Lithium metal complex oxide, positive electrode active material for lithium secondary batteries, positive electrode for lithium secondary batteries, and lithium secondary battery
The development of a lithium metal composite oxide with a tailored composition and structure addresses the challenge of high-rate discharge capacity in lithium secondary batteries, resulting in improved performance and extended battery life by optimizing pore distribution and elemental composition.
Patent Information
- Application Number
- PCT/JP2024/005465
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-31
- Filing Date
- 2024-02-16
- Publication Date
- 2024-12-05
AI Technical Summary
Lithium secondary batteries face challenges in achieving high-rate discharge capacity due to limitations in the performance of conventional lithium metal composite oxides used as positive electrode active materials.
A lithium metal composite oxide with specific compositional and structural characteristics, including a layered crystal structure, optimized pore distribution, and elemental composition, is developed to enhance discharge capacity. The composite oxide is represented by Li[Liα(Ni1−x−yM1xM2y)1−α]O2, where M1 is Mn or Al, M2 is selected from various elements, and the pore size distribution is tailored to improve electrolyte impregnation and reaction field formation.
The optimized lithium metal composite oxide significantly improves the high-rate discharge capacity, internal resistance, and cycle maintenance rate of lithium secondary batteries, leading to enhanced performance and extended battery life.
Smart Images

Figure JP2024005465_05122024_PF_FP_ABST
Abstract
Description
Lithium metal composite oxide, positive electrode active material for lithium secondary battery, positive electrode for lithium secondary battery, and lithium secondary battery
[0001] The present invention relates to a lithium metal composite oxide, a positive electrode active material for a lithium secondary battery, a positive electrode for a lithium secondary battery, and a lithium secondary battery.
[0002] In a lithium secondary battery, the positive electrode is made using a positive electrode active material containing, for example, a lithium metal composite oxide.
[0003] Conventionally, various lithium metal composite oxides have been proposed to improve the performance of lithium secondary batteries.
[0004] WO2019 / 069402A1
[0005] There is a demand for improved discharge capacity in lithium secondary batteries.
[0006] An object of the present invention is to provide a lithium metal composite oxide, a positive electrode active material for a lithium secondary battery, a positive electrode for a lithium secondary battery, and a lithium secondary battery that can improve high-rate discharge capacity.
[0007] The present invention has the following aspects: [1] A lithium metal composite oxide containing Li, Ni, and an element M, wherein the element M is at least one element selected from the group consisting of Co, Mn, Fe, Cu, Ti, Mg, Ca, Al, Zn, Sn, Zr, B, Si, Nb, W, Ta, Ba, S, and P, and having pores, wherein in a pore size distribution calculated for the pores by the Barrett-Joyner-Halenda method from a nitrogen adsorption isotherm, a maximum value dV1 of a rate dVp / ddp of an increase in a pore volume Vp of the pore with respect to an increase in the pore diameter dp of the pore satisfies the relationship shown in the following (Equation A1), within a range in which the rate dp / ddp of an increase in a pore surface area ap of the pore with respect to an increase in the pore diameter dp of the pore satisfies the relationship "dap / ddp≦0.10": A lithium metal composite oxide, wherein the maximum value dV2 of the dVp / ddp in the range where the dap / ddp satisfies the relationship "dap / ddp > 0.10" satisfies the relationship shown in the following (Formula A2): dV1≦1.00×10 -4 ...(Formula A1) dV2≧1.00×10 -4 ... (Formula A2) [2] The lithium metal composite oxide according to [1], wherein in the pore size distribution, the pore volume V satisfies the relationship shown in the following (Formula B): 3 / g≦V≦0.01 cm 3 / g ... (Equation B) [3] The lithium metal composite oxide according to [1] or [2], wherein in the pore size distribution, the pore surface area Ap satisfies the relationship shown in the following (Equation C): 2 / g≦Ap≦2.0m 2 / g ... (Formula C) [4] The lithium metal composite oxide according to any one of [1] to [3], wherein in the pore size distribution, the average pore diameter Adp satisfies the relationship shown in the following (Formula D). 10 nm ≦ Adp ≦ 40 nm ... (Formula D) [5] A lithium metal composite oxide represented by (Composition Formula I), wherein in (Composition Formula I), M1 is at least one element selected from the group consisting of Mn, Al, and Co, and M2 is at least one element selected from the group consisting of Fe, Cu, Ti, Mg, Ca, Zn, Sn, Zr, B, Si, Nb, W, Ta, Ba, S, and P, and wherein the relationships shown in the following (Formula Ia) to (Formula Id) are satisfied. Li[Li α (Ni (1-x-y) M1 x M2 y ) 1-α ]O 2... (Composition formula I) -0.1≦α≦0.2 ... (Formula Ia) 0≦x≦0.5 ... (Formula Ib) 0≦y≦0.7 ... (Formula Ic) 0<x+y<1 ... (Formula Id) [6] The lithium metal composite oxide according to any one of [1] to [5], wherein the amount of Co relative to the total amount of Ni and the element M is 10 mol % or less. [7] The lithium metal composite oxide according to [5], wherein in (Composition formula I), the relationship shown in the following (Formula Id_1) is satisfied: 0<x+y≦0.15 ... (Formula Id_1) [8] The lithium metal composite oxide according to any one of [1] to [7], wherein the metal site occupancy rate SR obtained by Rietveld analysis satisfies the relationship shown in the following (Formula E). 1.0%≦SR≦4.0% ... (Formula E) [9] The lithium metal composite oxide according to any one of [1] to [8], wherein the average crystallite size AK obtained by Rietveld analysis satisfies the relationship shown in the following (Formula F): 80 nm≦AK≦200 nm ... (Formula F)
[10] A positive electrode active material for a lithium secondary battery, comprising the lithium metal composite oxide according to any one of [1] to [9].
[11] A positive electrode for a lithium secondary battery, comprising the positive electrode active material for a lithium secondary battery according to
[10] .
[12] A lithium secondary battery, comprising the positive electrode for a lithium secondary battery according to
[11] .
[0008] According to the present invention, it is possible to provide a lithium metal composite oxide, a positive electrode active material for a lithium secondary battery, a positive electrode for a lithium secondary battery, and a lithium secondary battery, which are capable of improving high-rate discharge capacity.
[0009] FIG. 1A is a diagram showing an example of the rate dap / ddp of increase in the pore surface area ap of a pore relative to an increase in the pore diameter dp of the pore in an embodiment. FIG. 1B is a diagram showing an example of the rate dVp / ddp of increase in the pore volume Vp of a pore relative to an increase in the pore diameter dp of the pore in an embodiment. FIG. 1C is a diagram showing an example of the relationship between dap / ddp and dVp / ddp in an embodiment. FIG. 2 is a schematic diagram showing an example of a lithium secondary battery. FIG. 3 is a schematic diagram showing an example of an all-solid-state lithium secondary battery.
[0010] An example of an embodiment of the present invention will now be described.
[0011] In this specification, metal composite compounds are indicated using the abbreviation "MCC" (Metal Composite Compound). Lithium metal composite oxides are indicated using the abbreviation "LiMO" (Lithium Metal Composite Oxide). Positive electrode active materials for lithium secondary batteries are indicated using the abbreviation "CAM" (Cathode Active Material for Lithium Secondary Batteries). In addition, "Ni" and "Li" do not indicate nickel metal or lithium metal alone, but nickel element or lithium element. The same applies to other elements such as Co and Mn. Regarding the numerical range, for example, when it is described as "5-15 μm", it means a range from 5 μm to 15 μm, and means a numerical range including the lower limit of 5 μm and the upper limit of 15 μm. Furthermore, any combination of the numerical ranges of the respective physical properties, compositions, manufacturing conditions, etc. is possible. A lithium secondary battery refers to a battery in which an electrolyte (such as a non-aqueous electrolyte or a solid electrolyte) is disposed between a positive electrode and a negative electrode, and charging and discharging are performed by lithium ions moving between the positive electrode and the negative electrode via the electrolyte.
[0012] [A] LiMO [A-1] Crystal Structure In this embodiment, LiMO is a material used as a CAM. From the viewpoint of improving the discharge capacity at high rates, LiMO preferably has a layered structure.
[0013] The crystal structure of LiMO is more preferably a hexagonal or monoclinic crystal structure. The hexagonal crystal structure is P3, P3 1 , P3 2 , R3, P-3, R-3, P312, P321, P3 1 12. P3 1 21, P3 2 12. P3 2 21, R32, P3m1, P31m, P3c1, P31c, R3m, R3c, P-31m, P-31c, P-3m1, P-3c1, R-3m, R-3c, P6, P6 1 , P65 , P6 2 , P6 4 , P6 3 , P-6, P6 / m, P6 3 / m, P622, P6 1 22, P6 5 22, P6 2 22, P6 4 22, P6 3 22, P6mm, P6cc, P6 3 cm, P6 3 mc, P-6m2, P-6c2, P-62m, P-62c, P6 / mmm, P6 / mcc, P6 3 / mcm, and P6 3 / mmc. The monoclinic crystal structure is assigned to one space group selected from the group consisting of P2, P2 1 , C2, Pm, Pc, Cm, Cc, P2 / m, P2 1 / m, C2 / m, P2 / c, P2 1 Among the above, the crystal structure of LiMO is more preferably a hexagonal system belonging to the space group R-3m or a monoclinic system belonging to the space group C2 / m in order to obtain a lithium secondary battery with a high discharge capacity.
[0014] The crystal structure of LiMO can be confirmed by observation using a powder X-ray diffraction measurement device, such as an Ultima IV manufactured by Rigaku Corporation.
[0015] [A-2] Composition The composition of LiMO contains at least Li, Ni, and an element M.
[0016] The element M is at least one element selected from the group consisting of Co, Mn, Fe, Cu, Ti, Mg, Ca, Al, Zn, Sn, Zr, B, Si, Nb, W, Ta, Ba, S, and P.
[0017] LiMO preferably contains Li, Ni, and at least one element M1 selected from the group consisting of Co, Mn, and Al.
[0018] The LiMO is preferably represented by (composition formula I).
[0019] Li [Li α (Ni (1-x-y) M1 x M2 y ) 1-α ]O 2 ...(compositional formula I)
[0020] In (Composition Formula I), M1 is at least one element selected from the group consisting of Mn, Al, and Co. M2 is at least one element selected from the group consisting of Fe, Cu, Ti, Mg, Ca, Zn, Sn, Zr, B, Si, Nb, W, Ta, Ba, S, and P.
[0021] In (Composition Formula I), α, x, and y preferably satisfy the relationships shown in the following (Formula Ia) to (Formula Id): −0.1≦α≦0.2 (Formula Ia) 0≦x≦0.5 (Formula Ib) 0≦y≦0.7 (Formula Ic) 0<x+y<1 (Formula Id)
[0022] In (Composition Formula I), when the value of α satisfies the relationship shown in (Formula Ia), the internal resistance of the lithium secondary battery can be reduced and the high-rate discharge capacity can be improved. Furthermore, in (Composition Formula I), α is more preferably −0.03 or more, and even more preferably −0.02 or more. Furthermore, α is more preferably 0.1 or less, and even more preferably 0.07 or less. The range of α is more preferably −0.03≦α≦0.1, and even more preferably −0.02≦α≦0.07.
[0023] In (Composition Formula I), when the value of x satisfies the relationship shown in (Formula Ib), the internal resistance of the lithium secondary battery can be reduced, the high-rate discharge capacity can be increased, the life can be extended, and the rate characteristics can be improved. Furthermore, in (Composition Formula I), x is more preferably 0.01 or more, and even more preferably 0.02 or more. Furthermore, x is more preferably 0.4 or less, and even more preferably 0.3 or less. The range of x is more preferably 0.01≦x≦0.4, and even more preferably 0.02≦x≦0.3.
[0024] In (Composition Formula I), the value of y satisfies the relationship shown in (Formula Ic), thereby improving the cycle retention rate of the lithium secondary battery. Furthermore, when LiMO contains M2, in (Composition Formula I), y is more preferably 0.0002 or more, and even more preferably 0.0005 or more. Furthermore, y is more preferably 0.6 or less, and even more preferably 0.5 or less. The range of y is more preferably 0≦y≦0.6, more preferably 0.0002≦y≦0.6, and particularly preferably 0.0005≦y≦0.5.
[0025] In (Composition Formula I), the sum (x + y) of the values of x and y satisfies the relationship shown in (Formula Id), thereby improving the initial capacity and high-rate discharge capacity of the lithium secondary battery. Furthermore, in (Composition Formula I), (x + y) is more preferably less than 0.6, even more preferably 0.3 or less, and particularly preferably 0.15 or less. (x + y) is more preferably 0.01 or greater. Examples of ranges for (x + y) include 0.01≦x + y<0.6, 0.01≦x + y≦0.3, and 0.01≦x + y≦0.15. In particular, satisfying the relationship shown in the following (Formula Id_1) can improve the high-rate discharge capacity.
[0026] 0<x+y≦0.15... (Formula Id_1)
[0027] M2 is preferably at least one element selected from the group consisting of Ti, Mg, Zr, B, Nb, and W.
[0028] In the LiMO, the amount of Co relative to the total amount of Ni and element M is preferably 10 mol % or less, more preferably 5 mol % or less, even more preferably 3 mol % or less, particularly preferably 1 mol % or less, and may even be 0. When LiMO is represented by (composition formula I), the amount of Co can be calculated using the amount of Ni [Ni], the amount of M1 [M1], the amount of M2 [M2], and the amount of Co [Co] according to the following (formula II). When the amount of Co is within the above range, the operating voltage of the lithium secondary battery is less likely to increase and the electrolyte is less likely to decompose on the LiMO surface, thereby reducing resistance and further improving the high-rate discharge capacity of the lithium secondary battery.
[0029] 100.[Co] / ([Ni]+[M1]+[M2])...(Formula II)
[0030] <Method for Measuring Composition> The composition of LiMO is measured using, for example, an ICP optical emission spectrometer (Optima 7300 (manufactured by PerkinElmer Co., Ltd.) or the like). Prior to measuring the composition, a sample is dissolved in an acid or alkali depending on the element to be measured.
[0031] [A-3] Pores in LiMO LiMO has pores. Furthermore, LiMO is a powder. LiMO may be composed only of secondary particles formed by aggregation of primary particles, or may be a mixture of primary particles and secondary particles. For example, LiMO may contain a plurality of primary particles and secondary particles formed by aggregation of the plurality of primary particles.
[0032] The "primary particles" are particles that do not appear to have grain boundaries when LiMO is observed under a microscope (such as a scanning electron microscope) at a magnification of 1,000 to 30,000 times. The "secondary particles" are aggregates of these primary particles.
[0033] In the secondary particles constituting LiMO, pores are present between a plurality of primary particles.
[0034] The pore size (pore diameter) dp, pore surface area ap, and pore volume Vp of LiMO pores are obtained from the pore size distribution calculated by the Barrett-Joyner-Halenda method (BJH method) from the nitrogen adsorption isotherm. ap affects the reaction field of a lithium secondary battery, and Vp affects the impregnation (accessibility) of the electrolyte in the lithium secondary battery.
[0035] <Method for measuring pore volume ratio> The nitrogen adsorption isotherm is obtained by subjecting 10 g of a LiMO sample to vacuum degassing treatment using a vacuum heat treatment device (e.g., BELSORP-vacII (manufactured by Microtrac-Bell Co., Ltd.)), and then measuring the sample under liquid nitrogen (temperature 77 K) using an adsorption isotherm measurement device (e.g., BELSORP-mini (manufactured by Microtrac-Bell Co., Ltd.)). In the nitrogen adsorption isotherm, the amount of nitrogen adsorbed by a unit weight of LiMO is expressed as the volume of gaseous nitrogen at standard temperature and pressure (STP). The pore size distribution can be obtained by analyzing the nitrogen adsorption isotherm using the BJH method. From the pore size distribution, the average pore diameter Adp, pore volume V, and pore surface area Ap described below can be determined. The BJH method is a technique in which the shape of pores is assumed to be cylindrical and analysis is performed based on the relationship between the pore diameter at which capillary condensation occurs and the relative pressure of nitrogen (Kelvin equation), and is used to evaluate pores (mesopores, etc.) with a pore diameter dp of approximately 2-200 nm.
[0036] (Rate of increase in pore volume Vp, dVp / ddp) In the pore size distribution of LiMO obtained above, the rate of increase in ap relative to an increase in pore dp, dap / ddp, and the rate of increase in Vp relative to an increase in pore dp, dVp / ddp, satisfy a specific relationship as will be described below.
[0037] 1A is a diagram showing an example of pore dap / ddp, in which the horizontal axis represents pore dp and the vertical axis represents pore dap / ddp (the rate of change of ap relative to dp).
[0038] 1B is a diagram showing an example of dVp / ddp of a pore, in which the horizontal axis represents dp of the pore and the vertical axis represents dVp / ddp of the pore (the rate of change of Vp with respect to dp).
[0039] 1C is a diagram showing an example of the relationship between dap / ddp and dVp / ddp, in which the horizontal axis represents dap / ddp and the vertical axis represents dVp / ddp.
[0040] 1C , in the LiMO of this embodiment, the maximum value dV1 of dVp / ddp in the range where dap / ddp≦0.10 satisfies the relationship shown in the following formula A1. Furthermore, in the LiMO, the maximum value dV2 of dVp / ddp in the range where dap / ddp satisfies the relationship "dap / ddp>0.10" satisfies the relationship shown in the following formula A2.
[0041] dV1≦1.00×10 -4 ...(Formula A1) dV2≧1.00×10 -4 ...(Formula A2)
[0042] The range satisfying the relationship of "dap / ddp≦0.10" is a region in which the increase rate of the pore surface area relative to the increase in pore diameter is small, and is a region containing pores with few reaction sites in the electrode reaction. LiMO satisfying the above (Equation A1) means that in this region, the increase rate of the pore volume relative to the increase in pore diameter is small, and pores that are difficult to impregnate with the electrolyte are unlikely to be formed. In other words, LiMO satisfying the above (Equation A1) is thought to have few pores that are inefficient structures in the electrode reaction.
[0043] The range satisfying the relationship "dap / ddp>0.10" is a region in which the increase in pore surface area relative to the increase in pore diameter is large, and is a region containing pores with many reaction sites in the electrode reaction. LiMO satisfying the above (Equation A2) means that in this region, the increase in pore volume relative to the increase in pore diameter is large, and pores that are easy to impregnate with the electrolyte are formed. In other words, LiMO satisfying the above (Equation A2) is considered to have sufficient pores that are efficient in the electrode reaction.
[0044] Therefore, LiMO that satisfies the relationships shown in (Equation A1) and (Equation A2) can improve the high-rate discharge capacity of a lithium secondary battery.
[0045] From the viewpoint of improving the discharge capacity at high rates, dV1 is 0.90 × 10 -4 More preferably, 0.80 x 10 or less -4 More preferably, dV1 is 0.20×10 or less. -4 More preferably, 0.35×10 -4 More preferably, 0.50 × 10 -4 The range of dV1 is particularly preferably 0.20×10 -4 ≦dV1≦0.90×10 -4 More preferably, 0.35 × 10 -4 ≦dV1≦0.80×10 -4 is more preferably 0.50 × 10 -4 ≦dV1≦0.80×10 -4 is particularly preferred.
[0046] From the viewpoint of improving the discharge capacity at high rates, dV2 is 1.01 × 10 -4 More preferably, 1.03 × 10 -4 More preferably, dV2 is 2.50×10 -4 More preferably, 2.30 x 10 -4 More preferably, 2.00 x 10 -4 The following is particularly preferred: The range of dV2 is 1.01 x 10 -4 ≦dV2≦2.50×10 -4 More preferably, 1.03 × 10 -4 ≦dV2≦2.30×10 -4 is more preferably 1.03 × 10 -4 ≦dV2≦2.00×10 -4 is particularly preferred.
[0047] (Pore Volume V) The pore volume V of LiMO preferably satisfies the relationship shown in the following (Equation B): V is the pore volume in the pore diameter range of 2 to 200 nm in the pore diameter distribution.
[0048] 0.001 cm 3 / g≦V≦0.01 cm3 / g...(Formula B)
[0049] LiMO satisfying formula (B) has a sufficient pore volume and sufficient pores that provide a good balance between the impregnation of the electrolyte and the formation of reaction fields, and therefore, the LiMO can further improve the high-rate discharge capacity of lithium secondary batteries.
[0050] V is 0.009 cm 3 / g or less is more preferable, and 0.008 cm 3 / g or less is more preferable. 3 / g or more is more preferable, and 0.004 cm 3 / g or more is more preferable. 3 / g≦Vp≦0.009 cm 3 / g is more preferred, and 0.004 cm 3 / g≦Vp≦0.009 cm 3 / g is more preferable, and 0.004 cm 3 / g≦Vp≦0.008 cm 3 / g is particularly preferred.
[0051] (Pore Surface Area Ap) The pore surface area Ap of LiMO preferably satisfies the relationship shown in the following (Formula C): Ap is the pore surface area in the pore diameter range of 2 to 200 nm in the pore diameter distribution.
[0052] 0.5 m 2 / g≦Ap≦2.0m 2 / g...(Formula C)
[0053] LiMO that satisfies formula (C) has a sufficient pore surface area and facilitates the formation of a reaction field, which makes it possible to further improve the high-rate discharge capacity of a lithium secondary battery.
[0054] Ap is 0.7m 2 / g or more is more preferable, and 0.9m 2 / g or more is more preferable. 2 / g or less is more preferable, and 1.6m 2 / g or less is more preferable. 2 / g≦Ap≦1.8m2 / g is more preferable, and 0.9m 2 / g≦Ap≦1.6m 2 / g is more preferred.
[0055] (Average Pore Diameter Adp) The average pore diameter Adp of LiMO preferably satisfies the relationship shown in the following (Formula D).
[0056] 10nm≦Adp≦40nm...(Formula D)
[0057] LiMO that satisfies formula (D) has pores with an appropriate diameter that are effective for electrode reactions, and therefore can further improve the high-rate discharge capacity of lithium secondary batteries.
[0058] Adp is more preferably 35 nm or less, and even more preferably 30 nm or less. Adp is more preferably 15 nm or more, and even more preferably 20 nm or more. The range of Adp is more preferably 15 nm≦Adp≦35 nm, and even more preferably 20 nm≦Adp≦30 nm.
[0059] [A-4] Other Characteristics (Metal Site Occupancy Ratio SR) The metal site occupancy ratio SR of LiMO preferably satisfies the relationship shown in the following (Equation E).
[0060] 1.0%≦SR≦4.0%…(Formula E)
[0061] SR is the ratio of Ni and element M present in the Li layers (Li sites) constituting the layered structure of LiMO. When SR is equal to or less than the upper limit, the diffusion resistance in the lithium secondary battery is less likely to increase, and the decrease in discharge capacity at high rates can be further suppressed. When SR is equal to or greater than the lower limit, the volume change rate of the lithium secondary battery is less likely to increase, and damage, etc., is less likely to occur.
[0062] The SR is more preferably 3.5% or less, and even more preferably 3.0% or less. The SR is more preferably 1.1% or more, and even more preferably 1.2% or more. The SR range is more preferably 1.1%≦SR≦3.5%, and even more preferably 1.2%≦SR≦3.0%.
[0063] (Average Crystallite Size AK) The average crystallite size AK of LiMO preferably satisfies the relationship shown in the following (Formula F).
[0064] 80nm≦AK≦200nm…(Formula F)
[0065] When AK is within the above range, LiMO crystals grow appropriately and sufficiently, which can suppress an increase in the resistance of the lithium secondary battery and further improve the discharge capacity at high rates.
[0066] AK is more preferably 170 nm or less, even more preferably 150 nm or less, and particularly preferably 130 nm or less. AK is more preferably 90 nm or more, even more preferably 100 nm or more, and particularly preferably 105 nm or more. AK is more preferably in the range 90 nm≦AK≦170 nm, even more preferably 100 nm≦AK≦150 nm, and particularly preferably 105 nm≦AK≦130 nm.
[0067] <Method for measuring metal site occupancy and average crystallite size> SR and AK are calculated by performing Rietveld analysis on a powder X-ray diffraction pattern obtained by powder X-ray diffraction measurement. Rietveld analysis is a technique for comparing an actually measured powder X-ray diffraction pattern with a simulation pattern obtained from a crystal structure model, and optimizing the crystal structure parameters in the crystal structure model so as to minimize the difference between the two.
[0068] Powder X-ray diffraction measurement is performed using an X-ray diffractometer. For example, a D8 Advance (manufactured by Bruker) can be used as the X-ray diffractometer. Specifically, LiMO powder is filled into a dedicated substrate, and measurement is performed using a CuKα radiation source under conditions of a diffraction angle 2θ = 10°-90° and a sampling width of 0.02° to obtain a powder X-ray diffraction pattern. The obtained powder X-ray diffraction pattern is subjected to Rietveld analysis. The Rietveld analysis software used is TOPAS ver. 4.2 manufactured by Bruker. At this time, a layered rock salt crystal structure (Li 1-n Me n ) (Me 1-n Li n ) O 2The metal site occupancy rate n in the Li site is optimized using the above method. SR and AK can be calculated.
[0069] [B] Method for Producing LiMO A method for producing the above LiMO will be described.
[0070] When LiMO is produced, a mixing step and a firing step are carried out in sequence.
[0071] [B-1] Mixing Step In the mixing step, a mixture containing MCC, which is a precursor of LiMO, and a lithium compound is prepared.
[0072] [B-1-1] MCC MCC is a substance containing Ni and element M that constitute LiMO, and is, for example, a metal composite hydroxide, a metal composite oxide, or a mixture thereof.
[0073] The metal composite hydroxide used as MCC is produced, for example, by a known batch coprecipitation method or continuous coprecipitation method.
[0074] Hereinafter, the production method will be described in detail using a metal composite hydroxide containing Ni and element M as an example.
[0075] Specifically, a nickel salt solution and a metal salt solution of element M are reacted by the continuous coprecipitation method described in JP-A-2002-201028. This produces a metal composite hydroxide (Ni) containing Ni and element M. (1-a) M a (OH) 2 (0<a<1)) is produced.
[0076] The nickel salt that is the solute of the nickel salt solution is, for example, at least one of nickel sulfate, nickel nitrate, nickel chloride, and nickel acetate.
[0077] The metal salt of element M, which is the solute of the metal salt solution of element M, is, for example, at least one of cobalt sulfate, cobalt nitrate, cobalt chloride, cobalt acetate, manganese sulfate, manganese nitrate, manganese chloride, manganese acetate, aluminum sulfate, aluminum nitrate, aluminum chloride, and aluminum acetate.
[0078] The nickel salt solution and the metal salt solution of element M are prepared by dissolving nickel salt and metal salt of element M in a solution containing nickel salt and metal salt of element M (Ni (1-a) M a (OH) 2 ) are mixed in a ratio corresponding to the amount of water used as the solvent for these solutions.
[0079] In the process for producing the metal composite hydroxide, a complexing agent may be used. In this case, the molar ratio of the amount of the complexing agent to the total number of moles of the nickel salt and the metal salt of element M is, for example, greater than 0 and less than or equal to 2.
[0080] The complexing agent is a material capable of forming a complex in an aqueous solution with nickel ions and ions of element M. The complexing agent is, for example, at least one of an ammonium ion donor (ammonium hydroxide, ammonium sulfate, ammonium chloride, ammonium carbonate, ammonium fluoride, or the like), hydrazine, ethylenediaminetetraacetic acid, nitrilotriacetic acid, uracildiacetic acid, and glycine.
[0081] Before the pH of the mixture containing the nickel salt solution, the metal salt solution of element M, and any complexing agent changes from alkaline to neutral, an aqueous solution of an alkali metal hydroxide is added to the mixture, such as sodium hydroxide or potassium hydroxide.
[0082] The pH value of the mixed solution is measured when the temperature of the mixed solution is 40° C. If the temperature of the mixed solution sampled from the reaction tank is not 40° C., the mixed solution is heated or cooled to 40° C., and then the pH is measured.
[0083] The temperature of the reaction vessel is controlled, for example, within the range of 20-80°C, preferably within the range of 30-70°C.
[0084] During the reaction, the pH value of the mixture in the reaction vessel is controlled within the range of, for example, 9-13.
[0085] The reaction precipitate formed in the reaction tank is neutralized while being stirred. The time for neutralizing the reaction precipitate is, for example, in the range of 1 to 20 hours.
[0086] As a reaction vessel used in the continuous coprecipitation method, an overflow type reaction vessel can be used in order to separate the formed reaction precipitate.
[0087] When producing a metal composite hydroxide by a batch coprecipitation method, a reaction tank without an overflow pipe or an apparatus having a mechanism for concentrating the overflowed reaction precipitate in a concentration tank connected to an overflow pipe and circulating it back to the reaction tank may be used.
[0088] Here, various gases (for example, inert gases such as nitrogen, argon, or carbon dioxide, oxidizing gases such as air or oxygen, or a mixture thereof) may be supplied into the reaction vessel.
[0089] After the reaction is completed, the resulting reaction precipitate is isolated. The isolation is carried out, for example, by dehydrating the slurry containing the reaction precipitate by centrifugation, suction filtration, or the like. The reaction precipitate may also be washed before isolation.
[0090] The isolated reaction precipitate is then dried and sieved as necessary to obtain a metal composite hydroxide.
[0091] The reaction precipitate is preferably washed using water or an alkaline washing solution. The reaction precipitate is preferably washed using an alkaline washing solution, particularly an aqueous sodium hydroxide solution. Alternatively, the reaction precipitate may be washed using a washing solution containing sulfur. The sulfur-containing washing solution is, for example, an aqueous solution of potassium or sodium sulfate.
[0092] In the above example, a metal composite hydroxide is produced as MCC, but a metal composite oxide may also be prepared.
[0093] The metal composite oxide is produced, for example, by oxidizing a metal composite hydroxide (oxidation step). The oxidation step may be carried out multiple times as necessary. When multiple oxidation steps are carried out, the oxidation temperature refers to the temperature of the step in which oxidation was carried out at the highest temperature among the multiple oxidation steps.
[0094] The oxidation temperature is preferably in the range of 400 to 700° C., more preferably in the range of 450 to 680° C. The oxidation temperature means the set temperature of the device used for oxidation.
[0095] The time for maintaining the oxidation temperature in the oxidation step is preferably in the range of 0.1 to 20 hours, more preferably in the range of 0.5 to 10 hours. The temperature is increased to the oxidation temperature at a rate of, for example, 50 to 400°C / hour. The oxidation step is carried out in an atmosphere containing, for example, air, oxygen, nitrogen, argon, or a mixture thereof.
[0096] The inside of the apparatus used for oxidation may be an oxygen-containing atmosphere containing a moderate amount of oxygen. The oxygen-containing atmosphere may be a mixed gas atmosphere of an inert gas and oxygen, or an inert gas atmosphere in the presence of an oxidizing agent.
[0097] The oxygen-containing atmosphere should have a sufficient amount of oxygen atoms present to oxidize the transition metal.
[0098] When the oxygen-containing atmosphere is a mixed gas atmosphere containing an inert gas and oxygen, the atmosphere inside the apparatus is controlled by a method of passing oxygen through the apparatus or a method of bubbling oxygen into the mixed liquid.
[0099] The oxidizing agent may be a peroxide such as hydrogen peroxide, a peroxide salt such as permanganate, a perchlorate, a hypochlorite, nitric acid, a halogen, or ozone.
[0100] [B-1-2] Lithium Compound The lithium compound used in the production of LiMO is, for example, at least one powder of lithium carbonate, lithium nitrate, lithium acetate, lithium hydroxide, lithium hydroxide monohydrate, lithium oxide, lithium chloride, and lithium fluoride. Of these, it is preferable to use at least one of lithium hydroxide, lithium hydroxide monohydrate, and lithium carbonate as the lithium compound.
[0101] The lithium compound and MCC are mixed in consideration of the composition ratio of the final target product to obtain a mixture of the lithium compound and MCC. The amount (molar ratio) of Li contained in the lithium compound relative to the total amount of elements other than oxygen atoms (Ni and element M) contained in MCC, which is 1, is preferably 0.90 to 1.10, more preferably 0.95 to 1.10, and even more preferably 0.98 to 1.07.
[0102] [B-2] Firing Step In the firing step, the mixture prepared in the mixing step is fired to produce a fired product.
[0103] In the firing step, it is preferable to carry out primary firing and secondary firing in sequence.
[0104] The primary firing is carried out under the following firing conditions, for example: Primary firing temperature (retention temperature): 500-900° C. Primary firing time (retention time): 1-50 hours
[0105] The primary firing temperature is more preferably 550-850°C, and even more preferably 600-700°C. When the primary firing temperature is equal to or higher than the lower limit of the above range, LiMO having a strong crystal structure can be obtained. Furthermore, when the primary firing temperature is equal to or lower than the upper limit of the above range, volatilization of lithium ions on the surface of LiMO particles can be reduced. Note that the primary firing temperature or the secondary firing temperature described below refers to the set temperature of the firing apparatus. When primary firing or secondary firing is performed multiple times, the primary firing temperature or secondary firing temperature refers to the temperature of the stage where firing is performed at the highest temperature among the multiple primary firing stages or secondary firing stages.
[0106] The primary firing is carried out in an atmosphere containing air, oxygen, nitrogen, argon, or a mixture of these gases, depending on the composition, and is preferably carried out in an oxygen atmosphere.
[0107] The secondary firing is carried out under the following firing conditions, for example: Secondary firing temperature rise rate: 80° C. / hour or more Secondary firing temperature (retention temperature): 600-900° C. Secondary firing time (retention time): 1-50 hours
[0108] The secondary firing is carried out in a state where oxygen gas is supplied. Specifically, the secondary firing is carried out so that the BET specific surface area FS1 of the powder of the primary fired product obtained in the primary firing, the oxygen flow rate FS2 during the secondary firing (when heating and maintaining the temperature), and the sheath filling amount FS3 during the secondary firing satisfy the relationship shown in the following (Equation X). In the secondary firing, the powder of the primary fired product is placed in the internal space of a sheath, which is a rectangular parallelepiped container. The sheath filling amount FS3 corresponds to the ratio of the bottom area FS31 of the internal space of the sheath to the layer height FS32 of the powder of the primary fired product placed in the internal space of the sheath (i.e., FS3 = FS32 / FS31).
[0109] 1.50≦(FS2 / FS1)*FS3≦5.20 ... (Formula X)
[0110] (FS2 / FS1)*FS3 is more preferably 1.7 or more, even more preferably 1.9 or more, and particularly preferably 2.3 or more. Furthermore, (FS2 / FS1)*FS3 is more preferably 5.15 or less, even more preferably 5.10 or less, and particularly preferably 5.05 or less. When (FS2 / FS1)*FS3 is within the above range, the degree of sintering, which is influenced by the amount of oxygen relative to the BET specific surface area of the primary sintered product, and the uniformity of sintering, which is influenced by the ratio of the layer height to the bottom surface in the internal space of the sheath, are controlled in an appropriate balance, enabling efficient production of LiMO having a pore structure that satisfies the relationships shown in (Equation A1) and (Equation A2). Furthermore, the Adp, V, Ap, SR, and AK of LiMO can be adjusted to the above-mentioned ranges.
[0111] (Method for measuring BET specific surface area) Nitrogen gas is used as the adsorption gas to measure the BET specific surface area of the primary fired product. 2 / g) is measured, for example, by drying 1 g of the primary fired product in a nitrogen atmosphere at a temperature of 105° C. for 30 minutes and then using a BET specific surface area meter (for example, Macsorb (manufactured by Mountech Co., Ltd.)).
[0112] FS2 is preferably 0.1-10 L / min. FS3 is preferably 200-2000 cm 3 is preferred.
[0113] The primary and secondary firings are carried out using firing apparatuses such as a continuous static firing furnace or a fluidized bed firing furnace. Examples of the continuous static firing furnace include a tunnel furnace or a roller hearth kiln. Examples of the fluidized bed firing furnace include a rotary kiln.
[0114] The first or second firing may be carried out in the presence of an inert flux. The inert flux is added to an extent that the initial capacity of the LiMO battery is not impaired, and may remain in the fired product. Examples of inert fluxes that can be used include those described in WO 2019 / 177032 A1.
[0115] The secondary firing temperature increase rate is more preferably 100° C. / hour or more, and even more preferably 150° C. / hour or more.
[0116] The secondary firing temperature is set to a temperature higher than the primary firing temperature. The secondary firing temperature is more preferably 650-850°C, and even more preferably 700-820°C. When the secondary firing temperature is equal to or higher than the lower limit of the above range, LiMO having a strong crystal structure can be obtained. In addition, excessive sintering can be suppressed.
[0117] The secondary firing time is more preferably 2 to 20 hours. When the secondary firing time is equal to or less than the upper limit of the range, volatilization of lithium ions is suppressed, and deterioration of battery performance is suppressed. When the secondary firing time is equal to or greater than the lower limit of the range, crystal growth is promoted, and deterioration of battery performance is suppressed.
[0118] After the firing step, crushing may be carried out as appropriate.
[0119] The fired product obtained in the firing step may be subjected to a post-treatment step and a drying step as appropriate, and may further be crushed and sieved.
[0120] [B-3] Post-treatment Step In the post-treatment step, the fired product obtained in the firing step is subjected to post-treatment. Examples of post-treatment include washing the fired product using a cleaning solution such as water, ion-exchanged water, an alkaline aqueous solution, or a sulfate aqueous solution to remove impurities. In this case, the slurry concentration is preferably 40% by mass or more. Examples of washing times include 5-20 minutes. The slurry concentration (mass %) refers to the ratio of the mass of the fired product (WS) to the total mass (WS+WL) of the fired product (WS) and the cleaning solution (WL) (i.e., 100*WS / (WS+WL)).
[0121] In the washing step, examples of the method for bringing the baking product into contact with the washing liquid include a method in which the baking product is placed in each washing liquid and stirred, a method in which each washing liquid is poured onto the baking product as a shower of water, and a method in which the baking product is placed in each washing liquid and stirred, and then the baking product is separated from each washing liquid, and then each washing liquid is poured onto the separated baking product as a shower of water.
[0122] The temperature of the cleaning solution used for cleaning is preferably 15° C. or less, more preferably 10° C. or less, and even more preferably 8° C. or less. By controlling the temperature of the cleaning solution within the above range, excessive elution of lithium ions from the crystal structure of the fired product into the cleaning solution during cleaning can be suppressed.
[0123] [B-4] Drying Step In the drying step, the fired product that has been subjected to the post-treatment in the post-treatment step is dried.
[0124] In the drying step, the fired product is dried, for example, at a temperature of 100 to 400° C. The drying can be carried out, for example, by reduced pressure drying, vacuum drying, air blowing, heating, or a combination thereof.
[0125] LiMO can be produced by the above steps.
[0126] [C] Battery evaluation
[0127] When LiMO is used for battery evaluation, a positive electrode is fabricated from LiMO, and then a lithium secondary battery is fabricated using the fabricated positive electrode.Then, the "3C discharge capacity" of the fabricated lithium secondary battery is measured as a battery evaluation.
[0128] [C-1] Preparation of Positive Electrode for Lithium Secondary Battery In preparing a positive electrode for a lithium secondary battery, first, a paste-like positive electrode mixture is prepared. The positive electrode mixture is prepared by kneading a mixture of LiMO, a conductive material, and a binder. Here, acetylene black is used as the conductive material, and PVdF is used as the binder. Then, the materials are mixed in the following proportions. When preparing the positive electrode mixture, N-methyl-2-pyrrolidone is used as the organic solvent.
[0129] LiMO: 92 parts by mass Conductive material: 5 parts by mass Binder: 3 parts by mass
[0130] The paste-like positive electrode mixture prepared as described above is then applied to a current collector (aluminum foil with a thickness of 40 μm). The current collector to which the positive electrode mixture is applied is then vacuum dried for 8 hours in an atmosphere at a temperature of 150° C., thereby completing a positive electrode for a lithium secondary battery. Here, the electrode area of the positive electrode for a lithium secondary battery is 1.65 cm2. 2 Let's say.
[0131] [C-2] Preparation of Lithium Secondary Battery When preparing a lithium secondary battery, first, the positive electrode prepared as described above is placed on the top surface of the bottom cover of a coin-type battery CR2032 part (manufactured by Hosen Co., Ltd.). When placing it on the bottom cover, the aluminum foil side of the positive electrode for the lithium secondary battery faces downward. Then, a separator is placed on the top surface of the bottom cover on which the positive electrode is placed. A 25 μm thick polyethylene porous film is used as the separator.
[0132] Next, 300 μl of electrolyte is injected into the part. Here, the electrolyte is a mixture of the following materials in the following proportions, to which 1% by volume of vinylene carbonate is added, and further, LiPF 6 The electrolyte is a solution containing LiPF 6 The concentration is adjusted to 1 mol / l.
[0133] Ethylene carbonate: 30 parts by volume Dimethyl carbonate: 35 parts by volume Ethyl methyl carbonate: 35 parts by volume
[0134] Next, the negative electrode is placed on top of the separator. Here, metallic lithium is used as the negative electrode. Then, a top cover is placed via a gasket and crimped using a crimping machine. This completes the lithium secondary battery.
[0135] [C-3] Measurement of "3C discharge capacity" The lithium secondary battery prepared above was allowed to stand at room temperature for 12 hours to allow the separator and the positive electrode active material layer to be sufficiently impregnated with the electrolyte, and then the "3C discharge capacity" was measured under the following conditions.
[0136] Treatment temperature: 25°C Maximum charging voltage: 4.3V, charging current: 1CA, constant current / constant voltage charging Minimum discharging voltage: 2.5V, discharging current: 3CA, constant current discharging
[0137] [D] Lithium Secondary Battery An example of a positive electrode for a lithium secondary battery using LiMO as a CAM and a lithium secondary battery including the positive electrode for the lithium secondary battery will be described below. Hereinafter, the positive electrode for a lithium secondary battery may be referred to as the positive electrode.
[0138] An example of a lithium secondary battery suitable for use with the LiMO of this embodiment as a CAM includes a positive electrode, a negative electrode, a separator sandwiched between the positive electrode and the negative electrode, and an electrolyte solution disposed between the positive electrode and the negative electrode.
[0139] 2 is a schematic diagram showing an example of a lithium secondary battery. For example, a cylindrical lithium secondary battery 10 is manufactured as follows.
[0140] First, as shown in the partially enlarged view of Fig. 2, a pair of strip-shaped separators 1, a strip-shaped positive electrode 2 having a positive electrode lead 21 attached to one end thereof, and a strip-shaped negative electrode 3 having a negative electrode lead 31 attached to one end thereof are prepared. Then, the separator 1, the positive electrode 2, the separator 1, and the negative electrode 3 are stacked in this order, and the stack is wound to produce an electrode group 4.
[0141] The positive electrode 2 includes, for example, a positive electrode active material layer 2 a containing LiMO and a positive electrode current collector 2 b having the positive electrode active material layer 2 a formed on one surface thereof. The positive electrode 2 can be manufactured by first preparing a positive electrode mixture containing LiMO, a conductive material, and a binder, and then supporting the positive electrode mixture on one surface of the positive electrode current collector 2 b to form the positive electrode active material layer 2 a.
[0142] Examples of the negative electrode 3 include an electrode in which a negative electrode mixture containing a negative electrode active material (not shown) is supported on a negative electrode current collector, and an electrode made of a negative electrode active material alone, and can be manufactured in the same manner as the positive electrode 2.
[0143] Next, the electrode group 4 and an insulator (not shown) are housed in a battery can 5, and the bottom of the battery can 5 is then sealed. Then, the electrode group 4 is impregnated with an electrolyte solution 6 in the battery can 5, thereby interposing an electrolyte (not shown) between the positive electrode 2 and the negative electrode 3. Thereafter, the top of the battery can 5 is sealed with a top insulator 7 and a sealing body 8. In this way, a lithium secondary battery 10 is completed.
[0144] The shape of the electrode group 4 can be, for example, a columnar shape such that the cross-sectional shape when the electrode group 4 is cut perpendicular to the winding axis is a circle, an ellipse, a rectangle, or a rectangle with rounded corners.
[0145] The shape of a lithium secondary battery having such an electrode group 4 can be any shape specified in IEC 60086, a standard established by the International Electrotechnical Commission (IEC), or JIS C 8500. Examples of shapes include a cylindrical shape and a rectangular shape.
[0146] Furthermore, the lithium secondary battery is not limited to the above-mentioned wound type configuration, and may be a stacked type configuration in which a stacked structure of a positive electrode, a separator, a negative electrode, and a separator is repeatedly stacked. Examples of stacked lithium secondary batteries include so-called coin type batteries, button type batteries, and paper type (or sheet type) batteries.
[0147] The positive electrode, separator, negative electrode, and electrolyte constituting the lithium secondary battery can be those described in, for example,
[0113] to
[0140] of WO2022 / 113904A1, and the materials and manufacturing methods therefor.
[0148] [E] All-Solid-State Lithium Secondary Battery The LiMO of this embodiment can be used as a CAM for an all-solid-state lithium secondary battery.
[0149] FIG. 3 is a schematic diagram showing an example of an all-solid-state lithium secondary battery.
[0150] 3, the all-solid-state lithium secondary battery 1000 includes a laminate 100 having a positive electrode 110, a negative electrode 120, and a solid electrolyte layer 130, and an exterior body 200 that houses the laminate 100. The all-solid-state lithium secondary battery 1000 may have a bipolar structure in which LiMO and a negative electrode active material are disposed on both sides of a current collector. Specific examples of bipolar structures include the structure described in JP-A-2004-95400.
[0151] The positive electrode 110 includes a positive electrode active material layer 111 and a positive electrode current collector 112. The positive electrode active material layer 111 contains the above-described LiMO and solid electrolyte. The positive electrode active material layer 111 may also contain a conductive material and a binder.
[0152] The negative electrode 120 includes a negative electrode active material layer 121 and a negative electrode current collector 122. The negative electrode active material layer 121 contains a negative electrode active material. The negative electrode active material layer 121 may also contain a solid electrolyte and a conductive material.
[0153] The laminate 100 may have an external terminal 113 connected to the positive electrode current collector 112 and an external terminal 123 connected to the negative electrode current collector 122. In addition, the all-solid-state lithium secondary battery 1000 may have a separator between the positive electrode 110 and the negative electrode 120.
[0154] The all-solid-state lithium secondary battery 1000 further includes an insulator (not shown) that insulates the laminate 100 from the exterior body 200 , and a sealing body (not shown) that seals the opening 200 a of the exterior body 200 .
[0155] The exterior body 200 is a container formed from a highly corrosion-resistant metal material such as aluminum, stainless steel, or nickel-plated steel. Alternatively, the exterior body 200 may be a bag-shaped container made of a laminate film having corrosion resistance on at least one surface.
[0156] The shape of the all-solid-state lithium secondary battery 1000 may be, for example, a coin type, a button type, a paper type (or a sheet type), a cylindrical type, a square type, or a laminate type (pouch type).
[0157] As an example, the all-solid-state lithium secondary battery 1000 has one laminate 100, but is not limited to this. The all-solid-state lithium secondary battery 1000 may have a configuration in which the laminate 100 is used as a unit cell, and a plurality of unit cells (laminated bodies 100) are sealed inside an exterior body 200.
[0158] For the all-solid-state lithium secondary battery, for example, the configuration, materials and manufacturing method described in paragraphs
[0151] to
[0181] of WO2022 / 113904A1 can be used.
[0159] Examples and comparative examples will be described below with reference to Table 1. In Table 1, (Example 1) to (Example 3) correspond to examples, and (Example C1) and (Example C2) correspond to comparative examples.
[0160]
[0161] [1] Sample Preparation The procedure for preparing the LiMO samples according to each example will be described below. The BET specific surface area of the primary fired product of each example was measured according to the method described above (Method for measuring BET specific surface area).
[0162] (Example 1)
[0163] First, water was placed in a reaction vessel equipped with a stirrer and an overflow pipe, and then an aqueous sodium hydroxide solution was added, and the liquid temperature was maintained at 70°C (temperature of the reaction vessel).
[0164] A nickel sulfate aqueous solution, a manganese sulfate aqueous solution, and an aluminum sulfate aqueous solution were mixed so that the ratio of [Ni]:[Mn]:[Al] would be the value shown in Table 1 (93:3.5:3.5 in Example 1), to prepare a mixed raw material solution 1.
[0165] Nitrogen gas was circulated in the reaction vessel, and an aqueous ammonium sulfate solution was continuously added as a complexing agent while stirring the mixed raw material liquid 1. Then, an aqueous sodium hydroxide solution was added dropwise at appropriate times until the pH of the mixed liquid in the reaction vessel reached 11.4 (measurement temperature: 40°C), thereby obtaining a reaction precipitate 1.
[0166] The reaction precipitate 1 was washed using a 5 mass % aqueous sodium hydroxide solution. The reaction precipitate 1 was washed using an aqueous sodium hydroxide solution in an amount 20 times the mass of the reaction precipitate 1. The washed reaction precipitate 1 was dehydrated using a centrifuge, then washed with water, and further dehydrated to isolate the reaction precipitate 1. The isolated reaction precipitate 1 was dried at 105°C for 20 hours to obtain a metal composite hydroxide 1 containing Ni, Mn, and Al.
[0167] Metal composite hydroxide 1 was oxidized in an air atmosphere at 650° C. for 5 hours to obtain a metal composite oxide MCC1.
[0168] Next, a powder of lithium hydroxide monohydrate prepared as a lithium compound was mixed with a powder of MCC1 to obtain a mixture 1. Here, the mixture was mixed in such a ratio that the amount (molar ratio) of Li contained in lithium hydroxide monohydrate relative to the total amount of Ni, Mn, and Al contained in MCC1 was 1.05, and a mixture 1 was obtained.
[0169] Mixture 1 was subjected to primary firing in an oxygen atmosphere at a holding temperature of 650° C. for a holding time of 5 hours to obtain primary fired product 1.
[0170] Next, the powder of the primary fired product 1 was placed in the internal space of the sheath. At this time, the sheath filling amount FS3 was the value shown in Table 1.
[0171] The primary fired product 1 was then subjected to secondary firing in an oxygen atmosphere at a temperature increase rate of 300°C / hour, a holding temperature of 750°C, and a holding time of 5 hours. The secondary firing was performed while oxygen gas was being supplied. The oxygen flow rate FS2 during the secondary firing (during the temperature increase and holding) was 3.0 L / min.
[0172] At this time, the value ((FS2 / FS1)*FS3) obtained by dividing the oxygen flow rate FS2 by the BET specific surface area FS1 of the primary fired product 1 and multiplying the sheath filling amount FS3 was the value shown in Table 1.
[0173] The obtained fired product 1 was mixed with pure water (liquid temperature: 5°C) to prepare a slurry. The slurry was prepared so as to contain 50 mass% of the fired product. The slurry was stirred for 20 minutes. The fired product 1 was then dried under a nitrogen atmosphere at 210°C for 10 hours.
[0174] As a result, a sample of LiMO1 having the composition (α, x, y) shown in Table 1 was obtained.
[0175] (Example 2) A nickel sulfate aqueous solution, a manganese sulfate aqueous solution, and an aluminum sulfate aqueous solution were added and mixed so that the [Ni]:[Mn]:[Al] ratio was as shown in Table 1, and a sodium hydroxide aqueous solution was added dropwise from time to time so that the pH of the mixed solution in the reaction vessel became 11.0 (measurement temperature: 40°C), and secondary firing was performed under the conditions where ((FS2 / FS1)*FS3) was as shown in Table 1. A sample was thus prepared in the same manner as in (Example 1). LiMO2 samples having the composition (α, x, y) shown in Table 1 were obtained.
[0176] (Example 3) A nickel sulfate aqueous solution, a manganese sulfate aqueous solution, and an aluminum sulfate aqueous solution were added and mixed so that the [Ni]:[Mn]:[Al] ratio was as shown in Table 1, and a sodium hydroxide aqueous solution was added dropwise from time to time so that the pH of the mixed solution in the reaction vessel became 11.2 (measurement temperature: 40°C), and secondary firing was performed under the conditions where ((FS2 / FS1)*FS3) was as shown in Table 1. A sample was thus prepared in the same manner as in (Example 1). LiMO3 samples having the composition (α, x, y) shown in Table 1 were obtained.
[0177] (Example C1) A sample was prepared in the same manner as in (Example 1), except that a sodium hydroxide aqueous solution was added dropwise at appropriate times so that the pH of the mixed solution in the reaction vessel became 12.2 (measurement temperature: 40°C), and secondary baking was performed under the conditions where ((FS2 / FS1)*FS3) is shown in Table 1. As a result, a LiMO4 sample having the composition (α, x, y) shown in Table 1 was obtained.
[0178] (Example C2) A sample was prepared in the same manner as in (Example 2), except that secondary firing was performed under the conditions for ((FS2 / FS1)*FS3) shown in Table 1. As a result, a LiMO5 sample having the composition (α, x, y) shown in Table 1 was obtained.
[0179] [2] Characteristics of the Samples The characteristics of the LiMO samples prepared for each example were determined. The results are shown in Table 1.
[0180] [2-1] Composition of LiMO The composition of LiMO was measured according to the method described above in <Method for measuring composition>. The amount of Co relative to the total amount of Ni and element M was calculated according to the above (Equation II).
[0181] [2-2] Pore characteristics of LiMO As shown in Table 1, dV1, dV2, V, Ap, and Adp were determined as the pore characteristics of LiMO according to the method described above in <Method for measuring pore volume ratio>.
[0182] [2-2] Other Properties of LiMO As shown in Table 1, SR and AK were determined as other properties of LiMO in each example according to the method described above in <Method for measuring metal site occupancy and average crystallite size>.
[0183] [3] Battery Evaluation As described above, the LiMO samples prepared in each example were subjected to battery evaluation as shown in Table 1. The battery evaluation was performed according to the method described above in "[C] Battery Evaluation."
[0184] [4] Summary The results of each example will be explained.
[0185] [4-1] Regarding (Example 1) to (Example 3) In (Example 1) to (Example 3), as shown in Table 1, the composition of LiMO satisfies the relationships shown in the above (Formula Ia), (Formula Ib), (Formula Ic), (Formula Id), and (Formula Id_1).
[0186] Furthermore, LiMO in (Example 1) to (Example 3) satisfies the relationships shown in (Formula A1) and (Formula A2). Furthermore, LiMO in (Example 1) to (Example 3) satisfies the relationships shown in (Formula B), (Formula C), (Formula D), (Formula E), and (Formula F).
[0187] As a result, the lithium secondary batteries of (Example 1) to (Example 3) had a 3C discharge capacity of 150 mAh / g or more, as shown in Table 1, and favorable results were obtained.
[0188] [4-2] Results of (Example C1) and (Example C2) As shown in the table, the LiMO compositions of (Example C1) and (Example C2) satisfy the relationships shown in (Formula Ia), (Formula Ib), (Formula Ic), (Formula Id), and (Formula Id_1) above. In addition, the LiMO of (Example C1) and (Example C2) satisfy the relationships shown in (Formula B), (Formula C), (Formula D), and (Formula F).
[0189] However, LiMO of (Example C1) does not satisfy the relationship shown in (Formula A1), and LiMO of (Example C2) does not satisfy the relationship shown in (Formula A2).
[0190] Therefore, as shown in Table 1, the lithium secondary batteries of (Example C1) and (Example C2) had a 3C discharge capacity of less than 150 mAh / g.
[0191] According to the present invention, it is possible to provide LiMO, CAM, a positive electrode for a lithium secondary battery, and a lithium secondary battery that can improve high-rate discharge capacity.
[0192] 1...Separator, 2...Positive electrode, 2a...Positive electrode active material layer, 2b...Positive electrode current collector, 3...Aggressive electrode, 4...Electrode group, 5...Battery can, 6...Electrolyte, 7...Top insulator, 8...Sealing body, 10...Lithium secondary battery, 21...Positive electrode lead, 31...Aggressive electrode lead, 100...Laminate, 110...Positive electrode, 111...Positive electrode active material layer, 112...Positive electrode current collector, 113...External terminal, 120...Aggressive electrode, 121...Aggressive electrode active material layer, 122...Aggressive electrode current collector, 123...External terminal, 130...Solid electrolyte layer, 200...Exterior body, 200a...Opening, 1000...All-solid-state lithium secondary battery
Claims
1. A lithium metal composite oxide containing Li, Ni, and an element M, wherein the element M is at least one element selected from the group consisting of Co, Mn, Fe, Cu, Ti, Mg, Ca, Al, Zn, Sn, Zr, B, Si, Nb, W, Ta, Ba, S, and P, and having pores, wherein in a pore size distribution calculated for the pores by the Barrett-Joyner-Halenda method from a nitrogen adsorption isotherm, a maximum value dV1 of a rate dVp / ddp of an increase in a pore volume Vp of the pore relative to an increase in a pore diameter dp of the pore in a range in which the rate dap / ddp of an increase in a pore surface area ap of the pore relative to an increase in a pore diameter dp of the pore satisfies the relationship "dap / ddp≦0.10", satisfies the relationship shown in the following (Formula A1), A lithium metal composite oxide, in which the maximum value dV2 of the dVp / ddp in the range where the dap / ddp satisfies the relationship of "dap / ddp>0.10" satisfies the relationship shown in the following (Formula A2): dV1≦1.00×10 -4 ...(Formula A1) dV2≧1.00×10 -4 ...(Formula A2) 2. The lithium metal composite oxide according to claim 1, wherein in the pore size distribution, the pore volume V satisfies the relationship shown in the following (Equation B). 3 / g≦V≦0.01 cm 3 / g...(Formula B) 3. The lithium metal composite oxide according to claim 1 or 2, wherein in the pore size distribution, the pore surface area Ap satisfies the relationship shown in the following (Formula C). 2 / g≦Ap≦2.0m 2 / g...(Formula C) 4. The lithium metal composite oxide according to claim 1 or 2, wherein in the pore size distribution, the average pore size Adp satisfies the relationship shown in the following (Formula D): 10 nm≦Adp≦40 nm ... (Formula D) 5. A lithium metal composite oxide represented by (composition formula I), in which M1 is at least one element selected from the group consisting of Mn, Al, and Co, and M2 is at least one element selected from the group consisting of Fe, Cu, Ti, Mg, Ca, Zn, Sn, Zr, B, Si, Nb, W, Ta, Ba, S, and P, satisfying the relationships shown in the following (formula Ia) to (formula Id). The lithium metal composite oxide according to claim 1 or 2. α (Ni (1-x-y) M1 x M2 y ) 1-α ]O 2 ... (Composition formula I) -0.1≦α≦0.2 ... (Formula Ia) 0≦x≦0.5 ... (Formula Ib) 0≦y≦0.7 ... (Formula Ic) 0<x+y<1 ... (Formula Id) 6. The lithium metal composite oxide according to claim 1 or 2, wherein the amount of Co relative to the total amount of Ni and the element M is 10 mol % or less.
7. The lithium metal composite oxide according to claim 5, wherein in (composition formula I), the relationship shown in the following (formula Id_1) is satisfied: 0<x+y≦0.15 (formula Id_1) 8. The lithium metal composite oxide according to claim 1 or 2, wherein the metal site occupancy rate SR obtained by Rietveld analysis satisfies the relationship shown in the following (Equation E): 1.0%≦SR≦4.0% ... (Equation E) 9. The lithium metal composite oxide according to claim 1 or 2, wherein the average crystallite size AK obtained by Rietveld analysis satisfies the relationship shown in the following formula F: 80 nm≦AK≦200 nm ... (formula F).
10. A positive electrode active material for a lithium secondary battery, comprising the lithium metal composite oxide according to claim 1 or 2.
11. A positive electrode for a lithium secondary battery, comprising the positive electrode active material for a lithium secondary battery according to claim 10.
12. A lithium secondary battery comprising the positive electrode for lithium secondary batteries according to claim 11.
Citation Information
Patent Citations
High density nickel hydroxide coprecipitated with cobalt and manganese, and method for producing the same
JP2002201028A
Bipolar battery and its control method
JP2004095400A
Electrode, non-aqueous electrolyte battery, and battery pack
WO2019069402A1
Lithium metal composite oxide powder, positive electrode active substance for lithium secondary battery, positive electrode, and lithium secondary battery
WO2019177032A1
Method for producing lithium metal composite oxide
WO2022113904A1