Positive electrode for nonaqueous electrolyte secondary battery, and nonaqueous electrolyte secondary battery

The positive electrode for non-aqueous electrolyte secondary batteries, featuring a lithium-containing transition metal composite oxide with a sulfonic acid compound and a layered structure, addresses the challenge of low-temperature output characteristics by optimizing sulfonic acid compound distribution, resulting in improved reaction resistance and battery performance.

WO2024247683A1PCT designated stage expired Publication Date: 2024-12-05PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/017592
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-30
Filing Date
2024-05-13
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Existing non-aqueous electrolyte secondary batteries face challenges in improving output characteristics at low temperatures, as existing technologies like those described in Patent Document 1 are insufficient in addressing reaction resistance and diffusivity issues.

Method used

A positive electrode for non-aqueous electrolyte secondary batteries is designed with a lithium-containing transition metal composite oxide having a sulfonic acid compound represented by formula (I) on its surface, where the positive electrode mixture layer is divided into two parts, with a higher content of sulfonic acid compound in the surface region compared to the core region, optimizing the distribution to reduce reaction resistance and enhance output characteristics.

Benefits of technology

This configuration enhances the output characteristics at low temperatures by reducing reaction resistance on the surface of the positive electrode, while maintaining adequate conductivity, thereby improving the battery's performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024017592_05122024_PF_FP_ABST
    Figure JP2024017592_05122024_PF_FP_ABST
Patent Text Reader

Abstract

A positive electrode (11) for a nonaqueous electrolyte secondary battery according to one embodiment of the present disclosure has a positive electrode core body (30), and a positive electrode mixture layer (31) formed on the surface of the positive electrode core body, the positive electrode being characterized in that: the positive electrode mixture layer (31) includes a lithium-containing transition metal composite oxide as a positive electrode active material; a sulfonic acid compound represented by formula (I) is present on the particle surface of the lithium-containing transition metal composite oxide; and when the positive electrode mixture layer (31) is divided into two equal parts in the thickness direction, a region on the positive electrode core body (30) side of the positive electrode mixture layer (31) is defined as a first region (31a), and a region on the front surface side of the positive electrode mixture layer (31) is defined as a second region (31b), the content of the sulfonic acid compound in the second region (31b) is greater than the content of the sulfonic acid compound in the first region (31a). (In the formula, A represents a Group 1 element or a Group 2 element, R represents a hydrocarbon group, and n is 1 or 2.)
Need to check novelty before this filing date? Find Prior Art

Description

Positive electrode for non-aqueous electrolyte secondary battery and non-aqueous electrolyte secondary battery

[0001] The present disclosure relates to a positive electrode for a non-aqueous electrolyte secondary battery and a non-aqueous electrolyte secondary battery using the positive electrode.

[0002] In recent years, the applications of non-aqueous electrolyte secondary batteries have expanded to include power sources for electric vehicles and power storage devices for utilizing natural energy. Since the positive electrode significantly affects battery characteristics, including battery capacity, output characteristics, and cycle characteristics, much research has been conducted on the positive electrode. For example, Patent Document 1 discloses a positive electrode for a non-aqueous electrolyte secondary battery that uses, as a positive electrode active material, a lithium-containing transition metal composite oxide having a low-solubility Li salt scattered on its surface, with the aim of reducing reaction resistance during storage at high temperatures.

[0003] Japanese Patent Application Laid-Open No. 2019-169286

[0004] In non-aqueous electrolyte secondary batteries, improving output characteristics at low temperatures is an important issue. The technology described in Patent Document 1 does not adequately address this issue, and there is still much room for improvement.

[0005] A positive electrode for a non-aqueous electrolyte secondary battery according to one aspect of the present disclosure is a positive electrode for a non-aqueous electrolyte secondary battery having a positive electrode core and a positive electrode mixture layer formed on the surface of the positive electrode core, wherein the positive electrode mixture layer contains a lithium-containing transition metal composite oxide as a positive electrode active material, and a sulfonic acid compound represented by formula (I) is present on the particle surfaces of the lithium-containing transition metal composite oxide, and wherein when the positive electrode mixture layer is divided into two equal parts in the thickness direction and the region of the positive electrode mixture layer on the positive electrode core side is defined as a first region and the region of the positive electrode mixture layer on the surface side is defined as a second region, the content of the sulfonic acid compound in the second region is higher than the content of the sulfonic acid compound in the first region. (In the formula, A is a Group 1 or Group 2 element, R is a hydrocarbon group, and n is 1 or 2.)

[0006] A non-aqueous electrolyte secondary battery according to one embodiment of the present disclosure includes the positive electrode, a negative electrode, and a non-aqueous electrolyte.

[0007] According to the positive electrode for a nonaqueous electrolyte secondary battery of one aspect of the present disclosure, it is possible to provide a nonaqueous electrolyte secondary battery with improved output characteristics at low temperatures.

[0008] 1 is a schematic diagram illustrating an axial cross section of a nonaqueous electrolyte secondary battery (cylindrical battery) according to an embodiment; 2 is a cross section of a positive electrode according to an embodiment;

[0009] As a result of investigations by the present inventors, it has become clear that the presence of the sulfonic acid compound represented by the above formula (I) on the particle surface of the lithium-containing transition metal composite oxide used as the positive electrode active material makes it easier for insertion and desorption of Li to occur, thereby reducing the reaction resistance in the positive electrode.

[0010] The researchers then divided the positive electrode mixture layer into two equal parts in the thickness direction, defining the region on the positive electrode substrate side as the first region and the region on the surface side as the second region. They found that increasing the sulfonic acid compound content in the second region compared to the sulfonic acid compound content in the first region improved output characteristics at low temperatures. At low temperatures, the diffusibility of the nonaqueous electrolyte decreases, making the reaction on the surface side of the positive electrode more prominent than the reaction on the substrate side of the positive electrode. Therefore, by increasing the sulfonic acid compound content on the surface side of the positive electrode, the reaction resistance on the surface side of the positive electrode can be further reduced, improving output characteristics at low temperatures. Note that increasing the sulfonic acid compound content throughout the positive electrode mixture layer increases the overall electronic resistance of the positive electrode, resulting in no improvement in output characteristics at low temperatures. Furthermore, decreasing the sulfonic acid compound content throughout the positive electrode mixture layer insufficiently reduces the positive electrode's reaction resistance, resulting in no improvement in output characteristics at low temperatures.

[0011] Hereinafter, with reference to the drawings, an example of an embodiment of a positive electrode for a nonaqueous electrolyte secondary battery according to the present disclosure and a nonaqueous electrolyte secondary battery using the positive electrode will be described in detail. Note that the scope of the present disclosure includes configurations obtained by selectively combining the respective components of the multiple embodiments and modifications described below.

[0012] In the following, a cylindrical battery in which a wound electrode assembly 14 is housed in a cylindrical, bottomed exterior body 16 is exemplified as a nonaqueous electrolyte secondary battery; however, the exterior body of the battery is not limited to a cylindrical exterior body. The nonaqueous electrolyte secondary battery according to the present disclosure may be, for example, a prismatic battery with a prismatic exterior body, a coin-type battery with a coin-type exterior body, or a pouch-type battery with an exterior body composed of a laminate sheet including a metal layer and a resin layer. Furthermore, the electrode assembly is not limited to a wound type, but may also be a stacked type electrode assembly in which multiple positive electrodes and multiple negative electrodes are alternately stacked with separators interposed therebetween. Furthermore, the design of the nonaqueous electrolyte secondary battery according to the present disclosure is not limited to the design of the exemplified nonaqueous electrolyte secondary battery, and known nonaqueous electrolyte secondary battery designs may also be applied.

[0013] FIG. 1 is an axial cross-sectional view of a cylindrical nonaqueous electrolyte secondary battery 10 according to an embodiment. As shown in FIG. 1 , the nonaqueous electrolyte secondary battery 10 includes a wound electrode assembly 14, a nonaqueous electrolyte, and an exterior body 16 that accommodates the electrode assembly 14 and the nonaqueous electrolyte. The electrode assembly 14 includes a positive electrode 11, a negative electrode 12, and a separator 13, and has a wound structure in which the positive electrode 11 and the negative electrode 12 are spirally wound with the separator 13 interposed therebetween. The exterior body 16 is a cylindrical metal container with a bottom that is open on one axial side, and the opening of the exterior body 16 is closed by a sealing body 17. Hereinafter, for convenience of explanation, the sealing body 17 side of the battery will be referred to as the top, and the bottom side of the exterior body 16 will be referred to as the bottom.

[0014] The positive electrode 11, negative electrode 12, and separator 13 that make up the electrode assembly 14 are all rectangular, elongated bodies that are spirally wound in the longitudinal direction and stacked alternately in the radial direction of the electrode assembly 14. The separator 13 isolates the positive electrode 11 and the negative electrode 12 from each other. Two separators 13 are arranged, for example, to sandwich the positive electrode 11. The electrode assembly 14 includes a positive electrode lead 20 connected to the positive electrode 11 by welding or the like, and a negative electrode lead 21 connected to the negative electrode 12 by welding or the like. In the electrode assembly 14, the longitudinal direction of the positive electrode 11 and the negative electrode 12 is the winding direction, and the lateral direction of the positive electrode 11 and the negative electrode 12 is the axial direction. That is, the lateral end faces of the positive electrode 11 and the negative electrode 12 form the axial end faces of the electrode assembly 14.

[0015] Insulating plates 18 and 19 are disposed above and below the electrode body 14. In the example shown in Fig. 1 , the positive electrode lead 20 passes through a through hole in the insulating plate 18 and extends toward the sealing body 17, and the negative electrode lead 21 passes outside the insulating plate 19 and extends toward the bottom side of the exterior body 16. The positive electrode lead 20 is connected to the underside of an internal terminal plate 23 of the sealing body 17 by welding or the like, and a cap 27, which is the top plate of the sealing body 17 and is electrically connected to the internal terminal plate 23, serves as the positive electrode terminal. The negative electrode lead 21 is connected to the inner bottom surface of the exterior body 16 by welding or the like, and the exterior body 16 serves as the negative electrode terminal.

[0016] A gasket 28 is provided between the exterior body 16 and the sealing body 17 to ensure airtightness inside the battery. The exterior body 16 has a grooved portion 22 formed on its side surface that protrudes inward and supports the sealing body 17. The grooved portion 22 is preferably formed in an annular shape along the circumferential direction of the exterior body 16, and supports the sealing body 17 on its top surface. The sealing body 17 is fixed to the top of the exterior body 16 by the grooved portion 22 and the open end of the exterior body 16 that is crimped to the sealing body 17.

[0017] The sealing body 17 has a structure in which, in order from the electrode body 14 side, an internal terminal plate 23, a lower valve body 24, an insulating member 25, an upper valve body 26, and a cap 27 are stacked. Each member constituting the sealing body 17 has, for example, a disk or ring shape, and each member except for the insulating member 25 is electrically connected to one another. The lower valve body 24 and the upper valve body 26 are connected at their respective centers, and the insulating member 25 is interposed between their respective peripheral edges. When the internal pressure of the battery increases due to abnormal heat generation, the lower valve body 24 deforms and breaks, pushing the upper valve body 26 toward the cap 27, thereby interrupting the current path between the lower valve body 24 and the upper valve body 26. When the internal pressure further increases, the upper valve body 26 breaks, and gas is discharged from the opening of the cap 27.

[0018] 2, the positive electrode 11, the negative electrode 12, the separator 13, and the nonaqueous electrolyte that constitute the nonaqueous electrolyte secondary battery 10 will be described in detail below, particularly the positive electrode 11. FIG. 2 is a schematic diagram illustrating a cross section of the positive electrode 11.

[0019] [Positive Electrode] As shown in FIGS. 1 and 2 , the positive electrode 11 has a positive electrode core 30 and a positive electrode mixture layer 31 formed on the surface of the positive electrode core 30. The positive electrode mixture layer 31 is preferably formed on both sides of the positive electrode core 30. The positive electrode core 30 can be made of a foil of a metal, such as aluminum or an aluminum alloy, that is stable within the potential range of the positive electrode 11, or a film with such a metal disposed on the surface. The thickness of the positive electrode core 30 is, for example, 10 μm or more and 30 μm or less. The positive electrode mixture layer 31 includes, for example, a positive electrode active material, a conductive additive, and a binder. The positive electrode mixture layer 31 is preferably provided on both sides of the positive electrode core 30 except for the portion to which the positive electrode lead 20 is connected.

[0020] The weight of the positive electrode mixture layer 31 is, for example, 250 g / m 2 In this case, the effect of the present disclosure can be significantly exhibited while realizing a high capacity non-aqueous electrolyte secondary battery. From the viewpoint of increasing capacity, the basis weight of the positive electrode mixture layer 31 is set to 300 g / m 2 or more, and 2 The upper limit of the basis weight of the positive electrode mixture layer 31 is, for example, 600 g / m from the viewpoint of cycle characteristics. 2 Therefore, an example of a suitable range of the basis weight of the positive electrode mixture layer 31 is 250 g / m 2 Above, 600g / m 2 The thickness of the positive electrode mixture layer 31 is, for example, 10 μm or more and 200 μm or less on one side of the positive electrode substrate 30 .

[0021] The positive electrode 11 contains a lithium-containing transition metal composite oxide as a positive electrode active material. The lithium-containing transition metal composite oxide contains, for example, secondary particles formed by aggregation of primary particles. The particle size of the primary particles constituting the secondary particles of the lithium-containing transition metal composite oxide is, for example, 0.02 μm or more and 2 μm or less. The particle size of the primary particles is measured as the diameter of a circumscribed circle in a particle image observed with a scanning electron microscope (SEM). The average particle size of the secondary particles of the lithium-containing transition metal composite oxide is, for example, 2 μm or more and 30 μm or less. Here, the average particle size refers to the volume-based median diameter (D50). D50 refers to the particle size at which the cumulative frequency in the volume-based particle size distribution is 50% from the smallest particle size, and is also referred to as the median diameter. The particle size distribution of the secondary particles of the lithium-containing transition metal composite oxide can be measured using a laser diffraction particle size distribution analyzer (e.g., MT3000II, manufactured by Microtrac-Bell Corporation) using water as a dispersion medium.

[0022] The lithium-containing transition metal composite oxide has, for example, a layered structure. Examples of the layered structure of the lithium-containing transition metal composite oxide include a layered structure belonging to the space group R-3m and a layered structure belonging to the space group C2 / m. From the viewpoints of increasing capacity and stabilizing the crystal structure, the lithium-containing transition metal composite oxide preferably has a layered structure belonging to the space group R-3m. The layered structure of the lithium-containing transition metal composite oxide may include a transition metal layer and a Li layer.

[0023] The lithium-containing transition metal composite oxide contains, for example, 50 mol % or more of Ni and one or more elements selected from the group consisting of Co, Mn, and Al, based on the total number of moles of metal elements excluding Li.

[0024] The Ni content in the lithium-containing transition metal composite oxide is 50 mol% or more relative to the total number of moles of metal elements excluding Li. This allows for improved battery capacity. The Ni content may be 75 mol% or more, or may be 80 mol% or more, preferably 85 mol% or more, and more preferably 90 mol% or more. In addition, from the viewpoint of structural stabilization, the Ni content is preferably 99 mol% or less, more preferably 95 mol% or less.

[0025] The content of Co in the lithium-containing transition metal composite oxide is 0 mol % or more and 15 mol % or less relative to the total number of moles of metal elements excluding Li, and Co is an optional component. In other words, the lithium-containing transition metal composite oxide does not need to contain Co. By containing Co, the lithium-containing transition metal composite oxide can improve the heat resistance of the battery.

[0026] The content of Mn in the lithium-containing transition metal composite oxide is 0 mol % or more and 50 mol % or less relative to the total number of moles of metal elements excluding Li, and Mn is an optional component. In other words, the lithium-containing transition metal composite oxide does not need to contain Mn. By containing Mn, the lithium-containing transition metal composite oxide can stabilize its crystal structure.

[0027] The content of Al in the lithium-containing transition metal composite oxide is 0 mol % or more and 15 mol % or less with respect to the total number of moles of metal elements excluding Li, and Al is an optional component. In other words, the lithium-containing transition metal composite oxide does not necessarily contain Al.

[0028] The total content of Co, Mn, and Al in the lithium-containing transition metal composite oxide is, for example, 0 mol % or more and 50 mol % or less.

[0029] The lithium-containing transition metal composite oxide may further contain one or more elements selected from the group consisting of W, Mg, Mo, Nb, Ti, Si, Ca, Sr, and Zr. The contents of W, Mg, Mo, Nb, Ti, Si, Ca, Sr, and Zr in the lithium-containing transition metal composite oxide are each, for example, 0 mol % or more and 1 mol % or less, relative to the total number of moles of metal elements excluding Li. The total content of W, Mg, Mo, Nb, Ti, Si, Ca, Sr, and Zr is, for example, 0 mol % or more and 2 mol % or less.

[0030] The lithium-containing transition metal composite oxide is, for example, a compound represented by the general formula Li x Ni a M1 b M2 c O 2-y(wherein 0.8<x<1.2, 0.5≦a, 0≦b≦0.5, 0≦c≦0.02, 0≦y<0.05, a+b+c=1, M1 is one or more elements selected from the group consisting of Co, Mn, and Al, and M2 is one or more elements selected from the group consisting of W, Mg, Mo, Nb, Ti, Si, Ca, Sr, and Zr).

[0031] The content of elements constituting the lithium-containing transition metal composite oxide can be measured by an inductively coupled plasma atomic emission spectrometer (ICP-AES), an electron probe microanalyzer (EPMA), an energy dispersive X-ray analyzer (EDX), etc. The composition of the lithium-containing transition metal composite oxide may be the same or different between the first region 31a (see FIG. 2) and the second region 31b (see FIG. 2), which will be described later.

[0032] The sulfonic acid compound represented by formula (I) is present on the surface of the particles of the lithium-containing transition metal composite oxide. In the formula, A is a Group 1 or Group 2 element, R is a hydrocarbon group, and n is 1 or 2. A is preferably a Group 1 element. Among these, Li or Na is more preferred, and Li is particularly preferred. The sulfonic acid compound may be scattered so as to cover at least a portion of the surface of the secondary particles of the lithium-containing transition metal composite oxide, or may be present so as to cover the entire surface of the secondary particles. In addition, the sulfonic acid compound may be fixed to the surface of the primary particles of the lithium-containing transition metal composite oxide.

[0033] In formula (I), R is preferably an alkyl group. The number of carbon atoms in the alkyl group is preferably 5 or less, more preferably 3 or less. From the viewpoint of reducing reaction resistance, a suitable example of R is an alkyl group having 3 or less carbon atoms, and among these, a methyl group is preferred. In R, some of the hydrogen atoms bonded to the carbon may be substituted with fluorine. In formula (I), n is preferably 1.

[0034] Specific examples of the sulfonic acid compound include lithium methanesulfonate, lithium ethanesulfonate, lithium propanesulfonate, sodium methanesulfonate, sodium ethanesulfonate, magnesium methanesulfonate, lithium fluoromethanesulfonate, etc. Among these, at least one selected from the group consisting of lithium methanesulfonate, lithium ethanesulfonate, and sodium methanesulfonate is preferred, with lithium methanesulfonate being particularly preferred.

[0035] As shown in FIG. 2 , the positive electrode mixture layer 31 is divided into two equal parts in the thickness direction. The region of the positive electrode mixture layer 31 facing the positive electrode substrate 30 is defined as a first region 31a, and the region of the positive electrode mixture layer 31 facing the surface is defined as a second region 31b. The sulfonic acid compound content (Y) in the second region 31b is greater than the sulfonic acid compound content (X) in the first region 31a. In this case, the reaction resistance on the surface side of the positive electrode 11 can be further reduced, improving the battery output characteristics at low temperatures where the diffusibility of the nonaqueous electrolyte decreases. Furthermore, the presence of sulfonic acid compounds on the particle surfaces reduces the electronic conductivity of the lithium-containing transition metal composite oxide. Therefore, reducing the sulfonic acid compound content (X) in the first region 31a suppresses the decrease in the conductivity of the positive electrode mixture layer 31. As a result, the battery output characteristics at low temperatures can be improved.

[0036] The ratio (Y / X) of the sulfonic acid compound content (Y) in the second region 31b to the sulfonic acid compound content (X) in the first region 31a preferably satisfies 1 < (Y / X) ≦ 10, more preferably satisfies 1.5 ≦ (Y / X) ≦ 10, even more preferably satisfies 1.5 ≦ (Y / X) ≦ 8, and particularly preferably satisfies 2 ≦ (Y / X) ≦ 8. If (Y / X) is greater than 10, the conductivity of the positive electrode mixture layer 31 decreases, which may result in a decrease in the output characteristics of the battery at low temperatures.

[0037] The sulfonic acid compound content (X) in the first region 31a may be 0% by mass or more and 0.7% by mass or less, 0% by mass or more and 0.6% by mass or less, 0.1% by mass or more and 0.7% by mass or less, or 0.1% by mass or more and 0.6% by mass or less, relative to the total mass of the positive electrode active material in the first region 31a. Furthermore, the sulfonic acid compound content (X) in the first region 31a is preferably 0% by mass or more and 0.5% by mass or less, more preferably 0% by mass or more and 0.4% by mass or less, and even more preferably 0% by mass or more and 0.3% by mass or less, relative to the total mass of the positive electrode active material in the first region 31a. In other words, the first region 31a may not contain a sulfonic acid compound. The sulfonic acid compound content (Y) in the second region 31b may be 0.3 mass% or more and 2.5 mass% or less, 0.3 mass% or more and 2.3 mass% or less, 0.5 mass% or more and 2.5 mass% or less, or 0.5 mass% or more and 2.3 mass% or less, relative to the total mass of the positive electrode active material in the second region 31b. The sulfonic acid compound content (Y) in the second region 31b is preferably 0.3 mass% or more and 2.0 mass% or less, more preferably 0.5 mass% or more and 2.0 mass% or less, even more preferably 0.3 mass% or more and 1.5 mass% or less, and particularly preferably 0.5 mass% or more and 1.5 mass% or less. The sulfonic acid compound content (X) in the first region 31a and the sulfonic acid compound content (Y) in the second region 31b can be selectively combined within the ranges described above.

[0038] The presence of the sulfonic acid compound on the particle surface of the lithium-containing transition metal composite oxide can be confirmed by Fourier transform infrared spectroscopy (FT-IR). In the infrared absorption spectrum obtained by FT-IR, the positive electrode active material containing lithium methanesulfonate exhibits, for example, a peak at 1238 cm -1 , 1175 cm -1 , 1065 cm -1 , 785 cm -1 It has an absorption peak around 1238 cm -1, 1175 cm -1 , 1065 cm -1 The peak around 785 cm is due to the SO stretching vibration of lithium methanesulfonate. -1 The peak around 1000 nm is a peak due to the C-S stretching vibration derived from lithium methanesulfonate. In addition, the presence of a positive electrode active material containing a sulfonic acid compound other than lithium methanesulfonate can also be confirmed from the absorption peak derived from the sulfonic acid compound in the infrared absorption spectrum.

[0039] The presence of the sulfonic acid compound can also be confirmed by X-ray photoelectron spectroscopy (XPS). In the spectrum obtained by XPS, a peak with an intensity (c / s) of 200 or more and 1000 or less is observed in the positive electrode active material containing lithium methanesulfonate, where the binding energy is approximately 165 or more and 170 eV or less. The presence of the sulfonic acid compound on the particle surface of the lithium-containing transition metal composite oxide can also be confirmed by ICP, atomic absorption spectroscopy, synchrotron XRD measurement, TOF-SIMS, H-NMR, etc.

[0040] The content of sulfonic acid compounds can be quantified by quantitatively analyzing the sulfur element (S) and the transition metal element using, for example, an ICP atomic emission spectrometer (ICP-AES) and converting the ratio between them.

[0041] In addition to the sulfonic acid compound, a metal compound may be present on the surface of the secondary particles of the lithium-containing transition metal composite oxide. The metal compound contains, for example, one or more metal elements selected from the group consisting of Sr, Ca, W, Zr, rare earth elements, and Al. Examples of the Sr-containing compound include SrO, Sr(OH), and the like. 2 and SrCO 3 Examples of compounds containing Ca include CaO and Ca(OH). 2 and CaCO 3 Examples of compounds containing W include WO 3 Examples of the compound containing Al include Al 2 O 3 Examples of compounds containing Zr include ZrO 2 , Zr(OH)4 , Zr(CO 3 ) 2 and Zr(SO 4 ) 2 ・4H 2 Examples of rare earth-containing compounds include oxides, hydroxides, carbonates, sulfates, nitrates, and phosphates of rare earth elements. The metal compound may contain a plurality of types of these metal elements, and examples thereof include SrAlO 4 , CaAlO 4 The metal compound may further contain Li, and an example thereof is lithium tungstate.

[0042] A nonmetallic compound may be present on the surface of the lithium-containing transition metal composite oxide. The nonmetallic compound contains, for example, one or more nonmetallic elements selected from the group consisting of P and B. Examples of the P-containing compound include Li, 3-x H x P.O. 4 (0≦x≦3) can be exemplified. 3 BO 3 , Li 3 BO 3 , Li 2 B 4 O 7 Examples include:

[0043] The positive electrode active material, which is one example of the embodiment, can be produced by the following method: Note that the production method described here is only an example, and the method for producing the positive electrode active material is not limited to this method.

[0044] The manufacturing process of the positive electrode active material includes a synthesis step of obtaining a lithium-containing transition metal composite oxide, a washing step of washing the fired product with water and dehydrating it to obtain a cake-like composition, a drying step of drying the cake-like composition to obtain a powder-like composition, and an addition step of adding at least one of a sulfonic acid compound and a sulfonic acid solution to the cake-like composition or the powder-like composition.

[0045] In the synthesis step, for example, a metal oxide containing 50 mol% or more of Ni, 0 mol% or more and 15 mol% or less of Co, 0 mol% or more and 50 mol% or less of Mn, 0 mol% or more and 15 mol% or less of Al, and 0 mol% or more and 2 mol% or less of M2 (M2 is one or more elements selected from W, Mg, Mo, Nb, Ti, Si, Ca, Sr, and Zr) is mixed with a Li compound to obtain a mixture.

[0046] The metal oxide can be obtained, for example, by adding an alkaline solution such as sodium hydroxide dropwise to a stirred solution of a metal salt containing Ni and an arbitrary metal element (Co, Mn, Al, M, etc.) to adjust the pH to the alkaline side (e.g., 8.5 or more and 12.5 or less), thereby precipitating (co-precipitating) a composite hydroxide containing Ni and the arbitrary metal element, and then heat-treating the composite hydroxide. The heat-treatment temperature is not particularly limited, but is, for example, in the range of 250°C or more and 600°C or less.

[0047] Examples of Li compounds include Li 2 CO 3 , LiOH, Li 2 O 2 , Li 2 O, LiNO 3 , LiNO 2 , Li 2 SO 4 , LiOH·H 2 Examples of the metal oxide include O, LiH, and LiF. In order to easily adjust each of the above parameters to the ranges specified above, the mixing ratio of the metal oxide and the Li compound is preferably such that the molar ratio of the total amount of metal elements in the metal oxide to Li is in the range of 1:0.8 or more and 1:1.2 or less, and more preferably 1:1.0 or more and 1:1.1 or less.

[0048] Next, the synthesis step includes a calcination step in which the resulting mixture is calcined. The calcination step is a multi-stage calcination step that includes at least a first calcination step in which the mixture is calcined at 300°C or higher and 680°C or lower under an oxygen stream, and a second calcination step in which the calcined product obtained by the first calcination step is calcined at a temperature exceeding 680°C under an oxygen stream. In the first calcination step, the temperature is increased to a first set temperature of 680°C or lower at a first temperature increase rate of 0.2°C / min or higher and 4.5°C / min or lower. In the second calcination step, the temperature is increased to a second set temperature of 900°C or lower at a first temperature increase rate of 0.5°C / min or higher and 3.5°C / min or lower. Note that multiple first and second temperature increase rates may be set for each temperature range as long as they are within the above-specified range.

[0049] The holding time of the first set temperature in the first firing step is preferably 5 hours or less, more preferably 3 hours or less. The holding time of the first set temperature is the time during which the first set temperature is maintained after reaching the first set temperature, and the holding time may be zero. The holding time of the second set temperature in the second firing step is preferably 1 hour or more and 10 hours or less, more preferably 1 hour or more and 5 hours or less. The holding time of the second set temperature is the time during which the second set temperature is maintained after reaching the second set temperature. The firing of the mixture is carried out, for example, in an oxygen stream with an oxygen concentration of 60% or more, and the flow rate of the oxygen stream is set to 10 cm / s. 3 The flow rate shall be 0.2 mL / min or more and 4 mL / min or less per kg of the mixture, or 0.3 L / min or more per kg of the mixture.

[0050] In the washing step, the lithium-containing transition metal composite oxide is washed with water and dehydrated to obtain a cake-like composition. The particulate lithium-containing transition metal composite oxide obtained in the synthesis step can be used. By washing with water, unreacted lithium compounds added in the synthesis step and impurities other than the lithium compounds can be removed. When washing with water, for example, 300 g or more and 5000 g or less of lithium-containing transition metal composite oxide is added to 1 L of water. The water washing may be repeated multiple times. The dehydration after washing with water can be performed, for example, using a filter press.

[0051] In the drying step, the cake-like composition obtained in the washing step is dried to obtain a powdery composition. The drying step may be performed under a vacuum atmosphere. The drying conditions are, for example, 150°C or higher and 400°C or lower for 0.5 hours or longer and 15 hours or shorter.

[0052] In the adding step, at least one of a sulfonic acid compound and a sulfonic acid solution is added to the cake-like composition obtained in the washing step or the powder-like composition obtained in the drying step. This allows the sulfonic acid compound to adhere to the surface of the lithium-containing transition metal composite oxide. It is preferable to add at least one of a sulfonic acid compound and a sulfonic acid solution to the cake-like composition. The sulfonic acid compound to be added may be in the form of either a powder or a solution. The sulfonic acid solution is, for example, a methanesulfonic acid solution obtained by dissolving methanesulfonic acid in water. Li compounds remain in the cake-like composition, and these remaining Li compounds are dissolved in the water contained in the cake-like composition. Therefore, even when a sulfonic acid solution is added, a sulfonic acid compound containing Li is formed. To more easily achieve the effects of the present invention, a Li compound or a Li compound solution may be added to the cake-like composition or the powder-like composition together with the sulfonic acid solution, or a mixed solution of the sulfonic acid solution and the Li compound or the Li compound solution may be added to the cake-like composition or the powder-like composition in advance. The Li compound is, for example, LiOH, and the Li compound solution is, for example, a LiOH solution obtained by dissolving LiOH in water. The amounts of the Li compound and the sulfonic acid solution added to the cake-like composition preferably satisfy the relationship of 0≦Li compound / sulfonic acid≦1.3 in molar ratio. The concentrations of the sulfonic acid solution and the sulfonic acid compound solution are, for example, 0.5% by mass or more and 40% by mass or less. The addition step may be performed during or after the washing step, during or after the drying step, and the timing of the addition can be changed as appropriate.

[0053] A metal compound containing one or more metal elements selected from the group consisting of Sr, Ca, W, Zr, rare earth elements, and Al, and a nonmetallic compound containing one or more nonmetallic elements selected from the group consisting of P and B can be attached to the surface of the lithium-containing transition metal composite oxide by adding the raw material of the metal compound or nonmetallic compound during the synthesis process, after the synthesis process, during the cleaning process, after the cleaning process, during the drying process, after the drying process, or during the addition process. 2 , Sr(OH) 2 ・8H 2 O, SrO, SrCo 3 , SrSO 4 , Sr(NO 3 ) 2、 SrCl 2 , SrAlO 4 Examples of Ca raw materials include Ca(OH) 2 , CaO, CaCO 3 , CaSO 4 , Ca(NO 3 ) 2、 CaCl 2 , CaAlO 4 The Zr raw material is Zr(OH) 4 , ZrO 2 , Zr(CO 3 ) 2 , Zr(SO 4 ) 2 ・4H 2 Examples of rare earth raw materials include oxides, hydroxides, and carbonates of rare earth elements. Examples of W raw materials include tungsten oxide (WO 3 ), lithium tungstate (Li 2 WO 4 , Li 4 WO 5 , Li 6 W 2 O 9 As the W raw material, a solution containing W may be used. As the Al raw material, Al 2 O 3、 Al(OH) 3、 Al 2 (SO 4 ) 3The P raw material may be Al derived from a lithium-containing transition metal composite oxide. 3-x H x P.O. 4 (0≦x≦3) and the like. 3 BO 3 , Li 3 BO 3 , Li 2 B 4 O 7 These compounds may be pulverized to appropriately change the particle shape or particle size, or may be used as hydrates with the water content adjusted.

[0054] The positive electrode mixture layer 31 contains, for example, a conductive additive. Examples of the conductive additive contained in the positive electrode mixture layer 31 include carbon black (CB) such as furnace black (FB), acetylene black (AB), and ketjen black (KB), and carbon-based particles such as graphite. These may be used alone or in combination of two or more. The content of the conductive additive is, for example, 0.01% by mass or more and 10% by mass or less, and preferably 0.05% by mass or more and 5% by mass or less, relative to the total mass of the positive electrode active material.

[0055] The positive electrode mixture layer 31 also contains, for example, a binder. Examples of binders contained in the positive electrode mixture layer 31 include fluorine-containing polymers such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVDF), polyacrylonitrile (PAN), polyimide, acrylic resin, and polyolefin. Among these, it is preferable that the binder contains a fluorine-containing polymer. In this case, the effect of reducing the reaction resistance due to the sulfonic acid compound is significantly exhibited. Furthermore, the binder may be a combination of the above resins with carboxymethyl cellulose (CMC) or a salt thereof, polyethylene oxide (PEO), or the like.

[0056] When the binder contains a fluorine-containing polymer, the weight-average molecular weight of the fluorine-containing polymer is preferably 1,000,000 or more. In this case, even if the binder content is reduced, a positive electrode mixture layer 31 having good binding properties can be produced. The upper limit of the weight-average molecular weight of the fluorine-containing polymer is, for example, 5,000,000.

[0057] Here, the binder content in the second region 31b is preferably smaller than the binder content in the first region 31a. In this case, the reaction resistance on the surface side of the positive electrode 11 can be further reduced, and the output characteristics of the battery are further improved at low temperatures when the diffusibility of the non-aqueous electrolyte is reduced. Furthermore, by increasing the binder content in the first region 31a, the amount of binder in the positive electrode mixture layer 31 is ensured, and peeling of the positive electrode mixture layer 31 is suppressed. In other words, if the binder content is reduced throughout the positive electrode mixture layer 31, peeling of the positive electrode mixture layer 31 becomes more likely to occur.

[0058] The ratio of the binder content in the second region 31b to the binder content in the first region 31a is, for example, 0.2 to 1, and preferably 0.4 to 0.9. In this case, peeling of the positive electrode mixture layer 31 can be suppressed, and the output characteristics of the battery can be further improved.

[0059] The binder content in the first region 31 a is, for example, 0.1 to 10% by mass, and preferably 0.5 to 8% by mass, relative to the total mass of the positive electrode active material in the first region 31 a. The binder content in the second region 31 b is, for example, 0.1 to 5% by mass, and preferably 0.2 to 2% by mass, relative to the total mass of the positive electrode active material in the second region 31 b.

[0060] The positive electrode 11 can be produced by applying a positive electrode mixture slurry containing a positive electrode active material, a conductive additive, a binder, and the like onto the positive electrode core 30, drying the coating, and then compressing it to form positive electrode mixture layers 31 on both sides of the positive electrode core 30. The positive electrode mixture slurry may include multiple types of slurries each containing a positive electrode active material with a different sulfonic acid compound content, or multiple types of slurries each containing a different sulfonic acid compound content and having different blend ratios of the multiple positive electrode active materials. When multiple types of slurries each containing a different sulfonic acid compound content are used, the positive electrode mixture slurry may include, for example, a first positive electrode mixture slurry containing a first positive electrode active material in which a sulfonic acid compound is present on the particle surfaces of a lithium-containing transition metal composite oxide, and a second positive electrode mixture slurry containing a second positive electrode active material having a higher sulfonic acid compound content than the first positive electrode active material. Then, after the first positive electrode mixture slurry is applied onto the positive electrode core 30, the second positive electrode mixture slurry is applied onto the coating film. In this way, a two-layer structure positive electrode mixture layer 31 including a first positive electrode mixture layer formed from the first positive electrode mixture slurry and a second positive electrode mixture layer formed from the second positive electrode mixture slurry can be formed, but any method may be used for formation as long as it is possible to control the content rates of the sulfonic acid compound in the first region and the second region. In addition, when multiple types of slurries are used that contain multiple types of positive electrode active materials that differ in content of sulfonic acid compound and that have different blending ratios of the multiple types of positive electrode active materials, for example, a 1a positive electrode mixture slurry that contains a first positive electrode active material and a second positive electrode active material and in which the content of the first positive electrode active material is greater than the content of the second positive electrode active material, and a 2a positive electrode mixture slurry that contains the first positive electrode active material and the second positive electrode active material and in which the content of the second positive electrode active material is greater than the content of the first positive electrode active material are used. When the first region and the second region are formed as a first positive electrode mixture layer and a second positive electrode mixture layer, which are different layers, respectively, the ratio (T2 / T1) of the thickness (T2) of the second positive electrode mixture layer on the surface side of the positive electrode mixture layer 31 to the thickness (T1) of the first positive electrode mixture layer on the positive electrode core 30 side of the positive electrode mixture layer 31 is, for example, 0.1 or more and 10 or less, and preferably 0.2 or more and 5 or less. The number of types of positive electrode mixture layer slurries is not limited to two, and may be three or more.In other words, the positive electrode mixture layer 31 may have a multi-layer structure made up of three or more layers.

[0061] [Negative Electrode] The negative electrode 12 may have, for example, a negative electrode core and a negative electrode mixture layer formed on the surface of the negative electrode core, or a metal Li foil may be used as the negative electrode 12. Alternatively, the negative electrode 12 may have a negative electrode core, and lithium metal may be deposited on the surface of the negative electrode core upon charging. When the negative electrode 12 has a negative electrode mixture layer, the negative electrode mixture layer is preferably formed on both sides of the negative electrode core. The negative electrode core may be made of a foil of a metal that is stable within the potential range of the negative electrode 12, such as copper or a copper alloy, or a film with such a metal disposed on the surface. The thickness of the negative electrode core is, for example, 5 μm or more and 30 μm or less.

[0062] The negative electrode mixture layer contains, for example, a negative electrode active material and a binder. The thickness of the negative electrode mixture layer is, for example, 10 μm or more and 150 μm or less on one side of the negative electrode core. The negative electrode 12 can be produced, for example, by applying a negative electrode mixture slurry containing a negative electrode active material, a binder, etc. to the surface of the negative electrode core, drying the coating, and then rolling it to form a negative electrode mixture layer on both sides of the negative electrode core.

[0063] The negative electrode active material contained in the negative electrode mixture layer is not particularly limited as long as it can reversibly absorb and release lithium ions, and generally, carbon materials such as graphite are used. Graphite may be any of natural graphite such as flake graphite, lump graphite, and amorphous graphite, or artificial graphite such as lump artificial graphite and graphitized mesophase carbon microbeads. Furthermore, metals that alloy with Li, such as Si and Sn, metal compounds containing Si, Sn, and lithium-titanium composite oxides may also be used as the negative electrode active material. Furthermore, those provided with a carbon coating may also be used. For example, SiO x (0.5≦x≦1.6) or Li 2y SiO (2+y) A Si-containing compound in which fine particles of Si are dispersed in a lithium silicate phase represented by (0<y<2) may be used in combination with graphite.

[0064] Examples of binders contained in the negative electrode mixture layer include styrene butadiene rubber (SBR), nitrile butadiene rubber (NBR), carboxymethyl cellulose (CMC) or a salt thereof, polyacrylic acid (PAA) or a salt thereof (PAA-Na, PAA-K, etc., or a partially neutralized salt), polyvinyl alcohol (PVA), etc. These may be used alone or in combination of two or more.

[0065] [Separator] A porous sheet having ion permeability and insulating properties is used for the separator 13. Specific examples of the porous sheet include a microporous thin film, a woven fabric, and a nonwoven fabric. Suitable materials for the separator 13 include polyolefins such as polyethylene and polypropylene, and cellulose. The separator 13 may have a single-layer structure or a multi-layer structure. Furthermore, a highly heat-resistant resin layer such as an aramid resin may be formed on the surface of the separator 13.

[0066] A filler layer containing an inorganic filler may be formed at the interface between the separator 13 and at least one of the positive electrode 11 and the negative electrode 12. Examples of inorganic fillers include oxides and phosphate compounds containing metal elements such as Ti, Al, Si, and Mg. The filler layer can be formed by applying a slurry containing the filler to the surface of the positive electrode 11, the negative electrode 12, or the separator 13.

[0067] [Non-aqueous electrolyte] The non-aqueous electrolyte has ion conductivity (for example, lithium ion conductivity). The non-aqueous electrolyte may be a liquid electrolyte (electrolytic solution) or a solid electrolyte.

[0068] The liquid electrolyte (electrolytic solution) contains, for example, a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. Examples of the non-aqueous solvent that can be used include esters, ethers, nitriles such as acetonitrile, amides such as dimethylformamide, and mixed solvents of two or more of these. The non-aqueous solvent may contain a halogen-substituted compound in which at least a portion of the hydrogen atoms in these solvents are substituted with halogen atoms such as fluorine. Examples of the halogen-substituted compound include fluorinated cyclic carbonates such as fluoroethylene carbonate (FEC), fluorinated chain carbonates, and fluorinated chain carboxylic acid esters such as methyl fluoropropionate (FMP).

[0069] Examples of the esters include cyclic carbonates such as ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate; chain carbonates such as dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), methyl propyl carbonate, ethyl propyl carbonate, and methyl isopropyl carbonate; cyclic carboxylic acid esters such as γ-butyrolactone (GBL) and γ-valerolactone (GVL); and chain carboxylic acid esters such as methyl acetate, ethyl acetate, propyl acetate, methyl propionate (MP), and ethyl propionate (EP).

[0070] Examples of the ethers include 1,3-dioxolane, 4-methyl-1,3-dioxolane, tetrahydrofuran, 2-methyltetrahydrofuran, propylene oxide, 1,2-butylene oxide, 1,3-dioxane, 1,4-dioxane, 1,3,5-trioxane, furan, 2-methylfuran, 1,8-cineole, cyclic ethers such as crown ethers, 1,2-dimethoxyethane, diethyl ether, dipropyl ether, diisopropyl ether, dibutyl ether, dihexyl ether, ethyl vinyl ether, butyl vinyl ether, and methyl phenyl ether. and chain ethers such as ethyl phenyl ether, butyl phenyl ether, pentyl phenyl ether, methoxytoluene, benzyl ethyl ether, diphenyl ether, dibenzyl ether, o-dimethoxybenzene, 1,2-diethoxyethane, 1,2-dibutoxyethane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, 1,1-dimethoxymethane, 1,1-diethoxyethane, triethylene glycol dimethyl ether, and tetraethylene glycol dimethyl ether.

[0071] The electrolyte salt is preferably a lithium salt. Examples of the lithium salt include LiClO 4 , LiBF 4 , LiPF 6 , LiAlCl 4 , LiSbF 6 , LiSCN, LiCF 3 SO 3 , LiCF 3 CO 2 , LiAsF 6 , LiB 10 Cl 10 , lower aliphatic lithium carboxylates, LiCl, LiBr, LiI, phosphates, borates, and imide salts. Examples of phosphates include lithium difluorophosphate (LiPO 2 F 2Examples of the borate salt include lithium bis(oxalato)borate (LiBOB) and lithium difluoro(oxalato)borate (LiDFFOB). Examples of the imide salt include lithium bisfluorosulfonylimide (LiN(FSO 2 ) 2 ), lithium bistrifluoromethanesulfonyl imide (LiN(CF 3 SO 2 ) 2 ), lithium trifluoromethanesulfonate nonafluorobutanesulfonate imide (LiN(CF 3 SO 2 ) (C 4 F 9 SO 2 )), lithium bispentafluoroethanesulfonyl imide (LiN(C 2 F 5 SO 2 ) 2 Among these, LiPF is preferred from the viewpoint of ionic conductivity, electrochemical stability, etc. 6 The concentration of the lithium salt may be, for example, 4 mol or less, or 3 mol or less, preferably 1.8 mol or less, and more preferably 0.8 mol or more and 1.8 mol or less, per 1 L of the non-aqueous solvent.

[0072] The non-aqueous electrolyte may contain an additive such as an unsaturated carbonate ester, an acid anhydride, a phenol compound, a benzene compound, a nitrile compound, an isocyanate compound, a sultone compound, a sulfate compound, a borate ester compound, a phosphate ester compound, or a phosphite ester compound.

[0073] Examples of unsaturated cyclic carbonates include vinylene carbonate, 4-methylvinylene carbonate, 4,5-dimethylvinylene carbonate, 4-ethylvinylene carbonate, 4,5-diethylvinylene carbonate, 4-propylvinylene carbonate, 4,5-dipropylvinylene carbonate, 4-phenylvinylene carbonate, 4,5-diphenylvinylene carbonate, vinylethylene carbonate, and divinylethylene carbonate. One type of unsaturated cyclic carbonate may be used alone, or two or more types may be used in combination. Some of the hydrogen atoms in the unsaturated cyclic carbonate may be substituted with fluorine atoms. The acid anhydride may be an anhydride formed by intermolecular condensation of multiple carboxylic acid molecules, but is preferably an acid anhydride of a polycarboxylic acid. Examples of polycarboxylic acid anhydrides include succinic anhydride, maleic anhydride, and phthalic anhydride.

[0074] Examples of phenolic compounds include phenol, hydroxytoluene, etc. Examples of benzene compounds include fluorobenzene, hexafluorobenzene, cyclohexylbenzene (CHB), etc.

[0075] Examples of nitrile compounds include adiponitrile, pimelonitrile, propionitrile, and succinonitrile. Examples of isocyanate compounds include methyl isocyanate (MIC), diphenylmethane diisocyanate (MDI), hexamethylene diisocyanate (HDI), toluene diisocyanate (TDI), isophorone diisocyanate (IPDI), and bisisocyanatomethylcyclohexane (BIMCH). Examples of sultone compounds include propane sultone and propene sultone. Examples of sulfate compounds include ethylene sulfate, ethylene sulfite, dimethyl sulfate, and lithium fluorosulfate. Examples of borate ester compounds include trimethyl borate and tris(trimethylsilyl)borate. Examples of phosphate ester compounds include trimethyl phosphate and tris(trimethylsilyl)phosphate. Examples of phosphite ester compounds include trimethyl phosphite and tris(trimethylsilyl)phosphite.

[0076] As the solid electrolyte, for example, a solid or gel-like polymer electrolyte, an inorganic solid electrolyte, etc. can be used. As the inorganic solid electrolyte, a material known in all-solid-state lithium ion secondary batteries, etc. (for example, an oxide-based solid electrolyte, a sulfide-based solid electrolyte, a halogen-based solid electrolyte, etc.) can be used. The polymer electrolyte includes, for example, a lithium salt and a matrix polymer, or a non-aqueous solvent, a lithium salt, and a matrix polymer. As the matrix polymer, for example, a polymer material that absorbs the non-aqueous solvent and gels is used. As the polymer material, for example, a fluororesin, an acrylic resin, a polyether resin, etc. can be used.

[0077] The present disclosure will be explained in more detail below with reference to examples, but the present disclosure is not limited to these examples.

[0078] Example 1 Preparation of Positive Electrode Active Material [Ni 0.90 Co 0.05 Al 0.05 ](OH) 2The composite hydroxide represented by the formula (1) was calcined at 500°C for 8 hours to obtain a metal oxide containing Ni, Co, and Al. Next, lithium hydroxide monohydrate (LiOH·H) was added to the composite hydroxide represented by the formula (1) so that the molar ratio of Li to the total amount of Ni, Co, and Al was 1:1.03. 2 O) was mixed to obtain a mixture. Then, this mixture was placed under an oxygen flow (10 cm) with an oxygen concentration of 95%. 3 The mixture was heated from room temperature to 650°C at a temperature increase rate of 2.0°C / min under a temperature of 2 mL / min per kg of the mixture and 5 L / min per kg of the mixture, and then heated from 650°C to 740°C at a temperature increase rate of 0.5°C / min to obtain a lithium-containing transition metal composite oxide (synthesis step).

[0079] Water was added to the obtained lithium-containing transition metal composite oxide so that the slurry concentration was 1500 g / L, and the mixture was stirred for 15 minutes and filtered to obtain a cake-like composition (washing step). The obtained cake-like composition was then dried under vacuum at 180°C for 2 hours to obtain a powder-like composition (drying step). Powdered lithium methanesulfonate was then added to the obtained powder-like composition (addition step). Two types of positive electrode active materials with different lithium methanesulfonate contents were prepared. More specifically, a first positive electrode active material was prepared by adding lithium methanesulfonate so that the content of lithium methanesulfonate was 0.3 mass% relative to the total mass of the lithium-containing transition metal composite oxide, and a second positive electrode active material was prepared by adding lithium methanesulfonate so that the content of lithium methanesulfonate was 0.7 mass% relative to the total mass of the lithium-containing transition metal composite oxide. It was confirmed by Fourier transform infrared spectroscopy (FT-IR) that lithium methanesulfonate was present on the surfaces of the secondary particles of the lithium-containing transition metal composite oxides constituting the first positive electrode active material and the second positive electrode active material, respectively.

[0080] [Fabrication of Positive Electrode] The first positive electrode active material, acetylene black (AB), and a polymer having an average molecular weight of 1.2 × 10 were mixed in N-methyl-2-pyrrolidone (NMP). 6and polyvinylidene fluoride (PVdF) in a mass ratio of 98:1:1 to prepare a first positive electrode mixture slurry. A second positive electrode mixture slurry was prepared in the same manner as in preparing the first mixture slurry, except that the second positive electrode active material was used instead of the first positive electrode active material.

[0081] The first positive electrode mixture slurry was then applied to both sides of a positive electrode core made of aluminum foil. The second positive electrode mixture slurry was then applied to the coating of the first positive electrode mixture slurry, and the coating was dried and compressed. The electrode core was then cut to a predetermined electrode size, and a positive electrode was fabricated in which a two-layer structure positive electrode mixture layer including a lower layer (first positive electrode mixture layer) and an upper layer (second positive electrode mixture layer) was formed on both sides of the positive electrode core. Each positive electrode mixture slurry was applied so that the mass ratio of the first positive electrode mixture layer to the second positive electrode mixture layer was 50:50. In other words, the ratio (T2 / T1) of the thickness (T1) of the second positive electrode mixture layer to the thickness (T2) of the first positive electrode mixture layer was 1.0. Therefore, the sulfonic acid compound content of the first region was 0.3% by mass, and the sulfonic acid compound content of the second region was 0.7% by mass. The weight of the positive electrode mixture layer is 270 g / m 2 It was.

[0082] [Preparation of Negative Electrode] Natural graphite and a silicon compound were used as the negative electrode active material. Natural graphite, a silicon compound, carboxymethyl cellulose sodium (CMC-Na), and a dispersion of styrene-butadiene rubber (SBR) were mixed in a solids mass ratio of 95:5:1:1, and a negative electrode mixture slurry was prepared using water as a dispersion medium. The negative electrode mixture slurry was applied to both sides of a negative electrode core made of copper foil, and the coating was dried. The coating was then rolled using a roller and cut to a predetermined electrode size to obtain a negative electrode in which a negative electrode mixture layer was formed on both sides of the negative electrode core. An exposed portion in which the surface of the negative electrode core was exposed was provided in a portion of the negative electrode.

[0083] [Preparation of non-aqueous electrolyte] Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) were mixed in a volume ratio of 3:3:4. Lithium hexafluorophosphate (LiPF 6) was dissolved in the solution to a concentration of 1.2 mol / L to prepare a non-aqueous electrolyte.

[0084] [Preparation of Test Cell (Non-Aqueous Electrolyte Secondary Battery)] An aluminum lead was attached to the exposed portion of the positive electrode, and a nickel lead was attached to the exposed portion of the negative electrode, and the positive and negative electrodes were spirally wound with a polyolefin separator interposed therebetween to prepare a wound electrode assembly. This electrode assembly was placed in a cylindrical outer can with a bottom, and the non-aqueous electrolyte solution was poured into it. The opening of the outer can was then sealed with a sealer to obtain a test cell.

[0085] [Evaluation of Output Characteristics at Low Temperature] The test cell was charged to 4.2 V at a constant current of 0.2 C in a temperature environment of 25°C, and then subjected to constant voltage charging at 4.2 V until the current value reached 0.01 C. After a 1-hour pause, the test cell was discharged to 2.5 V at a constant current of 0.2 C, forming an initial cycle. Next, after a 1-hour pause, the test cell was again subjected to constant current charging at 0.2 C until the battery voltage reached 4.2 V, and then to constant voltage charging at 4.2 V until the current value reached 0.01 C. The ambient temperature was then changed to 5°C, and after a 2-hour pause, the test cell was discharged to 2.5 V at 1 C. After a 10-minute pause, the test cell was further discharged to 2.5 V at 0.02 C, and the initial output was calculated using the following formula: Initial output at low temperature = 1 C discharge capacity / (1 C discharge capacity + 0.02 C discharge capacity).

[0086] Example 2 A test cell was fabricated in the same manner as in Example 1, except that in the preparation of the positive electrode active material, lithium methanesulfonate was not added to the first positive electrode active material, and the content of lithium methanesulfonate in the second positive electrode active material was 1.0 mass %. In other words, the content of the sulfonic acid compound in the first region was 0 mass %, and the content of the sulfonic acid compound in the second region was 1.0 mass %.

[0087] Example 3 In the production of a positive electrode, the basis weight of the positive electrode mixture layer was 240 g / m 2 A test cell was fabricated in the same manner as in Example 1, except that the content of the sulfonic acid compound in the first region was 0.3 mass %, and the content of the sulfonic acid compound in the second region was 0.7 mass %.

[0088] Example 4 A test cell was fabricated in the same manner as in Example 1, except that in the preparation of the positive electrode active material, the content of lithium methanesulfonate in the first positive electrode active material was 0.3 mass % and the content of lithium methanesulfonate in the second positive electrode active material was 1.2 mass %. In other words, the content of the sulfonic acid compound in the first region was 0.3 mass %, and the content of the sulfonic acid compound in the second region was 1.2 mass %.

[0089] Example 5 A test cell was fabricated in the same manner as in Example 1, except that the content of PVdF in the first positive electrode mixture slurry was made higher than the content of PVdF in the second positive electrode mixture slurry. More specifically, the first positive electrode active material, acetylene black (AB), and a cellulose acylate having an average molecular weight of 1.2 × 10 6 The first positive electrode mixture slurry was prepared by mixing the second positive electrode active material, acetylene black (AB), and polyvinylidene fluoride (PVdF) having an average molecular weight of 1.2 × 10 6 and polyvinylidene fluoride (PVdF) in a mass ratio of 98.2:1:0.8 to prepare a second positive electrode mixture slurry.

[0090] Example 6 A test cell was fabricated in the same manner as in Example 1, except that the content of PVdF in the first positive electrode mixture slurry was made smaller than the content of PVdF in the second positive electrode mixture slurry. More specifically, a first positive electrode active material, acetylene black (AB), and a cellulose acylate having an average molecular weight of 1.2 × 10 6 The first positive electrode mixture slurry was prepared by mixing the second positive electrode active material, acetylene black (AB), and polyvinylidene fluoride (PVdF) having an average molecular weight of 1.2 × 10 6 and polyvinylidene fluoride (PVdF) in a mass ratio of 97.8:1:1.2 to prepare a second positive electrode mixture slurry.

[0091] Example 7 A test cell was fabricated in the same manner as in Example 1, except that in fabricating a positive electrode, the content of PVdF in the first positive electrode mixture slurry was made larger than the content of PVdF in the second positive electrode mixture slurry, and that both the first positive electrode mixture slurry and the second positive electrode mixture slurry used polyvinylidene fluoride (PVdF) with a small average molecular weight. More specifically, a first positive electrode active material, acetylene black (AB), and a PVdF polymer having an average molecular weight of 9.0 × 10 5 The first positive electrode mixture slurry was prepared by mixing the second positive electrode active material, acetylene black (AB), and polyvinylidene fluoride (PVdF) having an average molecular weight of 9.0×10 5 and polyvinylidene fluoride (PVdF) in a mass ratio of 98.2:1:0.8 to prepare a second positive electrode mixture slurry.

[0092] Comparative Example 1 A test cell was produced in the same manner as in Example 1, except that the addition step was not performed in the production of the positive electrode active material, and one type of positive electrode mixture slurry was used in the production of the positive electrode.

[0093] Comparative Example 2 A test cell was produced in the same manner as in Example 1, except that in the preparation of the positive electrode active material, the content of lithium methanesulfonate in each of the first and second positive electrode active materials was 0.5 mass % relative to the total mass of the lithium-containing transition metal composite oxide. That is, in the positive electrode of Comparative Example 2, the content of the sulfonic acid compound in each of the first and second regions was 0.5 mass %.

[0094] <Comparative Example 3> In the preparation of the positive electrode active material, the content of lithium methanesulfonate in each of the first positive electrode active material and the second positive electrode active material was 0.5 mass% relative to the total mass of the lithium-containing transition metal composite oxide, and in the preparation of the positive electrode, the basis weight of the positive electrode mixture layer was 240 g / m 2 Except for this, a test cell was produced in the same manner as in Example 1. That is, in the positive electrode of Comparative Example 2, the content of the sulfonic acid compound in each of the first region and the second region was 0.5 mass %.

[0095] Comparative Example 4 A test cell was fabricated in the same manner as in Example 1, except that in fabricating the positive electrode, the content of lithium methanesulfonate in the first positive electrode active material was 0.7% by mass and the content of lithium methanesulfonate in the second positive electrode active material was 0.3% by mass. That is, the content of the sulfonic acid compound in the first region was 0.7% by mass, and the content of the sulfonic acid compound in the second region was 0.3% by mass.

[0096] Comparative Example 5 A test cell was produced in the same manner as in Example 1, except that in the preparation of the positive electrode active material, the content of lithium methanesulfonate in each of the first and second positive electrode active materials was 0.3 mass% relative to the total mass of the lithium-containing transition metal composite oxide. That is, in the positive electrode of Comparative Example 2, the content of the sulfonic acid compound in each of the first and second regions was 0.3 mass%.

[0097] Comparative Example 6 A test cell was produced in the same manner as in Example 1, except that in the preparation of the positive electrode active material, the content of lithium methanesulfonate in each of the first and second positive electrode active materials was 0.7 mass% relative to the total mass of the lithium-containing transition metal composite oxide. That is, in the positive electrode of Comparative Example 2, the content of the sulfonic acid compound in each of the first and second regions was 0.7 mass%.

[0098] The initial outputs at low temperatures of the test cells of Examples 1 to 7 and Comparative Examples 1 to 6 are shown in Table 1. The initial outputs at low temperatures of the test cells of Examples 1 to 7 and Comparative Examples 1 to 6 shown in Table 1 are expressed relative to the initial output at low temperatures of the test cell of Comparative Example 1, which is set to 100. A larger value of the initial output at low temperatures indicates better output characteristics at low temperatures.

[0099]

[0100] As shown in Table 1, the test cells of the examples have improved initial output at low temperatures compared to the test cells of the comparative examples. In other words, by increasing the content of the sulfonic acid compound in the second region relative to the content of the sulfonic acid compound in the first region, output characteristics at low temperatures can be improved. On the other hand, the test cell of comparative example 2, in which the content of the sulfonic acid compound in the first and second regions is reduced, exhibits a smaller improvement in output characteristics at low temperatures compared to the test cells of the examples. This is presumably due to the sulfonic acid compound's insufficient effect in reducing the reaction resistance of the positive electrode. Furthermore, the test cell of comparative example 3, in which the content of the sulfonic acid compound in the first and second regions is increased, also exhibits a smaller improvement in output characteristics at low temperatures compared to the test cells of the examples. This is presumably due to the presence of the sulfonic acid compound on the particle surfaces, which reduces the electronic conductivity of the lithium-containing transition metal composite oxide and increases the electronic resistance of the entire positive electrode mixture layer.

[0101] Furthermore, the test cells of Examples 5 and 6, in which the binder content in the second region was made lower than the binder content in the first region, exhibited improved output characteristics at low temperatures compared to the test cell of Example 1. This is presumably because the reaction resistance on the surface side of the positive electrode was further reduced by reducing the binder content in the second region.

[0102] The present disclosure is further described by the following embodiments. Configuration 1: A positive electrode for a non-aqueous electrolyte secondary battery, having a positive electrode core and a positive electrode mixture layer formed on the surface of the positive electrode core, wherein the positive electrode mixture layer contains a lithium-containing transition metal composite oxide as a positive electrode active material, and a sulfonic acid compound represented by formula (I) is present on particle surfaces of the lithium-containing transition metal composite oxide, and when the positive electrode mixture layer is divided into two equal parts in the thickness direction and the region of the positive electrode mixture layer facing the positive electrode core is defined as a first region and the region of the positive electrode mixture layer facing the surface is defined as a second region, the content of the sulfonic acid compound in the second region is higher than the content of the sulfonic acid compound in the first region. (In the formula, A is a Group 1 or Group 2 element, R is a hydrocarbon group, and n is 1 or 2.) Configuration 2: The positive electrode for a non-aqueous electrolyte secondary battery according to Configuration 1, wherein a ratio (Y / X) of a content (Y) of the sulfonic acid compound in the second region to a content (X) of the sulfonic acid compound in the first region satisfies 1 < (Y / X) ≦ 10. Configuration 3: The positive electrode for a non-aqueous electrolyte secondary battery according to Configuration 1 or 2, wherein the content (X) of the sulfonic acid compound in the first region is 0% by mass or more and 0.5% by mass or less, relative to the total mass of the positive electrode active material in the first region, and the content (Y) of the sulfonic acid compound in the second region is 0.3% by mass or more and 2.0% by mass or less, relative to the total mass of the positive electrode active material in the second region. Configuration 4: The positive electrode for a non-aqueous electrolyte secondary battery according to any one of Configurations 1 to 3, wherein the positive electrode mixture layer further contains a binder, and the content of the binder in the second region is lower than the content of the binder in the first region.Configuration 5: The positive electrode for a non-aqueous electrolyte secondary battery according to any one of Configurations 1 to 4, wherein the positive electrode mixture layer further contains a binder, the binder including a fluorine-containing polymer, and the fluorine-containing polymer has a weight-average molecular weight of 1,000,000 or more.Configuration 6: The positive electrode for a non-aqueous electrolyte secondary battery according to any one of Configurations 1 to 5, wherein the lithium-containing transition metal composite oxide contains 50 mol % or more of Ni, and one or more elements selected from the group consisting of Co, Mn, and Al, relative to the total number of moles of metal elements excluding Li.Configuration 7: The positive electrode mixture layer has a basis weight of 250 g / m 2 The positive electrode for a non-aqueous electrolyte secondary battery according to any one of Configurations 1 to 6. Configuration 8: A non-aqueous electrolyte secondary battery comprising the positive electrode according to any one of Configurations 1 to 7, a negative electrode, and a non-aqueous electrolyte.

[0103] REFERENCE SIGNS LIST 10 nonaqueous electrolyte secondary battery, 11 positive electrode, 12 negative electrode, 13 separator, 14 electrode body, 16 exterior body, 17 sealing body, 18, 19 insulating plate, 20 positive electrode lead, 21 negative electrode lead, 22 grooved portion, 23 internal terminal plate, 24 lower valve body, 25 insulating member, 26 upper valve body, 27 cap, 28 gasket, 30 positive electrode core, 31 positive electrode mixture layer, 31a first region, 31b second region.

Claims

1. A positive electrode for a non-aqueous electrolyte secondary battery having a positive electrode core and a positive electrode mixture layer formed on a surface of the positive electrode core, wherein the positive electrode mixture layer contains a lithium-containing transition metal composite oxide as a positive electrode active material, and a sulfonic acid compound represented by formula (I) is present on a particle surface of the lithium-containing transition metal composite oxide, and when the positive electrode mixture layer is divided into two equal parts in a thickness direction and a region of the positive electrode mixture layer on the positive electrode core side is defined as a first region and a region of the positive electrode mixture layer on a surface side is defined as a second region, a content of the sulfonic acid compound in the second region is greater than a content of the sulfonic acid compound in the first region. (In the formula, A is a Group 1 or Group 2 element, R is a hydrocarbon group, and n is 1 or 2.) 2. The positive electrode for a nonaqueous electrolyte secondary battery according to claim 1, wherein a ratio (Y / X) of a content rate (Y) of the sulfonic acid compound in the second region to a content rate (X) of the sulfonic acid compound in the first region satisfies 1<(Y / X)≦10.

3. The positive electrode for a nonaqueous electrolyte secondary battery according to claim 1, wherein a content (X) of the sulfonic acid compound in the first region is 0 mass % or more and 0.5 mass % or less, relative to a total mass of the positive electrode active material in the first region, and a content (Y) of the sulfonic acid compound in the second region is 0.3 mass % or more and 2.0 mass % or less, relative to a total mass of the positive electrode active material in the second region.

4. The positive electrode for a non-aqueous electrolyte secondary battery according to claim 1, wherein the positive electrode mixture layer further contains a binder, and a content of the binder in the second region is smaller than a content of the binder in the first region.

5. The positive electrode for a non-aqueous electrolyte secondary battery according to claim 1, wherein the positive electrode mixture layer further contains a binder, the binder contains a fluorine-containing polymer, and the weight-average molecular weight of the fluorine-containing polymer is 1,000,000 or more.

6. The positive electrode for a nonaqueous electrolyte secondary battery according to claim 1, wherein the lithium-containing transition metal composite oxide contains 50 mol % or more of Ni, and one or more elements selected from the group consisting of Co, Mn and Al, relative to the total number of moles of metal elements excluding Li.

7. The weight of the positive electrode mixture layer is 250 g / m 2 The positive electrode for a non-aqueous electrolyte secondary battery according to claim 1 .

8. A non-aqueous electrolyte secondary battery comprising the positive electrode according to any one of claims 1 to 7, a negative electrode, and a non-aqueous electrolyte.

Citation Information

Patent Citations

  • Cathode active material, cathode using it and nonaqueous electrolyte secondary battery

    JP2009187940A

  • Positive electrode plate for secondary batteries and secondary battery using the same

    JP2015043257A

  • Positive electrode active material for lithium ion secondary battery, and lithium ion secondary battery

    JP2019169286A

  • Strip-type electrode for use in cylindrical jelly roll and lithium secondary battery including the same

    JP2020510980A

  • Cathode for lithium ion secondary battery and lithium ion secondary battery

    JP2022149660A