Composite materials

Laminating recycled polymer materials with waste glass fiber mats addresses the variability and inefficiency in existing recycling methods, resulting in composite materials with enhanced mechanical properties and sustainable waste management.

WO2024246507A1PCT designated stage expired Publication Date: 2024-12-05THE UNIV COURT OF THE UNIV OF EDINBURGH +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/GB2024/051362
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-07
Filing Date
2024-05-28
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

The challenge lies in creating composite materials with robust mechanical properties using recycled polymer materials and waste glass fiber mats, which often exhibit variability due to differences in polymer grades, additives, and contamination, and are typically discarded or landfilled, with existing recycling methods being costly and inefficient.

Method used

A novel method of laminating a layer of recycled polymer material with a layer of waste glass fiber mat, allowing for consistent and reproducible mechanical properties by minimizing fiber damage during the process, thereby offsetting variability and enhancing tensile modulus and strength.

Benefits of technology

This approach results in composite materials with improved mechanical properties, such as increased tensile strength and modulus, while also providing a sustainable solution for waste materials, reducing landfill waste and recycling costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GB2024051362_05122024_PF_FP_ABST
    Figure GB2024051362_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The present disclosure relates to composite materials comprising a recycled polymer material and a waste glass fiber material, and methods of manufacturing such composite materials. The described materials have been found to show a number of good mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Composite Materials

[0002] FIELD

[0003] The present disclosure relates to composite materials comprising a recycled polymer material and a waste glass fiber material, and methods of manufacturing such composite materials.

[0004] BACKGROUND

[0005] Currently, plastic packaging which generally includes high-density polyethylene (HDPE), polypropylene (PP), and polyethylene terephthalate (PET) are commonly recycled. However, a large proportion of single-use plastics packaging wastes that consist primarily of low-density polyethylene (LDPE), are not generally recycled due to their flexibility, low mechanical performance and low cost [1], Within the UK, it is estimated that five million tonnes of plastics are used every year [2], with 67% of this consisting of plastic packaging [3], However, LDPE films and bags are not collected with household recycling in the UK, an addition of which could significantly increase recycling rates.

[0006] Waste mixed plastics (wMP) originating from single-use plastics packaging primarily includes various grades of polyethylene including LDPE and HDPE. Such wMP has the potential to offer mechanical properties superior to LDPE alone. In addition, using such wMP can eliminate the need for separating the plastics in the recycling stream saving cost.

[0007] Glass fiber materials are used in numerous product applications, in particular as reinforcing structures in fiber resin composites or floorings, as facers for insulation material and in various other applications. The glass-based fiber mats usually end up as waste composite materials at the end of their lifetime. In addition, there is also a low percentage of direct production waste glass. Binder consolidated glass fiber nonwoven mat can become waste caused by optical defects and / or by quality defects. An amount of waste glass fiber is generated due to being out of specification required for a specific application. In the manufacturing process start-up and transition rolls are also discarded as waste. Such small percentage of binder solidified glass fiber-based production waste is not avoidable and, in view of the annual total manufactured tonnage, can be a significant amount.

[0008] Studies investigating polyethylene blends have generally only considered the effects on virgin materials. There have been some studies on blending recycled PEs / polyolefins in different proportions. For example, Yousif et al. [4] studied different blends of recycled LDPE (rLDPE), rHDPE, and rPP. Blending the three with different proportions was shown to improve the tensile stress up to 14-25% higher than the individual polymers alone, confirming the prospective increase in recycled plastics quality through blending. Similarly, Cecon et al. [5] investigated the effect of adding different amounts of post-consumer recycled polyethylene (PCRPE) on virgin polyethylenes of different densities (vLDPE, vLLDPE, vMDPE, and vHDPE). Both LDPE and LLDPE blends displayed increases up to 75% in the tensile modulus and 56% in the yield strength compared to those without PCRPE.

[0009] Mechanical properties of polyolefin blends can be increased further through reinforcement with glass fibers. There have been many studies investigating the effect of adding glass fiber reinforcement to mixed polyolefin blends [6-10], and on recycled polyolefin matrix composites with various reinforcements[11-16].

[0010] The method of manufacturing composites containing polyolefins and glass fibers is primarily done through melt mixing and extrusion of the plastics and glass fibers. While this may ensure a homogenous composite, extruding glass fibers shortens the length of the fibers, which can affect the mechanical properties of the resulting laminate. Ayadi

[0011] noted that after one extrusion of short glass fibers with HDPE that the viscosity of the composite increased, the fiber length decreased, and this decrease in fiber length increased as the glass fiber (GF) proportion in the composite increased.

[0011] A problem associated with the use of a recycled (e.g. mixed waste) polymer material is that such materials can be highly variable. In some examples, the variability might arise from mixtures of different grades and / or types of polymer, the presence of different additives, and / or the variability might be the result of contamination of the polymer material with residual amounts of an inseparable polymer material. This is a significant challenge for manufacturers looking to use such waste materials to manufacture new materials, which are often required to comprise certain mechanical properties and / or meet certain technical specifications.

[0012] A high amount of binder solidified glass fiber-based production waste ends up in landfill. Recycling of such waste glass fiber mats is typically done by thermal extraction, wherein the binder is combusted, thereby providing waste heat and wherein the waste extracted glass fiber is later added into the production of new glass. Thermal extraction is more costly compared to landfill and the binder is lost in the process.

[0013] Thus, there remains a need for new composite materials comprising recycled (e.g. mixed waste) polymer materials and, in some cases, comprising recycled (e.g. mixed waste) polymer materials and waste fiber, in particular waste glass fiber mat, and new methods of manufacturing of such composite materials.

[0014] SUMMARY

[0015] The present disclosure is based on the identification of a novel cohort of composite materials that can be made from recycled polymer materials and glass fibers (e.g. mixed waste polymer materials and waste glass fiber fabrics). In particular, the present inventors have identified a novel method of generating composite materials from recycled polymers (e.g. mixed waste polymers) and waste glass fiber mat, such as waste glass fiber nonwoven fabrics that provides a composite material with good and / or robust properties (e.g. mechanical properties). By way of example, it has been found that laminating a layer of recycled polymer material (e.g. mixed waste polymer material) and a layer of waste glass fiber mat (e.g. to provide a composite laminated material) can consistently and / or reproducibly provide composite materials with good mechanical properties (such as good levels of tensile modulus and tensile strength).

[0016] In particular, the inventors identified that laminating a layer of recycled polymer material (e.g. mixed waste polymer material) to a layer of glass fiber material in the form of a glass fiber mat, fabric or the like, offered significant improvements in mechanical properties in the composite material. Surprisingly, the level of improvement in these properties offsets and / or compensates for any variability associated with the use of recycled polymer materials (which may, for example contain different types and / or grades of polymer material (e.g. mixed waste polymer materials)) as a feedstock and / or starting material.

[0017] When a waste glass fiber fabric is used, surprisingly, the variability in waste glass fiber fabrics (e.g. mixed waste glass fiber fabrics) is also tolerated. Mixed in this context means glass fiber nonwoven fabrics having different thicknesses and areal weights, having different binders or other additives, and also having variable mechanical strength (e.g. tensile strength) in the manufacturing direction (e.g. machine direction (MD)) and traverse to the manufacturing direction (e.g. cross-machine direction (CMD)) and / or glass fiber fabrics have one or more defects (that may be the same or different) as described herein.

[0018] Thus, the methods described herein offer the potential for generating useful composite materials with consistent and / or reproducible mechanical properties, in spite of variation in the recycled polymer material and also variation in the waste glass fiber fabric starting material(s). As such, the present methods are particularly amenable for scaled-up and / or commercial manufacturing of composite materials using recycled polymer materials (e.g. mixed waste plastics) in combination with variable waste glass fiber materials.

[0019] Thus, according to an aspect of the disclosure, there is provided a composite material comprising: at least one layer of a waste glass fiber mat laminated to at least one layer of a recycled polymer material (e.g. a mixed waste polymer material); wherein the recycled polymer material has a density lower than about 1 g / cm3.

[0020] According to a further aspect of the disclosure, there is provided a method of making a composite material comprising:

[0021] (a) laminating at least one layer of a recycled polymer material to at least one layer of waste glass fiber mat; wherein the recycled polymer material has a density lower than about 1 g / cm3.

[0022] As noted above, the composite materials formed by way of the disclosed lamination method offer significant improvements in the mechanical properties of the composite. Without being bound by theory, the present inventors hypothesise that the improvement in properties may be attributable to a reduction in fiber damage during the lamination process, in comparison to techniques involving an extrusion based process (e.g. a process involving melt mixing of the polymer and glass fiber starting materials prior to extrusion of a composite material). In particular, as the fiber length of glass fibers can decrease during extrusion, it is believed that the disclosed composites (in laminate form and made by the methods disclosed herein) show less reduction in the fiber length than extruded composites, which may facilitate the observed improvement in mechanical properties. Indeed, it has been identified in some studies that the prior art extrusion based methods can result in a greater decrease in fiber length (of the glass fibers) as the glass fiber proportion in the composite increases (Ayadi et al,). This problem can be mitigated against by the lamination methods and composite laminates described herein, which can allow for increasing the proportions of the glass fiber in the composite without significant decrease in the fiber length of the glass fibers.

[0023] As noted above, the composite material comprises at least one layer of a waste glass fiber mat (e.g. a non-woven glass fiber mat).

[0024] As will be appreciated by the skilled addressee, in a non-woven glass fiber fabric or mat, the fibers may be laid down in a random orientation, however there can often be some bias towards the direction of travel during manufacture. Consequently, there may be a greater number of fibers aligned towards the machine direction (MD) than in the cross machine (traverse) direction (CMD). In addition, the nonwoven fabric or mat is stretched in the machine direction induced by belt transportation. Such orientation may affect the properties of the glass fiber fabric or mat and any composite materials produced from such mats, in particular the mechanical properties of the composite material may differ between the machine direction and the cross machine direction. The mechanical strength of the glass fiber fabric or mat is also strongly dependent on the areal weight (thickness) of the nonwoven fabric or mat. For a given glass fiber diameter, fiber length and binder content the mechanical strength increases proportionally with thickness.

[0025] As used herein, a waste glass fiber mat refers to a glass fiber mat that would otherwise be disposed of and / or end up in landfill. The waste glass fiber mat may be a post-consumer or pre-consumer waste glass fiber mat. As used herein, a post-consumer waste glass fiber mat may refer to a waste glass fiber mat that is generated by an end user. As used herein, a pre-consumer waste glass fiber mat may refer to a mat that is generated during the production or manufacture of a product. In some examples, it can be referred to as post-industrial waste glass fiber mat.

[0026] For example, the waste glass fiber mat may be material that is produced during the manufacturing process of a glass fiber mat that is an offcut and / or that does not meet specification (e.g. a certain technical specification) - this may sometimes be referred to as a post-industrial waste glass fiber mat. Where a glass fiber mat does not meet a certain technical specification, it may be referred to herein as “out of specification”.

[0027] In particular, the term waste glass fiber mat as used herein may refer to a glass fiber mat being out of specification. In some examples, the term waste glass fiber mat may refer to a mat which comprises one or more defects. The one or more defects may be selected from the group consisting of: wrinkles, stringers, ruptures, buckles, puckering, agglomerates, tension knuckles, discoloration, and deformations such as “tents” or clumps. Some of these defects may be the result of a rolling process and / or storage. For example, typical rolling defects may be tension knuckles and / or rupture of the rolled fabric.

[0028] As stated above, the composite material comprises at least one layer of a waste glass fiber mat. (This may also be sometimes be referred to herein as a waste glass fiber fabric). As would be understood by the skilled person, the production of a glass fiber fabric or mat material (e.g. a non-woven glass fiber fabric or mat material) may be a continuous process involving the laying down of a plurality of glass fibers and binding these together (e.g. using a binder). The properties of the glass fiber fabric or mat may be varied in accordance with the targeted end use, in particular, the binders, the length, amount and / or density of the glass fibers can be varied in order to provide a glass fiber fabric or mat with the desired properties (these desired properties may be referred to as a technical specification of the glass fiber fabric or mat). Therefore, in a continuous manufacturing process there may often be times when such parameters are being varied, for example when the manufacturer has produced a desired amount of a first type of glass fiber fabric or mat and wishes to begin production of a second type of glass fiber fabric or mat. This period may be considered as a transitional period where the parameters are being changed and may, for example, result in a plurality of binders being present in the glass fiber fabric or mat and / or result in a mixed weight glass fiber fabric or mat (e.g, with varying thickness) being produced. Such glass fiber fabrics or mats typically produced during these transitional periods generally end up in landfill (and so are encompassed within the expression “waste glass fiber mat” or “waste glass fiber fabric” as used herein). However, the present inventors have identified that these materials can be used to provide useful composites (when combined with recycled polymer materials) by way of the methods described herein.

[0029] Waste glass fiber nonwoven fabrics may be used as the glass fiber layers in the examples described herein. These nonwoven glass fiber fabrics typically comprise staple glass fibers having a typical nominal length of between about 5 mm to about 100 mm, preferably between about 5 mm and about 18 mm. Fiber diameters may typically be in the range of between about 1 pm to about 50 pm preferably between about 5 pm to about 16 pm. Preferably, fiber diameters of about 8 pm, and / or about 10 pm, and / or about 13 pm may be selected. The fabric (e.g. waste fabric) may comprise a single fiber class (diameter, length) or comprise blends of fiber diameters and / or lengths (e.g. blends of different fiber diameters and / or different fiber lengths).

[0030] The glass fibers may be longitudinally laid down randomly and bonded by a binder to form a nonwoven fabric. A typical binder is comprised in form of an aqueous solution comprising urea formaldehyde resin and polymer dispersions, a modified polycarboxylic acid and polyvinylacetate dispersion or a melamine formaldehyde resin. The fiber nonwoven fabric (e.g. waste fabric) sheets may have a nominal mean area weight of between 30 g / m2up to a nominal mean area weight of 300 g / m2. The nominal dry mass binder content may be between about 10 weight% to about 30 weight%, or between about 15 weight % to about 25 weight % (such as about 18 weight%) measured by loss on ignition testing, for example measured in accordance with DIN EN 13820. The waste glass fiber mat may comprise one or more additional components or additives. In some examples, the waste glass fiber mat may comprise a binder.

[0031] Suitable binders may be known to those skilled in the art and may include any binder that is capable of binding glass fibers together to form a fabric or mat. In some example, the binder may be selected from acrylic, melamine formaldehyde and urea formaldehyde binders, or combinations thereof.

[0032] In some examples, the binder (e.g. any one of those binders as defined herein), may be present in the waste glass fiber fabric or mat in an amount between about 5% and about 50%, based on the total weight of the waste glass fiber fabric or mat. In yet further examples, the binder may be present in the waste glass fiber fabric or mat in an amount between about 10% and about 30%, or between about 15% and about 25% by weight of a binder based on the total weight of the waste glass fiber fabric or mat. By way of further example, the binder may be present in the waste glass fiber fabric or mat in an amount between about 10% and about 19%, or between about 15% and about 18%, or between about 25% and about 30% by weight of a binder based on the total weight of the waste glass fiber fabric or mat.

[0033] As stated above, the composite material comprises at least one layer of a recycled polymer material and at least one layer of waste glass fiber mat.

[0034] As used herein, the term “recycled polymer material” may refer to a polymer material which would otherwise be disposed of and / or end up in landfill. By way of example, the recycled polymer material may be or comprise a post-consumer polymer waste material. As used herein, a post-consumer polymer waste material may refer to a polymer waste material that is generated by an end user. In other examples, the recycled polymer material may be or comprise a pre-consumer polymer waste material. As used herein, a pre-consumer polymer waste material may refer to a polymer waste material that is generated during the production or manufacture of a product.

[0035] In some examples, the recycled polymer material may be derived from packaging (such as films, containers, bottles or the like). Surprisingly, the present inventors have found that such recycled polymer materials (which typically show poor mechanical properties) can be used to provide composites with robust mechanical properties when made in accordance with the methods described herein.

[0036] The recycled polymer material may comprise two or more different polymers.

[0037] As used herein, different polymers may refer to polymers formed from different monomers, comprising different repeat units, polymers comprising different chemical or physical properties, polymers of a different molecular weight, polymers of a different density, and / or polymers of a different grade. In some examples, the different polymers may be polymers formed from different monomers. In other examples, the different polymers may be formed from the same monomers (and optionally may comprise the same repeat units) but may comprise different densities, different molecularweights (e.g. different number average molecular weights or different weight average molecular weights), different molecular weight distributions, and / or different grades.

[0038] In some examples, the recycled polymer material comprises a mixture of two or more thermoplastic polymers. The thermoplastic polymers may be selected from polyolefins (such as polyethylene and polypropylene), and the like. In some preferred examples, the recycled polymer material may comprise polyethylene and / or polypropylene.

[0039] Polyethylene is a polymer formed from an ethylene monomer and may be provided in a number of different grades or types. In particular, a polyethylene may vary in terms of the extent and type of branching, the crystal structure and its molecular weight. These variables may impact the mechanical properties. As used herein, the term “polyethylene” encompasses any suitable grade or type of polyethylene including, but not limited to, low density polyethylene (LDPE), linear low density polyethylene (LLDPE), medium density polyethylene (MDPE), high density polyethylene (HDPE), chlorinated polyethylene (CPE), very low density polyethylene (VLDPE), high molecular weight polyethylene (HMWPE), ultra-low-molecular weight polyethylene (LILMWPE) and ultra- high-molecular weight polyethylene (LIHMWPE).

[0040] Polypropylene is a polymer formed from a propylene monomer and, again, may be provided in a number of different types and grades such as random copolymer or impact copolymer (all of which are encompassed by the term “polypropylene” as used herein). The polypropylene may be provided as a homopolymer. Depending on the orientation of the pendant methyl group in the polymer chain, the polypropylene may be considered as isotactic, syndiotactic and atactic.

[0041] In yet further examples, the two or more different polymers may each be independently selected from high density polyethylene (HDPE), low density polyethylene (LDPE), polypropylene (PP), and combinations thereof.

[0042] As stated above, the recycled polymer material is any polymer material that comprises a density lower than water (e.g. a density lower than about 1 g / cm3). Such waste polymer materials may be easily sorted and / or separated from other waste polymer materials by allowing them to float in water. Thus, the method of forming the composite laminates described herein may comprise a step of adding a waste polymer material to water and / or separating the polymer material that floats. The separated polymer material may then be used as the recycled polymer material to make and / or form the composite laminates described herein.

[0043] In general, the majority of post-consumer polymer waste arises from packaging (e.g. food packaging). Polymers that are typically used in such packaging are various grades of polyethylene (particularly low density polyethylene and high density polyethylene) and / or polypropylene. Thus, in some examples, the recycled polymer materials used in the composite materials described herein may generally comprise and / or be selected from high density polyethylene (HDPE), low density polyethylene (LDPE), polypropylene (PP), and combinations thereof.

[0044] In some examples, the recycled polymer material may not comprise polyethylene terephthalate (PET), rubber (e.g. styrene-butadiene rubber) and / or a polyamide (such as nylon). In some examples, the recycled polymer material substantially does not comprise (or does not comprise) one or more, or all of the following: polyethylene terephthalate (PET), rubber (e.g. styrene-butadiene rubber) and polyamide (such as nylon).

[0045] The at least one layer of recycled polymer material may be provided in the form of a sheet or film. The sheet or film of recycled polymer material may be formed by pressing (e.g. compression molding) shredded polymer material under suitable heat and pressure conditions such that the shredded polymer material melts and bonds together. Such a step may be referred to sometimes as “thermocompression”. The shredded polymer material may be obtained by shredding recycled polymer material (e.g. recycled polymer films or sheets).

[0046] The recycled polymer material may be present in an amount between about 10% and about 90% by weight based on the total weight of the composite material. In some examples, the recycled polymer material may be present in an amount between about 20% and about 80%, or between about 50% and about 75% by weight based on the total weight of the composite material.

[0047] As described above, the at least one layer of a waste glass fiber mat is laminated to at least one layer of a recycled polymer material. As such, the composite material may be considered as a composite laminate material. As used herein, a composite laminate material may refer to layered material and / or may comprise two or more layers of material.

[0048] The composite laminate may be formed by laminating the at least one layer of waste glass fiber mat to the at least one layer of a recycled polymer material. In some examples, the step of laminating the layers together may comprise bonding the layers together by applying a suitable temperature and / or pressure such that the recycled polymer material melts and binds to the waste glass fiber mat, thus bonding the layers together.

[0049] In some examples, the composite laminate may be formed by coating at least one layer of a waste glass fiber mat with a layer of recycled polymer material. In such examples, the recycled polymer material (e.g. a shredded recycled polymer material) may be melted and then applied as a coating to provide the composite laminate. Such a method may be referred to as an extrusion coating process. One advantage of such a process is that it may be carried out continuously and so is particularly amenable to scaled-up manufacturing.

[0050] The composite material may comprise a plurality of layers of the recycled polymer material and / or may comprise a plurality of layers of the waste glass fiber mat. The exact number and arrangement of the layers may be selected in accordance with a desired end use of the composite material and / or may be dependent upon the desired mechanical properties of the composite material.

[0051] In some examples, the number of waste glass fiber mat layers may be from 5 to 20 times higher than the number of recycled polymer material layers in the composite material.

[0052] In many examples, the composite material may comprise at least one layer of a recycled polymer material sandwiched between at least a first and a second layer of a waste glass fiber mat. In such arrangements, the recycled polymer material may bind to each of the glass fiber layers, binding the layers together.

[0053] In some examples, the at least one layer of a recycled polymer material is sandwiched between a first section or block comprising one or more layers of the waste glass fiber mat and a second section or block comprising one or more layers of the waste glass fiber mat. In yet further examples, the composite material may comprise alternating sections or blocks of waste glass fiber mat and sections or blocks of recycled polymer material (each section or block comprising one or more layers of the waste glass fiber mat or the recycled polymer material).

[0054] By way of further example, the composite material may comprise alternating sections or blocks of: (i) a plurality of layers of the waste glass fiber mat; and (ii) one layer of recycled polymer material. In such arrangements, each one layer of recycled polymer material may be sandwiched between blocks of waste glass fiber mat, each block comprising a plurality of layers of the waste glass fiber mat. By way of further example, each block of the waste glass fiber mat may comprise between about 2 and 15 layers, between about 3 and 10, or between about 4 and 9 layers of the waste glass fiber mat.

[0055] The arrangement of layers with the composite laminate material may be referred to herein as the “lay up”.

[0056] The exact number of layers present in the composite may depend upon the thickness of each layer. In addition, the thickness of the (or each) layer of recycled polymer material and the (or each) layer of waste glass fiber may be varied and / or selected in accordance with the desired lay up of the layers and / or the desired volume of glass fiber.

[0057] During the lamination process, the recycled polymer material may melt and / or impregnate the layers of waste glass fiber mat (facilitating the bonding of these layers together). The degree and / or extent to which the recycled polymer material is able to impregnate the layers of waste glass fiber mat may depend upon a number of factors, including the thickness of the recycled polymer material layer, the thickness of the waste glass fiber mat layers, the overall number of these layers and / or the arrangement of these layers.

[0058] One factor which may impact the ability of the recycled polymer material to penetrate the waste glass fiber layers may be the porosity of the waste glass fiber layers. Typical pore sizes of the waste glass fiber layers may be between about 5 pm to about 50 pm, in particular between about 20 pm to about 40 pm, whereas the porosity (penetrability) is usually characterized by a measured air permeability. Air permeability as described herein may be measured in accordance to DIN EN ISO 9237. Air permeability measurements may be preferred over pore size inspection, as the measured air permeability is closely related to the overall (also depth) porosity, while pore size measurements solely reflect surface porosity. Typical air permeabilities that can help facilitate good penetration of the recycled polymer material in the glass fiber layer may be in the range of between about 1500 [l / m2s] to about 10000 [l / m2s], preferably between about 3000 [l / m2s] to about 5000 [l / m2s].

[0059] In some examples, the waste glass fibers may comprise a surface coating or sizing which is compatible with the recycled polymer material and / or which can enhance bonding between the waste glass fiber mat and the polymer layers. The sizing composition may comprise a film former having an average molecular weight of 1 ,000,000 Da to 1 ,700,000 Da (equivalent to g / mol), a lubricant, a surfactant and a silane composition comprising a silane coupling agent and at least a reactive group for coupling to a polymer chain of the recycled polymer material.

[0060] By way of example, a thicker layer of the recycled polymer material may impregnate a greater number of layers of the waste glass fiber mat. In some examples, where thinner layers of recycled polymer material are used, these may be interspersed between fewer numbers of layers of waste glass fiber mats.

[0061] Thus, the skilled addressee would be able to select an appropriate thickness, number of layers and / or arrangement of layers of both the glass fiber and recycled polymer material in order to provide a composite with the desired properties.

[0062] In some examples, the at least one layer of recycled polymer material may have a thickness between about 0.1 mm and about 20 mm, or between about 0.25 mm and 1 .5 mm. In some examples, the (or each) layer of recycled polymer material may have a thickness of about 0.5 mm. In other examples, the (or each) layer of recycled polymer material may have a thickness of about 0.95 mm (e.g. where an extrusion process is used to provide the laminate, the layer of recycled polymer material on the waste glass fiber mat may be about 0.95 mm).

[0063] In some examples, the (or each) layer of waste glass fiber mat may have a thickness between about 0.1 mm and about 3 mm, usually between about 0.3 mm and about 1 mm, such as between about 0.4 mm and 1 mm. In some examples, the waste glass fiber mat may have a thickness of about 0.4 mm or 1 mm.

[0064] In some examples, the areal weight of the waste glass fiber mat may be between about 30 g / m2and about 300 g / m2, between about 30 g / m2and about 100 g / m2, or between about 50 g / m2and about 150 g / m2. In some examples, the areal weight of the waste glass fiber mat may be between about 50 g / m2and about 100 g / m2. For example the areal weight of the waste glass fiber mat may be measured in accordance with the method as described in DIN EN 29 037-1.

[0065] In some examples, the waste glass fiber mat may have a tensile strength MD of between 100 N / 5cm and 1000 N / 5cm depending on its areal weight and thickness and measured according to DIN EN 29 073-3. Preferably the waste glass fiber mat may have a tensile strength MD between 200 N / cm and 400 N / 5cm for areal weights of between about 50 g / m2and about 100 g / m2and a thickness of between 0.4 mm and 1 mm.

[0066] In these examples the waste glass fiber mat may have a tensile strength CMD in transverse direction of between 100 N / cm and 250 N / 5cm for areal weights of between about 50 g / m2and about 100 g / m2and a thickness of between 0.4 mm and 1 mm. As explained above, the composite materials made by way of laminating a layer of recycled polymer material onto a layer of waste glass fiber material offer significant improvements in the mechanical properties of the material (which can offset and / or compensate for any variability associated with the use of recycled polymer materials and also waste glass fiber materials).

[0067] The inventors have further identified that the mechanical properties may be particularly improved in those examples comprising the glass fiber in an amount between about 5% and about 50% by volume based on the total volume of the composite material. In yet further examples, the composite material may comprise between about 15% and 40% by volume, or between about 20% and 35% by volume of the glass fiber, based on the total volume of composite material. In some examples, the composite material may comprise between about 24 and 27% by volume of the glass fiber based on the total volume of the composite material. The fiber volume fractions as defined herein may be determined in accordance with the methods described in the examples section and, in particular following the method described in ASTM standard D3171.

[0068] In some examples, the composite material may comprise a glass fiber fraction between about 5% and about 70%, between about 10% and about 60%, or between about 15% and 50% by weight, based on the total weight of the composite material. The glass fiber weight fractions as defined herein may be determined in accordance with the methods described in the examples section and, in particular following the method described in ASTM standard D3171.

[0069] As explained above, the addition of the waste glass fiber layer to the recycled polymer materials as described herein provides a significant level of improvement in the mechanical properties of the composite material which may be sufficient to offset and / or compensate any variability inherent to the use of a recycled polymer material. In particular, the composite laminate materials as described herein may show significant improvements in one or more of the following properties: tensile strength, tensile modulus, flexural strength, and flexural modulus.

[0070] By way of example, the composite material may comprise a tensile strength of at least about 5 MPa. In some examples, the tensile strength of the composite material may be at least 10 MPa, at least about 15 MPa, at least about 20 MPa, or at least about 30 MPa. In some examples, the tensile strength may be between about 25 MPa and about 50 MPa.

[0071] In some examples, the composite material may comprise between about 15% and 40% by volume, or between about 20% and 35% by volume of the glass fiber, and the tensile strength of the composite laminate may be at least about 15 MPa, or at least about 30 MPa.

[0072] The tensile strengths as defined herein may be determined in accordance with the methods described in the examples section and / or in accordance with the method described in ASTM D3039M-21.

[0073] By way of example, the composite material may comprise a tensile modulus of at least about 1 GPa. In some examples, the composite material may comprise a tensile modulus of at least about 1.5 GPa, or at least about 2 GPa. In some examples, the composite material may comprise a tensile modulus between about 1 GPa and about 10 GPa, such as between about 1 GPa and about 8 GPa, or between about 1 GPa and about 4 GPa.

[0074] In yet further examples, the composite material may comprise between about 15% and 40% by volume, or between about 20% and 35% by volume of the glass fiber, and the tensile modulus of the composite laminate may be at least about 1 GPa, or at least about 2 GPa. In yet further examples, the composite material may comprise at least about 15% by volume of the glass fiber (based on the total volume of the composite) and the tensile modulus of the composite may be at least about 3 GPa.

[0075] The tensile moduli as defined herein may be determined in accordance with the methods described in the examples section and / or in accordance with the method described in ASTM D3039M-21.

[0076] In some examples, the composite material may comprise a flexural modulus of at least about 0.5 GPa. In some examples, the flexural modulus of the composite material may be at least about 1 GPa, at least about 3 GPa, or at least about 5 GPa. In some examples, the flexural modulus of the composite material may be between about 0.5 GPa and about 20 GPa, or between about 1 GPa and 10 GPa. The flexural moduli as defined herein may be determined in accordance with the methods described in the examples section and / or in accordance with the method described in ASTM D790.

[0077] In some examples, the composite material may comprise a flexural strength of at least about 10 MPa, at least about 20 MPa, or at least about 30 MPa. The flexural strengths as defined herein may be determined in accordance with the methods described in the examples section and / or in accordance with the method described in ASTM D790.

[0078] In some examples, the composite material may comprise a compressive strength of at least about 10 MPa. In some examples, the compressive strength of the composite material may be at least about 15 MPa, at least about 20 MPa, or at least about 25 MPa. In some examples, the compressive strength of the composite material may be between about 10 MPa and 40 MPa. The compressive strengths as defined herein may be determined in accordance with the methods described in the examples section and / or in accordance with the method described in D6641-16.

[0079] In some examples, the composite material may comprise a compressive modulus of at least about 1 GPa, at least about 1.5 GPa, or at least about 2.0 GPa. In some examples, the compressive modulus may be between about 1 GPa and 7 GPa, such as between about 1.5 GPa and 6 GPa. The compressive moduli as defined herein may be determined in accordance with the methods described in the examples section and / or in accordance with the method described in D6641-16.

[0080] The tensile strengths, tensile moduli, flexural moduli, flexural strengths, compressive strengths and compressive moduli described above may refer to the same properties of the composite material comprising a glass fiber layer from a machine direction cut sample and / or from a cross machine direction cut sample.

[0081] The composite material may comprise voids throughout its structure. Such voids may be considered as defects to the composite material and higher void volumes can adversely impact the mechanical properties (e.g. in terms of variability in strength, susceptibility to moisture penetration and / or weathering, lower fatigue resistance and the like). In the examples described herein, a void content in the composite material may be less than about 20%, or less than about 15% based on the total volume of the composite material. In other examples, a void content in the composite material may be between about 1% and about 20%, between about 5% and about 15%, or between about 7% and about 13% based on the total volume of the composite material. The void content as defined herein may be determined in accordance with the method described in ASTM standard D3171 and / or in accordance with the methods defined in the examples section.

[0082] The density of the composite material may be varied in accordance with the desired end use (and may be dependent upon the processing conditions during the lamination step). In some examples, the density of the composite material may be at least about 0.25 g / cm3, at least about 0.50 g / cm3, at least about 0.75 g / cm3, or at least about 1.0 g / cm3. In some examples, the density of the composite material may be between about 0.50g / cm3and about 2.0 g / cm3, such as between about 1.0 g / cm3and 1.5 g / cm3.

[0083] A further example of the composite material may comprise: at least one layer of a waste glass fiber mat laminated to at least one layer of a recycled polymer material (e.g. a mixed waste polymer material), wherein the composite material comprises at least 10% by weight of the recycled polymer material and at least 10% by weight of the waste glass fiber mat based on the total weight of the composite. In a yet further example, the composite material may additionally comprise a void content of less than 15 % based on the total volume of the composite.

[0084] In any one or more of the example composite materials described herein, the layer of the recycled polymer material and / or the composite material may comprise multiple adjacent bonded areas of at least two different polymers, each area having a size of between 1 mm to 200 mm in one direction, preferably a size of between 5 mm to 50 mm in one direction.

[0085] In some examples, the composite material may comprise one or more layers of a different material (e.g. one, two, three, four or more layers of a different material). Within the context of the present disclosure, the different material may be an alternative material to the waste glass fiber materials and recycled polymer materials disclosed herein. In other words, the different material may not be a glass fiber mat and may not be a recycled polymer material. The type, nature, number and / or arrangement of the different material layer(s) used in the composite material may be selected based on a desired set of properties to be shown by the final composite material and, for example, may vary in accordance with the intended application and / or use of the composite material. In some examples, the one or more layers of the different material may be interspersed between the layers of waste glass fiber mat and / or the layers of the recycled polymer material. In some examples, the one or more layers of the different material may be arranged as one or more outer layers of the composite material. In some examples, there may be at least two layers of the different material, each one of which forms an outer layer of the composite material (e.g. the two layers of the different material may provide a sandwich laminate arrangement, the inner layers comprising the one or more waste glass fiber layers and the one or more recycled polymer material layers).

[0086] By way of example only, the different material layers may comprise, or be formed of, any one or more materials selected from the following: non-glass fiber composite materials, metals and alternative polymer materials. By way of example, the different material may be a carbon fiber-based material (e.g. a material comprising carbon fibers) such as recycled carbon fiber-based material (e.g. a material comprising carbon fibers and a polyolefin such as maleated polypropylene). Alternative examples of non-glass fiber-based materials may include aramids (e.g. Kevlar® and the like). In some examples, the different material layers may take the form of a fabric or web (e.g. a non- woven fabric), or a film. In other examples, the different material layer(s) may be or comprise a foam (e.g. a foam core). In some examples the foam may comprise an open- celled structure and, in other examples, a closed-cell structure. By way of further example, the different material layer(s) may be or comprise a polyolefin foam material (such as a polyethylene foam).

[0087] As stated above, the method for making the composite material comprises:

[0088] (a) laminating at least one layer of a recycled polymer material to at least one layer of waste glass fiber mat.

[0089] Various features of the composite material, the recycled polymer material and the waste glass fiber matl have been described above, primarily in the context of the composite material itself. However, for the avoidance of any doubt, it will be appreciated that these same features are equally applicable to any of the other aspects of the disclosure and, in particular, the method for making the composite material. For example, the further details and examples of the recycled polymer material and waste glass fiber mat described above are equally applicable to the method defined above. Further details relating to the specific method steps are provided below.

[0090] In some examples, the method may further comprise obtaining or providing a waste polymer material. The method may comprise separating the waste polymer material to provide the recycled polymer material as defined herein (and as used in the composite materials described herein). The step of separating may comprise adding or contacting the waste polymer material to or with water and then separating or removing the polymer material that floats. The separated polymer material may then be used as the recycled polymer material to make and / or form the composite laminates described herein. In particular, the step of separating may comprise separating polymer material that has a density lower than about 1 g / cm3. The separated polymer material (used to form the composite material) consequently comprises a density lower than about 1 gm / cm3.

[0091] Additionally or alternatively, the method may comprise shredding a recycled polymer material to provide a shredded recycled polymer material.

[0092] In some examples, the method may comprise pressing the shredded recycled polymer material to provide a sheet or film of recycled polymer material. In such examples, the sheet or film of recycled polymer material provides the at least one layer of recycled polymer material. In these examples, the layer of the recycled polymer material may comprise multiple adjacent bonded areas of at least two different polymers, each area having a size of between 1 mm to 200 mm in one direction. The step of pressing the shredded recycled polymer material may comprise pressing the material under suitable temperature and pressure conditions and for a suitable time period to allow the shredded polymer material to at least partially melt and bond together. In some examples, the shredded recycled polymer material may be heated to a temperature between about 50 °C and about 300 °C, such as between about 150 °C and about 250 °C, e.g. about 200 °C. In particular, the shredded recycled polymer material may be heated up to a temperature of about 200 °C. The present inventors have identified that for some examples (e.g. where the recycled polymer material comprises polyethylene and / or polypropylene), temperatures of above 200 °C are unsuitable as they lead to degradation.

[0093] In some examples, the shredded recycled polymer material may be subjected to a pressure between about 2 bar and about 5 bar, e.g. about 4 bar. In some examples, the shredded recycled polymer material may be pressed for at least about 1 minute, at least about 5 minutes, or at least about 10 minutes.

[0094] In some examples, the method may comprise providing a layer of waste glass fiber mat and coating the layer of waste glass fiber mat with a layer of recycled polymer material. In such examples, the method may comprise melting a recycled polymer material (optionally a shredded recycled polymer material) and coating the layer of waste glass fiber mat with the molten recycled polymer material (e.g. in an extrusion coating process). In such examples, the molten recycled polymer material cools, solidifies and / or binds to the layer of waste glass fiber mat to provide the at least one layer of waste glass fiber mat laminated to the at least one layer of recycled polymer material.

[0095] The extrusion coating process may facilitate a careful control of the layer thickness as the opening of the die used to apply the coating can be varied. Such examples are particularly amenable to scaled-up manufacture as the extrusion coating process may be continuous.

[0096] As described above, the methods described herein may be used to provide composite materials comprising a plurality of layers of the recycled polymer material and / or a plurality of layers of the waste glass fiber mat. In such examples, where a plurality of layers of either (or both) of the recycled polymer material and the waste glass fiber mat are required, the method may further comprise:

[0097] (a) stacking the plurality of layers of recycled polymer material and the plurality of layers of waste glass fiber mat in a desired arrangement or lay-up; and

[0098] (b) laminating the layers together. In some examples, the method may comprise sandwiching at least one layer of recycled polymer material between a first and second layer of waste glass fiber matand laminating the layers together.

[0099] In some examples, a construct (or two-layer construct) (e.g. comprising, consisting of, or consisting essentially of, a layer of waste glass fiber mat bonded (or prebonded) to a layer of recycled polymer material) may be provided by the extrusion coating process. Such a construct may be used as a “prepreg” in composite materials which comprise a greater numbers of layers of waste glass fiber mats. In other words, in some examples, at least one layer of waste glass fiber mat has been laminated to at least one layer of recycled polymer material prior to the lay-up of the desired arrangement of layers. One or more of these constructs (e.g. two-layer constructs) may then be laminated to additional layers of waste glass fiber mat during the lamination step to provide a final composite material.

[0100] Accordingly, in such examples, the method may comprise:

[0101] (a) stacking one or more constructs with a plurality of layers of waste glass fiber mat in a desired arrangement or lay-up, each construct comprising a layer of waste glass fiber mat laminated to a layer of recycled polymer material; and

[0102] (b) laminating the construct(s) and layers together.

[0103] In the methods described herein, the laminating step comprises bonding the layers together by applying a suitable temperature and pressure such that the recycled polymer material melts and binds to the waste glass fiber mat, bonding the layers together. In particular, the temperature and pressure may be any suitable temperature and pressure that causes the recycled polymer material to melt to a viscosity that facilitates the penetration and / or wetting of a porous glass fiber fabric layer. (This same process may apply whether or not the layer of recycled polymer material is provided on the construct, as per the example above). The skilled person will appreciate that the exact temperature, pressure and duration of the lamination step may depend upon a number of factors (including but not limited to, the number, nature, physical and chemical properties and arrangement of the layers) and would be able to select the appropriate conditions to facilitate the bonding of the layers together.

[0104] By way of example, the method may comprise heating the layers (e.g. a temperature between about 100 °C and about 300 °C, such as between about 100 °C and about 250 °C, or between about 150 °C and about 200 °C, or between about 160 °C and about 190 °C), under pressure (e.g. at a pressure between about 1 bar and 50 bar, such as between about 10 bar and 30 bar) such that the layers bond together. For example, such that the recycled polymer material is melted to a degree that facilitates its penetration into the waste glass fiber mat by viscous flow of the material. The temperature may such that it melts the recycled polymer material without causing degradation of the material (e.g. the temperature may be below a degradation temperature of the recycled polymer material). A suitable temperature and pressure may depend upon the nature of the recycled polymer material feedstock, e.g. a temperature of at least about 160 °C may be used for recycled polymer material comprising mixed polyolefins.

[0105] According to a yet further aspect of the disclosure, there is provided a composite material made in accordance with the methods described above and herein.

[0106] According to a yet further aspect, there is provided a use of the composite material as described herein, or made in accordance with the methods described herein, in any application.

[0107] Indeed, the composite materials as described herein (and as made by the methods described herein) may find use in a wide range of applications. The ability to provide composite materials comprising layers of recycled polymer material and layers of waste glass fiber matwith robust mechanical properties facilitates the use of these composite materials in any application that requires one or more of strength, impact resistance, durability and / or stiffness. By way of example only, the composite materials may find use in the construction sector (e.g. as a building material, optionally for low cost and / or temporary housing in disaster zones (e.g. hurricane-resistant panels)), in the transport sector (e.g. in automotive, railway, marine applications and the like), in the sports sector (e.g. in sports equipment), and in the agricultural sector (e.g. outdoor buildings for livestock or for storing crops, water reservoirs and other agricultural composite products and the like).

[0108] It should be noted that the terms “comprise”, “comprising” and / or “comprises” is / are used to denote that aspects and embodiments of this invention “comprise” a particular feature or features. It should be understood that this / these terms may also encompass aspects and / or embodiments which “consist essentially of” or “consist of’ the relevant feature or features.

[0109] The term “about” herein, when qualifying a number or value, may be used to refer to values that lie within ± 5% of the value specified.

[0110] As used herein, where any range is described as being between a lower limit and an upper limit, the defined range includes the defined endpoints (and so includes both the lower limit and upper limit values). As used herein, the terms “glass fiber" and “waste glass fiber” shall have the same technical meaning in regard of the chemical and mechanical properties of the glass fiber product (e.g. glass fiber mat, glass fiber layer).

[0111] DETAILED DESCRIPTION

[0112] The present disclosure will now be described, by way of example only, with reference to the following Figures:

[0113] Figure 1 : (a) shows waste mixed plastics (wMP) in shredded form; and (b) waste glass fabric / non-woven mat (wGF); and (c) to (h) show a number of defects or damages that may be present in a waste glass fiber fabric, e.g. defects or damages which render a glass fiber fabric unusable in an intended application (sometimes referred to herein as “out of specification”, in particular: (c) shows “stringers” that result out of a non-uniform dispersion of the glass fiber in the fabric, wherein staple glass fiber agglomerates may stick together in bundles, resulting in a net-like appearance in the glass fiber fabric; (d) shows an example of clumping in a glass fiber fabric, wherein a clump or clumps of glass fiber and binder material builds up in the fabric (sometimes causing delamination); (e) shows an example of a “tent” in a glass fiber fabric, the tent comprising a bulge in the glass fiber fabric; (f) shows an example of a “buckle” wherein the structure and / or surface of the waste glass fiber fabric becomes uneven and / or has a puckered appearance; (g) shows an example of a rupture in the waste glass fiber fabric; and (h) shows an example of a waste glass fiber fabric having uneven coloration, in particular, the black colour in the binder and / or the binder may be unevenly dispersed leading to white spots in the black fabric and an inhomogeneous appearance.

[0114] Figure 2 shows waste mixed plastics (wMP) pressed film.

[0115] Figure 3 shows manufactured rolls of waste mixed plastic coated waste glass fiber according to an example of the disclosure.

[0116] Figure 4 shows lay-ups of exemplary composite laminates, (a) laminate 1 (L1-MD-S-23); (b) laminate 2 (L2-MD-S-23); (c) laminate 3 (L3-MD-C-23); (d) laminate 4 (L4-MD-C-26); (e) laminate 5 (L5-CMD-C-24) (i) after first processing cycle (ii) after second processing cycle (f) laminate 6 (L6-CMD-C-25); (g) Laminate 7 (L7-CMD-C-29); (h) Laminate 8 (L8- CMD-C-25); (i) Laminate 9 (L9-CMD-C-25_40); (j) Laminate 10 (L10-MD-C-25); (k) of Laminate 11 (L11-CMD-C-25).

[0117] Figures 5a shows the frames used to manufacture example laminates 1-6; (a) shows mold 1 (M1); (b) shows mold 2 (M2). Figure 6 shows Mold 3 (M3), a two-piece mold with 2 mm cavity used to manufacture example laminates 7 - 11.

[0118] Figure 7 shows the theoretical tensile modulus of randomly oriented short glass fiber reinforced waste mixed plastics in laminate (top line) and extruded (bottom line) form using the Halpin-Tsai equation with the MT-LA approach.

[0119] Figure 8 shows a comparison of tensile strength between unreinforced waste mixed plastics and different waste mixed plastics laminates reinforced with waste glass fiber mat with samples cut in the machine direction (MD).

[0120] Figure 9 shows a comparison of tensile strength between unreinforced waste mixed plastics and different waste mixed plastics laminates reinforced with waste glass fiber mat with samples cut in the cross machine direction (CMD).

[0121] Figure 10 shows a comparison of tensile modulus between unreinforced waste mixed plastics and different waste mixed plastics laminates reinforced with waste glass fiber mat of samples cut in the machine direction. *L1-MD-S-23 samples tensile properties were calculated using the crosshead extension of the test frame, and not using the video extensometer to measure the strain values directly.

[0122] Figure 11 shows a comparison of tensile modulus between unreinforced waste mixed plastics and different waste mixed plastics laminates reinforced with waste glass fiber mat of samples cut in the cross machine direction.

[0123] Figure 12 shows a comparison of the flexural modulus between unreinforced waste mixed plastics and waste mixed plastic laminates reinforced with various amounts of waste glass fiber mat with samples cut in the machine direction.

[0124] Figure 13 shows a comparison of the flexural modulus between unreinforced waste mixed plastics and waste mixed plastic laminates reinforced with various amounts of waste glass fiber mat with samples cut in the cross machine direction.

[0125] Figure 14 shows the compressive strength of laminates reinforced with various amounts of waste glass fiber mat with samples cut in the machine direction.

[0126] Figure 15 shows the compressive strength of laminates reinforced with various amounts of waste glass fiber mat with samples cut in the cross machine direction.

[0127] Figure 16 shows the compressive modulus of laminates reinforced with various amounts of waste glass fiber mat with samples cut in the machine direction.

[0128] Figure 17 shows the compressive modulus of laminates reinforced with various amounts of waste glass fiber mat with samples cut in the cross machine direction. Figure 18 shows a scanning electron microscopy (SEM) image of a tensile fracture surface showing the interface between waste mixed plastics and waste glass fiber mat in example laminate 3 (L3-MD-C-23).

[0129] Figure 19 shows SEM images atx25 magnification showing the impregnation of the wMP across the thickness of example laminates 1-9.

[0130] Figure 20 shows stress (MPa) vs strain (%) for tensile test of new wGF / wMP example laminates.

[0131] Figure 21 shows stress (MPa) vs strain (%) for tensile test of black wGF / wMP example laminates.

[0132] Figure 22 shows force (N) vs displacement (mm) for tensile test new wGF / wMP example laminates.

[0133] Figure 23 shows force (N) vs displacement (mm) for tensile test of black wGF / wMP example laminates.

[0134] Figure 24 shows average tensile strength (left) and tensile modulus (right) for the new wGF / wMP and black wGF / wMP example laminates.

[0135] Figure 25 shows a comparison of ultimate tensile strength (UTS) and fiber volume fraction (FVF) of example wMP laminates with different wGF types and contents.

[0136] Figure 26 shows a plot of tensile modulus against fiber volume fraction (FVF) for example wMP laminates with different wGF types and contents.

[0137] Figure 27 shows stress (MPa) vs strain (%) for flexural test of new wGF / wMP example laminates.

[0138] Figure 28 shows stress (MPa) vs strain (%) for flexural test of black wGF / wMP example laminates.

[0139] Figure 29 shows force (N) vs mid-span deflection (mm) for flexural test of new wGF / wMP example laminates.

[0140] Figure 30 shows Force (N) vs mid-span deflection (mm) for flexural test of black wGF / wMP example laminates.

[0141] Figure 31 shows average flexure strength (left) and flexure modulus (right) for the new wGF / wMP and black wGF / wMP example laminates.

[0142] Figure 32 shows force (N) vs displacement (mm) for compressive test of new wGF / wMP example laminates.

[0143] Figure 33 shows force (N) vs displacement (mm), for compressive test of black wGF / wMP example laminates.

[0144] Figure 34 shows average compressive strength for the new wGF / wMP and black wGF / wMP example laminates. Figure 35 shows SEM micrographs showing the cross-section of a laminate with: (a) acrylic binder, new white wGF fabric based composite; and (b) melamine formaldehyde binder, black wGF based composites, both at x100 magnification.

[0145] Experimental:

[0146] Part A: Waste mixed plastics (wMP) / waste glass fiber (wGF) Composites

[0147] A.1. Materials

[0148] The primary material of focus in this study are waste mixed plastics (wMP) and waste glass fabric / nonwoven mat (wGF).

[0149] The wMP is washed, shredded, and supplied by PALTECH (Polymer Alloy Technology) (Figure 1a)

[0017] , PALTECH takes the plastic wastes originating from food packaging from Tesco Ireland stores

[0018] , These mixed plastics packaging wastes undergo one stage of sorting, which is float-sink separation. The wMP that float on water are collected by PALTECH. Therefore the wMP supplied by PALTECH contains mainly polyolefins having densities lower than water.

[0150] The waste glass fabric (wGF) used was waste glass fabric from the production of EVALITH DH100, supplied by Johns Manville (Figure 1b). The wGF is virgin production waste and consists of non-woven glass fabric (GF) mat with an organic binder (urea formaldehyde resin and polymer dispersion) present on the wGF surface. According to the specification of EVALITH DH100 glass fabric the organic binder content has a dry mass weight of approximately 22 to 23 wt% of the GF (measured by loss on ignition testing according to DIN EN 13820). The GF became wGF because of a low binder content in the range of 17 wt%. The wGF has an areal weight of 100 gsm (with binder) measured according to DIN EN 29 037-1. The used wGF material out of EVALITH DH100 has a mean air permeability at 100 Pa of 2500 l / m2*s (measured according to DIN EN ISO 9237). According to its specification the GF should have a mean tensile strength MD of 460 N / 5 cm and a mean tensile strength CMD of 260 N / 5 cm (measured according to DIN EN 29 073-3). The used wGF with such low binder content shows a lowered tensile strength of below 360 N / 5cm. The used wGF material out of EVALITH DH100 has a pore size of 31 pm. EVALITH DH100 material comprises glass fibers having a mean length of 18 mm and a mean diameter of 13 pm.

[0151] During manufacturing, rolling and transportation of a glass fabric material a number of defects can arise, leading to the glass fabric becoming waste glass fabric. Out of specification waste glass fabric can be a batch quantity wherein the binder content is below 19 wt% of the GF leading to a low tensile strength. A binder content above 25 wt% is also out of the specification, the higher amount of binder probably leading to decreased wettability. A mean tensile strength MD of less than 370 N / 5 cm and a mean tensile strength CMD of less than 200 N / 5 cm (measured according to DIN EN 29 073-3) are too low to perform the required strengthening in a composite application. Such production batch will be classified as waste glass fabric. In general, a decrease of the strength of more than 25 % of the targeted strength value, e.g. tensile strength classifies the manufactured glass fiber fabric as a waste glass fiber fabric.

[0152] Figures 1c to Figure 1h show a number of defects or damages that may cause a decreased tensile strength or make the glass fiber fabric unusable in a destined application. Figure 1c shows stringers that result out of a non-uniform dispersion of the glass fiber in the fabric, wherein staple glass fiber agglomerates stick together in bundles, building a net in the fabric, which leads to visual and mechanical inhomogeneities. Another defect that can be observed is clumping as shown in Figure 1d. In such examples, a clump or clumps of glass fiber and binder material builds up in the fabric and might even delaminate.

[0153] Due to internal stresses or due to local thermal stresses during thermal consolidation of the glass fiber fabric, the fabric can shrink, resulting inwrinkles, such as line wrinkles across the width or length of a batch. Another defect is local “tents” as illustrated in Figure 1e, wherein the glass fiber fabric locally bulges.

[0154] Visual defects might be caused by discoloration or uneven coloration. Figure 1h shows an example of a waste glass fiber fabric wherein the black colour in the binder and / or the binder is unevenly dispersed leading to white spots in the black fabric.

[0155] Defects or damages may also result out of rolling the glass fiber fabric for transportation and out of the transportation step. At the end of the manufacturing line the freshly manufactured glass fiber fabric is rolled onto a round carrier. If the tensile strength within the glass fiber fabric varies or the rolling speed or tension varies, buckles as illustrated in Figure 1f may result. At the buckles the fabric wrinkles or even may rupture as illustrated in Figure 1g.

[0156] According to the underlying invention as disclosed herein, waste glass fabric shall mean any arbitrary compilation of such glass fiber fabric material, whether in roll form or as shredded unregular sheets and / or glass fiber fabrics being out of specification and / or arbitrarily showing any kind of the illustrated and described defects or damages.

[0157] A.2. Manufacturing composites

[0158] Route 1 The first set of composite laminates were manufactured directly from the wMP shreds and wGF fabrics / non-woven mats. The wMP shreds were pressed in a hydraulic press prior to layup to create thin films with a thickness of approximately 0.5 mm (Figure 2) that can be easily stacked with the wGF.

[0159] To manufacture the wMP films, the wMP shreds were added between two flat metal plates at room temperature. Then the heating cycle started at a rate of 10 deg C / min until 200 degrees was reached, then the 4 bar pressure was added. It was held at 200 C under 4 bar pressure for 10 minutes before cooling back to room temperature.

[0160] A temperature below 200 °C is preferred for composites comprising waste glass fiber fabrics, such fabrics being consolidated with binders up to a dry mass binder content of between about 10 weight % to about 30 weight %, or between about 15 weight % to about 25 weight % (such as about 18 weight %). Binders contained in the waste glass fiber fabric like Urea Formaldehyde (UF), Acrylic and Melamine Formaldehyde (MF)will decompose and maybe even burn at elevated temperatures above 200°C.

[0161] Laminates were manufactured by compression molding with a PEI lab 450 hydraulic press, using three piece mold for laminates 1 to 6 (L1 to L6) (a steel frame in the middle and two flat metal plates on the top and bottom) and a two-piece mold for laminates 7 to 11 (L7 to L11) (cavity mold, M3 in Figure 6). The wGF and wMP were stacked according to the desired wGF content.

[0162] The processing cycle used in the hydraulic press was as follows:

[0163] 1 . Heating from 20 °C to 200 °C at a rate of 10 °C / min.

[0164] 2. Holding at 200 °C for 20 minutes at 25 bar pressure.

[0165] 3. Cooling from 200 °C to 20 °C at 10 °C / min at 25 bar pressure.

[0166] Route 2

[0167] A set of wMP coated wGF fabric was produced that can be used as a prepreg for manufacturing composites. The thickness of the wMP layer on the wGF was approximately 0.95 mm. The thickness of the coating can be varied as required. In this work, the coating thickness was kept constant around 0.95 mm. The coating of wGF with wMP is a continuous process and can be easily translated to an industrial scale.

[0168] The outcome of this continuous coating process is a roll of extruded sheet wMP with wGF bonded on the surface (Figure 3). This roll can be cut to the required laminate dimensions and compression molded to produce wMP / wGF laminates. Additional layers of wGF can be added to increase the glass fiber content of the laminate. Fiber Orientation

[0169] Due to the manufacturing process of short glass fiber non-woven mats, there is some orientation of the fibers towards the direction of travel during manufacturing. Therefore, there are more fibers aligned towards the machine direction (MD) than in the cross machine direction (CMD).

[0170] Example Laminates

[0171] Eleven laminates were produced using either route 1 or route 2, with different amounts of wMP and wGF mat. Test samples were taken from some laminates in the machine direction (MD), and from others in the cross machine direction (CMD). Descriptions of the laminates are provided below, with sample IDs marked by 'S' for shreds and 'C for coated. The samples cut in the machine direction are indicated by 'MD', while those cut in the cross machine direction are indicated by 'CMD'.

[0172] Examples laminates 1 to 11 are detailed below in Table 1 and their lay-ups are illustrated in Figures 4a to 4k.

[0173]

[0174] Table 1 showing details of processing route (i.e. route or 2 as defined above), number of wMP layers, wGF mat layers, thickness of composite laminate material, total wGF content (volume % based on total volume of composite laminate material); void content of the composite laminate material (volume % based on total volume of composite laminate material); and density for each of example laminates 1 to 11). *L5 was manufactured using two processing cycles.

[0175] Three separate molds were used for the manufacture of the laminates; two steel frames of varying thickness (3 mm and 2 mm) and one closed two piece cavity mold with cavity depth of 2 mm. As noted above, metal plates were placed on either side of each frame before compression molding. The mold / frames used are shown in Figures 5a and 5b.

[0176] Mold 1 (M1) had a thickness of 3 mm, allowing the manufacture of laminates with dimensions 350 x 300 x 3 mm, and was used to manufacture example laminates 1 - 4. Mold 1 (M2) had a thickness of 2 mm, allowing the manufacture of laminates with dimensions 350 x 300 x 2 mm. Mold 2 was used to manufacture example laminates 5 and 6.

[0177] Figure 6 shows the two-part mold (Mold 3 (M3)) used to manufacture example laminates 7 - 11 , with inner cavity dimensions of 350 x 300 x 2 mm.

[0178] A.3. Analysis of manufactured composite materials

[0179] Example laminates 1 to 11 were then analysed using the following test methods.

[0180] Density

[0181] The density of each plaque was measured using an OHALIS density determination kit, and following ASTM standard ASTM D792. Six samples were measured from each set. The following equation was used to determine the density of each sample, and an average was taken for each plaque.

[0182] Void content

[0183] To measure the void content, samples from each laminate were held in a Nabertherm furnace at 550 °C for 5 hours to completely remove the matrix. The fiber volume fraction (FVF) of each sample was calculated following ASTM standard D3171. The weight of the organic binder was taken into consideration when calculating the FVF of the samples.

[0184] Tensile testing

[0185] Tensile testing was used to determine the tensile strength and modulus of each type of laminate. Six samples measuring 250 x 25 x ~3 mm were tested on an Instron test frame fitted with a 10 kN load cell, and following ASTM D3039. Each sample was loaded at a speed of 2 mm / min until failure, and the values for the load and extension were recorded using the Bluehill® testing software. Flexural testing

[0186] Flexural testing was carried out following ASTM D790, using six samples from each laminate with a testing span of 48 mm. The testing speed used was 5.12 mm / min on an Instron 3369 test frame fitted with a 10 kN load cell, and the span to thickness ratio was 16:1 following the standard. The load and deflection values were recorded using the Bluehill® testing software.

[0187] Compression testing

[0188] Compression testing was carried out following ASTM D6641 , using six samples measuring 140 x 13 x ~3 mm. The testing speed used was 1.28 mm / min on an Instron 2269 test frame fitted with a 10 kN load cell, and the strain was measured using a video extensometer. Values for the load were recorded using the Bluehill® testing software.

[0189] Microscopy

[0190] Following the tensile testing, scanning electron microscopy (SEM) was used to analyse the fracture surface of the failed tensile specimens using a JEOL JSM series instrument. Each sample was prepared by gold spluttering to increase the conductivity, and the voltage used to observe the samples was 15 kV. Scanning electron micrographs were also used to see the quality of consolidation of the laminate.

[0191] Results and Discussion

[0192] Tensile testing

[0193] The tensile test results of the laminates are provided below. The Halpin Tsai equation was used to determine the theoretical tensile modulus of the laminate. The Mori-Tanaka laminated analogy(MT-LA) approach was used to obtain the coefficient a to use within the Halpin Tsai equation as this is more accurate for composites with 2-D dispersion of short fiber reinforcement

[0019] ,

[0194] The Halpin Tsai equation is as follows:

[0195] Ec= aEL+ (1 — a)ET

[0196] Where:

[0197] The MT-LA approach used: a = 0.339 - 0.0351^ - 0.642

[0198] Where:

[0199] Ec = Composite elastic modulus

[0200] EL = Longitudinal elastic modulus ET = Transverse elastic modulus

[0201] Em= Matrix elastic modulus

[0202] Er= Reinforcement elastic modulus Vf = Volume fraction

[0203] I = length of reinforcement r = radius of reinforcement a = constant coefficient

[0204] As the matrix is composed of waste materials, the proportion of each waste plastic present in the mix is unknown and cannot be predetermined. This can also vary from one batch to another. A range of values can therefore be expected by considering the moduli of LDPE, HDPE and PP with the Halpin Tsai equation, as shown in Figure 7 the wMP properties are likely to vary due to variation in the composition of the wMP, but when combined with mechanically superior wGF, the variability is reduced.

[0205] The Halpin Tsai equation can also be used to determine the expected tensile modulus for short fiber reinforced composites where the short fibers are uniformly distributed throughout the bulk matrix where short fibers are dispersed 3-dimensionally e.g. as observed in extruded or injection molded composites, by using a different alpha value, using the following equation: a = 0.13 + 0.0815^ - 1.669

[0206] Using that equation, the theoretical variation for wMP and wGF uniformly mixed in a composite can be calculated, and that is shown in the graph below (Figure 7, bottom line). From this it is clear that the tensile modulus is higher in a laminate (where short fibers are dispersed 2-dimensionally) than in a bulk composite (where short fibers are dispersed 3-dimensionally). Figure 7 illustrates the theoretical modulus for a non-woven glass fiber mat with random orientation (dispersed 2-dimensionally) and 0 vol% void content. The orientation of Evalith DH100 GF mat, on the other hand, has an MD to CMD ratio of 1.8. The wGF mat used here (Evalith DH100 GF) has a directionality (MD:CMD 1.8), so its reinforcing effect will be slightly different to an equivalent randomly oriented mat. There is no Halpin Tsai eqn form currently available that can take account of this directionality. The inventors have therefore used this form of Halpin Tsai as a close reference.

[0207] The experimentally measured tensile strength results of example laminates 1 - 11 as well as unreinforced wMP are shown in Figures 8 and 9 (in MD and CMD respectively).

[0208] The highest tensile strength of the wGF reinforced wMP laminates was found in Laminate 3 (L3-MD-C-23), with a value of 42.4 ± 1.2 MPa. As Laminate 3 has a wGF content of 23 vol%, the effect of adding 23 vol% wGF to unreinforced wMP is an increase in the tensile strength from 9.7 - 42.4 MPa, an increase of around 340%.

[0209] Figures 10 and 11 show the tensile modulus of example laminates 1 - 11 in MD and CMD respectively as well as the unreinforced wMP.

[0210] The highest tensile modulus of the glass fiber reinforced wMP laminates was found in Laminate 4 (L4-MD-C-26), with a value of 5.3 ± 0.2 GPa, which is 7.5% lower than the theoretically calculated tensile modulus. The lower experimental value can be attributed to the void content of the laminate, as the Halpin Tsai method assumes 0% void. The directionality also plays a role. With improved quality of consolidation and lower void content, this value is likely to match closely with the theoretically calculated values.

[0211] Flexural testing

[0212] The flexural modulus results of the investigated materials are given below in Figures 12 and 13 in MD and CMD respectively.

[0213] Compression testing

[0214] Figures 14 and 15 show the results of the compressive strength for laminates with samples cut in the MD and CMD respectively. Figure 16 and 17 show the compressive modulus for the laminates with samples cut in MD and CMD respectively.

[0215] Fracture surface analysis (Fiber / matrix interface) Figure 18 shows SEM micrographs of tensile fracture surfaces revealing the quality of interfacial bonding between the wMP and wGF. The two samples are from two different batches of samples made in the gap of one year.

[0216] The impregnation of wMP through the thickness of the laminates is shown in Figure 19. As shown in Figure 4a to 4k, two layers of wMP coated wGF mat were used with several layers of dry wGF layers. The permeation of molten wMP across all the wGF mat layers was found acceptably good in all the laminates.

[0217] Part B: Waste mixed plastics (wMP)Zwaste glass fiber (wGF) Composites

[0218] B.1. Materials

[0219] The materials used to produce the laminates are waste mixed plastics (wMP) and two different types of waste glass fiber mats (wGF) - in the form of a non-woven mat with two different binders. The two types of wGF that were used as the reinforcement are: o A black coloured wGF (this is referred to as black wGF here); it has a melamine-formaldehyde (MF) binder that contains some carbon black (hence the black colour) and has a nominal weight of 75 gsm (with binder), a 13 pm fiber diameter and a 12 mm fiber length (SM 75 / 1). o A white coloured wGF (this is referred to as new wGF here); it has an acrylic binder and has a nominal weight of 50 gsm (with binder), a 13 pm fiber diameter and 18 mm fiber length (FF 50 / 4).

[0220] The used wGF mat (black and white coloured) were classified as wGF because of visual defects in the waste glass fiber mat. These were staple glass fiber agglomerates, (stringers) and clumps of glass fiber and binder material.

[0221] All the three different wGF fabrics used are given in the table below.

[0222] Table 2 shows different wGF fibres used to produce composites B.2. Manufacturing composites

[0223] The manufacturing and the processing cycle of the laminates is the same as the one followed for the example wGF / wMP laminates as described for example laminates 1 to 11 above.

[0224] Briefly, 28 wGF mat plies were used in total and 2 wMP plies. The layup stacking sequence was: o 10 wGF plies, o One wMP coated wGF ply, o Eight wGF plies, o One wMP coated wGF ply, and finally, o 10 wGF plies.

[0225] The wMP coated wGF ply was produced in accordance with the method outlined in “Route 2” above.

[0226] The new wGF / wMP plies were placed within the steel mold’s top and bottom pieces (mold 3 as described above) and the processing cycle was followed. It should be noted that the same sequence was followed for both the new and the black wGF / wMP example laminates.

[0227] All example laminates were processed at 20 bar pressure and kept at 200°C for 20 min after which they were rapidly cooled down to lab room temperature. The nominal thickness of the laminates was around 3 mm and the consolidation appeared to be visually very good.

[0228] Example laminates 12 (new white wGF mat) and 13 (Black wGF mat) are detailed in Table 3 below.

[0229] * New: white wGF mat with acrylic binder and Black: Black wGF mat with MF binder

[0230] Table 3 shows details of laminate 12 and 13 Table 3 shows the experimental (measured) fiber volume fraction (FVF) properties for the new and the black wGF / wMP. Vv0id refers to the void volume ratio; Vmrefers to the matrix volume ratio; and Vf refers to the fiber volume ratio.

[0231] Matrix burn-off was used for the measurement of FVF Vf) in accordance with ASTM D3171-15.

[0232] Comparing Table 3 to the theoretical estimations presented in Table 4 and Table 5, a good agreement was observed (noting also that the theoretical estimations do not account for void content). It should be noted that the theoretical estimations are based on the wGF and wMP weight prior to the laminate manufacture / processing cycle.

[0233] Table 4. New wGF / wMP Table 5. Black wGF / wMP theoretical estimations. theoretical estimations. wMP vol % 77.13 wMP vol% 68.50 wGF vol % 12.87 wGF vol% 18.69 binder vol% 6.54 binder vol% 9.49

[0234] The tensile (samples extracted in MD), flexural (samples extracted in CMD), and compressive properties (samples extracted in CMD) of the two different types of laminates were assessed through experimental testing. Instron 3369 Tensile Tester with a 50kN load cell was used for all tests along with a digital image correlation (DIC) system for strain monitoring. The main results are presented in the accompanying figures as noted below.

[0235] With respect to tension, the ASTM D3039M-21 standard test method was followed and coupon specimens with nominal dimension of 250x25x3mm were extracted from the laminates. Seven tests per material type were performed. The resultant stress versus strain curves are presented in Figure 20 and Figure 21 and the force versus displacement curves are presented in Figure 22 and Figure 23 respectively. These plots are for both the new wGF / wMP and black wGF / wMP specimens.

[0236] The average tensile strength and modulus of both material types are shown in Figure 24.

[0237] Tensile Properties of Laminates produced with wGF mat fabrics with three different binders

[0238] The mechanical properties are in the same range with different binder types. This indicates that the proposed technology is likely to work with any wGF fabric type (Figures 25 and 26). Flexural Tests

[0239] Regarding the flexural tests, the ASTM D790 standard test method was followed and coupon specimens with nominal dimension of 125x13x3mm were extracted from the laminates. The span to thickness ratio was 32:1 as per standard requirements and seven tests per material type where performed. The resultant stress versus strain curves and the force versus displacement curves are presented in Figure 27 and Figure 28, and, Figure 29 and Figure 30, respectively. These plots are for both the new wGF / wMP and black wGF / wMP specimens.

[0240] The average flexure strength and modulus of both material types are shown in Figure 31.

[0241] Compression Test

[0242] For the compression tests, the D6641-16 standard test method was followed and coupon specimens with nominal dimension of 140x13x3mm were extracted from the laminates. Seven tests per material type where performed. The resultant force versus displacement curves are presented in Figure 32 and Figure 33 for the new wGF / wMP and black wGF / wMP specimens, respectively.

[0243] The average compressive strength of both material types is shown in Figure 34.

[0244] SEM Micrographs

[0245] The cross sections of the laminates show adequate impregnation of the wMP matrix across the thickness of the laminates (Figures 35a for new wGF / wMP and 35b for black wGF / wMP).

[0246] References

[0247] 1. Schyns, Z.O.G. and M.P. Shaver, Mechanical Recycling of Packaging Plastics: A Review. Macromolecular Rapid Communications, 2021. 42(3): p. 2000415.

[0248] 2. Smith, L., Plastic Waste. 2021 , House of Commons Library.

[0249] 3. Elliot, T. and L. Elliot, A PLASTIC FUTURE: PLASTICS CONSUMPTION AND WASTE MANAGEMENT IN THE UK. 2018.

[0250] 4. Yousif, B., K.O. Low, and N.s.M. El-Tayeb, Fabricating and Tensile Characteristics of Recycled Composite Materials. Journal of Applied Sciences, 2006. 6: p. 1380-1383. 5. Cecon, V.S., et al., The effect of post-consumer recycled polyethylene (PCRPE) on the properties of polyethylene blends of different densities. Polymer Degradation and Stability, 2021. 190: p. 109627.

[0251] 6. Alqaflah, A.M., et al., Preparation and characterization of glass fiber-reinforced polyethylene terephthalate / linear low density polyethylene (GF-PET / LLDPE) composites. Polymers for Advanced Technologies, 2018. 29(1): p. 52-60.

[0252] 7. Delli, E., et al., Fibre length and loading impact on the properties of glass fibre reinforced polypropylene random composites. Composite Structures, 2021. 263: p. 113678.

[0253] 8. Bajracharya, R.M., et al., Experimental and theoretical studies on the properties of injection moulded glass fibre reinforced mixed plastics composites. Composites Part A: Applied Science and Manufacturing, 2016. 84: p. 393-405.

[0254] 9. Avalos, F., M.A. Lopez-Manchado, and M. Arroyo, Crystallization kinetics of polypropylene III. Ternary composites based on polypropylene / low density polyethylene blend matrices and short glass fibres. Polymer, 1998. 39(24): p. 6173-6178.

[0255] 10. Gupta, A.K., et al., The effect of addition of high-density polyethylene on the crystallization and mechanical properties of polypropylene and glass-fiber-reinforced polypropylene. Journal of Applied Polymer Science, 1982. 27(12): p. 4669-4686.

[0256] 11. Ayadi, A., et al., Recycling effect on mechanical behavior of HDPE / glass fibers at low concentrations. Journal of Thermoplastic Composite Materials, 2011. 25(5): p. 523-536.

[0257] 12. Sormunen, P. and T. Karki, Compression Molded Thermoplastic Composites Entirely Made of Recycled Materials. Sustainability, 2019. 11: p. 631.

[0258] 13. Das, K., et al., Development of Recycled Polypropylene Matrix Composites Reinforced with Fly Ash. Journal of Reinforced Plastics and Composites, 2010. 29(4): p. 510-517.

[0259] 14. Gryczak, M., et al., Recycled low-density polyethylene composite to mitigate the environmental impacts generated from coal mining waste in Brazil. Journal of Environmental Management, 2020. 260: p. 110149.

[0260] 15. Martikka, O. and T. Karki, Promoting Recycling of Mixed Waste Polymers in Wood-Polymer Composites Using Compatibilizers. Recycling, 2019. 4(1): p. 6.

[0261] 16. Moreno, D.D.P. and C. Saron, Low-density polyethylene waste / recycled wood composites. Composite Structures, 2017. 176: p. 1152-1157.

[0262] 17. PALTECH Polymer Alloy Technology. 2022; Available from: https: / / paltech.ie / . 18. Raidio Teilifis Eireann, R. Tesco Ireland partners with Paltech to recycle soft plastics. 2021 [cited 2022; Available from: htps: / / www.rte.ie / news / business / 2021 / 0204 / 1195057-tesco-partners-with-paltech-to- recycle-soft-plastics / . 19. Shokrieh, M.M. and H. Moshrefzadeh-Sani, On the constant parameters of

[0263] Halpin-Tsai equation. Polymer, 2016. 106: p. 14-20.

Claims

CLAIMS:

1. A composite material comprising: at least one layer of a waste glass fiber mat laminated to at least one layer of a recycled polymer material; wherein the recycled polymer material has a density lower than about 1 g / cm3.

2. A composite material according to claim 1 , wherein the pore size in the waste glass fiber mat is between about 5 pm to about 50 pm.

3. A composite material according to claim 1 or 2, wherein the waste glass fiber mat comprises staple glass fibers having a nominal length of between about 5 mm to about 100 mm.

4. A composite material according to any one of the preceding claims, wherein the waste glass fiber mat comprises staple glass fibers having diameters in the range of between about 1 pm to 50 pm.

5. A composite material according to any one of the preceding claims, wherein the recycled polymer material is a mixed waste polymer material, and / or comprises at least two or more different polymers.

6. A composite material according to any one of the preceding claims, wherein the recycled polymer material comprises a mixture of two or more thermoplastic polymers, optionally selected from polyethylene, and polypropylene.

7. A composite material according to claim 5 or 6, wherein the two or more different polymers are each independently selected from high density polyethylene (HDPE), low density polyethylene (LDPE), linear low density polyethylene (LLDPE), medium density polyethylene (MDPE), chlorinated polyethylene (CPE), very low density polyethylene (VLDPE), high molecular weight polyethylene (HMWPE), ultra-low-molecular weight polyethylene (ULMWPE) and ultra-high-molecular weight polyethylene (UHMWPE), polypropylene (PP), and combinations thereof.

8. A composite material according to claim 6 or 7, wherein the recycled polymer material comprises multiple adjacent bonded areas of the two or more thermoplastic polymers, each area having a size of between 1 mm to 200 mm, preferably a size of between 5 mm to 50 mm in one direction.

9. A composite material according to any one of the preceding claims, wherein:(i) the recycled polymer material comprises or is a post-consumer or postindustrial mixed plastic waste material; and / or(ii) the waste glass fiber mat comprises or is a post-consumer or post-industrial waste glass fiber mat.

10. A composite material according to any one of the preceding claims, wherein the at least one layer of recycled polymer material is a film or sheet formed by pressing (e.g. compression molding) shredded polymer material under heat and pressure, optionally shredded waste polymer films or sheets.

11. A composite material according to any one of the preceding claims, wherein the composite material comprises a plurality of layers of the recycled polymer material and / or a plurality of layers of the waste glass fiber mat, and optionally wherein the number of waste glass fiber mat layers is between 5 to 20 times higher than the number of recycled polymer material layers.

12. A composite material according to any one of the preceding claims, wherein at least one layer of recycled polymer material is sandwiched between a first and second layer of the waste glass fiber mat.

13. A composite material according to any one of the preceding claims, wherein at least one layer of recycled polymer material is sandwiched between a first section or block comprising a plurality of layers of the waste glass fiber mat and a second section or block comprising a plurality of layers of the waste glass fiber mat.

14. A composite material according to any one of the preceding claims, wherein the composite material comprises the waste glass fiber mat in an amount between about 5% and about 50% by volume, between about 15% and 40% by volume, or between about 20% and 35% by volume, based on the total volume of composite material.

15. A composite material according to any one of the preceding claims, wherein the glass fiber fraction is between about 5% and about 70%, between about 10% and about 60%, or between about 15% and 50% by weight, based on the total weight of the composite material.

16. A composite material according to any one of the preceding claims, wherein a void content in the composite material is less than about 20%, or less than about 15% based on the total volume of the composite material.

17. A composite material according to any one of the preceding claims, wherein a void content in the composite material is between about 1 % and about 20%, between about 5% and about 15%, or between about 7% and about 13% based on the total volume of the composite material.

18. A composite material according to any one of the preceding claims, wherein the waste glass fiber mat comprises between about 5% and about 50%, between about 10% and about 30%, or between about 15% and about 25% by weight of a binder based on the total weight of the waste glass fiber mat, optionally wherein the binder is selected from acrylic and / or melamine formaldehyde and / or urea formaldehyde containing binder compositions.

19. A composite material according to any one of the preceding claims, wherein the at least one layer of the recycled polymer material has a thickness between about 0.1 mm and about 20mm, or between about 0.25 mm and 1 ,5mm.

20. A composite material according to any one of the preceding claims, wherein the at least one layer of waste glass fiber mat has a mean area weight of between 30 g / m2up to 300 g / m2and a corresponding thickness between about 0.1 mm and about 3mm, preferably about 0.3mm and about 1mm, such as between about 0.4mm and about 1 mm.21 . A composite material according to any one of the preceding claims, wherein the density of the composite material is at least about 0.25 g / cm3, at least about 0.50 g / cm3-,at least about 0.75 g / cm3, or at least about 1 .0 g / cm3or between about 0.50g / cm3and about 2.0 g / cm3, such as between about 1 .0 g / cm3and 1 .5 g / cm3.

22. A composite material according to any one of the preceding claims, wherein the tensile strength is at least about 5 MPa, at least 10 MPa, at least about 15 MPa, at least about 20 MPa, at least about 30 MPa, or between about 25 MPa and about 50 MPa.

23. A composite material according to any one of the preceding claims, wherein the flexural modulus is at least 0.5 GPa, at least about 1 GPa, at least about 3 GPa, at least about 5 GPa, or between about 0.5 GPa and 20 GPa, such as between about 1 GPa and 10 GPa.

24. A composite material according to any one of the preceding claims, comprising one or more (or all) of the following:(i) a tensile modulus of at least about 1 GPa, at least about 1.5 GPa, at least about 2 GPa, between about 1 GPa and about 10 GPa, between about 1 GPa and about 8 GPa, or between about 1 GPa and about 4 GPa;(ii) a flexural strength of at least about 10 MPa, at least about 20 MPa, or at least about 30 MPa;(iii) a compressive strength of at least about 10 MPa, at least about 15 MPa, at least about 20 MPa, at least about 25 MPa, or between about 10 MPa and 40 MPa; and / or(iv) a compressive modulus of at least about 1 GPa, at least about 1.5 GPa, at least about 2.0 GPa, between about 1 GPa and 7 GPa, or between about 1.5 GPa and 6 GPa.

25. A composite material according to any one of the preceding claims, wherein the recycled polymer material is present in an amount between about 10% and about 90%, between about 20% and about 80%, preferably between about 25% and about 80%, or between about 50% and about 75% by weight based on the total weight of the composite.

26. A composite material according to any one of the preceding claims, wherein the composite material comprises at least about 15% by volume of the glass fiber, based on the total volume of the composite material, and a tensile modulus of at least about 2 GPa or at least about 3 GPa.

27. A composite laminate according to any one of the preceding claims, comprising one or more, or all, of the following properties:(i) between about 20% and about 35% by volume of glass fibers based on the total volume of the composite material;(ii) a void between about 5% and about 15%, or between about 7% and about 13% based on the total volume of the composite material; and(ii) a density between about 1.0 g / cm3and 1.5 g / cm3.

28. A method for making a composite material comprising:(a) laminating at least one layer of a recycled polymer material to at least one layer of waste glass fiber mat; wherein the recycled polymer material has a density lower than about 1 g / cm3.

29. The method according to claim 28, wherein:(i) the recycled polymer material is a mixed waste polymer material;30. The method according to claim 28 or 29, further comprising: contacting waste polymer material with water; and then separating the polymer material that floats; wherein the separated polymer material is the recycled polymer material.31 . The method of any one of claims 28 to 30, further comprising:(a) shredding a recycled polymer material to provide a shredded recycled polymer material; and(b) pressing the shredded recycled polymer material to provide a sheet or film of recycled polymer material; wherein the sheet or film of mixed polymer material provides the at least one layer of recycled polymer material.

32. The method of any one of claims 28 to 31 , further comprising:(a) providing a layer of waste glass fiber mat; and(b) coating the layer of waste glass fiber mat with a layer of mixed waste polymer material to provide a layer of waste glass fiber mat coated with the mixed waste polymer material.

33. The method of any one of claims 28 to 32, wherein the composite laminate comprises a plurality of layers of the recycled polymer material and / or a plurality of layers of the waste glass fiber mat, the method further comprising:(a) stacking the plurality of layers of recycled polymer material and the plurality of layers of waste glass fiber mat in a desired arrangement or lay-up; and(b) laminating the layers together.

34. The method of any one of claims 28 to 33, further comprising: sandwiching at least one layer of recycled polymer material between a first and second layer of waste glass fiber mat and laminating the layers together.

35. The method of any one of claims 28 to 34, further comprising:(a) preparing one or more construct(s) prior to the lamination step, each construct comprising a layer of waste glass fiber mat bonded to a layer of recycled polymer material; and(b) laminating the one or more constructs to one or more additional layers of waste glass fiber mats to provide the composite material.

36. The method of any one of claims 28 to 35, wherein the laminating step comprises bonding the layers together by applying a temperature in between 150 °C and 200 °C and pressure in between 10 bar and 30 bar such that the recycled polymer material melts and binds to the at least one layers or plurality of layers of waste glass fiber mat, bonding the layers together.

37. The method of any one of claims 28 to 36, wherein the composite material is as defined in any one of claims 1 to 27.

38. Use of a composite material as defined in any one of claims 1 to 27, or made in accordance with the method of any one of claims 28 to 37, in the construction sector, in the transport sector, in the sports sector, and / or in the agricultural sector.

Citation Information

Patent Citations

  • Fiber-reinforced recycled thermoplastic composite and method

    US20010018118A1

  • Multilayer laminate for the manufacturing of insulating panels

    US20150292199A1

  • Structurally-reinforced plastic composite products produced with recycled waste glass fibers and recycled polymer compounds and process for making the same