Slurry for forming positive electrode of non-aqueous electrolyte secondary battery, positive electrode sheet, and non-aqueous electrolyte secondary battery

The use of a slurry with a specific particle size distribution in the positive electrode active material layer addresses shape stability and capacity issues in nonaqueous electrolyte secondary batteries, enhancing the formation and performance of the battery.

WO2024247852A1PCT designated stage expired Publication Date: 2024-12-05FUJIFILM CORP
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/018888
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-31
Filing Date
2024-05-22
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Nonaqueous electrolyte secondary batteries face challenges in forming a positive electrode active material layer with desired shape stability, especially when thick layers are applied, leading to potential collapse and reduced battery capacity.

Method used

A slurry for forming positive electrodes with a specific particle size distribution, comprising a large particle group A with a particle size of 5.0 μm or more and a small particle group B with a particle size less than 5.0 μm, where the frequency of large particles is 60% or more and small particles is 40% or less, and the liquid absorption amount of the dispersion medium satisfies certain formulas, enhancing shape stability and capacity.

Benefits of technology

The proposed slurry effectively prevents collapse of the positive electrode active material layer, ensuring excellent shape stability and increased battery capacity in nonaqueous electrolyte secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024018888_05122024_PF_FP_ABST
    Figure JP2024018888_05122024_PF_FP_ABST
Patent Text Reader

Abstract

Provided are a slurry for forming a positive electrode, a positive electrode sheet having a positive electrode active material layer that is formed using the slurry for forming the positive electrode, and a non-aqueous electrolyte secondary battery in which the positive electrode sheet is incorporated in a positive electrode, the slurry for forming the positive electrode comprising a positive electrode active material, an electrolyte, and a dispersion medium, the positive electrode active material including a large particle group A having a particle diameter of 5.0 μm or more and a small particle group B having a particle diameter of less than 5.0 μm, the frequency of the large particle group A being 60% or more and the frequency of the small particle group B being 40% or less when the total frequency in the number-based particle size distribution of the positive electrode active material is 100%, and the liquid absorption amount ηB (g / 100g) of the dispersion medium per 100 g of the small particle group B satisfying the relationship formula B1: 15≤ΗB≤30.
Need to check novelty before this filing date? Find Prior Art

Description

Slurry for forming positive electrode of non-aqueous electrolyte secondary battery, positive electrode sheet, and non-aqueous electrolyte secondary battery

[0001] The present invention relates to a slurry for forming a positive electrode of a nonaqueous electrolyte secondary battery, a positive electrode sheet, and a nonaqueous electrolyte secondary battery.

[0002] Non-aqueous electrolyte secondary batteries, typified by lithium-ion secondary batteries, have high energy density and excellent storage performance, low-temperature operation, etc., and are widely used in portable electronic devices such as mobile phones and laptop computers. Furthermore, larger batteries are being used in transportation equipment such as automobiles, and their use as storage devices for nighttime electricity and electricity generated by natural energy sources is also progressing.

[0003] Techniques for increasing the capacity of non-aqueous electrolyte secondary batteries have been studied. For example, Patent Document 1 discloses a technique for making an electrode active material layer function as a secondary battery in the form of a slurry containing a high amount of active material. Specifically, the document describes an electrochemical cell including: a positive electrode made of a non-binding material containing a first active material and an electrolyte solution in a first non-aqueous liquid electrolyte; a negative electrode made of a non-binding material containing a second active material and an electrolyte solution in a second non-aqueous liquid electrolyte; and an ion-permeable membrane disposed between the positive electrode and the negative electrode, wherein the positive electrode and the negative electrode each have a thickness of about 200 μm to about 3000 μm. According to the technology described in Patent Document 1, as in the above-mentioned positive and negative electrodes, the electrode active material layers (positive electrode active material layer and negative electrode active material layer) contain an electrolyte and are in a slurry state and unbound, so that the electrode active material layer can be made into a thick film while maintaining its flexibility, and no binder is required to bind the solid particles together, making it possible to significantly increase the overall charge capacity and energy density while maintaining the flexibility of the battery. A nonaqueous electrolyte secondary battery in which the electrode active material layer is formed in a slurry state containing an electrolytic solution (electrolyte), as described in Patent Document 1, may be referred to as a quasi-solid secondary battery in the following description.

[0004] Regarding the improvement of the performance of non-aqueous electrolyte secondary batteries, studies have focused on the positive electrode active material layer. For example, Patent Document 2 discloses a method for manufacturing an electrode for a lithium ion secondary battery, which includes: preparing first composite particles containing a first active material and a first binder; and second composite particles having higher fluidity than the first composite particles and containing a second active material and a second binder; providing a strip-shaped current collector on at least one longitudinal end of an elongated current collector, and supplying the first composite particles to a first portion, which is a strip-shaped region adjacent to the current collector; supplying the second composite particles to a second portion, which is a region closer to the center of the current collector in a width direction perpendicular to the longitudinal direction than the first portion; and rolling the first and second composite particles supplied onto the current collector to form an active material layer. In the examples, the method evaluates a positive electrode sheet having a positive electrode active material layer formed by the above manufacturing method. The technology of Patent Document 2 is said to enable the manufacture of an electrode while suppressing peeling or sliding of the active material layer.

[0005] Patent Document 3 discloses a nonaqueous electrolyte storage element including a positive electrode having a conductive substrate and a positive electrode composite layer laminated on the substrate, wherein the substrate is formed from an aluminum alloy containing 1% by mass or more of elements other than aluminum, the positive electrode composite layer contains particles A and B having different particle sizes as a positive electrode active material, the particle size ratio (A / B) of the particle A to the particle B is 3 or more, and the substrate has a tensile break strength of 250 MPa or more. The technology in Patent Document 3 is said to be able to suppress an increase in resistance due to repeated charging and discharging.

[0006] Patent Document 4 discloses a cathode active material containing first lithium composite oxide particles having a layered structure and second lithium composite oxide particles having a layered structure, wherein the first lithium composite oxide particles have an average particle size (D50) of 3.0 μm to 6.0 μm, the first lithium composite oxide particles have a dibutyl phthalate oil absorption of 15 mL / 100 g to 27 mL / 100 g, the second lithium composite oxide particles have an average particle size (D50) of 10.0 μm to 22.0 μm, and the second lithium composite oxide particles have a dibutyl phthalate oil absorption of 14 mL / 100 g to 22 mL / 100 g. The technology in Patent Document 4 is said to be able to increase the capacity of a non-aqueous electrolyte secondary battery and provide resistance to capacity decline during repeated charge and discharge.

[0007] Patent Document 5 also describes a battery including at least a positive electrode, a negative electrode, and an electrolyte, the positive electrode including at least a first positive electrode active material and a second positive electrode active material, the first positive electrode active material being represented by the formula (I): LiNi a Co b Mn c O 2 ...(I), and the second positive electrode active material is represented by the formula (II): LiNi d Co e Mn f O 2 ...(II), wherein in the formulas (I) and (II), a, b, c, d, e, and f satisfy the following: a>d, 0.4≦a≦0.6, 0.2≦b≦0.5, 0.1≦c≦0.2, a+b+c=1, 0.2≦d≦0.5, 0.1≦e≦0.2, 0.4≦f≦0.6, d+e+f=1. The lithium ion secondary battery is disclosed, wherein the electrolyte contains an electrolytic solution, the first positive electrode active material has a first oil absorption, and the second positive electrode active material has a second oil absorption, the second oil absorption being greater than the first oil absorption. The technology in Patent Document 5 is said to be able to improve cryogenic output.

[0008] JP 2017-147222 A JP 2015-230748 A WO 2018 / 155314 JP 2023-34700 A JP 2019-29212 A

[0009] In recent years, as the applications of non-aqueous electrolyte secondary batteries have expanded, there has been a demand for non-aqueous electrolyte secondary batteries with higher energy densities (higher capacities). For example, non-aqueous electrolyte secondary batteries are used as power sources for electric vehicles (EVs) and drones. Increasing the capacity of non-aqueous electrolyte secondary batteries is important for improving the driving range of EVs and the flight time of drones. To increase the capacity (energy density) of quasi-solid-state secondary batteries, attempts have been made to increase the content of ion-storing positive electrode active material in a slurry-like positive electrode active material layer. However, because the positive electrode active material layer of a quasi-solid-state battery does not use a binder, forming a thick positive electrode active material layer by thickly applying a positive electrode-forming slurry can result in partial collapse of the edges of the formed positive electrode active material layer during the manufacturing process of the non-aqueous electrolyte secondary battery, making it difficult to form a positive electrode active material layer with a desired shape (e.g., a rectangular cross section).

[0010] The present invention relates to a quasi-solid secondary battery, and its objective is to provide a positive electrode-forming slurry that has excellent formability (shape stability) of a positive electrode active material layer and can provide a nonaqueous electrolyte secondary battery that exhibits excellent battery performance. Another objective of the present invention is to provide a positive electrode sheet having a positive electrode active material layer formed using the positive electrode-forming slurry, and a nonaqueous electrolyte secondary battery in which the positive electrode sheet is incorporated into a positive electrode.

[0011] In view of the above problems, the present inventors have conducted extensive research and have found that, when a cathode active material having a specific particle size distribution is used as the cathode active material contained in a cathode-forming slurry for forming a cathode active material layer of a quasi-solid secondary battery, and when the liquid absorption capacity of a specific small particle cathode active material is increased within a specific range, even when a thick cathode active material layer is formed, collapse of the resulting cathode active material layer is suppressed, allowing a cathode active material layer of a desired shape to be efficiently formed, and furthermore, a higher capacity can be achieved for the resulting nonaqueous electrolyte secondary battery. The present invention was completed through further research based on this finding.

[0012] The above-described problems of the present invention have been solved by the following means: [1] A slurry for forming a positive electrode of a nonaqueous electrolyte secondary battery, comprising a positive electrode active material, an electrolyte, and a dispersion medium, wherein the positive electrode active material is composed of a large particle group A having a particle size of 5.0 μm or more and a small particle group B having a particle size of less than 5.0 μm, wherein, when the total frequency in a number-based particle size distribution of the positive electrode active material is taken as 100%, the frequency of the large particle group A is 60% or more and the frequency of the small particle group B is 40% or less, and the amount of liquid absorption of the dispersion medium by the small particle group B per 100 g, ηB (g / 100 g), satisfies the following formula B1: Formula B1: 15≦ηB≦30 [2] The slurry for forming a positive electrode according to [1], wherein the amount of liquid absorption of the dispersion medium by the large particle group A per 100 g, ηA (g / 100 g), satisfies the following formula A1: Formula A1: 2≦ηA≦25 [3] The slurry for forming a positive electrode according to [1] or [2], wherein the liquid absorption amount ηA satisfies the following formula A2: Formula A2: 2≦ηA≦7 [4] The slurry for forming a positive electrode according to any one of [1] to [3], wherein the liquid absorption amount ηB satisfies the following formula B2: Formula B2: 18≦ηB≦25 [5] The slurry for forming a positive electrode according to any one of [1] to [4], wherein the closest packing ratio calculated from the volume-based cumulative particle size distribution of the positive electrode active material is 80% or more. [6] A positive electrode sheet having a positive electrode active material layer formed using the positive electrode forming slurry according to any one of [1] to [5]. [7] A nonaqueous electrolyte secondary battery having the positive electrode sheet according to [6] as a positive electrode.

[0013] In the description of the present invention, a numerical range expressed using "to" means a range including the numerical values ​​written before and after "to" as the lower and upper limits. In the present invention, "non-aqueous electrolyte" means an electrolyte that does not substantially contain water. In other words, the "non-aqueous electrolyte" may contain a small amount of water within a range that does not impair the effects of the present invention. In the present invention, the "non-aqueous electrolyte" has a water concentration of 200 ppm (by mass) or less, preferably 100 ppm or less, and more preferably 20 ppm or less. Note that it is practically difficult to make a non-aqueous electrolyte completely anhydrous, and it usually contains 1 ppm or more of water. In the present invention, "non-aqueous solvent" also means a solvent that does not substantially contain water. In other words, the "non-aqueous solvent" may contain a small amount of water within a range that does not impair the effects of the present invention. In the present invention, the "non-aqueous solvent" has a water concentration of 200 ppm (by mass) or less, preferably 100 ppm or less, and more preferably 20 ppm or less. In reality, it is difficult to make a non-aqueous solvent completely free of water, and it usually contains 1 ppm or more of water.

[0014] The positive electrode active material layer formed using the positive electrode-forming slurry for nonaqueous electrolyte secondary batteries of the present invention can be made to be less susceptible to collapse. The positive electrode sheet of the present invention has excellent shape stability of the positive electrode active material layer, and by incorporating this as the positive electrode of a nonaqueous electrolyte secondary battery, a nonaqueous electrolyte secondary battery exhibiting excellent battery performance can be obtained. The nonaqueous electrolyte secondary battery of the present invention has excellent shape stability of the positive electrode active material layer and also has excellent battery performance.

[0015] FIG. 1 is a longitudinal sectional view showing a schematic diagram of a basic layer structure of an embodiment of a secondary battery according to the present invention.

[0016] Although preferred embodiments of the present invention will be described, the present invention is not limited to these embodiments except as defined in the present invention.

[0017] [Slurry for Forming Positive Electrode] The slurry for forming a positive electrode of a nonaqueous electrolyte secondary battery of the present invention (also referred to as "positive electrode slurry of the present invention") is a slurry (suspension, dispersion) containing a positive electrode active material, an electrolyte, and a dispersion medium, and is suitable for forming a positive electrode active material layer of a nonaqueous electrolyte secondary battery. In the positive electrode slurry of the present invention, the positive electrode active material comprises a large particle group A having a particle size of 5.0 μm or more and a small particle group B having a particle size of less than 5.0 μm, and when the total frequency in the number-based particle size distribution of the positive electrode active material is taken as 100%, the frequency of the large particle group A is 60% or more and the frequency of the small particle group B is 40% or less, and the amount of absorption of the dispersion medium by the small particle group B per 100 g, ηB (g / 100 g), satisfies the following formula B1. Formula B1: 15≦ηB≦30

[0018] In the positive electrode slurry of the present invention, the positive electrode active material is composed of large particle groups A and small particle groups B, and the amount of dispersion medium absorbed by the small particle groups B is controlled within the above range. It is believed that the small particle groups B, which retain a relatively large amount of dispersion medium, are present in the gaps between the large particle groups A and act as a binder, thereby effectively enhancing the interaction (adhesion) between the solid particles. As a result, even if the formed positive electrode active material layer has a thickness of about 350 μm, the formed positive electrode active material layer has excellent shape stability and can be thought of as being able to sufficiently increase the battery capacity of the resulting nonaqueous electrolyte secondary battery.

[0019] The positive electrode active material constituting the positive electrode slurry of the present invention is composed of a large particle group A having a particle size of 5.0 μm or more and a small particle group B having a particle size of less than 5.0 μm. That is, the positive electrode active material used in the present invention is roughly divided into a large particle group having a particle size including the threshold particle size of 5.0 μm and a particle group having a particle size smaller than this threshold particle size. The particle size can be measured using a particle size measuring device in accordance with the method for measuring number-based particle size distribution described below.

[0020] When the total frequency (total particle number of positive electrode active material particles) in the number-based particle size distribution of the positive electrode active material is taken as 100%, the frequency of large particle group A (the number of particles of positive electrode active material classified as large particle group A) is preferably 60 to 90%, more preferably 60 to 80%, and even more preferably 65 to 75%. When the total frequency (total particle number of positive electrode active material particles) in the number-based particle size distribution of the positive electrode active material is taken as 100%, the frequency of small particle group B (the number of particles of positive electrode active material classified as small particle group B) is preferably 10 to 40%, more preferably 20 to 40%, and even more preferably 25 to 35%. The method for controlling the frequency of large particle group A and small particle group B in the positive electrode active material as described above is not particularly limited, and can be controlled, for example, by mixing and using positive electrode active materials with different median diameters. The number-based particle size distribution of the positive electrode active material can be obtained by the method described in the examples.

[0021] In the positive electrode slurry of the present invention, the amount of liquid absorption ηB (g / 100g) of the dispersion medium per 100g of the small particle group B satisfies the formula B1: 15≦ηB≦30. If the amount of liquid absorption ηB is too low, the interaction between the particles of the small particle group B cannot be increased to the desired level, and the formed positive electrode active material layer is prone to collapse. On the other hand, if the amount of liquid absorption ηB is too high, the formed positive electrode active material layer is likely to become nearly powdery and is also prone to collapse. Here, in the present invention, the "amount of liquid absorption ηB of the dispersion medium per 100g of the small particle group B" means the amount of dispersion medium that 100g of the small particle group B can retain in its structure. The amount of liquid absorption ηB of the dispersion medium per 100g of the small particle group B can be determined as follows in accordance with JIS K6217-4:2017. -Method for measuring liquid absorption- An oil absorption measuring device (S-500 (product name), manufactured by Asahi Research Institute) is used to measure the liquid absorption. 0.5 g of the dispersion medium constituting the positive electrode slurry is added dropwise to 100 g of powder of the positive electrode active material, and the torque is measured, and the amount of dispersion medium added (mL) at which the torque reaches a maximum (maximum) is determined. When the positive electrode slurry of the present invention contains a mixed dispersion medium composed of two or more dispersion mediums as the dispersion medium, the liquid absorption is measured using this mixed dispersion medium as the "dispersion medium constituting the positive electrode slurry."

[0022] With respect to formula B1, the positive electrode slurry of the present invention preferably satisfies the following formula B2, and more preferably satisfies formula B3: Formula B2: 18≦ηB≦25 Formula B3: 18≦ηB≦23

[0023] The amount of liquid absorption of the small particle group B into the dispersion medium constituting the positive electrode slurry can be controlled by previously surface-smoothing at least the positive electrode active material classified as small particle group B and incorporating this into the positive electrode slurry. Examples of this surface-smoothing treatment include mixing. The atmosphere during the surface-smoothing treatment is not particularly limited, and from the perspective of preventing oxidation of the active material particle surface during treatment, it is preferable to carry out the surface-smoothing treatment in an inert gas atmosphere. For example, mixing can be carried out in an argon atmosphere, a nitrogen atmosphere, a nitrogen-hydrogen mixed atmosphere, or the like. The treatment device used in the surface-smoothing treatment is not particularly limited, and examples thereof include a planetary ball mill (trade name: P-5, manufactured by Fritsch), a jet mill pulverizer (trade name: JETMILL100, manufactured by Powrex Corporation), a powder treatment device Nobilta (trade name: NOB MINI, manufactured by Hosokawa Micron Corporation), and a powder treatment device Composite (trade name: CP15, manufactured by Nippon Coke and Engineering Co., Ltd.). The treatment conditions for the surface smoothing treatment are not particularly limited, and for example, mixing can be performed using a powder processing device Nobilta (trade name: NOB MINI, manufactured by Hosokawa Micron Corporation) in a nitrogen atmosphere at a rotation speed of 5,000 to 9,000 rpm for a treatment time of 5 to 20 minutes. As a result of the surface smoothing treatment, the liquid absorption amount ηB decreases.

[0024] In the positive electrode slurry of the present invention, the liquid absorption amount ηA (g / 100g) of the dispersion medium per 100g of the large particle group A can be expressed by the following formula A0, and preferably satisfies formula A1, and more preferably satisfies formula A2. A smaller liquid absorption amount ηA tends to have better shape stability. Formula A0: 2≦ηA≦30 Formula A1: 2≦ηA≦25 Formula A2: 2≦ηA≦7 The liquid absorption amount ηA can be measured in the same manner as the liquid absorption amount ηB. As with the small particle group B, the liquid absorption amount ηA of the dispersion medium of the large particle group A can be controlled to the above range by subjecting the large particle group A to a surface smoothing treatment. The surface smoothing treatment is the same as that described for the small particle group B. The liquid absorption amount ηA of the dispersion medium of the large particle group A can be calculated in the same manner as the liquid absorption amount ηB of the dispersion medium of the small particle group B.

[0025] The absolute value of the difference in liquid absorption amount (|ηB-ηA|) (g / 100 g) between the liquid absorption amount ηA of the dispersion medium of the large particle group A and the liquid absorption amount ηB of the dispersion medium of the small particle group B preferably satisfies the following formula C0, more preferably satisfies formula C1, and further preferably satisfies formula C2. Formula C0: 1≦|ηB-ηA|≦24 Formula C1: 1≦|ηB-ηA|≦21 Formula C2: 5≦|ηB-ηA|≦18

[0026] In the positive electrode slurry of the present invention, the close packing ratio of the positive electrode active material calculated from the volume-based cumulative particle size distribution of the positive electrode active material is preferably 75% or more, more preferably 80% or more. By controlling the particle size distribution of the positive electrode active material in this manner, the packing ratio of the positive electrode active material in the resulting positive electrode active material layer can be increased. This close packing ratio is an estimated value calculated based on data on the volume-based cumulative particle size distribution of the positive electrode active material contained in the positive electrode slurry of the present invention. Specifically, the close packing ratio can be calculated by the method described in the examples of the present invention.

[0027] The specific surface area of ​​the small particle group B is 8.0 to 13.0 m 2 / g, and 9.0 to 12.5 m 2 The specific surface area of ​​the large particle group A is preferably 5.0 to 8.5 m / g. 2 / g, and 5.2 to 8.3 m 2 / g is more preferable. The specific surface area of ​​each of the large particle group A and the small particle group B can be measured by the BET method as follows. -BET specific surface area measurement method- After drying 0.2 g of a sample at 120°C for 6 hours, measurement is performed using a BELSORP mini (trade name) manufactured by Microtrac under the following measurement conditions. Adsorption temperature: 77 K Adsorption gas: N 2 Equilibration time: 100 seconds Purge gas: He

[0028] As a method for producing the particle size distribution defined in the present invention, which is composed of large particle groups A and small particle groups B, a positive electrode active material having a large median diameter (D50) and a positive electrode active material having a small median diameter (D50) can be mixed and used as the positive electrode active material. The median diameter (D50) of the positive electrode active material having a large median diameter (D50) (positive electrode active material a, large particle group a) can be 6.0 to 20.0 μm, preferably 7.0 to 15.0 μm, more preferably 8.0 to 14.0 μm, and even more preferably 8.3 to 13.0 μm. The median diameter (D50) of the above-mentioned cathode active material (cathode active material b, small particle group b) having a small median diameter (D50) can be 0.1 to 4.0 μm, preferably 0.2 to 3.0 μm, more preferably 0.5 to 2.0 μm, and even more preferably 0.8 to 1.2 μm. To obtain the cathode active material a (large particle group a) and the cathode active material b (small particle group b) with a predetermined median diameter (D50), a conventional grinder or classifier can be used. The cathode active material obtained by the firing method may be used after washing with water, an acidic aqueous solution, an alkaline aqueous solution, or an organic solvent. The median diameter (D50) of the cathode active material a (large particle group a) and the cathode active material b (small particle group b) can be measured by the following method. -Method of measuring median diameter (D50)- The positive electrode active material is dispersed in water, and the particle diameter (volume-based median diameter D50 in water) obtained by measuring the particle diameter using a laser diffraction / scattering particle size distribution measuring device (for example, Particle LA-960V2 manufactured by HORIBA) is used. This also applies to the median diameter (D50) of solid particles other than the positive electrode active material.

[0029] The positive electrode slurry of the present invention may contain the same components as a typical positive electrode slurry, except that it contains a positive electrode active material composed of the large particle group A and the small particle group B, an electrolyte, and a dispersion medium. For example, it may contain a conductive additive, etc.

[0030] Each component constituting the positive electrode slurry of the present invention will be described in more detail below.

[0031] <Positive electrode active material> The positive electrode active material is preferably one that can reversibly insert and release lithium ions. There are no particular limitations on the material, and examples thereof include transition metal oxides, organic substances, sulfur, and other substances that can be composited with Li, as well as sulfur-metal composites. Among these, it is preferable to use lithium-containing transition metal oxides as the positive electrode active material, and transition metal element M a It is more preferable that the lithium-containing transition metal oxide contains at least one element selected from Co, Ni, Fe, Mn, Cu, and V. b (Elements of Group 1 (Ia) of the periodic table other than lithium, elements of Group 2 (IIa), Al, Ga, In, Ge, Sn, Pb, Sb, Bi, Si, P, B, etc.) may be mixed. The amount of the mixed element may be determined by the following formula: a The amount of Li / M is preferably 0 to 30 mol % relative to the amount of Li / M (100 mol %). a More preferably, the lithium-containing transition metal oxide is synthesized by mixing the above-mentioned components so that the molar ratio of the above-mentioned components is 0.3 to 2.2. Specific examples of the lithium-containing transition metal oxide include (MA) a lithium-containing transition metal oxide having a layered rock salt structure, (MB) a lithium-containing transition metal oxide having a spinel structure, (MC) a lithium-containing transition metal phosphate compound, (MD) a lithium-containing transition metal halide phosphate compound, and (ME) a ​​lithium-containing transition metal silicate compound.

[0032] (MA) Specific examples of lithium-containing transition metal oxides having a layered rock salt structure include LiCoO 2 (Lithium cobalt oxide [LCO]), LiNi 2 O 2 (lithium nickel oxide), LiNi 0.85 Co 0.10 Al 0.05O 2 (nickel cobalt lithium aluminum oxide [NCA]), LiNi 1/3 Co 1/3 Mn 1/3 O 2 (Lithium nickel manganese cobalt oxide [NMC]) and LiNi 0.5 Mn 0.5 O 2 (Lithium manganese nickel oxide). (MB) Specific examples of lithium-containing transition metal oxides having a spinel structure include LiMn 2 O 4 (LMO), LiCoMnO 4 , Li 2 FeMn 3 O 8 , Li 2 CuMn 3 O 8 , Li 2 CrMn 3 O 8 and Li 2 NiMn 3 O 8 Examples of the (MC) lithium-containing transition metal phosphate compound include LiFePO 4 and Li 3 Fe 2 (P.O. 4 ) 3 Olivine-type iron phosphate salts such as LiFeP 2 O 7 Iron pyrophosphates such as LiCoPO 4 Cobalt phosphates such as Li 3 V 2 (P.O. 4 ) 3 (MD) Examples of lithium-containing transition metal halide phosphate compounds include, for example, Li 2 FePO 4 Fluorophosphate iron salts such as F, Li 2 MnPO 4 Fluorophosphate manganese salts such as F and Li 2 CoPO 4 Examples of the (ME) lithium-containing transition metal silicate compound include cobalt fluoride phosphates such as Li2 FeSiO 4 , Li 2 MnSiO 4 and Li 2 CoSiO 4 In the present invention, the positive electrode active material is preferably a lithium-containing transition metal oxide (MA) having a layered rock salt structure and a lithium-containing transition metal phosphate compound (MC), and LiNi 1/3 Co 1/3 Mn 1/3 O 2 and LiFePO 4 is more preferred, and LiFePO 4 is more preferred.

[0033] The chemical formula of the compound obtained by the above calcination method can be measured by inductively coupled plasma (ICP) emission spectroscopy, or simply calculated from the difference in mass of the powder before and after calcination.

[0034] The surface of the positive electrode active material may be coated with an oxide such as another metal oxide, a carbon-based material, or the like. These surface coating layers can function as an interface resistance stabilizing layer. Examples of surface coating materials include metal oxides containing Ti, Nb, Ta, W, Zr, Al, Si, or Li. Specific examples include titanate spinel, tantalum-based oxides, niobium-based oxides, and lithium niobate-based compounds, such as Li 4 Ti 5 O 12 , Li 2 Ti 2 O 5 , LiTaO 3 , LiNbO 3 , LiAlO 2 , Li 2 ZrO 3 , Li 2 WO 4 , Li 2 TiO 3 , Li 2 B 4 O 7 , Li 3 P.O. 4 , Li 2 MoO 4 , Li 3 BO 3 , LiBO2 , Li 2 CO 3 , Li 2 SiO 3 , SiO 2 , TiO 2 , ZrO 2 , Al 2 O 3 , B 2 O 3 , and Li 3 AlF 6 Carbon-based materials such as C, SiC, and SiOC (carbon-doped silicon oxide) can also be used as the surface coating material.

[0035] The positive electrode active material is preferably surface-coated with a carbonaceous material from the viewpoint of increasing the electronic conductivity to a desired level. In this case, the positive electrode active material is preferably surface-coated with carbon (C). The carbon surface coating can be formed by baking the positive electrode active material in the presence of an additive (organic substance) that serves as a carbon source. Examples of the additive that can be used include styrene-maleic anhydride copolymer, polystyrene, and polycarbonate.

[0036] The surface of the positive electrode active material may be treated with sulfur or phosphorus. Furthermore, the particle surfaces of the positive electrode active material may be treated with actinic rays or an active gas (plasma, etc.) before or after the surface coating.

[0037] The positive electrode active materials may be used alone or in combination of two or more.

[0038] The content of the positive electrode active material in the total content of the positive electrode active material and the conductive additive in the positive electrode slurry is preferably 96.00 to 99.97 mass%, more preferably 98.00 to 99.97 mass%, still more preferably 99.00 to 99.95 mass%, still more preferably 99.20 to 99.90 mass%, still more preferably 99.50 to 99.80 mass%, still more preferably 99.55 to 99.80 mass%, and still more preferably 99.60 to 99.80 mass%.

[0039] <Conductive Aid> The positive electrode slurry of the present invention may contain a conductive aid. As the conductive aid, any known conductive aid may be used. For example, the conductive aid may be an electron conductive material such as graphites (e.g., natural graphite, artificial graphite, etc.), carbon blacks (e.g., acetylene black, ketjen black, furnace black, etc.), amorphous carbon (e.g., needle coke), carbon fibers (e.g., vapor-grown carbon fibers or carbon nanotubes), carbonaceous materials (e.g., graphene or fullerene), metal powders (e.g., copper, nickel, etc.), or conductive polymers (e.g., polyaniline, polypyrrole, polythiophene, polyacetylene, polyphenylene derivatives). In the present invention, the conductive aid is preferably a carbonaceous material, more preferably carbon blacks, and more preferably ketjen black. When a positive electrode active material and a conductive aid are used in combination, the conductive aid is one of the above conductive aids that does not undergo Li insertion and release during charging and discharging of the battery and does not function as an active material. Therefore, among the conductive additives, those that can function as an active material in the active material layer when the battery is charged and discharged are classified as active materials rather than as conductive additives. Whether or not a conductive additive functions as an active material when the battery is charged and discharged is not uniquely determined, but is determined by the combination with the active material.

[0040] Examples of commercially available conductive additives include the following: Ketjen black: carbon ECP (specific surface area = 890 m 2 / g), carbon ECP600JD (specific surface area = 1480 m 2 / g), carbon ECP200L (specific surface area = 430 m 2 / g) (both manufactured by Lion Corporation), carbon black: LITX300 (specific surface area = 180 m 2 / g), LITX-HP (specific surface area = 100 m 2 / g) (both manufactured by CABOT Corporation) Carbon nanotubes (CNT): BT1001M (specific surface area = 272 m 2 / g), BT1003M (specific surface area = 230 m 2 / g) (both manufactured by LG), JENOTUBE6A (specific surface area = 680 m 2 / g), JENOTUBE10B (specific surface area = 230m2 / g) (both from JEIO)

[0041] The conductive additive may be used alone or in combination of two or more.

[0042] The shape of the conductive additive is not particularly limited, but is preferably particulate. The median diameter (D50) of the conductive additive is also not particularly limited. For example, it is preferably 0.01 to 50 μm, more preferably 0.1 to 10 μm, and even more preferably 0.2 to 2.0 μm.

[0043] The conductive additive may be surface-treated. The surface treatment method is not particularly limited, and preferred are surface treatment using a chemical treatment agent and atomic layer deposition (ALD) treatment. Preferred examples of the chemical treatment agent include organosilicon compounds (more preferably, silane coupling agents) and organic phosphonic acid compounds, such as methyltrimethoxysilane (MTMS), octadecyltrimethoxysilane, hexamethyldisilazane, tetraethoxysilane, trifluoropropyltrimethoxysilane, vinyltrimethoxysilane, phenyltrimethoxysilane, 3-aminopropyltriethoxysilane, 1H,1H,2H,2H-perfluorooctyltriethoxysilane, trimethoxy(octyl)silane, 1H,1H,2H,2H-perfluorooctanephosphonic acid, 1-octylphosphonic acid, and perfluoropolyethertriethoxysilane (KY1903 (trade name)). In the ALD process, the layer to be deposited is HfO 2 , SiO 2 , ZrO 2 , Ta 2 O 5 , TiO 2 The following can be mentioned:

[0044] The content of the conductive additive relative to the total content of the positive electrode active material and the conductive additive in the positive electrode slurry is preferably 0.03 to 4.00 mass%, more preferably 0.03 to 2.00 mass%, even more preferably 0.05 to 1.00 mass%, still more preferably 0.10 to 0.80 mass%, still more preferably 0.20 to 0.50 mass%, still more preferably 0.20 to 0.45 mass%, and still more preferably 0.20 to 0.40 mass%.

[0045] <Electrolyte> The electrolyte may be any electrolyte used in electrolytic solutions for quasi-solid secondary batteries. Metal salts are preferred, including lithium salts, potassium salts, sodium salts, calcium salts, and magnesium salts. The lithium salt is preferably a lithium salt commonly used in electrolytes for lithium ion secondary batteries, including, for example, the following lithium salts:

[0046] (L-1) Inorganic lithium salt: LiPF 6 , LiBF 4 , LiAsF 6 , LiSbF 6 Inorganic fluoride salts such as LiClO 4 , LiBrO 4 , LiIO 4 perhalogenates such as LiAlCl 4 Inorganic chloride salts, etc.

[0047] (L-2) Fluorine-containing organic lithium salt: LiCF 3 SO 3 perfluoroalkanesulfonates such as LiN(CF 3 SO 2 ) 2 , LiN(CF 3 CF 2 SO 2 ) 2 , LiN(FSO 2 ) 2 , LiN(CF 3 SO 2 ) (C 4 F 9 SO 2 perfluoroalkanesulfonylimide salts such as LiC(CF 3 SO 2 ) 3 perfluoroalkanesulfonylmethide salts such as Li[PF 5 (CF 2 CF 2 CF 3 ) )], Li[PF 4 (CF 2 CF 2 CF 3 ) 2 ], Li[PF 3 (CF 2 CF2 CF 3 ) 3 ], Li[PF 5 (CF 2 CF 2 CF 2 CF 3 ) )], Li[PF 4 (CF 2 CF 2 CF 2 CF 3 ) 2 ], Li[PF 3 (CF 2 CF 2 CF 2 CF 3 ) 3 perfluoroalkyl fluorophosphates such as

[0048] (L-3) Oxalatoborate salts: lithium bis(oxalato)borate, lithium difluorooxalatoborate, etc.

[0049] Among these, LiPF 6 , LiBF 4 , LiAsF 6 , LiSbF 6 , LiClO 4 , Li(R f1 SO 3 ), LiN(R f1 SO 2 ) 2 , LiN(FSO 2 ) 2 , or LiN(R f1 SO 2 ) (R f2 SO 2 ) is preferred, and LiPF 6 , LiBF 4 , LiN(R f1 SO 2 ) 2 , LiN(FSO 2 ) 2 , or LiN(R f1 SO 2 ) (R f2 SO 2 ) is more preferred, and LiPF 6 is particularly preferred. f1 and R f2Each of the groups represents a perfluoroalkyl group, and the number of carbon atoms is preferably 1 to 6. The lithium salts used in the electrolytic solution of the present invention may be used alone or in any combination of two or more.

[0050] In the present invention, it is preferable to prepare an electrolytic solution by adding the above-mentioned electrolyte to a dispersion medium, and then use this electrolytic solution to prepare a positive electrode slurry. The concentration of the lithium salt in the electrolytic solution is usually 10.0 to 50.0 mass%, preferably 15.0 to 30.0 mass%, and the molar concentration is preferably 0.5 to 1.5 M.

[0051] <Dispersion medium> A non-aqueous solvent is used as the dispersion medium. As the non-aqueous solvent, an aprotic organic solvent is preferred, and among these, an aprotic organic solvent having 2 to 10 carbon atoms is more preferred. Examples of such non-aqueous solvents include linear or cyclic carbonate compounds, lactone compounds, linear or cyclic ether compounds, ester compounds, nitrile compounds, amide compounds, oxazolidinone compounds, nitro compounds, linear or cyclic sulfone or sulfoxide compounds, and phosphate ester compounds. Compounds having an ether bond, carbonyl bond, ester bond, or carbonate bond are preferred. These compounds may have a substituent.

[0052] Examples of non-aqueous solvents include ethylene carbonate, fluorinated ethylene carbonate, vinylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, γ-butyrolactone, γ-valerolactone, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, tetrahydropyran, 1,3-dioxolane, 4-methyl-1,3-dioxolane, 1,3-dioxane, 1,4-dioxane, and methyl acetate. , ethyl acetate, methyl propionate, ethyl propionate, methyl butyrate, methyl isobutyrate, methyl trimethylacetate, ethyl trimethylacetate, acetonitrile, glutaronitrile, adiponitrile, methoxyacetonitrile, 3-methoxypropionitrile, N,N-dimethylformamide, N-methylpyrrolidone (NMP), N-methyloxazolidinone, N,N'-dimethylimidazolidinone, nitromethane, nitroethane, sulfolane, trimethyl phosphate, dimethyl sulfoxide, dimethyl sulfoxide phosphate, and the like. These may be used alone or in combination of two or more. However, the nonaqueous solvent used in the present invention is not limited to these. The dispersion medium is preferably a mixed solvent of ethylene carbonate (EC), propylene carbonate (PC), and dimethyl carbonate (DMC).

[0053] The positive electrode slurry of the present invention does not contain a binder. The binder here refers to a binder used in general nonaqueous electrolyte secondary batteries, and includes, for example, thermoplastic resins such as fluororesins (polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), etc.), polyethylene, polypropylene, polyacrylic, and polyimide; elastomers such as ethylene-propylene-diene rubber (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), and fluororubber; and polysaccharide polymers.

[0054] The positive electrode slurry of the present invention preferably has a solids content (components other than the dispersion medium (solvent)) of more than 60 mass%, more preferably 65 mass% or more, and even more preferably 70 mass% or more. The solids content is preferably 60 to 95 mass%, more preferably 65 to 92 mass%, even more preferably 70 to 90 mass%, still more preferably 72 to 88 mass%, and particularly preferably 75 to 85 mass%.

[0055] <Other Components> The positive electrode slurry of the present invention may optionally contain an ionic liquid, a thickener, an antifoaming agent, a leveling agent, a dehydrating agent, an antioxidant, etc. These may be those typically used in nonaqueous electrolyte secondary batteries. When the positive electrode slurry of the present invention contains other components, the amount of the other components is preferably 0.05 to 1.5 parts by mass, more preferably 0.1 to 1.0 parts by mass, per 100 parts by mass of the total content of the positive electrode active material and the conductive additive.

[0056] <Method for preparing positive electrode slurry> The positive electrode slurry of the present invention can be prepared by mixing a positive electrode active material consisting of large particle group A and small particle group B, an electrolyte, a dispersion medium, and other optional components, for example, using any of various commonly used mixers.

[0057] [Positive Electrode Sheet] The positive electrode sheet of the present invention is a positive electrode sheet having a positive electrode active material layer formed using the positive electrode slurry of the present invention, and is a positive electrode sheet suitable as a positive electrode sheet for a nonaqueous electrolyte secondary battery. In the positive electrode sheet of the present invention, the positive electrode active material layer includes a positive electrode active material composed of a large particle group A having a particle size of 5.0 μm or more and a small particle group B having a particle size of less than 5.0 μm, and when the total frequency in the number-based particle size distribution of the positive electrode active material is 100%, the frequency of the large particle group A is 60% or more and the frequency of the small particle group B is 40% or less, and the amount of dispersion medium absorbed by the small particle group B per 100 g (ηB (g / 100 g)) satisfies the above formula B1.

[0058] In the present invention, the term "cathode sheet" refers to both a cathode sheet incorporated as a component of a nonaqueous electrolyte secondary battery (incorporated into the secondary battery) and a cathode sheet in the form of a cathode material prior to incorporation into the nonaqueous electrolyte secondary battery. That is, the structure (area, thickness, etc.) of the cathode sheet may be a structure used as a cathode or a structure that can be processed into a structure used as a cathode. The cathode sheet of the present invention may have a cathode active material layer formed using the cathode slurry of the present invention, and may be in a form in which the cathode active material layer and a cathode current collector are laminated. More specifically, the cathode active material layer may be laminated on both sides of the cathode current collector, or on one side of the cathode current collector. The cathode sheet is typically a sheet configured by laminating a cathode active material layer on a cathode current collector. The cathode active material layer may be composed of a single layer or multiple layers. The cathode sheet may further include other layers as needed. Examples of other layers include a protective layer (release sheet) and a coating layer. In the positive electrode sheet of the present invention, the positive electrode active material layer is preferably laminated in a state of being in direct contact with the positive electrode current collector.

[0059] In the positive electrode sheet of the present invention, the thickness of the positive electrode active material layer (slurry layer) is not particularly limited and can be, for example, 50 to 600 μm, preferably 150 to 500 μm, and more preferably 200 to 400 μm.

[0060] When the positive electrode sheet of the present invention has a positive electrode current collector, the positive electrode current collector constituting the positive electrode sheet of the present invention is not particularly limited, and a positive electrode current collector used in a typical secondary battery can be appropriately applied. For the positive electrode current collector typically used in these secondary batteries, reference can be made, for example, to JP 2016-201308 A, JP 2005-108835 A, JP 2012-185938 A, WO 2018 / 135395, etc. As the positive electrode current collector, aluminum, an aluminum alloy, etc. are preferred.

[0061] In the positive electrode sheet of the present invention, the positive electrode active material layer is less likely to collapse (peel off), and this collapse is usually more noticeable at the edges of the positive electrode active material layer.

[0062] The positive electrode sheet of the present invention can be obtained by forming a positive electrode active material layer using the positive electrode slurry of the present invention. For example, the positive electrode sheet of the present invention can be obtained by forming a film using the positive electrode slurry of the present invention. More specifically, a positive electrode current collector or the like is used as a substrate, and the positive electrode slurry of the present invention is applied thereon (optionally via another layer) to obtain a positive electrode sheet having a positive electrode active material layer on the substrate. The method for applying the positive electrode slurry is not particularly limited, and can be, for example, application using a roll coater, drop coating, placing the positive electrode slurry evenly on the positive electrode current collector or the like and then pressing (roll press or flat press), or placing the positive electrode slurry in a frame of a specified thickness and spreading it.

[0063] [Non-aqueous electrolyte secondary battery] The non-aqueous electrolyte secondary battery of the present invention (hereinafter also referred to as "secondary battery of the present invention") has the positive electrode sheet of the present invention as the positive electrode. The secondary battery of the present invention can have the same configuration as a normal non-aqueous electrolyte secondary battery, except that it has the positive electrode sheet of the present invention as the positive electrode. That is, the secondary battery of the present invention can be obtained by incorporating the positive electrode sheet of the present invention as the positive electrode of a normal non-aqueous electrolyte secondary battery.

[0064] Prior to describing the secondary battery of the present invention, the structure of a general non-aqueous electrolyte secondary battery will be described. FIG. 1 is a cross-sectional view showing a schematic representation of the laminated structure of a general non-aqueous electrolyte secondary battery 10, including operating parts when the battery is in operation. The non-aqueous electrolyte secondary battery 10 has a laminated structure including, as viewed from the negative electrode side, a negative electrode current collector 1, a negative electrode active material layer 2, a separator 3, a positive electrode active material layer 4, and a positive electrode current collector 5, in this order. The negative electrode active material layer 2, the positive electrode active material layer 4, and the space between them are filled with a non-aqueous electrolyte (not shown), and are separated by the separator 3. The separator 3 has pores, and during normal battery use, functions as a separator between the positive and negative electrodes, allowing electrolyte and ions to pass through the pores, insulating the positive and negative electrodes. With this structure, for example, in the case of a lithium-ion secondary battery, electrons (e - ) is supplied, and at the same time, lithium ions (Li +) moves and accumulates in the negative electrode. On the other hand, during discharge, the lithium ions (Li + ) is returned to the positive electrode side through the electrolyte, and electrons are supplied to the operating part 6. In the illustrated example, a light bulb is used as the operating part 6, and it is lit by discharge.

[0065] Next, the basic structure characteristic of quasi-solid secondary batteries will be described. As described above, in quasi-solid secondary batteries, the electrode active material layer is formed in a slurry state containing an electrode active material and an electrolyte. Therefore, the electrode active material layer is a layer using a slurry (suspension, dispersion) in which the electrode active material is dispersed in a non-aqueous electrolyte, which distinguishes the structure from a typical non-aqueous electrolyte secondary battery. That is, in a typical non-aqueous electrolyte secondary battery, a coating solution is prepared by dispersing the electrode active material in a medium that does not contain an electrolyte, and the coating solution is applied to a current collector to form a coating film. The coating film is then dried to form a thin-film electrode active material layer. This coating solution usually contains a binder, which firmly binds the electrode active material particles together to form a hard electrode active material layer. Since the non-aqueous electrolyte is present on the electrode active material layer thus formed (between the negative electrode active material layer and the positive electrode active material layer), even if there are portions in the electrode active material layer that can be penetrated by the non-aqueous electrolyte, the electrode active material layer is in the form of a hard solid particle layer overall, not a slurry layer. In contrast, in a quasi-solid secondary battery, the electrode active material layer is an electrode slurry layer formed by dispersing solid particles containing an electrode active material and a conductive additive in a non-aqueous electrolyte solution obtained by dissolving a lithium salt (electrolyte) in a non-aqueous solvent. For this electrode slurry layer to function as an electrode active material layer, strong binding between the electrode active material particles is not required, and therefore the electrode slurry layer usually does not contain a binder. Except for the fact that the electrode active material layer is an electrode slurry layer and that the electrode slurry layer is in contact with the separator, the basic layer configuration of a quasi-solid secondary battery is the same as the layer configuration shown in FIG. 1 .

[0066] The secondary battery of the present invention is the quasi-solid secondary battery described above, wherein the positive electrode active material layer is a slurry layer formed from the positive electrode slurry of the present invention, and the negative electrode active material layer can be a negative electrode active material layer formed from a conventional negative electrode slurry.

[0067] The secondary battery of the present invention is not particularly limited in terms of the materials and components, such as the negative electrode active material, negative electrode current collector, and separator, except that the positive electrode sheet of the present invention is used as the positive electrode of the secondary battery. These materials and components can be appropriately selected from those used in conventional secondary batteries. For details of the components and manufacturing methods typically used in these secondary batteries, see, for example, JP 2016-201308 A, JP 2005-108835 A, JP 2012-185938 A, and WO 2018 / 135395.

[0068] Regarding the method for producing the nonaqueous electrolyte secondary battery of the present invention, a conventional method can be appropriately adopted, except that the positive electrode sheet of the present invention is used as the positive electrode. For example, JP-A-2016-201308, JP-A-2005-108835, JP-A-2012-185938, JP-A-2017-147222, etc. can be appropriately referenced.

[0069] The nonaqueous electrolyte secondary battery of the present invention can be installed in electronic devices such as notebook computers, pen-input personal computers, mobile personal computers, electronic book players, mobile phones, cordless phone handsets, pagers, handheld terminals, portable fax machines, portable copiers, portable printers, headphone stereos, video camcorders, LCD televisions, handheld vacuum cleaners, portable CD players, mini-discs, electric shavers, transceivers, electronic organizers, calculators, memory cards, portable tape recorders, radios, backup power supplies, and memory cards. It can also be installed in consumer electronic devices such as automobiles, electric vehicles, motors, lighting fixtures, toys, game devices, road conditioners, clocks, flash devices, cameras, and medical devices (pacemakers, hearing aids, shoulder massagers, etc.). It can also be used for various military and space applications. It can also be combined with solar cells.

[0070] The present invention will be described in more detail below with reference to examples, but the present invention should not be construed as being limited thereto.

[0071] [Preparation of Positive Electrode Active Material] A positive electrode active material was prepared as follows.

[0072] <LFP1-1 to LFP1-3 (Large particle group a)> (LFP1-1) LFP (LiFePO 4 ) A powder raw material (P198-S13 (trade name), manufactured by LOPAL Corporation) was used. (LFP1-2 and LFP1-3) 20 g of LFP1-1 was placed in a powder processing device Nobilta (trade name: NOB MINI, manufactured by Hosokawa Micron Corporation), and surface smoothing treatment was performed in a nitrogen atmosphere at the rotation speed and for the treatment time shown in Table 1, to obtain powder-like positive electrode active materials LFP1-2 and LFP1-3, respectively.

[0073] <LFP2-1 to LFP2-6 (small particle group b)> (LFP2-1) LFP (LiFePO 4 ) A powder raw material (P198-T5 (trade name) manufactured by LOPAL) was used. (LFP2-2 to LFP2-6) 20 g of LFP2-1 was placed in a powder processing device Nobilta (trade name: NOB MINI, manufactured by Hosokawa Micron Corporation), and surface smoothing treatment was performed in a nitrogen atmosphere at the rotation speeds and for the treatment times shown in Table 1, to obtain powder-like positive electrode active materials LFP2-2 to LFP2-6, respectively.

[0074] <NMC1-1 to NMC1-3 (large particle group a)> (NMC1-1) NMC (LiNi 1/3 Co 1/3 Mn 1/3 O 2 ) A powder raw material (NCM111 (particle size 12 μm) (trade name) manufactured by Toshima Manufacturing Co., Ltd.) was used. (NMC1-2 and NMC1-3) 20 g of NMC1-1 was placed in a powder processing device Nobilta (trade name: NOB MINI, manufactured by Hosokawa Micron Corporation), and surface smoothing treatment was performed in a nitrogen atmosphere at the rotation speed and for the treatment time shown in Table 1, to obtain powder-like positive electrode active materials NMC1-2 and NMC1-3, respectively.

[0075] <NMC2-1 to NMC2-6 (small particle group b)> (NMC2-1) NMC (LiNi 1/3 Co 1/3 Mn 1/3 O 2) A powder raw material (NCM111 (particle size 2 μm) (trade name) manufactured by Toshima Manufacturing Co., Ltd.) was used. (NMC2-2 to NMC2-6) 20 g of NMC2-1 was placed in a powder processing device Nobilta (trade name: NOB MINI, manufactured by Hosokawa Micron Corporation), and surface smoothing treatment was performed in a nitrogen atmosphere at the rotation speeds and for the treatment times shown in Table 1, to obtain powder-like positive electrode active materials NMC2-2 to NMC2-6, respectively.

[0076] The number-based particle size distributions of LFP1-1 to LFP1-3 and NMC1-1 to NMC1-3 were obtained as described below, and each positive electrode active material contained substantially no particles with a particle size of less than 5.0 μm. The number-based particle size distributions of LFP2-1 to LFP2-6 and NMC2-1 to NMC2-6 were obtained as described below, and each positive electrode active material contained substantially no particles with a particle size of 5.0 μm or more.

[0077] (Method for Measuring Number-Based Particle Size Distribution) 0.01 g of each positive electrode active material was dispersed in ethanol to prepare a dispersion having a laser light (light with a wavelength of 650 nm) transmittance of 90% to 95%. The particle diameters (sphere-equivalent diameters) of all particles in the dispersion were measured using a particle size measuring device (LA-920 (trade name), manufactured by Horiba, Ltd.) to obtain number-based particle size distribution data (cumulative particle size distribution data).

[0078]

[0079] [Measurement of median diameter (D50)] The median diameter (D50) of the large particle group a and the small particle group b obtained above was determined as described above. The median diameter (D50) of the large particle group a and the small particle group b is shown in the "D50" column of Table 2.

[0080] [Measurement of Specific Surface Area] The specific surface areas of the large particle group a and the small particle group b obtained above were determined as described above. The specific surface areas of the large particle group a and the small particle group b are shown in the "Specific Surface Area" column of Table 2.

[0081] [Method for Evaluating Liquid Absorption Amount] The liquid absorption amount ηA of the large particle group a of the dispersion medium used in the slurry for forming a positive electrode (described later) and the liquid absorption amount ηB of the small particle group b of the dispersion medium used in the slurry for forming a positive electrode (described later) were measured as described above. The "Liquid Absorption Amount ηA" column in Table 2 shows the liquid absorption amount ηA of each large particle group a, and the "Liquid Absorption Amount ηB" column shows the liquid absorption amount ηB of each small particle group b.

[0082] [Method for Evaluating Closest Packing Ratio] A dispersion was prepared by dispersing 0.01 g of a positive electrode active material powder composed of large particle group A and small particle group B in the ratios shown in Table 2 in ethanol so as to have a laser light (light having a wavelength of 650 nm) transmittance of 90% to 95%. The particle diameters (sphere-equivalent diameters) of all particles in the dispersion were measured using a particle size measuring device (LA-920 (trade name), manufactured by Horiba, Ltd.), and volume-based cumulative particle size distribution data of the particle diameters was obtained. The cumulative particle size distribution data was input into a calculation software for estimating the void fraction of a multi-component particle packed bed (CALVOIDN.EXE, developed by Professor Emeritus Suzuki Michitaka, Powder and Particle Engineering Laboratory, Department of Chemical Engineering, Graduate School of Engineering, University of Hyogo. Reference URL: https: / / www.eng.u-hyogo.ac.jp / group / group42 / hakaru / calvoid.html), and an estimated void fraction was obtained. Furthermore, the closest packing fraction (closest packing fraction (%) = 100 - estimated void fraction). Note that, when the estimated void fraction was obtained, a constant value (εj = 0.36 for each component particle) was used as the void fraction εj when each component particle was packed alone, and the cumulative particle size distribution measured on a volume basis as above was used as the cumulative undersieve weight percentage Rj.

[0083] [Preparation of Non-Aqueous Electrolyte Solution I] A non-aqueous electrolyte solution I was prepared by dispersing ethylene carbonate (EC), propylene carbonate (PC), and dimethyl carbonate (DMC) in a mass ratio of EC:PC:DMC=3:4:3. 6 These were mixed to a concentration of 1M to prepare a non-aqueous electrolyte solution (non-aqueous electrolyte solution I).

[0084] [Preparation of Slurry for Positive Electrode Formation] 75 parts by mass of a positive electrode active material containing the large particle group A and small particle group B shown in Table 2 in the ratios shown in Table 2, 0.3 parts by mass of Ketjen black (Carbon ECP600JD (trade name), manufactured by Lion Corporation) as a conductive additive, and 24.7 parts by mass of nonaqueous electrolyte I were mixed in a centrifugal planetary mixer (Thinky Corporation: Awatori Rentaro ARE-310 (trade name)) at 1250 rpm for 90 seconds to obtain slurries for positive electrodes (Nos. 1 to 24). The positive electrode active material used to prepare the slurries for positive electrodes of Experiments Nos. 2 to 4, 6 to 12, 14 to 16, and 18 to 24 was a mixture of the large particle group A and the small particle group B, in which the large particle group A and the small particle group B had the number frequencies shown in Table 2.

[0085] [Preparation of Positive Electrode Sheet] Each of the positive electrode slurries obtained above was applied to one side of a 12 μm-thick positive electrode current collector (aluminum foil) to obtain a positive electrode sheet consisting of the positive electrode current collector and a positive electrode active material layer (slurry layer). The thickness of the positive electrode active material layer of this positive electrode sheet was 350 μm.

[0086] [Fabrication of Nonaqueous Electrolyte Secondary Battery] 1) Preparation of Negative Electrode Sheet 65 parts by mass of a negative electrode active material (artificial graphite, UF-G30, manufactured by Showa Denko KK), 1 part by mass of acetylene black (Li-100 (trade name), manufactured by Denka Co., Ltd.) as a conductive additive, and 34 parts by mass of nonaqueous electrolyte I were mixed in a centrifugal planetary mixer (Thinky Corporation: Awatori Rentaro (trade name)) at 1250 rpm for 90 seconds to obtain a negative electrode-forming slurry. The obtained negative electrode-forming slurry was coated on one side of a 12 μm-thick negative electrode current collector (copper foil), to obtain a negative electrode sheet consisting of the negative electrode current collector and a negative electrode active material layer (slurry layer). The thickness of the negative electrode active material layer of this negative electrode sheet was approximately 300 μm. 2) Preparation of Non-Aqueous Electrolyte Secondary Battery A separator was placed on the negative electrode sheet obtained above, followed by the positive electrode sheet obtained in the above "Preparation of Positive Electrode Sheet" to form a laminate of negative electrode current collector-negative electrode active material layer (slurry layer)-separator-positive electrode active material layer (slurry layer)-positive electrode current collector. An aluminum tab was attached to the end of the aluminum current collector of this laminate, and a nickel tab was attached to the end of the copper current collector by ultrasonic welding, to form an electrode assembly. This electrode assembly was sandwiched between two aluminum laminate films, and three sides were heat-sealed, with the remaining side vacuum-sealed to form a laminate-type non-aqueous electrolyte secondary battery (quasi-solid secondary battery).

[0087] [Method for evaluating shape stability during punching] Each of the positive electrode forming slurries obtained above was applied to one side of a 12 μm thick positive electrode current collector (aluminum foil) to a width of 5 cm, a length of 8 cm, and a thickness of 350 μm to obtain a positive electrode sheet consisting of a positive electrode current collector and a positive electrode active material layer (slurry layer). The center of each positive electrode sheet obtained above was punched out using a 2.5 cm square punching machine (manufactured by Nogami Giken Co., Ltd., clearance 1 μm), and all of the debris that fell off during this process was collected and weighed. Ten trials were performed, and the average value of the 10 measurements obtained was used as the weight of the debris. The weight of the debris obtained was evaluated according to the following evaluation criteria. -Evaluation criteria- A: 10 mg or less B: Over 10 mg and 50 mg or less C: Over 50 mg and 100 mg or less D: Over 100 mg and 150 mg or less E: Over 150 mg and 200 mg or less F: Over 200 mg

[0088] [Volumetric Energy Density Measurement Method] The positive electrode sheet used in preparing each of the nonaqueous electrolyte secondary batteries was punched out to a diameter of 10 mm. The positive electrode current collector was removed from the punched piece, and the thickness of the positive electrode active material layer was measured. The thickness of the negative electrode active material layer was measured in the same manner. The thickness of the power generating element was calculated by adding the thickness of the positive electrode current collector + the thickness of the positive electrode active material layer + the thickness of the separator + the thickness of the negative electrode active material layer + the thickness of the negative electrode current collector. The thickness of each constituent layer was measured using a constant pressure thickness meter (product name: PG-20J, manufactured by Teclock Corporation). The volume (L) of the power generating element was calculated by multiplying the thickness of the power generating element by the area of ​​the circular surface of the power generating element. Here, the volume (L) of the power generating element was calculated based on the ideal volume of the power generating element, without taking into account volume reduction due to collapse of the edges caused by punching the positive electrode sheet, etc. Separately, under Condition 1 described below, the nonaqueous electrolyte secondary battery obtained above was charged and discharged to measure the reference discharge capacity (Ah) and the average voltage (V) during discharge. The amount of electric power (Wh) was calculated by multiplying the reference discharge capacity (Ah) by the average voltage (V). The volumetric energy density of the nonaqueous electrolyte secondary battery was calculated by dividing the amount of electric power (Wh) thus obtained by the volume (L) of the power generating element obtained above. The obtained values ​​were evaluated according to the following evaluation criteria. -Evaluation Criteria- A: 420 Wh / L or more B: 410 Wh / L or more and less than 420 Wh / L C: 400 Wh / L or more and less than 410 Wh / L D: 380 Wh / L or more and less than 400 Wh / L E: 360 Wh / L or more and less than 380 Wh / L F: Less than 360 Wh / L <Condition 1. Charge / Discharge Conditions> (Charge / Discharge Conditions for Experiments No. 1 to 12 (Experiments using LFP as the positive electrode active material)) Constant current (CC)-constant voltage (CV) charge: current value 15 mA, upper limit voltage value 3.6 V, end current value 0.5 mA CC discharge: current value 15 mA, end voltage value 2.0 V (Charge / Discharge Conditions for Experiments No. 13 to 24 (Experiments using NMC as the positive electrode active material)) CC-CV charge: current value 15 mA, upper limit voltage value 4.2 V, end current value 0.5 mA CC discharge: current value 15 mA, upper limit voltage value 3.0 V

[0089] The results obtained are shown in Tables 2 and 3.

[0090]

[0091]

[0092]

[0093] (Notes for Table 2) For convenience, the information (median diameter) regarding "large particle group a" is also listed in the "large particle group A" column. Similarly, the information regarding "small particle group b" is also listed in the "small particle group B" column. "-" indicates that the component is not used.

[0094] As shown in Tables 2 and 3, when the positive electrode-forming slurry did not contain the large particle group A and the small particle group B at the frequencies specified in the present invention (Experiments Nos. 1, 4, 5, 13, 16, and 17), and when the absorption amount ηB of the dispersion medium of the small particle group B did not satisfy the formula B1: 15≦ηB≦30 (Experiments Nos. 11, 12, 23, and 24), the edge of the positive electrode active material in the positive electrode sheet was prone to collapse, resulting in poor shape stability. Furthermore, nonaqueous electrolyte secondary batteries having this positive electrode sheet as a positive electrode were poor in battery capacity (energy density). In contrast, when the positive electrode-forming slurry contained the large particle group A and the small particle group B at the frequency specified in the present invention and the amount of dispersion medium absorption ηB of the small particle group B satisfied the formula B1: 15≦ηB≦30 (Experiments Nos. 2, 3, 6-10, 14, 15, 18-22), even when a positive electrode active material layer having a thickness of 350 μm was formed, the resulting positive electrode sheet was free from edge collapse of the positive electrode active material, resulting in excellent shape stability. Furthermore, nonaqueous electrolyte secondary batteries having this positive electrode sheet as the positive electrode also had improved battery capacity.

[0095] While the present invention has been described in connection with embodiments thereof, we do not intend to limit our invention to any of the details of the description unless otherwise specified, and believe that the claims should be construed broadly without departing from the spirit and scope of the invention as set forth in the appended claims.

[0096] This application claims priority based on Japanese Patent Application No. 2023-90455, filed on May 31, 2023, the contents of which are incorporated herein by reference as part of the present specification.

[0097] REFERENCE SIGNS LIST 10 Non-aqueous electrolyte secondary battery 1 Negative electrode current collector 2 Negative electrode active material layer 3 Separator 4 Positive electrode active material layer 5 Positive electrode current collector 6 Operating part (light bulb)

Claims

1. A slurry for forming a positive electrode of a non-aqueous electrolyte secondary battery, comprising a positive electrode active material, an electrolyte, and a dispersion medium, the positive electrode active material being composed of a large particle group A having a particle size of 5.0 μm or more and a small particle group B having a particle size of less than 5.0 μm, the frequency of the large particle group A being 60% or more and the frequency of the small particle group B being 40% or less when the total frequency is taken as 100% in a number-based particle size distribution of the positive electrode active material, and the amount of absorption of the dispersion medium by the small particle group B per 100 g, ηB (g / 100 g), satisfies the following formula B1. Formula B1: 15≦ηB≦30 2. The slurry for forming a positive electrode according to claim 1, wherein the amount of the dispersion medium absorbed by the large particle group A per 100 g (g / 100 g) satisfies the following formula A1: 2≦ηA≦25.

3. The slurry for forming a positive electrode according to claim 2, wherein the amount of absorbed liquid ηA satisfies the following formula A2: 2≦ηA≦7.

4. The slurry for forming a positive electrode according to claim 3, wherein the liquid absorption amount ηB satisfies the following formula B2: 18≦ηB≦25.

5. The positive electrode forming slurry according to claim 4, wherein the positive electrode active material has a closest packing ratio calculated from a cumulative particle size distribution on a volume basis of 80% or more.

6. A positive electrode sheet having a positive electrode active material layer formed using the positive electrode forming slurry according to any one of claims 1 to 5.

7. A non-aqueous electrolyte secondary battery having the positive electrode sheet according to claim 6 as a positive electrode.

Citation Information

Patent Citations

  • Rechargeable lithium-ion secondary battery

    JP2005108835A

  • Nonaqueous secondary battery

    JP2012185938A

  • Method of manufacturing electrode for lithium ion secondary battery

    JP2015230748A

  • Nonaqueous electrolyte and nonaqueous secondary battery

    JP2016201308A

  • Lithium-ion battery

    JP2017147222A