Semiconductor device and method for manufacturing semiconductor device

The semiconductor device manufacturing method simplifies the copper via filling process by using electroless gold plating and subsequent copper, silver, nickel, or tin plating to achieve effective electrical connections and heat dissipation, addressing the cost and complexity issues of existing technologies.

WO2024247025A1PCT designated stage expired Publication Date: 2024-12-05MITSUBISHI ELECTRIC CORP

Patent Information

Application Number
PCT/JP2023/019866
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-29
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

The high cost and complexity of copper via filling in semiconductor devices due to the need for precise control of the plating process and the use of conductive metal nitrides for diffusion barriers, which are difficult to handle and costly, hinder the achievement of good electrical connections and heat dissipation.

Method used

A semiconductor device manufacturing method involving the formation of a gold coating layer on the via inner wall using electroless plating, followed by a second plating layer of copper, silver, nickel, or tin with larger crystal grains, eliminating the need for conductive metal nitrides and simplifying the process, thereby achieving good electrical connections and heat dissipation at a lower cost.

Benefits of technology

This method enables effective electrical connections and heat dissipation in the thickness direction without the risks of copper contamination, reducing equipment investment and costs while improving high-frequency characteristics and heat dissipation efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2023019866_05122024_PF_FP_ABST
    Figure JP2023019866_05122024_PF_FP_ABST
Patent Text Reader

Abstract

A semiconductor device (10) according to the present application is configured to comprise a substrate (1) of a semiconductor material, a surface electrode (3) formed on one surface of the substrate (1), and a solid via (10v) including: a covering layer (42) formed from gold, which covers the inner wall of a tubular hole opening on the other surface of the substrate (1) and having the surface electrode (3) as the bottom surface thereof, and in which is formed a depression (42d) depressed from the opening side toward the bottom surface; and a filler layer (43) filling the depression (42d) and formed from any of copper, silver, nickel, tin, and gold with a larger crystal grain size than the covering layer (42).
Need to check novelty before this filing date? Find Prior Art

Description

Semiconductor device and method for manufacturing the same

[0001] The present application relates to a semiconductor device and a method for manufacturing the semiconductor device.

[0002] In semiconductor devices having electrodes (vias) that penetrate the front and back surfaces of a semiconductor substrate, filling the vias with copper (Cu) plating, which is usually called Cu via filling, is expected to improve electrical connection, high-frequency characteristics, and heat dissipation.

[0003] Via filling with copper plating is performed by electrolytic plating, which requires precise control of the plating solution composition, applied voltage waveform, solution agitation, etc. (See, for example, Patent Document 1.) Furthermore, because there is concern that the electrical characteristics may deteriorate due to the diffusion of copper into the semiconductor, it is necessary to form a diffusion barrier layer on the inner wall of the via (See, for example, Patent Document 2.).

[0004] JP 2014-095104 A (paragraphs 0042 to 0050, Table 1) JP 2013-532903 A (paragraph 0039, Figure 13)

[0005] However, Cu via filling by electrolytic plating requires precise control of the plating process (composition of plating solution, applied voltage waveform, agitation of the solution), which poses problems of excessive equipment investment, increased costs for process management, etc. Furthermore, the diffusion barrier layer requires a material such as a conductive metal nitride, which has a complicated formation process and is difficult to handle, which also poses problems of excessive equipment investment, increased costs for process management, etc.

[0006] The present application discloses a technique for solving the above-mentioned problems, and aims to obtain a semiconductor device having good electrical connection and heat dissipation properties in the thickness direction at low cost.

[0007] The semiconductor device disclosed in the present application is characterized by comprising a substrate made of a semiconductor material, a solid via having an opening on the other side of the substrate, a first plating layer made of gold covering the inner wall of a cylindrical hole having the wiring member as its bottom surface and having a recess recessed from the opening side toward the bottom surface, and a second plating layer made of copper, silver, nickel, tin, or gold having a crystal grain size larger than that of the first plating layer and filling the recess.

[0008] The method for manufacturing a semiconductor device disclosed in the present application is characterized by including the steps of forming a wiring member on one side of a substrate made of a semiconductor material, forming a cylindrical hole on the other side of the substrate that opens and has the wiring member as its bottom, forming a first plating layer of gold by electroless plating so as to cover the inner wall of the cylindrical hole and form a recess that is recessed from the opening side toward the bottom, and forming a second plating layer of copper, silver, nickel, tin, or gold by electrolytic plating so as to fill the recess.

[0009] According to the semiconductor device or semiconductor device manufacturing method disclosed in the present application, a gold coating layer is formed on the inner wall of the via in a simple process without requiring excessively large equipment, so that a semiconductor device having good electrical connection and heat dissipation properties in the thickness direction can be obtained at low cost.

[0010] 1 is an end view illustrating a configuration of a via in a semiconductor device according to a first embodiment; FIG. 2 is an end view illustrating a configuration of a semiconductor device according to the first embodiment; FIG. 3 is an end view illustrating a configuration of a via of a semiconductor device according to the first embodiment; FIG. 4 is an end view illustrating a configuration of a coating layer of a via in a semiconductor device according to the first embodiment during a via filling step; FIG. 5 is a diagram illustrating a cross-sectional SEM image during a via filling step in a semiconductor device according to the first embodiment; FIG. 6 is a schematic end view illustrating a state at each stage during coating layer formation in via filling of a semiconductor device according to the first embodiment; FIG. 7 is an end view illustrating a configuration of a via in a semiconductor device according to a modification of the first embodiment; FIG. 8 is an end view illustrating a configuration of a via in a semiconductor device according to a comparative example; FIG. 9 is a diagram illustrating a cross-sectional SEM image during a via filling step in a semiconductor device according to the comparative example; FIG. 10 is an end view illustrating a configuration before a filling layer is formed in via filling of a semiconductor device according to a second embodiment; FIG. 11 is a flowchart illustrating a manufacturing method of a semiconductor device according to the second embodiment; FIG. 12 is an end view illustrating a configuration of a via in a semiconductor device according to the second embodiment; FIG. 10 is an end view for explaining the configuration of a via in a semiconductor device according to a modified example of embodiment 4. FIG. 11 is an end view for explaining the configuration of a via in a semiconductor device according to embodiment 5. FIG. 12 is an end view for explaining the configuration of a via in a semiconductor device according to a modified example of embodiment 5. FIG. 13 is an end view for explaining the configuration of a via in a semiconductor device according to embodiment 6. FIG. 14 is an end view for explaining the configuration of a via in a semiconductor device according to a modified example of embodiment 6. FIG. 15 is an end view for explaining the configuration of a via in a semiconductor device according to embodiment 7. FIG. 16 is an end view for explaining the configuration of a via in a semiconductor device according to a modified example of embodiment 7.

[0011] 1 to 9 are diagrams for explaining a semiconductor device according to a first embodiment and a method for manufacturing the semiconductor device. FIG. 1 is an end view corresponding to line A-A in FIG. 2 (described later) for explaining the configuration of the via of the semiconductor device, and FIG. 2 is an end view for explaining the configuration of the semiconductor device. FIG. 3 is a flowchart for explaining the manufacturing method of the semiconductor device. FIG. 4 is an end view corresponding to FIG. 1 during the via filling process for explaining the configuration of the coating layer of the via of the semiconductor device, showing the formation of a coating layer and before the formation of a filling layer, and FIG. 5 is a cross-sectional SEM image of a stage in the via filling process in which a coating layer similar to FIG. 4 has been formed. FIG. 6 is a schematic end view showing the state at each stage during the formation of the coating layer in via filling of the semiconductor device according to the first embodiment.

[0012] 7 is an end view corresponding to FIG. 4 at a stage where a covering layer is formed to explain the configuration of the via of the semiconductor device according to the modified example, while FIG. 8 is an end view at a stage where a covering layer is formed to explain the configuration of the via of the semiconductor device according to the comparative example, and FIG. 9 is a cross-sectional SEM image at a stage where a covering layer similar to FIG. 8 is formed in the via filling process.

[0013] The semiconductor device 10 according to the first embodiment is assumed to be, for example, a semiconductor device called a high electron mobility transistor (HEMT). As shown in FIGS. 1 and 2, a case will be described in which a via 10v is formed from the back surface directly below a source electrode 3s on the front surface (the upper surface in the figure). Note that the via 10v shown in FIG. 1 is a detailed view of the via 10v formed directly below the source electrode 3s in FIG. 2, but the via 10v does not necessarily have to be directly below the source electrode 3s, and may be located directly below a conductor layer (wiring member) formed on the front surface, including a wiring pattern.

[0014] In the semiconductor device 10, an epitaxial growth layer 2 is formed on a silicon carbide (SiC) substrate 1, and a source electrode 3s, a drain electrode 3d, and a gate electrode 3g (collectively, surface electrodes 3) are formed on the epitaxial growth layer 2. The via 10v is formed directly below the source electrode 3s, with the source electrode 3s serving as an etching stop layer. A metal layer is formed along the inner wall of the via 10v, and this metal layer serves as a seed layer 41. A covering layer 42 and a filling layer 43 are then formed in this order to form a filling body 4, thereby achieving via filling.

[0015] In the first and subsequent embodiments, a gallium nitride (GaN) HEMT on a silicon carbide substrate 1 will be described as an example, but the present invention is not limited to this. For example, similar effects can be obtained with other semiconductor substrates, such as compound semiconductors such as indium phosphide (InP), gallium nitride, and germanium silicide (SiGe), and silicon (Si)-based semiconductors. This is because gold (Au), which constitutes the coating layer 42 of the via 10v, is formed on the seed layer 41, regardless of the element type of the substrate 1.

[0016] Next, the details of the configuration of the semiconductor device 10 according to the first embodiment will be described together with the manufacturing method with reference to the flowchart in Figure 3. First, epitaxial growth, metal film formation, insulating film formation, and transfer patterning are repeatedly performed in a wafer process on the surface side (upper surface in Figures 1 and 2) of a substrate 1 made of SiC single crystal, to form an electrical circuit on the surface (step S100). The wafer process is performed on a disk-shaped substrate having a diameter of 4 to 8 inches and a thickness of 0.35 mm or 0.5 mm.

[0017] First, an epitaxially grown layer 2 is formed on a substrate 1. In the case of a gallium nitride HEMT, a laminated structure is generally formed in which an aluminum gallium nitride (AlGaN) layer is layered on a gallium nitride layer. Next, a source electrode 3s, a drain electrode 3d, and a gate electrode 3g are formed. For the source electrode 3s and the drain electrode 3d, a laminated structure such as titanium / aluminum / gold (Ti / Al / Au) or titanium / aluminum / nickel / gold (Ti / Al / Ni / Au) is used. For the gate electrode 3g, a laminated structure such as titanium / platinum / gold (Ti / Pt / Au) is used.

[0018] Thereafter, the source electrode 3s, the drain electrode 3d, and the gate electrode 3g are protected with an insulating film 9 made of, for example, silicon nitride (SiN). Note that after the source electrode 3s and the drain electrode 3d are formed and protected with the insulating film 9, only the gate electrode 3g portion may be opened by dry etching to form the gate electrode 3g, and the entire structure may again be protected with the insulating film 9. After this, wiring electrodes may be further attached. For the wiring electrodes, electrolytic gold plating or the like is used.

[0019] Once the wafer processing on the front surface is complete, the back surface (the lower surface in Figures 1 and 2) is processed by attaching the front surface of the wafer to a support substrate using a wax material. At this time, a tape material may be used instead of the wax material. The thickness of the wax material is, for example, 20 μm. The back surface of the wafer is ground and polished while still attached to the support substrate. For example, the substrate thickness is thinned to 50 μm. By thinning the substrate, the heat dissipation and high-frequency characteristics of the device are improved.

[0020] Next, the via processing process (steps S200 to S230) is performed. To form the via 10v, which is an electrode that penetrates the substrate 1, a resist material is applied using a spin coater, and then the resist is removed only from the processed area using transfer and development patterning. For example, the substrate is etched using ICP (Inductively Coupled Plasma) dry etching to form a through hole for the via 10v (step S200).

[0021] Once the through holes are formed, the applied resist material is removed by immersion in a stripping solution. This results in a semiconductor back surface with the inner surfaces of the through holes, which will become the vias 10v in the substrate 1, exposed. Smaller vias 10v are advantageous because they allow greater layout freedom, but if they are too small, the etching process for forming the through holes will not proceed and they will not be able to penetrate the substrate 1. For example, they are formed in a cylindrical shape with a diameter of 50 μm. Here, the aspect ratio (via depth / via diameter) of the vias 10v (through holes) is 1, but this varies depending on the substrate thickness and via shape, and can range from 1 to 5.

[0022] A seed layer 41 is formed to cover the inner wall of the formed through hole (step S210). The seed layer 41 is formed, for example, by stacking a 200 nm thick gold layer on a 50 nm thick titanium layer in contact with the substrate 1. The titanium layer is a film inserted to improve adhesion between the gold layer, which is the main component of the seed layer 41, and the substrate 1. Titanium nitride, tantalum (Ta), tungsten (W), chromium (Cr), etc. may be used instead of titanium. A platinum layer may also be inserted between the titanium layer and the gold layer. In this case, for example, the titanium layer may be 50 nm thick, the platinum layer may be 50 nm thick, and the gold layer may be 200 nm thick. An insulating film layer may also be inserted between the substrate 1 and the seed layer 41.

[0023] In order to promote the deposition reaction of electroless gold plating in the next step of forming the coating layer 42, it is necessary to cover the deposition surface of the seed layer 41 with a catalytic metal. The electroless plating reaction begins when the surface of the seed layer 41 is a gold layer. Other than gold, silver (Ag), copper (Cu), palladium (Pd), platinum, nickel, ruthenium (Ru), tin (Sn), etc. may also be used.

[0024] On the other hand, for metal surfaces with weak catalytic activity, the electroless plating reaction can be initiated by adding a step of immersing the surface in a pretreatment solution containing catalytic metal ions as a pretreatment for electroless plating. Once the plating reaction begins, the gold, which is the deposited metal, itself acts as a catalyst, so the reaction continues and a gold plating film can be obtained (autocatalytic electroless plating).

[0025] Since the seed layer 41 is interposed between the substrate 1 and the gold coating layer 42, it does not need to function as a barrier layer to prevent copper diffusion, as was feared in Patent Document 2. Therefore, there is no need to use materials that are difficult to handle and require complicated formation processes, such as conductive metal nitrides such as titanium nitride (TiN), tantalum nitride (TaN), tungsten nitride (WN), and titanium aluminum nitride (TiAlN).

[0026] After the seed layer 41 is formed, as shown in FIG. 4 , electroless gold plating is used to form a gold coating layer 42 having a recess 42d opening on the backside (step S220). The figure shows an example in which a conical recess 42d is formed, with a V-shaped cross section passing through the axial center of the through hole. The formation of the conical recess 42d can be achieved by adjusting the additive content of the electroless gold plating solution within an appropriate range. This additive suppresses plating deposition on the opening side (lower side in the figure) and preferentially deposits gold from the bottom surface (upper side in the figure) and inner peripheral surface of the seed layer 41.

[0027] As shown in the cross-sectional SEM (Scanning Electron Microscope) image of FIG. 5 , the above-described method successfully formed the covering layer 42 so as to have a conical recess 42d. Here, the thickness t42 (see FIG. 4 ) from the via bottom to the apex of the cone (bottom 42b of recess 42d) is preferably at least ¼ of the via height Hv. In other words, the depth Dd of recess 42d is preferably less than 4 / 3 of the via height Hv. This allows the via filling shape to be achieved without voids when forming the filling layer 43 by electroplating.

[0028] In FIG. 4 , the via height Hv is depicted as the dimension obtained by subtracting the thickness of the seed layer 41 from the thickness of the substrate 1 including the epitaxial growth layer 2. However, the thickness of the seed layer 41 is negligibly thin compared to the thickness of the substrate 1. Therefore, the sum of the thickness of the substrate 1 and the thickness of the epitaxial growth layer 2 is defined as the above-mentioned via height Hv. Meanwhile, the thickness t42 is preferably equal to or less than half the via height Hv. If the thickness t42 is greater than half the via height Hv, the amount of additive in the plating solution will be reduced, increasing the risk of the via opening becoming clogged, as shown in FIG. 9 . Furthermore, the lack of additive will result in the coating layer 42 on the backside of the wafer becoming too thick.

[0029] As mentioned above, the vertical growth of the plating can be suppressed by the additive. Therefore, as shown in Figure 6, once the plating grows through stages 1, 2, and 3 to a thickness t42 determined by the amount of additive, the gold plating does not grow even if the wafer is subsequently immersed in an electroless plating solution for, for example, two hours (from stage 3 to stage 4). Therefore, a coating layer 42 having recesses 42d with the same uniform thickness t42 can be formed in each of the multiple through holes within the substrate surface.

[0030] After the coating layer 42 is formed, the recess 42d shown in FIG. 1 is filled by electroplating to form a gold filling layer 43 with a larger crystal grain size than the coating layer 42 formed by electroless plating (step S230). This results in a solid via 10v in which the through-hole is filled with gold. To efficiently supply gold ions into the recess 42d, a pulse voltage may be applied. A depression may occur in the opening end of the via 10v (the lower surface in the figure), i.e., the filling layer 43, reflecting the recess 42d in the coating layer 42, but the presence or absence of this depression and its shape are not important.

[0031] The via 10v is completely filled with the filling layer 43 formed by electroplating, improving high-frequency characteristics and heat dissipation. If the gold film thickness on the back surface (bottom in the figure) of the wafer becomes too thick due to the complete filling of the via 10v, etching may be performed until the desired film thickness is reached. For example, argon (Ar) ion milling is used for dry etching, and for example, iodine (I)-based wet etching is used for wet etching.

[0032] Finally, the support substrate is peeled off from the wafer. The support substrate and wafer are heated to 100°C on a hot plate for at least one minute to melt the wax, and then the wafer is slid parallel to the wafer surface to peel them off. The wafer is then immersed in acetone heated to 50°C for 10 minutes to remove the wax from the surface (step S300). The higher the temperature and the longer the immersion time, the better the removability.

[0033] Modifications The recesses 42d of the coating layer 42 do not necessarily have to have a V-shaped (conical) cross-sectional shape as shown in Fig. 4, but may have a curved recessed shape as shown in the modification of Fig. 7. It is sufficient that the opening width Wd of the recesses 42d of the coating layer 42 decreases toward the bottom 42b, and the bottom 42b does not have to be pointed.

[0034] Comparative Example. In contrast, as shown in the comparative example in FIG. 8, the opening width Wd of the recess 42dC in the coating layer 42C must not be an overhanging shape with a portion that increases toward the bottom 42bC. If electroplating to form the filling layer 43C is performed in this state, the opening of the recess 42dC will be blocked, creating a void inside the via. If no additive is used, as shown in FIG. 9, the recess 42dC will have an overhanging shape, causing the via opening to be blocked first, resulting in a void 4v. Note that parts in the comparative example (FIGS. 8 and 9) that correspond to the embodiment are distinguished by adding a "C" to the end of their reference numerals.

[0035] In other words, by forming a coating layer 42 having a recess 42d that narrows toward the bottom 42b using electroless plating, the inside of the via 10v can be completely filled without any voids, together with a gold filling layer 43 formed by electrolytic plating and having a larger crystal grain size than the coating layer 42.

[0036] As a result, the inductance component of the via 10v is reduced, improving high-frequency characteristics. Furthermore, an improvement in heat dissipation of approximately 10% is expected compared to a hollow via structure (R. Baskaran, Allen W. Hanson, CS MANTECH Conference (USA), May 18-21, 2015, "Simulation of the Impact of Through-Substrate Vias on the Thermal Resistance of Compound Semiconductor Devices"). Furthermore, because the coating layer 42 is made of gold, there is no concern about a decrease in electrical reliability due to copper contamination.

[0037] Second Embodiment In the first embodiment, an example in which a portion covered with a coating layer remains on the rear surface of the wafer has been described. In the second embodiment, an example in which the coating layer is removed from the rear surface of the wafer will be described.

[0038] 10 to 12 are diagrams for explaining a semiconductor device according to a second embodiment and a method for manufacturing the semiconductor device, and Fig. 10 is a flowchart for explaining the method for manufacturing the semiconductor device. Fig. 11 is an end view corresponding to Fig. 3 used in explaining the first embodiment, for explaining the configuration of the semiconductor device after the formation of a covering layer and before the formation of a filling layer in via filling, and Fig. 12 is an end view corresponding to Fig. 1 used in explaining the first embodiment, for explaining the configuration of the via. Note that the same reference numerals are used for the same parts as in the first embodiment, and explanations of the same parts are omitted, and Figs. 2 and 4 used in the first embodiment are used.

[0039] The configuration of the semiconductor device 10 according to the second embodiment will be described together with the manufacturing process. As shown in the flowchart of FIG. 10 , the process up to the formation of the seed layer 41 is the same as that of the first embodiment. The formation of the coating layer 42 (step S220V) is also the same as that of the first embodiment, up to the formation of the gold coating layer 42 having the recess 42d opening on the back surface side and covering the back surface of the wafer, as described in FIG. 4 of the first embodiment. However, the process of forming the coating layer 42 (step S220V) according to the second embodiment adds a step of adjusting the coverage by etching away the layer of the coating layer 42 and the seed layer 41 that is deposited on the front surface (back surface of the wafer), as shown in FIG. 11 .

[0040] Etching can be performed using either dry etching or wet etching. For dry etching, argon ion milling, for example, is used. Dry etching can be used to etch titanium, gold, and platinum all at once. For wet etching, the chemical solution used varies depending on the layer to be removed. For gold, for example, an iodine-based chemical solution is used, and for titanium, buffered hydrofluoric acid (BHF) or a mixture of ammonia (NH3) and hydrogen peroxide (H2O2) is used.

[0041] Note that the seed layer 41 does not necessarily have to be etched. For example, by etching only the gold with an iodine-based chemical, the flat portion on the back surface of the wafer can have the surface of the gold base (titanium and platinum in this example) of the seed layer 41. Because a thicker layer of gold is deposited inside the through holes than on the flat portion, the surface is mainly gold.

[0042] 12, a metal film 44 is formed on the coating layer 42 and the rear surface of the wafer by sputtering (step S225), as shown in FIG. 12. For example, a titanium layer with a thickness of 50 nm and a gold layer with a thickness of 200 nm are used.

[0043] Thereafter, as in the first embodiment, a filling layer 43 is formed by electrolytic gold plating to fill the recess 42d (step S230). If the filling layer 43 becomes too thick, etching may be performed until the desired thickness is reached. For example, argon ion milling is used for dry etching, and for example, iodine-based wet etching is used for wet etching.

[0044] In the electroless gold plating used to form the coating layer 42, if the film thickness on the flat part of the back surface of the wafer becomes as thick as, for example, about 5 μm, the internal stress of the plating film becomes high, causing wafer warpage and chip warpage, which can lead to cracks, abnormalities in thermal resistance characteristics, and deterioration of handleability.

[0045] In contrast, in the semiconductor device 10 or semiconductor device manufacturing method according to the second embodiment, the plating film on the flat portion of the wafer back surface is etched back to reduce the gold thickness on the flat portion, thereby resolving the above-mentioned problem. However, when etched back, the gold on the flat portion is removed, which increases the electrical resistance of the flat portion and interferes with power supply in the subsequent electroplating process. Therefore, by forming the metal film 44 by sputtering or vapor deposition, similar to the reconstitution of the seed layer 41, the uniformity of the film and the filling characteristics within the via 10v can be ensured during electroplating in the process of forming the filling layer 43 (step S230).

[0046] In other words, by removing the portion of the coating layer 42 that covers the flat portion on the back surface of the wafer, wafer warpage is reduced, and wafer and chip cracks can be suppressed. Furthermore, the plating thickness of the flat portion is made more uniform across the wafer, which contributes to uniform chip characteristics and higher yields.

[0047] Embodiment 3. In the above-mentioned embodiments 1 and 2, examples were described in which the filling layer was made of the same gold as the coating layer, although the manufacturing methods and crystal grain sizes were different. In this embodiment 3, an example in which the filling layer is made of copper will be described.

[0048] 13 and 14 are intended to explain a semiconductor device according to a third embodiment and a method for manufacturing the semiconductor device, with Fig. 13 being an end view corresponding to Fig. 1 used to explain the first embodiment and intended to explain the via configuration of the semiconductor device, and Fig. 14 being an end view corresponding to Fig. 13 and intended to explain the via configuration of a semiconductor device according to a modified example. Note that the same reference numerals are used to designate the same parts as in the first embodiment, and explanations of the same parts will be omitted, with Figs. 2 to 4 used in the first embodiment being used.

[0049] In the third embodiment, the configuration of the covering layer 42 and the manufacturing method thereof (up to step S220) are the same as those in the first embodiment. However, in the first embodiment, the step of forming the filling layer 53 is performed by electrolytic plating, but by electrolytic plating of copper (electrolytic copper plating), to form the copper filling layer 53 as shown in FIG.

[0050] Modifications It is also possible to perform CMP (Chemical Mechanical Polishing) from the state of FIG. 13 where the filling layer 53 has been formed, to completely flatten the flat portion of the rear surface of the wafer, as shown in FIG.

[0051] As in the first embodiment, by forming a coating layer 42 having a recess 42d that tapers toward the bottom 42b by electroless plating, the interior of the via 10v can be completely filled without any voids together with the copper filling layer 53 formed by electrolytic plating. Furthermore, in the third embodiment, since the filling layer 53 is made of copper, CMP polishing can be performed without using special chemicals, making it easy to flatten the surface. Furthermore, in electrolytic plating, additives that are more effective for via filling have been developed for copper plating than for gold plating, making it easier to fill the recess 42d.

[0052] In other words, in the semiconductor device 10 or the method for manufacturing a semiconductor device according to the third embodiment, the inductor component of the via 10v is reduced, and high-frequency characteristics are improved. Compared to when the filler 4 is made entirely of copper, the gold coating layer 42 acts as a copper diffusion barrier in addition to the conductive nitride film disclosed in Patent Document 2, thereby improving the reliability of the device.

[0053] Furthermore, copper has better electrical and thermal conductivity than gold, which improves the device characteristics (electrical characteristics, high frequency characteristics, thermal characteristics) compared to when the filler 4 is made of gold alone. Furthermore, because the back surface of the wafer can be easily planarized, three-dimensional device design is possible in which the next layer is stacked on top of the planarized layer.

[0054] Embodiment 4 In the above-described embodiment 3, an example was described in which the filling layer in the semiconductor device of embodiment 1 is made of copper. In embodiment 4, an example will be described in which the filling layer in the semiconductor device of embodiment 2 is made of copper.

[0055] 15 and 16 are intended to explain a semiconductor device according to a fourth embodiment and a method for manufacturing the semiconductor device, with Fig. 15 being an end view corresponding to Fig. 12 used to explain the second embodiment and intended to explain the via configuration of the semiconductor device, and Fig. 16 being an end view corresponding to Fig. 15 and intended to explain the via configuration of a semiconductor device according to a modified example. Note that the same reference numerals are used to designate the same parts as those in the first and second embodiments, and explanations of the same parts will be omitted, with Figs. 2 and 4 used in the first embodiment and Figs. 10 and 11 used in the second embodiment being used.

[0056] In the fourth embodiment, the configuration of the covering layer 42 and the manufacturing method thereof (up to step S225) are the same as those in the second embodiment. However, in the fourth embodiment, the step of forming the filling layer 53 is performed by electrolytic plating, but by electrolytic plating of copper (electrolytic copper plating), to form the copper filling layer 53 as shown in FIG.

[0057] Modifications It is also possible to perform CMP polishing from the state of FIG. 15 after the filling layer 53 has been formed, so as to completely flatten the flat portion of the rear surface of the wafer, as shown in FIG.

[0058] As in the second embodiment, by forming a coating layer 42 having a recess 42d that tapers toward the bottom 42b by electroless plating, the interior of the via 10v can be completely filled without any voids together with the copper filling layer 53 formed by electrolytic plating. Furthermore, in the fourth embodiment, since the filling layer 53 is made of copper, CMP polishing can be performed without using special chemicals, making it easy to flatten the surface. Furthermore, in electrolytic plating, additives that are more effective for via filling have been developed for copper plating than for gold plating, making it easier to fill the recess 42d.

[0059] In other words, in the semiconductor device 10 or the method for manufacturing a semiconductor device according to the fourth embodiment, the inductance component of the via 10v is reduced, and high-frequency characteristics are improved. Compared to when the filler 4 is made entirely of copper, the gold coating layer 42 acts as a copper diffusion barrier in addition to the conductive nitride film, thereby improving the reliability of the device.

[0060] Furthermore, copper has better electrical and thermal conductivity than gold, which improves the device characteristics (electrical characteristics, high frequency characteristics, thermal characteristics) compared to when the filler 4 is made of gold alone. Furthermore, because the back surface of the wafer can be easily planarized, three-dimensional device design is possible in which the next layer is stacked on top of the planarized layer.

[0061] Embodiment 5 In the above-described embodiments 3 and 4, examples were described in which the composition of the filling layer was changed from gold to copper in comparison with embodiments 1 and 2. In this embodiment 5, an example will be described in which the composition of the filling layer is changed from gold to silver.

[0062] 17 and 18 are intended to explain a semiconductor device according to a fifth embodiment and a method for manufacturing the semiconductor device, with Fig. 17 being an end view corresponding to Fig. 1 used to explain the first embodiment and illustrating the via configuration of the semiconductor device, and Fig. 18 being an end view corresponding to Fig. 12 used to explain the second embodiment and illustrating the via configuration of a semiconductor device according to a modified example. Note that the same reference numerals are used to designate the same parts as in the first and second embodiments, and descriptions of the same parts will be omitted, and Figs. 2 to 4 used in the first embodiment and Figs. 10 and 11 used in the second embodiment will be used.

[0063] In the fifth embodiment, the configuration of the covering layer 42 and the manufacturing method thereof (up to step S220) are the same as those in the first embodiment. However, in the fifth embodiment, the step of forming the filling layer 63 is performed by electrolytic plating, but by electrolytic plating of silver (electrolytic silver plating), to form the silver filling layer 63 as shown in FIG.

[0064] In this modification, the configuration of the coating layer 42 and the manufacturing method thereof (up to step S225) are the same as those in the second embodiment. However, in this modification, the step of forming the filling layer 63 is performed by electrolytic plating, but by electrolytic plating of silver (electrolytic silver plating), to form the silver filling layer 63, as shown in FIG.

[0065] As in the first and second embodiments, by forming the covering layer 42 having the recess 42d tapering toward the bottom 42b by electroless plating, the inside of the via 10v can be completely filled without any voids together with the silver filling layer 63 formed by electrolytic plating. Furthermore, in the fifth embodiment, since the filling layer 63 is made of silver, there is no need to worry about copper contamination as in the first and second embodiments, and there is no concern about a decrease in electrical reliability.

[0066] Furthermore, since silver has better electrical and thermal conductivity than gold and copper, the inductor component of via 10v is lower than when filling body 4 is made of gold alone or when the filling layer is made of copper, and the device characteristics (electrical characteristics, high frequency characteristics, thermal characteristics) are improved.

[0067] Sixth Embodiment In the fifth embodiment described above, an example was described in which the composition of the filling layer was changed from gold to silver in comparison with the first and second embodiments. In the sixth embodiment, an example will be described in which the composition of the filling layer is changed from gold to nickel.

[0068] 19 and 20 are intended to explain a semiconductor device according to a sixth embodiment and a method for manufacturing the semiconductor device, with Fig. 19 being an end view corresponding to Fig. 1 used to explain the first embodiment and illustrating the via configuration of the semiconductor device, and Fig. 20 being an end view corresponding to Fig. 12 used to explain the second embodiment and illustrating the via configuration of a semiconductor device according to a modified example. Note that the same reference numerals are used to designate the same parts as in the first and second embodiments, and descriptions of the same parts will be omitted, and Figs. 2 to 4 used in the first embodiment and Figs. 10 and 11 used in the second embodiment will be used.

[0069] In the sixth embodiment, the configuration of the coating layer 42 and the manufacturing method thereof (up to step S220) are the same as those in the first embodiment. However, in the sixth embodiment, the step of forming the filling layer 73 is performed by electrolytic plating, but by electrolytic plating of nickel (Ni) (electrolytic nickel plating), to form the nickel filling layer 73 as shown in FIG.

[0070] In this modification, the configuration of the coating layer 42 and the manufacturing method thereof (up to step S225) are the same as those in the second embodiment. However, in this modification, the step of forming the filling layer 73 is performed by electrolytic plating, but by electrolytic plating of nickel (electrolytic nickel plating), to form the nickel filling layer 73, as shown in FIG.

[0071] As in the first and second embodiments, by forming a coating layer 42 having a recess 42d that tapers toward the bottom 42b by electroless plating, the inside of the via 10v can be completely filled with no voids, together with the silver filling layer 63 formed by electrolytic plating. Therefore, compared to a hollow via, improved heat dissipation and high-frequency characteristics due to suppression of inductor components are expected. Furthermore, in the sixth embodiment, the filling layer 73 is made of nickel, so there is no need to worry about copper contamination, as in the first and second embodiments, and there is no concern about a decrease in electrical reliability.

[0072] Furthermore, the backside of the high-frequency device is die-bonded using gold-tin (AuSn) solder, silver-tin (SnAg) solder, etc. However, when die-bonding is performed on a gold or copper surface using solder, a thick alloy layer is formed at the interface, resulting in poor conductivity, poor adhesion, and deterioration of thermal properties. However, in the sixth embodiment, the nickel that constitutes the filler layer 73 at the interface between the gold and the solder acts as a barrier layer, preventing these deteriorations in properties.

[0073] Embodiment 7 In the above-described embodiments 5 and 6, examples were described in which the composition of the filling layer was changed from gold to silver or nickel, as compared to embodiments 1 and 2. In this embodiment 7, an example will be described in which the composition of the filling layer is changed from gold to tin.

[0074] 21 and 22 are intended to explain a semiconductor device according to a seventh embodiment and a method for manufacturing the semiconductor device, with Fig. 21 being an end view corresponding to Fig. 1 used to explain the first embodiment and illustrating the via configuration of the semiconductor device, and Fig. 22 being an end view corresponding to Fig. 12 used to explain the second embodiment and illustrating the via configuration of a semiconductor device according to a modified example. Note that the same reference numerals are used to designate the same parts as those in the first and second embodiments, and descriptions of the same parts will be omitted, and Figs. 2 to 4 used in the first embodiment and Figs. 10 and 11 used in the second embodiment will be used.

[0075] In the seventh embodiment, the configuration of the coating layer 42 and the manufacturing method thereof (up to step S220) are the same as those in the first embodiment. However, in the seventh embodiment, the step of forming the filling layer 83 is performed by electrolytic plating, but by electrolytic plating of tin (electrolytic tin plating), to form the tin filling layer 83 as shown in FIG.

[0076] In this modification, the configuration of the coating layer 42 and the manufacturing method thereof (step S225) are the same as those in the second embodiment. However, in this modification, the step of forming the filling layer 83 is performed by electrolytic plating, but by electrolytic plating of tin (electrolytic tin plating), to form the tin filling layer 83, as shown in FIG.

[0077] As in the first and second embodiments, by forming a coating layer 42 having a recess 42d that tapers toward the bottom 42b by electroless plating, the interior of the via 10v can be completely filled without any voids with the tin filling layer 83 formed by electrolytic plating. Therefore, compared to a hollow via, improvements in heat dissipation and high-frequency characteristics due to suppression of inductor components are expected. Furthermore, in the seventh embodiment, since the filling layer 83 is made of tin, there is no need to worry about copper contamination, as in the first and second embodiments, and there is no concern about a decrease in electrical reliability.

[0078] Furthermore, the backside of the high-frequency device is die-bonded using gold-tin (AuSn) solder, silver-tin (SnAg) solder, etc., but this eliminates the need to apply solder. Furthermore, since the tin on the backside of the wafer is a component of the solder, the solder is essentially formed directly on the device, resulting in good adhesion.

[0079] Furthermore, although various exemplary embodiments and examples are described in this application, the various features, aspects, and functions described in one or more embodiments are not limited to the application of a particular embodiment, but may be applied to the embodiments alone or in various combinations. Therefore, countless modifications not illustrated are contemplated within the scope of the technology disclosed in this specification. For example, this includes cases where at least one component is modified, added, or omitted, and even cases where at least one component is extracted and combined with components of other embodiments.

[0080] As described above, the semiconductor device 10 of the present application includes a substrate 1 made of a semiconductor material, a wiring member formed on one surface (the upper surface in the figure) of the substrate 1, a first gold plating layer (coating layer 42) that covers the inner wall of a cylindrical hole that opens on the other surface of the substrate 1 and has the wiring member (surface electrode 3) as its bottom surface, and that has a recess 42d recessed from the opening side toward the bottom surface, and a solid via 10v that has a second plating layer (filling layer 43, 53, 63, 73, 83) that fills the recess 42d and is made of copper, silver, nickel, tin, or gold with a crystal grain size larger than that of the first plating layer (coating layer 42). This allows for a semiconductor device that is free from copper contamination and has good electrical connection and heat dissipation in the thickness direction via the via 10v to be obtained at low cost.

[0081] In particular, if the recess 42d is configured so as to widen from the bottom surface toward the opening, no voids will be generated, and a semiconductor device with excellent electrical conductivity and heat dissipation properties can be reliably obtained.

[0082] Furthermore, if the thickness t42 of the first plating layer (coating layer 42) to the bottom surface of the recess is set to at least 1 / 4 of the thickness of the substrate (via height Hv), the occurrence of voids can be more reliably prevented.

[0083] By having a metal film 44 containing any of titanium, tantalum, tungsten, chromium, and platinum interposed between the first plating layer (coating layer 42) and the second plating layer (filling layer 43, 53, 63, 73, 83), the plating film of filling layer 43 becomes uniform, and the embeddability within via 10v is further improved.

[0084] If the substrate 1 is made of any of silicon carbide, indium phosphide, gallium nitride, germanium silicide, germanium, and silicon, a semiconductor device with higher performance can be obtained.

[0085] As described above, the manufacturing method of semiconductor device 10 of the present application includes the steps of forming a wiring member on one surface of substrate 1 made of a semiconductor material, forming a cylindrical hole on the other surface of substrate 1 that opens and has the wiring member (surface electrode 3) as its bottom (steps S100-S200), forming a first gold plating layer (coating layer 42) by electroless plating to cover the inner wall of the cylindrical hole and form a recess 42d that recesses from the opening side toward the bottom (steps S220, S220V), and forming a second plating layer (filling layer 43) of copper, silver, nickel, tin, or gold by electrolytic plating to fill recess 42d (step S230). This allows for a semiconductor device that has good electrical connection and heat dissipation in the thickness direction via vias 10v to be obtained at low cost without worrying about copper contamination.

[0086] If the process includes a step (step S225) of forming a metal film 44 that covers the inner surface of the recess 42d by sputtering or vapor deposition, the plating film becomes uniform when forming the filling layer 43 by electroplating, and the embeddability within the via 10v is further improved.

[0087] 1: Substrate, 10: Semiconductor device, 10v: Via, 2: Epitaxial growth layer, 3: Surface electrode (wiring member), 4: Filler, 41: Seed layer, 42: Covering layer (first plating layer), 42d: Recess, 43: Filling layer (second plating layer), 44: Metal film, 53: Filling layer (second plating layer), 63: Filling layer (second plating layer), 73: Filling layer (second plating layer), 83: Filling layer (second plating layer), Dd: Depth, Hv: Via height, t42: Thickness, Wd: Opening width.

Claims

1. A semiconductor device comprising: a substrate made of a semiconductor material; a wiring member formed on one side of the substrate; and a solid via having an opening on the other side of the substrate, the wiring member forming a bottom of the cylindrical hole, a first plating layer of gold covering the inner wall of the hole and having a recess recessed from the opening side toward the bottom, and a second plating layer of copper, silver, nickel, tin, or gold having a larger crystal grain size than the first plating layer, filling the recess.

2. The semiconductor device according to claim 1, wherein the recess widens from the bottom surface toward the opening.

3. The semiconductor device according to claim 1 or 2, characterized in that the thickness of said first plating layer to the bottom surface of said recess is at least 1 / 4 of the thickness of said substrate.

4. A semiconductor device according to any one of claims 1 to 3, characterized in that it has a metal film containing any one of titanium, tantalum, tungsten, chromium, and platinum interposed between the first plating layer and the second plating layer.

5. The semiconductor device according to any one of claims 1 to 4, characterized in that the substrate is made of any one of silicon carbide, indium phosphide, gallium nitride, germanium silicide, germanium, and silicon.

6. A method for manufacturing a semiconductor device, comprising the steps of: forming a wiring member on one side of a substrate made of a semiconductor material, and forming a cylindrical hole that opens on the other side of the substrate and has the wiring member as a bottom surface; forming a first plating layer of gold by electroless plating so as to cover the inner wall of the cylindrical hole and to form a recess that is recessed from the opening side toward the bottom surface; and forming a second plating layer of copper, silver, nickel, tin or gold by electrolytic plating so as to fill the recess.

7. A method for manufacturing a semiconductor device according to claim 6, further comprising the step of forming a metal film by sputtering or vapor deposition to cover the inner surface of said recess.

Citation Information

Patent Citations

  • Semiconductor device and manufacture thereof

    JP1990214127A

  • Semiconductor device

    JP1993102200A

  • Method for manufacturing semiconductor element and semiconductor element

    JP2014112634A

  • Semiconductor device and method of manufacturing the same

    JP2022070436A

Cited By

  • Compound semiconductor back hole device, preparation method thereof and transistor

    CN121076034A

  • Compound semiconductor back hole device, method for manufacturing the same, and transistor

    CN121076034B