Multilayer ceramic capacitor

The integration of dummy electrodes within the multilayer ceramic capacitors addresses structural defects and moisture issues by maintaining uniform thickness and preventing exposure, thereby enhancing the capacitors' reliability and performance.

WO2024247445A1PCT designated stage expired Publication Date: 2024-12-05MURATA MFG CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/010405
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-02
Filing Date
2024-03-18
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Multilayer ceramic capacitors face structural defects due to step differences in thickness between internal electrode layers, leading to issues like peeling and moisture infiltration.

Method used

Incorporating dummy electrodes that are not exposed from the surface, these electrodes are arranged apart from the internal electrode layers and share the same plane, effectively eliminating step differences and enhancing structural integrity.

Benefits of technology

The solution effectively suppresses structural defects such as peeling and improves moisture resistance by ensuring uniform thickness and preventing moisture infiltration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024010405_05122024_PF_FP_ABST
    Figure JP2024010405_05122024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a multilayer ceramic capacitor capable of suppressing the occurrence of structural defects with respect to the multilayer ceramic capacitor. A multilayer ceramic capacitor according to the present invention comprises: a laminate that includes a plurality of laminated dielectric layers and a plurality of internal electrode layers laminated on the dielectric layers, and that has a first main surface and a second main surface opposite to each other in the lamination direction, a first lateral surface and a second lateral surface opposite to each other in the width direction orthogonal to the lamination direction, and a first end surface and a second end surface opposite to each other in the longitudinal direction orthogonal to the lamination direction and to the width direction; a first external electrode disposed on the first end surface; a second external electrode disposed on the second end surface; a third external electrode disposed on the first lateral surface; and a fourth external electrode disposed on the second lateral surface. The plurality of internal electrode layers include: a first internal electrode layer disposed on one of the plurality of dielectric layers and connected to the first external electrode and the second external electrode; a second internal electrode layer that is disposed on one of the plurality of dielectric layers different from the one having the first internal electrode layer disposed thereon, and that is connected to the third external electrode and the fourth external electrode; and a first dummy electrode separated from the first internal electrode layer and disposed on the same surface as the first internal electrode layer. The first dummy electrode is not exposed from the first lateral surface, the second lateral surface, the first end surface, and the second end surface.
Need to check novelty before this filing date? Find Prior Art

Description

Multilayer ceramic capacitors

[0001] The present invention relates to a multilayer ceramic capacitor.

[0002] Known multilayer ceramic capacitors include three-terminal capacitors, also known as multilayer feedthrough capacitors, which are used for noise reduction in electronic devices, etc. This three-terminal capacitor generates capacitance by having a first internal electrode extending to opposing surfaces A and a second internal electrode extending to surface B perpendicular to surface A, facing each other with a dielectric interposed therebetween. Such a multilayer capacitor is disclosed, for example, in Patent Document 1 (see Patent Document 1).

[0003] JP 2013-45808 A

[0004] However, as shown in the multilayer ceramic capacitor described in Patent Document 1, there are regions where only the first internal electrode is present in the stacking direction, regions where only the second internal electrode is present in the stacking direction, and regions where neither the first internal electrode nor the second internal electrode is present, which creates steps corresponding to the thickness of each internal electrode and may result in structural defects.

[0005] SUMMARY OF THE INVENTION Therefore, a primary object of the present invention is to provide a multilayer ceramic capacitor that can suppress the occurrence of structural defects in the multilayer ceramic capacitor.

[0006] A multilayer ceramic capacitor according to the present invention comprises a laminate including a plurality of laminated dielectric layers and a plurality of internal electrode layers laminated on the dielectric layers, the laminate having first and second main surfaces opposing each other in the lamination direction, first and second side surfaces opposing each other in a width direction perpendicular to the lamination direction, and first and second end surfaces opposing each other in a length direction perpendicular to the lamination direction and the width direction; a first external electrode disposed on the first end surface, a second external electrode disposed on the second end surface, a third external electrode disposed on the first side surface, and a fourth external electrode disposed on the second side surface. the plurality of internal electrode layers include a first internal electrode layer disposed on a plurality of dielectric layers and connected to the first external electrode and the second external electrode; a second internal electrode layer disposed on a plurality of dielectric layers different from the first internal electrode layer and connected to the third external electrode and the fourth external electrode; and a first dummy electrode spaced apart from the first internal electrode layer and disposed on the same plane as the first internal electrode layer, wherein the first dummy electrode is not exposed from the first side surface, the second side surface, the first end face, and the second end face.

[0007] The multilayer ceramic capacitor according to the present invention has a first dummy electrode that is spaced apart from the first internal electrode layer and that is arranged on the same plane as the first internal electrode layer, and the first dummy electrode is not exposed from the first side surface, the second side surface, the first end face, and the second end face, so that structural defects such as peeling due to steps corresponding to the thickness of the internal electrode layer between each dielectric layer can be suppressed.

[0008] According to the present invention, a multilayer ceramic capacitor capable of suppressing the occurrence of structural defects in the multilayer ceramic capacitor is provided.

[0009] The above and other objects, features and advantages of the present invention will become more apparent from the following detailed description of the preferred embodiments of the present invention, which proceeds with reference to the accompanying drawings.

[0010] FIG. 1 is an external perspective view showing an example of a multilayer ceramic capacitor (three-terminal multilayer ceramic capacitor) according to an embodiment of the present invention. FIG. 2 is a top view showing an example of a multilayer ceramic capacitor according to an embodiment of the present invention. FIG. 3 is a front view showing an example of a multilayer ceramic capacitor according to an embodiment of the present invention. FIG. 4 is a cross-sectional view taken along line IV-IV in FIG. 1. FIG. 5 is a cross-sectional view taken along line V-V in FIG. 1. FIG. 6 is a cross-sectional view taken along line VI-VI in FIG. 4. FIG. 7 is a cross-sectional view taken along line VII-VII in FIG. 4. FIG. 8 is a cross-sectional view showing a modified example of the first dummy electrode shown in FIG. 6. FIG. 9 is a cross-sectional view showing a modified example of the second dummy electrode shown in FIG. 7. FIG. 10 is a schematic cross-sectional view illustrating the arrangement of the first dummy electrode used in an experimental example. FIG. 11 is a schematic cross-sectional view illustrating the arrangement of the second dummy electrode used in an experimental example. FIG. 12 is a schematic cross-sectional view illustrating a method for measuring the width direction dimension of the dummy electrode in the experimental example.

[0011] 1. Multilayer Ceramic Capacitor A multilayer ceramic capacitor (three-terminal multilayer ceramic capacitor) according to the present invention will be described.

[0012] FIG. 1 is an external perspective view showing an example of a multilayer ceramic capacitor (three-terminal multilayer ceramic capacitor) according to an embodiment of the present invention. FIG. 2 is a top view showing an example of a multilayer ceramic capacitor according to an embodiment of the present invention. FIG. 3 is a front view showing an example of a multilayer ceramic capacitor according to an embodiment of the present invention. FIG. 4 is a cross-sectional view taken along line IV-IV in FIG. 1. FIG. 5 is a cross-sectional view taken along line VV in FIG. 1. FIG. 6 is a cross-sectional view taken along line VI-VI in FIG. 4. FIG. 7 is a cross-sectional view taken along line VII-VII in FIG. 4.

[0013] As shown in FIG. 1 , the multilayer ceramic capacitor 10 includes a laminate 12 and external electrodes 30 .

[0014] The laminate 12 has a plurality of dielectric layers 14 stacked one on top of the other, and a plurality of internal electrode layers 16 stacked on the dielectric layers 14. The dielectric layers 14 and the internal electrode layers 16 are stacked in a stacking direction x.

[0015] The laminate 12 has a substantially rectangular parallelepiped shape. The dimension of the laminate 12 in the length direction z is not necessarily longer than the dimension in the width direction y. The laminate 12 has a first main surface 12a and a second main surface 12b facing in the stacking direction x, a first side surface 12c and a second side surface 12d facing in the width direction y perpendicular to the stacking direction x, and a first end surface 12e and a second end surface 12f facing in the length direction z perpendicular to the stacking direction x and the width direction y.

[0016] The corners and ridges of this laminate 12 are rounded. The rounding prevents chipping and cracking of the laminate 12. A corner refers to a portion where three adjacent surfaces of the laminate intersect, and a ridge refers to a portion where two adjacent surfaces of the laminate intersect. Furthermore, the first main surface 12a and the second main surface 12b, the first side surface 12c and the second side surface 12d, and the first end surface 12e and the second end surface 12f may be partially or entirely uneven or have a roughened surface. The dielectric layers 14 and the internal electrode layers 16 are stacked in the stacking direction x.

[0017] As shown in Figures 4 and 5, the laminate 12 has, in the stacking direction x connecting the first main surface 12a and the second main surface 12b, an inner layer portion 18 in which a plurality of internal electrode layers 16 face each other, a first main surface side outer layer portion 20a formed from a plurality of dielectric layers 14 located between the first main surface 12a and the internal electrode layer 16 located closest to the first main surface 12a, and a second main surface side outer layer portion 20b formed from a plurality of dielectric layers 14 located between the second main surface 12b and the internal electrode layer 16 located closest to the second main surface 12b.

[0018] The first main surface side outer layer portion 20a is located on the first main surface 12a side of the laminate 12 and is an assembly of multiple dielectric layers 14 located between the first main surface 12a and the internal electrode layer 16 closest to the first main surface 12a.

[0019] The second main surface side outer layer portion 20b is located on the second main surface 12b side of the laminate 12 and is an assembly of multiple dielectric layers 14 located between the second main surface 12b and the internal electrode layer 16 closest to the second main surface 12b.

[0020] The region sandwiched between the first main surface side outer layer portion 20 a and the second main surface side outer layer portion 20 b is the inner layer portion 18 .

[0021] The dimensions of the laminate 12 are not particularly limited, but it is preferable that the dimension in the length direction z is 0.7 mm or more and 3.3 mm or less, the dimension in the width direction y is 0.3 mm or more and 1.4 mm or less, and the dimension in the stacking direction x is 0.2 mm or more and 0.7 mm or less.

[0022] The dielectric layer 14 can be formed of, for example, a dielectric material. Examples of such dielectric materials include dielectric ceramics containing components such as BaTiO3, CaTiO3, SrTiO3, or CaZrO3. When the dielectric material is a primary component, it may contain a secondary component, such as a manganese compound, an iron compound, a chromium compound, a cobalt compound, or a nickel compound, in a smaller amount than the primary component, depending on the desired characteristics of the laminate 12.

[0023] The thickness of the dielectric layer 14 after firing is preferably 0.7 μm or more and 1.3 μm or less. The number of dielectric layers 14 to be stacked is not particularly limited, but is preferably 200 to 500.

[0024] The laminate 12 has a plurality of first internal electrode layers 16a and a plurality of second internal electrode layers 16b as the plurality of internal electrode layers 16. The plurality of first internal electrode layers 16a and the plurality of second internal electrode layers 16b are embedded so as to be alternately arranged at equal intervals with the dielectric layers 14 sandwiched between them along the lamination direction x of the laminate 12.

[0025] 6 , the first internal electrode layer 16a includes a first opposing electrode portion 22a that faces the second internal electrode layer 16b via the dielectric layer 14, a first extraction electrode portion 24a that is extracted from the first opposing electrode portion 22a to the surface of the first end face 12e of the laminate 12, and a second extraction electrode portion 24b that is extracted from the first opposing electrode portion 22a to the surface of the second end face 12f of the laminate 12. Specifically, the first extraction electrode portion 24a is exposed on the surface of the first end face 12e of the laminate 12, and the second extraction electrode portion 24b is exposed on the surface of the second end face 12f of the laminate 12. Therefore, the first internal electrode layer 16a is not exposed on the surfaces of the first side face 12c and the second side face 12d of the laminate 12.

[0026] The shapes of the first opposing electrode portion 22a and the first and second extracted electrode portions 24a and 24b are not particularly limited, but are preferably short rectangles, although the corners of the first opposing electrode portion 22a and the first and second extracted electrode portions 24a and 24b may be rounded.

[0027] Furthermore, the length in the width direction y of the first extraction electrode portion 24a and the second extraction electrode portion 24b may be formed to be the same length as the length in the width direction y of the first opposing electrode portion 22a, or may be formed to be shorter than the length in the width direction y of the first opposing electrode portion 22a.

[0028] Furthermore, the shape of the first extraction electrode portion 24a may be tapered so that its length in the width direction y narrows toward the first end face 12e, and the shape of the second extraction electrode portion 24b may be tapered so that its length in the length direction z narrows toward the second end face 12f.

[0029] 7 , the second internal electrode layer 16b has a generally cross shape and includes a second opposing electrode portion 22b that faces the first internal electrode layer 16a via the dielectric layer 14, a third extraction electrode portion 24c that is extracted from the second opposing electrode portion 22b to the surface of the first side surface 12c of the laminate 12, and a fourth extraction electrode portion 24d that is extracted from the second opposing electrode portion 22b to the surface of the second side surface 12d of the laminate 12. Specifically, the third extraction electrode portion 24c is exposed on the surface of the first side surface 12c of the laminate 12, and the fourth extraction electrode portion 24d is exposed on the surface of the second side surface 12d of the laminate 12. Therefore, the second internal electrode layer 16b is not exposed on the surface of the first end face 12e or the surface of the second end face 12f of the laminate 12.

[0030] The shapes of the second opposing electrode portion 22b and the third and fourth extraction electrode portions 24c and 24d are not particularly limited, but are preferably short rectangles, although the corners of the second opposing electrode portion 22b and the third and fourth extraction electrode portions 24c and 24d may be rounded.

[0031] Furthermore, the shape of the third extraction electrode portion 24c may be tapered so that its length in the longitudinal direction z narrows toward the first side surface 12c, and the shape of the fourth extraction electrode portion 24d may be tapered so that its length in the longitudinal direction z narrows toward the second side surface 12d.

[0032] The first internal electrode layers 16a and the second internal electrode layers 16b may be alternately laminated with the dielectric layers 14 interposed therebetween, or a plurality of dielectric layers 14 on which the first internal electrode layers 16a are arranged may be laminated, and then a dielectric layer 14 on which the second internal electrode layers 16b are arranged may be laminated. In this way, the lamination pattern of the internal electrode layers 16 can be changed depending on the capacitance value that is desired to be realized.

[0033] The laminate 12 has a side portion (W gap) 26a of the laminate 12 located between one end in the width direction y of the first opposing electrode portion 22a of the first internal electrode layer 16a and the second opposing electrode portion 22b of the second internal electrode layer 16b and the first side surface 12c. The laminate 12 also has a side portion (W gap) 26b of the laminate 12 located between one end in the width direction y of the first opposing electrode portion 22a of the first internal electrode layer 16a and the second opposing electrode portion 22b of the second internal electrode layer 16b and the second side surface 12d.

[0034] The laminate 12 also has an end (L gap) 27a of the laminate 12 located between one end of the second opposing electrode portion 22b of the second internal electrode layer 16b in the length direction z and the first end face 12e, and an end (L gap) 27b of the laminate 12 located between one end of the second opposing electrode portion 22b of the second internal electrode layer 16b in the length direction z and the second end face 12f.

[0035] The first internal electrode layer 16a and the second internal electrode layer 16b can be made of an appropriate conductive material, for example, a metal such as Ni, Cu, Ag, Pd, or Au, or an alloy containing at least one of these metals, such as an Ag-Pd alloy.

[0036] The total number of the first internal electrode layers 16a and the second internal electrode layers 16b is preferably 200 or more and 500 or less.

[0037] The thickness of the first internal electrode layer 16a is preferably 0.3 μm or more and 0.6 μm or less, and the thickness of the second internal electrode layer 16b is preferably 0.3 μm or more and 0.6 μm or less.

[0038] The inner layer portion 18 of the laminate 12 further includes a first dummy electrode 28 and a second dummy electrode 29 .

[0039] The first dummy electrode 28 has one first dummy electrode 28a and the other first dummy electrode 28b.

[0040] The first dummy electrodes 28a, 28b are alternately stacked with the dielectric layers 14, and are arranged on the same plane as the first internal electrode layer 16a arranged on the dielectric layer 14. As shown in Fig. 6, each of the first dummy electrodes 28a, 28b is arranged spaced apart from the first internal electrode layer 16a.

[0041] The first dummy electrode 28a is disposed on the side portion 26a of the laminate 12 located on the first side surface 12c side. The first dummy electrode 28a is not exposed from the first side surface 12c, the second side surface 12d, the first end surface 12e, and the second end surface 12f. The first dummy electrode 28b is disposed on the side portion 26b of the laminate 12 located on the second side surface 12d side. The first dummy electrode 28b is not exposed from the first side surface 12c, the second side surface 12d, the first end surface 12e, and the second end surface 12f.

[0042] The distance w between the first dummy electrode 28a and the first side surface 12c a1 The distance w between the first dummy electrode 28b and the second side surface 12d is preferably 1 μm or more. a2 It is preferable that the distance w between the first dummy electrode 28a and the first internal electrode layer 16a in the width direction y is 1 μm or more. This makes it possible to suppress the penetration of moisture into the first internal electrode layer 16a. a3 is 1 μm or more, and the distance w between the first dummy electrode 28 b and the first internal electrode layer 16 a in the width direction y a4 When the thickness is 1 μm or more, the penetration of moisture into the first internal electrode layer 16 a can be further suppressed.

[0043] The length in the width direction y of the first dummy electrode 28a is preferably 68% to 96% of the shortest distance from the first internal electrode layer 16a to the first side surface 12c. Also, the length in the width direction y of the first dummy electrode 28b is preferably 68% to 96% of the shortest distance from the first internal electrode layer 16a to the second side surface 12d. Within this range, the first dummy electrodes 28a, 28b may also be arranged discontinuously or intermittently in the width direction y.

[0044] The length of the first dummy electrodes 28a, 28b in the longitudinal direction z is preferably 50% or more of the dimension in the longitudinal direction z of the laminate 12 (the distance connecting the first end face 12e and the second end face 12f). The first dummy electrodes 28a, 28b may be arranged discontinuously or intermittently, as long as the length is 50% or more of the dimension in the longitudinal direction z of the laminate 12 (the distance connecting the first end face 12e and the second end face 12f).

[0045] 8, one of the first dummy electrodes 28a may be further divided into a first dummy electrode 28a and a first dummy electrode 28a. In this case, the first dummy electrode 28a is arranged on the first end face 12e side of the side portion 26a of the laminate 12 located on the first side face 12c side. The first dummy electrode 28a is arranged on the second end face 12f side of the side portion 26a of the laminate 12 located on the first side face 12c side. The first dummy electrodes 28a and 28a are not exposed from the first side face 12c, the first end face 12e, and the second end face 12f.

[0046] 8, the other first dummy electrode 28b may be further divided into a first dummy electrode 28b1 and a first dummy electrode 28b2. In this case, the first dummy electrode 28b1 is arranged on the first end face 12e side of the side portion 26b of the laminate 12 located on the second side face 12d side. The first dummy electrode 28b2 is arranged on the second end face 12f side of the side portion 26b of the laminate 12 located on the second side face 12d side. The first dummy electrodes 28b1 and 28b2 are not exposed from the second side face 12d, the first end face 12e, and the second end face 12f.

[0047] The total length of one first dummy electrode 28a1 in the longitudinal direction z and the total length of the first dummy electrode 28a2 in the longitudinal direction z is preferably 50% or more of the dimension of the laminate 12 in the longitudinal direction z (the distance connecting the first end face 12e and the second end face 12f). Similarly, the total length of the other first dummy electrode 28b1 in the longitudinal direction z and the total length of the first dummy electrode 28b2 in the longitudinal direction z is preferably 50% or more of the dimension of the laminate 12 in the longitudinal direction z (the distance connecting the first end face 12e and the second end face 12f). In this way, the first dummy electrodes 28a, 28b may be arranged discontinuously or intermittently as long as their length is 50% or more of the dimension of the laminate 12 in the longitudinal direction z (the distance connecting the first end face 12e and the second end face 12f).

[0048] The main component of the first dummy electrodes 28a, 28b is preferably the same as the main component of the first internal electrode layer 16a. For example, when the first internal electrode layer 16a is Ni, the main component of the first dummy electrodes 28a, 28b is preferably Ni. If the main component of the first dummy electrodes 28a, 28b is the same as the main component of the first internal electrode layer 16a, structural defects due to differences in internal contraction caused by differences in the concentration of the metal component can be suppressed during the firing step in manufacturing the multilayer ceramic capacitor 10.

[0049] The second dummy electrode 29 has one second dummy electrode 29a and the other second dummy electrode 29b.

[0050] The second dummy electrodes 29a, 29b are alternately stacked with the dielectric layers 14, and are arranged on the same plane as the second internal electrode layers 16b arranged on the dielectric layers 14. As shown in Fig. 8, each of the second dummy electrodes 29a, 29b is arranged spaced apart from the second internal electrode layers 16b.

[0051] The second dummy electrode 29a is disposed on the first end face 12e side. Specifically, the second dummy electrode 29a is disposed at the end 27a of the laminate 12 located on the first end face 12e side, and is further disposed from the end 27a of the laminate 12 to the side portions 26a and 26b of the laminate 12. The second dummy electrode 29a is not exposed from the first side face 12c, the second side face 12d, and the first end face 12e. The second dummy electrode 29b is disposed on the second end face 12f side. Specifically, the second dummy electrode 29b is disposed at the end 27b of the laminate 12 located on the second end face 12f side, and is further disposed from the end 27b of the laminate 12 to the side portions 26a and 26b of the laminate 12. The second dummy electrode 29b is not exposed from the first side surface 12c, the second side surface 12d, and the first end surface 12e. That is, the second dummy electrode 29a is defined by the region extending from the unextracted region of the second internal electrode layer 16b to the first end surface 12e, the first side surface 12c, and the second side surface 12d, and the second dummy electrode 29b is defined by the region extending from the unextracted region of the second internal electrode layer 16b to the second end surface 12f, the first side surface 12c, and the second side surface 12d.

[0052] The distance w between the second dummy electrode 29a and the first side surface 12c b1 is preferably 1 μm or more, and the distance w between the second dummy electrode 29 a and the second side surface 12 d is preferably 1 μm or more. b2 is preferably 1 μm or more, and the distance w between the second dummy electrode 29 a and the first end face 12 e is b3 The distance w between the second dummy electrode 29b and the first side surface 12c is preferably 1 μm or more. b4 is preferably 1 μm or more, and the distance w between the second dummy electrode 29 b and the second side surface 12 d is preferably 1 μm or more. b5 is preferably 1 μm or more, and the distance w between the second dummy electrode 29 b and the second end face 12 f is b6 It is preferable that the distance w between the second dummy electrode 29a disposed on the side portion 26a of the laminate 12 and the second internal electrode layer 16b in the width direction y is 1 μm or more. This makes it possible to suppress the penetration of moisture into the second internal electrode layer 16b. b7is 1 μm or more, and the distance w in the width direction y between the second dummy electrode 29 a arranged on the side portion 26 b of the laminate 12 and the second internal electrode layer 16 b is b8 is 1 μm or more, and the distance w in the length direction z between the second dummy electrode 29 a arranged at the end 27 a of the laminate 12 and the second internal electrode layer 16 b b9 When the distance w between the second dummy electrodes 29a arranged on the side portions 26 of the laminate 12 and the second internal electrode layers 16b in the width direction y is 1 μm or more, the penetration of moisture into the second internal electrode layers 16b can be further suppressed. b10 is 1 μm or more, and the distance w b11 is 1 μm or more, and the distance w in the length direction z between the second dummy electrode 29 b arranged at the end 27 b of the laminate 12 and the second internal electrode layer 16 b b12 When the thickness is 1 μm or more, the penetration of moisture into the second internal electrode layer 16b can be further suppressed.

[0053] The length in the width direction y of the second dummy electrodes 29a arranged on the side portions 26a, 26b of the laminate 12 is preferably 70% to 96% of the shortest distance from the second internal electrode layer 16b to the first side surface 12c. Furthermore, the length in the width direction y of the second dummy electrodes 29a arranged on the side portions 26a, 26b of the laminate 12 is preferably 70% to 96% of the shortest distance from the second internal electrode layer 16b to the second side surface 12d. Within this range, the second dummy electrodes 29a, 29b may also be arranged discontinuously or intermittently in the width direction y.

[0054] The length in the longitudinal direction z of the second dummy electrode 29a arranged on the side portions 26a, 26b of the laminate 12 is preferably 50% or more of the distance from both lead electrode portions 24c, 24d of the second internal electrode layer 16b to the first end face 12e. Similarly, the length in the longitudinal direction z of the second dummy electrode 29b arranged on the side portions 26a, 26b of the laminate 12 is preferably 50% or more of the distance from both lead electrode portions 24c, 24d of the second internal electrode layer 16b to the second end face 12f.

[0055] 9, one of the second dummy electrodes 29a may be further divided into a second dummy electrode 29a and a second dummy electrode 29a. In this case, the second dummy electrode 29a is arranged on the first end face 12e side of the side portion 26a of the laminate 12 located on the first side face 12c side. The second dummy electrode 29a is arranged on the first end face 12e side of the side portion 26b of the laminate 12 located on the second side face 12d side. The second dummy electrodes 29a and 29a are not exposed from the first side face 12c, the second side face 12d, and the first end face 12e.

[0056] 9, one of the second dummy electrodes 29b may be further divided into a second dummy electrode 29b1 and a second dummy electrode 29b2. In this case, the second dummy electrode 29b1 is arranged on the second end face 12f side of the side portion 26a of the laminate 12 located on the first side face 12c side. The second dummy electrode 29b2 is arranged on the second end face 12f side of the side portion 26b of the laminate 12 located on the second side face 12d side. The second dummy electrodes 29b1 and 29b2 are not exposed from the first side face 12c, the second side face 12d, and the second end face 12f.

[0057] The length in the longitudinal direction z of the second dummy electrode 29a1 arranged on the side portion 26a of the laminate 12 and the second dummy electrode 29a2 arranged on the side portion 26b of the laminate 12 is preferably 50% or more of the distance from both lead electrode portions 24c, 24d of the second internal electrode layer 16b to the first end face 12e. Similarly, the length in the longitudinal direction z of the second dummy electrode 29b1 arranged on the side portion 26a of the laminate 12 and the second dummy electrode 29b2 arranged on the side portion 26b of the laminate 12 is preferably 50% or more of the distance from both lead electrode portions 24c, 24d of the second internal electrode layer 16b to the second end face 12f. In this way, the second dummy electrodes 29a, 29b may be arranged continuously, discontinuously, or intermittently.

[0058] The main component of the second dummy electrodes 29 a, 29 b is preferably the same as the main component of the second internal electrode layer 16 b. For example, when the second internal electrode layer 16 b is Ni, it is preferable that Ni be the main component of the second dummy electrodes 29 a, 29 b. If the main component of the second dummy electrodes 28 c, 28 d is the same as the main component of the second internal electrode layer 16 b, structural defects due to differences in internal contraction caused by differences in the concentration of the metal component can be suppressed in the firing step when manufacturing the multilayer ceramic capacitor 10.

[0059] The thickness of the first dummy electrodes 28a, 28b in the stacking direction is preferably approximately equal to the thickness of the first internal electrode layer 16a in the stacking direction. Furthermore, the thickness of the second dummy electrodes 29a, 29b in the stacking direction is preferably approximately equal to the thickness of the second internal electrode layer 16b in the stacking direction. Here, "approximately equal" means that the thickness of the first dummy electrode 28 and the second dummy electrode 29 in the stacking direction is 83% to 120% of the thickness of the internal electrode layer 16 in the stacking direction. This eliminates the step caused by the thickness of the first internal electrode layer 16a and the second internal electrode layer 16b. Therefore, structural defects due to peeling between the dielectric layers 14 and the laminate 12 can be suppressed.

[0060] In the inner layer portion 18, only the first dummy electrode 28 may be disposed, or only the second dummy electrode 29 may be disposed.

[0061] The thickness of each of the first dummy electrode 28 and the second dummy electrode 29 in the stacking direction is measured by the measurement method described below. That is, first, the cross section of the laminate 12 is polished along the width direction y or the length direction z to the extent that the first dummy electrode 28 or the second dummy electrode 29 is exposed. The cross section obtained by polishing the cross section is observed, for example, with a scanning electron microscope (SEM) manufactured by JEOL Ltd. The magnification is set to 9000 times or less, and a secondary electron image is used. The magnification and field of view of the SEM are set to a magnification that allows six layers of the first dummy electrode 28 or the second dummy electrode 29 to be observed, and five layers of the dielectric layer 14 to be observed. Then, the region where the first dummy electrode 28 or the second dummy electrode 29 is present is divided into thirds in the stacking direction (i.e., thirds in the width direction y or the length direction z), and the average thickness of the six layers in the central region within each region is calculated. At this time, the SEM image (secondary electron image) obtained by the SEM is enlarged and plotted for each layer, thereby making it possible to calculate the thickness of the first dummy electrode 28 and the second dummy electrode 29 in the stacking direction.

[0062] External electrodes 30 are arranged on the first end face 12e side, the second end face 12f side, the first side face 12c side, and the second side face 12d side of the laminate 12.

[0063] The external electrode 30 includes a base electrode layer 32. The surface of the base electrode layer 32 preferably includes a plating layer 34 disposed so as to cover the base electrode layer 32.

[0064] The external electrodes 30 include a first external electrode 30a, a second external electrode 30b, a third external electrode 30c, and a fourth external electrode 30d.

[0065] The first external electrode 30a is connected to the first internal electrode layer 16a and is disposed on the surface of the first end face 12e. The first external electrode 30a also extends from the first end face 12e of the laminate 12 and is disposed on part of the first principal surface 12a, part of the second principal surface 12b, and part of the first side surface 12c, part of the second side surface 12d. In this case, the first external electrode 30a is electrically connected to the first extraction electrode portion 24a of the first internal electrode layer 16a.

[0066] The second external electrode 30b is connected to the first internal electrode layer 16a and is disposed on the surface of the second end face 12f. The second external electrode 30b also extends from the second end face 12f of the laminate 12 and is disposed on part of the first main face 12a, part of the second main face 12b, and part of the first side face 12c, part of the second side face 12d. In this case, the second external electrode 30b is electrically connected to the second extraction electrode portion 24b of the first internal electrode layer 16a.

[0067] The third external electrode 30c is connected to the second internal electrode layer 16b and is arranged on the surface of the first side surface 12c. The third external electrode 30c also extends from the first side surface 12c of the laminate 12 and is arranged on a part of the first main surface 12a and a part of the second main surface 12b. In this case, the third external electrode 30c is electrically connected to the third extraction electrode portion 24c of the second internal electrode layer 16b.

[0068] The fourth external electrode 30d is connected to the second internal electrode layer 16b and is disposed on the surface of the second side surface 12d. The fourth external electrode 30d also extends from the second side surface 12d of the laminate 12 and is disposed on a part of the first main surface 12a and a part of the second main surface 12b. In this case, the fourth external electrode 30d is electrically connected to the fourth extraction electrode portion 24d of the second internal electrode layer 16b.

[0069] Within the laminate 12, capacitance is formed by the first opposing electrode portion 22a of the first internal electrode layer 16a and the second opposing electrode portion 22b of the second internal electrode layer 16b opposing each other via the dielectric layer 14. Therefore, capacitance can be obtained between the first external electrode 30a and the second external electrode 30b to which the first internal electrode layer 16a is connected and the third external electrode 30c and the fourth external electrode 30d to which the second internal electrode layer 16b is connected, and capacitor characteristics are exhibited.

[0070] The base electrode layer 32 includes at least one selected from a baked layer, a conductive resin layer, a thin film layer, etc. Hereinafter, each configuration when the base electrode layer 32 is the baked layer, the conductive resin layer, or the thin film layer will be described.

[0071] The base electrode layer 32 includes a first base electrode layer 32a, a second base electrode layer 32b, a third base electrode layer 32c, and a fourth base electrode layer 32d.

[0072] The first base electrode layer 32a is connected to the first internal electrode layer 16a and is disposed on the surface of the first end face 12e. The first base electrode layer 32a also extends from the first end face 12e and is disposed on parts of the first and second main faces 12a and 12b, as well as parts of the first and second side faces 12c and 12d. In this case, the first base electrode layer 32a is electrically connected to the first lead electrode portion 24a of the first internal electrode layer 16a. The second base electrode layer 32b is connected to the first internal electrode layer 16a and is disposed on the surface of the second end face 12f. The second base electrode layer 32b also extends from the second end face 12f and is disposed on parts of the first and second main faces 12a and 12b, as well as parts of the first and second side faces 12c and 12d. In this case, the second base electrode layer 32b is electrically connected to the second lead electrode portion 24b of the first internal electrode layer 16a.

[0073] The third base electrode layer 32c is connected to the second internal electrode layer 16b and is disposed on the surface of the first side surface 12c. The third base electrode layer 32c also extends from the first side surface 12c and is disposed on a portion of the first main surface 12a and a portion of the second main surface 12b. In this case, the third base electrode layer 32c is electrically connected to the third lead electrode portion 24c of the second internal electrode layer 16b. The fourth base electrode layer 32d is connected to the second internal electrode layer 16b and is disposed on the surface of the second side surface 12d. The fourth base electrode layer 32d also extends from the second side surface 12d and is disposed on a portion of the first main surface 12a and a portion of the second main surface 12b. In this case, the fourth base electrode layer 32d is electrically connected to the fourth lead electrode portion 24d of the second internal electrode layer 16b.

[0074] (In the case of a baking layer) The baking layer contains a glass component and a metal component. The glass component of the baking layer contains at least one selected from B, Si, Ba, Mg, Al, Li, etc. The metal component of the baking layer contains at least one selected from Cu, Ni, Ag, Pd, an Ag-Pd alloy, Au, etc. The baking layer may be a multi-layered layer. The baking layer is formed by applying a conductive paste containing a glass component and a metal component to the laminate 12 and baking it. The baking layer may be formed by simultaneously baking a laminated chip having an internal electrode layer 16 and a dielectric layer 14 and a conductive paste applied to the laminated chip, or by baking a laminated chip having an internal electrode layer 16 and a dielectric layer 14 to obtain the laminate 12, and then applying a conductive paste to the laminate 12 and baking it. In addition, when the baking layer is formed by simultaneously baking a laminated chip having an internal electrode layer 16 and a dielectric layer 14 and a conductive paste applied to the laminated chip, it is preferable to form the baking layer by baking a layer to which a dielectric material has been added instead of a glass component.

[0075] The thickness of the first base electrode layer 32a located on the first end face 12e in the length direction z connecting the first end face 12e and the second end face 12f at the center in the stacking direction x is preferably, for example, about 3 μm or more and 70 μm or less. The thickness of the second base electrode layer 32b located on the second end face 12f in the length direction z connecting the first end face 12e and the second end face 12f at the center in the stacking direction x is preferably, for example, about 3 μm or more and 70 μm or less. The thickness of the third base electrode layer 32c located on the first side face 12c in the width direction y connecting the first side face 12c and the second side face 12d at the center in the stacking direction x is preferably, for example, about 3 μm or more and 70 μm or less. The thickness of the fourth base electrode layer 32d located on the second side surface 12d in the width direction y connecting the first side surface 12c and the second side surface 12d at the center in the stacking direction x is preferably, for example, approximately 3 μm or more and 70 μm or less.

[0076] The thickness in the stacking direction x connecting the first and second principal surfaces 12a and 12b at the center in the length direction z connecting the first end face 12e and the second end face 12f of the first base electrode layer 32a located on a portion of the first and second principal surfaces 12a and 12b is preferably, for example, about 3 μm to 40 μm.Furthermore, the thickness in the stacking direction x connecting the first and second principal surfaces 12a and 12b at the center in the length direction z connecting the first end face 12e and the second end face 12f of the second base electrode layer 32b located on a portion of the first and second principal surfaces 12a and 12b is preferably, for example, about 3 μm to 40 μm. The thickness in the stacking direction x connecting the first and second main surfaces 12a and 12b of the third base electrode layer 32c located on a portion of the first and second main surfaces 12a and 12b at the center in the width direction y connecting the first and second side surfaces 12c and 12d is preferably, for example, about 3 μm to 40 μm.Furthermore, the thickness in the stacking direction x connecting the first and second main surfaces 12a and 12b of the fourth base electrode layer 32d located on a portion of the first and second main surfaces 12a and 12b at the center in the width direction y connecting the first and second side surfaces 12c and 12d is preferably, for example, about 3 μm to 40 μm.

[0077] The thickness in the width direction y connecting the first side surface 12c and the second side surface 12d at the center in the length direction z connecting the first end surface 12e and the second end surface 12f of the first base electrode layer 32a located on a part of the first side surface 12c and the second side surface 12d is preferably, for example, about 3 μm to 40 μm.Furthermore, the thickness in the width direction y connecting the first side surface 12c and the second side surface 12d at the center in the length direction z connecting the first end surface 12e and the second end surface 12f of the second base electrode layer 32b located on a part of the first side surface 12c and the second side surface 12d is preferably, for example, about 3 μm to 40 μm.

[0078] (Conductive Resin Layer) When a conductive resin layer is provided as the base electrode layer 32, the conductive resin layer is disposed on the baked layer so as to cover the baked layer. The conductive resin layer contains a metal and a thermosetting resin. The conductive resin layer may completely cover the base electrode layer or may cover only a portion of the base electrode layer.

[0079] Since the conductive resin layer contains a thermosetting resin, it is more flexible than a conductive layer made of, for example, a plating film or a fired conductive paste. Therefore, even if the feedthrough multilayer ceramic capacitor 10 is subjected to a physical shock or a shock due to a thermal cycle, the conductive resin layer functions as a buffer layer and can prevent cracks in the feedthrough multilayer ceramic capacitor 10.

[0080] The metal contained in the conductive resin layer can be Ag, Cu, Ni, Sn, Bi, or an alloy containing these. It is also possible to use a metal powder whose surface is coated with Ag. When using a metal powder whose surface is coated with Ag, it is preferable to use Cu, Ni, Sn, Bi, or an alloy powder thereof as the metal powder. The reason for using Ag conductive metal powder as the conductive metal is that Ag has the lowest resistivity among metals, making it suitable as an electrode material, and Ag is a noble metal that does not oxidize and has high weather resistance. Furthermore, it is possible to use a cheaper base metal while maintaining the above-mentioned properties of Ag.

[0081] Furthermore, the metal contained in the conductive resin layer may be Cu or Ni that has been subjected to an anti-oxidation treatment. The metal contained in the conductive resin layer may be a metal powder whose surface is coated with Sn, Ni, or Cu. When using a metal powder whose surface is coated with Sn, Ni, or Cu, it is preferable to use Ag, Cu, Ni, Sn, Bi, or an alloy powder thereof as the metal powder.

[0082] The metal contained in the conductive resin layer is mainly responsible for the electrical conductivity of the conductive resin layer. Specifically, when the conductive fillers come into contact with each other, a conductive path is formed inside the conductive resin layer.

[0083] The metal contained in the conductive resin layer may be spherical or flat, but it is preferable to use a mixture of spherical metal powder and flat metal powder.

[0084] The resin for the conductive resin layer may be any of various known thermosetting resins, such as epoxy resin, phenol resin, urethane resin, silicone resin, polyimide resin, etc. Among these, epoxy resin is one of the most suitable resins, as it has excellent heat resistance, moisture resistance, adhesion, etc.

[0085] The conductive resin layer preferably contains a curing agent together with the thermosetting resin. When an epoxy resin is used as the base resin, various known compounds such as phenol-based, amine-based, acid anhydride-based, imidazole-based, active ester-based, and amide-imide-based compounds can be used as the curing agent for the epoxy resin.

[0086] The conductive resin layer may be a multi-layered layer.

[0087] The thickness of the conductive resin layer located at the center of the stacking direction x of the laminate 12 located at the first end face 12e and the second end face 12f is preferably, for example, about 10 μm or more and 150 μm or less.

[0088] (In the case of a thin film layer) A thin film layer may be formed on the surface of the laminate 12 as the base electrode layer 32. When a thin film layer is provided as the base electrode layer 32, the thin film layer is formed by a thin film formation method such as a sputtering method or a vapor deposition method, and is a layer of 1 μm or less in thickness on which metal particles are deposited.

[0089] (Plating Layer) The plating layer 34 includes a first plating layer 34a arranged to cover the first base electrode layer 32a, a second plating layer 34b arranged to cover the second base electrode layer 32b, a third plating layer 34c arranged to cover the third base electrode layer 32c, and a fourth plating layer 34d arranged to cover the fourth base electrode layer 32d.

[0090] The plating layer 34 contains at least one selected from, for example, Cu, Ni, Sn, Ag, Pd, an Ag—Pd alloy, Au, and the like.

[0091] The plating layer 34 may also be formed of multiple layers. Preferably, the plating layer 34 has a two-layer structure consisting of Ni plating and Sn plating in that order. The Ni plating layer can prevent the base electrode layer 32 from being eroded by solder when mounting the multilayer ceramic capacitor 10. The Sn plating layer can also improve the wettability of the solder when mounting the multilayer ceramic capacitor 10, facilitating mounting.

[0092] The thickness of each plating layer 34 is preferably 4 μm or more and 10 μm or less.

[0093] Either or both of the third external electrode 30c and the fourth external electrode 30d may have a plating layer 34 formed directly on the surface of the laminate 12. That is, the multilayer ceramic capacitor 10 may have a structure including a plating layer 34 that is directly and electrically connected to the second internal electrode layer 16b. In such a case, the plating layer 34 may be formed directly after a catalyst is disposed on the surface of the laminate 12 as a pretreatment.

[0094] When the plating layer 34 is formed directly on the laminate 12, it is preferable that the plating layer 34 includes a lower layer plating electrode formed on the surface of the laminate 12 and an upper layer plating electrode formed on the surface of the lower layer plating electrode.

[0095] The lower layer plating electrode and the upper layer plating electrode each preferably contain at least one metal selected from, for example, Cu, Ni, Sn, Pb, Au, Ag, Pd, Bi, or Zn, or an alloy containing such a metal.

[0096] Furthermore, for example, when the first internal electrode layer 16 a and the second internal electrode layer 16 b are formed using Ni, it is preferable that the lower-layer plated electrodes are formed using Cu, which has good bonding properties with Ni. Note that the upper-layer plated electrodes may be formed as needed, and in particular, the third external electrode 30 c and the fourth external electrode 30 d may each be composed of only the lower-layer plated electrodes.

[0097] When the plating layer 34 is formed directly on the laminate 12, the plating layer 34 may have an upper layer plating electrode as the outermost layer, or another plating electrode may be formed on the surface of the upper layer plating electrode.

[0098] When the plating layer 34 is formed directly on the laminate 12, the thickness of each plating layer 34 is preferably 1 μm or more and 15 μm or less.

[0099] When the plating layer 34 is formed directly on the laminate 12, it is preferable that the plating layer 34 does not contain glass. In addition, the metal content per unit volume of the plating layer 34 is preferably 99% by volume or more.

[0100] The external electrodes 30 may be formed only with plating layers without providing the base electrode layer 32. Although not shown, a structure in which plating layers are provided without providing the base electrode layer 32 will be described below.

[0101] Any one or each of the first external electrode 30a to the fourth external electrode 30d may not be provided with the base electrode layer 32, and the plating layer may be formed directly on the surface of the laminate 12. That is, the multilayer ceramic capacitor 10 may have a structure including a plating layer electrically connected to the first internal electrode layer 16a and the second internal electrode layer 16b. In such a case, the plating layer may be formed after a catalyst is disposed on the surface of the laminate 12 as a pretreatment.

[0102] In addition, when a plating layer is formed directly on the laminate 12 without providing the base electrode layer 32, the amount of reduction in the thickness of the base electrode layer 32 can be converted into a lower profile, i.e., a thinner laminate 12, or the thickness of the inner layer portion 18, thereby improving the design freedom of the thin chip.

[0103] The plating layer preferably includes a lower-layer plating electrode formed on the surface of the laminate 12 and an upper-layer plating electrode formed on the surface of the lower-layer plating electrode. The lower-layer plating electrode and the upper-layer plating electrode each preferably include at least one metal selected from, for example, Cu, Ni, Sn, Pb, Au, Ag, Pd, Bi, or Zn, or an alloy containing such a metal. Furthermore, the lower-layer plating electrode is preferably formed using Ni, which has solder barrier properties, and the upper-layer plating electrode is preferably formed using Sn or Au, which have good solder wettability.

[0104] Furthermore, for example, when the first internal electrode layer 16a and the second internal electrode layer 16b are formed using Ni, it is preferable that the lower layer plating electrode is formed using Cu, which easily forms an alloy layer with Ni. This makes it difficult for gaps to occur between the internal electrode layer 16 and the lower layer plating electrode due to the Ni-Cu alloy layer, thereby obtaining the effect of further preventing moisture penetration.

[0105] The upper-layer plated electrodes may be formed as needed, and each of the first to fourth external electrodes 30a to 30d may be composed of only lower-layer plated electrodes. The upper-layer plated electrodes may be the outermost layer of the plating layer, or other plated electrodes may be formed on the surface of the upper-layer plated electrodes.

[0106] Here, when the external electrode 30 is formed by plating layers only without providing the base electrode layer 32, it is preferable that the thickness of each plating layer disposed without providing the base electrode layer 32 is 1 μm or more and 15 μm or less.

[0107] Furthermore, the plating layer preferably does not contain glass, and the metal content per unit volume of the plating layer is preferably 99% by volume or more.

[0108] The dimension in the length direction z of the multilayer ceramic capacitor 10 including the laminate 12, the first external electrode 30a, and the second external electrode 30b is defined as dimension L, the dimension in the stacking direction x of the multilayer ceramic capacitor 10 including the laminate 12, the first external electrode 30a, and the second external electrode 30b is defined as dimension T, and the dimension in the width direction y of the multilayer ceramic capacitor 10 including the laminate 12, the first external electrode 30a, and the second external electrode 30b is defined as dimension W. The dimensions of the multilayer ceramic capacitor 10 are preferably such that the dimension L in the length direction z is 0.8 mm to 3.4 mm, the dimension W in the width direction y is 0.4 mm to 1.5 mm, and the dimension T in the stacking direction x is 0.3 mm to 0.8 mm.

[0109] 2. Method for Manufacturing a Multilayer Ceramic Capacitor Next, one embodiment of a method for manufacturing a multilayer ceramic capacitor will be described.

[0110] First, a dielectric sheet for the dielectric layers and a conductive paste for the internal electrode layers are prepared. The dielectric sheet and the conductive paste for the internal electrode layers contain a binder and a solvent. The binder and the solvent may be known.

[0111] Then, the conductive paste for the internal electrode layers and the conductive paste for the dummy electrodes are printed in predetermined patterns on the dielectric sheets by, for example, gravure printing, screen printing, etc. In this way, a dielectric sheet on which the pattern of the first internal electrode layers and the pattern of the first dummy electrodes are formed, and a dielectric sheet on which the pattern of the second internal electrode layers and the pattern of the second dummy electrodes are formed are prepared.

[0112] Furthermore, by changing the size and arrangement of the pattern of the gravure printing plate used here, it is possible to control the length in the longitudinal direction z connecting the first end face and second end face of the first dummy electrode and the second dummy electrode, and it is also possible to control the length in the longitudinal direction z connecting the first end face and second end face between the third extraction electrode portion and the second dummy electrode, and the length in the longitudinal direction z connecting the first end face and second end face between the fourth extraction electrode portion and the second dummy electrode.

[0113] Furthermore, for example, when forming the print patterns of the internal electrode layers and dummy electrodes by gravure printing, the design of the gravure plate used in the gravure printing is set to the graphic patterns of the first internal electrode layer and the first dummy electrode, and by changing the structure corresponding to the graphic patterns of the second internal electrode layer and the second dummy electrode, the desired internal electrode layers and dummy electrodes can be formed, respectively. At this time, by changing the grooves of the gravure plate, the thickness in the stacking direction can be changed, and by changing the width of the grooves of the gravure plate, the shape of the dummy electrodes of this configuration can be changed.

[0114] Furthermore, when forming the printing patterns of the internal electrode layer and the dummy electrode by screen printing, the design of the screen printing mask is set to the graphic patterns of the first internal electrode layer and the first dummy electrode, and by changing the structure to correspond to the graphic patterns of the second internal electrode layer and the second dummy electrode, the desired internal electrode layer and dummy electrode can be formed, respectively.

[0115] Next, a predetermined number of dielectric sheets for outer layers, on which the patterns of the internal electrode layers and the patterns of the dummy electrodes are not printed, are laminated to form a portion that will become the second main surface side outer layer portion on the second main surface side. Then, a dielectric sheet on which the patterns of the first internal electrode layers and the patterns of the first dummy electrodes are printed, and a dielectric sheet on which the patterns of the second internal electrode layers and the patterns of the second dummy electrodes are printed are sequentially laminated on the portion that will become the second main surface side outer layer portion so as to form the structure of the present invention, to form a portion that will become the inner layer portion. After that, a predetermined number of dielectric sheets for outer layers, on which the patterns of the internal electrode layers and the patterns of the dummy electrodes are not printed, are further laminated on the portion that will become the inner layer portion, to form a portion that will become the first main surface side outer layer portion on the first main surface side. In this way, a laminated sheet is produced.

[0116] Subsequently, if necessary, the laminated sheets are pressed in the lamination direction by means of a hydrostatic press or the like to produce a laminated block.

[0117] The laminate block is then cut into predetermined shapes and dimensions to produce raw laminate chips. At this time, the raw laminate chips may be subjected to barrel polishing or the like to round off the corners and ridges of the laminate chips.

[0118] The raw laminate chip is then fired, and a laminate is produced in which the first internal electrode layer and the second internal electrode layer are disposed inside the laminate, the first internal electrode layer is extended to the first end face, and the second internal electrode layer is extended to the second end face. The firing temperature for the raw laminate chip depends on the ceramic material and the material of the conductive paste for the internal electrode layers, but is preferably 900°C or higher and 1300°C or lower.

[0119] Then, a third base electrode layer 32c of the third external electrode 30c is formed on the first side surface 12c of the laminate 12 obtained by firing, and a fourth base electrode layer 32d of the fourth external electrode 30d is formed on the second side surface 12d of the laminate 12. When forming a baked layer as the base electrode layer 32, a conductive paste containing a glass component and a metal component is applied, and then a baking process is performed to form the baked layer as the base electrode layer 32. The temperature of the baking process at this time is preferably 700°C or higher and 900°C or lower.

[0120] Next, a first base electrode layer 32a of the first external electrode 30a is formed on a first end face 12e of the laminate 12 obtained by firing, and a second base electrode layer 32b of the second external electrode 30b is formed on a second end face 12f of the laminate 12. As in the formation of the base electrode layers 32 of the third external electrode 30c and the fourth external electrode 30d, when a baked layer is formed as the base electrode layer 32, a conductive paste containing a glass component and a metal component is applied, and then a baking process is performed to form a baked layer as the base electrode layer 32. The temperature of the baking process at this time is preferably 700°C or higher and 900°C or lower.

[0121] When the base electrode layer is formed of a conductive resin layer, the conductive resin layer can be formed by the following method. The conductive resin layer may be formed on the surface of the baking layer, or the conductive resin layer may be formed directly on the surface of the laminate 12 without forming a baking layer. The conductive resin layer is formed by applying a conductive resin paste containing a thermosetting resin and a metal component to the baking layer or the surface of the laminate 12, and then performing a heat treatment at a temperature of 250°C to 550°C to thermally cure the resin and form a conductive resin layer. The heat treatment is preferably performed in an N2 atmosphere. To prevent the resin from scattering and the various metal components from oxidizing, the oxygen concentration is preferably kept below 100 ppm.

[0122] When the base electrode layer is formed as a thin film layer, the base electrode layer can be formed by a thin film formation method such as sputtering or vapor deposition. The base electrode layer formed as a thin film layer is a layer of metal particles deposited to a thickness of 1 μm or less.

[0123] (Thin Film Layer) When the base electrode layer 32 is formed as a thin film layer, masking or the like is performed, and the base electrode layer can be formed by a thin film formation method such as sputtering or vapor deposition in the area where the external electrode 30 is to be formed. The base electrode layer formed as a thin film layer is a layer of deposited metal particles having a thickness of 1 μm or less.

[0124] (Plating Electrode) Furthermore, an external electrode may be formed as a plating electrode using only a plating layer without providing the base electrode layer 32. In this case, it can be formed by the following method.

[0125] For any one or each of the first external electrode 30a to the fourth external electrode 30d, a plating layer may be formed directly on the surface of the laminate 12 without providing a base electrode layer 32. That is, the multilayer ceramic capacitor 10 may have a structure including plating layers directly and electrically connected to the first internal electrode layer 16a and the second internal electrode layer 16b. While either electrolytic plating or electroless plating may be used for plating, electroless plating has the disadvantage of requiring pretreatment using a catalyst or the like to improve the plating deposition rate, complicating the process. Therefore, electrolytic plating is usually preferred. Barrel plating is preferably used as the plating method. Furthermore, if necessary, an upper-layer plating electrode may be formed on the surface of the lower-layer plating electrode in the same manner.

[0126] Next, as necessary, a plating layer is formed on the surface of the base electrode layer 32, the surface of the conductive resin layer or the surface of the lower-layer plating electrode, and the surface of the upper-layer plating electrode. More specifically, in this embodiment, a plating layer is formed on the base electrode layer 32, which is a baked layer. The Ni plating layer and the Sn plating layer are formed sequentially, for example, by barrel plating. Either electrolytic plating or electroless plating may be used for the plating process. However, electroless plating has the disadvantage of requiring pretreatment using a catalyst or the like to improve the plating deposition rate, which complicates the process. Therefore, electrolytic plating is usually preferred.

[0127] In the manner described above, the multilayer ceramic capacitor 10 shown in FIG. 1 is manufactured.

[0128] 3. Experimental Example Next, an experiment was carried out to confirm the effects of the multilayer ceramic capacitor according to the present invention described above.

[0129] A. Experimental Example 1 In Experimental Example 1, laminate samples with different dimensions were manufactured, and an experiment was conducted to check for peeling by changing the lengths of the first dummy electrode and the second dummy electrode in the width direction y. The specifications of each sample used in each experiment are described below.

[0130] A-1. First Dummy Electrode (1) Specifications of Samples in Experimental Examples 1-1 and 1-2 In Experimental Examples 1-1 and 1-2, laminates of different dimensions were manufactured according to the manufacturing method of the multilayer ceramic capacitor described above, and then samples were fabricated in which the length of the first dummy electrode in the width direction y was changed. The length of the first dummy electrode in the length direction z was set to 50% of the dimension of the laminate in the length direction z.

[0131] As shown in FIG. 10, the first dummy electrodes were respectively arranged between the first internal electrode layer and the first side surface and between the first internal electrode layer and the second side surface (so-called side portions of the laminate).

[0132] More specifically, as shown in FIG. 10 , the first dummy electrode disposed between the first internal electrode layer and the first side surface is disposed so that the center line c1 representing ½L of the laminate coincides with the center of the first dummy electrode in the longitudinal direction z. Furthermore, this first dummy electrode is disposed so that the center line c2 in the width direction y of the distance w1 between the first internal electrode layer and the first side surface coincides with the center of the first dummy electrode in the width direction y. The first dummy electrode disposed between the first internal electrode layer and the second side surface is also disposed in a similar manner. The laminates used in Experimental Examples 1-1 and 1-2 did not include a second dummy electrode.

[0133] (Experimental Example 1-1) Structure of multilayer ceramic capacitor: 3 terminals Dimension L0 in length direction z of laminate: 1.10 mm ± 0.05 mm Dimension W0 in width direction y of laminate: 0.80 mm ± 0.05 mm Dimension T0 in lamination direction of laminate: 0.50 mm ± 0.05 mm Main component of inner dielectric layer: BaTiO3 Main component of outer dielectric layer: BaTiO3 Main component of first internal electrode layer: Ni Thickness of first internal electrode layer: 0.50 μm ± 0.10 μm Main component of first dummy electrode: Ni Thickness of first dummy electrode: 0.50 μm ± 0.10 μm Length of first dummy electrode in width direction y: see Table 1 Main component of second internal electrode layer: Ni Thickness of second internal electrode layer: 0.50 μm ± 0.10 μm Length in the width direction y of the lead electrode portion of the second internal electrode layer: 220 μm Distance between the first internal electrode layer and the side surface: 52 μm Distance between the opposing electrode portion of the second internal electrode layer and the side surface: 52 μm Distance between the opposing electrode portion of the second internal electrode layer and the end face: 52 μm Total number of first internal electrode layers and second internal electrode layers: 478

[0134] (Experimental Example 1-2) Structure of multilayer ceramic capacitor: 3 terminals Dimension L0 in length direction z of laminate: 1.10 mm ± 0.05 mm Dimension W0 in width direction y of laminate: 0.60 mm ± 0.05 mm Dimension T0 in lamination direction of laminate: 0.40 mm ± 0.05 mm Main component of inner dielectric layer: BaTiO3 Main component of outer dielectric layer: BaTiO3 Main component of first internal electrode layer: Ni Thickness of first internal electrode layer: 0.50 μm ± 0.10 μm Main component of first dummy electrode: Ni Thickness of first dummy electrode: 0.50 μm ± 0.10 μm Length of first dummy electrode in width direction y: see Table 2 Main component of second internal electrode layer: Ni Thickness of second internal electrode layer: 0.50 μm ± 0.10 μm Length in the width direction y of the lead electrode portion of the second internal electrode layer: 130 μm Distance between the first internal electrode layer and the side surface: 82 μm Distance between the opposing electrode portion of the second internal electrode layer and the side surface: 82 μm Distance between the opposing electrode portion of the second internal electrode layer and the end face: 62 μm Total number of first internal electrode layers and second internal electrode layers: 260

[0135] (2) Method for Calculating the Width-Directional Ratio of the First Dummy Electrode First, the laminate described above was solidified with resin. Next, the surface in the width direction × stacking direction (WT surface) was exposed, and the laminate was polished to 1 / 2 of the length direction dimension so that the first dummy electrode was exposed. In the polished surface in the width direction × stacking direction (WT surface), the space between the first internal electrode layer and the side surface was observed using a digital microscope (Keyence Corporation: VHX-8000, magnification 1000x).

[0136] In the polished width direction × stacking direction surface (WT surface), as shown in the enlarged view of the W gap portion in Fig. 12, when the dimension of the inner layer portion in the stacking direction is divided into four equal parts, the length in the width direction y of the first dummy electrode / (distance w1 in the width direction y from the side surface closest to the first dummy electrode to the first internal electrode layer) was measured in a total of five regions (a1 to a5) where first dummy electrodes are located between extensions of the boundary lines of the four equal parts and extensions of the boundary lines between the inner layer portion and each outer layer portion. Based on the above method, the average value of the length in the width direction y of the first dummy electrode / (distance w1 in the width direction y from the side surface closest to the first dummy electrode to the first internal electrode layer) when 1,000 laminates were measured was taken as the first dummy electrode ratio.

[0137] (3) Method for checking peeling: The longitudinal x lamination direction surface (LT cross section) of the laminate as a sample was exposed, and peeling was counted. 1000 pieces were prepared for each experimental example.

[0138] The evaluation results are shown in Tables 1 and 2.

[0139]

[0140] (4) Summary According to Experimental Example 1-1, when the ratio of first dummy electrodes was 66% or more, a favorable result of the peeling occurrence rate of 1% or less was obtained, as shown in Samples No. 5 to No. 12. Furthermore, according to Experimental Example 1-2, when the ratio of first dummy electrodes was 68% or more, a favorable result of the peeling occurrence rate of 1% or less was obtained, as shown in Samples No. 18 to No. 24.

[0141] On the other hand, according to Experimental Example 1-1, as shown in Samples 1 to 4, when the ratio of first dummy electrodes was 40% or less, the peeling incidence rate exceeded 1%. In particular, Sample 1, which was a sample without a first dummy electrode, had a relatively high peeling incidence rate of 68.3% compared to the other samples with a first dummy electrode. Furthermore, according to Experimental Example 1-2, as shown in Samples 13 to 17, when the ratio of first dummy electrodes was 66% or less, the peeling incidence rate exceeded 1%. In particular, Sample 13, which was a sample without a first dummy electrode, had a relatively high peeling incidence rate of 62.3% compared to the other samples with a second dummy electrode.

[0142] From the above results, it is clear that the occurrence of peeling can be suppressed by setting the ratio of the first dummy electrodes to at least 68% or more.

[0143] A-2. Second Dummy Electrode (1) Specifications of Samples in Experimental Examples 1-3 and 1-4 In Experimental Examples 1-3 and 1-4, laminates of different dimensions were manufactured according to the manufacturing method of the multilayer ceramic capacitor described above, and then samples were fabricated in which the length of the second dummy electrode in the width direction y was changed. The length of each second dummy electrode in the length direction z was set to 50% of the distance between the third lead electrode portion of the second internal electrode layer and both end faces, or the distance between the fourth lead electrode portion of the second internal electrode layer and both end faces.

[0144] 11 , the second dummy electrode is disposed on the first end face side between the second opposing electrode portion of the second internal electrode layer and the first and second side faces (so-called side portions of the laminate). Also, the second dummy electrode is disposed on the second end face side between the second opposing electrode portion of the second internal electrode layer and the first and second side faces (so-called side portions of the laminate).

[0145] More specifically, as shown in FIG. 11 , the second dummy electrode disposed on the first end face side between the second opposing electrode portion of the second internal electrode layer and the first side face is disposed so that the center line c3 of the distance between the third extraction electrode portion of the second internal electrode layer and the first end face coincides with the center of the second dummy electrode in the longitudinal direction z. Furthermore, this second dummy electrode is disposed so that the center line c4 of the distance w2 between the second opposing electrode portion of the second internal electrode layer and the first side face coincides with the center of the second dummy electrode in the width direction y. The other second dummy electrodes are disposed in a similar manner. The laminates used in Experimental Examples 1-3 and 1-4 did not include a first dummy electrode.

[0146] (Experimental Example 1-3) Structure of multilayer ceramic capacitor: 3 terminals Dimension L0 in length direction z of laminate: 1.10 mm ± 0.05 mm Dimension W0 in width direction y of laminate: 0.80 mm ± 0.05 mm Dimension T0 in lamination direction of laminate: 0.50 mm ± 0.05 mm Main component of dielectric layer of inner layer portion: BaTiO3 Main component of dielectric layer of outer layer portion: BaTiO3 Main component of first internal electrode layer: Ni Thickness of first internal electrode layer: 0.50 μm ± 0.10 μm Main component of second internal electrode layer: Ni Thickness of second internal electrode layer: 0.50 μm ± 0.10 μm Length of lead electrode portion of second internal electrode layer in width direction y: 220 μm Main component of second dummy electrode: Ni Thickness of second dummy electrode: 0.50 μm ± 0.10 μm Length of the second dummy electrode in the width direction y: See Table 3. Distance between the first internal electrode layer and the side surface: 52 μm. Distance between the opposing electrode portion of the second internal electrode layer and the side surface: 52 μm. Distance between the opposing electrode portion of the second internal electrode layer and the end surface: 52 μm. Total number of first internal electrode layers and second internal electrode layers: 478.

[0147] (Experimental Example 1-4) Structure of multilayer ceramic capacitor: 3 terminals (see FIG. 1) Dimension L0 in length direction z of laminate: 1.10 mm ± 0.05 mm Dimension W0 in width direction y of laminate: 0.60 mm ± 0.05 mm Dimension T0 in lamination direction of laminate: 0.40 mm ± 0.05 mm Main component of dielectric layer of inner layer portion: BaTiO3 Main component of dielectric layer of outer layer portion: BaTiO3 Main component of first internal electrode layer: Ni Thickness of first internal electrode layer: 0.50 μm ± 0.10 μm Main component of second internal electrode layer: Ni Thickness of second internal electrode layer: 0.50 μm ± 0.10 μm Length in width direction y of lead electrode portion of second internal electrode layer: 130 μm Main component of second dummy electrode: Ni Thickness of second dummy electrode: 0.50 μm±0.10 μm Length of second dummy electrode in width direction y: see Table 4 Distance between first internal electrode layer and side surface: 82 μm Distance between opposing electrode portion of second internal electrode layer and side surface: 82 μm Distance between opposing electrode portion of second internal electrode layer and end face: 62 μm Total number of first internal electrode layers and second internal electrode layers: 260

[0148] (2) Method for Calculating the Width-Direction Ratio of the Second Dummy Electrode The above-described laminate was solidified with resin. Next, the surface in the width direction × stacking direction (WT surface) was exposed, and the laminate was polished to ¼ of the length direction dimension so that the second dummy electrode was exposed. That is, polishing was performed in the dimension in the length direction z where the lead electrode portion of the second internal electrode layer was not present. In the surface in the width direction × stacking direction (WT surface) obtained by polishing, the space between the second internal electrode layer (GND internal electrode layer) and the side surface was observed with a digital microscope (Keyence Corporation: VHX-8000, magnification 1000x).

[0149] In the polished width direction × stacking direction surface (WT surface), as shown in the enlarged view of the W gap portion in Fig. 12, when the dimension of the inner layer portion in the stacking direction is divided into four equal parts, the length in the width direction y of the second dummy electrode / (distance w2 in the width direction y from the side surface closest to the second dummy electrode to the second internal electrode layer) was measured in a total of five regions (a1 to a5) where second dummy electrodes are located between extensions of the boundary lines of the four equal parts and extensions of the boundary lines between the inner layer portion and each outer layer portion. Based on the above method, the average value of the length in the width direction of the second dummy electrode / (distance w2 in the width direction y from the side surface closest to the second dummy electrode to the second internal electrode layer) when 1,000 laminates were measured was taken as the second dummy electrode ratio.

[0150] (3) Peeling Confirmation Method Peeling was confirmed by the same method as in Experimental Examples 1-1 and 1-2.

[0151] The evaluation results are shown in Tables 3 and 4.

[0152]

[0153] (4) Summary According to Experimental Example 1-3, when the proportion of second dummy electrodes was 68% or more, a favorable result of a peeling occurrence rate of 1% or less was obtained, as shown in Samples 30 to 36. Furthermore, according to Experimental Example 1-4, when the proportion of first dummy electrodes was 70% or more, a favorable result of a peeling occurrence rate of 1% or less was obtained, as shown in Samples 43 to 48.

[0154] On the other hand, according to Experimental Example 1-3, as shown in Samples 25 to 29, when the proportion of second dummy electrodes was 66% or less, the peeling incidence rate exceeded 1%. In particular, Sample 25, which did not include a second dummy electrode, had a relatively high peeling incidence rate of 72.2%, compared to the other samples in which first dummy electrodes were provided. Furthermore, according to Experimental Example 1-4, as shown in Samples 37 to 42, when the proportion of second dummy electrodes was 68% or less, the peeling incidence rate exceeded 1%. In particular, Sample 37, which did not include a second dummy electrode, had a relatively high peeling incidence rate of 60.1%, compared to the other samples in which second dummy electrodes were provided.

[0155] From the above results, it is clear that the occurrence of peeling can be suppressed by setting the proportion of the second dummy electrodes to at least 70% or more.

[0156] B. Experimental Example 2 In Experimental Example 2, multilayer ceramic capacitor samples with different dimensions were manufactured, and experiments were conducted to confirm moisture resistance reliability by changing the lengths of the first dummy electrode and the second dummy electrode in the width direction y. The specifications of the samples used in each experiment are described below.

[0157] B-1. First Dummy Electrode (1) Specifications of Samples in Experimental Examples 2-1 and 2-2 In Experimental Examples 2-1 and 2-2, multilayer ceramic capacitors of different dimensions were manufactured according to the above-described method for manufacturing a multilayer ceramic capacitor, and then samples were fabricated in which the length of the first dummy electrode in the width direction y was varied. The length of the first dummy electrode in the longitudinal direction z was set to 50% of the length of the laminate in the longitudinal direction z. The arrangement of the first dummy electrodes was the same as in Experimental Examples 1-1 and 1-2, as shown in FIG. 10 . Note that the laminates used in Experimental Examples 2-1 and 2-2 did not have second dummy electrodes.

[0158] (Experimental Example 2-1) Structure of multilayer ceramic capacitor: 3 terminals Dimension L of multilayer ceramic capacitor in length direction z: 1.20 mm ± 0.05 mm Dimension W of multilayer ceramic capacitor in width direction y: 0.90 mm ± 0.05 mm Dimension T of multilayer ceramic capacitor in lamination direction: 0.60 mm ± 0.05 mm Main component of inner dielectric layer: BaTiO3 Main component of outer dielectric layer: BaTiO3 Main component of first internal electrode layer: Ni Thickness of first internal electrode layer: 0.50 μm ± 0.10 μm Main component of first dummy electrode: Ni Thickness of first dummy electrode: 0.50 μm ± 0.10 μm Length of first dummy electrode in width direction y: see Table 5 Main component of second internal electrode layer: Ni Thickness of second internal electrode layer: 0.50 μm ± 0.10 μm Length in the width direction y of the lead electrode portion of the second internal electrode layer: 220 μm Distance between the first internal electrode layer and the side surface: 52 μm Distance between the opposing electrode portion of the second internal electrode layer and the side surface: 52 μm Distance between the opposing electrode portion of the second internal electrode layer and the end face: 52 μm Structure of the first external electrode and the second external electrode: Base electrode layer (Cu), plating layer (two-layer structure: Ni / Sn plating) Structure of the third external electrode and the fourth external electrode: Base electrode layer (Cu), plating layer (two-layer structure: Ni / Sn plating) Total number of first internal electrode layers and second internal electrode layers: 478

[0159] (Experimental Example 2-2) Structure of multilayer ceramic capacitor: 3 terminals Dimension L of multilayer ceramic capacitor in length direction z: 1.15 mm ± 0.05 mm Dimension W of multilayer ceramic capacitor in width direction y: 0.65 mm ± 0.05 mm Dimension T of multilayer ceramic capacitor in lamination direction: 0.45 mm ± 0.05 mm Main component of inner dielectric layer: BaTiO3 Main component of outer dielectric layer: BaTiO3 Main component of first internal electrode layer: Ni Thickness of first internal electrode layer: 0.50 μm ± 0.10 μm Main component of first dummy electrode: Ni Thickness of first dummy electrode: 0.50 μm ± 0.10 μm Length of first dummy electrode in width direction y: see Table 6 Main component of second internal electrode layer: Ni Thickness of second internal electrode layer: 0.50 μm ± 0.10 μm Length in the width direction y of the lead electrode portion of the second internal electrode layer: 130 μm Distance between the first internal electrode layer and the side surface: 82 μm Distance between the opposing electrode portion of the second internal electrode layer and the side surface: 82 μm Distance between the opposing electrode portion of the second internal electrode layer and the end face: 62 μm Configuration of the first external electrode and the second external electrode: Base electrode layer (Cu), plating layer (two-layer structure: Ni / Sn plating) Configuration of the third external electrode and the fourth external electrode: Base electrode layer (Cu), plating layer (two-layer structure: Ni / Sn plating) Total number of first internal electrode layers and second internal electrode layers: 260

[0160] (2) Method for Calculating the Width Direction Ratio of the First Dummy Electrode The ratio was calculated using the same method as in Experimental Examples 1-1 and 1-2.

[0161] (3) Method of Moisture Resistance Reliability Test: Each multilayer ceramic capacitor without peeling was mounted on a wiring board using solder, and the insulation resistance value was measured. Each sample of the multilayer ceramic capacitor mounted on the wiring board was placed in a high-temperature, high-humidity chamber, and a DC current of 4 V was applied between the first and second external electrodes of each multilayer ceramic capacitor at 125°C and 95% RH for 144 hours. The insulation resistance of each multilayer ceramic capacitor sample after the moisture resistance test was measured, and if the insulation resistance value after the moisture resistance test was one order of magnitude lower than the insulation resistance value before the moisture resistance test, it was judged as NG. Then, (number of NG / 70 capacitors) x 100 was calculated, and this value was defined as the NG rate.

[0162] The evaluation results are shown in Tables 5 and 6.

[0163]

[0164] (4) Summary According to Experimental Example 2-1, when the ratio of first dummy electrodes was 96% or less, good results were obtained with a NG rate of 1% or less in the moisture resistance reliability test, as shown in Sample Nos. 50 to 62. Furthermore, according to Experimental Example 2-2, when the ratio of first dummy electrodes was 97% or less, good results were obtained with a NG rate of 1% or less in the moisture resistance reliability test, as shown in Sample Nos. 67 to 79.

[0165] On the other hand, according to Experimental Example 2-1, when the ratio of first dummy electrodes was 96.5% or more, the NG rate in the moisture resistance reliability test exceeded 1%, as shown in Sample Nos. 63 to 66. Furthermore, according to Experimental Example 2-2, when the ratio of first dummy electrodes was 97.5% or more, the NG rate in the moisture resistance reliability test exceeded 1%, as shown in Sample Nos. 80 to 83.

[0166] From the above results, it is clear that a multilayer ceramic capacitor having high moisture resistance reliability can be obtained by setting the ratio of the first dummy electrodes to at least 96% or less.

[0167] B-2. Second Dummy Electrode (1) Specifications of Samples in Experimental Examples 2-3 and 2-4 In Experimental Examples 2-3 and 2-4, laminates of different dimensions were manufactured according to the manufacturing method of the multilayer ceramic capacitor described above, and then samples were fabricated in which the length of the second dummy electrode in the width direction y was varied. The length of the second dummy electrode in the length direction z was 50% of the distance between the lead electrode portion of the second internal electrode layer and the first end face, or the distance between the lead electrode portion of the second internal electrode layer and the second end face. The arrangement of the second dummy electrode was the same as in Experimental Examples 1-3 and 1-4, as shown in FIG. 11 . The laminates used in Experimental Examples 2-3 and 2-4 did not have a first dummy electrode.

[0168] (Experimental Example 2-3) Structure of multilayer ceramic capacitor: 3 terminals Dimension L of multilayer ceramic capacitor in length direction z: 1.20 mm ± 0.05 mm Dimension W of multilayer ceramic capacitor in width direction y: 0.90 mm ± 0.05 mm Dimension T of multilayer ceramic capacitor in lamination direction: 0.60 mm ± 0.05 mm Main component of inner dielectric layer: BaTiO3 Main component of outer dielectric layer: BaTiO3 Main component of first internal electrode layer: Ni Thickness of first internal electrode layer: 0.50 μm ± 0.10 μm Main component of second internal electrode layer: Ni Thickness of second internal electrode layer: 0.50 μm ± 0.10 μm Length of lead electrode portion of second internal electrode layer in width direction y: 220 μm Main component of second dummy electrode: Ni Thickness of second dummy electrode: 0.50 μm ± 0.10 μm Length of second dummy electrode in width direction y: See Table 7 Distance between first internal electrode layer and side surface: 52 μm Distance between opposing electrode portion of second internal electrode layer and side surface: 52 μm Distance between opposing electrode portion of second internal electrode layer and end face: 52 μm Structure of first external electrode and second external electrode: Base electrode layer (Cu), plating layer (two-layer structure: Ni / Sn plating) Structure of third external electrode and fourth external electrode: Base electrode layer (Cu), plating layer (two-layer structure: Ni / Sn plating) Total number of first internal electrode layers and second internal electrode layers: 478

[0169] (Experimental Example 2-4) Structure of multilayer ceramic capacitor: 3 terminals Dimension L of multilayer ceramic capacitor in length direction z: 1.15 mm ± 0.05 mm Dimension W of multilayer ceramic capacitor in width direction y: 0.65 mm ± 0.05 mm Dimension T of multilayer ceramic capacitor in lamination direction: 0.45 mm ± 0.05 mm Main component of inner dielectric layer: BaTiO3 Main component of outer dielectric layer: BaTiO3 Main component of first internal electrode layer: Ni Thickness of first internal electrode layer: 0.50 μm ± 0.10 μm Main component of second internal electrode layer: Ni Thickness of second internal electrode layer: 0.50 μm ± 0.10 μm Length of lead electrode portion of second internal electrode layer in width direction y: 130 μm Main component of second dummy electrode: Ni Thickness of second dummy electrode: 0.50 μm ± 0.10 μm Length of the second dummy electrode in the width direction y: See Table 8 Distance between the first internal electrode layer and the side surface: 82 μm Distance between the opposing electrode portion of the second internal electrode layer and the side surface: 82 μm Distance between the opposing electrode portion of the second internal electrode layer and the end face: 62 μm Structure of the first external electrode and the second external electrode: Base electrode layer (Cu), plating layer (two-layer structure: Ni / Sn plating) Structure of the third external electrode and the fourth external electrode: Base electrode layer (Cu), plating layer (two-layer structure: Ni / Sn plating) Total number of first internal electrode layers and second internal electrode layers: 260

[0170] (2) Method for Calculating the Width Direction Ratio of the Second Dummy Electrode The ratio was calculated using the same method as in Experimental Examples 1-3 and 1-4.

[0171] (3) Method of Moisture Resistance Reliability Test The test was carried out in the same manner as in Experimental Examples 2-3 and 2-4.

[0172] The evaluation results are shown in Tables 7 and 8.

[0173]

[0174] (4) Summary According to Experimental Example 2-3, when the second dummy electrode ratio was 96% or less, good results were obtained with a NG rate of 1% or less in the moisture resistance reliability test, as shown in Sample Nos. 84 to 97. Furthermore, according to Experimental Example 2-4, when the second dummy electrode ratio was 97% or less, good results were obtained with a NG rate of 1% or less in the moisture resistance reliability test, as shown in Sample Nos. 102 to 114.

[0175] On the other hand, according to Experimental Example 2-3, when the second dummy electrode ratio was 96.5% or more, the NG rate in the moisture resistance reliability test exceeded 1%, as shown in Sample Nos. 98 to 101. Also, according to Experimental Example 2-4, when the second dummy electrode ratio was 97.5% or more, the NG rate in the moisture resistance reliability test exceeded 1%, as shown in Sample Nos. 115 to 118.

[0176] From the above results, it is clear that a multilayer ceramic capacitor having high moisture resistance reliability can be obtained by setting the second dummy electrode ratio to at least 96% or less.

[0177] C. Experimental Results From the above results, Experimental Examples 1-1 to 1-4 revealed that the presence of the first dummy electrodes or the second dummy electrodes can reduce the peeling occurrence rate to 30%. Furthermore, Experimental Examples 1-1 and 1-2 confirmed that the peeling occurrence rate can be sufficiently suppressed by setting the first dummy electrode ratio to 68% or more. Furthermore, Experimental Examples 1-3 and 1-4 confirmed that the peeling occurrence rate can be sufficiently suppressed by setting the second dummy electrode ratio to 70% or more.

[0178] According to Experimental Examples 2-1 and 2-3, by setting the ratio of the first dummy electrodes to 96% or less, the NG rate in the moisture resistance reliability test can be reduced to 0%, and it was confirmed that there are no problems with moisture resistance. Also, according to Experimental Examples 2-3 and 2-4, by setting the ratio of the second dummy electrodes to 96% or less, the NG rate in the moisture resistance reliability test can be reduced to 0%, and it was confirmed that there are no problems with moisture resistance.

[0179] In the above-mentioned experimental example, when the first dummy electrode is arranged, the second dummy electrode is not arranged, and when the second dummy electrode is arranged, the first dummy electrode is not arranged, but the effects of the present invention can be obtained even when both the first dummy electrode and the second dummy electrode are arranged.

[0180] Furthermore, not limited to this experiment, even when the dimension of the first dummy electrode in the longitudinal direction of the laminate is increased, the proportion of conductive components increases, so the incidence of peeling can be suppressed.

[0181] As described above, although the embodiments of the present invention have been disclosed in the above description, the present invention is not limited thereto. In other words, various modifications can be made to the above-described embodiments in terms of mechanism, shape, material, quantity, position, arrangement, etc., without departing from the scope of the technical idea and purpose of the present invention, and such modifications are included in the present invention.

[0182] <1> A multilayer ceramic capacitor comprising: a laminate including a plurality of laminated dielectric layers and a plurality of internal electrode layers laminated on the dielectric layers, the laminate having first and second main surfaces opposing each other in a lamination direction, first and second side surfaces opposing each other in a width direction perpendicular to the lamination direction, and first and second end surfaces opposing each other in a length direction perpendicular to the lamination direction and the width direction; a first external electrode disposed on the first end surface; a second external electrode disposed on the second end surface; a third external electrode disposed on the first side surface; and a fourth external electrode disposed on the second side surface, wherein the plurality of internal electrode layers are comprised of: a first internal electrode layer disposed on the plurality of dielectric layers and connected to the first external electrode and the second external electrode; a second internal electrode layer disposed on the plurality of dielectric layers different from the first internal electrode layer and connected to the third external electrode and the fourth external electrode; a first dummy electrode spaced apart from the first internal electrode layer and disposed on the same plane as the first internal electrode layer, wherein the first dummy electrode is not exposed from the first side surface, the second side surface, the first end surface, or the second end surface.

[0183] <2> The multilayer ceramic capacitor according to <1>, further comprising a second dummy electrode disposed apart from the second internal electrode layer and on the same plane as the second internal electrode layer, wherein the second dummy electrode is not exposed from the first end face, the second end face, the first side face, and the second side face.

[0184] <3> The multilayer ceramic capacitor according to <1> or <2>, wherein the main component of the first dummy electrode is the same as the main component of the first internal electrode layer.

[0185] <4> The multilayer ceramic capacitor according to any one of <1> to <3>, wherein a distance between the first dummy electrode and one of the first side surface and the second side surface that is closest to the first dummy electrode is 1 μm or more, and a shortest distance between the first dummy electrode and the first internal electrode layer is 1 μm or more.

[0186] <5> The multilayer ceramic capacitor according to any one of <1> to <4>, wherein the thickness of the first dummy electrode in the stacking direction is 83% or more and 120% or less of the thickness of the first internal electrode layer in the stacking direction.

[0187] <6> The multilayer ceramic capacitor according to any one of <1> to <5>, wherein the first dummy electrode ratio is 68% or more and 96% or less of the shortest distance from the first internal electrode layer to the first side surface.

[0188] REFERENCE SIGNS LIST 10 Multilayer ceramic capacitor 12 Laminate 14 Dielectric layer 16, Internal electrode layer 16a First internal electrode layer 16b Second internal electrode layer 18 Internal layer portion 20a First main surface side outer layer portion 20b Second main surface side outer layer portion 22a First opposing electrode portion 22b Second opposing electrode portion 24a First lead electrode portion 24b Second lead electrode portion 24c Third lead electrode portion 24d Fourth lead electrode portion 26a, 26b Side portion (W gap) 27a, 27b End portion (L gap) 28, 29 Dummy electrodes 28, 28a, 28a1, 28a2, 28b, 28b1, 28b2 First dummy electrode 29, 29a, 29a1, 29a2, 29b, 29b1, 29b2 Second dummy electrode 30 External electrode 30a First external electrode 30b Second external electrode 30c Third external electrode 30d Fourth external electrode 32 Base electrode layer 32a First base electrode layer 32b Second base electrode layer 32c Third base electrode layer 32d Fourth base electrode layer 34 Plating layer 34a First plating layer 34b Second plating layer 34c Third plating layer 34d Fourth plating layer x Stacking direction y Width direction z Length direction

Claims

1. A laminate including a plurality of laminated dielectric layers and a plurality of internal electrode layers laminated on the dielectric layers, the laminate having a first main surface and a second main surface opposing each other in a lamination direction, a first side surface and a second side surface opposing each other in a width direction perpendicular to the lamination direction, and a first end surface and a second end surface opposing each other in a length direction perpendicular to the lamination direction and the width direction; a first external electrode disposed on the first end surface, a second external electrode disposed on the second end surface, a third external electrode disposed on the first side surface, and a fourth external electrode disposed on the second side surface, wherein the plurality of internal electrode layers are comprised of a first internal electrode layer disposed on the plurality of dielectric layers and connected to the first external electrode and the second external electrode, a second internal electrode layer disposed on the plurality of dielectric layers different from the first internal electrode layer, and connected to the third external electrode and the fourth external electrode, a first dummy electrode spaced apart from the first internal electrode layer and disposed on the same plane as the first internal electrode layer, wherein the first dummy electrode is not exposed from the first side surface, the second side surface, the first end face, and the second end face.

2. The multilayer ceramic capacitor according to claim 1, further comprising a second dummy electrode disposed apart from said second internal electrode layer and on the same plane as said second internal electrode layer, said second dummy electrode being not exposed from said first end face, said second end face, said first side face and said second side face.

3. The multilayer ceramic capacitor according to claim 1 or 2, wherein the main component of said first dummy electrode is the same as the main component of said first internal electrode layer.

4. A multilayer ceramic capacitor as described in any one of claims 1 to 3, wherein the distance between said first dummy electrode and one of said first side surface and said second side surface which is closest to said first dummy electrode is 1 μm or more, and the shortest distance between said first dummy electrode and said first internal electrode layer is 1 μm or more.

5. A multilayer ceramic capacitor according to any one of claims 1 to 4, wherein the thickness of said first dummy electrode in said lamination direction is 83% or more and 120% or less of the thickness of said first internal electrode layer in said lamination direction.

6. A multilayer ceramic capacitor as set forth in any one of claims 1 to 5, wherein the first dummy electrode ratio is 68% or more and 96% or less of the shortest distance from the first internal electrode layer to the first side surface.

Citation Information

Patent Citations

  • Laminated electronic component

    JP2002252136A

  • Through-type three-terminal electronic component

    JP2003022932A