Negative electrode sheet, battery, and electrical apparatus
By adopting a multi-layer structure and blind hole design in the negative electrode sheet of lithium-ion battery, combined with the use of natural graphite and artificial graphite, the problem of high cost of negative electrode materials is solved, and high energy density and fast charging capabilities are achieved.
Patent Information
- Application Number
- PCT/CN2024/071661
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-31
- Filing Date
- 2024-01-10
- Publication Date
- 2024-12-05
AI Technical Summary
It is difficult to balance the high energy density and fast charging capability of lithium-ion battery negative electrode materials and cost. Although artificial graphite has superior performance, it is costly.
The negative electrode sheet is adopted to include natural graphite and artificial graphite in sequence from the inside to the outside, and the efficiency of lithium embedded channels is improved through blind hole design, and chemical and physical pore making technology are combined to reduce costs.
It achieves a reduction in the cost of negative electrode materials while maintaining high energy density and fast charging capabilities, and achieves a balance between performance and economy.
Smart Images

Figure CN2024071661_05122024_PF_FP_ABST
Abstract
Description
Negative electrode, battery and electrical device
[0001] Cross-references
[0002] This application refers to Chinese patent application No. 202310638513.4, entitled “Negative Electrode Sheet and Lithium-ion Battery” filed on May 31, 2023, which is incorporated into this application in its entirety by reference. Technical Field
[0003] The present disclosure relates to the technical field of lithium-ion batteries, and in particular to a negative electrode plate, a battery, and an electrical device. Background Art
[0004] Lithium-ion batteries are a new type of green power source with the advantages of high energy, high battery voltage, wide operating temperature range, long storage life, and no memory effect. They have been widely used in military and civilian small appliances, as well as pure electric and hybrid new energy vehicles.
[0005] In some cases, artificial graphite is usually required as the active material for the negative electrode of lithium-ion batteries because it has advantages over natural graphite such as more balanced performance, better cycle performance, and better compatibility with the electrolyte. It is more conducive to obtaining high energy density and high fast charging capability, but it also inevitably leads to the defect of high cost.
[0006] Therefore, how to reduce the manufacturing cost of the negative electrode while maintaining high energy density and high fast charging capability has become an important issue that needs to be solved urgently.
[0007] Summary of the Invention
[0008] The present disclosure is made in view of the above-mentioned technical problems, and its purpose is to provide a negative electrode plate that uses both artificial graphite and natural graphite as negative electrode active materials to achieve a good balance between maintaining high energy density, high fast charging capability and controlling costs.
[0009] To this end, a first aspect of the present disclosure provides a negative electrode sheet, comprising:
[0010] a current collector; and
[0011] forming a negative electrode active material layer on the current collector;
[0012] Among them, the negative electrode active material layer includes at least two negative electrode active material layers from the inside to the outside, the negative electrode active material layer includes a negative electrode active material selected from natural graphite or artificial graphite, and the at least two negative electrode active material layers include at least one negative electrode active material layer containing natural graphite and at least one negative electrode active material layer containing artificial graphite.
[0013] The negative electrode active material layer formed on the current collector includes the case where the negative electrode active material layer is directly disposed on the current collector, and also includes the case where the negative electrode active material layer is indirectly disposed on the current collector, for example, other layers are disposed directly between the negative electrode active material layer and the current collector.
[0014] By introducing both natural graphite and artificial graphite into the negative electrode active material layer, the advantages of high energy density of artificial graphite and low cost of natural graphite can be taken into account, thereby achieving a compromise performance balance.
[0015] In any embodiment, the negative electrode active material layer includes a first negative electrode active material layer and a second negative electrode active material layer from the inside to the outside, the negative electrode active material in the first negative electrode active material layer includes natural graphite, and the negative electrode active material in the second negative electrode active material layer includes artificial graphite.
[0016] In any embodiment, one or more blind holes are provided in the first negative electrode active material layer, and the openings of the blind holes are located outside the first negative electrode active material layer, that is, the openings of the blind holes are provided on the side of the first negative electrode active material layer away from the current collector.
[0017] By setting blind holes in the first negative electrode active material layer, the artificial graphite in the second negative electrode active layer can penetrate into the first negative electrode active material layer, thereby forming an efficient lithium insertion channel and improving the fast charging capability.
[0018] In any embodiment, the depth of the blind hole is 1-80% of the thickness of the first negative electrode active material layer, preferably 10-70%, exemplarily 20-60%; and / or
[0019] The blind hole has a diameter of 20-300 μm, illustratively 80-150 μm; and / or
[0020] The spacing between the blind holes is 100-1000 μm, exemplarily 400-500 μm; and / or
[0021] The blind hole formation rate is 0.1%-10%, and illustratively 2%-4%.
[0022] In any embodiment, the blind holes are evenly distributed.
[0023] In any embodiment, the thickness of the first negative electrode active material layer is 10-200 μm, illustratively 50-100 μm.
[0024] In any embodiment, the thickness of the second negative electrode active material layer is 10-200 μm, and illustratively 50-100 μm.
[0025] In any embodiment, the thickness of the first negative electrode active material layer is greater than the thickness of the second negative electrode active material layer.
[0026] In any embodiment, the natural graphite has a median particle size of 5-20 μm; and / or
[0027] The median particle size of artificial graphite is 5-20 μm.
[0028] In any embodiment, the negative electrode active material layer includes, from the inside to the outside, a first negative electrode active material layer, a second negative electrode active material layer and a third negative electrode active material layer, the negative electrode active material in the first negative electrode active material layer includes artificial graphite, the negative electrode active material in the second negative electrode active material layer includes natural graphite, and the negative electrode active material in the third negative electrode active material layer includes artificial graphite.
[0029] In any embodiment, one or more blind holes are provided in the system consisting of the first negative electrode active material layer and the second negative electrode active material layer, and the opening of the blind hole is located outside the second negative electrode active material layer, that is, the opening of the blind hole is provided on the side of the second negative electrode active material layer away from the current collector.
[0030] By setting blind holes in the system consisting of the first negative electrode active material layer and the second negative electrode active material layer, the artificial graphite in the third negative electrode active layer can penetrate into the first negative electrode active material layer and the second negative electrode active material layer, thereby forming an efficient lithium insertion channel, connecting the innermost layer and the outermost layer, and improving the fast charging capability.
[0031] In any embodiment, the depth of the blind hole is 1-80%, exemplarily 10-70%, exemplarily 30-60%, of the thickness of the second negative electrode active material layer plus the thickness of the first negative electrode active material layer; and / or
[0032] The blind hole has a diameter of 20-500 μm, exemplarily 100-150 μm; and / or
[0033] The spacing between the blind holes is 100-1500 μm, exemplarily 400-500 μm; and / or
[0034] The blind hole formation rate is 0.1%-10%, and illustratively 2%-4%.
[0035] In any embodiment, the blind holes are evenly distributed.
[0036] In any embodiment, the thickness of the first negative electrode active material layer is 10-100 μm, illustratively 60-100 μm.
[0037] In any embodiment, the thickness of the second negative electrode active material layer is 10-200 μm, and illustratively 60-100 μm.
[0038] In any embodiment, the thickness of the third negative electrode active material layer is 10-100 μm, and illustratively is 20-40 μm.
[0039] In any embodiment, the thickness of the second negative electrode active material layer is greater than the thickness of the first negative electrode active material layer and / or the third negative electrode active material layer.
[0040] In any embodiment, the median particle size of the artificial graphite in the negative electrode active material of the first negative electrode active material layer is 5-20 μm; and / or
[0041] The median particle size of natural graphite in the negative electrode active material of the second negative electrode active material layer is 5-20 μm; and / or
[0042] The median particle size of the artificial graphite in the negative electrode active material of the third negative electrode active material layer is 5 to 20 μm.
[0043] A second aspect of the present disclosure provides a method for preparing a negative electrode sheet, comprising:
[0044] At least two negative electrode slurries containing negative electrode active materials are stacked and coated on a current collector and dried to obtain a negative electrode sheet;
[0045] The negative electrode active material is selected from natural graphite or artificial graphite, and the at least two negative electrode slurries containing the negative electrode active material include at least one negative electrode slurry containing natural graphite and at least one negative electrode slurry containing artificial graphite.
[0046] In any embodiment, the method comprises:
[0047] coating a first negative electrode slurry containing a negative electrode active material on a current collector and drying the slurry to form a first negative electrode active material layer, wherein the negative electrode active material includes natural graphite; and
[0048] coating a second negative electrode slurry containing a negative electrode active material on the first negative electrode active material layer and drying the slurry to form a second negative electrode active material layer, wherein the negative electrode active material includes artificial graphite;
[0049] To obtain the negative electrode.
[0050] In any embodiment, the method comprises:
[0051] Coating a first negative electrode slurry containing a negative electrode active material and a chemical pore former on a current collector, drying the slurry, and forming pores to form a first negative electrode active material layer containing one or more blind holes, wherein the negative electrode active material comprises natural graphite, and the openings of the blind holes are located outside the first negative electrode active material layer; and
[0052] coating a second negative electrode slurry containing a negative electrode active material on the first negative electrode active material layer and drying the slurry to form a second negative electrode active material layer, wherein the negative electrode active material includes artificial graphite;
[0053] To obtain the negative electrode.
[0054] In any embodiment, the method comprises:
[0055] coating a first negative electrode slurry containing a negative electrode active material on a current collector and drying the slurry to form a first negative electrode active material layer, wherein the negative electrode active material includes natural graphite;
[0056] Physically forming pores in the first negative electrode active material layer to form a first negative electrode active material layer containing one or more blind holes, wherein the openings of the blind holes are located outside the first negative electrode active material layer; and
[0057] coating a second negative electrode slurry containing a negative electrode active material on the first negative electrode active material layer containing one or more blind holes and drying the slurry to form a second negative electrode active material layer, wherein the negative electrode active material includes artificial graphite;
[0058] To obtain the negative electrode.
[0059] In any embodiment, the depth of the blind hole is 1-80% of the thickness of the first negative electrode active material layer, exemplarily 10-70%, exemplarily 20-60%; and / or
[0060] The blind hole has a diameter of 20-300 μm, illustratively 80-150 μm; and / or
[0061] The spacing between the blind holes is 100-1000 μm, exemplarily 400-500 μm and / or
[0062] The blind hole formation rate is 0.1%-10%, and illustratively 2%-4%.
[0063] In any embodiment, the blind holes are evenly distributed.
[0064] In any embodiment, the thickness of the first negative electrode active material layer is 10-200 μm, illustratively 50-100 μm.
[0065] In any embodiment, the thickness of the second negative electrode active material layer is 10-200 μm, and illustratively 50-100 μm.
[0066] In any embodiment, the natural graphite has a median particle size of 5-20 μm; and / or
[0067] The median particle size of artificial graphite is 5-20 μm.
[0068] In any embodiment, the method comprises:
[0069] coating a first negative electrode slurry containing a negative electrode active material on a current collector and drying the slurry to form a first negative electrode active material layer, wherein the negative electrode active material comprises artificial graphite;
[0070] coating a second negative electrode slurry containing a negative electrode active material on the first negative electrode active material layer and drying the slurry to form a second negative electrode active material layer, wherein the negative electrode active material includes natural graphite; and
[0071] coating a third negative electrode slurry containing a negative electrode active material on the second negative electrode active material layer and drying the slurry to form a third negative electrode active material layer, wherein the negative electrode active material includes artificial graphite;
[0072] To obtain the negative electrode.
[0073] In any embodiment, the method comprises:
[0074] coating a first negative electrode slurry containing a negative electrode active material and a chemical pore former on a current collector and semi-drying the slurry at low temperature to form a semi-dried first negative electrode active material layer, wherein the negative electrode active material comprises artificial graphite;
[0075] Coating a second negative electrode slurry containing a negative electrode active material on the semi-dried first negative electrode active material layer, drying at a high temperature, and forming pores to form a second negative electrode active material layer and forming one or more blind holes in a system consisting of the first negative electrode active material layer and the second negative electrode active material layer, wherein the negative electrode active material includes natural graphite, and the openings of the blind holes are located outside the second negative electrode active material layer; and
[0076] coating a third negative electrode slurry containing a negative electrode active material on the second negative electrode active material layer and drying the slurry to form a third negative electrode active material layer, wherein the negative electrode active material includes artificial graphite;
[0077] To obtain the negative electrode.
[0078] In any embodiment, the method comprises:
[0079] coating a first negative electrode slurry containing a negative electrode active material on a current collector and drying the slurry to form a first negative electrode active material layer, wherein the negative electrode active material comprises artificial graphite;
[0080] coating a second negative electrode slurry containing a negative electrode active material on the first negative electrode active material layer and drying the slurry to form a second negative electrode active material layer, wherein the negative electrode active material includes natural graphite;
[0081] Physically creating pores in a system consisting of the first negative electrode active material layer and the second negative electrode active material layer to form one or more blind holes, wherein the openings of the blind holes are located outside the second negative electrode active material layer; and
[0082] coating a third negative electrode slurry containing a negative electrode active material on the second negative electrode active material layer and drying the slurry to form a third negative electrode active material layer, wherein the negative electrode active material includes artificial graphite;
[0083] To obtain the negative electrode.
[0084] In any embodiment, the depth of the blind hole is 1-80%, exemplarily 10-70%, exemplarily 30-60%, of the thickness of the second negative electrode active material layer plus the thickness of the first negative electrode active material layer; and / or
[0085] The blind hole has a diameter of 20-500 μm, exemplarily 100-150 μm; and / or
[0086] The spacing between the blind holes is 100-1500 μm, exemplarily 400-500 μm; and / or
[0087] The blind hole formation rate is 0.1%-10%, and illustratively 2%-4%.
[0088] In any embodiment, the blind holes are evenly distributed.
[0089] In any embodiment, the thickness of the first negative electrode active material layer is 10-100 μm, illustratively 60-100 μm.
[0090] In any embodiment, the thickness of the second negative electrode active material layer is 10-200 μm, and illustratively 60-100 μm.
[0091] In any embodiment, the thickness of the third negative electrode active material layer is 10-100 μm, illustratively 20-40 μm.
[0092] In any embodiment, the median particle size of the artificial graphite in the negative electrode active material of the first negative electrode active material layer is 5-20 μm; and / or
[0093] The median particle size of natural graphite in the negative electrode active material of the second negative electrode active material layer is 5-20 μm; and / or
[0094] The median particle size of the artificial graphite in the negative electrode active material of the third negative electrode active material layer is 5 to 20 μm.
[0095] The third aspect of the present disclosure provides a lithium-ion battery comprising the negative electrode sheet according to the first aspect or the negative electrode sheet prepared by the method according to the second aspect. Typically, the lithium-ion battery in the present disclosure includes a battery cell, a battery module, a battery pack, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0096] In the accompanying drawings, unless otherwise specified, the same reference numerals throughout the multiple drawings represent the same or similar parts or elements. These drawings are not necessarily drawn to scale. It should be understood that these drawings only depict some embodiments disclosed in the present application and should not be regarded as limiting the scope of the present application. In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments of the present application will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For those of ordinary skill in the art, other drawings can be obtained based on the drawings without paying creative work.
[0097] FIG1 is a schematic diagram of pore formation in the method of Example 1 of the present disclosure, wherein the meanings of the respective reference numerals are as follows: 101 : current collector; 105 : second negative electrode active material layer; 106 : first negative electrode active material layer; 107 : blind hole; 108 : third negative electrode active material.
[0098] FIG2 is a schematic diagram of pore formation in the method of Example 4 of the present disclosure, wherein the meanings of the reference numerals are as follows: 101: current collector; 102: first negative electrode active material layer; 103: blind hole; 104: blind hole channel. DETAILED DESCRIPTION
[0099] Hereinafter, the negative electrode sheet, the method for preparing the same, and the embodiment of the lithium-ion battery containing the negative electrode sheet disclosed herein will be described in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there may be cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present disclosure and are not intended to limit the subject matter described in the claims.
[0100] " scope " in the present disclosure is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and selected lower limit and upper limit define the boundary of special scope.The scope that this mode limits can be to include end value or not include end value, and can be combined arbitrarily, and promptly any lower limit can form a scope with any 2 limit combinations.For example, if the scope of 60-120 and 80-110 is listed for specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected.In addition, if the minimum range value 1 and 2 listed, and if the maximum range value 3,4 and 5 listed, then the following scope can all be expected: 1-3,1-4,1-5,2-3,2-4 and 2-5.In the present disclosure, unless otherwise specified, numerical range " ab " represents the abbreviation of any real number combination between a and b, and wherein a and b are all real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is merely an abbreviation for these numerical combinations. In some exemplary embodiments, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0101] Unless otherwise specified, all embodiments and optional embodiments of the present disclosure can be combined with each other to form new technical solutions.
[0102] Unless otherwise specified, all steps of the present disclosure may be performed sequentially or randomly, and illustratively may be performed sequentially. For example, a method comprising steps (a) and (b) indicates that the method may comprise steps (a) and (b) performed sequentially, or may comprise steps (b) and (a) performed sequentially. For example, a method further comprising step (c) indicates that step (c) may be added to the method in any order, for example, the method may comprise steps (a), (b), and (c), or may comprise steps (a), (c), and (b), or may comprise steps (c), (a), and (b), etc.
[0103] Unless otherwise stated, the words “comprises,” “includes,” “has,” “contains” or any other variations thereof mentioned in this disclosure are intended to cover a non-exclusive inclusion.
[0104] Unless otherwise specified, the term "or" is inclusive in this disclosure. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0105] Unless otherwise specified, the indefinite articles "a" and "an" before an element or component in the present disclosure do not limit the quantity requirement (i.e., the number of times the element or component appears). Therefore, "a" or "an" should be interpreted as including one or at least one, and elements or components in the singular also include plural forms, unless the number is obviously intended to limit the singular form.
[0106] In some exemplary embodiments, a number of expressions will be referred to in the following description, and these expressions are defined to have the following meanings.
[0107] The term "negative electrode" refers to the electrode in the battery that has a lower potential and undergoes oxidation reaction.
[0108] The term "current collector" refers to any conductive substrate capable of conducting electrical current to an electrode during discharge or charge of a lithium-ion battery.
[0109] The term "negative electrode active material" refers to an active material that can insert (also called "dope") lithium.
[0110] The term "natural graphite" refers to graphite that occurs naturally in nature.
[0111] The term "synthetic graphite" refers to graphite that is produced or processed synthetically.
[0112] The term "from inside to outside" refers to the current collector being the inner layer and extending outward.
[0113] The term "blind via" refers to a via that connects a surface layer to an inner layer without penetrating the entire layer.
[0114] The term “a system consisting of the first negative electrode active material layer and the second negative electrode active material layer” means that the first negative electrode active material layer and the second negative electrode active material layer are regarded as one integral layer.
[0115] The term "pore formation ratio" refers to the ratio of the total volume of blind pores to the volume of the negative electrode active material layer.
[0116] The term "lithium-ion battery" refers to a type of rechargeable battery in which lithium ions move from the anode to the cathode during discharge and from the cathode to the anode during charge.
[0117] The term "median particle size" refers to D50, which is the particle size corresponding to the cumulative particle size distribution percentage of a sample reaching 50%. The median particle size in this disclosure is determined using a particle size analyzer-laser diffraction method. For details, please refer to the standard GB / T19077-2016.
[0118] Negative electrode
[0119] In order to at least partially solve one or more of the above problems and other potential problems, a first exemplary embodiment of the present disclosure provides a negative electrode sheet, comprising:
[0120] a current collector; and
[0121] forming a negative electrode active material layer on the current collector;
[0122] Among them, the negative electrode active material layer includes at least two negative electrode active material layers from the inside to the outside, the negative electrode active material layer includes a negative electrode active material selected from natural graphite or artificial graphite, and the at least two negative electrode active material layers include at least one negative electrode active material layer containing natural graphite and at least one negative electrode active material layer containing artificial graphite.
[0123] In some embodiments, the negative electrode active material layer includes a first negative electrode active material layer and a second negative electrode active material layer from the inside to the outside, the negative electrode active material in the first negative electrode active material layer includes natural graphite, and the negative electrode active material in the second negative electrode active material layer includes artificial graphite.
[0124] In some embodiments, one or more blind holes are provided in the first negative electrode active material layer, and the openings of the blind holes are located outside the first negative electrode active material layer.
[0125] In some embodiments, the depth of the blind hole is 1-80% or 10-70% or 20-60% of the thickness of the first negative electrode active material layer, for example, it can be specifically 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39%, 40%, 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49%, 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, 70%, 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79%, 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, 99%, 100%, 100%, 101%, 102%, 103%, 104%, 105%, 106%, 107%, 108%, 109%, 111 37%, 38%, 39%, 40%, 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49%, 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, 70%, 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79%, 80% or any value therebetween; and / or
[0126] The pore size of the blind hole is 20-300 μm or 80-150 μm, for example, it can be 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, 110 μm, 120 μm, 130 μm, 140 μm, 150 μm, 160 μm, 170 μm, 180 μm, 190 μm, 200 μm, 210 μm, 220 μm, 230 μm, 240 μm, 250 μm, 260 μm, 270 μm, 280 μm, 290 μm, 300 μm or any value in between; and / or
[0127] The spacing between the blind holes is 100-1000 μm or 400-500 μm, for example, it can be 100 μm, 110 μm, 120 μm, 130 μm, 140 μm, 150 μm, 160 μm, 170 μm, 180 μm, 190 μm, 200 μm, 210 μm, 220 μm, 230 μm, 240 μm, 250 μm, 260 μm, 270 μm, 280 μm, 290 μm, 300 μm, 310 μm, 320 μm, 330 μm, 340 μm, 350 μm, 360 μm, 370 μm, 380 μm, 390 μm. 5 70μm, 580μm, 590μm, 600μm, 610μm, 620μm, 630μm, 640μm, 650μm, 660μm, 670μm, 680μm, 690μm, 700μm, 710μm, 720μm, 730μm, 740μm, 750 μm, 760 μm, 770 μm, 780 μm, 790 μm, 800 μm, 810 μm, 820 μm, 830 μm, 840 μm, 850 μm, 860 μm, 870 μm, 880 μm, 890 μm, 900 μm, 910 μm, 920 μm, 930 μm, 940 μm, 950 μm, 960 μm, 970 μm, 980 μm, 990 μm, 1000 μm or any value therebetween; and / or
[0128] The porosity of the blind holes is 0.1%-10% or 2%-4%, for example, it can be 0.1%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10% or any value therebetween.
[0129] In some embodiments, the blind holes are evenly distributed.
[0130] There is no particular limitation on the thickness of the first negative electrode active material layer, and those commonly used in the art can be adopted. Typically, the thickness of the first negative electrode active material layer is 10-200 μm or 50-100 μm, for example, 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, 110 μm, 120 μm, 130 μm, 140 μm, 150 μm, 160 μm, 170 μm, 180 μm, 190 μm, 200 μm, or any value therebetween.
[0131] There is no particular limitation on the thickness of the second negative electrode active material layer, and those commonly used in the art can be adopted. Typically, the thickness of the second negative electrode active material layer is 10-200 μm or 50-100 μm, for example, 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, 110 μm, 120 μm, 130 μm, 140 μm, 150 μm, 160 μm, 170 μm, 180 μm, 190 μm, 200 μm, or any value therebetween.
[0132] For example, the thickness of the first negative electrode active material layer is greater than that of the second negative electrode active material layer. This configuration can better reduce costs.
[0133] There is no particular limitation on the particle size of the natural graphite, and those commonly used in the art can be used. Typically, the median particle size of the natural graphite is 5-20 μm, for example, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm, 18 μm, 19 μm, 20 μm, or any value therebetween.
[0134] There is no particular limitation on the particle size of the artificial graphite, and those commonly used in the art can be used. Typically, the median particle size of natural graphite is 5-20 μm, for example, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm, 18 μm, 19 μm, 20 μm, or any value therebetween.
[0135] There are no particular limitations on the composition of the first negative electrode active material layer and the second negative electrode active material layer, and those commonly used in the art may be used. Typically, the first negative electrode active material layer and the second negative electrode active material layer each include:
[0136] 90-97 wt % of the negative electrode active material, for example, 90 wt %, 91 wt %, 92 wt %, 93 wt %, 94 wt %, 95 wt %, 96 wt %, 97 wt %, or any value therebetween;
[0137] 1-5 wt % of a negative electrode conductive agent, for example, 1 wt %, 2 wt %, 3 wt %, 4 wt %, 5 wt % or any value therebetween;
[0138] 1-5 wt % of a negative electrode binder, for example, 1 wt %, 2 wt %, 3 wt %, 4 wt %, 5 wt % or any value therebetween; and
[0139] 1-3 wt % of a negative electrode thickener, for example, 1 wt %, 2 wt %, 3 wt % or any value therebetween;
[0140] The above weight percentages are based on the total weight of the negative electrode active material, the negative electrode conductive agent, the negative electrode binder and the negative electrode thickener.
[0141] As for the negative electrode active material, it is selected from natural graphite or artificial graphite.
[0142] There are no particular limitations on the negative electrode conductive agent, and any of those commonly used in the art may be used. Typically, the negative electrode conductive agent is selected from one or more of the following groups: conductive carbon black, carbon nanotubes, vapor-generated carbon fibers, Ketjen black, and graphene.
[0143] There is no particular limitation on the negative electrode binder, and any of those commonly used in the art may be used. Typically, the negative electrode binder is styrene-butadiene rubber and / or lithium polyacrylate.
[0144] There are no particular limitations on the negative electrode thickener, and those commonly used in the art may be used. Typically, the negative electrode thickener is selected from one or more of the following groups: sodium carboxymethylcellulose, polyvinylidene fluoride, lithium polyacrylate, and polyacrylonitrile.
[0145] In some embodiments, the negative electrode active material layer includes, from the inside to the outside, a first negative electrode active material layer, a second negative electrode active material layer, and a third negative electrode active material layer, the negative electrode active material in the first negative electrode active material layer includes artificial graphite, the negative electrode active material in the second negative electrode active material layer includes natural graphite, and the negative electrode active material in the third negative electrode active material layer includes artificial graphite.
[0146] In some embodiments, one or more blind holes are provided in the system consisting of the first negative electrode active material layer and the second negative electrode active material layer, and the openings of the blind holes are located outside the second negative electrode active material layer.
[0147] In some embodiments, the depth of the blind hole is 1-80% or 10-70% or 30-60% of the thickness of the second negative electrode active material layer plus the thickness of the first negative electrode active material layer, for example, it can be 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%. %, 48%, 49%, 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, 70%, 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79%, 80% or any value therebetween; and / or
[0148] The pore size of the blind hole is 20-500 μm or 100-150 μm, for example, it can be 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, 110 μm, 120 μm, 130 μm, 140 μm, 150 μm, 160 μm, 170 μm, 180 μm, 190 μm, 200 μm, 210 μm, 220 μm, 230 μm, 240 μm, 250 μm, 260 μm, 0 μm, 270 μm, 280 μm, 290 μm, 300 μm, 310 μm, 320 μm, 330 μm, 340 μm, 350 μm, 360 μm, 370 μm, 380 μm, 390 μm, 400 μm, 210 μm, 410 μm, 420 μm, 430 μm, 440 μm, 450 μm, 460 μm, 470 μm, 480 μm, 490 μm, 500 μm, or any value therebetween; and / or
[0149] The spacing between the blind holes is 100-1500 μm, exemplarily 400-500 μm, for example, 100 μm, 110 μm, 120 μm, 130 μm, 140 μm, 150 μm, 160 μm, 170 μm, 180 μm, 190 μm, 200 μm, 210 μm, 220 μm, 230 μm, 240 μm, 250 μm, 260 μm, 270 μm, 280 μm, 290 μm, 300μm, 310μm, 320μm, 330μm, 340μm, 350μm, 360μm, 370μm, 380μm, 390μm, 400μm, 410μm, 420μm, 4 30μm, 440μm, 450μm, 460μm, 470μm, 480μm, 490μm, 500μm, 510μm, 520μm, 530μm, 540μm, 550μm, 560 μm, 570μm, 580μm, 590μm, 600μm, 610μm, 620μm, 630μm, 640μm, 650μm, 660μm, 670μm, 680μm, 690μm m, 700μm, 710μm, 720μm, 730μm, 740μm, 750μm, 760μm, 770μm, 780μm, 790μm, 800μm, 810μm, 820μm, 830 μm, 840 μm, 850 μm, 860 μm, 870 μm, 880 μm, 890 μm, 900 μm, 910 μm, 920 μm, 930 μm, 940 μm, 950 μm, 960 μm, 970 μm, 980 μm, 990 μm, 1000 μm, 1100 μm, 1200 μm, 1300 μm, 1400 μm, 1500 μm, or any value therebetween; and / or
[0150] The porosity of the blind holes is 0.1%-10% or 2%-4%, for example, it can be 0.1%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10% or any value therebetween.
[0151] In some embodiments, the blind holes are evenly distributed.
[0152] There are no particular limitations on the thickness of the first negative electrode active material layer, and any thickness commonly used in the art may be employed. Typically, the thickness of the first negative electrode active material layer is 10-100 μm or 60-100 μm, for example, 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, or any value therebetween.
[0153] There is no particular limitation on the thickness of the second negative electrode active material layer, and those commonly used in the art can be adopted. Typically, the thickness of the second negative electrode active material layer is 10-200 μm or 60-100 μm, for example, 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, 110 μm, 120 μm, 130 μm, 140 μm, 150 μm, 160 μm, 170 μm, 180 μm, 190 μm, 200 μm, or any value therebetween.
[0154] There are no particular limitations on the thickness of the third negative electrode active material layer, and any thickness commonly used in the art may be employed. Typically, the thickness of the third negative electrode active material layer is 10-100 μm or 20-40 μm, for example, 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, or any value therebetween.
[0155] For example, the thickness of the second negative electrode active material layer is greater than the thickness of the first negative electrode active material layer and / or the third negative electrode active material layer. This configuration can better reduce costs.
[0156] There is no particular limitation on the particle size of natural graphite and artificial graphite, and those commonly used in the art can be used. Typically, the median particle size of the artificial graphite in the negative electrode active material of the first negative electrode active material layer is 5-20 μm, for example, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm, 18 μm, 19 μm, 20 μm or any value in between these values; and / or
[0157] The median particle size of the natural graphite in the negative electrode active material of the second negative electrode active material layer is 5-20 μm, for example, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm, 18 μm, 19 μm, 20 μm or any value in between these values; and / or
[0158] The median particle size of the artificial graphite in the negative electrode active material of the third negative electrode active material layer is 5-20 μm, for example, it can be 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm, 18 μm, 19 μm, 20 μm or any value between these values.
[0159] There are no particular limitations on the composition of the first negative electrode active material layer, the second negative electrode active material layer, and the third negative electrode active material layer, and those commonly used in the art may be used. Typically, the first negative electrode active material layer, the second negative electrode active material layer, and the third negative electrode active material layer each include:
[0160] 90-97 wt % of the negative electrode active material, for example, 90 wt %, 91 wt %, 92 wt %, 93 wt %, 94 wt %, 95 wt %, 96 wt %, 97 wt %, or any value therebetween;
[0161] 1-5 wt % of a negative electrode conductive agent, for example, 1 wt %, 2 wt %, 3 wt %, 4 wt %, 5 wt % or any value therebetween;
[0162] 1-5 wt % of the negative electrode binder, for example, 1 wt %, 2 wt %, 3 wt %, 4 wt %, 5 wt % or any value therebetween;
[0163] 1-3 wt % of a negative electrode thickener, for example, 1 wt %, 2 wt %, 3 wt % or any value therebetween;
[0164] The above weight percentages are based on the total weight of the negative electrode active material, the negative electrode conductive agent, the negative electrode binder and the negative electrode thickener.
[0165] As for the negative electrode active material, it is selected from natural graphite or artificial graphite.
[0166] There are no particular limitations on the negative electrode conductive agent, and any of those commonly used in the art may be used. Typically, the negative electrode conductive agent is selected from one or more of the following groups: conductive carbon black, carbon nanotubes, vapor-generated carbon fibers, Ketjen black, and graphene.
[0167] There is no particular limitation on the negative electrode binder, and any of those commonly used in the art may be used. Typically, the negative electrode binder is styrene-butadiene rubber and / or lithium polyacrylate.
[0168] There are no particular limitations on the negative electrode thickener, and those commonly used in the art may be used. Typically, the negative electrode thickener is selected from one or more of the following groups: sodium carboxymethylcellulose, polyvinylidene fluoride, lithium polyacrylate, and polyacrylonitrile.
[0169] Method for preparing negative electrode sheet
[0170] In order to at least partially solve one or more of the above problems and other potential problems, a second exemplary embodiment of the present disclosure provides a method for preparing a negative electrode sheet, comprising:
[0171] At least two negative electrode slurries containing negative electrode active materials are stacked and coated on a current collector and dried to obtain a negative electrode sheet;
[0172] The negative electrode active material is selected from natural graphite or artificial graphite, and the at least two negative electrode slurries containing the negative electrode active material include at least one negative electrode slurry containing natural graphite and at least one negative electrode slurry containing artificial graphite.
[0173] In some embodiments, the method comprises:
[0174] coating a first negative electrode slurry containing a negative electrode active material on a current collector and drying the slurry to form a first negative electrode active material layer, wherein the negative electrode active material includes natural graphite; and
[0175] coating a second negative electrode slurry containing a negative electrode active material on the first negative electrode active material layer and drying the slurry to form a second negative electrode active material layer, wherein the negative electrode active material includes artificial graphite;
[0176] To obtain the negative electrode.
[0177] There is no particular limitation on the composition of the first negative electrode slurry and the second negative electrode slurry, and those commonly used in the art can be used. Typically, the first negative electrode slurry and the second negative electrode slurry each include:
[0178] 5-30 wt % of the composition, for example, can be 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30 wt %, or any value therebetween; and
[0179] 70-95 wt% solvent, for example, 70, 71, 72, 73, 74, 75, 76, 77, 78, 79, 80, 81, 82, 83, 84, 85, 86, 87, 88, 89, 90, 91, 92, 93, 94, 95 wt%, or any value therebetween;
[0180] The composition comprises:
[0181] 90-97 wt % of the negative electrode active material, for example, 90 wt %, 91 wt %, 92 wt %, 93 wt %, 94 wt %, 95 wt %, 96 wt %, 97 wt %, or any value therebetween;
[0182] 1-5 wt % of a negative electrode conductive agent, for example, 1 wt %, 2 wt %, 3 wt %, 4 wt %, 5 wt % or any value therebetween;
[0183] 1-5 wt % of a negative electrode binder, for example, 1 wt %, 2 wt %, 3 wt %, 4 wt %, 5 wt % or any value therebetween; and
[0184] 1-3 wt % of a negative electrode thickener, for example, 1 wt %, 2 wt %, 3 wt % or any value therebetween;
[0185] The above weight percentages are based on the total weight of the negative electrode active material, the negative electrode conductive agent, the negative electrode binder and the negative electrode thickener.
[0186] In some embodiments, the method comprises:
[0187] Coating a first negative electrode slurry containing a negative electrode active material and a chemical pore former on a current collector, drying the slurry, and forming pores to form a first negative electrode active material layer containing one or more blind holes, wherein the negative electrode active material comprises natural graphite, and the openings of the blind holes are located outside the first negative electrode active material layer; and
[0188] coating a second negative electrode slurry containing a negative electrode active material on the first negative electrode active material layer and drying the slurry to form a second negative electrode active material layer, wherein the negative electrode active material includes artificial graphite;
[0189] To obtain the negative electrode.
[0190] In one embodiment, the first negative electrode slurry includes:
[0191] 5-30 wt % of the composition, for example, can be 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30 wt %, or any value therebetween; and
[0192] 70-95 wt% solvent, for example, 70, 71, 72, 73, 74, 75, 76, 77, 78, 79, 80, 81, 82, 83, 84, 85, 86, 87, 88, 89, 90, 91, 92, 93, 94, 95 wt%, or any value therebetween;
[0193] The composition comprises:
[0194] 85-95% by weight of the negative electrode active material, for example, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97% by weight, or any value therebetween;
[0195] 1-5 wt % of a negative electrode conductive agent, for example, 1 wt %, 2 wt %, 3 wt %, 4 wt %, 5 wt % or any value therebetween;
[0196] 1-5 wt % of the negative electrode binder, for example, 1 wt %, 2 wt %, 3 wt %, 4 wt %, 5 wt % or any value therebetween;
[0197] 1-3 wt % of a negative electrode thickener, for example, 1 wt %, 2 wt %, 3 wt % or any value therebetween; and
[0198] 1-10 wt% of pore former, for example, 1 wt%, 2 wt%, 3 wt%, 4 wt%, 5 wt%, 6 wt%, 7 wt%, 8 wt%, 9 wt%, 10 wt% or any value therebetween;
[0199] The above weight percentages are based on the total weight of the negative electrode active material, negative electrode conductive agent, negative electrode binder, negative electrode thickener and pore former.
[0200] In one embodiment, the second negative electrode slurry includes:
[0201] 5-30 wt % of the composition, for example, can be 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30 wt %, or any value therebetween; and
[0202] 70-95 wt% solvent, for example, 70, 71, 72, 73, 74, 75, 76, 77, 78, 79, 80, 81, 82, 83, 84, 85, 86, 87, 88, 89, 90, 91, 92, 93, 94, 95 wt%, or any value therebetween;
[0203] The composition comprises:
[0204] 90-97 wt % of the negative electrode active material, for example, 90 wt %, 91 wt %, 92 wt %, 93 wt %, 94 wt %, 95 wt %, 96 wt %, 97 wt %, or any value therebetween;
[0205] 1-5 wt % of a negative electrode conductive agent, for example, 1 wt %, 2 wt %, 3 wt %, 4 wt %, 5 wt % or any value therebetween;
[0206] 1-5 wt % of a negative electrode binder, for example, 1 wt %, 2 wt %, 3 wt %, 4 wt %, 5 wt % or any value therebetween; and
[0207] 1-3 wt % of a negative electrode thickener, for example, 1 wt %, 2 wt %, 3 wt % or any value therebetween;
[0208] The above weight percentages are based on the total weight of the negative electrode active material, the negative electrode conductive agent, the negative electrode binder and the negative electrode thickener.
[0209] In some embodiments, the method comprises:
[0210] coating a first negative electrode slurry containing a negative electrode active material on a current collector and drying the slurry to form a first negative electrode active material layer, wherein the negative electrode active material includes natural graphite;
[0211] Physically forming pores in the first negative electrode active material layer to form a first negative electrode active material layer containing one or more blind holes, wherein the openings of the blind holes are located outside the first negative electrode active material layer; and
[0212] coating a second negative electrode slurry containing a negative electrode active material on the first negative electrode active material layer containing one or more blind holes and drying the slurry to form a second negative electrode active material layer, wherein the negative electrode active material includes artificial graphite;
[0213] To obtain the negative electrode.
[0214] There is no particular limitation on the composition of the first negative electrode slurry and the second negative electrode slurry, and those commonly used in the art can be used. Typically, the first negative electrode slurry and the second negative electrode slurry each include:
[0215] 5-30 wt % of the composition, for example, can be 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30 wt %, or any value therebetween; and
[0216] 70-95 wt% solvent, for example, 70, 71, 72, 73, 74, 75, 76, 77, 78, 79, 80, 81, 82, 83, 84, 85, 86, 87, 88, 89, 90, 91, 92, 93, 94, 95 wt%, or any value therebetween;
[0217] The composition comprises:
[0218] 90-97 wt % of the negative electrode active material, for example, 90 wt %, 91 wt %, 92 wt %, 93 wt %, 94 wt %, 95 wt %, 96 wt %, 97 wt %, or any value therebetween;
[0219] 1-5 wt % of a negative electrode conductive agent, for example, 1 wt %, 2 wt %, 3 wt %, 4 wt %, 5 wt % or any value therebetween;
[0220] 1-5 wt % of a negative electrode binder, for example, 1 wt %, 2 wt %, 3 wt %, 4 wt %, 5 wt % or any value therebetween; and
[0221] 1-3 wt % of a negative electrode thickener, for example, 1 wt %, 2 wt %, 3 wt % or any value therebetween;
[0222] The above weight percentages are based on the total weight of the negative electrode active material, the negative electrode conductive agent, the negative electrode binder and the negative electrode thickener.
[0223] In some embodiments, the depth of the blind hole is 1-80% or 10-70% or 20-60% of the thickness of the first negative electrode active material layer, for example, it can be 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39%, 40%, 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49%, 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, 70%, 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79%, 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, 99%, 100%, 101%, 102%, 103%, 104%, 105%, 106%, 107%, 108%, 109%, 110 7%, 38%, 39%, 40%, 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49%, 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, 70%, 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79%, 80% or any value therebetween; and / or
[0224] The pore size of the blind hole is 20-300 μm or 80-150 μm, for example, it can be 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, 110 μm, 120 μm, 130 μm, 140 μm, 150 μm, 160 μm, 170 μm, 180 μm, 190 μm, 200 μm, 210 μm, 220 μm, 230 μm, 240 μm, 250 μm, 260 μm, 270 μm, 280 μm, 290 μm, 300 μm or any value in between; and / or
[0225] The spacing between the blind holes is 100-1000 μm or 400-500 μm, for example, 100 μm, 110 μm, 120 μm, 130 μm, 140 μm, 150 μm, 160 μm, 170 μm, 180 μm, 190 μm, 200 μm, 210 μm, 220 μm, 230 μm, 240 μm, 250 μm, 260 μm, 270 μm, 280 μm, 290 μm, 300 μm, 310 μm, 320 μm, 330 μm, 340 μm, 350 μm, 360 μm, 370 μm, 380 μm, 390 μm, 400 μm, 410 μm, 420 μm, 430 μm, 440 μm, 450 μm, 460 μm, 470 μm, 480 μm, 490 μm, 500 μm, 510 μm, 520 μm, 530 μm, 540 μm, 550 μm, 560 μm, 570 μm, 580 μm, 590 μm, 600 μm, 610 μm, 620 μm, 630 μm, 640 μm μm, 310μm, 320μm, 330μm, 340μm, 350μm, 360μm, 370μm, 380μm, 390μm, 400μm, 410μm, 420μm, 430μm m, 440μm, 450μm, 460μm, 470μm, 480μm, 490μm, 500μm, 510μm, 520μm, 530μm, 540μm, 550μm, 560μm, 570μm, 580μm, 590μm, 600μm, 610μm, 620μm, 630μm, 640μm, 650μm, 660μm, 670μm, 680μm m, 690μm, 700μm, 710μm, 720μm, 730μm, 740μm, 750μm, 760μm, 770μm, 780μm, 790μm, 80 0 μm, 810 μm, 820 μm, 830 μm, 840 μm, 850 μm, 860 μm, 870 μm, 880 μm, 890 μm, 900 μm, 910 μm, 920 μm, 930 μm, 940 μm, 950 μm, 960 μm, 970 μm, 980 μm, 990 μm, 1000 μm, or any value therebetween; and / or
[0226] The porosity of the blind holes is 0.1%-10% or 2%-4%, for example, it can be 0.1%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10% or any value therebetween.
[0227] In some embodiments, the blind holes are evenly distributed.
[0228] There is no particular limitation on the thickness of the first negative electrode active material layer, and those commonly used in the art can be adopted. Typically, the thickness of the first negative electrode active material layer is 10-200 μm or 50-100 μm, for example, 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, 110 μm, 120 μm, 130 μm, 140 μm, 150 μm, 160 μm, 170 μm, 180 μm, 190 μm, 200 μm, or any value therebetween.
[0229] There is no particular limitation on the thickness of the second negative electrode active material layer, and those commonly used in the art can be adopted. Typically, the thickness of the second negative electrode active material layer is 10-200 μm or 50-100 μm, for example, 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, 110 μm, 120 μm, 130 μm, 140 μm, 150 μm, 160 μm, 170 μm, 180 μm, 190 μm, 200 μm, or any value therebetween.
[0230] There is no particular limitation on the particle size of the natural graphite, and those commonly used in the art can be used. Typically, the median particle size of the natural graphite is 5-20 μm, for example, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm, 18 μm, 19 μm, 20 μm, or any value therebetween.
[0231] There is no particular limitation on the particle size of the artificial graphite, and those commonly used in the art can be used. Typically, the median particle size of natural graphite is 5-20 μm, for example, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm, 18 μm, 19 μm, 20 μm, or any value therebetween.
[0232] In one embodiment, the method comprises:
[0233] coating a first negative electrode slurry containing a negative electrode active material on a current collector and drying the slurry to form a first negative electrode active material layer, wherein the negative electrode active material comprises artificial graphite;
[0234] coating a second negative electrode slurry containing a negative electrode active material on the first negative electrode active material layer and drying the slurry to form a second negative electrode active material layer, wherein the negative electrode active material includes natural graphite; and
[0235] coating a third negative electrode slurry containing a negative electrode active material on the second negative electrode active material layer and drying the slurry to form a third negative electrode active material layer, wherein the negative electrode active material includes artificial graphite;
[0236] To obtain the negative electrode.
[0237] There is no particular limitation on the composition of the first negative electrode slurry, the second negative electrode slurry, and the third negative electrode slurry, and those commonly used in the art can be used. Typically, the first negative electrode slurry, the second negative electrode slurry, and the third negative electrode slurry each include:
[0238] 5-30 wt % of the composition, for example, can be 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30 wt %, or any value therebetween; and
[0239] 70-95 wt% solvent, for example, 70, 71, 72, 73, 74, 75, 76, 77, 78, 79, 80, 81, 82, 83, 84, 85, 86, 87, 88, 89, 90, 91, 92, 93, 94, 95 wt%, or any value therebetween;
[0240] The composition comprises:
[0241] 90-97 wt % of the negative electrode active material, for example, 90 wt %, 91 wt %, 92 wt %, 93 wt %, 94 wt %, 95 wt %, 96 wt %, 97 wt %, or any value therebetween;
[0242] 1-5 wt % of a negative electrode conductive agent, for example, 1 wt %, 2 wt %, 3 wt %, 4 wt %, 5 wt % or any value therebetween;
[0243] 1-5 wt % of a negative electrode binder, for example, 1 wt %, 2 wt %, 3 wt %, 4 wt %, 5 wt % or any value therebetween; and
[0244] 1-3 wt % of a negative electrode thickener, for example, 1 wt %, 2 wt %, 3 wt % or any value therebetween;
[0245] The above weight percentages are based on the total weight of the negative electrode active material, the negative electrode conductive agent, the negative electrode binder and the negative electrode thickener.
[0246] In one embodiment, the method comprises:
[0247] coating a first negative electrode slurry containing a negative electrode active material and a chemical pore former on a current collector and semi-drying the slurry at low temperature to form a semi-dried first negative electrode active material layer, wherein the negative electrode active material comprises artificial graphite;
[0248] Coating a second negative electrode slurry containing a negative electrode active material on the semi-dried first negative electrode active material layer, drying at a high temperature, and forming pores to form a second negative electrode active material layer and forming one or more blind holes in a system consisting of the first negative electrode active material layer and the second negative electrode active material layer, wherein the negative electrode active material includes natural graphite, and the openings of the blind holes are located outside the second negative electrode active material layer; and
[0249] coating a third negative electrode slurry containing a negative electrode active material on the second negative electrode active material layer and drying the slurry to form a third negative electrode active material layer, wherein the negative electrode active material includes artificial graphite;
[0250] To obtain the negative electrode.
[0251] In one embodiment, the first negative electrode slurry includes:
[0252] 5-30 wt % of the composition, for example, can be 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30 wt %, or any value therebetween; and
[0253] 70-95 wt% solvent, for example, 70, 71, 72, 73, 74, 75, 76, 77, 78, 79, 80, 81, 82, 83, 84, 85, 86, 87, 88, 89, 90, 91, 92, 93, 94, 95 wt%, or any value therebetween;
[0254] The composition comprises:
[0255] 85-95% by weight of the negative electrode active material, for example, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97% by weight, or any value therebetween;
[0256] 1-5 wt % of a negative electrode conductive agent, for example, 1 wt %, 2 wt %, 3 wt %, 4 wt %, 5 wt % or any value therebetween;
[0257] 1-5 wt % of the negative electrode binder, for example, 1 wt %, 2 wt %, 3 wt %, 4 wt %, 5 wt % or any value therebetween;
[0258] 1-3 wt % of a negative electrode thickener, for example, 1 wt %, 2 wt %, 3 wt % or any value therebetween; and
[0259] 1-10 wt% of pore former, for example, 1 wt%, 2 wt%, 3 wt%, 4 wt%, 5 wt%, 6 wt%, 7 wt%, 8 wt%, 9 wt%, 10 wt% or any value therebetween;
[0260] The above weight percentages are based on the total weight of the negative electrode active material, negative electrode conductive agent, negative electrode binder, negative electrode thickener and pore former.
[0261] There is no particular limitation on the composition of the second negative electrode slurry and the third negative electrode slurry, and those commonly used in the art can be used. Typically, the second negative electrode slurry and the third negative electrode slurry each include:
[0262] 5-30 wt % of the composition, for example, can be 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30 wt %, or any value therebetween; and
[0263] 70-95 wt% solvent, for example, 70, 71, 72, 73, 74, 75, 76, 77, 78, 79, 80, 81, 82, 83, 84, 85, 86, 87, 88, 89, 90, 91, 92, 93, 94, 95 wt%, or any value therebetween;
[0264] The composition comprises:
[0265] 90-97 wt % of the negative electrode active material, for example, 90 wt %, 91 wt %, 92 wt %, 93 wt %, 94 wt %, 95 wt %, 96 wt %, 97 wt %, or any value therebetween;
[0266] 1-5 wt % of a negative electrode conductive agent, for example, 1 wt %, 2 wt %, 3 wt %, 4 wt %, 5 wt % or any value therebetween;
[0267] 1-5 wt % of a negative electrode binder, for example, 1 wt %, 2 wt %, 3 wt %, 4 wt %, 5 wt % or any value therebetween; and
[0268] 1-3 wt % of a negative electrode thickener, for example, 1 wt %, 2 wt %, 3 wt % or any value therebetween;
[0269] The above weight percentages are based on the total weight of the negative electrode active material, the negative electrode conductive agent, the negative electrode binder and the negative electrode thickener.
[0270] In one embodiment, the method comprises:
[0271] coating a first negative electrode slurry containing a negative electrode active material on a current collector and drying the slurry to form a first negative electrode active material layer, wherein the negative electrode active material comprises artificial graphite;
[0272] coating a second negative electrode slurry containing a negative electrode active material on the first negative electrode active material layer and drying the slurry to form a second negative electrode active material layer, wherein the negative electrode active material includes natural graphite;
[0273] Physically creating pores in a system consisting of the first negative electrode active material layer and the second negative electrode active material layer to form one or more blind holes, wherein the openings of the blind holes are located outside the second negative electrode active material layer; and
[0274] coating a third negative electrode slurry containing a negative electrode active material on the second negative electrode active material layer and drying the slurry to form a third negative electrode active material layer, wherein the negative electrode active material includes artificial graphite;
[0275] To obtain the negative electrode.
[0276] There is no particular limitation on the composition of the first negative electrode slurry, the second negative electrode slurry, and the third negative electrode slurry, and those commonly used in the art can be used. Typically, the first negative electrode slurry, the second negative electrode slurry, and the third negative electrode slurry each include:
[0277] 5-30 wt % of the composition, for example, can be 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30 wt %, or any value therebetween; and
[0278] 70-95 wt% solvent, for example, 70, 71, 72, 73, 74, 75, 76, 77, 78, 79, 80, 81, 82, 83, 84, 85, 86, 87, 88, 89, 90, 91, 92, 93, 94, 95 wt%, or any value therebetween;
[0279] The composition comprises:
[0280] 90-97 wt % of the negative electrode active material, for example, 90 wt %, 91 wt %, 92 wt %, 93 wt %, 94 wt %, 95 wt %, 96 wt %, 97 wt %, or any value therebetween;
[0281] 1-5 wt % of a negative electrode conductive agent, for example, 1 wt %, 2 wt %, 3 wt %, 4 wt %, 5 wt % or any value therebetween;
[0282] 1-5 wt % of a negative electrode binder, for example, 1 wt %, 2 wt %, 3 wt %, 4 wt %, 5 wt % or any value therebetween; and
[0283] 1-3 wt % of a negative electrode thickener, for example, 1 wt %, 2 wt %, 3 wt % or any value therebetween;
[0284] The above weight percentages are based on the total weight of the negative electrode active material, the negative electrode conductive agent, the negative electrode binder and the negative electrode thickener.
[0285] There are no particular limitations on the negative electrode conductive agent used in the above methods, and any commonly used negative electrode conductive agent in the art may be employed. Typically, the negative electrode conductive agent is selected from one or more of the following groups: conductive carbon black, carbon nanotubes, vapor-generated carbon fibers, Ketjen black, and graphene.
[0286] There is no particular limitation on the negative electrode binder used in the above methods, and those commonly used in the art can be used. Typically, the negative electrode binder is styrene-butadiene rubber and / or lithium polyacrylate.
[0287] There is no particular limitation on the negative electrode thickener used in the above methods, and those commonly used in the art can be used. Typically, the negative electrode thickener is selected from one or more of the following groups: sodium carboxymethylcellulose, polyvinylidene fluoride, lithium polyacrylate, and polyacrylonitrile.
[0288] There are no particular limitations on the pore-forming agents used in the above methods, and any pore-forming agent commonly used in the art may be employed. Typically, the pore-forming agent is selected from one or more of the group consisting of hydrogen peroxide, urea, ammonium carbonate, ammonium bicarbonate, ammonium carbamate, calcium hydrogen phosphate, naphthalene, and 4-oxydiphenylsulfonylhydrazine (OBSH). Exemplarily, the pore-forming agent may include ammonium bicarbonate.
[0289] In some embodiments, the depth of the blind hole is 1-80% or 10-70% or 30-60% of the thickness of the second negative electrode active material layer plus the thickness of the first negative electrode active material layer, for example, it can be 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33%, 34%, 35%. , 36%, 37%, 38%, 39%, 40%, 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49%, 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, 70%, 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79%, 80% or any value therebetween; and / or
[0290] The pore size of the blind hole is 20-500 μm or 100-150 μm, for example, it can be 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, 110 μm, 120 μm, 130 μm, 140 μm, 150 μm, 160 μm, 170 μm, 180 μm, 190 μm, 200 μm, 210 μm, 220 μm, 230 μm, 240 μm, 250 μm, 260 μm, 0 μm, 270 μm, 280 μm, 290 μm, 300 μm, 310 μm, 320 μm, 330 μm, 340 μm, 350 μm, 360 μm, 370 μm, 380 μm, 390 μm, 400 μm, 210 μm, 410 μm, 420 μm, 430 μm, 440 μm, 450 μm, 460 μm, 470 μm, 480 μm, 490 μm, 500 μm, or any value therebetween; and / or
[0291] The spacing between the blind holes is 100-1500 μm or 400-500 μm, for example, 100 μm, 110 μm, 120 μm, 130 μm, 140 μm, 150 μm, 160 μm, 170 μm, 180 μm, 190 μm, 200 μm, 210 μm, 220 μm, 230 μm, 240 μm, 250 μm, 260 μm, 270 μm, 280 μm, 290 μm, 300 μm, 310 μm, 320 μm, 330 μm, 340 μm, 350 μm, 360 μm, 370 μm, 380 μm, 390 μm, 400 μm, 410 μm, 420 μm, 430μm, 440μm, 450μm, 460μm, 470μm, 480μm, 490μm, 500μm, 510μm, 520μm, 530μm, 540μm, 550μm, 560μm, 570μm, 580μm, 590μm, 600μm, 610μm, 620μm, 630μm, 640μm, 6 50μm, 660μm, 670μm, 680μm, 690μm, 700μm, 710μm, 720μm, 730μm, 740μm, 750μm, 7 60μm, 770μm, 780μm, 790μm, 800μm, 810μm, 820μm, 830μm, 840μm, 850μm, 860μm, 87 0 μm, 880 μm, 890 μm, 900 μm, 910 μm, 920 μm, 930 μm, 940 μm, 950 μm, 960 μm, 970 μm, 980 μm, 990 μm, 1000 μm, 1100 μm, 1200 μm, 1300 μm, 1400 μm, 1500 μm, or any value therebetween; and / or
[0292] The porosity of the blind holes is 0.1%-10% or 2%-4%, for example, it can be 0.1%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10% or any value therebetween.
[0293] In some embodiments, the blind holes are evenly distributed.
[0294] There are no particular limitations on the thickness of the first negative electrode active material layer, and any thickness commonly used in the art may be employed. Typically, the thickness of the first negative electrode active material layer is 10-100 μm or 60-100 μm, for example, 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, or any value therebetween.
[0295] There is no particular limitation on the thickness of the second negative electrode active material layer, and those commonly used in the art can be adopted. Typically, the thickness of the second negative electrode active material layer is 10-200 μm or 60-100 μm, for example, 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, 110 μm, 120 μm, 130 μm, 140 μm, 150 μm, 160 μm, 170 μm, 180 μm, 190 μm, 200 μm, or any value in between these values.
[0296] There are no particular limitations on the thickness of the third negative electrode active material layer, and any thickness commonly used in the art may be employed. Typically, the thickness of the third negative electrode active material layer is 10-100 μm or 20-40 μm, for example, 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, or any value therebetween.
[0297] There is no particular limitation on the particle size of natural graphite and artificial graphite, and those commonly used in the art can be used. Typically, the median particle size of the artificial graphite in the negative electrode active material of the first negative electrode active material layer is 5-20 μm, for example, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm, 18 μm, 19 μm, 20 μm or any value in between these values; and / or
[0298] The median particle size of the natural graphite in the negative electrode active material of the second negative electrode active material layer is 5-20 μm, for example, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm, 18 μm, 19 μm, 20 μm or any value in between these values; and / or
[0299] The median particle size of the artificial graphite in the negative electrode active material of the third negative electrode active material layer is 5-20 μm, for example, it can be 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm, 18 μm, 19 μm, 20 μm or any value between these values.
[0300] lithium-ion batteries
[0301] To at least partially address one or more of the aforementioned issues and other potential problems, a third exemplary embodiment of the present disclosure provides a lithium-ion battery comprising a negative electrode sheet according to the first exemplary embodiment or a negative electrode sheet prepared by the method of the second exemplary embodiment. Typically, the lithium-ion battery may be a single cell, a battery module, or a battery pack.
[0302] The following examples are provided. The examples described below are illustrative and are intended only to explain the present disclosure and are not to be construed as limiting the present disclosure. Where specific techniques or conditions are not specified in the examples, the methods were performed according to those described in the literature in the art or according to the product specifications. Reagents or instruments used without manufacturer's indication are all commercially available conventional products.
[0303] Example 1 (Preparation of negative electrode sheet by physical pore forming method, three-layer structure)
[0304] Referring to FIG1 , a negative electrode sheet is prepared, wherein: first, a system consisting of a first negative electrode active material layer 102 and a second negative electrode active material layer 105 is formed on a current collector 101; then, holes are formed in the system to form blind holes 107; finally, a third negative electrode active material layer 108 is formed on the second negative electrode active material layer 105. The specific method is as follows:
[0305] 95.5 parts by weight of artificial graphite (median particle size of 12 μm) as a negative electrode active material, 1 part by weight of carbon nanotubes as a conductive agent, 2 parts by weight of a mixture of styrene-butadiene rubber and lithium polyacrylate as a binder (mass ratio of 1:1), 1.5 parts by weight of sodium carboxymethyl cellulose as a thickener, and 1000 parts by weight of deionized water as a solvent were mixed to prepare a first negative electrode slurry. The prepared first negative electrode slurry was evenly coated on a current collector copper foil and dried by heating at 60° C. to form a first negative electrode active material layer. The thickness of the first negative electrode active material layer was 50 μm.
[0306] A second negative electrode slurry was prepared by mixing 95.5 parts by weight of natural graphite (median particle size of 18 μm) as a negative electrode active material, 1 part by weight of carbon nanotubes as a conductive agent, 2 parts by weight of a mixture of styrene-butadiene rubber and lithium polyacrylate as a binder (mass ratio of 1:1), 1.5 parts by weight of sodium carboxymethyl cellulose as a thickener, and 1000 parts by weight of deionized water as a solvent. The prepared second negative electrode slurry was evenly coated on the first negative electrode active material layer, and after heating and drying at 60° C., a second negative electrode active material layer was formed. The thickness of the second negative electrode active material layer was 60 μm.
[0307] A punching device (i.e., the electrode punching device disclosed in patent CN216084936U) is used to physically create pores in the system consisting of the first negative electrode active material layer and the second negative electrode active material layer to form a plurality of evenly distributed blind holes (pore creation rate of 4%). The openings of the blind holes are located outside the second negative electrode active material layer. The blind holes have a depth of 90 μm, a pore diameter of 200 μm, and a spacing of 400 μm between the blind holes.
[0308] A third negative electrode slurry was prepared by mixing 95.5 parts by weight of artificial graphite (median particle size of 12 μm) as a negative electrode active material, 1 part by weight of carbon nanotubes as a conductive agent, 2 parts by weight of a mixture of styrene-butadiene rubber and lithium polyacrylate as a binder (mass ratio of 1:1), 1.5 parts by weight of sodium carboxymethyl cellulose as a thickener, and 1000 parts by weight of deionized water as a solvent. The prepared third negative electrode slurry was evenly coated on the second negative electrode active material layer and dried by heating at 60° C. to form a third negative electrode active material layer. The thickness of the third negative electrode active material layer was 30 μm.
[0309] Then, cold pressing and cutting are performed to obtain the negative electrode sheet.
[0310] Example 2 (Chemical pore formation method for preparing negative electrode sheet, three-layer structure)
[0311] The negative electrode sheet is prepared by:
[0312] 90 parts by weight of artificial graphite (median particle size of 12 μm) as a negative electrode active material, 1 part by weight of carbon nanotubes as a conductive agent, 2 parts by weight of a mixture of styrene-butadiene rubber and lithium polyacrylate as a binder (mass ratio of 1:1), 2 parts by weight of sodium carboxymethyl cellulose as a thickener, and 5 parts by weight of ammonium bicarbonate as a pore-forming agent are mixed with 1000 parts by weight of deionized water as a solvent to prepare a first negative electrode slurry, and the prepared first negative electrode slurry is evenly coated on a current collector copper foil, and semi-dried at 50° C. to form a semi-dried first negative electrode active material layer, the thickness of the first negative electrode active material layer being 50 μm;
[0313] A second negative electrode slurry was prepared by mixing 95.5 parts by weight of natural graphite (median particle size of 18 μm) as a negative electrode active material, 1 part by weight of carbon nanotubes as a conductive agent, 2 parts by weight of a mixture of styrene-butadiene rubber and lithium polyacrylate as a binder (mass ratio of 1:1), 1.5 parts by weight of sodium carboxymethyl cellulose as a thickener, and 1000 parts by weight of deionized water as a solvent. The prepared second negative electrode slurry was evenly coated on the semi-dried first negative electrode active material layer. After high-temperature drying and pore formation at 60° C., a second negative electrode active material layer was formed. One or more evenly distributed blind holes (pore formation rate of 4%) were formed in the system consisting of the first negative electrode active material layer and the second negative electrode active material layer. The second negative electrode active material layer had a thickness of 60 μm, a depth of 90 μm, a pore diameter of 200 μm, and a spacing of 400 μm between the blind holes.
[0314] A third negative electrode slurry was prepared by mixing 95.5 parts by weight of artificial graphite (median particle size of 12 μm) as a negative electrode active material, 1 part by weight of carbon nanotubes as a conductive agent, 2 parts by weight of a mixture of styrene-butadiene rubber and lithium polyacrylate as a binder (mass ratio of 1:1), 1.5 parts by weight of sodium carboxymethyl cellulose as a thickener, and 1000 parts by weight of deionized water as a solvent. The prepared third negative electrode slurry was evenly coated on the second negative electrode active material layer and dried by heating at 60° C. to form a third negative electrode active material layer. The thickness of the third negative electrode active material layer was 30 μm.
[0315] Then, cold pressing and cutting are performed to obtain the negative electrode sheet.
[0316] Example 3 (no pores, three-layer structure)
[0317] The negative electrode sheet is prepared by:
[0318] 95.5 parts by weight of artificial graphite (median particle size of 12 μm) as a negative electrode active material, 1 part by weight of carbon nanotubes as a conductive agent, 2 parts by weight of a mixture of styrene-butadiene rubber and lithium polyacrylate as a binder (mass ratio of 1:1), 1.5 parts by weight of sodium carboxymethyl cellulose as a thickener, and 1000 parts by weight of deionized water as a solvent were mixed to prepare a first negative electrode slurry. The prepared first negative electrode slurry was evenly coated on a current collector copper foil and dried by heating at 60° C. to form a first negative electrode active material layer. The thickness of the first negative electrode active material layer was 50 μm.
[0319] A second negative electrode slurry was prepared by mixing 95.5 parts by weight of natural graphite (median particle size of 18 μm) as a negative electrode active material, 1 part by weight of carbon nanotubes as a conductive agent, 2 parts by weight of a mixture of styrene-butadiene rubber and lithium polyacrylate as a binder (mass ratio of 1:1), 1.5 parts by weight of sodium carboxymethyl cellulose as a thickener, and 1000 parts by weight of deionized water as a solvent. The prepared second negative electrode slurry was evenly coated on the first negative electrode active material layer, and after heating and drying at 60° C., a second negative electrode active material layer was formed. The thickness of the second negative electrode active material layer was 60 μm.
[0320] A third negative electrode slurry was prepared by mixing 95.5 parts by weight of artificial graphite (median particle size of 12 μm) as a negative electrode active material, 1 part by weight of carbon nanotubes as a conductive agent, 2 parts by weight of a mixture of styrene-butadiene rubber and lithium polyacrylate as a binder (mass ratio of 1:1), 1.5 parts by weight of sodium carboxymethyl cellulose as a thickener, and 1000 parts by weight of deionized water as a solvent. The prepared third negative electrode slurry was evenly coated on the second negative electrode active material layer and dried by heating at 60° C. to form a third negative electrode active material layer. The thickness of the third negative electrode active material layer was 30 μm.
[0321] Then, cold pressing and cutting are performed to obtain the negative electrode sheet.
[0322] Example 4 (Preparation of negative electrode sheet by physical pore forming method, two-layer structure)
[0323] Referring to FIG2 , a negative electrode sheet is prepared, wherein: first, a first negative electrode active material layer 102 is formed on a current collector 101 , and then holes are formed in the first negative electrode active material layer 102 to form blind holes 103 (including pores 104 ). The specific method is as follows:
[0324] 95.5 parts by weight of natural graphite (median particle size of 18 μm) as a negative electrode active material, 1 part by weight of carbon nanotubes as a conductive agent, 2 parts by weight of a mixture of styrene-butadiene rubber and lithium polyacrylate as a binder (mass ratio of 1:1), 1.5 parts by weight of sodium carboxymethyl cellulose as a thickener, and 1000 parts by weight of deionized water as a solvent were mixed to prepare a first negative electrode slurry. The prepared first negative electrode slurry was evenly coated on a current collector copper foil and heated and dried at 60° C. to form a first negative electrode active material layer. The thickness of the first negative electrode active material layer was 60 μm.
[0325] Physically pore forming is performed on the first negative electrode active material layer to form a plurality of evenly distributed blind holes (pore forming rate is 4%). The openings of the blind holes are located outside the first negative electrode active material layer. The blind holes have a depth of 90 μm, a pore diameter of 200 μm, and a spacing of 400 μm between the blind holes.
[0326] A second negative electrode slurry was prepared by mixing 95.5 parts by weight of artificial graphite (median particle size of 12 μm) as a negative electrode active material, 1 part by weight of carbon nanotubes as a conductive agent, 2 parts by weight of a mixture of styrene-butadiene rubber and lithium polyacrylate as a binder (mass ratio of 1:1), 1.5 parts by weight of sodium carboxymethyl cellulose as a thickener, and 1000 parts by weight of deionized water as a solvent. The prepared second negative electrode slurry was evenly coated on the first negative electrode active material layer, and after heating and drying at 60° C., a second negative electrode active material layer was formed. The thickness of the second negative electrode active material layer was 50 μm.
[0327] Then, cold pressing and cutting are performed to obtain the negative electrode sheet.
[0328] Example 5 (Chemical pore formation method for preparing negative electrode sheet, two-layer structure)
[0329] The negative electrode sheet is prepared by:
[0330] 90 parts by weight of natural graphite (median particle size of 18 μm) as a negative electrode active material, 1 part by weight of carbon nanotubes as a conductive agent, 2 parts by weight of a mixture of styrene-butadiene rubber and lithium polyacrylate as a binder (mass ratio of 1:1), 2 parts by weight of sodium carboxymethyl cellulose as a thickener, and 5 parts by weight of ammonium bicarbonate as a pore-forming agent are mixed with 1000 parts by weight of deionized water as a solvent to prepare a first negative electrode slurry. The prepared first negative electrode slurry is evenly coated on a current collector copper foil, and after high-temperature drying and pore formation at 60° C., a first negative electrode active material layer containing a plurality of evenly distributed blind holes (pore formation rate of 4%) is formed. The openings of the blind holes are located outside the first negative electrode active material layer, the blind holes have a depth of 90 μm, the pore diameter of the blind holes is 200 μm, the spacing between the blind holes is 400 μm, and the thickness of the first negative electrode active material layer is 60 μm.
[0331] A second negative electrode slurry was prepared by mixing 95.5 parts by weight of artificial graphite (median particle size of 12 μm) as a negative electrode active material, 1 part by weight of carbon nanotubes as a conductive agent, 2 parts by weight of a mixture of styrene-butadiene rubber and lithium polyacrylate as a binder (mass ratio of 1:1), 1.5 parts by weight of sodium carboxymethyl cellulose as a thickener, and 1000 parts by weight of deionized water as a solvent. The prepared second negative electrode slurry was evenly coated on the first negative electrode active material layer, and after heating and drying at 60° C., a second negative electrode active material layer was formed. The thickness of the second negative electrode active material layer was 50 μm.
[0332] Then, cold pressing and cutting are performed to obtain the negative electrode sheet.
[0333] Example 6 (no pores, two-layer structure)
[0334] 95.5 parts by weight of natural graphite (median particle size of 18 μm) as a negative electrode active material, 1 part by weight of carbon nanotubes as a conductive agent, 2 parts by weight of a mixture of styrene-butadiene rubber and lithium polyacrylate as a binder (mass ratio of 1:1), 1.5 parts by weight of sodium carboxymethyl cellulose as a thickener, and 1000 parts by weight of deionized water as a solvent were mixed to prepare a first negative electrode slurry. The prepared first negative electrode slurry was evenly coated on a current collector copper foil and heated and dried at 60° C. to form a first negative electrode active material layer. The thickness of the first negative electrode active material layer was 60 μm.
[0335] A second negative electrode slurry was prepared by mixing 95.5 parts by weight of artificial graphite (median particle size of 12 μm) as a negative electrode active material, 1 part by weight of carbon nanotubes as a conductive agent, 2 parts by weight of a mixture of styrene-butadiene rubber and lithium polyacrylate as a binder (mass ratio of 1:1), 1.5 parts by weight of sodium carboxymethyl cellulose as a thickener, and 1000 parts by weight of deionized water as a solvent. The prepared second negative electrode slurry was evenly coated on the first negative electrode active material layer, and after heating and drying at 60° C., a second negative electrode active material layer was formed. The thickness of the second negative electrode active material layer was 80 μm.
[0336] Then, cold pressing and cutting are performed to obtain the negative electrode sheet.
[0337] Example 7
[0338] It is basically the same as Example 1, except that the depth of the blind hole is 70 μm.
[0339] Example 8
[0340] It is basically the same as Example 1, except that the depth of the blind hole is 108 μm.
[0341] Example 9
[0342] It is basically the same as Example 1, except that the diameter of the blind hole is 100 μm.
[0343] Example 10
[0344] It is basically the same as Example 1, except that the diameter of the blind hole is 500 μm.
[0345] Example 11
[0346] It is basically the same as Example 1, except that the pitch of the blind holes is 100 μm.
[0347] Example 12
[0348] It is basically the same as Example 1, except that the pitch of the blind holes is 1500 μm.
[0349] Example 13
[0350] The method is basically the same as Example 1, except that the blind hole formation rate is 0.1%.
[0351] Example 14
[0352] The method is basically the same as Example 1, except that the hole formation rate of the blind hole is 10%.
[0353] Example 15
[0354] The method is basically the same as Example 1, except that the thickness of the first negative electrode active material layer is 10 μm.
[0355] Example 16
[0356] The method is basically the same as Example 1, except that the thickness of the first negative electrode active material layer is 70 μm.
[0357] Example 17
[0358] The method is basically the same as Example 1, except that the thickness of the second negative electrode active material layer is 10 μm.
[0359] Example 18
[0360] The method is basically the same as Example 1, except that the thickness of the second negative electrode active material layer is 70 μm.
[0361] Example 19
[0362] The method is basically the same as Example 1, except that the thickness of the third negative electrode active material layer is 10 μm.
[0363] Example 20
[0364] The method is basically the same as Example 1, except that the thickness of the third negative electrode active material layer is 50 μm.
[0365] Example 21
[0366] It is basically the same as Example 1, except that the median particle size of the artificial graphite in the negative electrode active material of the first negative electrode active material layer is 10 μm, the median particle size of the natural graphite in the negative electrode active material of the second negative electrode active material layer is 10 μm, and the median particle size of the artificial graphite in the negative electrode active material of the third negative electrode active material layer is 10 μm.
[0367] Example 22
[0368] It is basically the same as Example 1, except that the median particle size of the artificial graphite in the negative electrode active material of the first negative electrode active material layer is 20 μm, the median particle size of the natural graphite in the negative electrode active material of the second negative electrode active material layer is 25 μm, and the median particle size of the artificial graphite in the negative electrode active material of the third negative electrode active material layer is 20 μm.
[0369] Comparative Example 1 (one-layer structure)
[0370] 95.5 parts by weight of natural graphite (median particle size of 18 μm) as a negative electrode active material, 1 part by weight of carbon nanotubes as a conductive agent, 2 parts by weight of a mixture of styrene-butadiene rubber and lithium polyacrylate as a binder (mass ratio of 1:1), 1.5 parts by weight of sodium carboxymethyl cellulose as a thickener, and 1000 parts by weight of deionized water as a solvent were mixed to prepare a negative electrode slurry. The prepared negative electrode slurry was evenly coated on a current collector copper foil and heated and dried at 60° C. to form a first negative electrode active material layer. The thickness of the first negative electrode active material layer was 140 μm.
[0371] Then, cold pressing and cutting are performed to obtain the negative electrode sheet.
[0372] Comparative Example 2 (one-layer structure)
[0373] 95.5 parts by weight of artificial graphite (median particle size of 12 μm) as a negative electrode active material, 1 part by weight of carbon nanotubes as a conductive agent, 2 parts by weight of a mixture of styrene-butadiene rubber and lithium polyacrylate as a binder (mass ratio of 1:1), 1.5 parts by weight of sodium carboxymethyl cellulose as a thickener, and 1000 parts by weight of deionized water as a solvent were mixed to prepare a negative electrode slurry. The prepared negative electrode slurry was evenly coated on a current collector copper foil and heated and dried at 60° C. to form a first negative electrode active material layer. The thickness of the first negative electrode active material layer was 140 μm.
[0374] Then, cold pressing and cutting are performed to obtain the negative electrode sheet.
[0375] test
[0376] Test standards
[0377] The aperture of the blind hole is obtained by SEM electron microscope observation. The method for determining the aperture of the blind hole is to use the longest distance of the edge of the opening side of the hole, that is, to select two points on the edge of the opening side of the hole and measure the distance between the two points. The longest distance is the aperture of the blind hole.
[0378] The spacing between blind holes is obtained by SEM electron microscope observation. The spacing between blind holes refers to the shortest distance between the edges of the opening sides of two holes. That is, a point on the edge of the opening side of one hole and a point on the edge of the opening side of the other hole are selected, and the distance between the two points is measured. The shortest distance is the spacing between the blind holes.
[0379] The hole formation rate of blind holes is measured according to the following method:
[0380] For regular cylindrical holes, the hole-making rate of blind holes is per unit area (such as a 1mm2 electrode), the hole-making area is divided by the unit area, and then multiplied by the ratio of the hole-making depth to the total thickness.
[0381] For tapered holes, the hole-making rate of blind holes is per unit area (such as 1mm2 electrode), the hole-making area is divided by the unit area, multiplied by the ratio of the hole-making depth to the total thickness, and then multiplied by 1 / 3.
[0382] Test results
[0383] For specific test results, see Table 1 below.
[0384] Table 1
[0385] It can be clearly seen from the data of Examples 3 and 6 in Table 1 that the present disclosure, by adopting a method of superimposing an artificial graphite layer and a natural graphite layer, takes into account the advantages of high energy density of artificial graphite and low cost of natural graphite, thereby obtaining a compromise performance balance, that is, maintaining a high energy density and a short fast charging time while maintaining low cost. In some exemplary embodiments, it can also be clearly seen from the data of other embodiments in Table 1 that by forming pores in the negative electrode active material layer, an efficient lithium insertion channel can be formed, thereby improving the overall lithium insertion capacity compared to Examples 3 and 6, and obtaining a beneficial technical effect of better maintaining a good balance between high energy density, high fast charging capacity and controlling costs.
[0386] It should be noted that the present disclosure is not limited to the above-mentioned embodiments. The above-mentioned embodiments are merely examples, and within the scope of the technical solution of the present disclosure, embodiments having substantially the same structure as the technical concept and exerting the same effects are all included in the technical scope of the present disclosure. In addition, within the scope of the present disclosure, various modifications that can be imagined by those skilled in the art to the embodiments, and other methods constructed by combining some of the constituent elements of the embodiments are also included in the scope of the present disclosure.
Claims
1. A negative electrode sheet, comprising: current collector; and a negative electrode active material layer stacked with the current collector; The negative electrode active material layer comprises at least two stacked negative electrode active material layers, the negative electrode active material layer comprises a negative electrode active material selected from natural graphite or artificial graphite, and the at least two negative electrode active material layers comprise at least one negative electrode active material layer containing natural graphite and at least one negative electrode active material layer containing artificial graphite. 2 . The negative electrode sheet according to claim 1 , wherein the negative electrode sheet has at least one blind hole, and the blind hole at least passes through at least a portion of the negative electrode active material layer containing natural graphite.
3. The negative electrode sheet according to claim 2, wherein the negative electrode active material layer comprises a first negative electrode active material layer and a second negative electrode active material layer stacked in sequence, the first negative electrode active material layer is located between the second negative electrode active material layer and the current collector, the negative electrode active material in the first negative electrode active material layer comprises natural graphite, and the negative electrode active material in the second negative electrode active material layer comprises artificial graphite. 4 . The negative electrode sheet according to claim 3 , wherein the opening of the blind hole is located on a side of the first negative electrode active material layer facing the second negative electrode active material layer, and the blind hole contains the negative electrode active material in the second negative electrode active material layer.
5. The negative electrode plate according to claim 4, wherein the depth of the blind hole is 1-80%, preferably 10-70%, and more preferably 20-60% of the thickness of the first negative electrode active material layer; and / or The blind hole has a diameter of 20-300 μm, preferably 80-150 μm; and / or The spacing between the blind holes is 100-1000 μm, preferably 400-500 μm; and / or The blind hole has a pore formation rate of 0.1%-10%, preferably 2%-4%.
6. The negative electrode sheet according to any one of claims 3 to 5, wherein the thickness of the first negative electrode active material layer is 10-200 μm, preferably 50-100 μm; and / or The thickness of the second negative electrode active material layer is 10-200 μm, preferably 50-100 μm. 7 . The negative electrode sheet according to claim 3 , wherein the thickness of the first negative electrode active material layer is greater than the thickness of the second negative electrode active material layer.
8. The negative electrode sheet according to claim 2, wherein the negative electrode active material layer comprises a first negative electrode active material layer, a second negative electrode active material layer and a third negative electrode active material layer stacked in sequence, the first negative electrode active material layer is located between the second negative electrode active material layer and the current collector, the negative electrode active material in the first negative electrode active material layer comprises artificial graphite, the negative electrode active material in the second negative electrode active material layer comprises natural graphite, and the negative electrode active material in the third negative electrode active material layer comprises artificial graphite.
9. The negative electrode sheet according to claim 8, wherein the blind hole penetrates the second negative electrode active material layer and a portion of the first negative electrode active material layer, the opening of the blind hole is located on the side of the second negative electrode active material layer facing the third negative electrode active material layer, and the blind hole contains the negative electrode active material in the third negative electrode active material layer.
10. The negative electrode sheet according to claim 9, wherein the depth of the blind hole is 1-80%, preferably 10-70%, more preferably 30-60%, of the thickness of the second negative electrode active material layer plus the thickness of the first negative electrode active material layer; and / or The blind hole has a diameter of 20-500 μm, preferably 100-150 μm; and / or The spacing between the blind holes is 100-1500 μm, preferably 400-500 μm; and / or The blind hole has a pore formation rate of 0.1%-10%, preferably 2%-4%.
11. The negative electrode sheet according to any one of claims 8 to 10, wherein the thickness of the first negative electrode active material layer is 10-100 μm, preferably 60-100 μm; and / or The thickness of the second negative electrode active material layer is 10-200 μm, preferably 60-100 μm; and / or The thickness of the third negative electrode active material layer is 10-100 μm, preferably 20-40 μm.
12. The negative electrode sheet according to any one of claims 8-11, wherein the thickness of the second negative electrode active material layer is greater than the thickness of the first negative electrode active material layer; and / or the thickness of the second negative electrode active material layer is greater than the thickness of the third negative electrode active material layer.
13. The negative electrode plate according to any one of claims 1-12, wherein the orthographic projection of the bottom surface of the blind hole on the first plane is located within the orthographic projection of the opening of the blind hole on the first plane, and the first plane is perpendicular to the depth direction of the blind hole.
14. The negative electrode sheet according to any one of claims 1 to 13, wherein the median particle size of the artificial graphite in the negative electrode active material layer containing artificial graphite is 5-20 μm; and / or The median particle size of the natural graphite in the negative electrode active material layer containing natural graphite is 5-20 μm.
15. A battery comprising the negative electrode sheet according to any one of claims 1 to 14.
16. An electrical device comprising the battery according to claim 15, wherein the battery is used to provide electrical energy.
Citation Information
Patent Citations
Pole piece punching device and drying equipment
CN216084936U
Negative plate, preparation method thereof and battery
CN114583295A
Negative plate and battery comprising same
CN115954436A
Negative pole piece and lithium ion battery
CN116759533A
Secondary battery and apparatus including the secondary battery
US20210336244A1