Non-stick plastic container and manufacturing method therefor
By forming a silicon nitride layer and a dielectric layer on the plastic material, combined with magnetron sputtering technology, the hazards of PFAS substances in Teflon coating are solved, providing a safe and environmentally friendly non-stick and durability solution to meet the needs of the The performance requirements of non-stick pan products.
Patent Information
- Application Number
- PCT/CN2023/118506
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-09-07
- Filing Date
- 2023-09-13
- Publication Date
- 2024-12-05
AI Technical Summary
The existing Teflon coating contains PFAS substances, which are harmful to human health and the environment, and lacks alternative non-stick pot product solutions, which can not only meet the performance of non-stick pots without using PFAS substances.
Use plastic material as the substrate to form a silicon nitride layer on the surface, and add zirconium, chromium or titanium dielectric layers in some embodiments to form a silicon nitride layer or its composite layer through magnetron sputtering technology to ensure non-stickness and durability sex.
It achieves the effects of non-stickness, high temperature resistance, easy cleaning, high hardness, high wear resistance and organic chemical coating, while avoiding the use of PFAS, providing a safe and environmentally friendly alternative.
Smart Images

Figure CN2023118506_05122024_PF_FP_ABST
Abstract
Description
Non-stick plastic container and preparation method thereof Technical Field
[0001] The present invention relates to the technical field of non-stick coatings, and in particular to a non-stick plastic container and a preparation method thereof. Background Art
[0002] Teflon-coated nonstick pans, as well as heated plastic containers and bowls, have seen significant global adoption over the past few decades. The high-temperature, corrosion-resistant, and highly effective nonstick properties of Teflon coatings have made them ubiquitous in households, generating a market exceeding one trillion yuan. However, further research has revealed that the presence of PFAS (per- and polyfluoroalkyl substances) poses health and environmental risks. PFAS' chemical composition prevents them from degrading in the environment for extended periods. While this property makes PFAS highly valuable, it also carries the potential for long-term harm to the environment and humans, including carcinogenicity. With several US states banning PFAS, and Europe about to introduce similar regulations, the use of alternative coatings to Teflon has become an industry trend. To date, no better solution has been identified that achieves the desired nonstick performance while avoiding the use of PFAS.
[0003] Summary of the Invention
[0004] In view of the above shortcomings of the prior art, an object of the present invention is to provide a non-stick plastic container and a preparation method thereof, so as to prevent food from sticking to the container and facilitate cleaning.
[0005] To achieve the above-mentioned and other related objectives, a first aspect of an embodiment of the present application provides a non-stick plastic container, comprising:
[0006] a substrate made of a plastic material; and
[0007] a silicon nitride layer disposed on the substrate;
[0008] The silicon nitride layer is configured to be in contact with a food material.
[0009] In one embodiment of the present application, the non-stick plastic container further includes a zirconium dielectric layer disposed between the substrate and the silicon nitride layer.
[0010] In one embodiment of the present application, the non-stick plastic container further includes a chromium dielectric layer disposed between the substrate and the silicon nitride layer.
[0011] In one embodiment of the present application, the non-stick plastic container further includes a titanium dielectric layer disposed between the substrate and the silicon nitride layer.
[0012] In an embodiment of the present application, a thickness of the zirconium dielectric layer is 0.01 um to 2 um.
[0013] In an embodiment of the present application, a thickness of the chromium dielectric layer is 0.01 um to 2 um.
[0014] In an embodiment of the present application, a thickness of the titanium dielectric layer is 0.01 um to 2 um.
[0015] In an embodiment of the present application, a thickness of the silicon nitride layer is 0.01 um to 8 um.
[0016] A second aspect of the present invention provides a method for preparing a non-stick plastic container, the method comprising:
[0017] providing a substrate made of a plastic material; and
[0018] A silicon nitride layer is formed on a surface of the substrate by magnetron sputtering.
[0019] In an embodiment of the present application, a thickness of the silicon nitride layer is 0.01 um to 8 um.
[0020] In one embodiment of the present application, the silicon nitride layer is mixed with graphite to form a composite layer, wherein the ratio of silicon nitride is 95 wt % to 85 wt % and the ratio of graphite is 5 wt % to 15 wt %.
[0021] In one embodiment of the present application, the substrate is detachably mounted on a holding frame in a magnetron sputtering furnace. When the silicon nitride layer is formed by magnetron sputtering, the holding frame remains stationary.
[0022] In one embodiment of the present application, the substrate is detachably mounted on a holding frame in a magnetron sputtering furnace, and the holding frame is rotated when the silicon nitride layer is formed by magnetron sputtering.
[0023] A third aspect of the present invention provides a method for preparing a non-stick plastic container, the method comprising:
[0024] Providing a substrate made of a plastic material;
[0025] forming a dielectric layer on a surface of the substrate by magnetron sputtering; and
[0026] A silicon nitride layer is formed on a surface of the dielectric layer by magnetron sputtering.
[0027] In an embodiment of the present application, the dielectric layer is a zirconium dielectric layer.
[0028] In an embodiment of the present application, a thickness of the zirconium dielectric layer is 0.01 um to 2 um.
[0029] In an embodiment of the present application, the dielectric layer is a chromium dielectric layer.
[0030] In an embodiment of the present application, a thickness of the chromium dielectric layer is 0.01 um to 2 um.
[0031] In one embodiment of the present application, the dielectric layer is a titanium dielectric layer.
[0032] In an embodiment of the present application, a thickness of the titanium dielectric layer is 0.01 um to 2 um.
[0033] In an embodiment of the present application, a thickness of the silicon nitride layer is 0.01 um to 8 um.
[0034] In one embodiment of the present application, a composite layer of the silicon nitride layer and graphite is formed on a surface of the dielectric layer by magnetron sputtering.
[0035] In one embodiment of the present application, the substrate is detachably mounted on a holding frame in a magnetron sputtering furnace. When the dielectric layer and the silicon nitride layer are formed by magnetron sputtering, the holding frame remains stationary.
[0036] In one embodiment of the present application, the substrate is detachably mounted on a holding frame in a magnetron sputtering furnace, and the holding frame rotates when the dielectric layer and the silicon nitride layer are formed by magnetron sputtering.
[0037] As described above, the non-stick plastic container and preparation method thereof provided in the embodiments of the present application adopt a plastic material substrate, and then form a dielectric layer or a dielectric layer and a silicon nitride layer on the surface. The silicon nitride layer has a stable molecular structure and is non-toxic and harmless. It can replace Teflon-related products in the field of non-stick plastic containers. It can not only meet the non-stick performance but also does not use substances containing PFAS. It has the characteristics of high hardness, high wear resistance, high corrosion resistance, high temperature resistance, easy cleaning, no discoloration, no organic chemical coating, and long-lasting non-stick. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.
[0039] FIG1 is a schematic cross-sectional view of a partial structure of a first embodiment of a non-stick plastic container of the present application;
[0040] FIG2 is a schematic cross-sectional view of a partial structure of a second embodiment of the non-stick plastic container of the present application;
[0041] FIG2-1 is a schematic cross-sectional view of a partial structure of a third embodiment of the non-stick plastic container of the present application;
[0042] FIG3 is a schematic flow chart of a first embodiment of a method for preparing a non-stick plastic container according to the present invention;
[0043] FIG3-1 is a schematic flow chart of a third embodiment of a method for preparing a non-stick plastic container of the present application;
[0044] FIG4 is a schematic flow chart of a second embodiment of a method for preparing a non-stick plastic container according to the present invention;
[0045] FIG4-1 is a schematic flow chart of a third embodiment of a method for preparing a non-stick plastic container of the present application;
[0046] FIG5 is a schematic diagram of the structure of the magnetron sputtering furnace used in the preparation method in an embodiment of the present application, wherein the holding frame is stationary; and
[0047] FIG6 is a schematic structural diagram of a magnetron sputtering furnace used in the preparation method in an embodiment of the present application, wherein the holding frame rotates.
[0048] The numbers in the figure represent: 100, non-stick plastic container; 110, substrate; 120, dielectric layer; 130, silicon nitride layer; 200, magnetron sputtering furnace; 210, holding frame; 220, target material; S100, method for preparing non-stick plastic container; S101~S102, steps; S200, method for preparing non-stick plastic container; S201~S203, steps. DETAILED DESCRIPTION
[0049] The following will be combined with the drawings in the embodiments of this application to clearly and completely describe the technical solutions in the embodiments of this application. Obviously, the embodiments described are part of the embodiments of this application, not all of them. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of this application.
[0050] It should be noted that the structures, proportions, sizes, etc. illustrated in the drawings of this specification are only used to match the contents disclosed in the specification for people familiar with this technology to understand and read, and are not used to limit the limiting conditions for the implementation of the present invention. Therefore, they have no substantial technical significance. Any modification of the structure, change in the proportional relationship or adjustment of the size should still fall within the scope of the technical content disclosed by the present invention without affecting the efficacy and purpose that can be achieved by the present invention. At the same time, terms such as "upper", "lower", "left", "right", "middle", "first", "second", etc. quoted in this specification are only for the convenience of description and are not used to limit the scope of the implementation of the present invention. Changes or adjustments in their relative relationships should also be regarded as the scope of the implementation of the present invention without substantially changing the technical content.
[0051] The present application first provides a non-stick plastic container, wherein the non-stick plastic container can be a plastic food storage box, a plastic bowl or plate, etc., which is not specifically limited here. The present application uses a plastic bowl or plate as an example for illustration.
[0052] Please refer to Figure 1, which is a schematic cross-sectional view of a partial structure of a first embodiment of a non-stick plastic container of the present application. In this embodiment, the non-stick plastic container 100 includes a substrate 110 and a silicon nitride (Si3N4) layer 130. The substrate 110 of the non-stick plastic container 100 of the present application is made of a plastic material. In some embodiments, the silicon nitride layer 130 is disposed on the substrate 110 and is configured to contact a food. In some embodiments, the silicon nitride layer has a thickness of 0.01 μm to 8 μm.
[0053] Please refer to Figure 2, which is a schematic cross-sectional view of a partial structure of a second embodiment of the non-stick plastic container of the present application. In this embodiment, the non-stick plastic container 100 includes a substrate 110, a dielectric layer 120, and a silicon nitride layer 130. In some embodiments, the dielectric layer 120 is a zirconium dielectric layer having a thickness of 0.01 to 2 μm. In other embodiments, the dielectric layer 120 is a chromium dielectric layer having a thickness of 0.01 to 2 μm. In other embodiments, the dielectric layer 120 is a titanium dielectric layer having a thickness of 0.01 to 2 μm. In some embodiments, the silicon nitride layer has a thickness of 0.01 to 8 μm.
[0054] As described above, the non-stick plastic container provided in the embodiment of the present application adopts a base material of plastic material, and then forms a dielectric layer or a dielectric layer and a silicon nitride layer on the surface. The silicon nitride layer has a stable molecular structure and is non-toxic and harmless. It can replace Teflon-related products in the field of non-stick plastic containers. It can not only meet the non-stick performance but also does not use substances containing PFAS. It has the characteristics of high hardness, high wear resistance, high corrosion resistance, high temperature resistance, easy cleaning, no discoloration, no organic chemical coating, and long-lasting non-stick.
[0055] Please refer to Figure 2-1, which is a schematic cross-sectional view of the partial structure of the third embodiment of the non-stick plastic container of the present application. In order to increase hardness and wear resistance, a silicon nitride layer 130 is mixed with graphite to form a composite layer 130a disposed on the surface of the dielectric layer, wherein the ratio of silicon nitride is 95wt% to 85wt% and the ratio of graphite is 5wt% to 15wt%.
[0056] In addition, the embodiment of the present application further provides a method S100 for preparing a non-stick plastic container. Please refer to FIG3 , which is a flow chart of the first embodiment of the method for preparing a non-stick plastic container of the present application. The preparation method S100 includes but is not limited to the following steps.
[0057] In step S101, a substrate 110 is provided. The substrate 110 is made of a plastic material. The shape of the substrate 110 can be any pot or any food storage box, and is not specifically limited here.
[0058] In step S102 , a silicon nitride layer 130 is formed on a surface of the substrate 110 by magnetron sputtering.
[0059] In step S102, a silicon nitride layer 130 may be formed on a surface of the substrate 110 using a magnetron sputtering furnace 200 and a target (silicon nitride) 220. Referring to FIG5 , FIG5 is a schematic diagram of the structure of a magnetron sputtering furnace used in the preparation method according to an embodiment of the present application, wherein the substrate 110 is detachably mounted on a holder 210 within the magnetron sputtering furnace 200. When the silicon nitride layer 130 is formed by magnetron sputtering, the holder 210 remains stationary. Alternatively, referring to FIG6 , FIG6 is a schematic diagram of the structure of a magnetron sputtering furnace used in the preparation method according to an embodiment of the present application, wherein the substrate 110 is detachably mounted on a holder 210 within the magnetron sputtering furnace 200. When the silicon nitride layer 130 is formed by magnetron sputtering, the holder 210 rotates so that the silicon nitride layer 130 is uniformly formed on the surface of the substrate 110.
[0060] The following will introduce a specific embodiment of the first embodiment of the method S100 for preparing the non-stick plastic container shown in FIG. 3 .
[0061] For example, a plastic substrate 110 is mechanically polished. The polished plastic substrate 110 is then sandblasted and dust removed with compressed air. The substrate is then placed in a magnetron sputtering furnace 200. Thin film deposition is performed using a magnetron sputtering target (e.g., silicon nitride) (i.e., target material 220) in the magnetron sputtering furnace 200. After the film reaches a thickness of 0.01 to 8 μm, the substrate is removed, completing the thin film deposition process. Specific data is shown in the table below.
[0062]
[0063] 3-1 , in order to increase hardness and wear resistance, a step S102a is used to mix the silicon nitride layer 130 with graphite to form a composite layer 130a, wherein the ratio of silicon nitride is 95wt% to 85wt% and the ratio of graphite is 5wt% to 15wt%.
[0064] In addition, the embodiment of the present application further provides a method S200 for preparing a non-stick plastic container. Please refer to FIG4 , which is a flow chart of a second embodiment of the method for preparing a non-stick plastic container of the present application. The preparation method S200 includes but is not limited to the following steps.
[0065] In step S201, a substrate 110 is provided. The substrate 110 is made of a plastic material. The shape of the substrate 110 can be any pot or any food storage box, and is not specifically limited here.
[0066] In step S202 , a dielectric layer 120 is formed on a surface of the substrate 110 by magnetron sputtering.
[0067] In step S202, a magnetron sputtering furnace 200 and a target material (zirconium (Zr), chromium (Cr), or titanium (Ti)) may be used to form a dielectric layer 120 on a surface of the substrate 110. Step S202 is similar to the aforementioned step S102, with the only difference being the target material. The following description uses step S102 as an example, and the dielectric layer 102 is not labeled or exposed in Figures 5 and 6. The dielectric layer 120 may be a zirconium dielectric layer (target material is zirconium), a chromium dielectric layer (target material is chromium), or a titanium dielectric layer (target material is titanium). Please refer to Figure 5, which is a schematic diagram of the structure of the magnetron sputtering furnace used in the preparation method of the embodiment of the present application. The substrate 110 is detachably mounted on a holder 210 within the magnetron sputtering furnace 200. The holder 210 remains stationary while the dielectric layer 120 is formed by magnetron sputtering (not shown in Figure 5, but refer to Figure 2). Alternatively, please refer to Figure 6, which is a structural schematic diagram of the magnetron sputtering furnace used in the preparation method in an embodiment of the present application, wherein the substrate 110 is detachably arranged on a holding frame 210 in a magnetron sputtering furnace 200. When the dielectric layer 120 (not shown in Figure 6, refer to Figure 2) is formed by magnetron sputtering, the holding frame 210 is rotated so that the dielectric layer 120 (not shown in Figure 6, refer to Figure 2) is evenly formed on the surface of the substrate 110.
[0068] In step S203 , a silicon nitride layer 130 is formed on a surface of the dielectric layer 120 by magnetron sputtering.
[0069] In step S203, a silicon nitride layer 130 may be formed on a surface of the dielectric layer 120 using a magnetron sputtering furnace 200 and a target material 220 (silicon nitride). Referring to FIG5 , FIG5 is a schematic diagram of the structure of a magnetron sputtering furnace used in the preparation method according to an embodiment of the present application. In the magnetron sputtering furnace 200, a substrate 110 including the dielectric layer 120 (not shown in FIG5 , but refer to FIG2 ) is detachably mounted on a holder 210. The holder 210 remains stationary during the formation of the silicon nitride layer 130 by magnetron sputtering. Alternatively, please refer to Figure 6, which is a schematic diagram of the structure of a magnetron sputtering furnace used in the preparation method according to an embodiment of the present application. Here, a substrate 110 including a dielectric layer 120 (not shown in Figure 6, refer to Figure 2) is detachably mounted on a holder 210 within a magnetron sputtering furnace 200. During the formation of the silicon nitride layer 130 by magnetron sputtering, the holder 210 rotates to ensure that the silicon nitride layer 130 is evenly formed on the surface of the dielectric layer 120. A pump system is also provided for vacuuming.
[0070] The following will introduce a specific embodiment of the first embodiment of the method S200 for preparing the non-stick plastic container shown in FIG. 4 .
[0071] For example, a plastic substrate 110 is mechanically polished. The polished plastic substrate 110 is then sandblasted and dust removed with compressed air. The substrate is then placed in a magnetron sputtering furnace 200. Thin film deposition is performed using an arc target (e.g., zirconium, chromium, or titanium) and a magnetron sputtering target 220 (e.g., silicon nitride) in the magnetron sputtering furnace 200. Once the film reaches a thickness of 0.01 to 8 μm, the substrate is removed, completing the film deposition process. Specific data is shown in the table below.
[0072]
[0073] In addition, please refer to FIG. 4-1 . In order to increase hardness and wear resistance, a step S203 a is used to mix the silicon nitride layer 130 with graphite to form a composite layer 130 a disposed on the surface of the dielectric layer, wherein the ratio of silicon nitride is 95 wt % to 85 wt % and the ratio of graphite is 5 wt % to 15 wt %.
[0074] According to experiments, after the above processing, the surface covering material of the non-stick plastic container (dielectric layer and silicon nitride layer or composite layer) has the properties of high hardness, high wear resistance, high corrosion resistance, high temperature resistance, easy cleaning, no discoloration, no organic chemical coating, and long-lasting non-stick.
[0075] The preparation method in the embodiment of the present application adopts a plastic material as a substrate, and then forms a dielectric layer or a dielectric layer and a silicon nitride layer or a composite layer on the surface. The silicon nitride layer has a stable molecular structure and is non-toxic and harmless. It can replace Teflon-related products in the field of non-stick plastic containers. It can not only meet the non-stick performance but also does not use substances containing PFAS. It has the characteristics of high hardness, high wear resistance, high corrosion resistance, high temperature resistance, easy cleaning, no discoloration, no organic chemical coating, and long-lasting non-stick.
[0076] The above-described embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. These modifications or replacements do not deviate from the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present application, and should all be included in the scope of protection of the present application. All equivalent modifications or changes made by those with ordinary knowledge in the relevant technical field without departing from the spirit and technical ideas disclosed by the present invention should still be covered by the claims of the present invention.
Claims
1. A non-stick plastic container, characterized in that: include: A substrate made of a plastic material; as well as a silicon nitride layer disposed on the substrate; The silicon nitride layer is configured to contact with a food material.
2. A non-stick plastic container according to claim 1, characterized in that: The non-stick plastic container further comprises a zirconium dielectric layer disposed between the substrate and the silicon nitride layer.
3. The non-stick plastic container according to claim 1, characterized in that: The non-stick plastic container further comprises a chromium dielectric layer disposed between the substrate and the silicon nitride layer.
4. The non-stick plastic container according to claim 1, characterized in that: The non-stick plastic container further comprises a titanium dielectric layer disposed between the substrate and the silicon nitride layer.
5. The non-stick plastic container according to claim 2, characterized in that: The zirconium dielectric layer has a thickness of 0.01 um to 2 um.
6. The non-stick plastic container according to claim 3, characterized in that: The thickness of the chromium dielectric layer is 0.01um to 2um.
7. The non-stick plastic container according to claim 4, characterized in that: The thickness of the titanium dielectric layer is 0.01 um to 2 um.
8. The non-stick plastic container according to claim 1, characterized in that: The silicon nitride layer has a thickness of 0.01 um to 8 um.
9. The non-stick plastic container according to claim 1, characterized in that: The silicon nitride layer is mixed with graphite to form a composite layer, wherein the ratio of the silicon nitride layer is 95wt% to 85wt% and the ratio of the graphite is 5wt% to 15wt%.
10. A method for preparing a non-stick plastic container, characterized in that: The preparation method comprises: providing a substrate made of a plastic material; and A silicon nitride layer is formed on a surface of the substrate by magnetron sputtering.
11. A method for preparing a non-stick plastic container according to claim 10, characterized in that: The silicon nitride layer has a thickness of 0.01 um to 8 um.
12. A method for preparing a non-stick plastic container according to claim 10, characterized in that: The substrate is detachably arranged on a holding frame in a magnetron sputtering furnace. When the silicon nitride layer is formed by magnetron sputtering, the holding frame remains stationary.
13. A method for preparing a non-stick plastic container according to claim 10, characterized in that: The substrate is detachably arranged on a holding frame in a magnetron sputtering furnace. When the silicon nitride layer is formed by magnetron sputtering, the holding frame is rotated.
14. A method for preparing a non-stick plastic container, characterized in that: The preparation method comprises: Providing a substrate made of a plastic material; forming a dielectric layer on a surface of the substrate by magnetron sputtering; and A silicon nitride layer is formed on a surface of the dielectric layer by magnetron sputtering.
15. The method for preparing a non-stick plastic container according to claim 14, characterized in that: The dielectric layer is a zirconium dielectric layer, and a thickness of the zirconium dielectric layer is 0.01 um to 2 um.
16. The method for preparing a non-stick plastic container according to claim 14, characterized in that: The dielectric layer is a chromium dielectric layer, and a thickness of the chromium dielectric layer is 0.01 um to 2 um.
17. The method for preparing a non-stick plastic container according to claim 14, characterized in that: The dielectric layer is a titanium dielectric layer, and a thickness of the titanium dielectric layer is 0.01 um to 2 um.
18. The method for preparing a non-stick plastic container according to claim 14, characterized in that: The silicon nitride layer has a thickness of 0.01 um to 8 um.
19. The method for preparing a non-stick plastic container according to claim 14, characterized in that: The substrate is detachably arranged on a holding frame in a magnetron sputtering furnace. When the dielectric layer and the silicon nitride layer are formed by magnetron sputtering, the holding frame remains stationary.
20. The method for preparing a non-stick plastic container according to claim 14, characterized in that: The substrate is detachably arranged on a holding frame in a magnetron sputtering furnace. When the dielectric layer and the silicon nitride layer are formed by magnetron sputtering, the holding frame rotates.
21. The method for preparing non-stick plastic according to claim 14, characterized in that: The preparation method comprises: Providing a substrate made of a plastic material; forming a dielectric layer on a surface of the substrate by magnetron sputtering; and A composite layer of the silicon nitride layer and a graphite mixture is formed on a surface of the dielectric layer by magnetron sputtering.
Citation Information
Patent Citations
Wear-resistant anti-shoveling non-stick coating and manufacturing method thereof
CN115521671A
Nitriding corrosion-resistant non-stick inner pot
CN211354943U
Plastic container with barrier properties
JP2003104352A
Laminate with gas barrier film and method for manufacturing the same
JP2004114645A