Liquid compression molding material, electronic component, and semiconductor device
The liquid compression molding material, composed of epoxy resin, phenolic, acid anhydride curing agents, and inorganic fillers, addresses warpage and curing speed issues in semiconductor devices by controlling glass transition temperature and curing agent ratios, enhancing the reliability and efficiency of semiconductor device manufacturing.
Patent Information
- Application Number
- PCT/JP2024/007869
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-29
- Filing Date
- 2024-03-01
- Publication Date
- 2024-12-05
AI Technical Summary
Conventional liquid compression molding materials for semiconductor devices suffer from warpage due to thermal contraction differences during the curing process, and they lack fast curing properties, which affect productivity and product reliability.
A liquid compression molding material comprising an epoxy resin, a phenolic curing agent, an acid anhydride curing agent, and an inorganic filler, with a glass transition temperature range of 50°C to 120°C, optimized to reduce warpage and enhance curing speed by controlling the ratio of phenolic to acid anhydride curing agents and incorporating a curing accelerator.
The material effectively suppresses warpage and achieves rapid curing, ensuring the stability and reliability of semiconductor devices by balancing thermal expansion and curing speed, thereby improving manufacturing efficiency.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Liquid compression molding material, electronic components and semiconductor devices
[0001] The present invention relates to a liquid compression molding material, and to an electronic component and a semiconductor device manufactured using the same.
[0002] Many semiconductor elements, such as integrated circuits, that constitute semiconductor devices are encapsulated with an encapsulant. Molding methods for encapsulating semiconductor elements can be broadly divided into two categories: (i) transfer molding, in which a molten curable resin composition is pressure-injected into a cavity through a channel, such as a runner or gate, that supplies the resin composition to the cavity, and then cured; and (ii) compression molding, in which a granular or liquid curable resin composition is supplied directly onto a substrate or release film and cured without using a channel, such as a runner or gate. Among these molding methods, compression molding, which is more suitable for producing relatively large molded products, has recently been increasingly adopted as a molding method for encapsulating semiconductor elements. This is due, among other things, to the increasing popularity of wafer-level chip-size packaging (packaging that employs a processing process in which wafers are encapsulated in the form of wafers that have not yet been cut into chips after circuit formation has been completed) as a packaging method for semiconductor elements. Furthermore, when encapsulating various elements, such as semiconductor elements, using an encapsulant, an organic substrate may be used as the substrate instead of a wafer made of an inorganic material, such as silicon.
[0003] Conventional curable resin compositions used for encapsulating various elements such as semiconductor elements by compression molding have mainly been solid resin compositions such as granular ones. However, with the recent development of new compression molding techniques, liquid curable resin compositions (so-called liquid compression molding materials) have been increasingly used. Hereinafter, liquid compression molding materials may be abbreviated as "LCM (Liquid Compression Molding) materials."
[0004] In compression molding using this LCM material, warping of the sealed article (a component in which elements arranged on a substrate (wafer or organic substrate) are sealed with the sealing material (cured LCM material)) after the LCM material has hardened but before dicing (single division) is a major problem. Because the LCM material contains a thermosetting resin, a heat treatment is performed during the LCM material molding process to promote the curing reaction. Then, in the subsequent cooling process, various elements such as semiconductor elements, the cured LCM material (sealant), and the substrate (wafer or organic substrate) shrink according to their respective thermal expansion coefficients, resulting in variations in the dimensional changes of each component. As a result, warping occurs in the sealed article. In light of this situation, technologies related to LCM material aimed at suppressing warping have been proposed (for example, Patent Document 1).
[0005] Japanese Patent Application Laid-Open No. 2006-232950
[0006] On the other hand, from the viewpoint of productivity, it is also important for LCM materials to have a short curing time (fast curing).
[0007] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a liquid compression molding material that suppresses warping of a sealed article and has excellent fast-curing properties, as well as electronic components and semiconductor devices manufactured using the same.
[0008] The above object can be achieved by the present invention as follows: A liquid compression molding material according to a first aspect of the present invention comprises a resin composition containing (A) an epoxy resin, (B1) a phenolic curing agent, (B2) an acid anhydride curing agent, and (C) an inorganic filler, and the cured product of the resin composition has a glass transition temperature Tg in the range of 50°C to 120°C.
[0009] A second liquid compression molding material of the present invention comprises a resin composition containing (A) an epoxy resin, (B1) a phenolic curing agent, (B2) an acid anhydride curing agent, and (C) an inorganic filler, and the content of the inorganic filler (C) relative to the entire resin composition is 55% by mass to 85% by mass.
[0010] In one embodiment of the liquid compression molding material of the first and second aspects of the present invention, the (B1) phenolic curing agent preferably includes at least one selected from the group consisting of phenol novolac resin, alkylated phenol novolac resin, allylated phenol novolac resin, cresol novolac resin, phenol aralkyl resin (provided that the resin contains a phenylene skeleton and / or a biphenylene skeleton), naphthol aralkyl resin, triphenolmethane resin, and dicyclopentadiene-type phenolic resin.
[0011] In another embodiment of the liquid compression molding material of the first and second aspects of the present invention, it is preferable that the (B2) acid anhydride curing agent contains at least one selected from the group consisting of phthalic anhydride, methyl himic anhydride, alkenyl-substituted succinic anhydride, methyl nadic anhydride, and glutaric anhydride.
[0012] In another embodiment of the liquid compression molding material of the first and second aspects of the present invention, the viscosity at room temperature (25° C.) is preferably 10 Pa·s to 1000 Pa·s.
[0013] In another embodiment of the liquid compression molding material of the first and second aspects of the present invention, the resin composition is heat-cured at 180°C for 60 minutes to obtain a cured product having an elastic modulus at 260°C of 0.05 GPa to 0.5 GPa.
[0014] In another embodiment of the liquid compression molding material of the first and second aspects of the present invention, the ratio of the phenol equivalent b1 of the (B1) phenolic curing agent to the acid anhydride equivalent b2 of the (B2) acid anhydride curing agent, b1:b2, is preferably 10:90 to 90:10. In another embodiment of the liquid compression molding material of the first and second aspects of the present invention, it is preferable that the material further contains a (D) curing accelerator.
[0015] The electronic component of the present invention comprises an encapsulant made of a cured product of the liquid compression molding material of the first or second invention.
[0016] The semiconductor device of the present invention comprises a substrate, a semiconductor element disposed on the substrate, and a cured product of the first or second liquid compression molding material of the present invention that seals a gap between the semiconductor element and the substrate.
[0017] According to the present invention, it is possible to provide a liquid compression molding material that suppresses warping of a sealed article and has excellent fast-curing properties, as well as electronic components and semiconductor devices manufactured using the same.
[0018] <LCM Material (First Embodiment)> The LCM material of the first embodiment is made of a resin composition containing (A) an epoxy resin, (B1) a phenolic curing agent, (B2) an acid anhydride curing agent, and (C) an inorganic filler, and the glass transition temperature Tg of the cured product of the resin composition is in the range of 50°C to 120°C. The glass transition temperature Tg is the temperature at which the loss tangent (tan δ) reaches its maximum value in the curve of change in loss tangent (tan δ) versus temperature measured by DMA (Dynamic Mechanical Analysis). Details of the measurement method will be described later.
[0019] Generally, the elastic modulus of a cured resin composition varies significantly across the glass transition temperature Tg, with the cured product having a relatively high elastic modulus in the temperature range below the glass transition temperature Tg when the cured product is in a glassy state, and a relatively low elastic modulus in the temperature range above the glass transition temperature Tg when the cured product is in a rubbery state. Meanwhile, in a compression molding process using an LCM material, the heating temperature during molding and the post-cure heating temperature performed after molding are typically above 130°C. For this reason, the LCM material of the first embodiment has a cured product with a glass transition temperature Tg of 120°C or lower. This allows the elastic modulus of the cured product to be significantly reduced near the heating temperature during molding or post-cure, thereby alleviating internal stresses caused by differences in the degree of shrinkage of the components constituting the sealed article during the cooling process after heating, thereby suppressing warpage of the sealed article. From the viewpoint of suppressing warpage and facilitating application of the LCM material of the first embodiment even when the heating temperature during molding and post-curing is lower than normal, the glass transition temperature Tg is preferably 110°C or lower, more preferably 100°C or lower, and even more preferably 90°C or lower.
[0020] Furthermore, in the LCM material of the first embodiment, a combination of a (B1) phenolic curing agent and a (B2) acid anhydride curing agent is used as the (B) curing agent. The phenolic curing agent lowers the glass transition temperature (Tg) of the cured product compared to when an acid anhydride curing agent alone is used as the curing agent. Therefore, it is necessary to use a phenolic curing agent as the (B) curing agent in order to control the glass transition temperature (Tg) of the cured product so that the cured product has an elastic modulus suitable for suppressing warpage during molding and post-cure heat treatment. However, due to the low reactivity of phenolic curing agents, using a phenolic curing agent alone as the curing agent does not ensure sufficient rapid curing. Therefore, the LCM material of the first embodiment also uses an acid anhydride curing agent, which is relatively more reactive than the phenolic curing agent. This allows the LCM material of the first embodiment to ensure excellent rapid curing.
[0021] However, acid anhydride curing agents have the effect of increasing the glass transition temperature Tg of the cured product. Therefore, considering that an acid anhydride curing agent must also be used in the LCM material of the first embodiment to ensure excellent fast curing properties, the glass transition temperature Tg is 50°C or higher. Note that the glass transition temperature Tg is preferably 60°C or higher, and more preferably 71.5°C or higher. Here, a suitable combination of the upper and lower limits of the glass transition temperature Tg can be any value selected from the multiple upper limits described above and any value selected from the multiple lower limits described above.
[0022] As is clear from the above explanation, the glass transition temperature Tg of the cured product can be controlled by appropriately selecting the ratio of the phenol equivalent b1 of the (B1) phenolic curing agent to the acid anhydride equivalent b2 of the (B2) acid anhydride curing agent. In addition, the glass transition temperature Tg can also be controlled by appropriately selecting, for example, the epoxy equivalent of the (A) epoxy resin or the degree of flexibility-rigidity of the molecular chain structure of the (A) epoxy resin. To give a specific example, reducing the epoxy equivalent can increase the crosslink density of the cured product, thereby increasing the glass transition temperature Tg, and using an epoxy resin with a highly rigid skeletal structure can increase the glass transition temperature Tg.
[0023] Next, details of the various components used in the LCM material of the first embodiment and other physical properties other than the glass transition temperature Tg will be described.
[0024] (A) Epoxy Resin The epoxy resin used in the LCM material of the first embodiment is not particularly limited as long as it is any of various epoxy resins commonly used for semiconductor encapsulation. However, from the viewpoint of easily ensuring a viscosity suitable for the LCM material, it is preferable to use a liquid epoxy resin as the epoxy resin. Furthermore, the epoxy resin blended into the LCM material may be a single type of epoxy resin, or two or more types of epoxy resins may be used in combination.
[0025] Specific examples of epoxy resins include aromatic epoxy resins and aliphatic epoxy resins. Examples of aromatic epoxy resins include bisphenol A-type epoxy resins such as p-glycidyloxyphenyldimethyltrisbisphenol A diglycidyl ether; bisphenol F-type epoxy resins; novolac-type epoxy resins; fluorene-type epoxy resins; biphenyl aralkyl epoxy resins; diepoxy resins such as p-tert-butylphenyl glycidyl ether and 1,4-phenyldimethanol diglycidyl ether; biphenyl-type epoxy resins such as 3,3',5,5'-tetramethyl-4,4'-diglycidyloxybiphenyl; aminophenol-type epoxy resins such as diglycidylaniline, diglycidyltoluidine, triglycidyl-p-aminophenol, and tetraglycidyl-m-xylylenediamine; naphthalene-type epoxy resins; and epoxy resins having a plant-derived skeleton.
[0026] Examples of aliphatic epoxy resins include monofunctional aliphatic epoxy compounds having one epoxy group in the molecule, such as alkyl alcohol glycidyl ethers (butyl glycidyl ether, 2-ethylhexyl glycidyl ether, etc.) and alkenyl alcohol glycidyl ethers (vinyl glycidyl ether, allyl glycidyl ether, etc.); difunctional aliphatic epoxy compounds having two epoxy groups in the molecule, such as polyalkylene glycol diglycidyl ethers (e.g., alkylene glycol diglycidyl ether, polytetramethylene glycol diglycidyl ether), and alkenylene glycol diglycidyl ether; and polyfunctional aliphatic epoxy compounds having three or more epoxy groups in the molecule, such as polyglycidyl ethers of trifunctional or higher alcohols (e.g., trimethylolpropane triglycidyl ether, pentaerythritol (tri- or tetra-)glycidyl ether, dipentaerythritol (tri-, tetra-, penta-, or hexa-)glycidyl ether, etc.).
[0027] Among the various epoxy resins listed above, liquid bisphenol type epoxy, liquid naphthalene type epoxy, and liquid aminophenol type epoxy are preferred from the viewpoint of workability.
[0028] The content of epoxy resin in the entire resin composition constituting the LCM material is preferably 5% by mass to 40% by mass, more preferably 5% by mass to 30% by mass, and even more preferably 8% by mass to 25% by mass.
[0029] (B) Curing Agent In the LCM material of the first embodiment, a combination of a phenolic curing agent (B1) and an acid anhydride curing agent (B2) is used as the curing agent (B). Both the phenolic curing agent and the acid anhydride curing agent can be used without any particular limitation as long as they are known curing agents.
[0030] Phenolic curing agents have the effect of lowering the glass transition temperature (Tg) of the cured product compared to acid anhydride curing agents. Phenolic curing agents can be any monomer, oligomer, or polymer containing a phenolic hydroxyl group, such as phenol novolac resin, alkylated phenol novolac resin, allylated phenol novolac resin, cresol novolac resin, phenol aralkyl resin (including a phenylene and / or biphenylene skeleton), naphthol aralkyl resin, triphenolmethane resin, and dicyclopentadiene-type phenolic resin. The phenolic curing agent blended into the resin composition constituting the LCM material may be a single phenolic curing agent or a combination of two or more phenolic curing agents. From the standpoint of workability, it is preferable to use a phenolic curing agent that is liquid at 25°C. Furthermore, from the standpoint of lowering the glass transition temperature (Tg) of the cured product, phenolic novolac resins with minimal steric hindrance are particularly preferred.
[0031] Acid anhydride curing agents reduce the viscosity of the resin composition constituting the LCM material and increase the glass transition temperature (Tg) of the cured product. Examples of acid anhydride curing agents include phthalic anhydride (e.g., alkylated hydrophthalic anhydrides such as methyltetrahydrophthalic anhydride and methylhexahydrophthalic anhydride; hexahydrophthalic anhydride, etc.), methyl hydric anhydride, alkenyl-substituted succinic anhydride, methyl nadic anhydride, and glutaric anhydride. The acid anhydride curing agent blended into the resin composition constituting the LCM material may be a single acid anhydride curing agent, or two or more acid anhydride curing agents may be used in combination. Among these acid anhydride curing agents, methyltetrahydrophthalic anhydride and methylhexahydrophthalic anhydride are preferred because they have excellent electrical insulation properties and heat resistance, and are liquid at room temperature (25°C).
[0032] The blending ratio of the (B1) phenolic curing agent to the (B2) acid anhydride curing agent is not particularly limited, but the ratio of the phenol equivalent b1 of the (B1) phenolic curing agent to the acid anhydride equivalent b2 of the (B2) acid anhydride curing agent, i.e., the equivalent ratio b1:b2, is preferably 10:90 to 90:10, more preferably 15:85 to 85:15, even more preferably 35:65 to 80:20, and particularly preferably 50:50 to 80:20. The phenol equivalent b1 is calculated as the mass of the (B1) component / the hydroxyl group equivalent in the (B1) component, and the acid anhydride equivalent b2 is calculated as the mass of the (B2) component / the acid anhydride group equivalent in the (B2) component.
[0033] When the equivalent ratio b1:b2 is within the range of 10:90 to 90:10, it becomes easier to adjust the glass transition temperature Tg to within the range of 50°C to 120°C and ensure excellent fast curing properties. In addition, it also becomes easier to lower the modulus of elasticity at 260°C (high-temperature modulus of elasticity). The mass ratio of the (B1) phenolic curing agent to the (B2) acid anhydride curing agent is not particularly limited as long as the equivalent ratio b1:b2 can be adjusted within the range of 10:90 to 90:10. However, the mass ratio is usually preferably 10:90 to 90:10, more preferably 15:85 to 85:15, and even more preferably 35:65 to 80:20.
[0034] The content of the (B) curing agent (i.e., (B1) phenolic curing agent and (B2) acid anhydride curing agent) in the entire resin composition constituting the LCM material is preferably 2% by mass or more, more preferably 5% by mass or more, and even more preferably 8% by mass or more, from the viewpoint of ensuring sufficient curability. On the other hand, the upper limit of the content is not particularly limited, but from the viewpoint of the blending balance with other components blended in the resin composition, in practical terms, it is preferably 50% by mass or less, more preferably 30% by mass or less, and even more preferably 20% by mass or less.
[0035] (C) Inorganic Filler The inorganic filler is not particularly limited as long as it has the effect of reducing the linear expansion coefficient of the cured product of the resin composition constituting the LCM material. Examples of inorganic filler materials include silica, alumina, aluminum, aluminum nitride, silicon carbide, and silicon nitride. As the inorganic filler, silica or alumina is particularly preferred from the viewpoint of being able to increase the blending amount (filling amount) of the inorganic filler in the resin composition. In addition, the inorganic filler may be surface-treated with a surface treatment agent such as a silane coupling agent. In addition, the inorganic filler blended in the resin composition may be a single type of inorganic filler, or two or more types of inorganic fillers may be used in combination.
[0036] The shape of the inorganic filler is not particularly limited and may be any of spherical, amorphous, scaly, etc. The average particle size of the inorganic filler is preferably 0.001 μm to 10 μm, more preferably 0.005 μm to 7 μm, even more preferably 0.01 μm to 5 μm, and particularly preferably 0.03 μm to 3 μm. The average particle size refers to the volume average particle size D50 (the particle size at 50% of the cumulative size from the small diameter side of the volume-based particle size distribution) value measured using a laser diffraction particle size distribution measuring device.
[0037] To further reduce the viscosity of the LCM material while maintaining a high inorganic filler content, it is preferable to use a combination of two inorganic fillers with different volume average particle diameters D50. In this case, the ratio (DL / DS) of the volume average particle diameter D50 (DL) of the large inorganic filler to the volume average particle diameter D50 (DS) of the small inorganic filler is preferably 4 to 30, more preferably 8 to 15, and the ratio (AL / AS) of the content (AL) of the large inorganic filler to the content (AS) of the small inorganic filler is preferably 1 to 5, more preferably 2 to 4.
[0038] The content of inorganic filler in the entire resin composition constituting the LCM material is usually 90% by mass or less from the practical viewpoint of ensuring a practical viscosity that can be handled and facilitating the preparation of the LCM material, and from the viewpoint of ensuring a viscosity suitable for compression molding, 85% by mass or less is preferred, more preferably 80% by mass or less, even more preferably 78.5% by mass or less, and particularly preferably 77% by mass or less. Also, from the viewpoint of reducing the thermal expansion coefficient of the cured product and further suppressing warping, 55% by mass or more is preferred, more preferably 61.5% by mass or more, even more preferably 65% by mass or more, even more preferably 67% by mass or more, and particularly preferably 70% by mass or more. Note that suitable combinations of the upper and lower limits of the inorganic filler content can be appropriately combined by selecting any value selected from the multiple upper limits described above and any value selected from the multiple lower limits described above.
[0039] Other Components The LCM material of the first embodiment may further contain other components in addition to the above components (A) to (C), as needed. The other components are not particularly limited, but examples thereof include (D) a curing accelerator.
[0040] Specific examples of the (D) curing accelerator include imidazoles, salts of triphenylphosphine or tetraphenylphosphine, modified imidazole compounds, etc. Specific examples include 2-methylimidazole, 2-ethylimidazole (2-phenylimidazole), 2-phenyl-4-methylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2-phenyl-4,5-dihydroxymethylimidazole, 2,4-diamino-6-(2'-methylimidazolyl-(1'))-ethyl-s-triazine isocyanuric acid adduct, epoxy-imidazole adduct compounds, and acrylate-imidazole adduct compounds. Furthermore, the curing accelerator blended into the resin composition constituting the LCM material may be a single type, or two or more types of curing accelerators may be used in combination. From the standpoint of pot life, acrylate-imidazole adduct compounds are preferred as curing accelerators.
[0041] The content of the curing accelerator (D) in the entire resin composition constituting the LCM material is preferably 0.1 mass % to 5.0 mass %, more preferably 0.3 mass % to 4.0 mass %, and even more preferably 0.5 mass % to 3.0 mass %.
[0042] In addition to components (A) to (D), other components that can be added as needed include coupling agents, pigments, ion trapping agents, leveling agents, antioxidants, antifoaming agents, flame retardants, colorants, reactive diluents, elastomers, and mold release agents. The amounts of these other components can be selected appropriately depending on their types. Of course, one or more of the other components listed above do not necessarily have to be included in the resin composition that constitutes the LCM material.
[0043] Next, preferred physical properties of the LCM material and its cured product of the first embodiment will be described. The cured LCM material preferably has a modulus of elasticity at 260°C (high-temperature modulus of elasticity) measured by DMA method of 0.05 GPa to 0.50 GPa, more preferably 0.05 GPa to 0.40 GPa, even more preferably 0.05 GPa to 0.30 GPa, and particularly preferably 0.05 GPa to 0.20 GPa. By setting the high-temperature modulus of elasticity within the above-mentioned range, the encapsulant (cured LCM material) in the encapsulating component can easily deform in response to the thermal expansion of the substrate or element in contact with the encapsulant during heat treatment at high temperatures.
[0044] The linear expansion coefficient of the cured LCM material in the temperature range below the glass transition temperature Tg is preferably 50 ppm / °C or less, and more preferably 40 ppm / °C or less. From the perspective of suppressing warping of the sealed article, a smaller linear expansion coefficient is preferable. However, since the cured LCM material always contains a certain proportion of a matrix that is prone to thermal expansion (a matrix formed by curing components (A) and (B)), the lower limit of the linear expansion coefficient is practically 10 ppm / °C or more. When the linear expansion coefficient of the cured LCM material is relatively high, warping usually tends to occur and become more pronounced. However, even in such cases, since the cured LCM material of the first embodiment has a glass transition temperature Tg of 120°C or less, as described above, warping is extremely easy to suppress.
[0045] The viscosity of the LCM material of the first embodiment at 25°C is preferably 1000 Pa·s or less, more preferably 600 Pa·s or less, and even more preferably 300 Pa·s or less. While the lower limit of the viscosity is not particularly limited, a practical viscosity of 10 Pa·s or more is preferred. Furthermore, resin compositions for transfer molding require high fluidity (low viscosity) in order to be pressurized and injected into a cavity via a gate or runner. However, LCM materials used in compression molding do not require pressurized injection when supplying the LCM material into a cavity, so adequate fluidity is sufficient. Taking this into consideration, the viscosity may be 110 Pa·s or more.
[0046] The gel time of the LCM material of the first embodiment is preferably 300 seconds or less, more preferably 250 seconds or less, and even more preferably 180 seconds or less, from the viewpoint of rapid curing when the LCM material is cured at 150° C. However, if the gel time is too short, there is a high possibility that the LCM material will harden after the start of supply by coating the LCM material onto a substrate or release film, etc., but before molding is carried out. Therefore, the lower limit of the gel time is preferably around 100 to 120 seconds or more in practice, although this depends on the operating speed of the compression molding device actually used.
[0047] The LCM material of the first embodiment is prepared by mixing and stirring a mixture containing at least the essential components (A) to (C) constituting the LCM material, with optional addition of other components. Known mixing and stirring means, such as a roll mill or planetary mixer, can be used as appropriate for the mixing and stirring. When the (A) epoxy resin used to prepare the LCM material is solid, it is preferable to liquefy or fluidize the epoxy resin by heating or other means before mixing it with the remaining components. The mixing and stirring procedure is not particularly limited. For example, all components constituting the LCM material may be mixed simultaneously, or a premix may be prepared by first mixing only some of the components, and then the remaining components may be mixed into this premix. If it is difficult to uniformly disperse the (C) inorganic filler in the (A) epoxy resin, a premix may be prepared by first mixing the (A) epoxy resin and the (C) inorganic filler, and then the remaining components may be mixed into this premix.
[0048] LCM Material (Second Embodiment) The LCM material of this second embodiment comprises a resin composition containing (A) an epoxy resin, (B1) a phenolic curing agent, (B2) an acid anhydride curing agent, and (C) an inorganic filler, with the content of the inorganic filler (C) being 55% to 85% by mass relative to the total resin composition. By limiting the content of the inorganic filler to 85% by mass or less, warping can be suppressed, and by limiting the content to 55% by mass or more, excellent rapid curing properties can be obtained. The upper limit of the inorganic filler content is preferably 80% by mass or less, more preferably 78.5% by mass or less, and even more preferably 77% by mass or less. The lower limit is preferably 61.5% by mass or more, more preferably 65% by mass or more, even more preferably 67% by mass or more, and particularly preferably 70% by mass or more. Suitable combinations of the upper and lower limits of the inorganic filler content include any combination of a value selected from the above-described upper limit values and a value selected from the above-described lower limit values.
[0049] The glass transition temperature Tg of the cured product of the LCM material of the second embodiment is not particularly limited, but is preferably the same as that of the LCM material of the first embodiment. Furthermore, other factors than the content of inorganic filler and the glass transition temperature Tg can be the same as those of the LCM material of the first embodiment.
[0050] <Electronic Components and Semiconductor Devices> The cured products of the LCM materials of the first and second embodiments can be used as encapsulants for various electronic components. The electronic components of the present embodiments are not particularly limited in terms of the substrate material or the type of element, as long as they include a substrate such as a wafer or organic substrate, various elements such as semiconductor elements arranged on the substrate, and an encapsulant (the cured product of the LCM material of the first or second embodiment) that seals the gap between the elements and the substrate, but are particularly preferably semiconductor devices.
[0051] Specific examples of the present invention will be described below with reference to examples, but the present invention is not limited to the examples described below.
[0052] 1. Preparation of Epoxy Resin Compositions The LCM materials of Examples 1 to 23 and Comparative Examples 1 to 3 were prepared by mixing and stirring the raw materials using a roll mill so as to obtain the blending amounts shown in Tables 1 to 3. Details of each component used as a raw material are as follows. The blending amount of each component shown in the tables is in parts by mass.
[0053] 2. Raw material components used in preparing LCM material (A) Epoxy resins YDF-870GS (bisphenol F type epoxy resin: manufactured by Nippon Steel Chemical & Material) HP-4032D (naphthalene type epoxy resin: manufactured by DIC) jER630LSD (aminophenol type epoxy resin: manufactured by Mitsubishi Chemical) YX7400 (liquid epoxy resin: manufactured by Mitsubishi Chemical) (B1) Phenol-based hardeners MEH-8005 (liquid phenol novolac resin: manufactured by UBE, hydroxyl group equivalent: 135 g / eq) BRM-553 (solid phenol novolac resin: manufactured by AICA Kogyo, hydroxyl group equivalent: 108 g / eq) (B2) Acid anhydride-based hardeners HN-5500 (methylhexahydrophthalic anhydride: manufactured by Resonac, acid anhydride group equivalent: 168 g / eq)・HN-2200 (methyltetrahydrophthalic anhydride: manufactured by Resonac, acid anhydride group equivalent: 166 g / eq) ・MH-700 (mixture of 4-methylhexahydrophthalic anhydride and hexahydrophthalic anhydride: manufactured by New Japan Chemical Co., Ltd., acid anhydride group equivalent: 163 g / eq) (C) Inorganic fillers ・SE2200-SME (methacrylic surface-treated silica filler, average particle size: 0.5 μm, manufactured by Admatechs) ・YA050C-SM1 (methacrylic surface-treated silica filler, average particle size: 0.05 μm, manufactured by Admatechs) ・FB7SDX (silica filler, average particle size: 7 μm, manufactured by Denka) ・AG2051 SXM (phenylamino surface-treated alumina filler, average particle size: 1 μm, manufactured by Admatechs)
[0054] Other components (D) Curing accelerator: HX-3088FR (core-shell type curing accelerator: manufactured by Asahi Kasei) 2MA-OK (curing accelerator: manufactured by Shikoku Chemical Industry Co., Ltd.) Coupling agent: KBM-403 (silane coupling agent: manufactured by Shin-Etsu Chemical Co., Ltd.) Pigment: Special Black 4 (pigment: manufactured by Orien Engineered Carbons)
[0055] 3. Various Measurement and Evaluation Methods The following describes i) methods for measuring the glass transition temperature (Tg), coefficient of linear expansion (CTE), and high-temperature modulus of elasticity of the cured LCM material, ii) methods for measuring the viscosity of the LCM material, and iii) methods for evaluating the warpage and gel time of a component fabricated to resemble a semiconductor device. These measurement and evaluation methods were established based on a typical semiconductor device manufacturing process: The LCM material is applied to a release film at room temperature (25°C), the release film is placed in the lower mold of a compression molding machine heated to 150°C, and the mold is then combined with a substrate placed in the upper mold at 150°C (compression molding that also serves as a preliminary cure), followed by a post-cure (main cure) at 180°C for 60 minutes, followed by a reflow at 260°C.
[0056] (Glass Transition Temperature Tg) The glass transition temperature Tg of the LCM material was measured by DMA (Dynamic Mechanical Analysis) using a DMS6100 from Seiko Instruments Inc. (SII) on a cured product obtained by heat-curing the LCM material at 180°C for 60 minutes. The glass transition temperature Tg is the temperature at which the loss tangent (tanδ) reaches its maximum value in the change curve of tanδ versus temperature measured by the DMA method. Tanδ is calculated by dividing the loss modulus at a given temperature by the storage modulus at that temperature.
[0057] (Coefficient of Linear Expansion CTE) The coefficient of linear expansion CTE of the LCM material was measured by TMA (Thermomechanical Analysis) using a Bruker TMA4000SA on a measurement sample prepared by heat-curing the LCM material at 180°C for 60 minutes and processing the cured material into a predetermined shape. The slope in the 30°C-50°C range was determined based on the length of the measurement sample at 30°C and the length of the measurement sample at 50°C, and this slope was determined as the coefficient of linear expansion CTE.
[0058] (High-Temperature Elastic Modulus) The high-temperature elastic modulus of the LCM material was measured by heat-curing the LCM material at 180°C for 60 minutes, followed by dynamic mechanical analysis (DMA) using a DMS6100 manufactured by SII Corp. The storage modulus at 260°C was determined as the high-temperature elastic modulus.
[0059] (Viscosity) The viscosity of the LCM material was measured at 25° C. using a Brookfield DV-1 type viscometer at a rotation speed of 20 rpm.
[0060] (Warpage) Warpage was evaluated using the following procedure. First, the upper and lower molds in the compression molding machine were heated to 150°C, and then an FR4 substrate (GN74240: manufactured by Global Net Co., Ltd.) measuring 74 mm in length, 240 mm in width, and 300 μm in thickness was placed on the upper mold. Next, an LCM material was applied to the release film, and the release film was placed on the lower mold in the compression molding machine with the LCM-coated side facing up. The lower mold was then operated, and compression molding was performed at 150°C / 300 seconds. The size of the cured product formed on the FR4 substrate was 67 mm in length, 233 mm in width, and 250 μm in thickness. After compression molding was completed, the FR4 substrate on which the cured product had been formed was removed from the mold and placed in a dryer set to 180°C for 1 hour. This resulted in the preparation of an evaluation sample in which a layer of cured LCM material was formed on one side of the FR4 substrate. Next, this evaluation sample was placed on a horizontal table so that the surface on which the cured product layer was formed faced upward. In this state, the distance from the lower surface of the evaluation sample to the table was measured. The measurement was performed on the four corners of the evaluation sample, and the maximum value of the measured values at these four corners was taken as the warpage value.
[0061] (Gel Time) The gel time of the LCM material was measured using an automatic curing time measuring device "Madoka" manufactured by Matsuo Sangyo Co., Ltd. under measurement conditions of a rotation speed of 120 rpm, a test temperature of 150°C, and a sample volume of 0.3 ml. The shorter the gel time, the better the rapid curing property. However, if the gel time is too short, there is a high possibility that the LCM material will harden after the start of supply by coating the LCM material onto the substrate or release film, etc., but before molding. Therefore, the lower limit of the gel time is practically around 100 to 120 seconds or more, although it depends on the operating speed of the compression molding device actually used.
[0062] 4. Evaluation Results Tables 1 to 3 show the compounding compositions of the LCM materials of the examples and comparative examples, as well as the results of various measurements and evaluations.
[0063]
[0064]
[0065]
Claims
1. A liquid compression molding material comprising a resin composition containing (A) an epoxy resin, (B1) a phenol-based curing agent, (B2) an acid anhydride-based curing agent, and (C) an inorganic filler, wherein the glass transition temperature Tg of the cured product of the resin composition is in the range of 50°C to 120°C.
2. A liquid compression molding material comprising a resin composition containing (A) an epoxy resin, (B1) a phenol-based curing agent, (B2) an acid anhydride-based curing agent, and (C) an inorganic filler, wherein the content of the inorganic filler (C) in the entire resin composition is 55% by mass to 85% by mass.
3. The liquid compression molding material according to claim 1 or 2, wherein the (B1) phenol-based hardener comprises at least one selected from the group consisting of phenol novolac resins, alkylated phenol novolac resins, allylated phenol novolac resins, cresol novolac resins, phenol aralkyl resins (resins containing a phenylene skeleton and / or a biphenylene skeleton), naphthol aralkyl resins, triphenolmethane resins, and dicyclopentadiene-type phenolic resins.
4. The liquid compression molding material according to any one of claims 1 to 3, wherein the (B2) acid anhydride-based curing agent includes at least one selected from the group consisting of phthalic anhydride, methyl hymic anhydride, succinic anhydride substituted with an alkenyl group, methyl nadic anhydride, and glutaric anhydride.
5. The liquid compression molding material according to any one of claims 1 to 4, having a viscosity at room temperature (25°C) of 10 Pa·s to 1000 Pa·s.
6. The liquid compression molding material according to any one of claims 1 to 5, wherein the elastic modulus of the cured material obtained by heat curing the resin composition at 180°C for 60 minutes is in the range of 0.05 GPa to 0.5 GPa at 260°C.
7. The liquid compression molding material according to any one of claims 1 to 6, wherein the ratio of the phenol equivalent b1 of the (B1) phenol-based curing agent to the acid anhydride equivalent b2 of the (B2) acid anhydride-based curing agent, b1:b2, is 10:90 to 90:
10.
8. The liquid compression molding material according to any one of claims 1 to 7, further comprising (D) a curing accelerator.
9. An electronic component comprising a sealing material made of a cured product of the liquid compression molding material according to any one of claims 1 to 8.
10. A semiconductor device comprising: a substrate; a semiconductor element disposed on the substrate; and a hardened liquid compression molding material according to any one of claims 1 to 8, which seals a gap between the semiconductor element and the substrate.
Citation Information
Patent Citations
Epoxy resin casting composition
JP1989185318A
Thermosetting flux and solder paste
JP2005059028A
Method of manufacturing semiconductor light-emitting apparatus, and semiconductor light emitting apparatus
JP2011138985A
Epoxy resin composition for sealing optical semiconductor device and optical semiconductor device using the same
JP2011236318A
Thermosetting resin composition with diene / dienophile pair and repairability
JP2016514738A