Method for producing bridge steel plate with high efficiency and easy welding

By adopting top-bottom reblowing converter smelting, RH vacuum treatment and magnesium-aluminum wire magnesium treatment in bridge steel, combined with controlled cold-controlled rolling and tempering treatment, a specific metallographic structure is formed, and the low-temperature impact and welding performance of bridge steel are solved. The problem has significantly improved its low-temperature toughness and welding performance.

WO2024244268A1PCT designated stage expired Publication Date: 2024-12-05NANJING IRON & STEEL CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/126966
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-31
Filing Date
2023-10-27
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

The prior art is difficult to meet the requirements of low-temperature impact performance and welding performance while ensuring the strength of bridge steel. In particular, the requirements of ultra-thick bridge steel with low-temperature impact performance reaching more than 120J at -40℃, and the processing performance and welding performance are insufficient.

Method used

The top-bottom reblowing converter is used to smelve and iron boron and deoxygenation, combined with RH vacuum treatment and magnesium aluminum wire magnesium treatment, refining and casting, and the cold-controlled rolling process and tempering treatment are used to control chemical composition and metallographic phase. The tissue is constructed using weak-cold models and dynamic light pressure casting to avoid electromagnetic stirring and ultra-fast cooling to form a mixed tissue of granular bainite and acupuncture ferrite.

Benefits of technology

Improve the low-temperature toughness and welding performance of bridge steel plates, ensure the stability of strength and processing performance, inhibit the migration of austenite grain boundaries through the complexing of trace B and Nb and Ti, boron element promotes the nucleation of acupuncture ferrite, and magnesium Metallurgy refines the structure, high-temperature heating process promotes solid solution and precipitation, and improves welding and mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023126966_05122024_PF_FP_ABST
    Figure CN2023126966_05122024_PF_FP_ABST
Patent Text Reader

Abstract

A method for producing a bridge steel plate with high efficiency and easy welding, relating to the technical field of steel production, the chemical composition and mass percentage of the steel plate are as follows: C: 0.05% to 0.15%, Si: 0.10% to 0.50%, Mn: 0.90% to 1.70%, P≤0.020%, S≤0.010%, Nb: 0.010% to 0.090%, V≤0.03%, Ti: 0.008% to 0.030%, Cr≤0.30%, Ni≤0.30%, Mo≤0.20%, Cu≤0.30%, B: 0.0005% to 0.0020%, Mg: 0.0008% to 0.0015%, Al: 0.015% to 0.030%, and the balance is Fe and unavoidable impurities. By adopting smelting and rolling processes, a structure type mainly composed of granular bainite + ferrite + pearlite / acicular ferrite + granular bainite is obtained, constituting a bridge steel that meets the requirements of high efficiency and easy welding performance.
Need to check novelty before this filing date? Find Prior Art

Description

A method for producing high-efficiency and easy-to-weld bridge steel plates Technical Field

[0001] The present invention relates to the technical field of steel production, and in particular to a method for producing a high-efficiency and easily weldable bridge steel plate. Background Art

[0002] With the rapid development of my country's economy, infrastructure construction has been vigorously developed, among which the bridge industry has developed with each passing day. With the continuous improvement of bridge quality, heavy load, high speed and large span have become the main development directions. The new generation of high-performance bridge steel that integrates high strength, high toughness, low yield ratio, easy welding and other properties is the preferred material for key components of large-span and heavy-load railway steel bridges. The demand is clear and urgent.

[0003] The continuous improvement of bridge quality requires a qualitative change in steel quality. This is especially true for extra-thick bridge steel, which requires achieving a low-temperature impact resistance of 120J or higher at -40°C while maintaining strength. This is particularly challenging, as the steel plate's processing and weldability must also be considered. Therefore, developing efficient and easy-to-weld bridge products is crucial to the company's continued success.

[0004] Summary of the Invention

[0005] The present invention addresses the above technical problems, overcomes the shortcomings of the prior art, and provides a method for producing bridge steel plates that are highly efficient and easy to weld, comprising the following steps:

[0006] S1. Smelting: Top and bottom combined blown converter is used for smelting. Boron iron is added during the tapping process and deoxidation and alloying treatment is carried out. The molten steel is sent to LF for refining, deoxidation and slag alloying are carried out, and RH vacuum treatment is adopted with a vacuum degree of ≤3.0mbar. After the vacuum is completed, magnesium treatment is carried out using magnesium aluminum wire. After magnesium treatment, static stirring is carried out for 15 to 20 minutes.

[0007] S2. Casting: The refined molten steel is sent to the continuous casting for casting. The casting superheat is 15 to 35 degrees. No electromagnetic stirring is used. A weak cooling model is used for casting. Dynamic soft pressure is used. After the billet is cut, it is pile-cooled and surface inspected.

[0008] S3. Rolling: After surface inspection, the billet is sent to the heating furnace for heating at a temperature of 1200±50 degrees. The controlled cooling and controlled rolling process is adopted to ensure that the final rough rolling reduction rate is ≥20%. Ultra-fast cooling is used for cooling at a temperature of 450-650 degrees.

[0009] S4. Heat treatment: The steel plate is tempered at a temperature of 450 to 550 degrees and a holding time of 30 to 50 minutes. After heat treatment, the steel plate is sampled, inspected, marked, and put into storage for shipment.

[0010] The technical solution further defined in the present invention is:

[0011] The above-mentioned method for producing an efficient and easy-to-weld bridge steel plate has the following chemical composition and mass percentage: C: 0.05%~0.15%, Si: 0.10%~0.50%, Mn: 0.90%~1.70%, P≤0.020%, S≤0.010%, Nb: 0.010%~0.090%, V≤0.03%, Ti: 0.008%~0.030%, Cr≤0.30%, Ni≤0.30%, Mo≤0.20%, Cu≤0.30%, B: 0.0005%~0.0020%, Mg: 0.0008%~0.0015%, Al: 0.015%~0.030%, and the balance is Fe and unavoidable impurities.

[0012] The above-mentioned method for producing an efficient and easy-to-weld bridge steel plate has the following chemical composition and mass percentage: C: 0.09%~0.13%, Si: 0.20%~0.30%, Mn: 1.10%~1.50%, P≤0.013%, S≤0.006%, Nb: 0.020%~0.050%, V≤0.03%, Ti: 0.010%~0.020%, Cr: 0.10%~0.30%, Ni: 0.10%~0.30%, Mo: 0.08%~0.20%, Cu: 0.10%~0.30%, B: 0.0010%~0.0012%, Mg: 0.0010%~0.0013%, Al: 0.018%~0.020%, and the balance is Fe and unavoidable impurities.

[0013] The aforementioned method for producing an efficient and easy-to-weld bridge steel plate has a metallographic structure of granular bainite + ferrite + pearlite for steel grades Q345 to Q370 MPa, and a mixed structure of acicular ferrite + granular bainite for steel grades Q420 to Q550 MPa.

[0014] The above-mentioned method for producing a highly efficient and easily weldable bridge steel plate has a steel plate specification of 5 to 50 mm.

[0015] The beneficial effects of the present invention are:

[0016] (1) The carbon and manganese content design in the present invention can ensure the stability of product strength, while the lower carbon content can ensure the stability of ferrite content; Nb and Ti can refine the grain size of the structure, and at the same time, in the high temperature stage, carbonitride particles pin the original austenite grain boundary; trace B can be segregated at the original austenite grain boundary to play a solid solution dragging role, slowing down the migration of austenite grain boundaries, and the composite effect of Nb, B, and Ti microalloying elements inhibits the growth of austenite grain boundaries, thereby improving welding performance; the use of boron combines with N to form BN during the welding heat cycle cooling process, and precipitates on the surface of Ti (C, N) particles to form micron-sized particles, promoting the nucleation of acicular ferrite, significantly refining the M / A component, and improving low-temperature toughness;

[0017] (2) In the present invention, the boron element is added during the converter smelting process, which is conducive to the uniform distribution of the boron element in the molten steel. The high superheat and low cooling model smelting is adopted, which can promote the boron element to be fully dissolved in the ferrite during the casting process. Without using electromagnetic stirring technology, a large number of columnar crystals can be produced. During the rolling process, the columnar crystals are broken, which promotes the precipitation of the boron element, enhances the strength improvement of the boron element, and also promotes the production of boron composite inclusions, thereby improving the welding performance;

[0018] (3) The present invention adopts magnesium metallurgy technology, which effectively refines the grain size of the structure and promotes the formation of complex compounds of boron elements, avoiding the secondary oxidation of intergranular elements. At the same time, it absorbs oxygen elements in the welding process, improves the mechanical properties of boron elements, and avoids the adverse effects of single elements on the welding effect during the welding process. At the same time, the application of magnesium metallurgy technology weakens the adverse effects of manganese sulfide inclusions, improves the core quality of the ingot, and improves the adverse effects of not using electromagnetic stirring technology;

[0019] (4) The present invention adopts a high-temperature heating process, which can promote the full solid solution of boron, chromium, molybdenum, and copper elements, reduce the aggregation of intergranular elements, and strengthen the mechanical properties through precipitation during the rolling process. The high temperature increases the amount of carbon, nitrogen, and oxides produced by these elements, thereby strengthening the strength and reducing the adverse effects of welding;

[0020] (5) The present invention adopts a high-temperature tempering process, which can improve the internal stress of the steel plates of bridge steels of different strengths and enhance the secondary processing performance of the product. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] FIG1 is a metallographic structure diagram of a steel plate according to the present invention. DETAILED DESCRIPTION

[0022] Example 1

[0023] This embodiment provides a method for producing an efficient and easy-to-weld bridge steel plate, wherein the chemical composition and mass percentage of the steel plate are as follows: C: 0.013%, Si: 0.33%, Mn: 1.32%, P: 0.009%, S: 0.003%, Nb: 0.039%, V: 0.002%, Ti: 0.015%, Cr: 0.03%, Ni: 0.030%, Mo: 0:0050%, Cu: 0.030%, B: 0.0017%, Mg: 0.0011%, Al: 0.023%, and the remainder is Fe and unavoidable impurities.

[0024] Production includes the following steps:

[0025] S1. Smelting: The molten steel is smelted in a top-bottom combined-blowing converter. Boron iron is added during the tapping process and deoxidation and alloying treatment is performed. The molten steel is sent to LF for refining, deoxidation and slag formation, and alloy proportioning is refined. RH vacuum treatment is used with a vacuum degree of 1.3 mbar. After the vacuum is completed, magnesium treatment is performed using a magnesium-aluminum wire. After magnesium treatment, static stirring is performed for 19 minutes.

[0026] S2. Casting: The refined molten steel is sent to the continuous casting for casting. The casting superheat is 33 degrees. No electromagnetic stirring is used. A weak cooling model is used for casting. Dynamic soft pressure is used. After the billet is cut, it is pile-cooled and surface inspected.

[0027] S3, rolling: the billet after surface inspection is sent to the heating furnace for heating, the heating temperature is 1236 degrees, the controlled cooling and controlled rolling process is adopted, the final rough rolling reduction rate is 21%, and the ultra-fast cooling is adopted for cooling, the cooling temperature is 490 degrees;

[0028] S4. Heat treatment: The steel plate is tempered at a temperature of 480 degrees and a holding time of 35 minutes. After heat treatment, the steel plate is sampled, inspected, marked, and put into storage for shipment.

[0029] This embodiment provides a method for producing an efficient and easy-to-weld bridge steel plate, wherein the chemical composition and mass percentage of the steel plate are as follows: C: 0.09%, Si: 0.33%, Mn: 1.38%, P: 0.011%, S: 0.003%, Nb: 0.029%, V: 0.001%, Ti: 0.011%, Cr: 0.02%, Ni: 0.01%, Mo: 0.003%, Cu: 0.02%, B: 0.0009%, Mg: 0.0013%, Al: 0.022%, and the remainder is Fe and unavoidable impurities.

[0030] Production includes the following steps:

[0031] S1. Smelting: The molten steel is smelted in a top-bottom combined-blowing converter. Boron iron is added during the tapping process and deoxidation and alloying treatment is performed. The molten steel is sent to LF for refining, deoxidation and slag alloying are carried out, and RH vacuum treatment is adopted with a vacuum degree of 1.6 mbar. After the vacuum is completed, magnesium treatment is performed using a magnesium-aluminum wire. After magnesium treatment, static stirring is performed for 17 minutes.

[0032] S2. Casting: The refined molten steel is sent to the continuous casting for casting. The casting superheat is 19 degrees. No electromagnetic stirring is used. A weak cooling model is used for casting. Dynamic soft pressure is used. After the billet is cut, it is pile-cooled and surface inspected.

[0033] S3, rolling: the billet after surface inspection is sent to the heating furnace for heating, the heating temperature is 1263 degrees, the controlled cooling and controlled rolling process is adopted to ensure that the final rough rolling reduction rate is 22%, and the ultra-fast cooling is used for cooling, the cooling temperature is 610 degrees;

[0034] S4. Heat treatment: The steel plate is tempered at a temperature of 520 degrees and a holding time of 45 minutes. After heat treatment, the steel plate is sampled, inspected, marked, and put into storage for shipment.

[0035] Example 3

[0036] This embodiment provides a method for producing an efficient and easy-to-weld bridge steel plate, wherein the chemical composition and mass percentage of the steel plate are as follows: C: 0.10%, Si: 0.31%, Mn: 1.62%, P: 0.017%, S: 0.009%, Nb: 0.044%, V: 0.003%, Ti: 0.019%, Cr: 0.03%, Ni: 0.03%, Mo: 0.001%, Cu: 0.030%, B: 0.0017%, Mg: 0.0012%, Al: 0.026%, and the remainder is Fe and unavoidable impurities.

[0037] Production includes the following steps:

[0038] S1. Smelting: The molten steel is smelted in a top-bottom combined-blowing converter. Boron iron is added during the tapping process and deoxidation and alloying treatment is performed. The molten steel is sent to LF for refining, deoxidation and slag are refined, and the alloy ratio is refined. RH vacuum treatment is used with a vacuum degree of 1.0 mbar. After the vacuum is completed, magnesium treatment is performed using a magnesium-aluminum wire. After magnesium treatment, static stirring is performed for 18 minutes.

[0039] S2. Casting: The refined molten steel is sent to the continuous casting for casting. The casting superheat is 26 degrees. No electromagnetic stirring is used. A weak cooling model is used for casting. Dynamic soft pressure is used. After the billet is cut, it is pile-cooled and surface inspected.

[0040] S3, rolling: the billet after surface inspection is sent to the heating furnace for heating at 1160 degrees. The controlled cooling and controlled rolling process is adopted. The final rough rolling reduction rate is 21%. The ultra-fast cooling is adopted for cooling at 580 degrees.

[0041] S4. Heat treatment: The steel plate is tempered at a temperature of 490 degrees and a holding time of 48 minutes. After heat treatment, the steel plate is sampled, inspected, marked, and put into storage for shipment.

[0042] The properties of the steel plates of Examples 1, 2, and 3 are as follows:

[0043] Table 1 Tensile strength and impact test

[0044] In addition to the above embodiments, the present invention may also have other implementations. Any technical solution formed by equivalent replacement or equivalent transformation falls within the scope of protection required by the present invention.

Claims

1. A method for producing a highly efficient and easily weldable bridge steel plate, characterized in that: The following steps are involved: S1. Smelting: The top and bottom combined blowing converter is used for smelting. Boron iron is added during the steelmaking process and deoxidation and alloying treatment is performed; The molten steel is sent to LF for refining, deoxidation and slag making, and alloy fine proportioning is carried out. RH vacuum treatment is adopted, and the vacuum degree is ≤3.0mbar. After the vacuum is finished, magnesium treatment is carried out with magnesium-aluminum wire, and static stirring is carried out for 15-20min after magnesium treatment; S2. Casting: The refined molten steel is sent to continuous casting for casting. The casting superheat is 15 to 35 degrees. No electromagnetic stirring is used. A weak cooling model is used for casting. Dynamic light pressure is used. After the ingot is cut, it is piled and cooled and inspected. S3, rolling: the billet after surface inspection is sent to the heating furnace for heating, the heating temperature is 1200±50 degrees, the controlled cooling and controlled rolling process is adopted to ensure that the final rough rolling reduction rate is ≥20%, and the ultra-fast cooling is adopted for cooling, and the cooling temperature is 450~650 degrees; S4. Heat treatment: The steel plate is tempered at a temperature of 450 to 550 degrees and a holding time of 30 to 50 minutes. After heat treatment, the steel plate is sampled, inspected, marked, put into storage and shipped.

2. The method for producing a high-efficiency and easy-to-weld bridge steel plate according to claim 1, characterized in that: The chemical composition and mass percentage of the steel plate are as follows: C: 0.05% ~ 0.15%, Si: 0.10% ~ 0.50%, Mn: 0.90% ~ 1.70%, P ≤ 0.020%, S ≤ 0.010%, Nb: 0.010% ~ 0.090%, V ≤ 0.03%, Ti: 0.008% ~ 0.030%, Cr ≤ 0.30%, Ni ≤ 0.30%, Mo ≤ 0.20%, Cu ≤ 0.30%, B: 0.0005% ~ 0.0020%, Mg: 0.0008% ~ 0.0015%, Al: 0.015% ~ 0.030%, and the balance is Fe and unavoidable impurities.

3. The method for producing a high-efficiency and easy-to-weld bridge steel plate according to claim 2, characterized in that: The chemical composition and mass percentage of the steel plate are as follows: C: 0.09% ~ 0.13%, Si: 0.20% ~ 0.30%, Mn: 1.10% ~ 1.50%, P ≤ 0.013%, S ≤ 0.006%, Nb: 0.020% ~ 0.050%, V ≤ 0.03%, Ti: 0.010% ~ 0.020%, Cr: 0.10% ~ 0.30%, Ni: 0.10% ~ 0.30%, Mo: 0.08% ~ 0.20%, Cu: 0.10% ~ 0.30%, B: 0.0010% ~ 0.0012%, Mg: 0.0010% ~ 0.0013%, Al: 0.018% ~ 0.020%, and the balance is Fe and unavoidable impurities.

4. The method for producing a high-efficiency and easy-to-weld bridge steel plate according to claim 1, characterized in that: The metallographic structure of steel plates with steel grades of Q345 to Q370 MPa is granular bainite + ferrite + pearlite, and the metallographic structure of steel plates with steel grades of Q420 to Q550 MPa is a mixed structure of acicular ferrite + granular bainite.

5. The method for producing a high-efficiency and easy-to-weld bridge steel plate according to claim 1, characterized in that: The steel plate specifications are 5 to 50 mm.

Citation Information

Patent Citations

  • Method for producing boron steel by converter

    CN101503746A

  • Low-cost production method of boracic low-alloy-structured steel sheet billet

    CN103695600A

  • Heavy-gauge 420MPa-class low-yield-ratio low-temperature bridge steel and production method

    CN108998726A

  • Method for producing extremely low-cost boron-containing thin-gauge export alloy steel

    CN111778448A

  • 500MPa-grade weather-resistant bridge steel and manufacturing method thereof

    CN113025880A