Method for manufacturing non-aqueous electrolytic solution secondary battery, and non-aqueous electrolytic solution secondary battery

The method of using a non-aqueous electrolyte with a solvent of 4.0 kPa or more vapor pressure in the non-aqueous electrolyte secondary battery addresses the collapse and fluidity issues of the positive electrode active material layer, achieving higher battery performance by maintaining high fluidity and preventing disintegration, thereby improving energy density and cycle durability.

WO2024247853A1PCT designated stage expired Publication Date: 2024-12-05FUJIFILM CORP

Patent Information

Application Number
PCT/JP2024/018889
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-31
Filing Date
2024-05-22
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

The challenge in manufacturing non-aqueous electrolyte secondary batteries is to maintain high fluidity and ionic conductivity of the positive electrode active material layer while preventing collapse, as high content of solid particles in the slurry leads to decreased fluidity and performance issues due to the use of low viscosity solvents which are volatile and evaporate during coating, causing partial disintegration of the film.

Method used

A method involving a positive electrode active material layer formed with a non-aqueous electrolyte containing a solvent with a vapor pressure of 4.0 kPa or more, less than 1.0% by mass, and a high content of positive electrode active material, where the solvent is added to the slurry layer to enhance fluidity and prevent collapse, along with a conductive aid and electrolyte, ensuring high precision in forming the layer without a binder.

Benefits of technology

This approach results in a non-aqueous electrolyte secondary battery with a positive electrode active material layer exhibiting high fluidity and improved battery performance, including increased energy density and cycle durability, while preventing the collapse of the slurry-like layer, thus enhancing overall battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024018889_05122024_PF_FP_ABST
    Figure JP2024018889_05122024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a method for manufacturing a non-aqueous electrolytic solution secondary battery in which a positive electrode current collector, a positive electrode active material layer, a separator, a negative electrode active material layer, and a negative electrode current collector are laminated in the stated order, the method including: forming a slurry-like positive electrode active material layer by applying, onto the positive electrode current collector, a positive electrode forming slurry that contains a positive electrode active material, a conductive assistant, an electrolyte, and a non-aqueous solvent (I) in which the content of a solvent with a vapor pressure of at least 4.0 kPa is less than 1.0 mass%, the slurry containing at least 75 mass% of the positive electrode active material; and adding the solvent with a vapor pressure of at least 4.0 kPa to the slurry-like positive electrode active material layer. Also provided is a non-aqueous electrolytic solution secondary battery which can be obtained by using this manufacturing method.
Need to check novelty before this filing date? Find Prior Art

Description

Method for manufacturing non-aqueous electrolyte secondary battery and non-aqueous electrolyte secondary battery

[0001] The present invention relates to a method for manufacturing a nonaqueous electrolyte secondary battery and a nonaqueous electrolyte secondary battery.

[0002] Non-aqueous electrolyte secondary batteries, typified by lithium-ion secondary batteries, have high energy density and excellent storage performance, low-temperature operation, etc., and are widely used in portable electronic devices such as mobile phones and laptop computers. Furthermore, larger batteries are being used in transportation equipment such as automobiles, and their use as storage devices for nighttime electricity and electricity generated by natural energy sources is also progressing.

[0003] Techniques for increasing the capacity of non-aqueous electrolyte secondary batteries have been studied. For example, Patent Document 1 discloses a technique for making an electrode active material layer function as a secondary battery in the form of a slurry containing a high amount of active material. Specifically, the document describes an electrochemical cell including: a positive electrode made of a non-binding material containing a first active material and an electrolyte solution in a first non-aqueous liquid electrolyte; a negative electrode made of a non-binding material containing a second active material and an electrolyte solution in a second non-aqueous liquid electrolyte; and an ion-permeable membrane disposed between the positive electrode and the negative electrode, wherein the positive electrode and the negative electrode each have a thickness of about 200 μm to about 3000 μm. According to the technology described in Patent Document 1, like the above-mentioned positive and negative electrodes, the electrode active material layers (positive electrode active material layer and negative electrode active material layer) contain an electrolyte and are in a slurry state and unbound, so that the electrode active material layer can be made into a thick film while maintaining its flexibility, and no binder is required to bind the solid particles together, making it possible to significantly increase the overall charge capacity and energy density while maintaining the flexibility of the battery. A nonaqueous electrolyte secondary battery in which the electrode active material layers (positive electrode active material layer and / or negative electrode active material layer) are formed in a slurry state containing an electrolytic solution (electrolyte), as described in Patent Document 1, may be referred to as a quasi-solid secondary battery in the following description.

[0004] Furthermore, Patent Document 2 describes that when an electrode active material layer of a quasi-solid secondary battery is formed from an electrode active material slurry containing an electrode active material, a lithium salt, and a non-aqueous solvent, the water content of the electrode active material slurry is set to less than 500 ppm by mass, and that a non-aqueous electrolyte secondary battery (quasi-solid secondary battery) having an electrode active material layer formed in this manner has reduced internal resistance, high capacity, and excellent cycle durability.

[0005] JP 2017-147222 A JP 2019-186009 A

[0006] To further increase the capacity (energy density) of quasi-solid secondary batteries, attempts have been made to increase the content of a positive electrode active material, which stores and releases ions, in a slurry-like positive electrode active material layer containing a nonaqueous electrolyte. In this case, the positive electrode-forming slurry used to form the slurry-like positive electrode active material layer is increased in content of solid particles of the positive electrode active material, and this is then applied to a current collector. However, when the positive electrode active material content is increased in the slurry, the slurry becomes more like a powder, even though it contains the electrolyte, and its fluidity is reduced. This reduced fluidity reduces the ionic conductivity of the positive electrode active material layer. To improve the fluidity of the slurry, a certain amount of a low-viscosity nonaqueous solvent (low-viscosity solvent) is typically added to the nonaqueous solvent that serves as the medium for the nonaqueous electrolyte. However, after extensive research, the inventors have found that a coating formed by applying a positive electrode-forming slurry containing a low-viscosity solvent to a positive electrode current collector is prone to partial collapse, limiting the improvement of the resulting battery performance. This phenomenon was thought to be caused by the high volatility of the low-viscosity solvent, which caused the coating film to partially collapse as the low-viscosity solvent evaporated during coating film formation.

[0007] The present invention aims to provide a method for manufacturing a nonaqueous electrolyte secondary battery, which is a quasi-solid secondary battery, in which, in forming a slurry-like positive electrode active material layer containing a nonaqueous electrolyte, a positive electrode active material layer containing a high content of positive electrode active material is formed while collapse of this positive electrode active material layer can be sufficiently suppressed, and the positive electrode active material layer in the obtained battery has a nonaqueous electrolyte composition that exhibits sufficiently high fluidity, thereby making it possible to achieve higher battery performance, and a nonaqueous electrolyte secondary battery that can be obtained by this manufacturing method.

[0008] The above-mentioned object of the present invention is achieved by the following means.

[0009] [1] A method for manufacturing a non-aqueous electrolyte secondary battery having a positive electrode current collector, a positive electrode active material layer, a separator, a negative electrode active material layer, and a negative electrode current collector laminated in this order, the method comprising: applying a positive electrode-forming slurry containing a positive electrode active material, a conductive additive, an electrolyte, and a non-aqueous solvent (I) having a content of a solvent having a vapor pressure of 4.0 kPa or more of less than 1.0 mass %, the content of the positive electrode active material being 75 mass % or more, to the positive electrode current collector to form a slurry positive electrode active material layer; and adding a solvent having a vapor pressure of 4.0 kPa or more to the slurry positive electrode active material layer. [2] The method for manufacturing a non-aqueous electrolyte secondary battery according to [1], wherein the content of the solvent having a vapor pressure of 4.0 kPa or more in the non-aqueous solvent (I) is less than 0.1 mass %. [3] A method for producing a nonaqueous electrolyte secondary battery according to [1] or [2], wherein the separator has a contact angle of 45° or less with the solvent having a vapor pressure of 4.0 kPa or more. [4] A method for producing a nonaqueous electrolyte secondary battery according to any one of [1] to [3], comprising: forming a slurry negative electrode active material layer by applying a negative electrode-forming slurry containing a negative electrode active material, a conductive additive, an electrolyte, and the nonaqueous solvent (I) onto a negative electrode current collector; and adding a solvent having a vapor pressure of 4.0 kPa or more to the slurry negative electrode active material layer. [5] A nonaqueous electrolyte secondary battery obtained by the method for producing a nonaqueous electrolyte secondary battery according to any one of [1] to [4].

[0010] In the description of the present invention, a numerical range expressed using "to" means a range including the numerical values ​​written before and after "to" as the lower and upper limits. In the present invention, "nonaqueous electrolyte" means an electrolyte that does not substantially contain water. In other words, the "nonaqueous electrolyte" may contain a small amount of water within a range that does not impair the effects of the present invention. In the present invention, the "nonaqueous electrolyte" has a water concentration of 200 ppm (by mass) or less, preferably 100 ppm or less, and more preferably 20 ppm or less. Note that it is practically difficult to make a nonaqueous electrolyte completely anhydrous, and it usually contains 1 ppm or more of water. In the present invention, "nonaqueous solvent" also means a solvent that does not substantially contain water. In other words, the "nonaqueous solvent" may contain a small amount of water within a range that does not impair the effects of the present invention. In the present invention, the "nonaqueous solvent" has a water concentration of 200 ppm (by mass) or less, preferably 100 ppm or less, and more preferably 20 ppm or less. In practice, it is difficult to make the non-aqueous solvent completely anhydrous, and the non-aqueous solvent usually contains 1 ppm or more of water. In the present invention, the "collapse" of the slurry electrode active material layer means that a part of the slurry electrode active material layer is lost, a part of the electrode active material layer crumbles, or a part of the electrode active material layer cracks.

[0011] According to the method for producing a nonaqueous electrolyte secondary battery of the present invention, in forming a slurry-like positive electrode active material layer containing a nonaqueous electrolyte, it is possible to form a positive electrode active material layer having a high content of positive electrode active material while preventing collapse of the positive electrode active material layer, and the resulting nonaqueous electrolyte secondary battery has a nonaqueous electrolyte composition that exhibits sufficiently high fluidity, resulting in a nonaqueous electrolyte secondary battery that exhibits higher battery performance.Furthermore, the nonaqueous electrolyte secondary battery of the present invention has a positive electrode active material layer having a high content of positive electrode active material while preventing collapse of the positive electrode active material layer, and has a nonaqueous electrolyte composition that exhibits sufficiently high fluidity, resulting in higher battery performance.

[0012] FIG. 1 is a longitudinal cross-sectional view showing a schematic diagram of a basic layer structure of an embodiment of a nonaqueous electrolyte secondary battery.

[0013] Although preferred embodiments of the present invention will be described, the present invention is not limited to these embodiments except as defined in the present invention.

[0014] [Method for Manufacturing Nonaqueous Electrolyte Secondary Battery] In the method for manufacturing a nonaqueous electrolyte secondary battery of the present invention (also referred to as the "manufacturing method of the present invention"), the resulting nonaqueous electrolyte secondary battery has a structure in which a positive electrode current collector, a positive electrode active material layer, a separator, a negative electrode active material layer, and a negative electrode current collector are laminated in this order. This nonaqueous electrolyte secondary battery is a so-called quasi-solid secondary battery, and the positive electrode active material layer is a slurry-like positive electrode active material layer formed from a positive electrode-forming slurry containing a positive electrode active material, a conductive additive, an electrolyte, and a nonaqueous solvent. In this nonaqueous electrolyte secondary battery, it is preferable that the negative electrode active material layer is also a slurry-like negative electrode active material layer formed from a negative electrode-forming slurry containing a negative electrode active material, a conductive additive, an electrolyte, and a nonaqueous solvent.

[0015] In the manufacturing method of the present invention, a positive electrode-forming slurry containing a positive electrode active material, a conductive additive, an electrolyte, and a non-aqueous solvent containing less than 1.0 mass% of a solvent with a vapor pressure of 4.0 kPa or more is applied to a positive electrode current collector to form a slurry positive electrode active material layer. The method for applying the slurry is not particularly limited in the present invention, and can be, for example, application using a roll coater, drop coating, applying the slurry evenly to the current collector and then pressing (roll press or flat press), or applying the slurry within a frame of a specified thickness and spreading it. In the present invention, the positive electrode-forming slurry contains the positive electrode active material at a concentration of 75 mass% or more. As described above, at the stage of forming the slurry positive electrode active material layer, the positive electrode-forming slurry does not contain a solvent with a vapor pressure of 4.0 kPa or more, or if it does contain one, it is contained in the non-aqueous solvent in a small amount of less than 1.0 mass%. In other words, the slurry is substantially free of highly volatile solvents (low-viscosity solvents). By doing so, even when a slurry containing a high concentration of positive electrode active material, such as 75% by mass or more, is used, a positive electrode active material layer of the desired thickness or shape can be formed with high precision. When the active material is highly contained, even if a non-aqueous solvent is included, the state becomes somewhat similar to a powder. This state is also referred to as a "slurry" or "slurry-like" in the present invention. In other words, a mixture of solid particles, such as an active material or a conductive additive, and a non-aqueous solvent or an electrolyte solution is referred to as a "slurry" or "slurry-like" in the present invention. In the present invention, "vapor pressure" refers to the saturated vapor pressure at room temperature. That is, it refers to the vapor pressure at 25°C under standard atmospheric pressure (0.1 MPa).

[0016] The content of the positive electrode active material in the positive electrode forming slurry is preferably 76% by mass or more, more preferably 77% by mass or more, even more preferably 78% by mass or more, even more preferably 79% by mass or more, and even more preferably 80% by mass or more. The content of the positive electrode active material in the positive electrode forming slurry is usually 90% by mass or less, preferably 88% by mass or less, more preferably 86% by mass or less, even more preferably 84% by mass or less, even more preferably 83% by mass or less, and even more preferably 82% by mass or less. The content of the positive electrode active material in the positive electrode forming slurry is preferably 75 to 90% by mass, more preferably 76 to 88% by mass, even more preferably 77 to 86% by mass, even more preferably 78 to 84% by mass, even more preferably 79 to 83% by mass, and even more preferably 80 to 82% by mass. Furthermore, in the nonaqueous electrolyte secondary battery obtained by the manufacturing method of the present invention, the content of the positive electrode active material in the slurry positive electrode active material layer may be slightly reduced by the addition of a solvent having a vapor pressure of 4.0 kPa or more, but the amount of reduction is small. Therefore, in the nonaqueous electrolyte secondary battery obtained by the manufacturing method of the present invention, the preferred content of the positive electrode active material in the slurry positive electrode active material layer is the same as the preferred content of the positive electrode active material in the positive electrode-forming slurry described above.

[0017] In the non-aqueous solvent (also referred to as non-aqueous solvent (I)) constituting the positive electrode-forming slurry, the content of the solvent having a vapor pressure of 4.0 kPa or more is preferably less than 0.8% by mass, more preferably less than 0.6% by mass, even more preferably less than 0.4% by mass, even more preferably less than 0.2% by mass, even more preferably less than 0.1% by mass, and even more preferably less than 0.05% by mass. It is particularly preferable that the non-aqueous solvent (I) does not contain a solvent having a vapor pressure of 4.0 kPa or more. The vapor pressure of the solvent having a vapor pressure of 4.0 kPa or more is usually 80.0 kPa or less, preferably 60.0 kPa or less, 50.0 kPa or less, 40.0 kPa or less, 30.0 kPa or less, or 20.0 kPa or less. Specific examples of solvents having a vapor pressure of 4.0 kPa or more will be described later.

[0018] In the manufacturing method of the present invention, after forming the above-mentioned slurry positive electrode active material, the above-mentioned solvent having a vapor pressure of 4.0 kPa or more is added to this slurry positive electrode active material layer. This increases the fluidity of the slurry positive electrode active material layer and improves ionic conductivity, thereby effectively suppressing a decrease in discharge capacity during high current discharge, for example. The solvent having a vapor pressure of 4.0 kPa or more added to the slurry positive electrode active material layer preferably has a vapor pressure of 5.0 kPa or more, more preferably 6.0 kPa or more, and even more preferably 7.0 kPa or more. A preferred range of vapor pressure of the solvent having a vapor pressure of 4.0 kPa or more to be added to the slurry positive electrode active material layer is preferably 4.0 to 80.0 kPa, more preferably 5.0 to 60.0 kPa, even more preferably 6.0 to 50.0 kPa, still more preferably 7.0 to 40.0 kPa, even more preferably 7.0 to 30.0 kPa, and still more preferably 7.0 to 20.0 kPa.

[0019] The method for adding the solvent having a vapor pressure of 4.0 kPa or more to the slurry positive electrode active material layer is not particularly limited. For example, after the positive electrode-forming slurry is applied to a positive electrode current collector to form a slurry positive electrode active material layer, the solvent having a vapor pressure of 4.0 kPa or more can be added directly to the slurry positive electrode active material layer. Alternatively, after the positive electrode-forming slurry is applied to a positive electrode current collector to form a slurry positive electrode active material layer, a separator can be placed on the slurry positive electrode active material layer, and the solvent having a vapor pressure of 4.0 kPa or more can be added to the separator. Adding the solvent having a vapor pressure of 4.0 kPa or more to the separator can diffuse the solvent having a vapor pressure of 4.0 kPa or more into the slurry positive electrode active material layer, thereby allowing the solvent having a vapor pressure of 4.0 kPa or more to be added to the slurry positive electrode active material layer. Alternatively, a solvent having a vapor pressure of 4.0 kPa or more may be impregnated into the negative electrode active material layer of the negative electrode, and the negative electrode may be superimposed on a laminate of a positive electrode current collector, a slurry positive electrode active material layer, and a separator. This allows the solvent having a vapor pressure of 4.0 kPa or more to diffuse into the slurry positive electrode active material layer, thereby allowing the solvent having a vapor pressure of 4.0 kPa or more to be added to the slurry positive electrode active material layer. Alternatively, a solvent having a vapor pressure of 4.0 kPa or more may be impregnated into the negative electrode active material layer or the separator in the laminate of the negative electrode and the separator, and the laminate may be superimposed on a laminate of a positive electrode current collector and a slurry positive electrode active material layer. This allows the solvent having a vapor pressure of 4.0 kPa or more to diffuse into the slurry positive electrode active material layer, thereby allowing the solvent having a vapor pressure of 4.0 kPa or more to be added to the slurry positive electrode active material layer. The addition of a solvent having a vapor pressure of 4.0 kPa or more to the slurry positive electrode active material layer may be achieved by adding only the solvent having a vapor pressure of 4.0 kPa or more, or by mixing the solvent having a vapor pressure of 4.0 kPa or more with other components. Examples of other components include an electrolyte and a solvent having a vapor pressure of less than 4.0 kPa. When adding a solvent having a vapor pressure of 4.0 kPa or more to the slurry positive electrode active material layer, it is preferable to add the solvent without mixing with other components. This also applies to the addition of a solvent having a vapor pressure of 4.0 kPa or more to the slurry negative electrode active material layer described below.Regardless of the method described above for adding a solvent with a vapor pressure of 4.0 kPa or more to a slurry positive electrode active material layer, since solvents with a vapor pressure of 4.0 kPa or more are highly volatile, it is preferable to quickly prepare the battery to suppress this volatilization. Regarding the method for preparing a nonaqueous electrolyte secondary battery, a conventional method can be appropriately adopted, except for the steps characteristic of the present invention. For example, JP 2016-201308 A, JP 2005-108835 A, JP 2012-185938 A, JP 2017-147222 A, etc. can be appropriately referenced.

[0020] In the nonaqueous electrolyte secondary battery obtained by the manufacturing method of the present invention, the content of the solvent having a vapor pressure of 4.0 kPa or more in the nonaqueous solvent constituting the slurry positive electrode active material layer (when the entire nonaqueous solvent is taken as 100% by mass) is preferably 2.0 to 10.0% by mass, more preferably 3.0 to 9.0% by mass, even more preferably 3.5 to 8.0% by mass, even more preferably 4.0 to 7.0% by mass, and even more preferably 4.0 to 6.0% by mass. The content of the solvent having a vapor pressure of 4.0 kPa or more in the nonaqueous solvent can be determined by conventional methods. For example, a portion of the slurry positive electrode active material layer is sampled and mixed with an extraction solvent such as chloroform or dimethyl sulfoxide (DMSO), and the supernatant is then measured using liquid phase chromatography, gas chromatography, H-NMR, or the like, to thereby quantify the content.

[0021] In the nonaqueous electrolyte secondary battery obtained by the manufacturing method of the present invention, the contact angle of the solvent having a vapor pressure of 4.0 kPa or more (the solvent having a vapor pressure of 4.0 kPa or more contained in the slurry positive electrode active material layer of the nonaqueous electrolyte secondary battery, i.e., the solvent having a vapor pressure of 4.0 kPa or more added later to the slurry positive electrode active material layer during the manufacturing of the nonaqueous electrolyte secondary battery) with the separator is preferably 45° or less. Many solvents having a vapor pressure of 4.0 kPa or more have high polarity, while many separators have low polarity, such as polyolefin resins. When the polarity of the separator is low, for example, the contact angle of the solvent having a vapor pressure of 4.0 kPa or more with the separator can be controlled to 45° or less by modifying the surface properties by surface treating the separator. Examples of surface treatment methods for such separators include ceramic coating treatment (the ceramic to be coated can be, for example, Al 2 O 3 , TiO 2 , SiO 2 , zeolite, etc. If necessary, a coating treatment may be performed together with a binder. Examples of suitable treatments include surfactant treatments (e.g., treatment with polyoxyethylene alkyl ethers, polyoxyethylene alkylphenyl ethers, polyoxyethylene monofatty acid esters, polyoxyethylene-modified polydimethylsiloxanes, alkylimidazolines, etc.), plasma treatments, corona discharge treatments, ultraviolet treatments, and acid treatments. By ensuring that the contact angle of the solvent with a vapor pressure of 4.0 kPa or more with the separator is 45° or less, battery performance can be further improved. For example, the decrease in discharge capacity during high-current discharge can be effectively suppressed. The contact angle of the solvent with a vapor pressure of 4.0 kPa or more with the separator is preferably 5 to 45°, more preferably 10 to 40°, even more preferably 15 to 30°, and even preferably 20 to 30°. This contact angle can be determined by the method described in the Examples below.

[0022] The manufacturing method of the present invention preferably includes forming a slurry negative electrode active material layer by applying a negative electrode-forming slurry containing a negative electrode active material, a conductive additive, an electrolyte, and the nonaqueous solvent (I) onto a negative electrode current collector. More preferably, the method further includes adding a solvent having a vapor pressure of 4.0 kPa or more to the slurry negative electrode active material layer. The preferred vapor pressure range of the solvent having a vapor pressure of 4.0 kPa or more added to the slurry negative electrode active material layer is the same as the preferred vapor pressure range of the solvent having a vapor pressure of 4.0 kPa or more added to the slurry positive electrode active material layer. In a preferred embodiment of the manufacturing method of the present invention, a negative electrode-forming slurry containing a negative electrode active material, a conductive additive, an electrolyte, and the non-aqueous solvent (I) is applied to a negative electrode current collector to form a slurry negative electrode active material layer. Separately, as described above, a positive electrode-forming slurry containing a positive electrode active material, a conductive additive, an electrolyte, and the non-aqueous solvent (I) is applied to a positive electrode current collector to form a slurry positive electrode active material layer. The method for adding the solvent having a vapor pressure of 4.0 kPa or more is not particularly limited. For example, the method of adding a solvent having a vapor pressure of 4.0 kPa or more to the slurry positive electrode active material layer can be appropriately applied. The content of the negative electrode active material in the negative electrode-forming slurry is preferably 50 to 80% by mass, more preferably 55 to 75% by mass, and even more preferably 60 to 70% by mass. In the nonaqueous electrolyte secondary battery obtained by the production method of the present invention, the content of the solvent having a vapor pressure of 4.0 kPa or more in the nonaqueous solvent constituting the slurry negative electrode active material layer is preferably 2.0 to 10.0 mass %, more preferably 3.0 to 9.0 mass %, even more preferably 3.5 to 8.0 mass %, even more preferably 4.0 to 7.0 mass %, and even more preferably 4.0 to 6.0 mass %. Note that, since the solvent is diffused and homogenized in the laminate consisting of the positive electrode active material layer, separator, and negative electrode active material layer, in the nonaqueous electrolyte secondary battery, the content of the solvent having a vapor pressure of 4.0 kPa or more in the nonaqueous solvent constituting the slurry negative electrode active material layer is substantially the same as the content of the solvent having a vapor pressure of 4.0 kPa or more in the nonaqueous solvent constituting the slurry positive electrode active material layer.Furthermore, in the nonaqueous electrolyte secondary battery obtained by the manufacturing method of the present invention, the content of the negative electrode active material in the slurry negative electrode active material layer is slightly reduced by the addition of a solvent having a vapor pressure of 4.0 kPa or more, but the amount of reduction is small. Therefore, in the nonaqueous electrolyte secondary battery obtained by the manufacturing method of the present invention, the preferred content of the negative electrode active material in the slurry negative electrode active material layer is the same as the preferred content of the negative electrode active material in the negative electrode-forming slurry described above.

[0023] Both the positive electrode-forming slurry and the negative electrode-forming slurry typically contain a conductive additive. The content of the conductive additive in these slurries is preferably 0.02 to 6.00 mass%, more preferably 0.04 to 4.00 mass%, even more preferably 0.06 to 3.00 mass%, and still more preferably 0.07 to 2.5 mass%.

[0024] Next, the materials used in the manufacturing method of the present invention will be described.

[0025] <Positive electrode active material> The positive electrode active material is preferably one that can reversibly insert and release lithium ions. There are no particular limitations on the material as long as it exhibits the desired electronic conductivity, and examples thereof include transition metal oxides, organic substances, sulfur, and other substances that can be composited with Li, as well as sulfur-metal composites. Among these, it is preferable to use lithium-containing transition metal oxides as the positive electrode active material, and the transition metal element M a It is more preferable that the lithium-containing transition metal oxide contains at least one element selected from Co, Ni, Fe, Mn, Cu, and V. b (Elements of Group 1 (Ia) of the periodic table other than lithium, elements of Group 2 (IIa), Al, Ga, In, Ge, Sn, Pb, Sb, Bi, Si, P, B, etc.) may be mixed. The amount of the mixed element may be determined by the following formula: a The amount of Li / M is preferably 0 to 30 mol % relative to the amount of Li / M (100 mol %). aMore preferably, the lithium-containing transition metal oxide is synthesized by mixing the above-mentioned components so that the molar ratio of the above-mentioned components is 0.3 to 2.2. Specific examples of the lithium-containing transition metal oxide include (MA) a lithium-containing transition metal oxide having a layered rock salt structure, (MB) a lithium-containing transition metal oxide having a spinel structure, (MC) a lithium-containing transition metal phosphate compound, (MD) a lithium-containing transition metal halide phosphate compound, and (ME) a ​​lithium-containing transition metal silicate compound.

[0026] (MA) Specific examples of lithium-containing transition metal oxides having a layered rock salt structure include LiCoO 2 (Lithium cobalt oxide [LCO]), LiNi 2 O 2 (lithium nickel oxide), LiNi 0.85 Co 0.10 Al 0.05 O 2 (nickel cobalt lithium aluminum oxide [NCA]), LiNi 1/3 Co 1/3 Mn 1/3 O 2 (Lithium nickel manganese cobalt oxide [NMC]) and LiNi 0.5 Mn 0.5 O 2 (Lithium manganese nickel oxide). (MB) Specific examples of lithium-containing transition metal oxides having a spinel structure include LiMn 2 O 4 (LMO), LiCoMnO 4 , Li 2 FeMn 3 O 8 , Li 2 CuMn 3 O 8 , Li 2 CrMn 3 O 8 and Li 2 NiMn 3 O 8 Examples of the (MC) lithium-containing transition metal phosphate compound include LiFePO 4 and Li 3 Fe 2 (P.O. 4 ) 3Olivine-type iron phosphate salts such as LiFeP 2 O 7 Iron pyrophosphates such as LiCoPO 4 Cobalt phosphates such as Li 3 V 2 (P.O. 4 ) 3 (MD) Examples of lithium-containing transition metal halide phosphate compounds include, for example, Li 2 FePO 4 Fluorophosphate iron salts such as F, Li 2 MnPO 4 Fluorophosphate manganese salts such as F and Li 2 CoPO 4 Examples of the (ME) lithium-containing transition metal silicate compound include cobalt fluoride phosphates such as Li 2 FeSiO 4 , Li 2 MnSiO 4 and Li 2 CoSiO 4 In the present invention, the positive electrode active material is preferably a lithium-containing transition metal phosphate compound (MC), such as LiFePO 4 is more preferred.

[0027] The shape of the positive electrode active material is not particularly limited, but particulate form is preferred. The average particle size (average particle size in equivalent spheres) of the positive electrode active material is not particularly limited. For example, it can be 0.1 to 50 μm, preferably 0.2 to 30 μm, more preferably 0.5 to 20 μm, and even more preferably 0.8 to 10 μm. A conventional grinder or classifier can be used to adjust the positive electrode active material to a predetermined particle size. The positive electrode active material obtained by the calcination method may be used after washing with water, an acidic aqueous solution, an alkaline aqueous solution, or an organic solvent.

[0028] When a commercially available positive electrode active material is used, the average particle size of the positive electrode active material is the value listed in the manufacturer's catalog. When the manufacturer's average particle size information is unavailable or when a synthesized positive electrode active material is used, the positive electrode active material is dispersed in water and the particle size value (volume-based median diameter D50 in water) obtained by measuring with a laser diffraction / scattering particle size distribution measurement device (e.g., HORIBA Particle LA-960V2) is used. This also applies to the average particle size of solid particles other than the positive electrode active material.

[0029] The chemical formula of the compound obtained by the above calcination method can be measured by inductively coupled plasma (ICP) emission spectroscopy, or simply calculated from the difference in mass of the powder before and after calcination.

[0030] The surface of the positive electrode active material may be coated with an oxide such as another metal oxide, a carbon-based material, or the like. These surface coating layers can function as an interface resistance stabilizing layer. Examples of surface coating agents include metal oxides containing Ti, Nb, Ta, W, Zr, Al, Si, or Li. Specific examples include titanate spinel, tantalum-based oxides, niobium-based oxides, and lithium niobate-based compounds, such as Li 4 Ti 5 O 12 , Li 2 Ti 2 O 5 , LiTaO 3 , LiNbO 3 , LiAlO 2 , Li 2 ZrO 3 , Li 2 WO 4 , Li 2 TiO 3 , Li 2 B 4 O 7 , Li 3 P.O. 4 , Li 2 MoO 4 , Li 3 BO 3 , LiBO 2 , Li 2 CO 3 , Li 2 SiO 3 , SiO2 , TiO 2 , ZrO 2 , Al 2 O 3 , B 2 O 3 , and Li 3 AlF 6 Carbon-based materials such as C, SiC, and SiOC (carbon-doped silicon oxide) can also be used as the surface coating material.

[0031] The positive electrode active material may be surface-coated with a carbon-based material in order to increase the electronic conductivity to a desired level. In this case, the positive electrode active material is preferably surface-coated with carbon (C). The carbon surface coating can be formed by baking the positive electrode active material in the presence of an additive (organic substance) that serves as a carbon source. Examples of the additive that can be used include styrene-maleic anhydride copolymer, polystyrene, and polycarbonate.

[0032] The surface of the positive electrode active material may be treated with sulfur or phosphorus. Furthermore, the particle surfaces of the positive electrode active material may be treated with actinic rays or an active gas (plasma, etc.) before or after the surface coating.

[0033] The positive electrode active materials may be used alone or in combination of two or more.

[0034] In the positive electrode active material layer, the content of the positive electrode active material relative to the total content of the positive electrode active material and the conductive additive is preferably 95.00 to 99.95 mass %, more preferably 96.00 to 99.90 mass %, and even more preferably 97.00 to 99.80 mass %.

[0035] <Negative electrode active material> The negative electrode active material is preferably one that can reversibly absorb and release lithium ions. The material is not particularly limited as long as it has the desired properties, and examples thereof include carbonaceous materials, silicon-based materials, metal oxides, metal composite oxides, lithium alone, lithium alloys, and negative electrode active materials that can form alloys with lithium. Among these, carbonaceous materials or silicon-based materials are preferably used from the viewpoint of reliability.

[0036] The carbonaceous material used as the negative electrode active material is a material essentially composed of carbon. Examples include carbon black such as petroleum pitch, graphite (natural graphite, artificial graphite such as vapor-grown graphite, etc.), and carbonaceous materials obtained by calcining various synthetic resins such as PAN (polyacrylonitrile)-based resins and furfuryl alcohol resins. Further examples include various carbon fibers such as PAN-based carbon fiber, cellulose-based carbon fiber, pitch-based carbon fiber, vapor-grown carbon fiber, dehydrated PVA (polyvinyl alcohol)-based carbon fiber, lignin carbon fiber, glassy carbon fiber, and activated carbon fiber, as well as mesophase microspheres, graphite whiskers, and tabular graphite.

[0037] The metal oxides and metal composite oxides used as the negative electrode active material are not particularly limited as long as they are oxides capable of absorbing and releasing lithium. Amorphous oxides are preferred, and chalcogenides, which are reaction products of metal elements and elements of Group 16 of the periodic table, are also preferred. The term "amorphous" as used herein refers to an X-ray diffraction method using CuKα radiation that has a broad scattering band with a peak in the 2θ value range of 20° to 40°, and may also have crystalline diffraction lines. Among the above amorphous oxides and chalcogenides, amorphous oxides or chalcogenides of metalloid elements are more preferred, and oxides or chalcogenides consisting of one or a combination of two or more of elements from Groups 13 (IIIB) to 15 (VB) of the periodic table, Al, Ga, Si, Sn, Ge, Pb, Sb, and Bi, are particularly preferred. Specific examples of preferred amorphous oxides and chalcogenides include, for example, Ga, 2 O 3 , GeO, PbO, PbO 2 , Pb 2 O 3 , Pb 2 O 4 , Pb 3 O 4 , Sb 2 O 3 , Sb 2 O 4 , Sb 2 O 8 Bi 2 O 3 , Sb 2 O 8 Si2 O 3 , Sb 2 O 5 , Bi 2 O 3 , Bi 2 O 4 , GeS, PbS, PbS 2 , Sb 2 S 3 and Sb 2 S 5 are preferred.

[0038] The metal (composite) oxide and the chalcogenide preferably contain at least one of titanium and lithium as a constituent component from the viewpoint of charge / discharge characteristics at high current density. Examples of the lithium-containing metal composite oxide (lithium composite metal oxide) include, for example, composite oxides of lithium oxide and the metal (composite) oxide or the chalcogenide, more specifically, Li 2 SnO 2 Examples include:

[0039] The negative electrode active material preferably contains titanium atoms. More specifically, TiNb 2 O 7 (Niobium titanate oxide [NTO]), Li 4 Ti 5 O1 2 Lithium titanate (LTO) is preferred because it has small volume fluctuations during absorption and desorption of lithium ions, has excellent rapid charge and discharge characteristics, suppresses electrode deterioration, and enables an improvement in the life of the lithium ion secondary battery.

[0040] The lithium alloy as the negative electrode active material is not particularly limited as long as it is an alloy that is commonly used as a negative electrode active material for secondary batteries, and an example thereof is a lithium aluminum alloy.

[0041] The negative electrode active material capable of forming an alloy with lithium is not particularly limited as long as it is one commonly used as a negative electrode active material for secondary batteries. Such active materials undergo large expansion and contraction during charging and discharging, resulting in reduced solid particle binding as described above. However, the present invention achieves high binding by using the binder. Examples of such active materials include negative electrode active materials containing silicon or tin atoms, and metals such as Al and In. Negative electrode active materials containing silicon atoms (silicon-containing active materials) that enable higher battery capacity are preferred, and silicon-containing active materials with a silicon atom content of 40 mol% or more of the total constituent atoms are more preferred. Generally, negative electrodes containing these negative electrode active materials (e.g., Si negative electrodes containing silicon-containing active materials, Sn negative electrodes containing tin-containing active materials) can absorb more Li ions than carbon negative electrodes (e.g., graphite and acetylene black). In other words, the amount of Li ions absorbed per unit mass is increased. This increases battery capacity (energy density). As a result, the battery operating time can be extended. Examples of silicon-atom-containing active materials include silicon materials such as Si and SiOx (0<x≦1), and alloys containing titanium, vanadium, chromium, manganese, nickel, copper, or lanthanum (e.g., LaSi 2 , VSi 2 ), or structured active materials (e.g., LaSi2 / Si), as well as SnSiO 3 , SnSiS 3 Examples of the active material containing silicon atoms and tin atoms include SiOx itself as a negative electrode active material (semi-metal oxide), and can also be used as an active material (precursor material) that can be alloyed with lithium because it generates Si during battery operation. Examples of the negative electrode active material containing tin atoms include Sn, SnO, and SnO 2 , SnS, SnS 2 and active materials containing silicon atoms and tin atoms. Also, composite oxides with lithium oxide, for example, Li 2 SnO 2 Also included are:

[0042] The shape of the negative electrode active material is not particularly limited, but a particulate form is preferred. The average particle diameter of the negative electrode active material is preferably 0.1 to 60 μm. To achieve the desired particle diameter, a conventional grinder or classifier is used. For example, a mortar, ball mill, sand mill, vibration ball mill, satellite ball mill, planetary ball mill, swirling airflow jet mill, or sieve is preferably used. Wet grinding in the presence of water or an organic solvent such as methanol can also be performed during grinding. Classification is preferably performed to achieve the desired particle diameter. The classification method is not particularly limited, and a sieve, air classifier, or the like can be used as desired. Classification can be performed using either a dry method or a wet method.

[0043] The above-mentioned negative electrode active materials may be used singly or in combination of two or more. Among them, a combination of a silicon atom-containing active material and a carbonaceous material is preferred, and a combination of SiOx (0<x≦1) and graphite is particularly preferred. When SiOx (0<x≦1) and graphite are combined, the mass ratio (SiOx / graphite) is preferably 2 or less, more preferably 1 or less, and even more preferably 0.5 or less. When forming a negative electrode active material layer, the unit area (cm 2 The mass (mg) (basis weight) of the negative electrode active material per unit area is not particularly limited and can be determined appropriately depending on the designed battery capacity.

[0044] In the negative electrode active material layer, the content of the negative electrode active material relative to the total content of the negative electrode active material and the conductive additive is preferably 95.00 to 99.95 mass %, more preferably 96.00 to 99.90 mass %, and even more preferably 97.00 to 99.80 mass %.

[0045] <Conductive Aid> The slurry contains a conductive aid. There are no particular limitations on the conductive aid, and any commonly known conductive aid can be used. For example, the conductive aid may be an electron-conductive material such as graphites (e.g., natural graphite, artificial graphite, etc.), carbon blacks (e.g., acetylene black, ketjen black, furnace black, etc.), amorphous carbon (e.g., needle coke), carbon fibers (e.g., vapor-grown carbon fibers or carbon nanotubes), or carbonaceous materials (e.g., graphene or fullerene). Alternatively, metal powders or metal fibers (e.g., copper or nickel), or conductive polymers (e.g., polyaniline, polypyrrole, polythiophene, polyacetylene, or polyphenylene derivatives) may be used. When an electrode active material and a conductive aid are used in combination, those conductive aids that do not intercalate or deintercalate Li during charging and discharging the battery and do not function as an active material are considered conductive aids. Therefore, among conductive aids, those that can function as an active material in the active material layer during charging and discharging the battery are classified as active materials rather than conductive aids. Whether or not a conductive additive functions as an active material when a battery is charged and discharged is not uniquely determined, but is determined depending on the combination with the active material. One type of conductive additive may be used, or two or more types may be used.

[0046] The shape of the conductive additive is not particularly limited, but is preferably particulate. The average particle size (average particle size in equivalent sphere form) of the conductive additive is not particularly limited. For example, it is preferably 0.01 to 50 μm, more preferably 0.1 to 10 μm, and even more preferably 0.2 to 2.0 μm.

[0047] In either the positive electrode active material layer or the negative electrode active material layer, the content of the conductive additive relative to the total content of the active material and the conductive additive is preferably 0.05 to 7.00 mass%, more preferably 0.05 to 5.00 mass%, more preferably 0.10 to 4.00 mass%, and even more preferably 0.20 to 3.00 mass%.

[0048] <Non-aqueous Electrolyte> In the present invention, the positive electrode-forming slurry and the slurry positive electrode active material layer contain a non-aqueous electrolyte, which is composed of an electrolyte (electrolyte salt) and a non-aqueous solvent that dissolves the electrolyte.

[0049] (Electrolyte) As the electrolyte, any electrolyte that can be used as an electrolytic solution for a quasi-solid secondary battery can be used appropriately. The electrolyte is preferably a metal salt, such as lithium salt, potassium salt, sodium salt, calcium salt, or magnesium salt. As the lithium salt, lithium salts that are commonly used in electrolytes for lithium ion secondary batteries are preferred, such as the following lithium salts:

[0050] (L-1) Inorganic lithium salt: LiPF 6 , LiBF 4 , LiAsF 6 , LiSbF 6 Inorganic fluoride salts such as LiClO 4 , LiBrO 4 , LiIO 4 perhalogenates such as LiAlCl 4 Inorganic chloride salts, etc.

[0051] (L-2) Fluorine-containing organic lithium salt: LiCF 3 SO 3 perfluoroalkanesulfonates such as LiN(CF 3 SO 2 ) 2 , LiN(CF 3 CF 2 SO 2 ) 2 , LiN(FSO 2 ) 2 , LiN(CF 3 SO 2 ) (C 4 F 9 SO 2 perfluoroalkanesulfonylimide salts such as LiC(CF 3 SO 2 ) 3 perfluoroalkanesulfonylmethide salts such as Li[PF 5 (CF 2 CF 2 CF 3 ) )], Li[PF 4 (CF 2 CF 2 CF 3 ) 2 ], Li[PF 3 (CF 2 CF 2 CF3 ) 3 ], Li[PF 5 (CF 2 CF 2 CF 2 CF 3 ) )], Li[PF 4 (CF 2 CF 2 CF 2 CF 3 ) 2 ], Li[PF 3 (CF 2 CF 2 CF 2 CF 3 ) 3 perfluoroalkyl fluorophosphates such as

[0052] (L-3) Oxalatoborate salts: lithium bis(oxalato)borate, lithium difluorooxalatoborate, etc.

[0053] Among these, LiPF 6 , LiBF 4 , LiAsF 6 , LiSbF 6 , LiClO 4 , Li(R f1 SO 3 ), LiN(R f1 SO 2 ) 2 , LiN(FSO 2 ) 2 , or LiN(R f1 SO 2 ) (R f2 SO 2 ) is preferred, and LiPF 6 , LiBF 4 , LiN(R f1 SO 2 ) 2 , LiN(FSO 2 ) 2 , or LiN(R f1 SO 2 ) (R f2 SO 2 ) is more preferred, and LiPF 6 is particularly preferred. f1 and R f2represents a perfluoroalkyl group, preferably having 1 to 6 carbon atoms.

[0054] The non-aqueous electrolyte may contain one electrolyte alone or two or more electrolytes in any combination.

[0055] In the positive electrode-forming slurry and the slurry positive electrode active material layer, the electrolyte concentration in the nonaqueous electrolyte is not particularly limited as long as it functions as a nonaqueous electrolyte. For example, it can be 10.0 to 50.0 mass %, preferably 15.0 to 30.0 mass %. The molar concentration is preferably 0.5 to 1.5 M.

[0056] (Non-aqueous Solvent) The non-aqueous solvent serving as the medium for the non-aqueous electrolyte solution is preferably an aprotic organic solvent, and more preferably an aprotic organic solvent having 2 to 10 carbon atoms. Examples of such non-aqueous solvents include linear or cyclic carbonate compounds, lactone compounds, linear or cyclic ether compounds, ester compounds, nitrile compounds, amide compounds, oxazolidinone compounds, nitro compounds, linear or cyclic sulfone or sulfoxide compounds, and phosphate ester compounds. Among these, compounds having an ether bond, carbonyl bond, ester bond, or carbonate bond are preferred. These compounds may have a substituent.

[0057] Examples of the solvent (nonaqueous solvent) having a vapor pressure of 4.0 kPa or more include isobutyronitrile (4370 Pa), ethyl propionate (5333 Pa), propanenitrile (6314 Pa), dimethoxymethane (6394 Pa), dimethyl carbonate (7381 Pa), acetonitrile (11839 Pa), 2-methyltetrahydrofuran (13600 Pa), tetrahydrofuran (21600 Pa), methyl acetate (23100 Pa), and diethyl ether (58600 Pa). One or more of these can be used. The value of the vapor pressure is given in parentheses. The same applies below. The solvent having a vapor pressure of 4.0 kPa or more is preferably selected from acetonitrile, dimethyl carbonate, and diethyl ether, from the viewpoint of reducing the viscosity of the electrolyte, and more preferably selected from acetonitrile or dimethyl carbonate, with acetonitrile being particularly preferred.

[0058] Examples of solvents (nonaqueous solvents) having a vapor pressure of less than 4.0 kPa include sulfolane (0.8 Pa), adiponitrile (0.9 Pa), biphenyl (1.2 Pa), ethylene carbonate (1.3 Pa), propylene carbonate (4.0 Pa), N-methylpyrrolidone (46 Pa), fluoroethylene carbonate (51 Pa), γ-butyrolactone (60 Pa), dimethyl sulfoxide (80 Pa), benzonitrile (102 Pa), vinylene carbonate (335 Pa), diglyme (395 Pa), β-propiolactone (453 Pa), diethyl carbonate (1439 Pa), and ethyl methyl carbonate (3600 Pa). One or more of these may be used. As the solvent having a vapor pressure of less than 4.0 kPa, it is preferable to use one or more selected from ethylene carbonate, propylene carbonate, and ethyl methyl carbonate, from the viewpoint of reducing the viscosity of the electrolytic solution.

[0059] In the present invention, the content of the nonaqueous electrolyte in the positive electrode-forming slurry is preferably 8 to 23% by mass, more preferably 10 to 22% by mass, even more preferably 12 to 21% by mass, even more preferably 14 to 20% by mass, even more preferably 15 to 19% by mass, and particularly preferably 16 to 18% by mass. Furthermore, in a nonaqueous electrolyte secondary battery obtained by the production method of the present invention, the content of the nonaqueous electrolyte in the slurry positive electrode active material layer may increase slightly due to the addition of a solvent with a vapor pressure of 4.0 kPa or more, but the increase is small. Therefore, in a nonaqueous electrolyte secondary battery obtained by the production method of the present invention, the preferred content of the nonaqueous electrolyte in the slurry positive electrode active material layer is the same as the preferred content of the nonaqueous electrolyte in the positive electrode-forming slurry described above.

[0060] In the present invention, the negative electrode can be any negative electrode used in a general nonaqueous electrolyte secondary battery, without any particular limitations. In the present invention, the negative electrode is preferably a laminate of a negative electrode current collector and a slurry negative electrode active material layer, as described above. In this case, the negative electrode-forming slurry and the slurry negative electrode active material layer contain a nonaqueous electrolyte. The nonaqueous electrolytes described above as those that can be contained in the positive electrode-forming slurry and the slurry positive electrode active material layer can be preferably used as the nonaqueous electrolytes for the negative electrode-forming slurry and the slurry negative electrode active material layer. In the present invention, the content of the nonaqueous electrolyte in the negative electrode-forming slurry is preferably 18 to 48% by mass, more preferably 23 to 43% by mass, and even more preferably 28 to 38% by mass. Furthermore, in the nonaqueous electrolyte secondary battery obtained by the production method of the present invention, the content of the nonaqueous electrolyte in the slurry negative electrode active material layer can increase slightly when a solvent with a vapor pressure of 4.0 kPa or more is added, but the increase is small. Therefore, in the nonaqueous electrolyte secondary battery obtained by the production method of the present invention, the preferred content of the nonaqueous electrolyte in the slurry negative electrode active material layer is the same as the preferred content of the nonaqueous electrolyte in the negative electrode-forming slurry described above.

[0061] <Other Components> The above-described positive electrode-forming slurry and negative electrode-forming slurry may optionally contain an ionic liquid, a thickener, an antifoaming agent, a leveling agent, a dehydrating agent, an antioxidant, etc. These may be those typically used in nonaqueous electrolyte secondary batteries. When the above-described positive electrode-forming slurry and / or negative electrode-forming slurry contain other components, the amount of the other components is preferably 0.05 to 1.5 parts by mass, more preferably 0.1 to 1.0 parts by mass, per 100 parts by mass of the total content of the active material and the conductive additive.

[0062] The positive electrode-forming slurry and the negative electrode-forming slurry described above can be obtained by uniformly mixing the components constituting the slurry. The mixing method is not particularly limited, and any method commonly used in this technical field can be appropriately adopted.

[0063] [Non-aqueous electrolyte secondary battery] The non-aqueous electrolyte secondary battery of the present invention (hereinafter also referred to as "secondary battery of the present invention") is a non-aqueous electrolyte secondary battery obtained by the manufacturing method of the present invention. That is, it is a so-called quasi-solid secondary battery having a positive electrode current collector, a positive electrode active material layer, a separator, a negative electrode active material layer, and a negative electrode current collector in this order, with at least the positive electrode active material layer being in a slurry state. In the secondary battery of the present invention, it is preferable that both the positive electrode active material layer and the negative electrode active material layer are in a slurry state.

[0064] Prior to describing the secondary battery of the present invention, the structure of a general nonaqueous electrolyte secondary battery will be described. FIG. 1 is a cross-sectional view showing a schematic representation of the laminated structure of a general nonaqueous electrolyte secondary battery 10, including the working electrode when the battery is operated. The nonaqueous electrolyte secondary battery 10 has a laminated structure (hereinafter also referred to as an electrode laminate) including, as viewed from the negative electrode side, a negative electrode current collector 1, a negative electrode active material layer 2, a separator 3, a positive electrode active material layer 4, and a positive electrode current collector 5, in this order. The negative electrode active material layer 2 and the positive electrode active material layer 4 are filled with a nonaqueous electrolyte (not shown) and separated by the separator 3. The separator 3 has pores, and during normal battery use, functions as a separator between the positive and negative electrodes, insulating them by allowing the electrolyte and ions to pass through the pores. With this structure, for example, in the case of a lithium-ion secondary battery, electrons (e- ) is supplied, and at the same time, lithium ions (Li + ) moves and accumulates in the negative electrode. On the other hand, during discharge, the lithium ions (Li + ) is returned to the positive electrode side through the electrolyte, and electrons are supplied to the operating part 6. In the illustrated example, a light bulb is used as the operating part 6, and it is lit by discharge.

[0065] Next, the basic structure characteristic of quasi-solid secondary batteries will be described. As described above, in quasi-solid secondary batteries, the active material layers of the positive and / or negative electrodes are formed in a slurry state containing an active material and an electrolyte. Therefore, the structure of a quasi-solid secondary battery differs from that of a typical non-aqueous electrolyte secondary battery in that the active material layers of the positive and / or negative electrodes are layers using a slurry (suspension, dispersion) in which the active material is dispersed in a non-aqueous electrolyte. That is, in a typical non-aqueous electrolyte secondary battery, a coating solution is prepared in which the active material is dispersed in a medium that does not contain an electrolyte, and this coating solution is applied to a current collector to form a coating film. This coating film is then dried to form a thin-film active material layer. This coating solution usually contains a binder, which firmly binds the active material particles together to form a hard active material layer. Since the non-aqueous electrolyte solution is present on the active material layer thus formed (between the negative electrode active material layer and the positive electrode active material layer), the active material layer is in the form of a hard solid particle layer overall, not a slurry, even if there are portions in the active material layer through which the non-aqueous electrolyte solution can penetrate. In contrast, in a quasi-solid secondary battery, the active material layer of the positive electrode and / or negative electrode is a slurry layer (slurry layer) formed by dispersing solid particles containing an active material and a conductive additive in a non-aqueous electrolyte solution obtained by dissolving an electrolyte such as a lithium salt in a non-aqueous solvent. For this slurry layer to function as an active material layer, strong binding between the active material particles is not required, and therefore, this slurry layer usually does not contain a binder. Except for the fact that the active material layer of the positive electrode and / or negative electrode is a slurry layer and that the slurry layer is in contact with the separator, the basic layer configuration of a quasi-solid secondary battery is the same as the layer configuration shown in FIG. 1 .

[0066] In the secondary battery of the present invention, at least the positive electrode active material layer is a slurry layer. In the secondary battery of the present invention, it is preferable that both the positive electrode active material layer and the negative electrode active material layer are slurry layers.

[0067] In the secondary battery of the present invention, the thickness of the slurry active material layer (slurry layer) is not particularly limited and can be, for example, 5 to 500 μm, preferably 20 to 400 μm, more preferably 40 to 400 μm, even more preferably 80 to 350 μm, even more preferably 120 to 350 μm, and even more preferably 150 to 340 μm.

[0068] In the secondary battery of the present invention, the materials and components of the positive electrode current collector, negative electrode current collector, separator, etc. are not particularly limited. These materials and components can be appropriately selected from those used in conventional non-aqueous electrolyte secondary batteries. For details on the components and manufacturing methods typically used in these secondary batteries, see, for example, JP 2016-201308 A, JP 2005-108835 A, JP 2012-185938 A, and WO 2018 / 135395. As described above, it is preferable to treat the surface of the separator to enhance its wettability with the non-aqueous solvent that is the medium for the non-aqueous electrolyte.

[0069] The nonaqueous electrolyte secondary battery of the present invention can be installed in electronic devices such as notebook computers, pen-input personal computers, mobile personal computers, electronic book players, mobile phones, cordless phone handsets, pagers, handheld terminals, portable fax machines, portable copiers, portable printers, headphone stereos, video camcorders, LCD televisions, handheld vacuum cleaners, portable CD players, mini-discs, electric shavers, transceivers, electronic organizers, calculators, memory cards, portable tape recorders, radios, backup power supplies, and memory cards. It can also be installed in consumer electronic devices such as automobiles, electric vehicles, motors, lighting fixtures, toys, game devices, road conditioners, clocks, flash devices, cameras, and medical devices (pacemakers, hearing aids, shoulder massagers, etc.). It can also be used for various military and space applications. It can also be combined with solar cells.

[0070] The present invention will be described in more detail below with reference to examples, but the present invention should not be construed as being limited thereto.

[0071] [Preparation of Slurry for Positive Electrode Formation] <Preparation of Non-Aqueous Electrolyte (i)> Ethylene carbonate (EC) / propylene carbonate (PC) / ethyl methyl carbonate (EMC) were mixed in a mass ratio of 30 / 40 / 30 to prepare a non-aqueous solvent (I). This non-aqueous solvent (I) and LiPF 6 The non-aqueous electrolyte solution (i) was obtained by mixing the above. 6 The concentration was 1.1 M (mol / liter).

[0072] <Preparation of non-aqueous electrolyte solution (ii)> Ethylene carbonate (EC) / propylene carbonate (PC) / ethyl methyl carbonate (EMC) / acetonitrile (AN) were mixed in a mass ratio of 27 / 36 / 27 / 10 to prepare a non-aqueous solvent (II). 6 The non-aqueous electrolyte solution (ii) was obtained by mixing the above. 6 The concentration was 1.0 M (mol / liter).

[0073] <Preparation of Slurry (a) for Forming Positive Electrode> LiFePO was used as the positive electrode active material. 4 The positive electrode-forming slurry (a) was prepared by uniformly mixing the above-mentioned cellulose acylate (manufactured by Gelon) in an amount of 80 mass %, acetylene black (manufactured by Denka Company, Ltd.) in an amount of 2 mass % as a conductive additive (Denka Black) in an amount of 2 mass %, and the above-mentioned nonaqueous electrolyte solution (i) in an amount of 18 mass % using a centrifugal planetary mixer (manufactured by Thinky Corporation, product name: Awatori Rentaro).

[0074] <Preparation of Slurry (b) for Forming Positive Electrode> LiFePO was used as the positive electrode active material. 4 A positive electrode forming slurry (b) was obtained in the same manner as in the preparation of the positive electrode forming slurry (a), except that lithium nickel manganese cobalt oxide (NMC) was used instead of the above.

[0075] <Preparation of Positive Electrode-Forming Slurry (c)> A positive electrode-forming slurry (c) was obtained in the same manner as in the preparation of the positive electrode-forming slurry (a), except that the content of the positive electrode active material was 78 mass % and the content of the nonaqueous electrolyte solution (i) was 20 mass %.

[0076] <Preparation of positive electrode-forming slurry (d)> A positive electrode-forming slurry (d) was obtained in the same manner as in the preparation of the positive electrode-forming slurry (a), except that the content of the positive electrode active material was 82 mass % and the content of the nonaqueous electrolyte solution (i) was 16 mass %.

[0077] <Preparation of Positive Electrode-Forming Slurry (e)> A positive electrode-forming slurry (e) was obtained in the same manner as in the preparation of the positive electrode-forming slurry (a), except that the nonaqueous electrolyte solution (ii) was used instead of the nonaqueous electrolyte solution (i).

[0078] <Preparation of positive electrode-forming slurry (f)> A positive electrode-forming slurry (f) was obtained in the same manner as in the preparation of the positive electrode-forming slurry (e), except that the content of the positive electrode active material was 65% by mass and the content of the nonaqueous electrolyte solution (ii) was 33% by mass.

[0079] Test Example 1: Disintegration Test of Slurry Positive Electrode Active Material Layer The positive electrode-forming slurry was applied to a horizontally placed aluminum current collector so as to form a square having a thickness of 300 μm and a planar size of 4 cm × 4 cm, thereby producing a positive electrode consisting of the aluminum current collector and the slurry positive electrode active material layer. At this time, the area of ​​the slurry positive electrode active material layer was 4 cm × 4 cm = 16 cm 2 The positive electrode was placed on a horizontally placed adsorption plate so that the aluminum current collector was in contact with the positive electrode, and with the positive electrode fixed by adsorption, the adsorption plate was rotated 90° so that the surface direction of the slurry positive electrode active material layer (the two opposing sides of the square) was in the vertical direction (the direction of gravity). After maintaining this state for 1 minute, the adsorption plate was returned to the horizontal position, and the area of ​​the slurry positive electrode active material layer was measured. 2was measured. The area change rate was calculated using the formula below, and the calculated value was applied to the evaluation criteria below to evaluate the disintegration properties of the slurry positive electrode active material layer. The results are shown in the table below. In the formula below, the value between two "|"s is an absolute value. When the slurry positive electrode active material layer disintegrates, part of it hangs down in the vertical direction, increasing the area of ​​the slurry positive electrode active material layer, or the hanging part of the slurry positive electrode active material layer falls, causing defects in the slurry positive electrode active material layer, resulting in an increased area change rate. Area change rate (%) = [| (area X cm 2 -16cm 2 ) | / 16 cm 2 ] x 100 - Evaluation criteria - A: Less than 0.5% B: 0.5% or more and less than 1.0% C: 1.0% or more and less than 2.0% D: 2.0% or more and less than 3.0% E: 3.0% or more and less than 4.0% F: 4.0% or more and less than 5.0% G: 5.0% or more

[0080] [Preparation of Slurry for Forming Negative Electrode] 64 mass % of artificial graphite (UF-G30 manufactured by Showa Denko K.K.) as a negative electrode active material, 1 mass % of acetylene black (Denka Black manufactured by Denka Co., Ltd.) as a conductive additive, and 35 mass % of the nonaqueous electrolyte solution (i) were uniformly mixed using a centrifugal planetary mixer (manufactured by Thinky Corporation, product name: Awatori Rentaro) to obtain a slurry for forming a negative electrode.

[0081] [Surface treatment of separator] <Ceramic coating treatment> Al 2 O 3 A solution containing 5% by mass of the above, 0.5% by mass of styrene-butadiene rubber (SBR), and 94.5% by mass of ethanol was prepared, and this solution was applied to the entire surface of a polyethylene (PE) separator having a porosity of 45% and a thickness of 20 μm, followed by drying at 70° C. to obtain a separator with a ceramic-coated surface.

[0082] <Surfactant Treatment> A solution containing 1 mass % of polyoxyethylene alkyl ether (trade name: LEOCOL SC-50, manufactured by Lion Specialty Chemicals) and 99 mass % of ethanol was prepared, and this solution was applied to the entire surface of a PE separator having a porosity of 45% and a thickness of 20 μm, followed by drying at 70° C. to obtain a separator whose surface was treated with a surfactant.

[0083] <Method for measuring the contact angle of the additive solvent on the separator> The contact angle of the additive solvent on the separator was measured at 25°C by static contact angle measurement. A DMs-301 manufactured by Kyowa Interface Science Co., Ltd. was used as a contact angle meter. A 2 μL droplet of the additive solvent filled in a syringe was discharged and dropped onto a separator placed on the stage of the contact angle meter, and an image was taken from the side 5 seconds after the drop, and the angle between the droplet and the separator was measured to determine the contact angle.

[0084] [Fabrication of Nonaqueous Electrolyte Secondary Battery (Quasi-Solid Secondary Battery)] The positive electrode-forming slurry shown in the table below was applied to a thickness of 300 μm on an aluminum current collector measuring 8 cm in length and 5 cm in width to form a slurry positive electrode active material layer, thereby obtaining a positive electrode. The negative electrode-forming slurry prepared above was also applied to a copper current collector measuring 8 cm in length and 5 cm in width to a thickness of 300 μm to form a slurry negative electrode active material layer, thereby obtaining a negative electrode. A separator was then placed on the negative electrode slurry active material layer in contact with the negative electrode slurry active material layer, and a specific amount of the "additive solvent" shown in the table below was then added to the separator. Next, a positive electrode was placed on the separator so that the slurry positive electrode active material layer was in contact with the side of the separator opposite the slurry negative electrode active material layer. An aluminum tab was attached to the end of the aluminum current collector, and a nickel tab was attached to the end of the copper current collector by ultrasonic welding, respectively, to form an electrode group. This electrode group was sandwiched between two aluminum laminate films, three sides were heat-sealed, and the remaining side was vacuum-sealed to produce a laminated battery. In this way, each of the quasi-solid secondary batteries of Examples 1 to 11, Comparative Examples 1 to 3, and Reference Example was obtained.

[0085] Test Example 2: Battery Performance Test <Discharge Capacity Retention Rate> This laminate battery was initialized by charging under the following charging conditions and then discharging under the following discharging conditions. During this initialization, the initial discharge capacity was 100 mAh. Next, the battery was charged under the following test charging conditions and then discharged under the following test discharging conditions to measure the discharge capacity YmAh. The discharge capacity retention rate was calculated using the following formula, and the calculated value was applied to the following evaluation criteria to evaluate the battery performance. The results are shown in the table below. (Charging conditions) CC-CV charging: current value 10mA, upper limit voltage 3.6V, final current value 0.5mA (Discharging conditions) CC discharging: current value 10mA, upper limit voltage 2.0V (Test charging conditions) CC-CV charging: current value 10mA, upper limit voltage 3.6V, final current value 0.5mA (Test discharging conditions) CC discharging: current value 100mA, upper limit voltage 2.0V Discharge capacity retention rate (%) = (YmAh / 100mAh) x 100 - Evaluation criteria - A: 90% or more B: 85% or more and less than 90% C: 80% or more and less than 85% D: 75% or more and less than 80% E: 70% or more and less than 75% F: Less than 70%

[0086] <Volumetric energy density> After initializing each of the fabricated quasi-solid secondary batteries as described above, the discharge energy (Wh) was calculated from the discharge capacity (Ah) at 0.1 C (10 mA) and the average voltage (V). In addition, the total thickness (m) of the laminate consisting of the positive electrode current collector, the slurry positive electrode active material layer, the separator, the slurry negative electrode active material layer, and the negative electrode current collector, and the positive electrode area (m 2 ) and the volume (L) of the laminate (power generating element) was calculated. The volumetric energy density was calculated as discharge energy (Wh) / volume (L) of the power generating element, and evaluated according to the following evaluation criteria. -Evaluation criteria- A: 400 Wh / L or more B: 390 Wh / L or more and less than 400 Wh / L C: 380 Wh / L or more and less than 390 Wh / L D: 370 Wh / L or more and less than 380 Wh / L E: 360 Wh / L or more and less than 370 Wh / L F: Less than 360 Wh / L

[0087]

[0088] As shown in the table above, when a solvent with a vapor pressure of 4.0 kPa or more was added to the positive electrode-forming slurry and a slurry-like positive electrode active material layer was formed using this slurry, the slurry-like positive electrode active material layer was prone to collapse, resulting in poor battery performance (Comparative Examples 1 and 3). Note that the collapse test evaluated the collapse property when the surface direction of the slurry-like positive electrode active material layer was vertical. However, when the collapse property was high in this collapse test, even when a battery was fabricated with the slurry-like positive electrode active material layer maintained horizontally, fine cracks and the like were likely to occur in the slurry-like positive electrode active material layer due to the evaporation of the solvent with a vapor pressure of 4.0 kPa or more. This is thought to have resulted in poor battery performance. Furthermore, when a solvent with a vapor pressure of 4.0 kPa or more was not added to the positive electrode-forming slurry and a solvent with a vapor pressure of 4.0 kPa or more was not added later, the formed slurry-like positive electrode active material layer was less prone to collapse, but the battery performance was poor (Comparative Example 2). This is thought to be due in part to the fact that the slurry positive electrode active material layer has a high positive electrode active material content, resulting in reduced fluidity and a resulting reduced ionic conductivity. In the reference example, a solvent with a vapor pressure of 4.0 kPa or more is added to the positive electrode-forming slurry, and the slurry positive electrode active material layer is formed using this slurry. However, the content of the positive electrode active material in the positive electrode-forming slurry is low, at 65 mass%. In this reference example, it can be seen that the formed slurry positive electrode active material layer is less likely to collapse. In other words, it can be seen that the problem of the collapse of the formed slurry positive electrode active material layer becomes more apparent when the slurry positive electrode active material layer contains a higher amount of positive electrode active material (when the slurry positive electrode active material layer is in a state closer to a powder). In the reference example, the volumetric energy density was inferior due to the small amount of positive electrode active material used. In contrast to these results, in the quasi-solid secondary batteries obtained by the manufacturing method of the present invention, the slurry positive electrode active material layer contained a higher amount of the positive electrode active material, but the formed slurry positive electrode active material layer was less likely to collapse and had excellent battery performance (Examples 1 to 11).

[0089] While the present invention has been described in connection with embodiments thereof, we do not intend to limit our invention to any of the details of the description unless otherwise specified, and believe that the claims should be construed broadly without departing from the spirit and scope of the invention as set forth in the appended claims.

[0090] This application claims priority based on Japanese Patent Application No. 2023-090135, filed in Japan on May 31, 2023, the contents of which are incorporated herein by reference.

[0091] REFERENCE SIGNS LIST 10 Non-aqueous electrolyte secondary battery 1 Negative electrode current collector 2 Negative electrode active material layer 3 Separator 4 Positive electrode active material layer 5 Positive electrode current collector 6 Operating part (light bulb)

Claims

1. A method for manufacturing a non-aqueous electrolyte secondary battery comprising stacking a positive electrode current collector, a positive electrode active material layer, a separator, a negative electrode active material layer, and a negative electrode current collector in this order, the method comprising: applying a positive electrode forming slurry onto the positive electrode current collector, the positive electrode forming slurry containing a positive electrode active material, a conductive assistant, an electrolyte, and a non-aqueous solvent (I) having a content of less than 1.0 mass% of a solvent having a vapor pressure of 4.0 kPa or more, and having a content of the positive electrode active material of 75 mass% or more, to form a slurry positive electrode active material layer; and adding a solvent having a vapor pressure of 4.0 kPa or more to the slurry positive electrode active material layer.

2. The method for producing a nonaqueous electrolyte secondary battery according to claim 1, wherein the content of the solvent having a vapor pressure of 4.0 kPa or more in the nonaqueous solvent (I) is less than 0.1 mass %.

3. The method for producing a nonaqueous electrolyte secondary battery according to claim 1 or 2, wherein the contact angle of the solvent having a vapor pressure of 4.0 kPa or more with respect to the separator is 45° or less.

4. A method for producing the non-aqueous electrolyte secondary battery according to claim 1 or 2, comprising forming a slurry for forming a negative electrode, the slurry containing a negative electrode active material, a conductive assistant, an electrolyte, and the non-aqueous solvent (I), on a negative electrode current collector to form a slurry negative electrode active material layer, and adding a solvent having a vapor pressure of 4.0 kPa or more to the slurry negative electrode active material layer.

5. A nonaqueous electrolyte secondary battery obtained by the method for producing a nonaqueous electrolyte secondary battery according to claim 1 or 2.

Citation Information

Patent Citations

  • Rechargeable lithium-ion secondary battery

    JP2005108835A

  • Nonaqueous secondary battery

    JP2012185938A

  • Nonaqueous electrolyte and nonaqueous secondary battery

    JP2016201308A

  • Lithium-ion battery

    JP2017147222A

  • Method for manufacturing non-aqueous electrolyte secondary battery

    JP2019186009A

Cited By

  • Li ion product for accessible energy density optimization

    US20250239602A1