Gypsum block with low water requirement and preparation method therefor
By using a combination of gypsum powder, glass fiber and retarder in the preparation of gypsum blocks, combined with ultrasonic treatment, the water paste ratio of gypsum blocks is reduced, and the strength and water resistance caused by moisture escape in the prior art are solved. Problem, gypsum blocks with high strength and water resistance are achieved, and the drying process is simplified, energy-saving and environmentally friendly.
Patent Information
- Application Number
- PCT/CN2023/099460
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-26
- Filing Date
- 2023-06-09
- Publication Date
- 2024-12-05
AI Technical Summary
The existing gypsum blocks require too much water during the stirring process, resulting in water leakage, causing pores and capillaries, reducing the strength and water resistance of gypsum products.
By mixing gypsum powder, glass fibers, retarder and water, a first slurry is formed, and the gypsum particles, gas induction agent and the first slurry are ultrasonicized to form a second slurry, and then poured into a mold to form a mold. Using a combination of low water demand materials, including 100 parts of gypsum clinker, 30 to 50 parts of water, 0.1 to 1.5 parts of glass fiber, 0.01 to 0.05 parts of gas induction agent and 0.05 to 0.15 parts of retarder, to reduce the water paste ratio and improve the Strength and water resistance.
It realizes low water demand molding of gypsum blocks, reduces pores, improves strength and water resistance, and does not require drying, can dry naturally, save energy and reduce consumption.
Smart Images

Figure PCTCN2023099460-FTAPPB-I100001
Abstract
Description
A low water demand gypsum building block and preparation method thereof Technical Field
[0001] The present invention relates to, but is not limited to, the field of building materials technology, and in particular to, but is not limited to, a gypsum block that requires little mixing water during production. Background Art
[0002] Gypsum blocks are a new lightweight wall material that has been gradually developed in my country. They offer simple construction, lightweight construction, and excellent thermal and sound insulation. They offer irreplaceable advantages in terms of ease of construction, short construction times, and excellent wall smoothness.
[0003] The main raw material for gypsum blocks is gypsum. The theoretical water requirement for gypsum is 18.6%. However, to ensure the slurry maintains a certain fluidity, water must be added during the mixing process, far exceeding the theoretical water requirement—typically 60% to 80%. After the gypsum slurry hardens, excess water escapes from the hardened gypsum product, creating numerous voids and capillaries, which degrades the strength and water resistance of the hardened gypsum product.
[0004] SUMMARY OF THE INVENTION
[0005] The following is an overview of the subject matter described in detail herein. This overview is not intended to limit the scope of protection of this application.
[0006] The embodiment of the present application proposes a method for preparing low-water-demand gypsum blocks, which significantly reduces the water-to-cement ratio of the gypsum blocks, ensuring that the gypsum blocks can be formed at a low water-to-cement ratio and that the strength and water resistance of the gypsum blocks meet the requirements.
[0007] The present application provides a low-water-demand gypsum building block, which comprises, by weight:
[0008] The invention relates to a method for preparing a dihydrated gypsum obtained by hydrating 100 parts of gypsum clinker and 30 to 50 parts of water, 0.1 to 1.5 parts of glass fiber, 0.01 to 0.05 parts of air entraining agent, and 0.05 to 0.15 parts of retarder. The gypsum clinker is a mixture of gypsum powder and gypsum particles.
[0009] Alternatively, the gypsum blocks are composed by weight of:
[0010] The invention comprises 100 parts of gypsum clinker, 30 to 50 parts of dihydrate gypsum formed by hydration of water, 0.1 to 1.5 parts of glass fiber, 0.01 to 0.05 parts of air entraining agent and 0.05 to 0.15 parts of retarder.
[0011] On the other hand, the present application also provides a method for preparing the above-mentioned gypsum blocks, the preparation method comprising the following steps:
[0012] (1) mixing the gypsum powder, the glass fiber, the retarder and the water to obtain a first slurry;
[0013] (2) mixing the gypsum particles, the air entraining agent, and the first slurry and stirring them while performing ultrasonic treatment to obtain a second slurry;
[0014] (3) Pour the second slurry into a mold to form gypsum blocks.
[0015] In the present application, desulfurized gypsum clinker, natural gypsum clinker, phosphogypsum clinker and titanium gypsum clinker are used as raw materials, which is economical and environmentally friendly, and reduces the pollution of solid waste to the environment.
[0016] The gypsum blocks provided by the present application can reduce the water-to-plastic ratio of the entire gypsum, reduce gypsum porosity, and improve the strength and water resistance of the gypsum blocks. The gypsum blocks provided by the present application use little water and do not require drying after forming. They can be dried naturally in the air, thus saving energy and reducing consumption.
[0017] Other features and advantages of the present application will be described in the following description, and in part will become apparent from the description, or will be understood by practicing the present application. Other advantages of the present application can be realized and obtained by the solutions described in the description.
[0018] Details
[0019] The following describes the embodiments of the present application in detail. Unless there is a conflict, the embodiments and features in the embodiments of the present application can be combined with each other in any manner.
[0020] The present application provides a low-water-demand gypsum building block, which comprises, by weight:
[0021] 100 parts of gypsum clinker and 30 to 50 parts of water to form dihydrate gypsum, 0.1 to 1.5 parts of glass fiber, 0.01 to 0.05 parts of air entraining agent and 0.05 to 0.15 parts of retarder.
[0022] In some embodiments provided herein, the gypsum block is composed, by weight, of 100 parts of gypsum clinker and 30 to 50 parts of dihydrate gypsum formed by hydration of water, 0.1 to 1.5 parts of glass fiber, 0.01 to 0.05 parts of air entraining agent, and 0.05 to 0.15 parts of retarder.
[0023] In some embodiments provided herein, the gypsum clinker is selected from any one or more of desulfurized gypsum clinker, natural gypsum clinker, phosphogypsum clinker and titanium gypsum clinker.
[0024] In some embodiments provided herein, the gypsum clinker is a mixture of gypsum powder and gypsum particles, and the gypsum powder accounts for 30 wt.% to 40 wt.% of the gypsum clinker;
[0025] The specific surface area of the gypsum powder is 100m 2 / kg to 200m 2 / kg, the particle size of the gypsum powder is 20μm to 150μm; and the specific surface area is the Blaine specific surface area.
[0026] In some embodiments provided herein, the gypsum particles are flake-shaped particles with a diameter of 2 mm to 5 mm and a thickness of 1 mm to 2 mm.
[0027] In some embodiments provided herein, the gypsum particles are obtained by compressing gypsum powder using a tablet press.
[0028] In some embodiments provided herein, the density of the gypsum particles is 1.4 g / cm 3 Up to 1.6g / cm 3 .
[0029] In some embodiments provided herein, the glass fiber has a diameter of 10 μm to 20 μm and a length of 6 mm to 10 mm.
[0030] In some embodiments provided herein, the air entraining agent is selected from any one or more of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, and sodium fatty alcohol polyoxyethylene ether sulfate.
[0031] In some embodiments provided herein, the retarder is selected from any one or more of sodium citrate, tartaric acid, potassium tartrate, acrylic acid, sodium hexametaphosphate, and sodium polyphosphate.
[0032] On the other hand, the present application also provides a method for preparing the above-mentioned gypsum blocks, the preparation method comprising the following steps:
[0033] (1) mixing the gypsum powder, the glass fiber, the retarder and the water to obtain a first slurry;
[0034] (2) mixing the gypsum particles, the air entraining agent, and the first slurry and stirring them while performing ultrasonic treatment to obtain a second slurry;
[0035] (3) Pour the second slurry into a mold to form gypsum blocks.
[0036] In some embodiments provided herein, the duration of the ultrasound is 20s to 60s; and the frequency of the ultrasound is 25kHz to 60kHz.
[0037] In some embodiments provided in the present application, the second slurry is poured into a mold, and after forming and demoulding, it is placed in a natural drying place to dry in the sun to obtain gypsum blocks. DETAILED DESCRIPTION
[0038] Example 1
[0039] This embodiment provides a low-water-demand gypsum block, which includes: dihydrate gypsum formed by hydrating 100 parts by weight of desulfurized gypsum clinker and 35 parts by weight of water, 0.1 parts by weight of chopped glass fiber, 0.01 parts by weight of air entraining agent and 0.05 parts by weight of retarder.
[0040] The low water demand gypsum blocks of this embodiment are prepared by the following method:
[0041] (1) 30 parts by weight of gypsum powder (the specific surface area of gypsum powder is 155m 2 / kg, gypsum powder with a particle size of 40 μm to 120 μm), chopped glass fibers (with a diameter of 13 μm and a length of 6 mm), a retarder (sodium citrate) and water are mixed and stirred to obtain a first slurry;
[0042] (2) 70 parts by weight of gypsum particles (diameter 3 mm, thickness 1 mm, density 1.5 g / cm 3 ), an air entraining agent (sodium lauryl sulfate) and the first slurry are introduced into a mixer, and ultrasonicated for 30 seconds at an ultrasonic frequency of 45 kHz to obtain a second slurry;
[0043] (3) Pour the second slurry into a block forming machine, and place it in a natural drying place to dry in the sun after forming and demoulding to obtain gypsum blocks.
[0044] Example 2
[0045] This embodiment provides a low-water-demand gypsum block, which includes: dihydrate gypsum formed by hydrating 100 parts by weight of phosphogypsum clinker and 45 parts by weight of water, 1 part by weight of chopped glass fiber (diameter 13 μm, length 6 mm), 0.03 part by weight of an air-entraining agent (sodium dodecylbenzenesulfonate), and 0.1 part by weight of a retarder (tartaric acid).
[0046] The preparation method of the low water demand gypsum blocks of this embodiment is the same as that of embodiment 1. However, the weight of the gypsum powder is 40 parts by weight (the specific surface area of the gypsum powder is 155m 2 / kg, the particle size of gypsum powder is 40μm to 120μm, the weight of gypsum particles is 60 parts by weight (diameter 4mm, thickness 1.5mm, density 1.6g / cm 3 ).
[0047] Comparative Example 1
[0048] The only difference between this comparative example and Example 1 is that no gypsum particles are added to the gypsum blocks, the gypsum clinker is all gypsum powder, and the other components and preparation method are the same as those in Example 1.
[0049] Comparative Example 2
[0050] The only difference between this comparative example and Example 1 is that no gypsum powder is added to the gypsum blocks, the gypsum clinker is all gypsum particles, and the other components and preparation method are the same as those in Example 1.
[0051] Comparative Example 3
[0052] The only difference between this comparative example and Example 1 is that no retarder is added to the gypsum blocks, and the remaining components and preparation method are the same as those in Example 1.
[0053] Comparative Example 4
[0054] The only difference between this comparative example and Example 1 is that the gypsum blocks are not subjected to ultrasonic treatment, and the remaining components and preparation method are the same as those in Example 1.
[0055] Comparative Example 5
[0056] The only difference between this comparative example and Example 1 is that the gypsum particles in the gypsum blocks have a diameter of 8 mm, a thickness of 4 mm, and a particle density of 2.0 g / cm 3 The remaining components and preparation method are the same as those in Example 1.
[0057] Performance Testing
[0058] The mechanical properties of the gypsum blocks prepared in Examples 1 to 2 and Comparative Examples 1 to 5 were tested according to the JC / T698-2010 "Gypsum Block" standard. The test results are shown in Table 1 below.
[0059] Table 1 Implementation effect (solid)
[0060] The test results show that the strength and softening coefficient performance indicators of the low water demand gypsum blocks provided in this application are significantly better than the technical requirements of the solid gypsum block breaking load ≥2000N and softening coefficient ≥0.6 in the JC / T698-2010 "Gypsum Block" standard.
[0061] Although the embodiments disclosed in this application are as described above, the contents described are merely embodiments adopted to facilitate understanding of this application and are not intended to limit this application. Any person skilled in the art to which this application belongs may make any modifications and changes in the form and details of the implementation without departing from the spirit and scope disclosed in this application.
Claims
1. A low water demand gypsum block, wherein the gypsum block is measured by weight include: Dihydrate gypsum formed by hydration of 100 parts of gypsum clinker and 30 to 50 parts of water, 0.1 to 1.5 parts of glass fiber, 0.01 to 0.05 parts of air entraining agent and 0.05 to 0.15 parts of retarder.
2. The gypsum block according to claim 1, It is characterized in that The gypsum clinker is selected from any one or more of desulfurized gypsum clinker, natural gypsum clinker, phosphogypsum clinker and titanium gypsum clinker.
3. The gypsum block according to claim 1, It is characterized in that The gypsum clinker is a mixture of gypsum powder and gypsum particles, wherein the gypsum powder accounts for 30wt.% to 40wt.% of the gypsum clinker; The specific surface area of the gypsum powder is 100m 2 / kg to 200m 2 / kg, the particle size of the gypsum powder is 20μm to 150μm; The specific surface area is the Blaine specific surface area.
4. The gypsum block according to claim 3, It is characterized in that The gypsum particles are flake particles with a diameter of 2 mm to 5 mm and a thickness of 1 mm to 2 mm.
5. The gypsum block according to claim 3 or 4, It is characterized in that The density of the gypsum particles is 1.4 g / cm 3 Up to 1.6g / cm 3 .
6. The gypsum block according to any one of claims 1 to 4, It is characterized in that The glass fiber has a diameter of 10 μm to 20 μm and a length of 6 mm to 10 mm.
7. The gypsum block according to any one of claims 1 to 4, It is characterized in that The air entraining agent is selected from any one or more of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate and sodium polyoxyethylene fatty alcohol ether sulfate.
8. The gypsum block according to any one of claims 1 to 4, It is characterized in that The retarder is selected from any one or more of sodium citrate, tartaric acid, potassium tartrate, acrylic acid, sodium hexametaphosphate and sodium polyphosphate.
9. The method for preparing a gypsum block according to any one of claims 3 to 8, wherein the method The following steps are involved: Mixing the gypsum powder, the glass fiber, the retarder and the water to obtain a first slurry; The gypsum particles, the air entraining agent and the first slurry are mixed and stirred while being subjected to ultrasonic treatment to obtain a second slurry; The second slurry is poured into molds to form gypsum blocks.
10. The preparation method according to claim 9, It is characterized in that The duration of the ultrasound is 20s to 60s; the frequency of the ultrasound is 25kHz to 60kHz.
Citation Information
Patent Citations
Method for preparing gypsum building block with titanium gypsum
CN101920520A
Gypsum building block produced from regenerated aggregate and gypsum, and production method thereof
CN103936379A
Gypsum block produced and prepared by dry method
CN111469260A
Gypsum block
CN113248221A
KR20220085135A