Secondary battery

By configuring the negative electrode active material layer with a higher expansion rate at the ends than at the center, the secondary battery addresses the issue of internal short circuits and uneven charge/discharge reactions, maintaining surface contact and improving battery performance.

WO2024248105A1PCT designated stage expired Publication Date: 2024-12-05PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/019929
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-31
Filing Date
2024-05-30
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Secondary batteries with negative electrode active materials that expand during charging face issues of internal short circuits and uneven charge/discharge reactions due to differential surface pressure, leading to deformation and deterioration of battery characteristics.

Method used

The configuration of the negative electrode active material layer, where the expansion rate is higher at the ends than at the center in the width direction parallel to the winding axis, reduces surface pressure differences and maintains surface contact with the battery case, preventing deformation and improving charge/discharge uniformity.

Benefits of technology

This configuration suppresses short circuits, maintains high output characteristics, and enhances battery cycle characteristics by ensuring even electrolyte distribution and stable current collection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024019929_05122024_PF_FP_ABST
    Figure JP2024019929_05122024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed is a secondary battery which comprises: a positive electrode 15; a negative electrode 16 which has a negative electrode current collector and a negative electrode active material layer that is provided on the surface of the negative electrode active material layer; a separator 17 which is interposed between the positive electrode and the negative electrode; an electrode group 18 which is configured by winding the positive electrode and the negative electrode, with the separator being interposed therebetween; an electrolyte; and a battery case which houses the electrode group and the electrolyte. The negative electrode forms the outermost periphery of the electrode group. The outermost periphery has a current collector exposed part 161A in which the negative electrode current collector is exposed. The swelling ratio of the negative electrode active material layer associated with charging and discharging of the negative electrode is higher in end parts 16B, 16C in the width direction that is parallel to the winding axis of the negative electrode than in a central part 16A in the width direction.
Need to check novelty before this filing date? Find Prior Art

Description

secondary battery

[0001] The present disclosure relates to secondary batteries.

[0002] The negative electrodes of secondary batteries, such as lithium-ion secondary batteries, use negative electrode active materials capable of absorbing and releasing lithium ions, and graphite is commonly used as such a negative electrode active material. In recent years, composite materials containing silicon, which have a higher capacity density than graphite, have been investigated as negative electrode active materials.

[0003] Silicon-containing materials are promising as high-capacity anode materials for secondary batteries. However, silicon-containing materials undergo large expansion and contraction during charging and discharging, which makes the anode prone to swelling during charging.

[0004] Patent Document 1 discloses a nonaqueous electrolyte secondary battery including an electrode assembly in which a positive electrode and a negative electrode are wound with a separator interposed therebetween, the negative electrode including a first negative electrode active material and a second negative electrode active material having a larger expansion coefficient during charging than the first negative electrode active material, and the ratio of the second negative electrode active material near the inner end of the winding is smaller than the ratio of the second negative electrode active material near the outer end of the winding, where the ratio is defined as the ratio of the mass of the second negative electrode active material to the total mass of the first negative electrode active material and the second negative electrode active material. Patent Document 1 proposes that this configuration suppresses the occurrence of internal short circuits near the inner end of the electrode assembly.

[0005] International Publication No. 2022 / 024712

[0006] When a negative electrode active material with a large expansion coefficient during charging is used, the surface pressure at the center of the electrode assembly in the direction of the winding axis tends to be higher than the surface pressure at the upper and lower ends in the direction of the winding axis, which may result in deformation of the electrode assembly and cause a short circuit.

[0007] One aspect of the present disclosure relates to a secondary battery including: a positive electrode; a negative electrode having a negative electrode current collector and a negative electrode active material layer provided on a surface of the negative electrode current collector; a separator interposed between the positive electrode and the negative electrode; an electrode group formed by winding the positive electrode and the negative electrode with the separator interposed therebetween; an electrolyte; and a battery case accommodating the electrode group and the electrolyte, wherein the negative electrode forms an outermost periphery of the electrode group, and the outermost periphery has a current collector exposed portion where the negative electrode current collector is exposed, and the expansion rate of the negative electrode active material layer due to charge and discharge of the negative electrode is greater at the ends in a width direction parallel to a winding axis of the negative electrode than at a central portion in the width direction.

[0008] According to the present disclosure, the difference in surface pressure occurring between the center and the upper and lower ends of the electrode group is reduced, and short circuits due to deformation of the electrode group can be suppressed.

[0009] The novel features of the present invention are set forth in the appended claims, but the present invention, both in terms of structure and content, together with other objects and features of the present invention, will be better understood from the following detailed description taken in conjunction with the drawings.

[0010] 1 is a schematic diagram illustrating an example of a negative electrode used in a secondary battery according to an embodiment of the present disclosure;

[0011] Hereinafter, embodiments of the present disclosure will be described using examples, but the present disclosure is not limited to the examples described below. In the following description, specific numerical values, materials, etc. may be exemplified, but other numerical values, materials, etc. may be applied as long as the effects of the present disclosure are obtained. Note that components other than those characteristic of the present disclosure may be those of known secondary batteries. In this specification, when a "range from numerical value A to numerical value B" is mentioned, the range includes numerical value A and numerical value B. In the following description, when a lower limit and an upper limit are exemplified for numerical values ​​of specific physical properties or conditions, any of the exemplified lower limits and any of the exemplified upper limits can be arbitrarily combined, as long as the lower limit is not equal to or greater than the upper limit. When multiple materials are exemplified, one material may be selected from the materials and used alone, or two or more materials may be used in combination.

[0012] The present disclosure also encompasses combinations of two or more features arbitrarily selected from the appended claims, i.e., two or more features arbitrarily selected from the appended claims can be combined unless a technical contradiction arises.

[0013] A secondary battery according to an embodiment of the present disclosure includes a positive electrode, a negative electrode, a separator interposed between the positive electrode and the negative electrode, an electrode assembly formed by winding the positive electrode and the negative electrode with the separator interposed therebetween, an electrolyte, and a battery case containing the electrode assembly and the electrolyte. The negative electrode has a negative electrode current collector and a negative electrode active material layer provided on the surface of the negative electrode current collector. Similarly, the positive electrode can be configured with a positive electrode current collector and a positive electrode active material layer provided on the surface of the positive electrode active material layer.

[0014] During charging, the negative electrode active material contained in the negative electrode active material layer expands, causing the negative electrode active material layer to swell. If the expansion rate of the negative electrode active material layer is the same at the end and center in the width direction parallel to the winding axis of the negative electrode, a greater surface pressure is usually applied to the center than to the end. As a result, the electrode group may be deformed such that the center protrudes outward in the radial direction perpendicular to the winding axis (e.g., the outer shape of the electrode group may change from a cylindrical shape to a barrel shape). This may result in an internal short circuit or poor current collection at the upper and lower ends.

[0015] Furthermore, the electrolyte is pushed from the center, where the surface pressure is high, to the edges, where the surface pressure is low, resulting in less electrolyte in the center. This imbalance in electrolyte distribution can result in uneven charge / discharge reactions along the winding axis, which can degrade battery characteristics such as cycle performance.

[0016] However, in the secondary battery according to this embodiment, the expansion ratio of the negative electrode active material layer is greater at the ends in the width direction parallel to the winding axis of the negative electrode than at the center in the width direction. This increases the expansion ratio at the ends, thereby increasing the surface pressure applied to the ends (or decreases the expansion ratio at the center, thereby decreasing the surface pressure applied to the center), thereby reducing the difference in surface pressure between the center and the ends. As a result, short circuits due to protruding deformation at the center of the electrode group and poor current collection at the upper and lower ends can be suppressed. Additionally, non-uniformity in charge / discharge reactions is suppressed, thereby suppressing deterioration of battery characteristics such as cycle performance.

[0017] Here, the swelling rate of the negative electrode active material layer in a predetermined region is the thickness T of the negative electrode active material layer in the fully charged state in that region. C , T in the discharge state D Ratio B (= T C / T D ) means the thickness T C The thickness T is determined by disassembling a fully charged secondary battery, removing the negative electrode, washing the negative electrode with an organic solvent, measuring the thickness of the negative electrode with a contact-type constant pressure thickness meter, and subtracting the thickness of the negative electrode current collector. D is determined by disassembling a discharged secondary battery, removing the negative electrode, washing the negative electrode with an organic solvent, measuring the thickness of the negative electrode with a constant pressure thickness gauge, and subtracting the thickness of the negative electrode current collector. The fully charged state of a secondary battery refers to a state in which the battery is charged to a state of charge of, for example, 0.98 x C or more (SOC = 98% or more), where C is the rated capacity of the battery. The discharged state refers to a state in which the battery is discharged to a state of charge of 0.02 x C or less (DOD = 98% or more).

[0018] When the length in the width direction parallel to the winding axis of the negative electrode active material layer is defined as width W, the central portion of the negative electrode active material layer includes a position that is W / 2 from one end of the negative electrode active material layer in the width direction, and includes, for example, a region of the negative electrode active material layer that is a distance from one end in the width direction in the range of 0.4 W to 0.6 W. A region where the negative electrode current collector is exposed may be provided at the end of the negative electrode in the width direction, but a portion at the end of the negative electrode where no negative electrode active material layer is provided is not included in the width W. The width of the central portion of the negative electrode active material layer in the width direction may be 20% to 60% of the width W of the negative electrode where the negative electrode active material layer is provided.

[0019] The end portion of the negative electrode active material layer preferably includes one end (upper end) and the other end (lower end) in the width direction of the region in the negative electrode where the negative electrode active material layer is provided, and includes, for example, regions each having a width of 0.1 W from the upper end and the lower end.

[0020] In the electrode group, the negative electrode may be disposed closer to the outer periphery than the positive electrode. The outermost periphery of the electrode group is the negative electrode, and the negative electrode has a current collector exposed portion where the negative electrode current collector is exposed at the outermost periphery of the electrode group. In this case, the current collector exposed portion of the negative electrode can be in surface contact with the battery case, at least in a charged state. This improves current collection and reduces internal resistance, thereby improving output characteristics, particularly under high loads.

[0021] However, as described above, the negative electrode active material layer swells during charging, and the electrode assembly deforms, sometimes resulting in deformation in which the center of the electrode assembly bulges outward in the radial direction. This deformation causes the contact between the exposed current collector and the battery case to become linear or point contact via the center of the electrode assembly, and the upper and lower ends of the electrode assembly no longer make contact with the battery case. This may result in an increase in internal resistance, making it impossible to maintain high output characteristics.

[0022] In contrast, in the secondary battery according to this embodiment, the expansion rate of the negative electrode active material layer at the ends in the width direction parallel to the winding axis is set to be greater than that at the center, thereby reducing the difference in surface pressure between the center and the ends, thereby suppressing deformation of the electrode group during charging, maintaining surface contact between the exposed current collector portion and the battery case, and maintaining high output characteristics.

[0023] The outer surface of the outermost negative electrode of the electrode group may have a current collector exposed portion where 50% or more of the negative electrode current collector is exposed by area, and may also have a current collector exposed portion where 70% or more of the negative electrode current collector is exposed.

[0024] The expansion rate of the negative electrode active material layer in the center portion is B 1 The expansion rate of the negative electrode active material layer at the end is B 2 Let (B 1 <B 2 ). Ratio B 1 / B 2 is less than 1 and is preferably 0.985 or more (98.5% or more).

[0025] B 2 In contrast to B 1 The smaller the value of B, the more the surface pressure at the center is reduced, which suppresses deformation of the electrode group during charging and maintains good surface contact between the exposed current collector portion and the battery case. In addition, the electrolyte is prevented from being extruded from the center to the edges, which suppresses deterioration of battery characteristics, such as cycle characteristics. 2 In contrast to B 1 If the expansion ratio B is too small, the surface pressure at the center becomes too low, and the end portions of the electrode portion are likely to be deformed so as to protrude more than the center portion during charging, and the contact between the exposed portion of the current collector and the battery case may become a line contact or a point contact via the upper and lower ends of the electrode group. Furthermore, the electrolyte may accumulate in the center, reducing the amount of electrolyte present at the ends, which may make it impossible to suppress a deterioration in battery characteristics. 1 is the expansion rate B 2 When the contact resistance is 98.5% or more, deformation of the electrode group during charging is significantly suppressed, and good surface contact can be maintained between the exposed current collector portion and the battery case. In addition, the effect of suppressing deterioration of battery characteristics is enhanced.

[0026] As described above, the swelling ratio B means the ratio of the thickness of the negative electrode active material layer in a fully charged state to the thickness in a discharged state in a predetermined region. Therefore, when the thickness of the negative electrode active material layer is the same at the center and the end in a discharged state, the swelling ratio B 1 / B 2 is equal to the ratio of the thickness of the negative electrode active material layer at the center in a fully charged state to the thickness of the negative electrode active material layer at the end in a fully charged state.

[0027] The expansion rate of the negative electrode active material layer depends on the expansion rate of the materials (particularly the negative electrode active material) contained in the negative electrode active material layer during charging. The more negative electrode active material that easily expands during charging is contained, the higher the expansion rate of the negative electrode active material layer. For example, a material containing silicon as a negative electrode active material is known to have a large theoretical capacity but a large degree of expansion during charging.

[0028] The negative electrode active material layer may contain a silicon-containing material as the negative electrode active material. As the content of the silicon-containing material in the negative electrode active material layer increases, a higher capacity can be obtained, but the expansion ratio B of the negative electrode active material layer also increases. However, the expansion ratio B of the negative electrode active material layer at the end 2 is the expansion rate B of the negative electrode active material layer in the central portion. 1 By making it larger than 1 / 2, the difference in surface pressure between the end and center of the negative electrode active material layer can be reduced, and short circuits and deterioration of battery characteristics due to deformation of the electrode group can be suppressed.

[0029] Swelling rate B 1 and B 2 can be controlled by adjusting the content ratio of the negative electrode active material in the negative electrode active material layer. For example, when a negative electrode active material containing a silicon-containing material is used, the content ratio of the silicon-containing material in the negative electrode active material layer at the edge may be higher than the content ratio of the silicon-containing material in the negative electrode active material layer at the center. When a combination of multiple types of negative electrode active materials is contained in the negative electrode active material layer, the content ratio of the multiple types of negative electrode active materials may be made different between the edge and the center. This allows the expansion ratio B at the edge to be reduced. 2 is the swelling rate B at the center 1 In this way, a negative electrode having a negative electrode active material layer larger than the above-mentioned thickness can be obtained.

[0030] The secondary battery may be a non-aqueous electrolyte secondary battery, which is a secondary battery having a liquid, gel, or solid non-aqueous electrolyte, and includes lithium ion secondary batteries, lithium secondary batteries (lithium metal secondary batteries), all-solid-state secondary batteries, etc.

[0031] Hereinafter, embodiments of the secondary battery according to the present disclosure will be further described with reference to the drawings. In each drawing, the shape or features of each component do not necessarily reflect the actual dimensions, and are not necessarily depicted to the same scale.

[0032] FIG. 1 is a schematic diagram showing an example of a negative electrode used in a secondary battery according to an embodiment of the present disclosure, illustrating the state of the negative electrode before being wound together with a positive electrode and a separator to form an electrode assembly.

[0033] The negative electrode 16 is strip-shaped, with a length (width) in the winding direction D1 being longer than the length in the direction D2 parallel to the winding axis. The winding direction D1 is a direction perpendicular to the winding axis. The direction D2 parallel to the winding axis is also referred to as the "width direction D2" below. The negative electrode 16 includes a negative electrode current collector 161 and a negative electrode active material layer 162 formed on the negative electrode current collector 161.

[0034] The negative electrode 16 has a central portion 16A located in the center in the width direction D2, and end portions 16B and 16C adjacent to the central portion 16A. The end portions 16B and 16C are end portions (upper and lower ends) of the negative electrode 16 in the width direction D2, and are positioned opposite each other with the central portion 16A in between.

[0035] Swelling rate B of the negative electrode active material layer 162 provided on the ends 16B and 16C 2 is the expansion rate B of the negative electrode active material layer 162 provided in the central portion 16A. 1 This is greater than 1 / 2. When a secondary battery is constructed using an electrode group in which the negative electrode 16 is wound together with a positive electrode and a separator, the difference in surface pressure between the end portions 16B, 16C of the negative electrode active material layer and the central portion 16A can be reduced, and deformation of the electrode group in which the central portion 16A protrudes can be suppressed. Furthermore, migration of the electrolyte from the central portion 16A to the end portions 16B, 16C can be suppressed, and deterioration of battery characteristics such as cycle characteristics can be suppressed.

[0036] In the winding direction D1, the end portion located on the outer periphery of the winding has no negative electrode active material layer 162 and has an exposed portion 161A where the negative electrode current collector 161 is exposed. When an electrode group is formed, the exposed portion 161A of the negative electrode current collector 161 forms the surface exposed on the outermost periphery of the electrode group. At least in a charged secondary battery, the exposed portion 161A is in surface contact with the inner surface of the battery case and is electrically connected.

[0037] The width of the negative electrode active material layer 162 in the width direction D2 is represented by W. The width W of the central portion 16A in the width direction D2 1 is, for example, in the range of 0.2W to 0.9W or 0.2W to 0.6W. The width W of the ends 16B and 16C in the width direction D1 2 is, for example, in the range of 0.05W to 0.4W or 0.05W to 0.2W.

[0038] 2 is a schematic longitudinal cross-sectional view of a secondary battery according to an embodiment of the present disclosure. The secondary battery (hereinafter referred to as battery) 10 is cylindrical and includes an electrode group 18, a non-aqueous electrolyte (not shown), and a battery case (battery can) 22 that accommodates these. The electrode group 18 is formed by winding a positive electrode 15 and a negative electrode 16 with a separator 17 interposed therebetween. An annular groove 22a is formed near the open end of the battery can 22.

[0039] The opening of the battery can 22 is sealed with a sealing body 11 having a gasket 21 on its periphery. The sealing body 11 includes a valve body 12, a metal plate 13, and an annular insulating member 14 interposed between the outer periphery of the valve body 12 and the outer periphery of the metal plate 13. The valve body 12 and the metal plate 13 are connected to each other at their respective centers. A positive electrode lead 15L extending from the positive electrode 15 is connected to the metal plate 13. Thus, the valve body 12 functions as an external terminal for the positive electrode. A negative electrode lead 16L extending from the negative electrode 16 is connected (welded) to the inner surface of the bottom of the battery can 22. A first insulating plate 24 is disposed between one end face of the electrode group 18 and the bottom of the battery can 22. A second insulating plate 23 is disposed between the sealing body 11 and the other end face of the electrode group 18.

[0040] The secondary battery may have a cylindrical, coin, or button shape with a metal battery case, or may be a laminated battery with a battery case made of a laminate sheet that is a laminate of a barrier layer and a resin sheet. In the present disclosure, the type, shape, etc. of the secondary battery are not particularly limited.

[0041] Next, a secondary battery according to an embodiment of the present disclosure will be described in detail. The secondary battery includes, for example, a positive electrode, a negative electrode, an electrolytic solution (non-aqueous electrolyte), and a separator as described below.

[0042] [Positive Electrode] The positive electrode comprises, for example, a positive electrode current collector and a positive electrode active material layer (positive electrode mixture layer) formed on the surface of the positive electrode current collector and containing a positive electrode active material. The positive electrode mixture layer can be formed by applying a positive electrode slurry, in which the positive electrode mixture is dispersed in a dispersion medium, to the surface of the positive electrode current collector and drying the applied layer. The dried coating may be rolled as necessary. The positive electrode mixture layer may be formed on one surface or both surfaces of the positive electrode current collector. The positive electrode mixture contains a positive electrode active material as an essential component and may contain a binder, a thickener, etc. as optional components.

[0043] The positive electrode active material may be any material that can be used as a positive electrode active material for nonaqueous electrolyte secondary batteries (particularly lithium ion secondary batteries), but from the viewpoint of increasing capacity, it preferably contains a lithium transition metal composite oxide (composite oxide N) containing at least nickel as a transition metal. The proportion of the composite oxide N in the positive electrode active material is, for example, 70% by mass or more, or may be 90% by mass or more, or may be 95% by mass or more.

[0044] The composite oxide N may be, for example, a lithium transition metal composite oxide having a layered rock salt structure and containing Ni and at least one selected from the group consisting of Co, Mn, and Al. Hereinafter, a lithium transition metal composite oxide having a layered rock salt structure and containing Ni and at least one selected from the group consisting of Co, Mn, and Al, in which the proportion of Ni among metal elements other than Li is 80 atomic % or more, will also be referred to as a "composite oxide HN." The proportion of the composite oxide HN in the composite oxide N used as the positive electrode active material is, for example, 90 mass % or more, or even 95 mass % or more, or even 100%. The higher the proportion of Ni, the more lithium ions can be extracted from the composite oxide HN during charging, thereby increasing the capacity. Co, Mn, and Al contribute to stabilizing the crystal structure of the composite oxide HN with a high Ni content.

[0045] The composite oxide HN may be, for example, a compound represented by the formula: Li α Ni(1-x1-x2-yz)Co x1 Mn x2 Al y M z O 2+β The element M is an element other than Li, Ni, Co, Mn, Al, and oxygen. Mn contributes to stabilizing the crystal structure of the composite oxide HN, and containing inexpensive Mn in the composite oxide HN is advantageous for cost reduction. Al contributes to stabilizing the crystal structure of the composite oxide HN.

[0046] In the above formula, α, which indicates the atomic ratio of lithium, is, for example, 0.95≦α≦1.05. α increases or decreases with charge and discharge. The above range of α indicates the value in a discharged state. In (2+β), which indicates the atomic ratio of oxygen, β satisfies −0.05≦β≦0.05.

[0047] The atomic ratio of Ni, 1-x1-x2-y-z (=v), is, for example, 0.8 or more, or may be 0.85 or more, or 0.90 or more, or 0.95 or more. Furthermore, v may be 0.98 or less, or may be 0.95 or less. The atomic ratio of Co, x1, is, for example, 0.1 or less (0≦x1≦0.1), the atomic ratio of Mn, x2, is, for example, 0.1 or less (0≦x2≦0.1), the atomic ratio of Al, y, is, for example, 0.1 or less (0≦y≦0.1), and the atomic ratio of M, z, is, for example, 0≦z≦0.10.

[0048] The element M may be at least one selected from the group consisting of Ti, Zr, Nb, Mo, W, Fe, Zn, B, Si, Mg, Ca, Sr, Sc, and Y. In particular, when at least one selected from the group consisting of Nb, Sr, and Ca is contained in the composite oxide HN, it is thought that the surface structure of the composite oxide HN is stabilized, the resistance is reduced, and metal elution is further suppressed. It is more effective if the element M is unevenly distributed in the vicinity of the particle surface of the composite oxide HN.

[0049] The content of each metal element contained in the lithium-containing composite oxide is measured, for example, by inductively coupled plasma (ICP) emission spectrometry.

[0050] As the binder for the positive electrode, for example, a resin material is used. Examples of the binder include fluororesin, polyolefin resin, polyamide resin, polyimide resin, acrylic resin, vinyl resin, etc. One type of binder may be used alone, or two or more types may be used in combination.

[0051] Examples of conductive materials include carbon nanotubes (CNTs), carbon fibers other than CNTs, and conductive particles (for example, carbon black and graphite).

[0052] The dispersion medium used for the positive electrode slurry is not particularly limited, but examples thereof include water, alcohol, N-methyl-2-pyrrolidone (NMP), and mixed solvents thereof.

[0053] The positive electrode current collector may be, for example, a metal foil. The positive electrode current collector may be porous. Examples of porous current collectors include nets, punched sheets, and expanded metals. Examples of materials for the positive electrode current collector include stainless steel, aluminum, aluminum alloys, and titanium. The thickness of the positive electrode current collector is not particularly limited, but may be, for example, 1 to 50 μm, or 5 to 30 μm.

[0054] [Negative Electrode] The negative electrode comprises, for example, a negative electrode current collector and a negative electrode active material layer formed on the surface of the negative electrode current collector. The negative electrode current collector is composed of a sheet-like conductive material. The negative electrode active material layer is supported on one or both surfaces of the negative electrode current collector. The negative electrode active material layer is usually a layer or film composed of a negative electrode mixture. The thickness of the negative electrode active material is, for example, 10 μm to 150 μm per surface of the negative electrode current collector. The negative electrode active material layer can be formed, for example, by applying a negative electrode slurry, in which the negative electrode mixture is dispersed in a dispersion medium, to the surface of the negative electrode current collector and then drying the applied layer. The dried coating film may be rolled as necessary. The negative electrode active material layer may be formed on one surface or both surfaces of the negative electrode current collector.

[0055] The negative electrode mixture contains a negative electrode active material as an essential component, and may contain optional components such as a binder, a conductive agent, and a thickener. The negative electrode active material includes a material that electrochemically absorbs and desorbs lithium ions. Examples of materials that electrochemically absorb and desorb lithium ions include carbon materials and Si-containing materials. Examples of Si-containing materials include silicon oxide (SiOx: 0.5≦x≦1.5) and composite materials containing a silicate phase and silicon particles dispersed within the silicate phase.

[0056] Examples of carbon materials include graphite, easily graphitizable carbon (soft carbon), and non-graphitizable carbon (hard carbon). Among these, graphite is preferred because of its excellent charge / discharge stability and low irreversible capacity. Graphite refers to a material having a graphite-type crystal structure, and includes natural graphite, artificial graphite, graphitized mesophase carbon particles, and the like. One type of carbon material may be used alone, or two or more types may be used in combination.

[0057] Among negative electrode active materials, composite materials containing a silicate phase and silicon particles dispersed within the silicate phase can easily achieve high capacity because the content of silicon particles can be freely selected. Hereinafter, the silicate phase refers to a composite oxide phase containing silicon, oxygen, alkali metals, etc. Hereinafter, composite materials in which the silicate phase is a lithium silicate phase containing silicon, oxygen, and lithium will also be referred to as "LSX." The higher the content of silicon particles in LSX, the higher the negative electrode capacity. LSX absorbs lithium ions by alloying silicon with lithium. High capacity can be expected by increasing the content of silicon particles.

[0058] The crystallite size of the silicon particles dispersed in the lithium silicate phase is, for example, 5 nm or more. The silicon particles have a particulate phase of simple silicon (Si). When the crystallite size of the silicon particles is 5 nm or more, the surface area of ​​the silicon particles can be kept small, making it less likely for the silicon particles to deteriorate, which leads to the generation of irreversible capacity. The crystallite size of the silicon particles is calculated using the Scherrer equation from the half-width of the diffraction peak assigned to the Si(111) plane in the X-ray diffraction (XRD) pattern of the silicon particles.

[0059] A combination of LSX and a carbon material may be used as the negative electrode active material. Because LSX expands and contracts in volume with charge and discharge, a high LSX content in the negative electrode active material can easily cause poor contact between the negative electrode active material and the negative electrode current collector during charge and discharge. On the other hand, the combined use of LSX and a carbon material makes it possible to achieve excellent cycle characteristics while providing the negative electrode with the high capacity of silicon particles. The proportion of LSX in the total of LSX and the carbon material is preferably, for example, 3 to 30% by mass. This makes it easier to achieve both high capacity and improved cycle characteristics.

[0060] As described above, the negative electrode includes a central portion and an end portion, and the expansion rate of the negative electrode active material layer at the end portion is greater than that of the negative electrode active material layer at the central portion. Negative electrode active material layers with different expansion rates can be formed, for example, by applying a negative electrode slurry, in which a negative electrode mixture containing a first negative electrode active material is dispersed in a dispersion medium, to the central portion of the negative electrode current collector in the width direction, and then applying a negative electrode slurry, in which a negative electrode mixture containing a second negative electrode active material having a larger expansion rate during charging than the first negative electrode active material is dispersed in a dispersion medium, to the end portions of the negative electrode current collector in the width direction, followed by drying. The first negative electrode active material and the second negative electrode active material may each be a mixture of multiple active materials with different expansion rates. The first negative electrode active material and the second negative electrode active material may have different mixing ratios of the multiple active materials. For example, the first negative electrode active material and the second negative electrode active material may each be a mixture of a first material and a second material having a larger expansion coefficient during charging than the first material, and the content ratio of the second material relative to the total of the first and second materials in the second negative electrode active material may be higher than the content ratio of the second material relative to the total of the first and second materials in the first negative electrode active material. The first material may be, for example, a graphite material. The second material may be, for example, a silicon-containing material.

[0061] The negative electrode current collector may be, for example, a metal foil. The negative electrode current collector may be porous. Examples of the material for the negative electrode current collector include stainless steel, nickel, nickel alloy, copper, and copper alloy. The thickness of the negative electrode current collector is not particularly limited, but may be, for example, 1 to 50 μm, or 5 to 30 μm.

[0062] As the binder for the negative electrode, for example, a resin material is used. Examples of the binder include fluororesin, polyolefin resin, polyamide resin, polyimide resin, acrylic resin, vinyl resin, and rubber-like material (for example, styrene butadiene copolymer (SBR)). One type of binder may be used alone, or two or more types may be used in combination.

[0063] Examples of thickeners include cellulose derivatives such as cellulose ether. Examples of cellulose derivatives include carboxymethyl cellulose (CMC) and its modified forms, methyl cellulose, etc. One type of thickener may be used alone, or two or more types may be used in combination.

[0064] Examples of conductive materials include carbon nanotubes (CNTs), carbon fibers other than CNTs, and conductive particles (for example, carbon black and graphite).

[0065] The dispersion medium used for the negative electrode slurry is not particularly limited, but examples thereof include water, alcohol, N-methyl-2-pyrrolidone (NMP), and mixed solvents thereof.

[0066] [Non-aqueous electrolyte] The non-aqueous electrolyte contains a non-aqueous solvent and a solute dissolved in the non-aqueous solvent. The solute includes, for example, a lithium salt. Components of the non-aqueous electrolyte other than the non-aqueous solvent and the solute are additives. The non-aqueous electrolyte contains the above-mentioned sulfur-containing compound as an additive.

[0067] Examples of non-aqueous solvents that can be used include cyclic carbonates, chain carbonates, cyclic carboxylic acid esters, and chain carboxylic acid esters. Examples of cyclic carbonates include propylene carbonate (PC), ethylene carbonate (EC), and vinylene carbonate (VC). Examples of chain carbonates include diethyl carbonate (DEC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC). Examples of cyclic carboxylic acid esters include γ-butyrolactone (GBL) and γ-valerolactone (GVL). Examples of chain carboxylic acid esters include methyl acetate, ethyl acetate, propyl acetate, methyl propionate (MP), and ethyl propionate (EP). One type of non-aqueous solvent may be used alone, or two or more types may be used in combination.

[0068] Examples of lithium salts include lithium salts of chlorine-containing acids (LiClO4, LiAlCl4, LiB 10 Cl 10 etc.), lithium salts of fluorine-containing acids (LiPF6, LiPF2 O 2 , LiBF4, LiSbF6, LiAsF6, LiCF3SO3, LiCF3CO2, etc.), lithium salts of fluorine-containing acid imides (LiN(FSO2)2, LiN(CF3SO2)2, LiN(CF3SO2)(CF4F9SO2), LiN(CF5SO2)2, etc.), lithium halides (LiCl, LiBr, LiI, etc.), etc., can be used. One type of lithium salt may be used alone, or two or more types may be used in combination.

[0069] The concentration of the lithium salt in the nonaqueous electrolyte may be 1 mol / L or more and 2 mol / L or less, or 1 mol / L or more and 1.5 mol / L or less. By controlling the lithium salt concentration within the above range, an electrolyte solution having excellent ionic conductivity and appropriate viscosity can be obtained. However, the lithium salt concentration is not limited to the above.

[0070] [Separator] It is desirable to interpose a separator between the positive electrode and the negative electrode. The separator has high ion permeability and adequate mechanical strength and insulating properties. The separator may be made of a microporous thin film, woven fabric, nonwoven fabric, or the like. The separator is preferably made of polyolefin such as polypropylene or polyethylene.

[0071] <<Appendix>> The above embodiments disclose the following techniques. (Technology 1) A secondary battery comprising: a positive electrode; a negative electrode having a negative electrode current collector and a negative electrode active material layer provided on the surface of the negative electrode active material layer; a separator interposed between the positive electrode and the negative electrode; an electrode group formed by winding the positive electrode and the negative electrode with the separator interposed therebetween; an electrolyte; and a battery case accommodating the electrode group and the electrolyte, wherein in the electrode group, the negative electrode is disposed on the outer periphery of the positive electrode, the negative electrode is at the outermost periphery of the electrode group and has a current collector exposed portion where the negative electrode current collector is exposed, and the expansion rate of the negative electrode active material layer due to charge and discharge of the negative electrode is greater at the ends in the width direction parallel to the winding axis of the negative electrode than at the center in the width direction. (Technology 2) The secondary battery according to Technology 1, wherein the width in the width direction of the center portion is 20% to 60% of the width of the negative electrode where the negative electrode active material layer is provided on the negative electrode. (Technology 3) The swelling ratio B of the negative electrode active material layer in the central portion 1 the expansion rate B of the negative electrode active material layer at the end 2 Ratio B to 1 / B 2 is equal to or greater than 0.985 and less than 1. (Technology 4) The secondary battery according to any one of Technologies 1 to 3, wherein the negative electrode active material layer contains a silicon-containing material, and a content ratio of the silicon-containing material in the negative electrode active material layer at the end portion is higher than a content ratio of the silicon-containing material in the negative electrode active material layer at the center portion. (Technology 5) The secondary battery according to any one of Technologies 1 to 4, wherein the current collector exposed portion of the negative electrode contacts the battery case during charging.

[0072] [Examples] Hereinafter, the present disclosure will be specifically described based on examples and comparative examples, but the present invention is not limited to the following examples.

[0073] Assuming an electrode group housed in an 18700-type secondary battery, the surface pressure applied to the electrode group due to the expansion of the negative electrode was calculated by stress simulation. The analysis software used was ADVENTURECluster from SCSK Corporation. The configuration of the electrode group used in the analysis is shown below.

[0074] Positive electrode: Length in winding direction D1: 700 mm Thickness: 0.200 mm (during discharge) Number of turns: 18.1 turns Young's modulus: 1.5 GPa Poisson's ratio: 0.35 Negative electrode: Length in winding direction D1: 800 mm Thickness: 0.200 mm (during discharge, of which the thickness of the negative electrode active material layer is 0.190 mm) Number of turns: 21.6 turns Young's modulus: 1.0 GPa Poisson's ratio: 0.35 Separator: Length in winding direction D1: 780 mm (inner peripheral side), 810 mm (outer peripheral side) Thickness: 0.0135 mm (during discharge) Battery case: Young's modulus: 190 GPa Poisson's ratio: 0.3

[0075] The negative electrode was divided into three equal parts in the width direction D2, and divided into three regions consisting of a central portion 16A having a width W / 3 and end portions 16B and 16C adjacent to the central portion 16A, each having a width W / 3. 2 is constant, and the expansion rate B of the negative electrode active material layer in the central portion 16A is 1 The distribution of surface pressure within the electrode group in the charged state was determined while changing the temperature.

[0076] The radial position where the surface pressure was maximum was determined within the electrode group. 1 , the inner diameter is R 2 When the distance from the innermost peripheral surface of the electrode group is (R 1 -R 2 The surface pressure was maximum at a position where the height from the bottom surface of the electrode group was 20 to 35% of W / 2. The distribution of the surface pressure in the width direction D2 applied to the negative electrode at the radial position where the surface pressure was maximum was determined. The surface pressure P 1 , and the surface pressure P at a position in the width direction D2 where the height from the bottom surface of the electrode group is W / 3 (the boundary position between the central portion 16A and the end portion 16C) 2 Search for P 2 P for 1 The ratio P 1 / P 2 was evaluated as the surface pressure ratio.

[0077] Table 1 shows the expansion ratio B of the negative electrode active material layer. 1 Swelling rate B 2 Ratio B1 / B 2 and the surface pressure ratio P 1 / P 2 From Table 2, the relationship between the ratio B 1 / B 2 When decreasing from 1, the surface pressure ratio P 1 / P 2 The difference in surface pressure between the central portion 16A and the end portions 16B and 16C is reduced. 1 / B 2 When is 0.985 or more and less than 1, the surface pressure ratio P 1 / P 2 is a positive value close to 1, and the surface pressure difference can be reduced.

[0078]

[0079] The above expansion rate B 1 and B 2 A secondary battery having a negative electrode having the above formula is produced, for example, by the following production method.

[0080] [Fabrication of negative electrode] Si powder and SiO 2 The powders were mixed in a 1:1 molar ratio and subjected to a sublimation reaction at 1300°C under reduced pressure to produce SiO. The produced SiO was pulverized in a jet mill to an average particle size (D50) of 6 μm to obtain SiO powder. The SiO powder was then carbon-coated (C-coated) at 850°C by thermal CVD using a mixed gas of argon and propane as the carbon source.

[0081] 96 parts by mass of graphite powder as a negative electrode active material, 4 parts by mass of SiO powder, 0.8 parts by mass of carboxymethyl cellulose (CMC), 0.1 parts by mass of carbon nanotubes (CNT), and water are mixed together, and 1.2 parts by mass of styrene-butadiene rubber (SBR) and water are mixed with this mixture to prepare a first negative electrode mixture slurry.

[0082] Similarly, 95 parts by mass of graphite powder as a negative electrode active material, 5 parts by mass of SiO powder, 0.8 parts by mass of carboxymethyl cellulose (CMC), 0.1 parts by mass of carbon nanotubes (CNT), and water are mixed together, and 1.2 parts by mass of styrene-butadiene rubber (SBR) and water are mixed with this mixture to prepare a second negative electrode mixture slurry.

[0083] The first negative electrode mixture slurry is applied to the central surface of a copper foil serving as a negative electrode current collector, the coating is dried, and then the second negative electrode mixture slurry is applied to the edge surface of the copper foil, the coating is dried, and the coating is compressed to a predetermined thickness using a rolling roller to obtain a negative electrode in which negative electrode active material layers are formed on both sides of the negative electrode current collector.

[0084] [Preparation of Positive Electrode] LiNi as Positive Electrode Active Material 0.8 Co 0.15 Al 0.05 O 2 (NCA), acetylene black (AB), and polyvinylidene fluoride (PVDF) were mixed in a mass ratio of 94:5:1, and an appropriate amount of N-methyl-2-pyrrolidone (NMP) was added to prepare a positive electrode mixture slurry. Next, this positive electrode mixture slurry was applied to both surfaces of a positive electrode current collector made of aluminum foil, and the coating was dried to form a positive electrode mixture layer. The coating was compressed to a predetermined thickness using a rolling roller to obtain a positive electrode in which a positive electrode active material layer was formed on both surfaces of the positive electrode current collector.

[0085] [Preparation of Electrolyte Solution] An electrolyte solution was prepared by adding LiPF as a lithium salt to a mixed solvent containing ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) in a volume ratio of 3:3:4. The concentration of LiPF in the nonaqueous electrolyte solution was 1.2 mol / L.

[0086] [Fabrication of Secondary Battery] The positive and negative electrodes are wound around a core with a polyethylene microporous membrane separator interposed therebetween to obtain a cylindrical wound electrode assembly. An aluminum positive electrode lead is welded to the exposed part of the positive electrode current collector, and a nickel negative electrode lead is welded to the exposed part of the negative electrode current collector.

[0087] The electrode assembly is housed in a cylindrical outer can with a bottom, and the positive electrode lead is welded to a sealing member and the negative electrode lead is welded to the inner bottom surface of the outer can. After the nonaqueous electrolyte is poured into the outer can, the opening of the outer can is sealed with a sealing member to prepare a nonaqueous electrolyte secondary battery (height 70 mm, diameter 18 mm). 1 / B 2 A secondary battery having a negative electrode with a conductivity of 0.99 can be obtained.

[0088] In addition, in the production of the negative electrode, the content ratio of the SiO powder in the first negative electrode mixture slurry was changed to 3.5 parts by mass relative to 96.5 parts by mass of the graphite powder, and the expansion ratio B 1 / B 2 A secondary battery having a negative electrode with a capacitance of 0.985 is obtained.

[0089] In addition, in the production of the negative electrode, the content ratio of the SiO powder in the first negative electrode mixture slurry was changed to 3 parts by mass relative to 97 parts by mass of the graphite powder, and the expansion ratio B 1 / B 2 A secondary battery having a negative electrode with a conductivity of 0.98 can be obtained.

[0090] In addition, in the preparation of the negative electrode, the content ratio of the SiO powder in the first negative electrode mixture slurry was changed to 5 parts by mass (the same as that of the second negative electrode mixture slurry) relative to 95 parts by mass of the graphite powder, and the expansion ratio B 1 / B 2 A secondary battery having a negative electrode of 1 is obtained.

[0091] While the present invention has been described in terms of presently preferred embodiments, such disclosure is not to be interpreted as limiting. Various changes and modifications will no doubt become apparent to those skilled in the art to which the present invention pertains upon reading the above disclosure. It is therefore intended that the appended claims be interpreted to cover all changes and modifications that do not depart from the true spirit and scope of the invention.

[0092] The secondary battery according to the present disclosure is useful as a main power source for mobile communication devices, portable electronic devices, electric vehicles, and the like.

[0093] 10: nonaqueous electrolyte secondary battery, 11: sealing body, 12: valve body, 13: metal plate, 14: insulating member, 15: positive electrode, 15L: positive electrode lead, 16: negative electrode, 16L: negative electrode lead, 17: separator, 18: electrode group, 21: gasket, 22: battery can, 22a: annular groove portion, 23: second insulating plate, 24: first insulating plate, 161: negative electrode current collector, 162: negative electrode active material layer

Claims

1. A secondary battery comprising: a positive electrode; a negative electrode having a negative electrode current collector and a negative electrode active material layer provided on a surface of the negative electrode current collector; a separator interposed between the positive electrode and negative electrode; an electrode group formed by winding the positive electrode and the negative electrode with the separator interposed therebetween; an electrolyte; and a battery case accommodating the electrode group and the electrolyte, wherein the outermost periphery of the electrode group is the negative electrode, and the outermost periphery has a current collector exposed portion where the negative electrode current collector is exposed, and a swelling rate of the negative electrode active material layer due to charging and discharging of the negative electrode is greater at the ends in the width direction parallel to the winding axis of the negative electrode than at the central portion in the width direction.

2. The secondary battery according to claim 1, wherein the width of the central portion in the width direction is 20% to 60% of the width of the negative electrode where the negative electrode active material layer is provided.

3. The swelling ratio B of the negative electrode active material layer in the central portion 1 The swelling rate B of the negative electrode active material layer at the end 2 Ratio to B 1 / B 2 The secondary battery according to claim 1 , wherein the m / z value is equal to or greater than 0.985 and less than 1.

4. The secondary battery according to any one of claims 1 to 3, wherein the negative electrode active material layer contains a silicon-containing material, and a content ratio of the silicon-containing material in the negative electrode active material layer at the end portion is higher than a content ratio of the silicon-containing material in the negative electrode active material layer at the center portion.

5. The secondary battery according to any one of claims 1 to 3, wherein the exposed current collector portion of the negative electrode is in contact with the battery case at least during charging.

Citation Information

Patent Citations

  • Nonaqueous electrolyte secondary battery

    WO2022024712A1

  • Negative electrode pate for lithium secondary battery and lithium secondary battery using it

    JP2007220450A

  • Wound type secondary battery

    JP2015191879A

  • Lithium ion secondary battery

    JP2018106903A

  • Nonaqueous electrolyte secondary battery

    WO2019244818A1