Super-hard alloy and cutting tool

The cemented carbide composition, with its optimized tungsten carbide and binder phases, addresses the challenges of wear and chipping in cutting tools, enhancing tool life and thermal conductivity for efficient high-speed machining.

WO2024247093A1PCT designated stage expired Publication Date: 2024-12-05SUMITOMO ELECTRIC HARDMETAL CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2023/020055
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-30
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Modern cutting processes face challenges with increasingly difficult work materials, requiring improved machining efficiency, which demands stricter conditions such as higher cutting speeds, feed amounts, and depths of cut, leading to wear and chipping issues in cutting tools.

Method used

A cemented carbide composition comprising a first phase of tungsten carbide particles with specific size distribution, a cobalt binder phase, and a third phase of titanium, tantalum, niobium, zirconium, and carbon or nitrogen, optimized to provide excellent wear resistance and chipping resistance, thereby extending tool life.

Benefits of technology

The cemented carbide composition enhances wear resistance and chipping resistance, resulting in a cutting tool with improved tool life and thermal conductivity, reducing thermal wear even at high-speed machining conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-M000001
    Figure JPOXMLDOC01-APPB-M000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

Provided is a super-hard alloy that includes a first phase, a second phase and a third phase. The first phase comprises a plurality of tungsten carbide particles. The content of the first phase in the super-hard alloy is 65-85 vol%. The arithmetic mean diameter a of the tungsten carbide particles is 0.5-2.0 μm. This arithmetic mean diameter a and the standard deviation b of the particle diameter of the tungsten carbide particles satisfy a relationship represented by formula I: b<0.49a+0.063. In formula I, units for a and b are μm. The arithmetic mean diameter a and the number-based 10% cumulative particle diameter c of the tungsten carbide particles satisfy a relationship represented by formula II: c>0.34a+0.098. In formula II, units for a and c are μm. The second phase comprises cobalt. The content of cobalt in the super-hard alloy is 3-15 mass%. The third phase comprises: at least one element selected from the group consisting of titanium, tantalum, niobium, zirconium and tungsten; and at least one of carbon and nitrogen. The third phase does not contain tungsten carbide. The total content of titanium, tantalum, niobium and zirconium in the super-hard alloy is 2-8 mass%.
Need to check novelty before this filing date? Find Prior Art

Description

Cemented Carbide and Cutting Tools

[0001] The present disclosure relates to cemented carbides and cutting tools.

[0002] Conventionally, cemented carbide having a hard phase mainly composed of tungsten carbide (WC) and a binder phase mainly composed of an iron-group element has been used as a material for cutting tools. The cemented carbide described in Patent Document 1 has, as the hard phase, a phase consisting of at least one composite compound of carbide, nitride, and carbonitride containing tungsten (W) and a metal element other than W, in addition to the hard phase mainly composed of WC, and aims to improve chipping resistance by bonding the WC particles and the composite compound particles.

[0003] JP 2016-20541 A

[0004] The cemented carbide of the present disclosure is a cemented carbide including a first phase, a second phase, and a third phase, wherein the first phase is composed of a plurality of tungsten carbide particles, the content of the first phase in the cemented carbide is 65% by volume or more and 85% by volume or less, the tungsten carbide particles have an arithmetic mean diameter a of 0.5 μm or more and 2.0 μm or less, the arithmetic mean diameter a and the standard deviation b of the particle diameters of the tungsten carbide particles have a relationship of the following formula I: b<0.49a+0.063 Formula I In Formula I, the units of a and b are μm, the arithmetic mean diameter a and the 10% cumulative particle diameter c on a number basis of the tungsten carbide particles have a relationship of the following formula II: c>0.34a+0.098 Formula II In Formula II, the units of a and c are μm, the second phase is composed of cobalt, The cemented carbide has a cobalt content of 3% by mass or more and 15% by mass or less, the third phase is composed of at least one element selected from the group consisting of titanium, tantalum, niobium, zirconium, and tungsten, and at least one of carbon and nitrogen, the third phase does not contain tungsten carbide, and the total content of titanium, tantalum, niobium, and zirconium in the cemented carbide is 2% by mass or more and 8% by mass or less.

[0005] [Problem to be Solved by the Present Disclosure] In recent years, workpiece materials have become increasingly difficult to cut in cutting processes. Furthermore, demands for improved processing efficiency have led to stricter processing conditions, such as increased cutting speeds, feed rates, and depths of cut.

[0006] Therefore, an object of the present disclosure is to provide a cemented carbide that, when used as a tool material, can provide a cutting tool that has excellent wear resistance and fracture resistance and a long tool life, and to provide a cutting tool that has a long tool life.

[0007] [Effects of the Present Disclosure] According to the present disclosure, it is possible to provide a cemented carbide that, when used as a tool material, can provide a cutting tool that has excellent wear resistance and fracture resistance and a long tool life, as well as a cutting tool that has a long tool life.

[0008] [Description of Embodiments of the Present Disclosure] First, embodiments of the present disclosure will be listed and described. (1) The cemented carbide of the present disclosure is a cemented carbide including a first phase, a second phase, and a third phase, wherein the first phase is composed of a plurality of tungsten carbide particles, the content of the first phase in the cemented carbide is 65% by volume or more and 85% by volume or less, the tungsten carbide particles have an arithmetic mean diameter a of 0.5 μm or more and 2.0 μm or less, the arithmetic mean diameter a and the standard deviation b of the particle diameters of the tungsten carbide particles have a relationship of the following formula I: b<0.49a+0.063 Formula I In the formula I, the units of a and b are μm, the arithmetic mean diameter a and the 10% cumulative particle diameter c on a number basis of the tungsten carbide particles have a relationship of the following formula II: c>0.34a+0.098 Formula II In the formula II, the units of a and c are μm, the second phase is composed of cobalt, The cemented carbide has a cobalt content of 3% by mass or more and 15% by mass or less, the third phase is composed of at least one element selected from the group consisting of titanium, tantalum, niobium, zirconium, and tungsten, and at least one of carbon and nitrogen, the third phase does not contain tungsten carbide, and the total content of titanium, tantalum, niobium, and zirconium in the cemented carbide is 2% by mass or more and 8% by mass or less.

[0009] When used as a tool material, the cemented carbide of the present disclosure can provide a cutting tool that has excellent wear resistance and chipping resistance and can have a long tool life.

[0010] (2) In the above (1), a first image obtained by performing binarization on a backscattered electron image of a cross section of the cemented carbide may include a first region consisting of the first phase and a second region consisting of the second phase and the third phase, and the arithmetic mean diameter d of the second region in the first image may be 0.3 μm or more and 0.9 μm or less. The backscattered electron image may be obtained by photographing the cross section of the cemented carbide at 5000x magnification using a scanning electron microscope.

[0011] According to this, the presence of the second region with an appropriate grain size improves the wear resistance of the cemented carbide. If the grain size of the second region is small, wear due to shedding tends to progress during cutting. If the grain size of the second region is large, that is, if there is variation in the location of the second region, uneven wear tends to progress, and wear resistance tends to decrease.

[0012] (3) In the above (1) or (2), the tungsten carbide particles may have an arithmetic mean diameter a of 0.8 μm or more and 1.6 μm or less, thereby further improving the tool life.

[0013] (4) In any one of the above (1) to (3), the cobalt content of the cemented carbide may be 4% by mass or more and 11% by mass or less, thereby further improving the tool life.

[0014] (5) A cutting tool according to the present disclosure is a cutting tool including the cemented carbide according to any one of (1) to (4) above. The cutting tool according to the present disclosure has excellent wear resistance and chipping resistance and can have a long tool life.

[0015] [Details of the embodiment of the present disclosure] Specific examples of the cemented carbide of the present disclosure are described below.

[0016] In the present disclosure, the notation in the form of "A to B" means the upper and lower limits of a range (i.e., A or more and B or less), and when no unit is specified for A and a unit is specified only for B, the units of A and B are the same.

[0017] In the present disclosure, when a compound or the like is represented by a chemical formula, unless the atomic ratio is particularly limited, it is intended to include any conventionally known atomic ratio, and should not necessarily be limited to only those within the stoichiometric range.

[0018] In the present disclosure, when one or more numerical values ​​are recited as the lower limit and the upper limit of a numerical range, a combination of any one numerical value recited as the lower limit and any one numerical value recited as the upper limit is also considered to be disclosed. For example, when a1 or more, b1 or more, and c1 or more are recited as the lower limit and a2 or less, b2 or less, and c2 or less are recited as the upper limit, a1 or more and a2 or less, a1 or more and b2 or less, a1 or more and c2 or less, b1 or more and a2 or less, b1 or more and b2 or less, b1 or more and c2 or less, c1 or more and a2 or less, c1 or more and b2 or less, and c1 or more and c2 or less are considered to be disclosed.

[0019] [Embodiment 1: Cemented Carbide] A cemented carbide according to one embodiment of the present disclosure (hereinafter also referred to as "Embodiment 1") is a cemented carbide including a first phase, a second phase, and a third phase, wherein the first phase is composed of a plurality of tungsten carbide particles, and the content of the first phase in the cemented carbide is 65% by volume or more and 85% by volume or less, and the tungsten carbide particles have an arithmetic mean diameter a of 0.5 μm or more and 2.0 μm or less, and the arithmetic mean diameter a and the standard deviation b of the particle diameters of the tungsten carbide particles have a relationship expressed by the following formula I: b<0.49a+0.063 Formula I In Formula I, the units of a and b are μm, and the arithmetic mean diameter a and the 10% cumulative particle diameter c on a number basis of the tungsten carbide particles have a relationship expressed by the following formula II: c>0.34a+0.098 Formula II In Formula II above, the units of a and c are μm, the second phase is made of cobalt, and the cobalt content of the cemented carbide is 3% by mass or more and 15% by mass or less; the third phase is made of at least one element selected from the group consisting of titanium, tantalum, niobium, zirconium, and tungsten, and at least one of carbon and nitrogen, and the third phase does not contain tungsten carbide; and the total content of titanium, tantalum, niobium, and zirconium in the cemented carbide is 2% by mass or more and 8% by mass or less.

[0020] When used as a tool material, the cemented carbide of the present disclosure can provide a cutting tool that has excellent wear resistance and fracture resistance and can have a long tool life. The reason for this is not clear, but is presumed to be as follows.

[0021] (i) The cemented carbide of the present disclosure contains 65% by volume or more and 85% by volume or less of a first phase consisting of a plurality of tungsten carbide particles (hereinafter also referred to as "WC particles"). The tungsten carbide particles have high hardness and high thermal conductivity. Therefore, the cemented carbide of the present disclosure also has high hardness and high thermal conductivity, and cutting tools including the cemented carbide can have excellent wear resistance.

[0022] (ii) The cemented carbide of the present disclosure contains 3% by mass or more and 15% by mass or less of cobalt. Cobalt has high toughness. Therefore, the cemented carbide of the present disclosure also has high toughness, and cutting tools including the cemented carbide can have excellent chipping resistance.

[0023] (iii) The cemented carbide of the present disclosure includes a third phase consisting of at least one element selected from the group consisting of titanium, tantalum, niobium, zirconium, and tungsten, and at least one of carbon and nitrogen. The third phase can improve the reactivity and oxidation resistance of the cemented carbide. Therefore, a cutting tool including the cemented carbide has improved reactivity and oxidation resistance, which in turn improves wear resistance.

[0024] (iv) In the cemented carbide alloy of the present disclosure, the arithmetic mean diameter a of the tungsten carbide particles is 0.5 μm or more and 2.0 μm or less, and the arithmetic mean diameter a and the standard deviation b of the particle diameter of the tungsten carbide particles have the relationship of the following formula I: b<0.49a+0.063 Formula I The standard deviation b has a positive correlation with the arithmetic mean diameter a. Tungsten carbide particles that satisfy formula I exhibit high particle size uniformity regardless of the size of the arithmetic mean diameter a. In the cemented carbide alloy of the present disclosure, the arithmetic mean diameter a of the tungsten carbide particles and the 10% cumulative particle size c based on the number of tungsten carbide particles have the relationship of the following formula II: c>0.34a+0.098 Formula II Tungsten carbide particles that satisfy formula II exhibit few fine particles regardless of the size of the arithmetic mean diameter a. When the particle size of the tungsten carbide particles satisfies Formula I and Formula II, the tungsten carbide particles can be uniformly distributed in the cemented carbide structure. In the cemented carbide of the present disclosure, the tungsten carbide particles are uniformly distributed, so that cutting heat generated during cutting is easily dissipated to the outside of the cutting tool via the tungsten carbide particles. Therefore, a tool including the cemented carbide of the present disclosure has improved thermal conductivity, and is less susceptible to thermal wear even during high-speed cutting, which tends to increase the cutting edge temperature, and can have excellent wear resistance.

[0025] <First Phase> <Composition of First Phase> In the cemented carbide of the first embodiment, the first phase is composed of a plurality of tungsten carbide particles. Here, the tungsten carbide particles include not only "pure WC particles (including WC containing no impurity elements and WC with impurity elements below the detection limit)" but also "WC particles containing impurities therein, as long as the effects of the present disclosure are not impaired." Examples of impurities include iron (Fe), molybdenum (Mo), and sulfur (S).

[0026] <First Phase Content of Cemented Carbide> In the cemented carbide of embodiment 1, the first phase content of the cemented carbide is 65 vol% or more and 85 vol% or less. From the viewpoint of improving hardness, the lower limit of the first phase content of the cemented carbide is 65 vol% or more, or may be 66 vol% or more, 70 vol% or more, 72 vol% or more, or 75 vol% or more. From the viewpoint of improving toughness, the upper limit of the first phase content of the cemented carbide is 85 vol% or less, or may be 84 vol% or less, 80 vol% or less, or may be 78 vol% or less. The first phase content of the cemented carbide may be 70 vol% or more and 80 vol% or less, or may be 72 vol% or more and 84 vol% or less.

[0027] In the present disclosure, the content of the first phase in a cemented carbide is measured by the following procedure: (A1) A surface or cross section of the cemented carbide is subjected to mirror finishing. Examples of mirror finishing methods include polishing with diamond paste, using a focused ion beam (FIB) device, using a cross-section polisher (CP) device, and a combination of these methods.

[0028] (B1) The processed surface of the cemented carbide is photographed using a scanning electron microscope ("S-3400N" manufactured by Hitachi High-Technologies Corporation) to obtain a backscattered electron image. Six backscattered electron images are prepared. Each of the six backscattered electron images has a different photographed area. The photographed location can be set arbitrarily. The observation conditions are a magnification of 5000x and an accelerating voltage of 10 kV.

[0029] (C1) The six backscattered electron images obtained in (B1) above are imported into a computer using image analysis software (ImageJ, version 1.51j8: https: / / imagej.nih.gov / ij / ), and binarized to obtain six binarized images. The binarization is performed under conditions preset in the image analysis software by clicking the "Make Binary" button on the computer screen after importing the images. In the binarized image, the first region consisting of the first phase and the second region consisting of the second and third phases can be distinguished by their shades of color. For example, in the binarized image, the first phase is shown as a black region, and the second and third phases are shown as white regions.

[0030] (D1) In each of the six binarized images, a rectangular measurement field of 25.3 μm in length and 17.6 μm in width is set. Using the image analysis software, the area percentage (area %) of the first phase is measured in each of the six measurement fields, with the entire measurement field being used as the denominator.

[0031] (E1) Calculating the average area percentage (area %) of the first phase obtained in the six measurement fields. In the present disclosure, the average area percentage (area %) of the first phase obtained in the six measurement fields is defined as the content (volume %) of the first phase in the cemented carbide.

[0032] As far as the applicant has measured, it has been confirmed that, as long as measurements are made on the same sample, even if the above measurement is performed multiple times by changing the selected location of the measurement field, there is little variation in the measurement results, and that setting the measurement field arbitrarily will not be arbitrary.

[0033] <Arithmetic mean diameter a of tungsten carbide particles> In the cemented carbide of embodiment 1, the arithmetic mean diameter a of the tungsten carbide particles is 0.5 μm or more and 2.0 μm or less. In the present disclosure, the arithmetic mean diameter a of the tungsten carbide particles refers to the arithmetic mean of the circle-equivalent diameters of WC particles measured on the surface or cross section of the cemented carbide based on the number. When the arithmetic mean diameter a of the WC particles is 0.5 μm or more, cutting tools using the cemented carbide are less likely to experience shedding wear during use. When the arithmetic mean diameter a of the WC particles is 2.0 μm or less, the cemented carbide has excellent transverse rupture strength, and cutting tools using the cemented carbide can have excellent chipping resistance.

[0034] The lower limit of the arithmetic mean diameter a of the WC particles may be 0.50 μm or more, 0.60 μm or more, 0.70 μm or more, or 0.80 μm or more from the viewpoint of suppressing shedding wear. The upper limit of the arithmetic mean diameter a of the WC particles may be 2.00 μm or less, 1.80 μm or less, 1.60 μm or less, or 1.40 μm or less from the viewpoint of improving transverse rupture strength. The arithmetic mean diameter a of the WC particles may be 0.50 μm or more and 2.00 μm or less, 0.60 μm or more and 1.80 μm or less, 0.70 μm or more and 1.60 μm or less, 0.80 μm or more and 1.60 μm or less, or 0.80 μm or more and 1.40 μm or less.

[0035] In the present disclosure, the arithmetic mean diameter a of tungsten carbide particles is measured by the following procedures (A2) to (B2): (A2) Six binarized images are obtained by the same method as (A1) to (C1) described in the method for measuring the content of the first phase in cemented carbide.

[0036] (B2) A rectangular measurement field of view measuring 25.3 μm in height and 17.6 μm in width was set in each of the six binarized images obtained. Using image analysis software (ImageJ, version 1.51j8: https: / / imagej.nih.gov / ij / ), the circle-equivalent diameter (Heywood diameter: diameter equivalent to a circle with an equal area) of each of the tungsten carbide particles (first phase) in the six measurement fields was measured.

[0037] (C2) Calculate the number-based arithmetic mean of the circle-equivalent diameters based on all tungsten carbide particles in the six measurement fields, excluding those with a circle-equivalent diameter of 0.22 μm or less. In the present disclosure, this arithmetic mean corresponds to the arithmetic mean diameter a of the WC particles. The reason for excluding tungsten carbide particles with a circle-equivalent diameter of 0.22 μm or less when calculating the arithmetic mean diameter a is that the inventors have confirmed, through measurements, that particles with a circle-equivalent diameter of 0.22 μm or less often correspond to noise that is erroneously detected as tungsten carbide particles in image analysis.

[0038] As far as the applicant has measured, it has been confirmed that, as long as measurements are made on the same sample, even if the above measurement is performed multiple times by changing the selected location of the measurement field, there is little variation in the measurement results, and that setting the measurement field arbitrarily will not be arbitrary.

[0039] <Relationship Between Arithmetic Mean Diameter a of Tungsten Carbide Particles and Standard Deviation b of Particle Diameter of Tungsten Carbide Particles> In the cemented carbide of embodiment 1, the arithmetic mean diameter a of the tungsten carbide particles and the standard deviation b of the particle diameter of the tungsten carbide particles have the relationship represented by the following formula I: b<0.49a+0.063 Formula I In formula I, the units of a and b are μm.

[0040] The particle sizes of the tungsten carbide particles contained in the cemented carbide satisfying the relationship of formula I indicates that the particle sizes of the tungsten carbide particles are highly uniform, regardless of the magnitude of the arithmetic mean diameter a of the tungsten carbide particles. From the viewpoint of improving the uniformity of the particle size, the arithmetic mean diameter a and the standard deviation b may have the relationships of the following formulas IA and IB: b<0.49a+0.061 (formula IA) b<0.49a+0.059 (formula IB)

[0041] In the present disclosure, the standard deviation b of the particle size of tungsten carbide particles is measured by the following procedure. The circle-equivalent diameter (Heywood diameter: diameter equivalent to a circle with an equal area) of each of all tungsten carbide particles (first phase) in the six measurement fields is measured using the same method as (A2) to (B2) described in the measurement method for the arithmetic mean diameter a of tungsten carbide particles. The standard deviation b of the particle size of the tungsten carbide particles is calculated using the following formula based on all tungsten carbide particles in the six measurement fields, excluding tungsten carbide particles with circle-equivalent diameters of 0.22 μm or less.

[0042]

[0043] In the cemented carbide of embodiment 1, the arithmetic mean diameter a of the tungsten carbide particles and the 10% cumulative particle diameter c of the tungsten carbide particles based on the number thereof satisfy the relationship shown in formula II below: c > 0.34a + 0.098 formula II In formula II, the units of a and c are μm. In the present disclosure, the 10% cumulative particle diameter c of the tungsten carbide particles based on the number thereof refers to the cumulative 10% particle diameter from the smallest diameter side in the cumulative particle size distribution based on the number of tungsten carbide particles.

[0044] The particle sizes of the tungsten carbide particles contained in the cemented carbide satisfying the relationship of formula II indicates that there are few fine tungsten carbide particles, regardless of the size of the arithmetic mean diameter a of the tungsten carbide particles. From the viewpoint of reducing the number of fine tungsten carbide particles, the arithmetic mean diameter a and the 10% cumulative particle size c may have the relationships of formulas II-A and II-B below.

[0045] c>0.34a+0.099 Formula II-A c>0.34a+0.100 Formula II-B

[0046] In the present disclosure, the 10% cumulative particle size c on a number basis of tungsten carbide particles is measured by the following procedure. The circle-equivalent diameter (Heywood diameter: diameter equivalent to a circle with an equal area) of each of all tungsten carbide particles (first phase) in six measurement fields is measured using the same method as (A2) to (B2) described in the measurement method for the arithmetic mean diameter a of tungsten carbide particles. The 10% cumulative particle size c on a number basis is determined based on all tungsten carbide particles in the six measurement fields, excluding tungsten carbide particles with circle-equivalent diameters of 0.22 μm or less.

[0047] The cemented carbide of embodiment 1 includes a third phase consisting of at least one element selected from the group consisting of titanium, tantalum, niobium, zirconium, and tungsten, and at least one of carbon and nitrogen. Here, the third phase does not include tungsten carbide. The third phase is added for the purpose of improving the reactivity resistance and oxidation resistance of the cemented carbide. However, because the third phase has low thermal conductivity, when a cemented carbide including the third phase is used under cutting conditions that tend to increase the cutting edge temperature, such as high-speed machining, the cutting edge becomes hot, thermal wear tends to progress, and the wear resistance of the cutting tool tends to decrease. In the cemented carbide of embodiment 1, the particle size distribution of the tungsten carbide particles satisfies the above formulas I and II, so the tungsten carbide particles can be uniformly present in the cemented carbide structure, and cutting heat generated during cutting is easily released to the outside of the cutting tool through the tungsten carbide particles. Therefore, a tool including the cemented carbide of the present disclosure can have improved thermal conductivity, less thermal wear, and excellent wear resistance, even while containing the third phase.

[0048] <Second Phase> <Composition of Second Phase> In the cemented carbide of embodiment 1, the second phase is made of cobalt. The second phase is a binder phase that bonds the tungsten carbide particles that make up the first phase together.

[0049] In the present disclosure, the phrase "the second phase is composed of cobalt (Co)" also includes the case where "the second phase contains impurities together with cobalt, as long as the effects of the present disclosure are not impaired." Examples of impurities include manganese (Mn), magnesium (Mg), calcium (Ca), molybdenum (Mo), sulfur (S), and aluminum (Al).

[0050] <Cobalt Content of Cemented Carbide> In the cemented carbide of embodiment 1, the cobalt content of the cemented carbide is 3% by mass or more and 15% by mass or less. From the viewpoint of improving toughness, the lower limit of the cobalt content of the cemented carbide is 3% by mass or more, or may be 4% by mass or more, 5% by mass or more, or 6% by mass or more. From the viewpoint of improving hardness, the upper limit of the cobalt content of the cemented carbide is 15% by mass or less, or may be 11% by mass or less, or may be 9% by mass or less. The cobalt content of the cemented carbide may be 4% by mass or more and 11% by mass or less, or may be 5% by mass or more and 9% by mass or less.

[0051] In this disclosure, the cobalt content of cemented carbide is measured by cobalt titration. The cobalt titration is performed in accordance with the Japan Machine Tool Manufacturers' Association standard (TAS0054:2017) or ISO3909:1976. Specifically, the method is performed as follows: A cemented carbide sample is pulverized and passed through a 49-mesh sieve. The sample is dissolved in nitric acid and hydrofluoric acid, and ammonium citrate and aqueous ammonia are added. Potentiometric titration is then performed with potassium ferricyanide (red ferricyanide) using platinum and saturated calomel (tungsten) electrodes. The measurement device used is an "AUT-501" manufactured by DKK-TOA Corporation.

[0052] <Third Phase> <Composition of Third Phase> In the cemented carbide of embodiment 1, the third phase is composed of at least one element selected from the group consisting of titanium, tantalum, niobium, zirconium, and tungsten, and at least one of carbon and nitrogen. The third phase does not contain tungsten carbide. The third phase can improve the reactivity resistance and oxidation resistance of the cemented carbide. Therefore, a cutting tool including the cemented carbide has improved reactivity resistance and oxidation resistance.

[0053] In the present disclosure, the phrase "the third phase is composed of at least one element selected from the group consisting of titanium, tantalum, niobium, zirconium, and tungsten, and at least one of carbon and nitrogen" also includes the case where "the third phase contains impurities as long as the effects of the present disclosure are not impaired." Examples of impurities include manganese (Mn), magnesium (Mg), calcium (Ca), molybdenum (Mo), sulfur (S), and aluminum (Al).

[0054] The third phase may contain at least two elements selected from the group consisting of titanium, tantalum, niobium, zirconium and tungsten.

[0055] The third phase may include at least one selected from the group consisting of titanium carbide (TiC), tantalum carbide (TaC), niobium carbide (NbC), titanium nitride (TiN), titanium carbonitride (TiCN), zirconium carbonitride (ZrCN), zirconium carbide (ZrC), and solid solutions derived from these compounds. Examples of the solid solutions include WTiCN, WTiTaCN, and WTiTaNbZrCN.

[0056] In the present disclosure, it is confirmed by the following procedure that the third phase comprises at least one element selected from the group consisting of titanium, tantalum, niobium, zirconium, and tungsten, and at least one of carbon and nitrogen, and that the third phase does not contain tungsten carbide.

[0057] (A3) An arbitrary position of the cemented carbide is thinned using an ion slicer (apparatus: IB09060CIS (trademark) manufactured by JEOL Ltd.) to prepare a sample with a thickness of 30 to 100 nm. The acceleration voltage of the ion slicer is 6 kV for thinning and 2 kV for finishing.

[0058] (B3) The sample is observed at 50,000x magnification using a scanning transmission electron microscope (STEM) (apparatus: JFM-ARM300F (trademark) manufactured by JEOL Ltd.) to obtain a STEM-HAADF (high-angle annular dark field scanning transmission electron microscope) image. The imaging area of ​​the STEM-HAADF image is set to the center of the sample, that is, a position that does not include areas with properties that are clearly different from the bulk portion, such as the surface vicinity of the cemented carbide (a position where the imaging area is entirely the bulk portion of the cemented carbide). The measurement condition is an acceleration voltage of 200 kV.

[0059] (C3) A spot analysis is performed on a third phase present in a STEM-HAADF image using EDX (STEM-EDX) attached to the STEM, and the elements constituting the third phase are quantified. The spot size is set for each third phase to a range that includes only the third phase. When the quantification of the constituent elements satisfies the following conditions (a) and (b), it is confirmed that the third phase is composed of at least one element selected from the group consisting of titanium, tantalum, niobium, zirconium, and tungsten, and at least one of carbon and nitrogen. (a) The third phase contains at least one element selected from the group consisting of titanium, tantalum, niobium, zirconium, and tungsten, and at least one of carbon and nitrogen. (b) No impurity elements other than titanium, tantalum, niobium, zirconium, tungsten, carbon, and nitrogen are confirmed in the third phase, or the content of these impurity elements is less than 0.1 mass%.

[0060] When spot analysis of the third phase by EDX (STEM-EDX) detects only tungsten and carbon, and the carbon content relative to the total mass of tungsten and carbon is approximately 6.1 mass%, the third phase is determined to contain tungsten carbide. In other words, when spot analysis of the third phase by EDX (STEM-EDX) detects elements other than tungsten and carbon, the third phase is determined to not contain tungsten carbide.

[0061] <<Total Content of Titanium, Tantalum, Niobium, and Zirconium in the Cemented Carbide>> In the cemented carbide of embodiment 1, the total content of titanium, tantalum, niobium, and zirconium in the cemented carbide is 2% by mass or more and 8% by mass or less. From the viewpoint of improving reactivity resistance and oxidation resistance, the lower limit of the total content of titanium, tantalum, niobium, and zirconium in the cemented carbide is 2% by mass or more, or may be 3% by mass or more, or 4% by mass or more. From the viewpoint of improving the thermal conductivity of the cemented carbide, the upper limit of the total content of titanium, tantalum, niobium, and zirconium in the cemented carbide is 8% by mass or less, or may be 7% by mass or less, or may be 6% by mass or less. The total content of titanium, tantalum, niobium, and zirconium in the cemented carbide is 2% by mass or more and 8% by mass or less, or may be 3% by mass or more and 7% by mass or less, or may be 4% by mass or more and 6% by mass or less. Here, the third phase may contain at least two elements selected from the group consisting of titanium, tantalum, niobium, zirconium, and tungsten. In the present disclosure, the total content of titanium, tantalum, niobium, and zirconium in the cemented carbide means the total content of all of these elements when the cemented carbide contains all of titanium, tantalum, niobium, and zirconium, and when the cemented carbide contains one or more and three or less elements selected from the group consisting of titanium, tantalum, niobium, and zirconium, it means the total content of the contained elements.

[0062] In this disclosure, the total content of titanium, tantalum, niobium, and zirconium in the cemented carbide is measured by ICP optical emission spectroscopy. In this disclosure, the measuring device used for ICP optical emission spectroscopy is "ICPS-8100" (trademark) manufactured by Shimadzu Corporation.

[0063] <Arithmetic mean diameter of second region> In the cemented carbide of embodiment 1, in a first image obtained by performing binarization processing on a backscattered electron image of a cross section of the cemented carbide, a first region consisting of a first phase and a second region consisting of a second phase and a third phase are present, and the arithmetic mean diameter d of the second region in the first image may be 0.3 μm or more and 0.9 μm or less. The backscattered electron image is obtained by photographing the cross section of the cemented carbide at 5000x magnification using a scanning electron microscope. The lower limit of the arithmetic mean diameter d of the second region may be 0.3 μm or more, 0.4 μm or more, or 0.5 μm or more from the viewpoint of improving wear resistance by suppressing particle shedding. The upper limit of the arithmetic mean diameter d of the second region may be 0.9 μm or less, 0.8 μm or less, or 0.7 μm or less from the viewpoint of improving wear resistance by suppressing uneven wear. The arithmetic mean diameter d of the second region may be 0.4 μm or more and 0.8 μm or less, or 0.5 μm or more and 0.7 μm or less.

[0064] In the present disclosure, the arithmetic mean diameter d of the second region is measured by the following procedures (A4) to (B4): (A4) Six images after binarization processing are obtained by the same method as (A1) to (C1) described in the method for measuring the content of the first phase in a cemented carbide.

[0065] (B4) A rectangular measurement field of view measuring 25.3 μm in height and 17.6 μm in width is set in each of the six binarized images obtained. Using image analysis software (ImageJ, version 1.51j8: https: / / imagej.nih.gov / ij / ), the circle-equivalent diameter (Heywood diameter: diameter of a circle equivalent to an equal area) is measured for each of the second regions in the six measurement fields. The number-based arithmetic mean value of the circle-equivalent diameters is calculated based on all the second regions in the six measurement fields. In the present disclosure, this arithmetic mean value corresponds to the arithmetic mean diameter d of the second region.

[0066] As far as the applicant has measured, it has been confirmed that, as long as measurements are made on the same sample, even if the above measurement is performed multiple times by changing the selected location of the measurement field, there is little variation in the measurement results, and that setting the measurement field arbitrarily will not be arbitrary.

[0067] <Chromium Content> The cemented carbide of embodiment 1 may contain chromium (Cr). Chromium has the effect of inhibiting grain growth of tungsten carbide particles. In the cemented carbide, the percentage of chromium mass relative to the mass of cobalt may be 0% or more and 8% or less. This effectively prevents the raw material micro-WC particles from remaining in the resulting cemented carbide, effectively suppresses the generation of coarse grains, and improves tool life. In the cemented carbide, if the percentage of chromium mass relative to the mass of cobalt exceeds 8%, the solubility limit of chromium in cobalt is exceeded, and chromium precipitates in the cemented carbide in the form of carbides, etc., which tends to deteriorate the fracture resistance of the cemented carbide.

[0068] In the cemented carbide, the upper limit of the percentage of the mass of chromium relative to the mass of cobalt may be 7% or less, or 6% or less, from the viewpoint of improving chipping resistance. In the cemented carbide, the lower limit of the percentage of the mass of chromium relative to the mass of cobalt may be 1% or more, or 2% or more, from the viewpoint of suppressing the generation of coarse grains. In the cemented carbide, the percentage of the mass of chromium relative to the mass of cobalt may be 1% or more and 7% or less, or 2% or more and 6% or less.

[0069] The chromium content of the cemented carbide is measured by ICP emission spectroscopy.

[0070] <Zirconium Content> The cemented carbide of embodiment 1 may contain zirconium (Zr). Zirconium has the effect of improving the high-temperature hardness of the cemented carbide. In the cemented carbide, the percentage of the mass of zirconium relative to the mass of cobalt may be 0% or more and 6% or less. This improves the high-temperature hardness of the cemented carbide, thereby improving the tool life. In the cemented carbide, if the percentage of the mass of zirconium relative to the mass of cobalt exceeds 6%, the solid solubility limit of zirconium in cobalt is exceeded, and zirconium precipitates in the cemented carbide in the form of carbide, etc., which tends to deteriorate the fracture resistance of the cemented carbide.

[0071] In the cemented carbide, the upper limit of the percentage of the mass of zirconium relative to the mass of cobalt may be 5% or less, or 4% or less, from the viewpoint of a balance between fracture resistance and improved high-temperature hardness. In the cemented carbide, the lower limit of the percentage of the mass of zirconium relative to the mass of cobalt may be 0.5% or more, or 1% or more, from the viewpoint of improved high-temperature hardness. In the cemented carbide, the percentage of the mass of zirconium relative to the mass of cobalt may be 0.5% or more and 5% or more, or 1% or more and 4% or less.

[0072] The zirconium content of the cemented carbide is measured by ICP emission spectroscopy.

[0073] <Composition of Cemented Carbide> The cemented carbide of embodiment 1 includes a first phase, a second phase, and a third phase. The cemented carbide of embodiment 1 may also include the first phase, the second phase, and the third phase. The cemented carbide of embodiment 1 may include other phases in addition to the first, second, and third phases, as long as the effects of the present disclosure are not impaired. Examples of other phases include chromium carbides. The cemented carbide of embodiment 1 may include impurities in addition to the first, second, and third phases, as long as the effects of the present disclosure are not impaired. Examples of impurities include iron (Fe), molybdenum (Mo), sulfur (S), manganese (Mn), magnesium (Mg), calcium (Ca), and aluminum (Al). The impurity content of the cemented carbide (when two or more elements constitute the impurities, the total concentration of these elements) may be less than 0.1% by mass. The impurity content of the cemented carbide can be measured by ICP atomic emission spectroscopy.

[0074] <Method for manufacturing cemented carbide> The cemented carbide of embodiment 1 can be manufactured by, for example, carrying out a raw material powder preparation step, a mixing step, a molding step, a sintering step, and a cooling step in the above order. Each step will be described below.

[0075] <<Raw Material Powder Preparation Step>> In the raw material powder preparation step, raw material powders of all materials constituting the cemented carbide are prepared. As raw material powders, tungsten carbide powder, which is a raw material for the first phase, cobalt (Co) powder, which is a raw material for the second phase, titanium carbide (TiC) powder, titanium nitride (TiN) powder, tantalum carbide (TaC) powder, niobium carbide (NbC) powder, and zirconium carbide (ZrC) powder, which are raw materials for the third phase, are prepared (hereinafter, these are also collectively referred to as "third phase raw material powders"). Chromium carbide (Cr 3 C 2 ) powders can be prepared. These raw material powders can be commercially available.

[0076] As the tungsten carbide powder (hereinafter also referred to as "WC powder"), a tungsten carbide powder with a uniform particle size is prepared. Specifically, a WC powder is prepared having an average particle size of 1.5 μm or more and 6.0 μm or less, and a particle size distribution in which the ratio d10 / d90 of the 10% cumulative particle size d10 on a volume basis to the 90% cumulative particle size d90 on a volume basis is 0.2 or more and 0.5 or less. In the present disclosure, the particle size of each WC particle contained in the WC powder is measured by the FSSS (Fisher Sub-Sieve Sizer) method. The measuring instrument used in the FSSS method is the "Sub-Sieve Sizer Model 95" (trademark) manufactured by Fisher Scientific. The particle size distribution of the WC powder is measured using a particle size distribution measuring device (trade name: MT3300EX) manufactured by Microtrac.

[0077] The average particle size of the cobalt powder may be 0.5 μm or more and 3.0 μm or less. The average particle size of the third phase raw material particles may be 0.5 μm or more and 4.0 μm or less. The average particle size of the chromium carbide powder may be 1.0 μm or more and 2.0 μm or less. In the present disclosure, the average particle size of these powders refers to the average particle size measured by the FSSS (Fisher Sub-Sieve Sizer) method. The average particle size is measured using a "Sub-Sieve Sizer Model 95" (trademark) manufactured by Fisher Scientific.

[0078] In the mixing step, the raw material powders prepared in the preparation step are mixed to obtain a mixed powder. The content of each raw material powder in the mixed powder is appropriately adjusted taking into consideration the content of each component of the first, second, and third phases of the cemented carbide.

[0079] The mixing method is a method that can maintain a uniform particle size of the WC powder in the mixed powder after mixing. Specifically, a ball mill is used, and the media diameter is made smaller than conventional ones, the rotation speed is reduced, and the mixing time is shortened. This makes it possible to suppress the pulverization of WC particles. The media diameter can be, for example, 5 mm or more and 10 mm or less. The rotation speed can be, for example, 15 rpm or more and 30 rpm or less. The mixing time can be, for example, 15 hours or more and 36 hours or less. If the mixing time is less than 15 hours, voids are likely to occur in the cemented carbide due to insufficient mixing.

[0080] If a mixing method with a strong crushing force (for example, an attritor) is used, even if the particle size of the raw WC powder is uniform, the WC particles as a whole will be crushed into fine particles during mixing, resulting in a fine particle size of the WC powder after mixing, and coarse particles will be generated due to grain growth during sintering. Therefore, the manufacturing method of this embodiment does not employ a mixing method with a strong crushing force.

[0081] After the mixing step, the mixed powder may be granulated as necessary. Granulating the mixed powder makes it easier to fill the mixed powder into a die or mold during the molding step described below. A known granulation method can be applied to the granulation, and for example, a commercially available granulator such as a spray dryer can be used.

[0082] <<Forming Step>> The forming step is a step of forming the mixed powder obtained in the mixing step into a predetermined shape to obtain a molded body. The forming method and forming conditions in the forming step are not particularly limited, and general methods and conditions may be used. An example of the predetermined shape is a cutting tool shape.

[0083] <Sintering Step> In the sintering step, the compact obtained in the molding step is sintered to obtain a cemented carbide. In the method for producing a cemented carbide according to the present disclosure, the sintering temperature can be set to 1380°C or higher and 1500°C or lower. This allows the grain size of WC particles in the cemented carbide to be uniform. Furthermore, the generation of fine WC particles and coarse WC particles is suppressed.

[0084] If the sintering temperature is lower than 1380°C, voids will be generated in the cemented carbide, reducing the fracture resistance of the cemented carbide.If the sintering temperature is higher than 1500°C, the WC grains will coarsen due to grain growth, resulting in non-uniform grain sizes.

[0085] Cooling Step The cooling step is a step of cooling the cemented carbide after sintering. The cooling conditions may be any general conditions and are not particularly limited.

[0086] [Embodiment 2: Cutting Tool] The cutting tool of embodiment 2 includes the cemented carbide of embodiment 1. The cutting tool of embodiment 2 can include a cutting edge made of at least the cemented carbide of embodiment 1. In the present disclosure, the cutting edge refers to the portion involved in cutting, and in the cemented carbide, refers to the cutting edge ridge and the region of the cemented carbide that is within 0.5 mm of the cutting edge ridge toward the cemented carbide.

[0087] Examples of cutting tools include cutting tools, drills, end mills, indexable cutting tips for milling, indexable cutting tips for turning, metal saws, gear cutting tools, reamers, taps, and the like.

[0088] The cemented carbide of the second embodiment may constitute the entire tool or a part of the tool. Here, "constitute a part" refers to a mode in which the cemented carbide of the second embodiment is brazed to a predetermined position of any substrate to form a cutting edge.

[0089] The cutting tool of the second embodiment may further include a hard film that covers at least a part of the surface of the substrate made of cemented carbide. Examples of the hard film include diamond-like carbon, diamond, and Al. 2 O 3Alternatively, a film made of TiCN can be used.The hard film may be a CVD film formed by chemical vapor deposition (CVD).

[0090] The present embodiment will be described in more detail with reference to examples, although the present embodiment is not limited to these examples.

[0091] <Production of cemented carbide> <Preparation step> Powders having the compositions shown in the "raw material powder" column of Table 1 were prepared as raw material powders. A number of tungsten carbide (WC) powders with different average particle sizes and particle size distributions were prepared. The average particle size and d10 / d90 of the WC powders are shown in the "average particle size (μm)" and "d10 / d90" columns of "WC" in the "raw material powder" column of Table 1, respectively.

[0092] The average particle size of the cobalt (Co) powder is 1.2 μm, and the average particle size of the chromium carbide (Cr 3 C 2 ) powder has an average particle size of 1.5 μm, titanium carbide (TiC) powder has an average particle size of 1.5 μm, titanium nitride (TiN) powder has an average particle size of 2.0 μm, tantalum carbide (TaC) powder has an average particle size of 1.0 μm, niobium carbide (NbC) powder has an average particle size of 1.1 μm, and zirconium carbide (ZrC) powder has an average particle size of 1.5 μm.

[0093] <Mixing Step> Each raw material powder was mixed in the blending amount shown in the "mass %" column of "Raw Materials" in Table 1 to prepare a mixed powder. "Mas %" in the "Raw Materials" column of Table 1 indicates the percentage of the mass of each raw material powder with respect to the total mass of the raw material powders. Mixing was performed using a ball mill. The media diameter was 8 mm. The rotation speed and mixing time for each sample are as shown in the "Rotation Speed" and "Time" columns of "Mixing" in Table 2. The obtained mixed powder was spray-dried to obtain a granulated powder.

[0094]

[0095] <<Molding Step>> The obtained granulated powder was press-molded to prepare a chip-shaped compact.

[0096] <Sintering Step> The compact was placed in a sintering furnace and sintered in vacuum at the temperature and for the time shown in the "Temperature" and "Time" columns under "Sintering" in Table 2.

[0097] <Cooling Step> After the sintering was completed, the mixture was slowly cooled in an argon (Ar) gas atmosphere to obtain a cemented carbide.

[0098]

[0099] <Evaluation of Cemented Carbide> <Composition of Cemented Carbide> For each sample of cemented carbide, the first phase content of the cemented carbide, the cobalt content of the cemented carbide, and the total content of titanium, tantalum, niobium, and zirconium of the cemented carbide were measured. Specific measurement methods are as described in embodiment 1. The results are shown in the "First Phase Content," "Co Content," and "Total Content of Ti, Ta, Zr, and Nb" columns of "Cemented Carbide" in Table 3. The term "Ti, Ta, Zr, and Nb Content" does not necessarily indicate that each sample contains all of Ti, Ta, Zr, and Nb.

[0100] <Arithmetic mean diameter a, standard deviation b, and 10% cumulative particle diameter c of tungsten carbide particles> For each sample of cemented carbide, the arithmetic mean diameter a, standard deviation b, and 10% cumulative particle diameter c of the tungsten carbide particles were measured. The specific measurement method was as described in embodiment 1. The results are shown in Table 3 under "Arithmetic mean diameter a," "Standard deviation b," and "10% cumulative particle diameter c" for "WC particles" in the "First phase."

[0101] Based on the "arithmetic mean diameter a," "standard deviation b," and "10% cumulative particle diameter c" of each sample, it was confirmed whether each sample satisfied the relationships of the following formulas I and II. b<0.49a+0.063 Formula I c>0.34a+0.098 Formula II The results are shown in the "Formula I" and "Formula II" columns of Table 3. In "Formula I," "Yes" indicates that the relationship of formula I is satisfied, and "No" indicates that the relationship of formula I is not satisfied. In "Formula II," "Yes" indicates that the relationship of formula II is satisfied, and "No" indicates that the relationship of formula II is not satisfied.

[0102] <<Composition of the Second Phase>> In all samples, the second phase was confirmed to consist of cobalt.

[0103] <<Composition of Third Phase>> In each sample, the elements contained in the third phase were identified by STEM-EDX. The specific identification method is as described in embodiment 1. The results are shown in the "Composition" column of "Third Phase" in Table 4. In all samples, it was confirmed that the third phase was composed of the elements listed in Table 4 and that the third phase did not contain tungsten carbide.

[0104] <Arithmetic mean diameter d of second region> For each sample, the arithmetic mean diameter d of the second region was measured. The specific measurement method is as described in embodiment 1. The results are shown in the "Arithmetic mean diameter d" column of "Second region" in "First image" in Table 4.

[0105]

[0106]

[0107] <Cutting Test 1> Turning was performed under the following conditions using a cutting tool (tool model number: CNMG120408N-GU (manufactured by Sumitomo Electric Hardmetal Corporation)) for each sample, and the average wear volume Vb (mm) on the flank side of the cutting tool after 15 minutes of cutting was measured. The smaller the average wear volume Vb (mm), the better the wear resistance and the longer the tool life. In Cutting Test 1, when the average wear volume Vb (mm) is 0.35 mm or less, it is judged that the wear resistance is excellent and the tool life is long. The results are shown in the "Cutting Test 1" column in Table 5.

[0108] <Cutting conditions> Workpiece: S45C Processing: External turning of round bar Cutting speed: 350 m / min Feed rate: 0.25 mm / rev Depth of cut: 2.0 mm Cutting fluid: Water-soluble cutting oil The above cutting conditions correspond to high-speed processing.

[0109] <Cutting Test 2> Twenty cutting tools (tool model number: CNMG120408N-GU (manufactured by Sumitomo Electric Hardmetal Corporation)) for each sample were prepared, and turning was performed using these under the following conditions, and the breakage rate (%) after 20 seconds of cutting was measured. A smaller breakage rate indicates better fracture resistance and a longer tool life. In Cutting Test 2, a breakage rate of 25% or less was determined to indicate a long tool life. The results are shown in the "Cutting Test 2" column in Table 5.

[0110] <Cutting conditions> Workpiece: SCM440 (grooved round bar) Processing: Intermittent turning of grooved round bar Cutting speed: 120 m / min Feed rate: 0.15 mm / rev Depth of cut: 2.0 mm Cutting fluid: None

[0111] In this example, if the average wear amount Vb is 0.35 mm or less in cutting test 1 and the breakage rate is 25% or less in cutting test 2, the tool life is determined to be long.

[0112]

[0113] <Discussion> The cemented carbides and cutting tools of Samples 1 to 22 correspond to Examples. The cemented carbides and cutting tools of Samples 101 to 112 correspond to Comparative Examples. Samples 1 to 22 had excellent wear resistance and fracture resistance, and exhibited long tool life in both Cutting Test 1 and Cutting Test 2. Samples 101, 104 to 106, 108, 109, and 112 had insufficient wear resistance and insufficient tool life in Cutting Test 1. Samples 102, 103, 107, 110, and 111 had insufficient fracture resistance and insufficient tool life in Cutting Test 2.

[0114] Although the embodiments and examples of the present disclosure have been described above, it is intended from the beginning that the configurations of the above-described embodiments and examples may be appropriately combined and modified in various ways. The embodiments and examples disclosed herein are illustrative in all respects and should not be considered limiting. The scope of the present invention is defined by the claims, not by the above-described embodiments and examples, and is intended to include meanings equivalent to the claims and all modifications within the scope of the claims.

Claims

1. A cemented carbide including a first phase, a second phase, and a third phase, wherein the first phase is composed of a plurality of tungsten carbide particles, the content of the first phase in the cemented carbide is 65% by volume or more and 85% by volume or less, the arithmetic mean diameter a of the tungsten carbide particles is 0.5 μm or more and 2.0 μm or less, the arithmetic mean diameter a and the standard deviation b of the particle diameter of the tungsten carbide particles are related by the following formula I, b<0.49a+0.063 Formula I In the formula I, the units of a and b are μm, the arithmetic mean diameter a and the 10% cumulative particle diameter c based on the number of the tungsten carbide particles are related by the following formula II, c>0.34a+0.098 Formula II In the formula II, the units of a and c are μm, the second phase is composed of cobalt, a cobalt content of the cemented carbide is 3% by mass or more and 15% by mass or less; the third phase is composed of at least one element selected from the group consisting of titanium, tantalum, niobium, zirconium, and tungsten, and at least one of carbon and nitrogen; the third phase does not contain tungsten carbide; and the total content of titanium, tantalum, niobium, and zirconium in the cemented carbide is 2% by mass or more and 8% by mass or less.

2. The cemented carbide according to claim 1, wherein in a first image obtained by performing a binarization process on a backscattered electron image of a cross section of the cemented carbide, a first region consisting of the first phase and a second region consisting of the second phase and the third phase are present, the arithmetic mean diameter d of the second region in the first image is 0.3 μm or more and 0.9 μm or less, and the backscattered electron image is obtained by photographing the cross section of the cemented carbide at 5000 times magnification using a scanning electron microscope.

3. The cemented carbide according to claim 1 or 2, wherein the arithmetic mean diameter a of the tungsten carbide particles is 0.8 μm or more and 1.6 μm or less.

4. The cemented carbide according to any one of claims 1 to 3, wherein the cobalt content of the cemented carbide is 4 mass% or more and 11 mass% or less.

5. A cutting tool comprising the cemented carbide according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Super hard alloy and cutting tool

    JP2016020541A

  • Cemented carbide

    JP2010248560A

  • Cemented carbide

    JP2010248561A

  • WC-based super hard alloy and coating cut tool using the same

    JP2020094277A

  • Cemented carbide and cutting tool

    JP2022158173A