Adhesive joint structure and automobile component

The use of a Zn-Al-Mg-based plated steel with an uneven surface and a specific coating layer in adhesive bonded structures addresses durability and corrosion issues, enhancing adhesion and resistance in automotive parts.

WO2024247815A1PCT designated stage expired Publication Date: 2024-12-05NIPPON STEEL CORPORATION
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/018653
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-26
Filing Date
2024-05-21
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Adhesive bonded structures in automotive parts, particularly those using Zn-Al-Mg hot-dip plated steel, face challenges with adhesive durability and corrosion resistance due to surface cracks and eutectic structure exposure, leading to potential powdering or flaking and reduced adhesion.

Method used

A Zn-Al-Mg-based plated steel structure with a plating layer having an uneven surface and containing binary or ternary eutectic structures that extend to half the average thickness, combined with a coating layer containing organic resin and organosilicon phases, enhances adhesion and corrosion resistance by forming Si-O-Me bonds and preventing water infiltration.

Benefits of technology

The solution significantly improves adhesive durability and corrosion resistance, preventing adhesion deterioration and maintaining long-term adhesive strength even under humid conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024018653_05122024_PF_FP_ABST
    Figure JP2024018653_05122024_PF_FP_ABST
Patent Text Reader

Abstract

An adhesive joint structure is adopted which includes a first member, a second member, and an adhesive layer that joins the first member and the second member. Either or both of the first member and the second member include a steel material and a plating layer. The surface of the plating layer is an uneven surface. In a cross section of the plating layer, the relationship between a longitudinal length Lo of the plating layer in an observation region of the cross section and a total length Lr of the contour line of the surface of the plating layer in the observation region satisfies the following formula (1), and at least some of a plurality of massive binary eutectic structures or a plurality of massive ternary eutectic structures included in the plating layer are continuously present from the surface of the plating layer to a position at one-half an average thickness of the plating layer. (1): (Lr - Lo) / Lo × 100 ≥ 2.0 (%)
Need to check novelty before this filing date? Find Prior Art

Description

Adhesively bonded structures and automotive parts

[0001] This application claims priority to Japanese Patent Application No. 2023-087181, filed May 26, 2023, the contents of which are incorporated herein by reference.

[0002] In the transportation equipment industry, such as automobiles, adhesives are increasingly being used to join components together for purposes such as improving vehicle body rigidity, assisting in weld fracture, and joining dissimilar materials. Joining components together using adhesives is expected to significantly improve performance, making it important as a means of reducing the weight of vehicle bodies. Therefore, in developing adhesively bonded structures for vehicle body parts, such as those between metal components or between metal components and other materials, various studies are being conducted with the aim of improving the bonding strength between components.

[0003] For example, Patent Document 1 below proposes a technology in which an aluminum alloy material is used in which a predetermined oxide film is provided on the surface of an aluminum alloy substrate and a film having a siloxane bond is provided on the oxide film, and such aluminum alloy materials are joined to each other or to another member via an adhesive resin.

[0004] Furthermore, Patent Document 2 below proposes a technology in which a chemically treated metal plate is used in which a chemical conversion coating containing a water-soluble resin and a lubricant having a carbon-oxygen bond is formed on the surface of a metal substrate, and the chemically treated metal plate and a resin layer are joined via an adhesive layer.

[0005] Furthermore, Zn-Al-Mg-based hot-dip plated steel materials having a hot-dip Zn coating layer containing Al and Mg have excellent corrosion resistance. Therefore, the application of Zn-Al-Mg-based hot-dip plated steel sheets, for example, obtained by applying Zn-Al-Mg-based hot-dip plating to high-strength steel sheets, to automotive components has been considered. Known examples of Zn-Al-Mg-based hot-dip plated steel materials include those described in Patent Documents 3 and 4 listed below.

[0006] International Publication No. WO 2016 / 076344 International Publication No. WO 2017 / 169571 International Publication No. WO 2018 / 139619 International Publication No. WO 2018 / 139620

[0007] However, when an adhesive is used as a means for joining components, deterioration of the adhesive (reduced adhesion) inevitably leads to a decrease in component performance. This applies to both the technologies disclosed in Patent Document 1 and Patent Document 2. For this reason, it is difficult to provide a long-term guarantee for the application of adhesives in actual environments, and there have been cases where application has been restricted in some locations or the design has been designed in anticipation of deterioration. Furthermore, while the application of Zn-Al-Mg hot-dip plated steel, which has excellent corrosion resistance, to automotive parts has been considered, no technology has been considered for improving the adhesion between the Zn-Al-Mg hot-dip plated steel and the adhesive layer.

[0008] The present disclosure has been made in view of the above-mentioned problems, and an object of the present disclosure is to provide an adhesively bonded structure and an automotive part which are manufactured by bonding a member made of a Zn-Al-Mg-based plated steel material to another member with an adhesive, and which have excellent adhesive durability and end face corrosion resistance.

[0009] In order to solve the above problems, the present disclosure employs the following configuration. [1] A steel sheet comprising a first member, a second member, and an adhesive layer bonding the first member and the second member, wherein either or both of the first member and the second member is a plated steel material having a steel material and a plating layer disposed on at least a part of a surface of the steel material, and the plating layer has an average chemical composition, in mass%, of Al: 10.00 to 30.00%, Mg: 1.00 to 15.00%, Sn: 0.00 to 1.00%, Si: 0.00 to 2.00%, Ca: 0.00 to 2.00%, Ni: 0.00 to 1.00%, Fe: 0.01 to 15.00%, Sb: 0.00 to 0.50%, Pb: 0.00 to 0.50%, Cu: 0.00 to 1.00%, Ti: 0.00-1.00%, Cr: 0.00-1.00%, Nb: 0.00-1.00%, Zr: 0.00-1.00%, Mn: 0.00-1.00%, Mo: 0.00-1.00%, Ag: 0.00-1.00%, Li: 0.00-1.00%, Bi: 0.00-1.00%, V: 0.00-1.00%, Co: 0.00-1.00%, In: 0.00-1.00%, W: 0.00-1.00%, P: 0.00-1.00%, La: 0.00~0.50%, Ce: 0.00~0.50%, B : 0.00 to 0.50%, Y: 0.00 to 0.50%, Sr: 0.00 to 0.50%, Sb, Pb, Cu, Ti, Cr, Nb, Zr, Mn, Mo, Ag, Li, Bi, V, Co, In, W, P, La, Ce, B, Y, Sr total: 0.00 to 5.00%, balance: Zn and impurities, the surface of the plating layer is an uneven surface, in a cross section of the plating layer, the relationship between the longitudinal length Lo of the plating layer within an observation area of ​​the cross section and the total length Lr of the outline of the surface of the plating layer within the observation area satisfies the following formula (1), the plating layer includes one or both of a plurality of massive binary eutectic structures and a plurality of massive ternary eutectic structures, An adhesive bonded structure, in which at least a portion of the plurality of massive binary eutectic structures or the plurality of massive ternary eutectic structures exists continuously from the surface of the plating layer to a position that is 1 / 2 of the average thickness of the plating layer.(Lr-Lo) / Lo×100≧2.0(%) ... (1) [2] The adhesive bonded structure according to [1], wherein the first member is a plated steel material having the steel material and the plating layer, and the second member is any one of a galvannealed steel material, a fiber-reinforced plastic material, an aluminum alloy material, and a magnesium alloy material. [3] The adhesive bonded structure according to [1], wherein the plated steel material comprises the steel material, the plating layer, and a coating portion disposed on at least the uneven surface of the plating layer, and the adhesive layer bonds the first member and the second member via the coating portion. [4] The adhesive bonded structure according to [2], wherein the plated steel material comprises the steel material, the plating layer, and a coating portion disposed on at least the uneven surface of the plating layer, and the adhesive layer bonds the first member and the second member via the coating portion. [5] The coating portion contains an organic resin phase containing one or more of a urethane group, an epoxy group, and an ester group, and an organic compound phase consisting of an organosilicon compound containing at least one of an Si—O bond or an Si—OH bond, and an Si—C bond, and when the coating portion is analyzed by time-of-flight secondary ion mass spectrometry while Ar sputtering from the adhesive layer side to the plating layer side so as to include any location at the interface between the plating layer and the coating portion, a peak corresponding to an Si—O—Me bond is observed, and the value obtained by dividing the count number of the peak indicating the Si—O—Me bond by the sum of the count numbers of all secondary ions detected in a mass scan range of m / z = 0 to 300 is 1.0 × 10. -3The adhesive bonded structure according to [3] or [4], wherein Me is one or more elements selected from the group consisting of Zn, Al, Mg, and Fe that constitute the plating layer. [6] The adhesive bonded structure according to [1], wherein the plating layer includes an Fe-Al-based interfacial alloy layer in contact with the steel material, and wherein at least a portion of the binary eutectic structure or the ternary eutectic structure is present continuously from the surface of the plating layer to the Fe-Al-based interfacial alloy layer. [7] The adhesive bonded structure according to [1], wherein the following formula (2) is satisfied instead of formula (1), and the number of locations where at least a portion of the binary eutectic structure or the ternary eutectic structure is present continuously from the surface of the plating layer to a position half the average thickness of the plating layer is 3 to 15 per rectangular region on the surface of the plating layer having a long side of 500 μm and a short side of 150 μm: (Lr-Lo) / Lo×100≧6.0(%) ... (2) [8] The adhesive bonded structure according to [1], wherein the following formula (3) is satisfied instead of formula (1): (Lr-Lo) / Lo×100≧6.0(%) ... (2) [8] The adhesive bonded structure according to [1], wherein the number of locations where at least a portion of the multiple aggregates of the binary eutectic structure or the multiple aggregates of the ternary eutectic structure are continuously present from the surface of the plating layer to a position half the average thickness of the plating layer is 5 to 15 per rectangular region on the surface of the plating layer, the long side being 500 μm and the short side being 150 μm. (Lr-Lo) / Lo×100≧8.0(%) ... (3) [9] The adhesive bonded structure according to [1], wherein the locations where at least a portion of the multiple aggregates of the binary eutectic structure or the multiple aggregates of the ternary eutectic structure are continuously present from the surface of the plating layer to a position half the average thickness of the plating layer are located in recesses on the uneven surface of the plating layer.

[10] The adhesive bonded structure according to [6], wherein the portions of the plated layer where at least a portion of the binary eutectic structure or the ternary eutectic structure are present continuously from the surface of the plated layer to the Fe-Al-based interfacial alloy layer are located in the recesses of the uneven surface of the plated layer.

[11] The adhesive bonded structure according to [1], wherein the average chemical composition of the plated layer is such that Al and Mg are 10.00 to 25.00% and 4.50 to 15.00%, respectively.

[12] The adhesive bonded structure according to [1], wherein the average chemical composition of the plating layer is such that Al: 15.00 to 22.00% and Mg: 5.00 to 15.00%.

[13] The average chemical composition of the plating layer is such that Sn is 0.05 to 0.50%, and Mg is detected in the plating layer by X-ray diffraction measurement. 2 The adhesive bonded structure according to any one of [1],

[11] or

[12] , which contains a Sn phase.

[14] The adhesive bonded structure according to [1],

[11] or

[12] , wherein the average chemical composition of the plating layer contains one or both of La and Ce, and the total amount of La and Ce is 0.05 to 0.50%.

[15] The adhesive bonded structure according to

[13] , wherein the average chemical composition of the plating layer contains one or both of La and Ce, and the total amount of La and Ce is 0.05 to 0.50%.

[16] The adhesive bonded structure according to any one of [1] to [4], wherein the first member and the second member are further joined by a second joining.

[17] The adhesive bonded structure according to

[16] , wherein the second joining is by spot welding.

[18] An automotive part comprising the adhesive bonded structure according to any one of [1] to [4] or [6] to

[12] .

[19] An automobile part comprising the adhesive bonded structure according to [5].

[20] An automobile part comprising the adhesive bonded structure according to

[13] .

[21] An automobile part comprising the adhesive bonded structure according to

[14] .

[22] An automobile part comprising the adhesive bonded structure according to

[15] .

[23] An automobile part comprising the adhesive bonded structure according to

[16] .

[24] An automobile part comprising the adhesive bonded structure according to

[17] .

[0010] As described above, according to the above aspects of the present disclosure, it is possible to provide an adhesively bonded structure that is manufactured by bonding a member made of a Zn-Al-Mg-based plated steel material to another member with an adhesive, and that has excellent adhesive durability and corrosion resistance, and an automotive part that includes the adhesively bonded structure.

[0011] 1-1。 FIG. 1-2 is a schematic perspective view of a bonded structure according to an embodiment of the present disclosure. FIG. 1-3 is a schematic cross-sectional view of a plated steel material, which is an example of a first member. FIG. 1-4 is a schematic view showing an example of an observation field when a cross-section of a plating layer of a plated steel material is observed with a scanning electron microscope. FIG. 1-5 is a schematic view showing an example of an observation field when a cross-section of a plating layer of a plated steel material is observed with a scanning electron microscope. FIG. 1-6 is a schematic view showing an example of an observation field when a cross-section of a plating layer of a conventional plated steel material is observed with a scanning electron microscope. FIG. 1-7 is an enlarged schematic view of a bonding region of the bonded structure shown in FIG. 1-1. FIG. 1-8 is a partially enlarged cross-sectional view of a bonding region of the bonded structure shown in FIG. 1-1. FIG. 1-9 is an enlarged schematic view illustrating a bonding region of a bonded structure according to a modified example of the present disclosure. FIG. 1-1 is a schematic perspective view of a bonded structure according to another modified example of the present disclosure. FIG. 1-2 is a schematic perspective view of a bonded structure according to another modified example of the present disclosure. FIG. 1-3 is a schematic view illustrating the bonding state of a bonded structure according to another modified example of the present disclosure. FIG. 1-4 is a flowchart of an example of a method for manufacturing a bonded structure according to an embodiment of the present disclosure.

[0012] The present inventors have investigated a means for improving the adhesion of the adhesive layer to the coating layer. The metal structure of a Zn-Al-Mg hot-dip coating layer containing Al, Mg, and Zn contains various phases or structures. For example, in the early solidification stage, Al phase and MgZn phase are formed. 2 It is known that a binary eutectic structure or a ternary eutectic structure crystallizes in the later stage of solidification. The inventors have investigated and found that a binary eutectic structure or a ternary eutectic structure is formed by the Al phase and MgZn 2 It was found that the adhesive layer had better adhesion than the other layers.

[0013] In conventional Zn-Al-Mg hot-dip coatings, binary or ternary eutectic structures may be exposed on the surface of the coating layer. These binary or ternary eutectic structures are often distributed in the surface of the coating layer, specifically, in a range from the surface of the coating layer to a depth of ¼ to ⅓ of the average thickness of the coating layer. It has been previously believed that these eutectic structures exposed on the surface of the coating layer improve the adhesion of the adhesive layer. However, when manufacturing automotive components from coated steel sheets, the coated steel sheets must be subjected to various processes to obtain automotive components of the desired shape. However, the processed coating layer may develop fine cracks on its surface due to strain during processing. It has been found that when such cracks occur around the eutectic structures exposed on the surface of the coating layer, the eutectic structures surrounded by the cracks may detach from the coating layer, resulting in so-called powdering or flaking, which may not contribute to improving the adhesion of the adhesive layer.

[0014] In particular, since the Zn-Al-Mg hot-dip plating layer is harder than the conventional Zn-based plating layer, there is a possibility that a relatively large number of cracks may occur, which increases the frequency with which the eutectic structure falls off from the plating layer, and there is concern that the adhesion of the adhesive layer may decrease.

[0015] It was also expected that an uneven surface of the plating layer would be more effective in improving the adhesion of the adhesive layer than a flat surface.

[0016] Therefore, the inventors have conducted research and found that, after a hot-dip coating bath is applied to a steel material by a hot-dip coating method, by controlling the atmosphere from the time the coating bath is removed until the start of cooling, adjusting the cooling rate during cooling, and selecting a suitable cooling gas, a binary eutectic structure or a ternary eutectic structure can be continuously present to a position deeper than the surface of the coating layer, specifically, at least to a depth of half the average thickness of the coating layer from the surface of the coating layer, and even if cracks occur, the eutectic structure will not fall off from the coating layer, thereby preventing a decrease in the adhesion of the adhesive layer and ultimately suppressing deterioration of the adhesive durability. Furthermore, the inventors have found that by controlling the atmosphere, adjusting the cooling rate, and selecting a suitable cooling gas, the surface of the coating layer can be made uneven, thereby further improving the adhesive durability.

[0017] Furthermore, in an effort to further improve adhesion durability, it was discovered that by providing a coating between the plated steel material and the adhesive layer that contains a substance capable of forming a strong chemical bond with the plating layer of the plated steel material and a substance that has a high affinity with the resin of the adhesive that constitutes the adhesive layer, the penetration of water into the adhesive interface between the plated steel material and the adhesive layer, which was thought to be a cause of reduced adhesion, can be suppressed by the coating, thereby further improving adhesion durability. Note that the coating is an optional component in this disclosure.

[0018] Hereinafter, an adhesive bonded structure and an automotive part according to embodiments of the present disclosure will be described with reference to the drawings. In this specification and the drawings, components having substantially the same functional configurations are designated by the same reference numerals, and redundant description will be omitted.

[0019] (Configuration of Adhesively Bonded Structure) FIG. 1-1 is a schematic perspective view showing the entire structure of an adhesively bonded structure according to an embodiment of the present disclosure.

[0020] The adhesively bonded structure 1 shown in FIG. 1-1 includes a first member 2 and a second member 3. The first member 2 is a so-called hat-shaped metal member. That is, the first member 2 is a metal member having a hat-shaped cross section perpendicular to the longitudinal direction, which includes a web portion, a pair of vertical wall portions connected to both widthwise edges of the web portion, and a pair of flange portions connected to the vertical wall portions. The web portion has a rectangular shape that is long in one direction. The second member 3 has a shape that conforms to the inside of the web portion of the first member 2, and is bonded to the first member 2 via an adhesive layer 4 in an adhesive region 5 located inside the web portion. Here, the inside of the web portion refers to the region surrounded by the web portion and the vertical wall portions.

[0021] 1-1, in order to facilitate the explanation of the configuration of the adhesive bonded structure according to this embodiment, the explanation will be given assuming that the first member 2 is hat-shaped. However, as will be described later, the shapes of the members constituting the adhesive bonded structure according to this embodiment are not limited to the illustrated form. Furthermore, in this embodiment, it is sufficient that at least the first member 2 is made of plated steel. However, in the following explanation, as an example, a case will be described in which both the first member 2 and the second member 3 are made of plated steel. The configuration of the adhesive region 5 will be explained below with reference to FIG. 1-1.

[0022] <Regarding the first member 2> The first member 2 is made of, for example, a plated steel material 21, which will be described below. The plated steel material 21 will be described below. In the following description, the first member 2 is assumed to be a plated steel material, but the adhesive-bonded structure according to this embodiment is not limited to this. The second member 3 may also be a plated steel material, or both the first member 2 and the second member 3 may also be plated steel materials.

[0023] <Plated Steel Material 21> The first member 2 is made of a plated steel material 21. The plated steel material has a steel material and a plating layer disposed on at least a portion of the surface of the steel material. The average chemical composition of the plating layer is, in mass %, Al: 10.00 to 30.00%, Mg: 1.00 to 15.00%, Sn: 0.00 to 1.00%, Si: 0.00 to 2.00%, Ca: 0.00 to 2.00%, Ni: 0.00 to 1.00%, Fe: 0.01 to 15.00%, and Sb: 0.00 to 1.00%. 0.50%, Pb: 0.00-0.50%, Cu: 0.00-1.00%, Ti: 0.00-1.00%, Cr: 0.00-1.00%, Nb : 0.00 to 1.00%, Zr: 0.00 to 1.00%, Mn: 0.00 to 1.00%, Mo: 0.00 to 1.00%, Ag: 0.00 to 1.00%. 00%, Li: 0.00-1.00%, Bi: 0.00-1.00%, V: 0.00-1.00%, Co: 0.00-1.00%, In: 0.00%. 00-1.00%, W: 0.00-1.00%, P: 0.00-1.00%, La: 0.00-0.50%, Ce: 0.00-0.50%, B : 0.00 to 0.50%, Y: 0.00 to 0.50%, Sr: 0.00 to 0.50%, a total of Sb, Pb, Cu, Ti, Cr, Nb, Zr, Mn, Mo, Ag, Li, Bi, V, Co, In, W, P, La, Ce, B, Y, and Sr: 0.00 to 5.00%, and the balance: Zn and impurities. The plating layer has an uneven surface, and in a cross section of the plating layer, the relationship between the longitudinal length Lo of the plating layer within an observation region of the cross section and the total length Lr of the outline of the surface of the plating layer within the observation region satisfies the following formula (1), and the plating layer contains one or both of a plurality of massive binary eutectic structures and a plurality of massive ternary eutectic structures, and at least a portion of the plurality of massive binary eutectic structures or the plurality of massive ternary eutectic structures is continuously present from the surface of the plating layer to a position half the average thickness of the plating layer.

[0024] Fig. 1-2 shows a cross-sectional schematic diagram of a plated steel material 21. Fig. 1-2 is a schematic diagram for explaining the positional relationship between the steel material 11 and the plating layer 12. Note that in Fig. 1-2, the uneven surface of the plating layer 12 is not shown.

[0025] As shown in FIG. 1-2 , the plated steel material 21 according to this embodiment includes a steel material 11. The shape of the steel material 11 is not particularly limited. Furthermore, the material of the steel material 11 is not particularly limited. The steel material 11 may be, for example, a steel material standardized by the Japanese Industrial Standards (JIS) or the like, such as carbon steel, alloy steel, or high-tensile steel used for general structures or machine structures. Specific examples of such steel materials include cold-rolled steel, hot-rolled steel, hot-rolled steel sheet material for automotive structures, hot-rolled high-tensile steel sheet material for automotive processing, cold-rolled steel sheet material for automotive structures, cold-rolled high-tensile steel sheet material for automotive processing, and high-tensile steel material commonly referred to as hot-stamped steel that has been quenched during hot processing. The composition of such steel materials is not particularly limited. The steel material may be formed by processing a steel sheet, such as by hot pressing.

[0026] Furthermore, the steel material 11 constituting the plated steel material 21 according to this embodiment may be a high-tensile steel for automobile components.

[0027] The plated steel material 21 according to this embodiment has a plating layer 12 disposed on at least a portion of the surface of the steel material 11. In Fig. 1-2, the plating layer 12 is formed on one side of the steel material 11, but the plating layer 12 may be formed on both sides of the steel material 11. The plating layer 12 is preferably a plating film produced by a so-called hot-dip plating process.

[0028] The plating layer 12 is mainly composed of a Zn—Al—Mg alloy layer due to its chemical composition, which will be described later. Furthermore, the plating layer 12 of the plated steel material 21 according to this embodiment may include an Fe—Al-based interfacial alloy layer, mainly composed of Fe and Al, between the steel material 11 and the Zn—Al—Mg alloy layer. That is, the plating layer 12 may have a single-layer structure of a Zn—Al—Mg alloy layer, or a multilayer structure including a Zn—Al—Mg alloy layer and an Fe—Al-based interfacial alloy layer.

[0029] The chemical composition of the plating layer will be described below. The "%" designation for the content of each element in the chemical composition means "mass %." The content of an element in the chemical composition may be expressed as an element concentration (e.g., Zn concentration, Mg concentration, etc.).

[0030] "Adhesion of the adhesive layer" refers to the property of preventing peeling of the adhesive layer from the plating layer when an adhesive layer is provided on the surface of the plating layer, or when a coating portion is provided on the surface of the plating layer and an adhesive layer is further provided on the coating portion. "Plane corrosion resistance" refers to the property of preventing corrosion of the plating layer (specifically, the Zn-Al-Mg alloy layer) itself. "Edge corrosion resistance" refers to the property of suppressing corrosion of the steel material at the exposed portion of the steel material (for example, the cut edge of the plated steel material).

[0031] The plating layer according to this embodiment contains Zn and other alloying elements. The chemical composition of the plating layer will be described in detail below. Note that elements whose lower limit concentration is 0.00% are not essential for solving the problems of the plated steel material according to this embodiment, but are optional elements that are allowed to be included in the plating layer for the purpose of improving characteristics, etc.

[0032] <Al: 10.00 to 30.00%> Al contributes to improving planar corrosion resistance and workability. Therefore, the Al concentration is set to 10.00% or more. On the other hand, if Al is excessive, the Mg concentration and Zn concentration decrease relatively, deteriorating edge corrosion resistance. Therefore, the Al concentration is set to 30.00% or less. The Al concentration may be 10.00 to 25.00% or 15.00 to 22.00%. The Al concentration may be 11.00% or more, 13.00% or more, or 16.00% or more. The Al concentration may be 28.00% or less, 24.00% or less, or 20.00% or less.

[0033] <Mg: 1.00 to 15.00%> Mg is an essential element for ensuring flat corrosion resistance. 2 Mg is also necessary to crystallize Sn phases and the like. Therefore, the Mg concentration is set to 1.00% or more. On the other hand, if the Mg concentration is excessive, workability, particularly powdering properties, may deteriorate, and furthermore, flat corrosion resistance may deteriorate. Therefore, the Mg concentration is set to 15.00% or less. The Mg concentration may be 4.50 to 15.00% or 5.00 to 15.00%. The Mg concentration may be 2.00% or more, 3.00% or more, or 4.00% or more. The Mg concentration may be 13.00% or less, 10.00% or less, or 8.00% or less.

[0034] The elements described below, except for Fe and Zn, are all optional elements, and therefore the lower limit of each element is set to 0.00% or more.

[0035] <Sn: 0 to 1.00%> The Sn concentration may be 0.00%. On the other hand, Sn is an element that forms an intermetallic compound with Mg and improves the planar corrosion resistance of the plating layer. Therefore, the Sn concentration may be 0.05% or more, 0.10% or more, or 0.20% or more. However, if the Sn concentration is excessive, the planar corrosion resistance will deteriorate. Therefore, the Sn concentration is set to 1.00% or less. The Sn concentration may also be 0.80% or less, 0.60% or less, 0.50% or less, 0.20% or less, or 0.06% or less.

[0036] <Si: 0% to 2.00%> The Si concentration may be 0.00%. On the other hand, Si contributes to improving the plane corrosion resistance. 2 Si is an element necessary for crystallizing the Si phase. Therefore, the Si concentration may be greater than 0.00%, 0.01% or more, 0.05% or more, or 0.10% or more. On the other hand, if the Si concentration is excessive, the plane corrosion resistance deteriorates. Therefore, the Si concentration is set to 2.00% or less. The Si concentration may also be set to 1.80% or less, 1.50% or less, 1.20% or less, or 1.00% or less.

[0037] <Ca: 0% to 2.00%> The Ca concentration may be 0.00%. On the other hand, Ca is an element that can adjust the amount of Mg elution that is optimal for imparting flat surface corrosion resistance. Therefore, the Ca concentration may be 0.01% or more, or 0.02% or more. On the other hand, if the Ca concentration is excessive, flat surface corrosion resistance and workability deteriorate. Therefore, the Ca concentration is set to 2.00% or less. The Ca concentration may also be 1.00% or less, 0.50% or less, 0.10% or less, or 0.05% or less.

[0038] <Ni: 0 to 1.00%> The Ni concentration may be 0.00%. On the other hand, Ni contributes to improving edge corrosion resistance. Therefore, the Ni concentration may be 0.001% or more. On the other hand, if the Ni concentration is excessive, flat surface corrosion resistance will deteriorate. Therefore, the Ni concentration is set to 1.00% or less. The Ni concentration may also be 0.50% or less, 0.10% or less, or 0.01% or less.

[0039] <Fe: 0.01% to 15.00%> The Fe concentration may be 0.00%, but since Fe may be mixed into the plating layer from the base steel material, the plating layer may contain 0.01% or more. It has been confirmed that an Fe concentration of 15.00% or less does not adversely affect the performance of the plating layer. The Fe concentration may be, for example, 0.01% or more, 0.10% or more, or 0.50% or more. The Fe concentration is set to 15.00% or less. The Fe concentration may also be 10.00% or less, 5.00% or less, 2.00% or less, or 1.00% or less.

[0040] <Sb, Pb: 0 to 0.50% each> The concentrations of Sb and Pb may be 0.00%. On the other hand, Sb and Pb contribute to improving edge corrosion resistance. Therefore, the concentrations of Sb and Pb may be 0.01% or more, 0.03% or more, or 0.05% or more. On the other hand, excessive Sb and Pb concentrations deteriorate flat surface corrosion resistance. Therefore, the concentrations of Sb and Pb are set to 0.50% or less. The concentrations of Sb and Pb may also be 0.40% or less, 0.20% or less, or 0.10% or less.

[0041] <Cu, Ti, Cr, Nb, Zr, Mn, Mo, Ag, and Li: 0.00 to 1.00% each> The concentrations of Cu, Ti, Cr, Nb, Zr, Mn, Mo, Ag, and Li may each be 0.00%. On the other hand, these elements contribute to improving edge corrosion resistance. Therefore, the concentrations of these elements may each be 0.01% or more. On the other hand, excessive concentrations of these elements degrade flat surface corrosion resistance. Therefore, the concentrations of these elements are each set to 1.00% or less. The concentrations of these elements may each be set to 0.50% or less, 0.10% or less, 0.05% or less, or 0.03% or less.

[0042] <Bi, V, Co, In, W: 0.00 to 1.00% each> The concentrations of Bi, V, Co, In, and W may each be 0.00%. On the other hand, each of these elements contributes to improving edge corrosion resistance. Therefore, the concentrations of these elements may each be 0.001% or more, or 0.01% or more. On the other hand, excessive concentrations of these elements deteriorate planar corrosion resistance. Therefore, the concentrations of Bi, V, Co, In, and W are each set to 1.00% or less. The concentrations of these elements may each be 0.50% or less, 0.10% or less, 0.02% or less, or 0.01% or less.

[0043] <P: 0 to 1.00%> The P concentration may be 0.00%. On the other hand, P contributes to improving edge corrosion resistance. Therefore, the P concentration may be 0.005% or more, or 0.01% or more. On the other hand, if the P concentration is excessive, flat surface corrosion resistance deteriorates. Therefore, the P concentration is set to 1.00% or less. The P concentration may also be 0.05% or less, 0.03% or less, or 0.01% or less.

[0044] <B, Y, and Sr: 0 to 0.50% each> The concentrations of B, Y, and Sr may each be 0%. On the other hand, B, Y, and Sr contribute to improving edge corrosion resistance. Therefore, the concentrations of these elements may each be 0.001% or more, or 0.01% or more. On the other hand, excessive concentrations of B, Y, and Sr deteriorate planar corrosion resistance. Therefore, the concentrations of these elements are each set to 0.50% or less. The concentrations of these elements may each be set to 0.10% or less, 0.02% or less, or 0.01% or less.

[0045] <La, Ce: 0.00 to 0.50% each> The concentrations of La and Ce may be 0.00%. On the other hand, La and Ce contribute to improving edge corrosion resistance. Therefore, the concentrations of these elements may each be 0.01% or more. On the other hand, excessive concentrations of La and Ce deteriorate plane corrosion resistance. Therefore, the concentrations of these elements are each set to 0.50% or less. The concentrations of these elements may each be set to 0.10% or less, 0.05% or less, or 0.02% or less. Furthermore, the total amount of La and Ce is preferably set to 0.05 to 0.50%.

[0046] <Total of Sb, Pb, Cu, Ti, Cr, Nb, Zr, Mn, Mo, Ag, Li, Bi, V, Co, In, W, P, La, Ce, B, Y, Sr: 0.00 to 5.00%> The total of these elements is set to 0.00 to 5.00%. If the total exceeds 5.00%, flat surface corrosion resistance or edge corrosion resistance may decrease.

[0047] <Balance: Zn and Impurities> The balance of the components of the plating layer according to this embodiment is Zn and impurities. Zn is an element that provides the plating layer with flat corrosion resistance and edge corrosion resistance. Impurities refer to components contained in raw materials or components mixed in during the manufacturing process, but not intentionally added. For example, trace amounts of components other than Fe may be mixed into the plating layer as impurities due to mutual atomic diffusion between the base steel and the plating bath.

[0048] Furthermore, in the plating layer according to this embodiment, the total content of Al, Mg, and Zn is preferably 74.00% or more, and may be 80.00% or more, 90.00% or more, 95.00% or more, or 98.00% or more.

[0049] The chemical composition of the plating layer is measured by the following method. First, an acid containing an inhibitor that suppresses corrosion of steel is used to remove and dissolve the plating layer to obtain an acid solution. Next, the obtained acid solution is subjected to ICP analysis. This allows the chemical composition of the plating layer to be obtained. There are no particular restrictions on the type of acid, as long as it is an acid that can dissolve the plating layer. Note that the chemical composition measured by the above-mentioned means is the average chemical composition of the entire plating layer.

[0050] <Surface of Plated Layer> The surface of the plated layer in this embodiment is an uneven surface. The roughness of the uneven surface is expressed by the relationship between Lo and Lr, as shown in the following formula (1). That is, (Lr - Lo) / Lo x 100 needs to be 2.0(%) or more. If (Lr - Lo) / Lo x 100 is less than 2.0(%), the roughness of the uneven surface is small and the adhesion of the adhesive layer cannot be improved. (Lr - Lo) / Lo x 100 more preferably satisfies the following formula (2), and even more preferably satisfies the following formula (3). There is no particular upper limit for (Lr - Lo) / Lo x 100, but if it is too large, the surface smoothness of the plated layer may decrease, the average thickness of the adhesive layer may become non-uniform, and sufficient adhesive performance may not be obtained. Therefore, it is preferable that the upper limit be 40(%) or less, 20(%) or less, or 12(%) or less.

[0051] (Lr-Lo) / Lo×100≧2.0(%)…(1) (Lr-Lo) / Lo×100≧6.0(%)…(2) (Lr-Lo) / Lo×100≧8.0(%)…(3)

[0052] In Equations (1) to (3), the length Lo is the longitudinal length of the plating layer within the observation area of ​​the cross section of the plating layer, and Lr is the total length of the contour of the surface of the plating layer within the observation area. The observation area is the observation field when the cross section of the plating layer is observed with a scanning electron microscope. The longitudinal length of the plating layer that fits within the observation field is Lo, and the total length of the contour of the surface of the plating layer corresponding to the longitudinal length Lo of the plating layer is Lr. When measuring Lo and Lr, it is desirable to set the observation field when observed with a scanning electron microscope so that the longitudinal length Lo of the plating layer is 500 μm. Furthermore, multiple observation fields may be combined to create an observation field where the longitudinal length Lo of the plating layer is 500 μm. The observation field is positioned at a distance of 5 mm or more from the end of the plated steel material. If a weld is provided on the plated steel material, the observation field is positioned at a distance of 1 mm or more from the weld bead. Furthermore, if the plated steel material actually has a bent portion, the observation field is positioned at a distance of 2 mm or more from the bent portion. This eliminates the effects of cutting, welding, and bending the plated steel material on the surface quality of the plating layer from the measurement results. The observation field is preferably positioned in a flat area. However, plated steel may not have a flat area. For example, when plated steel is used as an exterior component of an automobile, the plated steel may have a gently curved shape overall and may not have a flat area. In this case, it is preferable to position the observation field in an area with a radius of curvature of 5 mm or more. The number of observation fields is 5. First, (Lr - Lo) / Lo x 100 is calculated for each of the five observation fields, and then the arithmetic mean of these values ​​is calculated. This arithmetic mean is considered to be (Lr - Lo) / Lo x 100 of the plated steel material.

[0053] FIG. 1-3 is a schematic diagram showing an example of an observation field when observed with a scanning electron microscope. FIG. 1-3 also shows the relationship between Lo and Lr. In FIG. 1-3, reference numeral 11 denotes a steel material, reference numeral 12 denotes a plating layer, and reference numeral 13 denotes an interface alloy layer. The double-headed arrows of reference numerals Lo and Lr respectively represent the lengths of Lo and Lr. FIG. 1-3 also schematically shows the uneven surface of the plating layer.

[0054] <Structure of the plating layer> The plating layer of this embodiment includes one or both of a plurality of massive binary eutectic structures and a plurality of massive ternary eutectic structures. The binary eutectic structure is a eutectic structure of an η-Zn phase and an Al-Zn phase, and the ternary eutectic structure is a eutectic structure of an Al phase, a Zn phase, and an MgZn phase. 2 These eutectic structures may be eutectic structures in which the phases constituting the eutectic structure are assembled in a lamellar form. That is, the binary eutectic structure may have a lamellar structure in which a lamellar η-Zn phase and a lamellar Al-Zn phase are superposed. The ternary eutectic structure may have a lamellar structure in which a lamellar Al phase, a lamellar Zn phase, and a lamellar MgZn phase are superposed. 2 It may have a lamellar structure with overlapping phases.

[0055] In addition to these eutectic structures, the plating layer also contains massive Al phase, Al-Zn phase, Zn phase, MgZn 2 The plating layer may contain a eutectoid structure containing a lamellar Zn phase and a lamellar Al phase. This eutectoid structure has a lamellar structure, but does not fall under the category of a binary or ternary eutectic structure.

[0056] In the plating layer of this embodiment, at least a portion of a plurality of massive binary or ternary eutectic structures is present continuously from the surface of the plating layer to a position halfway through the average thickness of the plating layer. At least a portion of these massive binary or ternary eutectic structures is exposed on the surface of the plating layer. Compared to other phases such as Al phase and Al-Zn phase, the binary or ternary eutectic structure has superior adhesion to an adhesive layer. Therefore, exposure of the binary or ternary eutectic structure on the surface of the plating layer improves the adhesion of the entire plating layer to an adhesive layer.

[0057] Furthermore, when cracks occur in the coating layer during processing of the plated steel material, the cracks often propagate along the boundary between the binary or ternary eutectic structure and other phases or structures. In this embodiment, at least a portion of the binary or ternary eutectic structure exists continuously up to a position half the average thickness of the coating layer. Therefore, cracks that occur during bending tend to propagate from the surface of the coating layer toward the steel material and are less likely to propagate in a direction parallel to the surface of the coating layer. Therefore, even if cracks occur, the eutectic structure is less likely to fall off from the coating layer, and powdering or flaking is suppressed. As a result, the coating adhesion of the coating layer is not reduced even when the coating layer is processed.

[0058] More preferably, the plating layer of this embodiment has at least a portion of a plurality of massive binary or ternary eutectic structures present continuously from the surface of the plating layer to the Fe-Al-based interfacial alloy layer, which further suppresses the occurrence of powdering or flaking and further improves the adhesion of the plating layer to the adhesive layer.

[0059] Figure 1-4 shows an enlarged schematic diagram of an example of a plating layer according to this embodiment. Figure 1-4 shows a schematic representation of the uneven surface of the plating layer, as well as the presence of a binary or ternary eutectic structure. The shaded areas in the figure represent the binary or ternary eutectic structure. In Figure 1-4, reference numeral 11 denotes a steel material, reference numeral 12 denotes a plating layer, reference numeral 13 denotes an interface alloy layer, and reference numeral 14 denotes a binary or ternary eutectic structure.

[0060] As shown in Figure 1-4, it can be seen that the binary or ternary eutectic structure 14 is continuous from the surface of the coating layer 12 toward the steel material 11 side. It can also be seen that the binary or ternary eutectic structure 14 exists continuously up to the Fe-Al-based interface alloy layer 13 on the steel material side of the coating layer 12. Note that Figure 1-4 shows an example in which most of the binary or ternary eutectic structure 14 is continuous up to the Fe-Al-based interface alloy layer 13 on the steel material 11 side of the coating layer 12, but the present embodiment is not limited to this, and the binary or ternary eutectic structure 14 that is continuous up to a 1 / 2 position of the coating layer 12 may also be included.

[0061] For reference, a cross-sectional schematic diagram of a conventional plating layer is shown in Figure 1-5. The conventional plating layer 112 has a flat surface, and the binary or ternary eutectic structure 114 is distributed near the interface alloy layer 113 of the plating layer 112 or near the surface of the plating layer, but no binary or ternary eutectic structure 114 is found that is continuous up to the halfway point of the plating layer 112.

[0062] Furthermore, the surface of the plating layer 12 of this embodiment is an uneven surface as exemplified in Figures 1-3 and 1-4, and the binary or ternary eutectic structure 14, which exists continuously to a depth of half the average thickness of the plating layer 12, is present in large amounts in the recesses of the uneven surface, as shown in Figure 1-4. This is because, as will be described later, the binary or ternary eutectic structure crystallizes in the latter half of the solidification process of the plating layer. The concentration of the binary or ternary eutectic structure in the recesses, combined with the geometric effect of the uneven surface, can improve paint adhesion.

[0063] In this embodiment, a binary eutectic structure or a ternary eutectic structure that exists continuously from the surface of the plating layer to the Fe—Al-based interface alloy layer may be present in large numbers in the recesses of the uneven surface.

[0064] As will be described later in the explanation of the manufacturing method, the binary or ternary eutectic structure begins to crystallize after the Al phase or Al-Zn phase has crystallized. The crystallization of these eutectic structures is thought to begin with nucleation in the region of the coating layer on the steel material side, more specifically, on the surface of the Fe-Al-based interface alloy layer. The crystallization of the eutectic structure is thought to progress toward the surface of the coating layer. Therefore, it is thought that most of the binary or ternary eutectic structure according to this embodiment exists continuously from the surface of the coating layer to the Fe-Al-based interface alloy layer.

[0065] However, when the internal structure of the coating layer is observed at any cross section, the entire binary or ternary eutectic structure is not always observed in a continuous form from the surface of the coating layer to the Fe-Al-based interfacial alloy layer. This is because the individual shapes of the blocky binary or ternary eutectic structures are irregular, and the form of the binary or ternary eutectic structure appears different depending on the position of the cross section.

[0066] According to the investigations conducted by the present inventors, if it is observed that at least a portion of a plurality of massive binary or ternary eutectic structures exists continuously from the surface of the plating layer to a position halfway through the average thickness of the plating layer, then it is highly likely that most of the binary or ternary eutectic structures exist in a continuous form from the surface of the plating layer to the Fe-Al-based interface alloy layer, and this is presumed to result in improved paint adhesion.

[0067] In this embodiment, the number of locations where the binary eutectic structure or ternary eutectic structure exists continuously from the surface of the plating layer to a position half the average thickness of the plating layer is preferably 1 to 15 locations per rectangular region on the surface of the plating layer with long sides of 500 μm and short sides of 150 μm. A number of locations less than 1 is not preferred because it results in insufficient paint adhesion. Furthermore, when the above formula (2) is satisfied, the number of such locations is preferably 3 to 15 locations. Furthermore, when the above formula (3) is satisfied, the number of such locations is preferably 5 to 15 locations.

[0068] The presence of a binary or ternary eutectic structure is confirmed as follows. A rectangular region with a long side of 500 μm and a short side of 150 μm is set on the surface of the plating layer. The location of this region is determined by the same means as the observation field for evaluating the roughness of the uneven surface of the plating layer, as described above. Within this region, the number and locations of binary or ternary eutectic structures exposed on the surface of the plating layer are confirmed. Next, the surface of the plating layer including this region is ground sequentially to depths of ¼, ½, ¾, and 9 / 10 of the average thickness of the plating layer, and then mirror-polished to obtain an observation surface. Then, the number and locations of binary or ternary eutectic structures on the observation surface at each of the ¼, ½, ¾, and 9 / 10 depths are confirmed. Then, the number of binary or ternary eutectic structures that appear at the same position is counted on the surface of the plating layer, at the 1 / 4 depth position, and at the 1 / 2 depth position. Whether or not a structure appears at the same position can be determined by counting the number of eutectic structures that appear at the same position if the eutectic structure is within a projection range of a radius of 15 μm from the center of gravity of the eutectic structure on the surface of the plating layer. Binary or ternary eutectic structures that appear at the same position are determined to exist continuously from the surface of the plating layer to a position half the average thickness of the plating layer. There are no particular limitations on the grinding method, but examples include precision machining such as polishing and focused ion beam machining (FIB machining).

[0069] Furthermore, it is confirmed whether a binary eutectic structure or a ternary eutectic structure appears at the same position at all of the plating layer surface, 1 / 4 depth, 1 / 2 depth, 3 / 4 depth, and 9 / 10 depth. As a result, it is determined that a binary eutectic structure or a ternary eutectic structure appearing at the same position exists continuously from the plating layer surface to the Fe-Al-based interface alloy layer.

[0070] The average thickness of the plating layer is defined as the average thickness of the plating layer in a rectangular region with long sides of 500 μm and short sides of 150 μm. The position at a height corresponding to the average thickness of the plating layer from the position of the interface between the steel material and the plating layer is estimated as the average surface position of the plating layer, and the ¼, ½, ¾, and 9 / 10 depths of the average thickness of the plating layer are determined based on the estimated surface position.

[0071] Furthermore, to confirm the presence of a binary eutectic structure or a ternary eutectic structure, if there is a portion in the adhesively bonded structure that is not bonded to the plated steel material and where the plating layer is exposed, that portion can be cut out to prepare a sample for confirming its presence. Furthermore, if the entire surface of the plated steel material in the adhesively bonded structure is bonded, the bonded portion can be carefully separated to expose the plating layer, and that portion can be cut out to prepare a sample for confirming its presence.

[0072] When the plating layer contains 0.05 to 0.5% Sn, the plating layer contains Mg 2 It is preferable that the Sn phase is contained. 2 Since the Sn phase is present in a small amount, its presence can be detected and confirmed by X-ray diffraction measurement using the θ-2θ method. 2 The inclusion of the Sn phase further improves the corrosion resistance of the edge of the plating layer. 2 X-ray diffraction measurement for detecting the Sn phase may be carried out by the θ-2θ measurement method.

[0073] The coating weight of the plating layer per side is, for example, 20 to 200 g / m 2 The amount of adhesion per side should be within the range of 20 g / m 2 By setting the coating weight per side to 200 g / m or more, the flat surface corrosion resistance and edge corrosion resistance of the plated steel material can be further improved. 2 By setting the following, the workability of the plated steel material can be further improved.

[0074] <<Coating portion 22>> Next, the coating portion 22 will be described. The plated steel material 21 according to this embodiment may have the coating portion 22 disposed on at least a portion of the plating layer. The coating portion 22 will be described below with reference to FIGS. 2-1 and 2-2.

[0075] Figure 2-1 is an enlarged schematic diagram of the adhesive region of the adhesive bonded structure shown in Figure 1-1, and is a schematic diagram for explaining the positional relationship between the coating portion 22, the adhesive layer 4, the first member 2, and the second member 3, as well as the organic compound phase contained in the coating portion 22.

[0076] FIG. 2-1 shows a state in which a coating portion 22 is formed on at least a portion of the surface of the plating layer of a plated steel material 21. At least a portion of the coating portion 22 is in contact with the adhesive layer 4, and the first member 2 is bonded to the second member 3 by the adhesive layer 4 via the coating portion 22. The coating portion 22 includes an organic resin phase containing at least one of a urethane group, an epoxy group, and an ester group, and an organic compound phase consisting of an organosilicon compound. The organosilicon compound of this embodiment includes a Si-C bond. The organosilicon compound of this embodiment also includes at least one of a Si-O bond and a Si-OH bond. That is, the organosilicon compound of this embodiment includes a Si-C bond and at least one of a Si-O bond and a Si-OH bond. The configuration of the coating portion 22 will be described in detail below.

[0077] As described above, the coating portion 22 according to this embodiment includes an organic resin phase containing one or more of a urethane group, an epoxy group, and an ester group, and an organic compound phase consisting of an organosilicon compound. More specifically, as shown schematically in FIG. 2-1 , in the coating portion 22, the organic resin phase having the specific functional groups exists mainly as resin particles 221, and has a structure in which the resin particles 221 are dispersed in an organic compound phase 223 consisting of an organosilicon compound. Note that the second member 3 includes, for example, a plated steel material 31 and a coating portion 32, and in the coating portion 32, resin particles 321 are dispersed in an organic compound phase 323, similar to the coating portion 22.

[0078] The presence of the organic compound phase 223, which is made of an organosilicon compound, in the coating portion 22 forms a chemical bond known as an Si-O-Me bond with the elements constituting the plating layer 12 of the plated steel material 21. Here, Me is a metal element that is the main component of the plating layer 12, i.e., Zn, Al, Mg, or Fe. The formation of such a primary bond strengthens the bond between the plating layer 12 of the plated steel material 21 and the coating portion 22, further improving adhesion between the plating layer 12 and the coating portion 22. As a result, water is less likely to penetrate the interface between the plating layer 12 and the coating portion 22 from the outside. This improves the adhesion durability between the plated steel material 21 and the adhesive layer 4 in the adhesive-bonded structure 1 according to this embodiment.

[0079] In the coating portion 22, the total volume ratio of the organic compound phase 223 and the inorganic compound phase is preferably 16 vol% to 84 vol% with respect to the total volume of the coating portion 22. When the total volume ratio of the organic compound phase 223 and the inorganic compound phase is 16 vol% or more with respect to the total volume of the coating portion 22, Si—O—Me bonds are sufficiently formed. When the volume ratio of the organic compound phase 223 and the inorganic compound phase is 84 vol% or less with respect to the total volume of the coating portion 22, the adhesion between the adhesive layer 4 and the coating portion 22 is further improved. The total volume ratio of the organic compound phase 223 and the inorganic compound phase is preferably 20 vol% or more, more preferably 30 vol% or more. The total volume ratio of the organic compound phase 223 and the inorganic compound phase is preferably 80 vol% or less, more preferably 70 vol% or less. When determining the total volume ratio of the organic compound phase 223 and the inorganic compound phase from the cross section of the coating portion 22, the total area ratio of the organic compound phase 223 and the inorganic compound phase to the cross-sectional area of ​​the coating portion 22 is determined to be the total volume ratio of the organic compound phase 223 and the inorganic compound phase.

[0080] In the coating portion 22, the volume fraction of the organic compound phase 223 is preferably 16 vol% to 84 vol% relative to the total volume of the coating portion 22. When the volume fraction of the organic compound phase 223 is 16 vol% or more relative to the total volume of the coating portion 22, Si—O—Me bonds are sufficiently formed. When the volume fraction of the organic compound phase 223 is 84 vol% or less relative to the total volume of the coating portion 22, the adhesion between the adhesive layer 4 and the coating portion 22 is improved. The volume fraction of the organic compound phase 223 is preferably 20 vol% or more, more preferably 30 vol%. The volume fraction of the organic compound phase 223 is preferably 80 vol% or less, more preferably 70 vol%. When determining the volume fraction of the organic compound phase 223 from the cross section of the coating portion 22, the volume fraction of the organic compound phase 223 is determined as the area fraction of the organic compound phase 223 relative to the cross-sectional area of ​​the coating portion 22.

[0081] The coating portion 22 may contain an inorganic compound phase made of an inorganic silicon compound. The volume fraction of the inorganic compound phase is preferably 10 vol% or less relative to the total volume of the coating portion 22. A volume fraction of the inorganic compound phase of 10 vol% or less further enhances adhesion between the metal portion 21 and the coating portion 22. The coating portion 22 does not necessarily contain an inorganic compound phase, so the lower limit is 0 vol%. When the coating portion 22 contains an inorganic compound, the strength of the coating portion 22 is improved, thereby improving adhesive strength. Examples of inorganic silicon compounds constituting the inorganic compound phase include colloidal silica and fumed silica. When determining the volume fraction of the inorganic compound phase from the cross-section of the coating portion, the area fraction of the inorganic compound phase relative to the cross-sectional area of ​​the coating portion 22 is determined as the volume fraction of the inorganic compound phase. The inorganic silicon compound is determined, for example, by performing elemental analysis on the cross-section of the coating portion using an electron probe microanalyzer (EPMA) and determining its constituent elements. The volume proportion of the inorganic silicon compound or the organic silicon compound is determined by observing the cross section of the material with a scanning electron microscope (SEM) after elemental analysis and determining the volume proportion from the SEM image obtained.

[0082] Furthermore, in the coating portion 22, the resin particles 221 are dispersed in the organic compound phase 223, and these resin particles 221 have one or more functional groups selected from the group consisting of urethane groups, epoxy groups, and ester groups. These functional groups are also present in large amounts in the resins that make up the adhesive, so when the coating portion 22 contains resin particles 221 having such functional groups, the adhesion at the interface between the coating portion 22 and the adhesive layer 4 is improved. As a result, a state is achieved in which water is less likely to penetrate the interface between the coating portion 22 and the adhesive layer 4 from the outside. This makes it possible to improve the adhesion durability between the coating portion 22 and the adhesive layer 4 in the adhesive bonded structure 1 according to this embodiment.

[0083] As described above, since the coating portion 22 contains an organic resin phase and an organic compound phase 223, the adhesion at the two interfaces in the coating portion 22 (the interface between the coating portion 22 and the metal portion 21, and the interface between the coating portion 22 and the adhesive layer 4) is improved, and the adhesive durability of the adhesive bonded structure 1 can be improved.

[0084] Here, the resin particles 221 constituting the organic resin phase as described above are not particularly limited as long as they are resin particles having one or more functional groups selected from the group consisting of a urethane group, an epoxy group, and an ester group. The resin particles 221 may be either a water-dispersible water-based resin that disperses in water or a solvent-based resin that disperses in an organic solvent, but a water-based resin is preferred from the viewpoints of production cost and environmental friendliness. The resin constituting the resin particles 221 is preferably a resin having a main skeleton containing carbon atoms.

[0085] Examples of water-based resins include water-dispersible resins such as urethane resin, epoxy resin, polyester resin, and mixed resins of two or more of these resins. When using polyester resin, the molecular weight is preferably 10,000 to 30,000. If the molecular weight is less than 10,000, it may be difficult to ensure sufficient processability. On the other hand, if the molecular weight exceeds 30,000, the bonding sites of the resin itself may decrease, making it difficult to ensure excellent adhesion to the adhesive layer 4. Furthermore, when crosslinking is performed using a curing agent such as melamine, the crosslinking reaction may not proceed sufficiently, resulting in a decrease in performance as the coating portion 22. In the case of urethane resin, the urethane resin is preferably in the form of an emulsion with an emulsion particle size of 10 to 100 nm (preferably 20 to 60 nm). Emulsion particle sizes that are excessively small may be costly. On the other hand, emulsion particle sizes that are excessively large may result in large gaps between emulsion particles when formed into a coating, thereby reducing the barrier properties of the coating portion 22. Examples of the type of urethane resin include ether-based, polycarbonate-based, and ester-based resins, which may be used alone or in combination.

[0086] On the other hand, examples of solvent-based resins include polyester resins, urethane resins, epoxy resins, and mixed resins of two or more of these resins.

[0087] The resin contained in the coating portion 22 may be a cross-linked resin having a cross-linked structure, or may be a non-cross-linked resin having no cross-linked structure. Preferred cross-linking agents (curing agents) that impart a cross-linked structure to the resin include melamine, isocyanate, silane compounds, zirconium compounds, and titanium compounds.

[0088] The amount of crosslinking agent added is preferably 5 to 30 parts by mass per 100 parts by mass of resin solids. If the amount of crosslinking agent added is less than 5 parts by mass, the crosslinking reaction with the resin may be reduced, resulting in insufficient performance as a coating film. On the other hand, if the amount of crosslinking agent added is more than 30 parts by mass, the crosslinking reaction may proceed too far, causing the coating portion 22 to become excessively hard and reducing processability. Furthermore, when a silane compound, zirconium compound, or titanium compound is used as a crosslinking agent, adding more than 30 parts by mass of crosslinking agent may further reduce paint stability, which is not preferred.

[0089] The particle shape of the resin particles 221 is not particularly limited, and can be, for example, a shape close to a sphere, such as a spherical shape, a pseudo-spherical shape (e.g., an ellipsoidal shape, an egg shape, a rugby ball shape, etc.), or a polyhedral shape (e.g., a soccer ball shape, a dice shape, or the brilliant cut shape of various gemstones, etc.), an elongated shape (e.g., a rod shape, a needle shape, a fiber shape, etc.), or a planar shape (e.g., a flake shape, a plate shape, a thin piece shape, etc.).

[0090] In the coating portion 22 according to this embodiment, the average particle size of the resin particles 221 is preferably, for example, 20 nm or more. Having an average particle size of the resin particles 221 of 20 nm or more is preferable because it can more reliably improve the affinity with the adhesive layer 4 as described above. The average particle size of the resin particles 221 is more preferably 30 nm or more, and even more preferably 50 nm or more. On the other hand, having an average particle size of the resin particles 221 of less than 200 nm is preferable because it can form a denser resin barrier layer and further improve the adhesion between the coating portion 22 and the adhesive layer 4. The average particle size of the resin particles 221 is more preferably 180 nm or less, and even more preferably 150 nm or less.

[0091] Here, the "average particle size" of the resin particles 221 refers to the average primary particle size when the resin particles 221 exist singly in the coating portion 22, and refers to the average secondary particle size representing the particle size of the resin particles in the aggregated state when the resin particles 221 exist in an aggregated state. The average particle size of the resin particles 221 is preferably determined by the following measurement method.

[0092] First, the adhesive bonded structure 1 is cut at a location where the coating portion 22 is disposed to expose the cross section, which is then polished to obtain a cross-sectional sample in the thickness direction of the coating portion 22 of the first member 2. Next, the coating portion 22 of the cross-sectional sample is observed with a scanning electron microscope to obtain an observation image of the cross section of the coating portion 22. Ten resin particles 221 present in the field of view of the observation image are randomly selected, and the equivalent circle diameter of each resin particle 221 is measured. The equivalent circle diameter of the resin particles 221 is taken as the average of the 10 resin particles 221.

[0093] Here, whether or not the coating portion 22 according to this embodiment contains at least one of a urethane group, an epoxy group, and an ester group can be determined by the following method. Similarly, whether or not the coating portion 22 contains an Si-C bond and at least one of an Si-O bond and an Si-OH bond can be determined by the following method.

[0094] First, the area of ​​the adhesive bonded structure 1 where the coating portion 22 is disposed is cut obliquely to expose the cross section, which is then polished to obtain a cross-sectional sample in the thickness direction of the coating portion 22 of the first member 2. Next, the coating portion 22 of the cross-sectional sample is analyzed using a micro-IR spectrometer, and a judgment is made based on whether vibration peaks derived from urethane groups, epoxy groups, ester groups, Si—O bonds, Si—C bonds, and Si—OH bonds are observed in the infrared absorption spectrum of the obtained coating portion 22. Specifically, in the obtained infrared absorption spectrum, -1 When a peak is observed around 1550 cm, it is determined that the compound contains an epoxy group. -1 Around 1740 cm -1 When a peak is observed in the vicinity of 1720 to 1740 cm, it is determined that the compound contains a urethane group. -1 When a peak is observed around 1250 to 1260 cm, it is determined that the compound contains an ester group. -1 When a peak is observed in the vicinity of 1000 to 1100 cm, it is determined that the compound contains Si-C bonds. -1 When a peak is observed in the vicinity of 3650-3690 cm, it is determined that the compound contains an Si—O bond. -1If a peak is observed near this point, it is determined that the coating portion 22 contains Si—OH bonds. Note that the cutting angle in the oblique cutting may be any angle as long as the coating portion 22 can be sufficiently enlarged.

[0095] Furthermore, in a cross section of the coating portion 22 according to this embodiment taken along the thickness direction (e.g., a cross section as shown in FIG. 3 ), the area ratio of the resin particles 221 preferably occupies 16% or more of the cross-sectional area of ​​the coating portion 22. That is, in the cross section, the area ratio of the resin particles 221 is preferably 16% or more of the cross-sectional area of ​​the coating portion 22. By making the area ratio of the resin particles 221 16% or more, it is possible to more reliably improve the affinity with the adhesive layer 4 as described above. The area ratio of the resin particles 221 in the cross section of the coating portion 22 is more preferably 30% or more, and even more preferably 40% or more. On the other hand, by making the area ratio of the resin particles 221 in the cross section 84% or less, it is possible to more reliably maintain the adhesion between the coating portion 22 and the metal portion 21 while further improving the affinity between the coating portion 22 and the adhesive layer 4. The area ratio of the resin particles 221 in the cross section of the coating portion 22 is more preferably 80% or less, and even more preferably 70% or less.

[0096] The area ratio of the resin particles 221 in the cross section of the coating 22 is preferably determined by the following measurement method. First, the portion of the adhesive bonded structure 1 where the coating 22 is disposed is cut to expose the cross section, which is then further polished to obtain a cross-sectional sample in the thickness direction of the coating 22 of the first member 2. Next, a thin-film sample for TEM observation is prepared from the coating 22 portion of the cross-sectional sample using FIB-microsampling and cryo-FIB-microsampling. The obtained thin-film sample for TEM observation is then observed using an FE-TEM, which is capable of analyzing microscopic areas. Five locations, each of which is divided equally in the width direction, are observed. At each observation location, EDS analysis (element mapping) is performed on the cross section near the interface between the metal portion and the adhesive layer to obtain elemental maps of C, O, and Si. The obtained elemental map is then binarized for C and other elements to calculate the average particle size and area ratio of the resin particles in the coating.

[0097] Furthermore, the organic compound phase 223 according to this embodiment is not particularly limited as long as it is an organosilicon compound containing a Si-C bond and at least one of a Si-O bond and a Si-OH bond, and it is preferable to use, for example, an organosilicon compound having a glycidoxy group or a mercapto group. By using an organosilicon compound having a glycidoxy group or a mercapto group as the organosilicon compound, it is possible to more reliably and more favorably form the Si-O-Me bond as described in detail below, and it is possible to more reliably achieve long-term adhesive durability. In addition to organosilicon compounds having glycidoxy or mercapto groups, organosilicon compounds having, for example, amino, vinyl, or methacryl groups may also be present. However, the inventors' investigations have revealed that when organosilicon compounds having amino, vinyl, or methacryl groups are used, the reaction between the organosilicon compound and the resin constituting the organic resin phase inside the coating 22 is more accelerated than the reaction at the interface between the metal portion 21 and the coating 22, making it difficult to achieve long-term adhesion durability. Therefore, from the perspective of achieving long-term adhesion durability by preventing the penetration of electrolytes such as water, it is preferable to use organosilicon compounds having glycidoxy or mercapto groups. As the organosilicon compound having a glycidoxy or mercapto group, commercially available organosilicon compounds that meet the conditions may be used, or organosilicon compounds prepared by organic synthesis may be used.

[0098] Here, in the coating 22 according to this embodiment, when the coating 22 is analyzed by time-of-flight secondary ion mass spectrometry (TOF-SIMS) while Ar sputtering the coating 22 from the adhesive layer 4 side toward the plating layer 12 side so as to include any location at the interface between the coating 22 and the plating layer 12 of the plated steel material 21, the following analysis results are preferably obtained. That is, in the TOF-SIMS analysis results, it is preferable that a peak corresponding to a Si-O-Me bond (Me: Zn, Al, Mg, Fe constituting the plating layer 12) is observed, and the count value of the peak indicating the Si-O-Me bond is 15 or more. Furthermore, it is preferable that the Total ion correction value (the value obtained by dividing the peak count number of the Si-O-Me bond by the sum of the count numbers of all detected secondary ions) has an Intensity (a.u.) of 1.0×10 -3 Specifically, the value obtained by dividing the count value of the peak showing the Si—O—Me bond by the total count value of all secondary ions detected in the mass scanning range m / z = 0 to 300 (Total Ion corrected value) is preferably 1.0 × 10 -3 It is preferable that this is equal to or greater than this.

[0099] Here, the peak corresponding to the Si—O—Me bond is observed at a position characteristic of each element Me, depending on the specific type of element Me. For example, when Me=Fe, a representative peak corresponding to the Si—O—Fe bond is observed at a position of mass (m / z) 100±0.1 in the TOF-SIMS analysis results, when Me=Zn, a representative peak corresponding to the Si—O—Zn bond is observed at a position of mass (m / z) 108±0.1 in the TOF-SIMS analysis results, when Me=Al, a representative peak corresponding to the Si—O—Al bond is observed at a position of mass (m / z) 71±0.1 in the TOF-SIMS analysis results, and when Me=Mg, a representative peak corresponding to the Si—O—Mg bond is observed at a position of mass (m / z) 68±0.1 in the TOF-SIMS analysis results.

[0100] These analysis results show that the reaction of forming Si—O—Me bonds proceeds efficiently at the interface between the plating layer 12 and the coating portion 22, and that a certain amount or more of Si—O—Me bonds are formed at the interface between the plating layer 12 and the coating portion 22. By forming a certain amount or more of Si—O—Me bonds at the interface between the plating layer 12 and the coating portion 22, even when the adhesively bonded structure 1 is exposed to a humid environment, it is possible to prevent water from penetrating the interface between the plated steel material 21 and the coating portion 22, and adhesive durability is maintained for a longer period of time.

[0101] The count value indicating the Si—O—Me bond as described above is more preferably 20 or more, and even more preferably 30. The Total Ion correction value is more preferably 1.3×10 -3 More preferably, it is 2.0 × 10 -3 It is preferable that:

[0102] The count value of the peak corresponding to the Si—O—Me bond at the interface between the plating layer 12 and the coating portion 22 can be measured as follows. First, the adhesive bond between the plating layer 12 and the coating portion 22 is cut at a 5-degree incline from the adhesive layer 4 side toward the plating layer 12 side using an oblique cutting device (SAICAS), and a sample is prepared by thinning the adhesive layer to approximately 1 μm using Ar sputtering. The portion of the adhesive layer thinned to approximately 1 μm is analyzed by TOF-SIMS while Ar sputtering is performed from the adhesive layer side toward the plating layer 12 side. After sputtering with an Ar beam from the surface to a certain depth, TOF-SIMS measurement is performed. Then, similar Ar sputtering and TOF-SIMS measurement are performed repeatedly to obtain the depth distribution of various elements and bonds. The primary ion species is Au. 3 + The acceleration voltage was 30 kV, and the sputtering rate was about 80 nm / min (SiO 2 The measurement area is 50 μm×50 μm.

[0103] Since each ion has a specific mass number, the above TOF-SIMS measurement measures the depth profile of the theoretical mass number of the target Si—O—Me bond. From the depth profile of the mass corresponding to the Si—O—Me bond, as well as the depth profiles of Me ions, which are the main component of the metal part, and C ions, which are the main component of the resin, the region from the rising portion of the count value of Me ions and the falling portion of the count value of C ions to the region where the count number of C ions becomes almost constant is considered to be the interface, and the count value corresponding to the Si—O—Me bond at this interface is measured.

[0104] The area ratio of the resin particles 221 and the count value of the Si—O—Me bonds in TOF-SIMS as described above can be set within a desired range when forming the coating portion 22 according to this embodiment by appropriately adjusting the selection and content of the raw materials for the organic resin phase and the raw materials for the organic compound phase 223, and by appropriately controlling the surface condition of the plating layer 12.

[0105] Other Components In addition to the components described above, the coating portion 22 may contain other additives, such as well-known additives such as oxide particles, extender pigments, solid lubricants, rust inhibitors, leveling agents, viscosity imparting agents, pigment anti-settling agents, and antifoaming agents.

[0106] <Average Thickness of Coating Portion 22> In the present embodiment, the average thickness of the coating portion 22 as described above is preferably 0.2 μm or more per side of the first member 2 (in other words, per side of the plated steel material 21). By making the average thickness of the coating portion 22 per side 0.2 μm or more, the above-described effects of providing the coating portion 22 can be more reliably achieved. The average thickness of the coating portion 22 per side is more preferably 0.4 μm or more, and even more preferably 0.5 μm or more. On the other hand, by making the average thickness of the coating portion 22 per side 1.5 μm or less, it is possible to ensure conductivity to the plating layer 12 via the coating portion 22. For example, it is possible to perform electrodeposition coating on the plating layer 12 via the coating portion 22 or spot welding on the plating layer 12 via the coating portion 22. The average thickness of the coating portion 22 per surface is more preferably 1.2 μm or less, and even more preferably 1.0 μm or less.

[0107] The average thickness of the coating portion 22 can be measured as follows. First, the portion of the adhesive bonded structure 1 where the coating portion 22 is disposed is cut in the thickness direction of the coating portion 22 to expose the cross section, and the cross section is further polished to obtain a cross-sectional sample of the coating portion 22 of the first member 2 in the thickness direction. Next, the coating portion 22 portion of the cross-sectional sample is observed with a scanning electron microscope to obtain an observation image of the cross section of the coating portion 22. For the coating portion 22 present in the field of view of the observation image, the thickness is measured at five positions that divide the field of view into five equal parts in the width direction, and the average value is calculated. The average thickness of the coating portion 22 is the average of the values ​​obtained in the five fields of view. In other words, the average thickness of the coating portion 22 is the average of the thicknesses at a total of 25 positions.

[0108] A known chemical conversion coating may be formed on the portion of the first member 2 that is not in contact with the adhesive layer 4 described above.

[0109] Figure 2-2 is a partially enlarged cross-sectional view of the adhesive region of the adhesive bonded structure shown in Figure 1-1, and is an enlarged cross-sectional view showing the configuration of the plating layer 12, coating portion 22, and adhesive layer 4 of the plated steel material 21 (first member 2).

[0110] 2-2, the thickness of the coating portion 22 is small compared to the unevenness of the surface of the plating layer 12, and the coating portion 22 does not completely fill in the recesses of the uneven surface, so that the surface configuration of the coating portion 22 reflects the unevenness of the surface of the plating layer 12. When an adhesive layer 4 is further laminated on the coating portion 22, the adhesive layer 4 penetrates into the recesses in the surface of the plating layer 12. This produces a so-called anchor effect, further increasing the adhesive strength of the adhesive layer 4.

[0111] <Regarding the second member 3> In the present embodiment, the second member 3 may be the same as the first member 2. That is, the second member 3 may have the above-described steel material 11 and the above-described plating layer 12 disposed on a portion of the surface of the steel material 11, and may further have a coating portion 22.

[0112] The second member 3 may also be made of a galvannealed steel material. In this case, the adhesive layer is bonded to the surface of the galvannealed layer of the galvannealed steel material. In addition, when the second member 3 is made of a galvannealed steel material, the coating portion 22 may be disposed on the surface of the galvannealed layer. In this case, the adhesive layer is bonded to the surface of the galvannealed layer via the coating portion 22. A galvannealed steel material is made by galvanizing a steel material and then alloying it to diffuse iron into the galvanizing, and is therefore more suitable as the second member 3 because it further suppresses deterioration in strength of the adhesive over time.

[0113] When the plating layer of the galvannealed steel material contains 7 to 15 mass% Fe, 0.05 to 0.5 mass% Al, and the remainder Zn and impurities, the adhesive strength of the adhesive is less likely to decrease over time, making it more suitable for the second member 3. In this embodiment, the galvannealed layer refers to a plating layer primarily composed of an Fe-Zn alloy formed when Fe in the steel diffuses into the Zn plating due to an alloying reaction. The Fe content is not particularly limited, but if the Fe content in the galvannealed layer is less than 7 mass%, a soft Zn-Fe alloy is formed on the plating surface, degrading press formability. If the Fe content exceeds 15 mass%, a brittle alloy layer develops at the interface with the base steel, degrading plating adhesion. Therefore, an Fe content of 7 to 15 mass% is appropriate in the galvannealed layer. In addition, when continuous hot-dip galvanizing is performed, Al is generally added to the plating bath in order to control the alloying reaction in the plating bath, so the plating contains 0.05 to 0.5 mass % of Al. In the alloying process, elements added to the steel diffuse simultaneously with the diffusion of Fe, so these elements are also contained in the plating.

[0114] The second member 3 may also be made of a fiber-reinforced plastic material. In this case, the second member 3 does not need to have the above-described coating portion 22. Fig. 3 shows an enlarged schematic diagram of a cross section of an adhesive bonded structure consisting of a second member without a coating portion 22 and a first member with a coating portion 22. Fig. 3 is a schematic diagram illustrating the positional relationship between the coating portion 22A, adhesive layer 4A, first member 2A, and second member 3A, as well as the organic compound phase contained in the coating portion 22A.

[0115] The adhesive-bonded structure 1A shown in Figure 3 has a first member 2A and a second member 3A, which are bonded together by an adhesive layer 4A. The first member 2A has a plated steel material 21A and a coating portion 22A formed on the surface of the plating layer of the plated steel material 21A. The coating portion 22A contains resin particles 221 and an organic compound phase 223. The second member 3A is bonded to the first member 2A via the adhesive layer 4A. Unlike the above-described embodiment, the second member 3A does not have a coating portion 32.

[0116] In this case, the fiber reinforced plastic material of the second member 3A is made of fiber reinforced plastics (FRP) which is a composite material made by incorporating reinforcing fibers into a matrix resin. Examples of reinforcing fibers used in fiber reinforced plastics include glass fiber and carbon fiber.

[0117] Furthermore, the second member 3 may be made of an aluminum alloy material. Using an aluminum alloy material for the second member 3 is preferable because it achieves weight reduction of the adhesive bonded structure. Examples of aluminum alloys include aluminum alloys containing one or more of Si, Fe, Cu, Mn, Mg, Cr, Zn, Ti, V, Zr, Pb, and Bi. Examples of materials for the second member 3 include commonly known aluminum alloys such as the 1000 series, 2000 series, 3000 series, 4000 series, 5000 series, 6000 series, and 7000 series described in JIS H4000:2006. Aluminum alloys such as the 5000 series and 6000 series, which have strength and formability, are suitable for the second member 3.

[0118] Furthermore, the second member 3 may be made of a magnesium alloy material. Examples of magnesium alloys that can be used for the second member 3 include magnesium alloys containing one or more of Al, Zn, Mn, Fe, Si, Cu, Ni, Ca, Zr, Li, Pb, Ag, Cr, Sn, Y, Sb, and other rare earth elements. Generally known magnesium alloys such as the AM series containing Al as specified in the ASTM standard, the AZ series containing Al and Zn, and the ZK series containing Zn can be used.

[0119] In either case, the adhesive bonded structure 1A has excellent adhesion durability.

[0120] <Regarding Adhesive Layer 4 > The adhesive layer 4 is disposed between the first member 2 and the second member 3 in the adhesive region 5 and bonds the first member 2 and the second member 3 together.

[0121] The adhesive layer 4 is mainly composed of an adhesive. The effect of the coating portion 22 described above is not impaired by the type of adhesive that constitutes the adhesive layer 4. Therefore, the adhesive that can be used for the adhesive layer 4 is not particularly limited, and examples that can be used include epoxy resin adhesives, polyester resin adhesives, urethane resin adhesives, adhesives obtained by mixing these adhesives with rubber or elastomer, and adhesives that have been made conductive. Among the above, from the viewpoint of initial adhesive strength, it is preferable that the adhesive layer 4 contain an epoxy resin adhesive or a urethane resin adhesive (i.e., a thermosetting adhesive).

[0122] Furthermore, it is preferable that the resin of the adhesive constituting the adhesive layer 4 has a common chemical structure with at least one of the resins in the coating portion 22 and the resins in the coating portion 32. This makes it possible to further improve the initial adhesion between the adhesive layer 4 and the coating portion 22 and the coating portion 32, and to further increase the adhesive strength of the adhesive bonded structure 1.

[0123] For example, the resin of the adhesive constituting the adhesive layer 4 may have a common main skeleton with at least one of the resin in the coating portion 22 and the resin in the coating portion 32. Alternatively, the resin of the adhesive constituting the adhesive layer 4 may have a common side chain functional group with at least one of the resin in the coating portion 22 and the resin in the coating portion 32.

[0124] The adhesive bonded structure 1 according to this embodiment has been described in detail above. According to this embodiment, at least the first member 2 is made of a plated steel material 21, the surface of the plating layer 12 of this plated steel material 21 is made uneven, and at least a portion of the multiple blocky binary eutectic structures or multiple blocky ternary eutectic structures contained in the plating layer is continuously present from the surface of the plating layer to a position halfway through the average thickness of the plating layer. This improves the adhesion of the adhesive layer 4 to the plating layer 12 and improves adhesion durability. Furthermore, because the plating layer is a Zn-Al-Mg hot-dip plating layer, it exhibits particularly excellent edge detection properties. Therefore, the adhesive bonded structure 1 according to this embodiment exhibits excellent adhesion durability and corrosion resistance.

[0125] Furthermore, the resin particles 221 and the organic compound phase 223 in the coating portions 22 and 32 prevent water from penetrating into the interface between the first member 2 and the adhesive layer 4 and the interface between the second member 3 and the adhesive layer 4, thereby preventing deterioration of the adhesive layer 4 and corrosion of the first member 2 and the second member 3. Therefore, the adhesive bonded structure 1 is prevented from losing its adhesive strength and has excellent adhesive durability.

[0126] (Regarding Modifications) One embodiment of the present disclosure has been described above. Below, several modification examples of the above embodiment of the present disclosure will be described. Note that each modification example described below may be applied alone to the above embodiment of the present disclosure, or may be applied in combination with the above embodiment of the present disclosure. Furthermore, each modification example may be applied in place of the configuration described in the above embodiment of the present disclosure, or may be applied in addition to the configuration described in the above embodiment of the present disclosure. Below, the differences between the above embodiment and each modification example will be mainly described, and similar points will not be described as appropriate.

[0127] The second member 3A is not limited to the above-described embodiment, and can be made of any material.

[0128] For example, in addition to the above-mentioned materials, resin materials, ceramic materials, etc. can be used as materials for the second member 3A.

[0129] The second member 3 may also be made of a steel material other than those described above. The steel material may be subjected to any surface treatment. Examples of surface treatment include, but are not limited to, various plating treatments such as zinc-based plating, aluminum-based plating, and tin-based plating; chemical conversion treatments such as zinc phosphate treatment, chromate treatment, and chromate-free treatment; and physical surface roughening treatments such as sandblasting or chemical surface roughening treatments such as chemical etching. Furthermore, multiple types of surface treatments may be applied. It is preferable that the surface treatment be at least a treatment aimed at imparting rust prevention properties.

[0130] Among steel materials, plated steel materials that have been subjected to plating treatment are particularly preferable as the metal part 21 because of their excellent corrosion resistance. Examples of plated steel materials that are particularly preferable as the metal part 21 include zinc-based plated steel materials, Ni-plated steel materials, alloyed Ni-plated steel materials obtained by heat-treating these steel materials to diffuse Fe into the Ni plating, Al-plated steel materials, tin-plated steel materials, and chromium-plated steel materials.

[0131] Among the various plated steel materials as described above, zinc-based plated steel sheet is suitable for the metal portion 21 because of its excellent corrosion resistance.

[0132] Furthermore, when the second member 3 is an electrogalvanized steel material, it may be a steel material plated only with zinc (generally called EG), or a zinc-nickel electroplated steel material. Furthermore, the hot-dip galvanized steel material may be one generally called GI, which contains 0.2% Al in the zinc plating layer, or one generally called Zn-Al alloy plated steel sheet, which contains 1 to 10% Al in the zinc plating layer.

[0133] Furthermore, the shape of the adhesive bonded structure according to this embodiment is not limited to that of the above-described embodiment. The shapes of the first and second members constituting the adhesive bonded structure according to this embodiment can be any shape, and any position can be selected for the adhesive portion between the first and second members. Furthermore, the adhesive bonded structure according to this embodiment may include members other than the first and second members. Figures 4 and 5 are schematic perspective views of an adhesive bonded structure according to another modification of this embodiment, and Figure 6 is a schematic view illustrating the adhesive state of the adhesive bonded structure according to another modification of this embodiment.

[0134] The adhesive bonded structure 1B shown in FIG. 4 includes a hat-shaped first member 2B and a flat plate-shaped second member 3B. The first member 2B is bonded to the second member 3B via an adhesive layer 4 at a bonding area 5B in the flange of the first member 2B. The adhesive bonded structure 1C shown in FIG. 5 includes a hat-shaped first member 2C and a hat-shaped second member 3C, which are arranged so that their flanges face each other. The opposing flanges of the first member 2C and the second member 3C are bonded via an adhesive layer 4C to form a bonding area 5C. Furthermore, the adhesive bonded structure 1D shown in FIG. 6 includes a hem portion formed by a second member 3D covering the edge of the plate-shaped portion of the first member 2D by hemming. The first member 2D and the second member 3D are bonded to each other via an adhesive layer 4D at the hem portion.

[0135] In any of the modified examples shown in Figures 4 to 6, at least the first member 2 is made of plated steel material 21, the surface of the plating layer 12 of the plated steel material 21 is made uneven, and at least a portion of the multiple blocky binary eutectic structures or multiple blocky ternary eutectic structures in the plating layer exists continuously from the surface of the plating layer to a position that is half the average thickness of the plating layer, so that the adhesive bonded structures 1B to 1D also have excellent adhesive durability and corrosion resistance.

[0136] Furthermore, in the above-described embodiment, the first member 2 and the second member 3 are bonded only by the adhesive layer 4, but the present disclosure is not limited to this, and adhesive bonding using an adhesive layer can be combined with another bonding method (second bonding).

[0137] The second bonding method that can be combined with the adhesive bonding is not particularly limited, and any bonding method can be used, such as fusion bonding, non-fusion bonding, mechanical bonding, etc.

[0138] For example, spot welding, arc welding, laser welding, etc. can be used as the fusion joining. Fusion joining can be applied when the first member and the second member have metal parts. Note that fusion joining may be performed after removing the adhesive layer, but if the adhesive layer is conductive, it can be performed without removing the adhesive layer.

[0139] Examples of non-fusion joining include friction stir welding, diffusion welding, pressure welding, etc. Examples of mechanical joining include rivet joining and screw joining.

[0140] (Regarding Applications) Next, applications of the adhesive bonded structure according to the present disclosure will be described. The applications of the adhesive bonded structure according to the present disclosure are not particularly limited, and it can be used as a component of any machine, building, structure, etc. In particular, the adhesive bonded structure according to the present disclosure has excellent water-resistant adhesion and is relatively lightweight due to the use of an adhesive. Therefore, the adhesive bonded structure according to the present disclosure is suitable for transportation equipment parts, particularly automobile parts, which are likely to be placed in environments where they come into contact with water and for which weight reduction is always required. Therefore, in one aspect, the present disclosure also relates to an automobile part equipped with the adhesive bonded structure according to the present disclosure.

[0141] Automotive parts to which the adhesive bonded structure according to the present disclosure can be applied include, but are not limited to, closed cross-section components bonded with flanges (e.g., A-pillars, B-pillars, side sills, etc.), components in which materials are partially laminated for the purpose of reinforcement or stiffening (e.g., B-pillar reinforcement, outer panel), and panel components with hemmed portions (doors, hoods, etc.).

[0142] (Method for Manufacturing Adhesively Bonded Structure) Next, a method for manufacturing the adhesively bonded structure 1 according to this embodiment will be described.

[0143] As shown in the flowchart of Figure 7, the manufacturing method of the adhesive bonded structure 1 according to this embodiment includes a member forming process for forming each of the first member 2 and second member 3 that constitute the adhesive bonded structure 1, and an adhesive bonding process for bonding the formed first member 2 and second member 3 together using a predetermined adhesive.

[0144] <Member Forming Process> As shown in the flowchart of FIG. 7 , the member forming process includes a base material manufacturing process in which base materials for the first member 2 and the second member 3 are manufactured using the materials for the first member 2 and the second member 3; a coating portion forming process in which a coating application liquid for forming the coating portion 22 is applied to at least a portion of the base material that will become at least the first member 2, and then drying or baking is performed to form the coating portion 22; and a forming process in which the base material of the first member 2 and the base material of the second member 3, on which the coating portion 22 has been formed, are formed into a desired shape as necessary.

[0145] <<Base Material Manufacturing Process>> In the base material manufacturing process, the base materials of the first member 2 and the second member 3 are manufactured using materials for the first member 2 and the second member 3. The method for manufacturing the base material is not particularly limited, and the base material may be manufactured in accordance with a conventional method using any of various known manufacturing methods used to form a desired base material.

[0146] For example, when a zinc-based plated steel sheet is used for the first member 2 and the second member 3, a hot-rolled steel sheet or a cold-rolled steel sheet is manufactured in a conventional manner, and a zinc-based plating layer is formed on the obtained hot-rolled steel sheet or cold-rolled steel sheet in a conventional manner. Also, when other metal materials, resin materials, FRP materials, ceramic materials, etc. are used as the base material, the other metal materials, resin materials, FRP materials, ceramic materials, etc. can be manufactured in a conventional manner using various known manufacturing methods. Hereinafter, a method for manufacturing a plated steel material will be described for the case where a plated steel material is used as the first member 2.

[0147] In a method for producing a plated steel material according to this embodiment, a steel sheet is annealed in a reducing atmosphere, and the steel sheet immediately after annealing is immersed in a hot-dip galvanizing bath and then pulled out, thereby forming a coating layer on the surface of the steel sheet. Next, cooling is performed by spraying a cooling gas while the temperature of the coating layer is reduced from the bath temperature to 260°C. During this process, the oxygen concentration in the atmosphere above the surface of the coating bath and the oxygen concentration in the atmosphere from when the steel sheet is pulled out of the coating bath until cooling is completed are controlled within the range of 100 to 5000 ppm. Furthermore, the average cooling rate while the temperature of the coating layer is reduced from the bath temperature to 260°C is set to 15°C / sec or higher. Furthermore, cooling is performed by spraying a cooling gas, and the dew point of the cooling gas is set to 0°C or higher.

[0148] That is, as shown in the flowchart of FIG. 7 , the method for producing a plated steel material of this embodiment comprises the steps of: (S1) annealing a steel sheet in a reducing atmosphere; (S2) immersing the steel sheet in a hot-dip galvanizing bath; (S3) withdrawing the steel sheet from the hot-dip galvanizing bath; and (S4) spraying cooling gas onto the steel sheet to which the hot-dip galvanizing bath has adhered; (A) in the immersion S2 and withdrawal S3, the oxygen concentration in the atmosphere above the bath surface of the hot-dip galvanizing bath is set to a range of 100 to 5000 ppm; (B) in the spraying S4, the dew point of the cooling gas is set to 0°C or higher; (C) in the spraying S4, the average cooling rate until the temperature of the coating layer is reduced from the temperature of the hot-dip galvanizing bath to 260°C is set to 15°C / second or higher; and (D) in the spraying S4, the oxygen concentration in the atmosphere from when the steel sheet is withdrawn from the coating bath to when cooling is completed is set to a range of 100 to 5000 ppm. The plated steel material of this embodiment is obtained by combining all of conditions A, B, C, and D. The details of the method for producing the plated steel material will be explained below in order.

[0149] (S1 Annealing) Annealing of the steel sheet to be used as the base sheet for plating is carried out in a reducing atmosphere. The reducing atmosphere and annealing conditions are not particularly limited. By this annealing, oxides present on the surface of the steel sheet are removed as much as possible.

[0150] (S2 Immersion) Next, the steel sheet immediately after annealing is immersed in a hot-dip galvanizing bath. The chemical composition of the galvanizing bath may be appropriately adjusted so as to obtain the chemical composition of the coating layer described above. The temperature of the galvanizing bath is not particularly limited, and a temperature at which hot-dip galvanizing can be performed may be appropriately selected. For example, the temperature of the galvanizing bath may be set to a value approximately 20°C or more higher than the melting point of the galvanizing bath.

[0151] (S3 Pulling Up) Next, the steel sheet is pulled up from the coating bath. The coating weight of the coating layer can be controlled by controlling the pulling speed of the steel sheet. If necessary, the coating weight of the coating layer may be controlled by wiping the steel sheet to which the coating layer has been attached. The coating weight of the coating layer is not particularly limited and can be, for example, within the range described above.

[0152] (S4 Spraying) Next, the coating layer is cooled. Cooling is performed by spraying cooling gas onto the steel sheet immediately after it has been pulled out of the hot-dip coating bath. Cooling by spraying cooling gas is performed continuously until the temperature of the steel sheet drops from the bath temperature to 260°C. The cooling conditions below 260°C are not particularly limited, and cooling by spraying cooling gas may be performed subsequently, or the steel sheet may be allowed to cool naturally.

[0153] The oxygen concentration in the atmosphere above the surface of the coating bath and the oxygen concentration in the atmosphere from when the steel sheet is pulled out of the coating bath until cooling is completed are controlled within the range of 100 to 5000 ppm. Preferably, the oxygen concentrations in these atmospheres are within the range of 100 to 1000 ppm. When the molten metal in the coating bath that has adhered to the steel sheet solidifies, an oxide film is formed on the outermost surface of the molten metal in the early stages of solidification, and the thickness of this oxide film is affected by the oxygen concentration in the atmosphere. Once the oxide film has an appropriate thickness, it begins to follow the changes in the surface shape of the coating layer during the subsequent solidification process, forming an uneven surface that satisfies the above formula (1).

[0154] If the oxygen concentration on the surface of the coating bath and in the atmosphere from the time the steel sheet is pulled out of the coating bath until the end of cooling is less than 100 ppm, an oxide film of sufficient thickness will not be formed, making it difficult to create an uneven surface for the coating layer. Furthermore, if the oxygen concentration in the atmosphere exceeds 5000 ppm, a relatively thick and flat oxide film will be formed in the early solidification stage. This oxide film will not follow the changes in the surface shape of the coating layer during the solidification process, resulting in a flat surface for the coating layer after solidification, which will not satisfy the above formula (1). Furthermore, if the oxygen concentration in the atmosphere exceeds 5000 ppm, the oxide film will be prone to cracking, which may make it difficult to maintain the shape of the coating layer during solidification. There are no particular limitations on the means for maintaining the oxygen concentration in the atmosphere above the surface of the coating bath within the range of 100 to 5000 ppm. For example, a cover may be provided to cover the surface of the coating bath, and a gas with an oxygen concentration of 100 to 5000 ppm may be supplied to the interior of the cover. The type of gas supplied to the surface of the coating bath is not particularly limited as long as the oxygen concentration is within the range of 100 to 5000 ppm, and may be a non-oxidizing gas such as nitrogen, an inert gas such as argon, or a mixture of these. In order to maintain the oxygen concentration in the atmosphere from the time the steel sheet is pulled out of the coating bath until cooling is completed within the range of 100 to 5000 ppm, for example, the oxygen concentration of the cooling gas sprayed onto the steel sheet may be set within the range of 100 to 5000 ppm. If air is used as the cooling gas, the cooling gas will have an excessive oxygen concentration, making it impossible to obtain a suitable coating layer.

[0155] Furthermore, by setting the dew point of the cooling gas to 0°C or higher, the shape-maintaining function of the oxide coating can be maintained. If the dew point of the cooling gas is below 0°C, a plating layer whose surface shape satisfies the above formula (1) cannot be obtained. There are no particular restrictions on the type of cooling gas, as long as the oxygen concentration is within the range of 100 to 5000 ppm. The cooling gas may be a non-oxidizing gas such as nitrogen, an inert gas such as argon, or a mixture of these.

[0156] The average cooling rate during the time period from the bath temperature until the temperature of the coating layer reaches 260°C is set to 15°C / second or more. There is no particular upper limit to the average cooling rate, but it may be, for example, 200°C / second or less. By setting the average cooling rate to 15°C / second or more, primary Al crystals (Al phase) and Al-Zn phases are sufficiently crystallized in the early stage of the solidification process. The average cooling rate during the time period from the bath temperature until the temperature of the coating layer reaches 260°C is a value calculated by the following formula. The cooling time is the time from when the steel sheet is pulled out of the coating bath until the temperature of the coating layer falls to 260°C. Average cooling rate = (bath temperature - 260) ÷ cooling time

[0157] As primary Al crystals (Al phase) and Al-Zn phases are fully crystallized in the early stages of the solidification process, the amount of molten metal on the steel sheet surface decreases. Then, as the temperature of the molten metal decreases, the crystallization of binary and ternary eutectic structures begins, forming such structures as to fill the periphery of the already crystallized Al phase and Al-Zn phase. Because the crystallization of the eutectic structure begins when the remaining amount of molten metal is low, the binary and ternary eutectic structures form recesses in the coating layer. Furthermore, the crystallization of the eutectic structure primarily begins in the region of the coating layer closer to the steel sheet. More specifically, crystallization begins from nucleation on the surface of the Fe-Al interfacial alloy layer and progresses toward the surface of the coating layer. As a result, the binary and ternary eutectic structures are continuously present from the steel sheet side of the coating layer toward the surface.

[0158] In this embodiment, after the production of the plated steel material, a process for generating cracks in the plating layer may be performed. Specifically, a bending back process using a tension leveler or a skin pass process may be performed. These conditions are preferably set to impart a total elongation of 0.2 to 2.0% to the steel material, which causes cracks in the plating layer and further enhances adhesion to the adhesive layer 4.

[0159] <<Coating Portion Forming Process>> In the present embodiment, the coating portion forming process may or may not be performed. When forming the coating portion 22 on the first member 2 or the second member 3, the coating portion forming process is performed. In the coating portion forming process, for example, when forming the coating portion 22 on the plated steel material 21 as the first member 2, a coating application liquid for forming the coating portion 22 is applied to at least a portion of the plating layer 12, and then drying or baking is performed to form the coating portion 22.

[0160] Here, the method for producing the coating solution is not particularly limited, and may involve using a solvent, such as water, that is appropriate for the organic resin used, blending an organic resin containing one or more of a urethane group, an epoxy group, and an ester group, and an organosilicon compound containing a Si—C bond and at least one of a Si—O bond and a Si—OH bond, in the solvent at a desired solid volume ratio, and mixing and stirring the resulting mixture by any of a variety of known methods.

[0161] The method for applying the coating liquid for forming the coating portion 22 is not particularly limited, and various known methods can be used as appropriate. For example, when the coating liquid is a viscous liquid, the coating liquid can be applied using known methods such as application by a discharge method from a slit nozzle or a circular nozzle, brush coating, blade coating, or spatula coating. Furthermore, when a coating liquid in which the above components are dissolved in a predetermined solvent is used, various known application methods can be used, such as brush coating, spray coating, bar coating, discharge coating from nozzles of various shapes, die coater coating, curtain coater coating, roll coater coating, and inkjet coating. In addition, various known methods such as bar coaters, roll coaters, screen printing, and powder coating can be used.

[0162] When forming a coating portion on the plated steel material according to this embodiment, it is preferable to apply the coating solution within 60 minutes after the formation of the plating layer. If the time until the coating solution is applied is within 60 minutes, chemical bonds are likely to be formed between the organosilicon compound and the plating layer, and when analyzed by TOF-SIMS, the count number of the peak corresponding to the Si-O-Me bond (Me: metal element) will be 15 or more. Furthermore, if the time until the coating solution is applied is within 60 minutes, the value obtained by dividing the count number of the peak indicating the Si-O-Me bond by the sum of the count numbers of all secondary ions detected in the mass scanning range m / z = 0 to 300 (Total Ion corrected value) will be 1.0 × 10 -3 That's all.

[0163] The drying and baking can be carried out, for example, by a heat treatment etc. The heating conditions are not particularly limited, and for example, the temperature can be 80° C. or higher and 250° C. or lower, and the drying and baking time can be 5 seconds or higher and 30 minutes or lower.

[0164] <<Forming Process>> In the forming process, the first member 2 having the coating portion 22 formed thereon and the second member 3 are formed into a desired shape as needed. The forming method is not particularly limited, and a processing means for obtaining the desired shape of the formed product may be selected from known metal processing methods. Furthermore, as needed, part of the forming process may be performed simultaneously with the adhesive bonding process described below.

[0165] <Adhesive Bonding Process> The adhesive bonding process is a process of bonding the formed first member 2 and second member 3 using a predetermined adhesive. In this process, a desired adhesive is first applied to the portions of the obtained first member 2 and second member 3 to be bonded (e.g., flange portions, etc.) to form adhesive regions 5. The first member 2 and second member 3 are then laminated together via the adhesive regions 5, and the adhesive is cured by heat treatment. The method for applying the desired adhesive is not particularly limited, and may involve applying a desired adhesive or placing a desired adhesive resin sheet. This allows for the adhesive-bonded structure 1 according to this embodiment to be obtained, in which the first member 2 and second member 3 are adhesively bonded via the adhesive layer 4.

[0166] In the adhesive bonding step, various painting processes or other bonding processes may be performed as needed. For example, the bonding processes may include mechanical bonding using bolts or rivets, or welding processes such as spot welding.

[0167] More specifically, for example, when manufacturing the adhesive bonded structure 1D shown in Figure 6, adhesive can be applied to one or both sides of the flange portion that joins the formed first member 2 and second member 3, the parts where the first member 2 and second member 3 are joined are laminated via the adhesive, and the adhesive is hardened by holding at room temperature or by heat treatment.

[0168] Furthermore, for example, when a first member 2 as a metal member is reinforced with a second member 3 as a fiber-reinforced plastic, as in the adhesive-bonded structure 1 shown in Figure 1, the adhesive-bonded structure 1 can be obtained by warm-molding the first member 2 and the second member 3 in a state where they are stacked via an adhesive.

[0169] The above is a brief description of the manufacturing method of the adhesive bonded structure 1 according to the present embodiment. Note that the adhesive bonded structure according to the present disclosure is not limited to those manufactured by the above-described manufacturing method, and can be manufactured by any manufacturing method.

[0170] The present disclosure will be described in more detail below with reference to examples. Note that the examples described below are merely examples of the present disclosure and are not intended to limit the present disclosure.

[0171] <Production of Plated Steel> First, plated steel was produced by the following procedure. A cold-rolled steel sheet (0.05C-0.1Si-0.2Mn) with a thickness of 1.6 mm was used as the base sheet for plating. First, the steel sheet was annealed. The annealed steel sheet was immersed in various hot-dip coating baths and then pulled out, thereby adhering a coating layer to the steel sheet surface. Next, various plated steel sheets were produced by cooling using a cooling gas from immediately after pulling out of the coating bath until the coating layer reached 260°C. The cooling gas was mainly composed of nitrogen gas. The oxygen concentration and dew point of the cooling gas were as shown in Table 2A and Table 2B.

[0172] The annealing conditions for annealing the steel sheet in a reducing atmosphere were a soaking temperature of 800°C and a soaking time of 10 seconds. The annealing atmosphere was a reducing atmosphere consisting of a mixed gas of 5% hydrogen and the balance nitrogen. The oxygen concentration in the annealing atmosphere was 20 ppm or less. The annealed steel sheet was then air-cooled with nitrogen gas until the immersion temperature reached the bath temperature + 20°C, after which it was immersed in the hot-dip galvanizing bath for about 3 seconds and then pulled up. The pulling-up speed was 20 to 200 mm / sec. During the pulling-up, N 2 The plating deposition weight was controlled by wiping gas.

[0173] The chemical compositions of the coating layers were as shown in Tables 1A and 1B. The manufacturing conditions were as shown in Tables 2A and 2B. The morphology of the binary or ternary eutectic structure in the coating layers was also evaluated, and the results are shown in Tables 3A and 3B. Furthermore, the coating adhesion and edge corrosion resistance of the coated steel sheets were evaluated, and the results are shown in Tables 4A and 4B.

[0174] The chemical composition of the plating layer, the metal structure of the plating layer, and the unevenness of the surface of the plating layer were evaluated by the above-mentioned methods. The unevenness of the surface of the plating layer was evaluated by setting an observation field in which the longitudinal length Lo of the plating layer was within a range of 500 μm. 2 The presence or absence of Sn phase was determined by X-ray diffraction measurement of the surface of the plating layer. 2The evaluation was made based on whether or not a diffraction peak of Sn was confirmed.

[0175] <Formation of Coating Portion> Next, a coating portion was formed on a part of the plated steel material by the following procedure.

[0176] First, the following five types of chemical conversion treatment agents were prepared for forming the coating portion.

[0177] (A1) A water-dispersed emulsion type polyurethane resin SF-150 manufactured by Daiichi Kogyo Co., Ltd. and 3-glycidoxypropyltriethoxysilane were blended in a solids volume ratio of 3:2 to prepare chemical conversion treatment agent A1.

[0178] (A2) A water-dispersed emulsion type polyurethane resin SF-150 manufactured by Daiichi Kogyo Co., Ltd. and 3-glycidoxypropyltriethoxysilane were blended in a solids volume ratio of 5:1 to prepare chemical conversion treatment agent A2.

[0179] (A3) A water-dispersed emulsion type polyurethane resin SF-150 manufactured by Daiichi Kogyo Co., Ltd. and 3-glycidoxypropyltriethoxysilane were blended in a solids volume ratio of 1:5 to prepare chemical conversion treatment agent A3.

[0180] (B) Toyobo Co., Ltd.'s polyester resin Vylon GK140 was dissolved in cyclohexanone as a solvent, and the resin was mixed with Nippon Cytec Industries Co., Ltd.'s imino group-type melamine Cymel 325 so that the solids volume ratio was 5:1. A curing catalyst (Catalyst 296-9: Nippon Cytec Industries Co., Ltd.) was added in an amount of 0.1% by volume relative to the resin solids content to prepare a resin solution, thereby preparing chemical conversion treatment agent B.

[0181] (C) Chemical conversion treatment agent C was prepared as an aqueous solution containing only 3-glycidoxypropyltriethoxysilane.

[0182] The above chemical conversion treatment agents were applied to the plating layer of plated steel materials so as to achieve film thicknesses after drying as shown in Tables 3A and 3B below, and then the coatings were dried and baked in an induction heating furnace at a maximum peak temperature (PMT) of 150°C to form coatings.

[0183] <Preparation of First Member and Second Member> As shown in Tables 1A to 3B, in Examples 1 to 29 and Comparative Examples 30 to 35, the plated steel material produced by the above-described procedure was used as the first member.

[0184] Furthermore, for the second member, the same material as that of the first member was used as the second member in Examples 1 to 10, 12 to 15, and 18 to 29 and Comparative Examples 30 to 35. In Tables 4A and 4B, the column for "Second member" is marked with "Same as left" for levels in which the same material as that of the first member was used as the material for the second member.

[0185] Furthermore, with regard to the second member, in Example 11, a galvannealed steel sheet (GA) having a tensile strength of 980 MPa at a thickness of 1.0 mm was used as the second member. In Example 16, a standard A5000 series aluminum sheet having a tensile strength of 290 MPa at a thickness of 1.0 mm was used as the second member. Furthermore, in Example 17, a commercially available CFRP sheet having a thickness of 1.0 mm was used as the second member.

[0186] <Adhesive Bonding Treatment> The prepared first member and second member were molded to produce a metallic hat-shaped member with a flange. As an adhesive for adhesively bonding the first member and the second member, an epoxy resin adhesive Penguin Cement #1066 manufactured by Sunstar Inc. was prepared by adding 5% by mass of 200 μm glass beads.

[0187] For each combination of the first member and the second member shown in Tables 1A to 3B below, the adhesive was applied to the surface of the first member, and the second member was then attached thereto. The adhesive was then cured by leaving it in an atmosphere of 170°C for 30 minutes, thereby producing a closed cross-section structure.

[0188] In Examples 10, 13, 16, and 20, bonded member structures were produced using spot welding in addition to the adhesive-applied portions. Specifically, spot welding was performed using a CF-type Cr—Cu electrode with a tip diameter of 5 mm and R40, with a nugget diameter of 3×t0.5 (t is the plate thickness [mm]) and a spot spacing of 30 mm. No adhesive was applied to the portions to be spot-welded.

[0189] <Electrodeposition coating of hat component> In order to observe the adhesive state in a corrosive environment, the hat-shaped component that had been subjected to the adhesive bonding treatment described above was subjected to a zinc phosphate treatment (SD5350 system: in accordance with the standard manufactured by Nippon Paint Industrial Coating Co., Ltd.), and then electrodeposition coating (PN110 Powernics Gray: in accordance with the standard manufactured by Nippon Paint Industrial Coating Co., Ltd.) was performed to a thickness of 20 μm, and the coating was baked at a baking temperature of 150° C. for 20 minutes.

[0190] <Evaluation of adhesive bonded structure> A plurality of samples were prepared by cutting out parts of the obtained adhesive bonded structure, and microscopic infrared spectroscopy and TOF-SIMS analysis were performed on vertical cross sections near the interface between the first member and the adhesive layer in accordance with the methods previously described.

[0191] In the microscopic infrared spectroscopy and TOF-SIMS analysis, the coating portion of the vertical cross section near the interface between the first member and the adhesive layer in the obtained adhesive bonded structure was enlarged by cutting at a 5-degree incline using an oblique cutting device (SAICAS, DN-20S model manufactured by Daipla Wintes). The microscopic infrared spectroscopy used was an IRT-5200 manufactured by JASCO Corporation, and the TOF-SIMS used was a TOF-SIMS TRIFT-V manufactured by ULVAC-PHI Corporation.

[0192] Here, in the microscopic infrared spectroscopy, mapping measurements were performed using the above-mentioned microscopic infrared spectroscopy analyzer. Whether or not the coating contained one or more of water-based polyurethane resin, epoxy resin, and polyester resin was determined based on the assignment of observed peaks derived from resin components in the infrared absorption spectrum of the obtained coating. Specifically, in the obtained infrared absorption spectrum,-1 When a peak is observed around 1550 cm, it is determined that the compound contains an epoxy group. -1 Around 1740 cm -1 When a peak is observed in the vicinity of 1720 to 1740 cm, it is determined that the compound contains a urethane group. -1 When a peak was observed around 0.05, it was determined that the sample contained an ester group. In the following, the case where it was determined that at least one of an epoxy group, a urethane group, and an ester group was contained is represented as "present," and the case where it was determined that these functional groups were not contained is represented as "absent."

[0193] Furthermore, in the TOF-SIMS analysis, the above-mentioned device was used to analyze an arbitrary point on the portion of the adhesive layer where the thickness was thinned to about 1 μm, while argon sputtering was performed from the adhesive layer side toward the metal member side. After sputtering to a certain depth with an Ar beam from the surface, TOF-SIMS measurement was performed, and then similarly, TOF-SIMS measurement was performed after sputtering, and this was repeated to obtain the depth distribution of various elements and bonds. The primary ion species was Au 3+ The acceleration voltage was 30 kV, and the sputtering rate was about 80 nm / min (SiO 2 The measurement area is 50 μm × 50 μm. The presence or absence of a peak indicating a Si—O—Me bond and the total ion correction value of 1.0 × 10 for the interface between the chemical conversion coating layer (or the adhesive layer if no chemical conversion coating layer is present) and the metal member are measured. -3 In the following, the evaluation was made as to whether or not the total ion correction value exceeded 1.0×10. -3 The above cases are represented as A, and the cases where there is no Si—O—Me bond or the Total Ion correction value is 1.0×10 -3 If the value was less than this, it was marked as B.

[0194] In addition, a sample was prepared by cutting out a portion of the resulting adhesive bonded structure, and a vertical cross section near the interface between the first member and the adhesive layer was observed using an SEM (SU3800 manufactured by Hitachi Ltd.) in accordance with the method previously described, and (Lr-Lo) / Lo (%) was calculated.

[0195] <Evaluation of Adhesion Durability> The resulting adhesive bonded structures of each example were evaluated for bond durability. First, the torsional rigidity of each adhesive bonded structure was measured and calculated using a torsion tester. Specifically, both ends of the adhesive bonded structure of each example were fixed with a jig, and only one end was rotated around the central axis of the adhesive bonded structure as the axis of rotation, thereby applying torsional deformation to the adhesive bonded structure. The torsional angle and torsional moment at this time were measured, and the torsional rigidity of each adhesive bonded structure was calculated from the relationship between the torsional angle and torsional moment in the elastic deformation range. Specifically, the initial slope of the torsional angle-torsional moment diagram was used as the relationship between the torsional angle and torsional moment in the elastic deformation range.

[0196] Next, a cyclic corrosion test was conducted in accordance with JASO (M609-91), and the adhesive bonded structures of each example were left standing for 4,800 hours to accelerate deterioration of the adhesive layer and the adhesive layer / chemical conversion coating layer interface. The torsional rigidity of each adhesive bonded structure after standing in the cyclic corrosion tester was measured and calculated using a torsion tester. The torsional rigidity was then compared with the torsional rigidity of each adhesive bonded structure of each example that had not been subjected to the deterioration test, and the rate of decrease in torsional rigidity due to deterioration was calculated. The resulting rate of decrease was used as an evaluation index for bond durability.

[0197] The rate of decrease in bending strength after the combined cyclic corrosion test relative to the bending strength before the test was calculated and evaluated according to the following evaluation criteria. A rating of C or higher was considered to be pass.

[0198] (Evaluation) AAA: Decrease rate less than 10% AA: Decrease rate 10% or more but less than 20% A: Decrease rate 20% or more but less than 30% B: Decrease rate 30% or more but less than 40% C: Decrease rate 40% or more but less than 50% D: Decrease rate 50% or more

[0199] <Simulated Edge Corrosion Resistance> The edge corrosion resistance was evaluated by preparing multiple samples by cutting out portions of the adhesive bonded structure, exposing a vertical cross section near the interface between the first member and the adhesive layer, and subjecting the vertical cross section to a neutral salt spray test as specified in JIS Z 2371, and examining the occurrence of red rust on the cut edge. The evaluation criteria for the red rust area ratio are as follows: "AAA", "AA", and "A" were considered to be acceptable.

[0200] (Evaluation) AAA: Red rust area ratio 10% or less after 2500 hours AA: Red rust area ratio 10% or less after 2000 hours A: Red rust area ratio 20% or less after 1500 hours B: Red rust area ratio more than 20% after 1500 hours

[0201] The results are shown in Tables 1A to 4B. The adhesive bonded structures of Nos. 1 to 29 had an uneven surface on the plating layer, multiple massive binary eutectic structures or multiple massive ternary eutectic structures were present in the plating layer, and a portion of the eutectic structure that existed continuously from the surface of the plating layer to half the thickness of the plating layer or to the depth of the Fe—Al-based interfacial alloy layer was located in the recesses of the uneven surface, the chemical composition of the plating layer and the morphology of the eutectic structure were within the ranges of the present disclosure, and both the adhesion durability and the edge corrosion resistance were excellent.

[0202] In No. 30, the amount of Al in the plating layer was insufficient, resulting in a small (Lr-Lo) / Lo×100 ratio and insufficient adhesion durability.

[0203] In No. 31, the amount of Al in the plating layer was excessive, which resulted in a small (Lr-Lo) / Lo×100 ratio and insufficient adhesion durability.

[0204] In No. 32, the amount of Mg in the plating layer was insufficient, resulting in a small (Lr-Lo) / Lo×100 ratio and insufficient adhesion durability.

[0205] In No. 33, the amount of Mg in the plating layer was excessive, which resulted in a small (Lr-Lo) / Lo×100 ratio and insufficient adhesion durability.

[0206] In No. 34, the oxygen concentration in the atmosphere from above the plating bath to the end of the cooling step exceeded 5000 ppm. As a result, in No. 34, (Lr-Lo) / Lo×100 was small, and the adhesion durability was insufficient.

[0207] In No. 35, the average cooling rate from the coating bath temperature to 260°C was low. As a result, in No. 35, primary Al crystals (Al phase or Al—Zn phase) were not sufficiently crystallized, the (Lr−Lo) / Lo×100 ratio was small, and the adhesion durability was insufficient.

[0208]

[0209]

[0210]

[0211]

[0212]

[0213]

[0214]

[0215]

[0216] Although the preferred embodiments of the present disclosure have been described in detail above with reference to the accompanying drawings, the present disclosure is not limited to such examples. It is clear that a person skilled in the art to which the present disclosure pertains can conceive of various modifications or alterations within the scope of the technical ideas set forth in the claims, and it is understood that these also naturally fall within the technical scope of the present disclosure.

[0217] REFERENCE SIGNS LIST 1, 1A, 1B, 1C, 1D Adhesively bonded structure 11 Steel material 12, 112 Plated layer 13, 113 Interface alloy layer 14, 114 Binary eutectic structure or ternary eutectic structure 2, 2A, 2B, 2C, 2D First member 21, 21A Metal part 22, 22A Coating part 221 Resin particle 223 Organic compound phase 3, 3A, 3B, 3C, 3D Second member 31 Plated steel material 32 Coating part 321 Resin particle 323 Organic compound phase 4, 4A, 4B, 4C, 4D Adhesive layer 5, 5B, 5C Adhesion region

Claims

1. A steel sheet comprising a first member, a second member, and an adhesive layer bonding the first member and the second member, wherein either or both of the first member and the second member is a plated steel material having a steel material and a plating layer disposed on at least a portion of a surface of the steel material, and the average chemical composition of the plating layer is, in mass%, Al: 10.00-30.00%, Mg: 1.00-15.00%, Sn: 0.00-1.00%, Si: 0.00-2.00%, Ca: 0.00-2.00%, Ni: 0.00-1.00%, Fe: 0.01-15.00%, Sb: 0.00-0.50%, Pb: 0.00-0.50%, Cu: 0.00-1.00%, Ti: 0.00-1.00%, Cr: 0.00-1.00%, Nb: 0.00-1.00%, Zr: 0.00-1.00%, Mn: 0.00-1.00%, Mo: 0.00-1.00%, Ag: 0.00-1.00%, Li: 0.00-1.00%, Bi: 0.00-1.00%, V: 0.00-1.00%, Co: 0.00-1.00%, In: 0.00-1.00%, W: 0.00-1.00%, P: 0.00-1.00%, La: 0.00~0.50%, Ce: 0.00~0.50%, B : 0.00 to 0.50%, Y: 0.00 to 0.50%, Sr: 0.00 to 0.50%, a total of Sb, Pb, Cu, Ti, Cr, Nb, Zr, Mn, Mo, Ag, Li, Bi, V, Co, In, W, P, La, Ce, B, Y, Sr: 0.00 to 5.00%, and the balance: Zn and impurities, wherein the surface of the plating layer is an uneven surface, and in a cross section of the plating layer, a relationship between a longitudinal length Lo of the plating layer within an observation area of ​​the cross section and a total length Lr of a contour line of the surface of the plating layer within the observation area satisfies the following formula (1), and the plating layer includes one or both of a plurality of massive binary eutectic structures and a plurality of massive ternary eutectic structures, An adhesive bonded structure, in which at least a portion of the binary eutectic structure or the ternary eutectic structure is present in a continuous manner from the surface of the plating layer to a position that is half the average thickness of the plating layer, (Lr-Lo) / Lox100≧2.0(%) (1) 2. The adhesively bonded structure according to claim 1, wherein the first member is a plated steel material having the steel material and the plating layer, and the second member is any one of a galvannealed steel material, a fiber-reinforced plastic material, an aluminum alloy material, or a magnesium alloy material.

3. The adhesive bonded structure described in claim 1, wherein the plated steel material comprises the steel material, the plating layer, and a coating portion disposed at least on the uneven surface of the plating layer, and the adhesive layer bonds the first member and the second member via the coating portion.

4. The adhesive joint structure described in claim 2, wherein the plated steel material comprises the steel material, the plating layer, and a coating portion arranged at least on the uneven surface of the plating layer, and the adhesive layer bonds the first member and the second member via the coating portion.

5. The coating contains an organic resin phase containing one or more of a urethane group, an epoxy group, and an ester group, and an organic compound phase consisting of an organosilicon compound containing at least one of a Si-O bond or a Si-OH bond, and a Si-C bond, and when the coating is analyzed by time-of-flight secondary ion mass spectrometry while Ar sputtering from the adhesive layer side to the plating layer side so as to include any location of the interface between the plating layer and the coating, a peak corresponding to a Si-O-Me bond is observed, and the value obtained by dividing the count number of the peak indicating the Si-O-Me bond by the total value of all secondary ion count numbers detected in the mass scanning range m / z = 0 to 300 is 1.0 x 10 -3 The adhesive bonded structure according to claim 3 or 4, wherein Me is one or more elements selected from the group consisting of Zn, Al, Mg and Fe which constitute the plating layer.

6. The adhesive bonded structure according to claim 1, wherein the plating layer includes an Fe-Al-based interface alloy layer in contact with the steel material, and at least a portion of the binary eutectic structure or the ternary eutectic structure in a plurality of clusters is present continuously from the surface of the plating layer to the Fe-Al-based interface alloy layer.

7. The adhesive bonded structure according to claim 1, which satisfies the following formula (2) instead of formula (1), and the number of locations where at least a portion of the binary eutectic structure or the ternary eutectic structure is continuously present from the surface of the plating layer to a position that is 1 / 2 the average thickness of the plating layer is 3 to 15 locations per rectangular region on the surface of the plating layer with long sides of 500 μm and short sides of 150 μm. (Lr-Lo) / Lo×100≧6.0(%) ... (2) 8. The adhesive bonded structure according to claim 1, which satisfies the following formula (3) instead of formula (1), and the number of locations where at least a portion of the binary eutectic structure or the ternary eutectic structure is present continuously from the surface of the plating layer to a position that is 1 / 2 the average thickness of the plating layer is 5 to 15 locations per rectangular region on the surface of the plating layer with long sides of 500 μm and short sides of 150 μm: (Lr-Lo) / Lo×100≧8.0(%) ... (3) 9. The adhesive bonded structure described in claim 1, wherein a portion of the binary eutectic structure or the ternary eutectic structure in a plurality of clusters is present continuously from the surface of the plating layer to a position that is 1 / 2 the average thickness of the plating layer, the portion being in a concave portion of the uneven surface of the plating layer.

10. The adhesive bonded structure described in claim 6, wherein a portion of the binary eutectic structure or the ternary eutectic structure is present continuously from the surface of the plating layer to the Fe-Al-based interface alloy layer, the portion being located in a recess of the uneven surface of the plating layer.

11. The adhesive bonded structure according to claim 1, wherein the average chemical composition of the plating layer is such that Al and Mg are Al: 10.00 to 25.00%, Mg: 4.50 to 15.00%.

12. The adhesive bonded structure according to claim 1, wherein the average chemical composition of the plating layer is such that Al and Mg are Al: 15.00 to 22.00%, Mg: 5.00 to 15.00%.

13. The average chemical composition of the plating layer is 0.05 to 0.50% Sn, and Mg is detected in the plating layer by X-ray diffraction measurement. 2 13. The adhesive bond structure of claim 1, claim 11 or claim 12, wherein a Sn phase is present.

14. The adhesive bonded structure according to claim 1, claim 11 or claim 12, wherein the average chemical composition of the plating layer contains one or both of La and Ce, the total amount of La and Ce being 0.05 to 0.50%.

15. The adhesive bonded structure according to claim 13, wherein the average chemical composition of the plating layer contains one or both of La and Ce, the total amount of La and Ce being 0.05 to 0.50%.

16. The adhesively bonded structure according to any one of claims 1 to 4, wherein the first member and the second member are further bonded together by a second bond.

17. The adhesively bonded structure of claim 16, wherein the second bond is a spot weld.

18. An automobile part comprising an adhesive bonded structure according to any one of claims 1 to 4 or claims 6 to 12.

19. An automobile part comprising the adhesive bonded structure according to claim 5.

20. An automotive part comprising the adhesive bonded structure according to claim 13.

21. An automotive part comprising the adhesive bond structure according to claim 14.

22. An automobile part comprising the adhesive bonded structure according to claim 15.

23. An automotive part comprising the adhesive bonded structure according to claim 16.

24. An automotive part comprising the adhesive bonded structure according to claim 17.

Citation Information

Patent Citations

  • Game machine

    JP2023087181A

  • Aluminum alloy material, bonded body, member for automobiles, and method for producing aluminum alloy material

    WO2016076344A1

  • Conversion-coated metal plate, surface-treated metal plate, composite member, and method for producing conversion-coated metal plate

    WO2017169571A1

  • Plated steel

    WO2018139619A1

  • Plated steel

    WO2018139620A1