Mixed silver powder, method for producing mixed silver powder, and conductive paste
The use of a mixed silver powder with specific particle distributions and surface treatment enhances the conductivity of conductive films, addressing the high specific resistance issue in conventional films and meeting the demands of advanced electronic devices.
Patent Information
- Application Number
- PCT/JP2024/019299
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-05-23
- Filing Date
- 2024-05-24
- Publication Date
- 2024-12-05
AI Technical Summary
Conductive films formed using conventional silver powders in conductive pastes have high specific resistance, which is not sufficient for the increasing performance demands of electronic devices.
A mixed silver powder comprising first, second, and tertiary silver particles with specific size and aspect ratio distributions, along with surface treatment using polyhydric carboxylic acids, is used to create a conductive paste that reduces the specific resistance of the conductive film.
The mixed silver powder effectively reduces the specific resistance of the conductive film by filling gaps and improving the density and conductivity of the film, making it suitable for advanced electronic applications.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Mixed silver powder, method for producing mixed silver powder, and conductive paste
[0001] The present invention relates to a mixed silver powder, a method for producing the mixed silver powder, and a conductive paste.
[0002] A method of forming electrodes, electrical wiring, etc. by applying or printing a conductive paste containing a conductive metal powder onto a substrate such as a film, a board, or an electronic component, and then heating it to dry and harden it has been widely used. However, with the recent increase in the performance of electronic devices, electrodes, electrical wiring, etc. formed using the conductive paste are required to have lower resistance, and this requirement is becoming stricter every year.
[0003] In response to the above demands, for example, Patent Document 1 proposes the use of a silver powder consisting of a flaky silver powder and a spherical silver powder, with a polyvalent carboxylic acid attached to the surface of at least one of the flaky silver powder and the spherical silver powder, as a conductive metal powder, in order to obtain a conductive paste composition having high conductivity (low resistance).
[0004] JP 2011-100573 A
[0005] Here, with regard to the silver powder (silver powder) that can be used in conventional conductive pastes, there is room for further improvement in terms of reducing the resistivity of the conductive film formed using the conductive paste.
[0006] Therefore, an object of the present invention is to provide a mixed silver powder capable of reducing the resistivity of a conductive film. Another object of the present invention is to provide a method for producing a mixed silver powder capable of reducing the resistivity of a conductive film. Another object of the present invention is to provide a conductive paste capable of reducing the resistivity of a conductive film.
[0007] As a result of extensive research by the present inventors to solve the above-mentioned problems, the present inventors have completed the present invention described below.
[0008] That is, the gist and configuration of the present invention for solving the above-mentioned problems is as follows.
[0009] [1] A mixed silver powder comprising first silver particles, second silver particles, and tertiary silver particles, wherein 100 or more silver particles are observed on a polished cross section of a resin block obtained by embedding the mixed silver powder in a resin, and the perimeter of each silver particle and the long side length and short side length of a rectangle that circumscribes the outer shape of each silver particle and has the smallest area are measured, whereby the first silver particles are silver particles having a long side length of 3 μm or more, the second silver particles are silver particles having a long side length of 0.5 μm or more and less than 3 μm, and the tertiary silver particles are silver particles having a long side length of less than 0.5 μm; the first silver particles have an average aspect ratio of 2 or more, the second silver particles have an average aspect ratio of 1.5 or more and less than 2, and the tertiary silver particles have an average aspect ratio of less than 1.5, a mixed silver powder in which the number ratio of the first silver particles is 0.5% or more and 5% or less, the number ratio of the second silver particles is 10% or more, and the number ratio of the tertiary silver particles is 15% or more in the mixed silver powder; an average value of the ratio α calculated by the following formula (1): ratio α=perimeter of second silver particle / (long side length of second silver particle×2+short side length of second silver particle×2) (1) is 0.84 or more; and a polyvalent carboxylic acid is adhered to the surface of at least one type of silver particle selected from the group consisting of the first silver particles, the second silver particles, and the tertiary silver particles.
[0010] [2] The mixed silver powder according to [1], in which a polycarboxylic acid is attached to the surfaces of the first silver particles and the second silver particles.
[0011] [3] The mixed silver powder according to [1] or [2], wherein the content of the polycarboxylic acid relative to the total of the first silver particles, the second silver particles, and the tertiary silver particles is 0.01% by mass or more and 0.15% by mass or less.
[0012] [4] The mixed silver powder according to any one of [1] to [3], wherein the polycarboxylic acid is at least one polycarboxylic acid selected from the group consisting of oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, dodecanedioic acid, malic acid, diethylglutaric acid, 3-methyladipic acid, butylmalonic acid, maleic acid, diglycolic acid, and citric acid.
[0013] [5] A method for producing a silver powder A having silver particles A1 and silver particles A2, and a silver powder B having silver particles B, comprising: a mixing step of mixing a silver powder A containing silver particles A1 and silver particles A2 with a silver powder B containing silver particles B to obtain a mixture; and a pretreatment step of treating at least one of the silver powders A and B with a polycarboxylic acid before the mixing step to attach a surface treatment agent thereto, or a posttreatment step of treating the mixture obtained in the mixing step with a polycarboxylic acid to attach a surface treatment agent thereto, wherein when 100 or more silver particles on a polished cross section of a resin block having the silver powder A embedded in a resin and 100 or more silver particles on a polished cross section of a resin block having the silver powder B embedded in a resin are observed, and the perimeter of the silver particles and the long side lengths and short side lengths of a rectangle that circumscribes the outer shape of the silver particles and has the smallest area are measured, the silver particles A1 have an average aspect ratio of 2 or more, and the silver particles A2 have an average aspect ratio of less than 2, and the average aspect ratio satisfies the following formula (2): [5] The method for producing a mixed silver powder according to any one of [1] to [4], wherein the average value of the ratio β calculated by the following formula is 0.84 or more, and the silver particles B have an average aspect ratio of less than 1.5.
[0014] [6] The method for producing a mixed silver powder according to [5], comprising the pretreatment step, in which the silver powder A is treated with the polycarboxylic acid to adhere a surface treatment agent thereto.
[0015] [7] The method for producing a mixed silver powder according to [5] or [6], wherein the usage rate of the polycarboxylic acid relative to the total of the silver powder A and the silver powder B is 0.01 mass% or more and 0.15 mass% or less.
[0016] [8] The method for producing a mixed silver powder according to any one of [5] to [7], wherein the polycarboxylic acid used in the surface treatment agent attachment treatment is at least one polycarboxylic acid selected from the group consisting of oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, dodecanedioic acid, malic acid, diethylglutaric acid, 3-methyladipic acid, butylmalonic acid, maleic acid, diglycolic acid, and citric acid.
[0017] [9] A conductive paste comprising the mixed silver powder according to any one of [1] to [4], a binder, and a solvent.
[0018] According to the present invention, a mixed silver powder capable of reducing the resistivity of a conductive film can be provided. Also, according to the present invention, a method for producing a mixed silver powder capable of reducing the resistivity of a conductive film can be provided. Also, according to the present invention, a conductive paste capable of reducing the resistivity of a conductive film can be provided.
[0019] FIG. 1 is a schematic diagram for explaining a method for specifying the long side length and short side length of a rectangle that circumscribes the outer shape of the cross section of a silver particle and has the smallest area. FIG. 2 is a scanning electron micrograph of the mixed silver powder according to Example 1. FIG. 3 is a scanning electron micrograph of the mixed silver powder according to Example 2. FIG. 4 is a scanning electron micrograph of the mixed silver powder according to Example 3. FIG. 5 is a scanning electron micrograph of the mixed silver powder according to Comparative Example 1. FIG. 6 is a scanning electron micrograph of the mixed silver powder according to Comparative Example 2. FIG. 7 is a scanning electron micrograph of the mixed silver powder according to Comparative Example 3. FIG. 8 is a scanning electron micrograph of the mixed silver powder according to Example 4. FIG. 9 is a scanning electron micrograph of the mixed silver powder according to Comparative Example 4. FIG. 10 is a scanning electron micrograph of the mixed silver powder according to Comparative Example 5.
[0020] The mixed silver powder of the present invention is suitable for use as a conductive filler for conductive pastes. A conductive paste using the mixed silver powder of the present invention can be used to form a conductive pattern or an electrode on a substrate. A conductive paste using the mixed silver powder of the present invention can be printed on a substrate by, for example, screen printing, offset printing, photolithography, or the like to form a conductive film such as a conductive pattern or an electrode (hereinafter, sometimes simply referred to as a "conductive film"). The mixed silver powder of the present invention can be obtained, for example, by the method for producing the mixed silver powder of the present invention.
[0021] (Terminology and Measurement Methods) First, prior to describing the embodiments, the terminology and measurement methods used in this specification will be described.
[0022] <Observation of Silver Particles> In this specification, silver particles can be observed by first placing a mixed silver powder or silver powder in a resin and a curing agent, solidifying the mixture, and polishing the mixture with a cross-section polisher to expose the cross-section of the silver particles. Each silver particle is then observed under a scanning electron microscope (SEM) at a predetermined magnification (e.g., 5,000x or 3,000x). Here, based on the contrast between the insulating resin and the conductive silver particles, silver particles with a clear outline and clearly visible peripheries are considered to have exposed cross-sections. Then, on a polished cross-section of a resin block in which the mixed silver powder or silver powder is embedded in a resin, 100 or more silver particles are arbitrarily selected from among the silver particles whose peripheries are clearly visible. Image analysis software is used to trace the peripheries of the silver particles, allowing the measurement of the long side length of the rectangle (hereinafter sometimes simply referred to as the "long side length"), the short side length of the rectangle (hereinafter sometimes simply referred to as the "short side length"), the perimeter, the area of the silver particle, and the maximum length of the silver particle. The resin and curing agent may be, for example, "Epofix Resin" and "Epofix Curing Agent" manufactured by Struers. The cross-section polisher may be, for example, "ArBlade5000" manufactured by Japan High-Technologies Corporation. The scanning electron microscope may be, for example, "JEOL JSM-IT300LV" manufactured by JEOL Ltd. The image analysis software may be, for example, "Image Analysis Particle Size Distribution Measurement Software Mac-View" manufactured by Mountec Co., Ltd.
[0023] Here, a method for determining the long and short side lengths of a rectangle that circumscribes the cross-sectional shape of a silver particle and has the smallest area will be described with reference to Figure 1. As shown in Figure 1, first, silver particles to be measured (100 or more) are selected. Next, the selected silver particles are rotated 360 degrees to create all possible rectangles that circumscribe the cross-sectional shape of the silver particle. Then, from these rectangles, the rectangle with the smallest area is selected, and the long and short side lengths of this rectangle are determined.
[0024] <Average Aspect Ratio> In this specification, the term "aspect ratio" refers to the ratio of the long side length to the short side length (long side length / short side length), and the term "average aspect ratio" refers to the average aspect ratio of individual silver particles within a range defined by the long side length values.
[0025] <Average Short Side Length> In this specification, the term "average short side length" refers to the average short side length of individual silver particles within a range defined by the long side length value.
[0026] <Average value of shape factor> In this specification, the "shape factor" refers to the average value of "π × (maximum length of silver particle / 2)" 2 The "average shape factor" is the average value of the individual shape factors of silver particles within a range defined by the value of the long side length. The unit of the maximum length of silver particles is "μm", and the unit of the area of silver particles is "μm 2 "
[0027] <Measurement of particle size distribution> In this specification, the cumulative 10% particle diameter (D 10 ), cumulative 50% particle diameter (D 50 ), cumulative 90% particle diameter (D 90 ), and cumulative 95% particle diameter (D 95 ), and the particle diameter of cumulative 100% (i.e., the largest particle) (D MAX ) was measured using a laser diffraction / scattering particle size distribution measuring device (Microtrac MT-3300 EXII, manufactured by Microtrac Bell Co., Ltd.).
[0028] <Method for Measuring the Polycarboxylic Acid Content> In this specification, the "polycarboxylic acid content" can be measured by first eluting the polycarboxylic acid from the mixed silver powder to which the polycarboxylic acid is attached with hydrochloric acid, then esterifying the polycarboxylic acid in the hydrochloric acid eluate into which the polycarboxylic acid has been eluted, then extracting the esterified polycarboxylic acid into an organic solvent, and then determining the amount of extracted adipic acid ester from a calibration curve for the polycarboxylic acid ester, and then calculating the amount of polycarboxylic acid by conversion calculation. For example, when the polycarboxylic acid is adipic acid, the adipic acid content can be measured according to the method for quantifying adipic acid described in JP 2012-122880 A. Note that when the polycarboxylic acid is adipic acid, the adipic acid content can also be measured by methylating the adipic acid on the surface of the sample silver powder using a hydrogen chloride-methanol reagent, extracting the resulting dimethyl adipate into an organic solvent, and measuring it by GC-MS.
[0029] <BET Specific Surface Area> In this specification, the "BET specific surface area" can be measured by a BET single-point method using nitrogen adsorption using a Macsorb HM-model 1210 (manufactured by MOUNTECH Co., Ltd.) In measuring the BET specific surface area, the degassing conditions before measurement are 60°C and 10 minutes.
[0030] <Ignition Loss (Ig-Loss) Value of Mixed Silver Powder> In this specification, the "ignition loss (Ig-Loss) value of mixed silver powder" refers to the amount of change in mass when heated from room temperature to 800°C. Specifically, it represents the amount of components other than silver contained in the mixed silver powder, and serves as an index of the amount of components remaining in the mixed silver powder, such as processing agents and additives used in the manufacturing process of the mixed silver powder. In this specification, the "ignition loss (Ig-Loss) value of mixed silver powder" can be calculated by precisely weighing a mixed silver powder sample (weighing value: w1), placing it in a porcelain crucible, heating it to 800°C, and holding it at 800°C for 30 minutes, a time sufficient to reach constant weight, followed by cooling and reweighing (weighing value: w2), and then calculating the "ignition loss (Ig-Loss) value (mass %) = (w1 - w2) / w1 × 100."
[0031] <Tap Density of Mixed Silver Powder> In this specification, the "tap density of mixed silver powder" can be calculated, for example, using a tap density measuring device (bulk specific gravity measuring device SS-DA-2, manufactured by Shibayama Scientific Co., Ltd.), by weighing 30 g of a silver powder sample, placing it in a 20 mL test tube, and tapping it 1,000 times at a drop of 20 mm, and then calculating the tap density from the formula "tap density = sample mass (g) / sample volume after tapping (mL)."
[0032] <Circle-equivalent diameter (Heywood diameter)> In this specification, the "circle-equivalent diameter (Heywood diameter)" can be calculated using the area of a silver particle measured by observing the cross section of the silver particle. Specifically, the circle-equivalent diameter (Heywood diameter) can be determined by creating a circle having the same area as the area of the silver particle.
[0033] <Viscosity of Conductive Paste> In this specification, the "viscosity of the conductive paste" can be the value measured when the cone spindle is rotated for 5 minutes using, for example, a Brookfield 5XHBDV-IIIUC rotational viscometer and a CPE-52 cone spindle at a measurement temperature of 25°C and a rotation speed of 1 rpm.
[0034] (Mixed Silver Powder) The mixed silver powder of the present invention is a mixed silver powder comprising first silver particles, second silver particles, and third silver particles, and is obtained by observing 100 or more silver particles on a polished cross section of a resin block in which the mixed silver powder is embedded in a resin, and measuring the perimeter of the silver particles and the long side length and short side length of a rectangle that circumscribes the outer shape of the silver particles and has the smallest area. The silver particles having a long side length of 3 μm or more are called first silver particles, silver particles having a long side length of 0.5 μm or more but less than 3 μm are called second silver particles, and silver particles having a long side length of 0.5 μm or more but less than 3 μm are called third silver particles. When silver particles having a length of less than 0.5 μm are used as the tertiary silver particles, the average aspect ratio of the first silver particles is 2 or more, the average aspect ratio of the second silver particles is 1.5 or more but less than 2, and the average aspect ratio of the tertiary silver particles is less than 1.5, the number ratio of the first silver particles to the mixed silver powder is 0.5% or more but 5% or less, the number ratio of the second silver particles is 10% or more, and the number ratio of the tertiary silver particles is 15% or more, the average value of the ratio α (also referred to as rectangularity) calculated by the following formula (1): ratio α = perimeter of second silver particle / (long side length of second silver particle × 2 + short side length of second silver particle × 2) (1) is 0.84 or more, and a polycarboxylic acid is attached to the surface of at least one type of silver particle selected from the group consisting of first silver particles, second silver particles, and tertiary silver particles. Such a mixed silver powder can reduce the resistivity of a conductive film. The reason for this is presumably that the relatively small third silver particles penetrate into the gaps between the first silver particles, which are advantageous for reducing the resistivity in the conductive film, reducing the void ratio of the conductive film and making the silver powder denser, resulting in fewer spaces in the conductive film where there are no silver particles, i.e., fewer areas with high resistance, and thus a reduction in resistivity. Furthermore, the presence of second silver particles with a long side length between the first and third silver particles in the conductive film, and the nearly rectangular shape of the second silver particles, which may lead to surface or line contact between the first and second silver particles and between the second silver particles themselves, further reduces the void ratio of the conductive film, further reducing the areas with high resistance and thus reducing the resistivity. Furthermore, the tendency for the aspect ratio to increase as the major axis increases is presumably responsible for the excellent packing properties and ease of sintering of the silver particles, resulting in improved conductivity of the resulting conductive film.The perimeter, rectangular long and short side lengths, average aspect ratio, number ratio, and ratio α of each silver particle can be adjusted by the properties of the silver powder that can be used as a raw material, the timing of the surface treatment agent deposition treatment described below, and the type and use rate of the polycarboxylic acid that can be used in the surface treatment agent deposition treatment.
[0035] <First Silver Particles> In the mixed silver powder of the present invention, the first silver particles are silver particles having a long side length of 3 μm or more.
[0036] In the mixed silver powder of the present invention, the average aspect ratio of the first silver particles must be 2 or more, preferably 2.3 or more, more preferably 2.5 or more, and even more preferably 3 or more. If the average aspect ratio of the first silver particles is 2 or more, the resistivity of the conductive film can be effectively reduced. On the other hand, the average aspect ratio of the first silver particles is, for example, 5 or less, or may be 4 or less, or 3.5 or less.
[0037] The average short side length of the first silver particles is, for example, 0.6 μm or more, or 1.0 μm or more, or 1.3 μm or more, and is, for example, 2.5 μm or less, or 2.0 μm or less, or 1.9 μm or less.
[0038] The average shape factor of the first silver particles is, for example, 2 or more, optionally 2.5 or more, or 3 or more, and is, for example, 6 or less, optionally 5 or less, or optionally 4 or less.
[0039] In the mixed silver powder of the present invention, the proportion of the first silver particles in the mixed silver powder must be 0.5% or more, preferably 1% or more, and more preferably 1.5% or more, and must be 5% or less, preferably 4% or less, and more preferably 3% or less. If the proportion of the first silver particles in the mixed silver powder is within the above range, the resistivity of the conductive film can be effectively reduced.
[0040] <Second Silver Particles> In the mixed silver powder of the present invention, the second silver particles are silver particles having a long side length of 0.5 μm or more and less than 3 μm.
[0041] In the mixed silver powder of the present invention, the average aspect ratio of the secondary silver particles must be 1.5 or more, preferably 1.6 or more, and more preferably 1.7 or more, and must be less than 2, and is preferably 1.95 or less, and more preferably 1.92 or less. When the average aspect ratio of the secondary silver particles is within the above range, the resistivity of the conductive film can be effectively reduced.
[0042] In the mixed silver powder of the present invention, the average value of the ratio α calculated by the following formula (1): ratio α = peripheral length of secondary silver particles / (long side length of secondary silver particles × 2 + short side length of secondary silver particles × 2) (1) must be 0.84 or more, and preferably 0.85 or more. The ratio α represents the rectangularity of the particle cross section, and the closer the value of the ratio α is to 1, the more rectangular the particle shape becomes. If the average value of the ratio α is 0.84 or more, the specific resistance of the conductive film can be effectively reduced. On the other hand, the average value of the ratio α is 1 or less, and may be, for example, 0.95 or less.
[0043] The average short side length of the second silver particles is, for example, 0.3 μm or more, or may be 0.4 μm or more, or 0.5 μm or more, and may be, for example, 1 μm or less, or 0.8 μm or less, or 0.7 μm or less.
[0044] The average shape factor of the second silver particles is, for example, 1.5 or more, optionally 1.7 or more, or 2 or more, and is, for example, 3 or less, optionally 2.5 or less, or optionally 2.3 or less.
[0045] In the mixed silver powder of the present invention, the proportion of secondary silver particles in the mixed silver powder must be 10% or more, and preferably 30% or more. If the proportion of secondary silver particles in the mixed silver powder is 10% or more, the resistivity of the conductive film can be effectively reduced.
[0046] <Tertiary silver particles> In the mixed silver powder of the present invention, the tertiary silver particles are silver particles having a long side length of less than 0.5 μm.
[0047] In the mixed silver powder of the present invention, the average aspect ratio of the tertiary silver particles must be less than 1.5, preferably 1.4 or less, and more preferably 1.35 or less. If the average aspect ratio of the tertiary silver particles is less than 1.5, the resistivity of the conductive film can be effectively reduced. On the other hand, the average aspect ratio of the tertiary silver particles is, for example, 1.1 or more, or may be 1.2 or more, or 1.25 or more.
[0048] The average short side length of the silver trioxide particles is, for example, 0.1 μm or more, or may be 0.2 μm or more, or 0.25 μm or more, and may be, for example, 0.5 μm or less, or 0.4 μm or less.
[0049] The average shape factor of the silver trioxide particles is, for example, 1.2 or more, optionally 1.4 or more, or 1.6 or more, and is, for example, 2.5 or less, optionally 2 or less, or optionally 1.75 or less.
[0050] In the mixed silver powder of the present invention, the proportion of tertiary silver particles in the mixed silver powder must be 10% or more, preferably 13% or more, and more preferably 15% or more. If the proportion of tertiary silver particles in the mixed silver powder is within the above range, the resistivity of the conductive film can be effectively reduced.
[0051] <Polycarboxylic Acid> In the mixed silver powder of the present invention, a polycarboxylic acid is adhered to the surface of at least one type of silver particle selected from the group consisting of first silver particles, second silver particles, and third silver particles. In order to effectively reduce the resistivity of the conductive film, it is preferable that the mixed silver powder has a polycarboxylic acid adhered to the surface of the first silver particles and the second silver particles.
[0052] Here, the polycarboxylic acid is not particularly limited and includes conventionally known polycarboxylic acids, but the polycarboxylic acid is preferably an aliphatic polycarboxylic acid, and more preferably a saturated aliphatic polycarboxylic acid, because it can effectively reduce the resistivity of the conductive film. More specifically, the polycarboxylic acid is preferably at least one polycarboxylic acid selected from the group consisting of oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, dodecanedioic acid, malic acid, diethylglutaric acid, 3-methyladipic acid, butylmalonic acid, maleic acid, diglycolic acid, and citric acid, and adipic acid is particularly preferred.
[0053] The content of the polycarboxylic acid relative to the total of the first silver particles, second silver particles, and third silver particles is preferably 0.01% by mass or more, more preferably 0.02% by mass or more, and is preferably 0.15% by mass or less, more preferably 0.1% by mass or less, and even more preferably 0.05% by mass or less. When the content of the polycarboxylic acid is within the above range, the resistivity of the conductive film can be effectively reduced.
[0054] <Characteristics of mixed silver powder> The cumulative 50% particle diameter (D) on a volume basis was measured by laser diffraction scattering particle size distribution measurement of the mixed silver powder. 50 ) is, for example, 1 μm or more and, for example, 3 μm or less.
[0055] The BET specific surface area of the mixed silver powder is, for example, 0.2 m 2 / g or more, and 2 / g or more, and 0.5m 2 / g or more, for example, 1 m 2 / g or less, and 2 / g or less, and 2 / g or less.
[0056] The ignition loss (Ig-Loss) value of the mixed silver powder is, for example, 0.05% by mass or more, or may be 0.1% by mass or more, or 0.3% by mass or more, and may be, for example, 3% by mass or less, or 1% by mass or less, or 0.5% by mass or less.
[0057] The tap density of the mixed silver powder is, for example, 3 g / mL or more, or may be 4 g / mL or more, or 5 g / mL or more, or may be, for example, 7 g / mL or less, or may be 6 g / mL or less.
[0058] (Method for Producing Mixed Silver Powder) The method for producing a mixed silver powder of the present invention includes a mixing step of mixing silver powder A containing silver particles A1 and silver particles A2 with silver powder B containing silver particles B to obtain a mixture, and a pretreatment step of treating at least one of silver powder A and silver powder B with a polycarboxylic acid before the mixing step to attach a surface treatment agent thereto, or a post-treatment step of treating the mixture obtained in the mixing step with a polycarboxylic acid to attach a surface treatment agent thereto. When 100 or more silver particles on a polished cross section of a resin block in which silver powder A is embedded in a resin and 100 or more silver particles on a polished cross section of a resin block in which silver powder B is embedded in a resin are observed, and the perimeter of the silver particles and the long side lengths and short side lengths of a rectangle that circumscribes the outer shapes of the silver particles and has the smallest area are measured, silver particles A1 have an average aspect ratio of 2 or more, and silver particles A2 have an average aspect ratio of less than 2, and the average aspect ratio satisfies the following formula (2): The average value of the ratio β (also referred to as rectangularity), calculated by the following formula: ratio β = perimeter of silver particles A2 / (long side length of silver particles A2 × 2 + short side length of silver particles A2 × 2) (2), is 0.84 or more, and silver particles B have an average aspect ratio of less than 1.5. The above-described method for producing a mixed silver powder can provide a mixed silver powder that can reduce the resistivity of a conductive film. Furthermore, the method for producing a mixed silver powder of the present invention can provide the above-described mixed silver powder of the present invention. The cross-sections of the silver particles in the method for producing a mixed silver powder of the present invention can be observed in the same manner as the cross-sections of the silver particles in the above-described mixed silver powder of the present invention.
[0059] In addition to the above-described pretreatment step, mixing step, and post-treatment step, the method for producing a mixed silver powder of the present invention may further include other steps, such as a crushing step of crushing silver particles A and / or silver particles B before the pretreatment step or the mixing step.
[0060] <Silver Powder A> Silver powder A contains silver particles A1 with a large aspect ratio and silver particles A2 with a smaller aspect ratio and a greater degree of rectangularity than silver particles A1.
[0061] [Silver Particles A1] Silver particles A1 are silver particles having an aspect ratio of at least 2. The proportion of silver particles A1 in the silver powder A is, for example, 5% or more and 50% or less.
[0062] The average aspect ratio of silver particles A1 is 2 or more, preferably 2.3 or more, more preferably 2.5 or more, and even more preferably 3 or more. When the average aspect ratio of silver particles A1 is 2 or more, a mixed silver powder that can effectively reduce the resistivity of a conductive film can be obtained. On the other hand, the average aspect ratio of silver particles A1 is, for example, 5 or less, or may be 4 or less, or 3.5 or less.
[0063] [Silver particles A2] Silver particles A2 are silver particles having an aspect ratio smaller than that of silver particles A1 and a rectangularity of the particle shape (ratio β described below) of 0.84 or more. Silver particles A2 are silver particles having an aspect ratio of less than 2. The rectangularity of silver particles having an aspect ratio of less than 2 is measured, and the average value of the measured rectangularity is 0.84 or more. The proportion of silver particles A2 in the silver powder A is preferably, for example, 50% to 95%.
[0064] The average aspect ratio of the silver particles A2 is preferably 1.4 or more and less than 2. When the average aspect ratio of the silver particles A2 is within the above range, a mixed silver powder can be obtained that can effectively reduce the resistivity of a conductive film.
[0065] In silver powder A, the average value of the ratio β calculated by the following formula (2): ratio β = perimeter of silver particles A2 / (long side length of silver particles A2 × 2 + short side length of silver particles A2 × 2) (2) must be 0.84 or more, and preferably 0.85 or more. The ratio β represents the rectangularity of the particle cross section, and the closer the value of the ratio β is to 1, the more rectangular the particle shape is. If the average value of the ratio β is 0.84 or more, the specific resistance of the conductive film can be effectively reduced. On the other hand, the average value of the ratio β is 1 or less, and may be, for example, 0.95 or less.
[0066] [Method for Preparing Silver Powder A] The method for preparing silver powder A is not particularly limited as long as silver particles A and silver particles B contained in silver powder A satisfy the predetermined requirements, and any conventionally known method can be used. An example of a method for preparing silver powder A will be described below, but the silver powder A used in the method for producing a mixed silver powder of the present invention is not limited to this method.
[0067] Silver powder A can be prepared by a method including the following steps: a reduction step of adding a reducing agent to an aqueous silver ammine complex solution to obtain a first liquid; a surface treatment agent addition step of adding a surface treatment agent to the first liquid to obtain a second liquid; a separation step of separating the spherical silver powder from the second liquid and drying it to obtain spherical silver powder having an aspect ratio of less than 1.5; and a step of stirring the spherical silver powder, a lubricant, and a medium in a container to partially flatten the particles to the extent that silver particles A1 have a large aspect ratio and silver particles A2 have an aspect ratio smaller than that of silver particles A1 and a greater degree of rectangularity.
[0068] In the reduction step, a reducing agent is added to an aqueous solution of a silver ammine complex to obtain a first solution. Here, in the reduction step, silver ions are reduced by the addition of the reducing agent, and silver particles (hereinafter referred to as core particles) can be precipitated.
[0069] Examples of reducing agents include hydrazine, hydrazine compounds, and formalin.
[0070] The silver ammine complex aqueous solution may be prepared by adding ammonia water or an ammonium salt to a raw material solution such as a silver nitrate aqueous solution or a silver oxide suspension. A pH adjuster may be added to the raw material solution or the silver ammine complex aqueous solution. Examples of the pH adjuster include common acids and bases, such as nitric acid and sodium hydroxide.
[0071] Surface Treatment Agent Addition Step In the surface treatment agent addition step, a surface treatment agent is added to the first liquid obtained in the reduction step to obtain a second liquid. Here, in the surface treatment agent addition step, the surface of the core particles may be coated with the surface treatment agent by adsorption or the like. Hereinafter, core particles coated with the surface treatment agent will be referred to as coated particles. The second liquid is a suspension (so-called slurry) or dispersion in which the coated particles are dispersed.
[0072] Examples of surface treatment agents include fatty acids such as stearic acid, palmitic acid, linoleic acid, linolenic acid, oleic acid, etc. Among these, unsaturated fatty acids such as linoleic acid, linolenic acid, oleic acid, etc. are preferred.
[0073] The amount of the surface treatment agent added in the surface treatment agent addition step is usually 0.05% by mass or more and 0.15% by mass or less relative to the mass of silver contained in the aqueous silver ammine complex solution.
[0074] The amount of surface treatment agent that adheres to the core particles in the surface treatment agent addition step and remains after the drying step is a value measured on the spherical silver powder after the drying step described below, with the type of surface treatment agent specified. The type of surface treatment agent can be specified by qualitative analysis by gas chromatography of the surface treatment agent that has been vaporized by heating the spherical silver powder.
[0075] The amount of surface treatment agent attached to the spherical silver powder can be determined according to the method for quantitative analysis of fatty acids described in Japanese Patent No. 5622543. Specifically, the silver powder is first dissolved in acid, and then an organic solvent is mixed therewith to extract the entire amount of surface treatment agent into the organic solvent phase. A predetermined amount of the organic solvent phase is then separated and evaporated to dryness, and the remaining solid matter is measured for its carbon content using a carbon-sulfur analyzer, whereby the amount of carbon attached can be calculated.
[0076] For example, if the surface treatment agent is specified to be stearic acid and the spherical silver powder does not contain any carbon source other than stearic acid, the method for measuring stearic acid is as follows.
[0077] When a calibration curve is obtained by measuring the carbon amount (strength) of each standard solution containing different amounts (mg) of stearic acid using a carbon-sulfur analyzer, the slope of the curve is defined as A (strength / mg). The mass X (mg) and concentration Y (%) of stearic acid in the silver powder can be calculated by extracting a predetermined amount b (mL) of the treatment agent extracted into a total organic solvent volume a (mL) from the silver powder treated with the treatment agent described above, measuring the amount of carbon found by measuring the residual solid matter, and defining the amount of silver powder dissolved in acid as M (g). The mass X and concentration Y of stearic acid can be calculated using the following formulas (A) and (B), respectively: X (mg) = (C / A x a / b) ... (A); Y (%) = X / (M x 1000) x 100 ... (B).
[0078] When oleic acid is used as a treatment agent, the carbon content is measured and determined in the same manner as above. Calculations for oleic acid are also performed using the calibration curve for stearic acid. Since the molecular weight of stearic acid is 284.48, of which the carbon content is 216.19, and the molecular weight of oleic acid is 282.46, of which the carbon content is 216.19, the oleic acid concentration Y' can be calculated using the following formula (C): Oleic acid concentration Y' (%) = Y x (216.19 / 284.48) x (282.46 / 216.19) (C)
[0079] The amount of the surface treatment agent attached is preferably 0.01% by mass or more and 0.11% by mass or less relative to the mass of the spherical silver powder.
[0080] - Separation step - In the separation step, the coated particles are separated from the second liquid. The aggregate of coated particles separated and dried in the separation step is called spherical silver powder. Note that the separation step may optionally include a washing and recovery step in which the coated particles are recovered from the second liquid and washed, and a drying step in which the coated particles are dried.
[0081] In the washing and recovery step, for example, the second liquid is dehydrated to form a cake-like aggregate of coated particles, and the cake of the aggregate of coated particles is washed. Washing in the washing and recovery step may be performed using, for example, pure water. Dehydration in the washing and recovery step may be performed by, for example, decantation or a filter press. The end point of washing may be determined using the electrical conductivity of the washing water. Specifically, the end of washing may be determined when the electrical conductivity of the washing water becomes a predetermined value or less. After washing, the coated particles may be subjected to a drying step in an aggregated state such as a cake-like state.
[0082] In the drying step, the aggregate of coated particles containing moisture and in an agglomerated state is dried. The drying step may be performed by vacuum drying or using an airflow dryer. In the drying step, a high-pressure air flow may be blown onto the aggregate of coated particles, or the cake or silver powder in the drying process may be placed in a mixer having a stirring rotor and stirred, thereby applying a dispersing force to the cake or silver powder in the drying process and promoting dispersion and drying.
[0083] In the drying step, the temperature of the silver powder is usually 100° C. or less. If the temperature of the silver powder is 100° C. or less, sintering between silver particles in the silver powder can be effectively prevented.
[0084] Since the spherical silver powder after drying may be in the form of lumps, a crushing or classification operation may be carried out simultaneously with or after the drying step in order to improve the handleability of the spherical silver powder. Here, improving the handleability of the spherical silver powder means, for example, loosening the spherical silver powder to an appropriate degree so as to ensure fluidity that does not interfere with the addition of a lubricant or the supply operation into an apparatus in the step (partial flattening step) described below, or so as to allow efficient processing in the apparatus.
[0085] The spherical silver powder obtained in the separation step has a specific surface area diameter of 1.3 μm or more and 2.0 μm or less, calculated from the specific surface area (BET specific surface area) determined by the BET method after mixing with a lubricant described later. Here, the specific surface area diameter is the specific surface area A (m 2 The specific surface area diameter (μm) can be calculated based on the specific surface area (A / g) and the density ρ of silver using the following formula (D): specific surface area diameter (μm)=6 / (A×ρ) (D)
[0086] -Partial flattening step- In this step, the spherical silver powder, a lubricant, and a medium are stirred in a container to obtain silver powder A that is partially flattened to the extent that the spherical silver powder becomes silver particles A1 having a large aspect ratio and silver particles A2 having a small aspect ratio and a high degree of rectangularity.
[0087] Here, the partial flattening step includes a lubricant mixing step in which the spherical silver powder and a lubricant are mixed for the purpose of uniformly dispersing the lubricant on the surface of the spherical silver powder. In the lubricant mixing step, a lubricant may be added to spherical silver powder that has been suitably disintegrated by crushing, and the mixture may be stirred and mixed using a crusher. For example, the silver powder may be placed in a Henschel-type mixer (manufactured by Mitsui Mining Co., Ltd., FM Mixer, Model FM75, using SO-type stirring blades) or a jet mill-type mixer, and the lubricant may be added and stirred to mix the spherical silver powder and the lubricant. The spherical silver powder may remain in a suitably aggregated state after the lubricant mixing step. In this step, the coated particles in the spherical silver powder after mixing with the lubricant collide with media in a container with a small number of collisions, thereby partially flattening the particles and obtaining silver powder A, which is an aggregate of silver particles coated with the lubricant. Among the coated particles in the silver powder, those that have undergone a relatively large number of collisions become silver particles A1, which have a large aspect ratio, while those that have undergone a relatively small number of collisions become silver particles A2, which have a small aspect ratio and a large degree of rectangularity. The number of collisions with the media is controlled by adjusting the filling rate of the media and silver powder in the stirring vessel and the amount of energy accumulated over time and the rotation speed of the stirring vessel so that silver particles A1 and silver particles A2 coexist (so that only silver particles A1 do not exist).
[0088] Examples of lubricants include fatty acids such as stearic acid, palmitic acid, linoleic acid, linolenic acid, and oleic acid. Among these, unsaturated fatty acids such as linoleic acid, linolenic acid, and oleic acid are preferred. The amount of lubricant added is, for example, 0.05% by mass or more and 0.3% by mass or less relative to the mass of the spherical silver powder.
[0089] For example, the partial flattening step may be performed by repurposing a so-called media mill, such as a ball mill or a bead mill. Known materials such as SUS and zirconia can be used as the media. Stirring in the media mill may be performed by rotating the container or a stirring paddle, or by vibrating the container.
[0090] The partially flattening step preferably includes a step of further performing a crushing treatment using a Henschel mixer, a jet mill mixer, or the like after the collision with the media. This crushing treatment crushes silver particles that have become too large due to the collision with the media, and the resulting particle size is reduced to a cumulative 90% particle diameter (D 90 ), cumulative 95% particle diameter (D 95 ), and the particle diameter of cumulative 100% (i.e., the largest particle) (D MAX It is also preferable to reduce the value of . Note that, in the crushing treatment step, it is preferable to use a jet mill type mixer, since it is possible to effectively reduce the particle sizes of various particles.
[0091] When a jet mill mixer is used in the above-described crushing step, the crushed silver powder may be treated in a cyclone or the like in the partial flattening step to remove small particles (such as shavings, e.g., particle size less than 0.1 μm). Note that the cyclone may be equipped with an additional airflow to increase collection efficiency.
[0092] <Silver Powder B> Silver powder B is made of silver particles B.
[0093] The average aspect ratio of silver particles B must be less than 1.5, preferably 1.4 or less, and more preferably 1.35 or less. When the average aspect ratio of silver particles B is less than 1.5, a mixed silver powder that can effectively reduce the resistivity of a conductive film can be obtained. On the other hand, the average aspect ratio of particles B is, for example, 1.1 or more, or may be 1.2 or more, or 1.25 or more.
[0094] The average shape factor of the silver particles B is, for example, 1 or more, or may be 1.3 or more, or 1.5 or more, and is, for example, 1.7 or less, or may be 1.6 or less.
[0095] The average equivalent circle diameter (Heywood diameter) of silver particles B is, for example, 0.1 μm or more, or may be 0.3 μm or more, and is, for example, 1 μm or less, or may be 0.5 μm or less.
[0096] The cumulative 50% particle size (D) of silver powder B measured by laser diffraction scattering particle size distribution measurement 50 ) is, for example, 0.3 μm or more, and may be 0.5 μm or more, and is, for example, 1.3 μm or less, and may be 1 μm or less.
[0097] The pre-treatment step, mixing step, and post-treatment step in the method for producing the mixed silver powder of the present invention will be described below.
[0098] <Pretreatment Step> In the pretreatment step, prior to the mixing step, a surface treatment agent is applied to at least one of silver powder A and silver powder B using a polycarboxylic acid. Here, in the pretreatment step, a mixed silver powder that can effectively reduce the resistivity of the conductive film can be obtained, so it is preferable to apply a surface treatment agent to silver powder A using a polycarboxylic acid.
[0099] In the pretreatment step, the treatment of adhering a surface treatment agent to the silver powder with a polycarboxylic acid is not particularly limited, and can be carried out using, for example, a crusher such as a sample mill or a Henschel mixer. The time for the treatment of adhering a surface treatment agent to the silver powder with a polycarboxylic acid is usually from 1 minute to 30 minutes.
[0100] The polycarboxylic acid used in the surface treatment agent attachment treatment in the pretreatment step is not particularly limited and may be any of those known in the art, but since a mixed silver powder capable of effectively reducing the resistivity of the conductive film can be obtained, the polycarboxylic acid is preferably an aliphatic polycarboxylic acid, and more preferably a saturated aliphatic polycarboxylic acid. More specifically, the polycarboxylic acid is preferably at least one polycarboxylic acid selected from the group consisting of oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, dodecanedioic acid, malic acid, diethylglutaric acid, 3-methyladipic acid, butylmalonic acid, maleic acid, diglycolic acid, and citric acid, and adipic acid is particularly preferred.
[0101] Here, the polycarboxylic acid may be used as a solution dissolved in a solvent. Examples of solvents that can be used to dissolve the polycarboxylic acid include alcohols such as methanol, ethanol, and propanol. Among these, ethanol is preferred.
[0102] In the pretreatment step, the use rate of the polycarboxylic acid relative to the total of silver powder A and silver powder B is preferably 0.01% by mass or more, more preferably 0.02% by mass or more, and preferably 0.15% by mass or less, more preferably 0.1% by mass or less, and even more preferably 0.05% by mass or less. When the content rate of the polycarboxylic acid is within the above range, a mixed silver powder capable of effectively reducing the resistivity of the conductive film can be obtained.
[0103] <Mixing Step> In the mixing step, a mixture is obtained by mixing silver powder A containing silver particles A1 and silver particles A2 with silver powder B consisting of silver particles B. Note that if a pretreatment step is carried out before the mixing step, the mixture obtained in the mixing step may correspond to the target mixed silver powder.
[0104] The mixing ratio of silver powder B to silver powder A (silver powder B / silver powder A) is, for example, 10 / 90 or more by mass, or may be 20 / 80 or more, or 30 / 70 or more, or may be, for example, 90 / 10 or less, 60 / 40 or less, or 40 / 60 or less. When the mixing ratio of silver powder B to silver powder A is within the above range, a mixed silver powder can be obtained that can effectively reduce the resistivity of the conductive film.
[0105] <Post-treatment step> In the post-treatment step, the mixture obtained in the mixing step is treated with a polycarboxylic acid to adhere a surface treatment agent. The mixture treated with the surface treatment agent in the post-treatment step can correspond to the target mixed silver powder.
[0106] In the post-treatment step, the treatment of the mixture with a polycarboxylic acid to adhere a surface treatment agent thereto can be carried out using, for example, a crusher such as a sample mill, a Henschel mixer, etc. The time for the treatment of the mixture with a polycarboxylic acid to adhere a surface treatment agent thereto is usually from 1 minute to 30 minutes.
[0107] The polycarboxylic acid used in the surface treatment agent attachment treatment in the post-treatment step is not particularly limited and may be any of those known in the art, but since a mixed silver powder capable of effectively reducing the resistivity of the conductive film can be obtained, the polycarboxylic acid is preferably an aliphatic polycarboxylic acid, and more preferably a saturated aliphatic polycarboxylic acid. More specifically, the polycarboxylic acid is preferably at least one polycarboxylic acid selected from the group consisting of oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, dodecanedioic acid, malic acid, diethylglutaric acid, 3-methyladipic acid, butylmalonic acid, maleic acid, diglycolic acid, and citric acid, and adipic acid is particularly preferred.
[0108] Here, the polycarboxylic acid may be used as a solution dissolved in a solvent. Examples of solvents that can be used to dissolve the polycarboxylic acid include alcohols such as methanol, ethanol, and propanol.
[0109] In the post-treatment step, the content of the polycarboxylic acid relative to the total of silver powder A and silver powder B is preferably 0.01% by mass or more, more preferably 0.02% by mass or more, and is preferably 0.15% by mass or less, more preferably 0.1% by mass or less, and even more preferably 0.05% by mass or less. When the content of the polycarboxylic acid is within the above range, a mixed silver powder capable of effectively reducing the resistivity of the conductive film can be obtained.
[0110] (Conductive Paste) The conductive paste of the present invention contains the above-mentioned mixed silver powder of the present invention, a binder, and a solvent, and may optionally contain components other than the mixed silver powder, binder, and solvent (hereinafter, these may be referred to as "other components"). Because the conductive paste of the present invention contains the mixed silver powder of the present invention, it can reduce the resistivity of the conductive film.
[0111] The content of the mixed silver powder in the conductive paste is preferably 50% by mass or more, more preferably 80% by mass or more, and is preferably 98% by mass or less, and more preferably 95% by mass or less. If the content of the mixed silver powder in the conductive paste is within the above range, the resistivity of the conductive film can be effectively reduced.
[0112] Examples of binders for the conductive paste include epoxy resins, acrylic resins, polyester resins, polyimide resins, polyurethane resins, phenoxy resins, silicone resins, ethyl cellulose, etc. These may be used alone or in combination of two or more.
[0113] Examples of the solvent (i.e., dispersion medium) for the conductive paste include terpineol, butyl carbitol, butyl carbitol acetate, texanol, etc. These may be used alone or in combination of two or more.
[0114] Other components that may be contained in the conductive paste include, for example, glass frit, dispersants, surfactants, viscosity modifiers, etc. These may be used alone or in combination of two or more.
[0115] For producing the conductive paste, that is, for dispersing and kneading, ultrasonic dispersion, a disper, a three-roll mill, a ball mill, a bead mill, a two-axis kneader, a planetary stirrer, or the like may be used.
[0116] The viscosity of the conductive paste is not particularly limited and can be selected appropriately depending on the purpose, but is preferably 150 Pa·s or more, more preferably 200 Pa·s or more, and preferably 800 Pa·s or less, and more preferably 750 Pa·s or less, under conditions of a paste temperature of 25°C and a rotation speed of 1 rpm. If the viscosity of the conductive paste is 150 Pa·s or more, the occurrence of "bleeding" during printing can be effectively suppressed. On the other hand, if the viscosity of the conductive paste is 800 Pa·s or less, the occurrence of printing unevenness can be effectively suppressed.
[0117] The conductive paste of the present invention is suitable for forming conductive films, i.e., for forming conductive patterns on substrates or electrodes. For example, it can be applied directly to various substrates such as silicon wafers for solar cells, films for touch panels, and glass for EL devices, or, if necessary, coated or printed onto a transparent conductive film on a substrate to form a conductive film. The conductive film obtained using the conductive paste of the present invention is suitable for use as an electrode or electrical wiring for, for example, collecting electrodes for solar cells, external electrodes for chip-type electronic components, RFID, electromagnetic wave shielding, vibrator bonding, membrane switches, electroluminescence, and the like.
[0118] The conductive paste can be printed on a substrate by, for example, screen printing, offset printing, photolithography, or the like, to form a conductive film of a desired shape.
[0119] The present invention will be described in more detail below using examples, but the present invention is not limited to the following examples in any way.
[0120] Example 1 Preparation of Silver Powder A Reduction Step First, 167.1 kg of a 26% by mass aqueous ammonia solution was added to 2922 kg of a silver nitrate aqueous solution containing 68.8 kg of silver as a silver ion aqueous solution to produce a silver ammine complex aqueous solution. Furthermore, 266 kg of a 6% by mass aqueous hydrazine solution was added as a reducing agent to this silver ammine complex aqueous solution to obtain a first liquid. The adding rate of the reducing agent was 80 L / min.
[0121] [Surface Treatment Agent Addition Step] Five minutes after the completion of the reducing agent addition, 68.8 g of oleic acid (0.1 mass % relative to the mass of silver contained in the aqueous silver ammine complex solution (calculated as 68.8 g of oleic acid / 68,800 g of silver x 100)) was added as a surface treatment agent. After the addition of the surface treatment agent, the mixture was stirred for five minutes to obtain a second liquid. The second liquid was in the form of a slurry containing coated particles.
[0122] [Separation Step] The second liquid was filtered, washed with water, and then dried to obtain spherical silver powder.
[0123] [Lubricant Mixing Step] 16.25 kg of the spherical silver powder was charged into a Henschel mixer (manufactured by Mitsui Mining Co., Ltd., FM mixer, model FM75, using an SO-type stirring blade) and stirred at 900 rpm for 1 minute. After that, 37.4 g of oleic acid (0.23 mass% relative to the mass of the spherical silver powder (calculated as 37.4 g oleic acid / 16,250 g spherical silver powder x 100)) was charged as a lubricant, and the mixture was mixed and stirred for 20 minutes at a stirring blade rotation speed of 2,200 rpm. This step was performed in multiple batches to obtain a lubricant-mixed silver powder in which the lubricant was dispersed on the surfaces of the silver particles.
[0124] [Step of Partially Flattening] 32 kg of the above-mentioned lubricant-mixed silver powder and 256 kg of SUS balls (diameter 1.6 mm) were charged into a vibration mill (FVR-20 model, manufactured by Chuo Kakoki Co., Ltd.) and treated at a vibration frequency of 780 vpm for 135 minutes to partially flatten the lubricant-mixed silver powder.
[0125] The partially flattened silver powder (hereinafter also referred to as "silver powder") was separated from the SUS balls and then crushed by stirring at 2600 rpm for 25 minutes in the above-mentioned Henschel mixer. Further, in order to remove coarse particles from the crushed silver powder, it was sieved using a dry sieving device (manufactured by Freund Turbo Corporation, TS125x200 type / screen with 27 μm openings) to obtain silver powder A.
[0126] [Cross-Section Observation of Silver Powder A] The silver particles in Silver Powder A were observed, and the average aspect ratio of Silver Particles A1, the average aspect ratio of Silver Particles A2, and the average ratio β calculated by the following formula (2) were calculated by the following method: Ratio β = perimeter of Silver Particles A2 / (long side length of Silver Particles A2 × 2 + short side length of Silver Particles A2 × 2) (2) Specifically, Silver Powder A was first placed in a resin (EpoFix resin, manufactured by Struers) and a hardener (EpoFix hardener, manufactured by Struers) and solidified, and the cross-sections of the silver particles were exposed by polishing with a cross-section polisher (ArBlade 5000, manufactured by Japan High-Technologies Corporation), and each silver particle was observed at 5,000x magnification with a scanning electron microscope (JEOL JSM-IT300LV, manufactured by JEOL Ltd.). Here, based on the contrast between the insulating resin and the conductive silver particles, silver particles with a clear outline and whose periphery can be clearly seen are considered to have an exposed cross section. Then, on the polished cross section of a resin block in which silver powder A was embedded in resin, 100 or more silver particles were arbitrarily selected from among the silver particles whose periphery could be clearly seen. Image analysis software (Mac-View, image analysis particle size distribution measurement software manufactured by Mountec Co., Ltd.) was used to trace the periphery of each silver particle to measure the long side length, short side length, and perimeter of each silver particle. The long side length and short side length were automatically calculated to minimize the area of a rectangle circumscribing the outline of each silver particle. Next, silver particles with an aspect ratio of 2 or greater were designated silver particles A1, and silver particles with an aspect ratio of less than 2 were designated silver particles A2. The average aspect ratio for silver particles A1, and the average aspect ratio and average β ratio for silver particles A2 were calculated. The results are shown in Table 1.
[0127] <Preparation of Silver Powder B> "AG-2-1C" manufactured by DOWA High-Tech Co., Ltd. was prepared as Silver Powder B. The volume-based cumulative 50% particle diameter (D 50 The particle diameter was 0.80 μm, and the average shape factor, measured using image analysis particle size distribution measurement software Mac-View manufactured by Mountech Co., Ltd., was 1.53, the average aspect ratio was 1.3, and the average Heywood diameter was 0.34 μm.
[0128] <Production of Mixed Silver Powder> [Pretreatment Step] First, a solution was prepared by dissolving 0.056 g of adipic acid (manufactured by Junsei Chemical Co., Ltd.) in 0.504 g of ethanol solvent. Next, this solution was added to 120 g of the silver powder A obtained above, and the mixture was mixed for 4.5 minutes using a sample mill (manufactured by Kyoritsu Riko Co., Ltd., SK-M10), thereby treating the surface of the silver powder A with adipic acid. Oleic acid is used as a surface treatment agent and lubricant in the manufacturing process of silver powder A, and this treatment allowed adipic acid to adhere to the surface of silver powder A as an additional surface treatment agent.
[0129] [Mixing Step] Silver powder A, which had been treated with a surface treatment agent in the pretreatment step, and silver powder B were mixed in a mass ratio of 60:40 (silver powder B / silver powder A = 40 / 60) to produce a mixture (i.e., a mixed silver powder). The resulting mixed silver powder was used to perform the various measurements described below. A scanning electron microscope photograph of the resulting mixed silver powder is shown in Figure 2.
[0130] [Measurement of BET Specific Surface Area] The BET specific surface area of the mixed silver powder obtained above was measured by the BET single-point method using nitrogen adsorption using a BET specific surface area measuring device (Macsorb HM-model 1210, manufactured by MOUNTECH Co., Ltd.). In measuring the BET specific surface area, the degassing conditions before measurement were 60°C and 10 minutes. The results are shown in Table 2.
[0131] [Measurement of particle size distribution] The cumulative 10% particle diameter (D 10 ), cumulative 50% particle diameter (D 50 ), cumulative 90% particle diameter (D 90 ), and cumulative 95% particle diameter (D95 ), and the particle diameter of cumulative 100% (i.e., the largest particle) (D MAX ) was measured by the following method. 50 ) to the cumulative 90% particle diameter (D 90 ) and cumulative 10% particle size (D 10 ) and the ratio of the difference [(D 90 -D 10 ) / D 50 The results are shown in Table 2. 0.1 g of the mixed silver powder was added to 40 mL of isopropyl alcohol (IPA) and dispersed for 2 minutes using an ultrasonic homogenizer (apparatus name: US-150T, manufactured by Nippon Seiki Seisakusho Co., Ltd.; 19.5 kHz, tip diameter 18 mm), and then the particle size distribution was measured using a laser diffraction / scattering particle size distribution analyzer (Microtrac MT-3300 EXII, manufactured by Microtrac Bell Corporation).
[0132] [Measurement of Ignition Loss (Ig-Loss)] The ignition loss (Ig-Loss) value of the mixed silver powder obtained above was determined by precisely weighing 3 g of the mixed silver powder sample (weight: w1), placing it in a porcelain crucible, heating it to 800°C, and holding it at 800°C for 30 minutes, a time sufficient to reach constant weight, followed by cooling and reweighing it (weight: w2), and calculating the ignition loss (Ig-Loss) value (mass %) = (w1 - w2) / w1 × 100. The results are shown in Table 2.
[0133] [Measurement of tap density] The tap density of the mixed silver powder obtained above was measured using a tap density measuring device (Shibayama Scientific Co., Ltd., bulk specific gravity measuring device SS-DA-2) by weighing 30 g of silver powder, placing it in a 20 mL test tube, and tapping it 1,000 times from a drop of 20 mm, and then calculating it from the formula "tap density = sample mass (g) / sample volume after tapping (mL)". The results are shown in Table 2.
[0134] [Cross-section observation of mixed silver powder] Silver particles in the mixed silver powder were observed, and the following were calculated by the following methods: (A) for the mixed silver powder (all silver particles), the overall average shape factor, the overall average long side length, the overall average short side length, and the overall average aspect ratio; (B) for the first silver particles, the number proportion, the average shape factor, the average short side length, and the average aspect ratio; (C) for the second silver particles, the number proportion, the average shape factor, the average short side length, and the average aspect ratio, as well as the average ratio α calculated by the following formula (1): Ratio α = perimeter of second silver particles / (long side length of second silver particles × 2 + short side length of second silver particles × 2) (1); and (D) for the tertiary silver particles, the number proportion, the average shape factor, the average short side length, and the average aspect ratio. Specifically, the mixed silver powder was first placed in a resin (Epofix resin, manufactured by Struers) and a hardener (Epofix hardener, manufactured by Struers) and solidified, and the cross-sections of the silver particles were exposed by polishing with a cross-section polisher (ArBlade 5000, manufactured by Japan High-Technologies Corporation). Each silver particle was then observed at 5,000x magnification (3,000x magnification in the case of Comparative Example 3, described below) with a scanning electron microscope (JEOL JSM-IT300LV, manufactured by JEOL Ltd.). Here, silver particles whose outlines are clear and whose peripheries are clearly visible due to the contrast between the insulating resin and the conductive silver particles are considered to have exposed cross-sections. Then, on the polished cross section of a resin block in which the mixed silver powder was embedded in resin, at least 100 silver particles were arbitrarily selected from among the silver particles whose peripheries were clearly visible. Image analysis software (Mac-View, image analysis particle size distribution measurement software manufactured by Mountec Co., Ltd.) was used to trace the periphery of each silver particle, thereby measuring the long side length, short side length, perimeter, area, and maximum length of each silver particle. The long side length and short side length were automatically calculated to determine the minimum area of a rectangle circumscribing the outer shape of each silver particle. Using these measured values, the overall average shape factor, overall average long side length, overall average short side length, and overall average aspect ratio were calculated for (A) the mixed silver powder (all silver particles). The results are shown in Table 2.Next, silver particles with a long side length of 3 μm or more were designated as first silver particles, silver particles with a long side length of 0.5 μm or more but less than 3 μm were designated as second silver particles, and silver particles with a long side length of less than 0.5 μm were designated as tertiary silver particles. (B) For the first silver particles, the number proportion, average shape factor, average short side length, and average aspect ratio were calculated. (C) For the second silver particles, the number proportion, average shape factor, average short side length, and average aspect ratio, as well as the average ratio α were calculated. (D) For the tertiary silver particles, the number proportion, average shape factor, average short side length, and average aspect ratio were calculated. The results are shown in Table 2.
[0135] <Preparation of Conductive Paste> The conductive paste contained the mixed silver powder obtained above in an amount of 91% by mass of Ag, 3.8% by mass of epoxy resin A (manufactured by ADEKA, EP4901E), 1.0% by mass of epoxy resin B (manufactured by Mitsubishi Chemical, jER1009), 0.2% by mass of curing agent (manufactured by Wako Pure Chemical Industries, boron trifluoride monoethylamine complex), and 4.0% by mass of solvent (BCA: butyl carbitol acetate). These were mixed and stirred at 1200 rpm for 30 seconds using a propellerless rotary and revolutionary stirring and degassing device (VMX-N360 manufactured by EME Corporation). The mixture was then kneaded using a three-roll mill (manufactured by EXAKT, 80S) with a roll gap of 100 μm to 20 μm to obtain a conductive paste. The viscosity of the obtained conductive paste was measured, and the viscosity was adjusted to 300 Pa s using BCA. The viscosity of the conductive paste was measured using a viscometer (DV-III, CP-52 cone, manufactured by Brookfield) at 25° C. and 1 rpm for 5 minutes.
[0136] <Formation of conductive film> A line pattern of 500 μm wide and 37.5 mm long was printed on the conductive paste obtained above using a screen printer (MT-320T manufactured by Microtec) at a squeegee pressure of 0.18 MPa to form a conductive paste film. The obtained film was then heat-cured at 200° C. for 30 minutes using an air circulation dryer to form a conductive film.
[0137] [Specific Resistivity Value] The average thickness of the obtained conductive film was measured by measuring the difference in level between the non-printed portion of the alumina substrate and the conductive film portion using a surface roughness meter (Surfcom 480B-12 manufactured by Tokyo Seimitsu Co., Ltd.). Next, the resistance value of the conductive film was measured using a digital multimeter (R6551 manufactured by ADVANTEST Co., Ltd.). The volume of the conductive film was then calculated from the size of the conductive film (average thickness, width, length), and the specific resistance value was calculated from this volume and the measured resistance value. The results are shown in Table 2.
[0138] (Example 2) Various operations and measurements were carried out in the same manner as in Example 1, except that the mixed silver powder was produced by the following method. The results are shown in Tables 1 and 2. A scanning electron microscope photograph of the obtained mixed silver powder is shown in Figure 3.
[0139] <Production of Mixed Silver Powder> [Pretreatment Step] "AG-2-1C" was prepared as silver powder B, and a surface treatment agent was applied using adipic acid. The silver powder B had a volume-based cumulative 50% particle diameter (D 50 The particle diameter was 0.80 μm, and the average shape factor, measured using image analysis particle size distribution measurement software Mac-View manufactured by Mountech Co., Ltd., for a total of 100 or more particle outer shapes, was 1.53, the average aspect ratio was 1.3, and the average Heywood diameter was 0.34 μm. For the surface treatment agent adhesion treatment using adipic acid, first, a solution was prepared by dissolving 0.084 g of adipic acid (manufactured by Junsei Chemical Co., Ltd.) in 0.756 g of ethanol solvent. Next, this solution was added to 120 g of "AG-2-1C" and mixed for 4.5 minutes using a sample mill (SK-M10 manufactured by Kyoritsu Riko Co., Ltd.), and the surface of Silver Powder B was treated with adipic acid.
[0140] [Crushing Step] First, 120 g of silver powder A obtained by the same method as the method for preparing silver powder A in Example 1 above was crushed for 4.5 minutes using a sample mill (SK-M10, manufactured by Kyoritsu Riko Co., Ltd.).
[0141] [Mixing Step] The silver powder A obtained in the above-mentioned crushing step and the silver powder B that had been treated to adhere a surface treatment agent were mixed in a mass ratio of 60:40 (silver powder B / silver powder A = 40 / 60) to produce a mixture (i.e., mixed silver powder).
[0142] (Example 3) Various operations and measurements were carried out in the same manner as in Example 1, except that the mixed silver powder was produced by the following method. The results are shown in Tables 1 and 2. A scanning electron microscope photograph of the obtained mixed silver powder is shown in Figure 4.
[0143] <Production of Mixed Silver Powder> [Mixing Step] First, 72 g of silver powder A obtained by the same method as the method for preparing silver powder A in Example 1 above was mixed with 48 g of silver powder B to obtain a mixture.
[0144] [Post-treatment step] A solution was prepared by dissolving 0.0336 g of adipic acid (manufactured by Junsei Chemical Co., Ltd.) in 0.3024 g of ethanol solvent. Next, this solution was added to 120 g of the mixture obtained in the above mixing step, and the mixture was mixed for 7.5 minutes using a sample mill (manufactured by Kyoritsu Riko Co., Ltd., SK-M10), and the surface of the mixture was treated with adipic acid to produce a mixed silver powder.
[0145] Comparative Example 1 Various operations and measurements were carried out in the same manner as in Example 1, except that without mixing in silver powder B, 120 g of silver powder A was taken, and a solution of adipic acid (0.0336 g of adipic acid manufactured by Junsei Chemical Co., Ltd.) dissolved in 0.3024 g of ethanol solvent was added, and the mixture was mixed for 4.5 minutes using a sample mill to adhere adipic acid to the silver powder surface as an additional surface treatment agent. The results are shown in Tables 1 and 2. A scanning electron microscope photograph of the resulting mixed silver powder is shown in Figure 5.
[0146] (Comparative Example 2) Various operations and measurements were carried out in the same manner as in Example 1, except that the mixed silver powder was produced by the following method. The results are shown in Tables 1 and 2. A scanning electron microscope photograph of the obtained mixed silver powder is shown in FIG.
[0147] <Production of Mixed Silver Powder> [Crushing Step] First, 120 g of silver powder A obtained by the same method as the preparation method of silver powder A in Example 1 above was crushed for 4.5 minutes using a sample mill (SK-M10, manufactured by Kyoritsu Riko Co., Ltd.).
[0148] [Mixing Step] The silver powder A obtained in the above-mentioned crushing step and the silver powder B were mixed in a mass ratio of 60:40 (silver powder B / silver powder A=40 / 60) to produce a mixture (i.e., mixed silver powder).
[0149] Comparative Example 3 Various operations and measurements were performed in the same manner as in Example 1, except that no surface treatment agent was added in the surface treatment agent addition step in Example 1, the second liquid was filtered, washed with water, dried, and then heat-treated at 150°C for 10 hours to promote particle aggregation, the amount of lubricant added in the lubricant mixing step was 48.8 g (0.30 mass% relative to the mass of the silver powder supplied to the lubricant mixing step), the partial flattening step was performed as follows, and the mixed silver powder was produced by the following method. The results are shown in Tables 1 and 2. A scanning electron microscope photograph of the obtained mixed silver powder is shown in Figure 7. Cross-sectional observation of the mixed silver powder in Comparative Example 3 was performed by observing each silver particle at 3,000x magnification using a scanning electron microscope.
[0150] [Step of Partially Flattening] 32 kg of the lubricant-mixed silver powder and 256 kg of SUS balls (diameter 1.6 mm) were placed in a vibration mill (FVR-20 model, manufactured by Chuo Kakoki Co., Ltd.) and subjected to a partial flattening treatment at a vibration frequency of 1,200 vpm for 120 minutes to partially flatten the lubricant-mixed silver powder, thereby obtaining silver powder. Since the vibration frequency was higher than in Example 1, flattening was more advanced than in Example 1, and the number of silver particles with a large aspect ratio increased.
[0151] The silver(II) powder was separated from the SUS balls and then crushed by stirring at 2600 rpm for 25 minutes in the above-mentioned Henschel mixer. Further, in order to remove coarse particles from the crushed silver(II) powder, it was sieved using a dry sieving device (manufactured by Freund Turbo Corporation, TS125x200 type / screen with 27 μm openings) to obtain silver powder A.
[0152] <Production of Mixed Silver Powder> [Pretreatment Step] "AG-2-1C" was prepared as Silver Powder B, and a surface treatment agent was applied using adipic acid. For the surface treatment agent application treatment using adipic acid, a solution was first prepared by dissolving 0.084 g of adipic acid (manufactured by Junsei Chemical Co., Ltd.) in 0.756 g of ethanol solvent. This solution was then added to 120 g of "AG-2-1C" and mixed for 4.5 minutes using a sample mill (SK-M10, manufactured by Kyoritsu Riko Co., Ltd.), thereby treating the surface of Silver Powder B with adipic acid.
[0153] [Mixing Step] The silver powder A obtained above and silver powder B that had been treated to adhere a surface treatment agent were mixed in a mass ratio of 60:40 (silver powder B / silver powder A=40 / 60) to produce a mixture (i.e., mixed silver powder).
[0154]
[0155]
[0156] As is clear from Table 2, the mixed silver powders of Examples 1 to 3 can reduce the resistivity of the conductive film compared to the mixed silver powders of Comparative Examples 1 to 3.
[0157] The adipic acid content in the mixed silver powder was measured using the following method. 0.1 g to 0.2 g of sample silver powder was weighed, and 1 mL of Hydrogen Chloride-Methanol Reagent (5-10%) [for Esterification] (manufactured by Tokyo Chemical Industry Co., Ltd.) was added as a methylation reagent using a measuring pipette. The mixture was then subjected to ultrasonic irradiation for 1 minute and warmed in a 50°C water bath for 30 minutes. Next, ultrasonic irradiation was performed for 1 minute, and the adipic acid eluted by these irradiations was methylated to produce dimethyl adipate. Next, 5 mL of hexane and 4 mL of distilled water were added to the sample solution after methylation, and shaking extraction was performed four times for 1 minute, thereby extracting dimethyl adipate into the organic solvent (hexane). Then, using methyl arachidate as an internal standard, hexane was added to the organic solvent into which dimethyl adipate had been extracted to a constant volume of 25 mL, and the resulting solution was subjected to measurement by MS ionization EI method using a gas chromatographic quantitative analyzer GC-MS (GC: Agilent Technologies 7980B, MS: Agilent Technologies 5977B), and the amount of adipic acid was calculated by conversion calculation from the amount of dimethyl adipate obtained. The amount of adipic acid (mass %) contained in the sample silver powder was quantified by comparing this calculated amount of adipic acid with the amount of sample silver powder.
[0158] When the amount of adipic acid contained in the mixed silver powder was examined using this method for measuring the content of adipic acid, it was 0.021% by mass in Example 1, 0.023% by mass in Example 2, 0.024% by mass in Example 3, 0.025% by mass in Comparative Example 1, and 0.022% by mass in Comparative Example 3. It was 0.001% by mass or less in Comparative Example 2, to which no adipic acid was added.
[0159] Example 4 Various operations and measurements were carried out in the same manner as in Example 1, except that the partial flattening step in the preparation of silver powder A and the production of the mixed silver powder were carried out by the following methods. The results are shown in Tables 3 and 4. A scanning electron microscope photograph of the obtained mixed silver powder is shown in Figure 8.
[0160] <Preparation of Silver Powder A> [Step of Partial Flattening] 32 kg of the above-mentioned lubricant-mixed silver powder and 256 kg of SUS balls (diameter 1.6 mm) were placed in a vibration mill (FVR-20 model, manufactured by Chuo Kakoki Co., Ltd.) and treated at a vibration frequency of 780 vpm for 135 minutes to partially flatten the lubricant-mixed silver powder.
[0161] The partially flattened silver powder was separated from the SUS balls and then mixed in a jet mill type mixer (Nisshin Engineering Jet Mill CJ-25) with compressed air (0.7 MPa) supplied per kg of silver powder at a rate of 11.6 m 3 The crushed silver powder was then crushed in a cyclone under the condition that the amount of air used for pneumatic transport per kg of silver powder was 46 m 3 The cyclone was treated under the conditions of (1) to (3), and small particles (shavings, for example, particle size less than 0.1 μm) were removed from the crushed silver powder. A device that adds an additional air flow to the cyclone to increase collection efficiency may be used.
[0162] <Production of Mixed Silver Powder> [Mixing Step] 84 g of the silver powder A obtained above and 36 g of silver powder B were mixed to obtain a mixture.
[0163] [Post-treatment step] A solution was prepared by dissolving 0.0336 g of adipic acid (manufactured by Junsei Chemical Co., Ltd.) in 0.3024 g of ethanol solvent. Next, this solution was added to 120 g of the mixture obtained in the above mixing step, and the mixture was mixed for 4.5 minutes using a sample mill (manufactured by Kyoritsu Riko Co., Ltd., SK-M10), and the surface of the mixture was treated with adipic acid to produce a mixed silver powder.
[0164] Comparative Example 4 Various operations and measurements were carried out in the same manner as in Example 4, except that without mixing in silver powder B, 120 g of silver powder A was taken, and a solution of adipic acid (0.0336 g of adipic acid manufactured by Junsei Chemical Co., Ltd.) dissolved in 0.3024 g of ethanol solvent was added, and the mixture was mixed for 4.5 minutes using a sample mill to adhere adipic acid to the silver powder surface as an additional surface treatment agent. The results are shown in Tables 3 and 4. A scanning electron microscope photograph of the resulting mixed silver powder is shown in Figure 9.
[0165] Comparative Example 5 Various operations and measurements were carried out in the same manner as in Example 4, except that the mixed silver powder was produced by the following method. The results are shown in Tables 3 and 4. A scanning electron microscope photograph of the obtained mixed silver powder is shown in FIG.
[0166] <Production of Mixed Silver Powder> [Crushing Step] First, 120 g of silver powder A obtained by the same method as the preparation method of silver powder A in Example 4 above was crushed for 4.5 minutes using a sample mill (SK-M10, manufactured by Kyoritsu Riko Co., Ltd.).
[0167] [Mixing Step] The silver powder A obtained in the above-mentioned crushing step and the silver powder B were mixed in a mass ratio of 70:30 (silver powder B / silver powder A=30 / 70) to produce a mixture (i.e., mixed silver powder).
[0168]
[0169]
[0170] As is clear from Table 4, the mixed silver powder of Example 4 can reduce the specific resistance of the conductive film compared to the mixed silver powders of Comparative Examples 4 and 5.
[0171] Furthermore, when the amount of adipic acid contained in the mixed silver powder was examined using the above-mentioned method for measuring the adipic acid content, it was 0.026% by mass in Example 4 and 0.026% by mass in Comparative Example 4. In Comparative Example 5, to which adipic acid was not added, it was 0.001% by mass or less.
[0172] According to the present invention, a mixed silver powder capable of reducing the resistivity of a conductive film can be provided. Also, according to the present invention, a method for producing a mixed silver powder capable of reducing the resistivity of a conductive film can be provided. Also, according to the present invention, a conductive paste capable of reducing the resistivity of a conductive film can be provided.
Claims
1. A mixed silver powder comprising first silver particles, second silver particles, and third silver particles, wherein 100 or more silver particles are observed on a polished cross section of a resin block obtained by embedding the mixed silver powder in resin, and the perimeter of the silver particles and the long side length and short side length of a rectangle which circumscribes the outer shape of the silver particles and has the smallest area are measured, and the first silver particles are silver particles having a long side length of 3 μm or more, the second silver particles are silver particles having a long side length of 0.5 μm or more and less than 3 μm, and the third silver particles are silver particles having a long side length of less than 0.5 μm. In this case, the first silver particles have an average aspect ratio of 2 or more, the second silver particles have an average aspect ratio of 1.5 or more and less than 2, and the third silver particles have an average aspect ratio of less than 1.5, the mixed silver powder having a number ratio of the first silver particles of 0.5% or more and 5% or less, a number ratio of the second silver particles of 10% or more, and a number ratio of the tertiary silver particles of 15% or more, an average value of a ratio α calculated by the following formula (1): ratio α=perimeter of second silver particle / (long side length of second silver particle×2+short side length of second silver particle×2) (1) of 0.84 or more, and a polyvalent carboxylic acid adhered to a surface of at least one type of silver particle selected from the group consisting of the first silver particles, the second silver particles, and the tertiary silver particles.
2. The mixed silver powder according to claim 1, wherein a polyvalent carboxylic acid is attached to the surfaces of the first silver particles and the second silver particles.
3. The mixed silver powder according to claim 1 or 2, wherein the content of the polyvalent carboxylic acid relative to the total of the first silver particles, the second silver particles, and the tertiary silver particles is 0.01 mass% or more and 0.15 mass% or less.
4. The mixed silver powder according to claim 1 or 2, wherein the polycarboxylic acid is at least one polycarboxylic acid selected from the group consisting of oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, dodecanedioic acid, malic acid, diethylglutaric acid, 3-methyladipic acid, butylmalonic acid, maleic acid, diglycolic acid and citric acid.
5. A method for producing a mixture comprising: a mixing step of mixing silver powder A containing silver particles A1 and silver particles A2, and silver powder B consisting of silver particles B to obtain a mixture; and a pretreatment step of treating at least one of the silver powders A and B with a polyvalent carboxylic acid before the mixing step, to attach a surface treatment agent thereto, or a post-treatment step of treating the mixture obtained in the mixing step with a polyvalent carboxylic acid to attach a surface treatment agent thereto, wherein when 100 or more silver particles on a polished cross section of a resin block in which the silver powder A is embedded in a resin and 100 or more silver particles on a polished cross section of a resin block in which the silver powder B is embedded in a resin are observed, and the perimeter of the silver particles and the long side lengths and short side lengths of a rectangle that circumscribes the outer shape of the silver particles and has the smallest area are measured, the silver particles A1 have an average aspect ratio of 2 or more, and the silver particles A2 have an average aspect ratio of less than 2, and the average aspect ratio satisfies the following formula (2):
2. The method for producing a mixed silver powder according to claim 1, wherein an average value of the ratio β calculated by: ratio β=perimeter of silver particles A2 / (length of long side of silver particles A2×2+length of short side of silver particles A2×2) (2) is 0.84 or more, and the silver particles B have an average aspect ratio of less than 1.
5.
6. A method for producing a mixed silver powder as described in claim 5, comprising the pretreatment step, in which the silver powder A is treated to adhere a surface treatment agent thereto using the polyvalent carboxylic acid.
7. A method for producing a mixed silver powder as described in claim 5 or 6, wherein the usage rate of the polyvalent carboxylic acid relative to the total of the silver powder A and the silver powder B is 0.01 mass% or more and 0.15 mass% or less.
8. A method for producing a mixed silver powder according to claim 5 or 6, wherein the polyvalent carboxylic acid used in the surface treatment agent attachment treatment is at least one polyvalent carboxylic acid selected from the group consisting of oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, dodecanedioic acid, malic acid, diethylglutaric acid, 3-methyladipic acid, butylmalonic acid, maleic acid, diglycolic acid and citric acid.
9. A conductive paste comprising the mixed silver powder according to claim 1 or 2, a binder, and a solvent.
Citation Information
Patent Citations
Silver powder, method for producing the same, resin-curing electroconductive paste and method for forming electroconductive film
JP2011140714A
Spherical silver powder and method for producing the same
JP2019108610A
Silver paste and method for producing joined body
JP2022139486A