Use of liquid compositions of carbon fillers
By employing a dispersant/solvent couple with specific rheological properties, the formulation of electrodes with high carbon nanotube content is achieved, addressing the limitations of existing methods and enhancing the environmental sustainability and performance of Li-ion battery electrodes.
Patent Information
- Application Number
- PCT/FR2024/050662
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-06-01
- Filing Date
- 2024-05-23
- Publication Date
- 2024-12-05
AI Technical Summary
Current methods for formulating electrodes in Li-ion batteries face challenges with low carbon nanotube content in dispersions, high solvent usage, and viscosity issues, which limit the carbon footprint reduction and stability of carbonaceous filler compositions during storage and transport.
The use of liquid compositions with carbonaceous fillers at 3.5-20% mass content, where the dispersant/solvent couple exhibits Newtonian behavior with a dynamic viscosity less than 1 Pa.s at 0.1 s^-1 and solubility greater than 15%, allowing for stable dispersion and reduced solvent usage.
Enables the formulation of electrodes with high carbon nanotube content, reducing solvent requirements and maintaining stability over time, including temperature variations, thereby improving the environmental impact and performance of battery electrodes.
Smart Images

Figure IMGF000016_0001 
Figure IMGF000014_0001 
Figure IMGF000016_0002
Abstract
Description
[0001] DESCRIPTION
[0002] TITLE: Use of liquid compositions of carbonaceous fillers
[0003] The present invention relates to the use of liquid compositions of carbonaceous fillers for the manufacture of electrodes for batteries, more particularly carbon nanotubes, in which the carbonaceous fillers in the liquid composition are present at mass contents of between 3.5 and 20%.
[0004] Background and Prior Art:
[0005] In a Li-ion battery electrode, it is necessary to formulate the electroactive material with additives (electronic conductive agent, polymer binder) to ensure that this layer has the mechanical and electrical properties necessary for its assembly in the battery and its subsequent proper functioning. The formulation requires the most appropriate combination of additives and proportions that guarantee the best compromise between proper functioning of the electrode and minimal additive content.
[0006] The evolution of environmental constraints and the manufacturing processes of electrodes and batteries containing them impose increasingly resource-efficient conditions, particularly with a view to reducing the carbon footprint within the framework of a life cycle analysis according to the ISO 14040 (2006) standard.
[0007] Carbon fillers are compounds that can take different forms, such as carbon blacks, carbon fibers and nanofibers, graphenes, fullerenes, as well as carbon nanotubes.
[0008] Carbon nanotubes are made of rolled graphite sheets, with diameters ranging from a few nanometers to a few tens of nanometers. They are available as single or multi-sheets. Carbon fillers are used to improve the electrical conductivity of battery electrodes. Carbon nanotubes obtained in various synthesis processes cannot be directly formulated because they are in the form of bundles or tangled balls. The same is true for other carbon fillers to a lesser extent, but often associated with carbon nanotubes, it is the latter that are often the compounds that determine the nature of the conditions necessary for the preparation of dispersions with high carbon filler contents.
[0009] Today, the use of carbon fillers in electrodes for batteries and in particular carbon nanotubes requires them to be properly dispersed beforehand in the form of a dispersion in a solvent with specific conditions. This is done using ultrasonic methods or under shear in the presence of a dispersant, which in particular allows the carbon nanotubes to be freed from their entanglements but requires significant quantities of solvent. Given the small quantities of carbon nanotubes present in these dispersions, it is therefore necessary to transport large quantities of material between the carbon nanotube production sites and their dispersion and the users, resulting in a very unfavorable carbon balance. In the known prior art, dispersions are reported whose carbon nanotube contents are always less than 5%, and rather around 1% accompanied by high viscosities.The low quantity of carbon charges present in the dispersions is a limitation to the use of these dispersions in electrodes because current electrode manufacturing processes seek to limit the presence of solvent as much as possible with the ultimate objective of preparing solvent-free electrodes (known as a "dry process" in English).
[0010] Thus, EP2550699 describes the preparation of liquid compositions of carbon nanotubes. However, the carbon nanotube contents in the solvent remain low, around 2%.
[0011] In EP37861 10, a carbon nanotube content of up to 5% with high dispersion viscosities is reported in the examples. However, the carbon nanotube concentration and the viscosity of the carbon nanotube dispersions is a limiting factor for their use.
[0012] A first technical problem consists of finding solutions that allow the incorporation of the maximum amount of carbon charges and in particular carbon nanotubes in a solvent because this is what presents the best carbon balance.
[0013] A second technical problem is to find solutions that allow these compositions to remain liquid over time because if a composition can be obtained liquid at the end of the manufacturing stage, it must remain so until its final destination allowing easy unloading after storage or transport to the final use, which is not always the case for the same carbon nanotube content depending on the solvent and dispersant pair used. The presence of other carbon fillers combined with the carbon nanotubes only amplifies the difficulties.
[0014] A third technical problem is the temperature stability of viscosity, because the manufacture, storage and use of these compositions must tolerate temperature variations.
[0015] The solutions that can be provided to resolve these technical problems are generally studied and characterized by rheology measurements. Unfortunately, the presence of carbon fillers and in particular the presence of carbon nanotubes largely masks the characteristics of the solvents and dispersants that are necessary to resolve these technical problems. This is why the applicant has studied more specifically the rheological behavior of the dispersant / solvent pairs in the absence of carbon fillers because it is these pairs that make it possible to predict the possibility of having compositions with high carbon filler contents.
[0016] The applicant has discovered that such compositions with a high carbon content solving these three technical problems are obtained when the rheological behavior of the dispersant / solvent pair obeys certain solubility conditions and remains Newtonian within the meaning of standard ISO 3219-1:2021, i.e. the dispersant / solvent pair must exhibit behavior in which the shear viscosity is independent of the shear rate, the shear stress and the time in the shear range 0-150s. -1 while remaining less than 1 Pa.s at the shear of 0.1 s -1 .
[0017] Such conditions are governed by the choice of the solvent-dispersant pair. The rheological behavior of the solvent-dispersant pair is more representative of the dispersion of carbonaceous fillers in the dispersant and solvent solution because it allows the selection of conditions allowing a stable dispersion over time of high-content carbonaceous fillers in a solvent, typically above 5%.
[0018] When the right conditions are met, it is possible to obtain liquid compositions of carbon nanotubes with mass contents of up to 20%. A dv50 measurement of less than 50 nm attests to the good dispersion of the carbon nanotubes within these compositions. With a combination of carbon nanotubes and carbon black, the Dv50 remains low with values of less than 600 nm. The compositions used in the invention remain stable over time, including at temperature.
[0019] These conditions are met when the dispersant has a solubility greater than 15% in the solvent on the one hand, and on the other hand the solvent-dispersant mixture with a content greater than 15% of dispersant has a dynamic viscosity at 0.1 s -1 less than 1 Pa.s, accompanied by Newtonian behavior in the shear range 0-150 s -1 . With these rheological conditions of the solvent-dispersant couple, an optimal range linking the viscosity and the carbonaceous filler content in a dispersion of carbonaceous fillers, solvent and dispersant can be identified.
[0020] In other words, if the dispersant is insufficiently soluble in the chosen solvent, i.e. it has a mass solubility of less than 15%, it is not possible to obtain dispersions with high carbon filler contents.
[0021] With the compositions used in the invention, it is now possible to respond to developments in the manufacturing process of electrodes requiring less solvent and with compositions that are stable over time. Summary of the invention:
[0022] The invention relates to the use of a composition for the formulation of electrodes, this composition comprising:
[0023] - carbon fillers in mass proportions of between 3.5 and 20% of the composition, chosen from carbon nanotubes and / or carbon blacks,
[0024] - at least one solvent, chosen from water, N-alkyl pyrrolidones such as N-methyl pyrrolidone, dimethyl sulfoxide, alkyl carbonates, cyrene™, dimethylformamide, acetates, furans, alcohols,
[0025] - at least one dispersant, chosen from polyvinylpyrrolidone homopolymers or copolymers, polyvinyl alcohol homopolymers or copolymers, polyacrylic acids homopolymers or copolymers comprising acrylic acid, polyacrylonitriles, polynitriles homopolymers and copolymers, linear polyesters or polyethers, polycarboxylate ethers alone or in combination, in which the solubility of the dispersant is greater than 15% by mass in the solvent alone and the mixture of which with the solvent alone has the following two conditions when it is solubilized at a content greater than 15% by mass:
[0026] - a dynamic viscosity at 0.1 s -1 < 1 Pa.s,
[0027] - Newtonian behavior in the gradient range 0-150 s' 1 , said composition has a carbon filler / dispersant mass ratio of between 10 / 1 and 1 / 1, preferably between 5 / 1 and 3 / 1, and a pH of between 5 and 13.
[0028] Detailed description:
[0029] By Newtonian behavior in the sense of ISO 3219-1:2021, it is considered that the dispersant / solvent pair must exhibit a behavior in which the shear viscosity is independent of the shear rate, the shear stress and the time in the shear range 0-150s -1 , with maximum viscosity variation in the shear range 0-150 s -1of 10%. The carbon fillers used in the context of the invention may be carbon nanofibers, synthetic graphite, graphite nanosheets, graphite nanoplatelets, graphene sheets, non-synthetic graphite, natural graphite, coke, graphitized carbon nanofibers, carbon nanotubes, or combinations thereof. The carbon nanotubes are multi-walled with a diameter between 8 and 50 nm and preferably between 8 and 20 nm (measured by transmission electron microscopy). The carbon nanotubes have a specific surface area measured by BET with a device of the ASAP 2460 type from Micrometrics of between 120 and 450 M 2 / g and preferably between 150 and 300 M 2 / g. They can be obtained by any type of process and are presented at the end of their synthesis in entangled form, bundles, or a combination of both. Carbon nanotubes can be purified, that is to say freed from the metal catalysts necessary for their synthesis. By purified carbon nanotubes is meant carbon nanotubes whose metal content is less than 200 ppm and preferably less than 50 ppm by a heat treatment in a neutral atmosphere and at a temperature above 200 °C with a treatment time that varies according to the temperature and is generally between 30 minutes and 3 hours. Carbon nanotubes can also be functionalized. Carbon nanotubes that have undergone a heat treatment in a neutral or reducing atmosphere or under partial pressure less than 0.8 Pa, and at a temperature above 200 °C constitute a variant of the invention.This heat treatment can also be obtained by compacting the carbon nanotubes during the drying operation of the compacted carbon nanotubes, for example in the presence of water.
[0030] The use of the compositions of the invention in electrode manufacturing processes thus makes it possible to use less solvent because the carbonaceous fillers in liquid dispersions are present at mass contents of between 3.5 and 20%, preferably between 5 and 14%, preferably between 5 and 11%, preferably between 6 and 10%, and even more preferably between 6 and 8%. Furthermore, the use of the compositions of the invention is possible after prolonged storage of one month, whether at room temperature or at 60°C.
[0031] Preferably, the carbon fillers used in the compositions of the invention consist of carbon nanotubes and / or carbon black. When it is carbon black associated with carbon nanotubes, the mass ratios of carbon nanotubes / carbon black can vary from 100 / 1 to 1 / 100, preferably from 100 / 5 to 1 / 5. Preferably, graphenes are excluded from the compositions of the invention.
[0032] The specific surface area of carbon blacks is less than 2000 m 2 / g, preferably less than 1000 m 2 / g, preferably less than 200 m 2 / g and a particle size less than 50pm measured by Malvern Mastersizer 3000.
[0033] Furthermore, being able to disperse a combination of carbon nanotubes and carbon black in a single dispersion at high levels allows for additional savings in solvent consumption and improved performance of electrodes in batteries. Until now, these two carbon fillers have been introduced separately and less closely into the electrodes.
[0034] When dispersing carbonaceous fillers with a solvent and a dispersant, any type of process can be used. This can be by ultrasound, extrusion, multiple extrusion, mixing, grinding in a suitable mill such as a ball mill or a combination of these processes.
[0035] The solvent can be a solvent or a mixture of solvents. From now on, we will talk about solvents, which includes mixtures of solvents.
[0036] The solvent is chosen from water, N-alkyl pyrrolidone, N-methyl pyrrolidone, dimethyl sulfoxide, alkyl carbonates, cyrene™, dimethylformamide, acetates, furans, alcohols and mixtures thereof. Preferably, it is N-methyl pyrrolidone. The N-methyl pyrrolidone may be pure or derived from a recycling or reuse process not including a distillation step. A solvent consisting mainly of one of the solvents listed above and a co-solvent not listed above would not be outside the scope of the invention.The dispersants are chosen from polyvinylpyrrolidone homopolymers or copolymers, polyvinyl alcohol homopolymers or copolymers, polyacrylic acids homopolymers or copolymers comprising acrylic acid, polyacrylonitriles, polynitriles homopolymers and copolymers, linear polyesters or polyethers, polycarboxylate ethers alone or in combination, and more particularly polyvinyl pyrrolidone homopolymers or copolymers and more preferably polyvinyl pyrrolidone homopolymers or copolymers whose molecular mass by weight is between 20,000 and 30,000 g / mol. Polyacrylic acids homopolymers or copolymers comprising mainly acrylic acid can be used in the form of their alkali salts, preferably Li. + or Na +). Subsequently, we will speak of dispersant, the dispersant being able to be composed alone or a mixture of dispersants of different natures or of the same nature but with different molecular characteristics (molecular masses, dispersity, polymolecularity).
[0037] It is considered that the dispersant may be a single dispersant or a mixture of dispersants. The presence of surfactants or other additives may also be considered. Thus the dispersant may be a dispersant or mixture of dispersants in the presence of at least one surfactant and / or other additive.
[0038] The mass ratio of carbonaceous fillers to dispersant is between 10 / 1 and 1 / 1 and preferably between 5 / 1 and 2 / 1 within the compositions of the invention.
[0039] The dispersant and solvent have the following combined characteristics:
[0040] - The dispersant must be soluble in the solvent at mass contents greater than 15% (condition A).
[0041] - The dispersant-solvent mixture according to condition A must have a dynamic viscosity at 0.1 s-1 less than 1 Pa.s for a mass content greater than 15% in the solvent (condition B).
[0042] - The dispersant-solvent mixture must exhibit Newtonian behavior in the gradient ranges between 0 and 150s-1 and dynamic viscosity less than 1 Pa.s (condition C). Solubility greater than 15% by mass means the possibility of dissolving more than 15 g of dispersant per 100 g of solution at temperatures between 15 and 25 ° C.
[0043] The solubility measurement of the dispersant in the solvent allows a selection according to criterion A. It is estimated that the maximum dispersant that can be solubilized in a solvent is the concentration beyond which a cloudiness appears.
[0044] Measurement of shear viscosity at 0.1 s -1of the dispersant - solvent couple makes it possible to verify that the value of 1 Pa.s is not exceeded (criterion B).
[0045] Dispersant-solvent couple viscosity measurement in the shear range between 0-150 s -1 allows us to verify that the behavior is Newtonian with a viscosity less than 1 Pa.s (criterion C).
[0046] The verification of the three criteria can be done by making two measurements within the reach of the person skilled in the art, that of the solubility in the solvent and reestablishment of the rheological curve of the viscosity as a function of the shear using a rheometer, according to the ISO 3219-2:2021 standard.
[0047] The general approach is given in Figure 7.
[0048] Viscosity measurements of the dispersant-solvent pairs show that the pairs selected within the framework of the invention meet the following inequality (figure 5):
[0049] Y < 0.0006e 0 2399X
[0050] Where Y is the viscosity at 0.1 s -1 in Pa.s and X is the mass content in % of dispersant.
[0051] The measurement of viscosities in the presence of carbonaceous fillers shows that the dispersions of the invention respond to the following inequality (figure 6):
[0052] Y1<0.0024e 1 2531X1
[0053] Where Y1 is the viscosity at 0.1 s -1in Pa.s and X1 is the mass content in % of carbon fillers. Other adjustments are necessary when it is desired to obtain high carbon nanotube contents. Thus, it has appeared that a basic pH favors high carbon filler contents. For these high contents, it is favorable for the compositions of the invention to have a pH of between 5 and 13.5, preferably between 7 and 12, preferably between 8 and 11, and more preferably between 9 and 11. The pH can be adjusted using a mineral or organic base, among which may be mentioned, without limitation, sodium, potassium, lithium hydroxides, sodium, potassium, lithium carbonates, amines. Preferably, these are sodium or lithium hydroxides or carbonates.
[0054] When using the compositions of the invention to formulate an electrode, it will be necessary to add the necessary compounds (active material, polymer binder, other additives). A pH adjustment may be made for shaping the electrode.
[0055] The invention also relates to an electrode using the compositions of the invention. The electrode may be a cathode or an anode.
[0056] The invention also relates to a battery comprising at least one electrode (anode or cathode) obtained using the compositions of the invention.
[0057] Description of the figures:
[0058] Figure 1: Quilt geometry used for rheology measurements.
[0059] Figure 2: Viscosity curve - flow of CMC in water.
[0060] Figure 3: Viscosity curve - flow of PVP1 in water.
[0061] Figure 4: Viscosity curve - flow of PVP2 in water.
[0062] Figure 5: Viscosity of dispersant-water solutions as a function of the content of
[0063] % by mass of dispersant.
[0064] Figure 6: Viscosity of dispersions as a function of the mass % content of carbonaceous fillers.
[0065] Figure 7: Flowchart for selecting dispersant-solvent pairs.
[0066] Examples: Products used for the study and preparation of dispersions:
[0067] Carbon charges:
[0068] -Carbon nanotubes (NTC 1 ): from Arkema, Graphistrength® C100 grade. NTC 1 are entangled carbon nanotubes.
[0069] -Carbon nanotubes (CNT 2): Prepared according to EP1846157 but using an aluminosilicate catalyst support. CNT2 are bundle-type carbon nanotubes.
[0070] -NTC3 are NTC1 type carbon nanotubes which have undergone heat treatment at a temperature above 200°C for 2 hours.
[0071] -Carbon black (NdC): source Imerys grade SUPER P®Li.
[0072] Solvents:
[0073] - Demineralized water.
[0074] -N-methyl pyrolidone, NMP.
[0075] Dispersants:
[0076] -Carboxy methyl cellulose (CMC): origin and grade Finnfix® 2G.
[0077] -Polyvinyl Pyrolidone (PVP1): source Sigma-Aldrich® reference 234257 with a molecular mass of 29000g / mol.
[0078] -Polyvinyl Pyrolidone (PVP2): from Nippon Shokubai K-85W with a molecular weight of 85000 g / mol.
[0079] -Poly acrylic acids: Polycarboxylate: from Coatex, grade ethacryl hf 50.
[0080] -PVDF: from Arkema Kynar® 761.
[0081] -hydrogenated nitrile rubber: from Lanxess grade Therban® AT 3404.
[0082] -Water-soluble lignin: source Sigma-Aldrich® grade 370959.
[0083] -pH adjuster: Sodium NaOH from Sigma-Aldrich®
[0084] Conditions for rheological measurements:
[0085] An imposed stress rheometer type MCR301 from ANTON PAAR is used. The standard used is ISO 3219-2:2021.
[0086] The measurements are carried out by flow stress scanning at 20 °C. The geometry used is of the duvet type for which the temperature regulation is ensured by the Peltier effect. The duvet geometry used is given in figure 1. The composition to be studied is introduced into the air gap of the duvet geometry using a disposable pipette. The shear gradient range varies in logarithmic mode from 0.1 to 1000 s-1 with measurement of 10 points per decade. Example 1: Study of dispersant - solvent couples and rheological measurement: The dispersant solutions in the solvent are prepared by dissolution at 20 °C in a device such as a beaker in the presence of stirring, with the compositions given in table 1.
[0087] The rheology measurements are carried out and the criteria met or not A, B, C are reported in table 1.
[0088] As an illustration, the rheological behavior of certain dispersant-solvent pairs is shown in figures 2, 3, 4.
[0089] [Table 1]
[0090]
[0091] Example 2:
[0092] In this series of examples, the behavior of dispersions of carbonaceous fillers in dispersant-solvent pairs is studied. The dispersions of carbonaceous fillers in a solvent in the presence of dispersant are carried out according to the method described in examples 7 and 8 of EP2550699 describing the case for the dispersant-solvent CMC pair -
[0093] Water. The same procedure is used to prepare the dispersions according to the examples in Table 2. Rheology measurements are taken immediately after preparation of the dispersions and after 1 month at room temperature and at 60°C. Dv 50 is measured immediately after preparation of the dispersions and after 1 month using a Malvern Mastersizer 3000 type device.
[0094] The results are reported in Table 2.
[0095] [Table 2]
[0096]
[0097] It can be seen that the examples outside the invention have low carbon load rates, around 3-4%, which constitute the maximum allowing the preparation of dispersions with a sufficiently low Dv and acceptable viscosity. Beyond these rates, it is not possible to obtain dispersions with satisfactory characteristics.
[0098] Furthermore, for these examples outside the invention, it is observed that the viscosity increases more significantly with time. When the storage temperature is 60°C, the viscosity is no longer measurable with the spindle used in Figure 1.
[0099] The examples of the invention show carbon load rates of up to 11% (example 2.12).
[0100] In all cases, the viscosity of the compositions of the invention remains low or moderate, and does not change significantly, even when the compositions remain at 60°C for one month. The effect of the heat treatment on the viscosity of the compositions is particularly significant (examples 2.10, 2.11, 2.12 and figure 6).
[0101] Thus, compared to conventional formulations containing less than 3% carbon fillers, compositions with a high carbon filler content make it possible to exploit electrode manufacturing processes with a more favorable environmental balance.
[0102] Example 3 - Electrode manufacturing and performance measurement:
[0103] In this example, electrical performance is measured in a cathode-type electrode formulation.
[0104] Cathodes are made with the dispersions immediately after preparing the dispersions (2.13a and 2.18a), then with the dispersions having been stored for 1 month at 23°C (2.13b and 2.18b) and finally with the dispersions having been stored for 1 month at 60°C (2.13c and 2.18c). This gives a series of cathodes having been made with dispersions having been stored differently in time and temperature.
[0105] A solution of 8% Kynar® HSV 1810 PVDF (Arkema) in NMP in an amount of 12.5 g was mixed with 4 g of the dispersion of example 2.13a, 2.13b, 2.13c using a disc mixer at 400 rpm. After 15 min of mixing, 98.5 g of NMC 622 and 10 g of additional NMP were gradually added.
[0106] Then, the dispersion is applied to a polyethylene terephthalate (PET) support at 100 μm thickness using a doctor blade, aiming for a coating thickness of 120 μm. The coating is dried in a ventilated oven for 30 min at 130 °C. This gives the cathodes C213a, C213b, C213c.
[0107] The coated PET sheet is cut to obtain 3x4 cm samples. The ends of each sample are coated with a silver-filled conductive ink. Electrical resistivity was measured using a Keithley electrometer.
[0108] The same protocol is applied to obtain the cathodes with the dispersions of example 2.18a, 2.18b and 2.18c by adjusting the dispersion quantities to obtain the same carbonaceous filler contents as for the C213 series. This gives the cathodes C218a, C218b, C218c.
[0109] The results of the electrical measurements are summarized in Table 3.
[0110] [Table 3] If for dispersions used immediately after their preparation the cathodes show similar resistivities, it should be noted that those of the invention allowed the use of dispersions with 11% carbon nanotubes, against 3% for the comparative example. When the dispersions are used after one month of storage the advantage of the dispersions of the invention is clear in relation to the dispersions of the comparative example.
[0111] Thus, not only does the invention allow the use of carbon filler dispersions with less solvent, but it also allows them to be used after one month of storage at room temperature or at 60°C while maintaining their initial quality.
Claims
CLAIMS 1 Use of a composition for the formulation of electrodes, this composition comprising: - carbon fillers in mass proportions of between 3.5 and 20% of the composition, chosen from carbon nanotubes and / or carbon blacks, - at least one solvent, chosen from water, N-alkyl pyrrolidones such as - N-methyl pyrrolidone, dimethyl sulfoxide, alkyl carbonates, cyrene™, dimethylformamide, acetates, furans, alcohols, - at least one dispersant, chosen from polyvinylpyrrolidone homopolymers or copolymers, polyvinyl alcohol homopolymers or copolymers, polyacrylic acids homopolymers or copolymers comprising acrylic acid, polyacrylonitriles, polynitriles homopolymers and copolymers, linear polyesters or polyethers, polycarboxylate ethers alone or in combination, in which the solubility of the dispersant is greater than 15% by mass in the solvent alone and the mixture of which with the solvent alone has the following two conditions when it is solubilized at a content greater than 15% by mass: - A dynamic viscosity at 0.1 s -1 < 1 Pa.s, - Newtonian behavior in the gradient range 0-150 s -1 , said composition has a carbon filler / dispersant mass ratio of between 10 / 1 and 1 / 1, preferably between 5 / 1 and 3 / 1, and a pH of between 5 and 13. 2 Use of a composition according to claim 1 in which the solvent is water or N-methyl pyrrolidone. 3 Use of a composition according to claim 1 in which the solvent is N-methyl pyrrolidone resulting from a recycling or reuse process not comprising a distillation step. 4 Use of a composition according to claim 1 to 3 in which the dispersant is chosen from polyvinyl pyrrolidone homopolymers or copolymers whose molecular mass by weight is between 20,000 and 30,000 g / mol, homopolymers or copolymers comprising acrylic acid, linear polyesters or polyethers, polycarboxylate ethers. 5 Use of a composition according to one of claims 1 to 4 in which the carbon fillers are chosen from multi-walled carbon nanotubes whose diameter can vary from 8-50 nm (measured by transmission electron microscopy) and a BET specific surface area of between 120 and 450 m 2 / g and having undergone heat treatment at a temperature above 200°C or not, carbon blacks with a BET specific surface area of less than 2000 m 2 / g and a particle size less than 50|im measured by Malvern Mastersizer 3000, or even graphenes, these carbon charges can be combined or not. 6 Electrode obtained with a use according to one of claims 1 to 5. 7 Battery comprising at least one electrode according to claim 6.
Citation Information
Patent Citations
Method for synthesis of carbon nanotubes
EP1846157A1
Masterbatch of carbon-based conductive fillers for liquid formulations, especially in li-ion batteries
EP2550699A1
Carbon nanotube dispersion and use for same
EP3786110A1
Shear thickening graphene composite conductive paste and preparation method thereof
CN115116649A
Electrode composite, battery electrode formed from said composite, and lithium battery comprising such an electrode