Thermally conductive heat dissipation composition and electronic device

A thermally conductive heat dissipation composition with specific viscosity characteristics and surfactant properties addresses the issue of dripping and enhances heat transfer between electronic components and heat sinks, achieving effective heat dissipation.

WO2024247845A1PCT designated stage expired Publication Date: 2024-12-05DENKA CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/018832
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-29
Filing Date
2024-05-22
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

The challenge is to develop a thermally conductive heat dissipation composition that prevents dripping during dispensing and ensures effective heat transfer between heat-generating electronic components and heat sinks, as existing greases with low viscosity tend to drip and reduce heat conduction due to air interfaces.

Method used

A thermally conductive heat dissipation composition with predetermined viscosity characteristics, including a matrix component and thermally conductive filler, containing Si-containing powder with a hydrophilic surface and a surfactant with specific monomer units, which exhibits thixotropic properties to maintain stability and enhance thermal conductivity.

Benefits of technology

The composition effectively suppresses dripping and improves heat dissipation by maintaining stability and high thermal conductivity, ensuring efficient transfer between electronic components and heat sinks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024018832_05122024_PF_FP_ABST
    Figure JP2024018832_05122024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a thermally conductive heat dissipation composition containing a matrix component and a thermally conductive filler, wherein when the shear rate is changed from 10 s-1 to 0.1 s-1 during viscosity measurement at 25°C, the time t until a viscosity η1 that was stable at a shear rate of 10 s-1 becomes a stable viscosity η2 at a shear rate of 0.1 s-1 is 30 seconds or less.
Need to check novelty before this filing date? Find Prior Art

Description

Thermally conductive heat dissipating composition and electronic device

[0001] The present invention relates to a thermally conductive heat-dissipating composition and an electronic device.

[0002] As heat-generating electronic components, such as central processing units (CPUs) in personal computers, become smaller and more powerful, the amount of heat generated per unit area by these electronic components has become extremely large. This amount of heat is approximately 20 times that of an iron. To prevent these heat-generating electronic components from breaking down over the long term, they must be cooled. Metal heat sinks and housings are used for cooling. However, when a heat-generating electronic component is placed in direct contact with a heat sink or similar, air is present at the interface, microscopically, which can impede heat conduction. Therefore, a thermally conductive material is inserted between the heat-generating electronic component and the heat sink or similar to efficiently transfer heat.

[0003] As a thermally conductive material, a particularly preferred one is a fluid grease in which a thermally conductive powder is filled into a liquid silicone, because it conducts heat particularly easily. Known greases include those in which a thermally conductive powder is contained in a liquid silicone base oil such as silicone oil, or in a low-viscosity silicone such as a low-molecular-weight silicone (for example, Patent Documents 1 to 4).

[0004] JP 2009-286855 A JP 2015-140395 A JP 2014-105283 A JP 2010-150399 A

[0005] From the perspective of application performance, it is better for grease to have low viscosity. However, when low viscosity grease is dispensed using a dispenser or pump, it tends to drip from the nozzle even after the pressure is removed. This is called "dripping." Dripping can result in the grease adhering to unintended locations, which is undesirable.

[0006] The present invention has been made in view of the above problems, and has an object to provide a thermally conductive, heat-dissipating composition that can suppress dripping, and an electronic device that includes the thermally conductive, heat-dissipating composition.

[0007] The present inventors have conducted extensive research to solve the above-mentioned problems, and as a result have found that the above-mentioned problems can be solved by using a thermally conductive, heat-dissipating composition having predetermined viscosity characteristics, which has led to the completion of the present invention.

[0008] That is, the present invention is as follows: [1] A composition containing a matrix component and a thermally conductive filler, wherein the shear rate is 10 s during viscosity measurement at 25°C. -1 From 0.1 seconds -1 When the shear rate was changed to 10 s -1 The viscosity η1 at a shear rate of 0.1 s -1

[0013]

[0014] A thermally conductive, heat-dissipating composition, wherein the time t until the viscosity reaches a stable value η2 at 100°C is 30 seconds or less. [2] The thermally conductive, heat-dissipating composition according to [1], which is a one-component or two-component curing type. [3] The thermally conductive, heat-dissipating composition according to [1] or [2], which contains a Si-containing powder. [4] The thermally conductive, heat-dissipating composition according to [3], wherein the surface of the Si-containing powder is hydrophilic. [5] The thermally conductive, heat-dissipating composition according to [3] or [4], wherein the median diameter (D50) of the Si-containing powder is 5 to 6,000 nm. [6] The thermally conductive, heat-dissipating composition according to any one of [3] to [5], wherein the content of the Si-containing powder is 0.01 to 1.00 parts by mass per 100 parts by mass of the thermally conductive filler. [7] The thermally conductive, heat-dissipating composition according to any one of [1] to [6], wherein the matrix component contains a surfactant. [8] The thermally conductive, heat-dissipating composition according to [7], wherein the surfactant comprises a copolymer having (meth)acrylic monomer units α having a carboxy group, (meth)acrylic monomer units β having a tertiary amino group, and (meth)acrylic monomer units γ having a siloxane skeleton. [9] The thermally conductive, heat-dissipating composition according to any one of [1] to [8], wherein the matrix component comprises an organopolysiloxane.

[10] The thermally conductive, heat-dissipating composition according to any one of [1] to [9], having a thermal conductivity of 4.0 W / m K or more.

[11] An electronic device comprising: an electronic component; the thermally conductive, heat-dissipating composition according to any one of [1] to

[10] ; and a heat sink, wherein the electronic component and the heat sink are in contact with each other via the thermally conductive, heat-dissipating composition.

[0009] According to the present invention, it is possible to provide a thermally conductive, heat-dissipating composition capable of suppressing dripping, and an electronic device including the thermally conductive, heat-dissipating composition.

[0010] 1 is a schematic diagram showing steps 1 to 5 performed to measure viscosity and identify time t.

[0011] Hereinafter, an embodiment of the present invention (hereinafter referred to as "the present embodiment") will be described in detail with reference to the drawings as necessary. However, the present invention is not limited to this embodiment, and various modifications are possible without departing from the spirit of the present invention. In the drawings, the same elements are given the same reference numerals, and redundant explanations will be omitted. Furthermore, positional relationships such as up, down, left, and right are based on the positional relationships shown in the drawings unless otherwise specified. Furthermore, the dimensional ratios of the drawings are not limited to those shown in the drawings.

[0012] 1. Thermally conductive, heat-dissipating composition The thermally conductive, heat-dissipating composition of this embodiment contains a matrix component and a thermally conductive filler, and is measured at 25°C by increasing the shear rate to 10 s -1 From 0.1 seconds -1 When the shear rate was changed to 10 s -1 The viscosity η1 at a shear rate of 0.1 s -1 The time t until the viscosity η2 is stabilized at η2 is 30 seconds or less.

[0013] In non-Newtonian fluids, changing the shear rate during viscosity measurement results in an increase or decrease in the measured viscosity. The thermally conductive, heat-dissipating composition of this embodiment is used in applications such as thermal grease, and it is desirable for the composition to have excellent applicability and for the grease to flow from the applied area after application without causing sagging. Therefore, it is desirable for the composition to have a low viscosity when the shear rate is high and a high viscosity when the shear rate is low. This characteristic is also known as thixotropy.

[0014] However, simply having thixotropy is not enough to prevent dripping that occurs after dispensing using a dispenser, pump, etc. Even if a grease has thixotropy, if the time it takes for the viscosity to change is long, the grease will drip from the outlet of the dispenser or the like when dispensing is stopped. In other words, dripping will occur.

[0015] Therefore, in the thermally conductive and heat-dissipating composition of this embodiment, the shear rate is 10 s -1 The viscosity η1 at a shear rate of 0.1 s -1 The time t until the viscosity η2 at the time point is stabilized is specified. This tends to improve drip resistance.

[0016] In this embodiment, the "time t until the viscosity stabilizes at η2" is defined as follows. Unless otherwise specified below, the viscosity measurement temperature is 25°C. First, the following steps 1 to 5 are performed continuously to obtain continuous viscosity measurement results for a total of 500 seconds. Then, at a shear rate of 10 s in step 4, -1 From step 5 shear rate 0.1 s -1 The time t required for the viscosity to stabilize at η2 when the shear rate is switched to η2 is measured. Figure 1 shows a schematic diagram showing how steps 1 to 5 are repeated to determine the time t. Step 1: Shear rate 0.1 s -1 Step 2: Shear rate 10 s -1 Step 3: Shear rate 0.1 s -1 Step 4: Shear rate 10 s -1 Step 5: Shear rate 0.1 s -1 Measure for 100 seconds

[0017] As shown in Figure 1, the shear rate in step 4 was 10 s -1 From step 5 shear rate 0.1 s -1 The determination that the viscosity is stable as η2 after switching to η2 is clear as shown in Figure 1. If we define this point more strictly, for example, at a shear rate of 0.1 s in step 5, -1 Viscosity η at a certain point p measured p and viscosity η 1 second after a certain point p p+1 The difference between p ) becomes 0.0 Pa s or more and less than 0.5 Pa s, the viscosity η at time p p may be defined as "stable as viscosity η2".

[0018] In measuring the time t, the shear rate was set to 10 s as in steps 1 to 5 in order to eliminate disturbance factors when measuring the change in viscosity and to align the history of the shear rate change applied to the sample. -1 and shear rate 0.1 s -1However, the number of steps is not limited to the above and may be more or less.

[0019] In this embodiment, the shear rate of the thermally conductive and heat-dissipating composition when discharged using a dispenser or pump is set to a reference value of 10 s -1 In this regard, depending on the specifications of the dispenser, pump, or other equipment, the shear rate of the thermally conductive and heat-dissipating composition may be less than 10 s -1 However, if the shear rate during actual use is 10 s -1 Even if it takes a value larger or smaller than this, the shear rate is 10 s -1 If the time t measured based on the reference value satisfies a predetermined range and the viscosity change rate is said to be equal to or faster than a predetermined rate, then dripping can be said to be suppressed.

[0020] In this embodiment, the reference value of the shear rate of the thermally conductive and heat-dissipating composition when the discharge is stopped is a shear rate of 0.1 s -1 is used.

[0021] The time t is 30 seconds or less, preferably 0 to 25 seconds, 0 to 23 seconds, 0 to 20 seconds, 0 to 18 seconds, or 0 to 15 seconds. When t is within the above range, dripping resistance tends to be further improved.

[0022] The viscosity η1 is not particularly limited, but is preferably 50 to 180 Pa s, 60 to 170 Pa s, or 70 to 160 Pa s. When η1 is within the above range, the thermally conductive, heat-dissipating composition tends to be easy to apply and has excellent handleability.

[0023] The viscosity η2 is not particularly limited, but is preferably 180 to 400 Pa s, 190 to 370 Pa s, or 200 to 350 Pa s. When η2 is within the above range, drip resistance tends to be further improved. Furthermore, after the thermally conductive, heat-dissipating composition is applied, the viscosity increases, and dripping tends to be better suppressed.

[0024] The ratio of viscosity η2 to viscosity η1 (η2 / η1) is preferably 1.0 to 8.0, 1.1 to 6.2, or 1.3 to 5.0. When the ratio (η2 / η1) is within the above range, the rate of change of viscosity is high, and the coating properties, dripping resistance, and sagging suppression tend to be excellent.

[0025] In this embodiment, the viscosity is not particularly limited, but can be measured, for example, in accordance with JIS Z 8803: 2011. In this embodiment, the viscosity is measured at 25°C unless otherwise specified.

[0026] The thermal conductivity of the thermally conductive, heat-dissipating composition of this embodiment is preferably 4.0 W / m K or more, 4.0 to 7.5 W / m K, 4.5 to 7.0 W / m K, or 5.0 to 6.5 W / m K. Having a thermal conductivity within the above range tends to result in better heat dissipation. The thermal conductivity can be adjusted by the type and amount of the thermally conductive filler used.

[0027] In this embodiment, the thermal conductivity can be measured by a known method. More specifically, although not particularly limited, the thermal conductivity can be measured by the method described in JIS A 1412-1:2016 or the method described in the examples below.

[0028] Each component of the thermally conductive, heat-dissipating composition of this embodiment will be described in detail below.

[0029] 1.1 Matrix Component The thermally conductive, heat-dissipating composition of this embodiment includes a matrix component. The matrix component may include a surfactant and / or an organopolysiloxane.

[0030] 1.1.1 Surfactant The surfactant of this embodiment is not particularly limited, but may include, for example, a copolymer αβγ having (meth)acrylic monomer units α having a carboxy group, (meth)acrylic monomer units β having a tertiary amino group, and (meth)acrylic monomer units γ having a siloxane skeleton, or may include other surfactants (e.g., acetylene glycol-based surfactants, fluorine-based surfactants, silicone-based surfactants). In particular, it is preferable to include the copolymer αβγ.

[0031] By using such a surfactant, the increase in viscosity of the thermally conductive, heat-dissipating composition can be kept within a usable range even when the thermally conductive filler is highly dispersed in the matrix, and the high dispersion of the thermally conductive filler ensures high thermal conductivity.

[0032] The desired viscosity change (thixotropy) is thought to occur, for example, by the following mechanism: at high shear rates, non-covalent bonds such as hydrogen bonds in the composition are broken, resulting in a low viscosity, and at low shear rates, non-covalent bonds such as hydrogen bonds are reformed, resulting in a high viscosity. The strength of these non-covalent bonds and the rates at which they are broken and reformed can affect the values ​​of viscosities η1 and η2, the ratio (η2 / η1), and the time t.

[0033] A typical surfactant, for example, is located on the surface of a thermally conductive filler, improving its affinity with the matrix and thereby improving dispersibility. On the other hand, the surface of a thermally conductive filler contains a large number of atoms that contribute to non-covalent bonding, such as hydroxyl groups and ionized atoms. Therefore, if the affinity between the surfactant and the thermally conductive filler is too high, the surfactant may cover the surface of the thermally conductive filler, which has functional groups such as hydroxyl groups, as described below, and the interaction between the thermally conductive fillers may be weakened.

[0034] Therefore, from the viewpoint of adjusting such affinity and adjusting the viscosities η1, η2, the ratio (η2 / η1), and the time t (hereinafter collectively referred to as "viscosity characteristics") to fall within the above ranges, preferred embodiments of the surfactant will be described in further detail below.

[0035] The content of the surfactant is preferably 1 to 40 parts by mass, 2 to 30 parts by mass, 3 to 20 parts by mass, or 5 to 15 parts by mass relative to 100 parts by mass of the content of the matrix component described below. When the content of the surfactant is within the above range, the dispersibility of the thermally conductive filler is further improved, and the viscosity characteristics tend to fall within a more appropriate range.

[0036] The weight-average molecular weight of the surfactant is preferably 20,000 to 150,000, more preferably 30,000 to 120,000, and even more preferably 40,000 to 100,000. When the weight-average molecular weight of the surfactant is within the above range, the dispersibility of the thermally conductive filler is further improved, and the viscosity characteristics tend to be within a more appropriate range. The weight-average molecular weight can be determined by GPC (gel permeation chromatography).

[0037] The copolymer αβγ will be described in more detail below. In this embodiment, "monomer" refers to a monomer having a polymerizable unsaturated bond before polymerization, and "monomer unit" refers to a repeating unit that constitutes part of the copolymer αβγ after polymerization and is derived from a specific monomer. Furthermore, (meth)acrylic includes acrylic and methacrylic, and (meth)acrylic monomers include (meth)acrylate and (meth)acrylamide. Furthermore, hereinafter, "(meth)acrylic monomer unit α" and the like will also be simply referred to as "unit α" and the like.

[0038] In the copolymer αβγ, the units α, β, and γ may be contained randomly or in blocks. In the copolymer αβγ, it is preferable that at least the units α and γ are contained as a random copolymer. When the units α and γ are contained as a random copolymer, the viscosity characteristics tend to fall within a more appropriate range.

[0039] 1.1.1.1. (Meth)acrylic monomer unit α having a carboxy group The unit α is a repeating unit having a carboxy group. When the copolymer αβγ contains such a monomer unit, the dispersibility of the thermally conductive filler is further improved.

[0040] Preferably, the unit α further has an electron-withdrawing group bonded to the carboxy group. Such an electron-withdrawing group is not particularly limited as long as it has the effect of stabilizing the negative charge on the carboxy group. For example, the unit α may be a unit derived from an acrylic monomer containing an electron-withdrawing substituent, such as a halogen element, on the carbon atom at the α-position of the carboxy group. The inclusion of such a monomer unit tends to further improve the dispersibility of the thermally conductive filler.

[0041] The unit α preferably does not have an electron-donating group bonded to the carboxy group or has a group with low electron-donating properties. Such electron-donating groups are not particularly limited as long as they have the effect of destabilizing the negative charge on the carboxy group. For example, the monomer unit α may be a unit derived from an acrylic monomer that does not contain an electron-donating group, such as a methyl group, at the carbon atom at the α-position of the carboxy group. The inclusion of such a monomer unit tends to further improve the dispersibility of the thermally conductive filler.

[0042] Such (meth)acrylic monomers are not particularly limited, but examples include acrylic acid, methacrylic acid, 2-acryloyloxyethyl succinic acid, 2-methacryloyloxyethyl succinic acid, etc. Among these, acrylic acid and 2-methacryloyloxyethyl succinic acid are preferred, and acrylic acid is more preferred. By including units derived from such monomers, affinity for the thermally conductive filler tends to be further improved, and dispersibility of the thermally conductive filler tends to be further improved. The unit α may be used alone or in combination of two or more types.

[0043] The content of the unit α is preferably 0.05 to 20.0 parts by mass, 0.08 to 6.0 parts by mass, 0.1 to 5.0 parts by mass, 0.3 to 4.0 parts by mass, or 0.5 to 3.0 parts by mass, relative to 100 parts by mass of the total of the units α, β, and γ. Within the above range, the content of the unit α may be 0.7 parts by mass or more, or 2.0 parts by mass or less. When the content of the monomer unit α is within the above range, the dispersibility of the thermally conductive filler is further improved, and the viscosity characteristics tend to fall within a more appropriate range.

[0044] 1.1.1.2. (Meth)acrylic Monomer Unit β Having a Tertiary Amino Group The unit β is a repeating unit having a tertiary amino group. The presence of such a monomer unit in the copolymer αβγ further improves the dispersibility of the thermally conductive filler.

[0045] Preferably, the unit β further has an electron-donating group bonded to the carbon atom adjacent to the nitrogen atom in the tertiary amino group. Such an electron-donating group is not particularly limited as long as it has the effect of stabilizing the positive charge on the tertiary amino group. The unit β may be, for example, a unit derived from an acrylic monomer containing an electron-donating substituent, such as a methyl group, on the carbon atom at the α-position of the tertiary amino group. The inclusion of such a monomer unit tends to further improve the dispersibility of the thermally conductive filler.

[0046] Preferably, the β unit does not have an electron-withdrawing group bonded to the carbon atom adjacent to the nitrogen atom in the tertiary amino group, or has a group with low electron-withdrawing properties. Such an electron-withdrawing group is not particularly limited as long as it has the effect of destabilizing the positive charge on the tertiary amino group. The β unit may be, for example, a unit derived from an acrylic monomer that does not contain a substituent of an electron-withdrawing group such as a carboxyl group on the carbon atom at the α-position of the tertiary amino group. The inclusion of such a monomer unit tends to further improve the dispersibility of the thermally conductive filler.

[0047] Such (meth)acrylic monomers are not particularly limited, but examples include dimethylaminoethyl methacrylate, diethylaminoethyl methacrylate, and 1,2,2,6,6-pentamethyl-4-piperidyl methacrylate. Among these, dimethylaminoethyl methacrylate and 1,2,2,6,6-pentamethyl-4-piperidyl methacrylate are preferred, and 1,2,2,6,6-pentamethyl-4-piperidyl methacrylate is more preferred. By including units derived from such monomers, affinity for the thermally conductive filler tends to be further improved, and the dispersibility of the thermally conductive filler tends to be further improved. The unit β may be used alone or in combination of two or more types.

[0048] The content of the unit β is preferably 0.02 to 4.00 parts by mass, 0.05 to 4.00 parts by mass, 0.07 to 3.00 parts by mass, 0.80 to 2.00 parts by mass, or 0.10 to 1.00 parts by mass, relative to 100 parts by mass of the total of the units α, β, and γ. Within the above range, the content of the unit β may be 0.30 parts by mass or more, or 0.80 parts by mass or less. When the content of the monomer unit β is within the above range, the dispersibility of the thermally conductive filler is further improved, and the viscosity characteristics tend to fall within a more appropriate range.

[0049] 1.1.1.3. (Meth)acrylic Monomer Unit γ Having a Siloxane Skeleton The unit γ is a repeating unit having a siloxane skeleton. The inclusion of such a monomer unit in the copolymer αβγ increases the affinity or compatibility of the copolymer αβγ with the organopolysiloxane described below, thereby ensuring that the viscosity characteristics fall within a more appropriate range.

[0050] Examples of the siloxane skeleton in the unit γ include organopolysiloxane skeletons such as dialkylpolysiloxane, diphenylpolysiloxane, and alkylphenylpolysiloxane. The alkyl contained in the siloxane skeleton is not particularly limited, but examples thereof include methyl, ethyl, propyl, butyl, pentyl, and hexyl groups. The phenyl group contained in the siloxane skeleton is not particularly limited, but examples thereof include phenyl and benzyl groups.

[0051] Such (meth)acrylic monomers are not particularly limited, but examples thereof include (meth)acrylic acid polysiloxanes in which the terminals of the siloxane skeletons are modified with (meth)acrylic acid, as described above. Specific examples include α-butyl-ω-(3-methacryloxypropyl)polydimethylsiloxane. The monomer unit γ may be used alone or in combination of two or more.

[0052] The number average molecular weight of the monomer unit γ is preferably 1,500 to 50,000, 3,000 to 30,000, or 4,000 to 20,000. When the number average molecular weight of the monomer unit γ is 50,000 or less, the viscosity characteristics tend to be within a more appropriate range. In addition, dripping resistance tends to be further improved. The number average molecular weight of the monomer unit γ can be determined by GPC (gel permeation chromatography).

[0053] The content of the unit γ is preferably 70.0 to 99.9 parts by mass, 80.0 to 99.5 parts by mass, 90.0 to 99.0 parts by mass, 93.0 to 99.0 parts by mass, or 96.0 to 99.0 parts by mass, relative to 100 parts by mass of the total of the units α, β, and γ. When the content of the unit γ is within the above range, the dispersibility of the thermally conductive filler is further improved, and the viscosity characteristics tend to fall within a more appropriate range. In addition, dripping resistance tends to be further improved.

[0054] The total content of the units α, β, and γ in the copolymer αβγ is preferably 90% by mass or more, 95% by mass or more, 99% by mass or more, or 100% by mass, based on the total amount of the copolymer αβγ. When the total content is within the above range, the dispersibility of the thermally conductive filler is further improved, and the viscosity characteristics tend to fall within a more appropriate range. The upper limit of the total content of the units α, β, and γ is not particularly limited, and may be, for example, 100% by mass, 99% by mass, 98% by mass, or 95% by mass.

[0055] 1.1.1.4. Production Method The method for producing the copolymer αβγ is not particularly limited, and known polymerization methods for (meth)acrylic monomers can be used. Examples of the polymerization method include radical polymerization and anionic polymerization. Among these, radical polymerization is preferred.

[0056] The thermal polymerization initiator used in the radical polymerization is not particularly limited, but examples thereof include azo compounds such as azobisisobutyronitrile; and organic peroxides such as benzoyl peroxide, tert-butyl hydroperoxide, and di-tert-butyl peroxide. Furthermore, the photopolymerization initiator used in the radical polymerization is not particularly limited, but examples thereof include benzoin derivatives. Furthermore, known polymerization initiators used in living radical polymerization such as ATRP and RAFT can also be used.

[0057] The polymerization conditions are not particularly limited and can be appropriately adjusted depending on the initiator and boiling point of the solvent used, and the types of other monomers.

[0058] The order of adding the monomers is not particularly limited. For example, when synthesizing a random copolymer, the monomers may be mixed to initiate polymerization, and when synthesizing a block copolymer, the monomers may be added sequentially to the polymerization system.

[0059] 1.1.2. Organopolysiloxane The shape of the organopolysiloxane of this embodiment is not particularly limited, and examples thereof include non-crosslinked organopolysiloxanes such as linear organopolysiloxanes, branched organopolysiloxanes, and cyclic organopolysiloxanes; and crosslinked organopolysiloxanes that are three-dimensionally crosslinked within the molecule.

[0060] Generally, organopolysiloxanes contain monofunctional units (R 1 SiO 1 / 2 ), bifunctional units (R 2 SiO 2 / 2 ), trifunctional unit (R 3 SiO 3 / 2 ), and a tetrafunctional unit (SiO 4 / 2 For example, a linear organopolysiloxane can be represented by the following formula: 1 SiO 1 / 2 ) and a bifunctional unit (R 2 SiO 2 / 2 ) (n3, n4 = 0 in the following formula), and the cyclic organopolysiloxane can be expressed as having a bifunctional unit (RSiO 2 / 2) (n1, n3, n4 = 0 in the following formula). In addition, branched organopolysiloxanes and three-dimensionally crosslinked organopolysiloxanes have a trifunctional unit (R 3 SiO 3 / 2 ) and / or tetrafunctional units (SiO 4 / 2 ), and further comprising a monofunctional unit (R 1 SiO 1 / 2 ), a bifunctional unit (R 2 SiO 2 / 2 ) can be expressed as having

[0061] A composition formula using such units can be expressed as follows: In the following formula, n1 to n4 indicate the composition ratio of each unit, and can be expressed as a ratio such that the sum of n1 to n4 is 1. Whether or not these units are contained can be measured by a known method such as Si-NMR. 1 ~R 3 Each of R can independently represent any group. 1 SiO 1 / 2 ) n1 (R 2 SiO 2 / 2 ) n2 (R 3 SiO 3 / 2 ) n3 (SiO 4 / 2 ) n4

[0062] The organopolysiloxane of this embodiment is not particularly limited, but examples thereof include non-curable organopolysiloxanes and curable organopolysiloxanes. The non-curable organopolysiloxane is not particularly limited, as long as it does not have the functional group that contributes to curing that the curable organopolysiloxane has, or is not used in combination with a catalyst. The curable organopolysiloxane is not particularly limited, but examples thereof include a combination of two organopolysiloxanes having functional groups that react with each other. Such curable organopolysiloxanes are not particularly limited, but examples thereof include addition-curable organopolysiloxanes, condensation-curable organopolysiloxanes, and peroxide-curable organopolysiloxanes.

[0063] More specifically, the organopolysiloxane of this embodiment is not particularly limited, but examples thereof include dimethylpolysiloxane, diphenylpolysiloxane, and methylphenylpolysiloxane. These organopolysiloxanes may have organic groups introduced into their side chains and / or terminals. Such organopolysiloxanes are not particularly limited, and examples thereof include non-reactive organopolysiloxanes such as long-chain alkyl-modified organopolysiloxanes, polyether-modified organopolysiloxanes, aralkyl-modified organopolysiloxanes, fatty acid ester-modified organopolysiloxanes, and fatty acid amide-modified organopolysiloxanes; and reactive organopolysiloxanes such as amine-modified organopolysiloxanes, epoxy-modified organopolysiloxanes, mercapto-modified organopolysiloxanes, carboxyl-modified organopolysiloxanes, carbinol-modified organopolysiloxanes, hydrogen-modified organopolysiloxanes, vinyl-modified organopolysiloxanes, and hydrosilyl-modified organopolysiloxanes. The organopolysiloxanes may be used alone or in combination of two or more.

[0064] The content of the organopolysiloxane is preferably 60 to 99 mass %, 70 to 98 mass %, or 80 to 95 mass %, based on the total amount of components other than the thermally conductive filler in the thermally conductive, heat-dissipating composition. By having the organopolysiloxane content within this range, the viscosity characteristics of the thermally conductive, heat-dissipating composition tend to be within a more appropriate range.

[0065] 1.2. Thermally Conductive Filler The thermally conductive, heat-dissipating composition of this embodiment contains a thermally conductive filler. The thermally conductive filler is a filler that has thermal conductivity. The thermal conductivity of the thermally conductive filler is not particularly limited, but is, for example, 10 W / m K or more.

[0066] Such thermally conductive fillers are not particularly limited, but examples thereof include aluminum oxide (hereinafter also referred to as "alumina"), aluminum nitride, boron nitride, silicon nitride, zinc oxide, aluminum hydroxide, metallic aluminum, magnesium oxide, diamond, carbon, indium, gallium, copper, silver, iron, nickel, gold, tin, metallic silicon, etc. In this embodiment, the thermally conductive filler does not include Si-containing powder, which will be described later, and the two are distinguished for convenience.

[0067] Among these, the thermally conductive filler preferably contains one or more selected from the group consisting of boron nitride, aluminum nitride, aluminum oxide, silicon nitride, silicon oxide, magnesium oxide, metallic aluminum, and zinc oxide, more preferably contains one or more selected from the group consisting of aluminum oxide, magnesium oxide, aluminum nitride, and metallic aluminum, and even more preferably contains aluminum oxide. This is because the thermally conductive filler has high thermal conductivity, high insulating properties, and is inexpensive. The thermally conductive filler may be used alone or in combination of two or more.

[0068] The average particle size of the thermally conductive filler is preferably 0.05 to 120.0 μm, and more preferably 0.1 to 70.0 μm. When the average particle size of the thermally conductive filler is within the above range, the flowability, dispersibility, and filling ability of the thermally conductive filler tend to be further improved.

[0069] The thermally conductive filler may be a mixture of fillers having different average particle sizes. Preferably, the thermally conductive filler is a combination of two or more of the thermally conductive filler (C1-1) having an average particle size of 30.0 to 100.0 μm, the thermally conductive filler (C1-2) having an average particle size of 1.5 to 25.0 μm, and the thermally conductive filler (C1-3) having an average particle size of 0.05 to 1.0 μm. It is more preferable to use at least the thermally conductive filler (C1-1) and the thermally conductive filler (C1-2). It is even more preferable to use all of the thermally conductive filler (C1-1), the thermally conductive filler (C1-2), and the thermally conductive filler (C1-3).

[0070] The average particle size of the thermally conductive filler can be measured using, for example, a Shimadzu SALD-20 laser diffraction particle size analyzer. The evaluation sample is prepared by adding 50 ml of pure water and 5 g of the thermally conductive filler powder to be measured to a glass beaker, stirring with a spatula, and then dispersing in an ultrasonic cleaner for 10 minutes. The dispersed solution of the thermally conductive filler powder is then added dropwise to the sampler section of the analyzer using a dropper. Measurements can be performed once the absorbance has stabilized. The laser diffraction particle size analyzer calculates the particle size distribution from the light intensity distribution data of the diffraction / scattering holes detected by the sensor. The average particle size is calculated by multiplying the measured particle size value by the relative particle amount (difference %) and dividing by the sum of the relative particle amounts (100%). The average particle size is the average diameter of the particles and can be calculated as the cumulative weight average value D50 (median diameter). D50 is the particle size with the highest occurrence rate. In this specification, the average particle size refers to D50 (median diameter).

[0071] In this case, the content of the thermally conductive filler (C1-1) is preferably 30 to 70 mass%, or 40 to 60 mass%, based on the total amount of the thermally conductive fillers. The content of the thermally conductive filler (C1-2) is preferably 10 to 50 mass%, or 20 to 40 mass%, based on the total amount of the thermally conductive fillers. The content of the thermally conductive filler (C1-3) is preferably 5 to 30 mass%, or 10 to 20 mass%, based on the total amount of the thermally conductive fillers. By using such thermally conductive fillers, the fluidity of the thermally conductive heat-dissipating composition of this embodiment and the dispersibility and filling ability of the thermally conductive filler tend to be further improved.

[0072] The content of the thermally conductive filler is preferably 400 to 3,000 parts by mass, 600 to 2,800 parts by mass, or 700 to 2,600 parts by mass relative to 100 parts by mass of the matrix component. When the content of the thermally conductive filler is 400 parts by mass or more, the thermal conductivity tends to be further improved, and when it is 3,000 parts by mass or less, the viscosity characteristics tend to fall within a more appropriate range.

[0073] 1.3 Si-containing powder The thermally conductive, heat-dissipating composition of this embodiment preferably contains a Si-containing powder. The Si-containing powder is a powder of a substance containing elemental Si, such as silica.

[0074] The surface of Si-containing powder is easily oxidized in the atmosphere, and this oxidized surface easily changes to a hydroxylated surface by chemical adsorption of water vapor. Therefore, Si-containing powders generally have hydroxyl groups on their surfaces. Si-containing powders with hydroxyl groups on their surfaces easily interact with each other through hydrogen bonds, and at low shear rates, the hydrogen bonds increase the viscosity of the thermally conductive, heat-dissipating composition. On the other hand, at high shear rates, the hydrogen bonds are broken, decreasing the viscosity of the thermally conductive, heat-dissipating composition. Therefore, when the thermally conductive, heat-dissipating composition of this embodiment contains a Si-containing powder, its thixotropy is thought to be improved. However, the factors that improve thixotropy are not limited to those mentioned above.

[0075] Furthermore, as mentioned above, the surfactant covers the surface of the thermally conductive filler, which can affect the interaction between the thermally conductive fillers. However, the Si-containing powder has a relatively low affinity with the surfactant, so it has little effect on the interaction of the surfactant. Therefore, the use of the Si-containing powder tends to increase the viscosity η2, shorten the time t, and provide good thixotropy. The affinity between the Si-containing powder and the surfactant, and between the thermally conductive filler and the surfactant, can be determined more specifically by measuring the zeta potential.

[0076] The zeta potential of alumina in water is a positive value of about 40 to 60 mV. In contrast, the zeta potential of a sample of alumina dispersed in copolymer αβγ gradually decreases as the amount of copolymer αβγ added increases. As an example, the zeta potential of a sample containing 0.005 g of alumina, 25 g of water, and 1.0 mass % copolymer αβγ can be about 0 mV. This change in zeta potential is thought to be due to the interaction of copolymer αβγ with alumina, which affects the zeta potential.

[0077] On the other hand, the zeta potential of silica in water is a negative value of about -40 to -60 mV. In contrast, the zeta potential of water in samples in which silica is dispersed with copolymer αβγ does not change significantly even when the amount of polymer αβγ added is increased. This maintenance of the zeta potential is thought to be due to the fact that copolymer αβγ does not interact easily with silica, which does not affect the zeta potential.

[0078] The example of alumina and silica is just one example, but as described above, by adjusting the combination of the thermally conductive filler, surfactant, and Si-containing powder, it is possible to adjust the viscosity at each shear rate and the time t for the viscosity to change.

[0079] In the present embodiment, the zeta potential is not particularly limited, but can be measured in accordance with, for example, JIS Z 8836:2017.

[0080] The Si-containing powder of this embodiment is not particularly limited, but examples thereof include Si-containing powders with hydrophilic surfaces and Si-containing powders with hydrophobic surfaces. Among these, Si-containing powders with hydrophilic surfaces are preferred. Furthermore, Si-containing powders with hydrophilic surfaces are not particularly limited, but examples thereof include silica powder and mullite powder. Among these, silica powder is preferred. Although the silica powder is not particularly limited, examples thereof include surface-treated silica powder and surface-untreated silica powder. From the viewpoint that it is preferable for the silica powder to have hydroxyl groups on its surface, surface-untreated silica powder is preferred. Furthermore, although the silica powder is not particularly limited, examples thereof include crystalline silica powder and fused silica powder.

[0081] Since the thermal conductivity of Si-containing powders is not as high as that of thermally conductive fillers, it is preferable to maximize the effect of the hydrogen bonds with a small content, and it is preferable to use Si-containing powders with a large surface area. From this perspective, the particle size of the Si-containing powder is preferably 2.0 to 5000.0 nm, 2.5 to 1000.0 nm, 3.0 to 500.0 nm, 3.5 to 100.0 nm, 4.0 to 50.0 nm, 4.5 to 30.0 nm, or 5.0 to 25.0 nm. Also, preferably, it is 5.0 to 500.0 nm, 5.0 to 1000.0 nm, 5.0 to 5000.0 nm, or 5.0 to 6000.0 nm.

[0082] From the viewpoint of improving the thermal conductivity of the thermally conductive heat dissipating composition of this embodiment, the content of the Si-containing powder is preferably 0.1 to 20.0 parts by mass, 0.2 to 15.0 parts by mass, 0.3 to 12.5 parts by mass, 0.4 to 11.5 parts by mass, or 0.5 to 10.0 parts by mass, relative to 100 parts by mass of the content of the matrix component.

[0083] The content of the Si-containing powder is preferably 0.01 to 1.00 parts by mass, 0.02 to 0.80 parts by mass, or 0.03 to 0.60 parts by mass, relative to 100 parts by mass of the thermally conductive filler. When the content of the Si-containing powder is within the above range, the thermally conductive, heat-dissipating composition tends to have both good thermal conductivity and thixotropy.

[0084] 1.4. Other Components The thermally conductive and heat-dissipating composition of this embodiment may contain a flame retardant aid, a flame retardant, a colorant, a tackifier, an ultraviolet absorber, an antioxidant, a fluorescent brightener, a photosensitizer, a thickener, a lubricant, an antifoaming agent, a surface conditioner, a glossing agent, or the like. The content of the other components is not particularly limited, but is, for example, 0.001 to 20.0 parts by mass, 0.1 to 15.0 parts by mass, or 0.5 to 10.0 parts by mass relative to 100 parts by mass of the matrix component. It may also be 0.001 to 0.2 parts by mass. Furthermore, the composition may not contain any other components.

[0085] 1.5. One-component thermally conductive, heat-dissipating composition The thermally conductive, heat-dissipating composition of this embodiment may be a one-component thermally conductive, heat-dissipating composition. Being a one-component composition, it can be used without the need to mix with other components, which is preferable in terms of handling. Each component of the one-component thermally conductive, heat-dissipating composition of this embodiment will be described in detail below.

[0086] 1.5.1 Organopolysiloxane Among the above-mentioned organopolysiloxane shapes, non-crosslinked organopolysiloxanes are preferred, and linear organopolysiloxanes are more preferred. Use of such organopolysiloxanes tends to result in viscosity characteristics within a more appropriate range.

[0087] Of the organopolysiloxanes described above, non-curable organopolysiloxanes are preferred. Use of such organopolysiloxanes tends to improve handling. More specifically, dimethylsilicone, diphenylsilicone, methylphenylsilicone, and non-reactive silicones are preferred, with dimethylsilicone being more preferred. Use of such organopolysiloxanes tends to result in viscosity characteristics within a more appropriate range.

[0088] 1.5.2. Silane Coupling Agent The one-component thermally conductive and heat-dissipating composition of this embodiment may further contain a silane coupling agent.

[0089] The silane coupling agent is not particularly limited, but examples thereof include epoxy silanes such as γ-glycidoxypropyltrimethoxysilane and β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; amino silanes such as aminopropyltriethoxysilane, ureidopropyltriethoxysilane and N-phenylaminopropyltrimethoxysilane; and hydrophobic silane compounds such as phenyltrimethoxysilane, methyltrimethoxysilane, octadecyltrimethoxysilane and n-decyltrimethoxysilane. Of these, hydrophobic silane compounds are more preferred.

[0090] The content of the silane coupling agent is not particularly limited, and may be, for example, 0.1 to 10.0 parts by mass, 0.1 to 5.0 parts by mass, 0.1 to 2.5 parts by mass, 0.1 to 1.0 parts by mass, or 0.1 to 0.5 parts by mass relative to 100 parts by mass of the matrix component. In addition, the silane coupling agent may not be contained.

[0091] 1.6. Two-component curing thermally conductive, heat-dissipating composition The thermally conductive, heat-dissipating composition of this embodiment may be a two-component curing thermally conductive, heat-dissipating composition containing a first component and a second component. Being a two-component curing composition tends to improve reliability. Furthermore, mixing the two components and curing them to form a cured product tends to improve durability.

[0092] 1.6.1. First Agent The first agent of this embodiment preferably contains the matrix component, the thermally conductive filler, and the Si-containing powder. Specific examples and preferred aspects of the surfactant, thermally conductive filler, and Si-containing powder are the same as those described in detail for the thermally conductive heat-dissipating composition, and therefore, redundant explanations will be omitted. Below, the non-overlapping parts of each component of the first agent of this embodiment will be described in detail.

[0093] 1.6.1.1 Organopolysiloxane The organopolysiloxane of the first agent of this embodiment preferably includes a reactive organopolysiloxane from among the organopolysiloxanes described above, and more preferably includes a vinyl-modified organopolysiloxane. The vinyl-modified organopolysiloxane is an organopolysiloxane having at least one vinyl group. The vinyl-modified organopolysiloxane may have a vinyl group on a side chain and / or at a terminal. Such an organopolysiloxane has a structural unit represented by the following formula (1-1) or a terminal structure represented by formula (1-2). The vinyl-modified organopolysiloxane may have, for example, at least one of the structural unit represented by formula (1-1) and the terminal structure represented by formula (1-2), and a structural unit represented by formula (1-3).

[0094]

[0095] In formulas (1-1), (1-2), and (1-3), R represents any monovalent hydrocarbon group which may have a substituent. That is, in the vinyl-modified organopolysiloxane, any monovalent hydrocarbon group which may have a substituent is bonded to a side chain of the siloxane skeleton.

[0096] Such monovalent hydrocarbon groups are not particularly limited, and examples thereof include alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, and dodecyl; cycloalkyl groups such as cyclopentyl and cyclohexyl; aryl groups such as phenyl, tolyl, xylyl, and naphthyl; aralkyl groups such as benzyl, 2-phenylethyl, and 2-phenylpropyl; and groups having a substituent in these groups. Examples of the substituent in the above monovalent hydrocarbon group include a halogen atom, particularly a fluorine atom or a chlorine atom.

[0097] The vinyl-modified organopolysiloxane is contained in the first agent either alone or in combination of two or more. The number of vinyl groups in the vinyl-modified organopolysiloxane contained in the first agent is preferably 2.0 or more on average per molecule. That is, when the first agent contains one type of vinyl-modified organopolysiloxane, it is preferable that the organopolysiloxane has two or more vinyl groups per molecule. When the first agent contains two or more types of vinyl-modified organopolysiloxane, it is preferable that the arithmetic average number of vinyl groups in each organopolysiloxane is 2.0 or more. By having the number of vinyl groups per molecule of 2.0 or more, the crosslink density can be adjusted, and the curing rate when the first agent and the second agent are mixed tends to be in a more suitable range. As a result, the dripping resistance of the two-component curing thermally conductive and heat-dissipating composition tends to be further improved. The upper limit of the number of vinyl groups in the vinyl-modified organopolysiloxane is not particularly limited, and may be, for example, an average of 4.0, 3.0, or 2.5 per molecule, and the average number of vinyl groups in the vinyl-modified organopolysiloxane per molecule may be 2.0.

[0098] The average number of vinyl groups per molecule of the vinyl-modified organopolysiloxane can be measured by NMR. Specifically, for example, measurement can be performed using an ECP-300NMR manufactured by JEOL, with the vinyl-modified organopolysiloxane dissolved in deuterated chloroform as a deuterated solvent. The average number of vinyl groups per molecule can be calculated by dividing the measurement result thus obtained by the average molecular weight of the vinyl-modified organopolysiloxane.

[0099] The vinyl-modified organopolysiloxane preferably contains at least an organopolysiloxane having vinyl groups at both ends. The use of such an organopolysiloxane tends to allow the crosslinking density to be adjusted, and the curing rate when the first and second components are mixed tends to be within a more suitable range. As a result, the dripping resistance of the two-cure type thermally conductive and heat-dissipating composition tends to be further improved. From the same perspective, the vinyl-modified organopolysiloxane preferably contains at least a polydimethylsiloxane having vinyl groups at both ends.

[0100] The viscosity of the vinyl-modified organopolysiloxane at 25°C is preferably 30 to 500 mPa·s, 50 to 400 mPa·s, or 70 to 300 mPa·s. When the viscosity of the vinyl-modified organopolysiloxane is 500 mPa·s or less, the viscosity characteristics of the first agent tend to be within a more appropriate range. When the viscosity of the vinyl-modified organopolysiloxane is 30 mPa·s or more, the mechanical strength of the cured product, such as the shear displacement and elongation at break, described below, tends to be further improved.

[0101] In this specification, the viscosity of organopolysiloxane at 25°C can be measured using a digital viscometer "DV-1" manufactured by Brookfield Corp. Using an RV spindle set and rotor No. 1, a container is used that can accommodate the rotor and that can hold organopolysiloxane up to the reference line, and the rotor is immersed in the organopolysiloxane, and the viscosity is measured at 25°C and 10 rpm.

[0102] As will be described later, a reactive organopolysiloxane such as a vinyl-modified organopolysiloxane undergoes an addition reaction with a reactive organopolysiloxane such as a hydrosilyl-modified organopolysiloxane that is preferably contained in the second part in the presence of an addition reaction catalyst. By appropriately adjusting the number of reactive groups in the reactive organopolysiloxane contained in the first part (e.g., the number of vinyl groups in the vinyl-modified organopolysiloxane), the number of reactive groups in the reactive organopolysiloxane contained in the second part (e.g., the number of hydrosilyl groups in the hydrosilyl-modified organopolysiloxane), and the viscosity, it is possible to control the viscosity of the first part and the second part, as well as the curing rate when the first part and the second part are mixed.

[0103] The content of the vinyl-modified organopolysiloxane is preferably 60 to 99 mass%, 70 to 98 mass%, or 80 to 95 mass%, relative to the total amount of components other than the thermally conductive filler in the first agent. When the content of the vinyl-modified organopolysiloxane is within the above range, the viscosity characteristics of the first agent tend to be within a more appropriate range, and the curing rate when the first and second agents are mixed tends to be within a more appropriate range.

[0104] The first agent of this embodiment may further contain an organopolysiloxane other than the vinyl-modified organopolysiloxane. From the viewpoint of improving the storage stability of the first agent, the other organopolysiloxane is preferably at least one selected from the group consisting of dimethylpolysiloxane, diphenylpolysiloxane, methylphenylpolysiloxane, and non-reactive organopolysiloxane.

[0105] The content of the other organopolysiloxane is preferably 0.1 to 10.0 mass%, 0.3 to 7.5 mass%, or 0.5 to 5.0 mass%, relative to the total amount of components other than the thermally conductive filler in the first agent. In addition, the other organopolysiloxane may not be contained.

[0106] 1.6.1.2. Addition Reaction Catalyst The first component of this embodiment preferably further contains an addition reaction catalyst. The addition reaction catalyst is not particularly limited as long as it catalyzes the addition reaction between the reactive organopolysiloxane, such as a vinyl-modified organopolysiloxane, contained in the first component and the hydrosilyl-modified organopolysiloxane contained in the second component. Examples of addition reaction catalysts include platinum compound catalysts, rhodium compound catalysts, and palladium compound catalysts. Of these, platinum compound catalysts are preferred. The use of such an addition reaction catalyst can keep the curing rate within a suitable range when the first and second components are mixed, which tends to further improve the dripping resistance of the two-component curing thermally conductive and heat-dissipating composition.

[0107] The platinum compound catalyst is not particularly limited, but examples thereof include simple platinum, platinum compounds, and platinum-supported inorganic powders. The platinum compound is not particularly limited, but examples thereof include chloroplatinic acid, platinum-olefin complexes, platinum-alcohol complexes, platinum coordination compounds, etc. Furthermore, the platinum-supported inorganic powder is not particularly limited, but examples thereof include platinum-supported alumina powder, platinum-supported silica powder, and platinum-supported carbon powder.

[0108] The addition reaction catalyst may be used alone or in combination of two or more. Furthermore, the addition reaction catalyst may be blended alone when preparing the first agent, or may be blended in a premixed state with other components, such as the vinyl-modified organopolysiloxane or other organopolysiloxanes.

[0109] The content of the addition reaction catalyst is preferably 0.1 to 30 parts by mass, 0.5 to 20 parts by mass, or 1 to 10 parts by mass, relative to 100 parts by mass of the matrix component. When the content of the addition reaction catalyst is within the above range, the curing speed when the first and second parts are mixed can be set within a suitable range, and the dripping resistance of the two-component curing thermally conductive and heat-dissipating composition tends to be further improved.

[0110] 1.6.1.3 Other Components The first agent of the present embodiment may contain other components. In addition to the components described above in the thermally conductive heat-dissipating composition, examples of other components include a reaction retarder.

[0111] The reaction retarder is not particularly limited as long as it is a component that retards the reaction when the first and second agents are mixed, but examples include alkenyl alcohols, of which 1-ethynyl-1-cyclohexanol is preferred. When the first agent contains a reaction retarder, the content of the reaction retarder is preferably 0.1 to 20.0 parts by mass, and more preferably 0.5 to 10.0 parts by mass, per 100 parts by mass of the matrix component. The reaction retarder may be contained only in the second agent and not in the first agent, or it may not be contained in either the first or second agent.

[0112] The first agent of the present embodiment is a compound represented by the following formula: 1 a R 2 b Si(OR 3 ) 4-(a+b) (R 1 are each independently an alkyl group having 1 to 15 carbon atoms, and R 2 are each independently a saturated or unsaturated monovalent hydrocarbon group having 1 to 8 carbon atoms, and R 3 are each independently an alkyl group having 1 to 6 carbon atoms, a is 1 to 3, b is 0 to 2, and a+b is 1 to 3.

[0113] Although such organosilanes have traditionally been used to improve the wettability of thermally conductive fillers, they are preferably not included in the first component of the two-component curing thermally conductive and heat-dissipating composition of this embodiment. In this embodiment, the viscosity characteristics of the first component tend to be within a more appropriate range compared to when the above-described organosilanes are included. The reason for this is not entirely clear, but it is thought that when the first component contains an organosilane, the copolymer αβγ and the organosilane compete with each other as components for improving the wettability of the thermally conductive filler, thereby reducing the effect of the copolymer αβγ.

[0114] Furthermore, when the first agent of the present embodiment contains a Si-containing powder, the organosilane as described above covers the Si-containing powder, preventing interactions such as hydrogen bonding between the Si-containing powders, and as a result, the thixotropy of the thermally conductive and heat-dissipating composition of the present embodiment tends to decrease. Therefore, from this perspective, it is preferable that the first agent does not contain the organosilane as described above.

[0115] R in the above formula 1 Although not particularly limited, examples of R include a methyl group, an ethyl group, a propyl group, a hexyl group, a nonyl group, a decyl group, a dodecyl group, and a tetradecyl group. 1 is preferably an alkyl group having 6 to 12 carbon atoms.

[0116] R in the above formula 2 Examples of the alkyl group include, but are not limited to, alkyl groups such as methyl, ethyl, propyl, hexyl, and octyl; cycloalkyl groups such as cyclopentyl and cyclohexyl; alkenyl groups such as vinyl and allyl; aryl groups such as phenyl and tolyl; aralkyl groups such as 2-phenylethyl and 2-methyl-2-phenylethyl; and halogenated hydrocarbon groups such as 3,3,3-trifluoropropyl, 2-(perfluorobutyl)ethyl, 2-(perfluorooctyl)ethyl, and p-chlorophenyl.

[0117] R in the above formula 3 Although there are no particular limitations on the group, it is, for example, an alkyl group having 1 to 6 carbon atoms such as a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, or a hexyl group, and preferably a methyl group or an ethyl group.

[0118] In the above formula, a is an integer of 1 to 3, preferably 1. Furthermore, b is an integer of 0 to 2, preferably 0. Furthermore, a+b is an integer of 1 to 3, preferably 1.

[0119] The content of the organosilane in the first agent is not particularly limited relative to 100 parts by mass of the thermally conductive filler, but may be, for example, 1 part by mass or less, 0.1 parts by mass or less, 0.01 parts by mass or less, or 0 parts by mass (i.e., no organosilane is included).

[0120] 1.6.1.4. Viscosity of the first agent at 25°C and a shear rate of 10 s -1 The viscosity at 1000 rpm is preferably 50 to 160 Pa·s, 60 to 150 Pa·s, or 70 to 140 Pa·s. When the viscosity is 50 Pa·s or more, the dripping resistance of the two-component curing thermally conductive and heat-dissipating composition tends to be further improved. When the viscosity is 160 Pa·s or less, the composition tends to be easier to handle and the coatability of the mixture obtained by mixing the first and second components tends to be further improved. Note that this viscosity is measured at a shear rate of 10 s -1 The definition of "stable" here is "a viscosity that is stable at a shear rate of 0.1 s -1 This is the same as the definition of "stable" when saying that the viscosity is stabilized at η2 at

[0121] The first agent and the second agent described later were subjected to a shear rate of 10 s at 25°C. -1 The viscosity at 1000 kJ / s can be measured using a rotational rheometer "HANKE MARSIII" manufactured by Thermo Fisher Scientific. More specifically, the viscosity at 1000 kJ / s can be measured using parallel plates with a diameter of 35 mm, a gap of 0.5 mm, a temperature of 25°C, and a shear rate of 10 s -1 The measurement can be performed under the following conditions.

[0122] 1.6.2. Second Agent The second agent of this embodiment preferably contains the matrix component, the thermally conductive filler, and the Si-containing powder. Specific examples and preferred aspects of the surfactant, thermally conductive filler, Si-containing powder, and other components are the same as those described in detail for the thermally conductive and heat-dissipating composition, and therefore, redundant explanations will be omitted. Below, the non-overlapping parts of each component of the first agent of this embodiment will be described in detail.

[0123] 1.6.2.1 Organopolysiloxane The organopolysiloxane of the second agent of this embodiment preferably contains a reactive organopolysiloxane from among the organopolysiloxanes described above, more preferably contains a vinyl-modified organopolysiloxane and / or a hydrosilyl-modified organopolysiloxane, and even more preferably contains a vinyl-modified organopolysiloxane and a hydrosilyl-modified organopolysiloxane.

[0124] The content of the organopolysiloxane is preferably 60 to 99 mass%, 70 to 98 mass%, or 80 to 95 mass%, relative to the total amount of components other than the thermally conductive filler in the second part. By having the content within the above range, the viscosity characteristics of the second part tend to fall within a more appropriate range, and the curing rate when the first part and the second part are mixed tends to fall within a more appropriate range.

[0125] In the second agent of the present embodiment, the mass ratio of the hydrosilyl-modified organopolysiloxane to the vinyl-modified organopolysiloxane ([mass of hydrosilyl-modified organopolysiloxane] / [mass of vinyl-modified organopolysiloxane]) is preferably 2.0 to 10.0, 2.5 to 7.5, or 3.0 to 6.0.

[0126] 1.6.2.1.1 Vinyl-modified organopolysiloxane Details of the vinyl-modified organopolysiloxane, such as specific examples and preferred embodiments, are the same as those of the vinyl-modified organopolysiloxane contained in the first agent, and redundant explanations will be omitted. The vinyl-modified organopolysiloxane contained in the first agent and the vinyl-modified organopolysiloxane contained in the second agent may be the same or different.

[0127] In the second agent, the content of the vinyl-modified organopolysiloxane is preferably 5 to 40 parts by mass, 7 to 35 parts by mass, 10 to 30 parts by mass, 12 to 28 parts by mass, or 15 to 25 parts by mass, per 100 parts by mass of the total of the organopolysiloxanes. By having the content of the vinyl-modified organopolysiloxane within the above range, the curing rate when the first agent and the second agent are mixed tends to be within a more suitable range.

[0128] 1.6.2.1.2. Hydrosilyl-Modified Organopolysiloxanes Hydrosilyl-modified organopolysiloxanes are organopolysiloxanes having at least one hydrosilyl group. The hydrosilyl-modified organopolysiloxane may have a hydrosilyl group on a side chain and / or at a terminal. Such organopolysiloxanes have a structural unit represented by the following formula (2-1) or a terminal structure represented by formula (2-2). The hydrosilyl-modified organopolysiloxane may have, for example, at least one of the structural unit represented by formula (2-1) and the terminal structure represented by formula (2-2), and a structural unit represented by formula (2-3).

[0129]

[0130] In formulas (2-1), (2-2), and (2-3), R represents any monovalent hydrocarbon group which may have a substituent. That is, in the hydrosilyl-modified organopolysiloxane, any monovalent hydrocarbon group which may have a substituent is bonded to a side chain of the siloxane skeleton.

[0131] Such monovalent hydrocarbon groups include the same monovalent hydrocarbon groups that may be contained in the vinyl-modified organopolysiloxane in the first agent.

[0132] The hydrosilyl-modified organopolysiloxane may be contained in the second agent either alone or in combination of two or more. For example, the second agent preferably contains, as the hydrosilyl-modified organopolysiloxane, at least hydrosilyl-modified organopolysiloxane E22 having hydrosilyl groups on side chains, and more preferably contains hydrosilyl-modified organopolysiloxane E21 having hydrosilyl groups on both terminals and the hydrosilyl-modified organopolysiloxane E22.

[0133] The hydrosilyl-modified organopolysiloxane E21 has at least two hydrosilyl groups at both ends of the organopolysiloxane skeleton. The hydrosilyl-modified organopolysiloxane E21 may further have a hydrosilyl group in a side chain. The hydrosilyl-modified organopolysiloxane E21 may be an organopolysiloxane having hydrosilyl groups only at both ends.

[0134] The hydrosilyl-modified organopolysiloxane E22 has at least one hydrogen atom in a side chain of the organopolysiloxane skeleton, and this hydrogen atom and a silicon atom constitute a hydrosilyl group. The hydrosilyl-modified organopolysiloxane E22 may further have hydrosilyl groups at both ends of the organopolysiloxane skeleton. The number of hydrosilyl groups in the hydrosilyl-modified organopolysiloxane E22 is preferably more than 2.0 on average per molecule, 2.5 or more on average per molecule, or 3.0 or more on average per molecule. The upper limit of the hydrosilyl groups in the hydrosilyl-modified organopolysiloxane E22 is not particularly limited, and may be, for example, 8.0, 6.0, or 5.0 on average per molecule.

[0135] The number of hydrosilyl groups in the hydrosilyl-modified organopolysiloxane contained in the second agent is preferably more than 2.0 on average per molecule, and 2.5 or more on average per molecule. That is, when the second agent contains one type of hydrosilyl-modified organopolysiloxane, it is preferable that the organopolysiloxane has more than two (i.e., three or more) hydrosilyl groups per molecule. When the second agent contains two or more types of hydrosilyl-modified organopolysiloxane, it is preferable that the arithmetic average number of hydrosilyl groups in each hydrosilyl-modified organopolysiloxane is more than 2.0.

[0136] Since the number of hydrosilyl groups in hydrosilyl-modified organopolysiloxane E21 and hydrosilyl-modified organopolysiloxane E22 can be controlled separately as described above, by appropriately mixing the two, it tends to be possible to control the viscosity of the second part while controlling its reactivity with the first part. In particular, when the second part contains hydrosilyl-modified organopolysiloxane E22, it tends to form a network structure when reacted with the vinyl-modified organopolysiloxane in the first part and the vinyl-modified organopolysiloxane in the second part, and to obtain a cured product with superior mechanical strength, such as shear displacement and elongation at break.

[0137] The average number of hydrosilyl groups per molecule of the hydrosilyl-modified organopolysiloxane may be measured by NMR. Specifically, for example, measurement may be performed using an ECP-300NMR manufactured by JEOL, with the hydrosilyl-modified organopolysiloxane dissolved in deuterated chloroform as a heavy solvent. The average number of hydrosilyl groups per molecule can be calculated by dividing the measurement result thus obtained by the average molecular weight of the hydrosilyl-modified organopolysiloxane.

[0138] The viscosity of the hydrosilyl-modified organopolysiloxane E21 at 25°C is preferably 5 to 100 mPa·s, 10 to 80 mPa·s, or 15 to 50 mPa·s. When the viscosity of the hydrosilyl-modified organopolysiloxane E21 is 100 mPa·s or less, the viscosity characteristics of the second part tend to be within a more appropriate range. When the viscosity of the hydrosilyl-modified organopolysiloxane E21 is 5 mPa·s or more, the mechanical strength of the cured product, such as the shear displacement and elongation at break, described below, tends to be further improved.

[0139] The viscosity of the hydrosilyl-modified organopolysiloxane E22 at 25°C is preferably 1 to 100 mPa·s, 2 to 90 mPa·s, or 3 to 80 mPa·s. When the viscosity of the hydrosilyl-modified organopolysiloxane E22 is 100 mPa·s or less, the viscosity characteristics of the second part tend to be within a more appropriate range. When the viscosity of the hydrosilyl-modified organopolysiloxane E22 is 1 mPa·s or more, the mechanical strength of the cured product, such as the shear displacement and elongation at break, described below, tends to be further improved. The viscosity of the hydrosilyl-modified organopolysiloxane E22 at 25°C may be 50 mPa·s or less, or 20 mPa·s or less, within the above range. Alternatively, in another embodiment, the viscosity of the hydrosilyl-modified organopolysiloxane E22 at 25°C may be 60 to 80 mPa·s, within the above range.

[0140] In the second agent, the content of the hydrosilyl-modified organopolysiloxane is preferably 60 to 95 parts by mass, 65 to 93 parts by mass, 70 to 90 parts by mass, or 75 to 88 parts by mass, per 100 parts by mass of the total of the organopolysiloxanes. When the content of the hydrosilyl-modified organopolysiloxane is within the above range, the curing rate when the first agent and the second agent are mixed tends to be within a more suitable range.

[0141] 1.6.2.2. Curing Inhibitor The second component of this embodiment preferably further contains a curing inhibitor. The curing inhibitor is an additive that is optionally added to control the reaction between the hydrosilyl group and the vinylsilyl group. In this embodiment, it is preferable that the first component contains an addition reaction catalyst, and the second component contains a curing inhibitor. The curing inhibitor is not particularly limited as long as it is a component that inhibits the reaction when the first component and the second component are mixed. Examples of the curing inhibitor include alkenyl alcohols, and 1-ethynyl-1-cyclohexanol is particularly preferred. The use of such a curing inhibitor can keep the curing rate when the first component and the second component are mixed within a suitable range, which tends to further improve the drip resistance of the two-component curing thermally conductive and heat-dissipating composition.

[0142] When the second part contains a cure inhibitor, the content of the cure inhibitor is preferably 0.1 to 20.0 parts by mass, and more preferably 0.5 to 10.0 parts by mass, per 100 parts by mass of the organopolysiloxane. By having the content of the cure inhibitor within this range, the curing rate when the first part and the second part are mixed can be set within a suitable range, and the dripping resistance of the two-component curing thermally conductive and heat-dissipating composition tends to be further improved.

[0143] The second agent of the present embodiment is a compound represented by the following formula: 1 a R 2 b Si(OR 3 ) 4-(a+b) (R 1 are each independently an alkyl group having 1 to 15 carbon atoms, and R 2 are each independently a saturated or unsaturated monovalent hydrocarbon group having 1 to 8 carbon atoms, and R 3 are each independently an alkyl group having 1 to 6 carbon atoms, a is 1 to 3, b is 0 to 2, and a+b is 1 to 3.) By not including the organosilane, the viscosity characteristics of the second agent tend to be within a more appropriate range.

[0144] The specific aspects of the organosilane are the same as those of the organosilanes that are preferably not contained in the first agent, and the content of the organosilane in the second agent is also the same as that in the first agent.

[0145] 1.6.2.3. Viscosity of the second part at 25°C and a shear rate of 10 s -1 The viscosity at 1000 rpm is preferably 50 to 160 Pa·s, 60 to 150 Pa·s, or 70 to 140 Pa·s. When the viscosity is 50 Pa·s or more, the dripping resistance of the two-component curing thermally conductive and heat-dissipating composition tends to be further improved. When the viscosity is 160 Pa·s or less, the composition tends to be easier to handle and the coatability of the mixture obtained by mixing the first and second components tends to be further improved. Note that this viscosity is measured at a shear rate of 10 s -1 The definition of "stable" here is "a viscosity that is stable at a shear rate of 0.1 s -1This is the same as the definition of "stable" when saying that the viscosity is stabilized at η2 at

[0146] 1.6.3. Cured Product The cured product of this embodiment is obtained by mixing the first and second parts of the two-component curing thermally conductive and heat-dissipating composition described above. More specifically, the cured product (crosslinked cured product) is obtained by mixing the first and second parts together in a mixture obtained by mixing the first and second parts, through an addition reaction between the reactive organopolysiloxanes contained in the first and second parts. For example, when the first part contains a vinyl-modified organopolysiloxane as the reactive organopolysiloxane and the second part contains a vinyl-modified organopolysiloxane and a hydrosilyl-modified organopolysiloxane as the reactive organopolysiloxane, the cured product is obtained through an addition reaction between the vinyl groups of the vinyl-modified organopolysiloxane in the first part and the vinyl-modified organopolysiloxane in the second part and the hydrosilyl groups of the hydrosilyl-modified organopolysiloxane.

[0147] After mixing the first and second parts, the mixture can be molded into a desired shape before curing to obtain a cured product having a desired shape. In addition, since the cured product of this embodiment contains a thermally conductive filler, it can be suitably used as a thermally conductive heat dissipation material.

[0148] The first and second components are mixed using a mixer such as a roll mill, kneader, Banbury mixer, or line mixer. More specifically, examples include kneading methods using a universal mixer, hybrid mixer, Trimix (manufactured by Inoue Seisakusho), or static mixer. The preferred molding method is the doctor blade method, but extrusion, pressing, calendar roll, or other methods may also be used depending on the viscosity of the resin. The reaction conditions for the addition reaction are not particularly limited, but are typically carried out at room temperature (e.g., 25°C) to 150°C for 0.1 to 24 hours.

[0149] The mixing ratio of the first agent and the second agent can be set appropriately depending on the types of the first agent and the second agent used and the purpose of use, but for example, the volume ratio of first agent:second agent may be 1.5:1.0 to 1.0:1.5, or may be 1.0:1.0.

[0150] 1.7. Uses The thermally conductive, heat-dissipating composition of this embodiment can be suitably used as a thermally conductive, heat-dissipating material.

[0151] 2. Electronic Device The electronic device of this embodiment includes a heat generating element, a heat sink, and the thermally conductive, heat dissipating composition or a cured product thereof, with the thermally conductive, heat dissipating composition or the cured product thereof disposed between the heat generating element and the heat sink. In this electronic device, the heat generating element and the heat sink are thermally coupled via the thermally conductive, heat dissipating composition.

[0152] Here, the heat generating body is not particularly limited, but examples thereof include heat generating electronic components such as motors, battery packs, circuit boards used in on-board power supply systems, power transistors, microprocessors, etc. Among these, electronic components used in on-board power supply systems for vehicles are preferred. Furthermore, the heat sink is not particularly limited as long as it is a component configured for the purpose of heat dissipation or heat absorption.

[0153] The method for bonding a heat generating element and a heat sink via a thermally conductive, heat-dissipating composition is not particularly limited. For example, an electronic device may be obtained by bonding a heat generating element and a heat sink using a thermally conductive, heat-dissipating composition that has been preheated and cured or semi-cured; an electronic device may be obtained by bonding a heat generating element and a heat sink using a thermally conductive, heat-dissipating composition and then heating the heat generating element and the heat sink; or an electronic device may be obtained by bonding a heat generating element and a heat sink using a thermally conductive, heat-dissipating composition. The heating conditions are not particularly limited, and examples include conditions of 25°C to 200°C for 0.5 hours to 24 hours.

[0154] The present invention will be described in more detail below using examples and comparative examples. The present invention is not limited to the following examples. Unless otherwise specified, the experiments were carried out at room temperature (25°C) and 1 atmosphere.

[0155] 1. Synthesis of copolymer The raw materials are as follows: ((meth)acrylic monomer α having a carboxy group) - acrylic acid, manufactured by Toagosei Co., Ltd. ((meth)acrylic monomer β having a tertiary amino group) - 1,2,2,6,6-pentamethyl-4-piperidyl methacrylate, "ADEKA STAB LA-82" manufactured by ADEKA Corporation ((meth)acrylic monomer γ having a siloxane skeleton) - α-butyl-ω-(3-methacryloxypropyl)polydimethylsiloxane, "Silaplane FM-0725" manufactured by JNC Corporation, number average molecular weight 10,000

[0156] The synthesis of copolymer αβγ-1 was carried out as follows. First, 1.5 parts by mass of acrylic acid, 0.5 parts by mass of 1,2,2,6,6-pentamethyl-4-piperidyl methacrylate, and 98 parts by mass of α-butyl-ω-(3-methacryloxypropyl)polydimethylsiloxane (γ-1) were added to an autoclave equipped with a stirrer. Next, 0.05 parts by mass of azobisisobutyronitrile (manufactured by Tokyo Chemical Industry Co., Ltd.) was added as an initiator relative to 100 parts by mass of the total (meth)acrylic monomers, and 1,000 parts by mass of a mixed solution of toluene (special reagent grade) and isopropyl alcohol (special reagent grade) in a volume ratio of 7:3 was added as a solvent, and the atmosphere inside the autoclave was replaced with nitrogen. Thereafter, the autoclave was heated in an oil bath at 65°C for 20 hours, and radical polymerization was carried out. After completion of polymerization, the mixture was degassed under reduced pressure at 120°C for 1 hour, yielding copolymer αβγ-1.

[0157] The polymerization rate relative to 100% of the charged amount of monomer was analyzed by gas chromatography and found to be 98% or more. From this, it was estimated that the ratio of each monomer unit contained in copolymer αβγ-1 was approximately the same as the charged ratio of the monomer.

[0158] The weight average molecular weight of the obtained copolymer αβγ-1 was determined as a weight average molecular weight converted to standard polystyrene using a GPC (gel permeation chromatography) method, and was found to be 65,000. The measurement conditions were as follows. High-speed GPC apparatus: "HLC-8020" manufactured by Tosoh Corporation Column: One "TSK guard column MP (xL)" manufactured by Tosoh Corporation, 6.0 mm ID x 4.0 cm, and two "TSK-GELMULTIPORE HXL-M" manufactured by Tosoh Corporation, 7.8 mm ID x 30.0 cm (theoretical plate number: 16,000), for a total of three (total theoretical plate number: 32,000) Developing solvent: tetrahydrofuran Detector: RI (differential refractometer)

[0159] 2. Preparation of First Agent First agents I-1 to I-8 were prepared by mixing the following components A1 to D1 and G1 according to the compounding ratios (parts by mass) shown in Table 1. Each component was mixed using a hybrid mixer ARE-310 (trade name, manufactured by Thinky Corporation). Note that blank spaces in Table 1 indicate that the corresponding compound was not used.

[0160] [Surfactant A1] Copolymer αβγ-1 obtained by the above synthesis method [Vinyl-modified organopolysiloxane B1] RH-Vi100E (trade name, manufactured by Runhe Chemical Industry Co., Ltd.), vinyl-modified organopolysiloxane, viscosity at 25°C: 105 mPa·s, average number of vinyl groups per molecule: 2, linear structure, vinyl group bonding position: both terminals [Thermal conductive filler C1] C1-1: DAW45S (trade name, manufactured by Denka Co., Ltd.), spherical alumina, average particle size: 45 μm, thermal conductivity: 35 W / m·K C1-2: DAW05 (trade name, manufactured by Denka Co., Ltd.), spherical alumina, average particle size: 5 μm, thermal conductivity: 35 W / m·K C1-3: ASFP40 (trade name, manufactured by Denka Company Limited), ultrafine alumina, average particle size: 0.4 μm, thermal conductivity 35 W / m K [Addition reaction catalyst D1] Platinum complex polymethylvinylsiloxane solution (trade name: Silicolyse Catalyst 12070, manufactured by Blue Star Silicone Co., Ltd.) [Si-containing powder G1] G1-1: FB-20D (trade name, manufactured by Denka Company Limited), specific surface area 1.0 m 2 / g, particle size (D50) 22000 nm, surface untreated. G1-2: FB-5D (trade name, manufactured by Denka Co., Ltd.), specific surface area 2.4 m 2 / g, particle size (D50) 5000 nm, surface untreated. G1-3: Aerosil 50 (trade name, manufactured by Nippon Aerosil Co., Ltd.), specific surface area 35 to 65 m 2 / g, particle size (D50) 30 nm, surface untreated. G1-4: Aerosil 200 (trade name, manufactured by Nippon Aerosil Co., Ltd.), specific surface area 175 to 225 m 2 / g, particle size (D50) 12 nm, surface untreated. G1-5: Aerosil 300 (trade name, manufactured by Nippon Aerosil Co., Ltd.), specific surface area 270 to 330 m 2 / g, particle size (D50) 7 nm, surface untreated. G1-6: Aerosil R974 (trade name, manufactured by Nippon Aerosil Co., Ltd.), specific surface area 150 to 190 m 2 / g, particle size (D50) 12 nm, surface treatment with dimethylsilyl G1-7: Aerosil RY200 (trade name, manufactured by Nippon Aerosil Co., Ltd.), specific surface area 80 to 120 m 2 / g, particle size (D50) 12 nm, surface treatment with dimethylpolysiloxane

[0161]

[0162] 3. Preparation of Second Agent Components A2 to C2 and E2 to G2 shown below were mixed according to the blending ratios (parts by mass) shown in Table 2 to prepare second agents II-1 to II-8. Each component was mixed using a hybrid mixer ARE-310 (trade name, manufactured by Thinky Corporation). Note that blank spaces in Table 2 indicate that the compound was not used.

[0163] [Surfactant A2] - Copolymer αβγ-1 obtained by the above synthesis method [Vinyl-modified organopolysiloxane B2] - RH-Vi100E (trade name, manufactured by Runhe Chemical Industry Co., Ltd.), vinyl-modified organopolysiloxane, viscosity at 25°C: 105 mPa·s, average number of vinyl groups per molecule: 2, linear structure, vinyl group bonding position: both terminals [Thermal conductive filler C2] - C2-1: DAW45S (trade name, manufactured by Denka Co., Ltd.), spherical alumina, average particle size: 45 μm, thermal conductivity: 35 W / m·K - C2-2: DAW05 (trade name, manufactured by Denka Co., Ltd.), spherical alumina, average particle size: 5 μm, thermal conductivity: 35 W / m·K C2-3: ASFP40 (trade name, manufactured by Denka Company Limited), ultrafine alumina, average particle size: 0.4 μm, thermal conductivity: 35 W / m·K [hydrosilyl-modified organopolysiloxane E2] E2-1: RH-H33 (trade name, manufactured by Runhe Chemical Industry Co., Ltd.), hydrosilyl-modified organopolysiloxane, viscosity at 25°C: 65 mPa·s, average number of hydrosilyl groups per molecule: 3 or more, linear structure, hydrosilyl group bonding position: side chain E2-2: RH-DH04 (trade name, manufactured by Runhe Chemical Industry Co., Ltd.), hydrosilyl-modified organopolysiloxane, viscosity at 25°C: 65 mPa·s, average number of hydrosilyl groups per molecule: 3 or more, linear structure, hydrosilyl group bonding position: side chain [Curing inhibitor F2] PA90 (manufactured by Elkem, trade name), a mixture of 1-ethynyl-1-cyclohexanol, polyorganosiloxane, and filler. [Si-containing powder G2] G2-1: FB-20D (manufactured by Denka, trade name), specific surface area 1.0 m. 2 / g, particle size (D50) 22000 nm, surface untreated. G2-2: FB-5D (trade name, manufactured by Denka Co., Ltd.), specific surface area 2.4 m 2 / g, particle size (D50) 5000 nm, surface untreated. G2-3: Aerosil 50 (trade name, manufactured by Nippon Aerosil Co., Ltd.), specific surface area 35 to 65 m 2 / g, particle size (D50) 30 nm, surface untreated. G2-4: Aerosil 200 (trade name, manufactured by Nippon Aerosil Co., Ltd.), specific surface area 175 to 225 m 2 / g, particle size (D50) 12 nm, surface untreated. G2-5: Aerosil 300 (trade name, manufactured by Nippon Aerosil Co., Ltd.), specific surface area 270 to 330 m 2 / g, particle size (D50) 7 nm, surface untreated. G2-6: Aerosil R974 (trade name, manufactured by Nippon Aerosil Co., Ltd.), specific surface area 150 to 190 m 2 / g, particle size (D50) 12 nm, surface dimethylsilyl treatment G2-7: Aerosil RY200 (trade name, manufactured by Nippon Aerosil Co., Ltd.), specific surface area 80 to 120 m 2 / g, particle size (D50) 12 nm, surface treated with dimethylpolysiloxane

[0164]

[0165] 4. Properties of the first and second agents (viscosity) First and second agents at 25°C and a shear rate of 10 s -1 The viscosity at 1000 kJ / s was measured using a rotational rheometer "HANKE MARS III" manufactured by Thermo Fisher Scientific. Specifically, parallel plates with a diameter of 35 mm were used, with a gap of 0.5 mm, a temperature of 25°C, and a shear rate of 10 s -1 The results are shown in Table 3. The viscosity was measured at a shear rate of 10 s -1 The definition of "stable" here is "a viscosity that is stable at a shear rate of 0.1 s -1 This is the same as the definition of "stable" when saying that the viscosity is stabilized at η2 at

[0166] 5. Evaluation 5.1. Thermal Conductivity Thermal conductivity was measured using a resin material thermal resistance measuring device (manufactured by Hitachi Technology Co., Ltd.) according to a method in accordance with ASTM D5470. Specifically, the first and second components were mixed in a static mixer at a volume ratio of 1:1, and the resulting mixture was sandwiched between copper jigs with thicknesses of 0.2 mm, 0.5 mm, and 1.0 mm and an area of ​​10 mm x 10 mm, and the thermal resistance value for each thickness was measured. The thermal conductivity of the thermally conductive resin composition was calculated from the slope L of the line obtained by plotting the thermal resistance value (°C / W) on the vertical axis and the thickness (mm) of the thermally conductive resin composition on the horizontal axis using the following formula: Thermal conductivity (W / mK) = 10 / L

[0167] 5.2 Time t and Viscosity Change Rate The viscosity change rate was measured using a rotational rheometer "HANKE MARS III" manufactured by Thermo Fisher Scientific. Specifically, the first and second components were mixed in a static mixer at a volume ratio of 1:1, and the resulting mixture was then passed through parallel plates with a diameter of 35 mm, with a gap of 0.5 mm, a temperature of 25°C, and a shear rate of 0.1 s. -1 The viscosity was measured for 100 seconds under the condition of -1 The measurement was carried out under the condition of a shear rate of 0.1 s -1 and shear rate 10 s -1 The viscosity measurement was repeated three times, and the third time was at a shear rate of 0.1 s -1 Viscosity η at a certain point p measured p and viscosity η 1 second after a certain point p p+1 The difference between p ) becomes 0.0 Pa s or more and less than 0.5 Pa s for the first time, -1 From 0.1 seconds -1 The time t elapsed from the time of the second change to time p was measured. The viscosity change rate was calculated as ([viscosity η at time p] p ]−[Shear rate 10 s -1 From 0.1 seconds -1 The shear rate 10 s immediately before the second change to -1 The viscosity was calculated by the following formula: [viscosity at 1000 kJ / t] / t.

[0168]

[0169] The thermally conductive, heat-dissipating resin composition of the present invention has industrial applicability as a heat-dissipating grease, a cured product, or the like for thermally connecting a heat generating element and a heat sink in an electronic device.

Claims

1. A matrix component and a thermally conductive filler are included, and the shear rate is 10 s during viscosity measurement at 25 °C. -1 From 0.1 s -1 When the shear rate was changed to 10 s -1 The viscosity η1 at a shear rate of 0.1 s -1 The thermally conductive, heat dissipating composition has a time t until the viscosity η2 at the temperature reaches a stable value of 30 seconds or less.

2. The thermally conductive, heat-dissipating composition according to claim 1, which is a one-component or two-component curing type.

3. The thermally conductive, heat dissipating composition according to claim 1, comprising a Si-containing powder.

4. The thermally conductive heat dissipating composition according to claim 3, wherein the surface of the Si-containing powder is hydrophilic.

5. The thermally conductive heat dissipating composition according to claim 3, wherein the Si-containing powder has a median diameter (D50) of 5 to 6000 nm.

6. The thermally conductive heat dissipating composition according to claim 3, wherein the content of said Si-containing powder is 0.01 to 1.00 parts by mass per 100 parts by mass of the content of said thermally conductive filler.

7. The thermally conductive, heat dissipating composition of claim 1, wherein the matrix component comprises a surfactant.

8. The thermally conductive heat dissipating composition according to claim 7, wherein the surfactant comprises a copolymer having (meth)acrylic monomer units α having a carboxy group, (meth)acrylic monomer units β having a tertiary amino group, and (meth)acrylic monomer units γ having a siloxane skeleton.

9. The thermally conductive, heat dissipating composition according to claim 1, wherein the matrix component comprises an organopolysiloxane.

10. The thermally conductive, heat dissipating composition according to claim 1, having a thermal conductivity of 4.0 W / m·K or more.

11. An electronic device comprising: an electronic component; the thermally conductive, heat dissipating composition according to any one of claims 1 to 10; and a heat sink, wherein the electronic component and the heat sink are in contact with each other via the thermally conductive, heat dissipating composition.

Citation Information

Patent Citations

  • Two-pack curable composition set, thermally conductive cured product, and electronic device

    WO2020080256A1

  • Copolymer, dispersant and resin composition

    WO2020209263A1

  • Inorganic oxide powder, resin composition, and compression molded product

    WO2022202592A1

  • Copolymer, surfactant, resin composition, and heat dissipation sheet

    WO2023090239A1