Electrode active material, electrode, and battery

By embedding carbon within the pores of titanium-containing oxide particles in solid-state batteries, the electrode resistance is reduced, enhancing electron conductivity and maintaining sinterability, thus improving the initial discharge capacity of solid-state batteries.

WO2024247489A1PCT designated stage expired Publication Date: 2024-12-05PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/014105
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-31
Filing Date
2024-04-05
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Solid-state batteries face challenges with high electrode resistance, which limits battery capacity, due to inadequate electron conduction paths in titanium-containing oxide particles when used in solid-state batteries, leading to decreased initial discharge capacity.

Method used

Incorporating a carbon material inside the pores of titanium-containing oxide particles with average pore diameters between 50 nm and 200 nm, creating multiple electron conduction paths and maintaining sinterability by reducing the amount of carbon-based conductive additives needed, thereby enhancing electron conductivity and interface formation with the solid electrolyte.

Benefits of technology

This approach improves the initial discharge capacity of solid-state batteries while maintaining electrode sinterability, reducing resistance, and promoting a good contact interface between the electrode active material and the solid electrolyte.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024014105_05122024_PF_FP_ABST
    Figure JP2024014105_05122024_PF_FP_ABST
Patent Text Reader

Abstract

An electrode active material (10) according to the present disclosure comprises oxide particles (1) that contain titanium and do not contain lithium, and a carbon material (2). The oxide particles (1) have a plurality of pores (11) that have an average pore diameter (S) of 50–200 nm. The carbon material (2) is present inside the pores (11). An electrode (100) according to the present disclosure comprises the electrode active material (10), and a solid electrolyte (20) that is in contact with the electrode active material (10). A battery (1000) according to the present disclosure comprises a positive electrode (200), a negative electrode (300), and an electrolyte layer (400) that is disposed between the positive electrode (200) and the negative electrode (300). The positive electrode (200) or the negative electrode (300) includes the electrode (100).
Need to check novelty before this filing date? Find Prior Art

Description

Electrode active material, electrode, and battery

[0001] The present disclosure relates to an electrode active material, an electrode, and a battery.

[0002] Research and development of solid-state batteries as next-generation batteries is actively underway. One of the challenges of solid-state batteries is the high resistance of their electrodes, which makes it difficult to extract the full battery capacity. Therefore, there is a need to reduce the resistance of the electrodes. To reduce the electrode resistance, it is important to form a good interface between the solid electrolyte and the electrode active material. For example, a sintered body of a solid electrolyte and an electrode active material is suitable for use as an electrode for a solid-state battery because it is easy to form a good interface between the solid electrolyte and the electrode active material.

[0003] Patent Document 1 discloses a method for producing titanium dioxide particles containing secondary particles formed by aggregation of anatase or rutile type primary particles, the secondary particles having a size of 0.005 to 1.0 cm 3 According to the pore distribution (FIG. 5) in Patent Document 1, the pore diameter of the secondary particles in the examples is about 10 nm or less.

[0004] Patent No. 5400607

[0005] In the prior art, it is desirable to improve the initial discharge capacity of a battery while maintaining the sinterability of the electrode.

[0006] The present disclosure provides an electrode active material comprising: oxide particles containing titanium and not containing lithium; and a carbon material, wherein the oxide particles have a plurality of pores with an average pore diameter of 50 nm or more and 200 nm or less, and the carbon material is present inside the pores.

[0007] According to the present disclosure, it is possible to improve the initial discharge capacity of a battery while maintaining the sinterability of the electrode.

[0008] FIG. 1 is a cross-sectional view showing a schematic configuration of an electrode active material in a first embodiment. FIG. 2 is a cross-sectional view showing a schematic configuration of an oxide particle in the first embodiment. FIG. 3 is an SEM image (30,000x magnification) showing an example of a cross section of an electrode active material in the first embodiment. FIG. 4 is an SEM image (20,000x magnification) showing an example of a cross section of an oxide particle in the first embodiment. FIG. 5 is a cross-sectional view showing a schematic configuration of an electrode in a second embodiment. FIG. 6 is a cross-sectional view showing a schematic configuration of a battery in a third embodiment. FIG. 7 is a Raman spectrum of the electrode active material in Example 3. FIG. 8 is a first cycle charge / discharge curve for the negative electrode half-cells of Examples 1 to 3 and Reference Example 1. FIG. 9 is a first cycle charge / discharge curve for the negative electrode half-cell of Example 4. FIG. 10 is a first cycle charge / discharge curve for the negative electrode half-cell of Example 5. FIG. 11 is a first cycle charge / discharge curve for the negative electrode half-cell of Example 6. FIG. 12 is a first cycle charge / discharge curve for the negative electrode half-cell of Reference Example 2. Fig. 13 shows the charge / discharge curves for the first cycle of the negative electrode half-cell of Reference Example 5. Fig. 14 is a graph showing the relationship between the number of cycles and the charge capacity of the negative electrode half-cells of Examples 1 and 2. In the negative electrode half-cell, the side from which Li is desorbed corresponds to charging (discharging in the battery). Fig. 15 is a graph showing the relationship between the number of cycles and the capacity retention rate of the negative electrode half-cells of Examples 1 and 2.

[0009] (Findings forming the basis of the present disclosure) The present inventors have investigated the use of titanium-containing oxides as electrode active materials. Titanium-containing oxides have advantages such as low cost mass production, excellent charge / discharge characteristics, and high safety, and are therefore considered promising as electrode active materials for solid-state batteries.

[0010] Titanium-containing oxides are known to be used in liquid batteries using electrolytes. Oxides for this purpose are produced, for example, by granulating primary particles into secondary particles. In liquid batteries, ion conduction paths are formed by the penetration of electrolyte into the pores of the secondary particles. The pore diameters of the pores in the secondary particles of oxides used in liquid batteries are typically small, on the order of 10 nm. This is because if the pore diameter is too large, the volume ratio of the electrode active material in the battery decreases, resulting in a decrease in battery capacity. However, according to the inventors' studies, when such oxide particles are used in solid-state batteries, good electron conduction paths are not formed inside the oxide particles, resulting in a decrease in electronic conductivity. As a result, the initial discharge capacity of the battery was confirmed to decrease.

[0011] The present inventors have conducted extensive research into titanium-containing oxides that are suitable for improving the initial discharge capacity of a battery while maintaining the sinterability of the electrode, and have arrived at the present invention.

[0012] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings. The present disclosure is not limited to the following embodiments.

[0013] (First embodiment) Fig. 1 is a cross-sectional view showing a schematic configuration of an electrode active material 10 in the first embodiment. Fig. 2 is a cross-sectional view showing a schematic configuration of an oxide particle 1 in the first embodiment. The electrode active material 10 is used, for example, in a positive electrode or a negative electrode of a solid-state battery. The positive electrode or negative electrode of the solid-state battery is produced, for example, by firing a compact of a powder material containing a powder of a solid electrolyte and a powder of the electrode active material 10.

[0014] In this specification, "sintering" refers to the phenomenon in which bonding occurs between particles when a compact of powder material is heated, causing the compact to become dense with volumetric shrinkage. "Firing" refers to the heat treatment for sintering.

[0015] In this embodiment, the electrode active material 10 includes oxide particles 1 that contain titanium but no lithium, and a carbon material 2. In the electrode active material 10, the oxide particles 1 have a plurality of pores 11 having an average pore diameter S of 50 nm or more and 200 nm or less. When a sintered electrode is used, as in an all-solid-state oxide battery, structural destruction due to expansion and contraction of the electrode active material becomes an issue. However, by using the electrode active material 10 of this embodiment as the electrode active material, the structural destruction can be alleviated.

[0016] The oxide particles 1 are a material capable of absorbing and releasing metal ions such as lithium ions. The oxide particles 1 can function as an active material. The carbon material 2 has electronic conductivity. The carbon material 2 is present inside the pores 11 of the oxide particles 1. This structure forms many electronic conduction paths between the oxide particles 1 and the carbon material 2. This allows electrons to be transported to the interior of the pores 11 of the oxide particles 1, thereby improving the electronic conductivity of the electrode active material 10. As a result, the initial discharge capacity of the battery is improved. Furthermore, because the carbon material 2 is disposed inside the pores 11 of the oxide particles 1, the amount of carbon-based conductive additive kneaded with the electrode active material 10 during the electrode forming process can be reduced. Therefore, the carbon-based conductive additive is less likely to penetrate between the particles of the solid electrolyte and does not hinder the sintering between the particles of the solid electrolyte. In other words, the electrode active material 10 of this embodiment can improve the sintering between the particles of the solid electrolyte, thereby improving the sintering of the electrode. Therefore, a good contact interface between the electrode active material 10 and the solid electrolyte is easily formed.

[0017] The presence of the oxide particle 1 in the pores 11 and the presence of the carbon material 2 in the pores 11 in the electrode active material 10 can be confirmed, for example, by observing a cross section of the electrode active material 10 with a scanning electron microscope (SEM). FIG. 3 is an SEM image (30,000x magnification) showing an example of a cross section of the electrode active material 10. FIG. 3 is an example of a cross-sectional SEM image of the electrode active material of Example 3, which will be described later. The cross-sectional SEM image of FIG. 3 was observed after embedding the electrode active material 10 in resin and then polishing the electrode active material 10 to expose its cross section. To clarify the presence state of the carbon material 2, the observation was performed in a manner that allowed for distinction between the carbon material 2 and the resin based on the contrast difference. Therefore, in the SEM image of FIG. 3, the dark areas represent the carbon material 2 present inside the pores 11. FIG. 4 is an SEM image (20,000x magnification) showing an example of a cross section of the oxide particle 1. The cross-sectional SEM image of Fig. 4 was obtained by embedding an oxide particle 1 in a resin, polishing the oxide particle 1 to expose its cross section, and then observing the image with a method that emphasizes image clarity, similar to Fig. 3 . In the SEM image of Fig. 4 , dark regions represent pores 11. As shown in Fig. 4 , the oxide particle 1 has a plurality of pores 11. As shown in Fig. 3 , the carbon material 2 is present inside the pores 11 of the oxide particle 1. More specifically, the carbon material 2 is present so as to coat the inner surfaces of the pores 11. The carbon material 2 may coat a portion of the inner surfaces of the pores 11.

[0018] The carbon material 2 does not have to be present inside all of the plurality of pores 11. The plurality of pores 11 may include pores 11 in which no carbon material 2 is present.

[0019] In this embodiment, the average pore diameter S of the plurality of pores 11 in the electrode active material 10 is 50 nm or more and 200 nm or less. The average pore diameter S may be 60 nm or more and 190 nm or less, or 70 nm or more and 180 nm or less. With such a structure, structural destruction due to expansion and contraction of the electrode active material 10 is likely to be alleviated.

[0020] The lower limit of the average pore diameter S may be 80 nm, 90 nm, or even 100 nm. With such a structure, structural destruction due to expansion and contraction of the electrode active material 10 is likely to be alleviated.

[0021] The upper limit of the average pore diameter S may be 170 nm, 160 nm, or even 150 nm. With such a structure, a decrease in the volume ratio of the electrode active material 10 in the battery is suppressed, and therefore a decrease in the battery capacity is likely to be suppressed.

[0022] The average pore diameter S of the pores 11 in the electrode active material 10 can be determined by, for example, mercury intrusion porosimetry.

[0023] In mercury intrusion porosimetry, high-pressure mercury is first injected into a sample having pores. The pore distribution can be determined from the relationship between the pressure applied to the mercury and the amount of mercury injected into the sample. The pore distribution can be measured, for example, using a mercury porosimeter. Specifically, the diameter D of the pores in the sample into which mercury has been injected can be determined from the following relational expression (I): In relational expression (I), γ is the surface tension of mercury, θ is the contact angle between the mercury and the wall surface of the sample, and P is the pressure applied to the mercury.

[0024] D=-4γcosθ÷P...(I)

[0025] The pressure P is changed in stages, and the amount of injected mercury is measured for each pressure P. The amount of injected mercury can be regarded as the cumulative value of the volume of pores up to a diameter D corresponding to a specific pressure P. This makes it possible to obtain a pore distribution in which the volume of pores is specified for each diameter D. The pore distribution is, for example, a graph showing the relationship between the diameter D of the pores and the log differential pore volume.

[0026] From the pore distribution obtained for the electrode active material 10, the average pore diameter S (median diameter) of the multiple pores 11 in the electrode active material 10 can be calculated. At this time, voids observed other than the intraparticle voids of the electrode active material 10, i.e., pores associated with interparticle voids, are excluded. The intraparticle voids and interparticle voids can be confirmed by cross-sectional SEM observation of the particles of the electrode active material 10.

[0027] The carbon material 2 may cover a portion of the outer surface 1s of the oxide particle 1. As shown in FIGS. 1 and 3, the oxide particle 1 may have an outer surface 1sa covered by the carbon material 2 and an outer surface 1sb not covered by the carbon material 2. As shown in FIGS. 1 and 3, in a cross section of the electrode active material 10, the length of the outer surface 1sa covered by the carbon material 2 may be shorter than the length of the outer surface 1sb not covered by the carbon material 2. With this structure, the carbon material 2 is less likely to inhibit the sintering between the particles of the electrode active material 10 and the solid electrolyte during the electrode forming process. As a result, deterioration of the sintering properties of the electrode is suppressed. Furthermore, ion transport between the electrode active material 10 and the solid electrolyte is promoted, thereby reducing the ionic resistance at the contact interface between the electrode active material 10 and the solid electrolyte. The length of the outer surface 1sa covered by the carbon material 2 and the length of the outer surface 1sb not covered by the carbon material 2 can be determined, for example, from an SEM image of the cross section of the electrode active material 10.

[0028] 1 and 3 , in the cross section of the electrode active material 10, the area occupied by the carbon material 2 present inside the pores 11 may be larger than the area occupied by the carbon material 2 covering the outer surfaces 1s of the pores 11. With such a structure, it is possible to improve the electronic conductivity of the electrode active material 10 and to suppress deterioration of the sinterability of the electrode in the stage of forming the electrode. The area occupied by the carbon material 2 present inside the pores 11 and the area occupied by the carbon material 2 covering the outer surfaces 1s of the pores 11 can be determined, for example, from an SEM image of the cross section of the electrode active material 10.

[0029] In the oxide particle 1, the plurality of pores 11 may include pores that communicate with the outside. The oxide particle 1 does not need to include completely closed voids that are not in communication with the outside. With such a structure, it is easy to arrange the carbon material 2 inside the pores 11 in the process of producing the electrode active material 10. The fact that the plurality of pores 11 include pores that communicate with the outside can be confirmed, for example, in an SEM image of a cross section of the electrode active material 10. For example, in the SEM image shown in FIG. 3, the carbon material 2 is present in most of the pores 11, confirming that these pores 11 are pores that communicate with the outside. Furthermore, in the SEM image of the cross section of the oxide particle 1 shown in FIG. 4, it can also be confirmed that the plurality of pores 11 include pores that communicate with the outside. In the SEM image of the cross section of the oxide particle 1, the non-communicating pores are observed as bubbles with no resin present because the resin cannot penetrate them. Note that bubbles are not confirmed in FIG. 4.

[0030] The oxide particles 1 may be secondary particles containing a plurality of primary particles. With such a structure, the average pore diameter S of the electrode active material 10 is likely to fall within the above-mentioned range.

[0031] The shape of the primary particles is not particularly limited, and may be, for example, plate-like, scale-like, needle-like, spherical, or oval-spherical.

[0032] For example, the pores 11 may be formed between two of the plurality of primary particles. The plurality of pores 11 may be formed three-dimensionally and continuously.

[0033] When the oxide particle 1 is a secondary particle, the secondary particle may be a sintered body of a plurality of primary particles. With such a structure, the primary particles are bonded to each other and densified, thereby forming a good ion conduction path inside the oxide particle 1. As a result, the ion conductivity inside the electrode active material 10 is further improved, and the initial discharge capacity of the battery is further improved. In the case of a solid-state battery that does not use a liquid electrolyte, it is desirable that the secondary particle be a sintered body of a plurality of primary particles.

[0034] The shape of the oxide particle 1 is not particularly limited. The shape of the oxide particle 1 is, for example, spherical or oval spherical. The shape of the oxide particle 1 may be needle-like, plate-like, or the like. When the oxide particle 1 is a secondary particle, the outer surface 1s of the oxide particle 1 may have an irregular shape resulting from a primary particle such as a spherical shape.

[0035] When the oxide particles 1 are secondary particles, the median diameter of the multiple primary particles in the electrode active material 10 may be 50 nm or more and 500 nm or less. With such a structure, the average pore diameter S of the electrode active material 10 is more likely to satisfy the above-mentioned numerical range.

[0036] In this specification, the term "median diameter" refers to the particle size when the cumulative volume in the volume-based particle size distribution is equal to 50%. The volume-based particle size distribution is measured using, for example, a laser diffraction measurement device.

[0037] The median diameter of the plurality of primary particles in the electrode active material 10 may be 60 nm or more and 400 nm or less, or may be 70 nm or more and 300 nm or less.

[0038] The lower limit of the median diameter of the multiple primary particles in the electrode active material 10 may be 80 nm, 90 nm, or even 100 nm. If the median diameter of the primary particles is large, the number of grain boundaries decreases. Therefore, from the viewpoint of ion conduction paths, it is desirable that the lower limit of the median diameter of the primary particles be in the above-mentioned numerical range.

[0039] The upper limit of the median diameter of the plurality of primary particles in the electrode active material 10 may be 250 nm, 200 nm, or even 150 nm. When the median diameter of the primary particles is small, it is easy to control the pore structure.

[0040] The median diameter of the oxide particles 1 in the electrode active material 10 may be more than 2 μm and less than 7 μm.

[0041] The electrode active material 10 can be present between particles of the solid electrolyte during the electrode forming stage. The electrode active material 10 having oxide particles 1 on the order of micrometers can reduce the total contact area between the electrode active material 10 and the solid electrolyte particles compared to when oxide particles on the order of nanometers are used. This reduces the influence of the solid electrolyte particles as a factor inhibiting sinterability, thereby improving the sinterability of the electrode. In other words, a good contact interface can be formed between the electrode active material 10 and the solid electrolyte. This reduces the resistance of the electrode. The sinterability of the electrode can be determined, for example, by the porosity of the electrode.

[0042] The median diameter of the oxide particles 1 in the electrode active material 10 may be 2.5 μm or more and 6.5 μm or less, or may be 3.5 μm or more and 6.0 μm or less.

[0043] The pore volume of the pores 11 in the electrode active material 10 of unit mass is V 10 The pore volume V is defined as 10 may be 0.01 mL / g or more and 0.5 mL / g or less. With such a structure, many electron conduction paths are easily formed between the oxide particles 1 and the carbon material 2, thereby further improving the electron conductivity of the electrode active material 10. As a result, the initial discharge capacity of the battery is further improved.

[0044] Pore ​​volume V 10 may be 0.015 mL / g or more and 0.5 mL / g or less, or 0.02 mL / g or more and 0.5 mL / g or less.

[0045] Pore ​​volume V 10 The lower limit may be 0.03 mL / g, or even 0.04 mL / g.

[0046] Pore ​​volume V 10 There is no particular upper limit to the pore volume V 10 The upper limit of the pore volume V may be, for example, 0.3 mL / g, or even 0.2 mL / g. 10When the volume ratio of the electrode active material 10 in the battery becomes too large, a decrease in the volume ratio of the electrode active material 10 in the battery and an accompanying decrease in the capacity of the battery can be suppressed. Furthermore, during the production of the battery, collapse of the electrode active material 10 in a step in which pressure is applied to the electrode active material 10, such as a pressing step, can be avoided.

[0047] The volume occupancy Rv of the carbon material 2 with respect to the pores 11 in the electrode active material 10 may be 0.5 volume % or more and 80 volume % or less. With such a structure, many electron conduction paths are easily formed between the oxide particles 1 and the carbon material 2, thereby further improving the electron conductivity of the electrode active material 10. As a result, the initial discharge capacity of the battery is further improved.

[0048] The volume occupancy Rv may be 1.0 vol% or more and 75 vol% or less, 3.0 vol% or more and 70 vol% or less, 5.0 vol% or more and 65 vol% or less, or 8.0 vol% or more and 61 vol% or less.

[0049] The volume occupancy Rv may be 0.5% by volume or more and 30% by volume or less. With such a structure, the pores 11 where the carbon material 2 is not present can suppress structural destruction due to expansion and contraction of the electrode active material 10, which tends to improve the cycle characteristics of the battery. This effect is more likely to occur when a sintered electrode in which the periphery of the electrode active material 10 is firmly bonded is used.

[0050] The pore volume of the pore 11 in the oxide particle 1 before the carbon material 2 is placed is defined as V1, and the pore volume of the pore 11 in the oxide particle 1 after the carbon material 2 is placed is defined as V 10 At this time, the volume occupancy Rv of the carbon material 2 with respect to the pores 11 in the electrode active material 10 is defined as 100×(V−V 10 ) / V1. Pore volume V1 and pore volume V 10 can be determined from the pore distribution obtained by, for example, the above-mentioned mercury intrusion porosimetry. Note that the pore volume V can be determined by mercury intrusion porosimetry after firing the oxide particles 1 after the carbon material 2 has been disposed therein to decompose and remove the carbon material 2.

[0051] The pore volume V can be calculated from the pore distribution obtained for the oxide particles 1 before the carbon material 2 is disposed. 10 In this calculation, voids observed other than the intraparticle voids of the oxide particle 1 and the electrode active material 10, i.e., pores associated with the interparticle voids, are excluded. The intraparticle voids and the interparticle voids can be confirmed by cross-sectional SEM observation of the oxide particle 1 and the electrode active material 10 particles.

[0052] The ratio Rw of the mass of the carbon material 2 to the mass of the electrode active material 10 may be 0.5% by mass or more and 30% by mass or less. In an electrode active material in which a carbon material is deposited on the surface of an oxide particle, if the mass of the carbon material is too large, the ionic conductivity of the electrode active material is impaired. Therefore, in such an electrode active material, it is common to minimize the amount of carbon material deposited. However, in the electrode active material 10 of this embodiment, the carbon material 2 is disposed inside the pores 11 rather than on the outer surfaces 1s of the oxide particles 1. Therefore, even if the ratio Rw of the mass of the carbon material 2 is 0.5% by mass or more and 30% by mass or less, the electronic conductivity of the electrode active material 10 can be improved without reducing the ionic conductivity.

[0053] The ratio Rw may be 1.0 mass % or more and 20 mass % or less, 1.0 mass % or more and 15 mass % or less, 1.0 mass % or more and 10 mass % or less, 1.0 mass % or more and 5 mass % or less, or even 1.0 mass % or more and 3 mass % or less. With such a structure, the capacity of the battery can be increased.

[0054] The mass ratio Rw of the carbon material 2 in the electrode active material 10 can be determined by, for example, measuring the weight loss of a sample by a simultaneous differential thermal analysis (TG-DTA) method. Specifically, a TG curve of the sample is obtained using a simultaneous differential thermal analysis and thermogravimetry measurement device. The weight loss of the sample is determined from the obtained TG curve. When the sample is the electrode active material 10, the weight loss corresponds to the amount of carbon lost due to decomposition and vaporization. Therefore, the weight loss is used as the mass W2 of the carbon material 2 in the electrode active material 10. The mass of the sample is then used as the mass W of the electrode active material 10. 10 The ratio Rw is used as 100 × W2 / W 10 It is calculated as:

[0055] 1580 cm in the Raman spectrum of the electrode active material 10 -1 Peak intensity I G 1360 cm -1 Peak intensity I D Ratio I D / I G The ratio I may be 0.6 or more and 1.4 or less. D / I G represents the degree of graphitization, i.e., the crystallinity, of the carbon material 2 contained in the electrode active material 10. D / I G The smaller the ratio I, the higher the crystallinity of the carbon material 2. D / I G When satisfies the above numerical range, the electrical conductivity of the carbon material 2 can be improved while maintaining high flexibility of the carbon material 2. When the electrical conductivity of the carbon material 2 is high, the electrical conductivity inside the electrode active material 10 is improved, making it easier to extract the initial discharge capacity of the battery. When the flexibility of the carbon material 2 is high, structural changes accompanying expansion and contraction of the electrode active material 10 are easily alleviated.

[0056] The content Ratm of carbon present on the outer surface 1s of the oxide particle 1 in the electrode active material 10 may be 15 atomic % or more and 80 atomic % or less. When the content Ratm of carbon present on the outer surface 1s of the oxide particle 1 satisfies the above numerical range, the electronic conductivity of the electrode active material 10 is improved.

[0057] The content Ratm may be 15 atomic % or more and 75 atomic % or less, 15 atomic % or more and 70 atomic % or less, or 15 atomic % or more and 65 atomic % or less. By setting the content Ratm within such a numerical range, it is possible to reduce the surface coverage of the carbon component, which is a factor inhibiting sintering in the electrode active material 10, and it is easy to form a good interface between the solid electrolyte and the electrode active material 10.

[0058] The lower limit of the content Ratm may be 20 atomic %, 25 atomic %, or even 30 atomic %. By setting the content within such a numerical range, it is possible to form a good interface between the solid electrolyte and the electrode active material 10 while improving the electronic conductivity of the electrode active material 10.

[0059] The carbon content Ratm present on the outer surface 1s of the oxide particles 1 in the electrode active material 10 can be determined, for example, by X-ray photoelectron spectroscopy (XPS). Specifically, the electrode active material 10 is filled into a powder cell and subjected to XPS analysis, thereby obtaining an XPS spectrum of the main elements including carbon. The peak area intensity in each XPS spectrum is used to calculate the proportion (atomic %) of each element. The calculated proportion (atomic %) of carbon element can be regarded as the content Ratm (atomic %).

[0060] The BET specific surface area of ​​the oxide particles 1 is 1 m 2 / g or more 7m 2 / g or less.

[0061] The BET specific surface area of ​​the electrode active material 10 is 2 m 2 / g or more 15m 2 / g or less.

[0062] The BET specific surface area of ​​the oxide particles 1 and the BET specific surface area of ​​the electrode active material 10 can be determined, for example, by converting the data of the adsorption isotherm obtained by the gas adsorption method using nitrogen gas described above using the BET (Brunauer-Emmett-Teller) method.

[0063] Examples of the oxide particles 1 include titanium(IV) oxide and composite oxides containing titanium and a transition metal other than titanium. These materials have the ability to absorb and release metal ions such as lithium ions, and are therefore suitable for use as electrodes in solid-state batteries, for example.

[0064] The oxide particles 1 are preferably capable of being co-sintered with the solid electrolyte. Specifically, it is preferable that they are less reactive with the solid electrolyte and maintain the crystal structure of the oxide even after sintering. For example, titanium (IV) oxide is less reactive with NASICON-type oxide solid electrolytes, which are typical oxide solid electrolytes, and is therefore suitable for the electrode active material 10 of this embodiment. The oxide particles 1 may contain titanium (IV) oxide.

[0065] Examples of titanium(IV) oxide include anatase type (tetragonal crystal) titanium oxide, rutile type (tetragonal crystal) titanium oxide, and brookite type (rectangular crystal) titanium oxide.

[0066] The titanium oxide may contain anatase-type titanium oxide. The main component of the titanium oxide may be anatase-type titanium oxide. Anatase-type titanium oxide is suitable, for example, as an electrode active material for lithium-ion secondary batteries. Furthermore, the use of anatase-type titanium oxide improves the sinterability of an electrode containing the electrode active material 10 and a solid electrolyte. "Main component" means the component that is contained in the largest amount by mass. 90% by mass or more of the titanium oxide may be anatase-type titanium oxide. The titanium oxide may contain substantially only anatase-type titanium oxide.

[0067] The structure of titanium oxide can be investigated by X-ray diffraction measurement or Raman spectroscopy. The ratio of components contained in titanium oxide can be confirmed by analyzing the results of X-ray diffraction measurement by the Rietveld method.

[0068] Examples of composite oxides containing titanium and a transition metal other than titanium include composite oxides containing titanium and niobium. Since composite oxides containing titanium and niobium also have the ability to absorb and release metal ions such as lithium ions, they are suitable for the electrode active material 10 of this embodiment. The composite oxide containing titanium and niobium has a composition of, for example, TiNbO.

[0069] Examples of the carbon material 2 include graphite having a six-membered ring network of carbon atoms, and amorphous carbon.

[0070] There is no particular limitation on the shape of the carbon material 2 itself. For example, the carbon material 2 may be fine particles of the carbon material 101 in the shape of a plate, needle, sphere, oval sphere, or the like.

[0071] <Method for Producing Electrode Active Material> A method for producing the electrode active material 10 of this embodiment will be described. The electrode active material 10 can be produced, for example, by the following method.

[0072] An oxide particle 1 having a plurality of pores 11 is prepared. The oxide particle 1 contains titanium and does not contain lithium. The method for producing the oxide particle 1 having a plurality of pores 11 is not particularly limited. The oxide particle 1 may be a secondary particle containing a plurality of primary particles. The secondary particle may be a sintered body of a plurality of primary particles.

[0073] The method for disposing the carbon material 2 inside the pores 11 of the oxide particles 1 is not particularly limited. For example, by using a liquid phase method, a mixture containing the oxide particles 1, a precursor of the carbon material 2, and a solvent such as ethanol is fired in an inert atmosphere, thereby disposing the carbon material 2 inside the pores 11 of the oxide particles 1. As the precursor of the carbon material 2, for example, a sugar and / or a sugar ester can be used. As the sugar and / or a sugar ester, for example, one or more compounds selected from the group consisting of glucose, fructose, xylose, sucrose, cellulose, and esters thereof can be used. Alternatively, the carbon material 2 may be disposed inside the pores 11 of the oxide particles 1 using a vapor phase deposition method such as a CVD method.

[0074] Second Embodiment A second embodiment will be described below. Descriptions that overlap with the first embodiment will be omitted as appropriate.

[0075] 5 is a cross-sectional view showing a schematic configuration of an electrode 100 according to the second embodiment. The electrode 100 includes the electrode active material 10 according to the first embodiment and a solid electrolyte 20 in contact with the electrode active material 10. The electrode 100 is manufactured by sintering a compact of a powder material including a powder of the electrode active material 10 and a powder of the solid electrolyte 20. The electrode 100 is used, for example, as a positive electrode or a negative electrode of a solid-state battery. This structure allows the initial discharge capacity of the battery to be improved while maintaining the sinterability of the electrode 100.

[0076] The solid electrolyte 20 may be an electrolyte suitable for forming the electrode 100. Examples of such electrolytes include oxide solid electrolytes. Examples of oxide solid electrolytes include solid electrolytes having a NASICON structure, solid electrolytes having a perovskite structure, solid electrolytes having a LISICON structure, and solid electrolytes having a garnet structure. Among these, a lithium-containing phosphate compound having a NASICON structure is suitable for the electrode 100.

[0077] The NASICON solid electrolyte is a material that can be sintered at a lower temperature than other oxide solid electrolytes, such as solid electrolytes having a perovskite structure or a garnet structure. The ability to sinter at a low temperature means that it is advantageous in suppressing the reaction between the electrode active material 10 and the solid electrolyte 20. Furthermore, if it can be sintered at a low temperature, the transition from anatase titanium oxide to rutile titanium oxide can also be avoided.

[0078] The lithium-containing phosphate compound is Li 1+x Al x Ge 2-x The compound may have a composition of (PO4)3 (0≦x≦2). When a compound having such a composition is used as the solid electrolyte 20 and the electrode active material 10 is used as the electrode active material, the effect of maintaining the sinterability of the electrode 100 is more sufficiently exhibited. In this specification, a compound having the above composition may be referred to as "LAGP."

[0079] Other examples of lithium-containing phosphate compounds include Li 1+x Al x Ti 2-x (PO4)3 (0≦x≦2). In this specification, a compound having the above composition may be referred to as "LATP".

[0080] LAGP is more suitable for the electrode 100 of the present disclosure. Since LAGP does not contain Ti, it has a wider potential window on the negative side (negative side) than LATP. In this case, it is possible to select a negative electrode active material with a lower potential. This is advantageous for providing a high-voltage, high-capacity battery. One example that exhibits this effect is the combination of LAGP and titanium (IV) oxide. Furthermore, LAGP is an electrolyte that can be sintered at a lower temperature than LATP. Being able to sinter at a lower temperature means that it is advantageous for suppressing the reaction between the electrode active material 10 and the solid electrolyte 20.

[0081] In the electrode 100, the solid electrolyte 20 forms a mesh-like sintered phase. For example, in a cross section of the electrode 100, the length of the interface between the particles of the electrode active material 10 and the sintered phase of the solid electrolyte 20, where they are in contact with each other without any gaps, may be on the order of micrometers, and the sintered phase of the solid electrolyte 20 may form a good interface with the particles of the electrode active material 10. The presence of such a contact interface contributes to a reduction in the resistance of the electrode 100.

[0082] The sintered phase of the solid electrolyte 20 may be a phase in which particles of the solid electrolyte 20 are bonded together and grain boundaries are lost. The sintered phase without grain boundaries exhibits excellent ionic conductivity and can form a good contact interface with particles of the electrode active material 10. Such a structure can be formed by using an amorphous solid electrolyte 20 as the raw material for the electrode 100. For example, the structure of the sintered phase can be confirmed by observing the cross section of the electrode 100 at a magnification of 10,000 times using an SEM.

[0083] In the electrode 100, particles of the electrode active material 10 are bonded to one another by the sintered phase of the solid electrolyte 20. The sintered phase of the solid electrolyte 20 includes a crystalline phase and an amorphous phase. If the sintered phase of the solid electrolyte 20 includes a crystalline phase, the electrode 100 preferably exhibits higher ionic conductivity. As described below, the crystalline phase can be formed by appropriately adjusting the firing temperature. For example, if firing is performed at a temperature equal to or higher than the crystallization temperature of the solid electrolyte 20, an electrode 100 including a crystalline solid electrolyte 20 can be obtained. However, the solid electrolyte 20 may also include an amorphous phase. If an amorphous phase is included, the flexibility of the solid electrolyte 20 increases, and volume changes due to expansion and contraction of the electrode active material 10 are more likely to be absorbed by the solid electrolyte 20.

[0084] The crystallinity of the solid electrolyte 20 can be examined by X-ray diffraction measurement or a differential scanning calorimeter (DSC). When X-ray diffraction measurement is used, if only a halo pattern is observed in the X-ray diffraction pattern of the solid electrolyte 20, the solid electrolyte 20 can be determined to be amorphous.

[0085] The electrode 100 may further include a conductive additive. Examples of the conductive additive include carbon materials such as graphite, carbon black, carbon fiber, and carbon nanotubes. The graphite may be natural graphite or artificial graphite. Examples of carbon black include acetylene black and ketjen black. The carbon material may be crystalline or amorphous. The conductive additive typically has a particle shape on the order of nanometers or micrometers. Examples of the particle shape include spherical, oval, scaly, and fibrous.

[0086] The content of the electrode active material 10 in the electrode 100 is, for example, 15% by mass or more and 60% by mass or less. The content of the solid electrolyte 20 in the electrode 100 is, for example, 30% by mass or more and 80% by mass or less. The content of the conductive additive in the electrode 100 may be, for example, 0.1% by mass or more and 10% by mass or less, 0.1% by mass or more and 5% by mass or less, or even 0.3% by mass or more and 2% by mass or less.

[0087] <Method for Manufacturing Electrode> A method for manufacturing the electrode 100 of this embodiment will be described. The electrode 100 can be manufactured by, for example, the following method.

[0088] The electrode 100 can be produced by firing a compact of a mixture of the electrode active material 10 and the solid electrolyte 20 .

[0089] First, raw materials are mixed to prepare a slurry (step S1). The raw materials for the slurry include, for example, the electrode active material 10, the solid electrolyte 20, a conductive additive, a binder, and a solvent. The binder and the solvent may be mixed in advance to prepare a binder solution, and the electrode active material 10, the solid electrolyte 20, and the conductive additive may be mixed into the binder solution to prepare the slurry.

[0090] The oxide particles 1 in the electrode active material 10 have a median diameter of more than 2 μm and less than 7 μm, as measured by a laser diffraction particle size distribution analyzer, for example. With such a structure, the sinterability of the electrode 100 can be improved.

[0091] In this specification, the term "median diameter" refers to the particle diameter when the cumulative volume in the volume-based particle size distribution is 50%. The volume-based particle size distribution is measured by a laser diffraction particle size distribution analyzer at the stage of raw materials such as the electrode active material 10. At the stage of the electrode 100, it is determined from a cross-sectional SEM image. The median diameter measured by the laser diffraction particle size distribution analyzer is usually larger than the median diameter determined from a cross-sectional SEM image.

[0092] The median diameter of the oxide particles 1 in the electrode active material 10 contained in the electrode 100 can be a value calculated from an electron microscope image of the cross section of the electrode 100. Specifically, the cross section of the electrode 100 is observed using an SEM. The magnification is, for example, 3000x. Image analysis software is used to measure the Feret diameters of the oxide particles 1 present in two different observation fields. The "Feret diameter" is the length of the perpendicular line formed by sandwiching a particle between two parallel lines in a fixed direction. The number of particles to be measured is, for example, 185 or more. That is, the width of the observation field is adjusted so that 185 or more particles are included in the two different observation fields. Next, the volume of each particle is calculated assuming that it is a sphere having the measured Feret diameter. The particle size (= Feret diameter, in 0.1 μm increments) is plotted on the horizontal axis, and the volume of the entire group of particles having that particle size is plotted on the vertical axis to create a particle size distribution. The particle size at which the cumulative volume in this particle size distribution is 50% is regarded as the median diameter of the oxide particles 1 in the electrode active material 10 contained in the electrode 100. The median diameter of the primary particles in the electrode active material 10 contained in the electrode 100 can also be determined by the same method.

[0093] The electrode active material 10, the solid electrolyte 20, and the conductive additive may each be a powder material. The median particle size of the solid electrolyte 20 is preferably smaller than the median particle size of the electrode active material 10. When the electrode active material 10 and the solid electrolyte 20 satisfy this relationship, the sinterability of the electrode 100 can be improved. As a result, the resistance of the electrode 100 can be reduced.

[0094] The ratio of the median diameter of the particles of the electrode active material 10 to the median diameter of the particles of the solid electrolyte 20 is, for example, 2 or more and 30 or less. When the electrode active material 10 and the solid electrolyte 20 satisfy this relationship, the sinterability of the electrode 100 can be improved. As a result, the resistance of the electrode 100 can be reduced. The ratio of the median diameter of the particles of the electrode active material 10 to the median diameter of the particles of the solid electrolyte 20 may be 4 or more and 30 or less, or 4 or more and 20 or less.

[0095] The BET specific surface area of ​​the particles of the electrode active material 10 is 1 m 2 / g or more 7m 2 / g or less. When the BET specific surface area of ​​the particles of the electrode active material 10 is appropriately adjusted, side reactions between the particles of the electrode active material 10 and the particles of the solid electrolyte 20 during firing are suppressed. As a result, the electrode 100 can have high ionic conductivity. If a side reaction occurs between the particles of the electrode active material 10 and the particles of the solid electrolyte 20, an interfacial resistance layer will be formed, so such side reactions should be suppressed.

[0096] The particles of the solid electrolyte 20 have a median diameter of, for example, 100 nm or more and 2000 nm or less.

[0097] The particles of the solid electrolyte 20 as a raw material may be amorphous. By pre-firing the amorphous solid electrolyte 20 in a temperature range above the glass transition temperature and below the crystallization temperature, a good interface can be formed with the particles of the electrode active material 10 at a low temperature. This is because the solid electrolyte 20 has good flexibility in a temperature range above the glass transition temperature and below the crystallization temperature. The ionic conductivity of the electrode 100 is improved by subsequently firing the solid electrolyte 20 in an appropriate temperature range above the crystallization temperature and below the melting point to increase the crystallinity of the solid electrolyte 20. Furthermore, the amorphous solid electrolyte 20 can be sintered at a lower temperature than the crystalline solid electrolyte 20. Being able to sinter at a low temperature is advantageous in terms of suppressing the reaction between the electrode active material 10 and the solid electrolyte 20.

[0098] The amorphous nature of the solid electrolyte 20 can be confirmed using a differential scanning calorimetry (DSC). For example, if the degree of crystallinity determined using DSC is 30% or less, the solid electrolyte 20 can be said to be amorphous. The degree of crystallinity is calculated using the following formula. The measured heat of crystallization refers to the amount of heat generated due to the crystallization of the solid electrolyte 20, which is the sample being measured. The heat of crystallization of a completely amorphous material refers to the amount of heat generated due to the crystallization of an amorphous solid electrolyte in which only a halo pattern is observed in the X-ray diffraction pattern.

[0099] Crystallinity (%) = 100 x (Qa-Qs) / Qa Qs: Measured heat of crystallization (J / g) Qa: Completely amorphous crystallization heat (J / g)

[0100] The binder is decomposed and removed by firing. Thermoplastic resins such as polyvinyl butyral, polyvinylidene fluoride, cellulose, acrylic, urethane, and polyvinyl alcohol can be used as the binder. The solvent is typically an organic solvent such as absolute alcohol (e.g., absolute ethanol), toluene, butyl acetate, or NMP. The slurry may also contain a plasticizer. The type of plasticizer is not particularly limited, and phthalate esters such as dioctyl phthalate and diisononyl phthalate can be used.

[0101] The conductive additive may be a carbon material. The carbon material may contain amorphous carbon. The particles of the carbon material have a median diameter of 70 nm or less and a particle size of 60 nm or less. 2 The carbon material may have a BET specific surface area of ​​100 / g or less. By using such a carbon material, the sinterability of the electrode 100 can be improved. The lower limit of the median diameter of the carbon material particles is not particularly limited, and is, for example, 10 nm. The lower limit of the BET specific surface area of ​​the carbon material particles is not particularly limited, and is, for example, 10 m 2 / g.

[0102] Next, the slurry is applied to a substrate to form a coating film (step S2). The substrate can be a resin substrate, a glass substrate, a ceramic substrate, or a metal substrate. After the coating film is formed, the solvent is removed from the coating film. This results in a molded body for an electrode. To remove the solvent from the coating film, the coating film may be heated or air-dried. If necessary, the coating film may be pressed or hot-pressed. The slurry may be molded and dried without using a substrate.

[0103] The slurry may be applied to a substrate to form a coating film, and then the coating film may be pulverized, and the raw material powder obtained by pulverization may be pressed or hot-pressed to produce a green body for an electrode.

[0104] Next, the electrode compact is pre-fired (step S3). Pre-fired is performed, for example, in air or in an inert atmosphere. The inert atmosphere is, for example, a nitrogen gas atmosphere or a rare gas atmosphere. A small amount of oxygen may be mixed into the inert atmosphere. The pre-fired temperature (ambient temperature) is, for example, 250°C to 600°C. The pre-fired firing time is, for example, 1 hour to 60 hours.

[0105] The pre-firing is desirably carried out in a temperature range where the binder is sufficiently removed, the solid electrolyte 20 softens above the glass transition temperature, and crystallization of the solid electrolyte 20 does not proceed. In this way, a good interface is formed between the electrode active material 10 and the solid electrolyte 20 as the binder is removed.

[0106] Next, the electrode compact is subjected to main firing (step S4). The main firing is carried out, for example, in air or in an inert atmosphere. The inert atmosphere is, for example, a nitrogen gas atmosphere or a rare gas atmosphere. A small amount of oxygen may be mixed into the inert atmosphere. The temperature (ambient temperature) of the main firing is, for example, 550°C to 900°C. The firing time of the main firing is, for example, 1 hour to 15 hours.

[0107] During the sintering, particles of the solid electrolyte 20 bond together to form a sintered phase without grain boundaries. The sintering is desirably carried out in a temperature range in which crystallization of the solid electrolyte 20 proceeds appropriately. As the crystallinity of the solid electrolyte 20 improves, the ionic conductivity of the electrode 100 improves.

[0108] The electrode 100 can be manufactured through the above steps.

[0109] Third Embodiment A third embodiment will be described below. Descriptions that overlap with the first and second embodiments will be omitted as appropriate.

[0110] 6 is a cross-sectional view showing a schematic configuration of a battery 1000 according to the third embodiment. The battery 1000 includes a positive electrode 200, a negative electrode 300, and an electrolyte layer 400. The electrolyte layer 400 is disposed between the positive electrode 200 and the negative electrode 300. The electrode 100 according to the second embodiment is used for the positive electrode 200 or the negative electrode 300. By using the electrode 100 for the positive electrode 200 or the negative electrode 300, it is possible to obtain the effect of improving the initial discharge capacity of the battery 100 while maintaining the sinterability of the electrode 100.

[0111] The electrode 100 in the second embodiment is preferably used in the negative electrode 300. That is, the negative electrode 300 may include the electrode 100. In this case, the electrode active material 10 behaves as the negative electrode active material. Since oxides containing titanium are suitable for negative electrode active materials, the electrode 100 is suitable for the negative electrode 300. Therefore, it is easy to obtain the effect of improving the initial discharge capacity of the battery 1000 while maintaining the sinterability of the electrode 100.

[0112] When the electrode 100 is used as the negative electrode 300, the electrode active material 10 does not contain lithium when the battery 1000 is in a state where no charge or discharge has been performed after assembly. In other words, the battery 1000 is in a fully discharged state.

[0113] However, the electrode 100 can also be used as the positive electrode 200. In this case, a material that is less noble than the oxide containing titanium, such as lithium metal, is used as the negative electrode active material.

[0114] The positive electrode 200 includes a positive electrode active material. The positive electrode active material is a material capable of absorbing and releasing metal ions such as lithium ions. Examples of the positive electrode active material include lithium-containing transition metal oxides and lithium-containing transition metal phosphates. Of these, lithium-containing transition metal phosphates are suitable for the positive electrode 200. Examples of lithium-containing transition metal phosphates include lithium iron phosphate, lithium vanadium phosphate, lithium cobalt phosphate, and lithium nickel phosphate. In addition to the positive electrode active material, the positive electrode 200 may also include a solid electrolyte, a conductive additive, and the like.

[0115] The electrolyte layer 400 includes a solid electrolyte. Examples of the solid electrolyte include a sulfide solid electrolyte, a halide solid electrolyte, a complex hydride solid electrolyte, a porous oxide solid electrolyte impregnated with an electrolyte solution, and an oxide solid electrolyte. The composition of the solid electrolyte included in the electrolyte layer 400 may be the same as or different from the composition of the solid electrolyte included in the positive electrode 200. The composition of the solid electrolyte included in the electrolyte layer 400 may be the same as or different from the composition of the solid electrolyte included in the negative electrode 300. The positive electrode 200, the electrolyte layer 400, and the negative electrode 300 may include solid electrolytes with the same composition.

[0116] In the battery 1000, the positive electrode 200, the negative electrode 300, and the electrolyte layer 400 may be composed of a sintered body. In this case, the positive electrode 200, the negative electrode 300, and the electrolyte layer 400 can be integrally formed by co-firing. By integrating the positive electrode 200, the negative electrode 300, and the electrolyte layer 400 by co-firing, the positive electrode 200, the negative electrode 300, and the electrolyte layer 400 can be reliably in contact with each other, thereby improving the conductivity of metal ions such as lithium ions.

[0117] <Method for Manufacturing Battery> A method for manufacturing the battery 1000 of this embodiment will be described. The battery 1000 can be manufactured, for example, by the following method.

[0118] First, slurries are prepared (step ST1). Specifically, a positive electrode slurry, an electrolyte layer slurry, and an anode slurry are prepared. These slurries can be prepared in accordance with the method described in step S1 of the second embodiment. Note that the electrolyte slurry does not contain an electrode active material or a conductive additive.

[0119] Next, green sheets are prepared (step ST2). Specifically, a positive electrode green sheet, an electrolyte layer green sheet, and a negative electrode green sheet are prepared using the positive electrode slurry, the electrolyte layer slurry, and the negative electrode slurry. The green sheets can be prepared by applying the slurry to a substrate to form a coating film, and then drying the coating film. The green sheets are peeled off from the substrate at an appropriate time.

[0120] Next, the green sheets are stacked (step ST3). Specifically, the positive electrode green sheet, the electrolyte layer green sheet, and the negative electrode green sheet are stacked in this order and pressed together to obtain a laminate including the positive electrode green sheet, the electrolyte layer green sheet, and the negative electrode green sheet.

[0121] Next, the pre-firing (step ST4) and the main firing (step ST5) are performed. The pre-firing and the main firing are performed as described in steps S3 and S4 of the second embodiment. Through the above steps, the sintered battery 1000 is obtained.

[0122] (Other Embodiments) (Additional Notes) The above description of the embodiments discloses the following techniques.

[0123] (Technology 1) An electrode active material comprising: oxide particles containing titanium and not containing lithium; and a carbon material, wherein the oxide particles have a plurality of pores with an average pore diameter of 50 nm or more and 200 nm or less, and the carbon material is present inside the pores.

[0124] According to the electrode active material of Technology 1, it is possible to improve the initial discharge capacity of the battery while maintaining the sinterability of the electrode.

[0125] (Technology 2) The electrode active material according to Technology 1, wherein the oxide particles are secondary particles containing a plurality of primary particles. With such a structure, the average pore diameter of the electrode active material is likely to satisfy the above-mentioned numerical range.

[0126] (Technology 3) The electrode active material according to Technology 2, wherein the secondary particles are sintered bodies of the plurality of primary particles. With such a structure, the primary particles are bonded to each other, which can further improve the ionic conductivity inside the particles. As a result, the initial discharge capacity of the battery is further improved.

[0127] (Technology 4) The electrode active material according to Technology 2 or 3, wherein the median diameter of the plurality of primary particles is 50 nm or more and 500 nm or less. With such a structure, the average pore diameter of the electrode active material is more likely to satisfy the above numerical range.

[0128] (Technology 5) The electrode active material according to any one of Technologies 1 to 4, wherein the oxide particles have a median diameter of more than 2 μm and less than 7 μm. Such a structure can improve the sinterability of the electrode. That is, it is possible to form a good contact interface between the electrode active material and the solid electrolyte. This reduces the resistance of the electrode.

[0129] (Technology 6) The electrode active material according to any one of Technologies 1 to 5, wherein the pore volume of the pores per unit mass of the electrode active material is 0.01 mL / g or more and 0.5 mL / g or less. With such a structure, many electron conduction paths are easily formed between the oxide particles and the carbon material, thereby further improving the electron conductivity of the electrode active material. As a result, the initial discharge capacity of the battery is further improved.

[0130] (Technology 7) The electrode active material according to any one of Technologies 1 to 6, wherein the volume occupancy of the carbon material with respect to the pores is 0.5% by volume or more and 80% by volume or less. With such a structure, many electron conduction paths are easily formed between the oxide particles and the carbon material, thereby further improving the electron conductivity of the electrode active material. As a result, the initial discharge capacity of the battery is further improved.

[0131] (Technology 8) The electrode active material according to any one of Technologies 1 to 7, wherein the plurality of pores include pores that communicate with the outside. With such a structure, it is easy to arrange a carbon material inside the pores in the process of producing the electrode active material.

[0132] (Technology 9) 1580 cm in the Raman spectrum of the electrode active material -1 Peak intensity I G 1360 cm -1 Peak intensity I D Ratio I D / I G The electrode active material according to any one of techniques 1 to 8, wherein the ratio I is 0.6 or more and 1.4 or less. D / I G When the value of the carbon material satisfies the above range, the electrical conductivity of the carbon material can be improved while maintaining high flexibility of the carbon material.

[0133] (Technology 10) The electrode active material according to any one of Technologies 1 to 9, wherein the oxide particles contain titanium oxide. Oxide particles having such a structure have the ability to absorb and release metal ions such as lithium ions, and are therefore suitable for, for example, electrodes of solid-state batteries.

[0134] (Technology 11) An electrode comprising: the electrode active material according to any one of Technologies 1 to 10; and a solid electrolyte in contact with the electrode active material.

[0135] According to the electrode of Technology 11, the initial discharge capacity of the battery can be improved while maintaining the sinterability of the electrode.

[0136] (Technology 12) The solid electrolyte is Li 1+x Al x Ge 2-x The electrode according to Technical 11, having a composition of (PO4)3 (0≦x≦2). When a compound having such a composition is used as a solid electrolyte and an electrode active material, the effect of maintaining the sinterability of the electrode is more fully exhibited.

[0137] (Technology 13) A battery comprising: a positive electrode; a negative electrode; and an electrolyte layer disposed between the positive electrode and the negative electrode, wherein the positive electrode or the negative electrode includes the electrode according to Technology 11 or 12.

[0138] According to the battery of Technique 13, the effect of improving the initial discharge capacity of the battery while maintaining the sinterability of the electrodes can be obtained.

[0139] (Technology 14) The battery according to Technology 13, wherein the negative electrode includes the electrode. With such a structure, it is easy to obtain the effect of improving the initial discharge capacity of the battery while maintaining the sinterability of the electrode.

[0140] Hereinafter, the present disclosure will be described in detail using examples and reference examples.

[0141] [Preparation of Electrode Active Material] Example 1 TiO2 (anatase type) particles were prepared as oxide particles. The TiO2 particles were porous secondary particles containing multiple primary particles. The primary particles had a median diameter of 82 nm. The secondary particles had a median diameter of 4.18 μm and a pore size of 5.17 nm. 2 / g, a pore volume of 0.071 mL / g, and an average pore diameter (median diameter) of 82 nm.

[0142] A mixture was obtained by mixing oxide particles and sucrose in a solvent. Ethanol was used as the solvent. The mass of carbon (C) contained in the sucrose was 1.5% relative to the mass of TiO2. Next, the solvent was removed while stirring the mixture in an 80°C environment, and a dried product was obtained. The dried product was then calcined in a nitrogen gas atmosphere at 800°C for 2 hours. In this way, particles of the electrode active material of Example 1 were obtained.

[0143] Example 2 Particles of an electrode active material of Example 2 were obtained in the same manner as in Example 1, except that the mass of carbon (C) contained in sucrose relative to the mass of TiO2 was changed to 3.0%.

[0144] Example 3 Particles of an electrode active material of Example 3 were obtained in the same manner as in Example 1, except that the mass of carbon (C) contained in sucrose relative to the mass of TiO2 was changed to 5.0%.

[0145] Reference Example 1 As particles of an electrode active material in Reference Example 1, the oxide particles of Example 1 were used.

[0146] [Measurement of Average Pore Diameter S] The average pore diameter S (nm) of the pores in the particles of the electrode active material of Examples 1 to 3 was determined by the method described above. Specifically, the pore distribution was measured using a mercury porosimeter (Autopore V 9620, manufactured by Micromeritics) under the following analysis conditions. The average pore diameter S (median diameter) was determined from the obtained pore distribution. The results are shown in Table 1.

[0147] <Analysis conditions> Sample: Approximately 0.2 g (collected in a standard 5 cc powder cell) Measurement range: Equivalent pore diameter D in the range of approximately 0.003 μm to 100 μm Initial pressure P: 3.5 psia (equivalent to a pore diameter of approximately 50 μm) Contact angle θ between mercury and the wall surface of the sample: 130° Surface tension γ of mercury: 485 dynes / cm

[0148] [Measurement of Volume Occupancy Rv of Carbon Material] The volume occupancy Rv (vol %) of the carbon material relative to the pores was determined for the electrode active material particles of Examples 1 to 3 by the method described above. Specifically, the pore distribution was measured under the above analysis conditions using a mercury porosimeter (Micromeritics, Autopore V 9620). The pore volume of TiO2 (0.071 mL / g) was used as the pore volume V1. The pore volume calculated from the pore distribution of the electrode active material particles was used as the pore volume V1. 10 The volume occupancy rate Rv was calculated as 100 × (V1 - V 10 The results are shown in Table 1.

[0149] [Measurement of the mass ratio Rw of the carbon material] The mass ratio Rw (mass %) of the carbon material was determined for the electrode active material particles of Examples 1 to 3 using the method described above. Specifically, a simultaneous differential thermal and thermogravimetric analyzer (TG / DTA STA300, manufactured by Hitachi High-Tech Science Corporation) was used to increase the temperature from room temperature to 900°C at a rate of 10°C / min under an air flow rate of 200 mL / min, thereby obtaining a TG curve for the sample. The weight loss of the sample was determined from the obtained TG curve. The weight loss was used as the mass W2 of the carbon material in the sample. The mass of the sample was then calculated based on the mass W of the electrode active material particles. 10 The ratio Rw was used as 100 × W2 / W 10 The results are shown in Table 1.

[0150] [Comparison I D / I G Measurement of 1580 cm in Raman spectrum for the electrode active materials of Examples 1 to 3 by the above-mentioned method. -1 Peak intensity I G 1360 cm -1 Peak intensity I D Ratio I D / I G Specifically, a Raman spectrum of the sample was obtained using a microscopic laser Raman spectrometer (NRS-5100, manufactured by JASCO Corporation) under the following analytical conditions. FIG. 7 shows the Raman spectrum of the electrode active material of Example 3. For example, the peak intensity I obtained from the Raman spectrum of FIG. G is 15.358, and the peak intensity ID The peak intensity I was 15.064. G and peak intensity I D Based on the ratio I D / I G The results are shown in Table 1.

[0151] <Analysis conditions> Measurement method: Microscopic measurement (×100) Laser wavelength: 532 nm, output 1.3 mW Slit: 100 μm × 1000 μm Aperture: diameter 4000 μm Exposure: 1 second × 3 times (100 points conversion) Measurement wavelength range: 950 cm -1 From 1900 cm -1

[0152] [Measurement of the carbon content (Ratm) present on the outer surface] Using the method described above, the carbon content (Ratm) (atomic %) present on the outer surface of the oxide particles was determined for the electrode active material particles of Examples 1 to 3 and Reference Example 1. Specifically, an XPS apparatus (PHI Quantera SXM, manufactured by ULVAC-PHI) was used to fill a powder cell with a sample and perform XPS analysis under the following analytical conditions to obtain XPS spectra of carbon, oxygen, titanium, and potassium. The peak area intensity in each XPS spectrum was used to calculate the proportion (atomic %) of each element. The calculated carbon proportion (atomic %) was considered to be the content (Ratm) (atomic %). The results are shown in Table 1.

[0153] <Analysis conditions> X-ray source: Monochromatic Al-Kα (1486.6 eV), 15 kV / 25 W Analysis area: 300 nm x 800 nm (scanning microfocus, 100 mmf) Photoelectron take-off angle: 45° <Neutralization conditions> Electron + floating ion neutralization <Measurement conditions> Step (eV): 1.0 (wide), 0.05 (narrow) Pass energy (eV): 280.0 (wide), 55.0 (narrow) Measurement time (ms): 60 (narrow)

[0154] [Measurement of Median Diameter] A laser diffraction particle size distribution analyzer (Malvern Panalytical, Mastersizer 3000) was used to measure the median diameter of the particles of the electrode active materials of Examples 1 to 3. The results are shown in Table 1.

[0155] [Measurement of BET Specific Surface Area] The BET specific surface area of ​​the electrode active materials of Examples 1 to 3 was measured using the method described above. Specifically, a nitrogen gas adsorption test was performed on the samples. Using analytical software (ASiQWin), analysis was performed by the BET method in the linear region of the adsorption isotherm, and the BET specific surface area was calculated. The results are shown in Table 1.

[0156]

[0157] [Preparation of Negative Electrode Pellets] Example 1 Using the electrode active material of Example 1 as the negative electrode active material, negative electrode pellets of Example 1 were prepared by the following method.

[0158] (Preparation of Binder Solution) A predetermined amount of acrylic resin powder was placed in a 150 cc container as a binder. Ethanol was added to the container so that the mass ratio of acrylic resin to ethanol was 15:140, and the mixture was stirred until the acrylic resin powder was completely dissolved. The stirring was carried out using a planetary centrifugal mixer (Thinky Corporation, Mixertaro) at 2000 rpm for 2 hours. In this way, the binder solution of Example 1 was obtained.

[0159] (Preparation of Negative Electrode Slurry) LAGP was used as the solid electrolyte. A carbon-based conductive additive was used as the conductive additive. An electrode active material, solid electrolyte, and conductive additive were prepared in a mass ratio of electrode active material:solid electrolyte:carbon-based conductive additive of 20:75:5. The electrode active material powder, solid electrolyte powder, and conductive additive powder were placed in a 58 mL container and stirred. Stirring was performed 100 times by hand. In this manner, the negative electrode mixture of Example 1 was obtained. Then, a binder solution was added to the container so that the mass ratio of negative electrode mixture:acrylic resin was 100:3.75. Furthermore, ethanol was added to the container so that the mass ratio of negative electrode mixture:ethanol was 100:116.25 and stirred. Stirring was performed using a planetary centrifugal mixer (Thinky Corporation, Mixertaro) at 2000 rpm for 30 minutes. In this manner, the negative electrode slurry of Example 1 was obtained.

[0160] (Molded body for negative electrode pellets) The negative electrode slurry was dried on a hot plate set at 80°C. After confirming that ethanol had been sufficiently removed from the negative electrode slurry, the dried film was coarsely pulverized and subjected to vacuum drying at 80°C for 2 hours. The coarsely pulverized product after vacuum drying was placed in a mortar and manually pulverized for 15 minutes to obtain a raw material powder for negative electrode pellets. Next, 122 mg of the raw material powder for negative electrode pellets was molded by uniaxial pressing using a press molding machine with a diameter of 10.5 mm. In this way, the molded body for negative electrode pellets of Example 1 was obtained. The pressing conditions were 276 MPa and 1 minute.

[0161] The negative electrode pellet compact was pre-fired using an electric furnace to remove the binder. The pre-fired conditions were 350°C (ambient temperature), in air, for 48 hours, with no gas flow, and a heating rate of 100°C / hour. Finally, the negative electrode pellet compact was subjected to main firing using an electric furnace. The main firing conditions were 650°C (ambient temperature), in a nitrogen atmosphere, for 2 hours, with a gas flow of 1 L / min, and a heating rate of 100°C / hour. In this way, the negative electrode pellet of Example 1 was obtained. The dimensions of the negative electrode pellet of Example 1 were a diameter of 9.51 mm and a thickness of 0.63 mm. The mass was 113.9 mg.

[0162] Example 2 A negative electrode pellet of Example 2 was produced in the same manner as in Example 1, except that the electrode active material of Example 2 was used as the negative electrode active material. The dimensions of the negative electrode pellet of Example 2 were a diameter of 9.50 mm, a thickness of 0.63 mm, and a mass of 113.2 mg.

[0163] Example 3 A negative electrode pellet of Example 3 was produced in the same manner as in Example 1, except that the electrode active material of Example 3 was used as the negative electrode active material. The dimensions of the negative electrode pellet of Example 3 were a diameter of 9.48 mm, a thickness of 0.63 mm, and a mass of 113.6 mg.

[0164] Reference Example 1 A negative electrode pellet of Reference Example 1 was produced in the same manner as in Example 1, except that the electrode active material of Reference Example 1 was used as the negative electrode active material. The dimensions of the negative electrode pellet of Reference Example 1 were a diameter of 9.51 mm, a thickness of 0.63 mm, and a mass of 113.8 mg.

[0165] Example 4 The electrode active material of Example 1 was used as the negative electrode active material. When preparing the negative electrode slurry, the electrode active material and the solid electrolyte were prepared so that the mass ratio of the electrode active material, solid electrolyte, and carbon-based conductive additive was 35:64:1. Except for these, a negative electrode pellet of Example 4 was produced in the same manner as in Example 1. The dimensions of the negative electrode pellet of Example 4 were a diameter of 9.52 mm and a thickness of 0.63 mm. The mass was 113.8 mg.

[0166] Example 5 A negative electrode pellet of Example 5 was produced in the same manner as in Example 4, except that the electrode active material of Example 2 was used as the negative electrode active material. The dimensions of the negative electrode pellet of Example 5 were a diameter of 9.57 mm, a thickness of 0.62 mm, and a mass of 113.9 mg.

[0167] Example 6 A negative electrode pellet of Example 6 was produced in the same manner as in Example 4, except that the electrode active material of Example 3 was used as the negative electrode active material. The dimensions of the negative electrode pellet of Example 6 were a diameter of 9.55 mm, a thickness of 0.61 mm, and a mass of 113.7 mg.

[0168] Reference Example 2 A negative electrode pellet of Reference Example 2 was produced in the same manner as in Example 4, except that the electrode active material of Reference Example 1 was used as the negative electrode active material. The dimensions of the negative electrode pellet of Reference Example 2 were a diameter of 9.65 mm, a thickness of 0.63 mm, and a mass of 114.9 mg.

[0169] Reference Example 3 The electrode active material of Reference Example 1 was used as the negative electrode active material. When preparing the negative electrode slurry, the electrode active material, solid electrolyte, and conductive additive were prepared in a mass ratio of electrode active material: solid electrolyte: carbon-based conductive additive of 35:62:3. Except for these, a negative electrode pellet of Reference Example 3 was produced in the same manner as in Example 1. The dimensions of the negative electrode pellet of Reference Example 3 were a diameter of 9.82 mm and a thickness of 0.65 mm. The mass was 113.8 mg.

[0170] Reference Example 4 The electrode active material of Reference Example 1 was used as the negative electrode active material. When preparing the negative electrode slurry, the electrode active material, solid electrolyte, and conductive additive were prepared in a mass ratio of electrode active material: solid electrolyte: carbon-based conductive additive of 35:60:5. Except for these, a negative electrode pellet of Reference Example 4 was produced in the same manner as in Example 1. The dimensions of the negative electrode pellet of Reference Example 4 were a diameter of 10.09 mm and a thickness of 0.68 mm. The mass was 113.5 mg.

[0171] [Measurement of Density of Negative Electrode Pellets] The density of the negative electrode pellets was calculated from the dimensions and mass of the negative electrode pellets of Examples 1 to 6 and Reference Examples 1 to 4. The results are shown in Table 2.

[0172] [Measurement of Porosity of Negative Electrode Pellets] The porosity of the negative electrode pellets of Examples 1 to 6 and Reference Examples 1 to 4 was determined using the following method. First, the true density of each material used to prepare the negative electrode pellets of Examples 1 to 6 and Reference Examples 1 to 4 was measured in advance. The porosity of the negative electrode pellet was calculated using the dimensions of the negative electrode pellet, the measured true density, and the content of each material. The negative electrode pellet was considered to contain only the electrode active material, solid electrolyte, and carbon-based conductive additive. The true density was measured by the He substitution method using a pycnometer (Ultrapyc 5000, manufactured by Anton Paar). Regarding LAGP (solid electrolyte), an amorphous material is used as the starting material, but it is difficult to evaluate the density after sintering. Therefore, the theoretical density was used as the true density of LAGP. The results are shown in Table 2.

[0173]

[0174] <<Discussion>> The negative electrode pellets of Examples 1 to 3 and Reference Example 1 differed in the mass ratio Rw of the carbon material in the negative electrode active material. Despite the increase in the carbon content in the electrode as the mass ratio Rw of the carbon material in the negative electrode active material increases, the negative electrode pellets of Examples 1 to 3 and Reference Example 1 exhibited substantially the same density and porosity. This is thought to be because the negative electrode pellets of Examples 1 to 3 maintained the sinterability of the negative electrode due to the formation of a favorable contact interface between the negative electrode active material and the solid electrolyte. The negative electrode pellets of Examples 4 to 6 and Reference Example 2 differed in the mass ratio Rw of the carbon material in the negative electrode active material. Despite the increase in the carbon content in the electrode as the mass ratio Rw of the carbon material in the negative electrode active material increases, the negative electrode pellets of Examples 4 to 6 and Reference Example 2 exhibited substantially the same density and porosity. This is thought to be because the sinterability of the negative electrode was maintained due to the formation of a good contact interface between the negative electrode active material and the solid electrolyte in the negative electrode pellets of Examples 4 to 6. These results show that the carbon material placed in the pores has almost no effect on the sinterability of the negative electrode. Furthermore, a comparison of Reference Examples 2 to 4 shows that reducing the amount of LAGP and increasing the amount of carbon-based conductive additive results in a deterioration in sinterability.

[0175] [Preparation of Bilayer Pellets] <<Examples 1 to 6, Reference Examples 1 to 4>> Bilayer pellets of Examples 1 to 6 and Reference Examples 1 to 4 were prepared by the following method using the raw material powders for negative electrode pellets of Examples 1 to 6 and Reference Examples 1 to 4. The bilayer pellets were composed of a negative electrode pellet and a solid electrolyte pellet.

[0176] (Preparation of Solid Electrolyte Slurry) LAGP was used as the solid electrolyte. Solid electrolyte powder was placed in a 6 mL container. A binder solution was added to the container so that the mass ratio of solid electrolyte powder to acrylic resin was 100:3.75. Furthermore, ethanol was added to the container so that the mass ratio of solid electrolyte powder to ethanol was 100:116.25, and the mixture was stirred. The stirring was performed using a planetary centrifugal mixer (Thinky Corporation, Mixertaro) at 2000 rpm for 30 minutes. In this manner, a solid electrolyte slurry was obtained.

[0177] (Molded body for two-layer pellets) The solid electrolyte slurry was dried on a hot plate set at 80° C. After confirming that ethanol had been sufficiently removed from the solid electrolyte slurry, the dried film was coarsely pulverized and subjected to vacuum drying treatment at 80° C. for 2 hours. The coarsely pulverized product after vacuum drying was placed in a mortar and manually pulverized for 15 minutes to obtain a raw material powder for solid electrolyte pellets.

[0178] Next, 15 mg of the raw material powder for the negative electrode pellets was filled into a tablet press with a diameter of 8 mm and pressed by hand for 1 second. Next, 50 mg of the raw material powder for the solid electrolyte pellets was filled and pressed by uniaxial pressing. In this way, a two-layer molded body for the negative electrode pellets and a molded body for the solid electrolyte pellets was obtained. The pressing conditions were 276 MPa and 1 minute.

[0179] The two-layer pellet molded body was pre-fired using an electric furnace to remove the binder. The pre-fired conditions were 350°C (ambient temperature), in air, for 48 hours, with no gas flow, and a heating rate of 100°C / hour. Finally, the two-layer pellet molded body was sintered using an electric furnace. The firing conditions were 650°C (ambient temperature), in a nitrogen atmosphere, for 2 hours, with a gas flow of 1 L / min, and a heating rate of 100°C / hour. In this manner, two-layer pellets of Examples 1 to 6 and Reference Examples 1 and 2 were obtained. Note that, in Reference Examples 3 and 4, as the amount of carbon-based conductive additive added increased, the sinterability of the negative electrode pellet, specifically the shrinkage rate, deteriorated, and the two-layer pellet warped due to the difference in shrinkage rate with the solid electrolyte pellet. Therefore, it was not possible to produce a two-layer pellet capable of charging and discharging.

[0180] [Evaluation of charge-discharge characteristics of negative electrode half-cell] A charge-discharge test of the negative electrode half-cell was carried out by the following method using the bilayer pellets of Examples 1 to 6 and Reference Examples 1 and 2. In the negative electrode half-cell, the side where Li is inserted corresponds to discharging (charging in a battery) and the side where Li is desorbed corresponds to charging (discharging in a battery). Therefore, the initial charge capacity C of the negative electrode half-cell was 11 corresponds to the initial discharge capacity of the battery, and the initial discharge capacity C of the negative electrode half cell 10 corresponds to the initial charge capacity of the battery.

[0181] First, a 290 nm thick Au thin film was formed on the negative electrode pellet side of the bilayer pellet by sputtering, and then the pellet was placed in a vacuum dryer and dried at 80°C for 1 hour. Next, a 300 μm thick Li metal foil was placed on the solid electrolyte pellet side of the bilayer pellet. The solid polymer electrolyte membrane was stacked so that the Au thin film, bilayer pellet, solid polymer electrolyte membrane, and Li metal foil were arranged in this order to obtain a laminate. A LiTFSI-PEO membrane was used as the solid polymer electrolyte membrane. The PEO:LiTFSI molar ratio in the LiTFSI-PEO membrane was 18:1. The laminate was placed in a sealed bipolar cell (HS Flat Cell, manufactured by Hosen Co., Ltd.) to obtain a negative electrode half cell. To avoid pellet cracking, the spring constant of the laminate in the stacking direction was selected to be 200 gf / mm.

[0182] Next, a charge / discharge test of the negative electrode half cell was performed in a constant current constant voltage (CCCV) mode at 60°C, and a charge / discharge curve for the first cycle was obtained. The negative electrode half cell was discharged at a constant current of 0.01C until the voltage reached 1.5V, and then discharged at a constant voltage of 1.5V for 5 hours. The negative electrode half cell was charged at a constant current of 0.01C until the voltage reached 3V, and then charged at a constant voltage of 3V for 5 hours. An electrochemical evaluation device (VSP-300, manufactured by Biologic) was used for charge / discharge. Figure 8 shows the charge / discharge curves for the first cycle of the negative electrode half cells of Examples 1 to 3 and Reference Example 1 superimposed. The charge capacity of the negative electrode half cell obtained from the charge / discharge curve for the first cycle was expressed as the initial charge capacity C 11 and the discharge capacity is called the initial discharge capacity C 10 The results are shown in Table 3.

[0183]

[0184] <<Discussion>> The negative electrode half-cells of Examples 1 to 3 and the negative electrode half-cell of Reference Example 1 had the same mass ratio of the carbon-based conductive additive used in the negative electrode pellets. However, the negative electrode half-cells of Examples 1 to 3 had a lower initial charge capacity C than the negative electrode half-cell of Reference Example 1. 11 The negative electrode half-cells of Examples 4 to 6 and the negative electrode half-cell of Reference Example 2 had the same mass ratio of the carbon-based conductive additive used in the negative electrode pellets. However, the negative electrode half-cells of Examples 4 to 6 had a higher initial charge capacity C than the negative electrode half-cell of Reference Example 2. 11 This is thought to be because the presence of the carbon material inside the pores of the negative electrode active material formed many electron conduction paths between the oxide particles and the carbon material, improving the electron conductivity of the electrode active material.

[0185] [Preparation of bilayer pellets] Reference Example 5 The electrode active material of Reference Example 1 was used as the negative electrode active material. When preparing the negative electrode slurry, the electrode active material, solid electrolyte, and conductive additive were prepared so that the mass ratio of electrode active material:solid electrolyte:carbon-based conductive additive was 20:75:5. Except for these, the bilayer pellet of Reference Example 5 was prepared by the same method as Reference Example 1.

[0186] Next, charge / discharge tests of negative electrode half cells were carried out using the bilayer pellets of Examples 4 to 6 and Reference Examples 2 and 5 in the same manner as described above. Figures 9 to 13 show the charge / discharge curves for the first cycle of the negative electrode half cells of Examples 4 to 6 and Reference Examples 2 and 5. The dashed lines in Figures 9 to 13 indicate the standard initial charge capacity of a liquid battery using an electrolyte solution. The shoulder capacity during discharge of the negative electrode half cell obtained from the charge / discharge curve for the first cycle was defined as the shoulder capacity during initial discharge, C S It is called 100 x C 11 / C 10 The value calculated by is called the initial charge-discharge efficiency. The results are shown in Table 4. Shoulder capacity C SIt is known that this occurs when LAGP (solid electrolyte) and TiO2 (oxide particles) react during firing, causing Ti elements to diffuse into the LAGP side and forming a LAGTP layer at the interface. It is also known that when Ti elements are incorporated into LAGP, the negative potential window shifts to a potential region higher than the driving potential of TiO2, causing reductive decomposition of the electrolyte layer and resulting in a decrease in efficiency. That is, the shoulder capacitance C S The occurrence of this phenomenon indicates that a LAGTP layer is formed at the interface between the LAGP and TiO2 layers, and the shoulder capacitance C S The larger the shoulder capacitance C, the greater the amount of LAGTP layer formed. S It is desirable to reduce the initial charge-discharge efficiency. Previous studies have shown that the presence of a carbon material promotes the reaction between LAGP and TiO2. However, as confirmed in Reference Example 5, for example, increasing the amount of carbon-based conductive additive reduces the shoulder capacity C S It can be confirmed that the use of an electrode active material having a structure in which a carbon material is arranged inside the pores results in an increase in the shoulder capacity C S It was found that the increase in

[0187]

[0188] <<Discussion>> From a comparison of the initial charge-discharge efficiencies of Examples 4 to 6 with those of Reference Examples 2 and 5, it was found that when a carbon material is disposed inside the pores of the negative electrode active material, the interface at which the LAGP (solid electrolyte) and the carbon-based conductive additive come into contact can be reduced, compared to when a carbon material is added as a conductive additive, and therefore a decrease in the initial charge-discharge efficiency is suppressed.

[0189] [Evaluation of cycle characteristics of negative electrode half-cell] Using the bilayer pellets of Examples 1 and 2, a charge-discharge test of the negative electrode half-cell was further carried out up to the 10th cycle in the same manner as described above. From the charge-discharge curve of the 10th cycle, the charge capacity C A 100×CA / C 11 The value calculated by the formula (2) is referred to as the capacity retention rate at the 10th cycle. The value calculated as the average value of the charge-discharge efficiencies {(discharge capacity / charge capacity) × 100} for each cycle from the 5th to the 10th cycle is referred to as the charge-discharge efficiency (%) for the 5th to the 10th cycle. The results are shown in Table 5. FIG. 14 shows the relationship between the cycle number and charge capacity for the negative electrode half-cells of Examples 1 and 2. Note that in the negative electrode half-cells, the side from which Li is desorbed corresponds to charging (discharging in the battery). FIG. 15 shows the relationship between the cycle number and capacity retention rate for the negative electrode half-cells of Examples 1 and 2.

[0190]

[0191] <<Discussion>> There was a difference in the volume fraction Rv of the carbon material relative to the pores in the negative electrode active material used in the negative electrode pellet between the negative electrode half-cell of Example 1 and the negative electrode half-cell of Example 2. From the results shown in Table 5 and Figures 14 and 15, it was found that when the volume fraction Rv was 30 volume % or less, the cycle characteristics tended to improve.

[0192] The solid electrolyte of the present disclosure can be used, for example, in automotive lithium-ion secondary batteries.

Claims

1. An electrode active material comprising: oxide particles containing titanium and no lithium; and a carbon material; wherein the oxide particles have a plurality of pores having an average pore diameter of 50 nm or more and 200 nm or less; and the carbon material is present inside the pores.

2. The electrode active material according to claim 1, wherein the oxide particles are secondary particles comprising a plurality of primary particles.

3. The electrode active material according to claim 2, wherein the secondary particles are sintered bodies of the plurality of primary particles.

4. The electrode active material according to claim 2, wherein the median diameter of the plurality of primary particles is 50 nm or more and 500 nm or less.

5. The electrode active material according to claim 1, wherein the median diameter of the oxide particles is greater than 2 μm and less than 7 μm.

6. The electrode active material according to claim 1, wherein the pore volume of the pores per unit mass of the electrode active material is 0.01 mL / g or more and 0.5 mL / g or less.

7. The electrode active material according to claim 1, wherein a volume occupancy rate of said carbon material in said pores is 0.5 volume % or more and 80 volume % or less.

8. The electrode active material according to claim 1, wherein the plurality of pores include interconnected pores.

9. 1580 cm in the Raman spectrum of the electrode active material -1 Peak intensity I G 1360 cm -1 Peak intensity I D Ratio I D / I G The electrode active material according to claim 1 , wherein the σ is 0.6 or more and 1.4 or less.

10. The electrode active material according to claim 1, wherein the oxide particles include titanium oxide.

11. An electrode comprising: an electrode active material according to any one of claims 1 to 10; and a solid electrolyte in contact with the electrode active material.

12. The solid electrolyte is Li 1+x A x Ge 2-x 12. The electrode of claim 11 having a composition of (PO4)3, where 0≦x≦2.

13. A battery comprising: a positive electrode; a negative electrode; and an electrolyte layer disposed between said positive electrode and said negative electrode, wherein said positive electrode or said negative electrode comprises the electrode according to claim 11.

14. The battery of claim 13, wherein said negative electrode comprises said electrode.

Citation Information

Patent Citations

  • Electrode active material and lithium battery using the same

    JP5400607B2

  • Method for manufacturing negative electrode active material for nonaqueous electrolyte secondary battery, and negative electrode active material for nonaqueous electrolyte secondary battery

    JP2017152114A

  • Negative electrode active material composite for lithium ion secondary battery and method of manufacturing the same

    JP2018160432A