Positive electrode for nonaqueous electrolyte secondary battery, and nonaqueous electrolyte secondary battery

The positive electrode for non-aqueous electrolyte secondary batteries, featuring a lithium-containing transition metal composite oxide with a sulfonic acid compound and a conductive additive mixture, enhances both output and cycle characteristics by reducing reaction resistance and forming a conductive path, addressing the conductivity challenges in existing technologies.

WO2024247677A1PCT designated stage expired Publication Date: 2024-12-05PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD

Patent Information

Application Number
PCT/JP2024/017560
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-29
Filing Date
2024-05-13
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Existing non-aqueous electrolyte secondary batteries face challenges in improving cycle characteristics during high-rate charging while maintaining output characteristics, as the presence of sulfonic acid compounds on the surface of lithium-containing transition metal composite oxides reduces electronic conductivity, leading to increased mixture resistance and potential deterioration of cycle characteristics.

Method used

A positive electrode comprising a lithium-containing transition metal composite oxide with a layered structure, coated with a sulfonic acid compound and a conductive additive mixture of carbon nanotubes and carbon black with average diameters of 20 nm or less, and optionally graphene, to reduce reaction resistance and enhance conductivity.

Benefits of technology

The solution effectively improves output characteristics and cycle retention during high-rate charging by forming a sufficient conductive path in the positive electrode mixture layer, addressing the conductivity and resistance issues associated with sulfonic acid compounds.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024017560_05122024_PF_FP_ABST
    Figure JP2024017560_05122024_PF_FP_ABST
Patent Text Reader

Abstract

A positive electrode (11) for a nonaqueous electrolyte secondary battery according to one embodiment of the present disclosure is characterized by comprising, as a positive electrode mixture layer, a positive electrode active material and an electroconductive auxiliary agent, and is characterized in that: the positive electrode active material includes a lithium-containing transition metal composite oxide having a layered structure, and a sulfonic acid compound which is present on the surfaces of the particles of lithium-containing transition metal composite oxide; the sulfonic acid compound is represented by formula (I); and the electroconductive auxiliary agent includes at least one selected from the group consisting of carbon nanotubes having an average diameter of 20 nm or less, carbon black, and graphene having an average thickness of 50 nm or less. (In the formula, A represents a Group 1 element or a Group 2 element, R represents a hydrocarbon group, and n is 1 or 2.)
Need to check novelty before this filing date? Find Prior Art

Description

Positive electrode for non-aqueous electrolyte secondary battery and non-aqueous electrolyte secondary battery

[0001] The present disclosure relates to a positive electrode for a non-aqueous electrolyte secondary battery and a non-aqueous electrolyte secondary battery using the positive electrode.

[0002] In recent years, the applications of non-aqueous electrolyte secondary batteries have expanded to include power sources for electric vehicles and power storage devices for utilizing natural energy. Since the positive electrode significantly affects battery characteristics, including battery capacity, output characteristics, and cycle characteristics, much research has been conducted on the positive electrode. For example, Patent Document 1 discloses a positive electrode for a non-aqueous electrolyte secondary battery that uses, as a positive electrode active material, a lithium-containing transition metal composite oxide having a low-solubility Li salt scattered on its surface, with the aim of reducing reaction resistance during storage at high temperatures.

[0003] Japanese Patent Application Laid-Open No. 2019-169286

[0004] In non-aqueous electrolyte secondary batteries, it is important to improve the cycle characteristics during high-rate charging while improving the output characteristics. The technology described in Patent Document 1 cannot fully address these issues, and there is still much room for improvement.

[0005] A positive electrode for a non-aqueous electrolyte secondary battery according to one embodiment of the present disclosure is a positive electrode for a non-aqueous electrolyte secondary battery having a positive electrode core and a positive electrode mixture layer formed on the surface of the positive electrode core, the positive electrode mixture layer including a positive electrode active material and a conductive additive, the positive electrode active material including a lithium-containing transition metal composite oxide having a layered structure and a sulfonic acid compound present on particle surfaces of the lithium-containing transition metal composite oxide, the sulfonic acid compound being a compound represented by formula (I), and the conductive additive including at least one selected from the group consisting of carbon nanotubes and carbon black having an average diameter of 20 nm or less, and graphene having an average thickness of 50 nm or less. (In the formula, A is a Group 1 or Group 2 element, R is a hydrocarbon group, and n is 1 or 2.)

[0006] A non-aqueous electrolyte secondary battery according to one embodiment of the present disclosure includes the positive electrode, a negative electrode, and a non-aqueous electrolyte.

[0007] According to a positive electrode for a nonaqueous electrolyte secondary battery according to one aspect of the present disclosure, it is possible to provide a nonaqueous electrolyte secondary battery having improved output characteristics and improved cycle characteristics during high-rate charging.

[0008] 1 is a diagram schematically illustrating an axial cross section of a nonaqueous electrolyte secondary battery (cylindrical battery) according to an embodiment.

[0009] As described above, improving the output characteristics of non-aqueous electrolyte secondary batteries is an important issue. As a result of studies by the present inventors, it has become clear that a non-aqueous electrolyte secondary battery with improved output characteristics can be realized by adding a sulfonic acid compound represented by the above formula (I) to the particle surface of a lithium-containing transition metal composite oxide used as a positive electrode active material. This is presumably because the function of the sulfonic acid compound makes it easier for Li to be inserted and removed, thereby reducing the reaction resistance in the positive electrode.

[0010] However, the presence of sulfonic acid compounds on the particle surface reduces the electronic conductivity of lithium-containing transition metal composite oxides, and the formation of conductive paths is insufficient with widely used conductive additives such as carbon black. As a result, the positive electrode mix resistance increases, and cycle characteristics during high-rate charging may deteriorate. Therefore, the inventors conducted extensive research to solve this problem and found that by combining a conductive additive with a special microstructure, it is possible to reduce the reaction resistance of the positive electrode while improving cycle characteristics during high-rate charging.

[0011] Hereinafter, with reference to the drawings, an example of an embodiment of a positive electrode for a nonaqueous electrolyte secondary battery according to the present disclosure and a nonaqueous electrolyte secondary battery using the positive electrode will be described in detail. Note that the scope of the present disclosure includes configurations obtained by selectively combining the respective components of the multiple embodiments and modifications described below.

[0012] In the following, a cylindrical battery in which a wound electrode assembly 14 is housed in a cylindrical, bottomed exterior body 16 is exemplified as a nonaqueous electrolyte secondary battery; however, the exterior body of the battery is not limited to a cylindrical exterior body. The nonaqueous electrolyte secondary battery according to the present disclosure may be, for example, a prismatic battery with a prismatic exterior body, a coin-type battery with a coin-type exterior body, or a pouch-type battery with an exterior body composed of a laminate sheet including a metal layer and a resin layer. Furthermore, the electrode assembly is not limited to a wound type, but may also be a stacked type electrode assembly in which multiple positive electrodes and multiple negative electrodes are alternately stacked with separators interposed therebetween. Furthermore, the design of the nonaqueous electrolyte secondary battery according to the present disclosure is not limited to the design of the exemplified nonaqueous electrolyte secondary battery, and known nonaqueous electrolyte secondary battery designs may also be applied.

[0013] FIG. 1 is an axial cross-sectional view of a cylindrical nonaqueous electrolyte secondary battery 10 according to an embodiment. As shown in FIG. 1 , the nonaqueous electrolyte secondary battery 10 includes a wound electrode assembly 14, a nonaqueous electrolyte, and an exterior body 16 that accommodates the electrode assembly 14 and the nonaqueous electrolyte. The electrode assembly 14 includes a positive electrode 11, a negative electrode 12, and a separator 13, and has a wound structure in which the positive electrode 11 and the negative electrode 12 are spirally wound with the separator 13 interposed therebetween. The exterior body 16 is a cylindrical metal container with a bottom that is open on one axial side, and the opening of the exterior body 16 is closed by a sealing body 17. Hereinafter, for convenience of explanation, the sealing body 17 side of the battery will be referred to as the top, and the bottom side of the exterior body 16 will be referred to as the bottom.

[0014] The positive electrode 11, negative electrode 12, and separator 13 that make up the electrode assembly 14 are all rectangular, elongated bodies that are spirally wound in the longitudinal direction and stacked alternately in the radial direction of the electrode assembly 14. The separator 13 isolates the positive electrode 11 and the negative electrode 12 from each other. Two separators 13 are arranged, for example, to sandwich the positive electrode 11. The electrode assembly 14 includes a positive electrode lead 20 connected to the positive electrode 11 by welding or the like, and a negative electrode lead 21 connected to the negative electrode 12 by welding or the like. In the electrode assembly 14, the longitudinal direction of the positive electrode 11 and the negative electrode 12 is the winding direction, and the lateral direction of the positive electrode 11 and the negative electrode 12 is the axial direction. That is, the lateral end faces of the positive electrode 11 and the negative electrode 12 form the axial end faces of the electrode assembly 14.

[0015] Insulating plates 18 and 19 are disposed above and below the electrode body 14. In the example shown in Fig. 1 , the positive electrode lead 20 passes through a through hole in the insulating plate 18 and extends toward the sealing body 17, and the negative electrode lead 21 passes outside the insulating plate 19 and extends toward the bottom side of the exterior body 16. The positive electrode lead 20 is connected to the underside of an internal terminal plate 23 of the sealing body 17 by welding or the like, and a cap 27, which is the top plate of the sealing body 17 and is electrically connected to the internal terminal plate 23, serves as the positive electrode terminal. The negative electrode lead 21 is connected to the inner bottom surface of the exterior body 16 by welding or the like, and the exterior body 16 serves as the negative electrode terminal.

[0016] A gasket 28 is provided between the exterior body 16 and the sealing body 17 to ensure airtightness inside the battery. The exterior body 16 has a grooved portion 22 formed on its side surface that protrudes inward and supports the sealing body 17. The grooved portion 22 is preferably formed in an annular shape along the circumferential direction of the exterior body 16, and supports the sealing body 17 on its top surface. The sealing body 17 is fixed to the top of the exterior body 16 by the grooved portion 22 and the open end of the exterior body 16 that is crimped to the sealing body 17.

[0017] The sealing body 17 has a structure in which, in order from the electrode body 14 side, an internal terminal plate 23, a lower valve body 24, an insulating member 25, an upper valve body 26, and a cap 27 are stacked. Each member constituting the sealing body 17 has, for example, a disk or ring shape, and each member except for the insulating member 25 is electrically connected to one another. The lower valve body 24 and the upper valve body 26 are connected at their respective centers, and the insulating member 25 is interposed between their respective peripheral edges. When the internal pressure of the battery increases due to abnormal heat generation, the lower valve body 24 deforms and breaks, pushing the upper valve body 26 toward the cap 27, thereby interrupting the current path between the lower valve body 24 and the upper valve body 26. When the internal pressure further increases, the upper valve body 26 breaks, and gas is discharged from the opening of the cap 27.

[0018] The positive electrode 11, the negative electrode 12, the separator 13, and the nonaqueous electrolyte that constitute the nonaqueous electrolyte secondary battery 10 will be described in detail below, with the positive electrode 11 being particularly described below.

[0019] [Positive Electrode] The positive electrode 11 has a positive electrode core 30 and a positive electrode mixture layer 31 formed on the surface of the positive electrode core 30. The positive electrode mixture layer 31 is preferably formed on both sides of the positive electrode core 30. For the positive electrode core 30, a foil of a metal such as aluminum or an aluminum alloy that is stable within the potential range of the positive electrode 11, or a film with such a metal disposed on the surface layer can be used. The thickness of the positive electrode core 30 is, for example, 10 μm or more and 30 μm or less.

[0020] The positive electrode mixture layer 31 includes, for example, a positive electrode active material, a conductive additive, and a binder. The positive electrode mixture layer 31 is preferably provided on both sides of the positive electrode core 30 except for the portion to which the positive electrode lead 20 is connected. The positive electrode 11 can be produced, for example, by applying a positive electrode mixture slurry including a positive electrode active material, a binder, a conductive additive, and the like to the surface of the positive electrode core 30, drying the coating, and then compressing it to form the positive electrode mixture layer 31 on both sides of the positive electrode core 30.

[0021] The weight of the positive electrode mixture layer 31 is, for example, 250 g / m 2 In this case, the effect of the present disclosure can be significantly exhibited while realizing a high capacity non-aqueous electrolyte secondary battery. From the viewpoint of increasing capacity, the basis weight of the positive electrode mixture layer 31 is set to 300 g / m 2 or more, and 2 The upper limit of the basis weight of the positive electrode mixture layer 31 is, for example, 600 g / m from the viewpoint of cycle characteristics. 2 Therefore, an example of a suitable range of the basis weight of the positive electrode mixture layer 31 is 250 g / m 2 Above, 600g / m 2 The thickness of the positive electrode mixture layer 31 is, for example, 10 μm or more and 200 μm or less on one side of the positive electrode substrate 30 .

[0022] The positive electrode 11 contains a lithium-containing transition metal composite oxide as a positive electrode active material. The lithium-containing transition metal composite oxide contains, for example, secondary particles formed by aggregation of primary particles. The particle size of the primary particles constituting the secondary particles of the lithium-containing transition metal composite oxide is, for example, 0.02 μm or more and 2 μm or less. The particle size of the primary particles is measured as the diameter of a circumscribed circle in a particle image observed with a scanning electron microscope (SEM). The average particle size of the secondary particles of the lithium-containing transition metal composite oxide is, for example, 2 μm or more and 30 μm or less. Here, the average particle size refers to the volume-based median diameter (D50). D50 refers to the particle size at which the cumulative frequency in the volume-based particle size distribution is 50% from the smallest particle size, and is also referred to as the median diameter. The particle size distribution of the secondary particles of the lithium-containing transition metal composite oxide can be measured using a laser diffraction particle size distribution analyzer (e.g., MT3000II, manufactured by Microtrac-Bell Corporation) using water as a dispersion medium.

[0023] The lithium-containing transition metal composite oxide has, for example, a layered structure. Examples of the layered structure of the lithium-containing transition metal composite oxide include a layered structure belonging to the space group R-3m and a layered structure belonging to the space group C2 / m. From the viewpoints of increasing capacity and stabilizing the crystal structure, the lithium-containing transition metal composite oxide preferably has a layered structure belonging to the space group R-3m. The layered structure of the lithium-containing transition metal composite oxide may include a transition metal layer and a Li layer.

[0024] The lithium-containing transition metal composite oxide contains, for example, 50 mol % or more of Ni and one or more elements selected from the group consisting of Co, Mn, and Al, based on the total number of moles of metal elements excluding Li.

[0025] The Ni content in the lithium-containing transition metal composite oxide is 50 mol% or more relative to the total number of moles of metal elements excluding Li. This allows for improved battery capacity. The Ni content may be 75 mol% or more, or may be 80 mol% or more, preferably 85 mol% or more, and more preferably 90 mol% or more. In addition, from the viewpoint of structural stabilization, the Ni content is preferably 99 mol% or less, more preferably 95 mol% or less.

[0026] The content of Co in the lithium-containing transition metal composite oxide is 0 mol % or more and 15 mol % or less relative to the total number of moles of metal elements excluding Li, and Co is an optional component. In other words, the lithium-containing transition metal composite oxide does not need to contain Co. By containing Co, the lithium-containing transition metal composite oxide can improve the heat resistance of the battery.

[0027] The content of Mn in the lithium-containing transition metal composite oxide is 0 mol % or more and 50 mol % or less relative to the total number of moles of metal elements excluding Li, and Mn is an optional component. In other words, the lithium-containing transition metal composite oxide does not need to contain Mn. By containing Mn, the lithium-containing transition metal composite oxide can stabilize its crystal structure.

[0028] The content of Al in the lithium-containing transition metal composite oxide is 0 mol % or more and 15 mol % or less with respect to the total number of moles of metal elements excluding Li, and Al is an optional component. In other words, the lithium-containing transition metal composite oxide does not necessarily contain Al.

[0029] The total content of Co, Mn, and Al in the lithium-containing transition metal composite oxide is, for example, 0 mol % or more and 50 mol % or less.

[0030] The lithium-containing transition metal composite oxide may further contain one or more elements selected from the group consisting of W, Mg, Mo, Nb, Ti, Si, Ca, Sr, and Zr. The contents of W, Mg, Mo, Nb, Ti, Si, Ca, Sr, and Zr in the lithium-containing transition metal composite oxide are each, for example, 0 mol % or more and 1 mol % or less, relative to the total number of moles of metal elements excluding Li. The total content of W, Mg, Mo, Nb, Ti, Si, Ca, Sr, and Zr is, for example, 0 mol % or more and 2 mol % or less.

[0031] The lithium-containing transition metal composite oxide is, for example, a compound represented by the general formula Li x Ni a M1 b M2 c O 2-y(wherein 0.8<x<1.2, 0.5≦a, 0≦b≦0.5, 0≦c≦0.02, 0≦y<0.05, a+b+c=1, M1 is one or more elements selected from the group consisting of Co, Mn, and Al, and M2 is one or more elements selected from the group consisting of W, Mg, Mo, Nb, Ti, Si, Ca, Sr, and Zr).

[0032] The content of elements constituting the lithium-containing transition metal composite oxide can be measured using an inductively coupled plasma atomic emission spectrometer (ICP-AES), an electron probe microanalyzer (EPMA), an energy dispersive X-ray analyzer (EDX), or the like.

[0033] The sulfonic acid compound represented by formula (I) is present on the particle surface of the lithium-containing transition metal composite oxide. In the formula, A is a Group 1 or Group 2 element, R is a hydrocarbon group, and n is 1 or 2. A is preferably a Group 1 element. Among these, Li or Na is more preferred, and Li is particularly preferred. The sulfonic acid compound may be scattered so as to cover at least a portion of the surface of the secondary particles of the lithium-containing transition metal composite oxide, or may be present so as to cover the entire surface of the secondary particles. In addition, the sulfonic acid compound may be fixed to the surface of the primary particles of the lithium-containing transition metal composite oxide.

[0034] In formula (I), R is preferably an alkyl group. The number of carbon atoms in the alkyl group is preferably 5 or less, more preferably 3 or less. From the viewpoint of reducing reaction resistance, a suitable example of R is an alkyl group having 3 or less carbon atoms, and among these, a methyl group is preferred. In R, some of the hydrogen atoms bonded to the carbon may be substituted with fluorine. In formula (I), n is preferably 1.

[0035] Specific examples of the sulfonic acid compound include lithium methanesulfonate, lithium ethanesulfonate, lithium propanesulfonate, sodium methanesulfonate, sodium ethanesulfonate, magnesium methanesulfonate, lithium fluoromethanesulfonate, etc. Among these, at least one selected from the group consisting of lithium methanesulfonate, lithium ethanesulfonate, and sodium methanesulfonate is preferred, with lithium methanesulfonate being particularly preferred.

[0036] The sulfonic acid compound reduces the reaction resistance in the positive electrode 11, thereby improving the output characteristics of the battery. Although this effect can be achieved even with a very small amount of sulfonic acid compound, the amount of sulfonic acid compound present on the particle surface of the lithium-containing transition metal composite oxide is preferably 0.1 mass% or more, and more preferably 0.3 mass% or more, relative to the mass of the lithium-containing transition metal composite oxide. Furthermore, from the viewpoint of cycle characteristics, the amount of sulfonic acid compound present on the particle surface of the lithium-containing transition metal composite oxide is preferably 1.0 mass% or less, and more preferably 0.8 mass% or less, relative to the mass of the lithium-containing transition metal composite oxide. Therefore, the amount of sulfonic acid compound is preferably 0.1 mass% or more and 1.0 mass% or less, and more preferably 0.3 mass% or more and 0.8 mass% or less, relative to the mass of the lithium-containing transition metal composite oxide.

[0037] The presence of the sulfonic acid compound on the particle surface of the lithium-containing transition metal composite oxide can be confirmed by Fourier transform infrared spectroscopy (FT-IR). In the infrared absorption spectrum obtained by FT-IR, the positive electrode active material containing lithium methanesulfonate exhibits, for example, a peak at 1238 cm -1 , 1175 cm -1 , 1065 cm -1 , 785 cm -1 It has an absorption peak around 1238 cm -1 , 1175 cm -1 , 1065 cm -1 The peak around 785 cm is due to the SO stretching vibration of lithium methanesulfonate. -1The peak around 1000 nm is a peak due to the C-S stretching vibration derived from lithium methanesulfonate. In addition, the presence of a positive electrode active material containing a sulfonic acid compound other than lithium methanesulfonate can also be confirmed from the absorption peak derived from the sulfonic acid compound in the infrared absorption spectrum.

[0038] The presence of the sulfonic acid compound can also be confirmed by X-ray photoelectron spectroscopy (XPS). In the spectrum obtained by XPS, a peak with an intensity (c / s) of 200 or more and 1000 or less is observed in the positive electrode active material containing lithium methanesulfonate, where the binding energy is approximately 165 or more and 170 eV or less. The presence of the sulfonic acid compound on the secondary particle surface of the lithium-containing transition metal composite oxide can also be confirmed by ICP, atomic absorption spectroscopy, synchrotron XRD measurement, TOF-SIMS, H-NMR, etc.

[0039] In addition to the sulfonic acid compound, a metal compound may be present on the surface of the secondary particles of the lithium-containing transition metal composite oxide. The metal compound contains, for example, one or more metal elements selected from the group consisting of Sr, Ca, W, Zr, rare earth elements, and Al. Examples of the Sr-containing compound include SrO, Sr(OH), and the like. 2 and SrCO 3 Examples of compounds containing Ca include CaO and Ca(OH). 2 and CaCO 3 Examples of compounds containing W include WO 3 Examples of the compound containing Al include Al 2 O 3 Examples of compounds containing Zr include ZrO 2 , Zr(OH) 4 , Zr(CO 3 ) 2 and Zr(SO 4 ) 2 ・4H 2 Examples of rare earth-containing compounds include oxides, hydroxides, carbonates, sulfates, nitrates, and phosphates of rare earth elements. The metal compound may contain a plurality of types of these metal elements, and examples thereof include SrAlO 4, CaAlO 4 The metal compound may further contain Li, and an example thereof is lithium tungstate.

[0040] A nonmetallic compound may be present on the surface of the lithium-containing transition metal composite oxide. The nonmetallic compound contains, for example, one or more nonmetallic elements selected from the group consisting of P and B. Examples of the P-containing compound include Li, 3-x H x P.O. 4 (0≦x≦3) can be exemplified. 3 BO 3 , Li 3 BO 3 , Li 2 B 4 O 7 Examples include:

[0041] The positive electrode active material, which is one example of the embodiment, can be produced by the following method: Note that the production method described here is only an example, and the method for producing the positive electrode active material is not limited to this method.

[0042] The manufacturing process of the positive electrode active material includes a synthesis step of obtaining a lithium-containing transition metal composite oxide, a washing step of washing the fired product with water and dehydrating it to obtain a cake-like composition, a drying step of drying the cake-like composition to obtain a powder-like composition, and an addition step of adding at least one of a sulfonic acid compound and a sulfonic acid solution to the cake-like composition or the powder-like composition.

[0043] In the synthesis step, for example, a metal oxide containing 50 mol% or more of Ni, 0 mol% or more and 15 mol% or less of Co, 0 mol% or more and 50 mol% or less of Mn, 0 mol% or more and 15 mol% or less of Al, and 0 mol% or more and 2 mol% or less of M2 (M2 is one or more elements selected from W, Mg, Mo, Nb, Ti, Si, Ca, Sr, and Zr) is mixed with a Li compound to obtain a mixture.

[0044] The metal oxide can be obtained, for example, by adding an alkaline solution such as sodium hydroxide dropwise to a stirred solution of a metal salt containing Ni and an arbitrary metal element (Co, Mn, Al, M, etc.) to adjust the pH to the alkaline side (e.g., 8.5 or more and 12.5 or less), thereby precipitating (co-precipitating) a composite hydroxide containing Ni and the arbitrary metal element, and then heat-treating the composite hydroxide. The heat-treatment temperature is not particularly limited, but is, for example, in the range of 250°C or more and 600°C or less.

[0045] Examples of Li compounds include Li 2 CO 3 , LiOH, Li 2 O 2 , Li 2 O, LiNO 3 , LiNO 2 , Li 2 SO 4 , LiOH·H 2 Examples of the metal oxide include O, LiH, and LiF. In order to easily adjust each of the above parameters to the ranges specified above, the mixing ratio of the metal oxide and the Li compound is preferably such that the molar ratio of the total amount of metal elements in the metal oxide to Li is in the range of 1:0.8 or more and 1:1.2 or less, and more preferably 1:1.0 or more and 1:1.1 or less.

[0046] Next, the synthesis step includes a calcination step in which the resulting mixture is calcined. The calcination step is a multi-stage calcination step that includes at least a first calcination step in which the mixture is calcined at 300°C or higher and 680°C or lower under an oxygen stream, and a second calcination step in which the calcined product obtained by the first calcination step is calcined at a temperature exceeding 680°C under an oxygen stream. In the first calcination step, the temperature is increased to a first set temperature of 680°C or lower at a first temperature increase rate of 0.2°C / min or higher and 4.5°C / min or lower. In the second calcination step, the temperature is increased to a second set temperature of 900°C or lower at a first temperature increase rate of 0.5°C / min or higher and 3.5°C / min or lower. Note that multiple first and second temperature increase rates may be set for each temperature range as long as they are within the above-specified range.

[0047] The holding time of the first set temperature in the first firing step is preferably 5 hours or less, more preferably 3 hours or less. The holding time of the first set temperature is the time during which the first set temperature is maintained after reaching the first set temperature, and the holding time may be zero. The holding time of the second set temperature in the second firing step is preferably 1 hour or more and 10 hours or less, more preferably 1 hour or more and 5 hours or less. The holding time of the second set temperature is the time during which the second set temperature is maintained after reaching the second set temperature. The firing of the mixture is carried out, for example, in an oxygen stream with an oxygen concentration of 60% or more, and the flow rate of the oxygen stream is set to 10 cm / s. 3 The flow rate shall be 0.2 mL / min or more and 4 mL / min or less per kg of the mixture, or 0.3 L / min or more per kg of the mixture.

[0048] In the washing step, the lithium-containing transition metal composite oxide is washed with water and dehydrated to obtain a cake-like composition. The particulate lithium-containing transition metal composite oxide obtained in the synthesis step can be used. By washing with water, unreacted lithium compounds added in the synthesis step and impurities other than the lithium compounds can be removed. When washing with water, for example, 300 g or more and 5000 g or less of lithium-containing transition metal composite oxide is added to 1 L of water. The water washing may be repeated multiple times. The dehydration after washing with water can be performed, for example, using a filter press.

[0049] In the drying step, the cake-like composition obtained in the washing step is dried to obtain a powdery composition. The drying step may be performed under a vacuum atmosphere. The drying conditions are, for example, 150°C or higher and 400°C or lower for 0.5 hours or longer and 15 hours or shorter.

[0050] In the addition step, at least one of a sulfonic acid compound and a sulfonic acid solution is added to the cake-like composition obtained in the washing step or the powder-like composition obtained in the drying step. This allows the sulfonic acid compound to adhere to the surface of the lithium-containing transition metal composite oxide. It is preferable to add at least one of a sulfonic acid compound and a sulfonic acid solution to the cake-like composition. The sulfonic acid compound to be added may be in either powder or solution form. The sulfonic acid solution is, for example, a methanesulfonic acid solution obtained by dissolving methanesulfonic acid in water. Li compounds remain in the cake-like composition, and these remaining Li compounds are dissolved in the water contained in the cake-like composition. Therefore, even when a sulfonic acid solution is added, a Li-containing sulfonic acid compound is formed. From the viewpoint of more easily achieving the effects of the present application, a Li compound or a Li compound solution may be added to the cake-like composition or the powder-like composition together with the sulfonic acid solution. Alternatively, a mixed solution in which a sulfonic acid solution and a Li compound or a Li compound solution are premixed may be added to the cake-like composition or the powder-like composition. The Li compound is, for example, LiOH, and the Li compound solution is, for example, a LiOH solution obtained by dissolving LiOH in water. The amounts of the Li compound and sulfonic acid solution added to the cake-like composition preferably satisfy the relationship of 0≦Li compound / sulfonic acid≦1.3 in molar ratio. The amount of sulfonic acid compound or sulfonic acid added is preferably 0.1% by mass or more and 1% by mass or less, and more preferably 0.3% by mass to 0.8% by mass, relative to the mass of the lithium-containing transition metal composite oxide. The concentrations of the sulfonic acid solution and the sulfonic acid compound solution are, for example, 0.5% by mass or more and 40% by mass or less. The addition step may be performed during the washing step, after the washing step, during the drying step, or after the drying step, and the timing of the addition can be changed as appropriate.

[0051] A metal compound containing one or more metal elements selected from the group consisting of Sr, Ca, W, Zr, rare earth elements, and Al, and a nonmetallic compound containing one or more nonmetallic elements selected from the group consisting of P and B can be attached to the surface of the lithium-containing transition metal composite oxide by adding the raw material of the metal compound or nonmetallic compound during the synthesis process, after the synthesis process, during the cleaning process, after the cleaning process, during the drying process, after the drying process, or during the addition process. 2 , Sr(OH) 2 ・8H 2 O, SrO, SrCo 3 , SrSO 4 , Sr(NO 3 ) 2、 SrCl 2 , SrAlO 4 Examples of Ca raw materials include Ca(OH) 2 , CaO, CaCO 3 , CaSO 4 , Ca(NO 3 ) 2、 CaCl 2 , CaAlO 4 The Zr raw material is Zr(OH) 4 , ZrO 2 , Zr(CO 3 ) 2 , Zr(SO 4 ) 2 ・4H 2 Examples of rare earth raw materials include oxides, hydroxides, and carbonates of rare earth elements. Examples of W raw materials include tungsten oxide (WO 3 ), lithium tungstate (Li 2 WO 4 , Li 4 WO 5 , Li 6 W 2 O 9 As the W raw material, a solution containing W may be used. As the Al raw material, Al 2 O 3、 Al(OH) 3、 Al 2 (SO 4 ) 3The P raw material may be Al derived from a lithium-containing transition metal composite oxide. 3-x H x P.O. 4 (0≦x≦3) and the like. 3 BO 3 , Li 3 BO 3 , Li 2 B 4 O 7 These compounds may be pulverized to appropriately change the particle shape or particle size, or may be used as hydrates with the water content adjusted.

[0052] As described above, the positive electrode mixture layer 31 contains a conductive additive. The conductive additive includes at least one selected from the group consisting of carbon nanotubes (CNTs) and carbon black (CB) having an average diameter of 20 nm or less, and graphene having an average thickness of 50 nm or less. The conductive additive may contain carbon materials other than the above-mentioned carbon materials, but is primarily composed of carbon nanotubes (CNTs) and carbon black (CB) having an average diameter of 20 nm or less, and graphene having an average thickness of 50 nm or less. Note that the term "major component" refers to the component that accounts for the largest mass proportion of the conductive additive. This ensures that a sufficient conductive path is formed in the positive electrode mixture layer 31, even when a sulfonic acid compound is present on the surface of the positive electrode active material particles. As a result, the positive electrode mixture resistance is reduced, and cycle characteristics during high-rate charging are improved.

[0053] The conductive additive may be substantially composed of at least one selected from the group consisting of carbon nanotubes (CNTs) and carbon black (CB) having an average diameter of 20 nm or less, and graphene having an average thickness of 50 nm or less, in which case the effects of the present disclosure are more pronounced.

[0054] Carbon nanotubes are generally conductive carbon fibers with an outer diameter (i.e., fiber diameter) of several tens of nanometers or less, and have an extremely large aspect ratio (ratio of fiber length to fiber diameter). The average aspect ratio of carbon nanotubes is, for example, 20 times or more, preferably 50 times or more. Carbon nanotubes with a high aspect ratio of 20 times or more form linear contact with the positive electrode active material and the positive electrode core, rather than point contact. Therefore, a good conductive path can be formed with the addition of a small amount.

[0055] The average diameter of the carbon nanotubes is 20 nm or less, preferably 15 nm or less, and more preferably 10 nm or less. Here, the average diameter of the carbon nanotubes refers to the average fiber diameter determined by image analysis using a transmission electron microscope (TEM). The fiber diameter refers to the length in the direction perpendicular to the fiber length direction. The lower limit of the average diameter of the carbon nanotubes is not particularly limited, but an example is 1 nm. The average diameter of the carbon nanotubes is determined by measuring the fiber diameters of 100 randomly selected carbon nanotubes and calculating the arithmetic average of the measured values.

[0056] The average fiber length of the carbon nanotubes is, for example, 0.5 μm or more, and may be 1 μm or more. The fiber length refers to the length of the carbon nanotubes when stretched linearly. An average fiber length of 0.5 μm or more further improves the conductivity of the positive electrode mixture layer 31. The upper limit of the average fiber length of the carbon nanotubes is not particularly limited, but an example is 100 μm. The average fiber length of the carbon nanotubes is determined by image analysis using a scanning electron microscope (SEM). The average fiber length of the carbon nanotubes is determined by measuring the lengths of 100 randomly selected carbon nanotubes and arithmetically averaging the measured values. The carbon nanotubes present in the positive electrode mixture layer 31 may be present in a bundle of multiple carbon nanotubes. The above average fiber length is calculated using the length of a single carbon nanotube present in the bundle of carbon nanotubes.

[0057] The carbon nanotubes may be either single-walled carbon nanotubes (SWCNT) or multi-walled carbon nanotubes (MWCNT), but are more preferably single-walled carbon nanotubes. Furthermore, single-walled carbon nanotubes and multi-walled carbon nanotubes may be used in combination as the conductive additive. Single-walled carbon nanotubes have a structure in which one layer of graphite sheets is formed into a tubular shape, while multi-walled carbon nanotubes have a structure in which multiple layers of graphite sheets are formed into a tubular shape. One example of a multi-walled carbon nanotube is a double-walled carbon nanotube, which has a two-wall structure.

[0058] The preferred BET specific surface area of ​​the carbon nanotubes varies depending on the type of carbon nanotube. For example, 2 / g or more, more preferably 250m 2 The upper limit of the BET specific surface area is not particularly limited, but is, for example, 2000 m 2 The BET specific surface area is measured in accordance with the BET method (nitrogen adsorption method) described in JIS R1626.

[0059] The average diameter of carbon black is 20 nm or less, preferably 15 nm or less. Here, the average diameter of carbon black refers to the average particle size determined by image analysis using a transmission electron microscope (TEM). Generally, carbon black is composed of smallest particles, also called domains, primary agglomerates of these smallest particles, and secondary agglomerates of these primary agglomerates. Here, primary agglomerates are also called aggregates, and secondary agglomerates are also called agglomerates. The lower limit of the average diameter of carbon black is not particularly limited, but an example is 1 nm.

[0060] The aspect ratio of carbon black (ratio of major axis to minor axis) is, for example, 1.2 to 2.5, or 1.3 to 2. The aspect ratio of carbon black refers to the aspect ratio of the primary aggregates described above. Carbon black with a high aspect ratio of 1.2 or more can form a good conductive path with the addition of a small amount.

[0061] Carbon black is sometimes called by different names depending on the manufacturing method. Specifically, it is called acetylene black manufactured by the acetylene method, furnace black manufactured by the furnace method, channel black manufactured by the channel method, etc. As long as the average diameter of carbon black is 20 nm or less, the effects of the present application are exhibited regardless of the manufacturing method, but carbon black with few impurities and high conductivity is more preferable.

[0062] The average thickness of the graphene is 50 nm or less, preferably 30 nm or less, and more preferably 20 nm or less. The thickness of the graphene is determined by image analysis using a transmission electron microscope (TEM). The average thickness of the graphene is determined by measuring the thickness of 100 randomly selected graphenes and calculating the arithmetic average of the measured values.

[0063] The size of the graphene in the planar direction is, for example, a major axis of 0.5 μm or more, preferably 1.0 μm or more. In this case, it is easy to improve the conductivity of the positive electrode mixture layer 31. The size in the planar direction refers to the average value of the longest diameter and the shortest diameter of the graphene plane. The upper limit of the size of the graphene in the planar direction is not particularly limited, but an example is 100 μm. The size in the planar direction of the graphene is determined by image analysis using a scanning electron microscope (SEM). 100 graphenes are arbitrarily selected, the lengths are measured, and the measured values ​​are arithmetically averaged. The aspect ratio of the graphene (the ratio of the major axis in the planar direction of the graphene to the thickness of the graphene) is preferably 10 or more.

[0064] The content of the conductive additive is preferably 2.0% by mass or less, and more preferably 1.0% by mass or less, relative to the total mass of the positive electrode active material. Even a small amount of the conductive additive forms a good conductive path in the positive electrode mixture layer 31, but the lower limit of the conductive additive content is preferably 0.01% by mass. Therefore, an example of a suitable content of the conductive additive is 0.01% by mass or more and 2.0% by mass or less, and more preferably 0.01% by mass or more and 1.0% by mass or less, relative to the total mass of the positive electrode active material.

[0065] The conductive additive may be supplied to the manufacturing process of the positive electrode 11 in the form of a conductive additive dispersion in which the conductive additive is mixed and dispersed in a liquid containing a dispersant and an aprotic polar solvent (dispersion medium), and then added to the positive electrode mixture slurry. Both the conductive additive and the dispersant may be supplied to the positive electrode mixture slurry in a solid state. Either or both of the conductive additive and the dispersant may be supplied to the positive electrode mixture slurry in a liquid state. The conductive additive and the dispersant may be supplied individually or as a mixture. When supplied in the form of a dispersion, the dispersant is dissolved in the polar solvent, and the conductive additive is dispersed in the polar solvent by the action of the dispersant. The solid content (conductive additive and dispersant) of the dispersion is, for example, 1% by mass or more and 20% by mass or less, but is not particularly limited. The conductive additive dispersion may also be added to the positive electrode mixture slurry in the form of a mixture in which a binder is premixed. The binder may be in either a solid or liquid state.

[0066] The dispersant may include, for example, a nitrile group-containing rubber. The nitrile group-containing rubber may be a copolymer of a monomer containing unsaturated nitrile and a conjugated diene as raw materials, and may be a copolymer essentially consisting of only unsaturated nitrile and conjugated diene. The molar ratio of unsaturated nitrile to conjugated diene is, for example, 10:90 or more and 70:30 or less. The weight-average molecular weight of the nitrile group-containing rubber is not particularly limited, but is, for example, 5,000 or more and 500,000 or less. Furthermore, at least a portion of the dispersant may function as a binder for the positive electrode mixture layer 31.

[0067] The nitrile group-containing rubber may be a hydrogenated nitrile rubber. The hydrogenated nitrile rubber contains, for example, structural units derived from an unsaturated nitrile, structural units derived from a conjugated diene, and structural units derived from a hydrogenated conjugated diene. An example of a suitable hydrogenated nitrile rubber is a partially hydrogenated nitrile rubber in which 80 mol% or more of the structural units derived from a conjugated diene have been hydrogenated. An example of an unsaturated nitrile is acrylonitrile or methacrylonitrile, preferably acrylonitrile. An example of a conjugated diene is a conjugated diene having 3 to 6 carbon atoms, preferably butadiene.

[0068] The nitrile group-containing rubber is preferably contained in an amount of 5% by mass or more and 1000% by mass or less relative to the total mass of the conductive assistant. The conductive assistant dispersion may contain only the nitrile group-containing rubber as a dispersant, or other dispersants may be used in combination. The mass ratio of the nitrile group-containing rubber in the dispersant is preferably 20% by mass or more, more preferably 30% by mass or more. Examples of other dispersants that can be used in combination with the nitrile group-containing rubber include polyvinyl alcohol, polyvinylpyrrolidone (PVP), polyalkylene oxide, polyvinyl acetal, polyvinyl ether, cellulose or its derivatives, chitins, chitosans, starch, and derivatives thereof. Among these, PVP or its derivatives (PVPs) are preferably used.

[0069] An aprotic polar solvent is used as the dispersion medium. The aprotic polar solvent may be any solvent that can dissolve the dispersant and disperse the conductive additive. Since the dispersion liquid is added to the positive electrode mixture slurry, the polar solvent is preferably miscible with the solvent of the positive electrode mixture slurry, and may be the same type of solvent as the solvent of the positive electrode mixture slurry. Examples of aprotic polar solvents include N-methyl-2-pyrrolidone (NMP), methyl ethyl ketone, tetrahydrofuran, dimethylformamide, acetone, ethyl acetate, and dimethyl sulfoxide. Among these, it is preferable to use NMP.

[0070] The positive electrode mixture layer 31 may also contain a binder. Examples of binders include fluorine-containing polymers such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVDF), polyacrylonitrile (PAN), polyimide, acrylic resin, and polyolefin. These resins may also be used in combination with cellulose or its derivatives, polyethylene oxide (PEO), and the like. The content of the binder is, for example, 0.1% by mass or more and 2% by mass or less, and preferably 0.5% by mass or more and 1.5% by mass or less, relative to the total mass of the positive electrode active material.

[0071] [Negative Electrode] The negative electrode 12 may have, for example, a negative electrode core 40 and a negative electrode mixture layer 41 formed on the surface of the negative electrode core 40, or a metal Li foil may be used as the negative electrode 12. Alternatively, the negative electrode 12 may have the negative electrode core 40, and lithium metal may be deposited on the surface of the negative electrode core 40 upon charging. When the negative electrode 12 has the negative electrode mixture layer 41, the negative electrode mixture layer 41 is preferably formed on both sides of the negative electrode core 40. The negative electrode core 40 may be made of a foil of a metal that is stable within the potential range of the negative electrode 12, such as copper or a copper alloy, or a film having such a metal disposed on the surface layer. The thickness of the negative electrode core 40 is, for example, 5 μm or more and 30 μm or less.

[0072] The negative electrode mixture layer 41 contains, for example, a negative electrode active material and a binder. The thickness of the negative electrode mixture layer 41 is, for example, 10 μm or more and 150 μm or less on one side of the negative electrode core 40. The negative electrode 12 can be produced, for example, by applying a negative electrode mixture slurry containing a negative electrode active material, a binder, and the like to the surface of the negative electrode core 40, drying the coating, and then rolling it to form a negative electrode mixture layer on both sides of the negative electrode core.

[0073] The negative electrode active material contained in the negative electrode mixture layer 41 is not particularly limited as long as it can reversibly absorb and release lithium ions, and generally, a carbon material such as graphite is used. The graphite may be any of natural graphite such as flake graphite, lump graphite, and amorphous graphite, or artificial graphite such as lump artificial graphite and graphitized mesophase carbon microbeads. Furthermore, as the negative electrode active material, metals that alloy with Li, such as Si and Sn, metal compounds containing Si, Sn, and lithium-titanium composite oxides, may also be used. Furthermore, these may be provided with a carbon coating. For example, SiO x (0.5≦x≦1.6) or Li 2y SiO (2+y) A Si-containing compound in which fine particles of Si are dispersed in a lithium silicate phase represented by (0<y<2) may be used in combination with graphite.

[0074] Examples of the binder contained in the negative electrode mixture layer 41 include styrene butadiene rubber (SBR), nitrile butadiene rubber (NBR), carboxymethyl cellulose (CMC) or a salt thereof, polyacrylic acid (PAA) or a salt thereof (PAA-Na, PAA-K, etc., or a partially neutralized salt), polyvinyl alcohol (PVA), etc. These may be used alone or in combination of two or more.

[0075] [Separator] A porous sheet having ion permeability and insulating properties is used for the separator 13. Specific examples of the porous sheet include a microporous thin film, a woven fabric, and a nonwoven fabric. Suitable materials for the separator 13 include polyolefins such as polyethylene and polypropylene, and cellulose. The separator 13 may have a single-layer structure or a multi-layer structure. Furthermore, a highly heat-resistant resin layer such as an aramid resin may be formed on the surface of the separator 13.

[0076] A filler layer containing an inorganic filler may be formed at the interface between the separator 13 and at least one of the positive electrode 11 and the negative electrode 12. Examples of inorganic fillers include oxides and phosphate compounds containing metal elements such as Ti, Al, Si, and Mg. The filler layer can be formed by applying a slurry containing the filler to the surface of the positive electrode 11, the negative electrode 12, or the separator 13.

[0077] [Non-aqueous electrolyte] The non-aqueous electrolyte has ion conductivity (for example, lithium ion conductivity). The non-aqueous electrolyte may be a liquid electrolyte (electrolytic solution) or a solid electrolyte.

[0078] The liquid electrolyte (electrolytic solution) contains, for example, a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. Examples of the non-aqueous solvent that can be used include esters, ethers, nitriles such as acetonitrile, amides such as dimethylformamide, and mixed solvents of two or more of these. The non-aqueous solvent may contain a halogen-substituted compound in which at least a portion of the hydrogen atoms in these solvents are substituted with halogen atoms such as fluorine. Examples of the halogen-substituted compound include fluorinated cyclic carbonates such as fluoroethylene carbonate (FEC), fluorinated chain carbonates, and fluorinated chain carboxylic acid esters such as methyl fluoropropionate (FMP).

[0079] Examples of the esters include cyclic carbonates such as ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate; chain carbonates such as dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), methyl propyl carbonate, ethyl propyl carbonate, and methyl isopropyl carbonate; cyclic carboxylic acid esters such as γ-butyrolactone (GBL) and γ-valerolactone (GVL); and chain carboxylic acid esters such as methyl acetate, ethyl acetate, propyl acetate, methyl propionate (MP), and ethyl propionate (EP).

[0080] Examples of the ethers include 1,3-dioxolane, 4-methyl-1,3-dioxolane, tetrahydrofuran, 2-methyltetrahydrofuran, propylene oxide, 1,2-butylene oxide, 1,3-dioxane, 1,4-dioxane, 1,3,5-trioxane, furan, 2-methylfuran, 1,8-cineole, cyclic ethers such as crown ethers, 1,2-dimethoxyethane, diethyl ether, dipropyl ether, diisopropyl ether, dibutyl ether, dihexyl ether, ethyl vinyl ether, butyl vinyl ether, and methyl phenyl ether. and chain ethers such as ethyl phenyl ether, butyl phenyl ether, pentyl phenyl ether, methoxytoluene, benzyl ethyl ether, diphenyl ether, dibenzyl ether, o-dimethoxybenzene, 1,2-diethoxyethane, 1,2-dibutoxyethane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, 1,1-dimethoxymethane, 1,1-diethoxyethane, triethylene glycol dimethyl ether, and tetraethylene glycol dimethyl ether.

[0081] The electrolyte salt is preferably a lithium salt. Examples of the lithium salt include LiClO 4 , LiBF 4 , LiPF 6 , LiAlCl 4 , LiSbF 6 , LiSCN, LiCF 3 SO 3 , LiCF 3 CO 2 , LiAsF 6 , LiB 10 Cl 10 , lower aliphatic lithium carboxylates, LiCl, LiBr, LiI, phosphates, borates, and imide salts. Examples of phosphates include lithium difluorophosphate (LiPO 2 F 2Examples of the borate salt include lithium bis(oxalato)borate (LiBOB) and lithium difluoro(oxalato)borate (LiDFFOB). Examples of the imide salt include lithium bisfluorosulfonylimide (LiN(FSO 2 ) 2 ), lithium bistrifluoromethanesulfonyl imide (LiN(CF 3 SO 2 ) 2 ), lithium trifluoromethanesulfonate nonafluorobutanesulfonate imide (LiN(CF 3 SO 2 ) (C 4 F 9 SO 2 )), lithium bispentafluoroethanesulfonyl imide (LiN(C 2 F 5 SO 2 ) 2 Among these, LiPF is preferred from the viewpoint of ionic conductivity, electrochemical stability, etc. 6 The concentration of the lithium salt may be, for example, 4 mol or less, or 3 mol or less, preferably 1.8 mol or less, and more preferably 0.8 mol or more and 1.8 mol or less, per 1 L of the non-aqueous solvent.

[0082] The non-aqueous electrolyte may contain an additive such as an unsaturated carbonate ester, an acid anhydride, a phenol compound, a benzene compound, a nitrile compound, an isocyanate compound, a sultone compound, a sulfate compound, a borate ester compound, a phosphate ester compound, or a phosphite ester compound.

[0083] Examples of unsaturated cyclic carbonates include vinylene carbonate, 4-methylvinylene carbonate, 4,5-dimethylvinylene carbonate, 4-ethylvinylene carbonate, 4,5-diethylvinylene carbonate, 4-propylvinylene carbonate, 4,5-dipropylvinylene carbonate, 4-phenylvinylene carbonate, 4,5-diphenylvinylene carbonate, vinylethylene carbonate, and divinylethylene carbonate. One type of unsaturated cyclic carbonate may be used alone, or two or more types may be used in combination. Some of the hydrogen atoms in the unsaturated cyclic carbonate may be substituted with fluorine atoms. The acid anhydride may be an anhydride formed by intermolecular condensation of multiple carboxylic acid molecules, but is preferably an acid anhydride of a polycarboxylic acid. Examples of polycarboxylic acid anhydrides include succinic anhydride, maleic anhydride, and phthalic anhydride.

[0084] Examples of phenolic compounds include phenol, hydroxytoluene, etc. Examples of benzene compounds include fluorobenzene, hexafluorobenzene, cyclohexylbenzene (CHB), etc.

[0085] Examples of nitrile compounds include adiponitrile, pimelonitrile, propionitrile, and succinonitrile. Examples of isocyanate compounds include methyl isocyanate (MIC), diphenylmethane diisocyanate (MDI), hexamethylene diisocyanate (HDI), toluene diisocyanate (TDI), isophorone diisocyanate (IPDI), and bisisocyanatomethylcyclohexane (BIMCH). Examples of sultone compounds include propane sultone and propene sultone. Examples of sulfate compounds include ethylene sulfate, ethylene sulfite, dimethyl sulfate, and lithium fluorosulfate. Examples of borate ester compounds include trimethyl borate and tris(trimethylsilyl)borate. Examples of phosphate ester compounds include trimethyl phosphate and tris(trimethylsilyl)phosphate. Examples of phosphite ester compounds include trimethyl phosphite and tris(trimethylsilyl)phosphite.

[0086] As the solid electrolyte, for example, a solid or gel-like polymer electrolyte, an inorganic solid electrolyte, etc. can be used. As the inorganic solid electrolyte, a material known in all-solid-state lithium ion secondary batteries, etc. (for example, an oxide-based solid electrolyte, a sulfide-based solid electrolyte, a halogen-based solid electrolyte, etc.) can be used. The polymer electrolyte includes, for example, a lithium salt and a matrix polymer, or a non-aqueous solvent, a lithium salt, and a matrix polymer. As the matrix polymer, for example, a polymer material that absorbs the non-aqueous solvent and gels is used. As the polymer material, for example, a fluororesin, an acrylic resin, a polyether resin, etc. can be used.

[0087] Hereinafter, the present disclosure will be further described with reference to examples and comparative examples, but the present disclosure is not limited to the following examples. Example 1 [Preparation of Positive Electrode Active Material] [Ni 0.90 Co 0.05 Al 0.05 ](OH) 2The composite hydroxide represented by the formula (1) was calcined at 500°C for 8 hours to obtain a metal oxide containing Ni, Co, and Al. Next, lithium hydroxide monohydrate (LiOH·H) was added to the composite hydroxide represented by the formula (1) so that the molar ratio of Li to the total amount of Ni, Co, and Al was 1:1.03. 2 O) was mixed to obtain a mixture. Then, this mixture was placed under an oxygen flow (10 cm) with an oxygen concentration of 95%. 3 The mixture was heated from room temperature to 650°C at a heating rate of 2.0°C / min under a temperature of 2 mL / min per kg of the mixture and 5 L / min per kg of the mixture, and then fired. The mixture was heated from 650°C to 740°C at a heating rate of 0.5°C / min, and fired to obtain a lithium-containing transition metal composite oxide (synthesis step).

[0088] Water was added to the obtained lithium-containing transition metal composite oxide so that the slurry concentration was 1500 g / L, and the mixture was stirred for 15 minutes and filtered to obtain a cake-like composition (washing step). The obtained cake-like composition was then dried under vacuum at 180°C for 2 hours to obtain a powder-like composition (drying step). Powdered lithium methanesulfonate was then added to the obtained powder-like composition (addition step). The lithium methanesulfonate was added so that the content of lithium methanesulfonate was 0.5 mass% relative to the total mass of the lithium-containing transition metal composite oxide, thereby obtaining the positive electrode active material of Example 1. The presence of lithium methanesulfonate on the surface of the secondary particles of the lithium-containing transition metal composite oxide was confirmed by Fourier transform infrared spectroscopy (FT-IR).

[0089] [Preparation of Conductive Aid Dispersion] Carbon black (first carbon black) having an average diameter (average particle size) of 19 nm and an average aspect ratio of 1.7 was used as the conductive aid, and polyvinylpyrrolidone (PVP) was used as the dispersant. The conductive aid and dispersant were dry-blended in a mass ratio of 10:1 to obtain powder, which was then added to N-methyl-2-pyrrolidone (NMP) and dispersed using a ball mill, thereby obtaining a conductive aid dispersion containing 10 mass% of the first carbon black.

[0090] [Preparation of Positive Electrode] The lithium-containing transition metal composite oxide was used as the positive electrode active material. The positive electrode active material, the conductive additive dispersion, and polyvinylidene fluoride (PVDF) were mixed in a solid mass ratio of 100:1:1, excluding the dispersant, and a positive electrode mixture slurry was prepared using N-methyl-2-pyrrolidone (NMP) as a dispersion medium. Next, the positive electrode mixture slurry was applied to both sides of a positive electrode core made of aluminum foil in a weight ratio of 240 g / m. 2 After drying the coating, the coating was rolled using a roller and cut to a predetermined electrode size to obtain a positive electrode having a positive electrode mixture layer formed on both sides of the positive electrode core. An exposed portion was then provided in part of the positive electrode, exposing the surface of the positive electrode core. The composite resistance of the fabricated positive electrode was measured using an electrode resistance measurement system (RM2610, manufactured by Hioki E.E. Corporation).

[0091] [Preparation of Negative Electrode] Natural graphite and a silicon compound were used as the negative electrode active material. Natural graphite, a silicon compound, carboxymethyl cellulose sodium (CMC-Na), and a dispersion of styrene-butadiene rubber (SBR) were mixed in a solids mass ratio of 95:5:1:1, and a negative electrode mixture slurry was prepared using water as a dispersion medium. The negative electrode mixture slurry was applied to both sides of a negative electrode core made of copper foil, and the coating was dried. The coating was then rolled using a roller and cut to a predetermined electrode size to obtain a negative electrode in which a negative electrode mixture layer was formed on both sides of the negative electrode core. An exposed portion in which the surface of the negative electrode core was exposed was provided in a portion of the negative electrode.

[0092] [Preparation of non-aqueous electrolyte] Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) were mixed in a volume ratio of 3:3:4. Lithium hexafluorophosphate (LiPF 6 ) was dissolved in the solution to a concentration of 1.2 mol / L to prepare a non-aqueous electrolyte.

[0093] [Preparation of Test Cell (Non-Aqueous Electrolyte Secondary Battery)] An aluminum lead was attached to the exposed portion of the positive electrode, and a nickel lead was attached to the exposed portion of the negative electrode, and the positive and negative electrodes were spirally wound with a polyolefin separator interposed therebetween to prepare a wound electrode assembly. This electrode assembly was placed in a cylindrical outer can with a bottom, and the non-aqueous electrolyte solution was poured into it. The opening of the outer can was then sealed with a sealer to obtain a test cell.

[0094] [Evaluation of Output Characteristics] The test cell was charged to 4.2 V at a constant current of 0.2 C in a temperature environment of 25°C, and then constant-voltage charged at 4.2 V until the current value reached 0.01 C. After a 1-hour rest, the test cell was discharged to 2.5 V at a constant current of 0.2 C, forming an initial cycle. Next, the test cell was again charged at a constant current of 0.2 C until the battery voltage reached 4.2 V, and then constant-voltage charged at 4.2 V until the current value reached 0.01 C, after which the test cell was discharged at 1 C to 2.5 V. After a 10-minute rest, the test cell was further discharged at 0.02 C to 2.5 V, and the initial output was calculated using the following formula: Initial output = 1 C discharge capacity / (1 C discharge capacity + 0.02 C discharge capacity).

[0095] [Evaluation of cycle characteristics during high-rate charging] The test cell was charged to 4.2 V at a constant current of 1 C in a temperature environment of 25°C, and then charged at a constant voltage of 4.2 V until the current value reached 0.01 C. After a 1-hour rest, the cell was discharged to 2.5 V at a constant current of 1 C, which constituted one cycle. The discharge capacity at 1 C after 200 cycles was measured. The capacity retention rate during high-rate charging was calculated using the following formula: Capacity retention rate = Discharge capacity at 1 C at 200th cycle / Discharge capacity at 1 C at 1st cycle

[0096] Example 2 In preparing the conductive additive dispersion, a carbon black having an average diameter (average fiber diameter) of 12 nm, an average fiber length of 1 μm, an average aspect ratio of 83, and a BET specific surface area of ​​220 m was used as the conductive additive for the positive electrode instead of the first carbon black. 2 A test cell was prepared in the same manner as in Example 1, except that multi-walled carbon nanotubes (first carbon nanotubes) having a solid content of 0.5 mass% relative to the total mass of the positive electrode active material were used.

[0097] Example 3 A test cell was produced in the same manner as in Example 1, except that in preparing the conductive additive dispersion, a conductive additive obtained by mixing the first carbon nanotubes and graphene in a mass ratio of 1:1 was used as the conductive additive for the positive electrode instead of the first carbon black, and the solid content of the first carbon nanotubes and graphene was 0.5 mass% with respect to the total mass of the positive electrode active material. The graphene had an average thickness of 50 nm and a size in the plane direction of 1 μm.

[0098] Example 4 A test cell was produced in the same manner as in Example 1, except that in preparing the conductive additive dispersion, hydrogenated nitrile rubber (H-NBR), which was a copolymer of acrylonitrile and butadiene with hydrogen substitution, was used instead of polyvinylpyrrolidone (PVP) as the dispersant.

[0099] Example 5 A test cell was produced in the same manner as in Example 2, except that in preparing the conductive additive dispersion, hydrogenated nitrile rubber (H-NBR), which was a copolymer of acrylonitrile and butadiene substituted with hydrogen, was used instead of polyvinylpyrrolidone (PVP) as the dispersant.

[0100] Example 6 A test cell was produced in the same manner as in Example 2, except that in preparing the conductive additive dispersion, nitrile-butadiene rubber (NBR) was used as the dispersant instead of polyvinylpyrrolidone (PVP).

[0101] Example 7 A test cell was produced in the same manner as in Example 2, except that in preparing the conductive additive dispersion, the solid content of the first carbon nanotubes was set to 1.2 mass% with respect to the total mass of the positive electrode active material, and hydrogenated nitrile rubber (H-NBR) obtained by hydrogen-substitution of a copolymer of acrylonitrile and butadiene was used instead of polyvinylpyrrolidone (PVP) as the dispersant.

[0102] Example 8 In preparing the conductive additive dispersion, hydrogenated nitrile rubber (H-NBR) obtained by hydrogen-substitution of a copolymer of acrylonitrile and butadiene was used instead of polyvinylpyrrolidone (PVP) as a dispersant. 2A test cell was prepared in the same manner as in Example 1, except that the coating was performed so that the thickness of the test cell was 100 μm.

[0103] Example 9 In preparing the conductive additive dispersion, hydrogenated nitrile rubber (H-NBR) obtained by hydrogen-substitution of a copolymer of acrylonitrile and butadiene was used instead of polyvinylpyrrolidone (PVP) as a dispersant. 2 A test cell was prepared in the same manner as in Example 2, except that the coating was performed so that the thickness of the test cell was 100 μm.

[0104] Example 10 In preparing the conductive additive dispersion, a conductive additive having an average diameter (average fiber diameter) of 2 nm, an average fiber length of 1 μm, an average aspect ratio of 500, and a BET specific surface area of ​​800 m was used instead of the first carbon black as the conductive additive for the positive electrode. 2 A test cell was prepared in the same manner as in Example 4, except that single-walled carbon nanotubes (second carbon nanotubes) having a mass of 0.1 mass % relative to the total mass of the positive electrode active material were used, the solid content of the second carbon nanotubes was set to 0.1 mass %, and the solid content of the dispersant was set to 0.4 mass %, relative to the total mass of the positive electrode active material.

[0105] Example 11 A test cell was produced in the same manner as in Example 4, except that in preparing the conductive additive dispersion, a conductive additive obtained by mixing first carbon nanotubes, which are multi-walled carbon nanotubes, and second carbon nanotubes, which are single-walled carbon nanotubes, in a mass ratio of 95:5 was used as the conductive additive for the positive electrode instead of the first carbon black, and the solid content of the first carbon nanotubes and the second carbon nanotubes was 0.4 mass% relative to the total mass of the positive electrode active material. The average diameter (average fiber diameter) of the conductive additive was 12 nm.

[0106] Comparative Example 1 A test cell was produced in the same manner as in Example 1, except that the addition step was not performed in the production of the positive electrode active material, and that carbon black having an average diameter (average particle size) of 30 nm and an average aspect ratio of 1.5 (second carbon black) was used as the conductive additive for the positive electrode instead of the first carbon black in the preparation of the conductive additive dispersion.

[0107] Comparative Example 2 A test cell was produced in the same manner as in Example 1, except that in preparing the conductive additive dispersion, the second carbon black was used instead of the first carbon black as the conductive additive for the positive electrode.

[0108] <Comparative Example 3> In the preparation of the conductive additive dispersion, the second carbon black was used instead of the first carbon black as the conductive additive for the positive electrode, and the positive electrode was fabricated with a basis weight of 270 g / m 2 A test cell was prepared in the same manner as in Example 1, except that the coating was performed so that the thickness of the test cell was 100 μm.

[0109] Comparative Example 4 A test cell was prepared in the same manner as in Example 1, except that the addition step was not carried out in the preparation of the positive electrode active material.

[0110] The mix resistance, initial output, and capacity retention rate of the test cells of Examples 1 to 11 and Comparative Examples 1 to 4 are shown in Table 1. The mix resistance, initial output, and capacity retention rate of the test cells of Examples 1 to 11 and Comparative Examples 1 to 4 shown in Table 1 are expressed relative to the mix resistance, initial output, and capacity retention rate of the test cell of Comparative Example 1, which is set to 100. A smaller mix resistance value indicates lower resistance, a larger initial output value indicates better output characteristics, and a larger capacity retention rate value indicates better cycle characteristics during high-rate charging.

[0111]

[0112] As shown in Table 1, the test cells of the examples have improved initial output and capacity retention rates compared to the test cells of the comparative examples. In other words, by having a sulfonic acid compound present on the particle surfaces of the lithium-containing transition metal composite oxide and using a conductive additive containing at least one selected from the group consisting of carbon nanotubes and carbon black having an average diameter of 20 nm or less and graphene having an average thickness of 50 nm or less, it is possible to improve the output characteristics and cycle characteristics during high-rate charging.

[0113] Furthermore, the test cell of Comparative Example 2, in which a sulfonic acid compound was present on the particle surfaces but carbon black having an average diameter of more than 20 nm was used as the conductive additive, had an improved initial output but no improved capacity retention rate compared to the test cell of Comparative Example 1. This is presumably because lithium-containing transition metal composite oxides having a sulfonic acid compound present on the particle surfaces have low electronic conductivity, and therefore, when carbon black having an average diameter of more than 20 nm is used as the conductive additive, the formation of conductive paths in the positive electrode mixture layer becomes insufficient.

[0114] Furthermore, the test cell of Example 4, which used carbon black having an average diameter of 20 nm or less as the conductive additive and H-NBR as the dispersant, showed a significantly improved capacity retention rate compared to the test cell of Example 1, which used PVP as the dispersant. This is presumably because the use of H-NBR as the dispersant allows the conductive additive to be dispersed more uniformly, thereby further improving the conductivity of the positive electrode mixture layer even when a sulfonic acid compound is present on the particle surface.

[0115] The present disclosure will be further described by the following embodiments. Configuration 1: A positive electrode for a non-aqueous electrolyte secondary battery, having a positive electrode core and a positive electrode mixture layer formed on the surface of the positive electrode core, the positive electrode mixture layer including a positive electrode active material and a conductive additive, the positive electrode active material including a lithium-containing transition metal composite oxide having a layered structure and a sulfonic acid compound present on particle surfaces of the lithium-containing transition metal composite oxide, the sulfonic acid compound being a compound represented by formula (I), and the conductive additive including at least one selected from the group consisting of carbon nanotubes and carbon black having an average diameter of 20 nm or less, and graphene having an average thickness of 50 nm or less. (wherein A is a Group 1 or Group 2 element, R is a hydrocarbon group, and n is 1 or 2.) Configuration 2: The positive electrode for a non-aqueous electrolyte secondary battery according to Configuration 1, wherein the lithium-containing transition metal composite oxide contains 50 mol % or more of Ni, relative to the total number of moles of metal elements excluding Li, and one or more elements selected from the group consisting of Co, Mn, and Al. Configuration 3: The positive electrode for a non-aqueous electrolyte secondary battery according to Configuration 1 or 2, further comprising a nitrile group-containing rubber as a dispersant for the conductive additive. Configuration 4: The positive electrode for a non-aqueous electrolyte secondary battery according to any one of Configurations 1 to 3, wherein the content of the conductive additive is 0.01 mass % or more and 2 mass % or less, relative to the total mass of the positive electrode active material. Configuration 5: The positive electrode for a non-aqueous electrolyte secondary battery according to any one of Configurations 1 to 4, wherein the carbon nanotubes are single-walled carbon nanotubes. Configuration 6: The positive electrode mixture layer has a basis weight of 250 g / m 2 The positive electrode for a non-aqueous electrolyte secondary battery according to any one of Configurations 1 to 5. Configuration 7: A non-aqueous electrolyte secondary battery comprising the positive electrode according to any one of Configurations 1 to 6, a negative electrode, and a non-aqueous electrolyte.

[0116] REFERENCE SIGNS LIST 10 nonaqueous electrolyte secondary battery, 11 positive electrode, 12 negative electrode, 13 separator, 14 electrode body, 16 exterior body, 17 sealing body, 18, 19 insulating plate, 20 positive electrode lead, 21 negative electrode lead, 22 grooved portion, 23 internal terminal plate, 24 lower valve body, 25 insulating member, 26 upper valve body, 27 cap, 28 gasket, 30 positive electrode core, 31 positive electrode mixture layer, 40 negative electrode core, 41 negative electrode mixture layer.

Claims

1. A positive electrode for a non-aqueous electrolyte secondary battery having a positive electrode core and a positive electrode mixture layer formed on a surface of the positive electrode core, wherein the positive electrode mixture layer includes a positive electrode active material and a conductive assistant, the positive electrode active material includes a lithium-containing transition metal composite oxide having a layered structure and a sulfonic acid compound present on particle surfaces of the lithium-containing transition metal composite oxide, the sulfonic acid compound is a compound represented by formula (I), and the conductive assistant includes at least one selected from the group consisting of carbon nanotubes and carbon black having an average diameter of 20 nm or less, and graphene having an average thickness of 50 nm or less. (In the formula, A is a Group 1 or Group 2 element, R is a hydrocarbon group, and n is 1 or 2.) 2. The positive electrode for a non-aqueous electrolyte secondary battery according to claim 1, wherein the lithium-containing transition metal composite oxide contains 50 mol % or more of Ni, and one or more elements selected from the group consisting of Co, Mn and Al, relative to the total number of moles of metal elements excluding Li.

3. The positive electrode for a non-aqueous electrolyte secondary battery according to claim 1, further comprising a nitrile group-containing rubber as a dispersant for the conductive assistant.

4. The positive electrode for a non-aqueous electrolyte secondary battery according to claim 1, wherein the content of the conductive assistant is 0.01 mass % or more and 2 mass % or less with respect to the total mass of the positive electrode active material.

5. The positive electrode for a non-aqueous electrolyte secondary battery according to claim 1, wherein the carbon nanotubes are single-walled carbon nanotubes.

6. The weight of the positive electrode mixture layer is 250 g / m 2 The positive electrode for a non-aqueous electrolyte secondary battery according to claim 1 .

7. A non-aqueous electrolyte secondary battery comprising the positive electrode according to any one of claims 1 to 6, a negative electrode, and a non-aqueous electrolyte.

Citation Information

Patent Citations

  • Positive electrode active material for lithium ion secondary battery, and lithium ion secondary battery

    JP2019169286A

  • Lithium ion secondary battery

    JP2016134218A

  • Non-aqueous electrolyte secondary battery

    WO2015146857A1

  • Secondary battery, battery pack, electric vehicle, electric tool and electronic device

    WO2018146865A1

Cited By

  • Conductive material dispersion, positive electrode manufactured using the same, and rechargeable lithium battery including the positive electrode

    EP4807808A1