Calcium titanate particle material, method for producing same, slurry composition, and resin composition

The calcium titanate particle material, produced through a spheroidization process and incorporating silicon dioxide, addresses the color change and transmission loss issues in electronic devices by optimizing particle characteristics, reducing dielectric loss tangent and maintaining high dielectric constant, thus enhancing material performance in electronic devices.

WO2024247054A1PCT designated stage expired Publication Date: 2024-12-05ADMATECHS CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2023/019961
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-29
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Calcium titanate materials used in electronic devices undergo color change when exposed to ultraviolet light, leading to transmission loss issues due to high dielectric loss tangent (Df) and the need for materials with high dielectric constant (Dk) that often exhibit high Df, and there is a requirement to reduce transmission loss by lowering Df.

Method used

A calcium titanate particle material with a circularity of 0.8 or more, specific surface area, and optimized volume average particle diameter is produced through a spheroidization process, incorporating silicon dioxide to suppress color change and reduce Df, and is dispersed in a slurry or resin composition.

Benefits of technology

The calcium titanate particle material effectively optimizes the relationship between particle diameter and specific surface area, suppressing color changes over time and reducing Df, thereby minimizing transmission loss in electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
Patent Text Reader

Abstract

The present invention addresses the problem of providing a calcium titanate particle material in which a color change caused by UV irradiation is suppressed. To solve this problem, a calcium titanate particle material according to the present invention has a circularity of 0.8 or more, a volume average particle diameter of a (μm), and a specific surface area of b (m2 / g), where a is at least 0.1 but not more than 8 and ab is less than 4. With this configuration, the relationship between the volume average particle diameter and the specific surface area can be made appropriate, and as a result, changes in color over time can be suppressed.
Need to check novelty before this filing date? Find Prior Art

Description

Calcium titanate particulate material, its manufacturing method, slurry composition, and resin composition

[0001] The present invention relates to a calcium titanate particulate material, a method for producing the same, a slurry composition, and a resin composition, and more particularly to a calcium titanate particulate material, a method for producing the same, and a slurry composition and a resin composition in which the calcium titanate particulate material is dispersed.

[0002] In recent years, electronic devices have become increasingly faster and operate at higher frequencies. As a result, reducing transmission loss in materials for electronic devices, such as substrate materials and encapsulants, has become an important issue. The magnitude of transmission loss is greatly influenced by the dielectric loss tangent (Df), and it is possible to reduce transmission loss by using materials with a low Df.

[0003] Some electronic device materials are required to have a high dielectric constant (Dk), but materials with a high Dk often have a high Df, so it is necessary to reduce Df to reduce transmission loss. Calcium titanate is a material that is likely to achieve high Dk and low Df (Patent Document 1).

[0004] International Publication No. 2022 / 124396

[0005] However, calcium titanate discolors when exposed to ultraviolet light, and as a result, resin compositions in which calcium titanate particles are dispersed in a resin material suffer from a problem of color and appearance changes over time.

[0006] The present invention was completed in view of the above-mentioned circumstances, and an object of the present invention is to provide a calcium titanate particulate material that is inhibited from changing in color upon irradiation with ultraviolet light, a method for producing the same, a slurry composition, and a resin composition.

[0007] The calcium titanate particulate material of the present invention, which solves the above problems, has a circularity of 0.8 or more, a volume average particle size of a (μm), and a specific surface area of ​​b (m 2 / g), a is 0.1 or more and 8 or less, and ab is less than 4.

[0008] The method for producing calcium titanate particulate material of the present invention, which solves the above-mentioned problems, includes a spheroidizing step in which raw particle material containing calcium titanate as a main component is dispersed in a carrier and introduced into a high-temperature atmosphere.

[0009] The slurry composition of the present invention, which solves the above-mentioned problems, comprises the calcium titanate particulate material of the present invention and a dispersion medium which is a liquid substance that disperses the calcium titanate particulate material.

[0010] The resin composition of the present invention, which solves the above-mentioned problems, comprises the calcium titanate particulate material of the present invention and a resin material for dispersing the calcium titanate particulate material.

[0011] The calcium titanate particulate material of the present invention has the above-described structure, and as a result, the relationship between the volume average particle size and the specific surface area can be optimized, and therefore, the change in color over time can be suppressed.

[0012] The calcium titanate particulate material of the present invention will be described in detail below based on embodiments. The calcium titanate particulate material of this embodiment can be suitably used as a material for electronic devices. A specific example of a suitable electronic device to which the calcium titanate particulate material is applicable is an antenna-in-package, and the material is preferably used as a slurry composition or a resin composition. Examples of resin compositions include prepregs, copper-clad laminates, and films. Note that, in this specification, a range of values ​​described as a to b includes the values ​​of a and b. Ranges excluding a and b can also be created by correction. Furthermore, when numerical values ​​are described in this specification, it is possible to adopt a numerical range with upper and lower limits defined by combining values ​​arbitrarily selected from those values. Furthermore, values ​​arbitrarily selected from those values ​​can be used as the upper or lower limit. The values ​​adopted as the upper or lower limit may or may not be included in the set range. Furthermore, one of the upper and lower limits may be included in the range, while the other may be excluded. (Calcium Titanate Particulate Material) The calcium titanate particulate material of this embodiment is primarily composed of calcium titanate. "Calcium titanate is the main component" means that the lower limit of the amount of calcium titanate is 50% by mass, and preferably the lower limit is 60%, 70%, 80%, 90%, 95%, 99%, or 100% by mass (unavoidable impurities or trace amounts of impurities may be included). Compounds that may be contained in addition to calcium titanate include iron oxide, molybdenum oxide, and silicon dioxide. The impurities may be contained in the calcium titanate crystals or as independent particles.

[0013] It is particularly preferable to contain silicon dioxide, as this further suppresses coloration. The upper limit of the silicon dioxide content can be 10 mass%, 7.5 mass%, or 5.0 mass%, and the lower limit can be 1.0 mass%, 2.0 mass%, or 3.0 mass%. These upper and lower limit values ​​can be arbitrarily combined. By setting the silicon dioxide content at or above this lower limit, coloration can be sufficiently suppressed, and by setting it at or below this upper limit, improvements in dielectric properties, such as an increased dielectric constant, can be realized.

[0014] The content of silicon dioxide can be set within the above range based on the total mass of the calcium titanate particulate material, and it is particularly preferable that the amount of silicon dioxide on the surface of the calcium titanate particulate material is within these upper and lower limit values.

[0015] In particular, the presence of silica on the surface can reduce the amount of ultraviolet light reaching calcium titanate. Specifically, it is more preferable that the silicon dioxide content measured by energy dispersive X-ray spectroscopy (EDX) is within the above-mentioned upper and lower limit ranges. EDX is a measurement method in which the measured value depends particularly on the atomic composition at the surface.

[0016] The calcium titanate particulate material of this embodiment has a circularity of 0.8 or more, preferably 0.85 or more, more preferably 0.9 or more, even more preferably 0.95 or more, and particularly preferably 0.99 or more.

[0017] The circularity was measured by taking a photograph with an SEM and calculating the circularity from the area and perimeter of the observed particle: (Circularity) = {4π × (area) ÷ (perimeter)} 2 The closer to 1 the particle is, the closer it is to a perfect sphere. Specifically, the average value measured for 100 particles using an image processing device (Sysmex Corporation: FPIA-3000) is used.

[0018] The calcium titanate particulate material of this embodiment has a volume average particle size of a (μm) and a specific surface area of ​​b (m 2 / g). a is 0.1 or more and 8 or less. The lower limit of a is more preferably 0.2 or 0.3, and more preferably 7.0, 6.0, 5.5, 5.0, 4.0, or 2.5. When a is equal to or more than this lower limit, dispersibility in a slurry composition such as a varnish is improved, and when a is equal to or less than this upper limit, the settling rate decreases, reducing the risk of separation.

[0019] The upper limit of b is preferably 2.2, 2.0, 1.8, or 1.5, and the lower limit is preferably 0.1, 0.2, or 0.4. ab is smaller than 4. The upper limit of ab is preferably 4.0, 3.5, 3.0, 2.5, or 2.0. The upper and lower limit values ​​of a, b, and ab can be combined in any desired manner.

[0020] The calcium titanate particulate material of this embodiment preferably has a water content of 800 ppm or less. The upper limit of the water content is more preferably 700 ppm, 600 ppm, 500 ppm, 400 ppm, or 300 ppm. The water content is measured by the Karl Fischer method. Reducing the water content can reduce the Df value and suppress side reactions when dispersed in a resin.

[0021] The calcium titanate particulate material of this embodiment preferably has a Df of 0.016 or less, more preferably 0.015 or less, even more preferably 0.010 or less, and particularly preferably 0.008 or less.

[0022] The calcium titanate particulate material of this embodiment preferably has a b* / a* ratio of 5 or more, more preferably 5.5 or more, and even more preferably 6.0 or more. The b* / a* ratio is measured by irradiating a surface of a material having a thickness of 5 mm or less with a mercury lamp at a light intensity of 11.5 kW / m 2 The sample is irradiated for 72 hours at 1000 kJ / cm² for 72 hours, and the dispersion is dispersed in a cyclohexane solution at a concentration of 33.3% by mass. The dispersion is measured using a color difference meter (for example, a spectrophotometer CM-5 manufactured by Konica Minolta).

[0023] The calcium titanate particulate material of this embodiment is preferably surface-treated. While the surface treatment agent is not particularly limited, it is preferable to use a silane compound such as a silane coupling agent or a silazane compound. Examples of silane compounds include those having organic functional groups, such as alkyl groups, phenyl groups, amino groups, phenylamino groups, vinyl groups, methacryl groups, and epoxy groups, either alone or in combination. Examples of silazane compounds include hexamethyldisilazane.

[0024] The surface treatment agent may be a single compound or a mixture of multiple compounds. The organic functional group is determined depending on the type of resin material and dispersion medium to be combined. The amount of the surface treatment agent is not particularly limited, but can be 0.1 to 5.0 parts by mass per 100 parts by mass of the calcium titanate particulate material. (Method for producing calcium titanate particulate material) The method for producing a calcium titanate particulate material of this embodiment is a method that can suitably produce the calcium titanate particulate material of this embodiment described above, and includes a spheroidizing step and other steps selected as necessary.

[0025] The spheroidization process involves heating and melting raw material particles in a high-temperature atmosphere to form spheroids, followed by rapid cooling to obtain particles with high circularity. The high-temperature atmosphere is not particularly limited, but is preferably at a temperature at which calcium titanate can be softened or melted.

[0026] The high-temperature atmosphere may be a flame or plasma formed by burning a mixture of a flammable gas and a combustion-supporting gas, such as propane gas, acetylene gas, or hydrogen gas.

[0027] The volume average particle size and particle size distribution of the calcium titanate particulate material obtained after the spheroidizing step are controlled according to the volume average particle size and particle size distribution of the raw material particulate material.

[0028] The raw particle material can be made to have the desired particle size distribution by grinding large particles into smaller particles, by granulating the calcium titanate during synthesis, by melting calcium titanate and granulating it with an atomizer, or by other methods.

[0029] The raw material particles are introduced into a high-temperature atmosphere in the form of a dispersion in a carrier, which can be a gas such as an inert gas like nitrogen, a combustion-promoting gas like oxygen, or a flammable gas like propane, or a liquid such as water, an alcohol like methanol or isopropanol, or a ketone like acetone.

[0030] The raw material particle material is a particle material mainly composed of calcium titanate, and its composition is the same as that of the calcium titanate to be produced, as described above, and therefore further explanation is omitted. Here, the composition of the raw material particle material is roughly reflected in the composition of the calcium titanate particle material to be produced, so the composition, purity, etc. of the raw material particle material are set according to the composition and purity of the calcium titanate particle material to be finally produced.

[0031] As mentioned above, if it is desired to increase only the silicon dioxide content on the surface of a calcium titanate particulate material, this can be achieved by attaching a particulate material made of silicon dioxide (silica particulate material) to the surface of the raw particulate material. It is preferable for the silica particulate material to have a smaller particle size than the raw particulate material, as this makes it easier to coat the surface of the raw particulate material. For example, silica particulate material with a particle size of approximately 1 to 100 nm can be used. These silica particulate materials can also be surface-treated with a silane compound or a silazane compound to introduce alkyl groups such as phenyl groups and methyl groups.

[0032] The silica particle material may be mixed in a dry state or in a wet state, and the mixing operation may be performed by stirring and mixing using a mixer, by pulverizing using a pulverizer such as a vibration mill, or by vibrating using ultrasonic irradiation or the like when mixing in a wet state.

[0033] When mixing in a wet state, the raw particle material and the silica particle material can be dispersed in a liquid carrier to form a slurry, which can be introduced into a high-temperature atmosphere.

[0034] The concentration of the raw material particles dispersed in the carrier and the speed at which the dispersion is supplied are not particularly limited. 3 The amount of raw granular material can be about 0.5 kg to 10 kg per 10000 kcal. The lower limit of the amount of raw granular material can be 1 kg or 2 kg, and the upper limit can be 10 kg, 8 kg, or 3 kg.

[0035] The feed rate of the dispersion may vary depending on the size of the flame, but may be about 5 kg / hour to 15 kg / hour of raw particle material, with upper limits of 15 kg / hour, 13 kg / hour, or 10 kg / hour, and lower limits of 5 kg / hour, 7 kg / hour, or 9 kg / hour.

[0036] The raw material particle material can be subjected to the same surface treatment as can be applied to the calcium titanate particulate material of this embodiment. Surface treatment has the advantage of improving fluidity. (Slurry Composition) The slurry composition of this embodiment is prepared by mixing the calcium titanate particulate material of this embodiment with a liquid dispersion medium, and dispersing the calcium titanate particulate material in the dispersion medium. The mixing ratio of the calcium titanate particulate material to the dispersion medium is not particularly limited, but the calcium titanate particulate material preferably accounts for 30% or more of the total mass, more preferably 50% or more, and even more preferably 70% or more.

[0037] As the dispersion medium, liquids known as solvents, such as alcohols such as methanol and isopropanol, alkanes such as hexane, and ketones such as acetone, as well as precursors of resin materials, such as liquid monomers, that subsequently harden and become non-liquid, can be used. Whether a material is liquid is determined by whether it remains liquid when used under specific conditions that can be set arbitrarily. Therefore, any material that becomes liquid at high or low temperatures when used can be used as a dispersion medium. Compounds that dissolve in dispersion mediums can also be dissolved in the dispersion medium.

[0038] The slurry composition of this embodiment may also contain particulate materials other than calcium titanate particulate material. For example, it may contain particulate materials made of inorganic materials such as silica and alumina, or particulate materials made of resin materials such as polyolefin and perfluoropolyolefin. (Resin Composition) The resin composition of this embodiment is obtained by mixing the calcium titanate particulate material of this embodiment with a resin material, and dispersing the calcium titanate particulate material in the resin material. The mixing ratio of the calcium titanate particulate material to the resin material is not particularly limited, but the calcium titanate particulate material preferably accounts for 80% or more of the total mass, more preferably 70% or more, and even more preferably 60% or more.

[0039] Examples of the resin material include precursors of thermosetting resins such as epoxy resins and urea resins before curing, thermoplastic resins such as polyolefins and polyesters, and their monomers. If the resin material is in a liquid state, it may correspond to the resin composition of this embodiment and may also correspond to the slurry composition of this embodiment.

[0040] The resin composition of the present embodiment may contain particulate materials other than calcium titanate particulate materials, such as particulate materials made of inorganic materials such as silica and alumina, and particulate materials made of resin materials such as polyolefin and perfluoropolyolefin.

[0041] The calcium titanate particulate material and its manufacturing method of the present invention will be described with reference to the following examples. (Test Example 1) A mixture of calcium titanate particles crushed by a milling operation and spherical silica was used as the raw particulate material. The content of spherical silica was 5.0% based on the mass of the entire raw particulate material. The spherical silica had a particle size of 10 nm, and the raw particulate material, which was a mixture of calcium titanate particles and spherical silica, was adhered to the surfaces of the calcium titanate particles.

[0042] 10 kg / hour of raw material particles was fed to a carrier consisting of nitrogen gas at 5 Nm 3The mixture was dispersed for 1 hour and then thrown into a flame formed in the furnace body (spheroidization step). The flame was a flammable gas of 5 Nm of propane gas. 3 / hour, oxygen 17 Nm as combustion supporting gas 3 It was formed using / time.

[0043] The raw material particles introduced into the flame melted and became spherical due to surface tension. They then fell away from the flame and solidified while remaining spherical upon cooling. The resulting spherical calcium titanate (calcium titanate particle material) was collected using a bag filter, cyclone, or other device and used as the test sample for this test example. (Test Examples 2 and 3) Raw material particles with different calcium titanate particle sizes were subjected to a spheroidization process under the conditions shown in Test Example 1 to prepare the test samples for each test example. The smaller the particle size of the calcium titanate particles, the smaller the particle size of the resulting test sample. (Test Examples 4 and 5) The test samples from Test Examples 1 and 2 were subjected to surface treatment to obtain the test samples for each test example. The surface treatment was performed using KBM-1003 as the surface treatment agent. (Test Example 6) The raw material particles used in the preparation of Test Example 1 were used as the test sample for this test example. (Test Example 7) A particle material obtained in the same manner as in Test Example 1, except that the raw particle material did not contain spherical silica but only calcium titanate particles, was used as the test sample for this comparative example. (Evaluation) For the test samples of each test example, the circularity, color a* and b*, volume-average particle size, specific surface area, water content, Df, and silicon dioxide concentration (SiO2 proportion: mass%) were measured. These measured values, as well as the values ​​of b* / a* and volume-average particle size x specific surface area, are shown in Table 1.

[0044] Measurements of circularity, color, and moisture content were performed using the methods described in the embodiments. The volume average particle size was measured using a laser diffraction particle size distribution analyzer. For the specific surface area, 1.0 g of each test sample was weighed out and placed in a measurement cell, and after pretreatment, the BET specific surface area value was measured. The measuring machine used was a "Macsorb HM model-1208" (manufactured by MACSORB). The pretreatment conditions were a degassing temperature of 200°C, a degassing time of 30 minutes, and a cooling time of 4 minutes.

[0045] Df was measured in accordance with JIS C 2138 (2007). Specifically, the relative permittivity and dielectric loss tangent at 1 GHz were measured using a Keysight Network Analyzer (product name "E5071C") and a cavity resonator perturbation method. Furthermore, the silicon dioxide concentration (SiO2 ratio: mass %) on the surface was measured by EDX. The mass-based content was calculated based on the obtained measurements.

[0046] As is clear from Table 1, the test samples of Test Examples 1 to 5 had a larger b* / a* ratio than the test sample of Test Example 6, and it was found that the change in color could be suppressed. In addition, the water content was small and Df could be reduced. The test samples of Test Examples 1 to 5 had a higher silicon dioxide content than the test sample of Test Example 6.

[0047] Test Examples 4 and 5, which were surface-treated, had slightly higher b* / a* values ​​than Test Examples 1 to 3, which were otherwise identical, demonstrating that surface treatment can suppress changes in color. Test Examples 4 and 5, which were surface-treated, also had lower water contents and smaller Df values. Furthermore, the test sample of Test Example 1, which contained silica, had a higher b* / a* value than the test sample of Test Example 7, which did not contain silica, demonstrating less change in color.

Claims

1. Circularity is 0.8 or more, volume average particle size is a (μm), specific surface area is b (m 2 / g), a is 0.1 or more and 8 or less, and ab is less than 4.

2. The calcium titanate particulate material according to claim 1, having a moisture content of 800 ppm or less.

3. The calcium titanate particulate material according to claim 1, having a dielectric tangent of 0.016 or less.

4. The calcium titanate particulate material according to claim 1, wherein the b* / a* ratio measured by the following measurement method is 5 or more. (Measurement method) 11.5 kW / m2 on a surface of 5 mm or less in thickness. 2 A sample is irradiated with a mercury lamp for 72 hours, and the dispersion is dispersed in a cyclohexane solution at a concentration of 33.3% by mass, and the dispersion is measured with a color difference meter.

5. The calcium titanate particulate material according to claim 1, having a silicon dioxide content of 1 to 10 mass % as measured by energy dispersive X-ray analysis.

6. The calcium titanate particulate material of claim 1 which has been surface treated.

7. A method for producing calcium titanate particulate material, comprising a spheronizing step in which raw particle material mainly composed of calcium titanate is dispersed in a carrier and introduced into a high-temperature atmosphere.

8. A slurry composition comprising the calcium titanate particulate material according to any one of claims 1 to 6 and a dispersion medium which is a liquid substance for dispersing the calcium titanate particulate material.

9. A resin composition comprising the calcium titanate particulate material according to any one of claims 1 to 6 and a resin material in which the calcium titanate particulate material is dispersed.

Citation Information

Patent Citations

  • Method of manufacturing spherical powder, spherical oxide powder and oxide powder

    JP2005015303A

  • Single crystal ceramic particle and spherical oxide powder

    JP2005112665A

  • Infrared reflective material, and paint and resin composition containing the same

    JP2013173953A

  • Molding resin composition and electronic component device

    WO2022124396A1