METHOD FOR PRODUCING TiAl-BASED ALLOY AND TiAl-BASED ALLOY
The method of controlled sintering and high-pressure processing of Ti and Al powders addresses the challenges of segregation in TiAl-based alloy production, resulting in high-quality alloys with enhanced mechanical properties and cost-effective manufacturing.
Patent Information
- Application Number
- PCT/JP2024/019589
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-29
- Filing Date
- 2024-05-28
- Publication Date
- 2024-12-05
AI Technical Summary
Current methods for producing TiAl-based alloys without prealloy powder face challenges such as macro segregation, porosity, and micro segregation, leading to high costs and low quality due to difficulties in sintering and casting, especially when using elemental powders as raw materials.
A method involving vacuum sintering of mixed Ti and Al powders with controlled temperature increase rates and isothermal holding times to adjust Al abundance, combined with high-pressure sintering and HIP treatment, to produce TiAl-based alloys with reduced segregation and improved mechanical properties.
This approach enables the production of TiAl-based alloys with high room temperature ductility and high-temperature strength, suppressing macro and micro segregation, and achieving net-shape or near-net-shape manufacturing, thereby reducing production costs and improving quality.
Smart Images

Figure JP2024019589_05122024_PF_FP_ABST
Abstract
Description
Method for producing TiAl-based alloy and TiAl-based alloy
[0001] The present invention relates to a technology for producing a TiAl-based alloy, which is a lightweight heat-resistant alloy, and more particularly to a technology for producing a TiAl-based alloy having practical properties without using pre-alloy powder as a raw material.
[0002] Titanium-aluminum-based alloys (TiAl-based alloys) are expected to be applied to aircraft, automobiles, and energy industry equipment due to their high specific strength and heat resistance. For example, TiAl-based alloys have already been adopted in some low-pressure turbine blades in aircraft engines as a key to improving fuel efficiency. The most well-known practical alloy currently in use is 4822 alloy (Ti-48Al-2Cr-2Nb at%), developed by GE in the 1990s. 4822 alloy is known as a second-generation alloy (casting alloy). Since the 2000s, third-generation alloys have been developed with increased amounts of β-Ti phase-stabilizing elements, such as Nb, focusing on forgeability and high-temperature properties. One well-known example is TNM alloy (Ti-43.5Al-4Nb-1Mo-0.1B at%).
[0003] Manufacturing methods for TiAl-based alloys can be broadly divided into two: the melting method and the powder method (element powder sintering method). In the melting method, TiAl-based alloys have high melting points and are highly reactive when melted. Therefore, a normal crucible cannot be used; instead, a water-cooled copper crucible must be used in a vacuum or in an inert gas atmosphere. This requires a specialized method, which can lead to the problem of high alloy costs. Furthermore, TiAl-based alloys have difficulty in castability, and when commercialized, they require additional HIP processing to prevent casting defects, which increases costs in terms of yield and quality assurance.
[0004] There have also been many research reports on the powder method. Most of them involve first creating a pre-alloy by melting, then atomizing or powdering it using various methods, and then sintering it into a bulk form. This method makes it possible to stabilize the quality, but it requires a long lead time and is expensive, just like the melting method.
[0005] On the other hand, manufacturing methods using elemental powders as raw materials without using pre-alloyed powders have also been studied for a long time, but when elemental powders are used as raw materials, TiAl-based alloys of practical quality cannot be obtained. This is due to the following problems: (1) the problem of leakage of molten liquid from the sintering mold and macrosegregation caused by fluidization when Al melts during heating in the sintering cycle, and (2) the problem that when Al penetrates around the Ti powder particles, an Al-rich phase is likely to remain on the surface of the Ti particles as a metastable phase (a phase richer than TiAl). 3 , Ti 2 Al 5 (1) The reason is that the standard energy of formation of high-Al compounds such as Cr tends to be low), (2) The amount of oxygen (O) inevitably increases with grain refinement, which adversely affects the mechanical properties of the product, and (3) Vacancy defects tend to occur due to insufficient pressure in the high-temperature range and the grain size of the raw materials. In other words, there are still many challenges to overcome in producing a practical TiAl-based alloy using raw material powders without using pre-alloyed powders.
[0006] In recent years, the technology of powder additive manufacturing (PASM) has been developed to three-dimensionally stack parts with complex shapes. However, when forming parts using TiAl-based alloys, pre-alloy powder is generally used, which, as mentioned above, has the inherent problem of high cost.
[0007] Patent Application No. 2019-051005, Patent Application No. 2019-211349, Patent Application No. 2022-038867
[0008] Musi, M., Clemens, H. et al.; Microstructure, Plasticity, and Ductility of a TNM+ Alloy Densified by Spark Plasma Sintering. Metals2022, 12, 1915, 1-22.Behrens, B., et al.; Influence of Dwell Time and Pressure on SPS Process with Titanium Aluminides. Metals2022, 12, 83,1-14Jeje, S. O. et al.; Spark plasma sintering of Ti-48Al intermetallic using elemental powder. International Journal of Advanced Manufacturing Technology (2019) 103:3025-3032Wenbin, F. et al.; Microstructure and properties of a TiAl alloy prepared by mechanical milling and subsequent reactive sintering. Materials Science and Engineering:A (2005) 403, Issues 1-2, 186-190Voisin T., Monchoux JP., Couret A. (2019). Near-Net Shaping of Titanium-Aluminum Jet Engine Turbine Blades by SPS. In: Cavaliere P. (eds) Spark Plasma Sintering of Materials. Springer, Cham.
[0009] The present invention has been made in view of the above, and aims to provide a technology for inexpensively producing a practical TiAl-based alloy without using pre-alloyed powder as a raw material, i.e., a TiAl-based alloy with reduced segregation, a fine structure, high room temperature ductility, and high temperature strength, as well as a technology for producing net-shape or near-net-shape TiAl-based alloy products using additive manufacturing.
[0010] The method for producing a TiAl-based alloy according to claim 1 is a method for producing a TiAl-based alloy by vacuum sintering a mixed raw material powder containing Ti powder and Al powder as main raw materials, and is characterized in that an alloy is obtained in which the Al abundance ratio in any 0.5 mm × 0.5 mm cross section within the sintered body is within ±3 at % of the Al fraction in the mixed raw material powder by increasing the temperature at a rate of 10°C per minute or less in a predetermined temperature range between 550°C and 750°C, or by providing an isothermal holding time while increasing the temperature in a stepwise manner.
[0011] According to the invention of claim 1, it is possible to obtain a TiAl-based alloy free of so-called macrosegregation or reduced to a level that does not pose a practical problem, that is, a TiAl-based alloy having high ductility at room temperature and high strength at high temperatures can be produced.
[0012] The first problem to be solved in the powder method is the macrosegregation problem caused by fluidization during heating when Al melts. The inventors have conducted extensive research and discovered that macrosegregation can be eliminated by increasing the temperature at a rate of 10°C per minute or less in a predetermined temperature range between 550°C and 750°C during sintering, or by increasing the temperature stepwise while providing an isothermal holding time, leading to the invention. The reaction with Ti that occurs simultaneously with Al melting results in TiAl 3 The formation of TiAl 3 Therefore, if the Al in the raw material powder is melted over a certain period of time rather than all at once, the individual Ti particles will come into contact with the molten liquid phase of the Al particles, forming fine and strong TiAl particles. 3In other words, the slow melting of Al makes it difficult for the Ti powder to settle or flow, and the TiAl 3 By employing this method even when producing a large-sized sintered body, it is possible to obtain an alloy in which the abundance ratio of Al in any 0.5 mm × 0.5 mm cross section within the sintered body is within ±3 at % of the Al fraction in the mixed raw material powder.
[0013] Here, macrosegregation refers to compositional variations large enough to be visible to the naked eye on an etched surface. To quantitatively evaluate macrosegregation, the area must be large enough to prevent the detection of compositional variations due to differences in the phases of the crystal grain structure, yet small enough to prevent segregation from becoming indistinguishable due to averaging. This is considered appropriate to be an area equivalent to approximately 15 crystal grains (≒0.05 mm square) in the microstructure, i.e., an area of at least approximately 0.15 mm square, but not larger than an area (≒approximately 3 mm square) that makes it difficult to average out segregation. In this application, a 0.5 mm x 0.5 mm cross section is used. However, 0.3 mm x 0.3 mm or even 0.15 mm x 0.15 mm can also be used as appropriate. Depending on the specification, a 1 mm x 1 mm cross section may also be used. Examples of methods for measuring macrosegregation include surface analysis using EDX (energy dispersive X-ray fluorescence analysis) and EPMA (electron probe microanalysis). Note that the "interior" of a sintered body does not include the surface layer. This is because the surface layer may be affected by mold or the like.
[0014] The tolerance of ±3 at% for macrosegregation in TiAl-based alloys is based on Figure 16 (Non-Patent Document 5), a Ti-Al phase diagram. As is clear from the figure, the phase is complex, and if the Al fraction differs (macrosegregation occurs), it is difficult to achieve the desired crystalline phase. Considering the 48 at% Al line, the tolerance for deviation from the Al fraction is at most ±3 at%, preferably ±2 at%, and more preferably ±1 at%. The Al fraction in the mixed raw material powder can be rephrased as the Al fraction in the target alloy composition, the total Al fraction in the blended raw material powders, the target Al fraction, etc.
[0015] The Ti powder and Al powder are, so to speak, a matrix, and the mixed raw material powder does not preclude the addition of other raw material powders. Each is a raw material powder, with the Ti powder and Al powder being the main powders. In this application, the mixed raw material powder is a mixture of raw material powders, and raw material powder basically refers to a powder of a single pure metal or a powder of a compound of a single composition (i.e., the raw material powder is not a mixture of multiple types of pure metal powders or metal compounds).
[0016] Incidentally, microsegregation may be reduced by carrying out a diffusion treatment in which the material is maintained at a temperature of 1200° C. or higher for an appropriate period of time simultaneously with or separately from the sintering.
[0017] The method for producing a TiAl-based alloy according to claim 2 is characterized in that, in the method for producing a TiAl-based alloy according to claim 1, a step of heating and sintering the mixed raw material powder at 1000°C or higher and a pressure higher than 10 MPa is included, thereby obtaining a TiAl-based alloy having a cross-sectional area ratio of porosity of 0.1% or less.
[0018] From a practical standpoint, the temperature range is preferably 1200°C to 1400°C, and the pressure is preferably 50 MPa to 200 MPa, for example. Porosity reduction depends on the temperature, pressure, and holding time; for example, if sintering is performed at 1000°C, a higher pressure should be used, and if pressurized at 10 MPa, a higher temperature and longer holding time should be used within the sinterable temperature range. Depending on the heat sintering method, SPS can apply a pressure of 50 MPa, and HIP can apply a pressure of approximately 100 MPa to 200 MPa. If powders of an appropriate particle size range are used as raw materials and sintered at a pressure of 100 MPa or higher, virtually no porosity is observed.
[0019] A third aspect of the present invention provides a method for producing a TiAl-based alloy according to the first aspect of the present invention, characterized in that the raw material powder used has Al having a particle size smaller than that of Ti in both maximum and average particle sizes.
[0020] According to the third aspect of the present invention, segregation can be more effectively suppressed.
[0021] The particle size evaluation can be performed using the results of particle size distribution measurement. Even if the heating rate between 550°C and 750°C is slowed down to a certain level or less, melting of one Al particle occurs at a time. In this case, in order to make it difficult for the Ti particles to fall freely in the Al liquid bath, that is, to make it difficult for segregation to occur, it is sufficient that the Al particle size is smaller on average than the Ti particle size. If the Al particles are an aggregate of smaller particle sizes, there will be more contact points with the Ti particles, and melting of each Al particle will not occur simultaneously, but Al will react at each contact point to form TiAl. 3 This is because the network is formed sequentially, preventing the Ti particles from being simultaneously enveloped in the molten Al pool. In other words, segregation in the microscopic region can be minimized. It is preferable that the average particle size of all raw material powders, including Ti, Al, Cr, and Nb, be in the range of 1 μm or more and less than 100 μm. It is also possible to determine the optimum particle size range for each element.
[0022] As described above, the methods of claims 1 to 3 make it possible to produce TiAl-based alloys with extremely few sintering defects such as macrosegregation, porosity, and microsegregation, which have been difficult to achieve with conventional powder methods. Representative sintering methods include spark plasma sintering (SPS), hot isostatic pressing (HIP), and hot pressing.
[0023] A fourth aspect of the present invention relates to a method for producing a TiAl-based alloy, which is the same as the first aspect of the present invention, except that the method further comprises the steps of: increasing the temperature at a rate of 10°C per minute or less in a predetermined temperature range between 550°C and 750°C, or increasing the temperature stepwise while providing an isothermal holding time; sintering the alloy at a temperature of 1000°C or higher and a pressure higher than 10 MPa; and then cooling the alloy to 900°C at a rate of 3°C / min or more. Note that these pressure sintering and cooling steps can also be applied to the methods described in the fifth or sixth aspects of the present invention.
[0024] In the cooling process described in claim 4, controlling the cooling rate is important because it can affect the quality characteristics of the product. In our research, we have also encountered a phenomenon in which differences in cooling rate depending on the sample size cause differences in the mechanical properties of the product. In particular, when producing large ingots, there is concern about the adverse effects of a slow cooling rate due to the volume effect. Therefore, regardless of size, the cooling rate is set to 3°C / min or more until the temperature drops to 900°C.
[0025] The method for producing a TiAl-based alloy described in claim 5 is a method for producing a TiAl-based alloy by using a powder additive manufacturing device to shape a mixed raw material powder whose main raw materials are Ti powder and Al powder in a non-oxidizing atmosphere, and is characterized in that beam scanning is performed so that every location in each layer is heated to 660°C or higher for 0.1 seconds or more to form a layered pre-sintered body, and the final sintered body is obtained by sintering using a HIP device at 1000°C or higher and a pressure higher than 10 MPa.
[0026] The method for producing a TiAl-based alloy according to claim 6 is the method for producing a TiAl-based alloy according to claim 5, characterized in that the ceramic powder and the pre-sintered body are placed in a metal capsule, the capsule is degassed and sealed, and then the entire capsule is heated and pressurized in an inert gas using a HIP device to perform the final sintering.
[0027] The present inventors further took on the challenge of obtaining a net-shape or near-net-shape alloy body by additive manufacturing, which has not been reported before in powder processes, and after extensive investigation, have achieved the inventions described in claims 5 and 6. First, in the first step, a powder additive manufacturing device is used to additively manufacture a mixed raw material powder containing Ti powder and Al powder as the main raw materials in a non-oxidizing atmosphere under the conditions described in the claims. What is obtained in this first step is TiAl 3The shaped body is an incomplete sintered body of raw material powders that are finely bonded together, mainly consisting of . In the second step, this shaped body is sintered in a HIP device. At this time, the shaped body may be directly pressurized and heated in an oxygen-free gas such as argon gas or nitrogen gas. A more versatile method is as follows: ceramic powder with an average particle size of 500 μm or less is placed in a metal capsule, the shaped body is embedded in the powder, and the capsule is sealed in a vacuum. The entire capsule is then heated to 1000°C or higher while being pressurized to 10 MPa or higher in an inert gas. This results in the final sintered body.
[0028] In the HIP process for additive manufacturing, the workpiece is usually pressed directly in a gas such as argon gas or nitrogen gas, but if there is porosity penetrating the workpiece, the pressing will not be complete. If the energy density during additive manufacturing is high and the porosity is close to zero, the problem of ineffective pressing due to gas intrusion is unlikely to occur. In the case of TiAl-based alloys, under such manufacturing conditions, depending on the shape, thermal stress after manufacturing can cause cracking. Therefore, it is more realistic to obtain a provisional sintered body by additive manufacturing under conditions that give a certain degree of porosity (note that the porosity here is defined as the true density obtained in the sintered body, ρ 1 and the specific gravity of the pre-sintered body is ρ X When this is the case, (ρ 1 -ρ X ) / ρ 1 (The value is defined by
[0029] TiAl obtained at the preliminary sintering stage 3 The phase is stable up to a relatively high temperature, and the diffusion effect of the subsequent HIP treatment gradually transforms the crystals into the final equilibrium phases of TiAl and Ti. 3The sintered body transforms into an Al phase. During this process, it retains its shape well, and even if the pre-sintered body contains voids, it shrinks while maintaining its shape (the voids are filled). Therefore, by vacuum-sealing a capsule using ceramic powder as an intermediate medium and then compressing it in a HIP apparatus, it is possible to obtain a final sintered body that shrinks while maintaining its shape. The inventors have confirmed that a pre-sintered body with a porosity of 25% can be obtained with a shape-maintaining final sintered body. That is, by creating a pre-sintered body with a shape similar to the void ratio and creating a density that is 75% or more of the true density of the final sintered body while anticipating reduction in size based on the porosity, it is possible to obtain a net-shape or near-net-shape final sintered body. The method of claim 5 or 6 also prevents internal oxidation due to trace amounts of oxygen contained in the inert gas. Furthermore, the powder additive manufacturing device sinters each layer by beam irradiation, and the beam used can be a laser beam or an electron beam.
[0030] The TiAl-based alloy according to claim 7 is a TiAl-based alloy obtained by the method according to any one of claims 1 to 6, characterized in that the relationships are 41.0≦Al≦48.0, 18≦100−(Al+Ti), where the element symbols in the formulas directly represent the at% of the element in the alloy, and further contains additional elements such that the relationships V+Nb+Ta≦12, Cr+Mn≦4.0, W+Mo≦1.5, and 1.0≦V+Nb+Ta+Cr+Mn+W+Mo are satisfied.
[0031] The TiAl-based alloy according to claim 8 is characterized in that the content of oxygen as an inevitable impurity in the TiAl-based alloy according to claim 7 is O≦0.5. Note that it is also preferable that the content of O≦0.5 in the alloy according to claim 9.
[0032] The TiAl-based alloy according to claim 9 is characterized in that, in the TiAl-based alloy according to claim 8, it further contains, as additional elements, elements that satisfy the relationships La≦0.15, B≦1.0, C+N≦2.0, and 0.01≦La+B+C+N.
[0033] Claim 7 can be expressed as follows without using mathematical formulas: A TiAl-based alloy obtained by the method of any one of claims 1 to 6, wherein the proportion (at %) of Al to the whole (100 at %) is 41.0 or more and 48.0 or less, the proportion (at %) of the remainder excluding Al and Ti to the whole is 18 or less, the alloy may contain V, Nb, or Ta as a β-phase stabilizing element, the proportion (at %) of their total to the whole being up to 12, the alloy may contain Cr or Mn, the proportion (at %) of their total to the whole being up to 4.0, and the alloy may further contain W or Mo, the proportion (at %) of their total to the whole being up to 1.5, with the proviso that the proportion (at %) of V, Nb, Ta, Cr, Mn, W, and Mo to the whole being 1.0 or more.
[0034] Claim 9 can be expressed as follows without using a formula: The TiAl-based alloy according to claim 8, characterized in that the ratios (at %) of La and B to the total are set to 0.15 and 1.0, respectively, or the upper limit of the total of C and N is set to 2.0, and the ratio (at %) of the total of La, B, C, and N to the total is set to 0.01 or more.
[0035] In order to practically use TiAl-based alloys, one of the requirements for imparting a minimum level of room temperature ductility is to prevent the coarsening of crystal grains and to impart a fine microstructure. As a result of extensive research, the inventors have achieved stable precipitation of the β phase while achieving the compositions described in claims 7 to 9.
[0036] The classification of added elements and the range of added amounts are explained below. (1) V, Nb, Ta: V, Nb, and Ta are members of the vanadium group in the periodic table, and are the group of elements that can most effectively replace Ti in the TiAl phase. Addition of these elements is expected to stabilize the β phase, as well as strengthen the solid solution of the TiAl phase and improve corrosion resistance. The total amount added is preferably in the range of 0.5 at% to 12.0 at%. If it is less than 0.5 at%, the effect of the addition cannot be obtained, and if it exceeds 12.0 at%, it will result in a decrease in ductility and an increase in specific gravity.
[0037] (2) Cr, Mn: Cr and Mn are neighboring elements on the periodic table, and as an addition to TiAl-based alloys, they stabilize the β phase and improve ductility. Because of concerns about the destabilization of the lamellar structure and the formation of unexpected precipitates, the upper limit of their total addition amount is set at 4.0 at%.
[0038] (3) Mo, W: Mo and W are in the same group in the periodic table and are both strong β-phase stabilizing elements. They are also expected to strengthen the solid solution of the TiAl phase and improve high-temperature strength. However, because they form unexpected precipitates and increase the specific gravity, the upper limit of their total addition is set at 1.5 at%.
[0039] (4) The elements in the group (1) to (3) all have the effect of stabilizing the β phase and suppressing grain growth in the high-temperature range, so it is preferable to set a minimum addition amount overall. A minimum addition of 1.0 at% (i.e., 1.0≦V+Nb+Ta+Cr+Mn+W+Mo) provides a grain refinement effect. Considering manufacturing efficiency, it is preferable to select elements that contribute to the stabilization of the γ and α2 phases that are ultimately desired. For example, a combination of Cr, Nb, and W can shorten the high-temperature holding time and improve manufacturability.
[0040] In addition to the above elements, small amounts of La, B, C, N, Fe, Co, Ni, Cu, Zr, Hf, Sn, Si, P, etc. may be added up to an upper limit of 1.0 at % in order to exhibit and improve predetermined properties.
[0041] In order to ensure the effectiveness of trace addition of La, B, C, and N, which are effective in improving properties, it is important to suppress the amount of oxygen (O), an unavoidable impurity, within a certain range. The amount of oxygen (O) to be controlled, and the addition of La, B, C, and N will be explained below.
[0042] (7) O: Reducing O, an unavoidable impurity in TiAl-based alloys derived from raw material powders or processes, is important for ensuring the required properties of the final product. By adopting the method of the present invention, even when using commercially available raw material powders (without special pretreatment), O can be reduced to approximately 0.5 at%. By making various adjustments, O can be reduced to 0.3 at%.
[0043] (5) La, B: TiAl-based alloys produced by the powder method tend to have lower room temperature ductility than castings melted in a vacuum. This is because when commercially available raw material powders are used, oxygen, an unavoidable impurity, tends to remain more easily than in the above-mentioned castings.
[0044] Therefore, the inventors have conducted extensive research and have arrived at the invention described in claim 9. That is, by adding 0.01 at% to 0.15 at% of La and / or 0.01 at% to 1.0 at% of B, it has been possible to reduce the amount of dissolved oxygen and obtain a TiAl-based alloy with a fine crystal structure that is excellent in room temperature tensile properties. 6 As a source of B, LaB 6 and Cr 2 B can be used as a raw material powder.
[0045] When La is added, LaAlO 3 Or La 2 O 3 The present inventors have found that this reduces the amount of oxygen dissolved in the matrix, facilitates the precipitation of γ single-phase grains, and improves room temperature ductility to the same level as that of the above-mentioned cast product. Furthermore, the oxides have the effect of pinning grain boundaries, maintaining fine grains in the TiAl-based alloy, and are therefore effective in improving ductility.
[0046] When B is added, it is mainly TiB or TiB 2 This also pins the grain boundaries of the TiAl-based alloy, improving ductility. The boride phase has a relatively high affinity for oxygen and can act as a trap site. Therefore, it also has the effect of reducing the amount of dissolved oxygen.
[0047] However, excessive addition of either element causes coarse precipitates, which can have adverse effects such as becoming the starting point for fatigue fracture. Furthermore, excess La actually reduces the mechanical properties of TiAl-based alloys. Therefore, it is preferable to limit the addition of La to 0.15 at% and the addition of B to 1.0 at%. However, to obtain effective effects, the lower limit of the total amount is set to 0.01 at%. Furthermore, when emphasis is placed on the creep strength of TiAl-based alloys, it is naturally acceptable to add only B, in order to avoid the effect of La shortening the rupture life.
[0048] (6) C, N: TiAl-based alloys are potentially required to withstand temperatures of 800°C or higher in terms of creep strength. In other words, by adding either or both of C and N in the range of 0.01≦C+N≦2.0, fine Ti 2 AlC or Ti 2 It is possible to significantly improve high-temperature creep strength by precipitating AlN or a composite phase of these at grain boundaries and lamellar layer boundaries. The amount of C+N added that does not significantly impair room-temperature ductility is 0.01≦C+N≦0.3.
[0049] The effects of La, B, C, and N described in (5) and (6) are naturally effective even when each element is added alone. That is, the minimum amount of each of the four elements to be added is 0.01≦La+B+C+N.
[0050] It is difficult to control the addition of each of the elements La, B, C, and N in such minute amounts using the melting method. On the other hand, the manufacturing method of the present invention is suitable because it allows for the elements to be pre-blended in the form of raw material powders that are homogeneously dispersed, and diffusion also progresses during sintering.
[0051] According to the present invention, it is possible to inexpensively produce a practical TiAl-based alloy without using pre-alloyed powder as a raw material, i.e., a TiAl-based alloy with high room temperature ductility and high temperature strength by suppressing segregation and making the structure fine, and it is also possible to produce net-shape or near-net-shape TiAl-based alloy products by additive manufacturing.
[0052] This is a photograph of a sliced test piece of a sintered body of a TiAl-based alloy produced by the elemental powder sintering method. It is a perspective view of a half-cut cross section of a cylindrical test piece showing the measurement points. It is an SEM photograph of each sample at each measurement point shown in Figure 2 and the Al concentration at the measurement points. It is a table showing the results of a tensile test when the particle size of the raw material powder is varied. It is a photograph of porosity observed on a fracture surface. It is a table showing an example of alloy production using two-stage sintering using an additive manufacturing device and an HIP device. It is a photograph of the appearance of a TiAl-based alloy that is a final sintered body. It is a table showing the results of a tensile test on samples of a Ti-Al-Cr-Nb-W-La-B-C system TiAl-based alloy with different cooling rates after sintering. It is a backscattered electron image of SPS sintered bodies of Ti-45 at% Al-4 at% Nb and Ti-45 at% Al-4 at% Cr according to the present invention, in which the heating rate was controlled. LaB 6 11(c) is a diagram showing the structure of an alloy to which LaB was added. 6 1 shows the stress-strain curve and a photograph of the fracture surface of an alloy containing LaB. 6 1 is a table showing the results of measuring the changes in room temperature ductility and creep rupture life of alloys with the addition of C and N. 2 is a diagram showing creep test results with the addition of C and N. 3 is a table showing a list of TiAl-based alloys of the present invention with different additive elements. 4 is a Ti-Al phase diagram showing the tolerance of macrosegregation in TiAl-based alloys of ±3 at %.
[0053] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings. Note that, although examples, example 1, comparative examples, comparative example 1, etc. are used in the following, they are independent sections and do not refer to the same sample.
[0054] <Confirmation of Macrosegregation> First, an experiment was conducted to confirm macrosegregation in a TiAl-based alloy. Figure 1 is a photograph of a sliced test piece of a sintered body of a TiAl-based alloy produced by the powder method. The alloy was a Ti-Al-Nb-Cr-W-N alloy, and SPS (spark plasma sintering) was used for sintering. The test piece was a 120 mm diameter x 60 mm cylinder sliced longitudinally at the center of the circle.
[0055] The dark area (a) in the figure is mainly composed of the γ-TiAl phase and α 2 -Ti 3 This is a normal structure consisting of a lamellar structure in which the Al phase is arranged in layers and a β / B2-Ti phase mixed together. The light-colored outer periphery (b) is where the β phase is increasing. EDX analysis using an SEM confirmed that the Al was diluted, while the other elements were concentrated at roughly the same ratio. This is thought to be because the Al on the periphery reached its melting point and liquefied, then gathered toward the center due to capillary action, resulting in a relative dilution of the Al on the periphery.
[0056] The upper surface (c1) and lower surface (c2) in the center of the interior are the last to melt, but with the addition of reaction heat from other sources, melting occurs all at once, resulting in the formation of a large melt pool. In particular, at the bottom (c1d) of the pool-like pattern on the upper surface, heavy elements precipitate and concentrate, resulting in an extremely increased amount of β phase. Meanwhile, at the top surface (c1u) of the pool, light Al concentrates and there is no β phase at all. When a large pool like the one shown in the figure is formed, the Al concentration varies significantly from location to location. At c1u, the Al concentration is 5 at% higher than the average, preventing the desired material (a homogeneous alloy with the designed composition) from being obtained. This macroscopically observable difference in Al concentration is called macrosegregation.
[0057] <Suppression of Macrosegregation> Based on the above example, a basic experiment was conducted to suppress macrosegregation that occurs with Al melting. Aiming for an alloy with a composition of 55 at% Ti-45 at% Al, a mixed raw material powder of pure Ti powder and pure Al powder in the same at% ratio was prepared, and SPS molding was performed using a carbon mold with a diameter of 30 mm and a thickness of 7 mm. The conditions were as follows:
[0058] - Temperature increase: 10°C / min - Pressure: 10 MPa up to 700°C, 30 MPa after 700°C, 50 MPa after 1300°C Sample No. 1: Room temperature → 1300°C x 1 h → Room temperature (natural cooling) Sample No. 2: Room temperature → 600°C x 1 h → 1300°C x 1 h → Room temperature (natural cooling) Sample No. 3: Room temperature → 800°C x 1 h → 1300°C x 1 h → Room temperature (natural cooling)
[0059] The microstructure of each sample was observed. Figure 2 is a perspective view of a half-cut cross section of a cylindrical test piece, showing the measurement points. The measurement points were the central position A in the thickness direction near the outer periphery, the upper surface side at the center of the cylinder B, the central position C at the center of the cylinder, and the lower surface side at the center of the cylinder D. Figure 3 shows SEM photographs of the above four points on each sample. The local Al concentration measured by EDX is also shown (here, the analytical value in a 1 mm x 1 mm cross section, which is a 100x field of view of the area photographed by SEM, was used).
[0060] As is clear from the photographs, sample No. 2 exhibits a similar appearance in all locations. On the other hand, samples No. 1 and No. 3 clearly have crystals with different appearances depending on the location. Looking at the Al concentration, only sample No. 2 shows a difference of less than 0.7%, while samples No. 1 and No. 3 show a difference of nearly 5%.
[0061] That is, it was confirmed that only in the case of SPS sintering with a 600°C holding step (Example No. 2) was an alloy with no variation obtained. On the other hand, in the case of no temperature holding step during heating (No. 1, Comparative Example 1) and the case of a high temperature holding step of 800°C with a temperature holding step (No. 3, Comparative Example 2), it was confirmed that there was a large variation in the Al concentration, with some locations exceeding ±3 at% of the target value of 45 at%.
[0062] From the viewpoint of the mechanical properties and other required specifications of TiAl-based alloys, the deviation from the target value must be within ±3 at% of the target value, preferably within ±2 at% of the target value, in a 1 mm x 1 mm cross section at any location within the sample, based on Al. The deviation from the target value of specimen No. 2 fully satisfies this required specification, being within ±1 at%. Therefore, while it has been impossible to obtain a practical alloy without using pre-alloys in the past, the present inventors have surprisingly discovered that a practical TiAl alloy can be produced even from a mixed raw material powder.
[0063] Considering the differences between the melting point of Al (approximately 660°C), the holding temperature of No. 2 (600°C), and the holding temperature of No. 3 (800°C), the inventors of the present application believed that if the heating process was such that Al melted little by little, i.e., at a constant rate or less, or if the heating process involved a temperature holding time, the Ti-Al compound network constantly forming on the surface would be maintained even while the solute element powder, such as Ti, was immersed in the low-viscosity Al melt. By controlling the temperature near the Al melting point, the viscosity would be maintained, making it difficult for a melt pool to form, preventing macroscopic convection and, as a result, suppressing macrosegregation. Specifically, the inventors conceived a method of gradual phase change near the Al melting point by slowing the heating rate or by providing a constant temperature step, which led to the present invention.
[0064] As the melting progresses to the inside, overheating occurs due to the reaction of Ti-Al compounds, and the melting progresses rapidly, which can cause convection in the melt pool. It may be effective to not only maintain the temperature once heated near the Al melting point, but also to lower it, or to repeat heating and cooling within a certain temperature range.
[0065] In addition, when controlling temperature in actual manufacturing processes, temperatures are measured externally using non-contact thermometers, etc., so temperature control must be carried out assuming that there is a difference of several tens of degrees between the measured temperature and the actual internal temperature.
[0066] Therefore, during heating, the temperature is increased at a rate of 10°C / min or less within a predetermined temperature range between 550°C and 750°C, or the temperature is increased (or decreased in some cases) in stages while an isothermal holding time is provided. Although this depends on the volume of the TiAl-based alloy to be produced, it is preferable that the larger the volume, the slower the heating rate and the longer the isothermal holding time. A preliminary test can be conducted based on the composition of the alloy to be produced to determine the predetermined temperature range and the heating rate of 10°C / min or less. Even if the predetermined temperature range is set to the maximum of 550°C to 750°C, if the heating rate is the maximum of 10°C / min, the time required to pass through this temperature range is 20 minutes.
[0067] By providing a buffer zone for temperature rise, the macroscopic Al segregation that would impair mechanical strength can be virtually eliminated, resulting in a homogeneous TiAl-based alloy. In this case, the alloy can be synthesized from metal powder without using pre-alloys (realizing low-cost alloy production).
[0068] The finer the metal raw material powder, the larger its specific surface area, which leads to the inclusion of oxygen due to surface oxidation (oxygen is an impurity in TiAl-based alloys and reduces their mechanical properties). Therefore, it is preferable to produce spherical powders of Ti and Al, which are the main components of the raw material powder, by atomization, which prevents the inclusion of oxygen, and it is also desirable to make the powder particle size uniform within a certain range.
[0069] <Porosity Reduction> The frequency of porosity can be reduced by applying pressure using SPS or HIP. In fact, even in TiAl alloys or TiAl-based alloys containing other elements, the cross-sectional area ratio of porosity can be reduced to 0.1% or less by pressure sintering. The porosity rate depends on the pressure and temperature. A recommended pressure is 10 MPa or higher, and a recommended temperature is 1000°C or higher. Figure 5 shows an example of porosity observed on the fracture surface of a Ti-45Al alloy sample sintered using SPS (sintering pressure: 10 MPa). While both SPS and HIP can achieve a porosity level (cross-sectional area ratio of 0.1% or less) that ensures practical strength, increasing the pressure can reduce porosity when high specifications are required. That is, the pressure should be 10 MPa or higher, and depending on the specifications, 50 MPa or higher, or even 100 MPa or higher, should be used (the sintering temperature should also be adjusted appropriately depending on the pressure).
[0070] <Suppression of Microsegregation> The relationship between Ti and Al particle size was also investigated. Ti-Al-Nb-Cr-W alloys were fabricated using the same composition, sintering conditions, and heat treatment conditions, with only the particle size of the raw material powder being different, and tensile tests were performed. The results are shown in Figure 4. Example 1 (raw material powder A) shows the results obtained using Al powder with a maximum particle size and average particle size both approximately two-thirds that of Ti powder. Example 2 (raw material powder B) shows the results obtained using powder with a maximum particle size and average particle size both less than half that of Ti powder. Comparative Example 1 (raw material powder C) shows the results obtained using Al powder with a maximum particle size and average particle size both larger than Ti. As shown in the figure, it was confirmed that making the Al particle size smaller than that of Ti leads to a reduction in microsegregation and is necessary for stabilizing the mechanical properties of the product.
[0071] <Cooling rate control> Next, the cooling rate after sintering was investigated. Cooling can be applied to sintered bodies obtained by temperature control, as well as to sintered bodies obtained by combining a powder additive manufacturing device and a HIP device. Figure 8 shows the results of tensile tests in which the cooling rate after sintering of a Ti-Al-Cr-Nb-W-La-B-C TiAl-based alloy was changed. The cooling rate is the average value measured from the sintering temperature down to 900°C.
[0072] Example 1 was rapidly cooled, and the 0.2% proof stress and tensile strength were relatively high, showing favorable results. On the other hand, Example 2 had a slower cooling rate than the other examples, and both the 0.2% proof stress and tensile strength were significantly lower than those of Example 1. Changes in the microstructure, such as an increase in lamellar spacing, were also confirmed separately. Thus, it was found that a slow cooling rate can significantly reduce mechanical properties. Therefore, appropriate active cooling is necessary. Depending on the composition, volume, and shape of the sintered compact, cooling should be controlled at 3°C / min or more, preferably 5°C / min or more, and in some cases 15°C / min.
[0073] <Alloy manufacturing method combining an additive manufacturing device and a HIP device> It is also possible to manufacture a TiAl-based alloy by combining an additive manufacturing device and a HIP device. First, a powder additive manufacturing device is used to sinter a mixed raw material powder containing Ti powder and Al powder as the main raw materials in a non-oxidizing atmosphere to obtain a pre-sintered body. This is a metastable TiAl 3 This is a preliminary sintering process to form a pre-sintered alloy body. At this time, a solidification reaction is carried out in each layer so that the density of the pre-sintered body is 75% or more of the true density of a test body that has been previously measured using powder of the same composition and subjected to main sintering, and a pre-sintered alloy body with a similar shape to the net shape is obtained. This can be achieved by performing beam scanning so that every location in each layer is heated to 660°C or higher for 0.1 seconds or more.
[0074] Next, the resulting pre-sintered body is cooled and then heated to 1000°C or higher at a gas pressure of 10 MPa or higher in a HIP apparatus. This pressure sintering process achieves thermal diffusion, forming a stable microphase, and the final sintered body can be obtained. During pressure sintering, ceramic powder is first placed in a capsule, the pre-sintered body is embedded in the powder, and the capsule is sealed in a vacuum. The entire capsule is then subjected to HIP treatment in an inert gas. This prevents oxidation caused by the compressed gas, and allows for a shrinkage rate corresponding to the voids to be achieved, resulting in a net-shape or near-net-shape molded body with virtually no voids, while maintaining its shape.
[0075] Figure 6 shows an example of alloy production using an additive manufacturing device, i.e., the powder method described above, in two stages of sintering, resulting in a 10 mm square alloy material with a stamped sample number. Figure 7 shows a photograph of the appearance of the final sintered body (TiAl-based alloy) after HIP processing. The sample number was stamped after preliminary sintering.
[0076] As is clear from FIGS. 6 and 7, even if the porosity of the pre-sintered body is about 25%, it is possible to produce a net-shape or near-net-shape TiAl-based alloy that shrinks uniformly and has a porosity of 0.
[0077] <Study on Improving Properties: Addition of Nb and Cr> To achieve higher mechanical properties, the microstructure of the sintered body must be made uniform and fine. Therefore, we decided to utilize the β phase in the alloy. The β phase facilitates plastic deformation and prevents coarsening of the crystalline structure at high temperatures above 1000°C. A mixed raw material powder containing Nb or Cr as a β-phase stabilizer was pressure-sintered. Figure 9 shows backscattered electron images of SPS sintered bodies of Ti-45Al-4Nb and Ti-45Al-4Cr according to the present invention, where the heating rate was controlled (note that the heating conditions were the same as for Sample No. 2). The white areas in the figure represent the β phase where Nb is concentrated. Ti-45Al is also shown as a comparative example (note that the comparative example shows a tendency toward coarsening of the grains).
[0078] According to the phase diagram, the addition of 4 at% Nb and 4 at% Cr to a TiAl-based alloy is insufficient to ensure stable dispersion of the β phase. However, due to the slow diffusion rate, the β phase is present ubiquitously at the grain boundaries of the α phase or γ phase, thereby suppressing grain coarsening. To achieve the coarsening suppression effect even with small addition amounts, it is preferable to set the average particle size of the raw material powders of Ti, Al, Nb, Cr, and various additive elements to 1 μm or more and less than 100 μm. Furthermore, V and Ta can be added in place of Nb or together with Nb, with a total upper limit of 12 at%. Similarly, Mn can be added in place of Cr or together with Cr, with a total upper limit of 4.0 at%. Furthermore, W and Mo can be added with a total upper limit of 1.5 at%.
[0079] <Study on improving properties: Control of contained O amount and addition of La and B> We investigated whether it is possible to reduce the amount of dissolved oxygen by precipitating the contained oxygen as an oxide. Specifically, we investigated whether it is possible to reduce the amount of dissolved oxygen by adding LaB 6 We decided to investigate the tensile ductility at room temperature when adding
[0080] LaB 6 The structure of the alloy to which La was added is shown in Figure 10. In the figure, (a) is an optical microscope image, (b) is a secondary electron image, (c) is a backscattered electron image, (d) is a mapping image of O, and (e) is a mapping image of La. Note that (b), (d), and (e) are images of approximately the same location.
[0081] The alloy in FIG. 10(c) is LaB 6 In the figure, Sp. 11 and Sp. 12 are composition analysis points. The spectrum analysis results (atomic %) at these points are shown in Figure 12. At Sp. 12, the precipitates were LaAlO 3 At point Sp. 11, the borides were TiB 2 Furthermore, these borides were often somewhat coarse in shape, such as needles or plates.
[0082] LaB 6 The addition of La clearly refines the grain size of the alloy. The precipitation of the oxides and borides pins the grain boundaries, resulting in a finer crystalline structure. This is also expected to improve ductility. Furthermore, because La absorbs oxidation, oxygen is consumed at a rate of 2 to 3 times (at%) the amount added as La. This effectively reduces the amount of oxygen dissolved in the TiAl phase, reducing the harmful effects of oxygen in the alloy.
[0083] LaB with La 0.1 at% 6 Additive sample and LaB 6 The results of the round bar reduction tensile test on the LaB2 sample and the non-additive sample are shown in Figure 12. Photographs of the fracture surfaces of the example and comparative example are also shown in the figure. Figure 13 shows the results of measuring the changes in room temperature ductility and creep rupture life. As is clear from Figures 12 and 13, the LaB2 sample 6 The addition of La refined the grain size, resulting in a triplex structure, and clearly improved the room temperature ductility, a property necessary for the practical application of TiAl-based alloys (the addition of La increased the fracture elongation from 0.4% to 1.0%). However, the creep rupture life was shortened. This is thought to be due to factors such as the grain refinement effect.
[0084] Next, LaB 6Experiments were conducted to examine the amount of addition. As a result, it was confirmed that when the alloy contains approximately 0.3 at% O, an addition amount of up to 0.15 at% or less in terms of La is preferable. However, if the addition amount is large, there is a high possibility that coarse precipitates will be formed and act as the starting point for fatigue fracture, thereby impairing other properties. Therefore, an addition amount of up to 0.10 at% or less in terms of La is more preferable. Furthermore, if the oxygen content of the alloy is smaller, the amount of La addition can also be reduced accordingly.
[0085] As described above, LaB 6 By adding La, a TiAl-based alloy having excellent room temperature ductility can be produced. Note that La can also be added in the form of LaN or the like.
[0086] <Study on Improvement of Properties: Addition of C and N> Next, the effect of adding C and N was studied. C and N are added to TiAlN at grain boundaries and lamellar layer boundaries in the alloy. 2 , TiAlC 2 These precipitate in the form of Cr, Nb, and Cu. This increases the resistance to grain boundary sliding at high temperatures, particularly enhancing creep strength. Therefore, Ti-Al-Cr-Nb-W alloys were manufactured in four patterns: C=N=0, 0.2C, 0.1C-0.1N, and 0.2N, and creep tests were conducted under an environment of 800°C and 200 MPa. Figure 14 shows the test results, showing the creep curves.
[0087] As is clear from the figure, it was confirmed that the addition of C and N has the effect of increasing creep strength, that is, decreasing the creep rate and extending the rupture life.
[0088] <Examples of the present invention and product analysis oxygen content> Figure 15 shows a list of TiAl-based alloys of the present invention with different additive elements. The figure also shows the results of tensile tests and creep tests, as well as density. The oxygen (O) content in the alloy was also measured. When the oxygen content is 0.5 at% or less, preferably 0.3 at%, the alloy tends to have a fine crystal structure and excellent room temperature tensile properties.
[0089] Example 1 contains 3 at% Nb and also contains Cr and W, aiming for high strength and ductility, and C and N are added to improve creep strength. Example 2 is a 4822 alloy composition. It has low strength and does not contain La, but room temperature tensile elongation is somewhat easier to achieve. Example 3 is based on the composition of Example 2, with W, La, B, and N added. It maintains ductility and has slightly improved strength. Example 4 is a material with high Nb and N addition. Its creep strength is quite high for a TiAl-based alloy. It is difficult to elongate at room temperature, and its specific gravity is somewhat high.
[0090] Comparative Example 1 has a composition equivalent to the TNM alloy, and Mo is added. Although La is added, the oxygen content of the Mo raw material is high, and the elongation at break is insufficient. Comparative Example 2 has LaB, which corresponds to 0.18 at% La. 6 The various properties, such as room temperature ductility, are not sufficiently high.
[0091] As explained above, according to the present invention, it is possible to provide a practical TiAl-based alloy without using pre-alloyed powder as a raw material, i.e., a TiAl-based alloy with high room temperature ductility and high temperature strength, by suppressing segregation and achieving a fine structure. Compared to conventional manufacturing techniques, it requires less energy and shortens the lead time, enabling inexpensive manufacturing. Furthermore, it is possible to manufacture net-shape or near-net-shape TiAl-based alloy products using additive manufacturing.
[0092] The present invention can be used in fields requiring high specific strength and heat resistance, such as aircraft and automobiles, for components that become or are exposed to high temperatures, and can also be applied to rocket technology such as satellite launches.
Claims
1. A method for producing a TiAl-based alloy by vacuum sintering a mixed raw material powder made mainly of Ti powder and Al powder, characterized in that by raising the temperature at a rate of 10°C per minute or less in a specified temperature range between 550°C and 750°C, or by providing an isothermal holding time while raising the temperature stepwise, an alloy is obtained in which the abundance ratio of Al in any 0.5 mm x 0.5 mm cross section within the sintered body is within ±3 at% of the Al fraction in the mixed raw material powder.
2. A method for producing a TiAl-based alloy as described in claim 1, characterized in that the method includes a step of heating and sintering the mixed raw material powder at 1000°C or higher and a pressure higher than 10 MPa to obtain a TiAl-based alloy having a cross-sectional area ratio of porosity of 0.1% or less.
3. A method for producing a TiAl based alloy as set forth in claim 1, characterized in that the raw material powder used has a smaller maximum and average particle size for Al than for Ti.
4. A method for producing a TiAl-based alloy as claimed in claim 1, characterized in that it includes a step of heating the material at a rate of 10°C per minute or less in a predetermined temperature range between 550°C and 750°C, or after providing an isothermal holding time while heating the material in a stepwise manner, sintering the material at 1000°C or higher and a pressure higher than 10 MPa, and then cooling the material to 900°C at a rate of 3°C / min or more.
5. A method for producing a TiAl-based alloy by using a powder additive manufacturing device to mold a mixed raw material powder consisting mainly of Ti powder and Al powder in a non-oxidizing atmosphere, characterized in that beam scanning is performed so that every location of each layer is heated to 660°C or higher for 0.1 seconds or more to form a laminated temporary sintered body, and a HIP device is used to sinter the material at 1000°C or higher and a pressure higher than 10 MPa to obtain a final sintered body.
6. A method for producing a TiAl-based alloy as described in claim 5, characterized in that a ceramic powder and the pre-sintered body are placed in a metal capsule, the capsule is degassed and sealed, and then the entire capsule is heated and compressed in an inert gas using a HIP device to perform final sintering.
7. A TiAl-based alloy obtained by the method according to any one of claims 1 to 6, characterized in that the following relationships are satisfied, with the element symbols in the formulas directly indicating the at% of the element in the alloy: 41.0≦Al≦48.0, 18≦100-(Al+Ti), and further the alloy contains the following additional elements so as to satisfy the following relationships: V+Nb+Ta≦12, Cr+Mn≦4.0, W+Mo≦1.5, 1.0≦V+Nb+Ta+Cr+Mn+W+Mo.
8. The TiAl-based alloy according to claim 7, characterized in that the oxygen, which is an unavoidable impurity, is O≦0.
5.
9. A TiAl-based alloy according to claim 8, further comprising as additive elements the following elements satisfying the relationships: La≦0.15, B≦1.0, C+N≦2.0, 0.01≦La+B+C+N.
Citation Information
Patent Citations
Game machine
JP2019051005A
Optical fiber route search method, optical fiber route search system, signal processing device, and program
JP2019211349A
Calibration device and calibration method
JP2022038867A
Powder metallurgy densification pressureless sintering method of Ti-Al alloy
CN111215623A
Preparation method of high-temperature-resistant titanium-aluminum alloy for aero-engine
CN113462917A
Cited By
Ceramic matrix composite material with high matrix toughness and preparation method thereof
CN118206384A
Die steel material for additive manufacturing lattice die and preparation process of die steel material