Bonding wire

The Cu bonding wire with a Pd-Ni coating layer addresses peeling and corrosion issues by ensuring uniform composition and thickness, enhancing adhesion and reliability at the second joint in high-temperature environments.

WO2024247286A1PCT designated stage expired Publication Date: 2024-12-05NIPPON MICROMETAL CORPORATION
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2023/023777
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-30
Filing Date
2023-06-27
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Conventional Cu bonding wires with Pd coating layers experience peeling issues, leading to galvanic corrosion and inadequate bonding reliability in high-temperature environments, while bare Cu wires have poor FAB shape and bonding at the first joint.

Method used

A Cu bonding wire with a coating layer containing a high concentration of Pd and Ni, specifically designed to have a uniform thickness and composition to prevent galvanic corrosion and enhance adhesion at the second joint, ensuring good initial bonding properties and FAB shape.

Benefits of technology

The alloy-coated Cu bonding wire achieves improved adhesion and bonding reliability at the second joint, suppressing galvanic corrosion and maintaining a stable FAB shape, even in harsh high-temperature conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure 00000036_0000
    Figure 00000036_0000
Patent Text Reader

Abstract

Provided is an alloy-coated Cu bonding wire comprising: a core material made of Cu or a Cu alloy; and a coating layer formed on the surface of the core material and having a total concentration of Pd and Ni of 90 atom % or more. In the concentration profile in the depth direction of the wire measured by Auger electron spectroscopy (AES) for measurement points in the depth direction including at least 50 points in the depth direction of the coating layer, the thickness of the coating layer is 10-130 nm. The average value X of the ratio CPd / CNi of Pd concentration CPd (atomic%) and Ni concentration CNi (atomic%) for all of the measurement points in the covering layer is 0.1-35.0. The total number of measurement points in which the absolute deviation from the average value X in the coating layer is 0.3X or less is 50% or more of the total number of measurement points in the covering layer. The wire contains a first additional element at a total concentration of 5-450 mass ppm for the entirety of the wire.
Need to check novelty before this filing date? Find Prior Art

Description

Bonding Wire

[0001] The present invention relates to a bonding wire.

[0002] Bonding wires are used to connect electrodes formed on semiconductor chips to electrodes on lead frames or substrates. The bonding wire connection process is completed by first bonding to an electrode on a semiconductor chip using a cylindrical bonding tool (capillary) through which the bonding wire is passed, then forming a loop, and then second bonding of the wire portion to an external terminal such as an electrode on a lead frame or substrate. The first bonding is performed by heating and melting the tip of the wire portion (hereinafter also referred to as the "tail") extending from the capillary with arc heat input, forming a free air ball (FAB; hereinafter simply referred to as the "ball") by surface tension, and then crimping the ball portion to an electrode on the semiconductor chip (hereinafter also referred to as "ball bonding"). The second bonding is performed by crimping the wire portion to an external terminal by applying ultrasonic waves and a load from the capillary to the wire portion (hereinafter also referred to as "wedge bonding") without forming a ball.

[0003] Until now, gold (Au) has been the mainstream material for bonding wire, but copper (Cu) is increasingly being used instead, primarily for LSI applications (see, for example, Patent Documents 1 to 3). Furthermore, with the recent spread of electric and hybrid vehicles, it is expected that Cu, which has high thermal conductivity and fusing current, will be used in automotive devices and also in power devices (power semiconductor devices) for high-power equipment such as air conditioners and solar power generation systems. Cu is therefore expected to be a highly efficient and reliable alternative.

[0004] Cu has the disadvantage of being more easily oxidized than Au, and as a method of preventing the surface oxidation of Cu bonding wire, a structure in which the surface of the Cu core material is coated with a metal such as Pd has been proposed (Patent Document 4). Also, a Pd-coated Cu bonding wire has been proposed in which the surface of the Cu core material is coated with Pd and Pd and Pt are further added to the Cu core material to improve the bonding reliability of the first joint (Patent Document 5).

[0005] Japanese Patent Application Laid-Open No. 61-48543 Japanese Patent Application Laid-Open No. 2018-503743 International Publication No. 2017 / 221770 Japanese Patent Application Laid-Open No. 2005-167020 International Publication No. 2017 / 013796

[0006] In recent years, bonding wires are required to exhibit good bonding reliability in harsh high-temperature environments.

[0007] The inventors conducted an evaluation based on these recent requirements and found that with conventional Cu bonding wires having a Pd coating layer, the Pd coating layer partially peels off during the wire connection process, exposing the Cu core material, and the contact area between the coated Pd portion and the exposed Cu portion is exposed to an environment containing oxygen, water vapor, and sulfur compound-based outgassing generated from the sealing resin in a high-temperature environment, causing local corrosion of the Cu, i.e., galvanic corrosion, and insufficient bonding reliability at the second bonded portion. On the other hand, with bare Cu bonding wires that do not have a Pd coating layer, although galvanic corrosion does not occur, the FAB shape is poor and, ultimately, the bondability at the first bonded portion is insufficient.

[0008] In the process of addressing the above-mentioned issues, we confirmed that alloy-coated Cu bonding wires, in which the surface of a Cu core material is coated with an alloy containing Ni and Pd, can provide good results in terms of FAB shape and bonding reliability in high-temperature environments, depending on the composition of the alloy coating. However, we found that there is room for improvement in the adhesion between the wire and the terminal at the second joint (hereinafter simply referred to as "adhesion of the second joint"). Hereinafter, in this specification, the adhesion of the second joint and the initial bonding strength of the second joint are collectively referred to as the initial bondability of the second joint.

[0009] The present invention provides a novel alloy-coated Cu bonding wire that provides a good FAB shape, has good initial bondability of the second joint, including adhesion of the second joint, and suppresses galvanic corrosion in high-temperature environments, resulting in good bonding reliability of the second joint.

[0010] As a result of extensive research into the above problems, the present inventors have found that the above problems can be solved by providing the following configuration, and have completed the present invention.

[0011] That is, the present invention includes the following: <1> A bonding wire including a core material made of Cu or a Cu alloy and a coating layer formed on the surface of the core material, the coating layer having a total concentration of Pd and Ni of 90 atomic % or more, wherein a concentration profile in the depth direction of the wire obtained by Auger electron spectroscopy (AES) measurement at 50 or more measurement points in the coating layer in the depth direction shows that the thickness of the coating layer is 10 nm or more and 130 nm or less, and the Pd concentration C Pd (atomic %) and Ni concentration C Ni (atomic %) ratio C Pd / C Ni A bonding wire in which, when the average value of X is defined as X, the average value X is 0.1 or more and 35.0 or less, the total number of measurement points in the coating layer having an absolute deviation from the average value X within 0.3X is 50% or more of the total number of measurement points in the coating layer, and the following condition (A) is satisfied. (A) The wire contains one or more elements (hereinafter referred to as "first additional element") selected from the group consisting of Ti, V, Cr, Mn, Fe, Co, Zn, Zr, Nb, Mo, Ru, Rh, Sn, Ta, W, Os, Ir, Pt, Au, and Bi, and the total concentration of the first additional element in the entire wire is 5 mass ppm or more and 450 mass ppm or less. <2> A bonding wire including a core material made of Cu or a Cu alloy and a coating layer formed on the surface of the core material, in which the total concentration of Pd and Ni is 90 atomic % or more, wherein, in a concentration profile in the depth direction of the wire obtained by measuring by Auger electron spectroscopy (AES) so that the number of measurement points in the depth direction is 50 or more in the coating layer, the thickness of the coating layer is 10 nm or more and 130 nm or less, and the concentration C of Pd at all measurement points in the coating layer is 100 ppm or more. Pd (atomic %) and Ni concentration C Ni (atomic %) ratio C Pd / C NiA bonding wire, wherein, when the average value of X is defined as X, the average value X is 0.1 or more and 35.0 or less, the total number of measurement points in the coating layer having an absolute deviation from the average value X within 0.3X is 50% or more of the total number of measurement points in the coating layer, and the following conditions (A) and (B) are satisfied. (A) The wire contains one or more elements (hereinafter referred to as "first additive elements") selected from the group consisting of Ti, V, Cr, Mn, Fe, Co, Zn, Zr, Nb, Mo, Ru, Rh, Sn, Ta, W, Os, Ir, Pt, Au, and Bi, and the total concentration of the first additive elements in the entire wire (wherein the concentration of Au is the concentration in the core material portion) is 5 mass ppm or more and 450 mass ppm or less. (B) The wire contains Au on the surface, and the concentration of Au in the entire wire is 0.5 mass% or less. <3> The bonding wire according to <1> or <2>, wherein the total number of measurement points in the coating layer having an absolute deviation of 0.2X from the average value X is 50% or more of the total number of measurement points in the coating layer. <4> For all measurement points in the coating layer, C Pd or C Ni<5> The bonding wire according to any one of <1> to <4>, wherein, when a linear approximation is performed by the least squares method, the difference between the maximum and minimum values ​​of the approximate straight line in the depth range of the coating layer is 20 atomic % or less. <5> The bonding wire according to any one of <1> to <4>, wherein the concentration profile in the depth direction of the wire is obtained by measuring by AES under the following <conditions> while digging down in the depth direction from the surface of the wire by Ar sputtering. <Conditions> The center of the wire width is positioned to be the center of the width of the measurement surface, and the width of the measurement surface is 5% to 15% of the wire diameter, and the length of the measurement surface is 5 times the width of the measurement surface. <6> The bonding wire according to any one of <1> to <5>, wherein the bonding wire contains one or more elements selected from the group consisting of B, P, and Mg (hereinafter referred to as "second additional element"), and the total concentration of the second additional element in the entire wire is 1 ppm by mass to 100 ppm by mass. <7> The bonding wire according to any one of <1> to <6>, which contains one or more elements selected from the group consisting of Se, Te, As, and Sb (hereinafter referred to as the "third additional element"), and the total concentration of the third additional element with respect to the entire wire is 1 mass ppm to 100 mass ppm. <8> The bonding wire according to any one of <1> to <7>, which contains one or more elements selected from the group consisting of Ga and Ge (hereinafter referred to as the "fourth additional element"), and the total concentration of the fourth additional element with respect to the entire wire is 0.011 mass% to 1.5 mass%. <9> The bonding wire according to any one of <1> to <8>, which contains one or more elements selected from the group consisting of In and Ag (hereinafter referred to as the "fifth additional element"), and the total concentration of the fifth additional element with respect to the entire wire is 1 mass ppm to 500 mass ppm.

[0012] According to the present invention, a novel alloy-coated Cu bonding wire can be provided that not only provides a good FAB shape but also has good initial bondability of the second joint, including adhesion of the second joint, and suppresses galvanic corrosion in high-temperature environments, thereby providing good bonding reliability of the second joint.

[0013] Fig. 1 is a schematic diagram for explaining the second bonded portion. Fig. 1 is also a schematic diagram for explaining the position of the evaluation surface (cross section) when evaluating the adhesion of the second bonded portion. Fig. 2 is a schematic cross-sectional view of the second bonded portion when cut at the position indicated by the two-dot chain line A-A in Fig. 1. Fig. 3 is a schematic diagram for explaining the position and dimensions of the measurement surface when performing composition analysis by AES.

[0014] The present invention will be described in detail below with reference to preferred embodiments. While the description may refer to drawings, each drawing merely shows the shape, size, and arrangement of components to the extent that the invention can be understood. The present invention is not limited to the following embodiments and examples, and can be modified and implemented as desired within the scope of the claims and their equivalents.

[0015] [Bonding Wire] The bonding wire of the present invention (hereinafter also simply referred to as "the wire of the present invention" or "wire") includes a core material made of Cu or a Cu alloy, and a coating layer formed on the surface of the core material, in which the total concentration of Pd and Ni is 90 atomic % or more, and in a concentration profile in the depth direction of the wire obtained by Auger electron spectroscopy (AES) measurement at 50 or more measurement points in the coating layer in the depth direction, the thickness of the coating layer is 10 nm or more and 130 nm or less, and the Pd concentration C Pd (atomic %) and Ni concentration C Ni (atomic %) ratio C Pd / C Ni The wire is characterized in that, when the average value of the above is X, the average value X is 0.1 or more and 35.0 or less, the total number of measurement points in the coating layer having an absolute deviation from the average value X within 0.3X is 50% or more of the total number of measurement points in the coating layer, and the wire satisfies the following condition (A): (A) The wire contains one or more elements ("first additional element") selected from the group consisting of Ti, V, Cr, Mn, Fe, Co, Zn, Zr, Nb, Mo, Ru, Rh, Sn, Ta, W, Os, Ir, Pt, Au, and Bi, and the total concentration of the first additional element in the entire wire is 5 ppm by mass or more and 450 ppm by mass or less.

[0016] As mentioned above, in recent years, bonding wires have been required to exhibit good bonding reliability in harsh high-temperature environments. For example, bonding wires used in automotive devices are required to have bonding reliability in high-temperature environments exceeding 150 ° C. The present inventors conducted an evaluation based on the characteristics required in recent years and found that conventional Cu bonding wires having a Pd coating layer may experience galvanic corrosion in high-temperature environments, resulting in insufficient bonding reliability at the second bond. Furthermore, with bare Cu bonding wires that do not have a Pd coating layer, although galvanic corrosion does not occur, the FAB shape is poor, and the crimp shape of the first bond is therefore inferior, making them inadequate for the narrow-pitch connections required for high-density mounting.

[0017] In contrast, a wire comprising a core material made of Cu or a Cu alloy and a coating layer formed on the surface of the core material in which the total concentration of Pd and Ni is 90 atomic % or more, and in a concentration profile in the depth direction of the wire obtained by AES measurement at 50 or more measurement points in the coating layer, the thickness of the coating layer is 10 nm or more and 130 nm or less, and the Pd concentration C Pd (atomic %) and Ni concentration C Ni (atomic %) ratio C Pd / C Ni When the average value of X is taken as X, the average value X is 0.1 or more and 35.0 or less, and the total number of measurement points in the coating layer where the absolute deviation from the average value X is within 0.3X is 50% or more of the total number of measurement points in the coating layer. The inventors have found that an alloy-coated Cu bonding wire can provide a good FAB shape and suppress galvanic corrosion in a high-temperature environment, thereby providing good bonding reliability of the second joint.

[0018] On the other hand, with regard to such alloy-coated Cu bonding wire, it was found that there is room for improvement in the initial bondability of the second bond, particularly the adhesion of the second bond, as described below. As mentioned above, in the second bond, ultrasonic waves and a load are applied to the wire portion from the capillary to crimp the wire onto the external terminal. FIG. 1 shows a schematic diagram of a second bond formed on an external terminal (not shown) viewed from directly above in a direction perpendicular to the main surface of the external terminal. In FIG. 1, a second bond 10 is formed at the tip of wire 1. While it is desirable for the wire and the external terminal to be sufficiently closely attached at the second bond, it was confirmed that with regard to the second bond formed using the above-mentioned alloy-coated Cu bonding wire, there are a certain proportion of areas where the wire and the external terminal are not in close contact, resulting in poor adhesion between the wire and the terminal. FIG. 2 shows a schematic cross-sectional view of the second bond when cut in a direction perpendicular to the main surface of the external terminal at the position indicated by the two-dot chain line A-A in FIG. 1. 2, a second bond 10 is formed on an external terminal 50, and the inventors have found that, with respect to the second bond formed using the above-mentioned alloy-coated Cu bonding wire, there tends to be a portion where the wire and the external terminal are not in close contact within a certain width from the ends of the second bond (the left and right ends of the second bond 10 in FIG. 2). This problem of adhesion at the second bond has not been apparent, at least in conventional bonding wires including bare Cu bonding wires, and is therefore considered to be a specific issue arising from the adoption of the above-mentioned specific alloy coating.

[0019] In contrast, the inventors have discovered that by using the above-mentioned specific alloy coating and a bonding wire that satisfies the above-mentioned condition (A), the excellent effects achieved by using the specific alloy coating can be maintained, while improving the adhesion of the second joint and achieving good initial bondability of the second joint.

[0020] <Core Material Made of Cu or Cu Alloy> The wire of the present invention includes a core material made of Cu or a Cu alloy (hereinafter, also simply referred to as "Cu core material").

[0021] The Cu core material is not particularly limited as long as it is made of Cu or a Cu alloy, and a known Cu core material that constitutes a conventional Pd-coated Cu wire known as a bonding wire may be used.

[0022] In the present invention, the concentration of Cu in the Cu core material can be, for example, 97 atomic % or more, 97.5 atomic % or more, 98 atomic % or more, 98.5 atomic % or more, 99 atomic % or more, 99.5 atomic % or more, 99.8 atomic % or more, 99.9 atomic % or more, or 99.95 atomic % or more at the center (axial core portion) of the Cu core material.

[0023] From the viewpoint of realizing an alloy-coated Cu bonding wire that improves the adhesion of the second joint and provides good initial bonding of the second joint, it is preferable that the Cu core material contains the first additive element so as to satisfy the above condition (A).

[0024] The Cu core material may also contain, for example, one or more dopants selected from the second, third, fourth, and fifth additional elements described below. The preferred contents of these dopants are as described below.

[0025] In one embodiment, the Cu core material is composed of Cu, a first additional element, and inevitable impurities. In another embodiment, the Cu core material is composed of Cu, a first additional element, one or more elements selected from a second additional element, a third additional element, a fourth additional element, and a fifth additional element described below, and inevitable impurities. The Cu core material may contain elements that constitute the coating layer described below.

[0026] <Coating Layer> The wire of the present invention includes a coating layer (hereinafter simply referred to as "coating layer") formed on the surface of a Cu core material, the coating layer having a total concentration of Pd and Ni of 90 atomic % or more.

[0027] In order to provide a good FAB shape and to suppress galvanic corrosion in a high-temperature environment and provide good bonding reliability at the second bonded portion, it is important that the coating layer of the wire of the present invention satisfies all of the following conditions (1) to (3) in the concentration profile in the depth direction of the wire obtained by AES measurement so that the number of measurement points in the coating layer in the depth direction is 50 or more (hereinafter simply referred to as the "concentration profile in the depth direction of the wire"). (1) The thickness of the coating layer is 10 nm or more and 130 nm or less. (2) The concentration C of Pd at all measurement points in the coating layer is Pd (atomic %) and Ni concentration C Ni (atomic %) ratio C Pd / C Ni (3) The total number of measurement points in the coating layer whose absolute deviation from the average value X is within 0.3X is 50% or more of the total number of measurement points in the coating layer.

[0028] In the present invention, when obtaining a concentration profile in the depth direction of the wire by AES, the measurement is performed so that the number of measurement points in the depth direction is 50 or more in the coating layer. Generally, depth analysis by AES can be performed at measurement intervals on the sub-nano order, so it is relatively easy to achieve 50 or more measurement points in relation to the thickness of the coating layer targeted by the present invention. If the number of measurement points is less than 50 as a result of the measurement, the measurement is performed again by reducing the sputtering rate or shortening the sputtering time, etc., so that the number of measurement points is 50 or more. This allows AES to measure 50 or more depth points in the coating layer, thereby obtaining a concentration profile in the depth direction of the wire. Although it depends on the thickness of the coating layer, it is more preferable to determine the AES measurement point interval so that the total number of measurement points in the coating layer is 70 (more preferably 100). Therefore, in a preferred embodiment, the coating layer of the wire of the present invention satisfies all of the above conditions (1) to (3) in the concentration profile in the depth direction of the wire obtained by measuring the coating layer by AES at 50 or more measurement points in the depth direction.

[0029] Condition (1) Condition (1) relates to the thickness of the coating layer. By including a coating layer that satisfies condition (1) in combination with conditions (2) and (3), the wire of the present invention can suppress galvanic corrosion in a high-temperature environment, thereby providing good bonding reliability at the second bonded portion, as well as a good FAB shape and, ultimately, a good crimped shape at the first bonded portion.

[0030] Regarding condition (1), the thickness of the coating layer (a calculation method based on the concentration profile in the depth direction of the wire will be described later) is 10 nm or more, preferably 12 nm or more, 14 nm or more, 15 nm or more, 16 nm or more, 18 nm or more, or 20 nm or more, more preferably 25 nm or more, 30 nm or more, 40 nm or more, or 50 nm or more, and even more preferably 60 nm or more, 70 nm or more, 80 nm or more, or 90 nm or more, from the viewpoint of realizing a good FAB shape. If the thickness of the coating layer is less than 10 nm, eccentricity occurs during FAB formation, deteriorating the FAB shape and the compression shape of the first bonded portion tends to deteriorate. Furthermore, the upper limit of the thickness of the coating layer is 130 nm or less, preferably 125 nm or less, 120 nm or less, 115 nm or less, or 110 nm or less, from the viewpoint of realizing a good FAB shape. If the thickness of the coating layer exceeds 130 nm, deformation or poor melting occurs during FAB formation, which tends to deteriorate the FAB shape and the compression bonded shape of the first bonded portion.

[0031] Condition (2) Condition (2) is the Pd concentration C Pd (atomic %) and Ni concentration C Ni (atomic %) ratio C Pd / C Ni By including a coating layer that satisfies condition (2) in addition to conditions (1) and (3), the wire of the present invention can suppress galvanic corrosion in a high-temperature environment, provide good bonding reliability at the second bonded portion, and also provide a good FAB shape, which in turn can provide a good crimped shape at the first bonded portion.

[0032] Regarding the condition (2), from the viewpoint of realizing good joining reliability of the second joint, the average value X is 35.0 or less, preferably 34.0 or less, more preferably 32.0 or less, 30.0 or less, 28.0 or less, 26.0 or less, 25.0 or less, 24.0 or less, 22.0 or less, or 20.0 or less. Pd / C Ni If X is more than 35.0, galvanic corrosion in a high-temperature environment cannot be suppressed, and sufficient high-temperature bonding reliability tends to be difficult to obtain at the second joint. From the viewpoint of increasing the initial bonding strength of the second joint and realizing good initial bonding properties at the second joint, the lower limit of the average value X is 0.1 or more, preferably 0.2 or more, 0.4 or more, 0.5 or more, 0.6 or more, 0.8 or more, 1.0 or more, or more than 1.0, and more preferably 1.5 or more, 2.0 or more, 2.5 or more, or 3.0 or more. If X is less than 0.1, sufficient initial bonding properties at the second joint tend to be difficult to obtain.

[0033] Condition (3) Condition (3) relates to the total number of measurement points in the coating layer having an absolute deviation of 0.3X or less from the average value X being 50% or more of the total number of measurement points in the coating layer. By including a coating layer that satisfies condition (3) in combination with conditions (1) and (2), the wire of the present invention can suppress galvanic corrosion in a high-temperature environment, thereby providing good bonding reliability at the second joint, and can also provide a good FAB shape and, ultimately, a good crimp shape at the first joint.

[0034] Condition (3), together with condition (2), indicates that the coating layer contains a PdNi alloy containing Pd and Ni in a predetermined ratio in a high concentration in the thickness direction of the coating layer while suppressing fluctuations in the Pd / Ni ratio. From the viewpoint of realizing better bonding reliability of the second bonded portion in a high-temperature environment and realizing a better FAB shape, it is more preferable that the total number of measurement points in the coating layer whose absolute deviation from the average value X is within 0.2X (more preferably within 0.18X, 0.16X, or 0.15X) is 50% or more of the total number of measurement points in the coating layer.

[0035] From the viewpoint of realizing better bonding reliability of the second bonded portion in a high-temperature environment and from the viewpoint of realizing a better FAB shape, the total number of measurement points in the coating layer whose absolute deviation from the average value X is within a predetermined range (the preferred range is as described above) is preferably 55% or more or 60% or more, more preferably 65% ​​or more, 70% or more or 75% or more, and even more preferably 80% or more, of the total number of measurement points in the coating layer.

[0036] From the viewpoint of further enjoying the effects of the present invention, in the concentration profile in the depth direction of the wire, the Pd concentration C Pd (atomic %) or Ni concentration C Ni When the average value X is less than 1, the difference between the maximum and minimum values ​​of the approximate line in the depth (thickness) range of the coating layer is preferably 20 atomic % or less, more preferably 15 atomic % or less, and even more preferably 10 atomic % or less, 8 atomic % or less, 6 atomic % or less, or 5 atomic % or less. Ni When the average value X of the coating layer is 1 or more, it is preferable that the difference between the maximum and minimum values ​​of the approximate line in the depth range of the coating layer is within the above range when the average value X of the coating layer is 1 or more. Pd When the atomic percentage (atomic %) is linearly approximated by the least squares method, it is preferable that the difference between the maximum and minimum values ​​of the approximate line within the depth range of the coating layer is within the above range.

[0037] The thickness of the coating layer under condition (1), the average value X and absolute deviation from the average value X under conditions (2) and (3), the total number of measurement points where the absolute deviation falls within a predetermined range, and the ratio of the total number of measurement points where the absolute deviation falls within a predetermined range to the total number of measurement points of the coating layer can be confirmed and determined by performing composition analysis using AES while digging from the surface of the wire in the depth direction (toward the center of the wire) using Ar sputtering. In detail, 1) after performing composition analysis of the wire surface, 2) sputtering with Ar and 3) composition analysis of the surface after sputtering are repeated to obtain concentration changes of each element in the depth direction (center) from the surface of the wire (so-called depth concentration profile), and confirmation and determination can be made based on this concentration profile. In the present invention, when obtaining the depth concentration profile, the unit of depth is SiO 2 It was converted.

[0038] When performing 1) compositional analysis of the wire surface and 3) compositional analysis of the surface after sputtering, the position and dimensions of the measurement surface are determined as follows. Note that, hereinafter, the width of the measurement surface refers to the dimension of the measurement surface in the direction perpendicular to the wire axis (wire thickness direction), and the length of the measurement surface refers to the dimension of the measurement surface in the wire axis direction (wire length direction). Further explanation will be given with reference to Figure 3. Figure 3 is a schematic plan view of a wire 1, in which the wire axis direction (wire length direction) corresponds to the vertical direction (up and down direction) in Figure 3, and the direction perpendicular to the wire axis (wire thickness direction) corresponds to the horizontal direction (left and right direction) in Figure 3. Figure 3 shows a measurement surface 2 in relation to the wire 1, and the width of the measurement surface 2 is the dimension w of the measurement surface in the direction perpendicular to the wire axis. a and the length of the measuring surface 2 is the dimension l of the measuring surface in the direction of the wire axis. a is.

[0039] The wire is positioned so that the center of its width in the direction perpendicular to the wire axis is the center of the width of the measurement surface, and the measurement surface is determined so that the width of the measurement surface is 5% to 15% of the wire diameter. The length of the measurement surface is set to be 5 times the width of the measurement surface. In Figure 3, the width of the wire is indicated by the symbol W, and the center of the wire width is indicated by the dashed line X. Therefore, the measurement surface 2 is positioned so that the center of its width coincides with the dashed line X, which is the center of the wire width, and the width w of the measurement surface is set to be 5 times the width of the measurement surface. a is determined to be 5% to 15% of the wire diameter (same value as the wire width W), that is, 0.05W to 0.15W. a Is, l a =5w a By determining the position and dimensions of the measurement surface as described above, it is possible to accurately measure the success or failure of conditions (1) to (3), which are suitable for providing good bonding reliability at the second bonded portion in a high-temperature environment and realizing a good FAB shape. It is also preferable to measure multiple locations (n≧3) of the measurement surface spaced 1 mm or more apart from each other in the wire axial direction and use the arithmetic average value.

[0040] The thickness of the coating layer under the above condition (1), the average value X and the absolute deviation from the average value X under the conditions (2) and (3), the total number of measurement points where the absolute deviation falls within a predetermined range, and the proportion of the total number of measurement points where the absolute deviation falls within a predetermined range to the total number of measurement points of the coating layer are based on the results of measurements under the conditions described in the section [Analysis of coating layer thickness by Auger electron spectroscopy (AES)] below.

[0041] The trend of the concentration profile in the depth direction obtained for the wire of one embodiment of the present invention will be described below. From the surface of the wire to a certain depth position, Pd and Ni tend to coexist at a high concentration in a constant ratio, i.e., there is a region (coating layer) where the total concentration of Pd and Ni is 90 atomic % or more, and the Pd concentration C Pd (atomic %) and Ni concentration C Ni (atomic %) ratio C Pd / C NiWhen the average value of the Pd concentration C is taken as X, there tends to be a certain number of measurement points whose absolute deviation from the average value X is within 0.3X. Further in the depth direction, the concentrations of Pd and Ni tend to decrease and the concentration of Cu tends to increase. In such a concentration profile in the depth direction, the Pd concentration C Pd (atomic %) and Ni concentration C Ni Focusing on the ratio C (atomic %), the thickness of the coating layer and the total number of measurement points of the coating layer can be calculated from the thickness of the region where the total concentration of Pd and Ni is 90 atomic % or more and the total number of measurement points. Pd / C Ni The average value X can be determined by arithmetically averaging the values, and the total number of measurement points whose absolute deviation from the average value X is within 0.3X can be determined by checking the absolute deviation from the average value X for all measurement points on the coating layer. As will be described later, when Au is further contained on the surface of the wire, the concentration profile in the depth direction tends to show a decrease in the Au concentration and an increase in the Pd and Ni concentrations from the surface of the wire to a very shallow position. In such a case, the Pd concentration C Pd (atomic %) and Ni concentration C Ni Focusing on the ratio (atomic %), the thickness of the coating layer and the total number of measurement points of the coating layer can be calculated from the thickness of the region where the total is 90 atomic % or more and the total number of measurement points. Pd / C Ni The average value X can be obtained by arithmetically averaging the values, and the total number of measurement points whose absolute deviation from the average value X is within 0.3X can be obtained by checking the absolute deviation from the average value X for all measurement points on the coating layer.

[0042] Other Preferred Conditions for the Coating Layer In the wire of the present invention, the coating layer more preferably satisfies one or both of the following conditions (4) and (5) based on the concentration profile in the depth direction of the wire, in addition to satisfying all of the above conditions (1) to (3): (4) The Pd concentration C Pd The average value of (atomic %) is X Pd When the average value X of the coating layer is Pd Absolute deviation from 0.1X PdThe total number of measurement points within the range is 50% or more of the total number of measurement points in the coating layer. (5) Ni concentration C for all measurement points in the coating layer Ni The average value of (atomic %) is X Ni When the average value X of the coating layer is Ni Absolute deviation from 0.1X Ni The total number of measurement points within the range is 50% or more of the total number of measurement points in the coating layer. Note that in conditions (4) and (5), the coating layer, its thickness, and the total number of measurement points are as described above in relation to conditions (1) to (3). When the wire of the present invention includes a coating layer that satisfies one or both of conditions (4) and (5) in addition to conditions (1) to (3), the wire of the present invention can achieve particularly good bonding reliability of the second bonded portion in a high-temperature environment and a particularly good FAB shape.

[0043] The coating layer may contain, for example, one or more dopants selected from the second additional element, the third additional element, the fourth additional element, and the fifth additional element described below. The preferred contents of these dopants are as described below.

[0044] The wire of the present invention may further contain Au on its surface. By further containing Au on the surface of the wire, the initial bondability of the second bonded portion can be further improved. When the wire of the present invention further contains Au on its surface, the concentration of Au relative to the entire wire may usually be 0.5 mass% or less, preferably 0.3 mass% or less or 0.2 mass% or less, and the lower limit may be, for example, 0.05 mass% or more, 0.1 mass% or more, etc. Therefore, in one embodiment, the wire of the present invention satisfies the following condition (B): (B) The wire surface contains Au, and the concentration of Au relative to the entire wire is 0.5 mass% or less.

[0045] In addition, when the wire of the present invention further contains Au on its surface, in determining whether the above condition (A) is met, the concentration of Au as the first additional element is the concentration in the core portion obtained by exposing the cross section of the wire and measuring the Cu core portion using an electron probe microanalyzer (EPMA) or secondary ion mass spectrometry (SIMS). In other words, when the wire of the present invention further contains Au on its surface, the "total concentration of the first additional element in the entire wire" in the above condition (A) is read as "total concentration of the first additional element in the entire wire (however, the concentration of Au is the concentration in the core portion)."

[0046] In one embodiment, the wire of the present invention includes a coating layer that satisfies the above conditions (1) to (3) and also satisfies the following conditions (A) and (B): (A) The wire includes one or more elements ("first additional elements") selected from the group consisting of Ti, V, Cr, Mn, Fe, Co, Zn, Zr, Nb, Mo, Ru, Rh, Sn, Ta, W, Os, Ir, Pt, Au, and Bi, and the total concentration of the first additional elements in the entire wire (wherein the concentration of Au is the concentration in the core material) is 5 ppm by mass or more and 450 ppm by mass or less; and (B) The wire surface contains Au, and the concentration of Au in the entire wire is 0.5% by mass or less.

[0047] According to the alloy-coated Cu bonding wire of the present invention containing the first additive element at the above-mentioned specific concentration, even if the Au concentration on the surface of the wire is low, for example, less than 10 atomic %, 8 atomic % or less, 6 atomic % or less, 5 atomic % or less, 4 atomic % or less, or 2 atomic % or less, the adhesion of the second bond can be improved and good initial bondability of the second bond can be achieved.

[0048] The composition analysis of the wire surface can be performed under the same conditions as those of 1) the composition analysis of the wire surface, which was explained in relation to the method for obtaining a concentration profile in the depth direction. That is, when performing composition analysis of the wire surface by Auger electron spectroscopy (AES), the position and dimensions of the measurement surface are determined as follows.

[0049] The wire is positioned so that the center of the wire width in the direction perpendicular to the wire axis is the center of the width of the measurement surface, and the measurement surface is determined so that the width of the measurement surface is 5% to 15% of the wire diameter. The length of the measurement surface is set to be 5 times the width of the measurement surface. By determining the position and dimensions of the measurement surface as described above, the Au concentration on the wire surface can be accurately measured, which is suitable for further improving the initial bondability of the second bond. In addition, it is preferable to perform measurements on multiple locations (n≧3) of measurement surfaces spaced 1 mm or more apart from each other in the wire axis direction and use the arithmetic average value.

[0050] The above-mentioned concentration of Au on the surface is based on the results of measurements performed under the conditions described in the section "Analysis of Wire Surface Composition by Auger Electron Spectroscopy (AES)" below.

[0051] In the wire of the present invention, the boundary between the Cu core material and the coating layer is determined based on the total concentration of Pd and Ni in the concentration profile in the depth direction of the wire. The position where the total concentration of Pd and Ni is 90 atomic % is determined as the boundary, and the region where the total concentration of Pd and Ni is less than 90 atomic % is the Cu core material, and the region where the total concentration of Pd and Ni is 90 atomic % or more is the coating layer. In the present invention, the boundary between the Cu core material and the coating layer does not necessarily have to be a grain boundary. The thickness of the coating layer can be determined by checking the concentration profile from the wire surface toward the wire center, and is calculated as the distance from depth position Z1 where the total concentration of Pd and Ni first reaches 90 atomic % or more to depth position Z2 where the total concentration of Pd and Ni first drops below 90 atomic % (where Z2 > Z1).

[0052] The wire of the present invention is characterized by including a coating layer that satisfies the above conditions (1) to (3). The average value X and absolute deviation from the average value X, the total number of measurement points where the absolute deviation is within a predetermined range, and the ratio of the total number of measurement points where the absolute deviation is within a predetermined range to the total number of measurement points in the coating layer are determined by the above boundary determination method, and the Pd concentration C Pd (atomic %) and Ni concentration C Ni The content is determined by taking into consideration the atomic percentage.

[0053] In one embodiment, the coating layer is made of Pd and Ni; and unavoidable impurities. In another embodiment, the coating layer is made of Pd and Ni; one or more elements selected from Au and the first additional element; and unavoidable impurities. In another embodiment, the coating layer is made of Pd and Ni; one or more elements selected from the second additional element, the third additional element, the fourth additional element, and the fifth additional element described below; and unavoidable impurities. In another embodiment, the coating layer is made of Pd and Ni; one or more elements selected from Au and the first additional element; one or more elements selected from the second additional element, the third additional element, the fourth additional element, and the fifth additional element described below; and unavoidable impurities. The coating layer may contain the elements that constitute the Cu core material described above.

[0054] The wire of the present invention is characterized by satisfying the following condition (A): (A) The wire contains one or more elements ("first additional elements") selected from the group consisting of Ti, V, Cr, Mn, Fe, Co, Zn, Zr, Nb, Mo, Ru, Rh, Sn, Ta, W, Os, Ir, Pt, Au, and Bi, and the total concentration of the first additional elements in the entire wire is 5 ppm by mass or more and 450 ppm by mass or less.

[0055] By including a coating layer that satisfies all of the above conditions (1) to (3) and also by satisfying the above conditions related to the first additive element, the wire of the present invention can provide a good FAB shape and good bonding reliability of the second joint in a high-temperature environment, and can also improve the adhesion of the second joint to achieve good initial bondability of the second joint.

[0056] Condition (A) relates to the total concentration of one or more elements selected from the group consisting of Ti, V, Cr, Mn, Fe, Co, Zn, Zr, Nb, Mo, Ru, Rh, Sn, Ta, W, Os, Ir, Pt, Au, and Bi, i.e., the first additional element, relative to the entire wire. Here, as described above, when the wire of the present invention further contains Au on its surface, the "total concentration of the first additional element relative to the entire wire" in condition (A) should be read as "the total concentration of the first additional element relative to the entire wire (however, the concentration of Au is the concentration in the core material portion)."

[0057] Regarding condition (A), from the viewpoint of realizing an alloy-coated Cu bonding wire that improves the adhesion of the 2nd bond and provides good initial bondability of the 2nd bond, the total concentration of the first additive element relative to the entire wire is 5 mass ppm or more, preferably 10 mass ppm or more, 15 mass ppm or more, 20 mass ppm or more, or 25 mass ppm or more, more preferably 30 mass ppm or more, 40 mass ppm or more, 50 mass ppm or more, 60 mass ppm or more, or 80 mass ppm or more, and even more preferably 100 mass ppm or more, 110 mass ppm or more, 120 mass ppm or more, 130 mass ppm or more, 140 mass ppm or more, or 150 mass ppm or more. In particular, when the total concentration of the first additive element relative to the entire wire is 100 mass ppm or more, it is preferable because it is easy to realize a bonding wire that improves the adhesion of the 2nd bond and provides even better initial bondability of the 2nd bond.

[0058] Regarding condition (A), from the viewpoint of realizing an alloy-coated Cu bonding wire that improves the adhesion of the second bond and provides good initial bondability of the second bond, the total concentration of the first additional element is 450 mass ppm or less with respect to the entire wire. The upper limit of the total concentration of the first additional element may be 440 mass ppm or less, 420 mass ppm or less, 400 mass ppm or less, etc. In addition, when the first additional element includes one or more elements selected from the group consisting of Ti, V, Cr, Mn, Fe, Co, and Zn (hereinafter also referred to as "1a additional element"), the upper limit of the total concentration of the 1a additional element may be 200 mass ppm or less, 180 mass ppm or less, 160 mass ppm or less, or 150 mass ppm or less. When the first additional element contains one or more elements selected from the group consisting of Zr, Nb, Mo, Ru, Rh, and Sn (hereinafter also referred to as "1b additional element"), the upper limit of the total concentration of the 1b additional element may be 350 ppm by mass or less, 340 ppm by mass or less, 320 ppm by mass or less, or 300 ppm by mass or less.

[0059] In the wire of the present invention, from the viewpoint of improving the adhesion of the second joint and realizing a bonding wire that exhibits even better initial bonding properties of the second joint, it is preferable that the first additive element be contained in the Cu core material.

[0060] The wire of the present invention may further contain one or more elements ("second additive elements") selected from the group consisting of B, P, and Mg. When the wire of the present invention contains the second additive element, the total concentration of the second additive element relative to the entire wire is preferably 1 mass ppm or more. This makes it possible to realize a bonding wire that provides a better crimped shape of the first bonded portion. The total concentration of the second additive element relative to the entire wire is more preferably 2 mass ppm or more, and even more preferably 3 mass ppm or more, 5 mass ppm or more, 8 mass ppm or more, 10 mass ppm or more, 15 mass ppm or more, or 20 mass ppm or more. From the viewpoint of suppressing hardening of the wire and reducing chip damage during the first bonding, the total concentration of the second additive element is preferably 100 mass ppm or less, more preferably 90 mass ppm or less, 80 mass ppm or less, 70 mass ppm or less, 60 mass ppm or less, or 50 mass ppm or less. Therefore, in a preferred embodiment, the wire of the present invention contains a second additional element, and the total concentration of the second additional element in the entire wire is 1 mass ppm or more and 100 mass ppm or less.

[0061] When the wire of the present invention contains the second additive element, the second additive element may be contained in either the Cu core material or the coating layer, or may be contained in both. From the viewpoint of realizing a bonding wire that provides a better crimped shape of the first bonded portion, it is preferable that the second additive element be contained in the Cu core material.

[0062] The wire of the present invention may further contain one or more elements ("third additive elements") selected from the group consisting of Se, Te, As, and Sb. When the wire of the present invention contains the third additive element, the total concentration of the third additive element relative to the entire wire is preferably 1 ppm by mass or more. This can improve the bonding reliability of the first bonded portion in a high-temperature, high-humidity environment. The total concentration of the third additive element relative to the entire wire is more preferably 2 ppm by mass or more, and even more preferably 3 ppm by mass or more, 5 ppm by mass or more, 8 ppm by mass or more, 10 ppm by mass or more, 15 ppm by mass or more, or 20 ppm by mass or more. From the viewpoint of realizing a good FAB shape and a good crimped shape of the first bonded portion, the total concentration of the third additive element is preferably 100 ppm by mass or less, and more preferably 90 ppm by mass or less, 80 ppm by mass or less, 70 ppm by mass or less, 60 ppm by mass or less, or 50 ppm by mass or less. Therefore, in a preferred embodiment, the wire of the present invention contains a third additional element, and the total concentration of the third additional element in the entire wire is 1 mass ppm or more and 100 mass ppm or less.

[0063] When the wire of the present invention contains a third additive element, the third additive element may be contained in either the Cu core material or the coating layer, or may be contained in both. From the viewpoint of realizing a bonding wire that provides even better bonding reliability of the first bonded portion under high-temperature and high-humidity environments, it is preferable that the third additive element be contained in the coating layer.

[0064] The wire of the present invention may further contain one or more elements selected from the group consisting of Ga and Ge ("fourth additional element"). When the wire of the present invention contains the fourth additional element, the total concentration of the fourth additional element relative to the entire wire is preferably 0.011 mass% or more. This can improve the bonding reliability of the first bonded portion in high-temperature environments. The total concentration of the fourth additional element relative to the entire wire is more preferably 0.015 mass% or more, and even more preferably 0.02 mass% or more, 0.025 mass% or more, 0.03 mass% or more, 0.031 mass% or more, 0.035 mass% or more, 0.04 mass% or more, 0.05 mass% or more, 0.07 mass% or more, 0.09 mass% or more, 0.1 mass% or more, 0.12 mass% or more, 0.14 mass% or more, 0.15 mass% or more, or 0.2 mass% or more. From the viewpoint of realizing a good FAB shape, a good crimped shape of the first bonded portion, and good initial bondability of the second bonded portion, the total concentration of the fourth additional element is preferably 1.5 mass% or less, and more preferably 1.4 mass% or less, 1.3 mass% or less, or 1.2 mass% or less. Therefore, in a preferred embodiment, the wire of the present invention contains the fourth additional element, and the total concentration of the fourth additional element with respect to the entire wire is 0.011 mass% or more and 1.5 mass% or less.

[0065] When the wire of the present invention contains a fourth additional element, the fourth additional element may be contained in either the Cu core material or the coating layer, or may be contained in both.

[0066] The wire of the present invention may further contain one or more elements selected from the group consisting of In and Ag ("fifth additional element"). When the wire of the present invention contains the fifth additional element, the total concentration of the fifth additional element in the entire wire is preferably 1 mass ppm or more. This can provide good bonding reliability of the second bonded portion even in a harsher high-temperature environment (e.g., 200°C). The total concentration of the fifth additional element in the entire wire is preferably 2 mass ppm or more, 3 mass ppm or more, 4 mass ppm or more, or 5 mass ppm or more, more preferably 6 mass ppm or more, 8 mass ppm or more, or 10 mass ppm or more, even more preferably 20 mass ppm or more, 30 mass ppm or more, or 40 mass ppm or more, and even more preferably 50 mass ppm or more, 60 mass ppm or more, or 70 mass ppm or more. The upper limit of the concentration of the fifth additional element in the entire wire may be set to, for example, 500 ppm by mass or less, 480 ppm by mass or less, 460 ppm by mass or less, 450 ppm by mass or less, taking into consideration costs, etc. Therefore, in a preferred embodiment, the wire of the present invention contains the fifth additional element, and the total concentration of the fifth additional element in the entire wire is 1 ppm by mass or more and 500 ppm by mass or less.

[0067] When the wire of the present invention contains a fifth additive element, the fifth additive element may be contained in either the Cu core material or the coating layer, or may be contained in both. From the viewpoint of realizing a bonding wire that exhibits good bonding reliability of the second bond in a harsh high-temperature environment, it is preferable that the fifth additive element be contained in the Cu core material.

[0068] The contents of the first additional element, the second additional element, the third additional element, the fourth additional element, and the fifth additional element in the wire can be measured by the method described later in [Measurement of element contents].

[0069] In the wire of the present invention, the total concentration of Cu, Ni, and Pd can be, for example, 98.5 mass % or more, 98.6 mass % or more, 98.7 mass % or more, or 98.8 mass % or more.

[0070] The diameter of the wire of the present invention is not particularly limited and may be determined appropriately depending on the specific purpose, but is preferably 13 μm or more, 15 μm or more, 18 μm or more, 20 μm or more, etc. The upper limit of the diameter is not particularly limited and may be, for example, 80 μm or less, 70 μm or less, or 50 μm or less.

[0071] The wire of the present invention provides a good FAB shape, has good initial bondability at the second bond, including adhesion at the second bond, and can suppress galvanic corrosion in high-temperature environments, resulting in good bonding reliability at the second bond. Therefore, the bonding wire of the present invention can be suitably used to connect electrodes on a semiconductor chip to external terminals such as electrodes on a lead frame or substrate.

[0072] <Method for Manufacturing Wire> An example of a method for manufacturing the bonding wire of the present invention will be described.

[0073] The raw copper used has a purity of 4N (99.99% by mass or higher) or higher, and an ingot containing each dopant is obtained by the method described below.

[0074] Methods for adding dopants such as the first additional element and, if added, the second, third, fourth, and fifth additional elements include, for example, incorporating them into the Cu core material, incorporating them into the coating layer, depositing them on the surface of the Cu core material, depositing them on the surface of the coating layer, and combinations of these methods, and these methods can be selected appropriately. In the method of incorporating a dopant into the Cu core material, the dopant component may be directly added to Cu, or a mother alloy containing a few percent of the dopant component may be used. In the method of incorporating a dopant into the coating layer, the dopant may be incorporated into a Pd or Ni plating bath (in the case of wet plating) or a target material (in the case of dry plating) when forming the coating layer. In the method of depositing on the surface of a Cu core material or on the surface of a coating layer, the surface of the Cu core material or the surface of the coating layer can be used as the deposition surface, and one or more deposition processes selected from (1) application of an aqueous solution ⇒ drying ⇒ heat treatment, (2) plating method (wet type), and (3) vapor deposition method (dry type) can be carried out.

[0075] The above-mentioned ingot is forged, rolled and drawn to prepare a wire (hereinafter also referred to as "intermediate wire") made of Cu or Cu alloy and having a diameter of about 0.7 to 2.0 mm.

[0076] Although electrolytic plating, electroless plating, vapor deposition, and the like can be used as methods for forming a coating layer on the surface of a Cu core material, electrolytic plating, which can stably control the film thickness, is industrially preferred. For example, a coating layer may be formed on the surface of an intermediate wire. The coating layer may also be applied at the ingot stage, or may be formed on the surface of the Cu core material after the intermediate wire is drawn to further thin it (e.g., after drawing it to the final wire diameter). The coating layer may be formed, for example, by providing a PdNi alloy layer containing Pd and Ni in a predetermined ratio on the surface of the Cu core material. From the viewpoint of forming a coating layer with excellent adhesion to the Cu core material, the coating layer may also be formed by providing a PdNi alloy layer containing Pd and Ni in a predetermined ratio on the surface of the Cu core material after strike plating a conductive metal. Furthermore, after forming a PdNi alloy layer containing Pd and Ni in a predetermined ratio, a layer containing at least one of Pd and Ni (for example, a Pd layer, a Ni layer, a PdNi alloy layer) may be further provided.

[0077] When forming a wire containing Au on the surface, it can be formed by providing an Au layer on the surface of the coating layer using the same method as described above.

[0078] In the wire drawing process, the wire is drawn to the final wire diameter (diameter of about 13 to 80 μm) using a wire drawing device using a diamond die. As for the heat treatment, in addition to the thermal refining heat treatment performed at the final wire diameter, an intermediate heat treatment performed during the wire drawing process may also be performed.

[0079] [Semiconductor Device] A semiconductor device can be manufactured by connecting electrodes on a semiconductor chip to external terminals such as electrodes on a lead frame or circuit board using the bonding wire for a semiconductor device of the present invention.

[0080] In one embodiment, the semiconductor device of the present invention includes a circuit board, a semiconductor chip, and a bonding wire for electrically connecting the circuit board and the semiconductor chip, and the bonding wire is the wire of the present invention.

[0081] In the semiconductor device of the present invention, the circuit board and semiconductor chip are not particularly limited, and known circuit boards and semiconductor chips that can be used to configure a semiconductor device may be used. Alternatively, a lead frame may be used instead of the circuit board. For example, a semiconductor device may be configured including a lead frame and a semiconductor chip mounted on the lead frame, as in the semiconductor device described in JP 2020-150116 A.

[0082] Examples of the semiconductor device include various semiconductor devices used in electrical appliances (e.g., computers, mobile phones, digital cameras, televisions, air conditioners, solar power generation systems, etc.) and vehicles (e.g., motorcycles, automobiles, trains, ships, aircraft, etc.).

[0083] The present invention will be specifically described below with reference to examples, although the present invention is not limited to the examples shown below.

[0084] (Sample) First, a method for preparing the sample will be described. The raw material Cu used had a purity of 4N (99.99% by mass or more) or higher. The first additional element, and if added, the second additional element, the third additional element, the fourth additional element, and the fifth additional element had a purity of 3N or higher, or a master alloy containing Cu and a few percent of these additional elements was used.

[0085] The core Cu alloy was first prepared by loading raw materials into a graphite crucible and heating them in a high-frequency furnace. 2The wire was heated to 1090-1800°C in an inert atmosphere of nitrogen gas or Ar gas to melt it, and then continuously cast into ingots with a diameter of 3-6 mm. The resulting ingots were then drawn to produce intermediate wires with a diameter of 0.7-2.0 mm. A commercially available lubricant was used in the drawing process, and the drawing speed was 20-150 m / min. The coating layer was formed using electroplating. Some wires (Examples Nos. 5, 9, 15, 27, 33, and 36) had an Au layer formed on the PdNi alloy layer. A Pd-Ni plating solution and an Au plating solution were prepared and adjusted as needed.

[0086] Thereafter, further wire drawing and other processes were carried out to process the wire into a final diameter of 20 μm. If necessary, intermediate heat treatment was carried out once or twice during the wire drawing process at 300 to 700°C for 2 to 15 seconds. When intermediate heat treatment was carried out, the wire was continuously swept and heated in N 2 After processing to the final wire diameter, the wire was continuously swept and N 2 The thermal refining treatment was performed while flowing nitrogen or Ar gas. The thermal refining treatment temperature was 200 to 600°C, the wire feed speed was 20 to 200 m / min, and the thermal refining time was 0.2 to 1.0 seconds. When the coating layer was thin, the thermal refining temperature was lowered and the wire feed speed was set to a higher value, and when the coating layer was thick, the thermal refining temperature was higher and the wire feed speed was set to a lower value.

[0087] (Test and Evaluation Methods) Test and evaluation methods will be described below.

[0088] [Composition Analysis of Wire Surface by Auger Electron Spectroscopy (AES)] For wires containing Au on their surface, the Au concentration on the wire surface was measured by Auger electron spectroscopy (AES) as follows, using the wire surface as the measurement surface. First, the bonding wire to be measured was fixed linearly to a sample holder. Next, the wire was positioned so that the center of the width of the wire in the direction perpendicular to the wire axis was the center of the width of the measurement surface, and the measurement surface was determined so that the width of the measurement surface was 5% to 15% of the wire diameter. The length of the measurement surface was 5 times the width of the measurement surface. Then, using an AES device (PHI-700 manufactured by ULVAC-PHI), composition analysis of the wire surface was performed at an acceleration voltage of 10 kV, and the surface Au concentration (atomic %) was determined. Note that the composition analysis by AES was performed on three measurement surfaces spaced 1 mm or more apart from each other in the wire axial direction, and the arithmetic average value was used. When determining the concentration of Au on the surface, gas components such as carbon (C), sulfur (S), oxygen (O), and nitrogen (N), non-metallic elements, etc. were not taken into consideration.

[0089] [Coating layer thickness analysis by Auger electron spectroscopy (AES)] Depth analysis by AES was used for the thickness analysis of the coating layer. Depth analysis by AES involves alternately performing composition analysis and sputtering to analyze changes in composition in the depth direction, and can obtain concentration changes of each element in the depth (center) direction from the wire surface (so-called depth direction concentration profile). Specifically, 1) composition analysis of the wire surface was performed by AES, and then 2) sputtering with Ar and 3) composition analysis of the surface after sputtering were repeated to obtain a concentration profile in the depth direction. The sputtering in 2) was performed with Ar. +The measurements were performed using ions and an acceleration voltage of 2 kV. In the surface composition analysis of 1) and 3), the dimensions of the measurement surface, the composition analysis by AES, and the conditions for calculating the concentration of each element were the same as those described in the above section [Composition Analysis of Wire Surface by Auger Electron Spectroscopy (AES)]. When obtaining a concentration profile in the depth direction using AES, measurements were performed so that there were 50 or more measurement points in the coating layer in the depth direction. The concentration profile in the depth direction was obtained for three measurement surfaces spaced 1 mm or more apart from each other in the wire axial direction.

[0090] - Thickness of the coating layer and the total number of measurement points of the coating layer - In the acquired concentration profile in the depth direction, the concentration profile from the wire surface to the wire center side was confirmed, and the Pd concentration C Pd (atomic %) and Ni concentration C Ni From the depth position Z1 where the total of (atomic %) reaches 90 atomic % or more for the first time, C Pd and C Ni The distance to depth position Z2 (where Z2 > Z1) where the sum of the values ​​of the SiO 2 and the SiO 3 values ​​first fell below 90 atomic % was determined as the thickness of the measured coating layer. The total number of measurement points from depth position Z1 to depth position Z2 was determined as the total number of measurement points of the coating layer. The thickness of the coating layer was determined by the arithmetic mean value of the values ​​obtained for the three measurement surfaces. It was also confirmed that the total number of measurement points of the coating layer for the wires of the examples was between 50 and 100. The depth measured by AES analysis was determined as the product of the sputtering rate and time. Generally, the sputtering rate is determined by the SiO 2 value obtained from the standard sample. 2 The depth analyzed by AES is measured using SiO 2 In other words, the unit of thickness of the coating layer is SiO 2 A conversion value was used.

[0091] - The total number of measurement points where the average value X and the absolute deviation from the average value X are within a predetermined range - The Pd concentration C for all measurement points of the coating layer in the acquired concentration profile in the depth direction Pd (atomic %) and Ni concentration C Ni (atomic %) ratio C Pd / C NiThe average value X was calculated by arithmetically averaging the values ​​of the coating layer. Pd / C Ni The absolute deviation from the average value X was calculated for each of the three measurement surfaces, and the total number of measurement points whose absolute deviation from the average value X was within 0.3X and the total number of measurement points whose absolute deviation from the average value X was within 0.2X were determined. The average value X was the arithmetic mean value of the values ​​obtained for the three measurement surfaces.

[0092] -C Pd or C Ni The slope of the approximate line (the difference between the maximum and minimum values ​​in the depth range of the coating layer) - C for all measurement points of the coating layer Pd (atomic %) or C Ni The average value X (atomic %) was linearly approximated by the least squares method, and the difference (atomic %) between the maximum and minimum values ​​of the approximated line in the depth range of the coating layer was calculated. Ni (atomic %) is linearly approximated by the least squares method, and if the average value X is 1 or more, C Pd The difference (atomic %) between the maximum and minimum values ​​of the approximate line within the depth range of the coating layer was calculated by arithmetic average of the values ​​obtained for the three measurement surfaces.

[0093] [Measurement of element content] The contents of the first additional element, the second additional element, the third additional element, the fourth additional element, and the fifth additional element in the wire were determined by analyzing a solution obtained by dissolving the bonding wire in strong acid using an ICP optical emission spectrometer and an ICP mass spectrometer, and detecting the concentration of the elements contained in the entire wire. As the analytical device, an ICP-OES ("PS3520UVDDII" manufactured by Hitachi High-Tech Science Corporation) or an ICP-MS ("Agilent 7700x ICP-MS" manufactured by Agilent Technologies, Inc.) was used. Note that for wires further containing Au on their surface, the concentration of Au as the first additional element was determined by exposing the cross section of the wire and measuring the Cu core portion using an electron beam microanalyzer (EPMA) or secondary ion mass spectrometry (SIMS).

[0094] [Fab Shape] The fabrication bonder (FAB) was fabricated on a lead frame using a commercially available wire bonder and observed with a scanning electron microscope (SEM) (number of evaluations: N=100). The fabrication current was set to 30-75 mA, the EFO gap was set to 762 μm, and the tail length was set to 254 μm. 2 +5% H 2 The gas was flowed at a rate of 0.4 to 0.6 L / min, and the diameter was set to 1.5 to 1.9 times the wire diameter. The FAB shape was judged as good if it was perfectly spherical, and poor if it was eccentric, irregular, or had poor melting properties. Evaluation was based on the following criteria:

[0095] Evaluation criteria: ◎: 5 ​​or less defects ○: 6 to 10 defects (no practical problem) ×: 11 or more defects

[0096] [Initial Bonding Properties of Second Bonded Portion] The initial bonding properties of the second bonded portion were evaluated by measuring and observing the bonding strength and adhesion of the second bonded portion. Specifically, the bonding strength of the second bonded portion was measured by a pull test. The adhesion properties of the second bonded portion were evaluated by observing the cross section of the second bonded portion using an SEM.

[0097] - Bonding strength of the second bond - Using a commercially available wire bonder, 80 wires each in the vertical and horizontal directions (320 wires in total) were bonded to an Ag-plated Cu alloy lead frame to prepare an evaluation sample. A pull test was then performed on the second bond. The pull strength value was the arithmetic average of the measurements of 15 wires in each direction, for a total of 60 wires.

[0098] - Adhesion of the 2nd bond - Using a commercially available wire bonder, 40 wires each in the vertical and horizontal directions (160 wires in total) were bonded onto a PPF-plated Cu alloy lead frame to prepare an evaluation sample. The 2nd bond was then subjected to cross-sectional polishing using an ion beam to prepare a sample for SEM observation. Specifically, the evaluation sample was cut in a direction perpendicular to the main surface of the lead frame at a position where the width of the 2nd bond is maximum when viewed from directly above in a direction perpendicular to the main surface of the lead frame, and the cross-section was polished to prepare a sample for SEM observation. Here, the width of the 2nd bond refers to the horizontal dimension of the 2nd bond 10 in FIG. 1. The cross-sectional polishing using an ion beam was performed in a direction perpendicular to the line passing through the center X of the wire width in FIG. 1 (along the two-dot chain line A-A in FIG. 1) at a position where the width of the 2nd bond is approximately maximum. The cross section of the second bonded portion of the obtained sample for SEM observation was observed using an SEM, and the ratio of the width where the wire and the lead frame were in close contact (L2 in FIG. 2) to the total width of the second bonded portion (L1 in FIG. 2), i.e., the adhesion rate (%) (= L2 / L1 × 100) was calculated. Three second bonded portions were observed and calculated, and the arithmetic average value was used.

[0099] The resulting second bonded portion was evaluated based on the bond strength (pull strength) and adhesion (adhesion rate) according to the following criteria.

[0100] Evaluation criteria: ⊚◎: Adhesion rate of 90% or more and pull strength of 8 gf or more ⊚: Adhesion rate of 90% or more and pull strength of 6 gf to less than 8 gf, or pull strength of 12 gf or more and adhesion rate of 80% to less than 90% ◯: Adhesion rate of 80% to less than 90% and pull strength of 6 gf to less than 12 gf ×: Adhesion rate less than 80% or pull strength less than 6 gf

[0101] [Bonding Reliability of Second Bonding Portion] The bonding reliability of the second bonding portion was evaluated by a high temperature storage life test (HTSL).

[0102] A sample was wedge-bonded to the lead portion of the lead frame using a commercially available wire bonder and sealed with a commercially available thermosetting epoxy resin to prepare a sample for testing the bonding reliability of the second bonding portion. The lead frame was a Cu alloy lead frame plated with 1 to 3 μm of Ag. The prepared sample for evaluating bonding reliability was exposed to an environment at a temperature of 175°C using a high-temperature incubator. The bonding life of the second bonding portion was determined by conducting a pull test on the wedge bonding portion every 500 hours, and the time until the pull strength value became half of the initial pull strength. The pull strength value was the arithmetic mean value of measurements taken at 50 randomly selected locations on the wedge bonding portion. The pull test after the high-temperature storage test was performed after removing the resin using acid treatment to expose the wedge bonding portion. Evaluation was then performed according to the following criteria.

[0103] Evaluation criteria: ⊚◎: Bonding life 3000 hours or more ⊚: Bonding life 2000 hours or more but less than 3000 hours ◯: Bonding life 1000 hours or more but less than 2000 hours ×: Bonding life less than 1000 hours

[0104] [Bonding Reliability of First Bonded Portion] The bonding reliability of the first bonded portion was evaluated by both a High Temperature Storage Life Test (HTSL) and a Highly Accelerated Temperature and Humidity Stress Test (HAST).

[0105] -HTSL- A sample for testing the bonding reliability of the first bonding portion was prepared by ball-bonding a sample to an electrode formed by depositing a 1.5 μm-thick film of an Al-1.0 mass % Si-0.5 mass % Cu alloy on a silicon substrate mounted on a typical metal frame using a commercially available wire bonder. The sample was then sealed with a commercially available thermosetting epoxy resin. The ball was formed under the conditions described in the [FAB Shape] section above. The prepared sample for evaluating bonding reliability was exposed to an environment at a temperature of 175°C using a high-temperature incubator. The bonding life of the first bonding portion was determined by conducting a shear test on the ball bonding portion every 500 hours, and the time until the shear strength value reached half of the initial shear strength was used. The shear strength value was the arithmetic mean value of measurements taken at 50 randomly selected locations on the ball bonding portion. The shear test after the high-temperature storage test was performed after removing the resin using acid treatment to expose the ball bonding portion. Evaluation was then performed according to the following criteria.

[0106] Evaluation criteria: ◎: Bonding life is 2000 hours or more ○: Bonding life is 1000 hours or more but less than 2000 hours ×: Bonding life is less than 1000 hours

[0107] -HAST- Samples for evaluating the bonding reliability of the first bonded portion, prepared using the same procedure as above, were exposed to a high-temperature, high-humidity environment at a temperature of 130°C and a relative humidity of 85% using an unsaturated pressure cooker tester, and a bias of 7 V was applied. The bonding life of the first bonded portion was determined by conducting a shear test on the ball bonded portion every 48 hours, and the time it took for the shear strength value to become half of the initial shear strength. The shear strength value was the arithmetic mean value of measurements taken at 50 randomly selected points on the ball bonded portion. The shear test was performed after removing the resin by acid treatment to expose the ball bonded portion. Evaluation was then performed according to the following criteria.

[0108] Evaluation criteria: ◎: Bonding life is 384 hours or more ○: Bonding life is 240 hours or more but less than 384 hours ×: Bonding life is less than 240 hours

[0109] [Bonded Shape] The bonded shape of the first bonded portion (the crushed shape of the ball) was evaluated by forming a ball using a commercially available wire bonder under the conditions described in the [FAB Shape] section above, crimping it to an electrode formed by depositing a 1.5 μm thick film of an Al-1.0 mass % Si-0.5 mass % Cu alloy on a Si substrate, and observing it from directly above with an optical microscope (number of evaluations N = 100). The crushed shape of the ball was judged as good if it was close to a perfect circle, and as poor if it was oval or petal-like. Evaluation was then performed according to the following criteria.

[0110] Evaluation criteria: ◎: No defects ○: 1 to 5 defects (no practical problems) ×: 6 or more defects

[0111] The evaluation results of the Examples and Comparative Examples are shown in Tables 1 and 2.

[0112]

[0113]

[0114] 1 Bonding wire (wire) 2 Measurement surface 10 Second bonding portion 50 External terminal X Center of wire width W Wire width (wire diameter) w a Measurement surface width l a Length of the measurement surface L1 Overall width of the second joint L2 Width where the wire and external terminal are in close contact at the second joint

Claims

1. A bonding wire comprising a core material made of Cu or a Cu alloy and a coating layer formed on the surface of the core material, the total concentration of Pd and Ni being 90 atomic % or more, wherein, in a concentration profile in the depth direction of the wire obtained by measuring 50 or more measurement points in the coating layer by Auger electron spectroscopy (AES), the thickness of the coating layer is 10 nm or more and 130 nm or less, and the concentration C of Pd at all measurement points of the coating layer is 100 nm or more and 100 nm or less. Pd (atomic %) and Ni concentration C Ni (atomic %) ratio C Pd / C Ni A bonding wire in which, when the average value of is X, the average value X is 0.1 or more and 35.0 or less, the total number of measurement points in the coating layer having an absolute deviation of 0.3X or less from the average value X is 50% or more of the total number of measurement points in the coating layer, and the following condition (A) is satisfied: (A) The wire contains one or more elements (hereinafter referred to as "first additive element") selected from the group consisting of Ti, V, Cr, Mn, Fe, Co, Zn, Zr, Nb, Mo, Ru, Rh, Sn, Ta, W, Os, Ir, Pt, Au, and Bi, and the total concentration of the first additive element in the entire wire is 5 ppm by mass or more and 450 ppm by mass or less.

2. A bonding wire comprising a core material made of Cu or a Cu alloy and a coating layer formed on the surface of the core material, the total concentration of Pd and Ni being 90 atomic % or more, wherein, in a concentration profile in the depth direction of the wire obtained by measuring 50 or more measurement points in the coating layer by Auger electron spectroscopy (AES), the thickness of the coating layer is 10 nm or more and 130 nm or less, and the Pd concentration C for all measurement points in the coating layer is Pd (atomic %) and Ni concentration C Ni (atomic %) ratio C Pd / C Ni A bonding wire in which, when the average value of is X, the average value X is 0.1 or more and 35.0 or less, the total number of measurement points in the coating layer having an absolute deviation of 0.3X or less from the average value X is 50% or more of the total number of measurement points in the coating layer, and the following conditions (A) and (B) are satisfied: (A) the wire contains one or more elements (hereinafter referred to as "first additive element") selected from the group consisting of Ti, V, Cr, Mn, Fe, Co, Zn, Zr, Nb, Mo, Ru, Rh, Sn, Ta, W, Os, Ir, Pt, Au, and Bi, and the total concentration of the first additive element in the entire wire (wherein the concentration of Au is the concentration in the core material portion) is 5 ppm by mass or more and 450 ppm by mass or less, and (B) the wire contains Au on the surface thereof, and the concentration of Au in the entire wire is 0.5% by mass or less.

3. The bonding wire according to claim 1 or 2, wherein the total number of measurement points in the coating layer having an absolute deviation of 0.2X or less from the average value X is 50% or more of the total number of measurement points in the coating layer.

4. For all measurement points of the coating layer, C Pd Or C Ni The bonding wire according to any one of claims 1 to 3, wherein when linear approximation is performed by the least squares method, the difference between the maximum value and the minimum value of the approximate straight line in the depth range of the coating layer is 20 atomic % or less.

5. The bonding wire according to any one of claims 1 to 4, wherein the concentration profile in the depth direction of the wire is obtained by measuring with AES under the following <conditions> while digging in the depth direction from the surface of the wire by Ar sputtering: <conditions> The center of the wire width is positioned to be the center of the width of the measurement surface, and the width of the measurement surface is 5% to 15% of the wire diameter, and the length of the measurement surface is 5 times the width of the measurement surface.

6. A bonding wire according to any one of claims 1 to 5, comprising one or more elements (hereinafter referred to as "second additive elements") selected from the group consisting of B, P and Mg, and the total concentration of the second additive elements in the entire wire is 1 ppm by mass or more and 100 ppm by mass or less.

7. A bonding wire according to any one of claims 1 to 6, comprising one or more elements (hereinafter referred to as "third additive elements") selected from the group consisting of Se, Te, As and Sb, and the total concentration of the third additive elements in the entire wire is 1 mass ppm or more and 100 mass ppm or less.

8. A bonding wire described in any one of claims 1 to 7, comprising one or more elements (hereinafter referred to as the "fourth additional element") selected from the group consisting of Ga and Ge, and the total concentration of the fourth additional element in the entire wire is 0.011 mass% or more and 1.5 mass% or less.

9. A bonding wire according to any one of claims 1 to 8, comprising one or more elements selected from the group consisting of In and Ag (hereinafter referred to as the "fifth additional element"), and the total concentration of the fifth additional element in the entire wire is 1 mass ppm or more and 500 mass ppm or less.

Citation Information

Patent Citations

  • Copper alloy wire for connecting semiconductor element

    JP1986048543A

  • Bonding wire and integrated circuit device using the same

    JP2005167020A

  • Corrosion and Moisture Resistant Copper Based Bonding Wire Containing Nickel

    JP2018503743A

  • Semiconductor device and manufacturing method thereof

    JP2020150116A

  • Bonding wire for semiconductor device

    WO2017013796A1