Composition for positive electrodes of nonaqueous electrolyte secondary batteries, positive electrode sheet, and nonaqueous electrolyte secondary battery
The use of a specific particle size distribution and surface tension range in the positive electrode composition for non-aqueous electrolyte secondary batteries addresses the challenge of achieving high energy density and shape stability, enhancing battery performance by maintaining the integrity of the active material layer.
Patent Information
- Application Number
- PCT/JP2024/018890
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-31
- Filing Date
- 2024-05-22
- Publication Date
- 2024-12-05
AI Technical Summary
Non-aqueous electrolyte secondary batteries face challenges in forming a positive electrode active material layer with high energy density and shape stability, particularly when reducing binder content or increasing the thickness of the active material layer, which can lead to collapse and poor battery performance.
A positive electrode composition using a combination of large and small particle groups with specific particle size distributions and surface tensions, where the large particles have a size of 5.0 μm or more and small particles less than 5.0 μm, with a frequency distribution of 60% or more for large particles and 40% or less for small particles, and surface tensions within defined ranges, to enhance interparticle interaction and shape stability.
The composition allows for the formation of a positive electrode active material layer with excellent shape stability and increased battery capacity, even with reduced binder content or thicker layers, resulting in improved non-aqueous electrolyte secondary battery performance.
Smart Images

Figure JP2024018890_05122024_PF_FP_ABST
Abstract
Description
Positive electrode composition for non-aqueous electrolyte secondary battery, positive electrode sheet, and non-aqueous electrolyte secondary battery
[0001] The present invention relates to a composition for a positive electrode of a non-aqueous electrolyte secondary battery, a positive electrode sheet using the composition, and a non-aqueous electrolyte secondary battery using the positive electrode sheet.
[0002] Non-aqueous electrolyte secondary batteries, typified by lithium-ion secondary batteries, have high energy density and excellent storage performance, low-temperature operation, etc., and are widely used in portable electronic devices such as mobile phones and laptop computers. Furthermore, larger batteries are being used in transportation equipment such as automobiles, and their use as storage devices for nighttime electricity and electricity generated by natural energy sources is also progressing.
[0003] The electrodes (positive and negative electrodes) of non-aqueous electrolyte secondary batteries generally have an electrode active material layer (positive electrode active material layer or negative electrode active material layer), which contains electrode active material particles capable of absorbing or releasing lithium ions during charge and discharge. The electrode active material layer is usually formed by preparing, coating, and drying a slurry (composition) containing constituent components of the electrode active material layer, such as the electrode active material. Regarding improving the performance of non-aqueous electrolyte secondary batteries, studies have been conducted focusing on the positive electrode active material layer.
[0004] For example, Patent Document 1 discloses a method for manufacturing an electrode for a lithium ion secondary battery, the method comprising: preparing first composite particles containing a first active material and a first binder; and second composite particles having higher fluidity than the first composite particles and containing a second active material and a second binder; providing a strip-shaped current collector on at least one end of a long current collector along its longitudinal direction, and supplying the first composite particles to a first portion, which is a strip-shaped region adjacent to the current collector; supplying the second composite particles to a second portion, which is a region closer to the center of the current collector in a width direction perpendicular to the longitudinal direction than the first portion; and rolling the first and second composite particles supplied onto the current collector to form an active material layer. In the examples, the method evaluates a positive electrode sheet having a positive electrode active material layer formed by the above manufacturing method. The technology of Patent Document 1 is said to enable the manufacture of an electrode while suppressing peeling or sliding of the active material layer.
[0005] Patent Document 2 also discloses a nonaqueous electrolyte storage element including a positive electrode having a conductive substrate and a positive electrode composite layer laminated on the substrate, wherein the substrate is formed from an aluminum alloy containing 1% by mass or more of elements other than aluminum, the positive electrode composite layer contains particles A and B having different particle sizes as a positive electrode active material, the particle size ratio (A / B) of the particle A to the particle B is 3 or more, and the substrate has a tensile break strength of 250 MPa or more. The technology in Patent Document 2 is said to be able to suppress an increase in resistance due to repeated charging and discharging.
[0006] JP 2015-230748 A International Publication No. 2018 / 155314
[0007] In recent years, as the applications of non-aqueous electrolyte secondary batteries have expanded, there has been a demand for non-aqueous electrolyte secondary batteries with higher energy densities (higher capacities). For example, non-aqueous electrolyte secondary batteries are used as power sources for electric vehicles (EVs) and drones, and increasing the capacity of non-aqueous electrolyte secondary batteries is important for improving the driving range of EVs and the flight time of drones. In order to increase the capacity (higher energy density) of non-aqueous electrolyte secondary batteries, there have been attempts to increase the content of positive electrode active material that stores ions in the positive electrode active material layer and, conversely, reduce the content of binder. However, if the amount of the binder added in the positive electrode composition used to form the positive electrode active material layer or in the positive electrode active material layer is reduced, or if the positive electrode composition is applied thickly to form a thick positive electrode active material layer, there is a problem that, during the manufacturing process of the nonaqueous electrolyte secondary battery, the edge of the formed positive electrode active material layer partially collapses, making it difficult to form a positive electrode active material layer having a desired shape (for example, a rectangular cross section).
[0008] An object of the present invention is to provide a positive electrode composition that has excellent formability (shape stability) of a positive electrode active material layer and can provide a nonaqueous electrolyte secondary battery that exhibits excellent battery performance. Another object of the present invention is to provide a positive electrode sheet having a positive electrode active material layer formed using the positive electrode composition, and a nonaqueous electrolyte secondary battery in which the positive electrode sheet is incorporated into a positive electrode.
[0009] In view of the above-mentioned problems, the present inventors have conducted extensive research and found that, when a cathode active material having a specific particle size distribution is used as the cathode active material contained in a cathode composition for forming a cathode active material layer and the surface tension of a specific small particle cathode active material is increased within a specific range, collapse of the resulting cathode active material layer can be suppressed, even if the amount of binder in the cathode composition or the cathode active material layer is reduced or the cathode active material layer is formed thick, and a cathode active material layer having a desired shape can be efficiently formed, and further, a higher capacity can be achieved for the resulting nonaqueous electrolyte secondary battery. The present invention was completed through further research based on this finding.
[0010] The above-described problems of the present invention have been solved by the following means. [1] A positive electrode composition for a non-aqueous electrolyte secondary battery, comprising a positive electrode active material composed of a large particle group A having a particle size of 5.0 μm or more and a small particle group B having a particle size of less than 5.0 μm, wherein, when the total frequency in a number-based particle size distribution of the positive electrode active material is taken as 100%, the frequency of the large particle group A is 60% or more and the frequency of the small particle group B is 40% or less, and the surface tension γB (mN / m) of the small particle group B with N-methylpyrrolidone satisfies the following formula B1: Formula B1: 15.0≦γB≦40.0 [2] The positive electrode composition according to [1], wherein the surface tension γA (mN / m) of the large particle group A with N-methylpyrrolidone satisfies the following formula A1: Formula A1: 15.0≦γA≦25.0 [3] The positive electrode composition according to [1] or [2], wherein the surface tension γA of the large particle group A satisfies the following formula A2: Formula A2: 18.0≦γA≦22.0 [4] The positive electrode composition according to any one of [1] to [3], wherein the surface tension γB of the small particle group B satisfies the following formula B2: Formula B2: 25.0≦γB≦35.0 [5] The positive electrode composition according to any one of [1] to [4], wherein the close packing ratio calculated from the volume-based cumulative particle size distribution of the positive electrode active material is 80% or more. [6] A positive electrode sheet having a positive electrode active material layer formed using the positive electrode composition according to any one of [1] to [5]. [7] A nonaqueous electrolyte secondary battery having the positive electrode sheet according to [6] as a positive electrode.
[0011] In the description of the present invention, a numerical range expressed using "to" means a range including the numerical values written before and after "to" as the lower and upper limits. In the present invention, "non-aqueous electrolyte" means an electrolyte that does not substantially contain water. In other words, the "non-aqueous electrolyte" may contain a small amount of water within a range that does not impair the effects of the present invention. In the present invention, the "non-aqueous electrolyte" has a water concentration of 200 ppm (by mass) or less, preferably 100 ppm or less, and more preferably 20 ppm or less. Note that it is practically difficult to make a non-aqueous electrolyte completely anhydrous, and it usually contains 1 ppm or more of water. In the present invention, "non-aqueous solvent" also means a solvent that does not substantially contain water. In other words, the "non-aqueous solvent" may contain a small amount of water within a range that does not impair the effects of the present invention. In the present invention, the "non-aqueous solvent" has a water concentration of 200 ppm (by mass) or less, preferably 100 ppm or less, and more preferably 20 ppm or less. In reality, it is difficult to make a non-aqueous solvent completely free of water, and it usually contains 1 ppm or more of water.
[0012] The positive electrode composition for a nonaqueous electrolyte secondary battery of the present invention can be used to form a positive electrode active material layer that is less likely to collapse. The positive electrode sheet of the present invention has excellent shape stability of the positive electrode active material layer, and by incorporating this as the positive electrode of a nonaqueous electrolyte secondary battery, a nonaqueous electrolyte secondary battery that exhibits excellent battery performance can be obtained. The nonaqueous electrolyte secondary battery of the present invention has excellent shape stability of the positive electrode active material layer and also excellent battery performance.
[0013] FIG. 1 is a longitudinal sectional view showing a schematic diagram of a basic layer structure of an embodiment of a secondary battery according to the present invention.
[0014] Although preferred embodiments of the present invention will be described, the present invention is not limited to these embodiments except as defined in the present invention.
[0015] [Positive Electrode Composition] The positive electrode composition for a nonaqueous electrolyte secondary battery of the present invention (hereinafter also referred to as the "positive electrode composition of the present invention") includes a positive electrode active material composed of a large particle group A having a particle size of 5.0 μm or more and a small particle group B having a particle size of less than 5.0 μm. In this positive electrode active material, when the total frequency in the number-based particle size distribution of the positive electrode active material is taken as 100%, the frequency of the large particle group A is 60% or more and the frequency of the small particle group B is 40% or less, and the surface tension γB (mN / m) of the small particle group B with respect to N-methylpyrrolidone satisfies the following formula B1: Formula B1: 15.0≦γB≦40.0 The positive electrode composition of the present invention can be suitably used as a material for forming a positive electrode active material layer constituting a nonaqueous electrolyte secondary battery. The positive electrode composition of the present invention is typically a slurry in which solid particles such as a positive electrode active material and a conductive additive are dispersed in a liquid medium.
[0016] In the positive electrode composition of the present invention, the positive electrode active material comprises a large particle group A and a small particle group B, and the surface tension of the small particle group B is controlled within the above range, thereby enhancing the surface activity of the small particle group B and effectively enhancing the interaction (adhesion) between the solid particles and with the binder. As a result, even if the thickness of the formed positive electrode active material layer is set to about 250 μm or the amount of binder used is reduced, the formed positive electrode active material layer has excellent shape stability, and the battery capacity of the obtained nonaqueous electrolyte secondary battery can be sufficiently increased.
[0017] The positive electrode active material constituting the positive electrode composition of the present invention is composed of a large particle group A having a particle size of 5.0 μm or more and a small particle group B having a particle size of less than 5.0 μm. That is, the positive electrode active material used in the present invention is roughly divided into a large particle group having a particle size including the threshold particle size of 5.0 μm and a particle group having a particle size smaller than this threshold particle size. The particle size can be measured using a particle size measuring device in accordance with the method for measuring number-based particle size distribution described below.
[0018] When the total frequency (total particle number of positive electrode active material particles) in the number-based particle size distribution of the positive electrode active material is taken as 100%, the frequency of large particle group A (the number of particles of positive electrode active material classified as large particle group A) is preferably 60 to 90%, more preferably 60 to 80%, and even more preferably 65 to 75%. When the total frequency (total particle number of positive electrode active material particles) in the number-based particle size distribution of the positive electrode active material is taken as 100%, the frequency of small particle group B (the number of particles of positive electrode active material classified as small particle group B) is preferably 10 to 40%, more preferably 20 to 40%, and even more preferably 25 to 35%. The method for controlling the frequency of large particle group A and small particle group B in the positive electrode active material as described above is not particularly limited, and can be controlled, for example, by mixing and using positive electrode active materials with different median diameters. The number-based particle size distribution of the positive electrode active material can be obtained by the method described in the examples.
[0019] In the positive electrode active material contained in the positive electrode composition of the present invention, the surface tension of the small particle group B with respect to N-methylpyrrolidone (NMP) is controlled to satisfy the formula B1: 15.0≦γB≦40.0. If the surface tension γB is too low, the interaction between the small particle group B particles and the binder cannot be increased to the desired level, and the formed positive electrode active material layer becomes prone to collapse. On the other hand, if the surface tension γB is too high, the formed positive electrode active material layer becomes powdery and also tends to collapse. The surface tension γB of the small particle group B with respect to N-methylpyrrolidone preferably satisfies the following formula B2, and more preferably satisfies formula B3. Formula B2: 25.0≦γB≦35.0 Formula B3: 28.0≦γB≦34.0 The surface tension (surface free energy) of the small particle group B with respect to NMP means the surface tension of the small particle group B as a whole with respect to NMP, and can be measured by a penetration velocity method. In the present invention, the surface tension of the small particle group B with respect to NMP is specified, but the dispersion medium used in the positive electrode composition of the present invention is not limited to NMP, and various dispersion mediums described below can be used. The method for measuring the surface tension of the positive electrode active material is described in detail below.
[0020] -Method for measuring the surface tension of the positive electrode active material-Measurements are carried out using a surface tensiometer (device name DY-700 (product name), manufactured by Kyowa Interface Science Co., Ltd.) and a powder contact angle measurement kit. 2.0 g of the positive electrode active material powder is placed in a container with an inner diameter of 1 cm (cross-sectional area S: 0.785 cm 2 The powder is packed into a cylinder of 1.5 cm diameter, and compressed to a height of 1.5 cm using a cylindrical rod having the same diameter as the inner diameter of the cylinder. The cylinder is set on the powder contact angle measurement kit, and hexadecane is allowed to penetrate the powder in the cylinder for 5 minutes (time t = 5 minutes (300 seconds)), and the penetration weight W L (g) was measured, and W L 2 / t is calculated. L 2 / t is the liquid density ρ of hexadecane L , liquid surface tension γ L , and liquid viscosity η L , and cosθ=1 into the Washburn equation below, and the constant ε 2 Determine r (in the Washburn formula, the unit of r is "m" and the porosity ε is a value in the range of 0.0 to 1.0). Liquid density ρ of hexadecane L , liquid surface tension γ L , and liquid viscosity η L The following constants are used based on literature values: Hexadecane: ρ L =0.775g / ml, γ L =27.6mN / m, η L = 3.5 mPa·s
[0021]
[0022] Next, the penetration weight W was measured in the same manner as above, except that NMP solvent was used instead of hexadecane. L (g) was measured, and W was calculated from the actual weight and the penetration time. L 2 / t and the ε obtained above 2 r is the ρ of NMP as follows: L , γ L , and η L and then substituted into the Washburn equation to derive the contact angle cos θ of the positive electrode active material with respect to NMP. L=1.03g / ml, γ L =40.3mN / m, η L The above operation (measurement of the penetration weight) is carried out four times (N=4) to obtain the average value of the contact angle cos θ with respect to NMP. The obtained contact angle cos θ can be substituted into the following formula to obtain the surface tension γB. γB = γ NMP ×cosθ where γ NMP is the surface tension of N-methylpyrrolidone (40.3 mN / m), and this surface tension is a constant.
[0023] The surface tension of the small particle group B with respect to the NMP can be controlled by previously subjecting a positive electrode active material classified as at least the small particle group B to a surface smoothing treatment and then blending the surface smoothing treatment into a positive electrode composition. Examples of this surface smoothing treatment include mixing. The atmosphere during the surface smoothing treatment is not particularly limited, and from the viewpoint of preventing oxidation of the active material particle surface during treatment, it is preferable to carry out the surface smoothing treatment in an inert gas atmosphere. For example, mixing can be carried out in an argon atmosphere, a nitrogen atmosphere, a nitrogen-hydrogen mixed atmosphere, or the like. The treatment device used in the surface smoothing treatment is not particularly limited, and examples thereof include a planetary ball mill (trade name: P-5, manufactured by Fritsch), a jet mill pulverizer (trade name: JETMILL100, manufactured by Powrex Corporation), a powder treatment device Nobilta (trade name: NOB MINI, manufactured by Hosokawa Micron Corporation), and a powder treatment device Composite (trade name: CP15, manufactured by Nippon Coke and Engineering Co., Ltd.). The treatment conditions for the surface smoothing treatment are not particularly limited, and for example, mixing can be performed using a powder treatment device Nobilta (product name: NOB MINI, manufactured by Hosokawa Micron Corporation) in a nitrogen atmosphere at a rotation speed of 5,000 to 9,000 rpm for a treatment time of 5 to 20 minutes. As a result of the surface smoothing treatment, a highly active surface is exposed on the surface of the positive electrode active material, and the surface tension is increased.
[0024] In the positive electrode composition of the present invention, the surface tension γA (mN / m) of the large particle group A with respect to N-methylpyrrolidone (NMP) preferably satisfies the following formula A0, preferably satisfies formula A1, and more preferably satisfies formula A2. Formula A0: 10.0≦γA≦25.0 Formula A1: 15.0≦γA≦25.0 Formula A2: 18.0≦γA≦22.0 In the present invention, the surface tension γB of the small particle group B is considered to have a greater influence on inter-particle interactions compared to the surface tension γA of the large particle group A due to its larger specific surface area. However, by setting the surface tension γB of the small particle group B in the above range and further setting the surface tension γA of the large particle group A in the above range, the effect can be further enhanced. The surface tension of the large particle group A with respect to NMP can be controlled to the above range by subjecting the large particle group A to a surface smoothing treatment, similar to that of the small particle group B. The surface smoothing treatment is the same as that described for the small particle group B. The surface tension γA of the large particle group A with respect to N-methylpyrrolidone (NMP) means the surface tension of the large particle group A as a whole with respect to NMP, and can be measured in the same manner as the surface tension γB of the small particle group B with respect to NMP.
[0025] In the positive electrode composition of the present invention, the close packing ratio of the positive electrode active material calculated from the volume-based cumulative particle size distribution of the positive electrode active material is preferably 75% or more, more preferably 80% or more. By controlling the particle size distribution of the positive electrode active material in this manner, the packing ratio of the positive electrode active material in the resulting positive electrode active material layer can be increased. This close packing ratio is an estimated value calculated based on data on the volume-based cumulative particle size distribution of the positive electrode active material contained in the positive electrode composition of the present invention. Specifically, the close packing ratio can be calculated by the method described in the examples of the present invention.
[0026] The specific surface area of the small particle group B is 8.0 to 13.0 m 2 / g, and 9.0 to 12.5 m 2 The specific surface area of the large particle group A is preferably 5.0 to 8.5 m / g. 2 / g, and 5.2 to 8.3 m 2 / g is more preferable. The specific surface area of each of the large particle group A and the small particle group B can be measured by the BET method as follows. -BET specific surface area measurement method- After drying 0.2 g of a sample at 120°C for 6 hours, measurement is performed using a BELSORP mini (trade name) manufactured by Microtrac under the following measurement conditions. Adsorption temperature: 77 K Adsorption gas: N 2 Equilibration time: 100 seconds Purge gas: He
[0027] As a method for producing the particle size distribution defined in the present invention, which is composed of large particle groups A and small particle groups B, a positive electrode active material having a large median diameter (D50) and a positive electrode active material having a small median diameter (D50) can be mixed and used as the positive electrode active material. The median diameter (D50) of the positive electrode active material having a large median diameter (D50) (positive electrode active material a, large particle group a) can be 6.0 to 20.0 μm, preferably 7.0 to 15.0 μm, more preferably 8.0 to 14.0 μm, and even more preferably 8.3 to 13.0 μm. The median diameter (D50) of the above-mentioned cathode active material (cathode active material b, small particle group b) having a small median diameter (D50) can be 0.1 to 4.0 μm, preferably 0.2 to 3.0 μm, more preferably 0.5 to 2.0 μm, and even more preferably 0.8 to 1.2 μm. To obtain the cathode active material a (large particle group a) and the cathode active material b (small particle group b) with a predetermined median diameter (D50), a conventional grinder or classifier can be used. The cathode active material obtained by the firing method may be used after washing with water, an acidic aqueous solution, an alkaline aqueous solution, or an organic solvent. The median diameter (D50) of the cathode active material a (large particle group a) and the cathode active material b (small particle group b) can be measured by the following method. -Method of measuring median diameter (D50)- The positive electrode active material is dispersed in water, and the particle diameter (volume-based median diameter D50 in water) obtained by measuring the particle diameter using a laser diffraction / scattering particle size distribution measuring device (for example, Particle LA-960V2 manufactured by HORIBA) is used. This also applies to the median diameter (D50) of solid particles other than the positive electrode active material.
[0028] The positive electrode composition of the present invention can contain the same components as those of a typical positive electrode composition, except that it contains a positive electrode active material composed of the large particle group A and the small particle group B. For example, it can contain a conductive additive, a binder, a dispersion medium, etc.
[0029] Each component constituting the positive electrode composition of the present invention will be described in more detail.
[0030] <Positive electrode active material> The positive electrode active material is preferably one that can reversibly insert and release lithium ions. There are no particular limitations on the material, and examples thereof include transition metal oxides, organic substances, sulfur, and other substances that can be composited with Li, as well as sulfur-metal composites. Among these, it is preferable to use lithium-containing transition metal oxides as the positive electrode active material, and transition metal element M a It is more preferable that the lithium-containing transition metal oxide contains at least one element selected from Co, Ni, Fe, Mn, Cu, and V. b (Elements of Group 1 (Ia) of the periodic table other than lithium, elements of Group 2 (IIa), Al, Ga, In, Ge, Sn, Pb, Sb, Bi, Si, P, B, etc.) may be mixed. The amount of the mixed element may be determined by the following formula: a The amount of Li / M is preferably 0 to 30 mol % relative to the amount of Li / M (100 mol %). a More preferably, the lithium-containing transition metal oxide is synthesized by mixing the above-mentioned components so that the molar ratio of the above-mentioned components is 0.3 to 2.2. Specific examples of the lithium-containing transition metal oxide include (MA) a lithium-containing transition metal oxide having a layered rock salt structure, (MB) a lithium-containing transition metal oxide having a spinel structure, (MC) a lithium-containing transition metal phosphate compound, (MD) a lithium-containing transition metal halide phosphate compound, and (ME) a lithium-containing transition metal silicate compound.
[0031] (MA) Specific examples of lithium-containing transition metal oxides having a layered rock salt structure include LiCoO 2 (Lithium cobalt oxide [LCO]), LiNi 2 O 2 (lithium nickel oxide), LiNi 0.85 Co 0.10 Al 0.05 O2 (nickel cobalt lithium aluminum oxide [NCA]), LiNi 1/3 Co 1/3 Mn 1/3 O 2 (Lithium nickel manganese cobalt oxide [NMC]) and LiNi 0.5 Mn 0.5 O 2 (Lithium manganese nickel oxide). (MB) Specific examples of lithium-containing transition metal oxides having a spinel structure include LiMn 2 O 4 (LMO), LiCoMnO 4 , Li 2 FeMn 3 O 8 , Li 2 CuMn 3 O 8 , Li 2 CrMn 3 O 8 and Li 2 NiMn 3 O 8 Examples of the (MC) lithium-containing transition metal phosphate compound include LiFePO 4 and Li 3 Fe 2 (P.O. 4 ) 3 Olivine-type iron phosphate salts such as LiFeP 2 O 7 Iron pyrophosphates such as LiCoPO 4 Cobalt phosphates such as Li 3 V 2 (P.O. 4 ) 3 (MD) Examples of lithium-containing transition metal halide phosphate compounds include, for example, Li 2 FePO 4 Fluorophosphate iron salts such as F, Li 2 MnPO 4 Fluorophosphate manganese salts such as F and Li 2 CoPO 4 Examples of the (ME) lithium-containing transition metal silicate compound include cobalt fluoride phosphates such as Li2 FeSiO 4 , Li 2 MnSiO 4 and Li 2 CoSiO 4 In the present invention, the positive electrode active material is preferably a lithium-containing transition metal oxide (MA) having a layered rock salt structure and a lithium-containing transition metal phosphate compound (MC), and LiNi 1/3 Co 1/3 Mn 1/3 O 2 and LiFePO 4 is more preferred, and LiFePO 4 is more preferred.
[0032] The chemical formula of the compound obtained by the above calcination method can be measured by inductively coupled plasma (ICP) emission spectroscopy, or simply calculated from the difference in mass of the powder before and after calcination.
[0033] The surface of the positive electrode active material may be coated with an oxide such as another metal oxide, a carbon-based material, or the like. These surface coating layers can function as an interface resistance stabilizing layer. Examples of surface coating materials include metal oxides containing Ti, Nb, Ta, W, Zr, Al, Si, or Li. Specific examples include titanate spinel, tantalum-based oxides, niobium-based oxides, and lithium niobate-based compounds, such as Li 4 Ti 5 O 12 , Li 2 Ti 2 O 5 , LiTaO 3 , LiNbO 3 , LiAlO 2 , Li 2 ZrO 3 , Li 2 WO 4 , Li 2 TiO 3 , Li 2 B 4 O 7 , Li 3 P.O. 4 , Li 2 MoO 4 , Li 3 BO 3 , LiBO2 , Li 2 CO 3 , Li 2 SiO 3 , SiO 2 , TiO 2 , ZrO 2 , Al 2 O 3 , B 2 O 3 , and Li 3 AlF 6 Carbon-based materials such as C, SiC, and SiOC (carbon-doped silicon oxide) can also be used as the surface coating material.
[0034] The positive electrode active material is preferably surface-coated with a carbonaceous material from the viewpoint of increasing the electronic conductivity to a desired level. In this case, the positive electrode active material is preferably surface-coated with carbon (C). The carbon surface coating can be formed by baking the positive electrode active material in the presence of an additive (organic substance) that serves as a carbon source. Examples of the additive that can be used include styrene-maleic anhydride copolymer, polystyrene, and polycarbonate.
[0035] The surface of the positive electrode active material may be treated with sulfur or phosphorus. Furthermore, the particle surfaces of the positive electrode active material may be treated with actinic rays or an active gas (plasma, etc.) before or after the surface coating.
[0036] The content of the positive electrode active material in the positive electrode composition is preferably 96.00 to 99.50% by mass, more preferably 96.00 to 99.40% by mass, still more preferably 97.00 to 99.40% by mass, still more preferably 98.00 to 99.30% by mass, still more preferably 98.50 to 99.20% by mass, and particularly preferably 99.00 to 99.15% by mass, based on the solid content of the composition.
[0037] <Conductive Aid> The positive electrode composition of the present invention may contain a conductive aid. As the conductive aid, a commonly known conductive aid may be used. For example, the conductive aid may be an electron-conductive material such as graphites (e.g., natural graphite, artificial graphite, etc.), carbon blacks (e.g., acetylene black, ketjen black, furnace black, etc.), amorphous carbon (e.g., needle coke), carbon fibers (e.g., vapor-grown carbon fibers or carbon nanotubes), carbonaceous materials (e.g., graphene or fullerene), metal powders (e.g., copper, nickel, etc.), or conductive polymers (e.g., polyaniline, polypyrrole, polythiophene, polyacetylene, or polyphenylene derivatives). In the present invention, the conductive aid is preferably a carbonaceous material, more preferably carbon blacks, and more preferably ketjen black. When a positive electrode active material and a conductive aid are used in combination, the conductive aid may be one of the above conductive aids that does not undergo Li insertion or release during charging and discharging of the battery and does not function as an active material. Therefore, among the conductive additives, those that can function as an active material in the active material layer when the battery is charged and discharged are classified as active materials rather than as conductive additives. Whether or not a conductive additive functions as an active material when the battery is charged and discharged is not uniquely determined, but is determined by the combination with the active material.
[0038] Examples of commercially available conductive additives include the following: Ketjen black: carbon ECP (specific surface area = 890 m 2 / g), carbon ECP600JD (specific surface area = 1480 m 2 / g), carbon ECP200L (specific surface area = 430 m 2 / g) (both manufactured by Lion Corporation), carbon black: LITX300 (specific surface area = 180 m 2 / g), LITX-HP (specific surface area = 100 m 2 / g) (both manufactured by CABOT Corporation) Carbon nanotubes (CNT): BT1001M (specific surface area = 272 m 2 / g), BT1003M (specific surface area = 230 m 2 / g) (both manufactured by LG), JENOTUBE6A (specific surface area = 680 m 2 / g), JENOTUBE10B (specific surface area = 230m2 / g) (both from JEIO)
[0039] The conductive additive may be used alone or in combination of two or more.
[0040] The shape of the conductive additive is not particularly limited, but is preferably particulate. The median diameter (D50) of the conductive additive is also not particularly limited. For example, it is preferably 0.01 to 50 μm, more preferably 0.1 to 10 μm, and even more preferably 0.2 to 2.0 μm.
[0041] The conductive additive may be surface-treated. The surface treatment method is not particularly limited, and preferred are surface treatment using a chemical treatment agent and atomic layer deposition (ALD) treatment. Preferred examples of the chemical treatment agent include organosilicon compounds (more preferably, silane coupling agents) and organic phosphonic acid compounds, such as methyltrimethoxysilane (MTMS), octadecyltrimethoxysilane, hexamethyldisilazane, tetraethoxysilane, trifluoropropyltrimethoxysilane, vinyltrimethoxysilane, phenyltrimethoxysilane, 3-aminopropyltriethoxysilane, 1H,1H,2H,2H-perfluorooctyltriethoxysilane, trimethoxy(octyl)silane, 1H,1H,2H,2H-perfluorooctanephosphonic acid, 1-octylphosphonic acid, and perfluoropolyethertriethoxysilane (KY1903 (trade name)). In the ALD process, the layer to be deposited is HfO 2 , SiO 2 , ZrO 2 , Ta 2 O 5 , TiO 2 The following can be mentioned:
[0042] The content (mass %) of the conductive additive is preferably 0.03 to 4.00 mass %, more preferably 0.03 to 2.00 mass %, still more preferably 0.05 to 1.00 mass %, and particularly preferably 0.10 to 0.80 mass %, of the solid content of the positive electrode composition.
[0043] <Dispersion Medium> The positive electrode composition of the present invention may contain a dispersion medium. The dispersion medium is not particularly limited. For example, it may be water or a non-aqueous solvent. As the non-aqueous solvent, an aprotic organic solvent is preferred, and an aprotic organic solvent having 2 to 10 carbon atoms is more preferred. Examples of such non-aqueous solvents include linear or cyclic carbonate compounds, lactone compounds, linear or cyclic ether compounds, ester compounds, nitrile compounds, amide compounds, oxazolidinone compounds, nitro compounds, linear or cyclic sulfone or sulfoxide compounds, and phosphate ester compounds. Compounds having an ether bond, carbonyl bond, ester bond, or carbonate bond are preferred. These compounds may have a substituent.
[0044] Examples of non-aqueous solvents include ethylene carbonate, fluorinated ethylene carbonate, vinylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, γ-butyrolactone, γ-valerolactone, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, tetrahydropyran, 1,3-dioxolane, 4-methyl-1,3-dioxolane, 1,3-dioxane, 1,4-dioxane, and methyl acetate. , ethyl acetate, methyl propionate, ethyl propionate, methyl butyrate, methyl isobutyrate, methyl trimethylacetate, ethyl trimethylacetate, acetonitrile, glutaronitrile, adiponitrile, methoxyacetonitrile, 3-methoxypropionitrile, N,N-dimethylformamide, N-methylpyrrolidone (NMP), N-methyloxazolidinone, N,N'-dimethylimidazolidinone, nitromethane, nitroethane, sulfolane, trimethyl phosphate, dimethyl sulfoxide, dimethyl sulfoxide phosphate, and the like. These may be used alone or in combination of two or more. However, the nonaqueous solvent used in the present invention is not limited to these. In the present invention, the dispersion medium is preferably N-methylpyrrolidone (NMP).
[0045] The positive electrode composition of the present invention preferably has a solids content (components other than the dispersion medium (solvent)) of 70% by mass or more, more preferably 72% by mass or more, even more preferably 74% by mass or more, and even more preferably 78% by mass or more. The solids content is preferably 70 to 95% by mass, more preferably 70 to 90% by mass, even more preferably 72 to 87% by mass, even more preferably 74 to 85% by mass, and particularly preferably 78 to 83% by mass.
[0046] <Other Components> The positive electrode composition of the present invention may contain, as desired, a binder, an ionic liquid, a thickener, an antifoaming agent, a leveling agent, a dehydrating agent, an antioxidant, and the like. These may be those typically used in nonaqueous electrolyte secondary batteries. Preferred binders are polyvinylene difluoride (PVDF) and styrene-butadiene copolymer (SBR). The content of the binder in the positive electrode composition of the present invention is preferably 0.10 to 3.00 mass%, more preferably 0.20 to 2.00 mass%, even more preferably 0.20 to 1.00 mass%, and particularly preferably 0.25 to 0.40 mass%, based on the solid content of the positive electrode composition.
[0047] <Method for preparing a positive electrode composition> The positive electrode composition of the present invention can be prepared as a mixture, preferably as a slurry, by mixing a positive electrode active material consisting of a large particle group A and a small particle group B with other optional components, for example, using any of various commonly used mixers.
[0048] [Positive Electrode Sheet] The positive electrode sheet of the present invention is a positive electrode sheet having a positive electrode active material layer formed using the positive electrode composition of the present invention, and is a positive electrode sheet suitable as a positive electrode sheet for a nonaqueous electrolyte secondary battery. In the positive electrode sheet of the present invention, the positive electrode active material contained in the positive electrode active material layer comprises a large particle group A having a particle size of 5.0 μm or more and a small particle group B having a particle size of less than 5.0 μm, and when the total frequency in the number-based particle size distribution of the positive electrode active material is 100%, the frequency of the large particle group A is 60% or more and the frequency of the small particle group B is 40% or less, and the surface tension γB (mN / m) of the small particle group B with respect to N-methylpyrrolidone satisfies the above formula B1.
[0049] In the present invention, the term "cathode sheet" refers to both a cathode sheet incorporated as a component of a nonaqueous electrolyte secondary battery (incorporated into the secondary battery) and a cathode sheet in the form of a cathode material prior to incorporation into the nonaqueous electrolyte secondary battery. That is, the structure (area, thickness, etc.) of the cathode sheet may be a structure used as a cathode or a structure that can be processed into a structure used as a cathode. The cathode sheet of the present invention may have a cathode active material layer formed using the cathode composition of the present invention, and may be in a form in which the cathode active material layer and a cathode current collector are laminated. More specifically, the cathode active material layer may be laminated on both sides of the cathode current collector, or on one side of the cathode current collector. The cathode sheet is typically a sheet configured by laminating a cathode active material layer on a cathode current collector. The cathode active material layer may be composed of a single layer or multiple layers. The cathode sheet may further include other layers as needed. Examples of other layers include a protective layer (release sheet) and a coating layer. In the positive electrode sheet of the present invention, the positive electrode active material layer is preferably laminated in a state of being in direct contact with the positive electrode current collector.
[0050] The thickness of the positive electrode active material layer is preferably 120 μm or more, and can be set to 120 to 500 μm, preferably 150 to 450 μm, more preferably 180 to 400 μm, and even more preferably 200 to 350 μm.
[0051] When the positive electrode sheet of the present invention has a positive electrode current collector, the positive electrode current collector constituting the positive electrode sheet of the present invention is not particularly limited, and a positive electrode current collector used in a typical secondary battery can be appropriately applied. For the positive electrode current collector typically used in these secondary batteries, reference can be made, for example, to JP 2016-201308 A, JP 2005-108835 A, JP 2012-185938 A, WO 2018 / 135395, etc. As the positive electrode current collector, aluminum, an aluminum alloy, etc. are preferred.
[0052] In the positive electrode sheet of the present invention, the positive electrode active material layer is less likely to collapse (peel off), and this collapse is usually more noticeable at the edges of the positive electrode active material layer.
[0053] In the positive electrode active material layer of the positive electrode sheet of the present invention, the binder is preferably unevenly distributed in contact with the small particle group B. Specifically, the binder uneven distribution rate is preferably 58% or more, more preferably 60% or more, even more preferably 70% or more, even more preferably 80% or more, and particularly preferably 85% or more. A practical upper limit for the binder uneven distribution rate is 99%. Therefore, the binder uneven distribution rate is preferably 58 to 99%, more preferably 60 to 98%, even more preferably 70 to 97%, even more preferably 80 to 96%, and particularly preferably 85 to 95%. The binder uneven distribution rate can be determined by measuring the element α derived from the binder in contact with the small particle group B in an element mapping image of a cross section of the positive electrode active material layer, quantifying the amount of α in contact with the small particle group B relative to the amount of element α in the entire element mapping image, and calculating the ratio ([amount of α in contact with the small particle group B] / [total amount of α] × 100 (%)). The uneven distribution of the binder is thought to occur when the binder moves to the periphery of the small particle group B during the drying step in forming the positive electrode active material layer. As a result of the uneven distribution of the binder, the bonds between the small particle group B become stronger, and it is thought that edge collapse can be suppressed to a higher level. The uneven distribution rate can be controlled by adjusting the surface tension, ratio, etc. of the large particle group A and the small particle group B.
[0054] The positive electrode sheet of the present invention can be obtained by forming a positive electrode active material layer using the positive electrode composition of the present invention. For example, the positive electrode sheet of the present invention can be produced by forming a film using the positive electrode composition of the present invention. More specifically, the positive electrode sheet can be prepared by forming the positive electrode active material layer on the positive electrode current collector or the like as a substrate. The positive electrode composition of the present invention is applied to the positive electrode current collector as a substrate (optionally via another layer) to form a coating film, which is then dried to obtain a positive electrode sheet having a positive electrode active material layer (coated and dried layer) on the substrate. The coating film may be subjected to a press treatment as necessary. The method for applying the positive electrode composition of the present invention to the positive electrode current collector is not particularly limited, and a conventional method can be used.
[0055] [Non-aqueous electrolyte secondary battery] The non-aqueous electrolyte secondary battery of the present invention (hereinafter also referred to as "secondary battery of the present invention") has the positive electrode sheet of the present invention as the positive electrode. The secondary battery of the present invention can have the same configuration as a conventional non-aqueous electrolyte secondary battery, except that it has the positive electrode sheet of the present invention as the positive electrode. That is, the secondary battery of the present invention can be obtained by incorporating the positive electrode sheet of the present invention as the positive electrode of a conventional non-aqueous electrolyte secondary battery.
[0056] The structure of a typical nonaqueous electrolyte secondary battery will be described below. FIG. 1 is a cross-sectional view showing a schematic representation of the laminated structure of a typical nonaqueous electrolyte secondary battery 10, including operating parts when the battery is in operation. The nonaqueous electrolyte secondary battery 10 has a laminated structure (hereinafter also referred to as an electrode laminate) including, as viewed from the negative electrode side, a negative electrode current collector 1, a negative electrode active material layer 2, a separator 3, a positive electrode active material layer 4, and a positive electrode current collector 5, in this order. The negative electrode active material layer 2, the positive electrode active material layer 4, and the space between them are filled with a nonaqueous electrolyte (not shown), and are separated by the separator 3. The separator 3 has pores, and during normal battery use, it functions as a separator between the positive and negative electrodes, allowing the electrolyte and ions to pass through the pores, thereby insulating the positive and negative electrodes. With this structure, for example, in the case of a lithium-ion secondary battery, electrons (e - ) is supplied, and at the same time, lithium ions (Li + ) moves and accumulates in the negative electrode. On the other hand, during discharge, the lithium ions (Li + ) is returned to the positive electrode side through the electrolyte, and electrons are supplied to the operating part 6. In the illustrated example, a light bulb is used as the operating part 6, and is turned on by discharge. The secondary battery of the present invention has the positive electrode sheet of the present invention instead of the positive electrode active material layer 4 and positive electrode current collector 5 of the above-mentioned general nonaqueous electrolyte secondary battery.
[0057] The secondary battery of the present invention is not particularly limited in terms of other components such as the negative electrode active material layer, negative electrode current collector, electrolyte (aqueous electrolyte, non-aqueous electrolyte) or solid electrolyte material, separator, etc., except that the positive electrode sheet of the present invention is used as the positive electrode of the secondary battery. These materials and components can be appropriately applied to those used in conventional secondary batteries. Furthermore, for the method of manufacturing the secondary battery of the present invention, conventional methods can be appropriately adopted, except that the positive electrode sheet of the present invention is used as the positive electrode. For the components and manufacturing methods typically used in these secondary batteries, reference can be made to, for example, JP 2016-201308 A, JP 2005-108835 A, JP 2012-185938 A, and WO 2020 / 067106 A.
[0058] The secondary battery of the present invention can be installed in electronic devices such as notebook computers, pen-input PCs, mobile PCs, electronic book players, mobile phones, cordless phone handsets, pagers, handheld terminals, portable fax machines, portable copiers, portable printers, headphone stereos, video camcorders, LCD televisions, handheld vacuum cleaners, portable CD players, mini-discs, electric shavers, transceivers, electronic organizers, calculators, memory cards, portable tape recorders, radios, backup power supplies, and memory cards. It can also be installed in consumer electronic devices such as automobiles, electric vehicles, motors, lighting fixtures, toys, game devices, road conditioners, clocks, flash devices, cameras, and medical devices (pacemakers, hearing aids, shoulder massagers, etc.). It can also be used for various military and space applications. It can also be combined with solar cells.
[0059] The present invention will be described in more detail below with reference to examples, but the present invention should not be construed as being limited thereto.
[0060] [Preparation of Positive Electrode Active Material] A positive electrode active material was prepared as follows.
[0061] <LFP1-1 to LFP1-3 (Large particle group a)> (LFP1-1) LFP (LiFePO 4) A powder raw material (P198-S13 (trade name), manufactured by LOPAL Corporation) was used. (LFP1-2 and LFP1-3) 20 g of LFP1-1 was placed in a powder processing device Nobilta (trade name: NOB MINI, manufactured by Hosokawa Micron Corporation), and surface smoothing treatment was performed in a nitrogen atmosphere at the rotation speed and for the treatment time shown in Table 1, to obtain powder-like positive electrode active materials LFP1-2 and LFP1-3, respectively.
[0062] <LFP2-1 to LFP2-6 (small particle group b)> (LFP2-1) LFP (LiFePO 4 ) A powder raw material (P198-T5 (trade name) manufactured by LOPAL) was used. (LFP2-2 to LFP2-6) 20 g of LFP2-1 was placed in a powder processing device Nobilta (trade name: NOB MINI, manufactured by Hosokawa Micron Corporation), and surface smoothing treatment was performed in a nitrogen atmosphere at the rotation speeds and for the treatment times shown in Table 1, to obtain powder-like positive electrode active materials LFP2-2 to LFP2-6, respectively.
[0063] <NMC1-1 to NMC1-3 (large particle group a)> (NMC1-1) NMC (LiNi 1/3 Co 1/3 Mn 1/3 O 2 ) A powder raw material (NCM111 (particle size 12 μm) (trade name) manufactured by Toshima Manufacturing Co., Ltd.) was used. (NMC1-2 and NMC1-3) 20 g of NMC1-1 was placed in a powder processing device Nobilta (trade name: NOB MINI, manufactured by Hosokawa Micron Corporation), and surface smoothing treatment was performed in a nitrogen atmosphere at the rotation speed and for the treatment time shown in Table 1, to obtain powder-like positive electrode active materials NMC1-2 and NMC1-3, respectively.
[0064] <NMC2-1 to NMC2-6 (small particle group b)> (NMC2-1) NMC (LiNi 1/3 Co 1/3 Mn 1/3 O 2) A powder raw material (NCM111 (particle size 2 μm) (trade name) manufactured by Toshima Manufacturing Co., Ltd.) was used. (NMC2-2 to NMC2-6) 20 g of NMC2-1 was placed in a powder processing device Nobilta (trade name: NOB MINI, manufactured by Hosokawa Micron Corporation), and surface smoothing treatment was performed in a nitrogen atmosphere at the rotation speeds and for the treatment times shown in Table 1, to obtain powder-like positive electrode active materials NMC2-2 to NMC2-6, respectively.
[0065] The number-based particle size distributions of LFP1-1 to LFP1-3 and NMC1-1 to NMC1-3 were obtained as described below, and each positive electrode active material contained substantially no particles with a particle size of less than 5.0 μm. The number-based particle size distributions of LFP2-1 to LFP2-6 and NMC2-1 to NMC2-6 were obtained as described below, and each positive electrode active material contained substantially no particles with a particle size of 5.0 μm or more.
[0066] (Method for Measuring Number-Based Particle Size Distribution) 0.01 g of each positive electrode active material was dispersed in ethanol to prepare a dispersion having a laser light (light with a wavelength of 650 nm) transmittance of 90% to 95%. The particle diameters (sphere-equivalent diameters) of all particles in the dispersion were measured using a particle size measuring device (LA-920 (trade name), manufactured by Horiba, Ltd.) to obtain number-based particle size distribution data (cumulative particle size distribution data).
[0067]
[0068] [Measurement of median diameter (D50)] The median diameter (D50) of the large particle group a and the small particle group b obtained above was determined as described above. The median diameter (D50) of the large particle group a and the small particle group b is shown in the "D50" column of Table 2.
[0069] [Measurement of Specific Surface Area] The specific surface areas of the large particle group a and the small particle group b obtained above were determined as described above. The specific surface areas of the large particle group a and the small particle group b are shown in the "Specific Surface Area" column of Table 2.
[0070] [Measurement of Surface Tension] The surface tensions of the large particle group a and the small particle group b obtained above with respect to NMP were determined as described above. The surface tensions of the large particle group a and the small particle group b are shown in the "Surface tension" column of Table 2.
[0071] [Preparation of Positive Electrode Composition and Positive Electrode Sheet] The positive electrode active material shown in Table 2, acetylene black (Li-100 (trade name), manufactured by Denka) as a conductive additive, polyvinylene difluoride (PVDF) as a binder, and N-methylpyrrolidone (NMP) as a dispersion medium were mixed to obtain positive electrode slurries (positive electrode compositions) (Nos. 1 to 24) in a concentration of 79.3% by mass of the positive electrode active material, 0.4% by mass of the conductive additive, 0.3% by mass of the binder, and 20.0% by mass of the dispersion medium. The positive electrode active material used to prepare the positive electrode slurries of Experiments Nos. 2 to 4, 6 to 12, 14 to 16, and 18 to 24 was a mixture of the large particle group a and the small particle group b, in which the large particle group A and the small particle group B had the number frequencies shown in Table 2. The positive electrode slurry was applied to one side of a 12 μm-thick positive electrode current collector (aluminum foil) (length: 200 mm, width: 150 mm) and dried at 120°C until the dispersion medium evaporated. Then, the positive electrode current collector was pressed using a roll press to obtain sheet-shaped positive electrode sheets (Nos. 1 to 24) each containing a positive electrode current collector and a positive electrode active material. Each positive electrode active material layer had a thickness of 250 μm.
[0072] [Method for Evaluating Closest Packing Ratio] A dispersion was prepared by dispersing 0.01 g of a positive electrode active material powder composed of large particle group A and small particle group B in the ratios shown in Table 2 in ethanol so as to have a laser light (light having a wavelength of 650 nm) transmittance of 90% to 95%. The particle diameters (sphere-equivalent diameters) of all particles in the dispersion were measured using a particle size measuring device (LA-920 (trade name), manufactured by Horiba, Ltd.), and volume-based cumulative particle size distribution data of the particle diameters was obtained. The cumulative particle size distribution data was input into a calculation software for estimating the void fraction of a multi-component particle packed bed (CALVOIDN.EXE, developed by Professor Emeritus Suzuki Michitaka, Powder and Particle Engineering Laboratory, Department of Chemical Engineering, Graduate School of Engineering, University of Hyogo. Reference URL: https: / / www.eng.u-hyogo.ac.jp / group / group42 / hakaru / calvoid.html), and an estimated void fraction was obtained. Furthermore, the closest packing fraction (closest packing fraction (%) = 100 - estimated void fraction). Note that, when the estimated void fraction was obtained, a constant value (εj = 0.36 for each component particle) was used as the void fraction εj when each component particle was packed alone, and the cumulative particle size distribution measured on a volume basis as above was used as the cumulative undersieve weight percentage Rj.
[0073] [Method for Evaluating Binder Distribution] The cross section of the positive electrode active material layer was observed using SEM-EDX (Energy Dispersive X-ray Spectroscopy) to determine the binder distribution rate. Specifically, the procedure was as follows. In a dry room, the center of one of the positive electrode sheets obtained above was punched out with a hand punch (manufactured by Nogami Giken Co., Ltd.) having an inner diameter of 10 mm to obtain a circular piece. The obtained circular piece was cut perpendicular to the main surface (thickness direction) of the circular piece at the center of the main surface (circular surface) to obtain a test piece for cross-sectional observation. The circular piece was transferred to an ion milling device IM4000 (manufactured by Hitachi High-Technologies Corporation) via a transfer vessel not exposed to the atmosphere, and cutting was performed using this ion milling device. The acceleration voltage during cutting was 6.0 kV, and the discharge voltage was 1.5 kV. The cross section (cross section in the thickness direction) of the positive electrode active material layer of the obtained test piece was observed by SEM using a field emission scanning electron microscope (FE-SEM (trade name), manufactured by JEOL Ltd., JSM-7100F) (accelerating voltage: 1.5 kV). The observed area was 20 μm × 16 μm. From this observation, the positions of the large particle group A and the small particle group B were read. For EDX observation, an energy dispersive X-ray analyzer (EDX) (Noran System 7 (trade name), manufactured by Thermo Fisher Scientific) was used, and an elemental mapping image of the cross section of the positive electrode active material layer was obtained at an accelerating voltage of 5 kV. The observed area was 20 μm × 16 μm. From the obtained elemental mapping image, the amount of F (fluorine) (derived from PVDF) in contact with the small particle group B was quantified. The amount of F in contact with the small particle group B relative to the total amount of F in the entire mapping image was calculated as the binder uneven distribution rate to the small particle group B (binder uneven distribution rate = [amount of F in contact with the small particle group B / total amount of F] × 100 (%)). Here, "F in contact with the small particle group B" means F in contact with only the small particle group B in the mapping image, and does not include F in contact with both the large particle group A and the small particle group B. The binder uneven distribution rate to the small particle group B is shown in the "binder uneven distribution rate" column of Table 3.
[0074] [Method for evaluating shape stability during punching] The center of each positive electrode sheet obtained above was punched using a 2.5 cm square punching machine (manufactured by Nogami Giken Co., Ltd., clearance 1 μm), and all of the debris that fell during this process was collected and weighed. Ten trials were performed, and the average value of the 10 measurements obtained was taken as the weight of the debris. The weight of the debris obtained was evaluated according to the following evaluation criteria. -Evaluation criteria- A: 5 mg or less B: More than 5 mg and 10 mg or less C: More than 10 mg and 15 mg or less D: More than 15 mg and 20 mg or less E: More than 20 mg and 25 mg or less F: More than 25 mg
[0075] [Fabrication of Nonaqueous Electrolyte Secondary Battery] 1) Preparation of Non-Aqueous Electrolyte 1 A mixed solvent of ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC) in a mass ratio of EC:DMC:EMC = 3:4:3 was added to the non-aqueous electrolyte solution 1. 6 These were mixed to a concentration of 1M to prepare a non-aqueous electrolyte solution (non-aqueous electrolyte solution 1).
[0076] 2) Preparation of Negative Electrode Sheet Negative electrode active material (artificial graphite), styrene-butadiene copolymer (SBR) as a binder, carboxymethyl cellulose (CMC) as a thickener, and water as a solvent were mixed in a mass ratio of negative electrode active material:SBR:CMC:water = 60:1.5:0.5:38 to obtain a negative electrode slurry. The negative electrode slurry was applied to one side of a 12 μm thick negative electrode current collector (copper foil) and dried at 150 ° C until the solvent volatilized. Thereafter, a pressing process was performed using a roll press to obtain a sheet-shaped negative electrode (negative electrode sheet) having a negative electrode current collector and a negative electrode active material layer. The thickness of this negative electrode active material layer was approximately 180 μm.
[0077] 3) Preparation of Non-Aqueous Electrolyte Secondary Battery The positive electrode sheet obtained in the above [Preparation of Positive Electrode Composition and Positive Electrode Sheet] and a negative electrode sheet were laminated with a separator interposed between them to obtain an electrode laminate consisting of a positive electrode current collector, a positive electrode active material layer, a separator, a negative electrode active material layer, and a negative electrode current collector. An aluminum tab was attached to the end of the positive electrode current collector, and a nickel tab was attached to the end of the negative electrode current collector by ultrasonic welding. A battery assembly was produced by housing this electrode laminate in a laminate container. A non-aqueous electrolyte 1 was poured into the container with the inlet open, and then the inlet was sealed to hermetically seal the container, producing a non-aqueous electrolyte secondary battery for evaluation testing.
[0078] [Volumetric Energy Density Measurement Method] The positive electrode sheet used in preparing each of the nonaqueous electrolyte secondary batteries was punched out to a diameter of 10 mm. The positive electrode current collector was removed from the punched piece, and the thickness of the positive electrode active material layer was measured. The thickness of the negative electrode active material layer was measured in the same manner. The thickness of the power generating element was calculated by adding the thickness of the positive electrode current collector + the thickness of the positive electrode active material layer + the thickness of the separator + the thickness of the negative electrode active material layer + the thickness of the negative electrode current collector. The thickness of each constituent layer was measured using a constant pressure thickness meter (product name: PG-20J, manufactured by Teclock Corporation). The volume (L) of the power generating element was calculated by multiplying the thickness of the power generating element by the area of the circular surface of the power generating element. Here, the volume (L) of the power generating element was calculated based on the ideal volume of the power generating element, without taking into account volume reduction due to collapse of the edges caused by punching the positive electrode sheet, etc. Separately, under Condition 1 described below, the nonaqueous electrolyte secondary battery obtained above was charged and discharged to measure the reference discharge capacity (Ah) and the average voltage (V) during discharge. The amount of electric power (Wh) was calculated by multiplying the reference discharge capacity (Ah) by the average voltage (V). The amount of electric power (Wh) thus obtained was divided by the volume (L) of the power generating element obtained above to calculate the volumetric energy density of the nonaqueous electrolyte secondary battery. The obtained values were evaluated according to the following evaluation criteria. -Evaluation Criteria- A: 400 Wh / L or more B: 390 Wh / L or more and less than 400 Wh / L C: 380 Wh / L or more and less than 390 Wh / L D: 370 Wh / L or more and less than 380 Wh / L E: 360 Wh / L or more and less than 370 Wh / L F: Less than 360 Wh / L <Condition 1. Charge / Discharge Conditions> (Charge / Discharge Conditions for Experiments No. 1 to 12 (Experiments using LFP as the positive electrode active material)) Constant current (CC)-constant voltage (CV) charge: current value 15 mA, upper limit voltage value 3.6 V, end current value 0.5 mA CC discharge: current value 15 mA, end voltage value 2.0 V (Charge / Discharge Conditions for Experiments No. 13 to 24 (Experiments using NMC as the positive electrode active material)) CC-CV charge: current value 15 mA, upper limit voltage value 4.2 V, end current value 0.5 mA CC discharge: current value 15 mA, upper limit voltage value 3.0 V
[0079] The results obtained are shown in Tables 2 and 3.
[0080]
[0081]
[0082]
[0083] (Notes for Table 2) For convenience, the information (median diameter) regarding "large particle group a" is also listed in the "large particle group A" column. Similarly, the information regarding "small particle group b" is also listed in the "small particle group B" column. "-" indicates that the component is not used.
[0084] As shown in Tables 2 and 3, when the positive electrode composition did not contain the large particle group A and the small particle group B at the frequencies specified in the present invention (Experiments Nos. 1, 4, 5, 13, 16, and 17), and when the surface tension γB of the small particle group B with respect to NMP did not satisfy the formula B1: 15.0≦γB≦40.0 (Experiments Nos. 11, 12, 23, and 24), the edge of the positive electrode active material in the positive electrode sheet was prone to collapse, resulting in poor shape stability. Furthermore, nonaqueous electrolyte secondary batteries having this positive electrode sheet as a positive electrode were poor in battery capacity (energy density). In contrast, when the positive electrode composition contained the large particle group A and the small particle group B at the frequency specified in the present invention, and further, the surface tension γB of the small particle group B with respect to NMP satisfied the formula B1: 15.0≦γB≦40.0 (Experiments Nos. 2, 3, 6-10, 14, 15, 18-22), even when the binder amount was as low as 0.3 mass% and a positive electrode active material layer having a thickness of 250 μm was formed, the resulting positive electrode sheet suppressed the collapse of the edge of the positive electrode active material, resulting in excellent shape stability. Furthermore, nonaqueous electrolyte secondary batteries having this positive electrode sheet as the positive electrode also showed improved battery capacity.
[0085] While the present invention has been described in connection with embodiments thereof, we do not intend to limit our invention to any of the details of the description unless otherwise specified, and believe that the claims should be construed broadly without departing from the spirit and scope of the invention as set forth in the appended claims.
[0086] This application claims priority based on Japanese Patent Application No. 2023-90456, filed on May 31, 2023, the contents of which are incorporated herein by reference as part of the present specification.
[0087] REFERENCE SIGNS LIST 10 Non-aqueous electrolyte secondary battery 1 Negative electrode current collector 2 Negative electrode active material layer 3 Separator 4 Positive electrode active material layer 5 Positive electrode current collector 6 Operating part (light bulb)
Claims
1. A positive electrode composition for a non-aqueous electrolyte secondary battery, comprising a positive electrode active material composed of a large particle group A having a particle size of 5.0 μm or more and a small particle group B having a particle size of less than 5.0 μm, in which, when the total frequency in a number-based particle size distribution of the positive electrode active material is taken as 100%, the frequency of the large particle group A is 60% or more and the frequency of the small particle group B is 40% or less, and the surface tension γB (mN / m) of the small particle group B to N-methylpyrrolidone satisfies the following formula B1. Formula B1: 15.0≦γB≦40.0 2. The positive electrode composition according to claim 1, wherein the surface tension γA (mN / m) of the large particle group A with respect to N-methylpyrrolidone satisfies the following formula A1: 15.0≦γA≦25.
0.
3. The positive electrode composition according to claim 2, wherein the surface tension γA of the large particle group A satisfies the following formula A2: 18.0≦γA≦22.
0.
4. The positive electrode composition according to claim 3, wherein the surface tension γB of the small particle group B satisfies the following formula B2: 25.0≦γB≦35.
0.
5. The positive electrode composition according to claim 4, wherein the positive electrode active material has a closest packing ratio calculated from a cumulative particle size distribution on a volume basis of 80% or more.
6. A positive electrode sheet having a positive electrode active material layer formed using the positive electrode composition according to any one of claims 1 to 5.
7. A non-aqueous electrolyte secondary battery having the positive electrode sheet according to claim 6 as a positive electrode.
Citation Information
Patent Citations
Rechargeable lithium-ion secondary battery
JP2005108835A
Nonaqueous secondary battery
JP2012185938A
Method of manufacturing electrode for lithium ion secondary battery
JP2015230748A
Nonaqueous electrolyte and nonaqueous secondary battery
JP2016201308A
Sewage sludge fermentation raw material and sewage sludge treatment method
JP2023090456A