double hydroxide based electrocatalyst layer coating on the anode, allowing chloride ion absorption to enhance oxygen evolution reaction activity and stability, eliminating the need for passivation layers and enabling direct alkaline seawater electrolysis.
The apparatus achieves high-performance, ClER-free alkaline seawater electrolysis with improved durability and reduced electricity consumption, demonstrating a nearly 100% relative Faradaic efficiency and 12.8% lower electricity costs compared to purified water-based systems.
Smart Images

Figure AU2024050578_05122024_PF_FP_ABST
Abstract
Description
HYDROGEN PRODUCTION FROM SEAWATERPRIORITY DOCUMENT
[0001] The present application claims priority from Australian Provisional Patent Application No. 2023901739 titled “HYDROGEN PRODUCTION FROM SEAWATER” and filed on 1 June 2023, the content of which is hereby incorporated by reference in its entirety.TECHNICAL FIELD
[0002] The present disclosure relates generally to electrolysis and, more specifically, to electrolysis of water.BACKGROUND
[0003] Hydrogen has been identified as the most important energy source in a quest to realise global zero emissions by 2050. Hydrogen production by electrolysis of water has attracted intensive interest as a way to produce pure hydrogen.1Currently, most types of water electrolysers, either mature alkaline electrolyser (AE) or emerging proton exchange membrane (PEM)-based, require the supply of highly purified water (e.g. deionized water) as feedstock.2As a result, large-scale water splitting in the future may affect the availability of freshwater resources and cause water stress.3A route to alleviate water stress caused by increased water usage for electrolysis would be to use (almost) infinite seawater as the water feedstock or solvent. However, the application of seawater in electrolysis is hindered by its complex composition, which includes major components such as chloride ions (Cl , -0.55 M), sodium ions (Na+, 0.48 M), magnesium ions (Mg2+, 0.05 M), calcium ions (Ca2+, 0.01 M), etc.4For example, on the anode of a sea water electrolyser, the chlorine evolution reaction (C1ER) competes with the oxygen evolution reaction (OER) due to their similar thermodynamic equilibrium potentials and a faster reaction rate for the C1ER.5,6The end result is that perchlorate ions (CIO ) are produced as the oxidation product of C1ER, and this leads to severe corrosion problems on the whole electrolyser.7
[0004] Currently, there are two ways to achieve seawater splitting: indirect seawater splitting and direct seawater splitting.8For indirect water splitting, seawater is first desalinated by reverse osmosis (RO) technology before being used in a commercial electrolyser. This approach solves the problems of C1ER and corrosion. However, the capacity of seawater desalination will not meet the demand for hydrogen production by water electrolysis.9 10For example, to achieve a water electrolyser capacity of 1400 GW in 2050, the purified water consumption will need to be -2550 Mt / year. The current reverse osmosis (RO) desalination capacity is only 540 Mt / year. Therefore, to balance the supply of RO-treatedseawater between living requirements and hydrogen production, there is a need to develop a direct seawater electrolysis technology without RO treatment.11 12
[0005] Industrial-scale direct seawater electrolysis remains challenging due to the presence of corrosive chloride ions (Cl ). Polymer electrolyte membrane (PEM) based water electrolysers show extremely high sensitivity to Cl because of the intrinsic properties of the noble metal catalysts used.13 14Anion exchange membrane (AEM) based water electrolysers have preliminarily demonstrated the feasibility of seawater as a feedstock but their performance is hindered by the limited mass transfer across the membrane caused by Cl blocking.15 16
[0006] Thus, a highly selective and durable oxygen evolution reaction (OER) electrocatalyst is currently a bottleneck for direct seawater splitting to produce hydrogen on a large scale.
[0007] Most approaches to date to using OER catalysts for seawater splitting focus on the repulsion of chloride ions (Cl ) from the catalyst surface to reduce the corrosion and side reaction issues.19,20This includes the construction of protective layers that stop the penetration of Cl or the design of an anion-rich surface for a catalyst that repels the Cl via electrostatic force.21,22However, these rejection strategies are faced with the issue of unsatisfactory durability because the modified layer is usually not stable enough under harsh operating conditions.
[0008] There is a need to provide systems, apparatus and processes for direct and high-performance alkaline natural seawater electrolysis at an industrial scale. Alternatively, or in addition, there is a need to provide systems, apparatus and processes for alkaline seawater electrolysis that provide a useful alternative to existing systems, apparatus and processes.SUMMARY
[0009] According to a first aspect, there is provided a saltwater electrolysis apparatus, the apparatus comprising an anode for generating oxygen from water containing chloride ions, the anode comprising an anode substrate and a metallic layered double hydroxide based electrocatalyst layer coating wherein the anode is configured so that, in use, absorption of chloride ions from alkaline saltwater to the electrocatalyst layer coating contributes to the OER activity and stability performance of the anode to provide direct and ClER-free alkaline saltwater electrolysis.
[0010] Notably, the anode of the saltwater electrolysis apparatus of the first aspect does not comprise a passivation layer. That is, in contrast to prior art systems which are designed or configured to reduce chloride ion adsorption at the electrode, the present apparatus is configured to allow chloride ion adsorption.
[0011] The apparatus of the first aspect can also be used to produce hydrogen directly from saltwater, the apparatus comprising: a cathode for generating hydrogen from water containing chloride ions, the cathode comprising a cathode substrate and a metal based electrocatalyst layer coating; and an anode comprising an anode substrate and a metallic layered double hydroxide based electrocatalyst layer coating wherein the anode is configured so that, in use, absorption of chloride ions from alkaline saltwater to the electrocatalyst layer coating contributes to the OER activity and stability performance of the anode to provide direct and ClER-free alkaline saltwater electrolysis.
[0012] According to a second aspect, there is provided a method of operating the saltwater electrolysis apparatus of the first aspect, comprising generating oxygen and hydrogen from saltwater.
[0013] In certain embodiments of the first and second aspects, the metallic layered double hydroxide is a mixed metal layered double hydroxide. In certain of these embodiments, the mixed metal layered double hydroxide is a nickel-based bimetallic layered double hydroxide. In certain of these embodiments, the nickel-based bimetallic layered double hydroxide is selected from one or more of the group consisting of nickel-iron layered double hydroxide, nickel-cobalt layered double hydroxide, nickel-aluminum layered double hydroxide, nickel-zinc layered double hydroxide, nickel-copper layered double hydroxide, nickel-manganese layered double hydroxide, nickel-iridium layered double hydroxide, and nickelruthenium layered double hydroxide.BRIEF DESCRIPTION OF THE FIGURES
[0014] Embodiments of the present disclosure will be discussed with reference to the accompanying figures wherein:
[0015] Figure 1 shows electrochemical activity evaluation in pure water and seawater in a three- electrode configuration, (a) shows LSV curves and (b) shows CV curves of NiFe LDH. (c) shows LSV curves and (d) shows CV curves of Ni(0H)2.
[0016] Figure 2 shows an XRD pattern of as-prepared NiFe LDH.
[0017] Figure 3 shows (a) HAADF images of as-prepared NiFe LDH. (b) Enlarged HAADF images of NiFe LDH. (c), (d), (e) The corresponding Energy-dispersive X-ray spectroscopy (EDS) elemental mapping of (c) Ni, (d) Fe and (e) O.
[0018] Figure 4 shows (a) digital photos of seawater taken from Henley Beach (Adelaide, South Australia, Australia) with 1 M KOH. (b) XRD pattern of white precipitation.
[0019] Figure 5 shows (a) LSV curves and (b) CV curves of NiFe LDH in 1 M KOH + 0.5 M NaCl.
[0020] Figure 6 shows the overpotential required to achieve 100 mA cm2for (a) NiFe LDH and (b)Ni(0H)2.
[0021] Figure 7 shows (a) LSV curves and (b) CV curves of Ni(0H)2in 1 M KOH + 0.5 M NaCl.
[0022] Figure 8 shows CV curves of NiCo LDH pure water and seawater.
[0023] Figure 9 shows in situ Raman spectra. NiFe LDH measured in (a) pure water and (b) seawater.
[0024] Figure 10 shows in situ Raman spectra. Ni(OH)2measured in (a) pure water and (b) seawater.
[0025] Figure 11 shows an in situ Raman contour map. (a), (b) NiFe LDH measured in a pure water and b seawater, (c), (d) Ni(OH)2measured in c pure water and d seawater. Applied potentials range from 1.3 V to 1.6 V with an interval of 25 mV.
[0026] Figure 12 shows the results of in situ XAS measurements, (a) Shifts in the Fe and Ni K-edge position and corresponding OER currents extracted from in situ XANES spectra, (b), (c) The k3-weighted Fourier-transformed EXAFS R-space patterns for (b) Fe and (c) Ni in seawater.
[0027] Figure 13 shows in situ XAS measurements. In situ XANES spectra of Fe K-edge of NiFe LDH in (a) pure water and (b) seawater.
[0028] Figure 14 shows in situ XAS measurements. In situ XANES spectra of Ni K-edge of NiFe LDH in (a) pure water and (b) seawater.
[0029] Figure 15 shows in situ XAS measurements. The k3-weighted Fourier-transformed EXAFS R- space patterns for (a) Fe and (b) Ni in pure water.
[0030] Figure 16 shows OER durability measurements, (a) OER stability test at a constant current density of 200 mA cm2for NiFe LDH in two electrolytes, (b) Potential differences at the start and the end of the stability test, (c) Amount of dissolved Ni and Fe ions after stability test determined by ICP-MS.(d) Ni 2p XPS spectra for NiFe LDH before and after stability test, (e) Peak area ratio of Ni3+ / Ni2+obtained from XPS results.
[0031] Figure 17 shows atomic ratio of Ni: Fe for different samples after stability test.
[0032] Figure 18 shows (a) High-resolution HAADF images of NiFe LDH after stability test in seawater, (b) The TEM image and corresponding Energy-dispersive X-ray spectroscopy (EDS) elemental mapping of (c) Ni, (d) Fe and (e) O.
[0033] Figure 19 shows the DEMS signals of16Oz (m / z 32),16O18O (m / z 34),18C>2 (m / z 36) for18O labelled NiFe LDH in (a) pure water and (b) seawater. Corresponding CV curves in (c) pure water and (d) seawater.
[0034] Figure 20 shows OER mechanism investigation, (a), (b) MSCVs signals of16O18O content from DEMS test on18O labelled NiFe LDH in (a) pure water and (b) seawater, (c), (d) In situ ATR-IR spectra of NiFe LDH in (c) pure water and (d) seawater, (e) Coverage of *OOH as a function of applied potentials, (f) Schematic illustration for structure evolution and OER mechanism transfer in pure water and seawater.
[0035] Figure 21 shows mass spectrometric cyclic voltammograms signals of18O2 content from DEMS test on18O labelled NiFe LDH in (a) pure water and (b) seawater.
[0036] Figure 22 shows (a, b) pH dependence of NiFe LDH (a) in pure water and (b) in seawater, (c) Current densities of NiFe LDH at 1.5V at different pH values.
[0037] Figure 23 shows an evaluation of overall water splitting performance on two-electrode configuration and scale-up test on a commercial AE. Overall water splitting performance on two- electrode configuration for (a) activity, (b) durability and (c) corresponding RFE and dissolution of Fe during durability test, (d) Optical image of the commercial AE. (e) Enlarged view of the electrolyser and schematic illustration of an electrolyser cell, (f) Polarization curves of AE using pure water and seawater at 80 °C. (g) A comparison of electricity expense for AE calculated from polarization curves, (h) Durability test for the commercial AE at a constant current density of 200 mA cm2.
[0038] Figure 24 shows the amount of O2 generated by seawater and pure water splitting determined by GC.DESCRIPTION OF EMBODIMENTS
[0039] Details of terms used herein are given below for the purpose of guiding those of ordinary skill in the art in the practice of the present disclosure. The terminology in this disclosure is understood to be useful for the purpose of providing a better description of particular embodiments and should not be considered limiting.
[0040] The following abbreviations are used in this disclosure and have the following meanings:AE: alkaline electrolyserAEM: Anion exchange membraneC1ER: chlorine evolution reactionC V : cyclic voltammogramNiFe LDH: nickel-iron layered double hydroxideOER: oxygen evolution reactionPEM: proton exchange membranePTFE: polytetrafluoroethyleneRFE: relative Faradaic efficiencyRHE: reversible hydrogen electrodeRO: reverse osmosisXPS: X-ray photoelectron spectroscopyXRD: X-Ray Powder DiffractionXAS: X-ray absorption spectroscopyHAADF: High-angle annular dark-fieldDEMS: Differential Electrochemical Mass SpectroscopyEDS: Energy-dispersive X-ray spectroscopy
[0041] Unless otherwise explained, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this disclosure belongs.
[0042] In the context of the present disclosure, the terms “about” and “approximately” are used in combination with an amount, number, or value, then that combination describes the recited amount, number, or value alone as well as the amount, number, or value plus or minus 20 % of that amount,number, or value. By way of example, the phrases “about 40 %” and “approximately 40 %” disclose both “40 %” and “from 32 % to 48 %, inclusive”.
[0043] The singular terms “a”, “an”, and “the” include plural referents unless context clearly indicates otherwise. The term “comprises” means “includes”. Therefore, comprising “A” or “B” refers to including A, including B, or including both A and B.
[0044] Although methods and materials similar or equivalent to those described herein can be used in the practice or testing of the present disclosure, suitable methods and materials are described herein. In case of conflict, the present specification, including explanations of terms, will control. In addition, the materials, methods, and examples are illustrative only and not intended to be limiting.
[0045] To develop a suitable catalyst for seawater splitting, the role of Cl needed to be clarified. Research on the role of Cl has previously been conducted using simulated seawater but it is still challenging to determine how the Cl interacts with the active sites of the catalysts precisely.23In addition to Cl -related issues, the durability of high-activity catalysts themselves, e.g. layer double hydroxide (LDH) catalysts, is also a challenge when running in a high-concentration alkaline electrolyte. This is because the high activity is usually contributed by high metal valence states, which can cause metal leaching and performance degradation under a high voltage operation.24
[0046] The present disclosure is predicated on the inventors surprising discovery that the absorption of Cl on the specific site of a nickel-iron layered double hydroxide (NiFe LDH) OER electrocatalyst has no significant negative impact, but rather is beneficial for the activity and stability enhancement in an alkaline electrolyser running with natural seawater. In situ spectroscopic investigations reveal a unique interaction between NiFe LDH active sites and Cl absorbents during the OER process. On one hand, more OER-active Ni sites with high chemical valence are created in seawater, thus increasing the activity. On the other hand, both Fe leaching and active lattice oxygen are suppressed by the adsorption of Cl on desired Fe sites, which improves the long-term stability of the catalyst. This approach achieves direct and efficient alkaline seawater electrolysis for the very first time on a commercial-scale electrolyser (120 cm2electrode area) with a nearly 100 % relative Faradaic efficiency (RFE). Accordingly, it reduces electricity consumption by 12.8 % and 20.7 % compared to the purified water-based alkaline electrolysis using NiFe LDH and commercial Ni catalyst, respectively.
[0047] Such outstanding performance is achieved by a Cl -promoted OER mechanism on a metallic double layer hydroxide catalyst, such as nickel-iron layered double hydroxide (NiFe-LDH). Although Cl is commonly perceived as detrimental to OER catalysts, the present inventors have demonstrated that the absorption of Cl on NiFe LDH catalyst has no significant negative impact, but rather is beneficial for the activity and stability enhancement in a commercial AE running with natural seawater.
[0048] The present disclosure provides an industrial-level direct alkaline seawater electrolysis pathway for hydrogen production.
[0049] The present inventors have achieved direct and stable seawater electrolysis on a commercial AE by utilizing the absorption of natural Cl from seawater feedstock. Different from the well-known view that Cl is harmful to the catalyst, the present inventors have surprisingly found that Cl is advantageous to the OER activity and stability of NiFe LDH. In situ spectroscopic experiments demonstrate that Cl adsorption on Fe sites can increase the Ni valence, as well as lower the Fe valence and stabilize the lattice oxygen during OER process. The former function results in high OER activity (254 mV overpotential for 100 mA cm2current density) and the latter enables NiFe LDH’s great stability in seawater. Owing to their beneficial interactions, the commercial-scale AE electrolyser, taking NiFe LDH as anode, decreases the electricity consumption from 5.41 kWh Nm3in pure water to 4.72 kWh Nm3in seawater. Aside from the increased energy efficiency, this seawater-based AE achieves excellent durability performance for over 100 hours at the current density of 200 mA cm2.
[0050] The work described herein demonstrates, for the first time, an alkaline natural seawater-based AE with NiFe LDH anode was operated stably at the relatively low energy consumption of 4.72 kWh Nm3H2 by taking advantage of interactions between Cl and anode material. As a comparison, this value is 5.41 for alkaline pure water electrolysis with the same anode and 5.95 for commercial Ni anode alkaline water electrolysis.
[0051] Disclosed herein is a saltwater electrolysis apparatus. The apparatus comprises an anode for generating oxygen from water containing chloride ions. The anode comprises an anode substrate and a metallic layered double hydroxide based electrocatalyst layer coating. The anode is configured so that, in use, absorption of chloride ions from alkaline saltwater to the electrocatalyst layer coating contributes to the OER activity and stability performance of the anode to provide direct and ClER-free alkaline saltwater electrolysis. The anode does not comprise a passivation layer.
[0052] The substrate may be formed from any suitable conductive material which may, for example, be a conductive metal such as nickel. The substrate may be a metallic foam, foil or mesh.
[0053] The electrocatalyst layer coating is a metallic layered double hydroxide such as a mixed metal layered double hydroxide. Without limitation, nickel-based bimetallic layered double hydroxides are particularly suitable. In exemplary embodiments disclosed herein, nickel-iron layered double hydroxide is used. However, it will be appreciated that other metal-layered double hydroxides or mixed metal-layered double hydroxides could also be used, such as nickel-cobalt layered double hydroxide, nickel-aluminum layered double hydroxide, nickel-zinc layered double hydroxide, nickel-copper layered double hydroxide,nickel-manganese layered double hydroxide, nickel-iridium layered double hydroxide, and nickelruthenium layered double hydroxide.
[0054] The saltwater electrolysis apparatus further comprises a cathode. Any suitable material can be used for the cathode. In exemplary embodiments disclosed herein, the cathode comprises nickel sulfide (NiSx). Accordingly, the apparatus can also be used to produce hydrogen directly from saltwater.
[0055] The saltwater electrolysis apparatus may also comprise apparatus for removing hydrogen and oxygen generated. The apparatus may be suitable for gas-liquid separation.
[0056] Also disclosed herein is a method of operating the saltwater electrolysis apparatus described herein, comprising generating oxygen and hydrogen from saltwater.
[0057] The apparatus and method may be used to generate hydrogen and oxygen from any suitable saline water, such as seawater. Prior to electrolysis, the saltwater is treated with a base to provide alkaline saltwater. Any suitable base can be used, such as potassium hydroxide. The alkaline seawater can have any pH>7, such as pH 7.5, pH 8.0, pH 8.5, pH 9.0, pH 9.5, pH 10.0, pH 10.5, pH 11.0, pH 11.5, pH 12.0, pH 12.5, pH 13.0, pH 13.5, pH 14.0. Preferably, the pH is >13.
[0058] In contrast to currently adopted Cl -blocking strategies used to avoid adsorption of Cl on the catalyst for seawater electrolysis, we deliberately utilized the specific adsorption behaviour of Cl on the catalyst surface, thus achieving overall improvement in the activity and stability of the catalyst.
[0059] Based on in situ spectroscopic measurements (Raman, XAS, ATR-IR, DEMS), the present inventors have demonstrated a Cl -boosted OER process in alkaline seawater. On one hand, more OER- active Ni sites with high chemical valence are created in seawater, thus increasing the activity. On the other hand, both Fe leaching and active lattice oxygen are suppressed by the adsorption of Cl on Fe sites, which improves the long-term stability of the catalyst.
[0060] The present inventors have developed a comprehensive understanding of the role of Cl with a new and effective method to achieve high-performance seawater splitting, while demonstrating its practical application in a scale-up system.EXAMPLES
[0061] Methods
[0062] Material Synthesis
[0063] For NiFe LDH, a piece of Ni foam (NF, 2 cm x 3 cm) was ultrasonicated with 1 M HC1 solution, ethanol and DI water, respectively. Every step lasted for 30 minutes to remove the oxides and organic species on the surface. Then, Ni(NO3)2-6H2O (0.99 mmol), Fe(NC>3)3-9H2O (0.33 mmol), NH4F (5 mmol), and urea (5 mmol) were dissolved in 20 mL DI water under ultrasonic treatment for 30 minutes. Afterward, the resultant solution was transferred to a 30 mL Teflon autoclave for a 12 hours hydrothermal reaction at 120 °C. After the hydrothermal reaction was completed, the NF was taken out and washed with DI water and ethanol. Finally, the NiFe LDH grown on NF was rested to be dried at room temperature. The synthesis of Ni (OH)2 was the same as that of NiFe LDH but Fe(NC>3)3-9H2O was not added. For the synthesis of NiCo LDH the method was the same as that of NiFe LDH except that the Fe(NC>3)3-9H2O was replaced with Co(NC>3)2-6H2O. NiSx was synthesized by a reported electrodeposition method.35Typically, 10 mM NiSCL, 0.5 M thiourea and Na2S20s were dissolved in 100 mL DI water as electrolyte. The pH was optimized to 4 by 1 M H2SO4. The polished Ni mesh was employed as working electrode, and the Ag / AgCl, Pt wire were used as reference and counter electrodes, respectively. The electrodeposition was conducted by a cathodic current density of 20 mA cm-2for 1800 seconds.
[0064] Electrochemical Measurements
[0065] The as-prepared catalyst grown on Ni foam was directly used as a working electrode with a fixed geometric area of 1 cm2. The Pt plate was used as the counter electrode and Hg / HgO (0.098V vs. RHE) was used as the reference electrode. All measured potentials were calibrated to the reversible hydrogen electrode (RHE) according to the equation of ERHE = EHg / HgO +0.098 V+ 0.059*pH, if not otherwise specified. The electrochemical data on three-electrode setup were corrected with 90 % iR loss unless otherwise stated. The catalysts were electrochemically activated by cyclic voltammogram (CV) for 20 cycles at a scan rate of 50 mV s1and then measured at a scan rate of 10 mV s1in an CL-satu rated electrolyte. For overall water splitting performance evaluation, the NiFe LDH and NiSxwere used as cathode and anode electrode, respectively. The H-cell is separated by Nafion 117 membrane. Their polarization curves on two-electrode setup were corrected with 75 % iR loss. The relative Faradaic efficiency was determined by the ratio of the amount of O2 generated in a seawater-electrolyte to that generated in a pure water-electrolyte. The amount of O2 after 15 minutes of electrolysis was measured by gas chromatography (GC, Agilent 8890). For the preparation of alkali-treated natural seawater, theseawater was first added with 1 M KOH and the resulting precipitations (Ca(0H)2, Mg(0H)2) were removed by centrifugation at 6000 rpm for 1 minute. Another electrolyte is prepared by dissolving 1 M KOH in DI water.
[0066] Characterisation
[0067] X-Ray Powder Diffraction (XRD) data was obtained by a Rigaku MiniFlex 600 X-Ray Diffractometer. The aberration-corrected transmission electron microscope images, high-angle annular dark-field imaging, and EDS and EELS mapping, were taken on an FEI Titan Themis 80-200 operating at 200 kV. X-ray photoelectron spectroscopy (XPS) analyses were carried out under ultra-high vacuum on a Kratos Axis Ultra with a Delay Line Detector photoelectron spectrometer using an aluminum monochromatic X-ray source.
[0068] In situ Raman Measurements
[0069] In situ Raman spectroscopy was operated on a confocal Raman microscope (Horiba LabRAM HR Evolution) with a 60X (1.0 N.A) water-immersion objective (Olympus). The laser wavelength used was 532 nm. A screen-printed electrode (Pine, RRPE1002C) was used as the electrode for potentiostatic tests on a CHI 760E electrochemical workstation. The Ag / AgCl electrode was used as the reference electrode and the Pt was used as the counter electrode.
[0070] In situ XAS measurements
[0071] The Ni / Fe K-edge XAS spectra were collected at the beamline of 1W1B beamline in Beijing Synchrotron Radiation Facility (BSRF). Double-crystal Si (111) was used as a monochromator and the energy was calibrated using Ni and Fe foils. The XAS spectra were obtained by standard ion chambers. The in situ XAS was performed in a homemade electrochemical cell connected to an electrochemical workstation. Catalyst-loaded carbon paper was used as the working electrode, with an Ag / AgCl electrode as the reference electrode and Pt wire as the counter electrode. The electrochemical cell was filled with Ch-saturated electrolytes.
[0072] In situ Attenuated Total Reflectance Infrared (ATR-IR ) Spectroscopy
[0073] The ATR-IR measurements were performed on Thermo-Fisher Nicolet iS20 equipped with a liquid nitrogen-cooled HgCdTe (MCT) detector using a VeeMax III ATR accessory (Pike Technologies). A silicon prism with gold through magnetron sputtering was employed as a working electrode. Ag / AgCl electrode and a platinum wire were used as reference electrode and counter electrode, respectively. ATR- IR data were obtained by 64 scans at 4 cm1spectral resolution. Electrocatalyst ink was prepared bydispersing 3 mg catalyst and 20 pl 5 wt% Nafion solution in 2 mL isopropanol, followed by 60 minutes ultrasonication. 20 pl ink was dropped on the silicon prism as working electrode. The 0.1 M KOH dissolved in pure water and seawater were taken as electrolytes for the ATR-IR test. Please note that the lower alkalinity was taken to avoid the interference caused by the oxidation of silicon in a strongly alkaline environment.
[0074] In situ DEMS measurements
[0075] DEMS measurements were conducted on DEMS (The Hidden HPR-40 DEMS). A polytetrafluoroethylene (PTFE) film with gold through magnetron sputtering was employed as a working electrode. NiFe LDH catalyst was coated on the working electrode. Ag / AgCl electrode and a platinum wire were used as reference electrode and counter electrode, respectively. The electrolyte was driven by a self-propelled syringe at a flow rate of 100 pl min1. The NiFe LDH catalysts were labelled with18O through CV for 100 cycles at a scan rate of 10 mV s-1. This labelling process enabled the exchange between16O from the catalyst lattice and18O from the electrolyte. After the labelling process, the cell and all of the electrodes were washed with H216O to remove the residual18O. After washing with H216O, CV measurements were carried out at 10 mV s-1 in 1 M KOH dissolved in pure water (H216O) or 1 M KOH dissolved in seawater (H216O). The gas products were determined by mass spectroscopy in real-time when the CV was conducted.
[0076] Commercial AE tests
[0077] The scale-up measurements were conducted on a commercial alkaline electrolyser (MDQ-30L- 1, Cockerill Jingli Hydrogen Technology Co., LTD.) with 6 cells. 20 L of the 30 wt% KOH @ pure water or 30 wt% KOH @ natural seawater (Bohai Sea, China) was used as an electrolyte with a flow rate of 65 L h '. The precipitations were removed by filtration. The NiFe LDH and NiSxon Ni mesh with a total geometric surface area of 120 cm2were employed as the anode electrode and cathode electrode, respectively. The performance was measured during the day and suspended at night to at a temperature of 80 °C ± 0.5 °C. The data on AE were presented without iR compensations.
[0078] Calculation of electricity expense for H2 production
[0079] The total electricity consumption for H2 production was calculated according to the equation:W = I x f U dt where W is the total electricity consumption. I is current and U is potential.
[0080] The amount of H2 generated is calculated according to the equation:V = 22.4 x I x t / (Z x F) where V is the volume of H2 produced. The value of Z (electron transfer number for Hydrogen evolution reaction) is 2, and F, the Faraday constant, is 96,485 C mol-1.
[0081] The electricity consumption is Q = W / V (kWh Nm3).
[0082] Results and discussion
[0083] OER activity comparison in three-electrode configuration
[0084] Figure 1 shows the linear sweep voltammetry (LSV) and cyclic voltammetry (CV) curves of NiFe LDH (Figures 2 and 3) and another typical OER catalyst Ni(OH)2 running in two different electrolytes. They are 1 M KOH dissolved in deionised (DI) water (denoted as pure water) and natural seawater (collected from Henley Beach, SA, Australia). The natural seawater was pre-treated with KOH as described herein (Figure 4). As shown in Figure la, the NiFe LDH tested in seawater performs better in terms of OER activity than in pure water. This increase can be rationalized by the formation of more high valence Ni species in seawater (Figure lb). A similar phenomenon was observed in simulated seawater (I M KOH + 0.5 M NaCl, Figures 5 and 6). However, for Ni(OH)2 without a Fe promoter, Cl involvement results in an opposite activation effect. The LSV curves show that Ni(OH)2 possesses worse OER activity in seawater than in pure water because the formation of high valence Ni is inhibited in the former (Figure 1c, d, Figure 7). In addition, the analogous NiCo LDH also delivers better OER performance with more high-valence Ni / Co species in seawater (Figure 8).
[0085] Structure evolution with Cl interaction
[0086] In situ Raman spectroscopy was conducted to determine the origin of activity enhancement for NiFe LDH in seawater (Figures 9, 10 and 11). Under 1.35 V, the NiFe LDH catalysts immersed in two electrolytes share the same weak peaks at 461 cm1and strong peaks at 535 cm1, which are assigned to the bending mode and Alg stretching modes of Ni(OH)2.25For NiFe LDH measured in pure water, as the anodic potential rises to 1.4 V, new peaks at 477 cm1and 556 cm1replace the initial two peaks (Figure I la). The pair of those new peaks can be assigned to NiOOH, indicating the phase transition from a - NiFe LDH to y -NiFeOOH, which is accompanied by the valence increase from Ni2+to Ni3+ / 4+. In comparison, early appearance of a / y transition was observed in seawater (e.g., 1.35 V, Figure 11b), agreeing well with the results obtained from CV tests that the addition of Cl facilitates the enhancement of Ni valence. As for Ni(OH)2, the characteristic peaks of y -NiOOH cannot be observed until voltagesreach 1.425 V whether in pure water or seawater (Figure l ie and lid). The different a / y transition behaviours of NiFe LDH and Ni(0H)2 strongly indicate both Fe and Cl- are necessary to facilitate the formation of the active y -phase during the OER process.
[0087] Atomic evolution with Cl interaction
[0088] To track the differences in the atomic evolution of catalyst in pure water and seawater under OER conditions, in situ X-ray absorption spectroscopy (XAS) was conducted. Ni and Fe’s valence evolutions as a function of applied potentials are illustrated by summarizing the X-ray absorption near edge structure (XANES) energy shifts with three reaction stages (Figures 12a, 13 and 14). From open circuit potential to 1.1 V (initial stage), the Fe and Ni K-edge shifts in the two electrolytes share a similar trend. Then, the Fe K-edge shifts remain nearly unchanged between 1.1 V and 1.45 V (pre-catalytic stage), while the Ni K-edge shift moves to a more positive value in seawater than in pure water. However, when the potential reaches 1.6 V (OER stage), the Fe K-edge shift measured in seawater abnormally moves backward (decreasing to 0.68 eV), while the Fe K-edge shift keeps rising in pure water as expected. Contrary to Fe, the Ni K-edge shift reaches the maximum value in seawater at 1.6 V, higher than that measured in pure water. This further indicates the Cl stabilizes the valence state of Fe and raises the valence state of Ni.
[0089] In k3-weighted Fourier transform extended X-ray absorption fine structure (FT-EXAFS) spectra (Figure 12b), a clear Fe-Cl peak can be observed in seawater after the potential reaches 1.45 V, which indicates the adsorption of Cl species on the Fe site. However, no significant peak of Ni-Cl can be observed at any applied potentials (Figures 12c and 15). This specific adsorption of Cl on the Fe site, not Ni, is responsible for the opposite valence evolution trends for them revealed by XANES, which can be explained by the classic Pearson’s hard-soft acid-base (HSAB) principle. It has been demonstrated that the Ni valence will increase to Ni4+for NiFe LDH under OER conditions, which is a harder Lewis acid than Fe3+site.26,27According to HSAB principle, harder acid tends to bind with harder base. Accordingly, Ni4+prefers to bind with OH and Fe3+prefers to bind with Cl because the OH is a harder base than Cl . In turn, the unique absorption of Cl on Fe3+stabilizes the oxidation state of Fe beyond the attack of OH . Considering that Fe with high valence unavoidably leads to its dissolution for NiFe LDH operated in pure water,28a low oxidation state of Fe in seawater probably is beneficial for its OER stability.
[0090] OER stability comparison in pure water and seawater
[0091] As widely recognized, Fe leaching is a major reason for the poor durability of NiFe LDH.29The OER stabilities of the NiFe LDH catalysts in two electrolytes were evaluated and compared using chronopotentiometry (Figure 16a). After 100 hours running, the NiFe LDH catalyst measured in seawater affords unexpectedly better OER stability with a 53 mV potential increase than that in pure water (300mV, Figure 16b), verifying the positive effect of Cl on OER stability. The amount of dissolved metal ions in different electrolytes was then detected by inductively coupled plasma mass spectrometry (ICP- MS).30As compared in Figure 16c, the minimum amount of dissolved Ni (70.3 ng mL ') and Fe ions (34.1 ng mF ') are found in seawater, which is lower than that tested in pure water. Besides, the ratio of Ni: Fe remains similar after the stability test in seawater, but this value increases from 2.82 to 3.25 in pure water, indicating a severe dissolution of Fe in the latter (Figure 17). Consequently, from the X-ray photoelectron microscopy (XPS) spectra of Ni 2p (Figure 16d, e), the less leaching of Fe enabled more Ni3+to remain after the test (accounting for 28 %), which ensured superior durability performance in seawater. The high-angle annular dark-field scanning transmission electron microscopy (HAADF-STEM) image and energy dispersion spectrum (EDS) mapping also show the defect-free lattice and even distribution of Fe in NiFe LDH after running in seawater (Figure 18). Taking structural evolution and ICP-MS results together, we can confirm that the adsorption of Cl keeps the Fe in a low valence, inhibiting the leaching of Fe, thus achieving stable long-term OER durability.
[0092] OER mechanism investigation
[0093] To bridge the remarkable OER performance and unique function of Cl on NiFe LDH, the OER mechanism in alkaline seawater was studied. In a pure water-based alkaline electrolyte, it has been widely known that NiFe LDH’s lattice oxygen directly takes part in the formation of O2, which is known as the so-called lattice oxygen mechanism (LOM).31Accordingly,18O isotope-labelling experiments were conducted using in situ differential electrochemical mass spectrometry (DEMS) to quantify the activity of lattice oxygen. The NiFe LDH catalyst was firstly labelled with18O isotopes via CV activation in H218O- based 1 M KOH electrolyte. Subsequently, the18O labelled catalysts were washed with H216O three times to remove the surface absorbed H218O. After washing, the DEMS collected the real-time signals of m / z= 32 (16O2), m / z=34 (16O18O), and m / z= 36 (18O2) during the CV measurements (Figure 19). Then the DEMS signals and CV curves are integrated to the mass spectrometric cyclic voltammograms (MSCVs). The MSCVs signals of16O18O and18O2 are normalized by the content of16O2, with the ordinate representing their ratio. As shown in Figure 20a, b and Figure 21,18O labelled NiFe LDH delivers more than three times as high content of16O18O and18O2 in pure water as that measured in seawater, indicating that the participation of lattice oxygen is suppressed in the latter. In addition, the less activity dependence on pH in seawater than in pure water also demonstrates that the activity of lattice oxygen is reduced by Cl adsorption (Figure 22). Such less active lattice oxygen can also explain the excellent durability of NiFe LDH in seawater because the active lattice oxygen usually leads to the instability of crystal structure.32,33
[0094] It should be noted that stabilized lattice oxygen cannot explain the enhanced OER activity in seawater as the LOM is inhibited. Besides LOM, another OER mechanism is described as the adsorbate evolution mechanism (AEM), which normally shows less activity than LOM. In situ attenuated totalreflection infrared (ATR-IR) was employed to investigate the participation of AEM by identifying the intensity of surface absorbed OOH (*OOH) intermediate (Figure 20c, d).34It is clear that the intensities of *OOH in seawater exceed that in pure water at all applied potentials, suggesting higher *OOH coverage (Figure 20e). Namely, although the EOM is suppressed, the AEM is facilitated for OER operated in seawater, which accounts for the enhanced activity.
[0095] Based on the electrochemical tests and a series of in situ spectroscopic measurements, we propose a Cl boosted OER process in alkaline seawater, including the atomic valence evolution, structural evolution and mechanism transfer (Figure 20f). In pure water, as the anodic potential rises, the valences of Ni and Fe increase to Ni3+and Fe4+with the OER proceeding via a LOM pathway. The improved Fe valence caused by the attack of OH- leads to its leaching and results in unsatisfactory durability performance. In seawater, due to the Cl adsorption on the Fe site, the Fe is protected from the attack of OH , thus suppressing leaching. Simultaneously, Ni valence is increased, with the AEM pathway dominating the OER. The improvement of Ni valence and promoted AEM explains the activity increase in seawater. The protective effect of Cl on Fe and the resultant suppression of Fe leaching, along with the stable lattice oxygen aid in the excellent stability performance.
[0096] H-cell and commercial AE device performance
[0097] The overall seawater-splitting performances were evaluated in an H-cell (electrode area: 1 cm2) and a commercial AE (electrode area: 120 cm2). NiFe EDH and NiSx were used as the anode and cathode electrodes, respectively.35For H-cell measurement, as expected, better overall electrochemical activity and durability were obtained in seawater than in pure water (Figure 23a, b). As a comparison, Ni(0H)2 showed a much worse activity and underwent a quick decline of stability in seawater because there is no such Cl promotion and protection mechanism. Additionally, the participation of C1ER was investigated by quantifying the amounts of O2 generated in two electrolytes (Figure 24). The RFE in seawater at 200 mA cm2operation is close to 100 % without C1ER, indicating that Cl -free seawater splitting is achieved (Figure 23c). As a key metric for measuring durability, the leaching of Fe was reduced by more than half, from 51 ng mF1to 16 ng mL1at the end of the test (Figure 23c).
[0098] To investigate the viability of the strategy for large-scale direct seawater electrolysis, a commercial AE was fabricated running at 80 °C (Figure 23d, e). As reported, the performance of alkaline seawater electrolysis is far inferior to that of alkaline pure water electrolysis, as also evidenced in using Ni(0H)2 anode in H-cell (Figure 23a).36However, in our scale-up system, the advantageous interactions between both Cl and NiFe LDH have compensated for these negative effects. The polarization curves (without iR compensation) in Figure 23f show that seawater-based AE has improved water electrolysis activity than that using pure water. As a result, when using highly active NiFe LDH, the electricity expense of H2 production decreased from 4.59 kWh Nm3H2 to 4.1 kWh Nm3H2 at 200 mA cm2operation current density and from 5.41 kWh Nm3H2 to 4.72 kWh Nm3H2 at 400 mA cm2from pure water to seawater running (Figure 23g). As a comparison, these values on a commercial Ni(OH)2-based pure water AE is 5 kWh and 5.95 kWh, respectively (Figure 23g). This means the seawater electrolysis with NiFe EDH anode decreases the electricity expense by 12.8 % to the pure water electrolysis with same anode and 20.7 % to the commercial pure water electrolysis. Additionally, at a constant current density of 200 mA cm2(10.08 E h1H2 generation rate), the commercial AE with NiFe EDH works stably for over 100 hours with no obvious failure for seawater electrolysis (Figure 23h).
[0099] In summary, we have achieved direct and ClER-free alkaline seawater electrolysis in a NiFe LDH-based commercial AE. The key to its stable operation in seawater is the utilization of the positive synergies between Cl and NiFe LDH. Via comprehensive electrochemical tests and a set of in situ spectroscopic measurements (Raman, XAS, ATR-IR, DEMS), it was found that the absorption of Cl in seawater contributes to the OER activity and stability performance for NiFe LDH. Thus, the commercial AE showed excellent durability performance for over 100 hours in naturally alkaline seawater. Besides, it processes a relatively low cost of 4.72 kWh Nm3H2 in natural seawater while it needs 5.41 kWh Nm3H2 in pure water. These findings not only provide a new understanding of the OER mechanism for typical catalysts in seawater, but also demonstrate its great potential for future scale-up H2 generation by alkaline seawater electrolysis.
[0100] The reference to any prior art in this specification is not, and should not be taken as, an acknowledgement or any form of suggestion that such prior art forms part of the common general knowledge.
[0101] It will be understood that the terms “comprise” and “include” and any of their derivatives (e.g. comprises, comprising, includes, including) as used in this specification, and the claims that follow, is to be taken to be inclusive of features to which the term refers, and is not meant to exclude the presence of any additional features unless otherwise stated or implied.
[0102] In some cases, a single embodiment may, for succinctness and / or to assist in understanding the scope of the disclosure, combine multiple features. It is to be understood that in such a case, these multiple features may be provided separately (in separate embodiments), or in any other suitable combination. Alternatively, where separate features are described in separate embodiments, these separate features may be combined into a single embodiment unless otherwise stated or implied. This also applies to the claims which can be recombined in any combination. That is a claim may be amended to include a feature defined in any other claim. Further a phrase referring to “at least one of’ a list of items refers to any combination of those items, including single members. As an example, “at least one of: a, b, or c” is intended to cover: a, b, c, a-b, a-c, b-c, and a-b-c.
[0103] It will be appreciated by those skilled in the art that the disclosure is not restricted in its use to the particular application or applications described. Neither is the present disclosure restricted in its preferred embodiment with regard to the particular elements and / or features described or depicted herein. It will be appreciated that the disclosure is not limited to the embodiment or embodiments disclosed, but is capable of numerous rearrangements, modifications and substitutions without departing from the scope as set forth and defined by the following claims.REFERENCES
[0104] 1. Wan, L., Pang, M., Le, J., Xu, Z. & Zhou, H. Oriented intergrowth of the catalyst layer in membrane electrode assembly for alkaline water electrolysis. Nat. Commun. 13, 7956 (2022).
[0105] 2. Xu, Q. et al. Anion Exchange Membrane Water Electrolyzer: Electrode Design, Lab-Scaled Testing System and Performance Evaluation. EnergyChem 4, 100087 (2022).
[0106] 3. Dresp, S., Dionigi, F., Klingenhof, M. & Strasser, P. Direct electrolytic splitting of seawater: Opportunities and challenges. ACS Energy Letters 4, 933-942 (2019).
[0107] 4. Jin, H. et al. Stable and Highly Efficient Hydrogen Evolution from Seawater Enabled by an Unsaturated Nickel Surface Nitride. Adv. Mater. 33, 1-8 (2021).
[0108] 5. Dionigi, F., Reier, T., Pawolek, Z., Gliech, M. & Strasser, P. Design Criteria, OperatingConditions, and Nickel-Iron Hydroxide Catalyst Materials for Selective Seawater Electrolysis.ChemSusChem 9, 962-972 (2016).
[0109] 6. Karlsson, R. K. B. & Cornell, A. Selectivity between Oxygen and Chlorine Evolution in the Chlor-Alkali and Chlorate Processes. Chem. Rev. 116, 2982-3028 (2016).
[0110] 7. Zhang, S. et al. A study on the interaction between chloride ions and CO2 towards carbon steel corrosion. Corros. Sci. 167, 108531 (2020).
[0111] 8. Zheng, Y. & Qiao, S. Z. Direct seawater splitting to hydrogen by a membrane electrolyzer. Joule 7, 20-22 (2023).
[0112] 9. Farra, P., Strasser, P. & Cowan, A. J. Previews Water electrolysis : Direct from the sea or not to be ? Joule 5, 1921-1923 (2021).
[0113] 10. He, C. et al. Future global urban water scarcity and potential solutions. Nat. Commun. 12,1-11 (2021).
[0114] 11. Kuang, Y. et al. Solar-driven, highly sustained splitting of seawater into hydrogen and oxygen fuels. Proc. Natl. Acad. Sci. U. S. A. 116, 6624-6629 (2019).
[0115] 12. Yu, L. et al. Non-noble metal-nitride based electrocatalysts for high-performance alkaline seawater electrolysis. Nat. Commun. 10, 1-10 (2019).
[0116] 13. Guo, J. et al. Direct seawater electrolysis by adjusting the local reaction environment of a catalyst. Nat. Energy 8, 264-272 (2023).
[0117] 14. Vos, J. G. et al. Selectivity Trends between Oxygen Evolution and Chlorine Evolution onIridium-Based Double Perovskites in Acidic Media. ACS Catal. 9, 8561-8574 (2019).
[0118] 15. Dresp, S. et al. Direct Electrolytic Splitting of Seawater: Activity, Selectivity,Degradation, and Recovery Studied from the Molecular Catalyst Structure to the Electrolyzer Cell Level. Adv. Energy Mater. 8, 1800338 (2018).
[0119] 16. Online, V. A., Bru, S., Hauke, P. & Strasser, P. Environmental Science Efficient direct seawater electrolysers using selective alkaline NiFe-LDH as OER catalyst in asymmetric electrolyte feeds f. 13, 1725-1729 (2020).
[0120] 17. Klingenhof, M. et al. Anion-Tuned Layered Double Hydroxide Anodes for AnionExchange Membrane Water Single-Cell Performance. ACS Energy Lett. 7, 3415-3422 (2022).
[0121] 18. Xu, Q. et al. EnergyChem Anion Exchange Membrane Water Electrolyzer : ElectrodeDesign , Lab-Scaled Testing System and Performance Evaluation. EnergyChem 4, 100087 (2022).
[0122] 19. Chang, J. et al. Dual-Doping and Synergism toward High-Performance SeawaterElectrolysis. Adv. Mater. 33, 2101425 (2021).
[0123] 20. Yu, L. et al. Ultrafast room-temperature synthesis of porous S-doped Ni / Fe(oxy)hydroxide electrodes for oxygen evolution catalysis in seawater splitting. Energy Environ. Sci. 13, 3439-3445 (2020).
[0124] 21. Obata, K. & Takanabe, K. A Permselective CeOx Coating To Improve the Stability ofOxygen Evolution Electrocatalysts. Angew. Chemie - Int. Ed. 57, 1616-1620 (2018).
[0125] 22. Kuang, Y. et al. Solar-driven, highly sustained splitting of seawater into hydrogen and oxygen fuels. Proc. Natl. Acad. Sci. U. S. A. 116, 6624-6629 (2019).
[0126] 23. Dresp, S. et al. Molecular Understanding of the Impact of Saline Contaminants andAlkaline pH on NiFe Layered Double Hydroxide Oxygen Evolution Catalysts. ACS Catal. 11, 6800-6809 (2021).
[0127] 24. Feng, C. et al. A self-healing catalyst for electrocatalytic and photoelectrochemical oxygen evolution in highly alkaline conditions. Nat. Commun. 12, 5980 (2021).
[0128] 25. Lee, S., Bai, L. & Hu, X. Deciphering Iron-Dependent Activity in Oxygen EvolutionCatalyzed by Nickel-Iron Layered Double Hydroxide. Angew. Chemie - Int. Ed. 59, 8072-8077 (2020).
[0129] 26. Liu, M., Min, K. A., Han, B. & Lee, L. Y. S. Interfacing or Doping? Role of Ce in HighlyPromoted Water Oxidation of NiFe-Layered Double Hydroxide. Adv. Energy Mater. 11, 1-11 (2021).
[0130] 27. Tu, Q. et al. Preferential Adsorption of Hydroxide Ions onto Partially Crystalline NiFe-Layered Double Hydroxides Leads to Efficient and Selective OER in Alkaline Seawater. ACS Appl. Energy Mater. 4, 4630-4637 (2021).
[0131] 28. Anantharaj, S., Kundu, S. & Noda, S. “The Fe Effect”: A review unveiling the critical roles of Fe in enhancing OER activity of Ni and Co based catalysts. Nano Energy 80, 105514 (2021).
[0132] 29. Chung, D. Y. et al. Dynamic stability of active sites in hydr(oxy)oxides for the oxygen evolution reaction. Nat. Energy 5, 222-230 (2020).
[0133] 30. Chen, R. et al. Layered Structure Causes Bulk NiFe Layered Double Hydroxide Unstable in Alkaline Oxygen Evolution Reaction. Adv. Mater. 31, 1903909 (2019).
[0134] 31. He, Z. et al. Activating lattice oxygen in NiFe-based (oxy)hydroxide for water electrolysis. Nat. Commun. 13, 2191 (2022).
[0135] 32. Wu, Z. Y. et al. Non-iridium-based electrocatalyst for durable acidic oxygen evolution reaction in proton exchange membrane water electrolysis. Nat. Mater. 22, 100-108 (2022).
[0136] 33. Wen, Y. et al. Stabilizing Highly Active Ru Sites by Suppressing Lattice OxygenParticipation in Acidic Water Oxidation. J. Am. Chem. Soc. 143, 6482-6490 (2021).
[0137] 34. Du, K. et al. Interface engineering breaks both stability and activity limits of RuO2 for sustainable water oxidation. Nat. Commun. 13, 5448 (2022).
[0138] 35. Wang, J. et al. Water Dissociation Kinetic-Oriented Design of Nickel Sulfides viaTailored Dual Sites for Efficient Alkaline Hydrogen Evolution. Adv. Funct. Mater. 31, 2008578 (2021).
[0139] 36. Xie, H. et al. A membrane-based seawater electrolyser for hydrogen generation. Nature612, 673-678 (2022).
Claims
CLAIMS1. A saltwater electrolysis apparatus, the apparatus comprising an anode for generating oxygen from water containing chloride ions, the anode comprising an anode substrate and a metal based electrocatalyst layer coating wherein the anode is configured so that, in use, absorption of chloride ions from alkaline saltwater to the electrocatalyst layer coating contributes to the OER activity and stability performance of the anode to provide direct and ClER-free alkaline saltwater electrolysis.
2. The saltwater electrolysis apparatus of claim 1, wherein the anode does not comprise a passivation layer.
3. The apparatus of any one of claims 1 to 2, wherein the metallic layered double hydroxide is a mixed metal layered double hydroxide.
4. The apparatus of claim 3, wherein the mixed metal layered double hydroxide is a nickel-based bimetallic layered double hydroxide.
5. The apparatus of claim 4, wherein the nickel-based bimetallic layered double hydroxide is selected from one or more of the group consisting of nickel-iron layered double hydroxide, nickel-cobalt layered double hydroxide, nickel-aluminum layered double hydroxide, nickel-zinc layered double hydroxide, nickel-copper layered double hydroxide, nickel-manganese layered double hydroxide, nickeliridium layered double hydroxide, and nickel-ruthenium layered double hydroxide.
6. The apparatus of claim 5, wherein the nickel-based bimetallic layered double hydroxide is nickeliron layered double hydroxide.
7. The apparatus of claim 6, wherein, in use, absorption of chloride ions from alkaline saltwater on Fe3+stabilizes the oxidation state of Fe at the anode.
8. The apparatus of any one of claims 1 to 7, wherein the apparatus further comprises a cathode for generating hydrogen from water containing chloride ions, the cathode comprising a cathode substrate and a metal based electrocatalyst layer coating.
9. The apparatus of any one of claims 1 to 8, wherein the electricity expense of H2 production is less than 4.5 kWh Nm3H2 at 200 mA cm2operation current density and / or less than 5.0 kWh Nm3H2 at 400 mA cm2.
10. The apparatus of any one of claims 1 to 9, wherein at a constant current density of 200 mA cm2the saltwater electrolysis apparatus works stably for over 100 hours with no substantial failure for seawater electrolysis.
11. A method of operating the saltwater electrolysis apparatus of any one of the preceding claims, comprising generating oxygen and hydrogen from saltwater.
Citation Information
Patent Citations
Layered double hydroxide nano-film electrode material, preparation method and application thereof
CN115011990A
Highly sustained electrodes and electrolytes for salty alkaline and neutral water splitting
US11326265B2
Electrolysis system and method for using same
WO2021229963A1
Anion exchange membrane type aqueous electrolytic cell
WO2022244805A1
Cited By
Catalyst and anode for hydrogen production by electrolysis as well as preparation method, activation method and use thereof
US12454765B2
Catalyst and anode for hydrogen production by electrolysis as well as preparation method, activation method and use thereof
US20250257483A1