Method for manufacturing nitride semiconductor substrate, method for manufacturing hybrid ic, and nitride semiconductor substrate
The method addresses the challenge of growing high-quality gallium nitride epitaxial layers on {110} silicon substrates by using a preflow step and specific gas supplies, achieving excellent surface morphology for hybrid ICs with both silicon-based and group III nitride-based devices, enhancing stability and cost-effectiveness.
Patent Information
- Application Number
- PCT/JP2024/018747
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-06-01
- Filing Date
- 2024-05-21
- Publication Date
- 2024-12-05
AI Technical Summary
The existing methods for growing gallium nitride epitaxial layers on silicon substrates with a {110} orientation result in poor surface morphology, making them unsuitable for device fabrication, while silicon-based devices like FinFETs and GAAs require {110} substrates, and group III nitride-based devices prefer {111} substrates, creating a challenge for manufacturing hybrid ICs with both types on the same substrate.
A method involving a silicon substrate with a {110} orientation, where a preflow step with an aluminum raw material is performed at 1000°C or higher, followed by forming a group III nitride base layer and a gallium nitride epitaxial layer using specific gas supplies, achieving a surface roughness of 2.00 nm or less, suitable for both silicon-based and group III nitride-based devices.
This method enables the production of nitride semiconductor substrates with excellent surface morphology, allowing for the coexistence of silicon-based and group III nitride-based devices on the same substrate, suitable for hybrid ICs, with improved stability and cost-effectiveness.
Smart Images

Figure JP2024018747_05122024_PF_FP_ABST
Abstract
Description
Nitride semiconductor substrate manufacturing method, hybrid IC manufacturing method, and nitride semiconductor substrate
[0001] The present invention relates to a method for manufacturing a nitride semiconductor substrate, a method for manufacturing a hybrid IC, and a nitride semiconductor substrate.
[0002] In cutting-edge silicon (Si) devices, FinFETs (Fin Field-Effect Transistors) and GAAs (Gate-All-Around) are fabricated on Si (110) substrates, which have high hole mobility. Meanwhile, in the case of GaN deposition on Si substrates (GaN on Si), power devices and light-emitting devices are generally fabricated by epitaxially growing gallium nitride (GaN) on Si (111) substrates, which have a matching crystal structure and small lattice mismatch.
[0003] Patent Document 1 describes an invention relating to a nitride semiconductor wafer and a method for manufacturing the nitride semiconductor wafer. Patent Document 1 describes that the plane orientation of the main surface of a high-resistivity, low-oxygen CZ silicon single crystal substrate can be (100), (110), (111), etc. As an example, it describes epitaxial growth of a nitride semiconductor on a silicon single crystal substrate with an axial orientation <111>.
[0004] Japanese Patent Application Laid-Open No. 2022-25512
[0005] The present inventors have actually investigated the epitaxial growth of gallium nitride on a Si(110) substrate and found that epitaxial growth of an initial AlN layer, a strain relaxation layer, and a GaN layer on a Si(110) substrate results in the formation of surface irregularities, resulting in poor morphology and making the substrate unsuitable for device fabrication. It was also found that the use of a Si(110) substrate results in a worse surface morphology (flatness or roughness) of the gallium nitride epitaxial layer compared to growth on a Si(111) substrate. In the fabrication of devices using a GaN-on-Si substrate, even when a silicon substrate with a {110} principal surface orientation is used, a nitride semiconductor substrate (GaN-on-Si(110)) is needed that improves the surface irregularities of the epitaxial layer and has a gallium nitride epitaxial layer with excellent surface morphology, and a method for manufacturing the same.
[0006] Furthermore, when fabricating Group III nitride devices on a silicon substrate as described above, epitaxial growth on a Si(111) substrate is preferred from the viewpoint of the quality of the GaN (Group III nitride) layer. On the other hand, when fabricating cutting-edge Si devices (FinFETs and GAA) on a silicon substrate, it is preferred to use a Si(110) substrate. However, when fabricating a hybrid IC in which silicon-based devices and Group III nitride-based devices coexist on the same silicon substrate, the silicon-based devices and Group III nitride-based devices will be formed on a silicon substrate with the same surface orientation.
[0007] Therefore, if a technology for growing a high-quality gallium nitride epitaxial layer on a Si(110) substrate (GaN on Si(110)) can be established, it will be possible to fabricate Group III nitride-based devices and silicon-based devices such as FinFETs and GAA on the same Si(110) substrate, thereby fabricating a hybrid IC. Thus, there is a need for a method for manufacturing a hybrid IC that uses a silicon substrate whose main surface has a {110} plane orientation (Si{110} substrate) and that includes a Group III nitride-based device including a gallium nitride epitaxial layer with excellent surface morphology, and a silicon-based device.
[0008] The present invention has been made to solve the above problems, and has as its object to provide a nitride semiconductor substrate using a silicon substrate whose main surface has a plane orientation of {110} and having a gallium nitride epitaxial layer with excellent surface morphology, a method for manufacturing the same, and a method for manufacturing a hybrid IC using a silicon substrate whose main surface has a plane orientation of {110} and having a Group III nitride-based device including a gallium nitride epitaxial layer with excellent surface morphology, and a silicon-based device.
[0009] The present invention has been made to achieve the above-mentioned object, and provides a method for manufacturing a nitride semiconductor substrate having a Group III nitride layer comprising a Group III nitride underlayer and a gallium nitride epitaxial layer on a silicon substrate, the method using a silicon substrate whose principal surface has a plane orientation of {110}, the method comprising the following steps: a preflow step of supplying a gas containing an aluminum source but not a nitrogen source onto the silicon substrate heated to 1000°C or higher; an underlayer formation step of supplying a gas containing a Group III source and a nitrogen source to form a Group III nitride underlayer on the silicon substrate; and an epitaxial layer formation step of supplying a gas containing a gallium source and a nitrogen source to form a gallium nitride epitaxial layer.
[0010] According to this method for manufacturing a nitride semiconductor substrate, a nitride semiconductor substrate having a gallium nitride epitaxial layer with excellent surface morphology can be manufactured using a silicon substrate whose principal surface has a plane orientation of {110}.
[0011] In this case, the method for manufacturing a nitride semiconductor substrate can be one in which an organoaluminum compound is used as the aluminum source.
[0012] This allows for a lower cost method for manufacturing a nitride semiconductor substrate.
[0013] At this time, the method for manufacturing a nitride semiconductor substrate can be such that the heating temperature of the silicon substrate in the preflow step is 1200° C. or less.
[0014] This allows a more stable preflow process to be carried out.
[0015] The present invention also provides a method for manufacturing a hybrid IC in which silicon-based devices and Group III nitride-based devices coexist on the same silicon substrate, the method comprising the steps of: using a silicon substrate having a principal surface with a {110} plane orientation; forming a mask having a first opening in a region on the silicon substrate where the Group III nitride-based device is to be provided; carrying out a preflow step of supplying a gas containing an aluminum source but not containing a nitrogen source onto the silicon substrate heated to 1000°C or higher; an underlayer formation step of supplying a gas containing a Group III source and a nitrogen source to form a Group III nitride underlayer on the silicon substrate; and an epitaxial layer formation step of supplying a gas containing a gallium source and a nitrogen source to form a gallium nitride epitaxial layer; providing the Group III nitride-based device in the first opening; then removing the mask in the region where the silicon-based device is to be provided to form a second opening; and providing the silicon-based device in the second opening.
[0016] According to this hybrid IC manufacturing method, a hybrid IC can be manufactured using a silicon substrate whose main surface has a {110} plane orientation, and which includes a group III nitride-based device including a gallium nitride epitaxial layer with excellent surface morphology, and a silicon-based device.
[0017] In this case, the method for manufacturing a hybrid IC can be one in which an organoaluminum compound is used as the aluminum raw material.
[0018] This allows for a lower cost method of manufacturing hybrid ICs.
[0019] At this time, the method for manufacturing a hybrid IC can be such that the heating temperature of the silicon substrate in the preflow process is 1200° C. or less.
[0020] This allows a more stable preflow process to be carried out.
[0021] The present invention has been made to achieve the above-mentioned object, and provides a nitride semiconductor substrate comprising a Group III nitride layer on a silicon substrate, wherein a primary surface of the silicon substrate has a plane orientation of {110}, the Group III nitride layer on the silicon substrate comprises a Group III nitride underlayer and a gallium nitride epitaxial layer on the Group III nitride underlayer, and the gallium nitride epitaxial layer has a surface roughness Ra of 2.00 nm or less.
[0022] Such a nitride semiconductor substrate, while using a silicon substrate with a {110} plane orientation on the main surface, has excellent surface morphology and is suitable for Group III nitride-based devices.
[0023] As described above, the nitride semiconductor substrate manufacturing method of the present invention makes it possible to manufacture a nitride semiconductor substrate having a gallium nitride epitaxial layer with excellent surface morphology using a silicon substrate having a (110) plane orientation of the main surface. The hybrid IC manufacturing method of the present invention makes it possible to manufacture a hybrid IC having a silicon-based device and a Group III nitride-based device including a gallium nitride epitaxial layer with excellent surface morphology using a silicon substrate having a {110} plane orientation of the main surface. The nitride semiconductor substrate of the present invention makes it possible to manufacture a nitride semiconductor substrate having excellent surface morphology and suitable for Group III nitride-based devices using a silicon substrate having a {110} plane orientation of the main surface.
[0024] 1 shows a specific example of a nitride semiconductor substrate according to the present invention; 2 shows a flow chart of a method for manufacturing a nitride semiconductor substrate and a method for manufacturing a hybrid IC according to the present invention; 3 shows a comparison of the surface morphology of a gallium nitride epitaxial layer in a nitride semiconductor substrate according to an example and a comparative example.
[0025] The present invention will be described in detail below, but the present invention is not limited thereto.
[0026] As described above, there has been a demand for a nitride semiconductor substrate using a silicon substrate whose principal surface has a plane orientation of {110} and having a gallium nitride epitaxial layer with excellent surface morphology, a method for manufacturing the same, and a method for manufacturing a hybrid IC using a silicon substrate whose principal surface has a plane orientation of {110} and having a Group III nitride-based device including a gallium nitride epitaxial layer with excellent surface morphology and a silicon-based device.
[0027] As a result of extensive investigations into the above-mentioned problems, the present inventors have found that a method for manufacturing a nitride semiconductor substrate comprising a Group III nitride layer comprising a Group III nitride underlayer and a gallium nitride epitaxial layer on a silicon substrate, the method comprising: a preflow step of using a silicon substrate whose main surface has a plane orientation of {110} and supplying a gas containing an aluminum source but not a nitrogen source onto the silicon substrate heated to 1000°C or higher; an underlayer formation step of supplying a gas containing a Group III nitride source and a nitrogen source to form a Group III nitride underlayer on the silicon substrate; and an epitaxial layer formation step of supplying a gas containing a gallium source and a nitrogen source to form a gallium nitride epitaxial layer, thereby making it possible to manufacture a nitride semiconductor substrate comprising a gallium nitride epitaxial layer with excellent surface morphology, even when using a silicon substrate whose main surface has a plane orientation of {110}, and have completed the present invention.
[0028] As a result of extensive research into the above-mentioned problems, the present inventors have discovered a method for manufacturing a hybrid IC in which silicon-based devices and Group III nitride-based devices coexist on the same silicon substrate, the method comprising the steps of: using a silicon substrate having a principal surface with a {110} plane orientation; forming a mask having a first opening in a region on the silicon substrate where the Group III nitride-based devices are to be provided; preflowing a gas containing an aluminum source but not a nitrogen source onto the silicon substrate heated to 1000° C. or higher; supplying a gas containing a Group III source and a nitrogen source to form a Group III nitride source layer on the silicon substrate; and The inventors have found that a hybrid IC can be manufactured using a silicon substrate whose main surface has a {110} plane orientation, and that the hybrid IC is equipped with a group III nitride device including a gallium nitride epitaxial layer with excellent surface morphology and a silicon device, by a method for manufacturing a hybrid IC, which comprises supplying a gas containing raw materials to form an epitaxial layer, providing the group III nitride device in the first opening, then removing the mask in the region where the silicon device is to be provided to form a second opening, and providing the silicon device in the second opening.
[0029] As a result of extensive research into the above-mentioned problems, the present inventors have found that a nitride semiconductor substrate comprising a Group III nitride layer on a silicon substrate, wherein the plane orientation of a main surface of the silicon substrate is {110}, the Group III nitride layer on the silicon substrate comprising a Group III nitride underlayer and a gallium nitride epitaxial layer on the Group III nitride underlayer, and wherein the gallium nitride epitaxial layer has a surface roughness Ra of 2.00 nm or less, can provide a nitride semiconductor substrate that has excellent surface morphology and is suitable for Group III nitride-based devices, despite using a silicon substrate whose main surface has a plane orientation of {110}, and have completed the present invention.
[0030] The following description will be made with reference to the drawings.
[0031] [Nitride Semiconductor Substrate] A nitride semiconductor substrate according to the present invention will be described with reference to Fig. 1. A nitride semiconductor substrate 100 according to the present invention comprises a silicon substrate 1 and a group III nitride layer 2 on the silicon substrate 1.
[0032] The plane orientation of the main surface of the silicon substrate 1 is {110}. The silicon substrate 1 is not particularly limited as long as the plane orientation of the main surface is {110}. The shape (circular, rectangular, etc.), size (thickness, diameter, etc.), oxygen concentration, resistivity (dopant concentration), manufacturing method of the silicon substrate (CZ, FZ), etc. are not particularly limited and can be appropriately set depending on the final design of the Group III nitride-based device. In this specification, the plane orientation {110} includes a plane equivalent to (110). Furthermore, "the plane orientation of the main surface is {110}" includes not only a plane orientation of the main surface that is not inclined from {110} (off-angle = 0°) but also a plane with an off-angle from {110} within ±8°.
[0033] The group III nitride layer 2 on the silicon substrate 1 includes a group III nitride underlayer 3 and a gallium nitride epitaxial layer 4 on the group III nitride underlayer 3. The roughness Ra of the surface 4a of the gallium nitride epitaxial layer 4 is 2.00 nm or less. The gallium nitride epitaxial layer 4 may be a multi-layer gallium nitride epitaxial layer having different dopant types and concentrations. The thickness of the gallium nitride epitaxial layer 4 is not particularly limited, but may be, for example, 0.8 μm or more and 10 μm or less. Within this range, a gallium nitride epitaxial layer having a surface roughness Ra of 2.00 nm or less can be reliably obtained. The lower limit of the roughness Ra of the surface 4a of the gallium nitride epitaxial layer 4 is 0.00 nm or more.
[0034] The III-nitride underlayer 3 may further include an initial layer 5 such as AlN on the surface of the silicon substrate 1, and a buffer layer 6 such as a graded composition layer or a superlattice layer.
[0035] The nitride semiconductor substrate according to the present invention uses a silicon substrate 1 whose principal surface has a plane orientation of {110}, yet has an excellent flat surface morphology with a roughness Ra of the surface 4 a of the gallium nitride epitaxial layer 4 of 2.00 nm or less, and is therefore suitable for Group III nitride-based devices.
[0036] [Method for Manufacturing Nitride Semiconductor Substrate] Next, a method for manufacturing a nitride semiconductor substrate according to the present invention will be described with reference to Fig. 2(A) . The method for manufacturing a nitride semiconductor substrate according to the present invention is a method for manufacturing a nitride semiconductor substrate 100 including a group III nitride layer 2 including a group III nitride underlayer 3 and a gallium nitride epitaxial layer 4 on a silicon substrate 1.
[0037] The method for manufacturing a nitride semiconductor substrate according to the present invention uses a silicon substrate 1 having a principal surface with a plane orientation of {110}, and includes the following steps: a preflow step of supplying a gas containing an aluminum source but not a nitrogen source onto the silicon substrate 1 heated to 1000° C. or higher, an underlayer formation step of supplying a gas containing a Group III source and a nitrogen source to form a Group III nitride underlayer 3 on the silicon substrate 1, and an epitaxial layer formation step of supplying a gas containing a gallium source and a nitrogen source to form a gallium nitride epitaxial layer 4. Each step will be described below.
[0038] (Preflow Process) This process can be performed in the same film-forming apparatus as the subsequent underlayer formation process and epitaxial layer formation process. A silicon substrate 1 having a {110} principal surface orientation is heated to 1000°C or higher, and a gas containing an aluminum source but not a nitrogen source is supplied. If a nitrogen source is contained, there is a risk of forming an AlN film, which does not constitute surface treatment prior to the formation of the underlayer on the silicon substrate 1 using an aluminum source, and therefore does not have the effect of planarizing the surface of the gallium nitride epitaxial layer 4.
[0039] The temperature to which the silicon substrate 1 is heated may be 1000° C. or higher, and the technical upper limit is below the melting point of the silicon substrate 1, but it is preferably 1200° C. or lower. Even if the temperature is set too high, the effect of the preflow process does not change significantly, but damage to the Si substrate and components of the film formation apparatus can be more stably suppressed. Therefore, when the stability and productivity of the preflow process are taken into consideration, a temperature of 1200° C. or lower is sufficient.
[0040] The time for supplying the gas containing the aluminum source material but not the nitrogen source material is not particularly limited. The lower limit can be, for example, 1 second or more, preferably 3 seconds or more, and more preferably 5 seconds or more. The upper limit can be, for example, 60 seconds or less, preferably 30 seconds or less, and more preferably 15 seconds or less. Within this range, the surface of the gallium nitride epitaxial layer 4 can be more stably planarized.
[0041] The gas containing an aluminum source but not containing a nitrogen source used in the preflow process is not particularly limited. It is preferable to use, for example, an organoaluminum compound as the aluminum source. Specific examples of organoaluminum compounds include trimethylaluminum (TMA) and triethylaluminum (TEA). These are used as film-forming materials for Group III nitrides, and when an organoaluminum compound is used in the subsequent underlayer formation process, the same gas can be used, which is suitable from the viewpoint of cost and for preventing contamination of the substrate and growth equipment. In addition, hydrogen (H 2 ) gas can be used.
[0042] The present inventors have investigated the reason why such a preflow process can make the surface roughness Ra of the gallium nitride epitaxial layer 2.00 nm or less and form a mirror surface. However, even if an analysis of the substrate immediately after the preflow process is attempted, it is believed that the Al layer, which is thought to have been formed very thinly, will be altered before analysis. Furthermore, after the nitride semiconductor substrate is manufactured, it is believed that the structure affected by the preflow process will be changed by heat treatments and other processes after the preflow process. Therefore, it was not possible to clarify the difference in the structure of the silicon substrate surface depending on whether or not the preflow process is performed. Thus, although the reason why the preflow process can make the surface of the gallium nitride epitaxial layer 2.00 nm or less in roughness Ra is unclear, it is possible that the preflow process forms an extremely thin Al layer of about a few angstroms, and the eutectic reaction with Si forms fine irregularities on the surface, which causes the {111} plane to appear and promote the lateral growth of a group III nitride layer such as GaN. In any case, by carrying out the preflow step according to the present invention, the surface roughness Ra of the surface of the gallium nitride epitaxial layer can be reduced to 2.00 nm or less, making it possible to form a mirror surface.
[0043] Prior to the preflow process, hydrogen (H 2 It is preferable to clean the surface of the silicon substrate by baking (heat treatment) in a .sup.3) gas atmosphere, but this is not necessarily required if the surface of the silicon substrate is in a clean state.
[0044] (Underlayer Forming Step) Next, the underlayer forming step will be described. After the above-described preflow step, a gas containing a Group III source and a nitrogen source is supplied to form a Group III nitride underlayer 3, which is part of the Group III nitride layer 2, on the silicon substrate 1. As the Group III nitride underlayer 3, an initial layer 5 such as AlN, or a buffer layer 6 such as a graded composition layer or a superlattice layer can be formed. The conditions for forming the Group III nitride underlayer 3 are not particularly limited.
[0045] (Epitaxial Layer Formation Step) After the base layer formation step, an epitaxial layer formation step is performed in which a gas containing a gallium source and a nitrogen source is supplied to form the gallium nitride epitaxial layer 4. The conditions for forming the gallium nitride epitaxial layer 4 are not particularly limited. For example, the gallium nitride epitaxial layer 4 may be formed by MOCVD, HVPE, or the like. As the gallium source, an organic gallium compound such as trimethylgallium (TMG) or triethylgallium (TEG) can be used. Note that the gallium nitride epitaxial layer 4 may be formed as a multi-layer gallium nitride epitaxial layer by varying the type and concentration of the dopant.
[0046] [Method for Manufacturing a Hybrid IC] Next, a method for manufacturing a hybrid IC according to the present invention will be described with reference to FIG. 2B . In the method for manufacturing a hybrid IC according to the present invention, a silicon substrate having a {110} surface orientation is used. A mask having a first opening is then formed on the silicon substrate, and a Group III nitride-based device such as an electronic device or a light-emitting device is provided in the first opening. The mask is then removed from the region where the silicon-based device is to be provided to form a second opening, and the silicon-based device is provided in the second opening. This allows for the manufacture of a hybrid IC in which a Group III nitride-based device having a gallium nitride epitaxial layer with a mirror-finished surface morphology, and a silicon-based device such as a FinFET (Fin Field-Effect Transistor) or GAA (Gate-All-Around), coexist on a <110> silicon substrate, which increases hole mobility.
[0047] (Formation of Group III nitride device) In the formation of a Group III nitride device in the hybrid IC manufacturing method according to the present invention, a Group III nitride device is formed in the first opening. The formation of this Group III nitride device involves the "preflow step," "underlayer formation step," and "epitaxial layer formation step" described in the nitride semiconductor substrate manufacturing method. Detailed descriptions of these steps are omitted here, as they are the same as those in the nitride semiconductor substrate manufacturing method.
[0048] (Formation of Silicon-Based Device) In the formation of a silicon-based device in the hybrid IC manufacturing method according to the present invention, a silicon-based device is formed in the second opening. Although there are no particular limitations on the silicon-based device, it is preferable to fabricate a FinFET or GAA in order to take advantage of the advantages of using a Si{110} substrate.
[0049] In this way, a hybrid IC can be fabricated in which silicon-based devices and group III nitride-based devices coexist.
[0050] First Embodiment A specific example of a method for manufacturing a nitride semiconductor substrate according to the present invention will be described below as a first embodiment. First, a Si (110) substrate is prepared. Hydrogen (H 2 ) The substrate surface is cleaned by baking. Then, before starting the growth of the initial AlN layer, TMA preflow is performed for, for example, within 60 seconds. After that, the initial AlN layer, Al x Ga 1-x A buffer layer, which is an N (x≧0) layer, is formed, and then an island-shaped SiN layer is formed, followed by a GaN layer. For electronic devices, an AlGaN layer is formed on the GaN layer to form a HEMT structure. For light-emitting devices, Al x Ga 1-x A light-emitting device can be fabricated by forming a GaN / InGaN MQW structure on an N(x≧0) buffer layer and then forming p-GaN. The buffer layer may have a graded composition or may be composed of multiple layers of different compositions, such as a stepped composition AlGaN layer, a superlattice AlGaN / GaN, a superlattice AlN / GaN, or an intermittent superlattice structure.
[0051] Further, the manufacturing conditions are shown with a specific example. Nitrogen (N 2 ) gas to hydrogen (H 2 ) gas, and the temperature was increased while hydrogen (H 2 ) The substrate surface is cleaned by baking. Then, TMA is supplied at 1000 to 1200°C to perform a preflow process. Next, TMA + NH 3Gas is supplied to form an initial layer of AlN, TMA, TMG (trimethylgallium), and NH 3 The gas is supplied to form a buffer layer of AlGaN with a thickness of 100 to 200 nm. The supply of TMA and TMG is stopped, and SiH 4 +NH 3 The supply of monosilane gas is stopped, and TMG is flowed to grow a GaN layer to a thickness of 15 to 50 nm. Next, a superlattice (SLs) buffer layer of 15 to 25 pairs of AlN / GaN is formed. After that, a GaN layer with a thickness of approximately 800 to 900 nm is formed, and a nitride semiconductor substrate is obtained.
[0052] Second Embodiment A specific example of a method for manufacturing a hybrid IC according to the present invention will be described below as the second embodiment. First, a Si (110) substrate is prepared. A thermal oxide film of about 100 nm is formed on the surface of the Si substrate, and a mask is formed using photolithography in the area where the Si device will be fabricated. The oxide film is then removed by dry etching from the area where the gallium nitride epitaxial layer will be grown, leaving the Si substrate exposed only in the area where the Group III nitride device will be fabricated (first opening). The subsequent fabrication of the Group III nitride device is the same as in the first embodiment.
[0053] After fabricating the group III nitride devices, the GaN film grown on the oxide film in the area where the silicon devices will be fabricated is removed by dry etching to protect the group III nitride (GaN) device area. After removing the poly-GaN film and exposing the oxide layer, the substrate is immersed in HF solution to remove the oxide layer and expose the Si substrate (second opening). Silicon devices are fabricated on the exposed Si substrate.
[0054] The present invention will be specifically explained below with reference to examples, but the present invention is not limited to these examples.
[0055] (Example) A p-type (boron concentration 6×10) substrate with a diameter of 150 mm was used as a substrate for epitaxial growth of GaN on Si. 14 atoms / cm 3 (Oxygen concentration 7 × 10 17 atoms / cm 3A Si (110) substrate was prepared. The Si (110) substrate was loaded into an MOCVD reactor, and hydrogen was used as the carrier gas. Upon reaching the epitaxial growth temperature of 1150°C, TMA (trimethylaluminum) preflow was performed for 6 seconds. Ammonia gas, the nitrogen source, was then introduced to form an initial AlN layer of 150 nm, followed by TMG (trimethylgallium) to form a 160 nm AlGaN layer. The TMA and TMG supply was interrupted, and monosilane gas was introduced to grow a 1 nm SiN layer in an island pattern. The monosilane gas supply was then stopped, and TMG was introduced to grow a 25 nm GaN layer. A 400 nm-thick buffer layer with 23 pairs of 4.2 nm AlN / 25 nm GaN layers was then formed on top of the buffer layer. An 820 nm GaN layer was then grown on top of the buffer layer to form a gallium nitride epitaxial layer.
[0056] Comparative Example A gallium nitride epitaxial layer was formed using the same process and conditions as in the example, except that preflow using TMA was not performed.
[0057] (Evaluation) First, the surface morphology of the gallium nitride epitaxial layer was evaluated. Specifically, the presence or absence of clouding was evaluated by visual observation with a condenser lamp, and observation with a differential interference contrast microscope was performed. As a result of the observation with a condenser lamp, clouding was observed on the surface of the gallium nitride epitaxial layer of the comparative example, whereas no clouding was observed on the surface of the gallium nitride epitaxial layer of the example, revealing that it was a mirror surface. Furthermore, as a result of observation with a differential interference contrast microscope, as shown in FIG. 3, unevenness was observed on the surface of the gallium nitride epitaxial layer of the comparative example, whereas the surface of the gallium nitride epitaxial layer of the example was found to be smooth. Furthermore, when the surface roughness of the gallium nitride epitaxial layer surface was measured using a stylus profiler (P-15, manufactured by KLA-Tencor Corporation), it was found to be Ra 1.86 nm in the example and Ra 12.5 nm in the comparative example. According to the examples of the present application, a gallium nitride epitaxial layer with a mirror-like surface having a surface roughness of Ra 2.00 nm or less could be obtained.
[0058] In addition, when XRD evaluation was performed to evaluate the crystallinity, only (002) and (004) diffraction peaks were detected in the gallium nitride epitaxial layer in both the example and the comparative example, and it was found that the (001) plane was aligned in the surface normal direction. In addition, the half-width of the GaN (002) rocking curve was 197 arcsec in the example and 211 arcsec in the comparative example. It was found that gallium nitride epitaxial layers with equivalent crystallinity were obtained in both the example and the comparative example.
[0059] As described above, according to the examples of the present invention, it was possible to manufacture nitride semiconductor substrates including a gallium nitride epitaxial layer having a surface roughness Ra of 2.00 nm or less, that is, a flat surface with good surface morphology.
[0060] The present invention is not limited to the above-described embodiments, which are merely examples, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and that provides similar effects is included within the technical scope of the present invention.
Claims
1. A method for manufacturing a nitride semiconductor substrate comprising a Group III nitride layer comprising a Group III nitride underlayer and a gallium nitride epitaxial layer on a silicon substrate, comprising: a silicon substrate having a principal surface with a {110} orientation; the method comprising the steps of: a preflow process for supplying a gas containing an aluminum source but not a nitrogen source onto the silicon substrate heated to 1000°C or higher; an underlayer formation process for supplying a gas containing a Group III source and a nitrogen source to form a Group III nitride underlayer on the silicon substrate; and an epitaxial layer formation process for supplying a gas containing a gallium source and a nitrogen source to form a gallium nitride epitaxial layer.
2. The method for producing a nitride semiconductor substrate according to claim 1, wherein an organoaluminum compound is used as the aluminum source.
3. The method for producing a nitride semiconductor substrate according to claim 1 or 2, wherein the heating temperature of said silicon substrate in said preflow step is 1200° C. or less.
4. A method for manufacturing a hybrid IC in which silicon-based devices and Group III nitride-based devices coexist on the same silicon substrate, comprising the steps of: using a silicon substrate whose main surface has a plane orientation of {110}; forming a mask having a first opening in a region on the silicon substrate where the Group III nitride-based device is to be provided; carrying out a preflow process of supplying a gas containing an aluminum source but not a nitrogen source onto the silicon substrate heated to 1000°C or higher; an underlayer formation process of supplying a gas containing a Group III source and a nitrogen source to form a Group III nitride underlayer on the silicon substrate; and an epitaxial layer formation process of supplying a gas containing a gallium source and a nitrogen source to form a gallium nitride epitaxial layer, providing the Group III nitride-based device in the first opening; and then removing the mask in the region where the silicon-based device is to be provided to form a second opening, and providing the silicon-based device in the second opening.
5. The method for producing a hybrid IC according to claim 4, wherein an organoaluminum compound is used as the aluminum source.
6. The method for manufacturing a hybrid IC according to claim 4 or 5, wherein the heating temperature of the silicon substrate in the preflow process is 1200° C. or less.
7. A nitride semiconductor substrate comprising a Group III nitride layer on a silicon substrate, wherein a principal surface of the silicon substrate has a plane orientation of {110}, the Group III nitride layer on the silicon substrate comprises a Group III nitride underlayer and a gallium nitride epitaxial layer on the Group III nitride underlayer, and the surface roughness Ra of the gallium nitride epitaxial layer is 2.00 nm or less.
Citation Information
Patent Citations
Solutions for Incorporation of Alternate Active Area Materials into Integrated Circuits
JP2009503871A
Nitride semiconductor wafer and manufacturing method of the same
JP2022025512A