Method for preparing solar cell, solar cell, and cell module
By forming a passivation layer and a conductive layer on the silicon substrate of the solar cell, and etching the edge regions and sides of the conductive layer, the copper deposition problem caused by the size error of the carrier plate and the cell is solved, and the conversion of the solar cell is improved Efficiency and component reliability.
Patent Information
- Application Number
- PCT/CN2024/089484
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-06-02
- Filing Date
- 2024-04-24
- Publication Date
- 2024-12-05
AI Technical Summary
During the deposition of transparent conductive layers, copper deposits in the gaps caused by the size error of the carrier plate and the cell are caused by heavy metal diffusion, reducing conversion efficiency and affecting component reliability.
A passivation layer and a conductive layer are formed on the silicon substrate, and a break is formed by etching the edge areas and sides of the conductive layer to avoid direct contact between the copper and the silicon layer, ensuring that the conductive layer on the entire surface is deposited and heavy metal is avoided in the gap.
It reduces the leakage and parallel resistance of solar cells, improves the filling factor and conversion efficiency, eliminates the component failure problems caused by heavy metal diffusion to the greatest extent, and improves the reliability of the components.
Smart Images

Figure CN2024089484_05122024_PF_FP_ABST
Abstract
Description
Method for preparing solar cell, solar cell and solar cell assembly
[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on June 2, 2023, with application number 202310664457.1 and invention name “Method for preparing solar cells, solar cells and battery components”, the entire contents of which are incorporated by reference into this application. Technical Field
[0002] The present invention relates to the technical field of solar cells, and in particular to a method for preparing a solar cell, a solar cell and a cell assembly. Background Art
[0003] Copper interconnect technology is an effective means of reducing the metallization cost of solar cells. Using copper interconnect technology to replace traditional screen silver paste printing technology to prepare grid electrodes is one of the most cutting-edge and popular technologies in the photovoltaic industry.
[0004] In the existing solar cell preparation process, during the deposition of the transparent conductive layer (such as ITO or TCO), in order to prevent wrap-around plating (i.e., growing a transparent conductive layer of a certain thickness on the non-coated surface), which causes the P-side and N-side of the cell to be conductive, thereby causing cell leakage and parallel resistance failure, a carrier is set in the edge area of the P-side and the side of the cell to avoid the formation of a transparent conductive layer in the edge area of the P-side and the side of the cell, thereby solving the problem of cell failure caused by wrap-around plating.
[0005] However, there are inevitably some discrepancies between the substrate and the cell dimensions. This means there will inevitably be a gap between the substrate and the cell. When depositing a metal seed layer (such as a Cu seed layer) during PVD, copper will inevitably be deposited in this gap. Copper, as a heavy metal, easily diffuses into the silicon layer, where it forms recombination centers within the silicon wafer, reducing the cell's conversion efficiency and impacting module reliability.
[0006] Summary of the Invention
[0007] The present invention aims to at least partially address one of the technical problems in the related art. To this end, the present invention provides a method for manufacturing a solar cell, a solar cell, and a solar cell module. This invention reduces the solar cell's leakage current (i.e., IRev2), improves the solar cell's parallel resistance (Rsh) and fill factor (FF), and increases conversion efficiency by approximately 0.05%. It also minimizes module failures caused by heavy metal diffusion, improving module reliability.
[0008] In one aspect of the present invention, a method for preparing a solar cell is provided. According to an embodiment of the present invention, the method comprises:
[0009] forming a first passivation layer on one side of the silicon substrate, and forming a second passivation layer on a side of the silicon substrate away from the first passivation layer;
[0010] forming an N-type amorphous silicon layer on a side of the first passivation layer away from the silicon substrate, and forming a P-type amorphous silicon layer on a side of the second passivation layer away from the silicon substrate;
[0011] forming a first conductive layer on a side of the N-type amorphous silicon layer away from the first passivation layer, and forming a second conductive layer on a side of the P-type amorphous silicon layer away from the second passivation layer;
[0012] forming a first metal seed layer on a side of the first conductive layer away from the N-type amorphous silicon layer, and forming a second metal seed layer on a side of the second conductive layer away from the P-type amorphous silicon layer;
[0013] Electroplating forms a first electrode layer on a side of the first metal seed layer away from the first conductive layer, and forms a second electrode layer on a side of the second metal seed layer away from the second conductive layer;
[0014] The edge area of the second conductive layer and / or the conductive layer formed by plating on the side of the cell are etched.
[0015] According to the method for preparing a solar cell according to an embodiment of the present invention, during the deposition of the first conductive layer and the second conductive layer, the entire surface of the first conductive layer and the second conductive layer can be formed. The conductive layer is an ideal barrier layer, thereby avoiding the problem of heavy metal (such as copper) being deposited in the gap between the carrier and the cell during the PVD deposition of the metal seed layer in the prior art, and avoiding direct contact between the heavy metal and the silicon layer. In the subsequent step, by etching the edge area of the second conductive layer and / or the conductive layer formed by plating around the side of the cell, a short circuit is formed between the P side and the N side of the cell, thereby preventing the P side and the N side of the cell from being conductive. As a result, the leakage of the solar cell (i.e., IRev2) is reduced, the parallel resistance (Rsh) and fill factor (FF) of the solar cell are improved, and the conversion efficiency is increased by approximately 0.05%. At the same time, the problem of component failure caused by heavy metal diffusion is eliminated to the greatest extent, and the reliability of the component end is improved.
[0016] In addition, the method for preparing a solar cell according to the above embodiment of the present invention may also have the following additional technical features:
[0017] In some embodiments of the present invention, the etching of the edge area of the second conductive layer and / or the conductive layer formed by plating on the side of the battery cell includes: forming an etching paste on the edge area of the second conductive layer and / or the conductive layer formed by plating on the side of the battery cell; baking the battery cell formed with the etching paste; and cleaning the battery cell with spraying water to clean the etched edge area of the second conductive layer and / or the conductive layer formed by plating on the side of the battery cell.
[0018] In some embodiments of the present invention, the width of the edge region of the second conductive layer is 150 μm-500 μm.
[0019] In some embodiments of the present invention, the baking temperature is 150-200° C., and the baking time is 40s-90s.
[0020] In some embodiments of the present invention, the spraying pressure of the spraying water is 2-3 kg / cm 2 .
[0021] In some embodiments of the present invention, a PVD magnetron sputtering method is used to deposit the first conductive layer on the entire surface of the N-type amorphous silicon layer away from the first passivation layer.
[0022] In some embodiments of the present invention, a PVD magnetron sputtering method is used to deposit the second conductive layer on the entire surface of the P-type amorphous silicon layer away from the second passivation layer.
[0023] In some embodiments of the present invention, the forming of a first metal seed layer on a side of the first conductive layer away from the N-type amorphous silicon layer and the forming of a second metal seed layer on a side of the second conductive layer away from the P-type amorphous silicon layer include: using a PVD magnetron sputtering method to deposit an initial first metal seed layer on a side of the first conductive layer away from the N-type amorphous silicon layer, and depositing an initial second metal seed layer on a side of the second conductive layer away from the P-type amorphous silicon layer; forming a first photosensitive resin layer on a side of the initial first metal seed layer away from the first conductive layer, and forming a second photosensitive resin layer on a side of the initial second metal seed layer away from the second conductive layer; and performing laser printing, exposure, and development on the first photosensitive resin layer and the second photosensitive resin layer according to a preset electrode pattern.
[0024] In some embodiments of the present invention, the electroplating to form a first electrode layer on a side of the first metal seed layer away from the first conductive layer and the forming of a second electrode layer on a side of the second metal seed layer away from the second conductive layer include: using an electroplating solution to sequentially electroplating to form the first electrode layer and a first protective layer on a side of the first metal seed layer away from the first conductive layer, and sequentially electroplating to form the second electrode layer and a second protective layer on a side of the second metal seed layer away from the second conductive layer; using an alkaline solution to remove the remaining first photosensitive adhesive layer and the second photosensitive adhesive layer; and using an acid solution to remove the first metal seed layer and the second metal seed layer in the non-electrode area.
[0025] In some embodiments of the present invention, before forming the first passivation layer and the second passivation layer, the silicon substrate is first subjected to a texturing process.
[0026] In some embodiments of the present invention, the first passivation layer and the second passivation layer are intrinsic amorphous silicon layers.
[0027] In some embodiments of the present invention, the thickness of the first passivation layer is 3 nm to 6 nm.
[0028] In some embodiments of the present invention, the thickness of the second passivation layer is 3 nm to 9 nm.
[0029] In some embodiments of the present invention, the thickness of the N-type amorphous silicon layer is 5 nm to 10 nm.
[0030] In some embodiments of the present invention, the thickness of the P-type amorphous silicon layer is 5 nm to 15 nm.
[0031] 16. The method according to any one of claims 1 to 7, in some embodiments of the present invention, wherein the first conductive layer and the second conductive layer are ITO.
[0032] In some embodiments of the present invention, the thickness of the first conductive layer is 90 nm to 110 nm.
[0033] In some embodiments of the present invention, the thickness of the second conductive layer is 90 nm to 110 nm.
[0034] In some embodiments of the present invention, the thickness of the first metal seed layer is 100 nm to 250 nm.
[0035] In some embodiments of the present invention, the thickness of the second metal seed layer is 100 nm to 250 nm.
[0036] In its second aspect, the present invention provides a solar cell. According to an embodiment of the present invention, the solar cell is produced using the method described in the above embodiment. This improves the solar cell's parallel resistance (Rsh) and fill factor (FF), boosting conversion efficiency by approximately 0.05%. It also minimizes component failures caused by heavy metal diffusion, improving component reliability.
[0037] In a third aspect, the present invention provides a battery assembly. According to an embodiment of the present invention, the battery assembly includes the solar cell described in the above embodiment. Thus, the battery assembly has all the advantages of the above solar cell, which will not be elaborated here.
[0038] Additional aspects and advantages of the present invention will be set forth in part in the description which follows and, in part, will be obvious from the description which follows, or may be learned by practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] The above and / or additional aspects and advantages of the present invention will become apparent and readily understood from the description of the embodiments with reference to the following drawings, in which:
[0040] FIG1 is a schematic diagram of a PVD electroplated transparent conductive layer in the prior art;
[0041] FIG2 is a flow chart of a method for preparing a solar cell according to an embodiment of the present invention;
[0042] FIG3 is a schematic structural diagram of a solar cell prepared in step S410 according to an embodiment of the present invention;
[0043] FIG4 is a schematic structural diagram of a solar cell prepared in step S420 according to an embodiment of the present invention;
[0044] FIG5 is a schematic structural diagram of a solar cell prepared in step S430 according to an embodiment of the present invention;
[0045] FIG6 is a schematic structural diagram of a solar cell prepared in step S530 according to an embodiment of the present invention;
[0046] FIG7 is a schematic diagram of the structure of a solar cell manufactured using the method according to an embodiment of the present invention.
[0047] Figure numerals: 100 - solar cell, 101 - silicon substrate, 102 - first passivation layer, 103 - second passivation layer, 104 - N-type amorphous silicon layer, 105 - P-type amorphous silicon layer, 106 - first conductive layer, 107 - second conductive layer, 108 - first metal seed layer, 109 - second metal seed layer, 110 - first electrode layer, 111 - second electrode layer, 112 - first protective layer, 113 - second protective layer, 114 - first photosensitive adhesive layer, 115 - second photosensitive adhesive layer, 200 - carrier, 300 - target atoms, 400 - upper target, 500 - lower target. DETAILED DESCRIPTION
[0048] The following embodiments of the present invention are described in detail. The embodiments described below are exemplary and are only used to explain the present invention, and are not to be construed as limiting the present invention. Where specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this field or the product specifications are used. Where the manufacturer of the reagents or instruments is not specified, all are conventional products that can be obtained commercially.
[0049] In the prior art, in order to prevent the P-side and N-side of the cell from being conductive due to wrap-around plating (i.e., growing a transparent conductive layer of a certain thickness on the non-coated surface), thereby causing the cell to leak and the parallel resistor to fail, a carrier 200 is generally provided at the edge area of the P-side and the side of the cell, as shown in FIG1 , to avoid the formation of a transparent conductive layer at the edge area of the P-side and the side of the cell, thereby solving the problem of cell failure caused by wrap-around plating. However, there will inevitably be a certain error in the size of the carrier and the cell, that is, there will inevitably be a certain gap between the carrier and the cell. When depositing a metal seed layer (e.g., a Cu seed layer) in PVD, copper will inevitably be deposited in the gap. Copper, as a heavy metal, is very easy to diffuse into the silicon layer. The diffused copper will form a recombination center inside the silicon wafer, thereby reducing the conversion efficiency of the cell and affecting the reliability of the component end. In FIG1 , 100 is a solar cell, 200 is a carrier, 300 is a target atom, 400 is an upper target, and 500 is a lower target. The width a of the carrier in the edge area of the cell is generally about 900 μm.
[0050] In view of this, in one aspect of the present invention, with reference to Figures 2-7, a method for preparing a solar cell is proposed. According to an embodiment of the present invention, the method includes: forming a first passivation layer 102 on one side of a silicon substrate 101, and forming a second passivation layer 103 on a side of the silicon substrate 101 away from the first passivation layer 102; forming an N-type amorphous silicon layer 104 on a side of the first passivation layer 102 away from the silicon substrate 101, and forming a P-type amorphous silicon layer 105 on a side of the second passivation layer 103 away from the silicon substrate 101; forming a first conductive layer 106 on a side of the N-type amorphous silicon layer 104 away from the first passivation layer 102, and forming a P-type amorphous silicon layer 105 on a side of the P-type amorphous silicon layer 105 away from the second passivation layer 103. The method further comprises forming a second conductive layer 107 by electroplating on the side of the first conductive layer 106 away from the N-type amorphous silicon layer 104, forming a first metal seed layer 108 on the side of the second conductive layer 107 away from the P-type amorphous silicon layer 105, forming a first electrode layer 110 by electroplating on the side of the first metal seed layer 108 away from the first conductive layer 106, and forming a second electrode layer 111 on the side of the second metal seed layer 109 away from the second conductive layer 107, and etching the edge area of the second conductive layer 107 and / or the conductive layer formed by plating around the side of the solar cell. As a result, the leakage of the solar cell (i.e., IRev2) is reduced, the parallel resistance (Rsh) and fill factor (FF) of the solar cell are improved, and the conversion efficiency is increased by approximately 0.05%. At the same time, the problem of component failure caused by heavy metal diffusion is eliminated to the greatest extent, and the reliability of the component end is improved.
[0051] The following is a detailed explanation of the principle by which the method for preparing solar cells proposed by the present invention can achieve the above-mentioned beneficial effects:
[0052] Specifically, referring to FIG. 2 , the above method includes the following steps:
[0053] S100: forming a first passivation layer and a second passivation layer
[0054] In this step, a first passivation layer 102 is formed on one side of the silicon substrate 101 , and a second passivation layer 103 is formed on a side of the silicon substrate 101 away from the first passivation layer 102 .
[0055] According to some embodiments of the present invention, the silicon substrate 101 may be textured to remove impurities and mechanical damage layers on the surface of the silicon substrate 101 to form a positive pyramid texture surface. For example, the size of the pyramid may be 2 μm to 8 μm.
[0056] In an embodiment of the present invention, the specific types of the first passivation layer 102 and the second passivation layer 103 are not particularly limited. For example, they can each be an intrinsic amorphous silicon layer. The method for preparing the first passivation layer 102 and the second passivation layer 103 is also not particularly limited. For example, the first passivation layer 102 and the second passivation layer 103 can be prepared by PECVD (plasma enhanced chemical vapor deposition). Specifically, the thickness of the first passivation layer 102 can be 3nm to 6nm; and / or the thickness of the second passivation layer 103 can be 3nm to 9nm.
[0057] S200: Forming an N-type amorphous silicon layer and a P-type amorphous silicon layer
[0058] In this step, an N-type amorphous silicon layer 104 is formed on a side of the first passivation layer 102 away from the silicon substrate 101 , and a P-type amorphous silicon layer 105 is formed on a side of the second passivation layer 103 away from the silicon substrate 101 .
[0059] In embodiments of the present invention, the method for preparing the N-type amorphous silicon layer 104 and the P-type amorphous silicon layer 105 is not particularly limited. For example, both the N-type amorphous silicon layer 104 and the P-type amorphous silicon layer 105 can be prepared by PECVD. For specific process parameters, reference can be made to the methods for preparing the N-type amorphous silicon layer 104 and the P-type amorphous silicon layer 105 in related art. According to some specific embodiments of the present invention, the thickness of the N-type amorphous silicon layer 104 can be 5 nm to 10 nm; and / or the thickness of the P-type amorphous silicon layer 105 can be 5 nm to 15 nm.
[0060] S300: forming a first conductive layer and a second conductive layer
[0061] In this step, a first conductive layer 106 is deposited on the entire surface of the N-type amorphous silicon layer 104 away from the first passivation layer 102 by using a PVD magnetron sputtering method; and / or, a second conductive layer 107 is deposited on the entire surface of the P-type amorphous silicon layer 105 away from the second passivation layer 103 by using a PVD magnetron sputtering method.
[0062] In the embodiments of the present invention, the types of the first conductive layer 106 and the second conductive layer 107 are not particularly limited. For example, they may be ITO (indium tin oxide) transparent conductive films. Specific preparation process parameters may refer to the preparation methods of the first conductive layer 106 and the second conductive layer 107 in related art. According to some specific embodiments of the present invention, the thickness of the first conductive layer 106 and the second conductive layer 107 may be independently 90 nm to 110 nm.
[0063] S400: forming a first metal seed layer and a second metal seed layer
[0064] In this step, a first metal seed layer 108 is formed on a side of the first conductive layer 106 away from the N-type amorphous silicon layer 104 , and a second metal seed layer 109 is formed on a side of the second conductive layer 107 away from the P-type amorphous silicon layer 105 , as shown in FIG3 .
[0065] In the embodiment of the present invention, the method for preparing the first metal seed layer 108 and the second metal seed layer 109 is not particularly limited. As a specific example, S400 includes the following steps:
[0066] S410: Using a PVD magnetron sputtering method, an initial first metal seed layer 108 is deposited on a side of the first conductive layer 106 away from the N-type amorphous silicon layer 104, and an initial second metal seed layer 109 is deposited on a side of the second conductive layer 107 away from the P-type amorphous silicon layer 105, as shown in FIG3.
[0067] S420 : forming a first photosensitive adhesive layer 114 on a side of the initial first metal seed layer 108 away from the first conductive layer 106 , and forming a second photosensitive adhesive layer 115 on a side of the initial second metal seed layer 109 away from the second conductive layer 107 , as shown in FIG4 .
[0068] S430: Laser printing is performed on the first and second photosensitive resin layers 114 and 115 according to the preset electrode pattern. The non-gridline areas (i.e., non-electrode areas) are exposed. Exposure triggers a series of cross-linking and polymerization reactions in the photosensitive resin film, rendering it insoluble in a weakly alkaline solution. The unexposed photosensitive resin areas are then cleaned and removed using a weakly alkaline solution (e.g., Na2CO3 solution) to form grooves, exposing the underlying metal seed layer and achieving development, as shown in FIG5 .
[0069] The principle is as follows: the photocurable components of liquid photosensitive adhesive include a photoinitiator, alkali-soluble macromolecules, and non-alkali-soluble reactive monomers. Upon exposure to ultraviolet light, the photoinitiator decomposes in the exposed portion, generating free radicals that initiate polymerization. The resulting polymerized photosensitive adhesive layer increases in molecular weight and forms a three-dimensional network structure, which reduces its solubility in weakly alkaline solutions, making it less soluble. In the unexposed portion of the adhesive layer, cross-linking and polymerization do not occur, and the alkali-soluble hydrophilic groups (carboxyl groups -COOH) react with the alkali solution, dissolving it.
[0070] It should be noted that printing, that is, exposure, is an important step in the pattern transfer of photosensitive adhesive. Its function is that under the irradiation of ultraviolet light, the polymerized monomer molecules in the photosensitive adhesive layer absorb light energy to produce a photopolymerization reaction, thereby forming the required circuit pattern.
[0071] According to some specific embodiments of the present invention, the thickness of the first metal seed layer 108 and the second metal seed layer 109 are independently 100 nm to 250 nm. Furthermore, the four edges and corners of the battery cell obtained in S430 can be wrapped with edge glue, with the width of the edge glue being less than or equal to 50 μm and the thickness of the edge glue being 10 μm to 15 μm.
[0072] S500: forming a first electrode layer and a second electrode layer
[0073] In this step, a first electrode layer 110 is formed by electroplating on a side of the first metal seed layer 108 away from the first conductive layer 106 , and a second electrode layer 111 is formed on a side of the second metal seed layer 109 away from the second conductive layer 107 .
[0074] As a specific example, S500 includes the following steps:
[0075] S510: Using an electroplating solution (e.g., a copper sulfate electroplating solution) to electroplate on a side of the first metal seed layer 108 away from the first conductive layer 106 to form a first electrode layer 110, and electroplate on a side of the second metal seed layer 109 away from the second conductive layer 107 to form a second electrode layer 111; then using an electroplating solution (e.g., a tin methanesulfonate electroplating solution) to electroplate on a side of the first electrode layer 110 away from the first metal seed layer 108 to form a first protective layer 112, and electroplate on a side of the second electrode layer 111 away from the second metal seed layer 109 to form a second protective layer 113.
[0076] According to some embodiments of the present invention, during the electroplating of the electrode layer, the electrolyte may be a CuSO4 solution, and the concentration of the CuSO4 solution may be 20 to 100 g / L. Furthermore, additives may be added to the CuSO4 solution. According to some specific embodiments of the present invention, the thickness of the formed copper grid line layer may be 8 to 10 μm.
[0077] According to some embodiments of the present invention, during the formation of the protective layer, when the metal forming the protective layer is tin, the Sn in the electrolyte 2+ The concentration of methylsulfonic acid can be 10-50 g / L, and the concentration of methanesulfonic acid can be 100-300 g / L. Further, additives can be added to the electrolyte. According to some specific embodiments of the present invention, the thickness of the formed tin layer can be 2 μm-5 μm.
[0078] It should be noted that in this step, the electrode layer and the protective layer are only electroplated in the grooves formed by exposure and development, that is, the electrode layer and the protective layer are only electroplated in the area without the photosensitive resin layer, and the electrode layer and the protective layer cannot be electroplated in the photosensitive resin layer area.
[0079] S520 : removing the remaining first photosensitive adhesive layer 114 and the second photosensitive adhesive layer 115 using an alkaline solution.
[0080] In this step, the remaining photosensitive resin layer and mask material are removed in an alkaline solution (eg, NaOH solution, KOH solution, etc.) According to some specific embodiments of the present invention, the concentration of the NaOH solution may be 10-20 g / L.
[0081] S530 : using an acid solution to remove the first metal seed layer 108 and the second metal seed layer 109 in the non-electrode region.
[0082] As a specific example, the metal seed layer in the non-gateline area can be removed in a mixed solution of dilute sulfuric acid and hydrogen peroxide to expose the conductive layer (ITO or TCO), as shown in Figure 6. According to some specific embodiments of the present invention, the concentration of H2SO4 in the acid solution can be 2.5g / L, and the concentration of H2O2 in the etching solution can be 10g / L.
[0083] S600: Etching the edge area of the second conductive layer and / or the conductive layer formed by plating on the side of the cell
[0084] In this step, the edge regions of the second conductive layer 107 and / or the conductive layer formed by the side plating of the cell are etched, as shown in FIG7 , to form a short circuit between the P-side and N-side of the cell, thereby preventing the P-side and N-side of the cell from being conductive, thus preventing cell leakage and shunt resistor failure. Preferably, only etching the edge regions of the second conductive layer 107 can achieve the purpose of preventing the P-side and N-side of the cell from being conductive, which is easier to achieve in the P-side etching process and has less impact on the cell.
[0085] According to some embodiments of the present invention, step S600 includes the following steps:
[0086] S610: Print or apply etching paste on the edge area of the second conductive layer 107 and / or the conductive layer formed by plating on the side of the battery cell.
[0087] According to some embodiments of the present invention, the width b of the edge region of the second conductive layer 107 is 150 μm to 500 μm (e.g., 150 / 200 / 250 / 300 / 350 / 400 / 450 / 500 μm), preferably 150 μm to 300 μm. Thus, a width of 150 μm to 500 μm of the conductive layer can be etched away from the edge region of the second conductive layer 107 to prevent conduction between the P-side and N-side of the solar cell. In the prior art, the width a of the substrate at the edge region of the second conductive layer 107 is generally approximately 900 μm. This significantly reduces the width of the conductive layer etched away in the present invention, allowing for greater retention of the conductive layer, thereby further improving the parallel resistance (Rsh), fill factor (FF), and conversion efficiency of the solar cell.
[0088] In the embodiments of the present invention, the specific composition of the etching paste is not particularly limited and can be flexibly selected according to actual needs in the art. Preferably, a phosphoric acid-based etching paste is used. As a specific example, the etching paste mainly comprises phosphoric acid, dibutyl glycol ether, additives, and water. It should be noted that the etching paste is commercially available.
[0089] S620: The cell with the etching paste is baked, for example, in a drying oven, to allow the etching paste to react with the conductive layer (ITO or TCO). According to some embodiments of the present invention, the baking temperature is 150-200° C. (for example, 150 / 160 / 170 / 180 / 190 / 200° C.) and the baking time is 40s-90s (for example, 40 / 50 / 60 / 70 / 80 / 90s).
[0090] S630: Use spray water to clean the cell to remove the edge area of the etched second conductive layer 107 and / or the conductive layer formed by the plating on the side of the cell. According to some embodiments of the present invention, the spray pressure of the spray water is 2-3 kg / cm 2 (For example, it can be 2 / 2.2 / 2.4 / 2.6 / 2.8 / 3kg / cm 2 ).
[0091] In summary, the present invention can form the entire surface of the first conductive layer 106 and the second conductive layer 107 during the deposition process. The conductive layer is an ideal barrier layer, thereby avoiding the problem of heavy metal (such as copper) being deposited in the gap due to the gap between the carrier and the cell in the process of PVD deposition of the metal seed layer in the prior art, and avoiding direct contact between the heavy metal and the silicon layer. In the subsequent steps, a short circuit is formed between the P side and the N side of the cell by etching the edge area of the second conductive layer 107 and / or the conductive layer formed by plating around the side of the cell, thereby avoiding the P side and the N side of the cell from being conductive. As a result, the leakage of the solar cell (i.e., IRev2) is reduced, the parallel resistance (Rsh) and fill factor (FF) of the solar cell are improved, and the conversion efficiency is improved by about 0.05%. At the same time, the component failure problem caused by heavy metal diffusion is eliminated to the greatest extent, and the reliability of the component end is improved.
[0092] In its second aspect, the present invention provides a solar cell. According to an embodiment of the present invention, the solar cell is produced using the method described in the above embodiment. This improves the solar cell's parallel resistance (Rsh) and fill factor (FF), boosting conversion efficiency by approximately 0.05%. It also minimizes component failures caused by heavy metal diffusion, improving component reliability.
[0093] In a third aspect, the present invention provides a battery assembly. According to an embodiment of the present invention, the battery assembly includes the solar cell of the above embodiment. Thus, the battery assembly has all the advantages of the above solar cell, which will not be repeated here.
[0094] Specifically, a battery module is a finished module with power output function produced by welding solar cells in series or parallel, and then undergoing processes such as lamination and packaging. The battery module includes photovoltaic glass, encapsulation film, battery cells, encapsulation film, backplane, etc.
[0095] The present invention will be further described in detail below with reference to specific examples. The examples are intended to illustrate the present invention only and are not intended to limit the present invention. Any process parameters, operating methods, and detection methods not mentioned herein are conventional methods used by those skilled in the art, or conventional parameters can be obtained through limited experiments.
[0096] Example 1
[0097] This embodiment provides a method for preparing a solar cell, comprising the following steps:
[0098] (1) Texturing and cleaning: Texturing and cleaning are performed on N-type single crystal silicon wafers to form a uniform “positive pyramid” texture surface on the surface of the silicon wafer. The size of the pyramid is in the range of 2μm to 8μm.
[0099] (2) PECVD-intrinsic amorphous silicon film deposition: A PECVD plasma deposition device is used to deposit a first intrinsic amorphous silicon film layer with a thickness of about 4 nm on the front side of the silicon wafer after texturing and cleaning, and a second intrinsic amorphous silicon film layer with a thickness of about 6 nm on the back side of the silicon wafer.
[0100] (3) PECVD-amorphous silicon film deposition: A PECVD plasma deposition device is used to deposit a phosphorus-doped amorphous silicon layer with a thickness of about 6.5 nm on the surface of the first intrinsic amorphous silicon film layer, and a boron-doped amorphous silicon layer with a thickness of about 10 nm on the surface of the second intrinsic amorphous silicon film layer.
[0101] (4) PVD-ITO deposition: Using PVD magnetron sputtering equipment, an ITO conductive film with a thickness of approximately 100 nm is deposited on the entire surface of the phosphorus-doped amorphous silicon layer, and an ITO conductive film with a thickness of approximately 100 nm is deposited on the entire surface of the boron-doped amorphous silicon layer. The N side is the front side, and the P side is the back side.
[0102] (5) PVD-Cu deposition: A copper seed layer thin film with a thickness of about 160 nm is deposited on the surface of the ITO conductive film on the P side and N side using PVD magnetron sputtering equipment.
[0103] (6) Coating: Coat the surface of the copper seed layer film on the front and back sides with photosensitive adhesive, covering the seed layer on both sides. The thickness of the photosensitive adhesive is controlled to be about 12 μm.
[0104] (7) Laser printing: The predetermined pattern is printed on the front and back of the photosensitive film by laser according to the designed grid line pattern, and the area outside the set grid line area is exposed. After the photosensitive film is exposed, a series of cross-linking polymerization reactions will occur, making it insoluble in weak alkaline solution.
[0105] (8) Development: Use a weakly alkaline Na2CO3 solution to clean and remove the unexposed photosensitive resin area to expose the underlying seed layer and form a groove.
[0106] (9) Edge wrapping: Wrap the four edges and corner positions of the yellow film obtained in step (8) with edge wrapping glue. The width of the edge wrapping glue is about 30 μm, and the thickness of the edge wrapping glue is about 12 μm.
[0107] (10) Electroplating: Electroplating copper grid lines in a 60g / L copper sulfate electroplating solution. The thickness of the copper grid lines is about 9μm. 2+ The tin protective layer is electroplated in a tin methanesulfonate electroplating solution with a concentration of about 30 g / L, and the thickness of the tin grid line is about 3 μm.
[0108] (11) De-filming and etching: First, remove the remaining photosensitive resin in a NaOH solution with a concentration of about 15g / L, and then remove the copper seed layer in the non-gate line area in a mixed solution of dilute sulfuric acid and hydrogen peroxide. The concentration of H2SO4 in the acid solution is about 2.5g / L, and the concentration of H2O2 is about 10g / L.
[0109] (12) ITO re-engraving: Use a coating machine to evenly print Xinghan Technology's etching paste on the edge of the ITO conductive film on the P side of the battery cell. The etching paste is about 200μm wide and then baked. The wafer coated with the etching paste is baked at a temperature of about 180℃ for about 60s; then spray water washing is performed with a spray pressure of about 2.5kg / cm 2 ,drying.
[0110] (13) Light Injection + IV Test: After film stripping and re-etching, the cells were subjected to light injection at a temperature of approximately 210°C for approximately 90 seconds. The finished cells were then tested for leakage current Irev2, parallel resistance Rsh, fill factor FF, and conversion efficiency. The test results are shown in Table 1.
[0111] Example 2
[0112] The difference between this embodiment and embodiment 1 is that:
[0113] (12) ITO re-engraving: Use a coating machine to evenly print the etching paste on the edge of the ITO conductive film on the P side of the battery cell. The etching paste width is about 150μm. Then bake the film coated with the etching paste at a temperature of about 150℃ for about 90s. Then spray water washing with a spray pressure of about 3kg / cm 2 ,drying.
[0114] The rest of the contents are the same as those in Example 1.
[0115] Example 3
[0116] The difference between this embodiment and embodiment 1 is that:
[0117] (12) ITO re-engraving: Use a coating machine to evenly print the etching paste on the edge of the ITO conductive film on the P side of the battery cell. The etching paste width is about 300 μm. Then bake the film coated with the etching paste at a temperature of about 200 ° C for about 40 seconds. Then spray water washing with a spray pressure of about 2 kg / cm 2 ,drying.
[0118] The rest of the contents are the same as those in Example 1.
[0119] Example 4
[0120] The difference between this embodiment and embodiment 1 is that:
[0121] (12) ITO re-engraving: Use a coating machine to evenly print the etching paste on the edge of the ITO conductive film on the P side of the cell. The etching paste width is about 500 μm. Then bake the film coated with the etching paste at a temperature of about 180 ° C for about 60 seconds. Then spray water washing with a spray pressure of about 2.5 kg / cm 2 ,drying.
[0122] The rest of the contents are the same as those in Example 1.
[0123] Comparative Example 1
[0124] The difference between this comparative example and Example 1 is only that:
[0125] (4) PVD-ITO deposition: Before PVD-ITO deposition, a carrier is set up in the edge area of the P surface and the side of the battery cell. Then, a PVD magnetron sputtering device is used to deposit an ITO conductive film with a thickness of about 100 nm on the surface of the phosphorus-doped amorphous silicon layer. At the same time, an ITO conductive film with a thickness of about 100 nm is deposited on the surface of the boron-doped amorphous silicon layer. This avoids the formation of an ITO conductive film in the edge area of the P surface and the side of the battery cell.
[0126] This comparative example does not include the ITO re-etching process in step (12).
[0127] The rest of the contents are the same as those in Example 1.
[0128] Table 1
[0129] It can be seen from Table 1 that, compared with Comparative Example 1, the leakage current IRev2 of Examples 1-4 is significantly reduced, and the parallel resistance Rsh, fill factor FF and conversion efficiency are significantly improved.
[0130] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential" and the like to indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as limiting the present invention.
[0131] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of the technical features being referred to. Thus, a feature identified as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, "plurality" means two or more, unless otherwise specifically defined.
[0132] In the present invention, unless otherwise expressly specified or limited, the terms "mounted," "connected," "connect," "fixed," etc. should be understood broadly. For example, they may refer to fixed connection, detachable connection, or integration; mechanical connection or electrical connection; direct connection or indirect connection through an intermediate medium; internal communication between two components or interaction between two components. Those skilled in the art will understand the specific meanings of the above terms in the present invention based on specific circumstances.
[0133] In the present invention, unless otherwise expressly specified or limited, when a first feature is "above" or "below" a second feature, it may mean that the first and second features are in direct contact, or that the first and second features are in indirect contact through an intermediary. Furthermore, when a first feature is "above," "above," or "above" a second feature, it may mean that the first feature is directly above or diagonally above the second feature, or simply means that the first feature is at a higher level than the second feature. When a first feature is "below," "below," or "below" a second feature, it may mean that the first feature is directly below or diagonally below the second feature, or simply means that the first feature is at a lower level than the second feature.
[0134] In the description of this specification, the reference terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" mean that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art can combine and combine different embodiments or examples described in this specification and features of different embodiments or examples without contradiction.
[0135] Although the embodiments of the present invention have been shown and described above, it will be understood that the above embodiments are illustrative and are not to be construed as limitations on the present invention. A person skilled in the art may change, modify, replace and modify the above embodiments within the scope of the present invention.
Claims
1. A method for preparing a solar cell, characterized in that: The following steps are involved: forming a first passivation layer on one side of the silicon substrate, and forming a second passivation layer on a side of the silicon substrate away from the first passivation layer; forming an N-type amorphous silicon layer on a side of the first passivation layer away from the silicon substrate, and forming a P-type amorphous silicon layer on a side of the second passivation layer away from the silicon substrate; forming a first conductive layer on a side of the N-type amorphous silicon layer away from the first passivation layer, and forming a second conductive layer on a side of the P-type amorphous silicon layer away from the second passivation layer; forming a first metal seed layer on a side of the first conductive layer away from the N-type amorphous silicon layer, and forming a second metal seed layer on a side of the second conductive layer away from the P-type amorphous silicon layer; Electroplating forms a first electrode layer on a side of the first metal seed layer away from the first conductive layer, and forming a second electrode layer on a side of the second metal seed layer away from the second conductive layer; The edge region of the second conductive layer and / or the conductive layer formed by plating on the side of the cell are etched.
2. The method according to claim 1, characterized in that The etching of the edge area of the second conductive layer and / or the conductive layer formed by plating around the side of the cell comprises: Forming an etching paste on the edge region of the second conductive layer and / or the conductive layer formed by plating on the side of the battery cell; Baking the cell formed with the etching paste; The battery cell is cleaned by spraying water, so as to clean off the edge area of the etched second conductive layer and / or the conductive layer formed by plating on the side of the battery cell.
3. The method according to claim 2, characterized in that The width of the edge region of the second conductive layer is 150 μm-500 μm.
4. The method according to claim 2, characterized in that: The baking temperature is 150-200° C., and the baking time is 40s-90s.
5. The method according to claim 2, characterized in that: The spraying pressure of the spraying water is 2-3kg / cm 2 .
6. The method according to claim 1, characterized in that A first conductive layer is formed by depositing the first conductive layer on the entire surface of the N-type amorphous silicon layer away from the first passivation layer using a PVD magnetron sputtering method.
7. The method according to claim 1, characterized in that A second conductive layer is formed by depositing the second conductive layer on the entire surface of the P-type amorphous silicon layer away from the second passivation layer using a PVD magnetron sputtering method.
8. The method according to any one of claims 1 to 7, characterized in that The forming of a first metal seed layer on a side of the first conductive layer away from the N-type amorphous silicon layer and the forming of a second metal seed layer on a side of the second conductive layer away from the P-type amorphous silicon layer comprises: Using a PVD magnetron sputtering method, depositing an initial first metal seed layer on a side of the first conductive layer away from the N-type amorphous silicon layer, and depositing an initial second metal seed layer on a side of the second conductive layer away from the P-type amorphous silicon layer; Forming a first photosensitive adhesive layer on a side of the initial first metal seed layer away from the first conductive layer, and forming a second photosensitive adhesive layer on a side of the initial second metal seed layer away from the second conductive layer; The first photosensitive resin layer and the second photosensitive resin layer are respectively subjected to laser printing, exposure and development according to a preset electrode pattern.
9. The method according to claim 8, characterized in that The step of electroplating the first electrode layer on a side of the first metal seed layer away from the first conductive layer, and forming the second electrode layer on a side of the second metal seed layer away from the second conductive layer comprises: Using an electroplating solution, sequentially electroplating on a side of the first metal seed layer away from the first conductive layer to form the first electrode layer and the first protective layer, and sequentially electroplating on a side of the second metal seed layer away from the second conductive layer to form the second electrode layer and the second protective layer; removing the remaining first photosensitive adhesive layer and the second photosensitive adhesive layer by using an alkaline solution; The first metal seed layer and the second metal seed layer in the non-electrode region are removed by using an acid solution.
10. The method according to any one of claims 1 to 7, characterized in that Before forming the first passivation layer and the second passivation layer, the silicon substrate is firstly subjected to a texturing process.
11. The method according to any one of claims 1 to 7, characterized in that: The first passivation layer and the second passivation layer are intrinsic amorphous silicon layers.
12. The method according to any one of claims 1 to 7, characterized in that The thickness of the first passivation layer is 3 nm to 6 nm.
13. The method according to any one of claims 1 to 7, characterized in that The thickness of the second passivation layer is 3 nm to 9 nm.
14. The method according to any one of claims 1 to 7, characterized in that The thickness of the N-type amorphous silicon layer is 5nm-10nm.
15. The method according to any one of claims 1 to 7, characterized in that The thickness of the P-type amorphous silicon layer is 5nm-15nm.
16. The method according to any one of claims 1 to 7, characterized in that The first conductive layer and the second conductive layer are ITO.
17. The method according to any one of claims 1 to 7, characterized in that The thickness of the first conductive layer is 90 nm to 110 nm.
18. The method according to any one of claims 1 to 7, characterized in that The thickness of the second conductive layer is 90 nm to 110 nm.
19. The method according to any one of claims 1 to 7, characterized in that: The thickness of the first metal seed layer is 100 nm to 250 nm.
20. The method according to any one of claims 1 to 7, characterized in that The thickness of the second metal seed layer is 100 nm to 250 nm.
21. A solar cell, characterized in that: Prepared by the method according to any one of claims 1 to 20.
22. A battery assembly, characterized in that: Comprising the solar cell as claimed in claim 21.
Citation Information
Patent Citations
Heterogeneous junction solar cell edge insulating method
CN106816493A
Preparation method of high-reliability heterojunction solar cell and solar cell
CN116169209A
Method for preparing solar cell, solar cell and cell module
CN116885033A
Solar cell and method for manufacturing solar cell
US20190006534A1